Nonaqueous electrolyte secondary battery

The non-aqueous electrolyte secondary battery design addresses the issue of surface pressure-induced performance deterioration by using a wound-type electrode group with an overlapped film piece and separator core, enhancing durability and cycle life.

WO2024214483A1PCT designated stage expired Publication Date: 2024-10-17PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010297
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-10
Filing Date
2024-03-15
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

The existing cylindrical lithium ion batteries face performance deterioration due to increased surface pressure during charging and discharging, which damages the electrode group and reduces battery performance when the separator tip is fixed to a hollow cylindrical member.

Method used

A non-aqueous electrolyte secondary battery design featuring a wound-type electrode group with a core portion that includes a film piece and a winding start region of the separator, where the film piece and the winding start region are overlapped and wound, and the innermost peripheral portion is closed by a bent portion, relieving surface pressure and preventing damage.

Benefits of technology

This design effectively suppresses the deterioration of battery performance by distributing stress evenly and preventing uneven deformation of the core, leading to increased cycle life and improved durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010297_17102024_PF_FP_ABST
    Figure JP2024010297_17102024_PF_FP_ABST
Patent Text Reader

Abstract

This nonaqueous electrolyte secondary battery comprises: a wound electrode group that has a positive electrode, a negative electrode, and a separator that is disposed between the positive electrode and the negative electrode; and a nonaqueous electrolyte. The electrode group has a core part for winding, the core part including a film piece and a winding starting region of the separator. The film piece and the winding starting region are wound while being stacked upon each other.
Need to check novelty before this filing date? Find Prior Art

Description

Nonaqueous electrolyte secondary battery CROSS-REFERENCE TO RELATED APPLICATIONS

[0001] This disclosure claims the benefit of priority to Japanese Patent Application No. 2023-063619, filed on April 10, 2023, in the Japan Patent Office, the entire contents of which are incorporated herein by reference.

[0002] The present disclosure relates to a non-aqueous electrolyte secondary battery.

[0003] Patent Document 1 proposes "a cylindrical lithium ion battery in which a positive electrode plate and a negative electrode plate are wound around an axis with a separator interposed therebetween to form a wound group, and the wound group is housed in a cylindrical battery container, wherein the wound group uses two pairs of separators, each of which is stacked between the positive electrode plate and the negative electrode plate, and the respective tip portions of the separators are integrated by welding, and each of the integrated tip portions is joined at a different position on the axis."

[0004] Japanese Patent Application Laid-Open No. 2001-229970

[0005] In Patent Document 1, a hollow cylindrical member is used as the “axial core.” However, if the leading end portion of the separator (i.e., the leading end of the winding start region) is fixed to the hollow cylindrical member, the surface pressure of the entire electrode group increases significantly during charge and discharge, which may damage the electrode group and reduce battery performance.

[0006] One aspect of the present disclosure relates to a non-aqueous electrolyte secondary battery including: a wound electrode group having a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode; and a non-aqueous electrolyte, wherein the electrode group has a core portion for winding, the core portion including a film piece and a winding start end region of the separator, the film piece and the winding start end region being overlapped and wound, and the innermost periphery of the core portion being closed by a bent portion formed when the overlapped film piece and the winding start end region are folded in half.

[0007] According to the present disclosure, it is possible to suppress the deterioration of performance of a non-aqueous electrolyte secondary battery. The novel features of the present invention are set forth in the appended claims, but the present invention, both in terms of structure and content, together with other objects and features of the present invention, will be better understood from the following detailed description taken in conjunction with the drawings.

[0008] 1 is a schematic diagram showing an example of the positional relationship between a winding core and wound film pieces, separators, and electrodes; FIG. 2 is a schematic cross-sectional view perpendicular to the axial direction of an example of a core part of an electrode group; FIG. 3 is a schematic cross-sectional view perpendicular to the axial direction of an example of an electrode group; and FIG. 4 is a longitudinal cross-sectional view schematically showing an example of a non-aqueous electrolyte secondary battery according to an embodiment of the present disclosure.

[0009] The following describes embodiments of the present disclosure using examples, but the present disclosure is not limited to the examples described below. In the following description, specific numerical values ​​and materials may be exemplified, but other numerical values ​​and materials may be applied as long as the effects of the present disclosure are obtained. In this specification, the term "numerical value A to numerical value B" includes numerical value A and numerical value B and can be read as "numerical value A or more and numerical value B or less." In the following description, when lower and upper limits are exemplified for numerical values ​​of specific physical properties or conditions, any of the exemplified lower limits and any of the exemplified upper limits can be arbitrarily combined, as long as the lower limit is not equal to or greater than the upper limit. When multiple materials are exemplified, one of the materials may be selected and used alone, or two or more of the materials may be used in combination.

[0010] The present disclosure relates to a non-aqueous electrolyte secondary battery, and the subject matter of the present disclosure generally encompasses batteries containing a non-aqueous electrolyte. The non-aqueous electrolyte may have, for example, lithium ion conductivity. The non-aqueous electrolyte secondary battery may be a lithium ion secondary battery, a lithium metal secondary battery, a solid electrolyte secondary battery, an all-solid-state battery, or the like.

[0011] Lithium metal secondary batteries are also simply called "lithium secondary batteries." In the negative electrode of a lithium secondary battery, lithium metal is deposited during charging and dissolves during discharging. Specifically, the negative electrode has at least a negative electrode current collector, and lithium metal is deposited on the negative electrode current collector.

[0012] A nonaqueous electrolyte secondary battery (hereinafter, "secondary battery (A)") according to an embodiment of the present disclosure includes a wound electrode group having a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode, and a nonaqueous electrolyte. The electrode group has, for example, a cylindrical outer shape, and the cross-sectional outer shape of the electrode group may be, for example, circular or elliptical.

[0013] The electrode group has a core for winding. The core includes the film piece and the winding start region of the separator, and the film piece and the winding start region are overlapped and wound. Hereinafter, such a core will also be referred to as "core (B)."

[0014] Since the core (B) is a roll of film pieces and a separator, it is flexible and can shrink and deform. Therefore, when the surface pressure of the entire electrode group increases significantly during charge and discharge, the core (B) acts to relieve the surface pressure. In other words, damage to the electrode group or a decrease in battery performance is suppressed.

[0015] The "surface pressure" refers to the pressure exerted in the radial direction of the electrode group by the core (B) pressing against the inner peripheral surface of the electrode group, and is also referred to as the "internal pressure" of the electrode group. The outer peripheral surface of the electrode group is usually pressed by a battery can or the like that houses the electrode group.

[0016] Even if a core corresponding to the core (B) is formed by winding only the film piece or only the winding start region of the separator, the electrode group may be damaged by the localized pressure from the winding start end of the electrode, resulting in a decrease in battery performance. It is believed that a core formed by winding only the film piece or only the separator is prone to uneven deformation when the surface pressure or internal pressure is relieved. Uneven deformation of the core can cause damage due to deformation of the electrode group. On the other hand, a core (B) formed by winding a film piece and a separator together tends to shrink while distributing stress throughout the core, and is less likely to deform unevenly.

[0017] It is preferable that the film piece is not interposed between the positive electrode and the negative electrode. However, the winding end of the film piece may be disposed on the outer circumferential side of the winding start end of the positive electrode or the negative electrode. In this case, the length of the film piece disposed on the outer circumferential side of the winding start end of the positive electrode or the negative electrode is preferably 40% or less, more preferably 10% or less, of the total length of the electrode.

[0018] The core (B) may be formed, for example, by winding the film piece and the separator multiple times around a bent portion or crease formed when the film piece and the separator are overlapped and folded in half. When the overlapped film piece and the separator are folded in half, the film piece may be folded so that it is wrapped around the separator's winding start region (i.e., with the film piece on the inside and the separator on the outside), or the separator's winding start region may be folded so that it is wrapped around the film piece (i.e., with the separator on the inside and the film piece on the outside).

[0019] As a result of folding in half, the winding start region of the film piece and the separator are simultaneously bent, forming a bent portion or crease at the very start of the closed winding, and two layers of separator are led out from the core portion (B). The winding start ends of the positive electrode and the negative electrode are respectively wrapped around the two layers of separator, and then the winding of the separator and the positive electrode and the negative electrode continues to form an electrode group.

[0020] The innermost periphery of the core (B) is closed by the overlapping film pieces and the bent portion formed when the winding start region is folded in half. In other words, the innermost periphery is formed by a bent portion and does not have a longitudinal end portion formed by the cross section of a film piece or separator. When the innermost periphery of the core (B) is formed by a bent portion, the resistance to shrinkage or deformation of the innermost periphery is very small. If the innermost periphery had a longitudinal end portion formed by the cross section of a separator or film piece, the edge of such an end portion could engage with a more outer component. This makes it difficult for the core (B) to shrink and deform smoothly with low resistance.

[0021] In the core (B), two layers of film pieces may be stacked and wound together with the separator winding start region one to ten times. This allows the core (B) to maintain higher strength and ensure high elasticity and flexibility. The number of layers of film pieces in the core (B) is the maximum number of layers in the core (B).

[0022] The greater the number of windings between the film piece and the winding start region of the separator, the greater the maximum diameter of the core (B). The maximum diameter of the core (B) may be, for example, 0.5 mm to 6 mm, 1.5 mm to 6 mm, or 2 mm to 5 mm. The core (B) may be selected depending on the diameter of the electrode group.

[0023] The maximum diameter of the core (B) is determined from an X-ray CT image of the cross section (cross section perpendicular to the winding axis of the electrode group) of the secondary battery (A) during discharge in the early stage of discharge. The maximum diameter of the innermost periphery of the negative electrode that can be observed in the CT image, i.e., the maximum diameter of the outline of the cross section of the core (B), is determined. The end of the core (B) may or may not coincide with the end of the outermost winding of the film piece.

[0024] The maximum diameter of the core is measured for the secondary battery (A) during discharge at the beginning of charge and discharge. "During discharge" refers to when the depth of discharge (DOD) is 90% or more. A depth of discharge (DOD) of 90% or more indicates a state in which 90% or more of the rated capacity of the battery has been discharged. "Initial charge and discharge" includes batteries after the first charge and discharge, batteries immediately after purchase, and batteries that have undergone one to several charge and discharge cycles after purchase.

[0025] Hereinafter, embodiments of the battery according to the present disclosure will be further described with reference to the drawings. In each drawing, the shape or features of each component do not necessarily reflect the actual dimensions, and are not necessarily depicted at the same scale. The same reference numerals are used for the same components in each drawing.

[0026] The winding is performed, for example, using a pair of rod-shaped bodies as a winding core. FIG. 1 shows an example of the positional relationship between the winding core and the film piece, separator, and electrodes to be wound. The cross section perpendicular to the longitudinal direction of each rod-shaped body 9a, 9b has a shape defined by an arc and a chord, typically a semicircle. First, the stacked film piece 30 and separator 13 are wound around the circumferential surface of the first rod-shaped body 9a. Then, the stacked film piece 30 and separator 13 are sandwiched between the plane corresponding to the chord of the first rod-shaped body 9a around which the film piece 30 and separator 13 are wound and the plane corresponding to the chord of another (second) rod-shaped body 9b, and the stacked film piece 30 and separator 13 are wound together between the pair of rod-shaped bodies 9a, 9b. After multiple windings, the entire film piece 30 is used to form the core (B). Two layers of separator are derived from the core (B). The two layers of separator are then wound around the winding start ends of the negative electrode 12 and the positive electrode 11 in turn. The winding of the separator, positive electrode, and negative electrode continues. When the winding is completed, the winding core is pulled out.

[0027] Although not limited thereto, when wound in the above manner, the electrode group may have a first space inside the innermost periphery of the core (B). FIG. 2 is a schematic cross-sectional view perpendicular to the axial direction of an example of the core (B) 14c of the electrode group 14. FIG. 3 is a schematic cross-sectional view perpendicular to the axial direction of an example of the electrode group 14. The first space R1 originates from the space occupied by the first rod-shaped body 9a and is formed when the first rod-shaped body 9a is pulled out. A second space R2 may be adjacent to the first space R1 via a portion of the film piece 30 and the winding start end region of the separator 13. The second space R2 originates from the space occupied by the second rod-shaped body 9b and is formed when the second rod-shaped body 9b is pulled out. The first space R1 can also be said to be a space surrounded by the closed winding start end.

[0028] One of the first space R1 and the second space R2 is surrounded by the film piece 30, and the other of the first space R1 and the second space R2 is surrounded by the winding start end region of the separator 13. When the overlapping film piece 30 and separator 13 are folded in half, if the film piece 30 is folded so that it is wrapped around the separator 13, a first space R1 surrounded by the film piece 30 and a second space R2 surrounded by the winding start end region of the separator 13 are formed. Conversely, if the separator 13 is folded so that it is wrapped around the film piece 30, a first space R1 surrounded by the winding start end region of the separator 13 and a second space R2 surrounded by the film piece 30 are formed.

[0029] The shape of the core (B) may be selected depending on the shape of the electrode group. When the cross-sectional shape of the electrode group is circular, the cross-sectional shape of the core (B) may also be circular. When the cross-sectional shape of the electrode group is elliptical, the cross-sectional shape of the core (B) may also be elliptical.

[0030] The material of the film piece is not particularly limited, but resin film, metal foil, etc. can be used. Among them, resin film is preferred because of its excellent flexibility.

[0031] The resin film is a film whose main component is a resin or an organic material, and 51% by mass or more of the resin film is composed of a resin or an organic material. The resin film may be formed, for example, of an insulating resin and may contain a filler dispersed in the insulating resin. Examples of the filler that can be used include inorganic particles, inorganic fillers, organic particles, and organic fillers. The resin film may be a stretched film, a non-porous film (a film without holes), or a film having a plurality of regularly arranged holes.

[0032] The resin material constituting the resin film is not particularly limited, but examples thereof include polyester resin, olefin resin, polyphenylene sulfide resin, acrylic resin, polycarbonate resin, polyether ether ketone resin, polyether sulfone resin, polyamide resin, polyimide resin, nylon resin, polyvinylidene chloride resin, polyvinylidene fluoride resin, ethylene-vinyl alcohol copolymer, polyvinyl alcohol resin, polystyrene resin, urethane resin, epoxy resin, etc. One type of resin may be used alone, or two or more types may be used in combination.

[0033] The polyester resin is preferably an aromatic polyester, and more preferably polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, etc. The film containing polyethylene terephthalate, etc. may be a non-stretched film or a biaxially stretched film.

[0034] Examples of the acrylic resin include polymethyl methacrylate.

[0035] The polyimide resin is preferably an aromatic polyimide.

[0036] The polyamide resin is preferably an aromatic polyamide (aramid resin).

[0037] Preferred olefin resins include polypropylene and polyethylene. Polypropylene includes unstretched polypropylene and biaxially oriented polypropylene. Polyethylene includes low-density polyethylene, medium-density polyethylene, high-density polyethylene, linear low-density polyethylene, and metallocene polyethylene. Furthermore, the olefin resin may be an ethylene-vinyl acetate copolymer, an ethylene-methyl acrylate copolymer, an ethylene-ethyl acrylate copolymer, an ethylene-methyl methacrylate copolymer, an ethylene-acrylic acid copolymer, an ethylene-methacrylic acid copolymer, an ionomer resin (e.g., an ethylene-acrylic acid copolymer, an ethylene-methacrylic acid copolymer), or the like.

[0038] Examples of methods for producing resin films include extrusion molding, such as the T-die method and inflation method. The stretched film may be a uniaxially stretched film or a sequentially (or simultaneously) biaxially stretched film. The resin film may be constructed by laminating two or more types of resin films. The resin may be in a crystalline state, an amorphous state obtained by a rapid cooling method, or a mixture of both. The surface of the resin film may be corona-treated or plasma-treated.

[0039] The metal material constituting the metal foil is not particularly limited and may contain one type of metal or an alloy containing two or more types of metals. Examples of metal materials include aluminum, magnesium, titanium, copper, iron, stainless steel, carbon steel, nickel, duralumin, cupronickel, bronze, brass, etc. Among these, stainless steel is preferred from the viewpoint of strength and durability, and austenitic stainless steel, which is less susceptible to embrittlement, is particularly preferred.

[0040] Considering the balance of strength, elasticity, flexibility, etc., the thickness of the resin film is preferably 0.005 mm or more and 0.1 mm or less, more preferably 0.01 mm or more and 0.06 mm or less, and may be 0.02 mm or more and 0.05 mm or less.

[0041] The thickness of the metal foil is not particularly limited, but considering the balance of strength, elasticity, flexibility, etc., it is more preferably 0.01 mm or more and 0.2 mm or less, and may be 0.05 mm or more and 0.15 mm or less.

[0042] The tensile strength of the film piece in the MD direction is, for example, 10 MPa or more and 400 MPa or less, preferably 100 MPa or more and 300 MPa or less, and may be 140 MPa or more and 250 MPa or less.

[0043] The elongation of the film piece is, for example, 3%, preferably 5% or more, or may be 30% or more, or may be 70% or more. Considering the balance between elasticity and flexibility, the elongation is preferably 500% or less, or may be 300% or less.

[0044] The tensile strength and elongation of the film piece are determined in accordance with JIS K 7161 (2014) in the case of a resin film, and in accordance with JIS Z 2241 (2022) in the case of a metal foil.

[0045] The secondary battery (A) may include an outer can that houses an electrode group and a nonaqueous electrolyte. The outer can is a metal case also called a battery can. The material of the outer can is required to have excellent strength and durability. The material of the outer can is not particularly limited, but may be metal, and among them, nickel-plated steel or stainless steel is desirable in terms of strength and durability. The shape of the outer can is, for example, a bottomed tubular shape (cylindrical, flat tubular, rectangular tubular, etc.). A sealing body is placed at the opening of the outer can to seal the battery.

[0046] The inner peripheral surface of the outer can faces the outer peripheral surface of the electrode assembly. The presence of the outer can further stabilizes the shape of the electrode assembly, and buckling of the electrodes (particularly on the outer peripheral side of the electrode assembly) is likely to be suppressed. The inner diameter of the outer can may be such that the outer peripheral surface of the electrode assembly of a lithium secondary battery in a discharged state after the initial charge / discharge comes into contact with the inner peripheral surface of the outer can.

[0047] The core (B) is particularly effective in lithium (metal) secondary batteries, which are secondary batteries (A) that experience extremely high surface pressure during charging. In the negative electrode of a lithium secondary battery, lithium metal precipitates during charging and dissolves during discharging. This results in a large change in the volume of the negative electrode, and a large change in the surface pressure inside the electrode group.

[0048] In a lithium secondary battery, for example, 70% or more of the rated capacity is realized by the deposition and dissolution of lithium metal. The movement of electrons at the negative electrode during charging and discharging is mainly due to the deposition and dissolution of lithium metal at the negative electrode. Specifically, 70 to 100% (e.g., 80 to 100% or 90 to 100%) of the movement of electrons (or current from another perspective) at the negative electrode during charging and discharging is due to the deposition and dissolution of lithium metal.

[0049] In a battery in which lithium metal is deposited on the negative electrode during charging, the open circuit potential (OCP) of the negative electrode at full charge (e.g., SOC 98% or higher) may be, for example, 70 mV or less relative to lithium metal (lithium dissolution and deposition potential). The open circuit potential (OCP) of the negative electrode at full charge may be measured by disassembling a fully charged battery under an argon atmosphere, removing the negative electrode, and assembling a cell using lithium metal as a counter electrode. The nonaqueous electrolyte of the cell may have the same composition as the nonaqueous electrolyte in the disassembled battery.

[0050] Hereinafter, the present disclosure will be further described in detail using a lithium (metal) secondary battery as an example.

[0051] [Negative Electrode] The negative electrode of a lithium secondary battery includes at least a negative electrode current collector that supports lithium metal that precipitates during charging. The thickness of the negative electrode current collector is not particularly limited and is, for example, 5 μm or more and 300 μm or less. The negative electrode current collector may include a metal foil, a resin sheet, or the like.

[0052] The metal material constituting the metal foil may be, for example, Cu, Ni, Fe, or an alloy containing these metal elements. Examples of the alloy include Cu alloys and Fe alloys (stainless steel, etc.). The metal foil may be stainless steel foil, copper foil (particularly oxygen-free copper foil), copper alloy foil, etc. Oxygen-free copper foil is copper foil with a low oxygen content.

[0053] The stainless steel foil is preferably an austenitic stainless steel foil. Austenitic stainless steel foil is resistant to embrittlement, has appropriate strength and flexibility, and is excellent in resistance to stress generated in the negative electrode. The austenitic stainless steel is stainless steel having an austenite ratio of 50% or more. The austenite ratio may be 70% or more, 90% or more, or even 100%.

[0054] The austenite fraction refers to the proportion (mass ratio) of austenite phase in stainless steel. When the contents of austenite phase, ferrite phase, and martensite phase in stainless steel are x, y, and z, respectively, the austenite fraction is calculated by {x / (x+y+z)}×100. The austenite structure has a face-centered cubic lattice structure (FCC structure), while the ferrite structure and martensite structure have a body-centered cubic lattice structure (BCC structure).

[0055] Oxygen-free copper foil refers to copper foil with an oxygen content of, for example, 50 ppm or less. Oxygen-free copper foil is less likely to become embrittled due to its low oxygen content. The oxygen content of oxygen-free copper foil may be 30 ppm or less, or may be 15 ppm or less. The oxygen content refers to the oxygen content in the base material excluding the oxide film covering the surface of the copper foil.

[0056] The oxygen-free copper foil may contain trace amounts of components other than copper (e.g., Ni, Cr, Fe, Zn, Sn, Ag, Pb, Bi, Cd, Hg, O, P, S, Se, Te, H, etc.). The Cu content in the copper foil may be 99.9 mass% or more, or 99.96 mass% or more. The copper foil may be a rolled copper foil. An example of oxygen-free copper is copper of alloy number C1020 in JIS H 3100.

[0057] The oxygen content in copper foil is measured by washing a copper foil sample with nitric acid (1+1) for 10 seconds to remove the oxide film on the sample surface. The above washing is repeated until the sample is reduced by 10% by mass or more. Next, the sample is washed with distilled water, alcohol, and acetone, in that order. The sample is then dried with hot air and immediately analyzed by inert gas fusion-infrared absorption method to determine the oxygen content in the sample. An oxygen and nitrogen simultaneous analyzer (LECO, TC-336) can be used as the analyzer.

[0058] The negative electrode current collector including a resin sheet may have a metal underlayer covering the surface of the resin sheet. The metal underlayer may cover, for example, 90% or more of the surface of the resin sheet.

[0059] The metal base layer preferably contains, for example, copper, nickel, chromium, stainless steel, titanium, silver, gold, tin, etc. In this case, the metal base layer is likely to ensure corrosion resistance, conductivity, etc., and is unlikely to alloy with lithium.

[0060] The resin sheet is a sheet whose main component is a resin or an organic material, and 51% by mass or more of the resin sheet is composed of a resin or an organic material. The resin sheet may be formed of, for example, an insulating resin and may contain a filler dispersed in the insulating resin. Examples of the filler that can be used include inorganic particles, inorganic fillers, organic particles, and organic fillers. The resin sheet may be a stretched sheet, a non-porous sheet (a sheet without holes), or a sheet having a plurality of regularly arranged holes.

[0061] The resin contained in the resin sheet is not particularly limited, and for example, the resin that can be used for the resin film described above may be used. For the purpose of improving adhesion, the surface of the resin sheet may be subjected to corona treatment or plasma treatment.

[0062] The resin sheet may contain a nitrogen-containing resin at least in its surface layer portion. 90% by mass or more of the surface layer portion may be the nitrogen-containing resin. The nitrogen-containing resin may contain nitrogen atoms in an amount of 3% by mass or more. Therefore, the nitrogen atom content of the surface layer portion may be 2.5% by mass or more.

[0063] When the base metal layer contains a transition metal, the transition metal has the effect of embrittling the resin sheet. In particular, when the transition metal layer contains copper, embrittlement of the resin sheet is likely to occur. It has also been found that lithium metal deposited on the negative electrode current collector significantly accelerates embrittlement of the resin sheet due to transition metals (e.g., copper damage). That is, in lithium secondary batteries, deterioration of the resin sheet due to the transition metal layer can occur significantly. In contrast, by incorporating a nitrogen-containing resin into at least the surface layer of the resin sheet, embrittlement of the resin sheet is significantly suppressed.

[0064] The nitrogen-containing resin may be a polymer having nitrogen atoms in the main chain or side chain. The nitrogen-containing resin may contain at least a nitrogen-hydrogen bond (N—H bond). The presence or absence of a nitrogen-hydrogen bond can be determined by infrared absorption spectroscopy. The infrared absorption peak specific to a nitrogen-hydrogen bond is at 1655 cm -1 Nearby (1640-1670 cm -1 ), 1530cm -1 Nearby (1515-1545 cm -1 ) etc.

[0065] The nitrogen-containing resin may be a polymer having at least one selected from the group consisting of a urea bond, a melamine structure, a triazine ring, an amino group, an amide bond, an aramid bond, an imide bond, a urethane bond, a carbodiimide bond, a uretdione structure, an isocyanurate ring, a nitrile group, and an amide group. Such a polymer may be, for example, a polyurethane resin, a polyurea resin, a melamine resin, a polyamide resin, an aramid resin, or a polyimide resin. Among these, polyurethane resins are excellent as current collector materials because of their high flexibility, high resistance to stresses caused by the expansion and contraction of electrodes, and resistance to breakage.

[0066] A lithium metal layer or a lithium alloy layer (hereinafter also referred to as a lithium underlayer) may be formed in advance on the surface of the negative electrode current collector.

[0067] The lithium alloy may contain elements other than lithium, such as aluminum, magnesium, indium, and zinc. By depositing lithium metal on a pre-formed lithium underlayer during charging, dendritic deposition can be more effectively suppressed. The thickness of the lithium underlayer is not particularly limited, but may be, for example, in the range of 5 μm to 25 μm.

[0068] The negative electrode may include a lithium ion occlusion layer (a layer that develops capacity by occlusion and release of lithium ions by a negative electrode active material (such as graphite)) supported on a negative electrode current collector. In this case, the open circuit potential of the negative electrode when fully charged may be 70 mV or less relative to lithium metal (dissolution and deposition potential of lithium). If the open circuit potential of the negative electrode when fully charged is 70 mV or less relative to lithium metal, lithium metal is present on the surface of the lithium ion occlusion layer when fully charged. In other words, the negative electrode develops capacity by deposition and dissolution of lithium metal.

[0069] The lithium ion storage layer is a layer of a negative electrode mixture containing a negative electrode active material. The negative electrode mixture may contain a binder, a thickener, a conductive agent, etc. in addition to the negative electrode active material.

[0070] Examples of the negative electrode active material include a carbonaceous material, a Si-containing material, and a Sn-containing material. The negative electrode may contain one or more negative electrode active materials. Examples of the carbonaceous material include graphite, easily graphitizable carbon (soft carbon), and hardly graphitizable carbon (hard carbon).

[0071] The conductive material is, for example, a carbon material, such as carbon black, acetylene black, ketjen black, carbon nanotubes, and graphite.

[0072] Examples of the binder include fluororesin, polyacrylonitrile, polyimide resin, acrylic resin, polyolefin resin, rubber polymer, etc. Examples of the fluororesin include polytetrafluoroethylene, polyvinylidene fluoride, etc.

[0073] [Positive Electrode] The positive electrode includes, for example, a positive electrode current collector and a positive electrode composite layer supported on the positive electrode current collector. The positive electrode composite layer includes, for example, a positive electrode active material, a conductive material, and a binder. The positive electrode composite layer may be formed on only one side of the positive electrode current collector, or may be formed on both sides. The positive electrode is obtained, for example, by applying a positive electrode composite slurry including a positive electrode active material, a conductive material, and a binder to both sides of the positive electrode current collector, drying the coating, and then rolling. For example, known materials may be used as the positive electrode active material, the binder, the conductive material, and the like.

[0074] The positive electrode active material is a material that absorbs and releases lithium ions. Examples of the positive electrode active material include lithium-containing transition metal oxides, transition metal fluorides, polyanions, fluorinated polyanions, and transition metal sulfides. Among these, lithium-containing transition metal oxides are preferred because of their low production cost and high average discharge voltage.

[0075] The lithium-containing transition metal oxide is a composite oxide containing lithium and a metal other than lithium, Me, where the metal Me contains at least a transition metal. Among the lithium-containing transition metal oxides, composite oxides having a rock salt type crystal structure with a layered structure (layered rock salt type) are preferred in terms of obtaining a high capacity.

[0076] The metal Me may contain Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Y, Zr, W, or the like as a transition metal element. The lithium-containing transition metal oxide may contain one or more transition metal elements. The metal Me preferably contains at least one transition metal element selected from the group consisting of Co, Ni, and Mn, and preferably contains at least Ni as the transition metal. The crystalline form may be single crystal, polycrystal, or both.

[0077] The lithium-containing transition metal oxide may contain one or more typical elements as needed. Examples of typical elements include Mg, Al, Ca, Zn, Ga, Ge, Sn, Sb, Pb, and Bi. The typical element may be Al. That is, the metal Me may contain Al as an optional component.

[0078] The lithium-containing transition metal oxide is, for example, a lithium-containing transition metal oxide represented by the general formula (1): Li a Ni b M 1-b O 2 In general formula (1), 0.9≦a≦1.2 and 0.65≦b≦1 are satisfied, and M is at least one element selected from the group consisting of Co, Mn, Al, Ti, Fe, Nb, B, Mg, Ca, Sr, Zr, and W.

[0079] The molar ratio mLi / mMe of the total amount mLi of Li contained in the positive electrode and negative electrode to the amount mMe of metal Me contained in the lithium-containing transition metal oxide is, for example, 1.2 or less, and may be 1.1 or less.

[0080] For the positive electrode current collector, for example, a foil-shaped or sheet-shaped metal material containing Al, Ti, Fe, etc. can be used. The metal material may be Al, an Al alloy, Ti, a Ti alloy, or an Fe alloy (stainless steel (SUS), etc.). From the viewpoint of suppressing breakage of the positive electrode during charge and discharge, a resin sheet with a metal base layer may be used for the positive electrode current collector. In the case of a positive electrode, the metal base layer preferably contains, for example, aluminum, stainless steel, etc.

[0081] The thickness of the positive electrode current collector is not particularly limited and is, for example, 5 μm or more and 300 μm or less.

[0082] [Separator] A porous sheet having ion permeability and insulating properties is used for the separator. Examples of porous sheets include thin films, woven fabrics, and nonwoven fabrics having micropores. The material of the separator is not particularly limited, but may be a polymer material. Examples of polymer materials include olefin resins, polyamide resins, and cellulose. Examples of olefin resins include polyethylene, polypropylene, and copolymers of ethylene and propylene. The separator may contain additives as needed. Examples of additives include inorganic fillers.

[0083] The thickness of the separator is not particularly limited, but is, for example, 5 μm or more and 80 μm or less, and more preferably 10 μm or more and 50 μm or less.

[0084] [Non-aqueous electrolyte] The non-aqueous electrolyte has ion conductivity (e.g., lithium ion conductivity). The non-aqueous electrolyte having lithium ion conductivity contains, for example, a non-aqueous solvent and lithium ions and anions dissolved in the non-aqueous solvent. The non-aqueous electrolyte may be liquid or gel-like. The liquid non-aqueous electrolyte is prepared by dissolving a lithium salt in a non-aqueous solvent. The dissolution of the lithium salt in the non-aqueous solvent generates lithium ions and anions.

[0085] As the lithium salt or anion, known materials used in non-aqueous electrolytes of lithium secondary batteries can be used. Specifically, BF 4 - , ClO 4 - , P.F. 6 - , C.F. 3 SO 3 - , C.F. 3 CO 2 - , anions of imides, anions of oxalate complexes, etc. Examples of the anions of imides include N(SO 2 CF 3 ) 2 - , N(SO 2 C m F 2m+1 ) x (SO 2 C n F 2n+1 ) y - (m and n are each independently an integer of 0 or 1 or greater, and x and y are each independently 0, 1, or 2, satisfying x+y=2.) The anion of the oxalate complex may contain boron and / or phosphorus. The non-aqueous electrolyte may contain one or more of these anions.

[0086] From the viewpoint of suppressing the deposition of lithium metal in a dendritic form, the nonaqueous electrolyte preferably contains at least an anion of an oxalate complex, and more preferably contains an oxalate complex anion having fluorine. The interaction between the oxalate complex anion having fluorine and lithium facilitates the uniform deposition of lithium metal in the form of fine particles. This makes it easier to suppress local deposition of lithium metal. The oxalate complex anion having fluorine may be combined with another anion. The other anion may be PF 6 - and / or anions of imides. Examples of the anion of the oxalate complex include bisoxalate borate anion and difluorooxalate borate anion (BF 2 (C2 O 4 ) - ), P.F. 4 (C 2 O 4 ) - , P.F. 2 (C 2 O 4 ) 2 - and the like, and it is desirable to use at least a difluorooxalatoborate anion.

[0087] Examples of non-aqueous solvents include esters, ethers, nitriles, amides, and halogen-substituted derivatives thereof. The non-aqueous electrolyte may contain one or more of these non-aqueous solvents. Examples of halogen-substituted derivatives include fluorides.

[0088] Examples of esters include carbonate esters and carboxylic acid esters. Examples of cyclic carbonate esters include ethylene carbonate, propylene carbonate, and fluoroethylene carbonate (FEC). Examples of chain carbonate esters include dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), and diethyl carbonate. Examples of cyclic carboxylic acid esters include γ-butyrolactone and γ-valerolactone. Examples of chain carboxylic acid esters include ethyl acetate, methyl propionate, and methyl fluoropropionate.

[0089] Examples of the ether include cyclic ethers and chain ethers. Examples of the cyclic ethers include 1,3-dioxolane, 4-methyl-1,3-dioxolane, tetrahydrofuran, and 2-methyltetrahydrofuran. Examples of the chain ethers include 1,2-dimethoxyethane, diethyl ether, ethyl vinyl ether, methyl phenyl ether, benzyl ethyl ether, diphenyl ether, dibenzyl ether, 1,2-diethoxyethane, and diethylene glycol dimethyl ether.

[0090] The concentration of the lithium salt in the non-aqueous electrolyte may be, for example, 0.5 mol / L or more and 3.5 mol / L or less. The concentration of the anion in the non-aqueous electrolyte may be 0.5 mol / L or more and 3.5 mol / L or less. The concentration of the anion of the oxalate complex in the non-aqueous electrolyte may be 0.05 mol / L or more and 1 mol / L or less.

[0091] FIG. 4 is a longitudinal cross-sectional view schematically illustrating a cross section parallel to the winding axis of a nonaqueous electrolyte secondary battery according to an embodiment of the present disclosure.

[0092] The battery 10 includes a cylindrical battery case, a wound electrode group 14 housed within the battery case, and a nonaqueous electrolyte (not shown). The battery case is composed of a cylindrical battery can 15 with a bottom and a sealing body 16 that seals the opening of the battery can 15. The battery can 15 has an annular step 21 formed by partially pressing the side wall from the outside near the opening. The sealing body 16 is supported by the surface of the step 21 on the opening side. A gasket 27 is disposed between the battery can 15 and the sealing body 16, thereby ensuring the hermeticity of the battery can. Within the battery can 15, insulating plates 17 and 18 are disposed at both ends of the electrode group 14 in the winding axis direction.

[0093] The sealing body 16 includes a filter 22, a lower valve body 23, an insulating member 24, an upper valve body 25, and a cap 26. The cap 26 is disposed outside the battery can 15, and the filter 22 is disposed inside the battery can 15. The lower valve body 23 and the upper valve body 25 are connected to each other at their respective centers, with an insulating member 24 interposed between their respective peripheral edges. The filter 22 and the lower valve body 23 are connected to each other at their respective peripheral edges. The upper valve body 25 and the cap 26 are connected to each other at their respective peripheral edges. The lower valve body 23 has an air vent. When the internal pressure of the battery can increases due to abnormal heat generation or the like, the upper valve body 25 expands toward the cap 26 and separates from the lower valve body 23. This breaks the electrical connection between the lower valve body 23 and the upper valve body 25. When the internal pressure further increases, the upper valve body 25 breaks, and gas is discharged through an opening formed in the cap 26.

[0094] The electrode group 14 has a core (B) 14c formed in the winding start region of the film piece 30 and the separator 13, and further includes a positive electrode 11, a negative electrode 12, and a separator 13 continuously wound around the core (B) 14c. The positive electrode 11, the negative electrode 12, and the separator 13 interposed therebetween are all long sheets (or strips) and are wound so that their width directions are parallel to the winding axis. The film piece 30 is contained only in the core (B) 14c.

[0095] The positive electrode 11 is electrically connected to a cap 26, which also serves as a positive electrode terminal, via a positive electrode lead 19. One end of the positive electrode lead 19 is connected, for example, near the center in the longitudinal direction of the positive electrode 11. The other end of the positive electrode lead 19 extending from the positive electrode 11 passes through a through-hole formed in the insulating plate 17 and is welded to the inner surface of the filter 22.

[0096] The negative electrode 12 is electrically connected to a battery can 15, which also serves as a negative electrode terminal, via a negative electrode lead 20. One end of the negative electrode lead 20 is connected to, for example, an end of the negative electrode 12 in the longitudinal direction, and the other end is welded to the inner bottom surface of the battery can 15.

[0097] In the illustrated example, a cylindrical nonaqueous electrolyte secondary battery having a wound electrode group has been described, but the shape of the lithium secondary battery is not limited to this, and it may be rectangular, and various shapes may be appropriately selected depending on the application, etc. Also, known configurations other than those described above can be used without particular limitation.

[0098] <<Supplementary Notes>> The above embodiments disclose the following technologies. (Technology 1) A nonaqueous electrolyte secondary battery comprising: a wound electrode group having a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode; and a nonaqueous electrolyte; the electrode group has a core for winding, the core including a film piece and a winding start region of the separator; the film piece and the winding start region are overlapped and wound; and the innermost periphery of the core is closed by a bent portion formed when the overlapped film piece and the winding start region are folded in half. (Technology 2) The nonaqueous electrolyte secondary battery according to Technology 1, wherein the film piece is wrapped by the winding start region at the bent portion. (Technology 3) The nonaqueous electrolyte secondary battery according to Technology 1 or 2, wherein the winding start region is wrapped by the film piece at the bent portion. (Technology 4) The electrode group has a first space inside the innermost periphery of the core portion and a second space adjacent to the first space via the film piece and the winding start end region, one of the first space and the second space being surrounded by the film piece, and the other of the first space and the second space being surrounded by the winding start end region. (Technology 5) The nonaqueous electrolyte secondary battery according to any one of Technologies 1 to 4, wherein two layers of the film piece are superimposed and wound together with the winding start end region one to ten times. (Technology 6) The nonaqueous electrolyte secondary battery according to any one of Technologies 1 to 5, wherein the film piece is a resin film. (Technology 7) The nonaqueous electrolyte secondary battery according to Technology 6, wherein the resin film has a thickness of 0.005 mm or more and 0.1 mm or less. (Technology 8) The nonaqueous electrolyte secondary battery according to any one of Technologies 1 to 7, wherein the maximum diameter of the core portion is 0.5 mm or more and 6 mm or less. (Technology 9) The nonaqueous electrolyte secondary battery according to any one of Technologies 1 to 8, wherein the tensile strength of the film piece in the MD direction is 10 MPa or more and 400 MPa or less. (Technology 10) The nonaqueous electrolyte secondary battery according to any one of Technologies 1 to 9, wherein the elongation of the film piece is 30% or more.(Technology 11) The nonaqueous electrolyte secondary battery according to any one of Technologies 1 to 10, wherein lithium metal precipitates in the negative electrode during charging and the lithium metal dissolves during discharging. (Technology 12) The nonaqueous electrolyte secondary battery according to any one of Technologies 1 to 11, wherein the negative electrode includes a negative electrode current collector that supports the lithium metal that precipitates during charging, and the negative electrode current collector includes a stainless steel foil, an oxygen-free copper foil, or a resin film.

[0099] Examples The nonaqueous electrolyte secondary battery according to the present disclosure will be described in more detail below with reference to examples and comparative examples, although the present disclosure is not limited to the following examples.

[0100] Example 1 (Preparation of Positive Electrode) 2.5 parts by mass of acetylene black and 2.5 parts by mass of polyvinylidene fluoride were added to 95 parts by mass of a positive electrode active material, and an appropriate amount of N-methyl-2-pyrrolidone was further added and stirred to prepare a positive electrode mixture slurry. The positive electrode active material used was a rock salt type lithium-containing transition metal oxide having a layered structure and containing Li, Ni, Co, and Al (the molar ratio of Li to the total of Ni, Co, and Al was 1.0).

[0101] The positive electrode composite slurry was applied to both sides of a strip of 14 μm thick Al foil (positive electrode current collector), dried, and the coating was rolled to obtain a laminate in which a positive electrode composite layer was formed on both sides of the positive electrode current collector. The laminate was cut to a predetermined electrode size to obtain a strip of positive electrode 11. An Al positive electrode lead 19 was attached to a predetermined position of the positive electrode 11.

[0102] (Preparation of negative electrode) Lithium silicate (Li) having an average particle size of 10 μm 2 O.2.1SiO 2) and raw silicon (3N, average particle size 10 μm) were mixed in a mass ratio of 50:50, and the mixture was loaded into a planetary ball mill pot. SUS balls (20 mm diameter) were placed in the pot, the lid was closed, and the mixture was milled in an inert atmosphere at 200 rpm for 50 hours. The powdered mixture was then removed from the inert atmosphere and fired at 600°C for 4 hours to obtain a sintered mixture (Si-containing material). The Si-containing material was then pulverized, passed through a 40 μm mesh, mixed with coal pitch, and fired in an inert atmosphere at 800°C for 5 hours to coat the surface of the Si-containing material with conductive carbon. The conductive carbon content was 5% by mass. A Si-containing material having a conductive layer with an average particle size of 10 μm was then obtained using a sieve.

[0103] The Si-containing material having a conductive layer and graphite were mixed in a mass ratio of 5:95 to form a negative electrode active material. The negative electrode active material, sodium carboxymethyl cellulose (CMC-Na), and styrene-butadiene rubber (SBR) were mixed in a mass ratio of 97.5:1:1.5, water was added, and the mixture was stirred using a mixer to prepare a negative electrode slurry.

[0104] The negative electrode composite slurry was applied to both sides of a strip of 12 μm thick electrolytic copper foil (negative electrode current collector), dried, and the coating was rolled to obtain a laminate in which a negative electrode composite layer was formed on both sides of the negative electrode current collector. The laminate was cut to a predetermined electrode size to obtain a strip-shaped negative electrode 12. A Ni negative electrode lead 20 was attached to a predetermined position of the negative electrode 12.

[0105] (Preparation of Separator) A separator (microporous film) made of polyethylene and having a thickness of 20 μm was prepared.

[0106] (Preparation of Film Piece) A stainless steel foil (SUS304) having a thickness of 0.12 mm and a tensile strength of 650 MPa and an elongation of 5% was prepared.

[0107] (Preparation of non-aqueous electrolyte A) LiPF 6 was dissolved in a mixed solvent containing ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 3:7. 6 was dissolved in a solution at a concentration of 1.0 mol / L to prepare a non-aqueous electrolyte A.

[0108] (Battery Assembly) A pair of rod-shaped bodies was used as a winding core to form an electrode group in an inert gas atmosphere. The cross section perpendicular to the longitudinal direction of each rod-shaped body was roughly semicircular. The separator was wound around the periphery of one rod-shaped body with the separator on the inside and the film piece on the outside, and the winding start region of the separator and the film piece were sandwiched between the pair of rod-shaped bodies and wound to form a core (B). The length of the film piece was determined so that the maximum diameter of the core (B) was 7 mm. The negative electrode and positive electrode were then sequentially wound with the two layers of separator extending from the core (B), and the separator, positive electrode, and negative electrode were wound to form an electrode group. After winding was completed, the winding core was removed.

[0109] A bag-shaped exterior body made of a laminate sheet having an Al layer was prepared, an electrode group was housed in the exterior body, and a non-aqueous electrolyte was injected, followed by sealing the exterior body to prepare a battery A1.

[0110] Example 2 Battery A2 was produced in the same manner as Battery A1, except that in forming the electrode group, a core (B) was formed by wrapping the film piece on the inner side and the separator on the outer side around the circumferential surface of a rod-shaped body.

[0111] Example 3 Battery A3 was fabricated in the same manner as Battery A2, except that an electrolytic copper foil (negative electrode current collector) without a negative electrode composite layer was used as the negative electrode, and nonaqueous electrolyte A was changed to nonaqueous electrolyte B. Nonaqueous electrolyte B was a mixture of 1,2-dimethoxyethane and 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether with LiPF 6 and LiBF 2 (C 2 O 4 ) were dissolved in the non-aqueous electrolyte. 6 The concentration of LiBF is 1 mol / L. 2 (C 2 O 4 The concentration of ) was 0.1 mol / L.

[0112] Example 4 A negative electrode having a lithium metal layer (lithium underlayer) was formed by pressure-bonding lithium metal foil (30 μm thick) to both sides of a negative electrode current collector in a dry atmosphere with a dew point of −30° C. or lower. Using this negative electrode, Battery A4 was fabricated in the same manner as Battery A2, except that non-aqueous electrolyte A was changed to non-aqueous electrolyte B.

[0113] Example 5 Battery A5 was produced in the same manner as Battery A4, except that a polyethylene terephthalate (PET) film having a thickness of 0.05 mm was used as the film piece.

[0114] Example 6 Battery A6 was produced in the same manner as Battery A4, except that a polypropylene (PP) film having a thickness of 0.05 mm was used as the film piece.

[0115] Example 7 Battery A7 was produced in the same manner as Battery A4, except that a polyimide (PI) film having a thickness of 0.038 mm was used as the film piece.

[0116] Example 8 Battery A8 was produced in the same manner as Battery A4, except that a PET film having a thickness of 0.038 mm was used as the film piece and the maximum diameter of the core portion (B) was changed to 3 mm.

[0117] Example 9 Battery A9 was fabricated in the same manner as Battery A4, except that a 0.02 mm thick PET film was used as the film piece, the maximum diameter of the core (B) was changed to 3 mm, and the negative electrode current collector was changed to oxygen-free copper foil (JIS H 3100, alloy number C1020 foil).

[0118] Example 10 Battery A10 was fabricated in the same manner as Battery A4, except that a 0.02 mm thick PET film was used as the film piece, the maximum diameter of the core (B) was changed to 3 mm, and the negative electrode current collector was changed to austenitic stainless steel foil (SUS316L).

[0119] Example 11 Battery A11 was produced in the same manner as Battery A4, except that a 0.02 mm thick PET film was used as the film piece, the maximum diameter of the core (B) was changed to 3 mm, and the negative electrode current collector was changed to a resin sheet with a metal base layer. The resin sheet with a metal base layer was a PET sheet (12 μm thick) with copper metal base layers (1.0 μm thick) formed on both sides.

[0120] Example 12 Battery A12 was produced in the same manner as Battery A11, except that in forming the electrode group, a core (B) was formed by wrapping the separator on the inner side and the film piece on the outer side around the circumferential surface of a rod-shaped body.

[0121] Comparative Example 1 In forming an electrode assembly, a core having a maximum diameter of 7 mm was formed by winding only the same film piece as that used in Battery A2 around the periphery of a cylindrical rod-shaped body having a circular cross section, and a two-layer separator was connected to this core with tape. Then, the negative electrode and positive electrode were sequentially wound with the two-layer separator connected to the core, and the separator, positive electrode, and negative electrode were wound together. Finally, the rod-shaped body was pulled out to form an electrode assembly. Battery B1 was fabricated in the same manner as Battery A2, except that the obtained electrode assembly was used.

[0122] Comparative Example 2 In forming an electrode group, a core having a maximum diameter of 3 mm was formed by winding only the same film piece as that used in Battery A8 around the periphery of a cylindrical rod-shaped body having a circular cross section, and a two-layer separator was connected to this core with tape. Then, the negative electrode and positive electrode were sequentially wound with the two-layer separator connected to the core, and the separator, positive electrode, and negative electrode were wound together. Finally, the rod-shaped body was pulled out to form an electrode group. Battery B2 was fabricated in the same manner as Battery A8, except that the obtained electrode group was used.

[0123] Comparative Example 3 Battery B3 was fabricated in the same manner as Battery B2, except that the same negative electrode as that used in Battery A10 was used in forming the electrode assembly.

[0124] The main characteristics of each battery obtained are shown in Table 1. Table 1 also shows the tensile strength and elongation of the film pieces used in each battery.

[0125]

[0126] [Evaluation: Number of Cycles] A charge / discharge test was carried out on each battery in a thermostatic chamber at 25° C. under the following conditions: The rest time between charge and discharge was 20 minutes.

[0127] (Charging) The battery was charged at a constant current of 2.15 mA per unit area (cm 2 ) of the electrode until the battery voltage reached 4.1 V, and then charged at a constant voltage of 4.1 V until the current value per unit area of ​​the electrode reached 0.54 mA.

[0128] (Discharge) Constant current discharge was carried out at a current of 2.15 mA per unit area of ​​the electrode until the battery voltage reached 3.75 V.

[0129] The above charge and discharge constitute one cycle, and charge and discharge were repeated. The number of cycles until the discharge capacity of the battery of Example 1 reached 80% of the initial discharge capacity was set to 100, and the number of cycles for the other batteries is shown in Table 1 as a relative value.

[0130] The number of cycles for Batteries A1 to A12 was significantly higher than for Batteries B1 to B3. This is thought to be because the core of Batteries A1 to A12 contracted during charge and discharge, mitigating the increase in surface pressure on the electrode assembly. The core of Batteries B1 to B3 also contracted during charge and discharge, but the film and separator had different slipperiness, preventing smooth deformation toward the inner periphery. This resulted in uneven deformation of the core, damaging the electrode assembly, and deteriorating cycle performance.

[0131] The nonaqueous electrolyte secondary battery of the present disclosure can be used in electronic devices such as mobile phones, smartphones, and tablet terminals, electric vehicles, hybrid vehicles, plug-in hybrid vehicles, and home storage batteries.

[0132] While the present invention has been described in terms of presently preferred embodiments, such disclosure is not to be interpreted as limiting. Various changes and modifications will no doubt become apparent to those skilled in the art to which the present invention pertains upon reading the above disclosure. It is therefore intended that the appended claims be interpreted to cover all changes and modifications that do not depart from the true spirit and scope of the invention.

[0133] 9a, 9b: Winding core (rod-shaped body), 10: Non-aqueous electrolyte secondary battery, 11: Positive electrode, 12: Negative electrode, 13: Separator, 14: Electrode group, 14c: Core, 15: Battery can, 16: Sealing body, 17, 18: Insulating plate, 19: Positive electrode lead, 20: Negative electrode lead, 21: Step, 22: Filter, 23: Lower valve body, 24: Insulating member, 25: Upper valve body, 26: Cap, 27: Gasket, 30: Film piece

Claims

1. A non-aqueous electrolyte secondary battery comprising: a wound electrode group having a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode; and a non-aqueous electrolyte, wherein the electrode group has a core for winding, the core including a film piece and a winding start end region of the separator, the film piece and the winding start end region are overlapped and wound, and the innermost periphery of the core is blocked by a bent portion formed when the overlapped film piece and the winding start end region are folded in half.

2. The nonaqueous electrolyte secondary battery according to claim 1, wherein the film piece is wrapped by the winding start end region at the bent portion.

3. The nonaqueous electrolyte secondary battery according to claim 1, wherein the winding start region at the bent portion is wrapped with the film piece.

4. The nonaqueous electrolyte secondary battery according to claim 1, wherein the electrode group has a first space inside the innermost periphery of the core portion and a second space adjacent to the first space via the film piece and a part of the winding start end region, one of the first space and the second space being surrounded by the film piece, and the other of the first space and the second space being surrounded by the winding start end region.

5. The nonaqueous electrolyte secondary battery according to claim 1, wherein the two layers of the film piece are overlapped and wound together with the winding start region one or more times and ten or less times.

6. The nonaqueous electrolyte secondary battery according to claim 1, wherein the film piece is a resin film.

7. The nonaqueous electrolyte secondary battery according to claim 6, wherein the resin film has a thickness of 0.005 mm or more and 0.1 mm or less.

8. The nonaqueous electrolyte secondary battery according to claim 1, wherein the maximum diameter of the core portion is 0.5 mm or more and 6 mm or less.

9. The nonaqueous electrolyte secondary battery according to claim 1, wherein the film piece has a tensile strength in the MD direction of 10 MPa or more and 400 MPa or less.

10. The nonaqueous electrolyte secondary battery according to claim 1, wherein the film piece has an elongation of 30% or more.

11. The nonaqueous electrolyte secondary battery according to claim 1, wherein lithium metal is precipitated in the negative electrode during charging, and the lithium metal dissolves during discharging.

12. The nonaqueous electrolyte secondary battery according to claim 1, wherein the negative electrode comprises a negative electrode current collector that supports the lithium metal that precipitates during charging, and the negative electrode current collector includes stainless steel foil, oxygen-free copper foil, or a resin film.

Citation Information

Patent Citations

  • Cylindrical lithium battery

    JP2001229970A

  • Manufacture of cylindrical type spiral battery

    JP1993299120A

  • Cylinder-shaped nonaqueous electrolyte battery