Redox flow battery electrodes
Ion implantation modifies carbon electrodes to create defect sites and nitrogen groups, addressing the limitations of existing carbon electrodes in redox flow batteries by enhancing electrochemical activity and wettability, leading to improved performance and cost-effective production.
Patent Information
- Application Number
- PCT/NZ2024/050034
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-03
AI Technical Summary
Current redox flow battery electrodes, particularly carbon-based ones, face challenges in achieving high electrochemical activity, wettability, and electrical conductivity, which limits their power density and efficiency, and existing processing methods like thermal oxidation and catalyst deposition are costly and inefficient for industrial-scale production.
The use of ion implantation to modify carbon electrodes by creating defect sites and nitrogen groups on the surface, which enhances electrochemical activity and wettability without compromising conductivity, and allows for precise control over the electrode's properties.
This approach results in carbon electrodes with improved electrochemical activity, reduced performance decay, and cost-effective industrial-scale production, while maintaining desirable electrical conductivity and hydrophilic properties, enhancing the overall performance of redox flow batteries.
Smart Images

Figure NZ2024050034_03102024_PF_FP_ABST
Abstract
Description
REDOX FLOW BATTERY ELECTRODES1. STATEMENT OF CORRESPONDING APPLICATIONS[1] This application claims priority to Australian Provisional Application No. 2023900842, filed 27 March 2023, the entire contents of which is herein incorporated by reference.2. FIELD OF INVENTION[2] The present disclosure relates to redox flow battery electrodes, and the associated methods and apparatus for producing same. The technology may find particular application in creating or modifying materials comprising carbon for use as electrodes in reduction-oxidation ("redox") flow batteries, however this should not be seen as limiting on the scope of the technology.3. BACKGROUND TO THE INVENTION[3] A shift towards generating energy from cleaner, more renewable energy sources has prompted a demand for reliable, cost-effective large-scale energy storage technologies. Among the various energy storage systems, redox flow batteries offer long cycling lifespans, ease of use, and decoupled power and energy densities.[4] Redox flow batteries (RFBs) are a type of rechargeable battery that store electrical energy in a liquid electrolyte solution. Unlike traditional batteries, where energy is stored in solid materials, RFBs use two separate liquid electrolyte solutions that are stored in tanks. These solutions are then pumped into the battery's electrochemical cell, where they undergo a chemical reaction that produces electrical energy.[5] RFBs work on the principle of reduction-oxidation "redox" reactions, which involve the transfer of electrons between two chemical species. In an RFB, the two electrolyte solutions are made up of different chemical species, which can be oxidized or reduced to store or release electrical energy. When the battery is charging, one of the solutions is oxidized and the other is reduced, and the process is reversed when the battery is discharging.[6] One of the advantages of RFBs is that they can be scaled up to store large amounts of electrical energy, making them suitable for grid-scale energy storage applications. They also have a relatively long cycle life and can be easily maintained by replacing the electrolyte solutions when they become depleted. However, RFBs currently have lower energy density and efficiency compared to traditional batteries, which makes them less suitable for applications that require high power density or portability.[7] One type of redox battery is the vanadium redox flow battery (VRFB). One advantage of VFRBs is that they do not suffer from irreversible cross-contamination of the redox species, which can be problematic in other redox flow battery systems. Extensive research into developing the different components of the VRFB has been done to improve battery performance and reduce overall cost, with considerable attention paid to enhancing the electrodes.[8] In RFBs, the electrodes play an important role in facilitating the redox reactions that occur between the two electrolyte solutions to generate electrical energy. RFBs typically have two types of electrodes: the positive electrode (also known as the cathode) and the negative electrode (also known as the anode). The positive electrode is typically made of a carbon material that is coated with a catalyst material, such as platinum or iridium, to facilitate the reduction of the oxidized species in the electrolyte solution.[9] The carbon material used as an electrode depends on the application and desired properties of the redox flow battery. The carbon material typically used is a carbon felt, carbon cloth or carbon paper. More recently there has been a shift towards porous, carbon materials such as carbon or graphite felt, as these exhibit good electrical conductivity, high chemical stability, high surface area, and low-cost. Unfortunately, these felts usually display poor electrochemical reversibility, therefore, most studies on felt electrodes concentrate on enhancing the reaction kinetics. Carbon felt is a synthetic material that may be made of graphite fibers that are needle-punched together to form a flexible, porous structure. The porosity of the carbon felt allows for a high surface area and high flow rate of the electrolyte solution, which is important for efficient redox reactions.
[0010] Ideally the electrode employed in a redox flow battery, would be chemically active, possesses high wettability, good electrical conductivity and have a high surface area. However, it is difficult to produce electrodes which meet all of these requirements. It can also be desirable to be able to modulate the specific properties of the electrode employed in a redox flow battery, to tune the attributes of the resulting redox flow battery. For carbon materials to be used as an electrode, these may be treated, prior to use in a redox flow battery, to modulate their specific mechanical / physical or chemicophysical or chemical properties.
[0011] One approach of treating carbon electrode materials is to use a process known as thermal oxidation. Thermal oxidation increases the number of functional groups in the surface of the felt by subjecting the felt to raised temperatures, typically to around 600°C for prolonged periods of time, such as for half an hour or more. Accordingly, this power intensive and relatively slow process, is not costefficient for the industrial-scale production of electrodes. It is also believed that heating the felt in thisway can reduce the electrical conductivity of the felt, which is undesirable in the production of carbon felt electrodes for use in RFBs.
[0012] Other methods of processing carbon electrode materials, involve depositing a catalyst onto the surface of the felt such as Rubidium or Platinum, using chemical, or physical vapour deposition. However, these processes are also relatively slow and are not conducive to industrial production.
[0013] It is an object of the present invention to address the foregoing problems or at least to provide the public with a useful choice.
[0014] All references, including any patents or patent applications cited in this specification are hereby incorporated by reference. No admission is made that any reference constitutes prior art. The discussion of the references states what their authors assert, and the applicants reserve the right to challenge the accuracy and pertinency of the cited documents. It will be clearly understood that, although a number of prior art publications are referred to herein, this reference does not constitute an admission that any of these documents form part of the common general knowledge in the art, in New Zealand or in any other country.
[0015] Throughout this specification, the word "comprise", or variations thereof such as "comprises" or "comprising", will be understood to imply the inclusion of a stated element, integer or step, or group of elements integers or steps, but not the exclusion of any other element, integer or step, or group of elements, integers or steps.
[0016] Further aspects and advantages of the present invention will become apparent from the ensuing description which is given by way of example only.4. SUMMARY OF THE INVENTION
[0017] Aspects of the technology relate to carbon materials as electrodes, and the associated methods and apparatus for producing same.
[0018] Reference herein to carbon electrodes should be understood to include any electrodes comprising carbon, including graphitised carbon, carbon felts, carbon cloth, carbon paper, carbon fibre, reticulated vitrified carbon, carbon composites (e.g., thermoplastic carbon composites), carbon meshes and foams. Naturally, this also encompasses, graphite felts, graphite cloth, graphite paper, graphite fibre, graphite composites, graphite meshes and foams. For sake of simplicity the foregoing will refer to these electrodes generally as carbon electrodes.
[0019] Reference herein to ion implantation should be understood to include processes where ions may be implanted into a substrate, where ions may not penetrate the surface of the substrate, where ions maydeflect from the surface of the substrate, and / or processes where ions may cause defects and edge sites on the substrate. Persons skilled in the relevant art will understand that the ion implantation process is a process where a substrate is bombarded with ions, i.e. ion bombardment. Persons skilled in the art should understand that in an ion implantation process, ion implantation in the substrate may or may not occur in every instance.
[0020] In one aspect of the technology, there is provided a carbon electrode for use in a redox flow battery. In another aspect there is provided a system for producing modified carbon electrodes. In another aspect there is provided methods of producing carbon electrodes.
[0021] In another aspect of the technology, there is provided carbon-based electrodes with defect sites and / or nitrogen groups in the carbon structure, which have been added via an ion implantation process. In some examples of the invention, implanted ion depth profile may be modulated by altering the ion fluence so to obtain the optimal nitrogen doping conditions for redox battery applications.
[0022] In some aspects of the invention, the inventors have prepared carbon and graphite electrodes with defect and / or edge sites only in the carbon structure.
[0023] In one aspect of the present technology, there is provided a carbon electrode for use in a redox flow battery, the carbon electrode comprising: at least one outer surface which has been modified using an ion implantation process, and an inner layer which is substantially unmodified by the ion implantation process.
[0024] In examples of the technology, the modified outer surface may comprise more defects or edge sites than the unmodified inner layer.
[0025] In examples of the technology, the modified outer surface may comprise surface atoms which are involved in bonds including -C-C, -C=C, -C-H, -C=O, -O-C=O, -C-O-, -C=N-, -N-C=O, aliphatic C-O, pyridinic- nitrogen, pyrrolic-nitrogen, quaternary-nitrogen, or oxidic-nitrogen bonds.
[0026] In examples of the technology, the carbon electrode may have a first outer surface and a second outer surface which is opposite to the first outer surface, and the inner layer is provided between the first outer surface and the second outer surface.
[0027] In examples of the technology, the first outer surface may have been modified using an ion implantation process, and the second outer surface has not been modified by an ion implantation process.
[0028] In examples of the technology, the first outer surface or second outer surface may comprise a label indicating the relative electrochemical activity of the first outer surface or second outer surface.
[0029] In examples of the technology, the first outer surface or the second outer may surface comprise: a first region which has been modified using an ion implantation process, and a second region which has not been modified using an ion implantation process
[0030] In examples of the technology, a distance between the first outer surface and second outer surface may define a thickness of the electrode, and wherein the at least one outer surface may be modified to a depth of less than or substantially equal to 5% of the thickness of the carbon electrode.
[0031] In examples of the technology, the at least one outer surface may be modified using an ion implantation process which accelerates ions into the surface of the carbon electrode with an ion implantation energy of between 0 keV and 99 keV.
[0032] In examples of the technology, the ion implantation process may have been configured to accelerate ions having an atomic mass of 14 u or greater.
[0033] In examples of the technology, the at least one outer surface may be modified using an ion implantation process which is configured to provide ions with a fluence range of between 1 x 1012ion / cm2to 1 x 1018ion / cm2.
[0034] In examples of the technology, the at least one outer surface may have an sp2 / sp3ratio in the range of 2.3 to 5 as determined by X-ray photoelectron spectroscopy as the ratio of the area of the fitted sp2peak (284.4 ± 1 eV) to the area of the fitted sp3peak (285 ± 1 eV) in the C Is spectra.
[0035] In examples of the technology, the at least one outer surface may have a degree of disorder (ID / IG) greater than 0.8 as determined by Raman spectroscopy when recorded at temperatures of 20°C + / - 10°C as the ratio of the intensity of the D-peak region (1350 ± 100 cm-1) to the intensity of the G-peak region (1580 ± 100 cm1).
[0036] In examples of the technology, the electrode may comprise: graphitised carbon, carbon felt, carbon cloth, carbon paper, carbon fibre, reticulated vitrified carbon, a carbon composite, a carbon mesh, a carbon foam, a graphite felt, graphite cloth, graphite paper, graphite fibre, a graphite composite, a graphite mesh and / or a graphite foam.
[0037] In one aspect of the present technology, there is provided a carbon electrode for use in a redox flow battery, comprising: a carbon electrode in the form a carbon sheet, having a first side and a second side, and wherein at least one of the first side or the second side is subjected to ion beam implantation, and the carbon sheet subjected to ion implantation has a degree of disorder (ID / IG) in the range of 0.8 to 3 as determined by Raman spectroscopy when recorded at temperatures of 20°C + / - 10°Cas the ratio of the intensity of the D-peak region (1350 ± 100 cm1) to the intensity of the G-peak region (1580 ± 100 cm1); and / or the carbon sheet subjected to ion implantation has an amorphisation ratio in the range of 1.4 to 7 as determined by Raman spectroscopy when recorded at temperatures of 20°C + / - 10°C as the ratio of the intensity of the G-peak region (1580 ± 100 cm1) to the intensity of the D"-peak region (1500 ± 100 cm1); and / or the carbon sheet subjected to ion implantation has a sp2 / sp3ratio in the range of 2.3 to 5 as determined by X-ray photoelectron spectroscopy as the ratio of the area of the fitted sp2peak (284.4 ± 1 eV) to the area of the fitted sp3peak (285 ± 1 eV) in the C Is spectra.
[0038] In examples of the technology, the carbon sheet subjected to ion beam implantation may be characterised by: a degree of disorder (ID / IG) in the range of 0.8 to 3 as determined by Raman spectroscopy when recorded at temperatures of 20°C + / - 10°C as the ratio of the intensity of the D-peak region (1350 ± 100 cm1) to the intensity of the G-peak region (1580 ± 100 cm1); an amorphisation ratio in the range of 1.4 to 7 as determined by Raman spectroscopy when recorded at temperatures of 20°C + / - 10°C as the ratio of the intensity of the G-peak region (1580 ± 100 cm1) to the intensity of the D"-peak region (1500 ± 100 cm1); and / or a sp2 / sp3ratio in the range of 2.3 to 5 as determined by X-ray photoelectron spectroscopy as the ratio of the area of the fitted sp2peak (284.4 ± 1 eV) to the area of the fitted sp3peak (285 ± 1 eV) in the C Is spectra.
[0039] In examples of the technology, the surface atoms may be involved in bonds such as -C-C, -C=C, - C-H, -C=O, -O-C=O, -C-O-, -C=N-, -N-C=O, aliphatic C-O, pyridinic-nitrogen, pyrrolic-nitrogen, quaternary- nitrogen, or oxidic-nitrogen bonds.
[0040] In another aspect of the present technology, there is provided a system for processing a carbon sheet for use in a redox flow battery, the system comprising: an ion implantation apparatus configured to treat the carbon sheet with ions having a mass greater than an electron, a fluence range of 1 x 1012ion / cm2to 1 x 1018ion / cm2, and an ion implantation energy between 0 keV and 99 keV. an ion implantation apparatus configured to treat a carbon sheet with ions having atomic mass between 1 and 131, a fluence range of 1 x 1012ion / cm2to 1 x 1018ion / cm2, and an ion beam implantation energy between 0 keV and 99 keV.
[0041] In examples of the technology, the ions may have atomic mass between 1 and 131, or 3 and 36, or 6 and 18.
[0042] In examples of the technology, the ions may have atomic mass between 1 and 131, or 3 and 36, or 6 and 18 and are singly charged ions.
[0043] In examples of the technology, the ions may comprise nitrogen, silicon, lithium, helium, neon, oxygen, carbon, and / or argon.
[0044] In examples of the technology, the ions may consist of either nitrogen, silicon, lithium, helium, neon, oxygen, carbon, and / or argon.
[0045] In examples of the technology, the ions may comprise nitrogen, neon, oxygen, carbon, and / or argon.
[0046] In examples of the technology, the ions may comprise either nitrogen and / or oxygen.
[0047] In examples of the technology, the ions may consist of either nitrogen, neon, oxygen, carbon, and / or argon.
[0048] In examples of the technology, the ions may consist of either nitrogen or oxygen.
[0049] In examples of the technology, the ions may be sourced by ionizing a dopant source gas. In some examples the dopant gas may comprise a C1-4 hydrocarbon, H2, BF3, B10H1 , B12H22, PH3, AsHs, PF5, AsF5, F Se, Ne, N2, Ar, GeF , GeF , SiF , and O2. Preferably, the dopant gas is a C1-4 hydrocarbon, H2, N2, O2, CO2, He, Ne, Ar.
[0050] In examples of the technology, the dopant gas may comprise a C1-4 alkane, a C2- alkene, or a C2- alkyne.
[0051] In examples of the technology, the dopant gas may comprise methane, ethane, or propane.
[0052] In examples of the technology, the ion implantation may be carried out in a vacuum, or otherwise at a pressure which is less than ambient. For example, the reduced pressure may be below an absolute pressure of 10-3mbar, such as an absolute pressure of between 10-4mbar and IO-7mbar.
[0053] In examples of the technology, the fluence range may be between 1 x 1012ion / cm2to 1 x 1018ion / cm2; 1 x 1013ion / cm2to 1 x 1017ion / cm2; 1 x 1013ion / cm2to 1 x 1016ion / cm2; or 1 x 1014ion / cm2to 1 x 1016ion / cm2.
[0054] In examples of the technology, the ion implantation energy may be between 0 keV and 99 keV. For example, the ion beam implantation energy may be between 0 keV and 50 keV, between 0 keV and 30 keV, between 5 keV and 30 keV, or between 10 keV and 30 keV.
[0055] In examples of the technology, the ion implantation apparatus may be configured to provide a treated carbon sheet wherein, at least one face of the carbon sheet: has a degree of disorder (ID / IG) in the range of 0.8 to 3 as determined by Raman spectroscopy as the ratio of the intensity of the D-peak region (1350 ± 100 cm1) to the intensity of the G-peak region (1580 ± 100 cm1); has an amorphisation ratio in the range of 1.4 to 7 as determined by Raman spectroscopy as the ratio of the intensity of the G-peak region (1580 ± 100 cm1) to the intensity of the D"-peak region (1500 ± 100 cm1); and / or has a sp2 / sp3ratio in the range of 2.3 to 5 as determined by X-ray photoelectron spectroscopy as the ratio of the area of the fitted sp2peak (284.4 ± 1 eV) to the area of the fitted sp3peak (285 ± 1 eV) in the C Is spectra.
[0056] In another aspect of the present technology, there is provided a method of producing a carbon electrode for a redox flow battery, the method comprising the steps of:A) positioning a carbon sheet in a vacuum chamber;B) treating at least one side of the carbon sheet by an ion implantation process; andC) removing the carbon sheet from the vacuum chamber, wherein the step of treating the carbon sheet is configured to produce a treated carbon sheet which: has a degree of disorder (ID / IG) in the range of 0.8 to 3 as determined by Raman spectroscopy as the ratio of the intensity of the D-peak region (1350 ± 100 cm1) to the intensity of the G-peak region (1580 ± 100 cm1); has an amorphisation ratio in the range of 1.4 to 7 as determined by Raman spectroscopy as the ratio of the intensity of the G-peak region (1580 ± 100 cm1) to the intensity of the D"-peak region (1500 ± 100 cm1); and / or has a sp2 / sp3ratio in the range of 2.3 to 5 as determined by X-ray photoelectron spectroscopy as the ratio of the area of the fitted sp2peak (284.4 ± 1 eV) to the area of the fitted sp3peak (285 ± 1 eV) in the C Is spectra.
[0057] In examples of the technology, the step of treating the carbon sheet via an ion implantation process may comprise using an ion beam comprising ions having atomic mass between 1 and 131, afluence range of 1 x 1012ion / cm2to 1 x 1018ion / cm2, and an ion beam implantation energy between 0 keV and 99 keV.
[0058] In examples of the technology, the step of treating the carbon sheet via an ion implantation process is performed using plasma immersion ion implantation and may comprise using a plasma comprising ions having atomic mass between 1 and 131, with implantation to a fluence range of 1 x 1012ion / cm2to 1 x 1018ion / cm2, and an ion implantation energy between 0 keV and 99 keV.5. BRIEF DESCRIPTION OF THE DRAWINGS
[0059] One or more embodiments of the technology will be described below by way of example only, and without intending to be limiting, with reference to the following drawings, in which:FIG. 1 shows a schematic view of a redox flow battery in accordance with one example of the present technology;FIG. 2A shows an isometric view of a carbon sheet / electrode in accordance with an example of the present technology;FIG. 2B shows an isometric view of a carbon sheet / electrode in accordance with another example of the present technology;FIG. 2C shows an isometric view of a carbon sheet / electrode in accordance with another example of the present technology;FIG. 3 shows a schematic view of a system / method of processing carbon sheets to form processed electrodes in accordance with the present technology;FIG. 4 shows an equivalent circuit diagram used for fitting electrochemical impedance spectroscopy (EIS) spectra in accordance with the present technology;FIG. 5 shows depth profiles for Nitrogen and Neon implantation as a function of ion fluence, in accordance with one example of the present technology; (a) Nitrogen (N+at 15 keV) implantation depth profiles for a fluence range of 1 x 1015- 4 x 1016ion cm'2, (b) Comparison of nitrogen (N+at 15 keV) and neon (Ne+at 9.5 keV) implantation profiles for a fluence of 1 x 1015ion cm'2.FIG. 6 shows the characterisation of pristine and ion-implanted carbon and graphite felts by Raman spectroscopy in accordance with one example of the present technology; First order Raman spectra of pristine felts and those ion-implanted at 1 xlO14, 1 xlO15, and 2 xlO16ion cm'2, specifically (a) Carbon felt - pristine and nitrogen-implanted, (b) Graphite felt - pristine and nitrogen-implanted, (c) Carbon felt - pristine and neon-implanted. (d) Graphite felt - pristine andneon-implanted. Second order Raman spectra of both pristine felts and those nitrogen-implanted at 1 xlO14and 1 xlO15ion cm'2, specifically (e) Carbon felt, (f) Graphite felt.FIG. 7 shows deconvoluted C Is XPS spectra for pristine carbon felt samples and nitrogen and neon-implanted samples at 4xl015ion cm'2;FIG. 8 shows deconvoluted O Is and N Is spectra for pristine carbon and graphite felts as well as those implanted with N2+, together with a comparison of the relative oxygen and nitrogen at. % content for pristine carbon and graphite felts as well as those implanted with l\h+;FIG. 9 shows polarisation curves for pristine and ion implanted felt electrodes, (a) Example polarisation curves of pristine carbon and graphite felts and those nitrogen-implanted at 1 xlO15ion cm'2. Comparison of the overpotential taken from the polarisation curve at 150 mA cm'2for varying implantation fluences for both (b) Carbon felt and (c) Graphite felt, (d) Example Impedance spectra of data points (marker) and fit (line) for pristine carbon and graphite felts and those nitrogen-implanted at 1 xlO15ion cm'2. Comparison of the RCT taken from the impedance spectra for varying implantation fluences for both (e) Carbon felt and (f) Graphite felt;FIG. 10 shows an example of impedance spectra fitted using an equivalent circuit, with a more pronounced semicircle in the high frequency region found for samples treated at a higher implantation fluence, (a) Carbon felt nitrogen-implanted at 4 xlO14ion cm'2, (b) Graphite felt nitrogen-implanted at 4 xlO16ion cm'2; andFIG. 11 shows the relationship between ion implantation fluence and electrode performance.6. BRIEF DESCRIPTION OF PREFERRED EMBODIMENTS OF THE INVENTION6.1. Overview of the Technology
[0060] FIG. 1 shows an example of a redox flow battery 100 in accordance with one example of the present technology. As shown, the redox flow battery comprises electrolyte storage tanks 102A, 102B, which contain an electrolyte solution 104. The electrolyte solution 104 is circulated through the redox flow system battery 100 using one or more fluid pumps 106 connected to one or more fluid conduits 107.
[0061] Between each electrolyte storage tank 102A, 102B, is an ion-selective membrane 108 and a pair of electrodes 110 which act as the anode and cathode of a conventional battery. In use a load 112 is connected between the electrodes, to create an electrical circuit. The flow of ions through the membrane, to each of the respective electrodes results in a current flow within the circuit, as should be familiar to those skilled in the art.
[0062] Many flow batteries use carbon electrodes due to their low cost, while still maintaining an adequate electrical conductivity. However, the use of traditional carbon electrodes can limit power density due to the carbon electrodes having low activity towards certain redox couples. Carbon electrodes are commonly provided as rectangular sheets of carbon material such as a carbon felt and can be provided in any size suitable for the application including in applications where the electrodes may have a surface area of 100 cm2or greater.
[0063] Accordingly, it can be advantageous to increase electrochemical activity, of the carbon electrodes to certain redox couples, to increase the wettability or hydrophilic properties of the carbon electrodes. Reference herein to the "activity" of the carbon sheets or resulting electrodes should be understood as the electrochemical activity of the respective carbon sheet or electrode, or otherwise the suitability of the electrode for use in a redox battery, due to its ability to facilitate ion transfer between the electrolyte solution and the electrode.
[0064] It can be desirable for the electrodes of these redox batteries to be as active as possible to provide an efficient battery, while maintaining desirable electrical conductivity, and hydrophilic properties in the respective electrolyte solutions 104.6.2. Ion Implantation
[0065] One aspect of the present technology is the use of ion implantation in the modification of carbon sheets, in order to provide active carbon electrodes suitable for use in redox battery applications.
[0066] While aspects of the present technology may be used on other carbon substrates such as powders, processing of carbon sheets enables the present invention to produce modified carbon electrodes in a cost and time efficient manner while also allowing a high degree of control over the resulting modified electrode.
[0067] Ion implantation is a process which comprises an ion source, where ions of a desired element are produced or provided, an accelerator configured to accelerate the particles, and a target chamber where the accelerated ions collide with the material to be implanted. Specific details of ion implantation equipment are not discussed in detail herein, and should be familiar to those skilled in the art.
[0068] The inventors have found that ion implantation techniques may be used to create defects in the surface of a carbon sheet and / or implant atoms with an atomic mass from 1 to 131 to the surface of the carbon sheet. In preferred examples of the technology, the inventors have used nitrogen, argon and oxygen atoms, to thereby increase the electrochemical activity of the carbon sheet in a redox flow battery, and / or otherwise may tune the properties of the carbon sheet, such as wettability, reduce performance decay, chemical resistance, and operational potential ranges, when used as an electrode in a redox flowbattery. Exemplification of the testing environment and corresponding results are summarised in FIG. 5 to FIG. 11, which are discussed in more detail below.
[0069] The inventors have found that beneficial results may be achieved using ions having an atomic mass of between 12 and 131, i.e., from carbon to xenon, with this range including ions of C1-4 hydrocarbons. As the skilled worker in the field would understand, the fluence and implantation energy may need to be modulated depending on ion species and properties of the carbon sheet in order to control the implantation depth. The inventors that found that in the ion implantation process, ions having an atomic mass of between 12 and 131, where the fluence range of 1 x 1012ion / cm2to 1 x 1018ion / cm2, and the implantation energy is between 0 keV and 99 keV, provides a suitable ion implantation depth in a carbon sheet, wherein the ion implanted carbon sheet as an electrode has suitable electrochemical activity.
[0070] In some examples of the technology, it may be beneficial to use ions of carbon, nitrogen, oxygen, neon and / or argon. While other implantation ions such as lithium, cobalt, and manganese may be used, there is increased global demand for these elements in light of a global transition away from fossil fuels. Accordingly, the ability to modify the surface characteristics of a carbon felt using low-cost abundant elements such as nitrogen, carbon, oxygen, neon and argon can provide significant economic, and environmental advantages.
[0071] The ion implantation process may employ ions generated from an ion source, which generates ions by introducing electrons into a vacuum chamber filled with the dopant source gas. The dopant feed stock gas is preferably C1-4 hydrocarbon H2, N2, O2, CO2, He, Ne, or Ar, or any combination thereof.
[0072] The inventors have found that in the ion implantation process, a fluence range of 1 x 1012ion / cm2to 1 x 1018ion / cm2is optimal in manufacturing a carbon sheet comprising functional surface groups, and / or sufficient surface defects such that the resulting modified carbon sheet has desirable electrochemical activity and / or electrical conductivity for use as an electrode.
[0073] The inventors have found that when the fluence range exceeds 1 x 1018ion / cm2an excessive number of defects may be created or generated on the surface of the carbon sheet, which may result in a carbon sheet with undesirable physicochemical properties for use as an electrode. Similarly, when the fluence range is too low, the overall effect of the ion implantation process on the carbon sheet is reduced to where it provides a lower influence on the activation of the carbon. Accordingly, in one aspect of the technology is can be advantageous to use a fluence range of between 1 x 1014ion / cm2to 1 x 1017ion / cm2to avoid these negative characteristics that can result from over or under exposure.
[0074] One benefit of the present technology is that the inventors have found that ion implantation may be performed using a relatively low ion beam implantation energy, such as between 0 keV and 99 keV. In contrast, conventional ion beam implantation energies can exceed several MV, and therefore there are potential energy savings provided by the present technology. In some examples of the technology, such as in the treatment of carbon felt electrodes, it has been found that an ion beam implantation energy between 5 keV and 30 keV can be suitable, particularly when used in combination with Carbon, Nitrogen, Oxygen, Neon and / or Argon ions.
[0075] Generally speaking, a greater implantation energy can result in a greater implanted ion depth, however the present technology has been found to provide significant improvements with relatively low ion implantation depths, such as generally just treating the surface of the carbon, or between 5nm and 250nm of the surface of the carbon. Accordingly, in the context of electrodes used in redox flow batteries, this represents a modification of the surface of the material up to a relative thickness of approximately 5%, such as approximately 1-2%. As one skilled in the art would understand, the present technology can allow this parameter to be adjusted depending on the other parameters employed in the ion implantation process, and the type of carbon electrode employed.
[0076] The skilled person in the art should understand that the ion beam or the carbon sheet can be oriented at a relative angle to one another, such that the angle of incidence can range from 0, i.e., substantially perpendicular to 45°. At larger angles of incidence, a significant fraction of the implanted ions may scatter out of the surface of the carbon sheet, so that the effective dose is reduced. As one in the art would appreciate this can be useful in creating long shadows or asymmetries in the carbon sheet if required.
[0077] The skilled person in the art would understand the implantation temperature is important in preventing decomposition near the surface region. One advantage of using ion implantation techniques as described herein, is that the treatment of the carbon sheet may be performed at relatively low temperatures such as below 293 degrees Kelvin, or approximately 20 degrees centigrade. As such the ion implantation and surface modification may be performed while maintaining minimal heating of the carbon sheet. As a result, negative effects of heating carbon in a vacuum such as a reduction in electrical conductivity, and / or a decrease in the wettability of the material may be largely avoided, while still allowing the activity of the carbon to be modified.
[0078] Another potential advantage of using the ion implantation technologies described herein is that it may be possible to limit the total temperature increase at the point of ion bombardment, to less than 60°C, and as such in addition to avoiding the negative side-effects of high temperature treatments, thetreated felt may be able to be handled by a user shortly after treatment, reducing the amount of cooling that would otherwise be required and improving the throughput of the system.
[0079] The use of Ion beam implantation is also beneficial over competing technologies such as chemical vapour deposition, or physical vapour deposition, as these techniques rely on condensation of a vapour on the surface of the carbon, which can be a slower process. Further advantages can include:• Better control over the surface modification process, which allows for greater precision in the thickness, composition, and properties of the deposited ions. Furthermore, the energy of the ions can be controlled precisely, allowing for tailored surface properties, and resulting electrode characteristics.• Reduced contamination. As ion implantation is a vacuum technique there is less contamination from other gases during the surface modification process.• A greater range of materials may be deposited, including metals, oxides, nitrides, and even polymers. This versatility makes it suitable for a broad range of applications, from semiconductor devices to optical coatings.• Low temperature deposition: ion implantation of carbon and hydrocarbon species can also deposit carbon films at lower temperatures than CVD, which can be important for temperaturesensitive substrates or when depositing multi-layer structures. This process is called ion beam deposition.
[0080] A skilled person in the art would understand how the parameters described here for ion beam implantation can be adapted for plasma immersion ion implantation.6.3. Electrode Categorisation
[0081] The use of ion implantation techniques as described herein has been found to provide beneficial characteristics for carbon electrodes, particularly for their use in redox flow batteries. Accordingly, there are benefits provided both from the systems, apparatus, and methods for treating carbon sheets, as well as the electrodes produced by these systems, apparatus, and methods. The inventors have therefore found that the treated carbon sheets produced by these systems may be characterised in the following ways.6.3.1. Relative Activity
[0082] One aspect of the technology is the use of ion implantation techniques on a carbon sheet or electrode 110. These are typically rectangular in shape, and have opposing outer surfaces referred to herein as a first side 202 and a second side 204. The thickness of the carbon sheet or electrode can bebetween approximately 0.1mm (in the case of carbon paper electrodes) up to around 10mm for thicker felt electrodes, however a common range is typically between approximately 2 mm and approximately 5mm. In particular as examples of the present technology relate to the surface treatment of the carbon sheet / electrode 110, the present technology may enable new redox flow battery electrodes to be produced at any thickness suitable for the application, while keeping production costs low. For example, in some applications it may be advantageous to provide a thicker carbon electrode for durability or reliability purposes, while in other applications it may be advantageous to provide a narrower electrode to conserve the available real-estate within the system.
[0083] In other words, aspects of the present technology relate to a carbon electrode which has at least one outer surface which is modified using an ion implantation process, and an inner layer 203 which remains substantially unmodified by the ion implantation process.
[0084] Keeping the inner layer 203 substantially unmodified by the ion implantation process may be particularly beneficial where the carbon material or felt has good conductivity and / or wettability characteristics which are desirable to maintain in the finished electrode. For example, other electrode modification techniques, such as heat and chemical immersion may be used to modify the electrochemical activity of the electrode as a whole, but these modifications can often reduce either the conductivity and / or wettability in addition to the electrochemical activity. Therefore, by being able to selectively modify portions of the electrode using an ion implantation technique, it is possible to preserve the desirable characteristics in the unmodified regions such as in the inner layer of the electrode.
[0085] The ion implantation techniques described herein may be used to treat certain areas of a carbon sheet / electrode, or alternatively just one side 202 / 204 of a carbon sheet or electrode 110. Accordingly, with reference to FIG. 2A the present technology allows the creation of a carbon electrode 110 in which a first side 202 of the electrode has a higher activity than a second side 204 of the electrode.
[0086] The use of the present technology to treat specific sides of a sheet / electrode should also not be seen as limiting on the present technology, for example with reference to FIG. 2B, the electrode 110 may be divided into a first region 206 and a second region 208, the first region has a higher activity than the second region. For example, the positioning of the first and second regions may be controlled by masking the ion beam during ion implantation, by not providing the ion beam in certain areas, and / or controlling the directionality, or timing of the activation of the beam.
[0087] The present technology should also not be limited to providing single areas having differing characteristics. For example, FIG. 2C shows one example of how a plurality of regions may be provided on a surface of an electrode. In the illustrated example alternating first 206 and second 208 regions areprovided, for example in a checkerboard pattern. However, these regions may be provided in any configuration suitable for a given redox application.
[0088] In some applications it may be beneficial for one or more sides / regions to remain untreated by the ion implantation processes described herein. This may be beneficial for example in situations where the untreated side / region has desirable characteristics such as a high wettability, or high electrical conductivity, which could be negatively affected by the ion implantation process.
[0089] Accordingly, the present technology can be used to provide an electrode having a first side 202 or region 206 with a first electrochemical activity, and a second side 204 or region 208 with a second electrochemical activity, the first electrochemical activity being greater than the second electrochemical activity.
[0090] This technology may therefore also be used to provide an electrode having a first side 202 or region 206 with a first electrical conductivity, and a second side 204 or region 208 with a second electrical conductivity, the first side 202 or region 206 having a greater electrical conductivity than the second side 204 or region 208. Similarly, an electrode may be provided having a first side 202 or region 206 with a first wettability and a second side 204 region 208 with a second wettability, wherein the first wettability is different to the second wettability.
[0091] In addition, the present technology may be used to deposit a range of different ions in the carbon sheet, accordingly, it may be possible to implant ions which are beneficial in some redox reactions, together with ions which are beneficial in other redox reactions so as to create a carbon sheet which is suited to a range of different redox reactions. For example, carbon electrodes 110 produced using the ion implantation processes described herein, may comprise and outer surface which has been modified to include a plurality of different deposited ions.6.3.2. Surface Characteristics
[0092] The inventors have found that by increasing the activity of the surface of the electrode, it is possible to provide an electrode which is more active overall this is believed to be as a result of the majority of the redox reactions occurring where the electrolyte meets the surface of the electrode. Accordingly, in comparison to untreated electrodes or heat / chemically treated electrodes a surface treated electrode can both reduce the number of ions required and improve the overall electrochemical activity of the electrode. The reduction in the number of ions required can translate to significant unit cost savings where the ions being implanted are rare or expensive due to market demand. For example, the price of lithium carbonate in China increased from approximately 37,000 CNY per tonne in October of 2020 to a peak of 597,500 CNY per tonne in November of 2022. Accordingly, by providing a process whichenables the surface activity of a carbon electrode to be increased, by either using less ions, and / or less expensive ions can translate to significant economic and environmental improvements.
[0093] For example, in one form of the technology, a carbon electrode is provided which has been modified with an ion implantation process which does not use lithium ions. In another example of the technology, a carbon electrode is provided which has been modified with an ion implantation process that uses carbon, nitrogen, oxygen, neon and / or argon ions.
[0094] The present technology also differs from techniques which are designed to fully coat or encase the electrode 110 with an electrochemically active coating such as using chemical immersion techniques, since these systems are reliant on using comparatively expensive coatings, and are slower and more complex to manufacture due to drying requirements. These processes can also negatively affect the electrode surface characteristics, as structure of the surface (such as the arrangement of fibres) can affect the overall conductivity, flow distribution, and create a pressure drop when the electrolyte is pumped through the electrode (thereby increasing pumping costs). A further benefit of the ion implantation process is that different ion treatments may be provided to different areas or outer surfaces of the electrode, for example to optimise specific regions or sides of the electrode.
[0095] Accordingly, in examples of the present technology an ion implantation process is used, in which ions are accelerated towards the surface of a carbon material, in order to create defects or edge sites in the surface structure of the carbon material, and as a result increase the chemical activity of the carbon material. Accordingly, in some examples of the technology it can be advantageous to use relatively heavy ions, such as those with an atomic mass of approximately 14 u (Nitrogen) or greater in order to improve the rate of formation of the surface defects in the carbon electrode.
[0096] As ion implantation is a surface treatment process, it is predominantly the outer layers of the electrodes which is modified by the present technology. This is different to most heat, and immersion treatment technologies, which generally affect the full cross section of the carbon sheet / felt. Accordingly, carbon sheets / electrodes treated by an ion implantation process may be identifiable from the depth of penetration of the implanted ions. Accordingly, carbon electrodes produced by the ion implantation techniques described herein can be found to have an implantation depth of between 5 nm, and 250 nm. In other examples, the ion implantation methods described herein may be configured to modify the outer surface to a depth of less than or substantially equal to 5% of the total thickness of the carbon electrode.
[0097] The increases in electrochemical activity provided by surface only treatment of the electrodes 110, was found to be an unexpected improvement over traditional bulk material processing techniques, which required treatment of the inner layers of the electrode.6.3.3. Raman Spectroscopy
[0098] As most graphitic materials are black in colour with a similar density, the characterization of graphitic samples to distinguish one from another is important. This is particularly important when considering the suitability for example of a carbon sheet or felt in redox flow battery applications. Accordingly, one method of characterising graphitic materials is to use Raman Spectroscopy.
[0099] Raman spectroscopy is a non-destructive analysis technique which provides information on the vibrational, rotational, and other states in the molecular system of the probed material. Specifically, Raman spectroscopy can provide information on the degree of graphitisation, disorder, crystallinity, and amorphisation of a carbon material due to the interaction of light with the chemical bonds within a material. For instance, the G-peak (typically present in the Raman spectra of a carbon-based material) generally found at approximately 1580 cm1provides information on the in-plane stretching of C=C bonds and is associated with a first order E2g longitudinal optical phonon mode. Also typically present in carbonbased materials, the intensity of the D-peak found at approximately 1350 cm1provides information on induced disorder brought about by edge sites, stacking faults, and atomic defects, and corresponds to a Alg breathing mode of a six-atom C-ring. In amorphous carbon-based materials, the D"-peak at approximately ~1500 cm1may be present, with an increase in D"-peak intensity indicating a decrease in crystallinity and an increase in amorphisation. Thus, Raman spectroscopy provides unique information on the carbon structure of materials, which is needed when defining qualities such as degree of graphitisation, crystallinity, defect density, amorphisation, and general information on the behaviour of the carbon matrix as a result of any modifications. This would allow a material which had undergone any modifications to be identified by a combination of difference characteristics such as, but not limited to, degree of graphitisation, crystallinity, defect density, amorphisation, and general information on the behaviour of the carbon matrix.
[0100] It should be appreciated to those skilled in the art that for graphitic materials, some of the most prominent features in the Raman spectra occur at approximately 1582 cm1, 1350 cm1, 1620 cm1, and 2700 cm1. These bands may be commonly known as the G, D, D', and G' bands respectively. Another band which is useful for determining the carbon amorphisation is the D" band at approximately 1500 + / - 100 cm-1. Measurements at these bands are preferably preformed using a laser excitation wavelength of approximately 532 nm (2.33 eV).
[0101] Methods of characterising electrodes as described herein may be performed by comparing the ratios of the intensity of these regions. For example, one key characteristic of the modified carbon sheet produced using the systems described herein comprises a degree of disorder in the range of 0.8 to 3,which is determined by the ratio of the intensity of the D-peak region (approximately 1350 + / - 100 cm1) to the intensity of the G-peak region (approximately 1580 + / - 100 cm-1).
[0102] A further method of characterising electrodes as described herein may be performed by analysing the amorphization ration of the carbon sheet, for example by comparing the ratio of the G-peak region (approximately 1580 + / - 100 cm-1) to the intensity of the D"-peak region (approximately 1500 + / - 100 cm’1). For example, it has been found that the face of the carbon sheet produced using the foregoing process may preferably have an amorphisation ratio in the range of 1.4 to 7.
[0103] While measurement of carbon amorphisation may be known to those skilled in the art, the inventors have found that measuring the D" peak from the lowest point between the D-peak and the G- peak may provide qualitative information on the degree of amorphisation at the material surface in order to minimise the influence of uncertainties from the peak fitting process. In contrast traditionally the D" peak would be measured from the intensity of the deconvoluted D" peak, which was found to be less consistent, accordingly, the amorphisation ratios described herein are preferably determined using this improved technique.
[0104] Further details of methods of measuring graphitic samples using Raman spectroscopy can further be found in "Studying disorder in graphite-based systems by Raman spectroscopy" (doi: 10.1039 / b613962k), published in April 2007 in Physical Chemistry, Chemical Physics 9(11):1276-91. The entire contents of which is herein incorporated by reference in its entirety.
[0105] Further examples of measuring amorphisation ratios are described in "The Importance of Interbands on the Interpretation of the Raman Spectrum of Graphene Oxide" (doi: 10.1021 / acs.jpcc.5b01590), published April 2015 in J. Phys. Chem. C 2015, 119, 18, 10123-10129. The entire contents of which is herein incorporated by reference in its entirety.6.3.4. X-Ray Photoelectron Spectroscopy
[0106] A further method of characterising carbon sheets in accordance with the present technology involves measuring the sp2 / sp3 ratios for example using X-ray photoelectron spectroscopy as should be familiar to those skilled in the art.
[0107] X-ray photoelectron spectroscopy (XPS) is a surface-sensitive, quantitative technique which can identify elements and their respective chemical and electronic states by irradiating the surface of a material under ultra-high vacuum using X-ray beams. From this, chemical states on the material surface are inferred by measuring the kinetic energy and number of ejected electrons. A typical XPS spectrum (often referred to as a survey spectrum) shows the number of excited and / or emitted electrons at a specific binding energy to identify different elements, with each identified element producing a set of XPSpeak / s. These peaks can be deconvoluted to provide information on the local bonding environment of an atomic species (i.e., C=C versus C-C, C-H) which is done by comparing the chemical shift in the binding energy from the nominal binding energy (i.e., 284.6 ± 0.2 eV for C Is). Thus, XPS provides information on the atomic percentage of different elements on the surface of a material (survey spectra), as well as relative percentages of the different chemical states of an element (high-resolution spectra). This would allow a material which had undergone any modifications to be identified by a combination of difference characteristics such as, but not limited to, elements present on the material surface, atomic percentage of each identified element, bonding and / or chemical state of each identified element, relative percentage of the identified bonding and / or chemical state of a single identified element, overall electronic structure, and density of the electronic states.
[0108] For example, the inventors have found that it can be advantageous for the modified carbon sheet to have a ratio of the area of the fitted sp2peak (284.4 ± 1 eV) to the area of the fitted sp3peak (285 ± 1 eV) in the C Is spectra of between 2.3 and 5.
[0109] While methods of determining sp2 / sp3ratios should be familiar to those skilled in the art, we note that further information is described in "sp2 / sp3 hybridization ratio in amorphous carbon from C Is corelevel shifts: X-ray photoelectron spectroscopy and first-principles calculation" (doi: 10.1103 / PhysRevB.65.045101), published January 2002, in Physical Review B 65(4). The entire contents of which is herein incorporated by reference in its entirety.6.3.5. Other Characteristic measurement technologies
[0110] While the foregoing examples of Raman and X-ray Photoelectron Spectroscopy may be used to determine the characteristics of electrodes produces under the foregoing conditions, it should be appreciated that other methods may also be used, including but not limited to Near Edge Spectroscopy. As such, while the materials produced using the aforementioned systems may be classified using alternative measurement techniques, the foregoing technology provides modified carbon sheets / electrodes having one or more of the characteristics described herein in relation to Raman, and / or X-Ray Photoelectron Spectroscopy.6.4. Methods of Modifying Carbon Sheets
[0111] In one example of the technology illustrated in FIG. 3, one or more carbon sheets 302 may be positioned within a vacuum chamber 304 (such as a chamber having an absolute pressure of < 10'4mbar) and at least one side or region of the carbon sheet treated by an ion implantation process, in order to form a treated carbon sheet or electrode 306.
[0112] For example, the ion implantation process may involve subjecting the at least one side or region of the carbon sheet to an ion beam comprising:• ions having atomic mass between 1 u and 131 u, preferably an atomic mass between 14 u and 131 u inclusive,• a fluence range of 1 x 1012ion / cm2to 1 x 1018ion / cm2, and• an ion beam implantation energy between 0 keV and 99 keV.
[0113] The carbon sheet or electrode which has then been processed by the ion implantation process should have at least one or more of the following characteristics:• Surface bonds consisting of carbon, nitrogen, and oxygen;• a degree of disorder (ID / IG) in the range of 0.8 to 3 as determined by Raman spectroscopy as the ratio of the intensity of the D-peak region (1350 ± 100 cm-1) to the intensity of the G-peak region (1580 ± 100 cm-1);• an amorphisation ratio in the range of 1.4 to 7 as determined by Raman spectroscopy as the ratio of the intensity of the G-peak region (1580 ± 100 cm-1) to the intensity of the D"-peak region (1500 ± 100 cm-l)a sp2 / sp3 ratio in the range of 2.3 to 5 as determined by X-ray photoelectron spectroscopy as the ratio of the area of the fitted sp2 peak (284.4 ± 1 eV) to the area of the fitted sp3 peak (285 ± 1 eV) in the C Is spectra; and / or• a carbon electrode with a surface which has been modified at a depth of up to 5% of the total material thickness.
[0114] It should be appreciated that both amorphous carbon, which is generally poorly performing for a redox flow electrode, and carbon defect sites (which are good for electrode performance) can be detected as sp3carbon. Accordingly, to more accurately detect the presence of carbon defect sites, it may be desirable for the carbon sheet or electrode to comprise an sp2 / sp3ratio in the range of 2.3 to 5 combined with an electrode which has a high degree of disorder (such as 0.8 to 3 as determined by Raman spectroscopy as the ratio of the intensity of the D-peak region (1350 ± 100 cm1) to the intensity of the G- peak region (1580 ± 100 cm1).
[0115] The process carbon sheet or electrode can then be removed from the vacuum chamber, and installed in a redox battery, or packaged for use / distribution.
[0116] In some examples of the technology, where certain sides or regions of the carbon sheet have been treated, it may be advantageous for the treated side (or vice versa) to be labelled or otherwise marked, so as to allow the redox battery manufacturer to position the electrode appropriately in the battery, for example with the more active side facing the electrolyte solution.
[0117] In some examples of the technology, it may be beneficial for the methods described herein to further comprise the step of heat treating the carbon sheet, either prior to, or following ion implantation. For example, heat treatment to temperatures above approximately 400 °C, may be used to modify the surface characteristics of the felt including for example the wettability of the carbon sheet. For example, the inventors have found that heating the carbon sheet in the presence of oxygen, can be used to increase the wettability of the carbon sheet or electrode, and conversely, removing oxygen-containing groups from the carbon sheet can reduce the wettability of the sheet.
[0118] It should be appreciated that the spectral analysis techniques described herein may be used to characterise the carbon sheets and electrodes produced using the present technology, and as such a further step may comprise performing spectral analysis on the carbon sheet, either prior to, or following ion implantation, and performing a secondary treatment such as a heat treatment depending on the results of the spectral analysis. In this way, carbon sheets which have a good wettability characteristic may be suitable for use in a redox battery without further requiring heat treatment.6.5. Modified Felt Products
[0119] In one example of the technology, a carbon electrode treated using an ion implantation process as described herein is provided with a label adhered or otherwise affixed to a first side of the electrode, the label indicating either the less active, or more active side of the electrode.6.6. Examples and Exemplification of the Technology6.6.1. Materials and methods6.6.1.1. Electrode preparation
[0120] The foregoing sets out the test environment which provides the results illustrated in the present specification, but should not be seen as limiting on the scope of the technology.
[0121] Carbon felt electrodes were prepared using commercially-available, polyacrylonitrile (PAN)-based carbon felt (C200, AvCarb) and graphite felt (G200, AvCarb) sheets. The felt was cut to a size of 0.6 cm2(1 cm by 0.6 cm) and cut through the midsection to give a thickness of 3 mm. The resulting felt sheets were then processing using ion implantation techniques described herein, and categorised using Raman and XPS spectroscopy, in accordance with the present technology.
[0122] For the purposes of the testing, the ion implantation took place in a sample chamber maintained under a vacuum having an absolute pressure of approximately 1 x 10'6mbar. A range of fluences from 1 x 1014to 4 x 1016ion cm-2were used for both l\h+ions (ion beam energy of 7.5 keV) and Ne+(ion beam energy of 9.5 keV) as illustrated in the following graphs and diagrams.6.6.1.2. Test Equipment
[0123] The surface morphology of the carbon and graphite felts were characterised using a scanning electron microscope (JEOL, Model JSM-IT300) unit, operated at an acceleration voltage of 15 kV. The elemental compositions and chemical states of the carbon felt samples were measured by XPS, using a Kratos Axis Ultra DLD with monochromatic Al-Karadiation (X = 1486.69 eV) and a spot size of 300 pm by 700 pm. The survey spectra and high-resolution spectra were recorded with a pass energy of 160 eV and 20 eV, respectively. A Shirley background correction and mixed Gaussian-Lorentzian line shape profiles were used as supplied by CasaXPS. Additionally, the sp2carbon peak was fitted with an asymmetrical tail. Data fitting was done so that the residual was minimised whilst using the least number of deconvoluted peaks to produce an appropriate fit.
[0124] Raman spectra were obtained via an Ocean Insight QEPro high-performance spectrometer, utilising an Ocean Insight 532 nm Raman diode laser (Energylaser = 2.33 eV, Powers > 50 mW) as the excitation source. An integration time of 75 s was used during each sample measurement, with each Raman spectrum acquired by averaging 5 scans of 75 s each. A Shirley background correction was applied to all Raman spectra, as provided by the CasaXPS software.6.6.1.3. Electrochemical measurements
[0125] Electrochemical measurements were carried out using a solution of 1.6 M VOSO4 (97%, Aldrich) dissolved in 3.4 M H2SO4 as the working electrolyte, which was electrochemically oxidised to achieve a solution of 50% SOC, 1.6 M VO2+ / VO2+in 3 M H2SO4. A counter electrolyte of 3 M H2SO4, a 6 cm2carbon felt counter electrode, and an Ag / AgCI reference electrode were all used in the half-cell counter chamber. The two chambers were separated by a N115 Nafion membrane (soaked in 0.5 M H2SO4 for at least 48 hours). The working electrolyte (80 mL) was pumped through the working side of the half-cell configuration at 200 mL min1, while the solution in the counter chamber was static. Dissolved oxygen was removed from the vanadium solution by bubbling argon through the electrolyte at 30 mL min1during all measurements.6.6.2. Material characterisation
[0126] Prior to any electrochemical measurements, a Pasteur pipette was used to gently suck internal air bubbles from each felt while immersed in electrolyte (1.6 M VOSO4 dissolved in 3 M H2SO4). This was then repeated in deionised water until the felt sample remained fully submerged with no apparent air bubbles.
[0127] Short charge and discharge tests (each lasting 60 s) were done over a range of 1 mA cm'2to 150 mA cm'2, with low current densities chosen to minimise concentration polarisation. Electrode overpotential was measured as the difference between the measured open circuit potential and therecorded potential versus the reference electrode from each charge or discharge test. Electrochemical impedance spectroscopy (EIS) measurements were recorded prior to each charge / discharge cycle over a frequency range of 0.5 MHz to 0.1 Hz and using a 10 mV rms AC perturbation. The resistance at -Zimagequal to zero during the high frequency measurements was taken as the electrolyte resistance and was used for post-run IR correction. All polarisation curves and impedance measurements were at room temperature (23 ± 1 °C) and carried out using a Gamry reference 3000AE potentiostat. Both the short charge and discharge tests and the EIS measurements were carried out twice with fresh ion-implanted electrode samples to ensure the validity of results. From this, the average value was taken and error bars for each data point were equal to the uncertainty calculated via the half range method, which should be familiar to those skilled in the art.
[0128] The capacitance of each sample was found by fitting impedance spectra to an equivalent circuit model (Fig. 4) consisting of an inductor, resistor, and two parallel resistor-capacitor (R-C) elements in series. Inductance was possibly due to deviations in potentiostat cable position throughout measurements, and was set to 0 H for spectra which did not show any -Zimagresponse below zero. The first resistor represents the electrolyte resistance, the first parallel R-C element represents the electrolyte / electrode surface at the membrane interface, and the second R-C element represents the charge-transfer resistance within the electrode pores. Both capacitors were replaced with a constant phase element to better simulate the double-layer capacitance. The mass diffusion behaviour at low frequencies was not modelled due to its complexity from the flowing electrolyte. The equivalent circuit model was fitted using the simplex method within Gamry's Echem analysis software.6.6.3. Ion implantation profile simulations
[0129] Simulations of the nitrogen-ion implantation depth profiles were conducted to show the theoretical distribution of nitrogen ions onto the felt electrode surface as a function of fluence. It was assumed that the ions were implanted onto a carbon surface, with a bulk density of 1.8 g cm'3as this is approximately the density of the fibres found in carbon (CF) and graphite felts (GF). As shown in FIG. 5(a), as the fluence is increased, the depth profile increases in height allowing for a higher nitrogen content at any given depth to be achieved. The nitrogen implantation profile can also be approximately matched via simulation of neon implantation which is shown in FIG. 5(b). This allows the conditions where neon implantation would match the damage profile from the nitrogen implantation to be extracted so that the effects of vacancies and changes in the carbon structure can also be investigated. The defects created by the path of the implanted ions can also be modelled with the majority of defects closer to the electrode surface compared to the implanted ion profile. Thus, fine-tuning the fluence can achieve the desired dopant concentration, implantation depth, and defect density.6.7. Raman spectroscopy
[0130] Raman spectroscopy was used to investigate the changes in bonding and degree of disorder introduced to the carbon and graphite felts as a result of the ion implantation as shown in FIG. 6a to FIG. 6D. The two main peaks often seen for carbon materials are the D peak at ~1350 cm'1representative of scattering from defects, edges, and disorder present in the carbon and the G peak at "'1580 cm'1which is a result of in-plane vibrations of sp2carbon. The ratio of these peak intensities, referred to as ID / IG, can be used to indicate the degree of defects. If the peak maxima drifts from their respective expected Raman shift, or if widening of these peaks occurs, peak fitting may be required to reveal the influence of less pronounced peaks, such as the D*, D", or D' peaks. These peaks can be an indication of a disordered graphitic lattice (D*), amorphous carbon (D"), or defects such as edge, vacancy, or sp3(D'). Peaks may also be seen in the second order Raman shift regions (2300 cm1to 3400 cm1), often with the most pronounced being the 2D peak at approximately 2700 cm1associated with the interactions between graphitic layers. Raman spectra were deconvoluted into 5 peaks for the first order Raman shift region (900 cm1to 1800 cm1) for both the carbon and graphite felt samples (Fig. 6e and 6f).
[0131] From the Raman spectra, it is clear that the carbon felt samples are highly amorphous in nature with the overall spectra shape remaining fairly consistent following nitrogen and neon ion implantation, regardless of fluence (Fig. 6a and 6c). However, the shape of the Raman spectra of the graphite felt samples changes significantly (Fig. 6b and 6d), and shows the impact of ion implantation on the carbon bonding at the electrode surface. It is obvious that implantation of the graphite felt resulted in an increasing degree of amorphous carbon and carbon bond defects, represented by the D* peak at 1200 cm1and the D" peak at 1500 cm1with increasing fluence. This is further supported by the decrease in intensity of the 2D peak found for the graphite felts treated at higher fluences (Fig. 6g and 6h). The increase in amorphous carbon content is a result of reduced crystallinity at the carbon fibre surface due to the increased disorder in the carbon lattice and the transition of sp2-C bonding to sp3-C. When comparing the Raman spectra of the GF samples to the CF samples, the G peak appears to be shifted approximately 10 cm'1towards a higher Raman shift, indicative of a more prominent contribution from the D' peak ("'1620 cm1). This suggests that the graphite felt, both the non-implanted and implanted samples, have a higher density of defects and edge sites compared to the carbon felt. Another aspect to note is the full width at half maximum (FWHM) of the D and G peaks of the CF Raman spectra, which are noticeably broader than the GF samples. This larger FWHM is a result of the distortion in the sp2bond length and angle, thus, a higher degree in amorphisation.
[0132] The amorphous carbon layer seen via Raman spectroscopy for the CF samples and GF samples treated at high implantation fluences was further probed via thermal treatment. A pristine carbon feltand a graphite felt implanted at a fluence of 4 x 1015ion cm'2was each thermally treated in a tube furnace at 900 °C for 1 hour (after a 15 °C / min temperature ramp) in an inert argon atmosphere. Raman spectroscopy was then done on the felt surface to determine the effects of thermal treatment on the degree of carbon amorphisation. No change in the amorphous region ("'1500 cm'1) was found after thermal treatment of the pristine CF, however, the degree of amorphisation of the GF sample implanted at 4 x 1015ion cm'2appeared to decrease. This suggests that the type of amorphous carbon already present on the CF surface and that which is introduced via ion implantation is different. Hence, it is hypothesised that any amorphisation introduced via ion implantation on the CF surface would not be seen in the amorphous region ("'1500 cm1) of the Raman spectra as it would overlap the amorphous nature of the CF surface already visible.6.8. X-ray photoelectron spectroscopy
[0133] X-ray photoelectron spectroscopy (XPS) was used to characterise the surface chemistry of both pristine carbon and graphite felts and those nitrogen-implanted across a range of varying fluence. The survey spectra show three peaks (C Is, O Is, and N Is) for the pristine CF and all the nitrogen-implanted GF, but only two peaks (C Is and O Is) for the pristine GF. This is to be expected, as during manufacturing the GF is thermally treated to up to approximately 2000 °C in an inert environment. This extent of graphitisation has been shown to remove the majority of nitrogen groups, as well as a significant amount of the oxygen groups. However, CF is only thermally treated around 1000 °C to 1300 °C in an inert environment (often referred to as carbonisation), which results in nitrogen and oxygen groups remaining present on the carbon fibres. Thus, using both carbon and graphite felts as the pristine electrode allows for the comparison of implanting nitrogen in a material either with or without an initial nitrogen content. Survey spectra of the pristine and nitrogen-implanted electrode samples were used to quantify the surface concentration of carbon, oxygen, and nitrogen (Table 1).Table 1. Carbon, oxygen, and nitrogen atomic content for each carbon and graphite felt sample extracted from the XPS survey spectra.Felt type Fluence Carbon Oxygen NitrogenTotal Total Total ion cm'2At. % At. % At. %Carbon - 89.9 7.4 2.7Carbon 1 x 101592.2 5.9 1.9Carbon 4 x l01591.8 6.0 2.2Carbon 1 x 101691.2 6.7 2.2Carbon 4 x l01690.1 6.1 3.8Graphite - 98.7 1.4Graphite 1 x 101597.7 1.9 0.4Graphite 4 x l01595.9 3.6 0.5Graphite 1 x 101696.2 3.0 0.7
[0134] High-resolution C Is spectra of each sample were deconvoluted to reveal the contributions of various carbon functional groups (Fig. 7a and 7b). A strong sp2carbon (C=C) and sp3carbon (C-C, C-H) signal at 284.1 ± 0.1 eV and 285.0 ± 0.1 eV, respectively, dominated the main peak of each spectra. Smaller peaks at 285.5 ± 0.1 eV, 286.0 ± 0.1 eV, 287.2 ± 0.1 eV, and 288.7 ± 0.1 eV were assigned to carbon singly bonded to nitrogen (C-N), alcohol / ether (C-O-R), carbonyl (C=O), and carboxyl / ester (O=C-O-R), respectively. It should be noted that contributions from groups such as C=N (287.2 ± 0.1 eV), N-C=O (288.7 ± 0.1 eV) and carbonate (290.5 ± 0.1 eV) are found at similar binding energies as those listed above.
[0135] A significant increase in the sp2carbon content after ion implantation was found for the carbon felt, shown by the shift in the main peak towards a lower binding energy as indicated by the dashed line (Fig. 7a). The opposite was observed for the graphite felt which initially has a high sp2-C content of 85%, with a decrease in sp2carbon content observed after ion implantation. This is represented by a widening of the main peak, quantified by an increase in the FWHM from 0.75 eV for the pristine GF to 0.82 - 1.2 eV for the implanted GF samples. This difference in initial sp2-C content for the two felt materials is to the manufacturing process, as the graphite felt underwent the additional graphitisation process. This shows that the initial carbon chemistry of the material dictates the impact that ion implantation has on the type of carbon bonding introduced, as reflected in literature. Often it is found that for graphite-like carbon materials (high sp2-C content) that the sp2carbon will decrease after ion implantation due to the rehybridisation of sp2to sp3carbon. However, for diamond-like carbon materials (high sp3-C content) it has been found that ion implantation will disrupt the sp3carbon lattice and thus introduce sp2carbon bonding. 1
[0136] A strong correlation between the content of sp2carbon and ion fluence was found for both the implanted carbon and graphite felts (Fig. 7c), where the sp2-C content appeared to decrease with increasing fluence. These changes in sp2carbon for the GF is reflected in the Raman spectra, which revealed an increase in the amorphous carbon with increasing fluence for the GF samples (Fig. 6b and 3d). The gradient of the fitted data for the GF implanted samples is steeper, indicating that there is a greater reduction in sp2with increasing implantation fluence compared to the CF implanted samples. There also appears to be a trend between the FWHM of the C Is high-resolution spectra and the implantation fluence for the carbon and graphite felt samples (Fig. 7d). This relates to the decreasing sp2-C seen with increasing fluence, as the increase in FWHM is due to the peak broadening analogous with a higher content of sp3- C, and oxygen and nitrogen functional groups found at binding energies above approximately 284.5 eV.
[0137] From the survey spectra, the overall oxygen content of the CF was seen to slightly decrease (Table 1) after implantation, indicating that oxygen functional groups were removed from the carbon fibre surface. The opposite occurred with the GF, with the oxygen content increasing after nitrogenimplantation and the inventors believe that this phenomenon is related to the oxidation of the fibre surface as the treated felts were re-exposed to air when exiting the vacuum chamber. The high-resolution O Is spectra (Fig. 8a and 8b) was used to evaluate the influence of implantation fluence on surface oxygen groups (Fig. 8e and 8f). The three main oxygen groups identified were C=O (01) at 531.1 ± 0.1 eV, aliphatic carbon - oxygen (O2) at 532.2± 0.1 eV, and aromatic carbon - oxygen (O3) at 533.2 ± 0.1 eV. The implanted GF samples also show an increasing content of aliphatic carbon - oxygen bonds after implantation, which may be linked to the increasing D" peak with increasing fluence as aliphatic carbon - oxygen sp3carbon bonds are often found as a part of amorphous carbon. However, the aliphatic carbon - oxygen content of the CF samples is higher and does not seem to significantly change, which is not surprising as the amorphous carbon content indicated by the Raman spectra does not appear to change post-implantation, or with varying fluence. The overall C=O content does not appear to significantly change for either the carbon or graphite samples.
[0138] The N Is region shows the changes in nitrogen functional groups as a result of ion implantation (Fig. 8g and 8h), with the spectra deconvoluted to up to four different nitrogen peaks (Fig. 8c and 8d). The four main nitrogen species identified being pyridinic-N (Nl) at 398.4 ± 0.1 eV, pyrrolic-N (N2) at 399.8 ± 0.2 eV, quaternary-N (N3) at 400.8 ± 0.1 eVs, and oxidic-N (N4) at 403.0 ± 0.2 eV. Both pyridinic-N and pyrrolic-N groups increase with increasing fluence for the carbon and graphite felts, implying that these nitrogen groups are more inclined to form during nitrogen implantation. These is especially evident when looking at the GF N Is spectra, as only pyrrolic is present at lower fluences (Fig. 8d). The preferential formation of pyridinic- and pyrrolic-N is thought to occur due to the greater defect density introduced tothe felt surface by the implanted ions, which in turn provides carbon sites for the nitrogen to bond to. This is in agreement with other studies, as pyridinic-N and pyrrolic-N more readily form on edge sites and defects introduced during nitrogen-implantation compared to graphitic-N. Interestingly, the overall nitrogen content of the carbon felts implanted at lower fluences (1 x 1015to 1 x 1016ion cm'2) appears to decrease when compared to the nitrogen content of the pristine CF material. We hypothesise that this may be a result of the higher initial nitrogen content of the carbon felt being removed by the implanted ions at the felt surface, but still being much greater than the amount of nitrogen being successfully implanted at low fluences. This is not the case with the GF, with initially no surface nitrogen groups for the pristine sample and increasing nitrogen content with increasing ion fluence.6.9. Electrochemical characterisation
[0139] To study the electrode activity of each sample, polarisation curves (Fig. 9a) for both the pristine carbon and graphite felts, and those implanted over a fluence range of 1 x 1014to 4 x 1016ion cm'2, were done using galvanostatic tests over a range of current densities. It is assumed that the majority of the extracted overpotential is the electrode activation polarisation, as a high vanadium concentration is used, the tests are done at low currents, and the reported overpotential values are IR-corrected. A correlation between electrode overpotential at 150 mA cm'2and implantation fluence was found for both the CF (Fig. 9b) and GF (Fig. 9c) samples, with improved electrode performance seen when the felts were treated at fluences less than approximately 1 x 1016ion cm'2. The carbon felt shows greater improvement compared to the graphite felt with both felt types reaching an electrode overpotential of ~45 mV. The graphite felt appears to have a limiting performance around 1 x 1015ion cm'2with electrode improvement trending back towards the GF pristine threshold, however, the CF samples remains enhanced down to the lowest treatment fluence of 1 x 1014ion cm'2. Other studies have also found this relationship between fluence and electrode performance, where an optimal implantation fluence is reached before the electrode activity declines at higher fluences. Neon implantation of both carbon and graphite felt was done to compare the electrochemical response to both nitrogen groups and structural defects (nitrogen implantation) versus structural defects only (neon implantation). The electrochemical performance of each Ne+-doped electrode followed the same trend as the N2+-doped samples (Fig. 9b and 9c), suggesting that structural defects and carbon vacancies, and not nitrogen groups, are the dominating characteristic for catalysing the positive vanadium reaction.
[0140] Additionally, the impedance spectra for each sample were fitted (Fig. 9d) and the reaction kinetics of each felt sample characterised by the extracted charge transfer resistance (RCT). The trend between RCT and fluence (Fig. 9e and 9f) is similar to that with electrode overpotential, as expected due to the correlation between RCT and overpotential. A lower charge transfer resistance is achieved for the carbonand graphite electrodes implanted at the lower fluence range, like that seen from the polarisation curves. Again, both the nitrogen- and neon-implanted felt samples follow the same trend in Rcr, suggesting that electron charge transfer is improved via structural defects and edge sites introduced by ion implantation. When comparing the EIS spectra of both CF and GF samples treated at a fluence lower than 2 x 1016ion cm'2(Fig. 10b) to a fluence of 2 x 1016ion cm'2and above (Fig. 10c) the inventors found a more pronounced semicircle in the high frequency region for the higher implantation fluence, represented by a R-CPE element between the electrolyte solution resistance and the RCT-CPE element. This was thought to be a result of the increase in amorphous carbon at higher fluences resulting in an impedance response similar to that of passive films at an electrode surface.
[0141] The electrochemical double layer capacitance (EDLC) of the carbon and graphite felt samples was investigated by fitting an equivalent circuit to each impedance spectra, as detailed above (see Fig. 4). An average EDLC of 0.21 ± 0.08 mF for the GF samples and 0.11 ± 0.07 mF for the CF samples was found, with no significant trend between capacitance and ion implantation fluence. No significant difference in capacitance was found between the N2+- and Ne+-doped samples. The slightly higher EDLC found for the graphite felts could be due to the slightly higher ratio of defects to graphitic carbon as found by Raman spectroscopy (Fig. 3a - d), with a higher EDLC often found for edge sites ("'50-70 pF cm'2) compared to basal planes (~2-3 pF cm'2). It was expected that there would not be a significant change in capacitance, as only the top layer of fibres at the electrode surface is altered by the ion implantation.
[0142] Based on the electrochemical performance of both the CF and GF samples, it was concluded that the electrode activity was enhanced by the introduction of defects. This is supported by the ID / IG ratio extracted from Raman spectra, where the ID / IG ratio is the highest for the same fluence (1 xlO15ion cm'2) where electrode overpotential is minimised (Fig. 11a). However, it was found that the electrode performance is inhibited for an implantation fluence above 1 xlO16ion cm'2for both the carbon and graphite felts. This is thought to be due to the increased amorphous carbon at the electrode surface (Fig. lib) compromising the electrical conductivity due to the increased lattice disorder reducing the charge carrier mobility. There did not appear to be any significant different between nitrogen- and neon- implantation which suggests that nitrogen groups are not important for facilitating the positive vanadium reaction.
[0143] Initially, defects and edge sites are created via the collision path of the implanted ions which results in a higher density of active sites to facilitate the VO2+ / VO2+redox reaction. However, increasing the treatment fluence increases the number of ion collisions occurring in the carbon lattice, which results in a decrease in sp2-C groups and the formation of an amorphous carbon layer, as quantified by XPS and Raman spectroscopy. Thus, the increased disorder in the carbon structure leads to badly defined edgesites and a lower density of active defect sites, which leads to a worsened electrode performance. This is also thought to lead to worsened conductivity at the electrode surface due to the lack of crystallinity and a disordered carbon lattice, which in turn adds to the electrode / electrolyte interfacial resistivity.6.10. Other Remarks
[0144] Unless the context clearly requires otherwise, throughout the description and the claims, the words "comprise", "comprising", and the like, are to be construed in an inclusive sense as opposed to an exclusive or exhaustive sense, that is to say, in the sense of "including, but not limited to".
[0145] The entire disclosures of all applications, patents and publications cited above and below, if any, are herein incorporated by reference.
[0146] Reference to any prior art in this specification is not, and should not be taken as, an acknowledgement or any form of suggestion that that prior art forms part of the common general knowledge in the field of endeavour in any country in the world.
[0147] The technology may also be said broadly to consist in the parts, elements and features referred to or indicated in the specification of the application, individually or collectively, in any or all combinations of two or more of said parts, elements or features.
[0148] Where in the foregoing description reference has been made to integers or components having known equivalents thereof, those integers are herein incorporated as if individually set forth.
[0149] It should be noted that various changes and modifications to the presently preferred embodiments described herein will be apparent to those skilled in the art. Such changes and modifications may be made without departing from the spirit and scope of the technology and without diminishing its attendant advantages. It is therefore intended that such changes and modifications be included within the present technology.
Claims
7. CLAIMS1. A carbon electrode for use in a redox flow battery, the carbon electrode comprising: at least one outer surface which has been modified using an ion implantation process, and an inner layer which is substantially unmodified by the ion implantation process.
2. The carbon electrode of claim 1, wherein the modified outer surface comprises more defects or edge sites than the unmodified inner layer.
3. The carbon electrode of claim 1 or 2, wherein the modified outer surface comprises surface atoms which are involved in bonds including -C-C, -C=C, -C-H, -C=O, -O-C=O, -C-O-, -C=N-, -N-C=O, aliphatic C-O, pyridinic-nitrogen, pyrrolic-nitrogen, quaternary-nitrogen, or oxidic-nitrogen bonds.
4. The carbon electrode of any one of the preceding claims, wherein the carbon electrode has a first outer surface and a second outer surface which is opposite to the first outer surface, and the inner layer is provided between the first outer surface and the second outer surface.
5. The carbon electrode of claim 4, wherein the first outer surface has been modified using an ion implantation process, and the second outer surface has not been modified by an ion implantation process.
6. The carbon electrode of claim 4, wherein the first outer surface or second outer surface comprises a label indicating the relative electrochemical activity of the first outer surface or second outer surface.
7. The carbon electrode of claim 4, wherein the first outer surface or the second outer surface comprises: a first region which has been modified using an ion implantation process, and a second region which has not been modified using an ion implantation process8. The carbon electrode of claim 4, wherein a distance between the first outer surface and second outer surface defines a thickness of the electrode, and wherein the at least one outer surface is modified to a depth of less than or substantially equal to 5% of the thickness of the carbon electrode.
9. The carbon electrode of any one of the preceding claims, wherein the at least one outer surface is modified using an ion implantation process which accelerates ions into the surface of the carbon electrode with an ion implantation energy of between 0 keV and 99 keV.
10. The carbon electrode of any one of the preceding claims, wherein the ion implantation process accelerated ions having an atomic mass of 14 u or greater.
11. The carbon electrode of any one of the preceding claims, wherein the at least one outer surface is modified using an ion implantation process which is configured to provide ions with a fluence range of between 1 x 1012ion / cm2to 1 x 1018ion / cm2.
12. The carbon electrode of any one of the preceding claims, wherein the at least one outer surface has a sp2 / sp3ratio in the range of 2.3 to 5 as determined by X-ray photoelectron spectroscopy as the ratio of the area of the fitted sp2peak (284.4 ± 1 eV) to the area of the fitted sp3peak (285 ± 1 eV) in the C Is spectra.
13. The carbon electrode of any one of the preceding claims, wherein the at least one outer surface has a degree of disorder (ID / IG) greater than 0.8 as determined by Raman spectroscopy when recorded at temperatures of 20°C + / - 10°C as the ratio of the intensity of the D-peak region (1350 ± 100 cm-1) to the intensity of the G-peak region (1580 ± 100 cm1).
14. The carbon electrode of any one of the preceding claims, wherein the electrode comprises: graphitised carbon, carbon felt, carbon cloth, carbon paper, carbon fibre, reticulated vitrified carbon, a carbon composite, a carbon mesh, a carbon foam, a graphite felt, graphite cloth, graphite paper, graphite fibre, a graphite composite, a graphite mesh and / or a graphite foam.
15. A method of preparing a carbon material for use as an electrode, comprising the steps of:(i) subjecting the carbon material to ions having an atomic mass of 14u or greater, wherein the ions are accelerated into the surface of the carbon material via an ion implantation apparatus to create a carbon electrode, wherein the ion implantation apparatus is configured to provide the ions with a fluence range of between 1 x 1012ion / cm2to 1 x 1018ion / cm2, and wherein the ion implantation apparatus is configured to use an implantation energy of between 0 keV and 99 keV.
16. The method according to claim 15, wherein the ions have an atomic mass of between 14 u and 131 u inclusive.
17. The method according to claim 15 or 16, wherein the method further comprises the step of ionizing a dopant source gas to provide the ions, wherein the dopant gas may comprise a C1-4 hydrocarbon, H2, N2, O2, CO2, He, Ne, or Ar.
18. The method according to any one of claims 15 to 17, wherein the ions have an atomic mass between 14 and 36 inclusive.
19. The method according to any one of claims 15 to 18, wherein the ions have an atomic mass between14 and 18 inclusive.
20. The method according to any one of claims 15 to 119, wherein the ion implantation apparatus is configured to provide the ions with a fluence range of between 1 x 1013ion / cm2to 1 x 1016ion / cm2.
21. The method according any one of claims 15 to 20, wherein the fluence range is between 1 x 1014ion / cm2to 1 x 1016ion / cm2.
22. The method according to any one of claims 15 to 21, wherein the implantation energy is between 0 keV and 50 keV.
23. The method according to claim 22, wherein the implantation energy is between 10 keV and 30 keV.
24. The method according to any one of claims 15 to 23, wherein the ion implantation apparatus is configured to accelerate the ions into the carbon material under a reduced pressure, wherein the reduced pressure is an absolute pressure of less than 10'3mbar.
25. The method according to any one of claims 15 to 24, wherein the ion implantation apparatus is configured to accelerate the ions into the carbon material under a reduced pressure, wherein the reduced pressure is an absolute pressure of between 10'4mbar and IO-7mbar.
26. The method according to any one of claims 15 to 25, wherein the carbon material, comprises one or more of: graphitised carbon, carbon felt, carbon cloth, carbon paper, carbon fibre, reticulated vitrified carbon, a carbon composite, a carbon mesh, a carbon foam, a graphite felt, graphite cloth, graphite paper, graphite fibre, a graphite composite, a graphite mesh and / or a graphite foam.
27. The method according to any one of claims 15 to 26, further comprising the steps of: positioning the carbon material in a vacuum chamber, subjecting at least one side of the carbon material to the ions to create the carbon electrode, and removing the carbon electrode from the vacuum chamber.
28. The method of any one of claims 15 to 27, wherein the carbon material is prepared for use in a redox flow battery.
29. A carbon electrode produced by the method of any one of the claims 15 to 28.
30. The carbon electrode of claim 29, wherein the carbon material has a degree of disorder (ID / IG) in the range of 0.8 to 3 as determined by Raman spectroscopy when recorded at temperatures of 20°C + / - 10°C as the ratio of the intensity of the D-peak region (1350 ± 100 cm1) to the intensity of the G-peak region (1580 ± 100 cm1), and / oran amorphisation ratio in the range of 1.4 to 7 as determined by Raman spectroscopy when recorded at temperatures of 20°C + / - 10°C as the ratio of the intensity of the G-peak region (1580 ± 100 cm1) to the intensity of the D"-peak region (1500 ± 100 cm1), and / or a sp2 / sp3ratio in the range of 2.3 to 5 as determined by X-ray photoelectron spectroscopy as the ratio of the area of the fitted sp2peak (284.4 ± 1 eV) to the area of the fitted sp3peak (285 ± 1 eV) in the C Is spectra.
31. The carbon electrode of claim 29 or 30, comprising surface atoms which are involved in bonds including -C-C, -C=C, -C-H, -C=O, -O-C=O, -C-O-, -C=N-, -N-C=O, aliphatic C-O, pyridinic-nitrogen, pyrrolic- nitrogen, quaternary-nitrogen, or oxidic-nitrogen bonds.
32. A system for treating a carbon material to provide an electrode, wherein the system comprises, an ion beam implantation apparatus configured to subject the carbon material to ions having a mass greater than an electron, and wherein the ion beam implantation apparatus is configured to provide a fluence range of the ions of between l x 1012ion / cm2to l x 1018ion / cm2, and an implantation energy of the ions of between 0 keV and 99 keV.
33. A carbon electrode, comprising: a carbon sheet, wherein at least part of the carbon sheet has been subjected to ion implantation, and wherein the part of the carbon sheet subjected to ion implantation: has a degree of disorder (ID / IG) in the range of 0.8 to 3 as determined by Raman spectroscopy as the ratio of the intensity of the D-peak region (1350 ± 100 cm1) to the intensity of the G-peak region (1580 ± 100 cm1); and / or has an amorphisation ratio in the range of 1.4 to 7 as determined by Raman spectroscopy as the ratio of the intensity of the G-peak region (1580 ± 100 cm1) to the intensity of the D"-peak region (1500 ± 100 cm1); and / or a sp2 / sp3ratio in the range of 2.3 to 5 as determined by X-ray photoelectron spectroscopy as the ratio of the area of the fitted sp2peak (284.4 ± 1 eV) to the area of the fitted sp3peak (285 ± 1 eV) in the C Is spectra.
34. The carbon electrode of claim 33, wherein the carbon sheet has been subjected to ion implantation consisting of:ions having a mass greater than or substantially equal to 14 u, a fluence range of between 1 x 1012ion / cm2to 1 x 1018ion / cm2, and an implantation energy of between 0 keV and 99 keV.
35. The carbon electrode, according to claim 33 or 34, comprising surface atoms which are involved in bonds including -C-C, -C=C, -C-H, -C=O, -O-C=O, -C-O-, -C=N-, -N-C=O, aliphatic C-O, pyridinic-nitrogen, pyrrolic-nitrogen, quaternary-nitrogen, or oxidic-nitrogen bonds.
Citation Information
Patent Citations
Preparation method and application of air electrode of modified lithium air battery
CN104064837A
Preparation method and application of doping content-controllable nitrogen-doped carbon material
CN107819111A
Carbon electrode modified by ion implantation
JP1985077984A
Battery electrode material, its manufacture, and electrochemical battery
JP2000030715A
Prelithiated lithium ion battery and making a prelithiated lithium ion battery
US20210075001A1