Molten lithium metal battery based on ceramic electrolyte sheet

By using ceramic electrolyte sheets and gas-conducting metal tube designs, combined with interface protection compositions and honeycomb coal configuration adsorption materials, the molding complexity and interface resistance problems of existing U-shaped tubular batteries are solved, and the performance of molten lithium metal batteries is improved. and stability.

WO2024213073A1PCT designated stage expired Publication Date: 2024-10-17METAGENESIS LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/087357
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-14
Filing Date
2024-04-12
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Existing molten lithium metal batteries based on U-shaped tubular solid electrolytes are difficult to form, complex in the preparation process, and have poor wettability between molten metal lithium and ceramic electrolytes, resulting in high interface resistance, which affects battery performance and cycle life.

Method used

Designed with ceramic electrolyte sheets, the convex shell is divided into upper and lower parts, the negative electrode compartment and the positive electrode compartment. The air-conducting metal pipe runs through it, and the liquid lithium-ion-conducting electrolyte is injected into the positive electrode compartment. The interface protection composition is used to improve the interface stability, and Honeycomb coal configuration adsorption material is used in the cathode compartment to optimize the lithium ion transmission path.

Benefits of technology

It simplifies the forming process of ceramic electrolyte sheets, improves the uniform contact of the negative electrode liquid protective layer, improves the wettability and lithium ion conductivity of the positive electrode material, reduces the lithium ion diffusion resistance, and improves the rate performance and electrochemical performance of the battery. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024087357_17102024_PF_FP_ABST
    Figure CN2024087357_17102024_PF_FP_ABST
Patent Text Reader

Abstract

A molten lithium metal battery based on a ceramic electrolyte sheet, comprising: a casing in the shape of the Chinese character "凸" and a ceramic electrolyte sheet, wherein the ceramic electrolyte sheet divides said casing into an upper part and a lower part, the upper part is a negative electrode chamber, the lower part is a positive electrode chamber, a positive electrode material is contained in the positive electrode chamber, and a lithium recess is formed in the negative electrode chamber; gas guide metal tubes, wherein the gas guide metal tubes are connected to and communicated with said casing, and openings of the air guide metal tubes are higher than the bottom surface of the ceramic electrolyte sheet; an upper cover and a negative electrode current collector, wherein the negative electrode current collector passes through the upper cover and is led out from the upper cover, the negative electrode current collector and the upper cover are sealed together by means of an insulating sealing material, the upper cover is arranged at the top of said casing and seals said casing, a negative electrode material is contained in the lithium recess, and a seal is formed between the lithium recess and said casing; and a bottom cover, wherein the bottom cover is connected to the bottom end of said casing.
Need to check novelty before this filing date? Find Prior Art

Description

A molten lithium metal battery based on ceramic electrolyte sheets

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to Chinese patent application No. 202310403017.0 filed in China on April 14, 2023, the entire contents of which are incorporated herein by reference. Technical Field

[0003] The present disclosure relates to the technical field of molten lithium metal batteries, and in particular to a molten lithium metal battery based on a ceramic electrolyte sheet. Background Art

[0004] With the progress of human society and the continuous development of the economy, non-renewable energy sources such as fossil fuels are becoming increasingly depleted, and the demand for clean, green, and low-carbon renewable energy is becoming increasingly urgent. Renewable energy sources such as solar and wind energy are not only environmentally friendly but also recyclable, making them ideal low-carbon energy sources. However, the instability and discontinuity of solar and wind power output make grid integration difficult, hindering the safe and stable operation of the power grid. Therefore, the development of a safe, stable, and scalable energy storage system is urgently needed.

[0005] Among many energy storage technologies, electrochemical energy is one of the important development directions of large-scale energy storage technology, that is, the use of batteries has attracted more and more attention.

[0006] Lithium batteries use lithium as an energy transport and storage medium. Lithium is the lightest metal element existing in nature and has a low redox potential (-3.04V). This gives lithium-ion batteries higher output voltage and energy density than other types of batteries.

[0007] The molten lithium metal batteries based on solid electrolytes developed in recent years are expected to be used in large-scale grid energy storage, backup power supplies and large electric vehicle power batteries due to their high safety, high energy density and low cost.

[0008] CN109075412A discloses a rechargeable lithium-air battery comprising a ceramic diaphragm forming a negative electrode chamber, a molten lithium negative electrode contained in the negative electrode chamber, an air positive electrode, and an anhydrous electrolyte. The battery is cylindrical in shape, with fins extending longitudinally along the cylinder and radially extending outward away from the battery core. The basic structure is supported by a hollow solid electrolyte cylinder (negative electrode chamber) that extends the length of the battery and serves as a battery diaphragm. Molten lithium metal is contained in a reservoir and annular cavity located at the top of the battery, allowing molten lithium to flow freely from the reservoir into the annular cavity. It is expected that the top layer of the molten negative electrode will not completely fill the top space of the battery. An electric heater element extends along the length of the battery and is positioned to keep the lithium in a molten state. The heater is part of the core structure, forming an annular cavity between the heater and the inner wall of the solid electrolyte, which contains the molten lithium. An expanded view of a radial plane cross-section of the battery shows a heater / spacer including the heater element, a finned positive electrode, an annular lithium cavity, a solid electrolyte cylinder, and a molten lithium negative electrode.

[0009] US20190006720A1 discloses a molten lithium-sulfur battery with a solid electrolyte, comprising: a sealed case; a solid electrolyte; a conductive metal foam having a plurality of pores; an anode containing the metal foam and lithium (Li) or a lithium alloy as the anode active material; and a cathode containing the metal foam and sulfur (S) or a sulfide as the cathode active material, wherein the metal foam is formed of iron (Fe) or nickel (Ni). The battery comprises a sealed case, a solid electrolyte, metal foam, a negative electrode containing the metal foam as a binder and lithium (Li) or a lithium alloy as the active material. A cathode containing the metal foam as a binder and sulfur (S) or a sulfide as the active material. The solid electrolyte is manufactured by sequentially stacking an atmosphere adjustment powder, multiple layers of electrolyte powder, and an atmosphere adjustment powder. The atmosphere adjustment powder can be formed of the same material as the solid electrolyte, or lithium-rich powder can be used.

[0010] CN112514136A discloses a molten lithium electrochemical cell based on a solid electrolyte, which includes a solid electrolyte, a positive electrode material and a negative electrode material. The solid electrolyte used is a U-shaped tube structure, molten metal lithium is filled inside the U-shaped tube as the negative electrode, and Sn-Pb alloy is filled between the outside of the U-shaped tube and the stainless steel shell as the positive electrode.

[0011] CN113678300A discloses an electrochemical cell comprising: an anode comprising lithium metal or a lithium alloy; a cathode comprising sulfur, selenium, or a mixture thereof; and a solid electrolyte positioned between the anode and the cathode, wherein the solid electrolyte is capable of conducting lithium ions. The cell comprises an anode comprising lithium metal or a lithium metal alloy, a cathode comprising sulfur or selenium, and the solid electrolyte, wherein the solid electrolyte is in the form of a tube adjacent to the anode and separating the anode from the cathode.

[0012] CN114335758A discloses a high-temperature molten lithium-iodine battery based on a garnet solid electrolyte, comprising a garnet solid electrolyte, a positive electrode material and a negative electrode material; the garnet solid electrolyte is LLZTO ceramic, the positive electrode material comprises CsI / LiI eutectic salt, and the negative electrode material is molten metal lithium. 6.4 La3Zr 1.4 Ta 0.6 O 12 ) The ceramic electrolyte tube is used as the solid electrolyte, the inside of the U-shaped tube is filled with eutectic iodide as the positive electrode, the outside of the U-shaped tube and the space between the stainless steel shell are filled with lithium metal as the negative electrode, and the graphite rod is used as the current collector for conduction, forming the basic structure of the garnet solid electrolyte high-temperature molten lithium-iodine battery.

[0013] The disclosed person is known for molten lithium metal batteries based on U-shaped tubular solid electrolytes. On the one hand, the U-shaped ceramic electrolyte tube is difficult to form and the preparation process is complicated. On the other hand, the poor wettability of molten metal lithium and ceramic electrolyte results in a large interface resistance, which reduces the overall performance of the battery. Liu Kai et al., Molten Lithium-Brass / Zinc Chloride System as High-Performance and Low-Cost Battery.Matter, 2020, 3, by providing a protective interface layer between the inner wall of the U-shaped tube electrolyte tube and the stainless steel mesh and the stainless steel mesh closely fitting the inner wall of the U-shaped tube to reduce the interface resistance of the molten metal lithium and the ceramic electrolyte. However, the disadvantage of the molten lithium metal battery structure based on ceramic U-shaped tube electrolyte is that the interface protective layer protecting the U-shaped tube is easy to fall off and deposit at the bottom of the tube, resulting in an increase in the internal resistance of the battery, affecting the battery cycle life. In addition, under long-term high temperature conditions, the supporting effect of the stainless steel mesh is weakened or loses its supporting effect, and it cannot fit closely with the U-shaped tube, resulting in an increase in the internal resistance of the battery or a short circuit, thereby affecting the performance of the battery.

[0014] Summary of the Invention

[0015] The present disclosure provides a molten lithium metal battery based on a ceramic electrolyte sheet.

[0016] In a first aspect, the present disclosure provides a molten lithium metal battery based on a ceramic electrolyte sheet, comprising:

[0017] A convex housing and a ceramic electrolyte sheet, wherein the ceramic electrolyte sheet divides the convex housing into an upper portion and an lower portion, the upper portion being a negative electrode compartment and the lower portion being a positive electrode compartment; the positive electrode compartment contains positive electrode material, and the negative electrode compartment is provided with a lithium tank; the upper surface of the ceramic electrolyte sheet is in close contact with the lithium tank;

[0018] an air-conducting metal tube, the air-conducting metal tube being connected to the convex shell and passing through the convex shell, and the tube opening of the air-conducting metal tube being higher than the bottom surface of the ceramic electrolyte sheet;

[0019] An upper cover and a negative electrode current collector, wherein the upper cover is annular, the negative electrode current collector passes through the upper cover and is led out from the upper cover, and is sealed with the upper cover by an insulating sealing material, and the upper cover is placed on top of the convex housing and seals the convex housing;

[0020] The lithium tank is used as a container for storing molten metal lithium, the lithium tank contains negative electrode materials, and a seal is formed between the lithium tank and the convex shell;

[0021] A bottom cover is connected to the bottom end of the convex shell.

[0022] Optionally, the ceramic electrolyte sheet, the lithium tank and the convex shell are sealed by an insulating sealing material.

[0023] The present disclosure provides a molten lithium metal battery based on a ceramic electrolyte sheet, wherein the molten lithium metal battery uses a ceramic electrolyte sheet to divide a convex shell into two parts, the upper part is a negative electrode compartment, and the lower part is a positive electrode compartment. The upper negative electrode compartment is provided with a lithium tank as a lithium storage chamber, and the lower positive electrode compartment is filled with positive electrode material. An air-conducting metal tube is connected to the convex shell and is connected to the positive electrode compartment. The liquid positive electrode lithium ion electrolyte can be vacuum-injected into the positive electrode compartment from the air-conducting metal tube.

[0024] Optionally, the lithium tank further includes an interface protection composition; the interface protection composition is a mixture of alkali metal salts or alkaline earth metal salts. Preferably, the interface protection composition is an alkali metal bromide salt or an alkaline earth metal bromide salt; preferably, the interface protection composition is any one of lithium bromide, sodium bromide, potassium bromide, and cesium bromide; preferably, the interface protection composition is a mixture of lithium bromide, potassium bromide, and cesium bromide.

[0025] Optionally, the diameter M of the interface protection composition is 3 to 400 mm, or M is 4 to 200 mm, or M is 5 to 50 mm, or M is 10 mm, or M is 15 mm, or M is 35 mm, or M is 40 mm.

[0026] Optionally, the thickness N of the interface protection composition is 0.2 to 300 mm, or N is 0.4 to 100 mm, or N is 0.5 to 50 mm, or N is 1 mm, or N is 5 mm, or N is 10 mm, or N is 20 mm.

[0027] Optionally, the ratio of the thickness N to the diameter M of the interface protection composition satisfies: 0.01≤N / M≤0.5, or 0.02≤N / M≤0.4, or 0.05≤N / M≤0.3, or 0.1≤N / M≤0.15.

[0028] Optionally, the negative electrode material is lithium or a lithium alloy; preferably, the negative electrode is a lithium-zinc alloy, a lithium-aluminum alloy, or a lithium-magnesium alloy.

[0029] Optionally, the diameter K of the negative electrode material is 3 to 400 mm, or K is 4 to 200 mm, or K is 5 to 50 mm, or K is 10 mm, or K is 15 mm, or K is 35 mm, or K is 40 mm.

[0030] Optionally, the thickness L of the negative electrode material is 0.2-300 mm, or L is 0.4-100 mm, or L is 0.5-50 mm, or L is 1 mm, or L is 5 mm, or L is 10 mm, or L is 20 mm.

[0031] Optionally, the ratio of the thickness L to the diameter K of the negative electrode material satisfies: 0.01≤L / K≤0.5, or 0.01≤L / K≤0.5, or 0.02≤L / K≤0.35, or 0.05≤L / K≤0.3, or 0.1≤L / K≤0.2.

[0032] Optionally, the interface protection composition is disposed between the ceramic electrolyte sheet and the negative electrode material.

[0033] The lithium tank of the molten lithium metal battery provided in the present disclosure is also provided with an interface protection composition, and the interface protection composition is provided between the ceramic electrolyte sheet and the negative electrode material. The melting point of the interface protection composition is lower than 500°C and is stable to molten lithium metal. For example, the interface protection composition can be a bromide salt mixture LiBr-KBr-CsBr. The interface protection composition is heated and melted to form a protective salt film on the surface of the ceramic electrolyte sheet, which can better protect the interface.

[0034] Optionally, the positive electrode compartment further includes a positive electrode ion-conducting electrolyte, which is introduced through a gas-conducting metal tube, and the positive electrode ion-conducting electrolyte is LiAlCl4; the liquid level of the positive electrode compartment is always higher than the bottom surface of the ceramic electrolyte sheet.

[0035] First, compared with ceramic tubes, the ceramic electrolyte sheet disclosed in the present invention is simpler to shape and easier to prepare.

[0036] In addition, in the present disclosure, the negative electrode compartment, ceramic electrolyte sheet and positive electrode compartment are designed as a top-down structure, which can make the negative electrode liquid phase protective layer in the negative electrode compartment contact evenly with the ceramic electrolyte sheet, avoiding the problem of loss of the liquid phase protective layer at the negative electrode in the existing U-shaped tube structure.

[0037] Furthermore, the battery structure provided by the present disclosure also includes a gas-conducting metal tube for introducing the positive electrode ion-conducting electrolyte, and the tube mouth of the gas-conducting metal tube is higher than the bottom surface of the ceramic electrolyte sheet. The existing technology usually mixes the solid-phase lithium-ion-conducting additive with the solid-phase positive electrode material, but the problems therein include: a. The additive and the positive electrode material are not mixed evenly; b. A small amount of additive cannot achieve a good lithium-ion-conducting effect. If more additives are used, it will occupy too much space in the positive electrode compartment. Since the space in the positive electrode compartment is limited, the positive electrode material will be reduced accordingly, resulting in a decrease in the capacity of the battery. The present disclosure adopts a gas-conducting metal tube design and a liquid lithium-ion-conducting electrolyte. The lithium-ion-conducting electrolyte is injected into the positive electrode compartment through the gas-conducting metal tube. The liquid lithium-ion-conducting electrolyte can not only improve the wettability of the positive electrode material and improve the lithium-ion-conducting ability, but also fill the gaps in the positive electrode material with the electrolyte, which will greatly reduce its occupied space and increase the capacity of the battery. If necessary, it can also be replenished. Furthermore, the design of the gas-conducting metal tube's opening being higher than the bottom surface of the ceramic electrolyte sheet ensures that the liquid level in the positive electrode compartment is always above the bottom of the ceramic electrolyte sheet, ensuring good contact between the positive electrode material and the ceramic electrolyte sheet. This provides a relatively good migration path for lithium ions and effectively reduces lithium ion diffusion resistance. Furthermore, the structural design of the gas-conducting metal tube effectively removes gas from the positive electrode compartment, resulting in a denser bond between the positive electrode materials.

[0038] Optionally, the molten lithium metal battery further includes: a lithium tank cover, which is arranged above the lithium tank and is used to close the opening of the lithium tank; one end of the negative electrode current collector is in contact with the ceramic electrolyte sheet, and the other end of the negative electrode current collector is led out from the lithium tank cover and the upper cover in sequence. In order to facilitate the addition of negative electrode materials and interface protection compositions into the lithium tank, the lithium tank described in the present disclosure can be a structure with an upward opening, so the lithium tank cover is correspondingly designed to close the opening of the lithium tank, so that a seal is formed between the lithium tank and the convex shell. At the same time, the close contact structure design between the negative electrode current collector and the ceramic electrolyte sheet further reduces the internal resistance of the battery, improves the rate performance of the battery, and thus improves the overall electrochemical performance of the battery.

[0039] Optionally, the diameter D of the ceramic electrolyte sheet is 5 to 500 mm, or D is 10 to 300 mm, or D is 15 to 200 mm, or D is 20 mm, or D is 30 mm, or D is 50 mm, or D is 80 mm.

[0040] Optionally, the diameter X of the lithium tank is 4 to 450 mm, or X is 8 to 300 mm, or X is 10 to 250 mm, or X is 15 mm, or X is 20 mm, or X is 30 mm, or X is 60 mm.

[0041] Optionally, the ratio of the diameter X of the lithium tank to the diameter D of the ceramic electrolyte sheet satisfies: 0.4≤X / D≤1.0, or 0.5≤X / D≤0.95, or 0.6≤X / D≤0.85, or 0.7≤X / D≤0.8.

[0042] Optionally, the height H of the positive electrode bin is 2 to 400 mm, or H is 3 to 200 mm, or H is 5 to 50 mm, or H is 10 mm, or H is 15 mm, or H is 35 mm, or H is 40 mm.

[0043] Optionally, the diameter Y of the positive electrode bin is 5 to 500 mm, or Y is 10 to 300 mm, or Y is 15 to 200 mm, or Y is 20 mm, or Y is 30 mm, or Y is 50 mm, or Y is 80 mm.

[0044] Optionally, the ratio of the height H to the diameter Y of the positive electrode compartment satisfies: 0.01≤H / Y≤0.8, or 0.03≤H / Y≤0.6, or 0.05≤H / Y≤0.5, or 0.1≤H / Y≤0.4, or 0.2≤H / Y≤0.3.

[0045] Optionally, the positive electrode material is a powder obtained by uniformly mixing lithium chloride LiCl and brass powder (CuZn alloy).

[0046] Optionally, the positive electrode lithium ion conductive electrolyte is poured in at a high temperature, which is not lower than 100°C.

[0047] Optionally, the insulating sealing material is a high-temperature resistant insulating material.

[0048] Optionally, the bottom cover is connected to the convex shell by welding.

[0049] Optionally, the upper cover is connected to the convex shell by welding.

[0050] Optionally, the gas-guiding metal tube is connected to the convex shell by welding.

[0051] Optionally, two symmetrically arranged gas-conducting metal tubes are connected to the convex shell, and the gas-conducting metal tubes are communicated with the interior of the positive electrode compartment.

[0052] Optionally, at least one layer of adsorption material is provided in the positive electrode compartment; the adsorption material includes at least one layer of open-pore structure, the open-pore structure includes a plurality of through holes arranged in a vertical direction, the interior of the holes of the open-pore structure is filled with the positive electrode material, and the non-pore part of the open-pore structure adsorbs the positive electrode ion-conducting electrolyte; the diameter of the holes in the open-pore structure is 3mm≤r1≤12mm, and the spacing y between the holes is ≤1mm.

[0053] Optionally, the adsorption material also includes at least one layer of non-opened porous structure, which is arranged on the bottom surface of the open porous structure and closes the bottom of the open porous structure; the interior of the pores of the open porous structure is filled with the positive electrode material, and the non-porous part of the open porous structure and the non-opened porous structure adsorb the positive electrode ion-conducting electrolyte; the diameter of the pores in the open porous structure r2 ≥ 3 mm, and the vertical distance h between the center position of the pores in the open porous structure and the adjacent non-opened porous structure is ≤ 6 mm.

[0054] Optionally, the open-pore structure is a honeycomb briquet configuration.

[0055] Optionally, the adsorption material is a three-dimensional structural material with alternating open-pore structures and non-open-pore structures.

[0056] Optionally, the adsorption material is made of carbon felt.

[0057] Solid-state batteries currently face the challenge of improving rate performance. As electrode thickness increases, the transport of lithium ions within the electrode pores becomes the rate-determining step in the battery's charge and discharge process. Under high-rate charge and discharge conditions, molten lithium batteries based on solid electrolytes experience a haphazard transfer of lithium ions within the cathode compartment, resulting in a tortuous transport process. This is due to the long ion transport distance within the cathode's high tortuosity, resulting in poor rate performance.

[0058] To address this problem, the present disclosure provides a molten lithium-ion battery positive electrode structure design using a honeycomb coal-shaped adsorption material. By filling the honeycomb coal with positive electrode material and adsorbing the lithium-ion conductive molten salt on the outside to form an efficient lithium-ion conductive channel and the ability to conduct electrons, the battery's rate performance is significantly improved. Specifically, referring to Figure 4, the adsorption material 13 is provided in the positive electrode compartment of the battery. The adsorption material 13 in Figure 4 only depicts a layer of open-pore structure. In this open-pore structure, the inside of the pore is filled with positive electrode material 14, and the non-porous structure between the pores adsorbs the positive electrode ion-conducting electrolyte. Lithium ions can be transmitted along the non-porous structure, thereby solving the problem of a long lithium ion transmission path. At the same time, in order to ensure that more positive electrode material can be filled in the pore, the diameter of the pore cannot be too small. However, it is also necessary to prevent the diameter of the pore from being too large. If the diameter of the pore is too large, the lithium ion transmission process will still have tortuous problems, so the size of the pore is limited, and the diameter of the pore in the open-pore structure is limited to 3mm≤r1≤12mm.

[0059] Therefore, at the same time, for some positive electrode bins with larger diameters, we want to set an open-pore material with a larger pore size in the positive electrode bin. In order to avoid the problem of the lithium ion transmission process being tortuous due to the large pores, the present disclosure further provides a structure of an adsorption material. Specifically, referring to Figure 13, the adsorption material 13 also includes at least one layer of non-opened-pore structure 16, and the non-opened-pore structure 16 is arranged on the bottom surface of the open-pore structure 15 and closes the bottom of the open-pore structure 15; the interior of the pores of the open-pore structure 15 is filled with the positive electrode material 14, and the non-porous part of the open-pore structure 15 and the non-opened-pore structure 16 adsorb the positive electrode ion-conducting electrolyte. In this adsorption material, the maximum diameter of the pores of the open-pore structure is not limited, but the vertical distance h from the center position of the pore to the adjacent non-opened-pore structure is limited to 6mm. In this way, lithium ions can be first transmitted to the non-opened-pore structure, and then transmitted along the non-porous structure in the open-pore structure. At this time, the lithium ion channel is L-shaped, which can also avoid the problem of tortuous lithium ion transmission process. Furthermore, the present disclosure may adopt a three-dimensional structure design of a molten lithium-ion battery positive electrode in which an open-pore structure of a honeycomb coal configuration is alternately designed with a non-open-pore adsorption material layer.

[0060] In summary, the adsorption material provided herein optimizes lithium-ion transport pathways, making it suitable for use in cathode compartments of various sizes while maintaining consistent battery rate performance. The adsorption material, such as carbon felt, possesses excellent electron conductivity and the ability to adsorb lithium-ion-conducting molten salts. Furthermore, the adsorption material exhibits high-temperature resistance of 250-400°C.

[0061] Optionally, the convex shell is made of 2 series stainless steel, 3 series stainless steel or 4 series stainless steel, preferably 304 material.

[0062] Optionally, the gas-guiding metal tube is made of 2 series stainless steel, 3 series stainless steel or 4 series stainless steel, preferably 304 material.

[0063] Optionally, the upper cover is made of 2 series stainless steel, 3 series stainless steel or 4 series stainless steel, preferably 304 material.

[0064] Optionally, the ceramic electrolyte sheet includes any one of a garnet-type oxide ceramic sheet, a lithium superion conductor (LISICON)-type oxide ceramic sheet, and a perovskite-type oxide ceramic sheet, preferably a garnet-type oxide ceramic sheet.

[0065] Optionally, the lithium tank is made of 2 series stainless steel, 3 series stainless steel or 4 series stainless steel, preferably 304 material.

[0066] Optionally, the bottom cover is made of 2 series stainless steel, 3 series stainless steel or 4 series stainless steel, preferably 304 material.

[0067] In a second aspect, the present disclosure provides a method for preparing the molten lithium metal battery as described above, comprising the following steps:

[0068] Placing the ceramic electrolyte sheet in the convex housing, dividing the convex housing into an upper negative electrode compartment and a lower positive electrode compartment, placing the lithium tank on the upper surface of the ceramic electrolyte sheet and within the negative electrode compartment; and sealing the ceramic electrolyte sheet, the lithium tank, and the convex housing with an insulating sealing material.

[0069] Loading the positive electrode material into the positive electrode compartment; optionally, first loading the adsorption material into the positive electrode compartment, and then loading the positive electrode material into the pores of the open pore structure of the adsorption material;

[0070] Connecting the bottom cover to the bottom of the convex housing;

[0071] Loading the negative electrode material into the lithium tank;

[0072] The upper cover is arranged on the top of the convex housing and the convex housing is sealed. The negative electrode current collector is led out from the upper cover. The connection between the negative electrode current collector and the upper cover is sealed with an insulating sealing material, and a seal is formed between the lithium tank and the convex housing;

[0073] The positive electrode lithium ion conductive electrolyte is vacuum-filled into the positive electrode compartment from the gas-conducting metal tube to form a molten lithium metal battery based on a ceramic electrolyte sheet.

[0074] Optionally, the molten lithium metal battery described in the present disclosure also includes a lithium tank cover. After the negative electrode material is loaded into the lithium tank, the lithium tank cover is placed above the lithium tank and is used to close the opening of the lithium tank; one end of the negative electrode current collector is in contact with the ceramic electrolyte sheet, and the other end of the negative electrode current collector is led out from the lithium tank cover and the upper cover in sequence. BRIEF DESCRIPTION OF THE DRAWINGS

[0075] FIG1 is a schematic diagram of a battery device according to Example 1.

[0076] FIG2 is a schematic diagram of a battery device according to Example 2.

[0077] FIG3 is a schematic diagram of a battery device according to Example 3.

[0078] FIG4 is a schematic diagram of a battery device according to Example 4.

[0079] FIG5 is a top view of a battery device.

[0080] FIG6 is a physical picture of the battery device.

[0081] FIG7 is a diagram showing the charge and discharge cycle data of the battery of Example 1.

[0082] FIG8 is a diagram showing the charge and discharge cycle data of the battery of Example 2.

[0083] FIG9 is a diagram showing the charge and discharge cycle data of the battery of Example 3.

[0084] FIG10 is a diagram showing the charge and discharge cycle data of the battery of Example 4.

[0085] FIG11 is a schematic diagram of a battery device of Comparative Example 1.

[0086] FIG12 is a charge-discharge cycle data diagram of Comparative Example 1.

[0087] FIG13 is a schematic diagram of the structure of the adsorption material.

[0088] 1. Convex shell, 2. Negative electrode current collector, insulating sealing material (3, 8), 4. Upper cover, 5. Lithium tank cover, 6. Lithium tank, 7. Negative electrode compartment, 9. Gas guide metal tube, 10. Ceramic electrolyte sheet, 11. Positive electrode compartment, 12. Bottom cover, 13. Adsorption material, 14. Positive electrode material, 15. Open-pore structure, 16. Non-open-pore structure. DETAILED DESCRIPTION

[0089] In order to further understand the present disclosure, preferred embodiments of the present disclosure are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present disclosure, rather than limiting the present disclosure.

[0090] The following describes some detailed embodiments of the present disclosure. Although the embodiments are described in the disclosure, they are not intended to limit the embodiments of the present disclosure to the contents shown. The embodiments of the present disclosure are only some examples of possible embodiments that may be formed in the claims. The remaining embodiments not shown in the claims and their alternatives, modifications, and equivalent embodiments are still within the scope of protection.

[0091] In order to achieve the above-mentioned objectives and effects, the present invention will be described below in conjunction with embodiments and drawings so that those skilled in the art can implement the present invention according to the following description.

[0092] First, please refer to Figures 1-4, which are three-dimensional sectional views of the present disclosure. It can be seen from the figures that the present disclosure provides a molten lithium metal battery based on a ceramic electrolyte sheet, and its structural design includes: 1. a convex shell, 2. a negative electrode current collector, an insulating sealing material (3, 8), 4. an upper cover, 5. a lithium tank cover, 6. a lithium tank, 7. a negative electrode compartment, 9. a gas-conducting metal tube, 10. a ceramic electrolyte sheet, 11. a positive electrode compartment, 12. a bottom cover, 13. an adsorption material, 14. a positive electrode material, 15. an open-pore structure, and 16. a non-open-pore structure.

[0093] Example 1

[0094] Positive electrode materials: LiCl powder, brass powder (wt%, Cu:Zn=52:48), LiAlCl4 (positive electrode lithium ion electrolyte, added to the positive electrode tank through the gas-conducting metal tube until the liquid level of the positive electrode ion-conducting electrolyte is higher than the bottom surface of the ceramic electrolyte sheet.

[0095] Anode material: LiZn alloy.

[0096] Battery reaction: positive electrode: Zn = Zn 2+ +2e

[0097] Anode: 2Li + +2e=2Li

[0098] The overall reaction of the battery: Zn + 2LiCl = ZnCl2 + 2Li

[0099] The masses of LiCl and brass powder were weighed to be 3.95 g and 7.26 g respectively (corresponding to the theoretical capacity of the battery of 2.5 Ah).

[0100] A molten lithium metal battery based on a ceramic electrolyte sheet, comprising:

[0101] A convex housing 1 and a ceramic electrolyte sheet 10, wherein the ceramic electrolyte sheet 10 divides the convex housing 1 into an upper portion and an lower portion, the upper portion being a negative electrode compartment 7 and a lower portion being a positive electrode compartment 11; the positive electrode 11 comprises positive electrode material, and the negative electrode compartment 7 is provided with a lithium tank 6; the upper surface of the ceramic electrolyte sheet 10 is in close contact with the lithium tank 6;

[0102] An air-conducting metal tube 9 is connected to the convex shell 1 and passes through the convex shell 1 for introducing the positive ion-conducting electrolyte, and the tube mouth of the air-conducting metal tube 9 is higher than the bottom surface of the ceramic electrolyte sheet 10;

[0103] An upper cover 4 and a negative electrode current collector 2, wherein the upper cover 4 is annular, the negative electrode current collector 2 passes through the upper cover 4 and is led out from the upper cover 4, and is sealed with the upper cover 4 through an insulating sealing material 3. The upper cover 4 is placed on the top of the convex housing 1 and seals the convex housing 1;

[0104] The lithium tank 6 is used as a container for storing molten metal lithium. The lithium tank 6 contains negative electrode materials. A seal is formed between the lithium tank 6 and the convex housing 1.

[0105] The bottom cover 12 is welded to the bottom end of the convex shell 1 .

[0106] The battery assembly process in this embodiment is as follows: Referring to Figure 1 , first, the ceramic electrolyte sheet 10, lithium tank 6, and convex housing 1 are sealed with insulating sealing material 8, wherein the lithium tank 6 is directly mounted on the ceramic electrolyte sheet 10. The diameter D of the ceramic electrolyte sheet 10 is 23 mm, and the diameter X of the lithium tank 6 is 18 mm.

[0107] Then, lithium chloride LiCl and brass powder are uniformly mixed into the positive electrode bin 11. The diameter Y of the positive electrode bin 11 is 38 mm and the height H is 5 mm.

[0108] While keeping the battery capacity unchanged, increasing the transverse diameter of the battery casing can reduce the thickness of the positive electrode and the migration distance of lithium ions, which is beneficial to improving the rate performance of the battery.

[0109] Furthermore, the bottom cover 12 is placed on the bottom of the convex housing 1 and welded together.

[0110] Subsequently, a bromide salt mixture LiBr-KBr-CsBr is placed in the lithium tank 6. The bromide salt mixture can better protect the interface, and its diameter M is 18 mm and thickness N is 1 mm. Then, the negative electrode material LiZn alloy is placed to form a negative electrode tank 7, wherein the diameter K of the negative electrode material LiZn alloy is 18 mm and the thickness L is 1 mm.

[0111] Furthermore, a lithium tank cover 5 is provided on the lithium tank 6 for closing the lithium tank 6, and an upper cover 4 is provided on the convex shell 1. The convex shell 1 and the upper cover 4 are connected together by welding. The negative electrode current collector 2 is led out from the lithium tank cover 5 and the upper cover 4. The connection between the negative electrode current collector 2 and the upper cover 4 is sealed with an insulating sealing material 3, and the insulating sealing material 3 is an insulating and high-temperature resistant material.

[0112] Finally, LiAlCl4 (positive electrode lithium ion electrolyte) is vacuum-filled into the positive electrode compartment 11 from the gas-conducting metal tube 9 under high temperature conditions and the gas-conducting metal tube 9 is welded to complete the assembly of the battery.

[0113] The charge and discharge data of the device are shown in FIG7 . The battery's first-cycle capacity utilization rate (capacity utilization rate = battery's first-cycle actual capacity / battery's theoretical capacity * 100%) is 98.7%, and the battery's coulombic efficiency reaches 91.6%.

[0114] Example 2:

[0115] Positive electrode materials: LiCl powder, brass powder (wt%, Cu:Zn=52:48), LiAlCl4 (positive electrode lithium ion conductive electrolyte, added to the positive electrode compartment from the gas-conducting metal tube until the liquid level of the positive electrode ion conductive electrolyte is higher than the bottom surface of the ceramic electrolyte sheet).

[0116] Anode material: LiZn alloy.

[0117] Battery reaction: positive electrode: Zn = Zn 2+ +2e

[0118] Anode: 2Li + +2e=2Li

[0119] The overall reaction of the battery: Zn + 2LiCl = ZnCl2 + 2Li

[0120] The masses of LiCl and brass powder were weighed to be 3.95 g and 7.26 g respectively (corresponding to the theoretical capacity of the battery of 2.5 Ah).

[0121] The structure of the molten lithium metal battery provided in Example 2 is the same as that of Example 1, but with some differences in size and structure, as described below.

[0122] Battery assembly process: Referring to Figure 2, first, the ceramic electrolyte sheet 10, the lithium tank 6 and the convex shell 1 are sealed with an insulating sealing material 8. The lithium tank 6 is directly set on the ceramic electrolyte sheet 10, wherein the diameter D of the ceramic electrolyte sheet 10 is 23 mm, and the diameter X of the lithium tank 6 is 18 mm.

[0123] Then, lithium chloride LiCl and brass powder are uniformly mixed into the positive electrode bin 11. The diameter Y of the upper part of the positive electrode bin 11 is 25 mm, the diameter Y of the lower part is 18 mm, and the height H is 7 mm.

[0124] Furthermore, the bottom cover 12 is placed on the bottom of the convex housing 1 and welded together.

[0125] Subsequently, a bromide salt mixture LiBr-KBr-CsBr is placed in the lithium tank 6. The bromide salt mixture can better protect the interface, and its diameter M is 18 mm and thickness N is 1 mm. Then, the negative electrode material LiZn alloy is placed to form a negative electrode tank 7, wherein the diameter K of the negative electrode material LiZn alloy is 18 mm and the thickness L is 1 mm.

[0126] Furthermore, a lithium tank cover 5 is provided on the lithium tank 6 for closing the lithium tank 6, and an upper cover 4 is provided on the convex shell 1. The convex shell 1 and the upper cover 4 are connected together by welding. The negative electrode current collector 2 is led out from the lithium tank cover 5 and the upper cover 4, and the connection between the negative electrode current collector 2 and the upper cover 4 is sealed with an insulating sealing material 3.

[0127] Finally, LiAlCl4 (positive electrode lithium ion electrolyte) is vacuum-filled into the positive electrode compartment 11 from the gas-conducting metal tube 9 under high temperature conditions and the gas-conducting metal tube 9 is welded to complete the assembly of the battery.

[0128] While maintaining the capacity of the battery unchanged, compared with Example 1, the longitudinal height is increased, the surface area ratio of the ceramic sheet to the positive electrode material area is increased, the tortuosity of lithium ion migration is improved, and it is beneficial to the migration of lithium ions.

[0129] The top view of the battery device is shown in Figure 5, and the actual device diagram of the battery is shown in Figure 6. Using the above-mentioned positive and negative electrode schemes, the charge and discharge data of the device are shown in Figure 8. The first cycle capacity utilization rate of the battery is 92.4%, and the coulombic efficiency of the battery reaches 94.6% (compared to the U-tube type coulombic efficiency of only 38.5% as shown in Figure 12). This shows that the dual gas-conducting metal tube design used in the battery device to infuse the lithium-ion electrolyte can further improve the wettability of the positive electrode material, and this structure can effectively remove the gas in the positive electrode compartment, making the positive electrode material more densely bonded. Moreover, the gas-conducting metal tube port of the convex shell is higher than the bottom design of the ceramic electrolyte sheet, which can ensure that the liquid level of the lower positive electrode compartment is always higher than the bottom of the ceramic electrolyte sheet, so that the positive electrode material has good contact with the electrolyte sheet, making the battery run better.

[0130] Example 3:

[0131] Positive electrode materials: LiCl powder, brass powder (wt%, Cu:Zn=52:48), LiAlCl4 (positive electrode lithium ion conductive electrolyte, added to the positive electrode compartment from the gas-conducting metal tube until the liquid level of the positive electrode ion conductive electrolyte is higher than the bottom surface of the ceramic electrolyte sheet).

[0132] Anode material: LiZn alloy.

[0133] Battery reaction: positive electrode: Zn = Zn 2+ +2e

[0134] Anode: 2Li + +2e=2Li

[0135] The overall reaction of the battery: Zn + 2LiCl = ZnCl2 + 2Li

[0136] The masses of LiCl and brass powder were weighed to be 3.95 g and 7.26 g respectively (corresponding to the theoretical capacity of the battery of 2.5 Ah).

[0137] The structure of the molten lithium metal battery provided in Example 3 is the same as that of Example 1, but with some differences in size and structure, as described below.

[0138] Battery assembly process: Referring to Figure 3, the ceramic electrolyte sheet 10, the lithium tank 6, and the convex shell 1 are first sealed with an insulating sealing material 8. The lithium tank 6 is directly placed on the ceramic electrolyte sheet 10. The diameter D of the ceramic electrolyte sheet 10 is 23 mm, and the diameter X of the lithium tank 6 is 18 mm.

[0139] Then, lithium chloride LiCl and brass powder are uniformly mixed into the positive electrode bin 11. The diameter Y of the positive electrode bin 11 is 38 mm and the height H is 5 mm.

[0140] Furthermore, the bottom cover 12 is placed on the bottom of the convex housing 1 and welded together.

[0141] Subsequently, a bromide salt mixture LiBr-KBr-CsBr is placed in the lithium tank 6. The bromide salt mixture can better protect the interface, and its diameter M is 18 mm and thickness N is 1 mm. Then, the negative electrode material LiZn alloy is placed to form a negative electrode tank 7, wherein the diameter K of the negative electrode material LiZn alloy is 18 mm and the thickness L is 1 mm.

[0142] Furthermore, a lithium tank cover 5 is provided on the lithium tank 6 for closing the lithium tank 6, and an upper cover 4 is provided on the convex shell 1. The convex shell 1 and the upper cover 4 are connected together by welding. The negative electrode current collector 2 is led out from the lithium tank cover 5 and the upper cover 4, and the connection between the negative electrode current collector 2 and the upper cover 4 is sealed with an insulating sealing material 3.

[0143] Finally, LiAlCl4 (positive electrode lithium ion conductive electrolyte) is vacuum poured into the positive electrode compartment 11 from the gas-conducting metal tube 9 under high temperature conditions and the gas-conducting metal tube 9 is welded to complete the assembly of the battery. The gas-conducting metal tube is L-shaped and is arranged on the side of the convex shell, but its tube mouth is still higher than the bottom surface of the ceramic electrolyte, which can ensure that the liquid level of the ion-conducting electrolyte in the positive electrode compartment is always higher than the bottom surface of the ceramic electrolyte sheet.

[0144] The charge and discharge data of the device are shown in Figure 9. The battery's first-cycle capacity utilization rate is 84.6%, and the battery's coulombic efficiency reaches 91.72%.

[0145] Example 4

[0146] Positive electrode materials: LiCl powder, brass powder (wt%, Cu:Zn=52:48), LiAlCl4 (positive electrode lithium ion conductive electrolyte, added to the positive electrode compartment from the gas-conducting metal tube until the liquid level of the positive electrode ion conductive electrolyte is higher than the bottom surface of the ceramic electrolyte sheet).

[0147] Anode material: LiZn alloy.

[0148] Battery reaction: positive electrode: Zn = Zn 2+ +2e

[0149] Anode: 2Li + +2e=2Li

[0150] The overall reaction of the battery: Zn + 2LiCl = ZnCl2 + 2Li

[0151] The masses of LiCl and brass powder were weighed to be 3.95 g and 7.26 g respectively (corresponding to the theoretical capacity of the battery of 2.5 Ah).

[0152] The structure of the molten lithium metal battery provided in Example 4 is basically the same as that of Example 1. The only difference is that adsorption material is added to the positive electrode compartment of the battery in this embodiment, see Figure 4 (only part of the adsorption material is drawn in Figure 4).

[0153] Battery assembly process: First, the ceramic electrolyte sheet 10, the lithium tank 6 and the convex shell 1 are sealed with an insulating sealing material 8. The lithium tank 6 is directly set on the ceramic electrolyte sheet 10. The diameter D of the ceramic electrolyte sheet 10 is 23 mm, and the diameter X of the lithium tank 6 is 18 mm.

[0154] Then add adsorption material to the positive electrode bin 11, and load the uniformly mixed powder of lithium chloride LiCl and brass powder into the inside of the pores of the adsorption material. The diameter Y of the positive electrode bin 11 is 38 mm, and the height H is 5 mm. The adsorption material is designed as a multi-layer open-pore structure, which can roughly fill the positive electrode bin. The pore diameter of the open-pore structure is 4.4 mm, and the distance between the pores is 0.5 mm.

[0155] Furthermore, the bottom cover 12 is placed on the bottom of the convex housing 1 and welded together.

[0156] Subsequently, a bromide salt mixture LiBr-KBr-CsBr is placed in the lithium tank 6. The bromide salt mixture can better protect the interface, and its diameter M is 18 mm and thickness N is 1 mm. Then, the negative electrode material LiZn alloy is placed to form a negative electrode tank 7, wherein the diameter K of the negative electrode material LiZn alloy is 18 mm and the thickness L is 1 mm.

[0157] Furthermore, a lithium tank cover 5 is provided on the lithium tank 6 for closing the lithium tank 6, and an upper cover 4 is provided on the convex shell 1. The convex shell 1 and the upper cover 4 are connected together by welding. The negative electrode current collector 2 is led out from the lithium tank cover 5 and the upper cover 4, and the connection between the negative electrode current collector 2 and the upper cover 4 is sealed with an insulating sealing material 3.

[0158] Finally, LiAlCl4 (positive electrode lithium ion electrolyte) is vacuum-filled into the positive electrode compartment 11 from the gas-conducting metal tube 9 under high temperature conditions and the gas-conducting metal tube 9 is welded to complete the assembly of the battery.

[0159] The charge and discharge data of the device are shown in Figure 10. The battery's first-cycle capacity utilization rate is 95.9%, and the battery's coulombic efficiency reaches 99.3%.

[0160] Comparative Example 1

[0161] The battery is shown in FIG11 , where 1 is the current collector network, 2 is the ceramic U-shaped tube, 3 is the LiBr-KBr-CsBr salt, and 4 is the electrode.

[0162] Positive electrode materials: LiCl powder, brass powder (wt%, Cu:Zn=52:48wt), LiAlCl4

[0163] Battery reaction: positive electrode: Zn = Zn 2+ +2e

[0164] Anode: 2Li + +2e=2Li

[0165] The overall reaction of the battery: Zn + 2LiCl = ZnCl2 + 2Li

[0166] Weigh 4.75 g of LiCl and 8.71 g of brass powder respectively (corresponding to a theoretical capacity of 3 Ah).

[0167] At high temperatures, the LiBr-KBr-CsBr salt not only prevents direct contact between lithium and the ceramic tube but also serves as a lithium ion conductor. A thin interfacial protective layer of LiBr-KBr-CsBr salt is first formed on the inner wall of the ceramic tube. A stainless steel mesh is then tightly bonded to the inner wall of the tube. This design prevents the generated metallic lithium from coming into direct contact with the U-shaped ceramic tube, preventing corrosion. However, the protective layer can dissipate and deposit at the bottom of the tube, causing the stainless steel and ceramic tube to lose their ability to conduct lithium ions. This loss of lithium ion conductivity creates dead lithium, resulting in low coulombic efficiency. As shown in Figure 12, the battery achieves 82.8% of its theoretical capacity in the first cycle, but its coulombic efficiency is only 38.5%, meaning a significant amount of lithium cannot be discharged. Furthermore, over prolonged high temperature conditions, the stainless steel mesh's supportive properties weaken or even disappear, preventing it from tightly bonding to the U-shaped tube. This increases the battery's internal resistance or even causes a short circuit, thus compromising battery performance.

[0168] In the present disclosure, the negative electrode compartment, ceramic electrolyte sheet and positive electrode compartment are designed as a top-down structure, which can make the negative electrode liquid phase protective layer and the electrolyte sheet contact evenly, avoiding the problem of loss of the liquid phase protective layer of the U-shaped tube at the negative electrode; the dual gas-conducting metal tube design adopted can further improve the wettability of the positive electrode material, and this structure can effectively remove the gas in the positive electrode compartment, making the positive electrode material more densely combined. Moreover, the design of the gas-conducting metal tube mouth of the convex shell being higher than the bottom surface of the ceramic electrolyte sheet can ensure that the liquid level of the lower positive electrode compartment is always higher than the bottom of the ceramic electrolyte sheet, so that the positive electrode material has good contact with the ceramic electrolyte sheet, providing a good migration path for lithium ions, and effectively reducing the lithium ion diffusion resistance; in addition, the present disclosure adopts a close contact structure design between the current collector and the ceramic electrolyte sheet, which further reduces the internal resistance of the battery, improves the rate performance of the battery, and thus improves the overall electrochemical performance of the battery.

[0169] Compared with the prior art, the present disclosure has at least the following beneficial effects:

[0170] (1) Compared with ceramic tubes, the ceramic electrolyte sheet disclosed in the present invention is simpler to shape and easier to prepare.

[0171] (2) In the present disclosure, the negative electrode compartment, ceramic electrolyte sheet and positive electrode compartment are designed as a top-down structure, which enables the negative electrode liquid phase protective layer in the negative electrode compartment to be in uniform contact with the ceramic electrolyte sheet, thereby avoiding the problem of loss of the liquid phase protective layer at the negative electrode in the existing U-tube structure.

[0172] (3) The present invention adopts the design of an air-conducting metal tube and the method of injecting a lithium-ion-conducting electrolyte into the positive electrode compartment through the air-conducting metal tube. The use of a liquid lithium-ion-conducting electrolyte can not only improve the wettability of the positive electrode material and enhance the lithium-ion-conducting ability, but also fill the gaps in the positive electrode material with the electrolyte, which greatly reduces the space occupied and increases the capacity of the battery. When necessary, liquid replenishment can also be performed.

[0173] (4) The design of the gas-conducting metal tube in the present disclosure being higher than the bottom surface of the ceramic electrolyte sheet can ensure that the liquid level in the positive electrode compartment is always higher than the bottom of the ceramic electrolyte sheet, so that the positive electrode material has good contact with the ceramic electrolyte sheet, providing a relatively good migration path for lithium ions and effectively reducing the lithium ion diffusion resistance.

[0174] (5) The structural design of the gas-conducting metal tube disclosed in the present invention can also effectively remove the gas in the positive electrode compartment, making the positive electrode material more densely bonded.

[0175] (6) The present disclosure adopts a structural design in which the current collector is in close contact with the ceramic electrolyte sheet, which further reduces the internal resistance of the battery, improves the rate performance of the battery, and thus improves the overall electrochemical performance of the battery.

[0176] (7) The positive electrode compartment designed in the present disclosure is also provided with an adsorption material. The inside of the pores in the open-pore structure of the adsorption material is filled with positive electrode material, and the outside adsorbs lithium-ion conductive molten salt to form a high-efficiency lithium-ion conductive channel and electron conductivity, thereby significantly improving the battery's rate performance. The three-dimensional structural design further optimizes the lithium-ion conductive channel, making it suitable for positive electrode compartments of various sizes.

[0177] Unless otherwise defined, the technical or scientific terms used in this disclosure shall have the ordinary meanings understood by persons having ordinary skills in the field to which this disclosure belongs. The words "first", "second" and similar terms used in this disclosure do not indicate any order, quantity or importance, but are only used to distinguish different components. The words "connected" or "connected" and similar terms are not limited to physical or mechanical connections, but may include electrical connections, whether direct or indirect. "Up", "down", "left", "right" and the like are only used to indicate relative positional relationships. When the absolute position of the object being described changes, the relative positional relationship also changes accordingly.

[0178] The above is a preferred embodiment of the present disclosure. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles described in the present disclosure. These improvements and modifications should also be regarded as the scope of protection of the present disclosure.

Claims

1. A molten lithium metal battery based on ceramic electrolyte sheets, include: A convex shell and a ceramic electrolyte sheet, wherein the ceramic electrolyte sheet divides the convex shell into two parts, the upper part is a negative electrode compartment, and the lower part is a positive electrode compartment; the positive electrode compartment includes positive electrode materials, and the negative electrode compartment is provided with a lithium tank; the upper surface of the ceramic electrolyte sheet is tightly fitted with the lithium tank; An air-conducting metal tube, the air-conducting metal tube is connected to the convex shell and passes through the convex shell, and the tube opening of the air-conducting metal tube is higher than the bottom surface of the ceramic electrolyte sheet; An upper cover and a negative electrode current collector, wherein the upper cover is annular, the negative electrode current collector passes through the upper cover and is led out from the upper cover, and is sealed with the upper cover through an insulating sealing material, and the upper cover is placed on the top of the convex shell and seals the convex shell; The lithium tank is used as a container for storing molten metal lithium, the lithium tank includes negative electrode material, and a seal is formed between the lithium tank and the convex shell; A bottom cover is connected to the bottom end of the convex shell.

2. The molten lithium metal battery according to claim 1, in, The ceramic electrolyte sheet, the lithium tank and the convex shell are hermetically sealed by an insulating sealing material.

3. The molten lithium metal battery according to claim 1, in, The lithium tank also includes an interface protection composition; The interface protection composition is a mixture of alkali metal salts or alkaline earth metal salts.

4. The molten lithium metal battery according to claim 1, in, The positive electrode compartment also includes a positive electrode ion-conducting electrolyte, and the positive electrode ion-conducting electrolyte is LiAlCl 4 ; The liquid level of the positive electrode compartment is always higher than the bottom surface of the ceramic electrolyte sheet.

5. The molten lithium metal battery according to claim 1, in, The molten lithium metal battery also includes: A lithium tank cover, which is disposed above the lithium tank and is used to close the opening of the lithium tank; One end of the negative electrode current collector is in contact with the ceramic electrolyte sheet, and the other end of the negative electrode current collector is led out from the lithium tank cover and the upper cover in sequence.

6. The molten lithium metal battery according to claim 1, in, The diameter D of the ceramic electrolyte sheet is 5 to 500 mm, the diameter X of the lithium tank is 4 to 450 mm, and the ratio of the diameter X of the lithium tank to the diameter D of the ceramic electrolyte sheet satisfies: 0.4≤X / D≤1.

0.

7. The molten lithium metal battery according to claim 3, in, The diameter M of the interface protection composition is 3 to 400 mm; and / or The thickness N of the interface protection composition is 0.2 to 300 mm; and / or The ratio of the thickness N to the diameter M of the interface protection composition satisfies: 0.01≤N / M≤0.

5.

8. The molten lithium metal battery according to claim 4, in, At least one layer of adsorption material is provided in the positive electrode compartment; The adsorption material comprises at least one layer of open-pore structure, wherein the open-pore structure comprises a plurality of through-holes arranged in a vertical direction, the inside of the pores of the open-pore structure is filled with the positive electrode material, and the non-pore part of the open-pore structure adsorbs the positive electrode ion-conducting electrolyte; The diameter of the hole in the open-pore structure is 3 mm ≤ r 1 ≤12mm, the spacing between holes y≤1mm.

9. The molten lithium metal battery according to claim 8, It is characterized in that The adsorption material further comprises at least one layer of non-opened pore structure, wherein the non-opened pore structure is arranged on the bottom surface of the open pore structure and closes the bottom of the open pore structure; the positive electrode material is filled in the pores of the open pore structure, and the non-pore part of the open pore structure and the non-opened pore structure adsorb the positive electrode ion-conducting electrolyte; The diameter r of the hole in the open-cell structure 2 ≥3mm, and the vertical distance h between the center of the hole in the open-pored structure and the adjacent non-open-pored structure is ≤6mm.

10. The method for preparing a molten lithium metal battery according to any one of claims 1 to 9, The following steps are involved: The ceramic electrolyte sheet is placed in the convex shell, the convex shell is divided into an upper negative electrode compartment and a lower positive electrode compartment, the lithium tank is arranged on the upper surface of the ceramic electrolyte sheet and the lithium tank is located in the negative electrode compartment; the ceramic electrolyte sheet, the lithium tank and the convex shell are sealed with an insulating sealing material; Loading positive electrode material and / or adsorption material into the positive electrode compartment; Connecting the bottom cover to the bottom of the convex shell; Loading the negative electrode material into the lithium tank; The upper cover is arranged on the top of the convex shell and the convex shell is sealed, the negative electrode current collector is led out from the upper cover, the connection between the negative electrode current collector and the upper cover is sealed with an insulating sealing material, and a seal is formed between the lithium tank and the convex shell; The positive electrode lithium ion electrolyte is vacuum-filled into the positive electrode compartment from the gas-conducting metal tube to form a A molten lithium metal battery based on a ceramic electrolyte sheet.

Citation Information

Patent Citations

  • Molten lithium oxygen electrochemical cell

    CN109075412A

  • Solid electrolyte-based molten lithium electrochemical cells

    CN112514136A

  • High energy density molten lithium-sulfur and lithium-selenium batteries with solid electrolyte

    CN113678300A

  • Molten lithium-sulfur battery with solid electrolyte and method of manufacturing the same

    US20190006720A1

  • Button lithium battery adopting lithium-ion solid electrolytic sheet as diaphragm and preparation method of battery

    CN109285983A