Lithium secondary battery

By using a positive electrode current collector with a composite elastic modulus of 17.0 GPa or less, the lithium secondary battery prevents peeling between the solid electrolyte and the current collector, improving battery reliability and durability while simplifying the manufacturing process.

WO2024214202A1PCT designated stage expired Publication Date: 2024-10-17NISSAN MOTOR CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/014819
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-12
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

In all-solid-state lithium secondary batteries, peeling occurs between the solid electrolyte layer and the positive electrode current collector when the solid electrolyte layer covers the positive electrode active material layer and extends to the current collector, leading to reliability issues and potential short circuits.

Method used

A lithium secondary battery design where the positive electrode current collector has a composite elastic modulus of 17.0 GPa or less on the main surface of the positive electrode active material layer, ensuring a gap between the solid electrolyte layer and the current collector, thereby preventing peeling and improving adhesion.

Benefits of technology

This configuration enhances the cycle durability of the battery, simplifies the handling of the fragile solid electrolyte layer, and reduces manufacturing time and costs by ensuring a stable interface between the solid electrolyte and the current collector.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023014819_17102024_PF_FP_ABST
    Figure JP2023014819_17102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides, in a lithium secondary battery provided with a solid electrolyte layer covering the outer side of a positive electrode active material layer and extending to a positive electrode current collector, a means that is capable of suppressing the occurrence of peeling between the solid electrolyte layer and the positive electrode current collector. According to the present invention, the lithium secondary battery provided with the solid electrolyte layer covering the outer side of the positive electrode active material layer uses a positive electrode current collector having a composite elastic modulus value of 17.0 [GPa] or less, the composite elastic modulus value being measured for a main surface on the positive electrode active material layer side by a spherical nanoindentation method.
Need to check novelty before this filing date? Find Prior Art

Description

Lithium secondary battery

[0001] The present invention relates to a lithium secondary battery.

[0002] In recent years, there has been active research and development into all-solid-state lithium secondary batteries that use oxide- or sulfide-based solid electrolytes. Solid electrolytes are materials primarily composed of ionic conductors that allow ionic conduction in a solid state. Therefore, all-solid-state lithium secondary batteries do not, in principle, encounter the various problems associated with flammable organic electrolytes that occur in conventional liquid-based lithium-ion secondary batteries. In addition, the use of high-potential, high-capacity positive electrode materials and high-capacity negative electrode materials generally leads to significant improvements in the battery's power density and energy density.

[0003] Even in such all-solid-state lithium secondary batteries, preventing a short circuit between the positive electrode and the negative electrode is important for improving the reliability of the battery. Here, as a technology for preventing a short circuit between the positive and negative electrodes, for example, International Publication No. 2018 / 110688 discloses a technology for an all-solid-state lithium secondary battery including a positive electrode current collector, a negative electrode current collector, and a powder laminate disposed between the positive electrode current collector and the negative electrode current collector, in which the powder laminate is configured from a positive electrode powder layer, a negative electrode powder layer, and a solid electrolyte layer disposed between the positive electrode powder layer and the negative electrode powder layer and covering the outer periphery of the positive electrode powder layer and the negative electrode powder layer. According to International Publication No. 2018 / 110688, such a configuration effectively prevents a short circuit between the positive and negative electrodes.

[0004] However, according to the investigations of the present inventors, it has been found that when the technology described in WO 2018 / 110688 is used, peeling may occur between the solid electrolyte layer and the positive electrode current collector, particularly when the solid electrolyte layer covers the positive electrode active material layer and extends to the positive electrode current collector.

[0005] Therefore, an object of the present invention is to provide a means capable of suppressing the occurrence of peeling between a solid electrolyte layer and a positive electrode current collector in a lithium secondary battery having a solid electrolyte layer that covers the outside of a positive electrode active material layer and extends to the positive electrode current collector.

[0006] The present inventors have conducted extensive research to solve the above-mentioned problems, and as a result, have found that in a lithium secondary battery including a solid electrolyte layer covering the outside of a positive electrode active material layer, the above-mentioned problems can be solved by using a positive electrode current collector whose main surface on the positive electrode active material layer side has a composite elastic modulus of a predetermined value or less, thereby completing the present invention.

[0007] That is, one aspect of the present invention relates to a lithium secondary battery including a power generating element including a positive electrode having a positive electrode active material layer disposed on the surface of a positive electrode current collector, a negative electrode, and a solid electrolyte layer interposed between the positive electrode and the negative electrode and containing a solid electrolyte. The lithium secondary battery is characterized in that the solid electrolyte layer extends to the positive electrode current collector so as to cover at least a portion of a side surface of the positive electrode active material layer, and the value of the composite elastic modulus measured by spherical nanoindentation on the main surface of the positive electrode current collector facing the positive electrode active material layer is 17.0 GPa or less.

[0008] Fig. 3 is a cross-sectional view schematically showing the overall structure of a stacked-type (internal parallel connection type) all-solid-state lithium secondary battery (stacked-type secondary battery) according to one embodiment of the present invention. Fig. 4 is an enlarged cross-sectional view of a unit cell layer of a stacked-type secondary battery according to one embodiment of the present invention. Fig. 5 is a perspective view of a stacked-type secondary battery according to one embodiment of the present invention. Fig. 6 is a side view seen from direction A shown in Fig. 3. Fig. 7 is an enlarged cross-sectional view of a unit cell layer of a stacked-type secondary battery according to another embodiment of the present invention.

[0009] One aspect of the present invention is a lithium secondary battery comprising a power generating element including a positive electrode having a positive electrode active material layer disposed on the surface of a positive electrode current collector, a negative electrode, and a solid electrolyte layer interposed between the positive electrode and the negative electrode and containing a solid electrolyte, wherein the solid electrolyte layer extends to the positive electrode current collector so as to cover at least a portion of the side surface of the positive electrode active material layer, and the composite elastic modulus measured by spherical nanoindentation on the main surface of the positive electrode current collector facing the positive electrode active material layer is 17.0 GPa or less. By adopting this configuration, in a lithium secondary battery having a solid electrolyte layer covering the outside of the positive electrode active material layer and extending to the positive electrode current collector, peeling between the solid electrolyte layer and the positive electrode current collector is suppressed. This can contribute to improving the cycle durability of the battery. Furthermore, by realizing an integrated structure of the positive electrode current collector, the positive electrode active material layer, and the solid electrolyte layer, the handleability of the normally fragile solid electrolyte layer is improved, and the time and cost required for the manufacturing process can be reduced.

[0010] The present embodiment will be described below with reference to the drawings, but the technical scope of the present invention should be determined based on the description of the claims and is not limited to the following embodiment. Note that the dimensional proportions in the drawings are exaggerated for the convenience of explanation and may differ from the actual proportions.

[0011] FIG. 1 is a cross-sectional view schematically illustrating the overall structure of a stacked-type (internal parallel connection type) all-solid-state lithium secondary battery (hereinafter simply referred to as a "stacked-type secondary battery") according to one embodiment of the present invention. The stacked-type secondary battery 10a shown in FIG. 1 has a structure in which a substantially rectangular power generating element 21, where charge and discharge reactions actually occur, is sealed inside a laminate film 29, which is a battery exterior. Note that FIG. 1 shows a cross-section of the stacked-type secondary battery during charging, and thus, a negative electrode active material layer 13 made of lithium metal is present between the negative electrode current collector 11' and the solid electrolyte layer 17. Furthermore, a pressure member (not shown) applies a restraining pressure to the stacked-type secondary battery 10a in the stacking direction of the power generating element 21. Therefore, the volume of the power generating element 21 is maintained constant.

[0012] As shown in FIG. 1 , a power generating element 21 of a stacked secondary battery 10 a of this embodiment has a configuration in which a negative electrode in which a negative electrode active material layer 13 containing lithium metal is disposed on both sides of a negative electrode current collector 11 ′, a solid electrolyte layer 17, and a positive electrode in which a positive electrode active material layer 15 containing a lithium transition metal composite oxide is disposed on both sides of a positive electrode current collector 11 ″ are laminated. Specifically, the negative electrode, solid electrolyte layer, and positive electrode are laminated in this order such that one negative electrode active material layer 13 and an adjacent positive electrode active material layer 15 face each other with the solid electrolyte layer 17 interposed therebetween. As a result, adjacent negative electrode, solid electrolyte layer, and positive electrode constitute one unit cell layer 19. Therefore, the stacked secondary battery 10 a shown in FIG. 1 can also be said to have a configuration in which a plurality of unit cell layers 19 are stacked and electrically connected in parallel.

[0013] A negative electrode current collector 25 and a positive electrode current collector 27 that are electrically connected to the respective electrodes (negative and positive electrodes) are attached to the negative electrode current collector 11′ and the positive electrode current collector 11″, respectively, and are configured to be sandwiched between the ends of the laminate film 29 and led out of the laminate film 29. The negative electrode current collector 25 and the positive electrode current collector 27 may be attached to the negative electrode current collector 11′ and the positive electrode current collector 11″ of the respective electrodes by ultrasonic welding, resistance welding, or the like, via a negative electrode terminal lead and a positive electrode terminal lead (not shown), respectively, as necessary.

[0014] In the above description, an embodiment of the lithium secondary battery according to one aspect of the present invention has been described using as an example a so-called lithium deposition type, stacked type (internal parallel connection type) all-solid-state lithium secondary battery in which lithium metal is deposited on the surface of the negative electrode current collector during charging. However, the type of lithium secondary battery to which the present invention can be applied is not particularly limited, and the present invention can also be applied to lithium secondary batteries that are not of the lithium deposition type and bipolar type lithium secondary batteries.

[0015] FIG. 2 is an enlarged cross-sectional view of a cell layer 19 of a stacked secondary battery according to one embodiment of the present invention. As shown in FIG. 2 , the cell layer 19 constituting the stacked secondary battery 10 a according to this embodiment has a positive electrode composed of a positive electrode current collector 11″ and a positive electrode active material layer 15 disposed on the surface thereof. A solid electrolyte layer 17 containing a solid electrolyte is disposed on the surface of the positive electrode active material layer 15 opposite the positive electrode current collector 11″. In the embodiment shown in FIG. 2 , the solid electrolyte layer 17 extends to reach the positive electrode current collector 11″ so as to cover the entire outer periphery of the positive electrode active material layer 15. In the embodiment shown in FIG. 2 , a carbon black layer 18 containing carbon black nanoparticles is provided on the main surface of the solid electrolyte layer 17 facing the negative electrode current collector 11′ in a region including the entire region where the positive electrode active material layer 15 faces the negative electrode current collector 11′ (in other words, a size slightly larger than the positive electrode active material layer 15 when the power generating element 21 is viewed from above). This carbon black layer 18 The carbon black constituting the negative electrode current collector 11′ has lithium ion conductivity, and therefore the carbon black layer 18 can conduct lithium ions. Therefore, the provision of the carbon black layer 18 does not impede the progress of the battery reaction. The carbon black layer 18 also has the function of suppressing the reaction between the lithium metal (negative electrode active material layer 13) deposited on the negative electrode current collector 11′ and the solid electrolyte contained in the solid electrolyte layer 17 during charging. Therefore, the carbon black layer 18 can be said to function as an ion-conductive reaction suppression layer.

[0016] FIG. 3 is a perspective view of a stacked secondary battery according to one embodiment of the present invention. FIG. 4 is a side view taken from direction A in FIG. 3 . As shown in FIGS. 3 and 4 , the stacked secondary battery 100 according to this embodiment includes the stacked secondary battery 10a shown in FIG. 1 , two metal plates 200 sandwiching the stacked secondary battery 10a, and bolts 300 and nuts 400 as fastening members. These fastening members (bolts 300 and nuts 400) function to secure the stacked secondary battery 10a in a sandwiched state between the metal plates 200. As a result, the metal plates 200 and the fastening members (bolts 300 and nuts 400) function as pressure members that pressurize (restrain) the stacked secondary battery 10a in the stacking direction. The pressure members are not particularly limited as long as they can pressurize the stacked secondary battery 10a in the stacking direction. A combination of a plate made of a rigid material, such as the metal plate 200, and the fastening members described above is typically used as the pressure members. Furthermore, the fastening members are not limited to the bolts 300 and nuts 400, and may include tension plates or the like that fix the ends of the metal plates 200 so as to restrain the stacked secondary battery 10a in the stacking direction.

[0017] The lower limit of the load applied to the stacked secondary battery 10a (confining pressure in the stacking direction of the stacked secondary battery) is, for example, 0.1 MPa or more, preferably 1 MPa or more, more preferably 3 MPa or more, and even more preferably 5 MPa or more. The upper limit of the confining pressure in the stacking direction of the stacked secondary battery is, for example, 100 MPa or less, preferably 70 MPa or less, more preferably 40 MPa or less, and even more preferably 10 MPa or less.

[0018] The main components of the stacked secondary battery 10a will be described below.

[0019] [Positive electrode current collector] The positive electrode current collector is a conductive member that functions as a flow path for electrons that are released from the positive electrode toward the power source as the charging reaction progresses and that flow from an external load toward the positive electrode as the discharging reaction progresses.

[0020] The positive electrode current collector used in the lithium secondary battery according to this embodiment is characterized in that the main surface on the positive electrode active material layer side has a composite elastic modulus of 17.0 GPa or less, as measured by spherical nanoindentation. This configuration suppresses peeling between the solid electrolyte layer and the positive electrode current collector in a lithium secondary battery having a solid electrolyte layer that covers the outside of the positive electrode active material layer and extends to the positive electrode current collector. This is thought to be because, when the positive electrode current collector and the solid electrolyte layer are bonded together with the positive electrode active material layer sandwiched therebetween during the manufacture of the lithium secondary battery, the material constituting the solid electrolyte layer is more likely to penetrate into the positive electrode current collector, which has a small composite elastic modulus, thereby improving adhesion between the positive electrode current collector and the solid electrolyte layer.

[0021] The value of the composite elastic modulus may be 17.0 [GPa] or less, and from the viewpoint of preventing peeling, the smaller this value, the more preferable. Specifically, the value of the composite elastic modulus is preferably 15.0 [GPa] or less, more preferably 13.0 [GPa] or less, even more preferably 11.0 [GPa] or less, even more preferably 10.2 [GPa] or less, even more preferably 9.0 [GPa] or less, particularly preferably 5.0 [GPa] or less, and most preferably 1.0 [GPa] or less. On the other hand, from the viewpoint of the strength and handleability of the positive electrode current collector itself, the value of the composite elastic modulus is preferably 0.5 [GPa] or more. That is, in a preferred embodiment, the value of the composite elastic modulus is 0.5 to 17.0 [GPa]. Note that the value of the composite elastic modulus of the positive electrode current collector is a value measured by the method described in the Examples section below.

[0022] The material constituting the positive electrode current collector is not particularly limited as long as the composite elastic modulus of the main surface on the positive electrode active material layer side is within the above-mentioned range. Examples of the material constituting the positive electrode current collector include metals and conductive resins (such as resins containing a non-conductive polymer material and a conductive filler). However, the main surface of the positive electrode current collector on the positive electrode active material layer side is preferably composed of an inorganic material such as a metal or a carbon material, and it is more preferable that the entire positive electrode current collector be composed of an inorganic material such as a metal or a carbon material. Among these, the material constituting the positive electrode current collector is preferably an etched aluminum foil whose main surface on the positive electrode active material layer side is etched, a carbon-coated aluminum foil whose main surface on the positive electrode active material layer side is coated with a carbon material, a roughened aluminum foil whose main surface on the positive electrode active material layer side is roughened, or a carbon foil. These materials may be purchased and etched, coated with a carbon material, roughened, or the like, or may be used by subjecting untreated materials to these treatments. The current collector may have a single layer structure made of a single material, or may have a laminate structure in which layers made of the above materials are appropriately combined. There are no particular restrictions on the thickness of the positive electrode current collector, but it is, for example, 10 to 100 μm.

[0023] [Positive Electrode Active Material Layer] The positive electrode constituting the lithium secondary battery according to this embodiment has a positive electrode active material layer containing a positive electrode active material. The positive electrode active material layer 15 is disposed on the surface of a positive electrode current collector 11″ as shown in FIG. 1 .

[0024] The positive electrode active material is not particularly limited as long as it can release lithium ions during the charging process of the secondary battery and absorb lithium ions during the discharging process. An example of such a positive electrode active material is a material containing an M1 element and an O element, where the M1 element contains at least one element selected from the group consisting of Li, Mn, Ni, Co, Cr, Fe, and P. An example of such a positive electrode active material is LiCoO 2 , LiMnO 2 , LiNiO 2 , Li(Ni-Mn-Co)O 2Layered rock salt active materials such as LiMn 2 O 4 , LiNi 0.5 Mn 1.5 O 4 Spinel-type active materials such as LiFePO 4 , LiMnPO 4 Olivine type active materials such as Li 2 FeSiO 4 , Li 2 MnSiO 4 Examples of oxide active materials other than those mentioned above include Si-containing active materials such as Li 4 Ti 5 O 12 , LiVO 2 In some cases, two or more types of positive electrode active materials may be used in combination. Of course, positive electrode active materials other than those mentioned above may also be used. In a preferred embodiment, the positive electrode active material layer 15 constituting the lithium secondary battery according to this embodiment is made of a layered rock salt type active material containing lithium and cobalt as the positive electrode active material (for example, Li(Ni—Mn—Co)O 2 ) is included.

[0025] The shape of the positive electrode active material may be, for example, particulate (spherical, fibrous), thin film, etc. When the positive electrode active material is particulate, its average particle size (D50) is, for example, preferably in the range of 1 nm to 100 μm, more preferably in the range of 10 nm to 50 μm, even more preferably in the range of 100 nm to 20 μm, and particularly preferably in the range of 1 to 20 μm. In this specification, the average particle size (D50) of the positive electrode active material can be measured by a laser diffraction scattering method.

[0026] The content of the positive electrode active material in the positive electrode active material layer is not particularly limited, but is preferably in the range of 30 to 99 mass %, more preferably in the range of 40 to 90 mass %, and even more preferably in the range of 45 to 80 mass %.

[0027] In the lithium secondary battery according to this embodiment, the positive electrode active material layer 15 preferably further contains a solid electrolyte. In this specification, the term "solid electrolyte" refers to a material mainly composed of an ion conductor capable of conducting ions in a solid state, and in particular, a material having a lithium ion conductivity of 1×10 at room temperature (25° C.). -5 S / cm or more, and this lithium ion conductivity is preferably 1×10 -4 The ionic conductivity is 200 S / cm or more. Here, the value of the ionic conductivity can be measured by an AC impedance method.

[0028] Examples of the solid electrolyte include a sulfide solid electrolyte and an oxide solid electrolyte. In a preferred embodiment of the lithium secondary battery according to this aspect, the solid electrolyte is preferably a sulfide solid electrolyte containing an S element, more preferably a sulfide solid electrolyte containing a Li element, an M element, and an S element, wherein the M element contains at least one element selected from the group consisting of P, Si, Ge, Sn, Ti, Zr, Nb, Al, Sb, Br, Cl, and I, from the viewpoint of exhibiting excellent lithium ion conductivity and being able to better follow volume changes of the electrode active material during charge and discharge, and even more preferably a sulfide solid electrolyte containing an S element, a Li element, and a P element.

[0029] The sulfide solid electrolyte is Li 3 P.S. 4 It may have a Li framework. 4 P 2 S 7 It may have a Li framework. 4 P 2 S 6 It may have a Li skeleton. 3 P.S. 4 Examples of sulfide solid electrolytes having a skeleton include LiI-Li 3 P.S. 4 , LiI-LiBr-Li 3 P.S. 4 , Li 3 P.S. 4 In addition, Li 4 P 2 S 7Examples of sulfide solid electrolytes having a skeleton include Li-P-S solid electrolytes called LPS. (4-x) Ge (1-x) P x S 4 (x satisfies 0<x<1) or the like. More specifically, for example, LPS (Li 2 S-P 2 S 5 ), Li 7 P 3 S 11 , Li 3.2 P 0.96 S., Li. 3.25 Ge 0.25 P 0.75 S 4 , Li 10 GeP 2 S 12 , or Li 6 P.S. 5 X (wherein X is Cl, Br or I). 2 S-P 2 S 5 " is written by Li 2 S and P 2 S 5 The same applies to other descriptions. Among them, the sulfide solid electrolyte is preferably LPS (Li 2 S-P 2 S 5 ), Li 6 P.S. 5 X (wherein X is Cl, Br or I), Li 7 P 3 S 11 , Li 3.2 P 0.96 S and Li 3 P.S. 4 is selected from the group consisting of:

[0030] The content of the solid electrolyte in the positive electrode active material layer is not particularly limited, but is preferably within the range of 1 to 70 mass %, more preferably within the range of 10 to 60 mass %, and even more preferably within the range of 20 to 55 mass %.

[0031] The positive electrode active material layer may further contain at least one of a conductive additive and a binder in addition to the positive electrode active material and the solid electrolyte. The thickness of the positive electrode active material layer varies depending on the configuration of the intended lithium secondary battery, but is preferably within a range of, for example, 0.1 to 1000 μm, and more preferably 40 to 100 μm.

[0032] [Solid Electrolyte Layer] The solid electrolyte layer is a layer interposed between the positive electrode and the negative electrode and contains a solid electrolyte (usually as a main component). The specific form of the solid electrolyte contained in the solid electrolyte layer is the same as that described above, and therefore a detailed description thereof will be omitted here. The content of the solid electrolyte in the solid electrolyte layer is, for example, preferably in the range of 10 to 100 mass%, more preferably in the range of 50 to 100 mass%, and even more preferably in the range of 90 to 100 mass%, relative to the total mass of the solid electrolyte layer. In addition to the solid electrolyte described above, the solid electrolyte layer may further contain a binder. The thickness of the solid electrolyte layer varies depending on the configuration of the intended lithium secondary battery, but is, for example, preferably in the range of 0.1 to 1000 μm, more preferably 10 to 40 μm.

[0033] [Negative Electrode Current Collector] The negative electrode current collector is a conductive member that functions as a flow path for electrons that are released from the negative electrode toward an external load as the discharge reaction progresses and that flow from the power source toward the negative electrode as the charge reaction progresses. There are no particular restrictions on the material that constitutes the negative electrode current collector. For example, metals and conductive resins can be used as materials for the negative electrode current collector. There are no particular restrictions on the thickness of the negative electrode current collector, but an example is 10 to 100 μm.

[0034] [Negative Electrode Active Material Layer] The negative electrode constituting the lithium secondary battery according to this embodiment has a negative electrode active material layer 13 containing a negative electrode active material. The negative electrode active material layer 13 is disposed on the surface of the negative electrode current collector 11′ as shown in FIG.

[0035] The specific type of negative electrode active material is not particularly limited. Examples of such negative electrode active materials include carbon materials, metal oxides, and metal active materials. Furthermore, a lithium-containing metal may be used as the negative electrode active material. Such a negative electrode active material is not particularly limited as long as it is a lithium-containing active material, and examples thereof include metallic lithium and lithium-containing alloys. Examples of lithium-containing alloys include alloys of Li with at least one of In, Al, Si, Sn, Mg, Au, Ag, and Zn. The negative electrode active material preferably includes metallic lithium or a lithium-containing alloy, a silicon-based negative electrode active material, or a tin-based negative electrode active material, and particularly preferably includes metallic lithium or a lithium-containing alloy. When metallic lithium or a lithium-containing alloy is used as the negative electrode active material, the lithium secondary battery according to this embodiment may be a so-called lithium deposition type in which lithium metal as the negative electrode active material is deposited on the negative electrode current collector during charging. Therefore, in this configuration, the thickness of the negative electrode active material layer increases as the charging process progresses and decreases as the discharging process progresses. The negative electrode active material layer does not need to be present during full discharge, but in some cases, a negative electrode active material layer made of a certain amount of lithium metal may be present during full discharge.

[0036] The content of the negative electrode active material in the negative electrode active material layer is not particularly limited, but is preferably within the range of 40 to 100 mass %, and more preferably within the range of 50 to 90 mass %, for example.

[0037] The negative electrode active material layer may further contain a solid electrolyte as needed. By including the solid electrolyte in the negative electrode active material layer, the ionic conductivity of the negative electrode active material layer can be improved. The specific form of the solid electrolyte contained in the negative electrode active material layer is the same as that described above, and therefore a detailed description thereof will be omitted here.

[0038] The content of the solid electrolyte in the negative electrode active material layer is, for example, preferably in the range of 1 to 60 mass %, and more preferably in the range of 10 to 50 mass %.

[0039] The negative electrode active material layer may further contain at least one of a binder and a conductive additive in addition to the above-described negative electrode active material and solid electrolyte. The thickness of the negative electrode active material layer varies depending on the configuration of the intended secondary battery, but is preferably within a range of, for example, 0.1 to 1000 μm, and more preferably 40 to 100 μm.

[0040] [Ion-Conductive Reaction Suppression Layer (Anode Intermediate Layer)] In the lithium secondary battery according to this embodiment, an ion-conductive reaction suppression layer (also referred to as an "anode intermediate layer") is preferably provided on at least a portion of the region of the main surface of the solid electrolyte layer facing the anode current collector, where the positive electrode active material layer faces the anode current collector. This ion-conductive reaction suppression layer has lithium ion conductivity and suppresses the reaction between lithium metal (anode active material layer) and the solid electrolyte. Therefore, by providing the ion-conductive reaction suppression layer, it is possible to prevent degradation of the solid electrolyte and a decrease in battery capacity caused by the reaction between lithium metal (anode active material layer) and the solid electrolyte without impeding the progress of the battery reaction. The lithium ion conductivity of the constituent material of the ion-conductive reaction suppression layer at 25°C is preferably 1×10 -4 [S / cm] or more, more preferably 1.5 × 10 -4 [S / cm] or more, and more preferably 2.0 × 10 -4 [S / cm] or more, and particularly preferably 2.5 × 10 -4 [S / cm] or more, and most preferably 3.0 × 10 -4 [S / cm] or more.

[0041] The constituent material of the ion-conductive reaction suppression layer is not particularly limited, and various materials capable of exhibiting the above-mentioned functions can be used. One example of a constituent material of the ion-conductive reaction suppression layer is nanoparticles having lithium ion conductivity. By including nanoparticles in the ion-conductive reaction suppression layer, a lithium secondary battery with particularly excellent ion-conductive reaction suppression layer functionality can be provided. Here, "nanoparticles" refers to particles having an average particle diameter on the nanometer (nm) scale. The "average particle diameter" of nanoparticles refers to the 50% cumulative diameter (D50) of the particle diameter (the maximum distance between any two points on the outline of the observed particle) measured by observing the cross section of a layer containing the nanoparticles with a scanning electron microscope (SEM). The average particle diameter of the nanoparticles is preferably 500 nm or less, more preferably 300 nm or less, even more preferably 150 nm or less, particularly preferably 100 nm or less, and most preferably 60 nm or less. In particular, when the average particle diameter of the nanoparticles is 60 nm or less, a lithium secondary battery with particularly excellent dendrite growth suppression effect can be provided. There is no particular lower limit to the average particle size of the nanoparticles, but it is usually 10 nm or more, and preferably 20 nm or more.

[0042] From the viewpoint of particularly excellent function as an ion-conductive reaction suppression layer, such nanoparticles preferably contain one or more elements selected from the group consisting of carbon, gold, platinum, palladium, silicon, silver, aluminum, bismuth, tin, and zinc, more preferably one or more of these elements or alloys thereof, even more preferably elemental carbon or silver, and particularly preferably elemental carbon and silver. Examples of materials consisting of elemental carbon include acetylene black, Vulcan (registered trademark), Black Pearl (registered trademark), carbon nanofiber, Ketjen Black (registered trademark), carbon nanotubes, carbon nanohorns, carbon nanoballoons, and fullerene. Note that when the ion-conductive reaction suppression layer contains such nanoparticles, the layer may further contain a binder.

[0043] There are no particular limitations on the average thickness of the ion-conductive reaction suppression layer. When the ion-conductive reaction suppression layer is a layer containing first nanoparticles, the average thickness is preferably 300 nm to 20 μm, more preferably 500 nm to 15 μm, and even more preferably 1 to 10 μm. The "average thickness" of the protective layer refers to the value calculated as the arithmetic mean value of thickness measurements taken at several to several dozen different locations on the ion-conductive reaction suppression layer constituting the lithium secondary battery.

[0044] [Positive and negative electrode current collectors] The material constituting the current collectors (25, 27) is not particularly limited, and known highly conductive materials conventionally used as current collectors for secondary batteries can be used. Metal materials such as aluminum, carbon-coated aluminum, copper, titanium, nickel, stainless steel (SUS), and alloys thereof are preferred as the constituent material of the current collectors. From the viewpoints of light weight, corrosion resistance, and high conductivity, aluminum and copper are more preferred, and aluminum is particularly preferred. The negative electrode current collector 25 and the positive electrode current collector 27 may be made of the same material or different materials.

[0045] The above description has been given using the stacked structure and layer arrangement of the stacked secondary battery 10a (lithium secondary battery) according to the embodiment shown in FIG. 2 as an example. However, the lithium secondary battery according to this embodiment can have various other stacked structures and layer arrangements. For example, the embodiment shown in FIG. 5 is an example of such an embodiment. In the embodiment shown in FIG. 5, the outer peripheral edge of the solid electrolyte layer 17 covering the side surface of the positive electrode active material layer 15 is tapered relative to the side surface of the positive electrode active material layer 15. This configuration can prevent current concentration at the outer peripheral edge of the positive electrode active material layer 15 during charge and discharge, and also suppress deterioration of the active material layer and the formation of dendrites, thereby preventing a decrease in cycle durability due to these factors.

[0046] Although the above description has been given using an example in which the secondary battery according to the present embodiment is an all-solid-state lithium secondary battery, the lithium secondary battery according to the present embodiment does not have to be an all-solid-state type. That is, the solid electrolyte layer may further contain a conventionally known liquid electrolyte (electrolytic solution). There is no particular limitation on the amount of liquid electrolyte (electrolytic solution) that can be contained in the solid electrolyte layer, but it is preferable that the amount be such that the shape of the solid electrolyte layer formed by the solid electrolyte is maintained and leakage of the liquid electrolyte (electrolytic solution) does not occur. Note that the liquid electrolyte (electrolytic solution) is a solution in the form of a conventionally known lithium salt dissolved in a conventionally known organic solvent. The liquid electrolyte (electrolytic solution) may further contain additives other than the organic solvent and the lithium salt. These additives may be used alone or in combination of two or more. Furthermore, when an additive is used in the electrolyte solution, the amount used can be adjusted as appropriate.

[0047] According to another aspect of the present invention, there is also provided a cathode-solid electrolyte layer laminate, which is a component of the lithium secondary battery according to the above-described aspect of the present invention. The laminate is characterized in that a cathode current collector, a cathode active material layer, and a solid electrolyte layer are laminated in this order, the solid electrolyte layer extends to the cathode current collector so as to cover at least a portion of the side surface of the cathode active material layer, and the composite elastic modulus measured by spherical nanoindentation on the main surface of the cathode current collector facing the cathode active material layer is 17.0 GPa or less. The configuration of each component of the laminate is as described above, and therefore detailed description thereof will be omitted here.

[0048] According to yet another aspect of the present invention, a method for producing the above-described positive electrode-solid electrolyte layer laminate is also provided. This method is characterized by including bonding the positive electrode current collector and solid electrolyte layer constituting the laminate, with the positive electrode active material layer sandwiched therebetween, by roll pressing or cold isostatic pressing (CIP). Bonding methods using roll pressing or cold isostatic pressing (CIP) are known per se, and either method can produce a laminate with a good bonded state. Furthermore, from the viewpoint of excellent handleability, bonding by roll pressing is preferred. There is no particular limitation on the temperature during roll pressing, but it is usually about 10 to 250°C. There is also no limitation on the linear pressure during roll pressing, but it is usually about 0.5 to 10 ton / cm. Furthermore, from the viewpoint of further suppressing the occurrence of cracks in the solid electrolyte layer, bonding by CIP is preferred. In particular, performing bonding by CIP under high-temperature conditions such as 30°C or higher, preferably 50°C or higher, and more preferably 80°C or higher can significantly suppress the occurrence of cracks in the solid electrolyte layer. There is no upper limit to the temperature during CIP, but it is usually not higher than 100° C. There is also no limit to the pressure during CIP, but it is usually about 200 to 800 MPa, and preferably 400 to 600 MPa.

[0049] The following embodiments are also included within the scope of the present invention: the lithium secondary battery according to claim 1 having the features of claim 2; the lithium secondary battery according to claim 1 or 2 having the features of claim 3; the lithium secondary battery according to any one of claims 1 to 3 having the features of claim 4; the lithium secondary battery according to claim 4 having the features of claim 5; a positive electrode-solid electrolyte layer laminate for use in the lithium secondary battery according to any one of claims 1 to 5 having the features of claim 6; and a method for producing a positive electrode-solid electrolyte layer laminate according to claim 6 having the features of claim 7.

[0050] The present invention will be described in more detail below using experimental examples. However, the technical scope of the present invention is not limited to the following experimental examples. Note that the following operations were performed in a glove box. Furthermore, the instruments and devices used in the glove box were thoroughly dried beforehand.

[0051] [Preparation of Positive Electrode Active Material Layer] First, LiNi as a positive electrode active material 0.8 Mn 0.1 Co 0.1 O 2 acetylene black as a conductive additive, and argyrodite (Li 6 P.S. 5 The powder mixture was weighed out to a mass ratio of 60:10:30 using PTFE (Titanium Dioxide), and mixed in an agate mortar. 2 parts by mass of PTFE was added as a binder to 100 parts by mass of the resulting mixed powder, and the mixture was lightly kneaded and then kneaded for 2 minutes in the mortar while applying a shear force.

[0052] The mixture thus obtained was formed using a hand roller and stretched to a thickness of 200 μm, and then passed through a tabletop roll press to finally prepare a positive electrode active material layer (thickness 70 μm).

[0053] [Fabrication of Laminate of Positive Electrode Active Material Layer and Positive Electrode Current Collector] A carbon-coated aluminum foil was prepared as a positive electrode current collector. The composite elastic modulus of the main surface of this positive electrode current collector (carbon-coated aluminum foil) was measured by the following method and found to be 0.65 [GPa].

[0054] (Method for measuring the composite elastic modulus of the positive electrode current collector) The composite elastic modulus was measured in an environment of 25 ° C. by a spherical nanoindentation method using a nanoindenter "TI980" manufactured by Hysitron Corporation as a measuring device. In addition, a spherical diamond indenter with an indenter tip radius of 10 μm was used as the measuring indenter. The measurement conditions were as follows: Measurement mode: Load-unload test Maximum indentation depth: 4000 nm Holding time when the maximum load was reached: 0 seconds Loading rate and unloading rate: 800 nm / sec In the measurement, the positive electrode current collector to be measured for the composite elastic modulus was fixed to a glass substrate with an adhesive, and then fixed to a sample stage with a vacuum chuck. Then, the relationship between the indentation depth and the indentation load was measured under the above-mentioned measurement conditions, and the relationship between the indentation strain and the average contact pressure was determined from the obtained measured values ​​(stress-strain curve). From the slope of the stress-strain curve thus obtained, the composite elastic modulus E during indentation was calculated based on Hertz's contact solution. r The Hertz contact solution is expressed by the following formula: Measurements were carried out at six different locations on each sample, and the arithmetic mean value was taken as the measured value.

[0055] Hertz's contact solution P = 4 / 3E r R 1/2 h 3/2 In the formula, P is the indentation load [mN], and E r is the composite elastic modulus [GPa], R is the indenter tip radius [μm], and h is the indentation depth [nm].

[0056] Next, the positive electrode active material layer prepared above was punched out to a size of 20 mm × 20 mm (corner R = 1 mm). Meanwhile, the positive electrode current collector prepared above was punched out to a size of 25 mm × 25 mm (corner R = 1 mm). The punched positive electrode active material layer was then placed in the center of the punched positive electrode current collector, and pressed using a roll press under a 25°C environment with a linear pressure of 1 ton / cm to prepare a laminate of the positive electrode active material layer and the positive electrode current collector.

[0057] [Preparation of a Laminate of Solid Electrolyte Layer / Positive Electrode Active Material Layer / Positive Electrode Current Collector] Styrene-butadiene rubber (SBR) as a binder was dissolved in mesitylene as a solvent to prepare a binder solution with a concentration of 5% by mass. On the other hand, argyrodite (Li) having an average particle size of 3 μm was used as a sulfide solid electrolyte. 6 P.S. 5 A solid electrolyte solution was prepared by dissolving HCl in mesitylene as a solvent, and these solutions were mixed to prepare a solid electrolyte slurry (solid content concentration: 47 mass %, solid electrolyte:binder=95:5 (mass ratio)).

[0058] Next, the solid electrolyte slurry prepared above was applied to the surface of a support made of stainless steel (SUS430) foil in an amount of 7.4 mg / cm 2 The solution was applied using an applicator so as to have a basis weight of 1000 mg / m². Thereafter, the solvent (mesitylene) was removed by drying on a hot plate at 80° C. for 10 minutes, thereby producing a solid electrolyte layer sheet.

[0059] The solid electrolyte layer sheet prepared above was punched out to a size of 25 mm × 25 mm (corner R = 1 mm). Next, the punched solid electrolyte layer sheet was placed at the center of the surface of the positive electrode active material layer side of the laminate of the positive electrode active material layer and the positive electrode current collector prepared above, and the support (stainless steel foil) of the sheet was peeled off.

[0060] The laminate thus obtained was placed in a 35 mm × 35 mm aluminum laminate pack and sealed using a vacuum sealer. The pack was then subjected to cold isostatic pressing (CIP) at 80°C and 500 MPa for 1 minute to produce a solid electrolyte layer / positive electrode active material layer / positive electrode current collector laminate. The thickness of the solid electrolyte layer in the laminate was 20 μm.

[0061] The pack was opened and the laminate was taken out, and the bonding state between the solid electrolyte layer and the positive electrode current collector was visually inspected, and it was found that the bonding state was good.

[0062] [Experimental Examples Using Various Positive Electrode Current Collectors] Using commercially available positive electrode current collectors made of the following materials and having the following composite elastic moduli (all units are [GPa]), laminates of solid electrolyte layer / positive electrode active material layer / positive electrode current collector were prepared by the same method as above, and the bonding state between the solid electrolyte layer and the positive electrode current collector was observed. As a result, for those in which a good bonding state was confirmed, the value of the composite elastic modulus is underlined (the results of the above experimental examples are also shown).

[0063] Carbon coated aluminum foil (composite modulus: 0.65) Etched aluminum foil (1) (composite modulus: 9.07, 30CB, manufactured by Nippon Capacitor Industrial Co., Ltd.) Etched aluminum foil (2) (composite modulus: 9.39, 20CB, manufactured by Nippon Capacitor Industrial Co., Ltd.) Etched aluminum foil (3) (composite modulus: 10.14, 20CB054, manufactured by Nippon Capacitor Industrial Co., Ltd.) Aluminum foil (composite modulus: 25.35) Copper foil (composite modulus: 53.35) Stainless steel (SUS430) foil (composite modulus: 59.25) Nickel foil (composite modulus: 89.42).

[0064] As described above, in the laminates using carbon-coated aluminum foil and etched aluminum foil with a composite elastic modulus of 17.0 GPa or less, the bonding state between the solid electrolyte layer and the positive electrode current collector was good. In contrast, in the laminates using aluminum foil, copper foil, stainless steel foil, and nickel foil with a composite elastic modulus of more than 17.0 GPa, the bonding state between the solid electrolyte layer and the positive electrode current collector was poor, and it was confirmed that peeling occurred between them, causing the solid electrolyte layer to become self-supporting.

[0065] As described above, by configuring a lithium secondary battery according to one embodiment of the present invention, in a lithium secondary battery including a solid electrolyte layer covering the outside of a positive electrode active material layer and extending to the positive electrode current collector, peeling between the solid electrolyte layer and the positive electrode current collector is suppressed, which can contribute to improving the cycle durability and the like of the battery.

[0066] 10a, 100 Stacked secondary battery, 11' Negative electrode current collector, 11" Positive electrode current collector, 13 Negative electrode active material layer, 15 Positive electrode active material layer, 17 Solid electrolyte layer, 18 Carbon black layer (ion-conductive reaction suppression layer), 19 Single cell layer, 21 Power generating element, 25 Negative electrode current collector, 27 Positive electrode current collector, 29 Laminate film, 200 Metal plate, 300 Volt, 400 Nut.

Claims

1. A lithium secondary battery comprising: a power generating element having a positive electrode in which a positive electrode active material layer is disposed on a surface of a positive electrode current collector; a negative electrode; and a solid electrolyte layer interposed between the positive electrode and the negative electrode and containing a solid electrolyte, wherein the solid electrolyte layer extends to the positive electrode current collector so as to cover at least a portion of a side surface of the positive electrode active material layer, and the value of the composite elastic modulus measured by spherical nanoindentation method for the main surface of the positive electrode current collector facing the positive electrode active material layer is 17.0 GPa or less.

2. The lithium secondary battery according to claim 1, wherein an outer peripheral edge of the solid electrolyte layer covering the side surface of the positive electrode active material layer is arranged in a tapered shape with respect to the side surface of the positive electrode active material layer.

3. The lithium secondary battery according to claim 1 or 2, wherein the composite elastic modulus is 0.5 to 17.0 GPa.

4. The lithium secondary battery according to claim 1 or 2, wherein the main surface of the positive electrode current collector facing the positive electrode active material layer is made of an inorganic material.

5. The lithium secondary battery according to claim 4, wherein the material constituting the positive electrode current collector is an etched aluminum foil, a carbon-coated aluminum foil, a roughened aluminum foil, or a carbon foil.

6. A positive electrode-solid electrolyte layer laminate for use in the lithium secondary battery according to claim 1 or 2, comprising the positive electrode current collector, the positive electrode active material layer, and the solid electrolyte layer laminated in this order, the solid electrolyte layer extending to the positive electrode current collector so as to cover at least a portion of a side surface of the positive electrode active material layer, and the composite elastic modulus measured by spherical nanoindentation method for the main surface of the positive electrode current collector facing the positive electrode active material layer is 17.0 GPa or less.

7. A method for producing a positive electrode-solid electrolyte layer laminate according to claim 6, comprising bonding the positive electrode current collector and the solid electrolyte layer together with the positive electrode active material layer sandwiched therebetween by roll pressing or cold isostatic pressing (CIP).

Citation Information

Patent Citations

  • Electrolytic aluminum foil, collector for accumulation device, electrode for accumulation device and accumulation device

    JP2015155564A

  • Method for manufacturing all solid secondary battery