Membrane electrolysis method for aqueous lithium salt solution
By charging a diluted lithium hydroxide solution into the cathode chamber and controlling the lithium hydroxide concentration, the membrane electrolysis method effectively addresses efficiency decreases and membrane damage issues, ensuring stable and efficient lithium recovery from aqueous lithium salt solutions.
Patent Information
- Application Number
- PCT/JP2024/013849
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-12
- Filing Date
- 2024-04-03
- Publication Date
- 2024-10-17
AI Technical Summary
Membrane electrolysis of aqueous lithium hydroxide solutions faces efficiency decreases and membrane damage due to increasing lithium hydroxide concentration and precipitation on the electrolyte membrane, leading to adverse effects.
Charging a lithium hydroxide aqueous solution with a concentration of 10% by mass or less and water into the cathode chamber of a membrane electrolyzer, followed by membrane electrolysis until a predetermined lithium hydroxide concentration is reached, and repeating these steps to maintain high efficiency and prevent lithium hydroxide deposition on the membrane.
This method achieves high efficiency in membrane electrolysis while preventing lithium hydroxide generation and deposition on the electrolyte membrane, thereby enhancing the process's stability and performance.
Smart Images

Figure JP2024013849_17102024_PF_FP_ABST
Abstract
Description
Membrane electrolysis method for lithium salt aqueous solution
[0001] The present invention relates to a method for membrane electrolysis of an aqueous lithium salt solution.
[0002] In recent years, with the widespread use of lithium ion batteries, methods have been considered for recovering valuable metals such as cobalt, nickel, manganese, and lithium from discarded lithium ion batteries and reusing them as materials for the lithium ion batteries.
[0003] Cited Document 1 discloses a system for recovering lithium from waste lithium-ion batteries, which includes the steps of: dissolving active material powder obtained by pretreating waste lithium-ion batteries in a mineral acid to obtain an acid solution of the active material containing at least lithium; separating at least one metal other than lithium from the acid solution to which lithium hydroxide has been added by solvent extraction to obtain a first aqueous lithium salt solution as a residual solution from the solvent extraction; and performing membrane electrolysis of the first aqueous lithium salt solution using an ion exchange membrane to obtain an aqueous lithium hydroxide solution, an acid, and a second aqueous lithium salt solution that is more dilute than the first aqueous lithium salt solution.
[0004] Patent No. 7060899
[0005] In membrane electrolysis of lithium hydroxide aqueous solution, the higher the lithium hydroxide concentration in the catholyte in the cathode chamber of the membrane electrolysis device, the more easily hydroxide ions move to the anode chamber, resulting in a decrease in membrane electrolysis efficiency. Furthermore, lithium hydroxide is easily deposited in and on the surface of the electrolytic membrane. The deposited lithium hydroxide can damage the electrolytic membrane, causing various adverse effects on membrane electrolysis.
[0006] Therefore, an object of the present invention is to provide a method for membrane electrolysis of an aqueous lithium salt solution, which includes a highly efficient membrane electrolysis step and is less likely to produce lithium hydroxide in or on the surface of the electrolytic membrane.
[0007] The present inventors have conducted extensive research in light of the above-mentioned problems and have found that a method for membrane electrolysis of a lithium salt aqueous solution, which includes a cathode chamber introducing step of introducing at least one selected from the group consisting of a first lithium hydroxide aqueous solution having a lithium hydroxide concentration of 10 mass % or less and water into a cathode chamber of a membrane electrolysis device, exhibits high efficiency and is less likely to produce lithium hydroxide in or on the surface of the electrolytic membrane. The present invention was completed based on these findings.
[0008] The present invention relates to a membrane electrolysis method for an aqueous lithium salt solution, including a cathode chamber introducing step of introducing at least one selected from the group consisting of a first aqueous lithium hydroxide solution having a lithium hydroxide concentration of 10% by mass or less and water into a cathode chamber of a membrane electrolysis device, and a membrane electrolysis step of performing membrane electrolysis until the lithium hydroxide concentration in the cathode chamber reaches a predetermined concentration. The cathode chamber introducing step and the membrane electrolysis step are preferably repeated sequentially. A portion of the second aqueous lithium hydroxide solution obtained in the membrane electrolysis step is preferably diluted with water to obtain the first aqueous lithium hydroxide solution. The present invention preferably further includes an acid dissolution step of dissolving an active material powder obtained by pretreating a waste lithium-ion battery in a mineral acid to obtain an acid solution of the active material containing at least lithium, a neutralization step of adding lithium hydroxide to the acid solution to neutralize the acid solution to obtain a neutralized solution, and a solvent extraction step of separating at least one metal, excluding lithium, from the active material powder by solvent extraction from the neutralized solution, and obtaining a lithium salt aqueous solution as a residue of the solvent extraction. A portion of the second lithium hydroxide aqueous solution obtained in the membrane electrolysis step is utilized in at least one step selected from the group consisting of the neutralization step and the solvent extraction step, and the mineral acid obtained in the membrane electrolysis step is utilized in the acid dissolution step. The electricity used for membrane electrolysis preferably includes electricity obtained from renewable energy. The electricity obtained from renewable energy preferably includes at least one selected from the group consisting of electricity obtained by solar power generation and electricity obtained by wind power generation.
[0009] The present invention provides a method for membrane electrolysis of an aqueous lithium salt solution, which includes a highly efficient membrane electrolysis step and is less likely to produce lithium hydroxide in or on the surface of the electrolytic membrane.
[0010] The present invention relates to a method for recovering lithium from an aqueous lithium salt solution, and an ion exchange membrane electrolytic cell for recovering lithium from the aqueous lithium salt solution.
[0011] The present invention will be described in more detail. Unless otherwise specified, the "to" in a numerical range indicates a range from above to below, and both end values are included. When a numerical range is indicated, the upper and lower limits can be combined as appropriate, and the resulting numerical range is also considered to be disclosed. Furthermore, in the description of the drawings, identical elements are given the same reference numerals, and redundant explanations will be omitted. Also, the dimensional proportions in the drawings have been exaggerated for the sake of explanation and may differ from the actual proportions.
[0012] The method for membrane electrolysis of a lithium salt aqueous solution of the present invention may start with an aqueous solution containing a dissolved lithium salt. The aqueous solution is not limited to a specific aqueous solution. Examples of the aqueous solution include seawater, brackish water, and / or brine derived from a salt lake, and aqueous solutions containing dissolved minerals. Furthermore, the method for membrane electrolysis of a lithium salt aqueous solution of the present invention may start with an active material powder 1 as shown in FIG. 1.
[0013] When the waste lithium-ion batteries are used lithium-ion batteries that have reached the end of their life as battery products or lithium-ion batteries that have been discarded as defective products during the manufacturing process, the active material powder 1 can be obtained by first discharging the batteries in salt water to discharge any remaining charge, then forming openings in the casings of the waste lithium-ion batteries, heat-treating (roasting) the batteries at a temperature in the range of 100 to 800°C, for example, or by pulverizing the batteries with a pulverizer such as a hammer mill or a jaw crusher without heat treatment, and then removing the casings, current collectors, etc. that constitute the waste lithium-ion batteries by sieving (classifying). Alternatively, the waste lithium-ion batteries after the discharge treatment may be pulverized with the pulverizer, and the casings, current collectors, etc. may be removed by sieving, followed by heat treatment at a temperature in the range or by no heat treatment, to obtain the active material powder 1.
[0014] When the waste lithium ion batteries are residual positive electrode materials or the like used in commercialization in a manufacturing process, they may be pulverized in the pulverizer after being heat-treated at a temperature in the above range without being subjected to the discharge treatment and the formation of openings, or without being heat-treated, and the current collectors and the like may be removed by sieving to obtain the active material powder 1. Furthermore, the waste lithium ion batteries may be pulverized in the pulverizer, the current collectors and the like may be removed by sieving, and the active material powder 1 may be obtained after being heat-treated at a temperature in the above range or without being heat-treated.
[0015] The membrane electrolysis method of the present invention preferably includes an acid dissolution step of dissolving the active material powder 1 obtained by pretreating the waste lithium-ion batteries in STEP 1 in a mineral acid to obtain an acid solution of the active material powder 1 containing at least lithium. The mineral acid includes, for example, at least one selected from the group consisting of hydrochloric acid, sulfuric acid, and nitric acid, preferably hydrochloric acid, and more preferably hydrochloric acid. In addition to lithium, the active material powder 1 contains valuable metals such as iron, aluminum, manganese, cobalt, and nickel.
[0016] The membrane electrolysis method of the present invention preferably includes a neutralization step (STEP 2) in which lithium hydroxide (LiOH) is added to the acid solution to neutralize the acid solution and obtain a neutralized solution. Furthermore, the membrane electrolysis method of the present invention preferably includes a solvent extraction step (STEP 3) in which at least one metal, excluding lithium, among the metals contained in the active material powder is separated from the neutralized solution by solvent extraction, and an aqueous lithium salt solution is obtained as the residual solution from the solvent extraction. In the solvent extraction, manganese, cobalt, and nickel, excluding lithium, among the valuable metals, are each solvent extracted separately, or iron and aluminum are separated and removed as their respective metal salt aqueous solutions 2, thereby obtaining a first aqueous lithium salt solution. When hydrochloric acid is used in the acid dissolution in STEP 1, the lithium salt contained in the first aqueous lithium salt solution becomes lithium chloride.
[0017] The method for membrane electrolysis of a lithium salt aqueous solution of the present invention includes a cathode chamber introduction step (STEP 4-1) of introducing at least one selected from the group consisting of a first lithium hydroxide aqueous solution having a lithium hydroxide concentration of 10 mass% or less and water into a cathode chamber of a membrane electrolysis device, and a membrane electrolysis step (STEP 4-2) of performing membrane electrolysis until the lithium hydroxide concentration in the cathode chamber reaches a predetermined concentration. In FIG. 1, STEP 4-1 and STEP 4-2 are shown as STEP 4. The cathode chamber introduction step and membrane electrolysis step can be performed using, for example, an electrolytic cell 11 shown in FIG. 2. The water may include at least one selected from the group consisting of industrial water, pure water, and tap water.
[0018] The electrolytic cell 11 is provided with an anode plate 12 on one of its inner surfaces and a cathode plate 13 on the inner surface opposite the anode plate 12, the anode plate 12 being connected to an anode 14 of a power supply, and the cathode plate 13 being connected to a cathode 15 of the power supply. The electrolytic cell 11 is also partitioned by an ion exchange membrane 16 into an anode chamber 17 containing the anode plate 12 and a cathode chamber 18 containing the cathode plate 13.
[0019] In the electrolytic cell 11, when electrolysis is carried out by supplying, for example, lithium chloride as the first lithium salt aqueous solution to the anode chamber 17, chloride ions are converted into chlorine gas (Cl) on the anode plate 12. 2 ), while the lithium ions migrate through the ion exchange membrane 16 to the cathode chamber 18.
[0020] In the cathode chamber 18, water (H 2 O) is hydroxide ion (OH - ) and hydrogen ions (H + ) and hydrogen ions are ionized into hydrogen gas (H 2), while hydroxide ions combine with lithium to produce a second lithium hydroxide aqueous solution 3. As the lithium hydroxide concentration in the second lithium hydroxide aqueous solution 3 increases, hydroxide ions tend to migrate toward the anode chamber 17, resulting in a decrease in membrane electrolysis efficiency. Furthermore, lithium hydroxide is more likely to deposit in and on the ion exchange membrane 16. If lithium hydroxide deposits, the ion exchange membrane 16 is damaged, causing various adverse effects on the membrane electrolysis process. Therefore, at least one selected from the group consisting of a first lithium hydroxide aqueous solution having a lithium hydroxide concentration of 10% by mass or less and water is introduced into the cathode chamber 18 at a flow rate sufficient to prevent a difference in lithium hydroxide concentration between the inlet and outlet of the cathode chamber 18. As a result, lithium ions transferred from the anode chamber 17 are rapidly diffused from the surface of the ion exchange membrane 16 on the cathode chamber 18 side, and lithium hydroxide is not deposited in and on the ion exchange membrane 16. The cathode chamber introduction process and the membrane electrolysis process may be repeated sequentially or simultaneously. The cathode chamber introduction step and the membrane electrolysis step are preferably repeated sequentially. In a typical ion exchange membrane electrolysis method for salt, a saline solution to be subjected to membrane electrolysis is continuously introduced into an electrolysis chamber, and the sodium hydroxide concentration at the inlet of the electrolysis chamber is about 28 mass %, but the concentration at the outlet rises to 32 to 35 mass %.
[0021] When the lithium salt aqueous solution to be subjected to the membrane electrolysis step contains sulfate ions, sulfuric acid can be obtained in the anode chamber 17. When the lithium salt aqueous solution to be subjected to the membrane electrolysis step contains nitrate ions, nitric acid can be obtained in the anode chamber 17. That is, mineral acid 4 can be obtained in the membrane electrolysis step, and this mineral acid 4 can be used to dissolve the active material powder 1 in STEP 1.
[0022] The second lithium hydroxide aqueous solution 3 obtained in the membrane electrolysis step is crystallized in STEP 5 to form lithium hydroxide monohydrate (LiOH.H 2 O), and by carbonating in STEP 6, lithium carbonate (Li 2 CO 3 The carbonation can be carried out by converting the second lithium hydroxide aqueous solution 3 into carbon dioxide gas (CO 2) can be reacted with
[0023] In this embodiment, a part of the second lithium hydroxide aqueous solution 3 obtained in the membrane electrolysis step may be diluted with water to obtain the first lithium hydroxide aqueous solution. Furthermore, a part of the second lithium hydroxide aqueous solution 3 may be used as at least one selected from the group consisting of the lithium hydroxide added to the acid solution in STEP 2 and the alkali used in the solvent extraction in STEP 3.
[0024] When the second lithium hydroxide aqueous solution 3 is used for solvent extraction in STEP 3, the second lithium hydroxide aqueous solution 3 is added to the extraction solvent. Since the extraction solvent used for solvent extraction in STEP 3 is a cation exchange extractant, its liquid property becomes acidic with continued use, and the extraction rate decreases. However, by adding the second lithium hydroxide aqueous solution 3, the decrease in the extraction rate can be suppressed.
[0025] When the second lithium hydroxide aqueous solution 3 is used for solvent extraction in STEP 3, the second lithium hydroxide aqueous solution 3 can be used for at least one of the solvent extractions of manganese, cobalt, and nickel, which are performed separately.
[0026] The electricity used in the membrane electrolysis step may include, for example, at least one renewable energy selected from the group consisting of electricity obtained by solar power generation and electricity obtained by wind power generation.
[0027] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples.
[0028] [Example 1] Using the membrane electrolysis device shown in Figure 2, membrane electrolysis was carried out until the lithium hydroxide concentration of the lithium hydroxide aqueous solution in the cathode chamber 18 changed from 2 mass % to 8 mass %. The current efficiency was 67%.
[0029] [Example 2] Membrane electrolysis was carried out in the same manner as in Example 1, except that the lithium hydroxide concentration of the lithium hydroxide aqueous solution in the cathode chamber 18 was kept constant at 5 mass %. The current efficiency was 64%.
[0030] [Example 3] Membrane electrolysis was carried out in the same manner as in Example 1, except that the lithium hydroxide concentration of the lithium hydroxide aqueous solution in the cathode chamber 18 was kept constant at 8 mass %. The current efficiency was 53%.
[0031] REFERENCE SIGNS LIST 1... active material powder, 2... metal salt aqueous solution, 3... lithium hydroxide aqueous solution, 4... mineral acid, 11... membrane electrolytic cell, 16... ion exchange membrane, 17... anode chamber, 18... cathode chamber
Claims
1. A method for membrane electrolysis of an aqueous lithium salt solution, comprising: a cathode chamber introduction step of introducing at least one selected from the group consisting of a first aqueous lithium hydroxide solution having a lithium hydroxide concentration of 10 mass% or less and water into a cathode chamber of a membrane electrolysis device; and a membrane electrolysis step of carrying out membrane electrolysis until the lithium hydroxide concentration in the cathode chamber reaches a predetermined concentration.
2. A method for membrane electrolysis of an aqueous lithium salt solution according to claim 1, characterized in that the cathode chamber introduction step and the membrane electrolysis step are repeated in sequence.
3. A method for membrane electrolysis of a lithium salt aqueous solution as described in claim 1, characterized in that a part of the second lithium hydroxide aqueous solution obtained in the membrane electrolysis step is diluted with water to obtain the first lithium hydroxide aqueous solution.
4. A method for membrane electrolysis of an aqueous lithium salt solution according to claim 1, further comprising: an acid dissolution step of dissolving an active material powder obtained by pretreating waste lithium ion batteries in a mineral acid to obtain an acid solution of the active material containing at least lithium; a neutralization step of adding lithium hydroxide to the acid solution to neutralize the acid solution to obtain a neutralized solution; and a solvent extraction step of separating at least one metal, excluding lithium, from the neutralized solution by solvent extraction, among the metals contained in the active material powder, and obtaining an aqueous lithium salt solution as a residual solution of the solvent extraction.
5. A method for membrane electrolysis of an aqueous lithium salt solution as described in claim 4, characterized in that a part of the second aqueous lithium hydroxide solution obtained in the membrane electrolysis step is utilized in at least one step selected from the group consisting of the neutralization step and the solvent extraction step, and the mineral acid obtained in the membrane electrolysis step is utilized in the acid dissolution step.
6. A method for membrane electrolysis of a lithium salt aqueous solution according to any one of claims 1 to 5, characterized in that the electricity used for the membrane electrolysis includes electricity obtained from renewable energy.
7. A method for membrane electrolysis of a lithium salt aqueous solution according to claim 6, characterized in that the electricity obtained from the renewable energy source includes at least one selected from the group consisting of electricity obtained from solar power generation and electricity obtained from wind power generation.
Citation Information
Patent Citations
Processing of lithium-containing materials
JP2015531826A
Electrochemical hydroxide systems and methods using metal oxidation
JP2017075398A
Positive electrode for alkaline water electrolysis
WO2015064644A1
Apparatus for producing lithium hydroxide and method for producing lithium hydroxide
WO2016132491A1
Method for fixing carbon dioxide, method for producing fixed carbon dioxide, and apparatus for fixing carbon dioxide
WO2021149281A1