Non-oriented electrical steel sheet, rotor core, motor, and method for producing non-oriented electrical steel sheet

WO2024210197A1PCT designated stage expired Publication Date: 2024-10-10NIPPON STEEL CORPORATION

Patent Information

Application Number
PCT/JP2024/014046
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-07
Filing Date
2024-04-05
Publication Date
2024-10-10

Smart Images

  • Figure JP2024014046_10102024_PF_FP_ABST
    Figure JP2024014046_10102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a non-oriented electrical steel sheet capable of providing high strength and excellent magnetic characteristics and excellent in dimensional accuracy after punching. A non-oriented electrical steel sheet according to the present embodiment contains, in % by mass, 3.1-4.5% of Si, further, Ti, Si, Al, Zr, Nb, V, Mo, Cr, C, La, Ce and N satisfy formula (1) and formula (2), the tensile strength TS is higher than 570 MPa, the work hardening amount WH of formula (3) is less than 15 MPa, the average crystal grain size D (μm) satisfies formula (4), and the yield elongation is 0.5% or more. (1): Si / 28+Ti / 48+Nb / 93+V / 51+Zr / 91+Mo / 96+Cr / 52>C / 12×750; (2): Si / 28+Al / 27+Ti / 48+Zr / 91+La / 139+Ce / 140>N / 14×1000; (3): WH=Y2.0-YS; (4): D<80-Si×10
Need to check novelty before this filing date? Find Prior Art

Description

Non-oriented electrical steel sheet, rotor core, motor, and method for manufacturing non-oriented electrical steel sheet

[0001] The present disclosure relates to a non-oriented electrical steel sheet, a rotor core, a motor, and a method for manufacturing the non-oriented electrical steel sheet.

[0002] Non-oriented electrical steel sheets are widely used as materials for motor cores. To obtain highly efficient motor cores, non-oriented electrical steel sheets are required to have excellent iron loss properties. Therefore, in order to manufacture non-oriented electrical steel sheets with excellent iron loss properties, steel sheets have been increasingly made with high alloys.

[0003] A motor core includes a stator core, which is a stator, and a rotor core, which is a rotor. Of the stator core and rotor core, the rotor core, in particular, is required to have both high strength and excellent magnetic properties (reduced iron loss degradation) for the following reasons: In recent years, motors for electric vehicles and hybrid vehicles have been designed to increase motor output by increasing motor rotation speed. Therefore, the load on the rotor core, which is the rotor, during motor operation has increased. Therefore, the rotor core is required to have high strength. Furthermore, since the rotor core is fixed to the rotating shaft, cooling it is difficult. Therefore, thermal management of the rotor core is also important. Iron loss in non-oriented electrical steel sheets ultimately becomes heat. Therefore, from the perspective of thermal management of the rotor core, it is necessary to reduce iron loss degradation in non-oriented electrical steel sheets.

[0004] A non-oriented electrical steel sheet having high strength and excellent magnetic properties is proposed in JP 2008-050686 A (Patent Document 1). In Patent Document 1, high strength and excellent magnetic properties are achieved by appropriately adjusting the chemical composition.

[0005] Japanese Patent Application Laid-Open No. 2008-050686

[0006] When manufacturing rotor cores from non-oriented electrical steel sheets, punching is performed on the non-oriented electrical steel sheets to produce punched products such as rotor core materials. High-alloy and high-strength non-oriented electrical steel sheets can be difficult to punch into the desired shape, resulting in reduced dimensional accuracy of the punched products. Specifically, unevenness may occur on the end surface (punched end surface) of the punched product after punching. When the punched end surface is uneven, when the punched product is assembled into a motor, it becomes difficult for the punched product to adhere to other components at the contact interface with the magnet, shaft, motor case, and other components. This creates challenges in fixing the motor core. Furthermore, it creates challenges in heat dissipation during thermal management of the motor core. Meanwhile, shear strain introduced into non-oriented electrical steel sheets causes deterioration of iron loss. This increases the heat generation of the motor core. Recently, rotor core materials have been punched into complex shapes to improve their functionality. As a result, the proportion of punched end faces in rotor core materials is increasing, and as a result, it is becoming increasingly important to reduce iron loss degradation caused by shear strain introduced into rotor core materials during punching.

[0007] An object of the present disclosure is to provide a non-oriented electrical steel sheet, a rotor core, a motor, and a method for manufacturing a non-oriented electrical steel sheet that has high strength and excellent magnetic properties and has excellent dimensional accuracy after punching.

[0008] The non-oriented electrical steel sheet of the present disclosure contains, in mass%, Si: 3.1 to 4.5%, C: 0.0025% or less, N: 0.0025% or less, O: 0.0400% or less, P: 0.100% or less, S: 0.0050% or less, Ti: 0.0100% or less, Mn: 2.0% or less, Al: 1.500% or less, Zr: 0 to 0.0100%, Nb: 0 to 0.0100%, V: 0 to 0.0100%, Mo: 0 to 0.100%, Cr: 0 to 2.000%, La: 0 to 0.0100%. %, Ce: 0 to 0.0100%, B: 0 to 0.0010%, Zn: 0 to 0.0050%, Ga: 0 to 0.0050%, Ge: 0 to 0.0050%, As: 0 to 0.0100%, Ni: 0 to 0.500%, Cu: 0 to 0.500%, Sn: 0 to 0.200%, Sb: 0 to 0.100%, Ca: 0 to 0.0050%, Nd: 0 to 0.0010%, Mg: 0 to 0.0030%, and the balance being Fe and impurities, and satisfying formula (1) and formula (2). Si / 28+Ti / 48+Nb / 93+V / 51+Zr / 91+Mo / 96+Cr / 52>C / 12×750 (1) Si / 28+Al / 27+Ti / 48+Zr / 91+La / 139+Ce / 140>N / 14×1000 (2) Here, the element symbols in formulas (1) and (2) are substituted with the corresponding element contents in mass%. When the corresponding element is not contained, "0" is substituted for the element symbol. In the non-oriented electrical steel sheet, the tensile strength TS is higher than 570 MPa. In the non-oriented electrical steel sheet, the stress at 2.0% strain is further substituted with Y 2.0 (MPa) and the yield stress is YS (MPa), the work hardening amount WH defined by the formula (3) is less than 15 MPa. 2.0 -YS (3) In the case of non-oriented electrical steel sheets, the average grain size D (μm) further satisfies formula (4), and the yield point elongation is 0.5% or more. D<80-Si×10 (4) Here, the element symbol in formula (4) is substituted with the corresponding element content in mass%. If the corresponding element is not contained, "0" is substituted for that element symbol.

[0009] The rotor core of the present disclosure includes a plurality of stacked rotor core materials, and the rotor core materials contain, in mass %, 3.1 to 4.5% Si, 0.0025% or less C, 0.0025% or less N, 0.0400% or less O, 0.100% or less P, 0.0050% or less S, 0.0100% or less Ti, 2.0% or less Mn, 1.500% or less Al, 0 to 0.0100% Zr, 0 to 0.0100% Nb, 0 to 0.0100% V, 0 to 0.100% Mo, 0 to 2.000% Cr, 0 to 0.0100% La, and 0% to 0.0100% C. e: 0 to 0.0100%, B: 0 to 0.0010%, Zn: 0 to 0.0050%, Ga: 0 to 0.0050%, Ge: 0 to 0.0050%, As: 0 to 0.0100%, Ni: 0 to 0.500%, Cu: 0 to 0.500%, Sn: 0 to 0.200%, Sb: 0 to 0.100%, Ca: 0 to 0.0050%, Nd: 0 to 0.0010%, Mg: 0 to 0.0030%, and the balance being Fe and impurities, and satisfying formula (1) and formula (2). Si / 28+Ti / 48+Nb / 93+V / 51+Zr / 91+Mo / 96+Cr / 52>C / 12×750 (1) Si / 28+Al / 27+Ti / 48+Zr / 91+La / 139+Ce / 140>N / 14×1000 (2) Here, the element symbols in formulas (1) and (2) are substituted with the corresponding element contents in mass%. When a corresponding element is not contained, "0" is substituted for that element symbol. The rotor core material further has a tensile strength TS higher than 570 MPa. The rotor core material further has a stress at 2.0% strain of Y 2.0 (MPa) and the yield stress is YS (MPa), the work hardening amount WH defined by the formula (3) is less than 15 MPa. 2.0 -YS (3) The rotor core material further has an average grain size D (μm) that satisfies formula (4), and a yield point elongation of 0.5% or more. D<80-Si×10 (4) Here, the element symbol in formula (4) is substituted with the corresponding element content in mass%. If the corresponding element is not contained, "0" is substituted for that element symbol.

[0010] The motor of the present disclosure includes the rotor core described above.

[0011] The method for manufacturing a non-oriented electrical steel sheet according to the present disclosure includes a hot rolling process, a cold rolling process, and a finish annealing process. In the hot rolling process, a slab is hot rolled to produce a hot-rolled steel sheet. In the cold rolling process, the hot-rolled steel sheet is cold rolled to produce a cold-rolled steel sheet. In the finish annealing process, the cold-rolled steel sheet is finish annealed in a finish annealing furnace. In the finish annealing process, the cold-rolled steel sheet is further annealed at a maximum temperature T1 of 950°C or less. Furthermore, the tension TE applied to the cold-rolled steel sheet at the maximum temperature T1 is set to 2.0 to 10.0 MPa. Furthermore, the residence time t0 (seconds) between the annealing temperatures T1 and 700°C in the heating zone, soaking zone, and cooling zone of the finish annealing furnace, and the residence time t1 (seconds) between the annealing temperatures T1 and 700°C in the cooling zone satisfy formulas (A) and (B). t1-t0>0 (A) t1 / t0≦3.0 (B) Furthermore, in the furnace atmosphere of the finish annealing furnace, at one or more locations selected from the heating zone, the soaking zone, and the cooling zone in the temperature range of 500°C or more, the hydrogen partial pressure P H2 (atm) relative to the water vapor partial pressure P H20 The ratio of oxygen to nitrogen (atm) is set to be higher than 0.05, or the oxygen concentration is set to be higher than 0.010%. Furthermore, the temperature gradient CG in the longitudinal direction of the cold-rolled steel sheet during the cooling process is set to be 20°C / m or less.

[0012] The non-oriented electrical steel sheet of the present disclosure has high strength and excellent magnetic properties, and has excellent dimensional accuracy after punching. The rotor core and the motor of the present disclosure are manufactured using the non-oriented electrical steel sheet of the present disclosure as a raw material. The manufacturing method of the non-oriented electrical steel sheet of the present disclosure can manufacture the above-mentioned non-oriented electrical steel sheet of the present disclosure.

[0013] FIG. 1 is a schematic diagram showing an example of a stress-strain curve. FIG. 2 is a schematic diagram showing an example of a stress-strain curve different from that of FIG. 1. FIG. 3 is a schematic diagram for explaining how to determine the yield point elongation when the upper yield point is not clear in the stress-strain curve. FIG. 4 is a plan view showing an example of a rotor core of this embodiment. FIG. 5 is a plan view showing an example of a stator core of this embodiment. FIG. 6 is a schematic diagram for explaining the definition of punching flatness in a dimensional accuracy evaluation test after punching in an example.

[0014] The present inventors have investigated and studied the causes of the reduction in dimensional accuracy and the deterioration of magnetic properties of punched products (rotor core materials, etc.) when punching non-oriented electrical steel sheets, which have high strength and excellent magnetic properties. As a result, the present inventors have come to the following findings.

[0015] During punching, when a non-oriented electrical steel sheet is forced into a die by a punch, the portion of the steel sheet near the surface of the sheet that is pushed by the punch is forced in the thickness direction. Meanwhile, the portion of the steel sheet that is in contact with the die is pulled toward the chips. Thus, the direction of stress imparted to the steel sheet during punching varies in a complex manner. Therefore, after the steel sheet breaks during punching, the degree of springback when the stress is released varies in the thickness direction of the steel sheet. As a result, unevenness occurs on the end surface (punched end surface) of the punched product, reducing the dimensional accuracy of the punched product. This reduction in dimensional accuracy is particularly noticeable when the tensile strength of the steel sheet is higher than 570 MPa.

[0016] When a steel sheet is deformed by punching, multiple dislocations are introduced into the steel sheet. If the dislocations introduced by deformation become entangled and work hardening progresses, the amount of springback when the stress is released after the steel sheet breaks during punching further increases. As a result, unevenness occurs on the end surface (punched end surface) of the punched product after punching, reducing the dimensional accuracy of the punched product.

[0017] Furthermore, in non-oriented electrical steel sheets, dislocations are introduced due to the shear strain imparted during punching. These dislocations degrade the magnetic properties. As work hardening progresses, dislocations become entangled and remain in the steel sheet. As work hardening progresses, the iron loss of the steel sheet deteriorates.

[0018] Taking the above mechanism into consideration, the inventors of the present invention thought that if the amount of work hardening could be reduced, the dimensional accuracy of the punched product after punching would be improved and iron loss deterioration could be suppressed. After further investigation, the inventors discovered that if the amount of work hardening WH defined by formula (3) is set to less than 15 MPa, excellent dimensional accuracy and excellent magnetic properties can be obtained after punching. WH = Y 2.0-YS (3)

[0019] The present inventors further investigated means for making the work hardening amount WH less than 15 MPa, and as a result, the present inventors obtained the following findings.

[0020] Silicon (Si) restricts the slip systems through which dislocations can move. Increasing the Si content in steel sheet restricts the slip systems through which dislocations can move. This suppresses dislocation entanglement due to the occurrence of cross slip. As a result, an increase in dislocation density is suppressed.

[0021] Furthermore, solute C and solute N in steel sheets tend to be anchored to dislocations. Dislocations anchored by solute C or solute N are less likely to move. Therefore, dislocations anchored by solute C or solute N tend to become entangled with moving dislocations. As a result, variations in dislocation density occur within the steel sheet. In order to reduce dislocations anchored by solute C or solute N, it is effective to reduce the solute C and solute N in the steel sheet.

[0022] In order to reduce the amount of solute C and N in a steel sheet, elements having a high affinity for C and / or N may be contained in the steel sheet, and C and N may be fixed as precipitates. Si, Ti, and Zr have a high affinity for C and N. Nb, V, Mo, and Cr have a high affinity for C. Al, La, and Ce have a high affinity for N. Therefore, if the steel sheet contains one or more elements from this group of elements, the amount of solute C and N in the steel sheet can be reduced.

[0023] Based on the above considerations, the inventors conducted a study from the viewpoint of chemical composition, and as a result, the inventors found that the composition is, in mass %, Si: 3.1 to 4.5%, C: 0.0025% or less, N: 0.0025% or less, O: 0.0400% or less, P: 0.100% or less, S: 0.0050% or less, Ti: 0.0100% or less, Mn: 2.0% or less, Al: 1.500% or less, Zr: 0 to 0.0100%, Nb: 0 to 0.0100%, V: 0 to 0.0100%, Mo: 0 to 0.100%, Cr: 0 to 2.000%, La: 0 to 0.0100%, Ce: 0 to 0.0100%, B: 0 to 0.0010%, Zn: 0 to 0.0050%, G It was believed that a non-oriented electrical steel sheet having a chemical composition consisting of a: 0 to 0.0050%, Ge: 0 to 0.0050%, As: 0 to 0.0100%, Ni: 0 to 0.500%, Cu: 0 to 0.500%, Sn: 0 to 0.200%, Sb: 0 to 0.100%, Ca: 0 to 0.0050%, Nd: 0 to 0.0010%, Mg: 0 to 0.0030%, and the balance being Fe and impurities, and further satisfying formulas (1) and (2), would achieve a tensile strength TS of more than 570 MPa, while also obtaining excellent magnetic properties and improving dimensional accuracy after punching. Si / 28+Ti / 48+Nb / 93+V / 51+Zr / 91+Mo / 96+Cr / 52>C / 12×750 (1) Si / 28+Al / 27+Ti / 48+Zr / 91+La / 139+Ce / 140>N / 14×1000 (2) Here, the element symbols in formulas (1) and (2) are substituted with the corresponding element contents in mass%. When the corresponding element is not contained, "0" is substituted for the element symbol.

[0024] However, even if a non-oriented electrical steel sheet satisfies the above-mentioned characteristics, although it has high strength and excellent magnetic properties, there are still cases where sufficient dimensional accuracy cannot be obtained after punching. Therefore, the present inventors conducted further studies and obtained the following findings.

[0025] In punching, the amount of springback increases as work hardening progresses. However, if the yield point elongation ratio, in which deformation progresses without work hardening, is increased, the non-uniformity of deformation in the thickness direction is reduced, resulting in improved dimensional accuracy. If the yield point elongation is 0.5% or more, the dimensional accuracy after punching is further improved.

[0026] On the other hand, an increase in the Si content tended to decrease the yield point elongation. The reason for this is thought to be as follows: As mentioned above, Si is thought to suppress dislocation entanglement and contribute to the suppression of work hardening. However, work hardening also occurs due to dislocation pile-up. Increasing the Si content restricts the slip system, thereby limiting the source of dislocation generation. As a result, the yield point elongation is thought to decrease.

[0027] Based on the above findings, the inventors considered that increasing the number of dislocation sources and dispersing them would be an effective way to increase yield point elongation. Further investigation revealed that reducing the grain size to increase the number of grain boundaries, which are dislocation sources, increases yield point elongation. Specifically, the inventors discovered that if the average grain size D satisfies formula (4), the yield point elongation is likely to be 0.5% or greater, improving the dimensional accuracy of the punched product after punching. D<80-Si×10 (4) Here, the Si content in mass % of the non-oriented electrical steel sheet is substituted for Si in formula (4).

[0028] The non-oriented electrical steel sheet of this embodiment has been completed based on the above technical concept, and its gist is as follows.

[0029] The non-oriented electrical steel sheet of the first configuration contains, in mass %, Si: 3.1 to 4.5%, C: 0.0025% or less, N: 0.0025% or less, O: 0.0400% or less, P: 0.100% or less, S: 0.0050% or less, Ti: 0.0100% or less, Mn: 2.0% or less, Al: 1.500% or less, Zr: 0 to 0.0100%, Nb: 0 to 0.0100%, V: 0 to 0.0100%, Mo: 0 to 0.100%, Cr: 0 to 2.000%, La: 0 to 0.010 0%, Ce: 0 to 0.0100%, B: 0 to 0.0010%, Zn: 0 to 0.0050%, Ga: 0 to 0.0050%, Ge: 0 to 0.0050%, As: 0 to 0.0100%, Ni: 0 to 0.500%, Cu: 0 to 0.500%, Sn: 0 to 0.200%, Sb: 0 to 0.100%, Ca: 0 to 0.0050%, Nd: 0 to 0.0010%, Mg: 0 to 0.0030%, and the balance being Fe and impurities, and satisfying formula (1) and formula (2). Si / 28+Ti / 48+Nb / 93+V / 51+Zr / 91+Mo / 96+Cr / 52>C / 12×750 (1) Si / 28+Al / 27+Ti / 48+Zr / 91+La / 139+Ce / 140>N / 14×1000 (2) Here, the element symbols in formulas (1) and (2) are substituted with the corresponding element contents in mass%. When the corresponding element is not contained, "0" is substituted for the element symbol. In the non-oriented electrical steel sheet, the tensile strength TS is higher than 570 MPa. In the non-oriented electrical steel sheet, the stress at 2.0% strain is further substituted with Y 2.0 (MPa) and the yield stress is YS (MPa), the work hardening amount WH defined by the formula (3) is less than 15 MPa. 2.0 -YS (3) In the non-oriented electrical steel sheet of the first configuration, the average grain size D (μm) further satisfies formula (4), and the yield point elongation is 0.5% or more. D<80-Si×10 (4) Here, the element symbol in formula (4) is substituted with the corresponding element content in mass%. If the corresponding element is not contained, "0" is substituted for that element symbol.

[0030] The non-oriented electrical steel sheet of the second configuration is the non-oriented electrical steel sheet of the first configuration, and contains, in mass%, Zr: 0.0001 to 0.0100%, Nb: 0.0001 to 0.0100%, V: 0.0001 to 0.0100%, Mo: 0.001 to 0.100%, Cr: 0.001 to 2.000%, La: 0.0001 to 0.0100%, Ce: 0.0001 to 0.0100%, B: 0.0001 to 0.0010%, Zn: 0.0001 to 0.0050%, Contains one or more elements selected from the group consisting of Ga: 0.0001 to 0.0050%, Ge: 0.0001 to 0.0050%, As: 0.0001 to 0.0100%, Ni: 0.001 to 0.500%, Cu: 0.001 to 0.500%, Sn: 0.001 to 0.200%, Sb: 0.001 to 0.100%, Ca: 0.0001 to 0.0050%, Nd: 0.0001 to 0.0010%, and Mg: 0.0001 to 0.0030%.

[0031] The rotor core of the first configuration includes a plurality of rotor core materials stacked on one another, and the rotor core materials contain, in mass %, 3.1 to 4.5% Si, 0.0025% or less C, 0.0025% or less N, 0.0400% or less O, 0.100% or less P, 0.0050% or less S, 0.0100% or less Ti, 2.0% or less Mn, 1.500% or less Al, 0 to 0.0100% Zr, 0 to 0.0100% Nb, 0 to 0.0100% V, 0 to 0.100% Mo, 0 to 2.000% Cr, 0 to 0.0100% La, and 0.0100% C. e: 0 to 0.0100%, B: 0 to 0.0010%, Zn: 0 to 0.0050%, Ga: 0 to 0.0050%, Ge: 0 to 0.0050%, As: 0 to 0.0100%, Ni: 0 to 0.500%, Cu: 0 to 0.500%, Sn: 0 to 0.200%, Sb: 0 to 0.100%, Ca: 0 to 0.0050%, Nd: 0 to 0.0010%, Mg: 0 to 0.0030%, and the balance being Fe and impurities, and satisfying formula (1) and formula (2). Si / 28+Ti / 48+Nb / 93+V / 51+Zr / 91+Mo / 96+Cr / 52>C / 12×750 (1) Si / 28+Al / 27+Ti / 48+Zr / 91+La / 139+Ce / 140>N / 14×1000 (2) Here, the element symbols in formulas (1) and (2) are substituted with the corresponding element contents in mass%. When a corresponding element is not contained, "0" is substituted for that element symbol. The rotor core material further has a tensile strength TS higher than 570 MPa. The rotor core material further has a stress at 2.0% strain of Y 2.0 (MPa) and the yield stress is YS (MPa), the work hardening amount WH defined by the formula (3) is less than 15 MPa. 2.0 -YS (3) The rotor core material further has an average grain size D (μm) that satisfies formula (4), and a yield point elongation of 0.5% or more. D<80-Si×10 (4) Here, the element symbol in formula (4) is substituted with the corresponding element content in mass%. If the corresponding element is not contained, "0" is substituted for that element symbol.

[0032] The rotor core of the second configuration is the rotor core of the first configuration, and the rotor core material contains, in mass%, Zr: 0.0001 to 0.0100%, Nb: 0.0001 to 0.0100%, V: 0.0001 to 0.0100%, Mo: 0.001 to 0.100%, Cr: 0.001 to 2.000%, La: 0.0001 to 0.0100%, Ce: 0.0001 to 0.0100%, B: 0.0001 to 0.0010%, and Zn: 0.0001 to 0.0050%. , Ga: 0.0001 to 0.0050%, Ge: 0.0001 to 0.0050%, As: 0.0001 to 0.0100%, Ni: 0.001 to 0.500%, Cu: 0.001 to 0.500%, Sn: 0.001 to 0.200%, Sb: 0.001 to 0.100%, Ca: 0.0001 to 0.0050%, Nd: 0.0001 to 0.0010%, and Mg: 0.0001 to 0.0030%.

[0033] The motor of this embodiment includes a rotor core having a first or second configuration.

[0034] The method for producing a non-oriented electrical steel sheet according to this embodiment is a method for producing a non-oriented electrical steel sheet according to the first or second configuration, and includes a hot rolling process, a cold rolling process, and a finish annealing process. In the hot rolling process, a slab is hot rolled to produce a hot-rolled steel sheet. In the cold rolling process, the hot-rolled steel sheet is cold rolled to produce a cold-rolled steel sheet. In the finish annealing process, the cold-rolled steel sheet is finish annealed in a finish annealing furnace. In the finish annealing process, the cold-rolled steel sheet is further annealed at a maximum temperature T1 of 950°C or less. Furthermore, the tension TE applied to the cold-rolled steel sheet at the maximum temperature T1 is set to 2.0 to 10.0 MPa. Furthermore, the residence time t0 (seconds) between the annealing temperatures T1 and 700°C in the heating zone, soaking zone, and cooling zone of the finish annealing furnace, and the residence time t1 (seconds) between the annealing temperatures T1 and 700°C in the cooling zone satisfy formulas (A) and (B). t1-t0>0 (A) t1 / t0≦3.0 (B) Furthermore, in one or more locations selected from the heating zone, the soaking zone, and the cooling zone in the temperature range of 500°C or higher in the furnace atmosphere of the finish annealing furnace, the hydrogen partial pressure P H2 (atm) relative to the water vapor partial pressure P H20The ratio of oxygen to nitrogen (atm) is set to be higher than 0.05, or the oxygen concentration is set to be higher than 0.010%. Furthermore, the temperature gradient CG in the longitudinal direction of the cold-rolled steel sheet during the cooling process is set to be 20°C / m or less.

[0035] The non-oriented electrical steel sheet of this embodiment will be described in detail below.

[0036] [Features of the Non-oriented Electrical Steel Sheet of the Present Embodiment] The non-oriented electrical steel sheet of the present embodiment satisfies the following features 1 to 5. (Feature 1) The chemical composition, in mass%, is: Si: 3.1 to 4.5%, C: 0.0025% or less, N: 0.0025% or less, O: 0.0400% or less, P: 0.100% or less, S: 0.0050% or less, Ti: 0.0100% or less, Mn: 2.0% or less, Al: 1.500% or less, Zr: 0 to 0.0100%, Nb: 0 to 0.0100%, V: 0 to 0.0100%, Mo: 0 to 0.100%, Cr: 0 to 2.000%, La: 0 to 0.0 100%, Ce: 0-0.0100%, B: 0-0.0010%, Zn: 0-0.0050%, Ga: 0-0.0050%, Ge: 0-0.0050%, As: 0-0.0100%, Ni: 0-0.500%, Cu: 0-0.500%, Sn: 0-0.200%, Sb: 0-0.100%, Ca: 0-0.0050%, Nd: 0-0.0010%, Mg: 0-0.0030%, and the balance being Fe and impurities. (Feature 2) The above chemical composition further satisfies formula (1) and formula (2). Si / 28+Ti / 48+Nb / 93+V / 51+Zr / 91+Mo / 96+Cr / 52>C / 12×750 (1) Si / 28+Al / 27+Ti / 48+Zr / 91+La / 139+Ce / 140>N / 14×1000 (2) Here, the element symbols in formulas (1) and (2) are substituted with the corresponding element contents in mass%. If the corresponding element is not contained, "0" is substituted for that element symbol. (Feature 3) Tensile strength TS is higher than 570 MPa. (Feature 4) The stress at 2.0% strain is expressed as Y 2.0 (MPa) and the yield stress is YS (MPa), the work hardening amount WH defined by the formula (3) is less than 15 MPa. 2.0-YS (3) (Feature 5) The average grain size D (μm) satisfies formula (4), and the yield point elongation is 0.5% or more. D<80-Si×10 (4) Here, the element symbols in formula (4) are substituted with the corresponding element contents in mass%. Features 1 to 5 are explained below.

[0037] [(Feature 1) Chemical Composition] The chemical composition of the non-oriented electrical steel sheet of this embodiment contains the following elements. Note that "%" regarding the element content in the chemical composition of the non-oriented electrical steel sheet and the rotor core material means mass % unless otherwise specified. The non-oriented electrical steel sheet is also simply referred to as "steel sheet."

[0038] Si: 3.1 to 4.5% Silicon (Si) increases the resistivity of steel sheets and reduces eddy current loss. Furthermore, Si dissolves in steel sheets to increase the strength of non-oriented electrical steel sheets. Si also restricts the slip systems through which dislocations can move. This suppresses dislocation entanglement and an increase in dislocation density. This improves dimensional accuracy after punching. If the Si content is less than 3.1%, the above effects cannot be fully achieved. On the other hand, if the Si content exceeds 4.5%, the punching workability of non-oriented electrical steel sheets decreases. Therefore, the Si content is 3.1 to 4.5%. The preferred lower limit of the Si content is 3.2%, more preferably 3.3%, and even more preferably 3.4%. The preferred upper limit of the Si content is 4.4%, more preferably 4.3%, and even more preferably 4.2%.

[0039] C: 0.0025% or less Carbon (C) is unavoidably contained. In other words, the C content is greater than 0%. C increases the strength of steel sheets. However, if the C content exceeds 0.0025%, the amount of solute C in the steel sheet becomes excessive. In this case, solute C adheres to dislocations during punching, restricting their movement. If there are many dislocations to which solute C adheres, the density of intertwined dislocations also increases. As a result, unevenness is likely to occur in punched products after punching, reducing the dimensional accuracy after punching. If the C content exceeds 0.0025%, excessive amounts of carbides and / or carbonitrides are formed. As a result, iron loss deteriorates. Therefore, the C content is 0.0025% or less. The lower limit of the C content is preferably 0.0001%, more preferably 0.0005%, even more preferably 0.0010%, even more preferably 0.0012%, even more preferably 0.0014%, and even more preferably 0.0016%. The upper limit of the C content is preferably 0.0024%, more preferably 0.0023%, even more preferably 0.0022%, and even more preferably 0.0021%.

[0040] N: 0.0025% or Less Nitrogen (N) is inevitably contained. In other words, the N content is greater than 0%. N increases the strength of steel sheets. Even if even a small amount of N is contained, the above effect can be achieved to some extent. However, if the N content exceeds 0.0025%, the amount of solute N in the steel sheet becomes excessive. In this case, the solute N adheres to dislocations during punching, restricting their movement. If there are many dislocations to which solute N adheres, the density of intertwined dislocations also increases. As a result, unevenness is likely to occur in punched products after punching, and the dimensional accuracy after punching decreases. If the N content exceeds 0.0025%, excessive amounts of nitrides and / or carbonitrides are formed. As a result, iron loss deteriorates. Therefore, the N content is 0.0025% or less. The lower limit of the N content is preferably 0.0001%, more preferably 0.0005%, even more preferably 0.0010%, even more preferably 0.0012%, even more preferably 0.0014%, and even more preferably 0.0016%. The upper limit of the N content is preferably 0.0024%, more preferably 0.0023%, even more preferably 0.0022%, and even more preferably 0.0021%.

[0041] O: 0.0400% or less Oxygen (O) is inevitably contained. In other words, the O content is greater than 0%. O forms oxides and reduces the magnetic properties of the steel sheet. Therefore, the O content is 0.0400% or less. The O content is preferably as low as possible. However, excessive reduction of the O content increases manufacturing costs. Therefore, from the viewpoint of industrial productivity, the preferred lower limit of the O content is 0.0001%, more preferably 0.0010%, and even more preferably 0.0020%. The preferred upper limit of the O content is 0.0370%, more preferably 0.0350%, even more preferably 0.0300%, and even more preferably 0.0200%.

[0042] P: 0.100% or less Phosphorus (P) is unavoidably contained. In other words, the P content is greater than 0%. P increases the strength of the steel sheet. Even if even a small amount of P is contained, the above effect can be obtained to some extent. However, if the P content exceeds 0.100%, the steel sheet becomes embrittled, workability decreases, and cracks may occur in the steel sheet during cold rolling. Therefore, the P content is 0.100% or less. The preferred lower limit of the P content is 0.001%, more preferably 0.005%, and even more preferably 0.007%. The preferred upper limit of the P content is 0.090%, more preferably 0.080%, and even more preferably 0.070%.

[0043] S: 0.0050% or less Sulfur (S) is an unavoidable impurity. In other words, the S content is greater than 0%. S generates MnS, which deteriorates iron loss. Therefore, the S content is 0.0050% or less. The lower the S content, the better. However, excessive reduction in the S content increases production costs. Therefore, from the viewpoint of industrial productivity, the preferred lower limit of the S content is 0.0001%, more preferably 0.0003%, and even more preferably 0.0005%. The preferred upper limit of the S content is 0.0047%, more preferably 0.0045%, even more preferably 0.0040%, even more preferably 0.0030%, even more preferably 0.0025%, and even more preferably 0.0020%.

[0044] [Elements Reducing Solute Carbon and / or Solute Nitrogen] The chemical composition of the non-oriented electrical steel sheet according to this embodiment further includes 0.0100% or less Ti, 2.0% or less Mn, 1.500% or less Al, 0 to 0.0100% Zr, 0 to 0.0100% Nb, 0 to 0.0100% V, 0 to 0.100% Mo, 0 to 2.000% Cr, 0 to 0.0100% La, and 0 to 0.0100% Ce. These elements fix the solute carbon and / or solute nitrogen in the steel sheet to form precipitates such as carbides, carbonitrides, or nitrides. As a result, these elements reduce the solute carbon and solute nitrogen, which can cause a decrease in dimensional accuracy after punching.

[0045] Ti: 0.0100% or less Titanium (Ti) is unavoidably contained. In other words, the Ti content is greater than 0%. Ti combines with C and / or N to form precipitates, reducing solute C and solute N. This improves dimensional accuracy after punching. Ti also increases the strength of the steel sheet by forming precipitates. Even if even a small amount of Ti is contained, the above effects can be achieved to some extent. However, if the Ti content exceeds 0.0100%, excessive precipitates are formed, deteriorating the magnetic properties. Therefore, the Ti content is 0.0100% or less. The preferred lower limit of the Ti content is 0.0001%, more preferably 0.0005%, and even more preferably 0.0010%. The upper limit of the Ti content is preferably 0.0090%, more preferably 0.0080%, even more preferably 0.0070%, still more preferably 0.0060%, and still more preferably 0.0055%.

[0046] Mn: 2.0% or less Manganese (Mn) is unavoidably contained. That is, the Mn content is greater than 0%. Mn combines with C to form carbides, reducing solute C. Mn also increases the resistivity of the steel sheet and reduces eddy current loss. Even if even a small amount of Mn is contained, the above effects can be obtained to some extent. However, if the Mn content exceeds 2.0%, the magnetic flux density of the steel sheet decreases. Therefore, the Mn content is 2.0% or less. The preferred lower limit of the Mn content is 0.1%, more preferably 0.2%, and even more preferably 0.5%. The preferred upper limit of the Mn content is 1.8%, more preferably 1.6%, and even more preferably 1.4%.

[0047] Al: 1.500% or less Aluminum (Al) is unavoidably contained. In other words, the Al content is greater than 0%. Al combines with N to form nitrides, reducing the amount of solute N. This improves dimensional accuracy after punching. Al also increases the strength of the steel sheet by forming nitrides. Even if even a small amount of Al is contained, the above effects can be achieved to some extent. However, if the Al content exceeds 1.500%, excessive oxides are formed in the steel sheet, deteriorating the magnetic properties. Therefore, the Al content is 1.500% or less. The preferred lower limit of the Al content is 0.001%, more preferably 0.004%, even more preferably 0.005%, even more preferably 0.010%, even more preferably 0.050%, and even more preferably 0.100%. The upper limit of the Al content is preferably 1.450%, more preferably 1.400%, even more preferably 1.300%, even more preferably 1.100%, and even more preferably 0.900%. In this specification, the Al content means the content of sol. Al (acid-soluble Al).

[0048] Zr: 0 to 0.0100% Zirconium (Zr) does not necessarily need to be contained. That is, the Zr content may be 0%. When contained, that is, when the Zr content exceeds 0%, Zr combines with C and / or N to form precipitates, reducing solute C and solute N. As a result, Zr improves the dimensional accuracy after punching. Zr also increases the strength of the steel sheet by forming precipitates. Even if even a small amount of Zr is contained, the above effects can be achieved to some extent. However, if the Zr content exceeds 0.0100%, excessive precipitates will form. In this case, magnetic properties will deteriorate. Therefore, the Zr content is 0 to 0.0100%. The preferred lower limit of the Zr content is 0.0001%, more preferably 0.0005%, and even more preferably 0.0010%. The upper limit of the Zr content is preferably 0.0095%, more preferably 0.0090%, even more preferably 0.0080%, and still more preferably 0.0070%.

[0049] Nb: 0 to 0.0100% Niobium (Nb) does not necessarily need to be contained. In other words, the Nb content may be 0%. When contained, Nb combines with C to form carbides, reducing the amount of solute C. As a result, Nb improves the dimensional accuracy after punching. Nb also increases the strength of the steel sheet by forming carbides. Even if even a small amount of Nb is contained, the above effects can be achieved to some extent. However, if the Nb content exceeds 0.0100%, excessive carbides are formed. In this case, magnetic properties deteriorate. Therefore, the Nb content is 0 to 0.0100%. The preferred lower limit of the Nb content is 0.0001%, more preferably 0.0005%, and even more preferably 0.0010%. The upper limit of the Nb content is preferably 0.0090%, more preferably 0.0080%, even more preferably 0.0070%, even more preferably 0.0050%, even more preferably 0.0040%, even more preferably 0.0030%, and even more preferably 0.0025%.

[0050] V: 0 to 0.0100% Vanadium (V) does not necessarily need to be contained. In other words, the V content may be 0%. When vanadium (V) is contained, that is, when the V content exceeds 0%, V combines with C to form carbides, reducing the amount of solute C. As a result, V improves the dimensional accuracy after punching. V also increases the strength of the steel sheet by forming carbides. Even if even a small amount of V is contained, the above effects can be achieved to some extent. However, if the V content exceeds 0.0100%, excessive carbides are formed. In this case, magnetic properties deteriorate. Therefore, the V content is 0 to 0.0100%. The preferred lower limit of the V content is 0.0001%, more preferably 0.0005%, and even more preferably 0.0010%. The upper limit of the V content is preferably 0.0090%, more preferably 0.0080%, even more preferably 0.0070%, even more preferably 0.0050%, even more preferably 0.0040%, even more preferably 0.0030%, and even more preferably 0.0025%.

[0051] Mo: 0 to 0.100% Molybdenum (Mo) does not necessarily have to be contained. That is, the Mo content may be 0%. When contained, that is, when the Mo content exceeds 0%, Mo combines with C to form carbides, reducing the amount of solute C. As a result, Mo improves the dimensional accuracy after punching. Mo also increases the strength of the steel sheet by forming carbides. Even if even a small amount of Mo is contained, the above effects can be achieved to some extent. However, if the Mo content exceeds 0.100%, excessive carbides are formed. In this case, magnetic properties deteriorate. Therefore, the Mo content is 0 to 0.100%. The preferred lower limit of the Mo content is 0.001%, more preferably 0.005%, even more preferably 0.010%, and even more preferably 0.030%. The preferred upper limit of the Mo content is 0.090%, even more preferably 0.080%, and even more preferably 0.070%.

[0052] Cr: 0 to 2.000% Chromium (Cr) does not necessarily have to be contained. That is, the Cr content may be 0%. When chromium is contained, that is, when the Cr content exceeds 0%, Cr combines with C to form carbides, reducing the amount of solute C. As a result, Cr improves the dimensional accuracy after punching. Cr also increases the strength of the steel sheet. Even if even a small amount of Cr is contained, the above effects can be achieved to some extent. However, if the Cr content exceeds 2.000%, excessive carbides are formed. In this case, magnetic properties deteriorate. Therefore, the Cr content is 0 to 2.000%. The preferred lower limit of the Cr content is 0.001%, more preferably 0.005%, even more preferably 0.010%, and even more preferably 0.050%. The upper limit of the Cr content is preferably 1.800%, more preferably 1.500%, even more preferably 1.400%, and still more preferably 1.000%.

[0053] La: 0 to 0.0100% Lanthanum (La) is an optional element and does not necessarily need to be contained. In other words, the La content may be 0%. When contained, that is, when the La content exceeds 0%, La bonds with N to form nitrides, reducing the amount of solute N. As a result, La improves the dimensional accuracy after punching. La also increases the strength of the steel sheet by forming nitrides. Even if even a small amount of La is contained, the above effects can be achieved to some extent. However, if the La content exceeds 0.0100%, excessive nitrides are formed in the steel sheet. In this case, the magnetic properties deteriorate. Therefore, the La content is 0 to 0.0100%. The preferred lower limit of the La content is 0.0001%, more preferably 0.0005%, even more preferably 0.0010%, and even more preferably 0.0020%. The upper limit of the La content is preferably 0.0090%, more preferably 0.0080%, even more preferably 0.0075%, and still more preferably 0.0070%.

[0054] Ce: 0 to 0.0100% Cerium (Ce) is an optional element and does not necessarily need to be included. In other words, the Ce content may be 0%. When included, that is, when the Ce content exceeds 0%, Ce combines with N to form nitrides, reducing the amount of solute N. As a result, Ce improves the dimensional accuracy after punching. Ce also increases the strength of the steel sheet by forming nitrides. Even if even a small amount of Ce is included, the above effects can be achieved to some extent. However, if the Ce content exceeds 0.0100%, excessive nitrides are formed in the steel sheet, deteriorating the magnetic properties. Therefore, the Ce content is 0 to 0.0100%. The preferred lower limit of the Ce content is 0.0001%, more preferably 0.0005%, even more preferably 0.0010%, and even more preferably 0.0015%. The upper limit of the Ce content is preferably 0.0090%, more preferably 0.0080%, and still more preferably 0.0070%.

[0055] The balance of the chemical composition of the non-oriented electrical steel sheet of this embodiment is composed of Fe and impurities. Here, the impurities are those that are mixed in from raw materials such as ore and scrap, or from the manufacturing environment, during industrial production of the non-oriented electrical steel sheet. The content of these impurities is permissible within a range that does not adversely affect the non-oriented electrical steel sheet of this embodiment.

[0056] The non-oriented electrical steel sheet of this embodiment may further contain B: 0 to 0.0010%, Zn: 0 to 0.0050%, Ga: 0 to 0.0050%, Ge: 0 to 0.0050%, As: 0 to 0.0100%, Ni: 0 to 0.500%, Cu: 0 to 0.500%, Sn: 0 to 0.200%, Sb: 0 to 0.100%, Ca: 0 to 0.0050%, Nd: 0 to 0.0010%, and Mg: 0 to 0.0030%. All of these elements are optional and may not be contained. Each element will be described below.

[0057] [B, Zn, Ga, Ge, and As] B, Zn, Ga, Ge, and As are impurities in the non-oriented electrical steel sheet of this embodiment.

[0058] B: 0 to 0.0010% Boron (B) is an optional element and does not necessarily need to be contained. In other words, the B content may be 0%. When contained, that is, when the B content exceeds 0%, B forms nitrides. B nitrides inhibit recrystallization during finish annealing. Therefore, the B content is 0 to 0.0010%. An excessive reduction in the B content increases production costs. Therefore, from the viewpoint of industrial productivity, the preferred lower limit of the B content is 0.0001%, more preferably 0.0002%, and even more preferably 0.0003%. The preferred upper limit of the B content is 0.0009%, more preferably 0.0008%, and even more preferably 0.0007%.

[0059] Zn: 0 to 0.0050% Zinc (Zn) is an optional element and does not necessarily need to be contained. In other words, the Zn content may be 0%. If zinc is contained, that is, if the Zn content exceeds 0%, no particular problems will arise as long as the Zn content is 0.0050% or less. Therefore, the Zn content is 0 to 0.0050%. Excessive reduction of the Zn content increases production costs. Therefore, from the viewpoint of industrial productivity, the preferred lower limit of the Zn content is 0.0001%, more preferably 0.0002%, and even more preferably 0.0003%. The preferred upper limit of the Zn content is 0.0020%, more preferably 0.0010%, and even more preferably 0.0005%.

[0060] Ga: 0 to 0.0050% Gallium (Ga) is an optional element and does not necessarily need to be contained. In other words, the Ga content may be 0%. If gallium (Ga) is contained, that is, if the Ga content exceeds 0%, no particular problems arise as long as the Ga content is 0.0050% or less. Therefore, the Ga content is 0 to 0.0050%. Excessive reduction of the Ga content increases production costs. Therefore, from the viewpoint of industrial productivity, the preferred lower limit of the Ga content is 0.0001%, more preferably 0.0002%, and even more preferably 0.0003%. The preferred upper limit of the Ga content is 0.0040%, more preferably 0.0035%, even more preferably 0.0030%, even more preferably 0.0020%, even more preferably 0.0010%, and even more preferably 0.0005%.

[0061] Ge: 0 to 0.0050% Germanium (Ge) is an optional element and does not necessarily need to be contained. In other words, the Ge content may be 0%. If germanium (Ge) is contained, that is, if the Ge content exceeds 0%, no particular problems arise as long as the Ge content is 0.0050% or less. Therefore, the Ge content is 0 to 0.0050%. Excessive reduction of the Ge content increases production costs. Therefore, from the viewpoint of industrial productivity, the preferred lower limit of the Ge content is 0.0001%, more preferably 0.0002%, and even more preferably 0.0003%. The preferred upper limit of the Ge content is 0.0040%, more preferably 0.0035%, even more preferably 0.0030%, even more preferably 0.0020%, even more preferably 0.0010%, and even more preferably 0.0005%.

[0062] As: 0 to 0.0100% Arsenic (As) is an optional element and does not necessarily need to be contained. In other words, the As content may be 0%. If arsenic (As) is contained, that is, if the As content exceeds 0%, no particular problems arise as long as the As content is 0.0100% or less. Therefore, the As content is 0 to 0.0100%. Excessive reduction of the As content increases production costs. Therefore, from the viewpoint of industrial productivity, the preferred lower limit of the As content is 0.0001%, more preferably 0.0002%, even more preferably 0.0003%, even more preferably 0.0005%, and even more preferably 0.0010%. The preferred upper limit of the As content is 0.0070%, even more preferably 0.0060%, even more preferably 0.0050%, and even more preferably 0.0030%.

[0063] [Ni and Cu] Ni and Cu are optional elements that increase the strength of the non-oriented electrical steel sheet.

[0064] Ni: 0 to 0.500% Nickel (Ni) is an optional element and does not necessarily need to be contained. In other words, the Ni content may be 0%. When contained, that is, when the Ni content is greater than 0%, Ni increases the strength of the non-oriented electrical steel sheet. Even if even a small amount of Ni is contained, the above effect can be obtained to some extent. However, if the Ni content exceeds 0.500%, the steel sheet becomes embrittled and its workability decreases. Therefore, the Ni content is 0 to 0.500%. The preferred lower limit of the Ni content is 0.001%, more preferably 0.005%, even more preferably 0.010%, even more preferably 0.020%, even more preferably 0.050%, and even more preferably 0.100%. The preferred upper limit of the Ni content is 0.450%, even more preferably 0.400%, even more preferably 0.350%, even more preferably 0.300%, and even more preferably 0.250%.

[0065] Cu: 0 to 0.500% Copper (Cu) is an optional element and does not necessarily need to be contained. That is, the Cu content may be 0%. When contained, that is, when the Cu content is greater than 0%, Cu increases the strength of the non-oriented electrical steel sheet. Even if even a small amount of Cu is contained, the above effect can be obtained to some extent. However, if the Cu content exceeds 0.500%, the steel sheet becomes embrittled and its workability decreases. Therefore, the Cu content is 0 to 0.500%. The preferred lower limit of the Cu content is 0.001%, more preferably 0.005%, even more preferably 0.010%, even more preferably 0.030%, even more preferably 0.050%, and even more preferably 0.100%. The preferred upper limit of the Cu content is 0.450%, even more preferably 0.400%, even more preferably 0.350%, even more preferably 0.250%, and even more preferably 0.150%.

[0066] [Sn and Sb] Sn and Sb are optional elements. Both Sn and Sb reduce the iron loss of the non-oriented electrical steel sheet.

[0067] Sn: 0 to 0.200% Tin (Sn) is an optional element and does not necessarily need to be contained. That is, the Sn content may be 0%. When contained, that is, when the Sn content exceeds 0%, Sn segregates on the surface of the steel sheet and suppresses oxidation and nitridation during finish annealing. Sn also improves the texture of the steel sheet and increases the magnetic flux density, thereby reducing the iron loss of the non-oriented electrical steel sheet. Even if even a small amount of Sn is contained, the above effects can be achieved to some extent. However, if the Sn content exceeds 0.200%, the steel sheet becomes embrittled and its workability decreases. Therefore, the Sn content is 0 to 0.200%. The preferred lower limit of the Sn content is 0.001%, more preferably 0.003%, even more preferably 0.005%, even more preferably 0.010%, even more preferably 0.030%, and even more preferably 0.050%. The upper limit of the Sn content is preferably 0.180%, more preferably 0.160%, even more preferably 0.150%, and still more preferably 0.120%.

[0068] Sb: 0 to 0.100% Antimony (Sb) is an optional element and does not necessarily need to be contained. That is, the Sb content may be 0%. When contained, that is, when the Sb content exceeds 0%, Sb, like Sn, segregates on the surface of the steel sheet and suppresses oxidation and nitridation during finish annealing. Sb also improves the texture of the steel sheet and increases the magnetic flux density. This reduces the iron loss of the non-oriented electrical steel sheet. Even if even a small amount of Sb is contained, the above effects can be obtained to some extent. However, if the Sb content exceeds 0.100%, the steel sheet becomes embrittled and its workability decreases. Therefore, the Sb content is 0 to 0.100%. The preferred lower limit of the Sb content is 0.001%, more preferably 0.005%, even more preferably 0.010%, and even more preferably 0.030%. The upper limit of the Sb content is preferably 0.080%, more preferably 0.070%, even more preferably 0.060%, and still more preferably 0.050%.

[0069] [Ca, Nd, and Mg] Ca, Nd, and Mg are optional elements that promote the growth of crystal grains during finish annealing and improve the magnetic properties of the non-oriented electrical steel sheet.

[0070] Ca: 0 to 0.0050% Calcium (Ca) is an optional element and does not necessarily need to be contained. In other words, the Ca content may be 0%. When contained, that is, when the Ca content exceeds 0%, Ca combines with S during the casting of molten steel to form coarse precipitates, such as coarse sulfides and / or coarse oxysulfides. The particle size of the coarse precipitates is approximately 1 to 2 μm. The coarse precipitates adsorb fine inhibitors, such as MnS, TiN, and AlN, with particle sizes of approximately 100 nm, that are formed in the steel sheet during manufacturing processes after the casting process. This suppresses the inhibition of grain growth by the inhibitors during final annealing. Therefore, grain growth is promoted during final annealing. As a result, the magnetic properties of the non-oriented electrical steel sheet are improved. Even if even a small amount of Ca is contained, the above effects can be obtained to some extent. However, if the Ca content exceeds 0.0050%, excessive coarse precipitates are formed. In this case, recrystallization and grain growth during the finish annealing step are inhibited. Therefore, the Ca content is 0 to 0.0050%. The preferred lower limit of the Ca content is 0.0001%, more preferably 0.0005%, and even more preferably 0.0010%. The preferred upper limit of the Ca content is 0.0045%, more preferably 0.0040%, and even more preferably 0.0035%.

[0071] Nd: 0 to 0.0010% Neodymium (Nd) is an optional element and does not necessarily need to be contained. In other words, the Nd content may be 0%. When Nd is contained, that is, when the Nd content exceeds 0%, Nd, like Ca, forms coarse precipitates and suppresses the inhibition of grain growth by inhibitors during final annealing. Therefore, grain growth is promoted during final annealing. As a result, the magnetic properties of the non-oriented electrical steel sheet are improved. Even if even a small amount of Nd is contained, the above effect can be achieved to some extent. However, if the Nd content exceeds 0.0010%, excessive coarse precipitates are formed. In this case, recrystallization and grain growth during the final annealing process are inhibited. Therefore, the Nd content is 0 to 0.0010%. The preferred lower limit of the Nd content is 0.0001%, more preferably 0.0002%, and even more preferably 0.0003%. The upper limit of the Nd content is preferably 0.0008%, more preferably 0.0006%, and even more preferably 0.0004%.

[0072] Mg: 0 to 0.0030% Magnesium (Mg) is an optional element and does not necessarily need to be contained. That is, the Mg content may be 0%. When contained, that is, when the Mg content exceeds 0%, Mg, like Ca, forms coarse precipitates and suppresses the inhibition of grain growth by inhibitors during final annealing. Therefore, grain growth is promoted during final annealing. As a result, the magnetic properties of the non-oriented electrical steel sheet are improved. Even if even a small amount of Mg is contained, the above effect can be achieved to some extent. However, if the Mg content exceeds 0.0030%, excessive coarse precipitates are formed. In this case, recrystallization and grain growth during the final annealing process are inhibited. Therefore, the Mg content is 0 to 0.0030%. The preferred lower limit of the Mg content is 0.0001%, more preferably 0.0002%, and even more preferably 0.0003%. The upper limit of the Mg content is preferably 0.0025%, more preferably 0.0020%, even more preferably 0.0015%, and still more preferably 0.0010%.

[0073] [Method for Measuring Chemical Composition of Non-Oriented Electrical Steel Sheet] The chemical composition of the non-oriented electrical steel sheet of this embodiment can be measured by a well-known elemental analysis method in accordance with JIS G0321:2017. Specifically, chips are collected from the steel sheet using a drill. The collected chips are dissolved in acid to obtain a solution. The solution is subjected to ICP-AES (Inductively Coupled Plasma Atomic Emission Spectrometry) to perform elemental analysis of the chemical composition. The C content and S content are determined by a well-known high-frequency combustion method (combustion-infrared absorption method). The N content is determined by a well-known inert gas fusion-thermal conductivity method. The O content is determined by a well-known inert gas fusion-infrared absorption method.

[0074] The content of each element is determined by rounding off the measured value to the nearest significant digit based on the significant digits specified in this embodiment. For example, the Si content of the steel sheet in this embodiment is determined to one decimal place. Therefore, the Si content is determined to one decimal place by rounding off the measured value to one decimal place.

[0075] Similarly, the contents of elements other than the Si content of the steel sheet of this embodiment are also determined by rounding off the measured value to the smallest digit specified in this embodiment, and the value obtained is the content of the element.

[0076] Rounding off means rounding down if the fraction is less than 5, and rounding up if the fraction is 5 or more.

[0077] [(Feature 2) Regarding Formulas (1) and (2)] The non-oriented electrical steel sheet of this embodiment further satisfies formulas (1) and (2): Si / 28 + Ti / 48 + Nb / 93 + V / 51 + Zr / 91 + Mo / 96 + Cr / 52 > C / 12 × 750 (1) Si / 28 + Al / 27 + Ti / 48 + Zr / 91 + La / 139 + Ce / 140 > N / 14 × 1000 (2) Here, the element symbols in formulas (1) and (2) are substituted with the corresponding element contents in mass%. When a corresponding element is not contained, "0" is substituted for the element symbol.

[0078] [Regarding Formula (1)] Formula (1) is a formula for sufficiently reducing solute C in a steel sheet by forming carbides or carbonitrides. The left side of formula (1) is composed of elements that bond with C to form carbides or carbonitrides. When formula (1) is satisfied, carbides or carbonitrides are sufficiently formed, thereby sufficiently reducing solute C.

[0079] [Regarding formula (2)] Formula (2) is a formula for sufficiently reducing solute N by forming nitrides or carbonitrides. The left side of formula (2) is composed of elements that bond with N to form nitrides or carbonitrides. When formula (2) is satisfied, nitrides or carbonitrides are sufficiently formed, thereby sufficiently reducing solute N.

[0080] [(Feature 3) Tensile strength TS] The non-oriented electrical steel sheet of this embodiment has a tensile strength TS of more than 570 MPa. That is, the non-oriented electrical steel sheet of this embodiment has high strength. The preferred lower limit of the tensile strength TS of the non-oriented electrical steel sheet of this embodiment is 575 MPa, and more preferably 580 MPa. The upper limit of the tensile strength TS is not particularly limited. However, when Features 1 and 2 are satisfied, the upper limit of the tensile strength TS is, for example, 750 MPa.

[0081] [Method for measuring stress-strain curve] The tensile strength TS of the non-oriented electrical steel sheet of this embodiment is measured by the following method. A JIS No. 5 tensile test piece specified in JIS Z2241:2011 is taken from the non-oriented electrical steel sheet. Using the taken tensile test piece, a tensile test is carried out in air at room temperature in accordance with JIS Z2241:2011 to obtain a stress-strain curve. The tensile strength TS (MPa) is determined from the obtained stress-strain curve.

[0082] [(Feature 4) Work Hardening Amount WH] In the non-oriented electrical steel sheet of this embodiment, the stress at 2.0% strain is further set to Y 2.0 (MPa) and the yield stress is YS (MPa), the work hardening amount WH defined by the formula (3) is less than 15 MPa. 2.0 -YS (3)

[0083] If dislocations grow excessively during punching, there is a high possibility that dislocations to which solute C or solute N is fixed will increase. If the number of dislocations to which solute C or solute N is fixed increases, regions with a high density of dislocations entangled with each other will be formed locally. In this case, unevenness is likely to occur in the punched product after punching, and sufficient dimensional accuracy cannot be obtained.

[0084] The amount of work hardening WH correlates with the dislocation density. If the amount of work hardening WH is less than 15 MPa, the dislocation density is sufficiently suppressed during punching. Therefore, the occurrence of dislocations where solute C or solute N is fixed can be sufficiently suppressed. Therefore, the occurrence of irregularities caused by punching in the punched product after punching is suppressed, and sufficient dimensional accuracy can be obtained.

[0085] The upper limit of the work-hardening amount WH is preferably 14 MPa, more preferably 13 MPa, even more preferably 12 MPa, even more preferably 11 MPa, and even more preferably 10 MPa. The work-hardening amount WH is preferably as low as possible. In consideration of industrial productivity, the lower limit of the work-hardening amount WH is preferably 2 MPa, more preferably 1 MPa, and most preferably 0 MPa.

[0086] [Work-hardening amount WH evaluation test] The work-hardening amount WH can be determined by the following method. A stress-strain curve is obtained by conducting the tensile test described in the above-mentioned [Method for measuring a stress-strain curve]. FIG. 1 is a schematic diagram of an example of a stress-strain curve. Referring to FIG. 1, the maximum stress value within the strain range of 0 to 0.2% plastic strain is defined as the "yield strength YS" (MPa). In FIG. 1, an upper yield point P0 occurs on the stress-strain curve within the strain range L0 of 0 to 0.2% plastic strain. Therefore, when a stress-strain curve has an upper yield point as shown in FIG. 1, the stress at the upper yield point P0 is defined as the yield strength YS (MPa).

[0087] On the other hand, in the case of a stress-strain curve in which the upper yield point P0 does not occur, as in the stress-strain curve shown in Figure 2, when the strain is in the range L0 from 0 to 0.2% plastic strain, the stress at the position of 0.2% plastic strain becomes the maximum value. Therefore, in this case, the 0.2% proof stress is taken as the yield strength YS (MPa).

[0088] 1 and 2, in the stress-strain curve, the stress at 2.0% strain is expressed as Y 2.0 (MPa).

[0089] The obtained yield strength YS (MPa) and stress Y 2.0 (MPa) is used to calculate the amount of work hardening WH (MPa) using equation (3). 2.0 In this case, WH is defined as 0 (MPa).

[0090] [(Feature 5) Average Grain Size D] In the non-oriented electrical steel sheet of this embodiment, the average grain size D (μm) further satisfies formula (4), and the yield point elongation is 0.5% or more: D<80−Si×10 (4) Here, Si in formula (4) is substituted with the Si content in mass% in the chemical composition of the non-oriented electrical steel sheet.

[0091] Fn is defined as follows: Fn = 80 - Si x 10. If the average grain size D (μm) is less than Fn, the number of dislocation sources during deformation can be increased, dispersing the dislocation sources. In this case, dislocations do not occur locally during deformation of the steel sheet during punching, but occur dispersedly. This suppresses dislocation entanglement. As a result, the yield elongation is likely to be 0.5% or more, and non-uniformity of deformation in the sheet thickness direction during punching can be reduced. As a result, dimensional accuracy after punching can be improved.

[0092] The lower limit of the average crystal grain size D is preferably 10 μm, more preferably 15 μm, and even more preferably 20 μm. The upper limit of the average crystal grain size D is preferably 75−Si×10 (μm), more preferably 70−Si×10 (μm), and even more preferably 65−Si×10 (μm).

[0093] The lower limit of the yield point elongation is preferably 0.6%, more preferably 0.7%, even more preferably 1.0%, and still more preferably 1.5%. The upper limit of the yield point elongation is not particularly limited, but is preferably about 7.0%.

[0094] [Method for measuring average grain size D] The average grain size D is determined by the following method. A cross section (L cross section) parallel to the rolling direction of the non-oriented electrical steel sheet is used as the observation surface. The observation surface is mirror-polished, and then the mirror-polished observation surface is etched using a nital solution. The etched observation surface is observed using an optical microscope at a magnification of 100 times, and a photographic image of the observation field is generated. Using the photographic image, the average grain size D (μm) is determined by the method of calculating the number of grains within a rectangular region described below in accordance with JIS G0551:2013 "Steel - Microscopic test method for grain size."

[0095] Specifically, in the L cross section, a rectangular area is drawn, surrounded by lines parallel to the thickness direction and the surface direction (rolling direction), in a region consisting only of recrystallized grains, excluding unrecrystallized regions. This rectangular area is the observation field. The area A of the rectangular area is 0.5 mm 2 The area of ​​one rectangle is 0.5 mm 2 If this is not possible, draw multiple rectangular areas and make the total area A of the rectangular areas 0.5 mm 2 Make sure it is above that.

[0096] The number of crystal grains in the rectangular region is counted. Specifically, the number of crystal grains that exist inside the rectangular region and do not contact any of the sides of the rectangular region is defined as N1. The number of crystal grains that intersect with any of the four sides of the rectangular region excluding the four corners (four vertices of the rectangle) is defined as N2. 2 The number of all rectangular areas drawn to secure the above area is N3. The total area A (mm 2 ), and the numbers of crystal grains N1 to N3 are used to calculate the average crystal grain size D (μm) according to formula (I).

[0097] [Method for measuring yield elongation] The yield elongation is determined by the following method. A tensile test piece is taken from a non-oriented electrical steel sheet. A tensile test is carried out in air at room temperature in accordance with JIS Z2241:2011 to determine the yield elongation (%). A JIS No. 5 tensile test piece is used as the tensile test piece.

[0098] If the upper yield point is not clearly visible, the yield elongation (%) is determined using the following method. Referring to Figure 3, the yield strength YS (MPa) is determined in the stress-strain curve obtained by the tensile test based on the method described in the above-mentioned [Work hardening amount WH evaluation test]. The strain value at the determined yield strength YS is designated as ε1. In the stress-strain curve after the strain value ε1, the maximum strain value ε2 is identified in the region where the stress is maintained within the range of the yield stress YS ±1.0% as the strain increases. Using ε1 and ε2, the yield elongation is determined using the following formula: Yield elongation (%) = ε2 - ε1

[0099] [Effects of the Non-oriented Electrical Steel Sheet of the Present Embodiment] The non-oriented electrical steel sheet of the present embodiment satisfies Features 1 to 5. Therefore, the non-oriented electrical steel sheet of the present embodiment has high strength and sufficient magnetic properties, and yet also provides excellent dimensional accuracy after punching.

[0100] [Method for manufacturing non-oriented electrical steel sheet] An example of a method for manufacturing a non-oriented electrical steel sheet according to this embodiment will be described. The method for manufacturing a non-oriented electrical steel sheet according to this embodiment includes the following steps: (Step 1) Hot rolling step (Step 2) Hot-rolled sheet annealing step (Step 3) Cold rolling step (Step 4) Finish annealing step Of the above steps 1 to 4, step 2 is an optional step. In other words, step 2 does not have to be performed. Each step will be described below.

[0101] [(Step 1) Hot Rolling Step] In the hot rolling step, a slab is hot rolled to produce a hot-rolled steel sheet. The slab is produced by a known method, for example, by continuous casting.

[0102] The prepared slab is subjected to hot rolling. The various conditions for hot rolling are not particularly limited. The slab heating temperature is, for example, 1100 to 1200°C. The finish rolling temperature is, for example, 800 to 1100°C. The coiling temperature is, for example, 700 to 800°C. A hot-rolled steel sheet is manufactured through the above steps.

[0103] [(Step 2) Hot-rolled sheet annealing step] The hot-rolled sheet annealing step is an optional step. That is, the hot-rolled sheet annealing step may or may not be performed. If performed, annealing is performed on the hot-rolled steel sheet in the hot-rolled sheet annealing step. The hot-rolled sheet annealing may be box annealing or continuous annealing. The annealing conditions in the hot-rolled sheet annealing step are not particularly limited. In the case of box annealing, the annealing temperature is, for example, 750°C to 850°C, and the holding time at the annealing temperature is, for example, 1 hour to 30 hours. In the case of continuous annealing, the annealing temperature is, for example, 900°C to 1000°C, and the holding time at the annealing temperature is, for example, 1 second to 100 seconds. If necessary, a well-known pickling treatment may be performed on the hot-rolled steel sheet before annealing in the hot-rolled sheet annealing step and / or the hot-rolled steel sheet after annealing.

[0104] [(Step 3) Cold Rolling Step] In the cold rolling step, cold rolling is performed on the hot-rolled steel sheet produced in the hot rolling step or the hot-rolled steel sheet after the hot-rolled sheet annealing step to produce a cold-rolled steel sheet. Cold rolling may be performed once or multiple times. When cold rolling is performed multiple times, intermediate annealing may be performed after cold rolling and before the next cold rolling is performed.

[0105] [(Step 4) Finish Annealing Step] Finish annealing is performed on the cold-rolled steel sheet produced by the cold rolling step in a finish annealing furnace. In finish annealing, the cold-rolled steel sheet finished to the final thickness is annealed to recrystallize and grow crystal grains. In the finish annealing step, the following conditions 1 to 5 are satisfied. (Condition 1) Annealing is performed at a maximum temperature T1 (°C) of 950°C or less. (Condition 2) The tension TE applied to the cold-rolled steel sheet at the maximum temperature T1 (°C) is 2.0 to 10.0 MPa. (Condition 3) The residence time t0 (seconds) between the annealing temperatures T1 and 700°C in the heating zone, soaking zone, and cooling zone of the finish annealing furnace, and the residence time t1 (seconds) between 700 and 500°C in the cooling zone satisfy formulas (A) and (B). t1-t0>0 (A) t1 / t0≦3.0 (B) (Condition 4) In the furnace atmosphere of the finish annealing furnace, at one or more locations selected from the heating zone, the soaking zone, and the cooling zone in the temperature range of 500°C or more, the hydrogen partial pressure P H2 (atm) relative to the water vapor partial pressure P H20 The ratio of oxygen to nitrogen (atm) is set to be higher than 0.05, or the oxygen concentration is set to be higher than 0.010% by volume. (Condition 5) The temperature gradient CG in the longitudinal direction of the cold-rolled steel sheet during the cooling process is set to be 20°C / m or less. Conditions 1 to 5 will be explained below.

[0106] [(Condition 1) Regarding the maximum reachable temperature T1] The maximum reachable temperature T1 is set to 950°C or less. If the maximum reachable temperature T1 exceeds 950°C, solution of carbides and nitrides occurs in the steel sheet. As a result, the work hardening amount WH defined by formula (3) becomes 15 MPa or more. Therefore, the maximum reachable temperature T1 is set to 950°C or less. A known temperature is sufficient as the lower limit of the maximum reachable temperature T1. The lower limit of the maximum reachable temperature T1 is, for example, 800°C.

[0107] [(Condition 2) Tension TE at Maximum Temperature T1] The tension TE applied to the cold-rolled steel sheet at the maximum temperature T1 is set to 2.0 to 10.0 MPa. Specifically, the tension TE is applied in the rolling direction (longitudinal direction) of the cold-rolled steel sheet. If the tension TE is less than 2.0 MPa, dislocation sources are not sufficiently obtained in the steel sheet. In this case, even if the non-oriented electrical steel sheet satisfies formula (4), the yield elongation will be less than 0.5%. On the other hand, if the tension TE exceeds 10.0 MPa, residual strain will occur in the steel sheet. In this case, the work hardening amount WH will be 15 MPa or more.

[0108] [(Condition 3) Residence Times t0 and t1] In finish annealing, the residence time t0 (seconds) between the annealing temperatures T1 and 700°C in the heating zone, soaking zone, and cooling zone of the finish annealing furnace, and the residence time t1 (seconds) between 700 and 500°C in the cooling zone satisfy the following formulas (A) and (B): t1 - t0 > 0 (A) t1 / t0 ≦ 3.0 (B) Here, the residence time t0 includes the time during the heating process from 700°C to the maximum temperature T1, the holding time at the maximum temperature T1, and the time during the cooling process from the maximum temperature T1 to 700°C in the heating zone, soaking zone, and cooling zone. The residence time t1 corresponds to the time from 700 to 500°C in the cooling zone, and does not include the time during the heating process (heating zone) from 500 to 700°C.

[0109] In the annealing temperature range of T1 to 700°C, carbides and nitrides are likely to dissolve, and solute C and solute N are likely to be formed. On the other hand, the temperature range of 700 to 500°C is a temperature range in which carbides, carbonitrides, and nitrides are likely to be formed. Solute C and solute N adhere to dislocations and inhibit dislocation movement. If the number of dislocations whose movement is inhibited increases, dislocation entanglement increases. Therefore, in the non-oriented electrical steel sheet of this embodiment, solute C and solute N are reduced as much as possible.

[0110] FA is defined as follows: FA = t1 - t0 FA corresponds to the left side of formula (A). When FA is greater than 0, that is, when the residence time t1 is longer than the residence time t0, the dissolved carbon and nitrogen can be re-immobilized as carbides, carbonitrides, and nitrides while suppressing the solutionization of carbides and nitrides that were formed before the finish annealing. Therefore, the amount of dissolved C and N in the steel sheet can be reduced. As a result, the work hardening amount WH can be reduced to less than 15 MPa.

[0111] FB is defined as follows: FB = t1 / t0 FB corresponds to the left side of formula (B). If FB exceeds 3.0, solute C and solute N remaining in the steel sheet without precipitating as precipitates will be fixed to dislocations. In this case, dislocations are more likely to pile up, and the amount of work hardening WH increases. If FB is 3.0 or less, the amount of work hardening WH can be sufficiently suppressed.

[0112] [(Condition 4) Regarding oxygen potential] In the final annealing, the hydrogen partial pressure P H2 (atm) relative to the water vapor partial pressure P H20 (atm) ratio is set to be higher than 0.05, or the oxygen concentration is set to be higher than 0.010%.

[0113] The hydrogen partial pressure P in the atmosphere of the finishing annealing furnace H2 (atm) relative to the water vapor partial pressure P H20 The ratio of (atm) to (atm) is defined as the oxygen potential. When the oxygen potential is higher than 0.05 or the oxygen concentration is higher than 0.010% in one or more locations selected from the heating zone, the soaking zone, and the cooling zone in the temperature range of 500°C or higher in the furnace atmosphere of a finish annealing furnace, decarburization of the steel sheet during finish annealing is promoted. In this case, the amount of solute C in the steel sheet can be sufficiently reduced. As a result, the work hardening amount WH can be made less than 15 MPa.

[0114] [(Feature 5) Regarding the temperature gradient CG in the longitudinal direction of the cold-rolled steel sheet during the cooling process] During the cooling process, the temperature gradient in the longitudinal direction (rolling direction) of the cold-rolled steel sheet from the maximum temperature T1 to 500°C is defined as CG (°C / m). The temperature gradient CG is calculated based on the sheet running distance from the maximum temperature T1 to 500°C and the temperature difference obtained by subtracting 500°C from the maximum temperature T1. If the temperature gradient CG during the cooling process exceeds 20°C / m, residual strain occurs in the steel sheet due to thermal strain. In this case, the work hardening amount WH becomes 15 MPa or more. Therefore, the temperature gradient CG is set to 20°C / m or less.

[0115] [Other Steps] In the above-described manufacturing method, a coating step may be carried out after the final annealing step. In the coating step, an insulating coating is applied to the surface of the non-oriented electrical steel sheet after the final annealing step. The type of insulating coating is not particularly limited. The insulating coating may be an organic component or an inorganic component.

[0116] The non-oriented electrical steel sheet of this embodiment can be manufactured by the above manufacturing method. Note that the manufacturing method of the non-oriented electrical steel sheet of this embodiment is not particularly limited as long as it satisfies Features 1 to 5.

[0117] [Regarding the rotor core] The rotor core of this embodiment is manufactured using the non-oriented electrical steel sheet of this embodiment as a material. Fig. 4 is a plan view showing an example of a rotor core 1. Referring to Fig. 4, the rotor core 1 includes a plurality of rotor core materials 2. The rotor core materials 2 are plate-shaped. More specifically, the rotor core materials 2 are disk-shaped. The rotor core 1 is configured by stacking a plurality of rotor core materials 2.

[0118] The shape of the rotor core material 2 is not particularly limited as long as it is plate-shaped. FIG. 4 shows the rotor core material 2 for a permanent magnet synchronous motor as an example. However, the rotor core material 2 may have other shapes as long as it is plate-shaped. For example, when the motor is a reluctance motor, the rotor core material 2 may be plate-shaped having a plurality of salient poles, or may be plate-shaped having a plurality of through-holes that serve as flux barriers. Furthermore, when the motor is an induction motor, the rotor core material 2 may have a plurality of through-holes in which induced current paths made of copper, aluminum die-cast, or the like are installed.

[0119] As described above, the rotor core material 2 is a stamped product manufactured by stamping the non-oriented electrical steel sheet of this embodiment. Therefore, the rotor core material 2 satisfies the above-mentioned features 1 to 5. Specifically, the rotor core material 2 contains, in mass %, Si: 3.1 to 4.5%, C: 0.0025% or less, N: 0.0025% or less, O: 0.0400% or less, P: 0.100% or less, S: 0.0050% or less, Ti: 0.0100% or less, Mn: 2.0% or less, Al: 1.500% or less, Zr: 0 to 0.0100%, Nb: 0 to 0.0100%, V: 0 to 0.0100%, Mo: 0 to 0.100%, Cr: 0 to 2.000%, La: 0 to 0.010 0%, Ce: 0 to 0.0100%, B: 0 to 0.0010%, Zn: 0 to 0.0050%, Ga: 0 to 0.0050%, Ge: 0 to 0.0050%, As: 0 to 0.0100%, Ni: 0 to 0.500%, Cu: 0 to 0.500%, Sn: 0 to 0.200%, Sb: 0 to 0.100%, Ca: 0 to 0.0050%, Nd: 0 to 0.0010%, Mg: 0 to 0.0030%, and the balance being Fe and impurities, and satisfying formula (1) and formula (2). Si / 28+Ti / 48+Nb / 93+V / 51+Zr / 91+Mo / 96+Cr / 52>C / 12×750 (1) Si / 28+Al / 27+Ti / 48+Zr / 91+La / 139+Ce / 140>N / 14×1000 (2) Here, the element symbols in formulas (1) and (2) are substituted with the corresponding element contents in mass %. When a corresponding element is not contained, "0" is substituted for the element symbol. Furthermore, rotor core material 2 has a tensile strength TS higher than 570 MPa. Furthermore, rotor core material 2 has a stress at 2.0% strain higher than Y 2.0 (MPa) and the yield stress is YS (MPa), the work hardening amount WH defined by the formula (3) is less than 15 MPa. 2.0 -YS (3) Furthermore, in the rotor core material 2, the average grain size D (μm) satisfies formula (4), and the yield point elongation is 0.5% or more. D<80-Si×10 (4) Here, the element symbol in formula (4) is substituted with the corresponding element content in mass %. If the corresponding element is not contained, "0" is substituted for that element symbol.

[0120] [Regarding the stator core] A stator core may be manufactured using the non-oriented electromagnetic steel sheet of this embodiment as a material. Fig. 5 is a plan view of the stator core 3. Referring to Fig. 5, the stator core 3 includes a plurality of stator core materials 4. The stator core materials 4 are in the shape of an annular plate. The stator core 3 is configured by stacking a plurality of stator core materials 4.

[0121] The stator core material 4 includes a plurality of teeth 41. The plurality of teeth 41 are arranged with gaps between each other in the circumferential direction of the stator core material 4. Each tooth 41 extends in the radial direction of the stator core material 4.

[0122] The stator core material 4 is manufactured by punching the non-oriented electrical steel sheet of this embodiment and then performing stress relief annealing. Therefore, the stator core material 4 satisfies the above-mentioned features 1 and 2.

[0123] Specifically, the stator core material 4 contains, in mass %, Si: 3.1 to 4.5%, C: 0.0025% or less, N: 0.0025% or less, O: 0.0400% or less, P: 0.100% or less, S: 0.0050% or less, Ti: 0.0100% or less, Mn: 2.0% or less, Al: 1.500% or less, Zr: 0 to 0.0100%, Nb: 0 to 0.0100%, V: 0 to 0.0100%, Mo: 0 to 0.100%, Cr: 0 to 2.000%, La: 0 to 0.010 0%, Ce: 0 to 0.0100%, B: 0 to 0.0010%, Zn: 0 to 0.0050%, Ga: 0 to 0.0050%, Ge: 0 to 0.0050%, As: 0 to 0.0100%, Ni: 0 to 0.500%, Cu: 0 to 0.500%, Sn: 0 to 0.200%, Sb: 0 to 0.100%, Ca: 0 to 0.0050%, Nd: 0 to 0.0010%, Mg: 0 to 0.0030%, and the balance being Fe and impurities, and satisfying formula (1) and formula (2). Si / 28+Ti / 48+Nb / 93+V / 51+Zr / 91+Mo / 96+Cr / 52>C / 12×750 (1) Si / 28+Al / 27+Ti / 48+Zr / 91+La / 139+Ce / 140>N / 14×1000 (2) Here, the element symbols in formulas (1) and (2) are substituted with the corresponding element contents in mass%. When the corresponding element is not contained, "0" is substituted for the element symbol.

[0124] [Method for measuring chemical composition of rotor core material 2 and stator core material 4] The chemical compositions of the rotor core material 2 and the stator core material 4 can be measured based on the method described in [Method for measuring chemical composition of non-oriented electrical steel sheet] above. Specifically, chips are collected from the rotor core material 2 or the stator core material 4 using a drill. The collected chips are dissolved in acid to obtain a solution. ICP-AES is performed on the solution to perform elemental analysis of the chemical composition. The C content and S content are determined using the well-known high-frequency combustion method (combustion-infrared absorption method). The N content is determined using the well-known inert gas fusion-thermal conductivity method. The O content is determined using the well-known inert gas fusion-infrared absorption method.

[0125] [Method for measuring stress-strain curve of rotor core material 2] The tensile strength TS of the rotor core material 2 is measured by the following method. A JIS No. 5 tensile test piece specified in JIS Z2241:2011 is taken from the rotor core material 2. If a JIS No. 5 tensile test piece cannot be taken from the rotor core material 2 due to its small size, a scaled-down JIS No. 5 tensile test piece is taken from the rotor core material 2. Using the taken tensile test piece, a tensile test is carried out in air at room temperature in accordance with JIS Z2241:2011 to obtain a stress-strain curve. The tensile strength TS (MPa) is determined from the obtained stress-strain curve. When a tensile test is carried out using a scaled-down test piece, the test is carried out based on the strain rate specified in Annex JB of the above standard.

[0126] [Test for evaluating work-hardening amount WH of rotor core material 2] The work-hardening amount WH of the rotor core material 2 is determined by the method described in the above-mentioned [Test for evaluating work-hardening amount WH]. At this time, the stress-strain curve used is the stress-strain curve obtained by the above-mentioned [Method for measuring the stress-strain curve of the rotor core material 2].

[0127] [Method for measuring average crystal grain size D of rotor core material 2] The average crystal grain size D of the rotor core material 2 is determined by the method described in the above-mentioned [Method for measuring average crystal grain size D]. Note that the cross section (L cross section) of the rotor core material 2 parallel to the rolling direction is used as the observation surface.

[0128] [Method for measuring yield elongation of rotor core material 2] The yield elongation of the rotor core material 2 is determined by the following method. Specifically, a JIS No. 5 tensile test piece is taken from the rotor core material 2. A tensile test is conducted at room temperature in the air in accordance with JIS Z2241:2011 to determine the yield elongation (%). Note that if a JIS No. 5 tensile test piece cannot be taken because the rotor core material 2 is too small in size, a scaled-down test piece for the JIS No. 5 tensile test piece is taken from the rotor core material 2. When a tensile test is conducted using a scaled-down test piece, the test is conducted based on the strain rate specified in Annex JB of the above standard.

[0129] If the upper yield point is not clearly visible, the yield elongation (%) is determined by the following method. Referring to FIG. 3, the yield strength YS (MPa) is determined in the stress-strain curve obtained by the tensile test based on the method described in the above-mentioned [Test for evaluating the amount of work hardening WH of the rotor core material 2]. The strain value at the determined yield strength YS is designated as ε1. In the stress-strain curve after the strain value ε1, the maximum strain value ε2 is identified in the region where the stress is maintained within the range of the yield stress YS ±1.0% as the strain increases. Using ε1 and ε2, the yield elongation is determined by the following formula: Yield elongation (%) = ε2 - ε1

[0130] [Method for manufacturing rotor core 1] The rotor core 1 is manufactured by the following method. A rotor core blank 2 is manufactured by punching from the non-oriented electrical steel sheet of this embodiment. Specifically, the rotor core blank 2 is punched out by punching. The punched rotor core blanks 2 are stacked to manufacture the rotor core 1.

[0131] [Regarding the Motor] The motor of this embodiment includes the rotor core 1 described above. The motor further includes a well-known stator core. Because the motor of this embodiment includes the rotor core of this embodiment, the rotor core has high strength and sufficient magnetic properties.

[0132] The stator core 3 described above may be used as the stator core included in the motor core. The stator core 3 is manufactured by the following method. Using the non-oriented electromagnetic steel sheet of this embodiment as a material, a stator core blank 4 is manufactured by punching. A plurality of stator core blanks 4 are stacked to manufacture the stator core 3.

[0133] The stator core material 4 manufactured by punching using the non-oriented electromagnetic steel sheet of this embodiment has high dimensional accuracy. Therefore, it is superior in terms of dimensional accuracy to a stator core manufactured using a conventional non-oriented electromagnetic steel sheet having a tensile strength of more than 570 MPa. The stator core 3 manufactured using the non-oriented electromagnetic steel sheet of this embodiment is subjected to stress relief annealing after laminating the stator core material 4. This makes it possible to improve the efficiency of a motor incorporating the stator core 3.

[0134] Non-oriented electrical steel sheets having the chemical compositions shown in Table 1 (Tables 1A to 1C) were produced by the following method.

[0135]

[0136]

[0137]

[0138] In Table 1C, "T" in the "Formula (1)" column means that formula (1) is satisfied, and "F" means that formula (1) is not satisfied. "T" in the "Formula (2)" column means that formula (2) is satisfied, and "F" means that formula (2) is not satisfied.

[0139] The slabs (steel billets) were hot-rolled to produce hot-rolled steel sheets with a thickness of 2.0 mm. The slab heating temperature was 1100 to 1200°C. The finish rolling temperature was 800 to 1100°C. The coiling temperature was 700 to 800°C. The hot-rolled steel sheets were subjected to hot-rolled sheet annealing by continuous annealing, in which the sheets were soaked at 1000°C for 60 seconds. The steel sheets after the hot-rolled sheet annealing were cold-rolled to produce cold-rolled steel sheets with a thickness of 0.25 mm.

[0140] The cold-rolled steel sheets thus produced were subjected to final annealing. The maximum temperature reached in the final annealing, T1 (°C), tension, TE (MPa), residence time, t0 (seconds) and residence time, t1 (seconds), FA, FB, and oxygen potential, P H20 / P H2 The oxygen concentration (%) and temperature gradient CG (°C / m) are shown in Table 2. Non-oriented electrical steel sheets with each test number were manufactured by the above manufacturing process.

[0141]

[0142] [Evaluation Tests] The following evaluation tests were carried out on the non-oriented electrical steel sheets with each test number: (Test 1) Chemical composition measurement test (Test 2) Tensile strength TS measurement test (Test 3) Work hardening amount WH evaluation test (Test 4) Average grain size D measurement test (Test 5) Yield point elongation measurement test (Test 6) Magnetic property evaluation test (Test 7) ​​Dimensional accuracy evaluation test after punching Tests 1 to 7 are explained below.

[0143] [(Test 1) Chemical Composition Measurement Test] The chemical composition of the non-oriented electrical steel sheet of each test number was determined according to the method described in the above-mentioned [Method for measuring the chemical composition of non-oriented electrical steel sheet]. As a result, the chemical compositions of the non-oriented electrical steel sheets of each test number were as shown in Table 1 (Tables 1A to 1C).

[0144] [(Test 2) Tensile Strength TS Measurement Test] The tensile strength TS (MPa) of the non-oriented electrical steel sheet of each test number was determined according to the method described in the above-mentioned [Method for Measuring Stress-Strain Curve]. The obtained tensile strengths TS (MPa) are shown in Table 3.

[0145]

[0146] [(Test 3) Work-hardening amount WH evaluation test] The work-hardening amount WH (MPa) of the non-oriented electrical steel sheet of each test number was determined according to the method described in the above-mentioned [Work-hardening amount WH evaluation test]. The obtained work-hardening amounts WH (MPa) are shown in Table 3.

[0147] [(Test 4) Measurement of average grain size D] The average grain size D (μm) of the non-oriented electrical steel sheets of each test number was determined according to the method described in the above [Method for measuring average grain size D]. The obtained average grain sizes D are shown in Table 3.

[0148] [(Test 5) Yield point elongation measurement test] The yield point elongation (%) of the non-oriented electrical steel sheet of each test number was determined according to the method described in the "Method for measuring yield point elongation" above. The obtained yield point elongation (%) is shown in Table 3. In Table 3, "80-Si×10" indicates the Fn value. In addition, in Table 3, "T" in the "Formula (4)" column means that formula (4) is satisfied, and "F" means that formula (4) is not satisfied.

[0149] [(Test 6) Magnetic Property Evaluation Test] The magnetic flux density B 50 (T) and iron loss W 5/1000 (W / kg) was calculated. 50 Evaluation test] For the non-oriented electrical steel sheets of each test number, the magnetic flux density B 50(L) , and the magnetic flux density B in the direction perpendicular to the rolling direction (direction C) 50(C)Specifically, Epstein test pieces were cut out in the L direction and the C direction from the non-oriented electrical steel sheets of each test number in accordance with JIS C 2550-1:2011. The cut-out Epstein test pieces were subjected to the electrical steel strip test method in accordance with JIS C 2550-1:2011 and 2550-3:2011, and the magnetic flux density B at 5000 A / m in the L direction and the C direction was measured. 50(L) (T) and B 50(C) (T) was measured. The magnetic flux density B in the L direction 50(L) (T) and C direction magnetic flux density B 50(C) The arithmetic mean value of the magnetic flux density B 50 The obtained magnetic flux density B 50 (T) is shown in Table 3.

[0150] [Iron loss W 5/1000 Evaluation Test] The above-mentioned magnetic flux density B 50 Epstein test specimens were prepared in the same manner as in the evaluation test. The Epstein test specimens were cut out in two ways: by shear cutting with a clearance set to 20 μm, and by electrical discharge machining. That is, two types of test specimens were prepared for each test number: an Epstein test specimen cut out by shear cutting, which simulates punching, and an Epstein test specimen cut out by electrical discharge machining. Each Epstein test specimen was subjected to the electromagnetic steel strip test method in accordance with JIS C 2550-1:2011 and 2550-3:2011, and the iron loss W at 1000 Hz and 0.5 T in the L direction (rolling direction) and C direction (direction perpendicular to the rolling direction) was measured. 5/1000(L) (W / kg) and iron loss W 5/1000(C) (W / kg) was measured. Iron loss in the L direction (rolling direction) W 5/1000(L) and iron loss W in the C direction (direction perpendicular to the rolling direction) 5/1000(C) The arithmetic mean value of (W / kg) is the iron loss W 5/1000 (W / kg). Iron loss W in the Epstein test piece by shear cutting 5/1000 (W / kg) is compared with the "iron loss W 5/1000 The iron loss W of the Epstein test piece by electrical discharge machining is shown in the "Shear Cutting" column. 5/1000 (W / kg) is compared with the "iron loss W 5/1000 (W / kg)" in the "Electric Discharge Machining" column. Iron loss in shear cutting W5/1000 (W / kg) to iron loss W in EDM 5/1000 (W / kg) is subtracted from the iron loss deterioration amount ΔW 5/1000 (W / kg). Iron loss deterioration amount Δ iron loss W 5/1000 (W / kg) is shown in Table 3.

[0151] [(Test 7) ​​Evaluation of Dimensional Accuracy After Punching] The dimensional accuracy of the non-oriented electrical steel sheets of each test number after punching was evaluated by the following test. Ring-shaped samples (punched products) with an inner diameter of 90 mm and an outer diameter of 100 mm were prepared from the non-oriented electrical steel sheets of each test number by punching them using a die with a clearance of 8% of the sheet thickness. Furthermore, the prepared ring-shaped samples were cut at 45° intervals around the normal to the non-oriented electrical steel sheets from the rolling direction of the non-oriented electrical steel sheets to obtain eight test pieces. Each test piece was embedded in resin, and the cut surfaces were polished by 1 mm or more to remove the influence of deformation during cutting. After polishing, the cut surfaces near the punched end surface on the inner peripheral surface and the cut surfaces near the punched end surface on the outer peripheral surface were observed using an optical microscope at 100x magnification. As shown in Figure 6, a line segment 20 is drawn connecting point P1 where the sag surface 10 transitions to the punched end surface 11 and the burr tip P2 of the punched end surface 11. A line segment 21 is drawn parallel to line segment 20 and tangent to the punched end surface 11 protruding from line segment 20. The distance d between line segment 20 and line segment 21 is calculated. The arithmetic mean value of the distances d calculated for eight test pieces (eight on the cut surface near the punched end surface on the inner peripheral surface side, eight on the cut surface near the punched end surface on the outer peripheral surface side, a total of 16 on the inner peripheral surface side and the outer peripheral surface side) was defined as the punched flatness (μm). The obtained punched flatness is shown in Table 3 as "Punched Flatness (μm)".

[0152] [Evaluation Results] Referring to Tables 1 to 3, test numbers 1 to 30 satisfied features 1 to 5. Therefore, the non-oriented electrical steel sheets with these test numbers had a magnetic flux density B 50 is 1.60T or more, and the iron loss W 5/1000 Iron loss in shear cutting W 5/1000 Iron loss deterioration amount ΔW minus 5/1000 The flatness of the punched portion was 25 μm or less, and the dimensional accuracy after punching was excellent.

[0153] On the other hand, test numbers 31 to 34 did not satisfy formula (1) or formula (2). Therefore, the punching flatness exceeded 25 μm, and sufficient dimensional accuracy was not obtained during punching. Furthermore, the iron loss degradation amount ΔW 5/1000 was more than 2.0, and excellent magnetic properties were not obtained.

[0154] In test numbers 35 and 36, the Si content was too low. Therefore, the tensile strength TS was too low. Furthermore, the work hardening amount WH was 15 MPa or more. As a result, the iron loss deterioration amount ΔW 5/1000 was more than 2.0, and excellent magnetic properties were not obtained.

[0155] In test numbers 37 and 38, the Si content was too low. Therefore, the work hardening amount WH was 15 MPa or more. As a result, the punching flatness exceeded 25 μm, and sufficient dimensional accuracy was not obtained during punching. Furthermore, the iron loss deterioration amount ΔW 5/1000 was more than 2.0, and excellent magnetic properties were not obtained.

[0156] Test Nos. 39 and 40 did not satisfy Condition 1 in the finish annealing process. Therefore, the work hardening amount WH was 15 MPa or more. Furthermore, formula (4) was not satisfied, and the yield point elongation was also less than 0.5%. As a result, the punching flatness exceeded 25 μm, and sufficient dimensional accuracy was not obtained during punching. Furthermore, the iron loss degradation amount ΔW 5/1000 was more than 2.0, and excellent magnetic properties were not obtained.

[0157] In test numbers 41 and 42, the tension TE at the maximum temperature T1 was too low. Therefore, the yield elongation was less than 0.5%. As a result, the punching flatness exceeded 25 μm, and sufficient dimensional accuracy was not obtained during punching. Furthermore, the iron loss degradation amount ΔW 5/1000 was more than 2.0, and excellent magnetic properties were not obtained.

[0158] In test numbers 43 and 44, the tension TE at the maximum temperature T1 was too high. Therefore, the work hardening amount WH was 15 MPa or more. As a result, the punching flatness exceeded 25 μm, and sufficient dimensional accuracy was not obtained during punching. Furthermore, the iron loss deterioration amount ΔW 5/1000was more than 2.0, and excellent magnetic properties were not obtained.

[0159] In test numbers 45 and 46, FA did not satisfy formula (A) in the finish annealing process. Therefore, the work hardening amount WH was 15 MPa or more. As a result, the punching flatness exceeded 25 μm, and sufficient dimensional accuracy was not obtained during punching. Furthermore, the iron loss degradation amount ΔW 5/1000 was more than 2.0, and excellent magnetic properties were not obtained.

[0160] In test numbers 47 and 48, FB did not satisfy formula (B). Therefore, the work hardening amount WH was 15 MPa or more. As a result, the punching flatness exceeded 25 μm, and sufficient dimensional accuracy was not obtained during punching. Furthermore, the iron loss deterioration amount ΔW 5/1000 was more than 2.0, and excellent magnetic properties were not obtained.

[0161] Test Nos. 49 and 50 did not satisfy Condition 4 in the finish annealing process. Therefore, the work hardening amount WH was 15 MPa or more. As a result, the punching flatness exceeded 25 μm, and sufficient dimensional accuracy was not obtained during punching. Furthermore, the iron loss deterioration amount ΔW 5/1000 was more than 2.0, and excellent magnetic properties were not obtained.

[0162] In test numbers 51 and 52, the temperature gradient CG was too large. As a result, the work hardening amount WH was 15 MPa or more. As a result, the punching flatness exceeded 25 μm, and sufficient dimensional accuracy was not obtained after punching. Furthermore, the iron loss degradation amount ΔW 5/1000 was more than 2.0, and excellent magnetic properties were not obtained.

[0163] Rotor cores having the shape shown in FIG. 4 were manufactured using the non-oriented electrical steel sheets of test numbers 1 to 30 in Example 1. Specifically, punching was performed on the non-oriented electrical steel sheets of each test number. In the punching process, rotor core blanks were produced by punching using a die with a clearance of 8% of the sheet thickness. Multiple rotor core blanks were stacked to form a rotor core. The diameter of the rotor core blank was 70 mm.

[0164] The following evaluation tests were conducted on the rotor cores with each test number: (Test 1) Tensile strength TS measurement test (Test 2) Work hardening amount WH evaluation test (Test 3) Average grain size D measurement test (Test 4) Yield point elongation measurement test (Test 5) Magnetic property evaluation test (Test 6) Dimensional accuracy evaluation test after punching Tests 1 to 6 are explained below.

[0165] [(Test 1) Tensile Strength TS Measurement Test] A rotor core material was separated from the rotor core. The tensile strength TS (MPa) of the rotor core material was determined according to the method described above in [Method for Measuring Stress-Strain Curve of Rotor Core Material 2]. The size of the tensile test specimen taken from the rotor core material was a parallel portion width of 2.50 mm, a gauge length of 5.00 mm, a thickness of 0.25 mm, and a total length of 25 mm. The tensile strength TS (MPa) of the rotor core material is shown in Table 4.

[0166] [(Test 2) Work-hardening amount WH evaluation test] The work-hardening amount WH of the rotor core material was determined according to the method described in the above-mentioned [Work-hardening amount WH evaluation test of rotor core material 2]. The work-hardening amounts WH (MPa) of the obtained rotor core materials are shown in Table 4.

[0167] [(Test 3) Measurement test of average crystal grain size D] A rotor core blank was separated from the rotor core. The average crystal grain size D (μm) of the rotor core blank was determined according to the method described in [Method for measuring average crystal grain size D of rotor core blank 2] above. The average crystal grain size D (μm) of the obtained rotor core blank is shown in Table 4.

[0168] [(Test 4) Yield Elongation Measurement Test] A rotor core blank was separated from the rotor core. The yield elongation (%) of the rotor core blank was determined according to the method described in the above-mentioned [Method for Measuring Yield Elongation of Rotor Core Blank 2]. The dimensions of the tensile test specimen taken from the rotor core blank were a parallel portion width of 2.50 mm, a gauge length of 5.00 mm, a thickness of 0.25 mm, and a total length of 25 mm. The yield elongation (%) of the rotor core blank is shown in Table 4.

[0169] [(Test 5) Magnetic Property Evaluation Test] A rotor core material was separated from the rotor core. A small test piece for single sheet magnetic measurement having a size that could be sampled was produced from the separated rotor core material by electrical discharge machining. The size of the small test piece was 10 mm x 20 mm x sheet thickness. Using the small test piece and a single sheet tester, the magnetic flux density B of the rotor core material was measured in accordance with the Single Sheet Tester (SST) described in JIS C 2556:2015. 50 (T) and iron loss W 5/1000 The magnetic flux density B (W / kg) of the obtained rotor core material was calculated. 50 (T) and iron loss W 5/1000 (W / kg) is shown in Table 4.

[0170] [(Test 6) Evaluation Test for Dimensional Accuracy After Punching] The punched rotor core blank was cut at 45° intervals around the central axis of the rotor core blank to obtain eight test pieces, including the outer peripheral surface side of the rotor core blank during punching. Each test piece was embedded in resin, and the cut surface was polished by 1 mm or more to eliminate the influence of deformation during cutting. After polishing, the cut surface near the outer peripheral surface of the rotor core blank was observed using an optical microscope at 100x magnification. As shown in Figure 6, a line segment 20 was drawn connecting point P1, where the sagging surface 10 transitions to the punched end surface 11, and the burr tip P2 of the punched end surface 11. A line segment 21 was drawn that was parallel to line segment 20 and tangent to the punched end surface 11 protruding from line segment 20. The distance d between line segment 20 and line segment 21 was calculated. The arithmetic mean value of the distances d calculated for the eight test pieces (a total of eight) was defined as the punching flatness (μm). The punched flatness (μm) of the obtained rotor core blanks is shown in Table 4. Note that with respect to the inner peripheral surface side of the rotor core blank, the punched end surface at the time of punching may not be maintained due to processing such as when inserting the shaft. Therefore, as described above, the dimensional accuracy was evaluated at the punched end surface in the vicinity of the outer peripheral surface of the rotor core blank.

[0171]

[0172] [Evaluation Results] As shown in Table 4, the rotor core materials with test numbers 1 to 30 satisfied features 1 to 5. Therefore, the rotor core materials with these test numbers had a punching flatness of 25 μm or less, and were excellent in dimensional accuracy after punching. 50 is 1.60T or more, and iron loss W 5/1000 The magnetic strength was 16.9 W / kg or less, and high strength and excellent magnetic properties were obtained.

[0173] While preferred embodiments of the non-oriented electrical steel sheet of the present disclosure have been described above, the non-oriented electrical steel sheet of the present disclosure is not limited to these examples. It is clear that a person skilled in the art can conceive of various modifications or alterations within the scope of the ideas described in the claims, and it is understood that these modifications or alterations also fall within the technical scope of the non-oriented electrical steel sheet of the present disclosure.

Claims

1. A non-oriented electrical steel sheet having, by mass%, the following: Si: 3.1 to 4.5%, C: 0.0025% or less, N: 0.0025% or less, O: 0.0400% or less, P: 0.100% or less, S: 0.0050% or less, Ti: 0.0100% or less, Mn: 2.0% or less, Al: 1.500% or less, Zr: 0 to 0.0100%, Nb: 0 to 0.0100%, V: 0 to 0.0100%, Mo: 0 to 0.100%, Cr: 0 to 2.000%, La: 0 to 0.0100%, Ce: 0 to 0.0100%, B: 0 to 0.0010%, Zn: 0 to 0.0050%, A steel sheet comprising Ga: 0-0.0050%, Ge: 0-0.0050%, As: 0-0.0100%, Ni: 0-0.500%, Cu: 0-0.500%, Sn: 0-0.200%, Sb: 0-0.100%, Ca: 0-0.0050%, Nd: 0-0.0010%, Mg: 0-0.0030%, and the balance being Fe and impurities, and satisfying formula (1) and formula (2), having a tensile strength TS higher than 570 MPa, and a stress at 2.0% strain of Y 2.0 A non-oriented electrical steel sheet, in which, when Y (MPa) is the strained strength and YS (MPa), the amount of work hardening defined by formula (3) is less than 15 MPa, the average grain size D (μm) satisfies formula (4), and the yield elongation is 0.5% or more. Si / 28+Ti / 48+Nb / 93+V / 51+Zr / 91+Mo / 96+Cr / 52>C / 12×750 (1) Si / 28+Al / 27+Ti / 48+Zr / 91+La / 139+Ce / 140>N / 14×1000 (2) WH=Y 2.0 -YS (3) D<80-Si×10 (4) Here, the element symbols in formulas (1), (2) and (4) are substituted with the content of the corresponding element in mass%. When the corresponding element is not contained, "0" is substituted for the element symbol.

2. The non-oriented electrical steel sheet according to claim 1, comprising, in mass%, Zr: 0.0001 to 0.0100%, Nb: 0.0001 to 0.0100%, V: 0.0001 to 0.0100%, Mo: 0.001 to 0.100%, Cr: 0.001 to 2.000%, La: 0.0001 to 0.0100%, Ce: 0.0001 to 0.0100%, B: 0.0001 to 0.0010%, Zn: 0.0001 to 0.0050%, Ga: 0.0001 to 0.0050%, Ge: 0.0001 to 0.0050%, As: 0.0001 to 0.0100%, A non-oriented electrical steel sheet containing one or more selected from the group consisting of Ni: 0.001-0.500%, Cu: 0.001-0.500%, Sn: 0.001-0.200%, Sb: 0.001-0.100%, Ca: 0.0001-0.0050%, Nd: 0.0001-0.0010%, and Mg: 0.0001-0.0030%.

3. A rotor core material having a plurality of rotor core materials stacked on top of each other, the rotor core materials having, in mass %, Si: 3.1 to 4.5%, C: 0.0025% or less, N: 0.0025% or less, O: 0.0400% or less, P: 0.100% or less, S: 0.0050% or less, Ti: 0.0100% or less, Mn: 2.0% or less, Al: 1.500% or less, Zr: 0 to 0.0100%, Nb: 0 to 0.0100%, V: 0 to 0.0100%, Mo: 0 to 0.100%, Cr: 0 to 2.000%, La: 0 to 0.0100%, Ce: 0 to 0.0100%, B: 0 to 0.0010%, Zn: 0-0.0050%, Ga: 0-0.0050%, Ge: 0-0.0050%, As: 0-0.0100%, Ni: 0-0.500%, Cu: 0-0.500%, Sn: 0-0.200%, Sb: 0-0.100%, Ca: 0-0.0050%, Nd: 0-0.0010%, Mg: 0-0.0030%, and the balance being Fe and impurities, and satisfies formula (1) and formula (2), has a tensile strength TS higher than 570 MPa, and has a stress at 2.0% strain of Y 2.0A rotor core, in which, when Y (MPa) is the strained strength and YS (MPa) is the yield stress, the work hardening amount WH defined by formula (3) is less than 15 MPa, the average grain size D (μm) satisfies formula (4), and the yield elongation is 0.5% or more. Si / 28+Ti / 48+Nb / 93+V / 51+Zr / 91+Mo / 96+Cr / 52>C / 12×750 (1) Si / 28+Al / 27+Ti / 48+Zr / 91+La / 139+Ce / 140>N / 14×1000 (2) WH=Y 2.0 -YS (3) D<80-Si×10 (4) Here, the element symbols in formulas (1), (2) and (4) are substituted with the content of the corresponding element in mass%. When the corresponding element is not contained, "0" is substituted for the element symbol.

4. A rotor core according to claim 3, wherein the rotor core material contains, in mass%, Zr: 0.0001-0.0100%, Nb: 0.0001-0.0100%, V: 0.0001-0.0100%, Mo: 0.001-0.100%, Cr: 0.001-2.000%, La: 0.0001-0.0100%, Ce: 0.0001-0.0100%, B: 0.0001-0.0010%, Zn: 0.0001-0.0050%, Ga: 0.0001-0.0050%, Ge: 0.0001-0.0050%, As: 0.0001-0.0100%, A rotor core containing one or more selected from the group consisting of Ni: 0.001-0.500%, Cu: 0.001-0.500%, Sn: 0.001-0.200%, Sb: 0.001-0.100%, Ca: 0.0001-0.0050%, Nd: 0.0001-0.0010%, and Mg: 0.0001-0.0030%.

5. A motor comprising the rotor core according to claim 3 or 4.

6. A method for producing a non-oriented electrical steel sheet according to claim 1 or 2, comprising: a hot rolling process for hot rolling a slab to produce a hot rolled steel sheet; a cold rolling process for cold rolling the hot rolled steel sheet to produce a cold rolled steel sheet; and a finish annealing process for finish annealing the cold rolled steel sheet in a finish annealing furnace, wherein in the finish annealing process, the cold rolled steel sheet is annealed at a maximum temperature T1 of 950°C or less, a tension TE applied to the cold rolled steel sheet at the maximum temperature T1 is set to 2.0 to 10.0 MPa, and a residence time t0 (seconds) between annealing temperatures T1 and 700°C in the heating zone, soaking zone and cooling zone of the finish annealing furnace and a residence time t1 (seconds) between 700 and 500°C in the cooling zone satisfy formulas (A) and (B), In the furnace atmosphere of the finish annealing furnace, at one or more points selected from the heating zone, the soaking zone, and the cooling zone in a temperature range of 500 ° C. or more, a hydrogen partial pressure P H2 (atm) vs. water vapor partial pressure P H20 (atm) is made higher than 0.05, or the oxygen concentration is made higher than 0.010%, and a temperature gradient CG in the longitudinal direction of the cold-rolled steel sheet during the cooling process is made 20°C / m or less.

Citation Information

Patent Citations

  • Nonoriented silicon steel sheet having excellent strength and magnetic property and its production method

    JP2008050686A

  • Non-oriented electromagnetic steel sheet superior in workability, and manufacturing method therefor

    JP2002294414A

  • Nonoriented silicon steel sheet having excellent magnetic property and blanking workability

    JP2005105407A

  • Nonoriented electromagnetic steel sheet and manufacturing method therefor

    JP2018178196A

  • Non-oriented electromagnetic steel sheet and manufacturing method therefor, and motor core and manufacturing method therefor

    JP2019178372A

Cited By

  • Non-oriented electromagnetic steel sheet, motor core, and motor

    WO2025229787A1

  • Non-oriented electrical steel plate and manufacturing method therefor

    WO2026124372A1