Modified polyphenylene sulfide and modification method therefor, polyphenylene sulfide solid separator, pre-prepared zinc salt separator and manufacturing method therefor, injection-ready zinc-manganese secondary battery and manufacturing and application methods therefor

Through modified polyphenylene sulfide and prefabricated zinc salt separator technology, the problems of short life, poor low-temperature performance and uneven electrolyte infiltration of zinc-manganese secondary batteries have been solved, achieving higher battery consistency and safety, and simplifying manufacturing process.

WO2024212909A1PCT designated stage expired Publication Date: 2024-10-17JIANGSU UNIV
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/086497
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-01-12
Filing Date
2024-04-08
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Existing zinc-manganese secondary batteries have short lifespan, poor low-temperature performance, uneven electrolyte infiltration, poor battery consistency, and potential safety hazards during storage and transportation.

Method used

Modified polyphenylene sulfide is used to generate chlorocatechol structural molecules through hydrothermal synthesis of chlorine reduction and hydrogenation reactions to improve the adsorption performance of the separator. The electrolyte is pre-filled into the separator through a prefabricated zinc salt separator to avoid electrolyte injection into storage and storage. During transportation, the electrodes were prepared using a semi-dry method to improve porosity and cycling stability.

Benefits of technology

It extends the life of zinc-manganese secondary batteries, improves low-temperature performance, simplifies the manufacturing process, enhances battery storage and transportation safety, and improves production efficiency and battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024086497_17102024_PF_FP_ABST
    Figure CN2024086497_17102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided are a modified polyphenylene sulfide and a modification method therefor, a polyphenylene sulfide solid separator, a pre-prepared zinc salt separator and a manufacturing method therefor, and an injection-ready zinc-manganese secondary battery and manufacturing and application methods therefor. Tetra-chloro-benzoquinone in a polyphenylene sulfide powder is subjected to chlorine reduction and hydrogenation reactions via hydrothermal synthesis to generate chlorocatechol structural molecules, and the adsorption performance of the polyphenylene sulfide-based solid separator on harmful molecules is improved; also, upon integration into a battery assembly process, weld points are protected, and in a chemical synthesis process, a method of firstly injecting an aqueous solution electrolyte and then adding an alcohol is utilized, the cycling stability of the battery is improved, and the operating temperature interval of the battery is widened. In the manufacturing process of the pre-prepared zinc salt separator, an electrolyte zinc salt is pre-placed into a composite glue solution of a solid separator and upper and lower supporting separators, the problem where high-concentration electrolytes in zinc-manganese secondary batteries find difficulty in uniformly infiltrating into battery electrode pieces is solved, and the production efficiency and the battery performance of zinc-manganese secondary batteries are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Modified polyphenylene sulfide and modification method thereof, polyphenylene sulfide solid diaphragm, prefabricated zinc salt diaphragm and manufacturing method thereof, note zinc-manganese secondary battery and manufacturing and application method thereof Technical Field

[0001] The present invention belongs to the technical field of secondary batteries, and specifically relates to a modified polyphenylene sulfide and a modification method thereof, a polyphenylene sulfide solid diaphragm, a prefabricated zinc salt diaphragm and a manufacturing method thereof, a zinc-manganese secondary battery and its manufacturing and application methods. Background Art

[0002] Aqueous zinc-manganese secondary batteries (Zn-Mn batteries) have attracted widespread attention from researchers in recent years due to their safety, environmental friendliness, abundant resources, and low cost. Commercial aqueous Zn-Mn batteries at the ampere-hour level are difficult to apply and promote due to their short lifespan and poor low-temperature performance. Existing improvements involve adding low-temperature additives, such as alcohols, PEG, and PVA, to the aqueous electrolyte to form a eutectic solution, effectively lowering the freezing point of the electrolyte and thus developing low-temperature Zn-Mn secondary batteries. However, the addition of additives increases the likelihood of side reactions. In particular, significant capacity decay can be observed during the initial formation cycle. This is due to the harmful components produced by these side reactions, which shuttle between the positive and negative electrodes and degrade each other. Further improvements are needed. Furthermore, patent ZL202110122474.3 mentions the use of tetrachlorobenzoquinone as an anion adsorbent, which forms a dipole adsorption with the harmful components, increasing the cationic transference number of the separator and effectively suppressing the occurrence of side reactions. However, tetrachlorobenzoquinone contains a high chlorine content, and over long periods of cycling, the chloride ions can cause corrosion and failure of the current collector.

[0003] At present, the production process of aqueous battery electrodes generally adopts wet coating. Patent 202211223026.3 and Patent 202210355256.9 propose the use of a semi-dry process to manufacture electrodes for zinc-manganese secondary batteries. The dry electrode manufacturing process for zinc-manganese secondary batteries can effectively avoid a series of problems such as uneven slurry, difficult viscosity control, complex solvent removal, stratification of electrode components and powder loss of pole pieces during the wet coating process. However, it also brings challenges. For example, the porosity of dry electrodes is low, less than 30%, resulting in low injection efficiency. In particular, the concentration of zinc-manganese secondary battery electrolyte is high (>2mol / L) and the viscosity is very high, making it difficult to achieve uniform infiltration, resulting in very uneven distribution of electrolyte in the battery pole piece and separator. To solve this problem, the infiltration effect of the battery is generally improved by increasing the infiltration time and raising the shelf temperature, but this will undoubtedly waste a lot of time and energy, greatly reducing the production efficiency of the battery.

[0004] Furthermore, in the field of electrochemical energy storage, ensuring long-term, effective storage and safe transportation of batteries are also pressing challenges. Existing storage methods typically pre-inject electrolyte into the battery, which poses safety risks during transportation and storage. Over extended storage time, the electrolyte in the battery decomposes, significantly reducing its capacity and potentially causing a short circuit, resulting in wasted resources.

[0005] Chinese invention patent 202110380015.5 and patent application 202210444350.1 provide a sandwich structure composite diaphragm based on polyphenylene sulfide solid diaphragm. Although this diaphragm structure can effectively avoid dendrites, it still cannot solve the wetting problem of the aqueous diaphragm, resulting in uneven distribution of zinc salts inside the ampere-hour zinc-manganese secondary battery and poor battery consistency.

[0006] Therefore, it is necessary to develop a new type of separator and secondary battery to solve the above problems.

[0007] Summary of the Invention

[0008] On one hand, to address the short lifespan and poor low-temperature performance of commercial ampere-hour-class aqueous zinc-manganese secondary batteries, the present invention provides a modified polyphenylene sulfide suitable for long-life, wide-temperature-range ampere-hour-class zinc-manganese secondary batteries and a method for manufacturing the same. By hydrothermally synthesizing tetrachlorobenzoquinone in the polyphenylene sulfide powder through a chlorine-reducing and hydrogenation reaction to generate chlorocatechol-structured molecules, the modified polyphenylene sulfide-based solid-state separator improves the adsorption performance of harmful molecules. This, combined with solder joint protection during battery assembly and a formation method that first injects an aqueous electrolyte followed by alcohol addition, improves battery cycle stability, broadens the battery's service temperature range, and enhances its low-temperature resistance.

[0009] A polyphenylene sulfide modification method suitable for a solid-state separator of an ampere-hour-level zinc-manganese secondary battery with a long life and a wide temperature range is disclosed. The method comprises: mixing polyphenylene sulfide powder, tetrachlorobenzoquinone, and deionized water in a mass ratio of 10:0.25-0.75:1-12, and subjecting the mixture to a hydrothermal reaction at 180-240°C. During the hydrothermal reaction, chloride ions are removed from the tetrachlorobenzoquinone molecules, while hydroxyl groups are added, thereby generating molecules with a chlorocatechol structure.

[0010] Furthermore, the constant temperature time of the hydrothermal reaction temperature is 1-4 hours, and the reaction atmosphere is air, oxygen, nitrogen or argon.

[0011] The modified polyphenylene sulfide prepared by the polyphenylene sulfide modification method is characterized in that molecules with chlorocatechol structures are loaded in the polyphenylene sulfide solid diaphragm; the chlorocatechol molecules are one or a mixture of 2,5-dichlorohydroquinone, 2,3,5,6-tetrachlorophenol, 3,4,5-trichlorocatechol, tetrachlorohydroquinone, 3,4,6-trichlorocatechol, etc.

[0012] A polyphenylene sulfide solid diaphragm made from the modified polyphenylene sulfide.

[0013] Furthermore, the polyphenylene sulfide solid diaphragm made of the modified polyphenylene sulfide has zinc ion selective permeability.

[0014] The present invention also provides a prefabricated zinc salt separator, a pre-filled zinc-manganese secondary battery, and a method for manufacturing the same. During the manufacturing process, the prefabricated zinc salt separator incorporates the electrolyte zinc salt into a composite adhesive solution formed by the solid separator and upper and lower support separators. This solves the problem of high-concentration electrolyte in zinc-manganese secondary batteries having difficulty evenly infiltrating the battery electrodes. Furthermore, the prefabricated zinc-manganese secondary battery can be manufactured without the need for electrolyte refilling during storage and transportation, thereby improving the production efficiency and battery performance of the zinc-manganese secondary battery.

[0015] The method for manufacturing a prefabricated zinc salt diaphragm is characterized by comprising the following steps:

[0016] (1) After one of the polyphenylene sulfide solid diaphragm A and the upper support diaphragm B is dipped in or coated with glue C, the two are laminated together so that the glue C is located between the polyphenylene sulfide solid diaphragm A and the upper support diaphragm B, and then the upper support diaphragm B and the solid diaphragm A are composited by rolling; the composited upper support diaphragm B and the solid diaphragm A are dried to obtain a double-layer prefabricated zinc salt diaphragm D;

[0017] (2) After the exposed surface of the polyphenylene sulfide solid diaphragm A of the double-layer prefabricated zinc salt diaphragm D and one of the lower support membrane F are dipped in or coated with glue E, the two are laminated so that the glue E is located in the glue tank where the glue E is stored, the glue E is dipped in and the excess glue is scraped off with a scraper, or the glue E is placed between the polyphenylene sulfide solid diaphragm A and the lower support membrane F, and then the lower support membrane F is composited with the double-layer prefabricated zinc salt diaphragm D by rolling, and the composite three-layer diaphragm is dried to obtain a prefabricated zinc salt diaphragm H;

[0018] The upper supporting membrane B and the lower supporting membrane F are both porous membranes, and the glue C and glue E are mixtures of organic adhesive and / or inorganic adhesive, electrolyte zinc salt and solvent.

[0019] Furthermore, the mass ratio of the organic binder, the inorganic binder, the electrolyte salt and the solvent is 0-10:0-10:10-80:10-80.

[0020] Furthermore, the organic adhesive is a mixture of one or more of polyvinyl alcohol (PVA), polyacrylate (PAA), and polytetrafluoroethylene (PTFE); the inorganic adhesive is a mixture of one or more of sodium bentonite, zinc dihydrogen phosphate, and lithium montmorillonite powder; the electrolyte zinc salt is a mixture of one or more of zinc trifluoromethanesulfonate, zinc sulfate, zinc chloride, and zinc perchlorate; and the solvent is a mixture of one or more of deionized water, nitrogen methyl pyrrolidone (NMP), alcohol, and propylene glycol.

[0021] Furthermore, the thickness of the polyphenylene sulfide solid membrane A is 5-60 μm, and the porous membrane is one of polyethylene membrane (PE), polypropylene membrane (PP), cellulose membrane, non-woven membrane, and PET membrane, and its thickness is 3-30 μm.

[0022] Furthermore, the dosage of the glue solution C and glue solution E is 5-30 mg / cm2; the drying temperature for both times is 50-100°C; after drying, the dry glue single layer load is 2-15 mg / cm2, and the thickness of the prefabricated zinc salt membrane H is 70-200 μm.

[0023] The prefabricated zinc salt diaphragm manufactured by the manufacturing method of the prefabricated zinc salt diaphragm is characterized in that it includes a polyphenylene sulfide solid diaphragm A and an upper supporting diaphragm B and a lower supporting diaphragm F located on both sides of the polyphenylene sulfide solid diaphragm A, and a mixture including an organic adhesive and / or an inorganic adhesive and an electrolyte salt is filled between the upper supporting diaphragm B, the lower supporting diaphragm F and the polyphenylene sulfide solid diaphragm A, and the mass ratio of the solid content is 0-10:0-10:10-80:10-80.

[0024] Furthermore, the polyphenylene sulfide solid diaphragm A is made of the modified polyphenylene sulfide.

[0025] Furthermore, the manufacturing equipment of the polyphenylene sulfide solid diaphragm A includes a powder processing system, a high-speed shearing machine, a screw extruder, a horizontal cold roller press, and a horizontal hot roller press;

[0026] The powder processing system includes an air compressor, an air storage tank, a cold dryer, a drying adsorption tower, a purification column, an air preheating system, a powder heating system, a supersonic shear mixer, and a gas-solid separation tower that are connected in sequence; the supersonic shear mixer has a semi-closed cavity, the air outlet of the purification column is connected to the air inlet of the semi-closed cavity of the supersonic shear mixer, and the air preheating system is arranged on the air pipeline between the purification column and the supersonic shear mixer; the powder heating system is arranged at the discharge port of the semi-closed cavity of the supersonic shear mixer; the discharge port of the semi-closed cavity of the supersonic shear mixer is connected to the gas-solid separation tower through a pipeline, and the gas-solid separation tower is provided with an air outlet at the top, a discharge port at the bottom, and an air hammer air inlet in the middle;

[0027] The powder processed by the powder processing system is sent to the high-speed shearing machine and enters the screw extruder after shearing. The horizontal cold roller press and the horizontal hot roller press are arranged downstream of the screw extruder in sequence, and a heated conveying guide rail is set between the horizontal cold roller press and the horizontal hot roller press.

[0028] Furthermore, there are multiple drying adsorption towers, which are arranged in parallel and respectively connected to the air outlet of the cold dryer and the air inlet of the purification column; the gas source of the air hammer is the dry compressed air bypass after the purification column, and the air hammer function is achieved by intermittently releasing compressed air.

[0029] Furthermore, the method for manufacturing the polyphenylene sulfide solid diaphragm A comprises the following steps:

[0030] (1) Flour making:

[0031] Dissolving metal chloride A in deionized water to prepare solution B, mixing tetrachlorobenzoquinone with polyphenylene sulfide powder to prepare mixed powder C, mixing solution B and mixed powder C to prepare slurry D, charging slurry D into a closed reactor for hydrothermal reaction, and washing the powder after the reaction to neutral state and drying it to prepare powder E;

[0032] (2) Fibrosis:

[0033] The polytetrafluoroethylene powder and powder E are mixed uniformly in a mixer to form powder F, and the mixing process is carried out under the temperature condition that the polytetrafluoroethylene is in a glassy state;

[0034] After being compressed by the air compressor, cold-dried, dry-adsorbed, purified, and preheated, the dry air G passes through the nozzle and enters the semi-enclosed cavity, where it is accelerated to supersonic speed, forming a supersonic jet H of extremely dry air.

[0035] Preheated powder F is added to a semi-enclosed cavity and sheared by a supersonic jet H of extremely dry air. The molecular chains of polytetrafluoroethylene in powder F stretch and open, forming a physical bond with the powder in F without chemical reaction, thus obtaining powder I.

[0036] The powder I is blown into the solid-gas separation tower along with the air flow. There is a dust removal filter inside the separation tower to separate the solid powder and gas. The gas is discharged directly, and the powder adhering to the filter is blown by the air hammer into the receiving bucket below.

[0037] (3) Film making:

[0038] The powder I is added to a high-speed shearing machine for secondary fiberization. After discharge, it enters a screw extruder and is extruded into multiple continuous thick strips or continuous thick cakes J. It then enters a horizontal cold roller press for primary thinning. After thinning, it enters a heated conveyor rail, is heated and fed into a horizontal hot roller press for secondary thinning, and the two edges are cut off to form a finished solid diaphragm L, which is then wound.

[0039] Furthermore, the metal chloride A in the powder making process is one or a mixture of lithium chloride, sodium chloride, zinc chloride, magnesium chloride, and aluminum chloride; the polyphenylene sulfide powder is a cross-linked highly crystalline polyphenylene sulfide powder with a crystallinity of >60% and a D50 of 3-25 μm; the mass ratio of the metal chloride, deionized water, tetrachlorobenzoquinone, and polyphenylene sulfide is 0-3:3-30:0.1-0.75:5-15; the atmosphere in the hydrothermal reactor is air or argon, the hydrothermal reaction temperature is 150-250° C., and the hydrothermal reaction time is 1-4 hours; and the volume filling rate of the hydrothermal reaction is 20%-70%.

[0040] Furthermore, during the fiberization process, the relative humidity (RH) of the dry air G at room temperature of 25°C is <10%; the power of the air compressor is greater than or equal to 15kW, and preferably greater than 30kW for continuous production; the dew point of the supersonic jet H of the ultra-dry air is lower than -40°C; the dry adsorption process is to use multiple dry adsorption towers containing molecular sieves, the total weight of the molecular sieves is greater than 200kg, and the multiple dry adsorption towers alternately work and regenerate, and the alternation time is 3-12 minutes.

[0041] Furthermore, during the fiberization process, the air is preheated to a temperature of 30-60°C before entering the nozzle, and the powder F is preheated to a temperature of 40-220°C before entering the semi-enclosed cavity.

[0042] Furthermore, in the film-making process, the shape of the multiple continuous thick strips or continuous thick cakes J is determined by the extrusion head mold of the screw extruder, and the diameter of the continuous thick strips or the thickness of the continuous thick cakes is between 3-12 mm; the roller surface temperature of the horizontal cold roller press is -10-30°C; the thickness after the first thinning is 0.3-1.5 mm; the temperature of the heated conveying guide rail is 90-150°C; the roller surface temperature of the horizontal hot roller press is 110-160°C; the thickness after the second thinning is 5-60 μm.

[0043] The method for manufacturing a spare zinc-manganese secondary battery made of the prefabricated zinc salt diaphragm is characterized in that the prefabricated zinc salt diaphragm H is placed between the manganese oxide positive electrode and the zinc negative electrode, and the tabs are welded, and a battery cell is prepared by using a stacking machine or a winding machine, and is placed in a battery shell or an aluminum-plastic film bag, packaged for standby use, and stored; and a sealable liquid injection port is left on the battery shell or the aluminum-plastic film bag.

[0044] Furthermore, the manganese oxide positive electrode is a manganese dioxide dry electrode manufactured using a semi-dry process, and the manganese oxide is one or a mixture of α-MnO2, β-MnO2, γ-MnO2, δ-MnO2, Mn2O3, Mn3O4, and LiMn2O4; the zinc negative electrode is one of a zinc powder dry electrode, zinc foil, and galvanized copper foil manufactured using a semi-dry process.

[0045] Furthermore, after the tab welding is completed, the welding point is provided with water-blocking insulation protection.

[0046] Furthermore, the water-blocking insulation protection of the welding point is achieved by wrapping it with a water-blocking insulation tape, coating it with an aluminum oxide layer, or applying resin for protection; the resin is one or more of epoxy resin, phenolic resin, furan resin, and unsaturated polyester; the tab is a nickel tab, a copper tab, a titanium tab, or a molybdenum tab.

[0047] Furthermore, after obtaining the battery cell, an external supporting mechanism is required to increase the preload force between the prefabricated zinc salt separator H, the manganese oxide positive electrode and the zinc negative electrode, and reduce the inter-electrode distance so that the inter-electrode distance is controlled within 50-120 μm.

[0048] Furthermore, the outer packaging of the battery shell adopts a water-blocking, gas-blocking and acid-corrosion-resistant material, and the water-blocking, gas-blocking and acid-corrosion-resistant material is a non-porous film.

[0049] Furthermore, the non-porous membrane is preferably a composite membrane of one or more of biaxially oriented polypropylene film (BOPP), cast polypropylene film (CPP), polyethylene terephthalate (PET), polyethylene (PE), and polypropylene (PP) non-porous membranes.

[0050] Furthermore, the manufacturing method of the manganese oxide positive electrode includes the following steps: first, after mixing manganese dioxide and polytetrafluoroethylene, using dry supersonic jet gas to open the molecular chains of polytetrafluoroethylene and physically adhere to the positive electrode material powder below the glass transition temperature of polytetrafluoroethylene, then spraying alcohol solution on the fiberized powder, and after mixing and shearing granulation, hot rolling to form a positive electrode film, and then cold rolling multiple layers of positive electrode film to form a composite positive electrode self-supporting film with a thickness of 100-150 μm, and finally combining the composite positive electrode self-supporting film with a sandblasted stainless steel foil with a glue-coated surface through a hot rolling machine.

[0051] Furthermore, the method for manufacturing the zinc negative electrode comprises the following steps:

[0052] Mix zinc powder, conductive agent, toughening conductive agent, cationic slow-release agent and hydrogen evolution inhibitor in a mixer to form powder A;

[0053] The polytetrafluoroethylene powder and powder A are mixed uniformly in a mixer to form powder B; the mixing process is carried out at a temperature where the polytetrafluoroethylene (PTFE) is in a glassy state;

[0054] The powder B and the alcohol-water mixed solvent are continuously rubbed in a ball mill under high-speed rotation by the ball milling beads, so that the PTFE is drawn into a network structure. The molecular chains of the polytetrafluoroethylene in the powder B are extended and opened, forming physical adhesion with the powder in the powder A. The hydrogen evolution inhibitor reacts with the surface of the zinc powder to undergo a reduction reaction. After the above process is completed, the micelle C is obtained by filtration.

[0055] The micelle C is formed into a uniform micelle after banburying, and then sheared and granulated to produce millimeter-sized granules E with uniform size;

[0056] The granular material E is hot-pressed into a negative electrode film F by a horizontal hot roller press, and then rolled up using a porous release paper as a support belt. The entire roll of negative electrode film F covered with the release paper is dried to remove some of the solvent.

[0057] Using a hot pressing lamination process, the semi-dried negative electrode film F after removing the release paper is thermally laminated on both sides of the adhesive-coated stainless steel foil to form an electrode;

[0058] Furthermore, the zinc powder is powdered particles with a particle size of 5-20 μm; the conductive agent is one or both of super-P and ECP; the toughening conductive agent is one or both of artificial graphite and high-purity graphite; the cationic slow-release agent is an inorganic powder that is electronegative and expands in volume when exposed to water; the hydrogen evolution inhibitor is a metal compound that can undergo a reduction reaction with the zinc powder in an alcohol-water solvent; and the weight percentages of the zinc powder, the conductive agent, the toughening conductive agent, the cationic slow-release agent, the polytetrafluoroethylene, and the hydrogen evolution inhibitor powder are as follows: 60%-90%: 1%-10%: 1%-10%: 1%-10%: 3%-15%: 0.1%-5%.

[0059] Furthermore, the cationic sustained-release agent is one or more of bentonite, montmorillonite powder, illite powder, kaolin powder, and halloysite powder; and the hydrogen evolution inhibitor is one or more of indium chloride, copper chloride, indium sulfate, and copper sulfate.

[0060] Furthermore, the alcohol-water mixed solvent is a mixed solvent of water and isopropyl alcohol, propylene glycol or ethanol, and the volume percentage of water to alcohol is: 40%-80%: 20%-60%; the solid content of the uniform micelle is 40%-60%.

[0061] Furthermore, the granular material E is rolled once on a horizontal hot roller press to achieve a negative electrode film F with a thickness of 90-200 μm, and the hot roller pressing temperature is 55-95° C.

[0062] Furthermore, during the thermal lamination of the semi-dried negative electrode film F with the stainless steel foil, the adhesive-coated stainless steel foil is sandwiched between two sheets of negative electrode film F, each with its release paper removed. The sheets are unwound at the same speed and then fed into two counter-rotating horizontal hot roller presses. The pressing temperature is 30-120°C. The roller gap width is adjusted to control the pressure, ensuring that the negative electrode film F is laminated to the adhesive-coated stainless steel foil. Excessive deformation of the negative electrode film F, which could potentially break the stainless steel foil, is avoided due to excessive roller pressure.

[0063] Furthermore, the glue-coated stainless steel foil is obtained by printing a highly conductive paste on both sides of the stainless steel foil using a gravure printing machine. The surface of the stainless steel foil needs to be sandblasted before glue coating to remove surface rolling oil. The highly conductive paste is composed of high-purity graphite, a non-hydrophilic adhesive and a non-aqueous solvent.

[0064] The remarkably zinc-manganese secondary battery manufactured by the remarkably zinc-manganese secondary battery manufacturing method is characterized in that it consists of a manganese oxide positive electrode, a zinc negative electrode, a three-layer prefabricated zinc salt diaphragm H, and a battery shell or an aluminum-plastic film bag with a sealable liquid injection port. The manganese oxide positive electrode, the zinc negative electrode, and the three-layer prefabricated zinc salt diaphragm H are placed in the battery shell or the aluminum-plastic film bag after the tabs are welded.

[0065] The application method of the remarkably zinc-manganese secondary battery is characterized in that the remarkably zinc-manganese secondary battery does not require liquid injection during storage and transportation; before being put into use, pure water, seawater or a dilute electrolyte is injected into the battery; preferably, the dilute electrolyte is a salt solution of one or more of zinc sulfate, sodium sulfate, magnesium sulfate, sodium chloride, and zinc trifluoromethanesulfonate with a concentration of 0.01 mol / L to 1 mol / L, and the solvent is a mixture of one or more of water, ethanol, methanol, propylene glycol, isopropyl alcohol, and glycerol; preferably, the amount of injected liquid is 1-20 mL / Ah.

[0066] The formation method of the remarked zinc-manganese secondary battery is characterized in that, during the battery formation process, an electrolyte containing only water as a solvent is first injected into the secondary battery, and a discharge is performed once with a small current formation of a current density of 1-20 mA / g, and then 0-40 cycles of charge and discharge are performed. After that, an organic solvent is injected in the discharged state of the battery, and then vacuum packaging is performed. The organic solvent is an organic solvent that can lower the freezing point of water after mixing with water, and the volume ratio of the aqueous solution electrolyte to the organic solvent is 5:0.3-5.

[0067] Furthermore, the electrolyte with water as solvent is a 2-3 mol / L aqueous solution of zinc trifluoromethanesulfonate, a 2-3 mol / L aqueous solution of zinc sulfate or a 2-3 mol / L aqueous solution of zinc chloride; and the injection volume is 3-10 mL / Ah.

[0068] Furthermore, the organic solvent is alcohol, dimethyl sulfoxide, propylene carbonate, or acetonitrile.

[0069] Furthermore, the alcohol is one or a mixture of methanol, isopropanol, ethylene glycol, propylene glycol, and glycerol.

[0070] The beneficial effects of the present invention are as follows:

[0071] The method for manufacturing a prefabricated zinc salt separator described herein prefabricates an electrolyte zinc salt into a composite adhesive solution formed between a solid separator and upper and lower support separators during separator manufacturing, thereby forming a prefabricated zinc salt composite separator. This provides a zinc-manganese secondary battery manufactured with this prefabricated zinc salt separator with the advantage of not requiring electrolyte injection during storage and transportation. When the zinc-manganese secondary battery is put into use, it only requires injection of pure water, seawater, or a low-viscosity dilute electrolyte. This not only effectively solves the problem of high-concentration electrolyte difficulty in uniformly infiltrating the interior of the battery electrodes during zinc-manganese secondary battery manufacturing, thereby improving battery performance, but also simplifies the secondary battery manufacturing process and production efficiency, enhancing storage and transportation performance.

[0072] Furthermore, it should be noted that when using a zinc-manganese secondary battery, simply add a liquid capable of forming an aqueous electrolyte environment to the battery case or aluminum-plastic film bag to ensure normal charge and discharge. The added solution offers a wide range of options, including water, zinc-containing solutions, or solutions with different cations, such as seawater, forming dual-cationic or multi-cationic systems, which diversify the positive electrode reactions. For example, when pure water is added, zinc ions in the prefabricated zinc salt separator dissolve, leaving the electrolyte with only zinc ions. Dissolution / deposition reactions of zinc-manganese oxide occur on the surface of the manganese oxide positive electrode. When seawater is added, the dissolution of zinc ions in the prefabricated zinc salt separator and the sodium and magnesium ions in the added seawater form a multi-ion system, with the smaller sodium ions intercalating into the manganese oxide. The coexistence of ion intercalation / extraction mechanisms and dissolution / deposition mechanisms in the positive electrode can significantly increase the capacity of aqueous secondary batteries. Furthermore, the multi-cationic system can improve zinc deposition kinetics, effectively preventing dendrites and improving the system's cycling stability.

[0073] Compared with the prior art, the prefabricated zinc salt diaphragm and the pre-assembled zinc-manganese secondary battery of the present invention have the following advantages:

[0074] (1) By pre-adding electrolyte salt, it is ensured to be evenly distributed inside the battery, effectively preventing excessive growth of dendrites in specific areas.

[0075] (2) Significantly improved the battery filling efficiency and overall production efficiency.

[0076] (3) Effectively avoid the precipitation of electrolyte salts in the cycle of zinc-manganese secondary batteries, thereby extending the cycle life of the battery and improving the storage life of the battery.

[0077] The present invention discloses a method for producing a modified polyphenylene sulfide suitable for long-life, wide-temperature-range, ampere-hour zinc-manganese secondary batteries. This method utilizes a simple hydrothermal synthesis method, using inexpensive deionized water as a proton-providing reactant. During the hydrothermal reaction, tetrachloro-p-benzoquinone loses some of its chloride ions, and the quinone groups are hydrogenated to hydroxyl groups, forming electron-withdrawing groups that more readily bind to anions. The resulting chlorocatechol structures readily undergo dipole adsorption with anions, fluorides, chlorides, hydrides, and the like, thereby preventing the transport of harmful molecules between the positive and negative electrodes of the zinc-manganese secondary battery and significantly increasing the ion transference number of the polyphenylene sulfide solid-state separator. Furthermore, the resulting chlorocatechol has a lower melting point, which helps the polyphenylene sulfide separator soften at processing temperatures between 100 and 200°C, resulting in a thinner, smoother, and non-porous solid-state separator.

[0078] During the manufacturing process of the polyphenylene sulfide solid diaphragm described in the present invention, the air source used in the fiberization process is dry ambient air with a relative humidity (RH) of <10% at room temperature of 25°C. The purpose is to achieve extremely dry air with a dew point of -40°C after the cold drying and dry adsorption steps of the production line, thereby minimizing the energy consumption during the air drying process. The purpose of obtaining extremely dry air is to enable better fiberization of PTFE and prevent moisture absorption caused by high static electricity in the PTFE fibers after shear friction, which may cause subsequent film breakage. In addition, the present invention first uses a horizontal cold roller press to thin the continuous thick strips or continuous thick cakes. The temperature at this time needs to be below the softening temperature of PPS (130°C). The purpose is simply to control the uniformity of the feed during the subsequent hot roller pressing. The purpose of using a heated conveyor guide is to heat the continuous thin cake (0.3-1.5mm) after the primary thinning to above the deformation temperature of PPS. After passing through the horizontal hot roller press, the PPS crystal particles undergo thermoplastic deformation, which can be better pressed into a film. After the hot-pressed film is trimmed, the trimmed material can be recycled into a high-speed shearing machine, achieving 100% powder utilization and further reducing costs. The resulting polyphenylene sulfide solid-state separator has the following characteristics: low porosity, high electrical conductivity, high ion transference number, strong ion selectivity, and significant ion rectification, effectively suppressing metal anode dendrites.

[0079] The positive and negative electrodes of the present invention are prepared using a semi-dry process, and the powders of the positive and negative electrodes are entangled and bundled with fiberized PTFE. During the charge and discharge process, the dissolution / deposition of the positive and negative electrode materials will not cause the electrodes to become powdered. During the preparation of the semi-dry zinc powder negative electrode, the surface of the zinc powder is treated by electroless indium plating, electroless copper plating, acetic acidization or phosphorylation, which effectively inhibits hydrogen evolution of the zinc powder. A cationic chelating agent is added to the semi-dry zinc negative electrode to stabilize the changes in ion concentration in the electrolyte, thereby obtaining a more stable cycle. In addition, inorganic powders such as bentonite, montmorillonite powder, illite powder, kaolin powder, and halloysite powder are introduced into the semi-dry zinc negative electrode. When exposed to water, the volume expands several to several dozen times, effectively fixing the water content, reducing the solid content of the micelles, and preventing the micelles from sticking to the rollers during the subsequent film pressing process due to excessive solvent. During the drying process after film formation, the volume of the inorganic powders shrinks, introducing pores, thereby improving the porosity of the semi-dry electrode. Inorganic powders such as bentonite, montmorillonite powder, illite powder, kaolin powder, halloysite powder, etc. have strong electronegativity and can effectively absorb excess cations (Mn 2+ , H + , Zn 2+ ), plays the role of cation slow release, slowing down the cation (Mn 2+ , H + , Zn 2+) fluctuates greatly, stabilizes the pH value of the electrolyte, and provides high reversibility of the system. In addition, the present invention directly introduces a hydrogen evolution inhibitor during the ball milling fiberization process. While the slurry is ball milled, the hydrogen evolution inhibitor undergoes a sufficient reduction reaction with the surface of the zinc powder, fully passivates the surface of the zinc powder, and ensures that hydrogen evolution is effectively inhibited after the electrode is made. In addition, the hydrophobic effect of the PTFE entanglement network can also protect the zinc powder. The zinc negative electrode has the following characteristics: (1) it can effectively inhibit dendrites; (2) it has a cation slow release effect; (3) it has an excellent three-dimensional conductive network and many stripping / deposition active sites; (4) the PTFE entanglement network structure is stable; (5) the porosity is large; and (6) it can effectively avoid hydrogen evolution at the zinc negative electrode.

[0080] In addition, the present invention implements water-blocking and insulating protection measures on the welding points during the assembly process of the zinc-manganese secondary battery, which is very important during the cycle of the zinc-manganese secondary battery. If the welding points are in contact with the electrolyte, electrochemical corrosion is very likely to occur during the charge and discharge process, resulting in low battery energy efficiency and even short circuit failure. An external supporting mechanism is added to reduce the inter-electrode distance and strengthen the close fit between the pole pieces, thereby avoiding the side reactions of hydrogen and oxygen evolution caused by excessive inter-electrode distance. The occurrence of side reactions of the battery during the charge and discharge process is greatly avoided, thereby ensuring the cycle stability of the battery and greatly improving the electrochemical performance of the battery; without affecting the battery capacity, rate performance and energy density, the service temperature of the battery is broadened.

[0081] The present invention adopts glue-coated sandblasted stainless steel. After sandblasting, the rolling oil is removed from the surface of the stainless steel, and the rough surface has stronger adhesion with the conductive layer and the zinc powder negative electrode film. The conductive glue layer applied is a mixture of high-purity graphite and a non-hydrophilic adhesive, which can effectively prevent water from corroding the stainless steel current collector and prevent the electrode film and the current collector foil from falling off.

[0082] During the formation process of the zinc-manganese secondary battery, an electrolyte containing only water as a solvent is first injected for preliminary formation, and then an alcohol solvent is added for formation. This avoids excessive participation of alcohol in side reactions during the initial circulation process, which leads to the generation of more harmful impurities. Initially, only water in the solvent participates in the reaction. At room temperature, a hydrated solid electrolyte layer is preferentially constructed to form a stable zinc ion migration shell. Then, alcohol is introduced to lower the freezing point of the solvent, avoid precipitation of electrolyte salts at low temperatures, and stabilize and expand the operating temperature of the electrolyte. BRIEF DESCRIPTION OF THE DRAWINGS

[0083] Figures 1, 2, and 3 are pyrolysis gas chromatography-mass spectrometry (PGC-MS) of polyphenylene sulfide powder modified by hydrothermal reaction, which are used to confirm the presence of chlorocatechol-like structural molecules in the reaction products.

[0084] FIG4 is a comparison photo of the H-type cell before and after electrodialysis in the selective permeability test of the polyphenylene sulfide solid membrane in Example 2.

[0085] FIG5 is a schematic structural diagram of the prefabricated zinc salt diaphragm of the present invention.

[0086] FIG6 is a picture of the prefabricated zinc salt membrane in Example 1.

[0087] FIG7 is a schematic diagram of the battery coil core structure of the remarked zinc-manganese secondary cylindrical battery after winding in the present invention.

[0088] FIG8 is a charge and discharge curve diagram of the remark zinc-manganese secondary cylindrical battery in Example 1 after being filled with seawater.

[0089] FIG9 is a charge and discharge cycle diagram of the remarked zinc-manganese secondary cylindrical battery in Example 1 after being filled with seawater.

[0090] FIG10 is a comparison of the capacities of the zinc-manganese secondary cylindrical batteries of Example 3-7 after being filled with different electrolytes.

[0091] FIG11 is a laminated core pack of a zinc-manganese secondary battery in Example 8 before welding point protection.

[0092] FIG12 is a laminated core pack of a zinc-manganese secondary battery after welding point protection in Example 8. FIG.

[0093] FIG13 is a diagram of the annotated zinc-manganese secondary battery packaged in aluminum-plastic film in Example 8.

[0094] FIG14 is a stable cycle curve of the remarked zinc-manganese secondary battery in Example 8 after undergoing a water-first followed by alcohol formation system.

[0095] FIG15 is a charge-discharge curve of the remarked zinc-manganese secondary battery in Example 9 at 7° C. after the formation process of water first and then alcohol.

[0096] FIG16 is a charge and discharge curve at 0° C. of the remarked zinc-manganese secondary battery in Example 10 after the formation process of water first and then alcohol.

[0097] FIG17 is a charge and discharge curve of the remarked zinc-manganese secondary battery in Example 11 at -10° C. after the formation process of water first and then alcohol.

[0098] FIG18 is a schematic structural diagram of the powder processing system described in Example 12.

[0099] FIG19 is a flow chart of the film formation of the polyphenylene sulfide solid diaphragm A described in Example 12.

[0100] FIG20 is a surface SEM image of the polyphenylene sulfide solid diaphragm A described in Example 13.

[0101] FIG21 is a cross-sectional SEM image of the polyphenylene sulfide solid diaphragm A described in Example 13.

[0102] FIG22 is a surface SEM image of the negative electrode film described in Example 18.

[0103] FIG23 is an SEM image of the spatial entangled network structure composed of PTFE in the cross section of the negative electrode membrane described in Example 18.

[0104] In the figure: 1-upper supporting membrane B, 2-glue C, 3-polyphenylene sulfide solid membrane A, 4-glue E, 5-lower supporting membrane F, 6-prefabricated zinc salt membrane H, 7-positive electrode, 8-negative electrode, 9-winding core. DETAILED DESCRIPTION

[0105] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. The elements and features described in one embodiment of the present invention may be combined with the elements and features shown in one or more other embodiments. It should be noted that for the purpose of clarity, the representation and description of components and processes that are not related to the present invention and are known to those of ordinary skill in the art are omitted in the description. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative work are within the scope of protection of the present invention.

[0106] A polyphenylene sulfide (PPS) modification method for a solid-state separator suitable for long-life, wide-temperature-range, ampere-hour-class zinc-manganese secondary batteries involves mixing PPS powder, tetrachlorobenzoquinone (TCBQ), and deionized water, followed by a hydrothermal reaction at a temperature of 180-240°C for 1-4 hours in an atmosphere of air, oxygen, nitrogen, or argon. The mass ratio of PPS powder, TCBQ, and deionized water is 10:0.25-0.75:1-12. After the hydrothermal reaction, the TCBQ molecules undergo a reaction that removes chloride ions and adds hydroxyl groups, generating chlorocatechol-like molecules, including 2,5-dichlorohydroquinone, 2,3,5,6-tetrachlorophenol, 3,4,5-trichlorocatechol, tetrachlorohydroquinone, and 3,4,6-trichlorocatechol, or a mixture thereof.

[0107] Example 1: Polyphenylene sulfide modification

[0108] Polyphenylene sulfide powder, tetrachlorobenzoquinone, and deionized water were mixed in a mass ratio of 10:0.5:3 and subjected to a hydrothermal reaction at 210°C for 2 hours in an air atmosphere. After the hydrothermal reaction, the resulting powder was analyzed by pyrolysis gas chromatography-mass spectrometry (PGC-MS), revealing that the tetrachlorobenzoquinone molecules underwent a reaction that removed chloride ions and added hydroxyl groups, generating chlorocatechol-like molecules, including 2,5-dichlorohydroquinone, 3,4,5-trichlorocatechol, and tetrachlorohydroquinone, as shown in Figures 1, 2, and 3, respectively.

[0109] Example 2: Polyphenylene sulfide modification

[0110] Polyphenylene sulfide powder, tetrachlorobenzoquinone, and deionized water were mixed in a mass ratio of 10:0.5:6 and subjected to a hydrothermal reaction at 210°C for 2 hours in an air atmosphere. Pyrolysis gas chromatography-mass spectrometry (PGC-MS) analysis of the resulting powder revealed that the tetrachlorobenzoquinone molecules underwent a reaction that removed chloride ions and added hydroxyl groups, generating chlorocatechol-like molecules, including 2,5-dichlorohydroquinone, 3,4,5-trichlorocatechol, tetrachlorohydroquinone, and 3,4,6-trichlorocatechol.

[0111] Permselectivity of a polyphenylene sulfide solid membrane made from modified polyphenylene sulfide: The permselectivity of polyphenylene sulfide solid membrane A was tested using an H-type cell and electrodialysis. 70 mL of colorless, transparent dilute sulfuric acid (pH 4) was added to the anode compartment of the H-type cell, and 70 mL of a dark brown, transparent aqueous solution (1 mol / L ZnSO₄, 0.1 mol / L Na₂SO₄, 0.1 mol / L Li₂SO₄, 0.1 mol / L MnSO₄, 0.1 mol / L NiSO₄, 0.1 mol / L CoSO₄, 0.1 mol / L CuSO₄, 0.1 mol / L FeSO₄, 0.1 mol / L K₂SO₄, and 0.1 mol / L MgSO₄) was added to the cathode compartment. Pt metal electrodes were used at both the anode and cathode, and the electrodialysis test was conducted for 24 hours at a cell voltage of 3.25 V. Figure 4 shows a comparison of the H-type cell before and after electrodialysis. After electrodialysis, the dilute sulfuric acid in the left cathode cell showed no color change, but significant deposits were observed beneath the electrode. The Pt electrode surface showed significant deposits and a small number of bubbles. The right anode cell remained dark brown, a characteristic of heavy metals. Table 1 shows the changes in metal ion concentrations in the mother liquor measured by ICP before and after electrodialysis. This confirms that only zinc ions permeate the polyphenylene sulfide solid separator A, a key factor in ensuring the optimal performance of the rechargeable zinc-manganese secondary battery.

[0112] Table 1 shows the changes in the concentration of metal ions in the mother liquor before and after electrodialysis

[0113] The prefabricated zinc salt diaphragm described in the present invention includes a polyphenylene sulfide solid diaphragm A and an upper supporting diaphragm B and a lower supporting diaphragm F located on both sides of the polyphenylene sulfide solid diaphragm A. A mixture including an organic adhesive and / or an inorganic adhesive and an electrolyte zinc salt is filled between the upper supporting diaphragm B, the lower supporting diaphragm F and the polyphenylene sulfide solid diaphragm A.

[0114] As shown in FIG5 , the content of the adhesive liquid C between the upper support membrane B and the polyphenylene sulfide solid membrane A and the content of the adhesive liquid E between the upper support membrane B, the lower support membrane F and the polyphenylene sulfide solid membrane A can be the same or different. The ratio of the organic binder, the inorganic binder, the electrolyte salt and the solvent in the adhesive liquid C and the adhesive liquid E is 0-10:0-10:10-80:10-80, and the amount of the adhesive liquid C and the adhesive liquid E is 5-30 mg / cm 2 After drying, a solid mixed adhesive layer is formed, and the dry adhesive single layer load is 2-15mg / cm 2 The thickness of the prefabricated zinc salt separator is 70-200 μm. The organic binder is a mixture of one or more polymer binders such as polyvinyl alcohol (PVA), polyacrylate (PAA), and polytetrafluoroethylene (PTFE); the inorganic binder is a mixture of one or more inorganic powders such as sodium bentonite, zinc dihydrogen phosphate, and lithium montmorillonite powder; the electrolyte salt is a mixture of one or more inorganic salts such as zinc trifluoromethanesulfonate, zinc sulfate, zinc chloride, and zinc perchlorate; and the solvent is a mixture of one or more solvents such as deionized water, nitrogen methyl pyrrolidone (NMP), alcohol, and propylene glycol.

[0115] The polyphenylene sulfide solid membrane A has a thickness of 5-60 μm. The upper support membrane B and the lower support membrane F are both porous membranes, and their materials and thicknesses can be the same or different; they are selected from porous membranes such as polyethylene membrane (PE), polypropylene membrane (PP), cellulose membrane, non-woven membrane, and PET membrane with a thickness of 3-30 μm.

[0116] The preparation method of the prefabricated zinc salt diaphragm can be prepared by dipping the glue from the glue storage tank, or by coating the glue on the diaphragm and then laminating the three layers of diaphragm. The following embodiment uses the dipping method as an example for specific description.

[0117] The aforementioned zinc-manganese secondary battery includes a positive electrode, a negative electrode, and the prefabricated zinc salt separator. The prefabricated zinc salt separator H is placed between the manganese oxide positive electrode and the zinc negative electrode, and the tabs are welded. The battery cell is then prepared using a laminating machine or a winding machine and placed in a battery case with a sealable liquid injection port or an aluminum-plastic film bag for packaging and storage. In the aforementioned zinc-manganese secondary battery, the manganese oxide positive electrode is a dry-process manganese dioxide electrode manufactured using a semi-dry process, and the manganese oxide is a mixture of one or more manganese oxides such as α-MnO2, β-MnO2, γ-MnO2, δ-MnO2, Mn2O3, Mn3O4, and LiMn2O4. The zinc negative electrode is a dry-process zinc powder electrode manufactured using a semi-dry process, zinc foil, or galvanized copper foil.

[0118] The rechargeable zinc-manganese secondary battery does not require liquid injection during storage. When the battery is needed, pure water, seawater, or a dilute electrolyte is injected into the battery at a rate of 1-20 mL / Ah. After sealing the injection port, a chargeable and dischargeable zinc-manganese secondary battery is obtained. The dilute electrolyte is a salt solution of one or more salts, such as zinc sulfate, sodium sulfate, magnesium sulfate, sodium chloride, and zinc trifluoromethanesulfonate, with a concentration of 0.01 mol / L to 1 mol / L. The solvent is one or more of water, ethanol, methanol, propylene glycol, isopropyl alcohol, and glycerol. The dilute electrolyte can also be directly seawater.

[0119] Example 3: Prefabricated zinc salt diaphragm and zinc-manganese secondary battery

[0120] A polyphenylene sulfide solid separator A is fed into the laminating machine via a guide rail. The upper supporting separator B, which passes through a tank containing adhesive C, picks up adhesive C. Excess adhesive is scraped off with a scraper. The upper supporting separator B is then laminated with the polyphenylene sulfide solid separator A on a platform. Rolling completes the lamination of the upper supporting separator B and solid separator A. The upper supporting separator B is a hydrophilic polyethylene (PE) separator. The adhesive C consists of polyvinyl alcohol (PVA), zinc dihydrogen phosphate, the electrolyte salt zinc trifluoromethanesulfonate, and water in a mass ratio of 1:1:50:48. The laminated separator is dried in a tunnel oven at 70°C, cut into two layers of prefabricated zinc salt separator D, and rolled.

[0121] The polyphenylene sulfide side of the double-layer prefabricated zinc salt membrane D is passed through the glue tank for storing the glue E to pick up the glue E, and the excess glue is scraped off with a scraper, and then compounded with the lower support membrane F on the platform, and then the lower support membrane F and the double-layer prefabricated zinc salt membrane D are completed by rolling. The support membrane F is a hydrophilic polyethylene film (PE), and the glue E is composed of polyvinyl alcohol (PVA), sodium bentonite, electrolyte salt zinc trifluoromethanesulfonate and water, and the mass ratio of the four is 1:1:50:48. The three-layer membrane after compounding is dried in a tunnel furnace to obtain a three-layer prefabricated zinc salt membrane H, and then rolled up. The temperature of the tunnel furnace is 70°C. The appearance of the prefabricated zinc salt membrane made in this embodiment is shown in Figure 6.

[0122] The β-MnO2 dry electrode and the dry electrode made of zinc powder are used as the positive and negative electrodes respectively, and are wound with the prefabricated zinc salt separator H to form a battery core, which is then placed in an 18650 battery shell to form a remark zinc-manganese secondary cylindrical battery. Figure 7 is a structural schematic diagram of the battery core after the remark zinc-manganese secondary cylindrical battery is wound. When the battery needs to be used, seawater is injected into the battery in an amount of 5mL / Ah. After the liquid injection port is sealed, the zinc-manganese secondary battery can be charged and discharged. Figure 8 is a charge and discharge curve diagram of the remark zinc-manganese secondary cylindrical battery in this embodiment after being filled with seawater. Its charge and discharge curve is consistent with the curve of a conventional zinc-manganese secondary battery. Figure 9 is a charge and discharge cycle diagram of the remark zinc-manganese secondary cylindrical battery in this embodiment after being filled with seawater. The battery cycle is stable, and there is no obvious attenuation after 150 cycles.

[0123] Furthermore, to prevent the side effects of hydrogen and oxygen evolution from occurring at the exposed electrode surfaces during charge and discharge, this embodiment applies insulating and waterproof tape to the exposed current collectors of the β-MnO2 dry-process electrode and the zinc powder dry-process electrode for protection. The stainless steel current collector and the tabs are then joined together using resistance welding. The outer packaging of the remarked zinc-manganese secondary battery is made of PP and has an external support mechanism, which reduces the inter-electrode spacing to 65μm.

[0124] Example 4: Prefabricated zinc salt diaphragm and zinc-manganese secondary battery

[0125] A polyphenylene sulfide solid separator A is fed into the laminating machine via a guide rail. The upper supporting separator B is then laminarized with the adhesive C, which is then scraped off with a scraper. The laminarized separator B is then laminated with the polyphenylene sulfide solid separator A on a platform. The laminarized separator B is then rolled together. The upper supporting separator B is a hydrophilic polypropylene (PP) separator. The adhesive C consists of polyacrylate (PAA), zinc dihydrogen phosphate, the electrolyte zinc trifluoromethanesulfonate, and water in a mass ratio of 1:2:45:52. The laminated separator is dried in a tunnel oven at 80°C, cut into two layers of prefabricated zinc salt separator D, and rolled.

[0126] The polyphenylene sulfide side of the double-layer prefabricated zinc salt separator D is passed through a tank containing adhesive E to pick up adhesive E. Excess adhesive is scraped off with a scraper and then laminated with the lower support membrane F on a platform. The lower support membrane F and the double-layer prefabricated zinc salt separator D are then laminated by roller pressing. The support membrane F is a hydrophilic polyethylene (PE) film, and the adhesive E consists of polyacrylate (PAA), lithium-based montmorillonite powder, the electrolyte salt zinc trifluoromethanesulfonate, and water in a mass ratio of 1:2:45:52. The laminated three-layer separator is then dried in a tunnel oven to produce the three-layer prefabricated zinc salt separator H, which is then rolled up. The tunnel oven temperature is 80°C.

[0127] A γ-MnO2 dry-process electrode and zinc foil are used as the positive and negative electrodes, respectively, along with a prefabricated zinc salt separator H. This is then laminated to form a cell, which is then encased in an aluminum-plastic film to create a pre-filled zinc-manganese secondary battery. When the battery is needed, a 0.5 mol / L ZnSO4 solution is injected at a rate of 10 mL / Ah. After sealing the injection port, charging and discharging can begin.

[0128] Example 5: Prefabricated zinc salt diaphragm and zinc-manganese secondary battery

[0129] A polyphenylene sulfide solid separator A is fed into the laminating machine via a guide rail. The upper supporting separator B, which passes through a tank containing adhesive C, picks up adhesive C. Excess adhesive is scraped off with a scraper. The upper supporting separator B is then laminated with the polyphenylene sulfide solid separator A on a platform. Rolling completes the lamination of the upper supporting separator B and solid separator A. The upper supporting separator B is a hydrophilic polypropylene (PP) separator. The adhesive C consists of polytetrafluoroethylene (PTFE), zinc dihydrogen phosphate, the electrolyte zinc sulfate, and water in a mass ratio of 5:7:38:50. The laminated separator is dried in a tunnel oven at 100°C, cut into two layers of prefabricated zinc salt separator D, and rolled.

[0130] The polyphenylene sulfide side of the double-layer prefabricated zinc salt separator D is passed through a tank containing adhesive E to pick up adhesive E. Excess adhesive is scraped off with a scraper and then laminated with the lower support membrane F on a platform. The lower support membrane F and the double-layer prefabricated zinc salt separator D are then laminated by roller pressing. The support membrane F is a hydrophilic polyethylene (PE) film, and the adhesive E consists of polytetrafluoroethylene (PTFE), lithium-based montmorillonite powder, the electrolyte zinc sulfate, and water in a mass ratio of 5:7:38:50. The laminated three-layer separator is then dried in a tunnel oven to produce the three-layer prefabricated zinc salt separator H, which is then rolled up. The tunnel oven temperature is 100°C.

[0131] LiMn2O4 dry-process electrodes and dry-process electrodes made of zinc powder are used as the positive and negative electrodes, respectively, along with a prefabricated zinc salt separator H. This is then laminated to form a cell, encased in an aluminum-plastic film to create a pre-filled zinc-manganese secondary battery. When the battery is needed, water is injected at a rate of 8 mL / Ah. Once the injection port is sealed, charging and discharging can begin.

[0132] Example 6: Prefabricated zinc salt diaphragm and zinc-manganese secondary battery

[0133] A polyphenylene sulfide solid separator A is fed into the laminating machine via a guide rail. The upper supporting separator B, which passes through a tank containing adhesive C, picks up adhesive C. Excess adhesive is scraped off with a scraper. The upper supporting separator B is then laminated with the polyphenylene sulfide solid separator A on a platform. Rolling completes the lamination of the upper supporting separator B and solid separator A. The upper supporting separator B is a hydrophilic polypropylene (PP) separator. The adhesive C consists of polytetrafluoroethylene (PTFE), zinc dihydrogen phosphate, the electrolyte zinc sulfate, and water in a mass ratio of 5:7:38:50. The laminated separator is dried in a tunnel oven at 100°C, cut into two layers of prefabricated zinc salt separator D, and rolled.

[0134] The polyphenylene sulfide side of the double-layer prefabricated zinc salt separator D is passed through a tank containing adhesive E to pick up adhesive E. Excess adhesive is scraped off with a scraper and then laminated with the lower support membrane F on a platform. The lower support membrane F and the double-layer prefabricated zinc salt separator D are then laminated by roller pressing. The support membrane F is a hydrophilic polyethylene (PE) film, and the adhesive E consists of polytetrafluoroethylene (PTFE), lithium-based montmorillonite powder, the electrolyte zinc sulfate, and water in a mass ratio of 5:7:38:50. The laminated three-layer separator is then dried in a tunnel oven to produce the three-layer prefabricated zinc salt separator H, which is then rolled up. The tunnel oven temperature is 100°C.

[0135] LiMn2O4 dry-process electrodes and dry-process electrodes made of zinc powder are used as the positive and negative electrodes, respectively, and are laminated with a prefabricated zinc salt separator H to form a battery cell. This is then encased in an aluminum-plastic film to create a pre-filled zinc-manganese secondary battery. When the battery is needed, a 1 mol / L mixed solution of MgSO4 and NaCl is injected into the battery at a rate of 7 mL / Ah. After sealing the injection port, charging and discharging can begin.

[0136] Example 7: Prefabricated zinc salt diaphragm and zinc-manganese secondary battery

[0137] A polyphenylene sulfide solid separator A is fed into the laminating machine via a guide rail. The upper supporting separator B, which passes through a tank containing adhesive C, picks up adhesive C. Excess adhesive is scraped off with a scraper. The upper supporting separator B is then laminated with the polyphenylene sulfide solid separator A on a platform. Rolling completes the lamination of the upper supporting separator B and solid separator A. The upper supporting separator B is a cellulose separator. The adhesive C consists of polytetrafluoroethylene (PTFE), zinc dihydrogen phosphate, the electrolyte zinc sulfate, and water in a mass ratio of 4:2:5:2:40. The laminated separator is dried in a tunnel oven at 85°C, cut into two layers of prefabricated zinc salt separator D, and rolled.

[0138] The polyphenylene sulfide side of the double-layer prefabricated zinc salt separator D is passed through a tank containing adhesive E to pick up adhesive E. Excess adhesive is scraped off with a scraper and then laminated with the lower support membrane F on a platform. Rolling completes the lamination of the lower support membrane F and the double-layer prefabricated zinc salt separator D. The support membrane F is a cellulose membrane, and the adhesive E consists of polytetrafluoroethylene (PTFE), lithium-based montmorillonite powder, the electrolyte zinc sulfate, and water in a mass ratio of 4:2:52:40. The laminated three-layer separator is then dried in a tunnel oven to produce the three-layer prefabricated zinc salt separator H, which is then rolled up. The tunnel oven temperature is 85°C.

[0139] LiMn2O4 dry-process electrodes and dry-process electrodes made of zinc powder are used as the positive and negative electrodes, respectively, and are laminated with a prefabricated zinc salt separator H to form a battery cell. This is then encased in an aluminum-plastic film to create a pre-filled zinc-manganese secondary battery. To use the battery, a 1 mol / L mixed solution of Na2SO4 and KCl is injected into the battery at a rate of 8 mL / Ah. After sealing the injection port, charging and discharging can begin.

[0140] Figure 10 compares the capacities of the zinc-manganese secondary batteries in Example 3-7 after adding different electrolytes. It is clear that the addition of cations other than zinc ions, forming dual-ion and multi-ion systems, results in greater capacity and, consequently, higher energy density.

[0141] Example 8

[0142] To prevent side reactions during the charge and discharge process of the zinc-manganese secondary battery, the zinc-manganese secondary battery in this embodiment uses a γ-MnO2 semi-dry process positive electrode and a zinc powder semi-dry process negative electrode as electrodes. A prefabricated zinc salt separator is made from the polyphenylene sulfide solid separator made from the hydrothermally modified polyphenylene sulfide powder in Example 1. After the electrodes and prefabricated zinc salt separator are stacked, the stainless steel current collector and the nickel tab are resistance welded. After welding, the welds are protected with epoxy resin to achieve a water-resistant and insulating effect. Figures 11 and 12 respectively show the laminated core pack of the zinc-manganese secondary battery before and after weld protection. The battery is then packaged with aluminum-plastic film as the outer packaging material, as shown in Figure 13.

[0143] Furthermore, this embodiment also relates to a formation method for the zinc-manganese secondary battery prepared above. Specifically, the battery is first injected with a 1 mol / L sodium sulfate aqueous solution at a rate of 7 mL / Ah. A low current of 10 mA / g is used for formation and discharge, followed by three cycles of charge and discharge at this low current. While the battery is discharged, methanol is injected into the battery, resulting in a volume ratio of 5:0.7 between the aqueous electrolyte and the alcohol, and the battery is then vacuum-sealed. Figure 14 shows the charge-discharge curves at 7°C for the zinc-manganese secondary battery prepared in this embodiment after undergoing a formation process characterized by water followed by alcohol.

[0144] Example 9

[0145] In order to avoid the occurrence of side reactions during the charge and discharge process of the zinc-manganese secondary battery, the zinc-manganese secondary battery in this embodiment uses a γ-MnO2 semi-dry process positive electrode and a zinc powder semi-dry process negative electrode as the electrodes, and a polyphenylene sulfide solid diaphragm made from the polyphenylene sulfide powder after hydrothermal modification in Example 2 is used to make a prefabricated zinc salt diaphragm. After the electrodes and the prefabricated zinc salt diaphragm material are stacked, the stainless steel current collector of the positive electrode and the nickel tab, and the copper current collector of the negative electrode and the copper tab are resistance welded, and the welding points are protected with unsaturated polyester.

[0146] Furthermore, this embodiment also relates to a formation method for the zinc-manganese secondary battery prepared above. Specifically, the battery is first injected with a 1 mol / L sodium chloride aqueous solution at a rate of 8 mL / Ah. A discharge is performed using a low-current formation method of 20 mA / g. After 10 cycles of low-current charge and discharge, the battery is then injected with isopropyl alcohol (at a volume ratio of 5:2) while in the discharged state. The battery is then vacuum-sealed. Figure 15 shows the stable cycling curve of the zinc-manganese secondary battery prepared in this embodiment after undergoing a formation method characterized by water-first followed by alcohol.

[0147] Example 10

[0148] To prevent side reactions during the charge and discharge process, the zinc-manganese secondary battery in this embodiment uses a semi-dry ε-MnO2 positive electrode and a semi-dry zinc powder negative electrode as electrodes. A prefabricated zinc salt separator is made from a polyphenylene sulfide solid-state separator made from hydrothermally modified polyphenylene sulfide powder. After the electrode and separator materials are stacked, the stainless steel current collector is welded to the titanium tabs using resistance welding, and the welds are protected with epoxy resin.

[0149] Furthermore, this embodiment also relates to a formation method for the zinc-manganese secondary battery prepared above. Specifically, the battery is first injected with a 1 mol / L zinc sulfate aqueous solution at a volume of 10 mL / Ah. A low-current formation process is then performed using 20 mA / g for one discharge. After 10 cycles of low-current charge and discharge, ethylene glycol is injected with the battery in a discharged state, with the volume ratio of aqueous electrolyte to alcohol being 5:3. The battery is then vacuum-sealed. Figure 16 shows the charge-discharge curves at 0°C for the remarkably zinc-manganese secondary battery prepared in this embodiment after undergoing a formation process of water followed by alcohol.

[0150] Example 11

[0151] In order to avoid the occurrence of side reactions during the charge and discharge process of the zinc-manganese secondary battery, the remark zinc-manganese secondary battery in this embodiment uses a β-MnO2 semi-dry positive electrode, a zinc powder semi-dry negative electrode, and a polyphenylene sulfide solid diaphragm made of hydrothermally modified polyphenylene sulfide powder to make a prefabricated zinc salt diaphragm. After the lamination is completed, the stainless steel current collector of the positive electrode is welded to the nickel tab, and the copper current collector of the negative electrode is welded to the copper tab using resistance welding, and the welding points are protected with furan resin.

[0152] Furthermore, this embodiment also relates to a formation method for the zinc-manganese secondary battery prepared above. Specifically, the battery is first injected with a 1 mol / L aqueous zinc trifluoromethanesulfonate solution at a rate of 8 mL / Ah. A low-current formation process is then performed using 20 mA / g for one discharge. After five cycles of low-current charge and discharge, the battery is then injected with isopropyl alcohol (at a volume ratio of 5:5) while in the discharged state. The battery is then vacuum-sealed. Figure 17 shows the charge-discharge curves of the zinc-manganese secondary battery prepared in this embodiment at -10°C after undergoing a formation process characterized by water followed by alcohol.

[0153] Example 12: Equipment and method for manufacturing polyphenylene sulfide solid diaphragm

[0154] This embodiment discloses a manufacturing device for a polyphenylene sulfide solid diaphragm, including a powder processing system, a high-speed shearing machine, a screw extruder, a horizontal cold roller press, and a horizontal hot roller press.

[0155] The powder processing system includes an air compressor, an air storage tank, a cold dryer, a drying adsorption tower, a purification column, an air preheating system, a powder heating system, a supersonic shear mixer, and a gas-solid separation tower, which are connected in sequence. Figure 18 is a structural schematic diagram of the powder processing system described in this embodiment. The supersonic shear mixer has a semi-enclosed cavity. The air outlet of the purification column is connected to the air inlet of the semi-enclosed cavity of the supersonic shear mixer, and the air preheating system is arranged on the air pipeline between the purification column and the supersonic shear mixer. The powder heating system is arranged at the discharge port of the semi-enclosed cavity of the supersonic shear mixer. The discharge port of the semi-enclosed cavity of the supersonic shear mixer is connected to the gas-solid separation tower through a pipeline. The gas-solid separation tower is provided with an air outlet at the top, a discharge port at the bottom, and an air hammer air inlet in the middle. There are multiple drying adsorption towers, and multiple drying adsorption towers are arranged in parallel, respectively connected to the air outlet of the cold dryer and the air inlet of the purification column. The gas source of the air hammer is the dry compressed air bypass after the purification column, and the air hammer function is achieved by intermittently releasing compressed air.

[0156] The film-forming process of the powder processed by the powder handling system is completed by the high-speed shear, screw extruder, horizontal cold roller press, and horizontal hot roller press shown in Figure 19. The powder processed by the powder handling system is fed into the high-speed shear, sheared, and then into the screw extruder. The horizontal cold roller press and horizontal hot roller press are sequentially arranged downstream of the screw extruder, with a heated conveyor rail installed between the horizontal cold roller press and the horizontal hot roller press.

[0157] Example 13: Preparation method of polyphenylene sulfide solid diaphragm

[0158] This embodiment discloses a method for preparing a polyphenylene sulfide solid diaphragm using the polyphenylene sulfide solid diaphragm manufacturing equipment, and the specific steps are as follows:

[0159] 3 parts by mass of LiCl were dissolved in 12 parts by mass of deionized water to prepare a LiCl solution, 0.5 parts by mass of tetrachlorobenzoquinone and 10 parts by mass of cross-linked highly crystalline polyphenylene sulfide powder (crystallinity>70%) were mixed to prepare a mixed powder C, the LiCl solution and the mixed powder C were mixed to form a slurry D, and the slurry D was charged into a closed reactor for a hydrothermal reaction. The hydrothermal reaction atmosphere was air, the temperature was 210°C, the reaction time was 2 hours, and the hydrothermal reaction filling rate was 30%. After the reaction, the powder was washed and neutrally dried to prepare powder E.

[0160] 6wt% polytetrafluoroethylene powder and 94wt% powder E are mixed in a mixer to form powder F. The mixing process is carried out at a temperature where the polytetrafluoroethylene is in a glassy state. Dry ambient air G (RH = 5%) is compressed by a 15kW air compressor, cold-dried, dry-adsorbed, and purified. The dry-adsorption process uses two drying adsorption towers containing molecular sieves weighing a total of 400kg. The two towers alternate between operation and regeneration for 6 minutes. The dried and purified gas is preheated to 45°C, passes through a nozzle, enters a semi-enclosed cavity, and is accelerated to supersonic speeds, forming a supersonic jet H of extremely dry air with a dew point of -40°C. Powder F is preheated to 100°C and added to a semi-enclosed cavity. It is frictionally sheared by a supersonic jet H of extremely dry air. The molecular chains of the polytetrafluoroethylene in powder F stretch and open, forming a physical adhesion with the powder in F without chemical reaction, thus obtaining powder I. Powder I is then blown into a solid-gas separation tower along with the airflow. A dust removal filter is installed inside the separation tower to separate the solid material and the gas. The gas is discharged directly, and the powder adhering to the filter element is blown into the receiving bucket below by an air hammer. The air hammer's gas source is a purified dry compressed air bypass, and the air hammer function is achieved by intermittently releasing compressed air.

[0161] Powder I is added to a high-speed shear for secondary fiberization. After discharge, it enters a screw extruder and is extruded into 10 continuous thick strips J, each with a diameter of 8 mm. These strips J then enter a horizontal cold roller press with a roller surface temperature of 20°C for primary thinning to 0.8 mm. After thinning, they enter a heated conveyor rail at 130°C, where they are heated and fed into a horizontal hot roller press with a roller surface temperature of 130°C for secondary thinning to 30 μm. The two edges are trimmed to form the finished solid diaphragm L, which is then rolled up. The trimmed material K is recovered and added to the high-speed shear for reuse. Figure 20 shows a surface SEM image of the solid diaphragm, and Figure 21 shows a cross-sectional SEM image of the solid diaphragm. The solid diaphragm is a dense membrane composed of an entangled network structure formed by fibrous PTFE and plastically deformed PPS crystal particles. The porosity is extremely low, with the integral porosity calculation in this figure being 3%.

[0162] Example 14: Preparation method of polyphenylene sulfide solid diaphragm

[0163] 1 part by mass of NaCl was dissolved in 9 parts by mass of deionized water to prepare a NaCl solution, 0.25 parts by mass of tetrachlorobenzoquinone was mixed with 10 parts by mass of cross-linked highly crystalline polyphenylene sulfide powder (crystallinity>60%) to prepare a mixed powder C, the NaCl solution and the mixed powder C were mixed to form a slurry D, and the slurry D was charged into a closed reactor for a hydrothermal reaction. The hydrothermal reaction atmosphere was air, the temperature was 200°C, the reaction time was 3 hours, and the hydrothermal reaction filling rate was 40%. After the reaction, the powder was washed and neutrally dried to prepare powder E.

[0164] 5wt% polytetrafluoroethylene powder and 95wt% powder E are mixed in a mixer to form powder F. The mixing process is carried out at a temperature where the polytetrafluoroethylene is in a glassy state. Dry ambient air G (RH = 8%) is compressed by a 30kW air compressor, cold-dried, dry-adsorbed, and purified. The dry-adsorption process uses two drying adsorption towers containing molecular sieves weighing a total of 500kg. The two towers alternate between operation and regeneration for 8 minutes. The dried and purified gas is preheated to 50°C, passes through a nozzle, enters a semi-enclosed cavity, and is accelerated to supersonic speeds, forming a supersonic jet H of extremely dry air with a dew point of -45°C. Powder F is preheated to 120°C and added to a semi-enclosed cavity. It is frictionally sheared by a supersonic jet H of extremely dry air. The molecular chains of the polytetrafluoroethylene in powder F stretch and open, forming a physical adhesion with the powder in F without chemical reaction, thus obtaining powder I. Powder I is then blown into a solid-gas separation tower along with the airflow. A dust removal filter is installed inside the separation tower to separate the solid material and the gas. The gas is directly discharged, and the powder adhering to the filter element is blown into the receiving bucket below by an air hammer. The air hammer's gas source is a purified dry compressed air bypass, and the air hammer function is achieved by intermittently releasing compressed air.

[0165] The powder I is added to a high-speed shearing machine for secondary fiberization. After discharge, it enters a screw extruder and is extruded into a continuous thick cake J with a diameter of 10 mm. The continuous thick cake J enters a horizontal cold roller press with a roller surface temperature of 10°C for primary thinning to 1 mm. After thinning, it enters a heated conveyor rail at 130°C, and while being heated, it enters a horizontal hot roller press with a roller surface temperature of 120°C for secondary thinning to 35 μm. The two edges are cut off to make a finished solid diaphragm L, which is then wound up. The trimmed material K is recovered and added to the high-speed shearing machine for reuse.

[0166] Example 15: Preparation method of polyphenylene sulfide solid diaphragm

[0167] 2 parts by mass of ZnCl2 were dissolved in 10 parts by mass of deionized water to prepare a ZnCl2 solution, 0.3 parts by mass of tetrachlorobenzoquinone and 10 parts by mass of cross-linked highly crystalline polyphenylene sulfide powder (crystallinity>60%) were mixed to prepare a mixed powder C, the ZnCl2 solution and the mixed powder C were mixed to form a slurry D, and the slurry D was charged into a closed reactor for a hydrothermal reaction. The hydrothermal reaction atmosphere was argon, the temperature was 220°C, the reaction time was 1.5 hours, and the hydrothermal reaction filling rate was 50%. After the reaction, the powder was washed and neutrally dried to prepare powder E.

[0168] 4wt% polytetrafluoroethylene powder and 96wt% powder E were mixed in a mixer to form powder F. The mixing process was carried out at a temperature where the polytetrafluoroethylene was in a glassy state. Dry ambient air G (RH = 6%) was compressed by a 30kW air compressor, cold-dried, dry-adsorbed, and purified. The dry-adsorption process employed two drying adsorption towers containing molecular sieves weighing a total of 1000kg. The towers alternated between operation and regeneration for 7 minutes. The dried and purified gas was preheated to 47°C, passed through a nozzle, and entered a semi-enclosed cavity, where it was accelerated to supersonic speeds, forming a supersonic jet H of extremely dry air with a dew point of -42°C. Powder F is preheated to 125°C and added to a semi-enclosed cavity. It is frictionally sheared by a supersonic jet H of extremely dry air. The molecular chains of the polytetrafluoroethylene in powder F stretch and open, forming a physical adhesion with the powder in F without chemical reaction, thus obtaining powder I. Powder I is then blown into a solid-gas separation tower along with the airflow. A dust removal filter is installed inside the separation tower to separate the solid material and the gas. The gas is directly discharged, and the powder adhering to the filter element is blown into the receiving bucket below by an air hammer. The air hammer's gas source is a purified dry compressed air bypass, and the air hammer function is achieved by intermittently releasing compressed air.

[0169] The powder I is added to a high-speed shearing machine for secondary fiberization. After discharge, it enters a screw extruder and is extruded into a continuous thick cake J with a diameter of 7 mm. It enters a horizontal cold roller press with a roller surface temperature of 25°C for primary thinning to 0.8 mm. After thinning, it enters a heated conveyor rail at 130°C, and while being heated, it enters a horizontal hot roller press with a roller surface temperature of 130°C for secondary thinning to 40 μm. The two edges are cut off to make a finished solid diaphragm L, which is then wound up. The trimmed material K is recovered and added to the high-speed shearing machine for reuse.

[0170] Example 16: Preparation method of polyphenylene sulfide solid diaphragm

[0171] 3.5 parts by mass of MgCl2 were dissolved in 9 parts by mass of deionized water to prepare a MgCl2 solution, 0.45 parts by mass of tetrachlorobenzoquinone and 11 parts by mass of cross-linked highly crystalline polyphenylene sulfide powder (crystallinity>60%) were mixed to prepare a mixed powder C, the MgCl2 solution and the mixed powder C were mixed to form a slurry D, and the slurry D was charged into a closed reactor for a hydrothermal reaction in an air atmosphere at a temperature of 215°C for 3 hours and a hydrothermal reaction loading rate of 30%. After the reaction, the powder was washed and neutrally dried to prepare powder E.

[0172] 4wt% polytetrafluoroethylene powder and 96wt% powder E are mixed in a mixer to form powder F. The mixing process is carried out at a temperature where the polytetrafluoroethylene is in a glassy state. Dry ambient air G (RH = 6%) is compressed by a 30kW air compressor, cold-dried, dry-adsorbed, and purified. The dry-adsorption process uses two drying adsorption towers containing molecular sieves weighing a total of 600kg. The two towers alternate between operation and regeneration for 8 minutes. The dried and purified gas is preheated to 45°C, passes through a nozzle, enters a semi-enclosed cavity, and is accelerated to supersonic speeds, forming a supersonic jet H of extremely dry air with a dew point of -40°C. Powder F is preheated to 130°C and added to a semi-enclosed mold cavity. It is frictionally sheared by a supersonic jet H of extremely dry air. The molecular chains of the polytetrafluoroethylene in powder F stretch and open, forming a physical adhesion with the powder in F without chemical reaction, thus obtaining powder I. Powder I is then blown into a solid-gas separation tower along with the airflow. A dust removal filter is installed inside the separation tower to separate the solid material and the gas. The gas is directly discharged, and the powder adhering to the filter element is blown into the receiving bucket below by an air hammer. The air hammer's gas source is a purified dry compressed air bypass, and the air hammer function is achieved by intermittently releasing compressed air.

[0173] The powder I is added to a high-speed shearing machine for secondary fiberization. After discharge, it enters a screw extruder and is extruded into a continuous thick cake J with a diameter of 9 mm. It enters a horizontal cold roller press with a roller surface temperature of 15°C for primary thinning to 0.9 mm. After thinning, it enters a heated conveyor rail at 130°C, and while being heated, it enters a horizontal hot roller press with a roller surface temperature of 130°C for secondary thinning to 40 μm. The two edges are cut off to make a finished solid diaphragm L, which is then wound up. The trimmed material K is recovered and added to the high-speed shearing machine for reuse.

[0174] Example 17: Method for manufacturing a manganese oxide positive electrode,

[0175] First, manganese dioxide and polytetrafluoroethylene are mixed. Below the glass transition temperature of polytetrafluoroethylene, dry supersonic jet gas is used to open the molecular chains of polytetrafluoroethylene and physically adhere to the positive electrode material powder. Then, an alcohol solution is sprayed on the fiberized powder. After mixing and shearing granulation, it is hot rolled to form a positive electrode membrane. Then, through multiple cold rolling processes, the multi-layer positive electrode membrane is composited into a composite positive electrode self-supporting membrane with a thickness of 100-150μm. Finally, the composite positive electrode self-supporting membrane is composited with a sandblasted stainless steel foil coated with glue using a hot roller press.

[0176] Example 18: Method for manufacturing a zinc negative electrode,

[0177] Zinc powder, ECP, high-purity graphite, montmorillonite powder, and indium chloride are mixed uniformly in a mixer at a ratio of 74wt%:7wt%:5wt%:5wt%:1wt% to obtain powder A; 8wt% polytetrafluoroethylene powder and 92wt% powder A are mixed uniformly in a mixer at 0°C to obtain powder B; material B is added to a mixed solvent prepared by adding ethanol and deionized water in a volume ratio of 1:1 in a planetary ball mill, and the ball mill beads are rotated at high speed in a wet state, and continuous friction is applied to make the PTFE wire drawing into a network structure, and the indium chloride reacts with the zinc powder. After the above process is completed, micelles C are filtered to obtain micelles; micelles C are mixed to form uniform micelles, which are sheared and granulated to produce millimeter-sized particles E of uniform size with a solid content of 50%; particles E are rolled once on a horizontal hot roller press to obtain a 150μm negative electrode film F, and the hot rolling temperature is 80°C. The negative electrode membrane F is trimmed under the horizontal hot roller to meet the membrane width requirements. The trimmed material can be shredded again and put into the granular material E to complete the recycling of the edge material. The trimmed negative electrode membrane F is attached to the support belt of the porous release paper to complete the winding. After winding, the entire roll is dried to remove part of the solvent. The solid content of the semi-dry negative electrode membrane F is 65%. The surface and cross-sectional structures of the negative electrode membrane F are shown in Figures 22 and 23. The entangled network structure formed by PTFE can make the structure of the electrode more stable. Using a hot pressing composite process, the semi-dried negative electrode membrane F after the release paper is removed is thermally composited on both sides of the coated stainless steel foil to form an electrode.

[0178] Example 19: Method for manufacturing a zinc negative electrode

[0179] Zinc powder, SP, high-purity graphite, illite powder, and copper chloride are uniformly mixed in a mixer at a ratio of 50wt%:15wt%:15wt%:10wt%:2wt% to obtain powder A. 8wt% polytetrafluoroethylene powder and 92wt% powder A are uniformly mixed in a mixer at 5°C to obtain powder B. Powder B is added with a certain amount of alcohol solvent in a planetary ball mill. In a wet state, the ball mill beads rotate at high speed, causing the material to continuously rub and form a wire-like structure. The molecular chains of the polytetrafluoroethylene in powder B are extended and opened, forming physical adhesion with the powder in A. The copper chloride and zinc powder undergo a reduction reaction. After the above process is completed, micelles C are filtered to obtain micelles. The micelles C are mixed to form uniform micelles, which are then sheared and granulated to produce millimeter-sized particles E of uniform size with a solid content of 75%. The particles E are rolled once on a horizontal hot roller press to obtain a 120μm negative electrode film F. The hot rolling temperature is 90°C. The negative electrode film F is trimmed beneath a horizontal heated roller to the required film width. The trimmed film is then shredded and added to the pelletized material E for recycling. The trimmed negative electrode film F is then applied to a porous release paper carrier and wound up. After winding, the entire roll is dried to remove some of the solvent. The solids content of the semi-dried negative electrode film F is approximately 60%. Using a hot-pressing lamination process, the semi-dried negative electrode film F, after the release paper is removed, is thermally laminated to both sides of a coated stainless steel foil to form the electrode.

[0180] Example 20: Method for manufacturing a zinc negative electrode

[0181] Zinc powder, ECP, artificial graphite, kaolin, and indium sulfate are uniformly mixed in a mixer at a ratio of 60wt%:10wt%:8wt%:10wt%:4wt% to obtain powder A. 8wt% polytetrafluoroethylene powder and 92wt% powder A are uniformly mixed in a mixer at 5°C to obtain powder B. Powder B is added with a certain amount of alcohol solvent in a planetary ball mill. The milling beads rotate at high speed while wet, causing the powder to continuously rub and form a wire-like structure. The molecular chains of the polytetrafluoroethylene in powder B are extended and opened, forming physical adhesion with the powder in A. The indium sulfate and zinc powder undergo a reduction reaction. After the above process is completed, micelles C are filtered to obtain micelles. The micelles C are mixed to form uniform micelles, which are then sheared and granulated to produce uniform millimeter-sized particles E with a solid content of 75%. The particles E are rolled once on a horizontal hot roller press to obtain a 120μm negative electrode film F. The hot rolling temperature is 90°C. The negative electrode film F is trimmed beneath a horizontal heated roller to the required film width. The trimmed film is then shredded and added to the pelletized material E for recycling. The trimmed negative electrode film F is then applied to a porous release paper carrier and wound up. After winding, the entire roll is dried to remove some of the solvent. The solids content of the semi-dried negative electrode film F is approximately 60%. Using a hot-pressing lamination process, the semi-dried negative electrode film F, after the release paper is removed, is thermally laminated to both sides of a coated stainless steel foil to form the electrode.

[0182] Example 21: Method for manufacturing a zinc negative electrode

[0183] Zinc powder, SP, artificial graphite, halloysite powder, and copper sulfate are mixed uniformly in a mixer at a ratio of 67wt%:5wt%:5wt%:10wt%:5wt% to obtain powder A; 8wt% polytetrafluoroethylene powder and 92wt% powder A are mixed uniformly in a mixer at 0°C to obtain powder B; material B is added with a certain amount of alcohol solvent in a planetary ball mill, and the ball mill beads are rotated at high speed in a wet state, causing it to continuously rub and draw into a mesh structure. The molecular chains of polytetrafluoroethylene in powder B are extended and opened, forming physical adhesion with the powder in A, and copper sulfate and zinc powder undergo a reduction reaction. After the above process is completed, micelles C are filtered to obtain micelles; micelles C are mixed to form uniform micelles, which are sheared and granulated to produce millimeter-sized particles E of uniform size with a solid content of 70%; particles E are rolled once on a horizontal hot roller press to obtain a 100μm negative electrode film F, and the hot rolling temperature is 95°C. The negative electrode film F is trimmed beneath a horizontal heated roller to the required film width. The trimmed film is then shredded and added to the pelletized material E for recycling. The trimmed negative electrode film F is then applied to a porous release paper carrier and wound up. After winding, the entire roll is dried to remove some of the solvent. The solids content of the semi-dried negative electrode film F is approximately 55%. Using a hot-pressing lamination process, the semi-dried negative electrode film F, after the release paper is removed, is thermally laminated to both sides of a coated stainless steel foil to form the electrode.

Claims

1. A polyphenylene sulfide modification method, characterized in that: After mixing polyphenylene sulfide powder, tetrachlorobenzoquinone and deionized water in a mass ratio of 10:0.25-0.75:1-12, a hydrothermal reaction is carried out at 180-240° C. During the hydrothermal reaction, chloride ions are removed from tetrachlorobenzoquinone molecules and hydroxyl groups are increased, thereby generating molecules with a chlorocatechol structure.

2. The polyphenylene sulfide modification method according to claim 1, characterized in that: The constant temperature time of the hydrothermal reaction temperature is 1-4 hours, and the reaction atmosphere is air, oxygen, nitrogen or argon.

3. The modified polyphenylene sulfide prepared by the polyphenylene sulfide modification method according to any one of claims 1 to 2, characterized in that: The polyphenylene sulfide solid diaphragm is loaded with molecules of chlorocatechol structure; the chlorocatechol structure molecules are one or a mixture of 2,5-dichlorohydroquinone, 2,3,5,6-tetrachlorophenol, 3,4,5-trichlorocatechol, tetrachlorohydroquinone, 3,4,6-trichlorocatechol and the like.

4. A polyphenylene sulfide solid diaphragm made from the modified polyphenylene sulfide according to claim 3.

5. The polyphenylene sulfide solid diaphragm according to claim 4, characterized in that: The polyphenylene sulfide solid diaphragm has zinc ion selective permeability.

6. A method for manufacturing a prefabricated zinc salt diaphragm, characterized in that: The following steps are involved: (1) After one of the polyphenylene sulfide solid diaphragm A and the upper support diaphragm B is dipped in or coated with glue C, the two are laminated together so that the glue C is located between the polyphenylene sulfide solid diaphragm A and the upper support diaphragm B, and then the upper support diaphragm B and the solid diaphragm A are composited by rolling; the composite upper support diaphragm B and the solid diaphragm A are dried to obtain a double-layer prefabricated zinc salt diaphragm D; (2) After the exposed surface of the polyphenylene sulfide solid diaphragm A of the double-layer prefabricated zinc salt diaphragm D and one of the lower support membranes F are dipped or coated with glue E, the two are laminated so that the glue E is located, the glue E is dipped through a glue tank storing the glue E, and the excess glue is scraped off with a scraper, or the glue E is placed between the polyphenylene sulfide solid diaphragm A and the lower support membrane F, and then the lower support membrane F is composited with the double-layer prefabricated zinc salt diaphragm D by rolling, and the composite three-layer diaphragm is dried to obtain a prefabricated zinc salt diaphragm H; The upper supporting membrane B and the lower supporting membrane F are both porous membranes, and the glue C and glue E are mixtures of organic adhesives and / or inorganic adhesives, electrolyte zinc salts, and solvents.

7. The method for manufacturing a prefabricated zinc salt diaphragm according to claim 6, characterized in that: The mass ratio of the organic binder, the inorganic binder, the electrolyte salt and the solvent is 0-10: 0-10: 10-80: 10-80.

8. The method for manufacturing a prefabricated zinc salt diaphragm according to claim 6, characterized in that: The organic adhesive is a mixture of one or more of polyvinyl alcohol (PVA), polyacrylate (PAA), and polytetrafluoroethylene (PTFE); the inorganic adhesive is a mixture of one or more of sodium bentonite, zinc dihydrogen phosphate, and lithium montmorillonite powder; the electrolyte zinc salt is a mixture of one or more of zinc trifluoromethanesulfonate, zinc sulfate, zinc chloride, and zinc perchlorate; and the solvent is a mixture of one or more of deionized water, nitrogen methyl pyrrolidone (NMP), alcohol, and propylene glycol.

9. The method for manufacturing a prefabricated zinc salt diaphragm according to claim 6, characterized in that: The thickness of the polyphenylene sulfide solid diaphragm A is 5-60 μm, and the porous diaphragm is one of a polyethylene diaphragm (PE), a polypropylene diaphragm (PP), a cellulose film, a non-woven fabric film, and a PET film, and the thickness thereof is 3-30 μm.

10. The method for manufacturing a prefabricated zinc salt diaphragm according to claim 6, characterized in that: The dosage of the glue C and glue E is 5-30 mg / cm 2 The drying temperature for both times was 50-100℃; after drying, the single layer loading of dry glue was 2-15mg / cm 2 , the thickness of the prefabricated zinc salt membrane H is 70-200 μm.

11. The method for manufacturing a prefabricated zinc salt diaphragm according to claim 6, characterized in that: The polyphenylene sulfide solid diaphragm A is made of the modified polyphenylene sulfide described in claim 3 or 4.

12. The method for manufacturing a prefabricated zinc salt diaphragm according to claim 10, characterized in that: The manufacturing equipment of the polyphenylene sulfide solid diaphragm A includes a powder processing system, a high-speed shearing machine, a screw extruder, a horizontal cold roller press, and a horizontal hot roller press; The powder processing system includes an air compressor, an air storage tank, a cold dryer, a drying adsorption tower, a purification column, an air preheating system, a powder heating system, a supersonic shear mixer, and a gas-solid separation tower which are connected in sequence; the supersonic shear mixer has a semi-closed cavity, the air outlet of the purification column is connected to the air inlet of the semi-closed cavity of the supersonic shear mixer, and the air preheating system is arranged on the air pipeline between the purification column and the supersonic shear mixer; the powder heating system is arranged at the discharge port of the semi-closed cavity of the supersonic shear mixer; the discharge port of the semi-closed cavity of the supersonic shear mixer is connected to the gas-solid separation tower through a pipeline, and the gas-solid separation tower is provided with an air outlet at the top, a discharge port at the bottom, and an air hammer air inlet in the middle; The powder processed by the powder processing system is sent to the high-speed shearing machine, and enters the screw extruder after shearing. The horizontal cold roller press and the horizontal hot roller press are arranged downstream of the screw extruder in sequence, and a heating conveying guide rail is arranged between the horizontal cold roller press and the horizontal hot roller press.

13. The method for manufacturing a prefabricated zinc salt diaphragm according to claim 12, characterized in that: There are multiple drying adsorption towers, which are arranged in parallel and respectively connected to the air outlet of the cold dryer and the air inlet of the purification column; the gas source of the air hammer is the dry compressed air bypass after the purification column, and the air hammer function is achieved by intermittently releasing compressed air.

14. The method for manufacturing a prefabricated zinc salt diaphragm according to claim 12 or 13, characterized in that: The method for manufacturing the polyphenylene sulfide solid diaphragm A comprises the following steps: (1) Flour making: The metal chloride A is dissolved in deionized water to prepare a solution B, tetrachlorobenzoquinone and polyphenylene sulfide powder are mixed to prepare a mixed powder C, the solution B and the mixed powder C are mixed to prepare a slurry D, the slurry D is loaded into a closed reactor for hydrothermal reaction, and after the reaction is completed, the powder is washed and neutrally dried to prepare a powder E; (2) Fibrosis: The polytetrafluoroethylene powder and powder E are uniformly mixed in a mixer to obtain powder F, and the mixing process is carried out under the temperature condition that the polytetrafluoroethylene is in a glassy state; After being compressed, cold-dried, dry-adsorbed, purified, and preheated by an air compressor, the dry air G passes through a nozzle and enters a semi-enclosed cavity, where it is accelerated to supersonic speed, forming a supersonic jet H of extremely dry air; The powder F is preheated and added into the semi-enclosed cavity, where it is frictionally sheared by the supersonic jet H of extremely dry air. The molecular chains of polytetrafluoroethylene in the powder F are extended and opened, forming physical adhesion with the powder in F without chemical reaction, thereby obtaining powder I. The powder I is blown into the solid-gas separation tower along with the air flow. There is a dust removal filter inside the separation tower to separate the solid powder and gas. The gas is discharged directly, and the powder adhering to the filter element is blown into the receiving barrel below by the air hammer; (3) Film making: The powder I is added to a high-speed shearing machine for secondary fiberization, and then enters a screw extruder to be extruded into a plurality of continuous thick strips or continuous thick cakes J, and enters a horizontal cold roller press for primary thinning. After thinning, it enters a heated conveying guide rail, and enters a horizontal hot roller press while being heated and fed for secondary thinning. The two edges are cut off to form a finished solid diaphragm L, which is then rolled up.

15. The method for manufacturing a prefabricated zinc salt diaphragm according to claim 14, characterized in that: The metal chloride A in the powder making process is one or a mixture of lithium chloride, sodium chloride, zinc chloride, magnesium chloride, and aluminum chloride; the polyphenylene sulfide powder is a cross-linked high-crystalline polyphenylene sulfide powder with a crystallinity of >60% and a D50 of 3-25 μm; the mass ratio of the metal chloride, deionized water, tetrachlorobenzoquinone, and polyphenylene sulfide is 0-3:3-30:0.1-0.75:5-15; the atmosphere in the hydrothermal reactor is air or argon, the hydrothermal reaction temperature is 150-250°C, and the hydrothermal reaction time is 1-4 hours; the volume filling rate of the hydrothermal reaction is 20%-70%.

16. The method for manufacturing a prefabricated zinc salt diaphragm according to claim 14, characterized in that: During the fiberization process, the relative humidity (RH) of the dry air G at room temperature of 25°C is less than 10%; the power of the air compressor is greater than or equal to 15kW, and preferably greater than 30kW for continuous production; the dew point of the supersonic jet H of the ultra-dry air is lower than -40°C; the dry adsorption process is to use multiple dry adsorption towers containing molecular sieves, the total weight of the molecular sieves is greater than 200kg, and the multiple dry adsorption towers work and regenerate alternately, and the alternation time is 3-12 minutes.

17. The method for manufacturing a prefabricated zinc salt diaphragm according to claim 14, characterized in that: During the fiberization process, the preheating temperature of the air before entering the nozzle is 30-60°C, and the preheating temperature of the powder F entering the semi-enclosed cavity is 40-220°C.

18. The method for manufacturing a prefabricated zinc salt diaphragm according to claim 14, characterized in that: The film making process comprises a plurality of continuous thick strips or continuous thick cakes J, whose shapes are determined by the extrusion head die of the screw extruder, and the diameter of the continuous thick strips or the thickness of the continuous thick cakes is between 3-12 mm; the roller surface temperature of the horizontal cold roller press is -10-30°C; the thickness after the first thinning is 0.3-1.5 mm; the temperature of the heated conveying guide rail is 90-150°C; the roller surface temperature of the horizontal hot roller press is 110-160°C; the thickness after the second thinning is 5-60 μm.

19. The prefabricated zinc salt diaphragm manufactured by the method for manufacturing a prefabricated zinc salt diaphragm according to any one of claims 6 to 10, characterized in that: It includes a polyphenylene sulfide solid separator A and an upper supporting separator B and a lower supporting separator F located on both sides of the polyphenylene sulfide solid separator A. A mixture including an organic adhesive and / or an inorganic adhesive and an electrolyte salt is filled between the upper supporting separator B, the lower supporting separator F and the polyphenylene sulfide solid separator A, respectively.

20. The prefabricated zinc salt diaphragm manufactured by the method for manufacturing a prefabricated zinc salt diaphragm according to any one of claims 10 to 18, characterized in that: It comprises a polyphenylene sulfide solid diaphragm A and an upper supporting diaphragm B and a lower supporting diaphragm F located on both sides of the polyphenylene sulfide solid diaphragm A, and a mixture of an organic adhesive and / or an inorganic adhesive and an electrolyte salt is filled between the upper supporting diaphragm B, the lower supporting diaphragm F and the polyphenylene sulfide solid diaphragm A, and the polyphenylene sulfide solid diaphragm A is made of the modified polyphenylene sulfide described in claim 3.

21. A method for manufacturing a rechargeable zinc-manganese battery made of the prefabricated zinc salt diaphragm according to claim 19 or 20, characterized in that: The prefabricated zinc salt diaphragm H is placed between the manganese oxide positive electrode and the zinc negative electrode, and the tabs are welded. A battery cell is prepared by using a stacking machine or a winding machine, and is placed in a battery shell or an aluminum-plastic film bag, packaged for standby use, and stored; a sealable liquid injection port is left on the battery shell or the aluminum-plastic film bag.

22. The method for manufacturing a zinc-manganese secondary battery according to claim 21, characterized in that: The manganese oxide positive electrode is a manganese dioxide dry electrode manufactured by semi-dry technology, and the manganese oxide is one or a mixture of α-MnO2, β-MnO2, γ-MnO2, δ-MnO2, Mn2O3, Mn3O4, LiMn2O4; the zinc negative electrode is one of zinc powder dry electrode, zinc foil, and galvanized copper foil manufactured by semi-dry technology.

23. The method for manufacturing a zinc-manganese secondary battery according to claim 21, characterized in that: After the welding of the tabs is completed, the welding points are protected by water-blocking insulation.

24. The method for manufacturing a zinc-manganese secondary battery according to claim 23, characterized in that: The water-blocking insulation protection of the welding point is to wrap it with a water-blocking insulation tape, apply an aluminum oxide layer or smear resin protection; the resin is one or more of epoxy resin, phenolic resin, furan resin, and unsaturated polyester; the pole ear is a nickel pole ear, a copper pole ear, a titanium pole ear or a molybdenum pole ear.

25. The method for manufacturing a zinc-manganese secondary battery according to claim 21, characterized in that: After obtaining the battery cell, an external holding mechanism is used to increase the pre-tightening force between the prefabricated zinc salt diaphragm H, the manganese oxide positive electrode and the zinc negative electrode, so that the inter-electrode distance is controlled at 50-120 μm.

26. The method for manufacturing a zinc-manganese secondary battery according to claim 21, characterized in that: The outer packaging of the battery shell is made of a water-blocking, gas-blocking and acid-resistant material, and the water-blocking, gas-blocking and acid-resistant material is a non-porous film.

27. The method for manufacturing a zinc-manganese secondary battery according to claim 26, characterized in that: The non-porous film is one or a composite film of biaxially oriented polypropylene film (BOPP), cast polypropylene film (CPP), polyethylene terephthalate (PET), polyethylene (PE), and polypropylene (PP) non-porous films.

28. The method for manufacturing a zinc-manganese secondary battery according to claim 21, characterized in that: The manufacturing method of the manganese oxide positive electrode comprises the following steps: firstly, manganese dioxide is mixed with polytetrafluoroethylene, and below the glass transition temperature of polytetrafluoroethylene, dry supersonic jet gas is used to open the molecular chain of polytetrafluoroethylene and physically adhere to the positive electrode material powder, and then an alcohol solution is sprayed on the fiberized powder, and after banburying and shearing granulation, hot rolling is performed to form a positive electrode film, and then the multi-layer positive electrode film is compounded into a composite positive electrode self-supporting film with a thickness of 100-150 μm through multiple cold rolling, and finally the composite positive electrode self-supporting film is compounded with a sandblasted stainless steel foil with a surface coated with glue through a hot rolling machine.

29. The method for manufacturing a zinc-manganese secondary battery according to claim 21, characterized in that: The method for manufacturing the zinc negative electrode comprises the following steps: Mix zinc powder, conductive agent, toughening conductive agent, cationic slow-release agent and hydrogen evolution inhibitor in a mixer to make powder A; the cationic slow-release agent is an inorganic powder with electronegativity and volume expansion when exposed to water; the hydrogen evolution inhibitor is a metal compound that can undergo reduction reaction with zinc powder in an alcohol-water solvent; the weight percentage of zinc powder, conductive agent, toughening conductive agent, cationic slow-release agent, polytetrafluoroethylene and hydrogen evolution inhibitor powder is: 60%-90%: 1%-10%: 1%-10%: 1%-10%: 3%-15%: 0.1%-5%; The polytetrafluoroethylene powder and powder A are mixed in a mixer to form powder B; the mixing process is carried out at a temperature where the polytetrafluoroethylene (PTFE) is in a glassy state; The powder B and the alcohol-water mixed solvent are in a ball mill, and the ball mill beads are constantly rubbed during high-speed rotation to make the PTFE wire drawing present a mesh structure, the molecular chain of the polytetrafluoroethylene in the powder B is extended and opened, and forms physical adhesion with the powder in the powder A, and the hydrogen evolution inhibitor reacts with the surface of the zinc powder by reduction reaction. After the above process is completed, the micelle C is obtained by filtration; The micelle C is kneaded to form a uniform micelle, which is then sheared and granulated to form millimeter-sized granules E of uniform size; The granular material E is hot-pressed into a negative electrode film F by a horizontal hot roller press, and a porous release paper is used as a support belt to complete the winding. The whole roll of the negative electrode film F covered with the release paper is dried to remove part of the solvent; The semi-dried negative electrode film F after the release paper is peeled off is thermally laminated on both sides of the glue-coated stainless steel foil to form an electrode by using a hot pressing composite process.

30. The method for manufacturing a zinc-manganese secondary battery according to claim 29, characterized in that: The zinc powder is powdered particles with a particle size of 5-20 μm; the conductive agent is one or both of super-P and ECP; the toughening conductive agent is one or a mixture of artificial graphite and high-purity graphite.

31. The method for manufacturing a zinc-manganese secondary battery according to claim 29, characterized in that: The cationic sustained-release agent is one or more of bentonite, montmorillonite powder, illite powder, kaolin powder, and halloysite powder; the hydrogen evolution inhibitor is one or more of indium chloride, copper chloride, indium sulfate, and copper sulfate.

32. The method for manufacturing a zinc-manganese secondary battery according to claim 29, characterized in that: The alcohol-water mixed solvent is a mixed solvent of water and isopropanol, propylene glycol or ethanol, and the volume percentage of water to alcohol is: 40%-80%: 20%-60%; the solid content of the uniform micelle is 40%-60%.

33. The method for manufacturing a zinc-manganese secondary battery according to claim 29, characterized in that: The granular material E is rolled once by a horizontal hot roller press to obtain a negative electrode film F with a thickness of 90-200 μm, and the hot roller pressing temperature is 55-95° C.

34. The method for manufacturing a zinc-manganese secondary battery according to claim 29, characterized in that: When the semi-dried negative electrode film F is thermally compounded with the stainless steel foil, the glue-coated stainless steel foil is sandwiched between two negative electrode films F with the release paper removed, unwound at the same speed, and enters two relatively rotating horizontal hot roller presses. The roller pressing temperature is 30-120°C. By adjusting the roller gap width and controlling the pressure, the negative electrode film F can be just compounded on the glue-coated stainless steel foil to avoid excessive deformation of the negative electrode film F and breaking of the stainless steel foil due to excessive roller pressure.

35. The method for manufacturing a zinc-manganese secondary battery according to claim 29, characterized in that: The glue-coated stainless steel foil is made by printing high-conductivity paste on both sides of the stainless steel foil using a gravure printing machine. The surface of the stainless steel foil needs to be sandblasted before glue coating to remove surface rolling oil. The high-conductivity paste is composed of high-purity graphite, non-hydrophilic adhesive and non-aqueous solvent.

36. A rechargeable zinc-manganese secondary battery manufactured by the rechargeable zinc-manganese secondary battery manufacturing method according to any one of claims 21 to 29, characterized in that: The battery is composed of a manganese oxide positive electrode, a zinc negative electrode, a three-layer prefabricated zinc salt diaphragm H and a battery shell or an aluminum-plastic film bag with a sealable liquid injection port. The manganese oxide positive electrode, the zinc negative electrode and the three-layer prefabricated zinc salt diaphragm H are placed in the battery shell or the aluminum-plastic film bag after the tabs are welded.

37. The application method of the zinc-manganese secondary battery according to claim 36, characterized in that: The remarked zinc-manganese secondary battery does not need to be injected during storage and transportation; before being put into use, pure water, seawater or dilute electrolyte is injected into the battery; preferably, the dilute electrolyte is a salt solution of one or more of zinc sulfate, sodium sulfate, magnesium sulfate, sodium chloride, and zinc trifluoromethanesulfonate with a concentration of 0.01 mol / L to 1 mol / L, and its solvent is a mixture of one or more of water, ethanol, methanol, propylene glycol, isopropanol, and glycerol; preferably, the amount of injected liquid is 1-20 mL / Ah.

38. The formation method of the zinc-manganese secondary battery according to claim 36, characterized in that: In the battery formation process, firstly, an electrolyte with only water as solvent is injected into the secondary battery, and a discharge is performed once with a small current formation of current density of 1-20 mA / g, and then 0-40 cycles of charge and discharge are performed. Then, in the battery discharge state, an organic solvent is injected, and then vacuum packaging is performed. The organic solvent is an organic solvent that can reduce the freezing point of water after mixing with water, and the volume ratio of the aqueous solution electrolyte to the organic solvent is 5:0.3-5.

39. The formation method of the zinc-manganese secondary battery according to claim 37, characterized in that: The electrolyte with water as solvent is 2-3 mol / L zinc trifluoromethanesulfonate aqueous solution, 2-3 mol / L zinc sulfate aqueous solution or 2-3 mol / L zinc chloride aqueous solution; the injection volume is 3-10 mL / Ah.

40. The formation method of the zinc-manganese secondary battery according to claim 37, characterized in that: The organic solvent is alcohol, dimethyl sulfoxide, propylene carbonate, and acetonitrile.

41. The formation method of the zinc-manganese secondary battery according to claim 39, characterized in that: The alcohol is one or a mixture of methanol, isopropanol, ethylene glycol, propylene glycol and glycerol.

Citation Information

Patent Citations

  • Polymer composite solid electrolyte and preparation method and application thereof

    CN106450424A

  • High-safety high-volume-energy-density quasi-solid-state lithium-ion battery and manufacturing method thereof

    CN111864272A

  • Zinc ion solid electrolyte, application of zinc ion solid electrolyte in quasi-solid zinc ion battery and preparation method of zinc ion solid electrolyte

    CN113078372A

  • Ampere-hour level zinc-manganese secondary battery and manufacturing method thereof

    CN115588784A

  • Modified polyphenylene sulfide, solid-state diaphragm, ampere-hour-grade zinc-manganese secondary battery and manufacturing and formation method of ampere-hour-grade zinc-manganese secondary battery

    CN117264212A