Electrolyte, energy storage device, energy storage module, and electric device

By controlling the conductivity, viscosity, density and lithium salt concentration of the electrolyte to meet specific numerical ranges and relational expressions, the problem of difficulty in ensuring process performance and cost when improving the electrical performance of the electrolyte is solved, and rapid development of products with ideal performance is achieved. Electrolyte has better electrical properties and reasonable cost.

WO2024212694A1PCT designated stage expired Publication Date: 2024-10-17XIAMEN HITHIUM ENERGY STORAGE TECHNOLOGY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/076019
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-12
Filing Date
2024-02-05
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

It is difficult for existing electrolytes to ensure good process performance and reasonable production costs while improving electrical performance, resulting in limited performance improvement of energy storage devices.

Method used

By controlling the conductivity, viscosity, density and lithium salt concentration of the electrolyte to meet specific numerical ranges and relational expressions, an electrolyte with ideal performance can be quickly developed to ensure that the electrolyte has good process performance and reasonable production while improving electrical performance. cost.

Benefits of technology

It realizes the rapid development of electrolyte with ideal performance in a short time and with less consumable materials, ensuring that the electrolyte has excellent electrical properties, good process performance and reasonable production cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024076019_17102024_PF_FP_ABST
    Figure CN2024076019_17102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to an electrolyte, an energy storage device, an energy storage module, and an electric device. The electrolyte is used for the energy storage device and satisfies 23.1≤-15×ϲ2+28.53×c+0.64×μ+16.47×ρ-σ≤25.3, wherein c is the numerical value of the lithium salt concentration in the electrolyte and falls within the range of 0.6-1 mol / L, μ is the numerical value of the viscosity of the electrolyte at the temperature of 25°C and falls within the range of 1.6-3.0 mPa.s, ρ is the numerical value of the density of the electrolyte and falls within the range of 1.1-1.3 g / cm3, and σ is the numerical value of the conductivity of the electrolyte and falls within the range of 8-12 ms / cm. The conductivity, viscosity, density and lithium salt concentration of the electrolyte are controlled to satisfy the described numerical ranges and the described relation, so that an electrolyte having ideal performance can be rapidly developed with short time consumption and few consumables, thereby achieving good process performance and rational production cost while ensuring improved electrical performance of the electrolyte.
Need to check novelty before this filing date? Find Prior Art

Description

Electrolyte and energy storage device, energy storage module, electrical equipment

[0001] Related cross-references

[0002] This disclosure claims priority to Chinese patent application number 2023103872006, filed with the Patent Office of China on April 12, 2023, entitled “An electrolyte and energy storage device, energy storage module, and electrical equipment,” the entire contents of which are incorporated herein by reference. Technical Field

[0003] The present application relates to the field of energy storage technology, and in particular to an electrolyte and energy storage device, an energy storage module, and electrical equipment. Background Art

[0004] At present, the process of developing electrolytes requires a lot of time to prepare and test different formulas. It is not only time-consuming and consumable, but the developed electrolytes can only make certain trade-offs between the three aspects of electrical performance, process performance and production cost to achieve a balance between the three. For example, in order to make the electrolyte have better electrical performance, the process of the electrolyte is often required to be higher, but this will also lead to an increase in production costs. Conversely, in order to ensure good process performance, the electrical performance of the electrolyte is more difficult to improve, and it is difficult to break through a certain performance indicator, which in turn makes it difficult to further improve the relevant performance of the energy storage device. Therefore, it is necessary to make certain trade-offs between the electrical performance, process performance and cost of the electrolyte to balance these three indicators.

[0005] In other words, it is difficult for current electrolytes to simultaneously meet the requirements of improved electrical performance, good process performance and appropriate cost. In particular, it is difficult to develop an electrolyte that meets the above requirements while consuming less time, consumables and at low cost.

[0006] Summary of the Invention

[0007] In order to solve the above technical problems, the present application discloses an electrolyte and an energy storage device, an energy storage module, and an electrical equipment to solve the problem that the current electrolyte is difficult to improve electrical performance while ensuring good process performance and cost.

[0008] In a first aspect, an embodiment of the present application provides an electrolyte for an energy storage device, wherein the electrolyte satisfies the following relationship: 23.1≤-15×c 2 +28.53×c+0.64×μ+16.47×ρ-σ≤25.3, where

[0009] c is the concentration of the lithium salt in the electrolyte, and the concentration of the lithium salt is 0.6 mol / L to 1 mol / L;

[0010] μ is the viscosity of the electrolyte at 25° C., and the viscosity of the electrolyte at 25° C. is 1.6 mPa.s to 3.0 mPa.s;

[0011] ρ is the density of the electrolyte, which is 1.1 g / cm 3 ~1.3g / cm 3 ;

[0012] σ is the value of the conductivity of the electrolyte, and the conductivity is 8 ms / cm to 12 ms / cm.

[0013] In a second aspect, an embodiment of the present application provides an energy storage device, which includes the electrolyte as described in the first aspect.

[0014] In a third aspect, the present application provides an energy storage module, which includes a box body and the energy storage device as described in the second aspect arranged in the box body.

[0015] In a fourth aspect, an embodiment of the present application provides an electrical device, which includes an electrical device body and an energy storage device as described in the second aspect arranged in the electrical device body, and the energy storage device is used to supply power to the electrical device body.

[0016] Compared with the prior art, the present invention has the following advantages:

[0017] The embodiments of the present application control the conductivity, viscosity, density and lithium salt concentration of the electrolyte to meet the above-mentioned numerical ranges and relationship expressions, and can quickly develop an electrolyte with ideal performance in a short time and with low material consumption, thereby ensuring that the electrolyte can improve electrical performance while also having good process performance and reasonable production costs.

[0018] On the one hand, based on the preset values ​​of electrolyte viscosity, density, and lithium salt concentration, the electrolyte conductivity value can be quickly determined. Since conductivity has a significant impact on the internal resistance and rate characteristics of the energy storage device, the determined conductivity value can be used to determine whether the developed electrolyte has superior electrical performance, thereby quickly and in advance determining whether the electrolyte developed based on the above electrolyte viscosity, density, conductivity, and lithium salt concentration values ​​has good performance. On the other hand, because the viscosity, density, conductivity, and lithium salt concentration values ​​of the developed electrolyte are all within the range of the embodiments of the present application, it can be ensured that the developed electrolyte not only has superior electrical performance, but also has good process performance and reasonable production costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the following briefly introduces the drawings required for use in the embodiments. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0020] FIG1 is a graph showing the cycle performance of batteries using the electrolytes of Examples 1 to 3 and Comparative Example 1 of the present application. DETAILED DESCRIPTION

[0021] The following will be combined with the drawings in the embodiments of this application to clearly and completely describe the technical solutions in the embodiments of this application. Obviously, the embodiments described are only part of the embodiments of this application, not all of the embodiments. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.

[0022] In this application, terms such as "upper," "lower," "left," "right," "front," "back," "top," "bottom," "inner," "outer," "center," "vertical," "horizontal," "transverse," and "longitudinal" indicate positions or locations based on the positions or locations shown in the accompanying drawings. These terms are primarily intended to better describe this application and its embodiments and are not intended to limit the devices, elements, or components indicated to having a specific orientation, or to being constructed or operated in a specific orientation.

[0023] Furthermore, some of the above terms may be used to express other meanings besides indicating a position or location. For example, the term "on" may also be used to indicate a dependency or connection in certain circumstances. Those skilled in the art will understand the specific meanings of these terms in this application based on the specific circumstances.

[0024] Furthermore, the terms "installed," "disposed," "provided with," "connected," and "connected" should be interpreted broadly. For example, they can refer to fixed connections, removable connections, or integral structures; mechanical connections or electrical connections; direct connections, indirect connections through an intermediary, or internal communication between two devices, elements, or components. Those skilled in the art will understand the specific meanings of these terms in this application based on the specific circumstances.

[0025] Furthermore, the terms "first," "second," etc., are primarily used to distinguish between different devices, elements, or components (which may or may not be of the same type and configuration), and are not intended to indicate or imply the relative importance or quantity of the devices, elements, or components indicated. Unless otherwise specified, "plurality" means two or more.

[0026] The technical solution of the present application will be further described below with reference to the embodiments and drawings.

[0027] For energy storage device products (such as lithium batteries), in addition to the positive and negative electrodes having a significant impact on the performance of the energy storage device products, the electrolyte also has a significant impact. The relevant technology not only requires a lot of time and the use of a large number of reagents and consumables to prepare the formula during the development process of the electrolyte, but also requires a lot of performance testing to confirm whether the formula meets the requirements. However, even with this kind of exploratory formula development with a long cycle, high time consumption, and many consumables, the results are often highly uncertain, making it difficult to ensure that the developed electrolyte has high electrical performance and process performance, and a reasonable production cost. Therefore, the practice of the relevant technology is to make appropriate trade-offs between the three factors of the electrolyte's electrical performance, process performance, and production cost, that is, to meet the needs by developing an electrolyte with relatively suitable electrical performance, process performance that can also meet production requirements, and production costs that are not too high. However, this leads to a clear bottleneck in the improvement of the electrolyte's electrical performance indicators, making it difficult to further improve the electrical performance while meeting process performance and production costs, which in turn makes it difficult to further improve the electrical performance of the energy storage device.

[0028] Taking the rate charge and discharge characteristics of energy storage devices as an example, if the conductivity of the electrolyte is increased by increasing the lithium salt concentration, thereby improving the rate charge and discharge characteristics of the energy storage device, then as the lithium salt concentration increases, not only will the conductivity increase, but the viscosity of the electrolyte will also increase. When the viscosity of the electrolyte increases, on the one hand, it will affect the process performance of the electrolyte, making the injection effect and the infiltration effect worse. On the other hand, when the viscosity of the electrolyte increases to a certain extent, it will cause the conductivity to decrease. It can be seen that the electrical properties and process performance of the electrolyte are two properties that are difficult to balance. In addition, increasing the lithium salt concentration will also increase the cost of the electrolyte due to the increase in the amount of lithium salt used.

[0029] Based on the above analysis, it can be seen that it is difficult for relevant technologies to quickly develop a more ideal electrolyte in a short time and with less consumables, so that the electrolyte can improve electrical performance while also having appropriate process performance and production costs.

[0030] The embodiments of the present application propose an electrolyte for an energy storage device, an energy storage device, an energy storage module, and electrical equipment. By creatively exploring the electrolyte conductivity, density, viscosity, lithium salt concentration within a specific parameter range and the specific relationships that need to be satisfied therebetween, an electrolyte with more reasonable performance can be developed more quickly, so that while improving electrical performance, it still ensures good process performance and production costs.

[0031] In a first aspect, an embodiment of the present application provides an electrolyte for an energy storage device, wherein the electrolyte satisfies the following relationship: 23.1≤-15×c 2 +28.53×c+0.64×μ+16.47×ρ-σ≤25.3, where

[0032] c is the concentration of the lithium salt in the electrolyte, and the concentration of the lithium salt is 0.6 mol / L to 1 mol / L;

[0033] μ is the viscosity of the electrolyte at 25° C., and the viscosity of the electrolyte at 25° C. is 1.6 mPa.s to 3.0 mPa.s;

[0034] ρ is the density of the electrolyte, which is 1.1 g / cm 3 ~1.3g / cm 3 ;

[0035] σ is the value of the conductivity of the electrolyte, and the conductivity is 8 ms / cm to 12 ms / cm.

[0036] It should be noted that, in the calculation process of the above relationship, only the values ​​of lithium salt concentration, viscosity, density and conductivity are selected for calculation, and physical units are not involved in the calculation.

[0037] The embodiments of the present application control the conductivity, viscosity, density and lithium salt concentration of the electrolyte to meet the above-mentioned numerical ranges and relationship expressions, and can quickly develop an electrolyte with ideal performance in a short time and with low material consumption, thereby ensuring that the electrolyte can improve electrical performance while also having good process performance and reasonable production costs.

[0038] On the one hand, according to the preset electrolyte viscosity, density and lithium salt concentration values, the conductivity value of the electrolyte can be quickly determined. Since conductivity has an important influence on the internal resistance and rate characteristics of the energy storage device, it is possible to know whether the developed electrolyte has better electrical properties based on the determined conductivity value, thereby quickly judging in advance whether the electrolyte developed according to the above electrolyte viscosity, density, conductivity and lithium salt concentration values ​​has good performance. In other words, unlike the technical solution in the related art that requires first trying the formula and then testing the performance to judge the rationality of the formula development, the embodiment of the present application can be determined by 23.1≤-15×c 2+28.53×c+0.64×μ+16.47×ρ-σ≤25.3This relationship can first quickly determine whether the electrolyte developed based on specific electrolyte viscosity, density, conductivity and lithium salt concentration values ​​has better electrical properties, and then determine the specific formula for the electrolyte with better performance. For electrolytes that do not have better performance prospects, there is no need to spend time and reagents on formula development, so that electrolytes with reasonable performance can be developed more quickly and more preparedly.

[0039] Specifically, according to the preset viscosity, density and lithium salt concentration values ​​of the electrolyte, the conductivity is calculated in combination with the above relationship. After quickly determining that the electrolyte developed according to the above four parameter values ​​has good performance, the lithium salt concentration required for the electrolyte formula can be determined first, and then the type of lithium salt can be determined and the corresponding lithium salt concentration can be calculated. Then, by selecting suitable organic solvents and additives, an electrolyte formula that meets the above conductivity, density and viscosity requirements can be obtained.

[0040] On the other hand, since the viscosity, density, conductivity and lithium salt concentration values ​​of the developed electrolyte are all within the range of the embodiments of the present application, it can be ensured that the developed electrolyte not only has better electrical properties, but also has good process performance and reasonable production cost.

[0041] The concentration of the lithium salt in the electrolyte is in the range of 0.6 mol / L to 1 mol / L, including any value within this numerical range, such as the concentration of the lithium salt is 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L or 1 mol / L. The above range of lithium salt concentration is conducive to ensuring that the conductivity and viscosity of the entire electrolyte formula reach the corresponding range. The lithium salt concentration is neither too low, resulting in low conductivity, nor too high, resulting in excessive electrolyte viscosity, lithium salt crystallization, and thus reduced conductivity. In addition, since the above lithium salt concentration is not high, there is no need to use a large amount of expensive lithium salt when developing the formula, which is conducive to further reducing production costs.

[0042] The viscosity range of the electrolyte is controlled to be 1.6mPa.s to 3.0mPa.s at 25°C, which includes any point value within this numerical range. For example, the viscosity of the electrolyte at 25°C is 1.6mPa.s, 1.8mPa.s, 2mPa.s, 2.2mPa.s, 2.5mPa.s, 2.8mPa.s or 3mPa.s. Within this viscosity range, the electrolyte has good fluidity, which helps to reduce the contact angle between the electrolyte and the positive and negative electrodes, so that the electrolyte exhibits better wetting performance on the positive and negative electrodes. Not only that, when the electrolyte is injected into the battery cell of the energy storage device, this viscosity range of the electrolyte is also conducive to reducing the occurrence of spraying, overflowing and other phenomena, reflecting the good process performance of the electrolyte.

[0043] It can be understood that the process performance of the electrolyte in the embodiment of the present application refers to the performance characteristics exhibited during the production process of the energy storage device using the electrolyte. For example, the process performance of the electrolyte can be reflected in the injection effect of the electrolyte into the battery cell, the wetting ability of the electrolyte on the electrode sheet, etc.

[0044] The density range of the electrolyte is 1.1g / cm 3 ~1.3g / cm 3 Including any point value within this numerical range, for example, the density of the electrolyte is 1.1g / cm 3 , 1.15g / cm 3 , 1.2g / cm 3 , 1.25g / cm 3 or 1.3 g / cm 3 . Under the conditions of this density range, there is no need to add more additional electrolyte, that is, the filling effect of the electrolyte into the battery cell can be guaranteed, ensuring the full infiltration of the electrolyte into the electrode sheet, thereby improving the electrical performance of the energy storage device in terms of capacity and cycle life. Specifically, when the amount of electrolyte injected into the battery cell is too small, some areas of the battery cell will often not be filled with electrolyte, resulting in black spots on the electrode sheet, insufficient utilization of the battery cell capacity, and rapid capacity decay during the battery cycle charge and discharge. Although the above problems can be improved by increasing the injection amount of the electrolyte, since the electrolyte is more expensive, the more the amount added, the higher the cost of the energy storage device. The density of the electrolyte in the embodiment of the present application is relatively lower, that is, when the same mass of electrolyte is added, the electrolyte in the embodiment of the present application has a larger volume, and its filling area in the battery cell is larger, which can fill the internal space of the battery cell more fully. In this way, without increasing the amount of electrolyte and production costs, the electrode sheets can still be fully immersed in the electrolyte, which not only helps to fully utilize the capacity of the electrode sheets, but also helps to improve the battery cycle charge and discharge life.

[0045] The electrolyte conductivity ranges from 8 ms / cm to 12.0 ms / cm, including any value within this numerical range. For example, the electrolyte conductivity is 8 ms / cm, 9 ms / cm, 10 ms / cm, 11 ms / cm, or 12 ms / cm. Within this conductivity range, the energy storage device is advantageously provided with good rate charge and discharge performance.

[0046] When the conductivity is greater than or equal to 9 ms / cm, it is considered to be relatively high, which has a positive impact on the rate charge and discharge performance of the energy storage device. However, when the conductivity is less than 9 ms / cm, the electrolyte of the embodiment of the present application can also be quickly developed to obtain an electrolyte with better electrical performance by regulating the relationship between the viscosity, density, conductivity and lithium salt concentration of the electrolyte.

[0047] As a preferred embodiment, the electrolyte in the embodiment of the present application has a conductivity of 8ms / cm to 8.9ms / cm. Compared with a conductivity of 9ms / cm or above, 8ms / cm to 8.9ms / cm is a case of lower conductivity. Unlike the related art where low electrolyte conductivity leads to poor electrical performance of the electrolyte, although the embodiment of the present application adopts a lower conductivity, it is still possible to obtain an electrolyte with excellent electrical performance, reasonable process performance and production cost.

[0048] Furthermore, the electrolyte comprises the above-mentioned lithium salt, an organic solvent, and an additive, wherein the mass percentage of the additive in the electrolyte is 1wt% to 8wt%, and the mass percentage of the organic solvent in the electrolyte is 50wt% to 95wt%. By controlling the amount of the organic solvent and additive within the above-mentioned range, combined with the quickly confirmed lithium salt concentration, the required amount of each component of the electrolyte can be quickly and reasonably determined, which is conducive to better controlling the corresponding performance parameters such as electrolyte viscosity and density, so that the viscosity of the electrolyte at 25°C meets 1.6mPa.s to 3.0mPa.s and the density of the electrolyte meets 1.1g / cm 3 ~1.3g / cm 3 .

[0049] The mass percentage of the additive in the electrolyte is 1 wt% to 8 wt%, including any value within this numerical range, for example, the mass percentage of the additive in the electrolyte is 1 wt%, 2 wt%, 3 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt%, or 8 wt%. The mass percentage of the organic solvent in the electrolyte is 50 wt% to 95 wt%, including any value within this numerical range, for example, the mass percentage of the organic solvent in the electrolyte is 50 wt%, 60 wt%, 65 wt%, 70 wt%, 80 wt%, 90 wt%, or 95 wt%.

[0050] The materials of each component in the electrolyte are described below.

[0051] Optionally, the lithium salt includes at least one of lithium hexafluorophosphate, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium tetrafluoroborate, lithium bis(oxalatoborate) or lithium difluorooxalatoborate.

[0052] Optionally, the organic solvent comprises a cyclic organic solvent and / or a linear organic solvent;

[0053] When the organic solvent includes the cyclic organic solvent, the cyclic organic solvent includes at least one of ethylene carbonate, propylene carbonate, dioxolane or sulfolane;

[0054] When the organic solvent includes the linear organic solvent, the linear organic solvent includes at least one of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethyl acetate, methyl acetate, propyl propionate, ethyl butyrate, ethyl propionate, 1,2-dimethoxyethane, diethylene glycol dimethyl ether, tetramethylsilane or adiponitrile.

[0055] Preferably, the organic solvent includes the cyclic organic solvent and the linear organic solvent, and the mass ratio of the cyclic organic solvent to the linear organic solvent is 0.05-2.

[0056] Optionally, the additive includes at least one of vinylene carbonate, fluoroethylene carbonate, 1,3-propane sultone, vinyl sulfate, tris(trimethylsilyl)phosphate, tris(trimethylsilyl)borate, methylene disulfonate, vinyl ethylene carbonate, lithium bis(oxalatoborate), lithium difluorooxalatoborate or lithium difluorophosphate.

[0057] The electrolyte of the embodiment of the present application adopts the above-mentioned component materials, which makes the electrolyte more versatile. While meeting the requirements of better electrical performance, stable process performance and low cost, it is more adaptable to a variety of different positive and negative electrode material systems.

[0058] In a second aspect, embodiments of the present application further provide an energy storage device, comprising the electrolyte described in the first aspect, which may be a lithium battery. The energy storage device further comprises a positive electrode sheet, a negative electrode sheet, and a separator, wherein the separator is disposed between the positive electrode sheet and the negative electrode sheet. The positive electrode sheet, the negative electrode sheet, and the separator are assembled to form a battery cell, and the electrolyte is injected into the battery cell to soak the positive and negative electrode sheets.

[0059] Optionally, the energy storage device is a square shell energy storage device, a cylindrical energy storage device or a soft package energy storage device.

[0060] In a third aspect, embodiments of the present application further provide an energy storage module comprising a housing and an energy storage device as described in the second aspect, disposed within the housing. Multiple energy storage devices are housed within the housing, and the multiple energy storage devices are connected in at least one of series and parallel configurations. The energy storage module secures and protects the energy storage devices.

[0061] Fourthly, embodiments of the present application further provide an electrical device, which can be an energy storage base station, an electric vehicle, a ship, a bus, or the like. The electrical device includes an electrical device body and an energy storage device according to the second aspect disposed within the electrical device body, the energy storage device being configured to supply power to the electrical device body. The electrical device body includes a positive electrode and a negative electrode. The positive electrode sheet of the energy storage device is electrically connected to the positive electrode of the device, and the negative electrode sheet is electrically connected to the negative electrode of the device.

[0062] The electrolyte, energy storage device, energy storage module, and electrical equipment of the embodiments of the present application are further described below in conjunction with more specific embodiments.

[0063] Example 1

[0064] This embodiment provides an electrolyte for an energy storage device, comprising a lithium salt, an organic solvent, and an additive. The lithium salt is lithium hexafluorophosphate with a concentration c of 0.6 mol / L; the organic solvent comprises ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate in a mass ratio of 5:2:3; and the additives are vinylene carbonate and fluoroethylene carbonate, with the mass fraction of vinylene carbonate in the electrolyte being 3% by weight and the mass fraction of fluoroethylene carbonate in the electrolyte being 1.5%.

[0065] The electrolyte solution was measured to have a viscosity of 1.74 mPa.s and a density of 1.2 g / cm at 25°C. 3 , the conductivity σ is 8.06ms / cm. The electrolyte satisfies the following relationship: 23.1≤-15×c 2 +28.53×c+0.64×μ+16.47×ρ-σ≤25.3.

[0066] Example 2

[0067] The only difference between this embodiment and embodiment 1 is the concentration of the lithium salt. In this embodiment, the lithium salt is lithium hexafluorophosphate with a concentration c of 0.7 mol / L. The viscosity μ of the electrolyte at 25°C is measured to be 1.82 mPa·s, and the density ρ is 1.19 g / cm 3 , the conductivity σ is 9.267ms / cm. The electrolyte satisfies the following relationship: 23.1≤-15×c 2 +28.53×c+0.64×μ+16.47×ρ-σ≤25.3.

[0068] Example 3

[0069] The only difference between this embodiment and embodiment 1 is the concentration of the lithium salt. In this embodiment, the lithium salt is lithium hexafluorophosphate with a concentration c of 0.8 mol / L. The viscosity μ of the electrolyte at 25°C is measured to be 1.91 mPa·s, and the density ρ is 1.2 g / cm 3 , the conductivity σ is 9.974ms / cm. The electrolyte satisfies the following relationship: 23.1≤-15×c 2 +28.53×c+0.64×μ+16.47×ρ-σ≤25.3.

[0070] Example 4

[0071] The only difference between this embodiment and embodiment 1 is the concentration of the lithium salt. In this embodiment, the lithium salt is lithium hexafluorophosphate with a concentration c of 0.9 mol / L. The viscosity μ of the electrolyte at 25°C is measured to be 2.25 mPa·s, and the density ρ is 1.2 g / cm 3 , the conductivity σ is 10.57ms / cm. The electrolyte satisfies the following relationship: 23.1≤-15×c 2 +28.53×c+0.64×μ+16.47×ρ-σ≤25.3.

[0072] Example 5

[0073] The only difference between this embodiment and embodiment 1 is the concentration of the lithium salt. In this embodiment, the lithium salt is lithium hexafluorophosphate with a concentration c of 1.0 mol / L. The viscosity μ of the electrolyte at 25°C is measured to be 2.55 mPa·s, and the density ρ is 1.22 g / cm 3 , the conductivity σ is 10.94ms / cm. The electrolyte satisfies the following relationship: 23.1≤-15×c 2 +28.53×c+0.64×μ+16.47×ρ-σ≤25.3.

[0074] Example 6

[0075] This embodiment provides an electrolyte for an energy storage device, comprising a lithium salt, an organic solvent, and an additive. The lithium salt is lithium hexafluorophosphate with a concentration c of 0.8 mol / L; the organic solvent is composed of ethylene carbonate and ethyl methyl carbonate in a mass ratio of 2:8; and the additives are vinylene carbonate and fluoroethylene carbonate, with the mass fraction of vinylene carbonate in the electrolyte being 3% by weight and the mass fraction of fluoroethylene carbonate in the electrolyte being 1.5%.

[0076] The electrolyte solution was measured to have a viscosity of 2.1 mPa.s and a density of 1.17 g / cm at 25°C. 3 , the conductivity σ is 10.44ms / cm. The electrolyte satisfies the following relationship: 23.1≤-15×c 2 +28.53×c+0.64×μ+16.47×ρ-σ≤25.3.

[0077] Example 7

[0078] This embodiment provides an electrolyte for an energy storage device, comprising a lithium salt, an organic solvent, and an additive. The lithium salt has a concentration c of 1 mol / L and specifically comprises 0.9 mol / L of lithium hexafluorophosphate and 0.1 mol / L of lithium bis(fluorosulfonyl)imide; the organic solvent comprises ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate in a mass ratio of 3:4:3; and the additives are vinylene carbonate and fluoroethylene carbonate, with the mass fraction of vinylene carbonate in the electrolyte being 3% by weight and the mass fraction of fluoroethylene carbonate being 1.5% by weight.

[0079] The electrolyte solution was measured to have a viscosity of 2.4 mPa.s and a density of 1.19 g / cm at 25°C. 3 , the conductivity σ is 11.66ms / cm. The electrolyte satisfies the following relationship: 23.1≤-15×c 2 +28.53×c+0.64×μ+16.47×ρ-σ≤25.3.

[0080] Comparative Example 1

[0081] This embodiment provides an electrolyte for an energy storage device, comprising a lithium salt, an organic solvent, and an additive. The lithium salt has a concentration c of 1 mol / L and specifically comprises 0.9 mol / L of lithium hexafluorophosphate and 0.1 mol / L of lithium bis(fluorosulfonyl)imide; the organic solvent comprises ethylene carbonate and diethyl carbonate in a mass ratio of 7:3; and the additives are vinylene carbonate and fluoroethylene carbonate, with the mass fraction of vinylene carbonate in the electrolyte being 3% by weight and the mass fraction of fluoroethylene carbonate being 1.5% by weight.

[0082] The electrolyte solution was measured to have a viscosity of 4.8 mPa.s and a density of 1.25 g / cm at 25°C. 3 , the conductivity σ is 9.45ms / cm. The electrolyte does not satisfy the following relationship: 23.1≤-15×c 2 +28.53×c+0.64×μ+16.47×ρ-σ≤25.3.

[0083] Comparative Example 2

[0084] This comparative example provides an electrolyte for an energy storage device. The only difference between this comparative example and Example 6 is the organic solvent. In this comparative example, the organic solvent is composed of ethylene carbonate and ethyl methyl carbonate in a mass ratio of 1:9.

[0085] The electrolyte was measured to have a viscosity of 1.35 mPa.s and a density of 1.08 g / cm at 25°C. 3 , the conductivity σ is 4.52ms / cm. The electrolyte does not satisfy the following relationship: 23.1≤-15×c2 +28.53×c+0.64×μ+16.47×ρ-σ≤25.3.

[0086] Comparative Example 3

[0087] This comparative example provides an electrolyte for an energy storage device. The only difference between this comparative example and Example 6 is the organic solvent. In this comparative example, the organic solvent is composed of ethylene carbonate and ethyl methyl carbonate in a mass ratio of 6:4.

[0088] The electrolyte solution was measured to have a viscosity of 5.32 mPa.s and a density of 1.31 g / cm at 25°C. 3 , the conductivity σ is 5.27ms / cm. The electrolyte does not satisfy the following relationship: 23.1≤-15×c 2 +28.53×c+0.64×μ+16.47×ρ-σ≤25.3.

[0089] Comparative Example 4

[0090] This comparative example provides an electrolyte for an energy storage device. The only difference between this comparative example and Example 6 is the lithium salt concentration. The lithium salt in this comparative example is lithium hexafluorophosphate with a concentration c of 0.5 mol / L. The viscosity μ of this electrolyte at 25°C is measured to be 1.68 mPa·s, and the density ρ is 1.18 g / cm 3 , the conductivity σ is 6.75ms / cm. The electrolyte satisfies the following relationship: 23.1≤-15×c 2 +28.53×c+0.64×μ+16.47×ρ-σ≤25.3.

[0091] Comparative Example 5

[0092] This comparative example provides an electrolyte for an energy storage device. The only difference between this comparative example and Example 6 is the lithium salt concentration. The lithium salt in this comparative example is lithium hexafluorophosphate with a concentration c of 1.1 mol / L. The viscosity μ of this electrolyte at 25°C is measured to be 2.64 mPa·s, and the density ρ is 1.22 g / cm 3 , the conductivity σ is 10.34ms / cm. The electrolyte satisfies the following relationship: 23.1≤-15×c 2 +28.53×c+0.64×μ+16.47×ρ-σ≤25.3.

[0093] It should be noted that, for the electrolytes of Examples 1 to 7 and Comparative Examples 1 to 5, the conductivity was tested by a conductivity meter, the viscosity was tested by an Ubbelohde viscometer, the test environmental conditions were a temperature of 25±1°C and a humidity ≤2% (i.e., the conditions of a drying room), and the density was tested by a densitometer.

[0094] The values ​​of lithium salt concentration, electrolyte viscosity, density, and conductivity for Examples 1 to 7 and Comparative Examples 1 to 5, as well as the calculated results of the relationship, are shown in Table 1 below. When the calculated result of the relationship is between 23 and 25.3, the relationship is determined to be satisfied. When the values ​​of lithium salt concentration, electrolyte viscosity, density, and conductivity are all within the ranges specified in the embodiments of this application and satisfy the relationship, the electrolyte has excellent electrical properties, good process performance, and reasonable production costs.

[0095] Table 1 Electrolyte parameters and relationship tables of Examples 1 to 7 and Comparative Examples 1 to 5

[0096] The following is an explanation of the performance test of the electrolyte

[0097] (1) Wetting effect and injection efficiency test: The electrolytes configured in Examples 1 to 7 and Comparative Examples 1 to 5 were injected into the battery cells using vacuum and positive pressure injection methods. The injection process specifically includes: vacuuming, maintaining at -98 kPa for 60 seconds; pressurizing, maintaining at 600 kPa for 240 seconds and at -98 kPa for 60 seconds; breaking vacuum for 20 seconds. Such a process is called an injection cycle. The number of cycles required for each embodiment and comparative example to infiltrate 50% pores, 60% pores, 70% pores, and 80% pores of the battery cells was measured, and the detailed data are shown in Table 2 below.

[0098] Table 2 Wetting performance test of electrolytes of Examples 1 to 7 and Comparative Examples 1 to 5

[0099] From the results of the number of cycles required for the infiltration of each embodiment and comparative example in Table 2, it can be seen that to achieve the same proportion of infiltration effect, the lower the viscosity of the electrolyte, the fewer cycles are required, indicating that the lower the viscosity of the electrolyte, the better the infiltration effect.

[0100] In addition, the fewer cycles required to wet 80% of the pores, the higher the injection efficiency.

[0101] (2) Constant current charge and discharge tests were performed at a temperature of 25°C and a current density of 1C to measure the number of cycles and the capacity retention of the batteries using the electrolytes of Examples 1 to 3 and Comparative Example 1. The test results are shown in FIG1 . It should be noted that the four lines from top to bottom in FIG1 correspond to the cycle stability test results of Example 1, Example 2, Example 3, and Comparative Example 1, respectively.

[0102] The experimental results are described in detail below.

[0103] 1. Comparison of the experimental results from Examples 1 to 5 reveals that the viscosity and conductivity of the electrolyte both increase with increasing lithium salt concentration. However, combined with the experimental results from Comparative Example 5, it is clear that while the viscosity of the electrolyte continues to rise with increasing lithium salt concentration, the conductivity does not increase with increasing lithium salt content, but instead decreases. This suggests that there is an optimal range for lithium salt concentration in the electrolyte, and a higher concentration is not always better.

[0104] 2. By comparing the experimental results of Examples 1 to 3 and Comparative Example 1, it can be seen that although the conductivity of the electrolyte in Example 1 is the lowest, it has the best cycle stability. Although the conductivity of the electrolyte in Comparative Example 1 is between the levels of Examples 2 and 3, the viscosity of the electrolyte in Comparative Example 1 is relatively large, resulting in a sharp attenuation of the cycle capacity, and the wetting effect on the electrode sheet is also deteriorated, and the injection efficiency is poor. It can be seen that conductivity has an optimal range, and the greater the conductivity, the better. The cycle stability performance of the energy storage device is also affected by the viscosity of the electrolyte to a certain extent. In addition, Example 1 of the present application still has better cycle stability under the characteristics of low conductivity, indicating that the embodiment of the present application can obtain a low-conductivity electrolyte, which improves its electrical performance while also having good process performance and reasonable production costs.

[0105] 3. Comparing the experimental results of Examples 1 to 7 shows that as the viscosity of the electrolyte increases, the number of cycles required to wet the cell pores increases, indicating that both the wetting performance and the injection efficiency (i.e., process performance) gradually decrease. Taking into account process performance, cycle stability, and production cost, Examples 1 to 3 have better overall performance, with Example 1 achieving the best results.

[0106] Furthermore, further analysis of the experimental results of Comparative Examples 1 to 3 reveals that the viscosity of the electrolytes in Comparative Examples 1 and 3 is too high, significantly increasing the number of cycles required to wet the cell pores, demonstrating the significant impact of electrolyte viscosity on process performance. The viscosity and density of the electrolyte in Comparative Example 2 are both below the ranges of the present invention. While the process performance is good, the conductivity is too low, resulting in poor electrical performance of the electrolyte, which still fails to meet the electrolyte requirements for superior electrical performance, good process performance, and reasonable production costs.

[0107] 4. Comparison of the experimental results of Examples 1 to 7, Comparative Examples 4, and 5 reveals that the conductivity of Comparative Example 4 is too low. Although the lithium salt concentration, electrolyte density and viscosity, and the relationship all fall within the ranges specified in the present embodiments, the low conductivity still affects the rate charge and discharge characteristics of the energy storage device. In Comparative Example 5, the high lithium salt concentration and high electrolyte viscosity result in poor process performance.

[0108] The above is a detailed introduction to the electrolyte and energy storage device, energy storage module, and electrical equipment disclosed in the embodiments of the present application. Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the core idea of ​​the technical solution of the present application: At the same time, for general technical personnel in this field, based on the ideas of the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. An electrolyte, the electrolyte being used for an energy storage device, characterized in that: The electrolyte satisfies the following relationship: 23.1≤-15×c 2 +28.53×c+0.64×μ+16.47×ρ-σ≤25.3, where c is the value of the concentration of lithium salt in the electrolyte, and the concentration of lithium salt is 0.6 mol / L to 1 mol / L; μ is the value of the viscosity of the electrolyte at 25° C., and the viscosity of the electrolyte at 25° C. is 1.6 mPa.s to 3.0 mPa.s; ρ is the value of the density of the electrolyte, and the density of the electrolyte is 1.1 g / cm 3 ~1.3g / cm 3 ; σ is the value of the conductivity of the electrolyte, and the conductivity is 8 ms / cm to 12 ms / cm.

2. The electrolyte according to claim 1, characterized in that The electrical conductivity is 8 ms / cm to 8.9 ms / cm.

3. The electrolyte according to any one of claims 1 to 2, characterized in that The electrolyte further comprises an organic solvent and an additive, wherein the mass percentage of the additive in the electrolyte is 1wt% to 8wt%, and the mass percentage of the organic solvent in the electrolyte is 50wt% to 95wt%.

4. The electrolyte according to claim 3, characterized in that The lithium salt includes at least one of lithium hexafluorophosphate, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium tetrafluoroborate, lithium bis(oxalatoborate) or lithium difluorooxalatoborate.

5. The electrolyte according to claim 3, characterized in that The organic solvent includes a cyclic organic solvent and / or a linear organic solvent; When the organic solvent includes the cyclic organic solvent, the cyclic organic solvent includes at least one of ethylene carbonate, propylene carbonate, dioxolane or sulfolane; When the organic solvent includes the linear organic solvent, the linear organic solvent includes at least one of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethyl acetate, methyl acetate, propyl propionate, ethyl butyrate, ethyl propionate, 1,2-dimethoxyethane, diethylene glycol dimethyl ether, tetramethylsilane or adiponitrile.

6. The electrolyte according to claim 5, characterized in that The organic solvent includes the cyclic organic solvent and the linear organic solvent, and the mass ratio of the cyclic organic solvent to the linear organic solvent is 0.05-2.

7. The electrolyte according to claim 3, characterized in that The additive includes at least one of vinylene carbonate, fluoroethylene carbonate, 1,3-propane sultone, vinyl sulfate, tris(trimethylsilyl)phosphate, tris(trimethylsilyl)borate, methylene disulfonate, vinyl ethylene carbonate, lithium bis(oxalatoborate), lithium difluorooxalatoborate or lithium difluorophosphate.

8. An energy storage device, characterized in that: The energy storage device comprises the electrolyte according to any one of claims 1 to 7.

9. An energy storage module, characterized in that: The energy storage module includes a box body and an energy storage device as claimed in claim 8 disposed in the box body.

10. An electrical device, characterized in that: The electrical equipment comprises an electrical equipment body and an energy storage device as claimed in claim 8 disposed in the electrical equipment body, wherein the energy storage device is used to supply power to the electrical equipment body.

Citation Information

Patent Citations

  • Electrolyte, preparation method thereof, lithium ion battery and lithium ion capacitor

    CN109003835A

  • High-power and high-voltage-resistant lithium ion battery electrolyte and preparation method thereof

    CN111082142A

  • Electrolyte, preparation method thereof and electrochemical device

    CN115411369A

  • Electrolyte, battery and electric equipment