Secondary battery

The secondary battery design with a low friction surface on the non-opposed portion of the negative electrode in the wound-type electrode body addresses deformation issues by allowing the electrode to slip, thereby preventing self-discharge and internal short circuits, enhancing the battery's stability and performance.

WO2024214611A1PCT designated stage expired Publication Date: 2024-10-17PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD

Patent Information

Application Number
PCT/JP2024/013739
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-10
Filing Date
2024-04-03
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Conventional secondary batteries with wound-type electrode bodies experience deformation due to charging and discharging, leading to potential self-discharge through internal short circuits, as local stress is applied during expansion and contraction, particularly at the center of the electrode body.

Method used

A secondary battery design featuring a wound-type electrode body with a negative electrode composite layer on a core, where the negative electrode has a non-opposed portion with a low friction surface (static friction coefficient of 0.4 or less) facing the separator, preventing deformation by allowing the electrode to slip and reduce stress during charging and discharging.

Benefits of technology

The low friction surface on the non-opposed portion effectively suppresses electrode plate deformation, reducing the risk of self-discharge and internal short circuits, as demonstrated by the absence of deformation in tested batteries after multiple charge-discharge cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024013739_17102024_PF_FP_ABST
    Figure JP2024013739_17102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a secondary battery with which electrode plate deformation caused by charging and discharging can be suppressed. This secondary battery has an electrode body in which a positive electrode (11) and a negative electrode (12) that has a negative electrode mixture layer (50) disposed on a negative electrode core body (48) are wound with a separator interposed therebetween. The secondary battery is characterized in that the negative electrode (12) has, at a winding start-side end, an outer peripheral-side non-facing section (44) and an inner peripheral-side non-facing section (46) that do not face the positive electrode (11), with the separator interposed therebetween, and at least one of the surface on the outer peripheral-side non-facing section (44) and the surface on the inner peripheral-side non-facing section (46) has a low-friction region in which the coefficient of static friction with the facing separator is 0.4 or less.
Need to check novelty before this filing date? Find Prior Art

Description

secondary battery

[0001] The present disclosure relates to secondary batteries.

[0002] Secondary batteries such as lithium-ion secondary batteries are used as power sources for a wide range of devices, including electric vehicles, and there is a demand for ever-higher capacity. In secondary batteries that include a wound electrode assembly in which a positive electrode, a negative electrode, and a separator are wound together, stress may be applied locally within the electrode assembly when the electrode assembly expands during charging and discharging, potentially resulting in plate deformation in which at least one of the positive electrode and the negative electrode deforms. In particular, local stress is likely to be applied to the center (winding core) of the electrode assembly, leading to plate deformation at the electrode winding start end.

[0003] For example, Patent Document 1 discloses a nonaqueous electrolyte secondary battery including a wound electrode assembly in which a positive electrode and a negative electrode having a negative electrode active material layer formed on the surface of a strip-shaped negative electrode current collector are spirally wound with a separator interposed therebetween, the negative electrode including a negative electrode lead joined to the end of the negative electrode current collector at the winding start side, and wound one or more times from the inner end in the winding direction without facing the positive electrode via the separator, and including an insulating tape attached to the negative electrode current collector so as to straddle the surface of the negative electrode lead in the winding direction. According to Patent Document 1, by attaching the insulating tape to the negative electrode current collector so as to straddle the surface of the negative electrode lead, it is possible to suppress deformation of the electrode plate due to charge and discharge.

[0004] International Publication No. 2018 / 180748

[0005] However, conventional technologies may cause plate deformation depending on the charge / discharge conditions, leaving room for improvement. Since plate deformation can lead to, for example, self-discharge due to an internal short circuit in the battery, it is important to suppress plate deformation.

[0006] Therefore, an object of the present disclosure is to provide a secondary battery capable of suppressing deformation of electrode plates caused by charging and discharging.

[0007] The present disclosure provides a secondary battery having an electrode assembly in which a positive electrode and a negative electrode having a negative electrode composite layer disposed on a negative electrode core are wound with a separator interposed therebetween, wherein the negative electrode has a non-facing portion at a winding start end that does not face the positive electrode with the separator interposed therebetween, and the surface of the non-facing portion has a low-friction region in which the friction coefficient between the negative electrode and the opposing separator is 0.4 or less.

[0008] According to the present disclosure, a secondary battery capable of suppressing deformation of electrode plates due to charging and discharging can be provided.

[0009] FIG. 2 is a schematic cross-sectional view of a secondary battery that is an example of an embodiment. FIG. 3 is a diagram schematically showing a portion of the inner end side in the winding direction of an electrode body in the A-A cross section of FIG. 1. FIG. 4 is a schematic cross-sectional view showing the state of the winding start end sides of the negative electrode and positive electrode before winding. FIG. 5 is a schematic cross-sectional view showing an example of the configuration of an insulating tape. FIG. 6 is a schematic cross-sectional view showing the state of the winding start end sides of the negative electrode and positive electrode before winding in Example 1. FIG. 7 is a schematic cross-sectional view showing the state of the winding start end sides of the negative electrode and positive electrode before winding in Comparative Example 1. FIG. 8 is a schematic view of an apparatus for measuring the static friction coefficient.

[0010] An example of an embodiment of a secondary battery according to the present disclosure will be described in detail below.

[0011] Fig. 1 is a schematic cross-sectional view of a secondary battery according to an embodiment. The secondary battery 10 shown in Fig. 1 includes a wound electrode assembly 14 formed by winding a positive electrode 11 and a negative electrode 12 with a separator 13 interposed therebetween, a non-aqueous electrolyte, insulating plates 18a and 18b disposed above and below the electrode assembly 14, and a battery case 15 serving as an exterior body. The battery case 15 includes a case body 16 that houses the electrode assembly 14, the non-aqueous electrolyte, and the like, and a sealing body 17 that closes the opening of the case body 16. The battery case 15 is not limited to a cylindrical or rectangular metal case, and may be, for example, a resin case formed by laminating a resin sheet (a so-called laminate type).

[0012] The non-aqueous electrolyte is, for example, an electrolyte having lithium ion conductivity, and may be a liquid electrolyte (electrolytic solution) or a solid electrolyte.

[0013] The liquid electrolyte (electrolytic solution) contains, for example, a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. Examples of the non-aqueous solvent include esters, ethers, nitriles, amides, and mixed solvents of two or more of these. Examples of the non-aqueous solvent include ethylene carbonate (EC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), diethyl carbonate (DEC), and mixed solvents of these. The non-aqueous solvent may contain a halogen-substituted compound (e.g., fluoroethylene carbonate) in which at least a portion of the hydrogen atoms of these solvents are substituted with halogen atoms such as fluorine. Examples of the electrolyte salt include LiPF 6 Lithium salts such as

[0014] Furthermore, examples of the solid electrolyte that can be used include solid or gel polymer electrolytes, inorganic solid electrolytes, etc. Examples of the inorganic solid electrolyte that can be used include materials known in all-solid-state lithium ion secondary batteries (e.g., oxide-based solid electrolytes, sulfide-based solid electrolytes, halogen-based solid electrolytes, etc.) Examples of the polymer electrolyte include a lithium salt and a matrix polymer, or a non-aqueous solvent, a lithium salt, and a matrix polymer. Examples of the matrix polymer include a polymer material that absorbs a non-aqueous solvent and gels. Examples of the polymer material include fluororesins, acrylic resins, and polyether resins. The non-aqueous electrolyte is just one example, and aqueous electrolytes may also be used if applicable.

[0015] The case body 16 is, for example, a cylindrical metal container with a bottom. A gasket 27 is provided between the case body 16 and the sealing body 17 to ensure airtightness inside the battery. The case body 16 has, for example, a protruding portion 21, which is a portion of the side surface that protrudes inward and supports the sealing body 17. The protruding portion 21 is preferably formed in an annular shape along the circumferential direction of the case body 16, and supports the sealing body 17 on its upper surface.

[0016] The sealing body 17 has a structure in which a filter 22, a lower valve body 23, an insulator 24, an upper valve body 25, and a cap 26 are stacked in this order from the electrode body 14 side. Each component constituting the sealing body 17 has, for example, a disk or ring shape, and each component except for the insulator 24 is electrically connected to one another. The lower valve body 23 and the upper valve body 25 are connected to one another at their respective centers, with the insulator 24 interposed between their respective peripheral edges. If the internal pressure of the secondary battery 10 increases due to heat generation caused by an internal short circuit or the like, for example, the lower valve body 23 may deform and rupture, pushing the upper valve body 25 toward the cap 26, thereby interrupting the current path between the lower valve body 23 and the upper valve body 25. If the internal pressure further increases, the upper valve body 25 may rupture, allowing gas to be discharged through the opening of the cap 26.

[0017] In the secondary battery 10 shown in FIG. 1 , the positive electrode lead 19 attached to the positive electrode 11 extends through a through-hole in the insulating plate 18a toward the sealing body 17 and is connected by welding or the like to the underside of the filter 22, which is the bottom plate of the sealing body 17. As a result, the cap 26, which is the top plate of the sealing body 17 and is electrically connected to the filter 22, serves as the positive electrode terminal. Also, in the secondary battery 10 shown in FIG. 1 , the negative electrode lead 20a connected to the winding start end of the negative electrode 12 and the negative electrode lead 20b connected to the winding end end of the negative electrode 12 extend through the insulating plate 18b toward the bottom side of the case body 16 and are connected to the inner bottom surface of the case body 16 by welding or the like. As a result, the case body 16 serves as the negative electrode terminal.

[0018] FIG. 2 is a schematic diagram showing the inner end side of the electrode assembly in the winding direction of the A-A cross section in FIG. 1 . In FIG. 2 , to make the arrangement easier to understand, the negative electrode 12 is shown with a solid line, the positive electrode 11 with a dashed line, and the separator 13 with a dashed line. Also, in FIG. 2 , the gaps between the positive electrode 11, the negative electrode 12, and the separator 13 are exaggerated. The electrode assembly 14 is formed by winding the positive electrode 11 and the negative electrode 12 with the separator 13 interposed therebetween. The electrode assembly 14 is produced, for example, by stacking a strip-shaped positive electrode 11, a strip-shaped negative electrode 12, and a pair of strip-shaped separators 13 in the order of one separator 13, the positive electrode 11, the other separator 13, and the negative electrode 12, and then spirally winding this stack. In the electrode assembly 14, the longitudinal direction of each electrode is the winding direction, and the width direction of each electrode is the winding axis direction.

[0019] As shown in Fig. 2, the negative electrode 12 has, at the winding start end, a non-facing portion 40 composed of an outer peripheral non-facing portion 44 and an inner peripheral non-facing portion 46 that do not face the positive electrode 11 via the separator 13. The negative electrode 12 also has an insulating member, which will be described later. Although the insulating member is not shown in Fig. 2, the insulating member is disposed on the non-facing portion 40. The negative electrode 12 also has a facing portion 42 that faces the positive electrode 11 via the separator 13. The facing portion 42 is wound following the non-facing portion 40.

[0020] The non-facing portion 40 has an outer circumferential non-facing portion 44 and an inner circumferential non-facing portion 46. The outer circumferential non-facing portion 44 is a non-facing portion located on the outer side in the radial direction of the wound negative electrode 12, and the inner circumferential non-facing portion 46 is a non-facing portion located on the inner side in the radial direction of the wound negative electrode 12. The non-facing portion 40 (the outer circumferential non-facing portion 44 and the inner circumferential non-facing portion 46) shown in FIG. 2 is wound 1.5 times from the winding start end (point E1 in FIG. 2) of the negative electrode 12. That is, the non-facing portion 40 (the outer circumferential non-facing portion 44 and the inner circumferential non-facing portion 46) extends from point E1 in FIG. 2 along the winding direction to point E2. The number of winding turns of the non-facing portion 40 (the outer circumferential non-facing portion 44 and the inner circumferential non-facing portion 46) is not particularly limited, but is preferably 1.5 turns or more, and more preferably 1.5 turns or more and 3 turns or less.

[0021] In this embodiment, the surface of the non-facing portion 40 has a low-friction region in which the static friction coefficient between the non-facing portion and the opposing separator 13 is 0.4 or less. By having the low-friction region on the surface of the non-facing portion 40, even if local stress is applied to the center of the electrode assembly, for example, during charging and discharging, the negative electrode 12 at the winding start end side slides, alleviating the stress on the electrode and suppressing plate deformation associated with charging and discharging. The static friction coefficient in the low-friction region is preferably 0.3 or less, for example, in order to suppress plate deformation associated with charging and discharging. Furthermore, from a manufacturing standpoint, the lower limit of the static friction coefficient is preferably 0.05 or more. Here, the surface of the non-facing portion 40 in the present disclosure may be the surface of the non-facing portion 40 itself, or the surface of a member (e.g., an insulating member described below) disposed on the non-facing portion. The entire surface of the non-facing portion may be configured to have the low-friction region, or only a portion of the surface of the non-facing portion may be configured to have the low-friction region. 2, the non-facing portion 40 has an outer peripheral non-facing portion 44 and an inner peripheral non-facing portion 46, and it is sufficient that the low friction region is provided on at least one of the surface of the outer peripheral non-facing portion 44 and the surface of the inner peripheral non-facing portion 46. A method for measuring the static friction coefficient is described in the Examples section.

[0022] The low-friction region can be formed by modifying the surface of the non-facing portion 40 itself, but as will be described later, it is preferable to employ a method of disposing an insulating member on the non-facing portion 40. An example of an embodiment in which an insulating member is disposed on the non-facing portion 40 (the outer peripheral non-facing portion 44 and the inner peripheral non-facing portion 46) will be described below.

[0023] 3 is a schematic cross-sectional view showing the state of the winding start end sides of the negative electrode and positive electrode before winding. As shown in FIG. 3, the negative electrode 12 has a negative electrode core 48 and a negative electrode composite material layer 50 disposed on the negative electrode core 48. The negative electrode composite material layer 50 may be formed on only one side of the negative electrode core 48, or may be formed on both sides of the negative electrode core 48. In the negative electrode 12 shown in FIG. 3, the outer peripheral side non-facing portion 44 is composed of the negative electrode composite material layer 50 disposed on the negative electrode core 48 and an outer peripheral side exposed portion 48a where the negative electrode composite material layer 50 is not disposed on the negative electrode core 48. However, this configuration is not limited thereto, and for example, the outer peripheral side non-facing portion 44 may be composed of the negative electrode composite material layer 50 disposed on the negative electrode core 48, or the outer peripheral side exposed portion 48a where the negative electrode composite material layer 50 is not disposed on the negative electrode core 48. Similarly, the inner peripheral side non-facing portion 46 is not limited to being composed of the negative electrode composite layer 50 arranged on the negative electrode core 48 and the inner peripheral side exposed portion 48b on which the negative electrode composite layer 50 is not arranged on the negative electrode core 48, but may be composed of the inner peripheral side exposed portion 48b on which the negative electrode composite layer 50 is not arranged on the negative electrode core 48, or may be composed of the negative electrode composite layer 50 arranged on the negative electrode core 48.

[0024] The negative electrode 12 has a first insulating member 52a disposed on the outer circumferential non-facing portion 44 and a second insulating member 52b disposed on the inner circumferential non-facing portion 46. The first insulating member 52a shown in FIG. 3 is disposed on the negative electrode composite material layer 50 in the outer circumferential non-facing portion 44 and on the outer circumferential exposed portion 48a. The first insulating member 52a may be disposed entirely or partially on the negative electrode composite material layer 50 in the outer circumferential non-facing portion 44, or may be disposed entirely or partially on the outer circumferential exposed portion 48a. The second insulating member 52b shown in FIG. 3 is disposed on the negative electrode composite material layer 50 in the inner circumferential non-facing portion 46 and on the inner circumferential exposed portion 48b. The second insulating member 52b may be disposed entirely or partially on the negative electrode composite material layer 50 in the inner circumferential non-facing portion 46, or may be disposed entirely or partially on the inner circumferential exposed portion 48b.

[0025] As described above, in order to suppress plate deformation due to charging and discharging, it is sufficient that the low-friction region is provided on at least one of the surfaces on the outer peripheral non-facing portion 44 and the inner peripheral non-facing portion 46. Therefore, it is sufficient that the low-friction region is provided on at least one of the surfaces of the first insulating member 52a arranged on the outer peripheral non-facing portion 44 and the surface of the second insulating member 52b arranged on the inner peripheral non-facing portion 46. In other words, it is sufficient that at least one of the static friction coefficient between the surface of the insulating member 52a arranged on the outer peripheral non-facing portion 44 and the opposing separator (not shown) and the static friction coefficient between the surface of the second insulating member 52b arranged on the inner peripheral non-facing portion 46 and the opposing separator (not shown) satisfies the above range.

[0026] For example, in order to suppress deformation of the electrode plate due to charging and discharging, when the negative electrode 12 is wound, the first insulating member 52a is preferably positioned on the outer peripheral non-facing portion 44 for 1.5 or more revolutions in the circumferential direction of the outer peripheral non-facing portion 44 (i.e., the winding direction of the negative electrode 12), and more preferably is positioned on the outer peripheral non-facing portion 44 for 1.5 or more revolutions and 3 or less revolutions.

[0027] The first insulating member 52a may be disposed on the negative electrode composite material layer 50 in the outer circumferential non-facing portion 44, or may be disposed on the outer circumferential exposed portion 48a in the outer circumferential non-facing portion 44. Alternatively, as shown in FIG. 3 , the first insulating member 52a may be disposed on both the outer circumferential exposed portion 48a in the outer circumferential non-facing portion 44 and the negative electrode composite material layer 50. In this embodiment, for example, in terms of suppressing plate deformation associated with charge and discharge, it is preferable that the low-friction region be provided on at least one of the surface of the negative electrode composite material layer 50 in the outer circumferential non-facing portion 44 and the surface of the negative electrode composite material layer 50 in the inner circumferential non-facing portion 46. In consideration of this point, when the first insulating member 52a is disposed on the outer circumferential non-facing portion 44, the first insulating member 52a may be disposed on the negative electrode composite material layer 50 in the outer circumferential non-facing portion 44, and the surface of the first insulating member 52a on the negative electrode composite material layer 50 may have the low-friction region. That is, when the first insulating member 52a is placed on the outer peripheral non-facing portion 44, the first insulating member 52a may be placed on the negative electrode composite layer 50 in the outer peripheral non-facing portion 44, and the static friction coefficient between the surface of the first insulating member 52a on the negative electrode composite layer 50 and the opposing separator may be set to be within the above range.

[0028] Furthermore, in the present embodiment, for example, in terms of suppressing plate deformation due to charge and discharge, the low-friction region on the surface of negative electrode composite material layer 50 in outer peripheral non-facing portion 44 preferably occupies 80% or more and 100% or less of the area of ​​the entire surface of negative electrode composite material layer 50 in outer peripheral non-facing portion 44. In consideration of this point, when first insulating member 52a is placed on negative electrode composite material layer 50 in outer peripheral non-facing portion 44, the low-friction region on the surface of first insulating member 52a may occupy 80% or more and 100% or less of the area of ​​the entire surface of negative electrode composite material layer 50 in outer peripheral non-facing portion 44. In other words, the area ratio of the low-friction region on the surface of first insulating member 52a overlapping with negative electrode composite material layer 50 in outer peripheral non-facing portion 44 may be 80% or more and 100% or less.

[0029] 3, in order to suppress deformation of the electrode plate due to charging and discharging, the first insulating member 52a is preferably arranged from the circumferential inner edge 44a of the outer circumferential non-facing portion 44 onto the outer circumferential non-facing portion 44. Note that the first insulating member 52a may protrude from the outer circumferential non-facing portion 44 and be arranged on the outer circumferential facing portion, but in terms of, for example, battery capacity, it is desirable that the first insulating member 52a is not arranged on the outer circumferential facing portion.

[0030] For example, in order to suppress deformation of the electrode plate due to charging and discharging, it is preferable that the second insulating member 52b be arranged on the inner non-facing portion 46 over a circumferential direction of the inner non-facing portion 46 of at least 0.9 times, and that the area ratio overlapping with the inner non-facing portion 46 is at least 50% and at most 100%.

[0031] The second insulating member 52b may be disposed on the negative electrode composite material layer 50 in the inner circumferential non-facing portion 46, or may be disposed on the inner circumferential exposed portion 48b in the inner circumferential non-facing portion 46. Alternatively, as shown in FIG. 3 , the second insulating member 52b may be disposed on both the inner circumferential exposed portion 48b and the negative electrode composite material layer 50 in the inner circumferential non-facing portion 46. In the present embodiment, as described above, it is preferable that the low-friction region be provided on at least one of the surface of the negative electrode composite material layer 50 in the outer circumferential non-facing portion 44 and the surface of the negative electrode composite material layer 50 in the inner circumferential non-facing portion 46. In consideration of this point, when the second insulating member 52b is disposed on the inner circumferential non-facing portion 46, the second insulating member 52b may be disposed on the negative electrode composite material layer 50 in the inner circumferential non-facing portion 46, and the surface of the second insulating member 52b on the negative electrode composite material layer 50 may have the low-friction region. That is, when the second insulating member 52b is disposed on the inner circumferential non-facing portion 46, the second insulating member 52b may be disposed on the negative electrode composite material layer 50 in the inner circumferential non-facing portion 46, and the static friction coefficient between the surface of the second insulating member 52b on the negative electrode composite material layer 50 and the opposing separator may be within the above range. Furthermore, in the present embodiment, the surface of the inner circumferential exposed portion 48b preferably has the above-described low-friction region, for example, in terms of suppressing plate deformation associated with charging and discharging. Taking this into consideration, when the second insulating member 52b is disposed on the inner circumferential non-facing portion 46, the second insulating member 52b may be disposed on the inner circumferential exposed portion 48b in the inner circumferential non-facing portion 46, and the surface of the second insulating member 52b on the inner circumferential exposed portion 48b may have the above-described low-friction region. That is, when the second insulating member 52b is placed on the inner non-facing portion 46, the second insulating member 52b may be placed on the inner exposed portion 48b within the inner non-facing portion 46, and the coefficient of friction between the surface of the second insulating member 52b on the inner exposed portion 48b and the opposing separator may be set to be within the above range.

[0032] 3, in order to suppress deformation of the electrode plate due to charging and discharging, the second insulating member 52b is preferably arranged from the circumferential inner edge 46a of the inner non-facing portion 46 onto the inner non-facing portion 46. Note that the second insulating member 52b may protrude from the inner non-facing portion 46 and be arranged on the inner facing portion, but in terms of, for example, battery capacity, it is desirable that the second insulating member 52b is not arranged on the inner facing portion.

[0033] Examples of insulating members applicable to the first insulating member 52a and the second insulating member 52b include insulating sheets and insulating tapes. The insulating member preferably contains a fluororesin as its main component, in order to reduce the coefficient of static friction between the insulating member and the separator and facilitate the formation of the low-friction region on the surface. It is more preferable for the insulating member to contain at least one of polytetrafluoroethylene (PTFE) and tetrafluoroethylene-hexafluoropropylene (FEP) as its main component. In this disclosure, the term "main component" refers to a component that accounts for 50% by mass or more of the total amount of constituent components. In other words, "mainly composed of at least one of PTFE and FEP" means that at least one of PTFE and FEP is contained in an amount of 50% by mass or more. The insulating member may also be, for example, a sheet having a coating film formed on the surface of a resin sheet. The coating film preferably contains, for example, a fluororesin as a main component, and preferably contains at least one of PTFE and FEP as a main component, in order to reduce the static friction coefficient between the coating film and the separator and to facilitate the formation of the low-friction region on the surface.

[0034] 4 is a schematic cross-sectional view showing an example of the configuration of an insulating tape. The insulating tape 52 described below is applied to the first insulating member 52a and the second insulating member 52b described above. The insulating tape 52 includes, for example, a base layer 54 and an adhesive layer 56. The insulating tape 52 has a laminated structure in which the adhesive layer 56 and the base layer 54 are laminated in this order from the non-facing portion side. Therefore, the surface of the base layer 54 becomes the surface of the insulating tape 52 that faces the separator. The thickness of the insulating tape 52 is preferably 0.02 mm or more and 0.1 mm or less, for example, in terms of flexibility, strength, etc.

[0035] The base layer 54 preferably contains a fluororesin as a main component, and more preferably contains at least one of polytetrafluoroethylene (PTFE) and tetrafluoroethylene-hexafluoropropylene (FEP) as a main component, for example, to reduce the coefficient of static friction between the base layer 54 and the separator and facilitate the formation of the low-friction region on the surface. The base layer 54 may also contain other resins, such as polyolefin (e.g., polyethylene, polypropylene, etc.), polystyrene, polyester (e.g., polyethylene terephthalate, etc.), polyimide, polyamide, polyamideimide, polycarbonate, polyphenylene sulfide, etc.

[0036] The adhesive layer 56 is a layer that mainly provides the insulating tape 52 with adhesiveness to the negative electrode 12. The adhesive layer 56 is formed by applying an adhesive to one surface of the base layer 54. The adhesive that constitutes the adhesive layer 56 may be a hot-melt type that becomes adhesive when heated or a thermosetting type that hardens when heated, but from the viewpoint of productivity and the like, an adhesive that is adhesive at room temperature is preferable. Examples of adhesives include acrylic adhesives and synthetic rubber adhesives.

[0037] The insulating tape 52 is not limited to the form shown in FIG. 4 and may have, for example, an inorganic particle-containing layer between the base layer 54 and the adhesive layer 56. The inorganic particle-containing layer has, for example, a structure in which inorganic particles are dispersed in a resin matrix constituting the layer. The inorganic particle-containing layer is formed, for example, by applying a resin solution containing inorganic particles to one surface of the base layer 54. Examples of inorganic particles include metal oxide particles, metal nitride particles, metal fluoride particles, and metal carbide particles. Examples of resin matrices include acrylic resins, urethane resins, and elastomers thereof.

[0038] The negative electrode core 48 constituting the negative electrode 12 can be made of a foil of a metal such as copper or a copper alloy that is stable within the potential range of the negative electrode, or a film having such a metal disposed on the surface thereof. The thickness of the negative electrode core 48 is, for example, in the range of 7 μm to 50 μm.

[0039] Furthermore, the negative electrode mixture layer 50 constituting the negative electrode 12 contains, for example, a negative electrode active material, a binder, etc. The thickness of the negative electrode mixture layer 50 is, for example, in the range of 10 μm to 100 μm. The negative electrode mixture layer 50 can be produced, for example, by applying a negative electrode mixture slurry containing the negative electrode active material, the binder, etc. onto the negative electrode core 48, drying the coating, and then rolling it.

[0040] The negative electrode active material contained in negative electrode composite layer 50 is not particularly limited as long as it can reversibly absorb and release lithium ions, and examples thereof include carbon materials, Si-based materials, etc. From the viewpoint of increasing the capacity of the battery, it is preferable that the negative electrode active material contains a Si-based material.

[0041] The carbon material may be, for example, a conventionally known carbon material used as a negative electrode active material, and examples thereof include natural graphite such as flake graphite, lump graphite, and amorphous graphite, and artificial graphite such as lump artificial graphite (MAG) and graphitized mesophase carbon microbeads (MCMB).

[0042] The Si-based material is not particularly limited as long as it can reversibly absorb and release ions such as lithium ions, and examples thereof include Si particles, Si-containing alloy particles, Si compound particles, etc. Among these, Si compound particles are preferred.

[0043] Examples of the Si compound particles include Si compound particles having a silicate phase and Si particles dispersed in the silicate phase, Si compound particles having a silicon oxide phase and Si particles dispersed in the silicon oxide phase, and Si compound particles having a carbon phase and Si particles dispersed in the carbon phase.

[0044] The silicate phase preferably contains at least one element selected from lithium, sodium, potassium, rubidium, cesium, francium, beryllium, magnesium, calcium, strontium, barium, and radium, for example, from the viewpoint of high lithium ion conductivity, etc. Among these, a silicate phase containing lithium (hereinafter sometimes referred to as a lithium silicate phase) is preferred, for example, from the viewpoint of high lithium ion conductivity, etc.

[0045] The lithium silicate phase can be, for example, a compound of the formula: Li 2z SiO 2+z (0<z<2) From the viewpoints of stability, ease of preparation, lithium ion conductivity, and the like, z preferably satisfies the relationship 0<z<1, and more preferably z=1 / 2.

[0046] The Si compound particles in which Si particles are dispersed in a silicon oxide phase can be, for example, a compound represented by the general formula SiO x (preferably in the range of 0<x<2, and more preferably in the range of 0.5≦x≦1.6). Si compound particles in which Si particles are dispersed in a carbon phase are represented, for example, by the general formula SixC1y (preferably in the range of 0<x≦1 and 0<y≦1, and more preferably in the range of 0.3≦x≦0.45 and 0.7≦y≦0.55).

[0047] Preferably, a conductive coating made of a highly conductive material is formed on the particle surface of the Si-based material. Examples of conductive coatings include carbon coatings, metal coatings, and metal compound coatings, but carbon coatings are preferred in terms of electrochemical stability. The carbon coating can be formed, for example, by a CVD method using acetylene, methane, or the like, or by a method in which coal pitch, petroleum pitch, phenolic resin, or the like is mixed with a silicon-based active material and heat-treated. Alternatively, the conductive coating may be formed by adhering a conductive filler such as carbon black to the particle surface of the Si-based material using a binder.

[0048] The content of the Si-based material is preferably, for example, 5 mass % or more relative to the total mass of negative electrode mixture layer 50 in terms of increasing the capacity of the battery.

[0049] The negative electrode active material may contain, in addition to a carbon material and a Si-based material, other materials capable of reversibly absorbing and releasing lithium ions, such as Sn, alloys containing Sn, Sn-based materials such as tin oxide, and Ti-based materials such as lithium titanate.

[0050] Examples of binders include fluorine-based resins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), polyimide-based resins, acrylic-based resins, polyolefin-based resins, styrene-butadiene rubber (SBR), carboxymethyl cellulose (CMC) or a salt thereof, polyacrylic acid (PAA) or a salt thereof, polyvinyl alcohol (PVA), and polyethylene oxide (PEO).

[0051] The positive electrode 11 has a positive electrode core and a positive electrode composite layer formed on the surface of the positive electrode core. The positive electrode composite layer is preferably formed on both sides of the positive electrode core. The positive electrode core can be made of a foil of a metal such as aluminum that is stable within the potential range of the positive electrode 11, or a film with such a metal disposed on the surface. The positive electrode composite layer contains, for example, a positive electrode active material, a binder, a conductive agent, etc. The positive electrode composite layer can be produced, for example, by applying a positive electrode composite slurry containing a positive electrode active material, a binder, a conductive agent, etc. onto the positive electrode core, drying the coating, and then rolling it.

[0052] The positive electrode active material contained in the positive electrode mixture layer can be, for example, a lithium transition metal oxide containing a transition metal element such as Co, Mn, or Ni. x CoO 2 , Li x NiO 2 , Li x MnO 2 , Li x Co y Ni 1-y O 2 , Li x Co y M 1-y O z , Li x Ni 1-y M y O z , Li x Mn 2 O 4 , Li x Mn 2-y M y O 4 , LiMPO 4 , Li 2 MPO 4F (M: at least one of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, and B, 0<x≦1.2, 0<y≦0.9, 2.0≦z≦2.3). These may be used alone or in combination. In terms of increasing the capacity of the battery, the positive electrode active material is preferably Li x NiO 2 , Li x Co y Ni 1-y O 2 , Li x Ni 1-y M y O z It is preferable that the lithium transition metal oxide contains a lithium nickel composite oxide such as (M: at least one of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, and B; 0<x≦1.2, 0<y≦0.9, 2.0≦z≦2.3). Inorganic particles such as tungsten oxide, aluminum oxide, and lanthanoid-containing compounds may be adhered to the surface of the lithium transition metal oxide particles.

[0053] Examples of the conductive agent contained in the positive electrode mixture layer include carbon materials such as carbon black (CB), acetylene black (AB), ketjen black, carbon nanotubes (CNT), graphene, and graphite. Examples of the binder contained in the positive electrode mixture layer include the same binders as those used in the negative electrode 12.

[0054] The separator 13 may be, for example, a porous sheet having ion permeability and insulating properties. Specific examples of porous sheets include a microporous thin film, a woven fabric, and a nonwoven fabric. Suitable materials for the separator include olefin-based resins such as polyethylene and polypropylene, and cellulose. The separator 13 may be a laminate having a cellulose fiber layer and a thermoplastic resin fiber layer such as an olefin-based resin. Alternatively, the separator 13 may be a multilayer separator including a polyethylene layer and a polypropylene layer, and the surface of the separator 13 may be coated with a material such as an aramid-based resin or ceramic.

[0055] The present disclosure will be further described below with reference to examples, but the present disclosure is not limited to these examples.

[0056] Example 1 [Preparation of Positive Electrode] 100 parts by mass of LiNi 0.88 Co 0.09 Al 0.03 O 2 1 part by mass of acetylene black (AB) and 0.9 parts by mass of polyvinylidene fluoride (PVDF) were mixed, and an appropriate amount of N-methyl-2-pyrrolidone (NMP) was added to prepare a positive electrode composite slurry. Next, the positive electrode composite slurry was applied to both sides of a 15 μm thick aluminum foil, and the coating was dried. Then, the coating was rolled using a roller and cut to a predetermined electrode size, and a positive electrode having a positive electrode composite layer formed on both sides of the positive electrode core was produced. An exposed portion where no positive electrode composite layer was disposed on the positive electrode core was provided in the longitudinal center of the positive electrode, and an aluminum positive electrode lead was welded to the exposed portion.

[0057] [Preparation of Negative Electrode] 92 parts by mass of graphite powder, 6 parts by mass of Si-based material, 1 part by mass of sodium carboxymethyl cellulose (CMC-Na), and 1 part by mass of a styrene butadiene rubber (SBR) dispersion were mixed, and an appropriate amount of water was added to prepare a negative electrode composite slurry. Next, the negative electrode composite slurry was applied to both sides of an 8 μm-thick copper foil, and the coating was dried. The coating was then rolled using a roller and cut to a predetermined electrode size, producing a negative electrode in which a negative electrode composite layer was formed on both sides of the negative electrode core. Exposed portions where the negative electrode composite layer was not disposed on the negative electrode core were provided at both longitudinal ends of both sides of the negative electrode, and nickel negative electrode leads were welded to each exposed portion at both ends. Furthermore, an insulating member was disposed at the end of the negative electrode's longitudinal end, which was the end closest to the winding start. A fluororesin tape with an acrylic adhesive coated on a fluororesin substrate was used as the insulating member. The position of the insulating member in Example 1 is described below.

[0058] 5 is a schematic cross-sectional view showing the state of the winding start end sides of the negative electrode and positive electrode before winding in Example 1. In Example 1, a first insulating member 52a (fluororesin tape) was arranged on outer peripheral exposed portion 48a in outer peripheral non-facing portion 44 of negative electrode 12 and on negative electrode composite material layer 50 so that the base layer was the tape surface, and a second insulating member 52b (fluororesin tape) was arranged on inner peripheral exposed portion 48b in inner peripheral non-facing portion 46 of negative electrode 12 and on negative electrode composite material layer 50 so that the base layer was the tape surface. The area ratio of first insulating member 52a arranged on outer peripheral non-facing portion 44 that overlaps with outer peripheral exposed portion 48a in outer peripheral non-facing portion 44 is 100%, and the area ratio that overlaps with negative electrode composite material layer 50 in outer peripheral non-facing portion 44 is 94%. Furthermore, when the negative electrode 12 is wound, the first insulating member 52a is arranged over 2.1 circumferential turns in the outer non-facing portion 44 (number of turns: 2.1 turns). On the other hand, the area ratio of the second insulating member 52b arranged on the inner non-facing portion 46 that overlaps with the inner non-facing portion 46 is 97%. Furthermore, when the negative electrode 12 is wound, the second insulating member 52b is arranged over 2.1 circumferential turns in the inner non-facing portion 46 (number of turns: 2.1 turns).

[0059] <Static Friction Coefficient> The static friction coefficient between the surface of the fluororesin tape used as the first insulating member 52a arranged on the outer circumferential non-facing portion 44 and the second insulating member 52b arranged on the inner circumferential non-facing portion 46 and the opposing separator when a wound-type electrode body was fabricated was 0.20. That is, the surface of the first insulating member 52a and the surface of the second insulating member 52b each have a low-friction region with a static friction coefficient of 0.20 between the opposing separator. As described above, the area ratio of the first insulating member 52a overlapping with the negative electrode composite material layer 50 in the outer circumferential non-facing portion 44 is 94%. Therefore, the low-friction region on the surface of the first insulating member 52a occupies 94% of the entire surface area of ​​the negative electrode composite material layer 50 in the outer circumferential non-facing portion 44.

[0060] The static friction coefficient was measured as follows. FIG. 7 is a schematic diagram of an apparatus for measuring the static friction coefficient. The apparatus 60 shown in FIG. 7 includes a test stand 62, a pulley 64, a wire 66 wound around the pulley, and a weight 68 attached to one end of the wire 66 and placed on the test stand 62. A first test piece 70 was fixed to the bottom surface of the weight 68. A second test piece 72 was fixed to the test stand 62 so as to face the first test piece 70 fixed to the bottom surface of the weight 68. The other end of the wire 66 was connected to a tensile tester (not shown). The tensile tester was, for example, an Autograph (Shimadzu Corporation, Model AG-X). The weight 68 had a weight of 630 g. The first test piece 70 was a separator (dimensions: 4 cm × 3 cm) onto which 0.1 mL of nonaqueous electrolyte was dropped. The nonaqueous electrolyte was the same as that used in nonaqueous electrolyte secondary batteries. The second test piece 72 was a fluororesin tape (dimensions: 10 cm × 6 cm), with the substrate layer being the surface facing the separator. In Example 2 described later, an FEP sheet was prepared as the second test piece 72. In Comparative Example 1 described later, two test pieces were prepared as the second test piece 72: a negative electrode composite layer formed on copper foil and a polypropylene tape. In Comparative Example 2 described later, a polypropylene tape was prepared as the second test piece 72. When the polypropylene tape was used as the test piece, the substrate layer was the surface facing the separator.

[0061] During the measurement, the tensile tester is driven and an external force is applied to the weight 68 via the wire 66 at a rate of 20 mm / min. The external force is gradually increased, and the force at which the separator begins to move is measured as the static friction force. The coefficient of static friction is then calculated using the following formula: μ s =F s / F p μ s : coefficient of static friction F s : Static friction force (N) F p : Normal force generated by the mass of the weight 68 (= 1.96 N)

[0062] [Preparation of non-aqueous electrolyte] 5 parts by mass of vinylene carbonate (VC) was added to 100 parts by mass of a mixed solvent in which ethylene carbonate (EC) and dimethyl carbonate (DMC) were mixed at a volume ratio of 3:7, and lithium hexafluorophosphate (LiPF6 A non-aqueous electrolyte was prepared by dissolving 1.5 mol / L of ammonium hydroxide in water.

[0063] [Fabrication of Non-Aqueous Electrolyte Secondary Battery] The positive and negative electrodes were wound with a separator interposed therebetween to fabricate a wound electrode assembly. Insulating plates were placed on the top and bottom of the electrode assembly, and the electrode assembly was housed in a case body. The negative electrode lead was welded to the bottom of the case body, and the positive electrode lead was welded to a sealing member. After injecting a non-aqueous electrolyte into the case body, the opening of the case body was sealed with a sealing member via a gasket to fabricate a non-aqueous electrolyte secondary battery.

[0064] Example 2 A nonaqueous electrolyte secondary battery was fabricated in the same manner as in Example 1, except that an FEP sheet was used instead of the fluororesin tape used as the insulating member in Example 1. The static friction coefficient between the surface of the FEP sheet used as the insulating member arranged on the outer circumferential non-facing portion 44 and the inner circumferential non-facing portion 46 and the opposing separator when a wound electrode body was fabricated was 0.40. That is, the surface of the first insulating member 52a and the surface of the second insulating member 52b both have a low-friction region with a static friction coefficient of 0.40 between them and the opposing separator.

[0065] Comparative Example 1 Fig. 6 is a schematic cross-sectional view showing the state of the winding start end of the negative electrode and positive electrode before winding in Comparative Example 1. In Comparative Example 1, a first insulating member 52a was disposed on the outer peripheral exposed portion 48a in the outer peripheral non-facing portion 44 of the negative electrode 12 and on the negative electrode composite material layer 50 so that the base layer was the tape surface. The area ratio of the first insulating member 52a disposed on the outer peripheral non-facing portion 44 that overlaps with the outer peripheral exposed portion 48a in the outer peripheral non-facing portion 44 is 100%, and the area ratio of the first insulating member 52a that overlaps with the negative electrode composite material layer 50 in the outer peripheral non-facing portion 44 is 13%. Furthermore, when the negative electrode 12 is wound, the first insulating member 52a is disposed around the outer peripheral non-facing portion 44 for 1.0 lap in the circumferential direction (number of laps: 1.0 lap). For the first insulating member 52a, a polypropylene tape having an acrylic adhesive coated on a polypropylene substrate was used.

[0066] The static friction coefficient between the surface of the polypropylene tape used as the first insulating member 52a arranged on the outer circumferential non-facing portion 44 and the separator that faces when the wound electrode body is fabricated was 0.42. The static friction coefficient between the surface of the negative electrode composite material layer 50 of the outer circumferential non-facing portion 44 that is not covered with polypropylene tape and the separator that faces when the wound electrode body is fabricated was 0.59. In the inner circumferential non-facing portion 46 where no polypropylene tape is arranged, the static friction coefficient between the surface of the negative electrode composite material layer 50 of the inner circumferential non-facing portion 46 and the separator that faces when the wound electrode body is fabricated was 0.59, and the static friction coefficient between the inner circumferential exposed portion 48b of the inner circumferential non-facing portion 46 and the separator that faces when the wound electrode body is fabricated was 0.41.

[0067] Comparative Example 2 A nonaqueous electrolyte secondary battery was fabricated in the same manner as in Example 1, except that the polypropylene tape used in Comparative Example 1 was used instead of the fluororesin tape used as the insulating member in Example 1.

[0068] [Evaluation of Plate Deformation] The nonaqueous electrolyte secondary batteries of each Example and Comparative Example were charged at a constant current of 0.3 It until the battery voltage reached 4.2 V, and then charged at a constant voltage of 4.2 V until the current reached 0.02 It. Subsequently, the batteries were discharged at a constant current of 1.0 It until the battery voltage reached 2.7 V. This charge / discharge cycle was repeated 10 times. Then, after the 10 cycles, the cross section of the center of the electrode assembly of the nonaqueous electrolyte secondary batteries was observed using an X-ray CT scanner (Shimadzu Corporation, SMX-225CT FPD HR) to confirm the occurrence of plate deformation. The results are summarized in Table 1.

[0069]

[0070] Plate deformation was observed in Comparative Examples 1 and 2, but not in Examples 1 and 2. From these results, it can be said that by having a low-friction region in which the surface on the non-facing portion has a static friction coefficient of 0.4 or less with respect to the opposing separator, as in the Examples (i.e., by making the static friction coefficient between the surface on the non-facing portion and the opposing separator 0.4 or less), it is possible to suppress the occurrence of plate deformation due to charge and discharge.

[0071] [Notes] (1) A secondary battery having an electrode assembly in which a positive electrode and a negative electrode having a negative electrode composite layer disposed on a negative electrode core are wound with a separator interposed therebetween, wherein the negative electrode has a non-facing portion at a winding start end that does not face the positive electrode with the separator interposed therebetween, and a surface on the non-facing portion has a low-friction region in which the static friction coefficient between the negative electrode and the facing separator is 0.4 or less. (2) The secondary battery according to (1) above, in which the static friction coefficient is 0.3 or less. (3) The secondary battery according to (1) or (2) above, in which the static friction coefficient is 0.05 or more. (4) The secondary battery according to any one of (1) to (3) above, in which the negative electrode includes an insulating member disposed on the non-facing portion, and a surface of the insulating member has the low-friction region. (5) The secondary battery according to (4) above, in which the insulating member is an insulating tape. (6) The secondary battery according to (5), wherein the insulating tape has a laminated structure in which an adhesive layer and a base material layer are laminated in this order from the non-facing portion. (7) The secondary battery according to (6), wherein the base material layer contains a fluororesin as a main component. (8) The secondary battery according to (4), wherein the insulating member contains at least one of polytetrafluoroethylene (PTFE) and tetrafluoroethylene-hexafluoropropylene copolymer (FEP) as a main component. (9) The secondary battery according to any one of (4) to (8), wherein the insulating member has a thickness of 0.02 mm or more and 0.1 mm or less. (10) The secondary battery according to any one of (1) to (9), wherein the non-facing portion includes an outer circumferential non-facing portion and an inner circumferential non-facing portion, and at least one of a surface on the negative electrode composite material layer in the outer circumferential non-facing portion and a surface on the negative electrode composite material layer in the inner circumferential non-facing portion has the low-friction region. (11) The secondary battery according to (10), wherein the low-friction region occupies an area of ​​80% to 100% of the entire surface of the negative electrode composite layer in the outer non-facing portion. (12) The secondary battery according to any one of (1) to (11), wherein the non-facing portion includes an inner non-facing portion, the inner non-facing portion having an inner exposed portion where the negative electrode composite layer is not formed on the negative electrode core, and the surface of the inner exposed portion has the low-friction region.

[0072] REFERENCE SIGNS LIST 10 Secondary battery, 11 Positive electrode, 12 Negative electrode, 13 Separator, 14 Electrode body, 15 Battery case, 16 Case body, 17 Sealing body, 18a, 18b Insulating plate, 19 Positive electrode lead, 20a, 20b Negative electrode lead, 21 Protruding portion, 22 Filter, 23 Lower valve body, 24 Insulator, 25 Upper valve body, 26 Cap, 27 Gasket, 40 Non-facing portion, 42 Facing portion, 44 Outer peripheral non-facing portion, 44a, 46a Circumferential inner edge, 46 Inner peripheral non-facing portion, 48 Negative electrode core, 48a Outer peripheral exposed portion, 48b Inner peripheral exposed portion, 50 Negative electrode composite layer, 52 Insulating tape, 52a First insulating member, 52b Second insulating member, 54 Base material layer, 56 Adhesive layer, 60 Device, 62 Test stand, 64 pulley, 66 wire, 68 weight, 70 first test piece, 72 second test piece.

Claims

1. A secondary battery having an electrode body in which a positive electrode and a negative electrode having a negative electrode composite layer disposed on a negative electrode core are wound with a separator interposed therebetween, wherein the negative electrode has a non-facing portion at the end on the winding start side that does not face the positive electrode via the separator, and the surface on the non-facing portion has a low-friction region in which the friction coefficient between the negative electrode and the opposing separator is 0.4 or less.

2. The secondary battery according to claim 1, wherein the static friction coefficient is 0.3 or less.

3. The secondary battery according to claim 1 or 2, wherein the static friction coefficient is 0.05 or more.

4. The secondary battery according to claim 1 or 2, wherein the negative electrode includes an insulating member disposed on the non-facing portion, and a surface of the insulating member has the low friction region.

5. The secondary battery according to claim 4, wherein the insulating member is an insulating tape.

6. The secondary battery according to claim 5, wherein the insulating tape has a laminated structure in which an adhesive layer and a base material layer are laminated in this order from the non-facing portion side.

7. The secondary battery according to claim 6, wherein the base layer contains a fluororesin as a main component.

8. The secondary battery according to claim 4, wherein the insulating member contains at least one of polytetrafluoroethylene (PTFE) and tetrafluoroethylene-hexafluoropropylene copolymer (FEP) as a main component.

9. The secondary battery according to claim 4, wherein the insulating member has a thickness of 0.02 mm or more and 0.1 mm or less.

10. A secondary battery as described in claim 1 or 2, wherein the non-facing portion includes an outer circumferential non-facing portion and an inner circumferential non-facing portion, and at least one of a surface on the negative electrode mixture layer in the outer circumferential non-facing portion and a surface on the negative electrode mixture layer in the inner circumferential non-facing portion has the low friction region.

11. The secondary battery according to claim 10, wherein the low-friction region occupies an area of ​​80% or more and 100% or less of the entire surface of the negative electrode mixture layer in the outer circumferential non-facing portion.

12. A secondary battery as described in claim 1 or 2, wherein the non-facing portion includes an inner circumferential side non-facing portion, the inner circumferential side non-facing portion has an inner circumferential side exposed portion on which no negative electrode composite layer is formed on the negative electrode core, and a surface on the inner circumferential side exposed portion has the low friction region.

Citation Information

Patent Citations

  • Secondary battery using non-aqueous electrolyte

    WO2018180748A1

  • Alkaline secondary battery and its manufacturing method

    JP2002042859A

  • Nonaqueous electrolyte secondary battery

    JP2022168456A

  • Separator for lithium ion secondary battery and method for manufacturing the separator

    WO2008059806A1

  • Non-aqueous electrolyte secondary battery