Secondary battery and electric apparatus
By using an inactive layer containing A element and a redox potential difference-driven mutual dissolution technology of B element in secondary batteries, the problem of rapid consumption of metal anodes and dendrites is solved, and the energy density and cycle stability of the battery are improved.
Patent Information
- Application Number
- PCT/CN2024/082261
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-12
- Filing Date
- 2024-03-18
- Publication Date
- 2024-10-17
AI Technical Summary
The metal negative electrode in existing lithium secondary batteries and sodium secondary batteries is prone to chemical/electrochemical reactions with the electrolyte, leading to rapid consumption, dendrite formation and battery short circuit risks. It is also difficult to form a stable solid electrolyte interface layer, affecting the battery's performance. Energy density and cycling stability.
An inactive layer containing A element is used as the negative electrode base layer, and by adjusting its specific surface area, shape structure or adding a negative electrode protective film, B element is used as the active material, and the redox potential difference drives the mutual dissolution of B element and A element to form a uniform alloy to inhibit dendrite growth and protect active materials.
It effectively inhibits the formation of metal dendrites, reduces the consumption of active materials, improves the cycle stability and energy density of the battery, and extends the service life of the battery.
Smart Images

Figure CN2024082261_17102024_PF_FP_ABST
Abstract
Description
Secondary batteries and electrical devices Technical Field
[0001] The present disclosure relates to the field of secondary batteries, and in particular to liquid, semi-solid, and solid secondary batteries and electrical devices. Background Art
[0002] Secondary batteries are essential materials for electrical energy transfer and are widely used in new energy vehicles, portable electronics, energy storage, and other fields. As the most important secondary battery currently, graphite's low theoretical specific capacity limits further increases in the energy density of lithium-ion batteries. In contrast, metal anodes offer ultra-high theoretical specific capacity and extremely low redox potentials, which are beneficial for further improving battery energy density and have become a research focus in recent years.
[0003] At present, there are still some technical problems in the direct use of metal negative electrodes in lithium secondary batteries, sodium secondary batteries, and other secondary batteries in commercial applications. Metal negative electrodes usually have high reactivity and are prone to chemical / electrochemical reactions with electrolytes, resulting in rapid consumption of the metal negative electrode and electrolyte, which reduces the coulombic efficiency of the battery. In addition, many metal ions have a directional growth trend during the reduction and deposition process, which makes the metal tend to deposit in a dendritic manner, which leads to huge volume deformation of the metal negative electrode during the cycle, making it difficult to form a stable solid electrolyte interface layer (Solid-Electrolyte Interphase, SEI) on the surface of the metal negative electrode, and there is a risk of metal dendrites piercing the isolation membrane and causing battery short circuit. In addition, the uneven deposition / stripping of metal ions causes metal dendrites to easily peel off from the metal negative electrode body, and SEI blocks the electron transmission path, resulting in loss of active material, causing the battery to continuously lose capacity and easily explode. Furthermore, the SEI formed during the cycling of the metal anode helps to prevent the mutual consumption between the metal anode and the electrolyte. However, conventional electrolytes cannot form a stable solid electrolyte interface film on the metal anode, thus failing to provide long-term, high-efficiency protection for metal anode batteries. Therefore, the industry urgently needs to develop new battery materials to address the above issues, in order to improve the energy density of secondary batteries and inhibit the occurrence of side reactions and dendrite formation during the cycling process.
[0004] In some recent methods and reports, some researchers have also considered that the intrinsic deposition pattern of metallic lithium leads to the growth of lithium dendrites, and have come up with the idea of interfering with the growth pattern of metallic lithium dendrites by co-deposition of other ions. Although lithium has the most negative redox potential, ordinary ions are difficult to co-deposit with lithium ions, but the redox potentials of sodium and lithium are relatively close. If lithium and sodium ions are present in the electrolyte at the same time, lithium ions and sodium ions are expected to co-deposit within a certain potential range, thereby breaking the intrinsic growth pattern of metallic lithium dendrites, thereby weakening or even eliminating the formation of dendrites. However, in the above reaction process, lithium and sodium elements act as active substances and reversibly participate in the charge transfer during the battery charging and discharging process. The preparation of the electrolyte is relatively complicated, and it is not easy to achieve a sustainable reaction. In addition, Chinese patent application CN107093706A discloses a method for preparing a lithium battery negative electrode, which relates to the fields of solid-state batteries and liquid batteries. This invention is intended to solve the problems of low gram-to-gram capacity, easy growth of dendrites, low initial coulombic efficiency, and low battery energy density of traditional graphite negative electrodes. The process includes: Step 1: Mixing 75% to 90% by weight of a carbon material, 5% to 20% by weight of a conductive agent, and 5% to 10% by weight of a binder in a specific ratio to form an adsorbent or porous intermediate layer; then coating the intermediate layer on a current collector to a thickness of 1μm to 70μm; Step 2: Evenly vapor-depositing a metal layer with a thickness of 1μm to 30μm on the intermediate layer; Step 3: After completing Steps 1 and 2, connecting the tab to the current collector to complete the preparation of the battery negative electrode. It is used in both solid-state and liquid-state battery fields. However, the battery negative electrode in the aforementioned patent application has the following disadvantages in terms of structure and preparation method: 1. Complex structure. To inhibit the growth of lithium dendrites, the intermediate layer of the negative electrode is required to function. As stated in paragraph 0022 of its specification, it "uses an intermediate material layer to regulate the distribution of lithium ions on the surface of the negative electrode, avoids the aggregation of lithium ions in time and space, and achieves a uniform distribution of lithium ions on the surface of the negative electrode, thereby inhibiting the appearance of lithium dendrites. The structure of the negative electrode of the lithium battery can effectively inhibit the generation of lithium dendrites." 2. It is difficult to avoid the consumption of active lithium. For lithium batteries, the negative electrode protection film (ie SEI) is repeatedly regenerated during the use of the battery. In this patent application, as an active material, the metal layer covering the surface of the intermediate material layer cannot guarantee that the negative electrode protection film does not consume lithium during the regeneration process, thereby reducing the capacity of the battery. 3. The intermediate material layer is located below the metal layer, which makes it difficult to effectively increase the specific surface area of the metal layer, increases the current density on the negative electrode surface during the battery cycle, and easily leads to excessive formation of SEI and excessive passivation of the negative electrode by SEI.
[0005] Therefore, there is an urgent need in the art to develop a new type of secondary battery that can overcome the above technical deficiencies.
[0006] Summary of the Invention
[0007] In order to solve the problems existing in existing lithium secondary batteries, sodium secondary batteries and other secondary battery technologies, the present application provides a secondary battery with a simple process, wherein a metal-containing inactive layer is used as the negative electrode base layer in the negative electrode plate, and another metal element with a redox potential lower than the at least one metal element contained in the inactive layer is used as the active material, which reversibly participates in the electrochemical reaction, and optionally by adjusting the specific surface area, shape structure of the inactive layer or adding a negative electrode protective film or a negative electrode enhancement film, it can effectively solve the problems of dendrite growth on the negative electrode plate, high complexity of the existing process, low conductivity, etc. The inactive negative electrode base layer plays the role of inhibiting dendrite growth, protecting the active material, and providing raw materials for the formation and regeneration of the negative electrode protective film, thereby reducing the consumption of active material and improving the service life of the battery.
[0008] In the present application, the active material undergoes a valence change during the charge and discharge process, and a reversible electrochemical reaction occurs. The inactive layer is a functional auxiliary material that achieves uniform deposition of active materials and eliminates dendrite growth. This functional auxiliary material is a key material for forming a negative electrode protective film (i.e., SEI) and for dynamically repairing the negative electrode protective film, and is also one of the core points of the present invention. The B element ions are reduced in the form of B element metal during charging, and the B element metal is oxidized to B element ions during discharging, so the active material is the B element. Specifically, the A element is not embedded in the positive electrode material or the positive electrode material is preferentially embedded in the B element, so the A element ions cannot be reversibly embedded in and out of the positive electrode material, that is, the A element ions cannot reversibly participate in the electrochemical reaction during the charge and discharge process of the battery, that is, they cannot reversibly participate in the charge and discharge of the battery.
[0009] The present disclosure provides a novel secondary battery and an electrical device, thereby overcoming the above technical deficiencies.
[0010] In one aspect, the present disclosure provides a secondary battery comprising a positive electrode, an electrolyte (including liquid, semi-solid, solid electrolytes, etc.) and a negative electrode, wherein:
[0011] The negative electrode plate includes a negative electrode base layer, and the negative electrode base layer includes at least one inactive layer containing element A;
[0012] The electrolyte includes B element as an active material;
[0013] Wherein, the element A is at least one of sodium, potassium, magnesium and calcium;
[0014] The B element is at least one of lithium, sodium, potassium, magnesium and calcium;
[0015] The element B is different from the element A, and the redox reaction potential of the element B is lower than that of the element A.
[0016] In a preferred embodiment, the secondary battery further comprises an A-based negative electrode protection film located on at least a portion of the surface of the negative electrode base layer.
[0017] In another preferred embodiment, the A-based negative electrode protection film can conduct B element ions; the negative electrode base layer provides a source of A element for the formation and regeneration of the negative electrode protection film during repeated charge and discharge of the secondary battery.
[0018] In another preferred embodiment, the negative electrode plate further includes a negative electrode enhancement film located on at least a portion of the surface of the A-based negative electrode protection film, wherein the components constituting the negative electrode enhancement film are substances that do not chemically react with the electrolyte; further, the components constituting the negative electrode enhancement film are substances that do not chemically react with the electrolyte, nor with the B element metal and / or the inactive layer containing the A element. The negative electrode enhancement film can effectively increase the specific surface area of the negative electrode plate, reduce the current density of the negative electrode during the charge and discharge process, improve the electrode charge and discharge capacity and compatibility with side reactions in the battery, reduce the thickness of the negative electrode protection film (SEI) film, prevent SEI from excessive passivation of the negative electrode, and inhibit the formation of metal dendrites. At the same time, the negative electrode enhancement film can reduce the excessive formation of SEI under high temperature conditions, and improve the capacity retention rate and electrochemical performance of the secondary battery at different temperatures.
[0019] In another preferred embodiment, the negative electrode plate satisfies at least one of the following conditions:
[0020] (1) The specific surface area S of the negative electrode base layer 负 Meet 0.001m 2 / g≤S 负 ≤100m 2 / g;
[0021] (2) The surface roughness R of the negative electrode base layer 负 Satisfy 0.01μm≤R 负 ≤250μm;
[0022] (3) The porosity K of the negative electrode base layer 负 Satisfy 0%≤K 负 ≤50%;
[0023] (4) The thickness d of the negative electrode base layer 负 Satisfy: 2μm≤d 负 ≤500μm;
[0024] (5) The surface density C of the negative electrode base layer 负Meets: 0.2mg / cm 2 ≤C 负 ≤50mg / cm 2 ;
[0025] (6) Median particle size D of the particles of the negative electrode base layer 50负 Satisfy 0.05μm≤D 50负 ≤200μm;
[0026] (7) The negative electrode base layer has a striped structure, and the minimum dimension of the stripes is in the range of 0.05 μm to 200 μm;
[0027] (8) The atomic percentage of the A element in the negative electrode base layer is between 10% and 100%; or
[0028] (9) The mass percentage of the B element in the negative electrode base layer is between 0% and 70%.
[0029] In another preferred embodiment, the inactive layer containing element A and element B include any one of the following combinations: magnesium inactive layer and sodium element; magnesium inactive layer and lithium element; magnesium inactive layer and potassium element; magnesium inactive layer and calcium element; sodium inactive layer and potassium element; sodium inactive layer and lithium element; sodium inactive layer and calcium element; calcium inactive layer and potassium element; calcium inactive layer and lithium element; or potassium inactive layer and lithium element.
[0030] In another preferred embodiment, the secondary battery further includes a separator, and a second negative electrode reinforcement film disposed on at least a portion of the separator.
[0031] In another preferred embodiment, the separator itself is at least partially the second negative electrode reinforcement film.
[0032] In another preferred embodiment, the inactive layer containing element A is in the form of a lamellar structure, a stripe structure, a three-dimensional structure, and / or a granular structure.
[0033] In another preferred embodiment, the negative electrode base layer further comprises element B dissolved in at least one inactive layer containing element A, and the amount of element B is 0-70% by mass based on the total mass of the negative electrode base layer.
[0034] In another preferred embodiment, the active material of the positive electrode plate does not undergo a reversible electrochemical reaction with the ions of element A or preferentially undergoes a reversible electrochemical reaction with the ions of element B; preferably, the active material of the positive electrode plate is a polyanion salt type, a metal oxide type or a compound type.
[0035] In another preferred embodiment, the electrolyte comprises at least one anion selected from fluoride-containing anions.
[0036] In another preferred embodiment, the electrolyte comprises at least one anion selected from at least one of bis(fluorosulfonyl)imide, hexafluorophosphate, bis(trifluoromethanesulfonyl)imide, difluorooxalatoborate, tetrafluoroborate, hexafluoroarsenate, and difluorophosphate.
[0037] In another preferred embodiment, the solvent of the electrolyte is selected from at least one of ether compounds, acetal compounds and ketal compounds.
[0038] In another preferred embodiment, the concentration of the electrolyte is in the range of 0.5 mol / L to 7 mol / L.
[0039] In another aspect, the present disclosure provides an electric device including the secondary battery. Beneficial effects:
[0040] Compared with the prior art, the present application relies on an inactive negative electrode base layer containing element A (for example, a metallic sodium layer) as an inactive material layer to inhibit the growth of metal dendrites (for example, metallic lithium dendrites) of the active material B element, thereby protecting the active B element and reducing the consumption of the B element. The process is simple, the structure is simple, and the time consumption is short. The regeneration of the A-based negative electrode protective film (for example, a sodium-based negative electrode protective film) reduces the consumption of the active B element (for example, lithium) by consuming the A element (for example, sodium), and can further eliminate the formation of dendrites. At the same time, the A-based negative electrode protective film can further enhance the mutual solubility of the A element metal and the B element metal while improving the ionic conductivity of the active material. The negative electrode base layer containing the inactive layer of element A provides a source of element A for the regeneration of the A-based negative electrode protective film, reducing the consumption of the active material element B in the secondary battery; moreover, the negative electrode reinforcement film can increase the specific surface area of the negative electrode plate, effectively reducing the current density on the negative electrode surface during the battery cycle, thereby inhibiting the excessive passivation of the negative electrode plate by SEI, and optimizing the battery's capacity retention rate, rate performance and cycle stability. In addition, unlike the mechanism in the prior art that uses two or more metal elements as active materials to reversibly participate in the battery charging and discharging process and inhibit the formation of metal dendrites, the element A in this application does not participate in the charge transfer during the secondary battery charging and discharging process as an active material, and will not reversibly change its valence state during the battery charging and discharging process. The present invention uses cations of a single metal as a carrier, which is beneficial to reducing the manufacturing, use and management costs of the battery. The element A ions cannot be embedded in the positive electrode material or the positive electrode material preferentially embeds the element B ions. Therefore, the element A ions cannot be reversibly embedded in and out of the positive electrode material, that is, the element A ions cannot reversibly gain or lose electrons during the battery charging and discharging process. The negative electrode base layer containing the inactive layer of element A eliminates element B metal dendrites through the mechanism of the galvanic cell and the formation of a BA alloy. The A-based negative electrode protective film further eliminates dendrites. The negative electrode base layer containing the inactive layer of element A also provides a source of element A for the regeneration of the A-based negative electrode protective film, reducing the consumption of the active material element B in the secondary battery.
[0041] These and other features and advantages will become apparent from reading the following detailed description and referring to the associated drawings.It is to be understood that both the foregoing general description and the following detailed description are illustrative only and are not restrictive of the aspects claimed. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 is a schematic diagram of the structure of a negative electrode sheet in a specific embodiment of the present application, which includes at least one layer of layered A element metal or A element alloy inactive material as the negative electrode base layer, and at least a portion of the negative electrode reinforcement film layer is embedded in the A-based negative electrode protection layer and / or the negative electrode base layer.
[0043] FIG2 is a SEM image of the negative electrode base layer after the battery cycle is completed in Example 3 of the present application.
[0044] FIG3 is a SEM image of the negative electrode base layer in Comparative Example 4 of the present application after the battery cycle is completed. DETAILED DESCRIPTION
[0045] The present application is described in detail below with reference to the accompanying drawings, and the features of the present application will be further revealed in the following specific description.
[0046] " Scope " disclosed herein is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a scope with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for a particular parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0047] In this application, unless otherwise specified, all embodiments and preferred embodiments mentioned herein can be combined with each other to form a new technical solution. In this application, unless otherwise specified, all technical features and preferred features mentioned herein can be combined with each other to form a new technical solution.
[0048] In this application, unless otherwise specified, the terms "include" and "comprising" used herein may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.
[0049] In the description herein, unless otherwise indicated, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied by any of the following conditions: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0050] It should be understood that, in the description of the present invention, the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, features defined as "first", "second", etc. may explicitly or implicitly include one or more of such features. In the description of the present invention, unless otherwise specified, "multiple" means two or more.
[0051] It should be noted that, in the description of the present invention, unless otherwise expressly specified or limited, the terms "disposed," "connected," and "connected" should be understood in a broad sense. For example, they may refer to fixed connections, detachable connections, or integral connections; mechanical connections or electrical connections; direct connections or indirect connections through an intermediate medium; and internal connections between two components. Those skilled in the art will understand the specific meanings of the above terms in the present invention based on specific circumstances.
[0052] In order to solve the problems of dendrite formation and active material consumption in the charge and discharge cycle of the metal negative electrode in the prior art, while maintaining the high energy density of the battery, the present disclosure provides a negative electrode plate with an inactive layer of metal A or element A alloy as the negative electrode base layer. When the redox reaction potential of element B is lower than that of element A, the negative electrode base layer of metal A or element A alloy can eliminate the metal dendrites of element B deposited on its surface. The negative electrode base layer containing element A is the source of element A in the negative electrode protective film. The negative electrode base layer is an inactive layer. By participating in the formation and regeneration of the negative electrode protective film, it can reduce the consumption of active element B and has the function of protecting element B. Active metals have a direct impact on the battery capacity and reversibly participate in the transfer of charge during the battery charge and discharge process. Inactive metals have no direct impact on the battery capacity and cannot reversibly participate in the electrochemical reaction during the battery charge and discharge process.
[0053] Because the redox reaction potential of element B is lower than that of element A, when element B metal deposits on the surface of the inactive layer containing element A in the form of dendrites, the dendrites and the inactive layer locally form a galvanic cell, allowing the element B metal in the dendrites to dissolve as ions and redeposit on the surface of the inactive layer containing element A, where it gains electrons and is reduced. Furthermore, the high degree of mutual solubility between element B and element A causes the two layers to diffuse and fuse, forming a uniform alloy. The ultimate result is that when element B metal is deposited on the surface of the inactive layer containing element A, no element B metal dendrites are formed.
[0054] In the present disclosure, metal dendrites are eliminated through the principle of primary cells, and the possibility of metal dendrite formation is eliminated from the principle level. The present disclosure adopts an inactive layer containing element A metal or element A alloy as the negative electrode base layer, and element B is used as the active material. When element B ions are deposited on the surface of the inactive layer containing element A in the form of dendrites, element B metal dendrites and element A inactive layer form a primary cell in a local area. The redox reaction potential of element B is lower than that of element A. Driven by the redox reaction potential difference between element A and element B, element B metal dendrites are dissolved in the form of element B ions and obtain electrons on the surface of the inactive layer containing element A to be reduced and deposited. Element A metal and element B metal are mutually soluble. Element B metal deposited on the surface of element A metal or element A alloy can rapidly diffuse and fuse with the inactive layer containing element A. The final result is: when metal B is deposited on the surface of the inactive layer containing element A, no element B metal dendrites are generated. Unlike the prior art, which employs two or more metal ions as charge carriers to suppress metal dendrite formation, the present disclosure employs an element A ion that does not act as a charge carrier but reversibly participates in charge transfer during battery charging and discharging. Element A eliminates element B metal dendrites through the mechanism of the primary cell and the formation of a BA alloy. The present invention utilizes a single metal cation as a charge carrier, which helps reduce the manufacturing, use, and management costs of the battery.
[0055] In a first aspect of the present disclosure, a secondary battery is provided, comprising a positive electrode sheet, an electrolyte, and a negative electrode sheet, wherein:
[0056] The negative electrode plate includes a negative electrode base layer, and the negative electrode base layer includes at least one inactive layer containing element A;
[0057] The electrolyte includes B element as an active material;
[0058] Wherein, the element A is at least one of sodium, potassium, magnesium and calcium;
[0059] The B element is at least one of lithium, sodium, potassium, magnesium and calcium;
[0060] The element B is different from the element A, and the redox reaction potential of the element B is lower than that of the element A.
[0061] In the present disclosure, the secondary battery further includes an A-based negative electrode protection film located on at least a portion of the surface of the negative electrode base layer.
[0062] In the present disclosure, the A-based negative electrode protective film can conduct element B ions and further enhance the mutual solubility of element A metal and element B metal. The negative electrode base layer containing the inactive layer of element A provides a source of element A for the formation and regeneration of the negative electrode protective film during the battery charge and discharge process.
[0063] In the present disclosure, the negative electrode plate further includes a negative electrode reinforcement film located on at least a portion of the surface of the A-based negative electrode protection film.
[0064] In the present disclosure, the negative electrode of the secondary battery should also meet at least one of the following conditions:
[0065] (i) Specific surface area S of the negative electrode base layer 负 Meet 0.00lm 2 / g≤S 负 ≤100m 2 / g, preferably 0.01m 2 / g≤S 负 ≤50m 2 / g,0.1m 2 / g ≤S 负 ≤30m 2 / g,1m 2 / g≤S 负 ≤10m 2 / g or any numerical range consisting of the end values of the above range; the specific surface area S 负 When controlled within the above range, the process of element B dissolving into the negative electrode base layer can be facilitated, which is conducive to the rapid integration of element B in the negative electrode base layer and improves the high-current charge and discharge performance of the secondary battery. In addition, a higher specific surface area is conducive to reducing the actual current density of the negative electrode during the battery cycle, reducing the thickness of the SEI, preventing excessive passivation of the negative electrode by the SEI, improving the fault tolerance of the negative electrode during production, manufacturing, and use, and optimizing the battery's capacity retention, rate performance, and cycle stability.
[0066] (ii) Surface roughness R of the negative electrode base layer 负 Satisfy 0.01μm≤R 负 ≤250μm, preferably 5μm≤R 负≤50μm; higher roughness is beneficial to increase the specific surface area of the negative electrode, reduce the actual current density of the negative electrode sheet, and prevent excessive passivation of the negative electrode by SEI; or
[0067] (iii) Porosity K of the negative electrode base layer 负 Satisfy 0%≤K 负 ≤50%, 5% <K 负 ≤40%, 10% <K 负 ≤30%, 20% <K 负 ≤25% or any numerical range consisting of the above range, preferably 0% <K 负 ≤30%. A higher porosity is beneficial to increasing the specific surface area of the negative electrode, promoting the diffusion of electrolytes and ions, improving the rate performance of the battery, preventing excessive passivation of the negative electrode by SEI, and better inhibiting the formation of metal dendrites.
[0068] In the present disclosure, the surface density C of the negative electrode base layer is 负 Meets: 0.2mg / cm 2 ≤C 负 ≤50mg / cm 2 , 1mg / cm 2 ≤C 负 ≤40mg / cm 2 , 4mg / cm 2 ≤C 负 ≤25mg / cm 2 , 7mg / cm 2 ≤C 负 ≤10mg / cm 2 Or any numerical range consisting of the end values of the above range, preferably 1 mg / cm 2 ≤C 负 ≤10mg / cm 2 ; C 负 is the surface density of the negative electrode substrate, in mg / cm 2 .
[0069] In the present disclosure, the surface density of the negative electrode substrate layer needs to be controlled within the range of 0.2 to 50 mg / cm 2 If the surface density is within the above range, the negative electrode substrate layer cannot effectively suppress the formation of B element metal dendrites. If the surface density is too high, the thickness of the negative electrode substrate layer increases, and the distance and resistance of ion diffusion increase, resulting in an increase in battery impedance during charging and discharging, thereby reducing the fast charging capability and the energy density of the battery cell. Controlling the surface density of the negative electrode substrate layer within the above range can improve the fast charging capability of the battery, suppress the formation of B element metal dendrites, and ensure that the battery energy density is not too low. 负It can be adjusted mainly by controlling the coating machine parameters. For example, when using extrusion coating, the coating gap, slit gap, flow channel width, flow rate (pump speed), coating speed, etc. can be controlled to control the surface density.
[0070] In the present disclosure, the thickness d of the negative electrode base layer is 负 Satisfy: 2μm≤d 负 ≤500μm、10μm≤d 负 ≤400μm、20μm≤d 负 ≤250μm、50μm≤d 负 ≤100μm or any numerical range consisting of the end values of the above range, preferably 10μm≤d 负 ≤100μm, where d 负 is the thickness of the negative electrode base layer, in μm.
[0071] In the present disclosure, the A element metal particles are in the form of nanoparticles or micron particles, and the median particle size D 50负 Satisfy 0.05μm≤D 50负 ≤200μm、0.5μm≤D 50负 ≤150μm、1μm≤D 50负 ≤100μm、10μm≤D 50负 ≤50μm or any numerical range consisting of the end values of the above range, preferably 1μm≤D 50负 ≤100μm; D 50负 The median diameter of the particles constituting the negative electrode base layer is expressed in μm.
[0072] In the present disclosure, smaller A element metal particles can increase the specific surface area of the negative electrode base layer, promote the fusion of A element metal and B element metal, thereby further reducing the probability of forming B element metal dendrites. If the particle size of the A element metal particles is too large, the diffusion path of the B element in the A element metal particles becomes longer, the resistance to the escape of the B element increases, and the A element metal particles are easily broken, resulting in an increase in internal resistance. The smaller the particle size of the A element metal particles, the smaller the diffusion distance of the B element when it is embedded in the negative electrode, and the easier it is to embed. Moreover, the smaller the A element metal particles, the more channels there are for the embedding and escape of the B element, which is more conducive to increasing the speed of fusion of the A element metal and the B element metal. Under high-rate charge and discharge conditions, the voltage hysteresis is smaller, that is, the higher the high current charge and discharge performance is. However, if the particle size of the A element metal particles is too small, the specific surface area of the negative electrode base layer in contact with the electrolyte is too large, and the SEI film formed during the first charge and discharge process consumes more A element and electrolyte, which is likely to cause greater irreversible capacity loss.
[0073] In the present disclosure, the inactive layer containing element A and element B include any one of the following combinations: magnesium inactive layer and sodium element, magnesium inactive layer and lithium element, magnesium inactive layer and potassium element, magnesium inactive layer and calcium element, sodium inactive layer and potassium element, sodium inactive layer and lithium element, sodium inactive layer and calcium element, calcium inactive layer and potassium element, calcium inactive layer and lithium element, or potassium inactive layer and lithium element.
[0074] In the present disclosure, the secondary battery further includes a separator and a second negative electrode reinforcement film disposed on at least a portion of the separator. The second negative electrode reinforcement film can further increase the specific surface area of the inactive layer containing element A, further improving the fusion rate of element A metal and element B metal, thereby further preventing dendrite growth.
[0075] In the present disclosure, the separator itself is at least partially the second negative electrode reinforcement film.
[0076] In the present disclosure, the negative electrode enhancement film is a substance that does not chemically react with the electrolyte. Preferably, the negative electrode enhancement film can further be a substance that does not chemically react with the electrolyte, the B element metal, and the A-containing element inactive layer, including at least one component selected from a non-metallic element, an oxide (e.g., aluminum oxide), a fluoride (e.g., sodium fluoride), a carbide (e.g., tungsten carbide), a carbon material (e.g., carbon nanotubes), a nitride (e.g., silicon nitride), and a silicide (e.g., titanium silicide), and is at least partially embedded in the inactive layer. Preferably, the negative electrode enhancement film is composed of sodium fluoride, lithium fluoride, aluminum oxide, boron nitride, carbon nanotubes, carbon black, or a combination thereof.
[0077] In the present disclosure, the negative electrode reinforcement film may be compacted above the negative electrode base layer (or facing the positive electrode sheet) or below the negative electrode base layer (or facing away from the positive electrode sheet).
[0078] In the present disclosure, the negative electrode base layer can selectively exist on the current collector of the negative electrode plate in the form of a sheet or layer, granular, strip, or three-dimensional structure. By further setting the shape of the negative electrode base layer, the contact area between the electrolyte and the negative electrode base layer is increased, that is, the specific surface area of the negative electrode base layer is increased, thereby further improving the performance of the negative electrode base layer in dissolving the element B. The present disclosure uses a sheet or layer, granular, strip, or three-dimensional structure containing an inactive layer of element A as the negative electrode base layer, which inhibits the growth of metal dendrites of element B. At the same time, the negative electrode base layer has the advantages of a large specific surface area and good conductivity, which can improve the battery's fault tolerance, cycle life, and rate performance, and optimize the battery's capacity retention rate and cycle stability.
[0079] In the present disclosure, the negative electrode sheet includes a current collector for supporting the negative electrode base layer, such as copper foil.
[0080] In the present disclosure, the A element metal particles are distributed on the negative electrode base layer in a uniform or non-uniform manner; when the negative electrode base layer has a particle structure, the particle size distribution of the negative electrode base layer particles conforms to the statistical normal distribution characteristics.
[0081] In the present disclosure, the minimum dimension of the A element metal particles or strip-like structures is between 0.05 μm and 200 μm, between 0.5 μm and 150 μm, between 5 μm and 100 μm, between 30 μm and 50 μm, or any numerical range consisting of the end values of the above ranges, preferably between 1 μm and 100 μm. When the negative electrode base layer has a strip-like structure, the minimum dimension is the thickness of the strip-like structure of the negative electrode base layer.
[0082] In the present disclosure, a certain amount of element B may be pre-dissolved in the negative electrode base layer, so that the negative electrode base layer further comprises element B dissolved in at least one inactive layer containing element A. Based on the total mass of the negative electrode base layer, the metal element B is 0-70 mass%, 1-60 mass%, 10-50 mass%, 20-30 mass%, 0-10 mass%, or any numerical range consisting of the end values of the above ranges, preferably 0.1-50 mass%. The pre-dissolved element B can compensate for the loss of the active material element B during the long cycle of the secondary battery, thereby improving the cycle life of the secondary battery while preventing the growth of element B metal dendrites at the negative electrode.
[0083] In the present disclosure, the number of atoms of the element A in the negative electrode base layer accounts for 10%-100%, 20%-90%, 30%-80%, 40%-70%, 50%-60%, 10%-15%, or any numerical range consisting of the end values of the above ranges, preferably 50%-100%. Using the element A alloy as the negative electrode is beneficial to reducing the manufacturing cost of the negative electrode plate, further improving the ability of the negative electrode base layer to dissolve the element B, further improving the ability of the negative electrode base layer to inhibit the growth of element B dendrites, and further extending the cycle life of the secondary battery.
[0084] Figure 1 illustrates the structure of a negative electrode sheet in accordance with a specific embodiment of the present application, comprising at least one layer of layered inactive material containing element A metal or element A alloy as a negative electrode substrate layer, with at least a portion of the negative electrode reinforcement film layer embedded within the A-based negative electrode protective layer and / or the negative electrode substrate layer. As shown in Figure 1 , the negative electrode sheet 1 comprises a current collector 11, at least one inactive layer containing element A (negative electrode substrate layer) formed on the surface of the current collector 12, an A-based negative electrode protective film 13 formed on at least a portion of the surface of the negative electrode substrate layer 12, and a negative electrode reinforcement film 14 formed on at least a portion of the surface of the A-based negative electrode protective film 13.
[0085] In the present disclosure, the active material of the positive electrode plate does not undergo a reversible electrochemical reaction with the ions of element A or preferentially undergoes a reversible electrochemical reaction with the ions of element B; preferably, the active material of the positive electrode plate is a polyanion salt type, a metal oxide type, or a compound type.
[0086] In the present disclosure, the electrolyte comprises a solvent and a fluorine-containing salt. The electrolyte comprises at least one anion selected from fluorine-containing anions, preferably at least one selected from bis(fluorosulfonyl)imide, hexafluorophosphate, bis(trifluoromethanesulfonyl)imide, difluorooxalatoborate, tetrafluoroborate, hexafluoroarsenate, and difluorophosphate.
[0087] In the present disclosure, the solvent of the electrolyte is selected from at least one of an ether compound, an acetal compound and a ketal compound. In a preferred embodiment, the solvent is an ether solvent. More preferably, the solvent is ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, polyethylene glycol dimethyl ether, ethylene glycol methyl ether ethyl ether, ethylene glycol diethyl ether, diethylene glycol methyl ether ethyl ether, diethylene glycol diethyl ether, triethylene glycol methyl ether ethyl ether, triethylene glycol diethyl ether, tetraethylene glycol methyl ether ethyl ether, tetraethylene glycol diethyl ether, ethylene glycol methyl ether propyl ether, ethylene glycol ethyl ether propyl ether, ethylene glycol dipropyl ether, diethylene glycol methyl ether propyl ether, diethylene glycol ethyl ether propyl ether, diethylene glycol dipropyl ether, triethylene glycol methyl ether propyl ether, triethylene glycol ethyl ether At least one of propyl ether, triethylene glycol dipropyl ether, tetraethylene glycol methyl ether propyl ether, tetraethylene glycol ethyl ether propyl ether, tetraethylene glycol dipropyl ether, ethylene glycol methyl ether butyl ether, ethylene glycol ethyl ether butyl ether, ethylene glycol propyl ether butyl ether, ethylene glycol dibutyl ether, diethylene glycol methyl ether butyl ether, diethylene glycol ethyl ether butyl ether, diethylene glycol propyl ether butyl ether, diethylene glycol dibutyl ether, triethylene glycol methyl ether butyl ether, triethylene glycol ethyl ether butyl ether, triethylene glycol propyl ether butyl ether, triethylene glycol dibutyl ether, tetraethylene glycol methyl ether butyl ether, tetraethylene glycol ethyl ether butyl ether, tetraethylene glycol propyl ether butyl ether, and tetraethylene glycol dibutyl ether. The preferred electrolyte solvent used in the present disclosure has low reactivity with the A element metal.
[0088] In the present disclosure, the concentration of the electrolyte is 0.5mol / L-7mol / L, 1mol / L-5mol / L, 2mol / L-4mol / L or any numerical range consisting of the end values of the above ranges. In some embodiments of the present application, the electrolyte also includes additives, and the additives include, but are not limited to: 1,3-dioxolane, 1,4-dioxane, trioxymethylene, lithium nitrate, lithium fluorosulfonate, sulfur dioxide, fluoroethylene carbonate, 12-crown ether-4, 15-crown ether-5 and 18-crown ether-6. In some embodiments, the mass content of the additive in the electrolyte is 0.1% to 20%, 1% to 15% or 5% to 10%.
[0089] In a second aspect of the present disclosure, an electric device is provided, comprising the secondary battery.
[0090] secondary batteries
[0091] The secondary battery of this application includes a positive electrode (pole), a negative electrode (pole), and an electrolyte. During the battery's charge and discharge process, active ions are embedded and released back and forth between the positive and negative electrodes. The electrolyte acts as a conductor of ions between the positive and negative electrodes.
[0092] [Positive electrode]
[0093] In the secondary battery of the present application, the positive electrode plate includes a positive electrode current collector and a positive electrode film layer (or positive electrode active material layer) provided on at least one surface of the positive electrode current collector and including a positive electrode active material. For example, the positive electrode current collector has two surfaces opposite to each other in the thickness direction of the positive electrode current collector, and the positive electrode film layer is provided on any one or both of the two opposite surfaces of the positive electrode current collector. In the secondary battery of the present application, the positive electrode current collector may be a metal foil or a composite current collector. For example, the metal foil may be an aluminum foil, and the composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material base layer. The composite current collector can be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene PP, polyethylene terephthalate PET, polybutylene terephthalate PBT, polystyrene PS, polyethylene PE and its copolymers, etc.).
[0094] In the secondary battery of the present application, the positive electrode active material (substance) can be a positive electrode active material for a secondary battery known in the art. For example, the positive electrode active material may include one or more of the following: olivine-structured phosphates, transition metal oxides, and their respective modified compounds. However, the present application is not limited to these materials, and other conventional materials that can be used as positive electrode active materials for secondary batteries may also be used, including but not limited to layered oxides containing B element ions, polyanionic materials, or Prussian blue-based materials.
[0095] In some embodiments, the positive electrode film layer may also optionally include a binder. Non-limiting examples of binders that can be used for the positive electrode film layer may include one or more of the following: polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer and fluorine-containing acrylate resin. In an embodiment of the present application, each of the first positive active material layer and / or the second positive active material layer independently contains a binder selected from polyvinylidene fluoride, polyacrylic acid, polytetrafluoroethylene, polyimide and a combination thereof.
[0096] In some embodiments, the positive electrode film layer may further optionally include a conductive agent. Examples of conductive agents for the positive electrode film layer may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. In an embodiment of the present application, the first positive electrode active material layer and / or the second positive electrode active material layer each independently contain a conductive agent selected from graphite, carbon black, acetylene black, graphene, carbon nanotubes, and combinations thereof.
[0097] In one embodiment of the present application, the positive electrode can be prepared in the following manner: the above-mentioned components for preparing the positive electrode, such as the positive electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as N-methylpyrrolidone) to form a uniform positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.
[0098] [Negative electrode]
[0099] In the secondary battery of the present application, the negative electrode plate does not exclude other additional functional layers in addition to the negative electrode base layer. For example, in certain embodiments, the negative electrode plate of the present application may further include a conductive primer layer (e.g., composed of a conductive agent and a binder) sandwiched between the negative electrode current collector and the negative electrode base layer and disposed on the surface of the negative electrode current collector. In other embodiments, the negative electrode plate of the present application may further include a covering protective layer covering the surface of the second negative electrode film layer.
[0100] In the secondary battery of the present application, the negative electrode current collector may be a metal foil or a composite current collector. For example, the metal foil may be a copper foil, silver foil, iron foil, or a foil composed of alloys of the above metals. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material base layer. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer material base layer (such as a base layer made of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene PE, and copolymers thereof).
[0101] [Electrolytes]
[0102] The electrolyte conducts ions between the positive and negative electrodes. The electrolyte can be selected from at least one of a solid electrolyte, a semi-solid electrolyte, and a liquid electrolyte. In one embodiment of the present application, the electrolyte may optionally contain additives. For example, the additives may include one or more of the following: negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high-temperature performance, additives that improve battery low-temperature performance, etc.
[0103] [Isolation film]
[0104] In one embodiment of the present application, the secondary battery further comprises a separator, which separates the anode side of the secondary battery from the cathode side, and provides selective permeation or blocking for substances of different types, sizes and charges in the system. For example, the separator can insulate electrons, physically isolate the positive and negative electrodes of the secondary battery, prevent internal short circuits and form an electric field in a certain direction, and at the same time allow ions in the battery to pass through the separator and move between the positive and negative electrodes. In one embodiment of the present application, the material used to prepare the separator may include one or more of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film. When the separator is a multi-layer composite film, the materials of each layer can be the same or different. In an embodiment of the present application, the separator is selected from polyolefin separators, polyester separators, polyimide separators, polyamide separators and cellulose separators.
[0105] In one embodiment of the present application, the positive electrode sheet, negative electrode sheet and separator can be made into an electrode assembly / bare cell through a winding process or a lamination process.
[0106] In one embodiment of the present application, the secondary battery may include an outer packaging that can be used to encapsulate the above-mentioned electrode assembly and electrolyte. In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. In other embodiments, the outer packaging of the secondary battery can be a soft package, such as a bag-type soft package. The material of the soft package can be plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), etc.
[0107] The shape of the secondary battery of the present application may be cylindrical, square or any other shape. The outer packaging may include a shell and a cover plate, and the shell may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell has an opening connected to the receiving cavity, and the cover plate can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can be formed into an electrode assembly through a winding process or a lamination process, and the electrode assembly is encapsulated in the receiving cavity, and the electrolyte is impregnated in the electrode assembly. The number of electrode assemblies contained in the secondary battery may be one or more.
[0108] In one embodiment of the present application, several secondary batteries may be assembled together to form a battery module. The battery module includes two or more secondary batteries, and the specific number depends on the application of the battery module and the parameters of a single battery module.
[0109] In a battery module, multiple secondary batteries may be arranged sequentially along the length of the battery module. Of course, they may also be arranged in any other manner. Furthermore, the multiple secondary batteries may be secured using fasteners. Optionally, the battery module may further include a housing having a storage space, wherein the multiple secondary batteries are housed in the storage space.
[0110] In one embodiment of the present application, two or more of the aforementioned battery modules can be assembled into a battery pack. The number of battery modules contained in the battery pack depends on the application of the battery pack and the parameters of the individual battery modules. The battery pack can include a battery box and multiple battery modules disposed within the battery box. The battery box includes an upper box body and a lower box body. The upper box body can cover the lower box body and fit well therewith to form an enclosed space for accommodating the battery modules. The two or more battery modules can be arranged in the battery box in any desired manner.
[0111] In one embodiment of the present application, an exemplary battery pack may include a battery case and a plurality of battery modules disposed within the battery case. The battery case includes an upper case and a lower case, with the upper case covering the lower case and forming an enclosed space for accommodating the battery modules. The plurality of battery modules may be arranged in any manner within the battery case.
[0112] Electrical devices
[0113] In one embodiment of the present application, an electrical device of the present application includes at least one of the secondary battery, battery module, or battery pack of the present application, and the secondary battery, battery module, or battery pack can be used as a power source for the electrical device or as an energy storage unit for the electrical device. The electrical device includes, but is not limited to, mobile digital devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships, satellites, energy storage systems, etc.
[0114] Another example device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is generally required to be lightweight and thin, and may use a secondary battery as a power source.
[0115] In the following, the influence of the secondary battery manufactured according to the embodiment of the present application on the performance of the electrochemical device is characterized based on specific examples. However, it should be pointed out that the scope of protection of the present application is defined by the claims and is not limited to the above specific embodiments.
[0116] Example
[0117] Unless otherwise specified, all raw materials used in the present invention were of analytical grade and all water used was deionized water.
[0118] 1. Preparation of positive electrode sheet
[0119] 10 wt% of polyvinylidene fluoride was dissolved in N-methylpyrrolidone as a binder, and 80 wt% of a polyanion salt-type positive electrode active material containing element B (see Table 1-12 below for details) and 10 wt% of conductive carbon black were added to prepare a uniformly dispersed positive electrode slurry. The positive electrode slurry was evenly coated on the surface of the aluminum foil current collector and transferred to a vacuum oven for thorough drying. The obtained positive electrode sheet was rolled and punched to obtain the target positive electrode disc.
[0120] 2. Preparation of negative electrode sheet
[0121] In an Ar atmosphere, element A (see Table 1-12 below for details) metal, or element A metal and other alloy component powders are placed in a stainless steel crucible, heated until completely melted and fully stirred, and then cooled to obtain an inactive layer material containing element A.
[0122] The inactive layer material containing element A is compounded on the surface of the copper foil by cold pressing or hot pressing to obtain a negative electrode base layer with a layered structure. Alternatively, the inactive layer material containing element A is compounded on the surface of the copper foil by atomization spraying or sputtering to obtain a negative electrode base layer with a granular structure. Alternatively, the inactive layer material containing element A is compounded on the surface of the copper foil by extrusion to obtain a negative electrode base layer with a strip structure. Alternatively, the inactive layer material containing element A is compounded on the surface of the copper foil by atomization spraying or sputtering to obtain a negative electrode base layer with a three-dimensional structure.
[0123] The negative electrode reinforcement film material is compounded on the surface of the negative electrode base layer by cold pressing or hot pressing to obtain the negative electrode plate.
[0124] 3. Preparation of Isolation Membrane
[0125] A polypropylene porous polymer film is used as the separator.
[0126] 4. Preparation of Electrolyte
[0127] Under an Ar atmosphere, a fully dried fluorine-containing salt (for details, see Table 12 below, hexafluorophosphate, hexafluoroarsenate, or tetrafluoroborate) or a non-fluorine-containing salt (lithium nitrate) is dissolved in an organic solvent of ethylene glycol dipropyl ether, and the mixture is thoroughly stirred to prepare an electrolyte.
[0128] 5. Preparation of Button Cells
[0129] The positive electrode sheet, separator, and negative electrode sheet are stacked in order, with the separator placed between the positive and negative electrode sheets to serve as an isolation layer, and the electrolyte is added to assemble the button battery.
[0130] According to the above preparation method, button batteries of Examples 1-54 and Comparative Examples 1-24 were prepared.
[0131] According to the test results of Examples 1 to 4 in Table 1 below, when element A is sodium and element B is lithium (Example 1, Na-Li); element A is magnesium and element B is lithium (Example 2, Mg-Li), element A is calcium and element B is lithium (Example 3, Ca-Li), or element A is sodium and element B is calcium (Example 4, Na-Ca) (all satisfying that the redox potential of element B is lower than that of element A), the negative electrode base layer containing element A can effectively suppress the formation of metal dendrites of element B, and the secondary battery has good cycle performance (expressed in the number of cycles, <500 is "poor", 500-530 is "medium", and >530 is "excellent") and first cycle coulombic efficiency (expressed in first cycle efficiency). According to the test results of Comparative Example 1 (Li-Na), when the redox reaction potential of element B is higher than that of element A, the structure of the negative electrode base layer containing element A is unstable, and the formation of metal dendrites of element B cannot be effectively suppressed, and the cycle life and first cycle coulombic efficiency of the secondary battery decrease. The test results of Comparative Examples 2 (Cu-Li) and 3 (Mg-Zn) show that when element A is not sodium, potassium, magnesium, or calcium, and / or element B is not lithium, sodium, potassium, magnesium, or calcium, the negative electrode substrate layer containing element A is unable to suppress the formation of metal dendrites of element B, resulting in a decrease in the cycle life and first-cycle coulombic efficiency of the secondary battery. The test results of Comparative Examples 4 (Li-Li) and 5 (Na-Na) show that when element A and element B are the same element, dendrite formation cannot be effectively suppressed, similarly resulting in a decrease in the cycle life and first-cycle coulombic efficiency of the secondary battery.
[0132] Figure 2 is a SEM image of the negative electrode base layer after the battery cycle is completed in Example 3 of the present application. As shown in Figure 2, there is almost no dendrite formation in the negative electrode base layer.
[0133] Figure 3 is a SEM image of the negative electrode base layer after the battery cycle is completed in Comparative Example 4 of the present application. As shown in Figure 3, a large number of dendrites are formed in the negative electrode base layer.
[0134] Table 1
[0135] According to the test results of Examples 5 to 9 in Table 2 below, when element A is magnesium, element B is sodium (Example 5, Mg-Na), and the specific surface area of the negative electrode base layer is 0.001 m 2 / g; Element A is sodium, Element B is lithium (Example 6, Na-Li), and the specific surface area of the negative electrode base layer is 0.1m 2 / g; Element A is magnesium, Element B is sodium (Example 7, Mg-Na), and the specific surface area of the negative electrode base layer is 1m 2 / g; Element A is sodium, Element B is lithium (Example 8, Na-Li), and the specific surface area of the negative electrode base layer is 10m 2 / g; or element A is sodium, element B is calcium (Example 9, Na-Ca), and the specific surface area of the negative electrode base layer is 100m 2 / g, that is, when the specific surface area of the negative electrode base layer is 0.001m 2 / g to 100m 2 / g range, the current density on the negative electrode surface is low, which will not cause excessive growth of the A-based negative electrode protective film and excessive passivation of the negative electrode. The fusion of element A and element B is rapid, and the formation of metal dendrites of element B is suppressed. The secondary battery has a high first cycle coulombic efficiency and ideal cycle performance. According to the test results of Comparative Example 6 (Na-Li), when the specific surface area of the negative electrode base layer is too small (0.0001m 2 / g), the current density of the negative electrode is large, which causes excessive growth of the A-based negative electrode protective film and excessive passivation of the negative electrode. The fusion rate of element A and element B is low, and metal dendrites of element B are easily formed, resulting in a decrease in the first cycle coulomb efficiency and cycle life of the battery. According to the test results of Comparative Example 7 (Na-Ca), when the specific surface area of the negative electrode base layer is too large (150m 2 / g), the formation of the A-based negative electrode protection film consumes too much electrolyte, resulting in a decrease in the first cycle coulombic efficiency and cycle life of the battery.
[0136] Table 2
[0137] According to the test results of Examples 10 to 14 in Table 3 below, when element A is magnesium and element B is potassium (Example 10, Mg-K), the surface roughness of the negative electrode base layer is 0.01 μm; when element A is magnesium and element B is potassium (Example 11, Mg-K), the surface roughness of the negative electrode base layer is 5 μm; when element A is sodium and element B is lithium (Example 12, Na-Li), the surface roughness of the negative electrode base layer is 30 μm; when element A is sodium and element B is calcium (Example 13, Na-Ca), and the surface roughness of the negative electrode base layer is 0.01 μm. The surface roughness of the bottom layer is 50 μm; or when element A is sodium and element B is lithium (Example 14, Na-Li), and the surface roughness of the negative electrode base layer is 250 μm, that is, when the surface roughness of the negative electrode base layer is in the range of 0.01 μm to 250 μm, the current density on the negative electrode surface is low, which will not cause excessive growth of the A-based negative electrode protective film and excessive passivation of the negative electrode. The fusion of element A and element B is rapid, and the formation of metal dendrites of element B is suppressed. The secondary battery has a higher first-cycle coulombic efficiency and ideal cycle performance. According to the test results of Comparative Example 8 (Na-Li), when the surface roughness of the negative electrode base layer is too low (0.005 μm), the current density of the negative electrode is large, which causes excessive growth of the A-based negative electrode protective film and excessive passivation of the negative electrode. The fusion rate of element A and element B is low, and metal dendrites of element B are easily formed, resulting in a decrease in the first-cycle coulombic efficiency and cycle life of the battery. According to the test results of Comparative Example 9 (Na-Ca), when the surface roughness of the negative electrode base layer is too large (350 μm), the specific surface area of the negative electrode base layer is large, and the formation of the A-based negative electrode protective film consumes too much electrolyte, resulting in a decrease in the first cycle coulombic efficiency and cycle life of the battery.
[0138] Table 3
[0139] According to the test results of Examples 15 to 18 in Table 4 below, when element A is sodium and element B is lithium (Example 15, Na-Li), and the porosity of the negative electrode base layer containing element A is 0.10%; when element A is magnesium and element B is potassium (Example 16, Mg-K), and the porosity of the negative electrode base layer containing element A is 10%; when element A is sodium and element B is lithium (Example 17, Na-Li), and the porosity of the negative electrode base layer containing element A is 30%; or when element A is When magnesium, element B is potassium (Example 18, Mg-K), and the porosity of the negative electrode base layer containing element A is 50%, that is, when the porosity of the negative electrode base layer containing element A is in the range of 0%-50%, the energy density of the battery is high, the negative electrode base layer does not consume too much electrolyte in the process of forming SEI, the solubility of element B in the negative electrode base layer is strong, the ability of the negative electrode base layer to inhibit the formation of metal dendrites of element B is strong, the diffusion ability of electrolyte and ions in the negative electrode is strong, and the battery has good cycle performance. According to the test results of Comparative Example 10 (Na-Li), when the porosity of the negative electrode base layer containing element A is too high (60%), the energy density of the battery is low, the negative electrode base layer consumes too much electrolyte in the process of forming SEI, and the first cycle coulomb efficiency and cycle capacity of the battery are reduced.
[0140] Table 4
[0141] According to the test results of Examples 19 to 23 in Table 5, when element A is sodium, element B is lithium (Example 19, Na-Li), and the surface density of the negative electrode base layer is 0.2 mg / cm 2 , the thickness of the negative electrode base layer is 2 μm; when element A is magnesium, element B is calcium (Example 20, Mg-Ca), and the surface density of the negative electrode base layer is lmg / cm 2 , the thickness of the negative electrode base layer is 10 μm; when element A is sodium, element B is lithium (Example 21, Na-Li), and the surface density of the negative electrode base layer is 5 mg / cm 2 , the thickness of the negative electrode base layer is 50 μm; when element A is magnesium, element B is calcium (Example 22, Mg-Ca), and the surface density of the negative electrode base layer is 10 mg / cm 2 , the thickness of the negative electrode base layer is 100 μm; or when element A is sodium, element B is lithium (Example 23, Na-Li), and the surface density of the negative electrode base layer is 50 mg / cm 2 When the thickness of the negative electrode base layer is 500 μm, that is, when the surface density of the negative electrode base layer is 0.2 mg / cm 2 -50mg / cm 2When the thickness of the negative electrode base layer is within the range of 2μm-500μm, the secondary battery has a high energy density and good cycle performance. The negative electrode base layer containing element A can effectively inhibit the formation of metal dendrites of element B. According to the test results of Comparative Example 11 (Mg-Ca), when the surface density of the negative electrode base layer containing element A is too low (0.05mg / cm 2 ), the negative electrode base layer is difficult to effectively inhibit the formation of metal dendrites of element B, and the cycle performance of the battery deteriorates. According to the test results of Comparative Example 12 (Na-Li), when the surface density of the negative electrode base layer containing A is too high (60 mg / cm 2 ) and the thickness of the negative electrode base layer is too high (600μm), the energy density of the battery is low, the diffusion distance and diffusion resistance of the B element dissolved in the negative electrode base layer increase, and it is difficult to fully participate in the battery cycle process, thereby deteriorating the battery cycle performance.
[0142] Table 5
[0143] According to the test results of Examples 24 to 28 in Table 6 below, when element A is magnesium and element B is calcium (Example 24, Mg-Ca), the particle size of the particles constituting the negative electrode base layer is 0.05 μm; when element A is magnesium and element B is calcium (Example 25, Mg-Ca), the particle size of the particles constituting the negative electrode base layer is 1 μm; when element A is sodium and element B is lithium (Example 26, Na-Li), the particle size of the particles constituting the negative electrode base layer is 50 μm; when element A is magnesium and element B is sodium (Example 27, Mg-Na) , and the particle size of the particles constituting the negative electrode base layer is 100μm; or when element A is sodium and element B is lithium (Example 28, Na-Li), and the particle size of the particles constituting the negative electrode base layer is 200μm, that is, when the particle size of the particles constituting the negative electrode base layer is in the range of 0.05μm to 200μm, the negative electrode base layer containing element A has a strong dissolving ability for element B, and the negative electrode base layer does not consume too much electrolyte when forming a negative electrode protective film containing element A. It has a strong ability to inhibit the formation of metal dendrites of element B, and the battery has good cycle performance. According to the test results of Comparative Example 13 (Mg-Na), it can be seen that when the particle size of the particles constituting the negative electrode base layer is too small (0.01μm), the negative electrode base layer consumes too much electrolyte when forming a negative electrode protective film containing element A, which deteriorates the first cycle coulomb efficiency and cycle performance of the battery. According to the test results of Comparative Example 14 (Na-Li), when the particle size of the particles constituting the negative electrode base layer is too large, the diffusion distance and diffusion resistance of element B in the negative electrode base layer containing element A increase, the battery impedance increases, and the ability of the negative electrode base layer to inhibit the formation of metal dendrites of element B decreases, thereby deteriorating the cycle performance of the battery.
[0144] Table 6
[0145] According to the test results of Examples 29 to 32 in Table 7 below, it can be seen that when element A is sodium, element B is lithium (Example 29, Na-Li), and the material of the negative electrode reinforcement film is lithium fluoride; when element A is sodium, element B is lithium (Example 30, Na-Li), and the material of the negative electrode reinforcement film is sodium fluoride; when element A is magnesium, element B is potassium (Example 31, Mg-K), and the material of the negative electrode reinforcement film is carbon nanotubes; or when element A is magnesium, element B is potassium (Example 32, Mg-K), and the material of the negative electrode reinforcement film is conductive carbon black, that is, when the component constituting the negative electrode reinforcement film is a substance that does not chemically react with the electrolyte, element B, and the inactive layer containing element A, the consumption rate of element B in the battery is low, the negative electrode reinforcement film has a stable structure, thereby continuously increasing the specific surface area of the negative electrode base layer, stabilizing the surface state of the negative electrode base layer, inhibiting the formation of metal dendrites, reducing the actual current density of the negative electrode, and improving the cycle performance of the battery. According to the test results of Comparative Example 15 (Na-Li), when the component of the negative electrode reinforcement film (aluminum powder) can react with the B element, the consumption rate of the B element in the battery is high, and the structure of the negative electrode reinforcement film is unstable, which leads to the structural instability of the negative electrode base layer, and the negative electrode is prone to form dendrites, which deteriorates the cycle performance of the battery.
[0146] Table 7
[0147] According to the test results of Examples 33 to 37 and Comparative Examples 16 to 17 in Table 8 below, when element A is sodium and element B is lithium (Example 33, Na-Li), and the negative electrode base layer has a striped structure, the minimum dimension of the stripes is 0.05 μm; when element A is magnesium and element B is calcium (Example 34, Mg-Ca), and the negative electrode base layer has a striped structure, the minimum dimension of the stripes is 1 μm; when element A is sodium and element B is lithium (Example 35, Na-Li), and the negative electrode base layer has a striped structure, the minimum dimension of the stripes is 50 μm; when element A is magnesium and element B is calcium (Example 36, Mg-Ca), , and the negative electrode base layer is a striped structure, and the minimum dimension of the stripes is 100μm; or when element A is sodium and element B is lithium (Example 37, Na-Li), and the negative electrode base layer is a striped structure, and the minimum dimension of the stripes is 200μm, that is, when the negative electrode base layer is a stripe structure, and the minimum dimension of the stripe is in the range of 0.05μm to 200μm, the negative electrode base layer containing element A has a strong solubility for element B, and the negative electrode base layer does not consume too much electrolyte in the process of forming SEI, and has a strong ability to inhibit the formation of metal dendrites of element B, and the battery has a higher first-cycle coulomb efficiency and better cycle performance. The test results for Comparative Example 16 (Mg-Ca) show that when the minimum dimension of the stripes constituting the negative electrode base layer is too small (0.01 μm), the negative electrode base layer consumes too much electrolyte during the formation of the negative electrode protective film containing element A, resulting in a decrease in the battery's first-cycle coulombic efficiency and deterioration in cycle performance. The test results for Comparative Example 17 (Na-Li) show that when the minimum dimension of the stripes constituting the negative electrode base layer is too large (300 μm), the diffusion distance and diffusion resistance of element B in the negative electrode base layer increase, deteriorating the battery's cycle performance.
[0148] Table 8
[0149] According to the test results of Examples 38 to 42 in Table 9 below, when element A is sodium and element B is lithium (Example 38, Na-Li), and the mass percentage of element A in the negative electrode base layer is 99%, the mass percentage of element B in the negative electrode base layer is 1%; when element A is sodium and element B is lithium (Example 39, Na-Li), and the mass percentage of element A in the negative electrode base layer is 90%, the mass percentage of element B in the negative electrode base layer is 10%; when element A is magnesium and element B is sodium (Example 40, Mg-Na), and the mass percentage of element A in the negative electrode base layer is 70%, the mass percentage of element B in the negative electrode base layer is 10%. The mass percentage of the element is 30%; when element A is sodium, element B is lithium (Example 41, Na-Li), and the mass percentage of element A in the negative electrode base layer is 50%, and the mass percentage of element B in the negative electrode base layer is 50%; or when element A is magnesium, element B is sodium (Example 42, Mg-Na), and the mass percentage of element A in the negative electrode base layer is 30%, and the mass percentage of element B in the negative electrode base layer is 70%, that is, when the mass percentage of element B in the negative electrode base layer is in the range of 0%-70%, the consumption of element B during the battery cycle is suppressed, and the battery cycle performance is better. According to the test results of Comparative Examples 18 to 19 (Na-Li), when the mass percentage of the B element in the negative electrode base layer is greater than 70% (i.e., 75% and 100%), the solubility performance of the negative electrode base layer for the B element decreases, the diffusion ability of the B element in the negative electrode base layer is weak, the negative electrode base layer is difficult to effectively inhibit the formation of B element metal dendrites, and the cycle performance of the battery deteriorates.
[0150] Table 9
[0151] According to the test results of Examples 43 to 47 in Table 10 below, when element A is sodium and element B is lithium (Example 43, Na-Li), and the number of atoms of element A in the negative electrode base layer accounts for 10%; when element A is magnesium and element B is sodium (Example 44, Mg-Na), and the number of atoms of element A in the negative electrode base layer accounts for 30%; when element A is sodium and element B is lithium (Example 45, Na-Li), and the number of atoms of element A in the negative electrode base layer accounts for 50%; when element A is magnesium and element B is sodium (Example 46, M g-Na), and the number of atoms of element A in the negative electrode base layer accounts for 70%; or when element A is sodium and element B is lithium (Example 47, Na-Li), and the number of atoms of element A in the negative electrode base layer accounts for 100%, that is, when the number of atoms of element A in the negative electrode base layer accounts for 10% to 100%, the negative electrode base layer containing element A has a strong dissolving ability for element B, can effectively inhibit the growth of metal dendrites of element B, reduce the consumption of active element B during the regeneration process of the A-based negative electrode protective film, and improve the cycle performance of the battery. According to the test results of Comparative Example 20 (Mg-Na) and Comparative Example 21 (Na-Li), when the content of element A in the negative electrode base layer is less than 10%, the ability of the negative electrode base layer to dissolve element B is weak, the effect of inhibiting the formation of metal dendrites of element B is poor, and the cycle performance of the battery is poor.
[0152] Table 10
[0153] According to the test results of Examples 48 to 51 in Table 11 below, when element A is magnesium and element B is potassium (Example 48, Mg-K), and the electrolyte concentration is 0.5 mol / L; when element A is sodium and element B is lithium (Example 49, Na-Li), and the electrolyte concentration is 2 mol / L; when element A is magnesium and element B is potassium (Example 50, Mg-K), and the electrolyte concentration is 5 mol / L; or when element A is sodium and element B is lithium (Example 51, Na-Li), and the electrolyte concentration is 7 mol / L, that is, when the electrolyte concentration is in the range of 0.5 mol / L to 7 mol / L, the electrolyte has good ion conductivity and film-forming effect of element B, can effectively inhibit the formation of metal dendrites of element B, inhibit the occurrence of side reactions in the battery, and the battery has a high cycle life. The test results for Comparative Example 22 (Na-Li) show that when the electrolyte concentration is too low (0.2 mol / L), the electrolyte ionic conductivity is low, the battery concentration polarization is large during cycling, and the battery cycle life is short. The test results for Comparative Example 23 (Na-Li) show that when the electrolyte concentration is too high (8 mol / L), the electrolyte viscosity is too high, the electrolyte ionic conductivity is low, the battery polarization is large, and the battery cycle life is reduced.
[0154] Table 11
[0155] According to the test results of Examples 52 to 54 in Table 12 below, when element A is sodium, element B is lithium (Example 52, Na-Li), and the anion forming the negative electrode protective film is PF6 - , the main component of the negative electrode protective film is sodium fluoride; when element A is sodium, element B is lithium (Example 53, Na-Li), and the anion forming the negative electrode protective film is BF4 - , the main component of the negative electrode protective film is sodium fluoride; or when element A is sodium, element B is lithium (Example 54, Na-Li), and the anion forming the negative electrode protective film is AsF6 - When the main component of the negative electrode protective film is sodium fluoride, that is, when the electrolyte contains at least one anion that is a fluoride-containing anion, and the main component of the A-based negative electrode protective film is metal fluoride, the secondary battery has good cycle performance, the transmission resistance of the B element ions in the A-based negative electrode protective film is small, and the A-based negative electrode protective film can effectively block the side reactions between the negative electrode base layer and the electrolyte, reducing the consumption of active substances in the battery. According to the test results of Comparative Example 24 (Na-Li), when the component of the A-based negative electrode protective film is not mainly metal fluoride, the resistance of the B element ions to pass through the A-based negative electrode protective film is large, the side reactions between the negative electrode base layer and the electrolyte are intensified, resulting in the formation of metal dendrites and the consumption of active substances, and worsening the cycle performance of the battery.
[0156] Table 12
[0157] Test Method
[0158] 1. Specific surface area S 负
[0159] According to the national standard "GB / T 19587-2004 Method for Determining the Specific Surface Area of Solids by the BET Principle of Gas Adsorption", the test is performed using an adsorption characterization analyzer. The powder sample to be tested is placed in a U-shaped sample tube, and a mixed gas containing a certain proportion of adsorbate flows through the sample. The adsorption amount of the adsorbate molecules (N2) by the sample to be tested is determined based on the change in gas concentration before and after adsorption, thereby obtaining the specific surface area S. 负 .
[0160] 2. Median particle size D 50负
[0161] Median particle size D 50负 D is the median particle size of the metal or alloy particles constituting the negative electrode base layer, in μm. 50负The particle size corresponding to the cumulative volume percentage of metal or alloy particles in the negative electrode base layer reaches 50%. According to the national standard "GB / T 19077-2016 Particle Size Distribution Laser Diffraction Method", the sample is dispersed under pressure and the particle size of the material is characterized by a laser particle size analyzer. The test results are expressed as median particle size D 50负 Indicates the average particle size.
[0162] 3. Roughness Ra
[0163] Roughness, as used herein, refers to the microscopic geometric features consisting of small spacings and tiny peaks and valleys that remain on the surface of the processed inactive layer. "Roughness Ra," a parameter representing the surface roughness of industrial products, is expressed in terms of the "arithmetic mean roughness Ra" specified in the Japanese Industrial Standard (JIS B 0601-1994), and can be measured using, for example, a surface roughness meter or confocal laser microscope. The surface roughness of the inactive negative electrode base layer satisfies Ra requirements of 0.01 μm ≤ Ra ≤ 250 μm.
[0164] 4. Porosity
[0165] Calculate the volume of the negative electrode according to its size and weigh the dry mass m of the negative electrode. p , from which the dry density ρ of the negative electrode is calculated p Then, the negative electrode sheet is immersed in an inert organic solvent (e.g., ethylene glycol dibutyl ether) for 10 hours, the negative electrode sheet is taken out, the flowing liquid on the surface of the negative electrode sheet is wiped off, and its wet weight is weighed. The mass m of ethylene glycol dibutyl ether absorbed by the negative electrode sheet is determined based on the difference between the wet weight and the dry weight. a , the density of ethylene glycol dibutyl ether ρ a The porosity of the negative electrode sheet is calculated based on the known parameters.
[0166] It can be seen that the overall porosity takes into account the total porosity of the substrate layer and the coating. However, when other components in the substrate layer and coating of each different negative electrode plate remain unchanged, the total porosity very intuitively reflects the porosity of the negative electrode base layer of the negative electrode plate of the present invention.
[0167] 5. Surface density of negative electrode base layer
[0168] The square negative electrode substrate layer with a size of 10 cm*10 cm was weighed to obtain its mass, which was then divided by its area to obtain the surface density.
[0169] 6.Thickness of negative electrode base layer
[0170] A 10cm*10cm square negative electrode sheet was placed, with its corners aligned, between two 10cm*10cm stainless steel sheets of uniform thickness and a defined thickness H1. The total thickness H2 of the two stainless steel sheets plus the negative electrode sheet was measured, and the thickness H3 of the negative electrode sheet was calculated using the formula H3=H2-2H1. When the negative electrode sheet is double-sided coated, the approximate thickness H5 of the negative electrode base layer is calculated using the formula H5=(H3-H4) / 2, where H4 is the thickness of the current collector. When the negative electrode sheet is single-sided coated, the approximate thickness H5 of the negative electrode base layer is calculated using the formula H5=H3-H4, where H4 is the thickness of the current collector.
[0171] 7. Cyclic performance test
[0172] At 25°C, the secondary batteries prepared in the Examples and Comparative Examples were subjected to full charge and discharge cycle testing at a 0.5C rate. The number of cycles at which the battery capacity reached 80% or less of its initial capacity was recorded (recorded as the nth cycle). A higher n indicates better cycling performance. A cycle greater than 530 cycles indicates excellent cycling performance, a cycle between 500 and 530 cycles indicates fair cycling performance, and a cycle less than 500 cycles indicates poor cycling performance.
Claims
1. A secondary battery, comprising a positive electrode sheet, an electrolyte and a negative electrode sheet, characterized in that: The negative electrode plate includes a negative electrode base layer, and the negative electrode base layer includes at least one inactive layer containing element A; The electrolyte includes a B element as an active material; Wherein, the A element is at least one of sodium, potassium, magnesium and calcium, and the B element is at least one of lithium, sodium, potassium, magnesium and calcium; The B element is different from the A element, and the redox reaction potential of the B element is lower than that of the A element.
2. The secondary battery according to claim 1, characterized in that: It also includes an A-based negative electrode protection film located on at least a portion of the surface of the negative electrode base layer.
3. The secondary battery according to claim 2, characterized in that: The negative electrode plate also includes a negative electrode enhancement film located on at least a portion of the surface of the A-based negative electrode protection film.
4. The secondary battery according to claim 3, characterized in that: The negative electrode enhancement film is a material that does not chemically react with the electrolyte.
5. The secondary battery according to claim 4, characterized in that: The negative electrode enhancement film is a material that does not chemically react with the B element metal and / or the inactive layer containing the A element.
6. The secondary battery according to any one of claims 1 to 5, characterized in that: The negative electrode plate meets at least one of the following conditions: (1) The specific surface area S of the negative electrode base layer 负 Meet 0.001m 2 / g≤S 负 ≤100m 2 / g; (2) The surface roughness R of the negative electrode base layer 负 Satisfy 0.01μm≤R 负 ≤250μm; (3) The porosity K of the negative electrode base layer 负 Satisfy 0%≤K 负 ≤50%; (4) The thickness d of the negative electrode base layer 负 Satisfy: 2μm≤d 负 ≤500μm; (5) The surface density C of the negative electrode base layer 负 Meet: 0.2mg / cm 2 ≤C 负 ≤50mg / cm 2 ; (6) The median particle size D of the particles of the negative electrode base layer 50负 Satisfy 0.05μm≤D 50负 ≤200μm; (7) The negative electrode substrate layer has a stripe structure, and the minimum dimension of the stripes is in the range of 0.05 μm to 200 μm; (8) The atomic number of the A element in the negative electrode base layer accounts for between 10% and 100%; or (9) The mass percentage of the B element in the negative electrode base layer is between 0% and 70%.
7. The secondary battery according to any one of claims 1 to 5, characterized in that: The inactive layer containing element A is combined with element B in any of the following ways: a combination of a magnesium inactive layer and a sodium element, a combination of a magnesium inactive layer and a lithium element, a combination of a magnesium inactive layer and a potassium element, a combination of a magnesium inactive layer and a calcium element, a combination of a sodium inactive layer and a potassium element, a combination of a sodium inactive layer and a lithium element, a combination of a sodium inactive layer and a calcium element, a combination of a calcium inactive layer and a potassium element, a combination of a calcium inactive layer and a lithium element, or a combination of a potassium inactive layer and a lithium element.
8. The secondary battery according to any one of claims 1 to 5, characterized in that: It also includes a separator, and a second negative electrode enhancement film disposed on at least a portion of the separator; and / or the separator itself is at least partially the second negative electrode enhancement film.
9. The secondary battery according to any one of claims 1 to 5, characterized in that: The inactive layer containing the A element is in the form of a lamellar structure, a stripe structure, a three-dimensional structure and / or a particle structure.
10. The secondary battery according to any one of claims 1 to 5, characterized in that: The negative electrode base layer further comprises a B element dissolved in at least one inactive layer containing an A element, and the B element accounts for 0-70 mass % based on the total mass of the negative electrode base layer.
11. The secondary battery according to any one of claims 1 to 5, characterized in that: The active material of the positive electrode plate does not undergo a reversible electrochemical reaction with the A element ions or preferentially undergoes a reversible electrochemical reaction with the B element ions.
12. The secondary battery according to any one of claims 1 to 5, characterized in that: The active material of the positive electrode plate is of polyanion salt type, metal oxide type or compound type.
13. The secondary battery according to any one of claims 1 to 5, characterized in that: The electrolyte comprises at least one anion selected from fluoride-containing anions.
14. The secondary battery according to claim 13, characterized in that: The electrolyte comprises at least one anion selected from at least one of bis(fluorosulfonyl)imide, hexafluorophosphate, bis(trifluoromethanesulfonyl)imide, difluorooxalatoborate, tetrafluoroborate, hexafluoroarsenate and difluorophosphate.
15. The secondary battery according to any one of claims 1 to 5, characterized in that: The solvent of the electrolyte is selected from at least one of an ether compound, an acetal compound and a ketal compound.
16. The secondary battery according to any one of claims 1 to 5, characterized in that: The concentration of the electrolyte is in the range of 0.5 mol / L to 7 mol / L.
17. An electrical device comprising the secondary battery according to any one of claims 1 to 16.
Citation Information
Patent Citations
Preparation method of anode of lithium battery
CN107093706A
3D porous zinc-loaded current collector, sodium or potassium-philic battery negative electrode and preparation and application thereof
CN110828828A
Lithium battery copper current collector metal induction layer and preparation method thereof
CN111969212A
Laminated lithium metal battery negative electrode material, preparation method thereof and lithium metal secondary battery
CN112750982A
Negative electrode for all-solid-state battery, preparation method of negative electrode and all-solid-state battery