Tubular diffusion electrode for electroreduction of carbon dioxide, and preparation and use thereof
The tubular diffusion electrode prepared by using metal powder or oxide powder solves the problems of traditional electrode degradation and binder aging in a highly alkaline environment, achieving stable operation and efficient CO2 mass transfer and diffusion, and is suitable for industrial applications.
Patent Information
- Application Number
- PCT/CN2024/085783
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-12
- Filing Date
- 2024-04-03
- Publication Date
- 2024-10-17
AI Technical Summary
Traditional CO2 electroreduction diffusion electrodes suffer from electrode degradation and binder aging and loosening in highly alkaline environments, resulting in unstable performance and inability to meet the requirements for long-term stable operation in industrialization.
Using a tubular diffusion electrode with metal powder or metal oxide powder as the precursor, a gas channel with a porous layered structure is formed through the casting liquid and extrusion molding process to achieve controllable number and pore size and reduce the thickness of the electrode and cost, and enhance CO2 mass transfer and diffusion capabilities.
It achieves stable operation of the electrode in a highly alkaline environment, enhances CO2 mass transfer and diffusion capabilities, and reduces the risk of electrode loosening and degradation. It is suitable for industrial-scale applications, and can adjust chemical reaction paths through subsequent surface catalysis.
Smart Images

Figure CN2024085783_17102024_PF_FP_ABST
Abstract
Description
Tubular diffusion electrode for carbon dioxide electroreduction and its preparation and application Technical Field
[0001] The present invention relates to the field of electrochemical catalysis, and in particular to a tubular diffusion electrode for carbon dioxide electroreduction, and the preparation and application thereof. Background Art
[0002] Converting CO2 into fuels and chemicals is a new and transformative negative carbon technology. Compared with thermal catalysis under harsh conditions, electrocatalytic CO2 reduction can be carried out at room temperature and pressure, with lower energy and equipment requirements, and has significant advantages in practical applications. Although significant progress has been made in CO2 electroreduction, the long mass transfer distance in H-type electrolyzers hinders CO2 transport, resulting in very limited current density, which is far below the requirements of industrial applications. One strategy to address this problem is to coat a highly active catalyst on a microporous layer decorated with superhydrophobic polytetrafluoroethylene and conductive carbon particles to construct a gas diffusion electrode.
[0003] In the prior art, the gas diffusion electrode is mainly composed of a catalytic layer, a microporous layer and a gas diffusion layer, wherein the catalytic layer is mainly composed of an active catalyst, a hydrophobic binder and a conductive additive. This gas diffusion electrode not only alleviates the mass transport limitation of CO2, but also expands the scope of application of electrocatalytic CO2 reduction to highly alkaline electrolytes (such as 1.0M KOH or higher). However, long-term operation in a highly alkaline environment will cause the gas diffusion electrode to degrade, limiting the mass transport of CO2. At the same time, the binder integrated in the gas diffusion electrode may age and loosen during long-term CO2 electrolysis, affecting the stability of performance and failing to meet the conditions for long-term stable operation in industrialization.
[0004] Summary of the Invention
[0005] In response to the shortcomings of the existing technology, the present invention provides a tubular diffusion electrode for carbon dioxide electroreduction and its preparation and application, with the aim of solving the technical problems of electrode degradation, binder aging and loosening, and unstable performance of traditional electrocatalytic CO2 reduction diffusion electrodes that exist in long-term operation in a high alkaline environment.
[0006] The technical solution adopted in the present invention is as follows:
[0007] The present application provides a tubular diffusion electrode for CO2 electroreduction, wherein the tubular diffusion electrode uses metal powder or metal oxide powder as a precursor, is obtained by preparing a casting pipe liquid, extrusion molding, and thermal curing, and a plurality of gas channels extending along the axial direction are formed in the tubular diffusion electrode, and a porous layered structure is formed on the side wall of the gas channel. The porous layered structure is a layered structure with a large number of small pores distributed therein, and the number and pore size of the small pores can be controlled and adjusted by changing the precursor particle size, the casting pipe liquid ratio, and the thermal curing temperature to control the rate at which the powder particles form sintering necks.
[0008] Further technical solutions are:
[0009] The pores in the porous hierarchical structure have a pore diameter of 0.5 to 20 μm.
[0010] The outer contour of the cross section of the tubular diffusion electrode is circular with a diameter of 1 to 10 mm. The plurality of axially extending gas channels are evenly distributed along the circumference, the cross section of the gas channels is elliptical, and the wall thickness of the gas channels is 40 to 300 μm.
[0011] The present application also provides a method for preparing the tubular diffusion electrode for CO2 electroreduction as described above, comprising:
[0012] The polyethyleneimine was dried at 60°C;
[0013] Using metal powder or metal oxide powder as a precursor, mixing the precursor with N-methylpyrrolidone, and uniformly dispersing the precursor by ultrasonication;
[0014] Adding dry polyethyleneimine to the mixture of the precursor and N-methylpyrrolidone, heating and stirring to completely dissolve the polyethyleneimine, and cooling to obtain a pipe casting solution;
[0015] The casting liquid is transferred to an extrusion device and extruded at room temperature to obtain a tubular diffusion electrode precursor containing a polymer;
[0016] The tubular diffusion electrode precursor is calcined at high temperature and then reduced in a hydrogen atmosphere to obtain the tubular diffusion electrode.
[0017] Further technical solutions are:
[0018] The mass ratio of the precursor, polyethyleneimine and N-methylpyrrolidone in the pipe casting liquid is (20-32): (3-10): (10-20).
[0019] The metal powder is at least one of silver, gold, nickel, iron, and copper, and the metal oxide powder is at least one of nickel oxide, ferroferric oxide, and copper oxide.
[0020] The particle size of the precursor ranges from 50 μm to 150 nm.
[0021] The calcination temperature of the tubular diffusion electrode precursor is 300-1000°C, and the reduction temperature is 300-700°C.
[0022] The present application also provides an application of the tubular diffusion electrode for CO2 electroreduction, wherein the tubular diffusion electrode serves as both a CO2 overflow device and a working electrode to catalyze CO2 electroreduction. The specific steps are as follows:
[0023] Encapsulating one end of the tubular diffusion electrode, and continuously introducing CO2 from the inlet of the gas channel at the unencapsulated end, forcing the introduced CO2 to continuously diffuse through the porous layered structure to the electrode surface;
[0024] Under the condition of continuous CO2 flow, the tubular diffusion electrode with one end packaged is placed in the cathode electrolyte for activation treatment, and then constant potential electrolysis is used to achieve efficient CO2 electroreduction.
[0025] Further technical solutions are:
[0026] One end of the tubular diffusion electrode is encapsulated with epoxy resin glue.
[0027] The beneficial effects of the present invention are as follows:
[0028] Compared with the multi-component composition of traditional diffusion electrodes, the CO2 electroreduction tubular diffusion electrode of the present invention is composed only of metal, and has electrical conductivity, catalysis and gas diffusion properties. It is not easy for the electrode to loosen or degrade during long-term electrolysis of CO2 in a highly alkaline environment, and can operate stably, showing great commercial application potential.
[0029] Compared with the fixed CO2 diffusion channel in the traditional diffusion electrode, the tubular diffusion electrode of the present invention can control the rate at which powder particles form sintering necks by changing the precursor particle size, the casting liquid ratio and the thermal curing temperature, thereby achieving controllable adjustment of the number and diameter of pores in its porous layered wall. The internal elliptical gas channel can play a good supporting role, minimize the thickness of the porous layered wall, thereby shortening the CO2 mass transfer distance and enhancing CO2 mass transfer diffusion.
[0030] Compared with the coating preparation process of traditional diffusion electrodes, the tubular diffusion electrode of the present invention is obtained by extrusion molding and thermal curing, which has a simple process, controllable process and low cost; and compared with traditional diffusion electrodes, the obtained tubular diffusion electrode has a small volume, a large surface area, a high surface area to volume ratio, good mechanical strength, is conducive to compact assembly and mass production, and is suitable for large-scale application.
[0031] Compared with the one-time molding of conventional diffusion electrodes, the tubular diffusion electrode of the present invention can also be used to adjust the subsequent surface catalytic active species and change the chemical reaction path to obtain different terminal products.
[0032] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be obvious from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] FIG1 is a cross-sectional view of a tubular diffusion electrode according to Example 1 of the present invention.
[0034] FIG2 is a SEM image of the porous layered structure of the tubular diffusion electrode according to Example 1 of the present invention.
[0035] FIG3 is a physical picture of the tubular diffusion electrode assembly structure prepared in Example 3 of the present invention.
[0036] In the figure: 1. gas channel; 2. side wall; 3. porous layered structure; 4. diffusion electrode part; 5. connecting piece; 6. nut. DETAILED DESCRIPTION
[0037] The specific embodiments of the present invention are described below with reference to the accompanying drawings.
[0038] Example 1 of the present application provides a tubular diffusion electrode for CO2 electroreduction.
[0039] Example 1
[0040] Referring to Figures 1 and 2 , the tubular diffusion electrode, using metal powder or metal oxide powder as a precursor, is formed by preparing a casting solution, extruding, and then thermally curing. The tubular diffusion electrode comprises four axially extending gas channels 1, with a porous layered structure 3 formed on the sidewalls 2 of each channel. The porous layered structure 3 is a layered structure with a large number of small pores, as shown in the right image of Figure 1 (a partial enlargement of location 3 in the left image of Figure 1 ). A SEM image of the porous layered structure 3 is shown in Figure 2 . The number and diameter of the small pores can be controlled by varying the precursor particle size, the casting solution ratio, and the thermal curing temperature to control the rate at which the powder particles form sintering necks.
[0041] The pores in the porous hierarchical structure have a pore diameter of 0.5 to 20 μm.
[0042] The wall thickness of the gas channel is 40 to 300 μm.
[0043] The outer contour of the cross section of the tubular diffusion electrode is circular, with a diameter of 1 to 10 mm. A plurality of gas channels 1 extending in the axial direction are evenly distributed along the circumference, and the cross section of the gas channels 1 is elliptical.
[0044] The tubular diffusion electrode of Example 1 features a "porous layered wall" on its side, which facilitates CO2 diffusion. Adjusting the number and diameter of the pores modulates CO2 diffusion within the "porous layered wall." Furthermore, the internal elliptical gas channel 1 provides excellent support, minimizing the thickness of the "porous layered wall," thereby shortening the CO2 mass transfer distance and enhancing CO2 diffusion.
[0045] The present application also provides a method for preparing the tubular diffusion electrode for CO2 electroreduction described in Example 1, comprising:
[0046] The polyethyleneimine was dried at 60°C;
[0047] Using metal powder or metal oxide powder as a precursor, mixing the precursor with N-methylpyrrolidone, and uniformly dispersing the precursor by ultrasonication;
[0048] Adding dry polyethyleneimine to the mixture of the precursor and N-methylpyrrolidone, heating and stirring to completely dissolve the polyethyleneimine, and cooling to obtain a pipe casting solution;
[0049] The casting liquid is transferred to an extrusion device and extruded at room temperature to obtain a tubular diffusion electrode precursor containing a polymer;
[0050] The tubular diffusion electrode precursor is calcined at high temperature and then reduced in a hydrogen atmosphere to obtain the tubular diffusion electrode.
[0051] The mass ratio of the precursor, polyethyleneimine and N-methylpyrrolidone in the pipe casting liquid is (20-32): (3-10): (10-20).
[0052] The metal powder is at least one of silver, gold, nickel, iron, and copper, and the metal oxide powder is at least one of nickel oxide, ferroferric oxide, and copper oxide.
[0053] The particle size of the precursor ranges from 50 μm to 150 nm.
[0054] The calcination temperature of the tubular diffusion electrode precursor is 300-1000°C, and the reduction temperature is 300-700°C.
[0055] Compared to the coating preparation process of traditional diffusion electrodes, the tubular diffusion electrodes of the present invention are produced through extrusion molding and thermal curing, which features a simple, controllable process and low cost. Furthermore, compared to traditional diffusion electrodes, the resulting tubular diffusion electrodes are compact, have a large surface area, a high surface area-to-volume ratio, and excellent mechanical strength, facilitating compact assembly and mass production, making them suitable for large-scale applications. Compared to the one-step molding of traditional diffusion electrodes, the tubular diffusion electrodes produced in the present invention also allow for subsequent adjustment of surface catalytically active species, altering the chemical reaction pathway to obtain different end products.
[0056] The specific process of the preparation method is described below with reference to Examples 2-9.
[0057] Example 2
[0058] Commercially available polyethyleneimine was dried overnight at 60°C. Silver powder with a particle size of 150 nm was mixed with N-methylpyrrolidone and uniformly dispersed by ultrasonication. The dried polyethyleneimine was then added to the mixture of silver powder and N-methylpyrrolidone and heated and stirred until the polyethyleneimine was completely dissolved (the mass ratio of silver powder to polyethyleneimine to N-methylpyrrolidone was 20:3:10). After cooling, a casting solution was obtained. The casting solution was transferred to an extruder and extruded at room temperature to produce a polymer-containing silver tubular diffusion electrode precursor. Finally, the silver tubular diffusion electrode precursor was calcined at 600°C in air and then reduced at 400°C under hydrogen to obtain a single-component silver tubular diffusion electrode A1 with a tube diameter of 1 mm, a wall thickness of 40 μm, and a pore diameter of 0.5 μm.
[0059] Example 3
[0060] Commercially available polyethyleneimine was dried overnight at 60°C. Meanwhile, gold powder with a particle size of 300 nm was mixed with N-methylpyrrolidone and uniformly dispersed by ultrasonication. The dried polyethyleneimine was then added to the mixture of gold powder and N-methylpyrrolidone, heated and stirred until the polyethyleneimine was completely dissolved (the mass ratio of gold powder to polyethyleneimine to N-methylpyrrolidone was 25:5:15). After cooling, a casting solution was obtained. The casting solution was transferred to an extruder and extruded at room temperature to produce a polymer-containing gold tubular diffusion electrode precursor. Finally, the gold tubular diffusion electrode precursor was calcined at 700°C in air and then reduced at 500°C under hydrogen to obtain a single-component gold tubular diffusion electrode A2 with a tube diameter of 3 mm, a wall thickness of 60 μm, and a pore diameter of 2 μm.
[0061] Example 4
[0062] Commercially available polyethyleneimine was dried overnight at 60°C. Meanwhile, nickel powder with a particle size of 1 μm was mixed with N-methylpyrrolidone and uniformly dispersed by ultrasonication. The dried polyethyleneimine was then added to the mixture of nickel powder and N-methylpyrrolidone, heated and stirred until the polyethyleneimine was completely dissolved (the mass ratio of nickel powder to polyethyleneimine to N-methylpyrrolidone was 32:10:20). After cooling, a casting solution was obtained. The casting solution was transferred to an extruder and extruded at room temperature to produce a polymer-containing nickel tubular diffusion electrode precursor. Finally, the nickel tubular diffusion electrode precursor was calcined at 900°C in air and then reduced at 350°C under hydrogen to obtain a single-component nickel tubular diffusion electrode A3 with a tube diameter of 5 mm, a wall thickness of 100 μm, and a pore diameter of 10 μm.
[0063] Example 5
[0064] Commercially available polyethyleneimine was dried overnight at 60°C. Iron powder with a particle size of 20 μm was mixed with N-methylpyrrolidone and uniformly dispersed by ultrasonication. The dried polyethyleneimine was then added to the mixture of iron powder and N-methylpyrrolidone, heated and stirred until the polyethyleneimine was completely dissolved (the mass ratio of iron powder to polyethyleneimine to N-methylpyrrolidone was 20:3:10). After cooling, a casting solution was obtained. The casting solution was transferred to an extrusion machine and extruded at room temperature to produce a polymer-containing iron tubular diffusion electrode precursor. Finally, the iron tubular diffusion electrode precursor was calcined at 1000°C in air and then reduced at 700°C under hydrogen to obtain a single-component iron tubular diffusion electrode A4 with a tube diameter of 8 mm, a wall thickness of 200 μm, and a pore diameter of 15 μm.
[0065] Example 6
[0066] Commercially available polyethyleneimine was dried overnight at 60°C. Copper powder with a particle size of 50 μm was mixed with N-methylpyrrolidone and uniformly dispersed by ultrasonication. The dried polyethyleneimine was then added to the mixture of copper powder and N-methylpyrrolidone and heated and stirred until the polyethyleneimine was completely dissolved (the mass ratio of copper powder to polyethyleneimine to N-methylpyrrolidone was 25:5:15). After cooling, a casting solution was obtained. The casting solution was transferred to an extruder and extruded at room temperature to produce a polymer-containing copper tubular diffusion electrode precursor. Finally, the copper tubular diffusion electrode precursor was calcined at 300°C in air and then reduced at 300°C under hydrogen to obtain a single-component copper tubular diffusion electrode A5 with a tube diameter of 10 mm, a wall thickness of 300 μm, and a pore diameter of 20 μm.
[0067] Example 7
[0068] Commercially available polyethyleneimine was dried overnight at 60°C. Nickel oxide powder with a particle size of 1 μm was then mixed with N-methylpyrrolidone and uniformly dispersed by ultrasonication. The dried polyethyleneimine was then added to the mixture of nickel oxide powder and N-methylpyrrolidone, heated and stirred until the polyethyleneimine was completely dissolved (the mass ratio of nickel oxide powder to polyethyleneimine to N-methylpyrrolidone was 32:10:20). After cooling, a casting solution was obtained. The casting solution was transferred to an extruder and extruded at room temperature to obtain a polymer-containing nickel tubular diffusion electrode precursor. Finally, the nickel tubular diffusion electrode precursor was calcined at 900°C in air and then reduced at 350°C under hydrogen to obtain a single-component nickel tubular diffusion electrode A6 with a tube diameter of 4.5 mm, a wall thickness of 90 μm, and a pore diameter of 9 μm.
[0069] Example 8
[0070] Commercially available polyethyleneimine was dried overnight at 60°C. Iron oxide powder with a particle size of 20 μm was mixed with N-methylpyrrolidone and uniformly dispersed by ultrasonication. The dried polyethyleneimine was then added to the mixture of iron oxide powder and N-methylpyrrolidone, heated and stirred until the polyethyleneimine was completely dissolved (the mass ratio of iron oxide powder to polyethyleneimine to N-methylpyrrolidone was 20:3:10). After cooling, a casting solution was obtained. The casting solution was transferred to an extruder and extruded at room temperature to produce a polymer-containing iron tubular diffusion electrode precursor. Finally, the iron tubular diffusion electrode precursor was calcined at 1000°C in air and then reduced at 700°C under hydrogen to obtain a single-component iron tubular diffusion electrode A7 with a tube diameter of 8.1 mm, a wall thickness of 210 μm, and a pore diameter of 15.1 μm.
[0071] Example 9
[0072] Commercially available polyethyleneimine was dried overnight at 60°C. Copper oxide powder with a particle size of 50 μm was mixed with N-methylpyrrolidone and uniformly dispersed by ultrasonication. The dried polyethyleneimine was then added to the mixture of copper oxide powder and N-methylpyrrolidone, heated and stirred until the polyethyleneimine was completely dissolved (the mass ratio of copper oxide powder to polyethyleneimine to N-methylpyrrolidone was 25:5:15). After cooling, the resulting casting solution was transferred to an extruder and extruded at room temperature to produce a polymer-containing copper tubular diffusion electrode precursor. Finally, the copper tubular diffusion electrode precursor was calcined at 350°C in air and then reduced at 350°C under hydrogen to produce a single-component copper tubular diffusion electrode A8 with a tube diameter of 9.5 mm, a wall thickness of 285 μm, and a pore diameter of 17 μm.
[0073] Table 1 Parameters and results of Examples 2 to 9
[0074] As shown in Table 1, by changing the precursor particle size, casting liquid ratio and thermal curing temperature to control the rate of powder particles forming sintering necks, the number and pore size of the pores in the porous layered structure of the tubular diffuse electrode side wall can be controlled.
[0075] Example 10 of the present application provides an application of tubular diffusion electrodes A1-A8 prepared using Examples 2-9.
[0076] Example 10
[0077] An application of a tubular diffusion electrode for CO2 electroreduction, wherein the tubular diffusion electrode serves as both a CO2 overflow device and a working electrode to catalyze CO2 electroreduction, and the specific steps are as follows:
[0078] Epoxy resin is used to encapsulate one end of each tubular diffusion electrode A1-A8 to form a one-end encapsulated diffusion electrode section 4. The unencapsulated end of the diffusion electrode section 4 is connected to a nut 6 via a connector 5, which in turn connects to the external CO2 gas line. The assembled structure of the encapsulated electrodes is shown in Figure 3.
[0079] Prepare an H-type electrolytic cell containing 0.1 mol / L KHCO3 catholyte;
[0080] Eight tubular diffusion electrodes are used for CO2 electroreduction, including:
[0081] First, CO2 is continuously introduced into the tubular diffusion electrode from the inlet of the gas channel at the unpackaged end, forcing the introduced CO2 to diffuse through the porous layered structure to the electrode surface;
[0082] Then, the electrode is placed in the cathode electrolyte and activated. Those skilled in the art will understand that the specific operations of the activation treatment include: testing the window voltage of the electroreduction by power-on and activating the surface material of the catalyst;
[0083] Finally, CO2 was continuously introduced into the electrolyte, and constant potential electrolysis was used to electrocatalyze CO2 reduction at a voltage of -1.3 V (vs. RHE) for 60 min.
[0084] The product compositions of the electroreduction at tubular diffusion electrodes A1-A8 were determined online by gas chromatograph, and the CO Faraday efficiencies were 45.6%, 42.3%, 50.3%, 52.7%, 62.5%, 49.7%, 51.9% and 63.1%, respectively.
[0085] Compared with the multi-component composition of traditional diffusion electrodes, the CO2 electroreduction tubular diffusion electrode of the present invention is composed only of metal, and has electrical conductivity, catalysis and gas diffusion properties. It is not easy for the electrode to loosen or degrade during long-term electrolysis of CO2 in a highly alkaline environment, and can operate stably, showing great commercial application potential.
[0086] Those skilled in the art will understand that the foregoing descriptions are merely preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art will be able to modify the technical solutions described in the foregoing embodiments or substitute equivalents for some of the technical features. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention shall be included within the scope of protection of the present invention.
Claims
1. A tubular diffusion electrode for CO2 electroreduction, characterized in that: The tubular diffusion electrode is made of metal powder or metal oxide powder as a precursor, and is obtained by extrusion molding and thermal curing. A plurality of gas channels extending along the axial direction are formed in the tubular diffusion electrode, and a porous layered structure is formed on the side wall of the gas channel. The porous layered structure is a layered structure with a large number of small holes distributed therein, and the number and pore size of the small holes can be controllably adjusted by changing the particle size of the precursor and the thermal curing temperature.
2. The tubular diffusion electrode for CO2 electroreduction according to claim 1, characterized in that: The pores in the porous hierarchical structure have a pore size of 0.5 to 20 μm.
3. The tubular diffusion electrode for CO2 electroreduction according to claim 1, characterized in that: The outer contour of the cross section of the tubular diffusion electrode is circular with a diameter of 1 to 10 mm. The plurality of gas channels extending along the axial direction are evenly distributed along the circumference, the cross section of the gas channel is elliptical, and the wall thickness of the gas channel is 40 to 300 μm.
4. A method for preparing a tubular diffusion electrode for CO2 electroreduction according to any one of claims 1 to 3, characterized in that: include: The polyethyleneimine was dried at 60°C; Using metal powder or metal oxide powder as a precursor, mixing the precursor with N-methylpyrrolidone, and uniformly dispersing the precursor by ultrasonication; Adding dry polyethyleneimine to the mixture of the precursor and N-methylpyrrolidone, heating and stirring to completely dissolve the polyethyleneimine, and cooling to obtain a pipe casting liquid; The casting liquid is transferred to an extrusion device and extruded at room temperature to obtain a tubular diffusion electrode precursor containing a polymer; The tubular diffusion electrode precursor is calcined at high temperature and then reduced in a hydrogen atmosphere to obtain the tubular diffusion electrode.
5. The method for preparing a tubular diffusion electrode for CO2 electroreduction according to claim 4, characterized in that: The mass ratio of the precursor, polyethyleneimine and N-methylpyrrolidone in the pipe casting liquid is (20-32): (3-10): (10-20).
6. The method for preparing a tubular diffusion electrode for CO2 electroreduction according to claim 4, characterized in that: The metal powder is at least one of silver, gold, nickel, iron and copper, and the metal oxide powder is at least one of nickel oxide, ferroferric oxide and copper oxide.
7. The method for preparing a tubular diffusion electrode for CO2 electroreduction according to claim 4, characterized in that: The particle size of the precursor ranges from 50 μm to 150 nm.
8. The method for preparing a tubular diffusion electrode for CO2 electroreduction according to claim 4, characterized in that: The calcination temperature of the tubular diffusion electrode precursor is 300-1000°C, and the reduction temperature is 300-700°C.
9. Use of a tubular diffusion electrode for CO2 electroreduction as claimed in any one of claims 1 to 3, characterized in that: The tubular diffusion electrode serves as both a CO2 overflow device and a working electrode to catalyze CO2 electroreduction. The specific steps are as follows: Encapsulating one end of the tubular diffusion electrode, and continuously introducing CO2 from the inlet of the gas channel at the unencapsulated end, forcing the introduced CO2 to continuously diffuse through the porous layered structure to the electrode surface; Under the condition of continuous CO2 flow, a tubular diffusion electrode with one end sealed is placed in the cathode electrolyte to activate it. The product is treated with a constant potential electrolysis to achieve efficient CO2 electroreduction.
10. The use of the tubular diffusion electrode for CO2 electroreduction according to claim 9, characterized in that: One end of the tubular diffusion electrode is encapsulated by using epoxy resin glue.
Citation Information
Patent Citations
Gas diffusion electrode for preparing carbon monoxide by electrolyzing carbon dioxide and preparation method of gas diffusion electrode
CN113445064A
Preparation method and application of silver hollow fiber electrode
CN114959761A
Tubular diffusion electrode for carbon dioxide electroreduction and preparation and application thereof
CN116288463A
Electrode-supported tubular solid-oxide electrochemical cell
US20170101719A1
Gas diffusion electrode for carbon dioxide treatment, method for production thereof, and electrolysis cell having a gas diffusion electrode
US20210207277A1
Cited By
Preparation method of flow-through gas diffusion electrode for electrochemical CO2 reduction
CN119615227A