Covering material for power storage device, production method for covering material and power storage device
The laminate exterior material with a treated metal foil layer addresses the challenges of shape diversity and weight reduction in power storage devices by enhancing moldability and formability, improving energy density and flexibility.
Patent Information
- Application Number
- PCT/JP2024/014601
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-10
- Filing Date
- 2024-04-10
- Publication Date
- 2024-10-17
AI Technical Summary
Conventional metal exterior materials for power storage devices face challenges in accommodating diverse shapes and reducing weight, leading to issues such as cracks and pinholes during the molding process, which affects the energy density and moldability of these devices.
A laminate exterior material composed of a base material layer, a metal foil layer, and a heat-fusible resin layer, where the metal foil layer's surface is treated to have specific root mean square gradient, kurtosis, and skewness values at a laser wavelength of 408 nm, enhancing moldability and formability.
The treated laminate exterior material achieves improved moldability and formability, reducing the likelihood of cracks and pinholes, thereby increasing the energy density and flexibility of power storage devices.
Smart Images

Figure JP2024014601_17102024_PF_FP_ABST
Abstract
Description
Exterior material for power storage device, manufacturing method thereof, and power storage device
[0001] The present disclosure relates to an exterior material for an electricity storage device, a method for producing the same, and an electricity storage device.
[0002] Various types of electricity storage devices have been developed, and in all of them, exterior materials are essential components for sealing electricity storage device elements such as electrodes and electrolytes. Conventionally, metal exterior materials have been widely used as exterior materials for electricity storage devices.
[0003] Meanwhile, in recent years, with the increasing performance of electric vehicles, hybrid electric vehicles, personal computers, cameras, mobile phones, etc., there has been a demand for electricity storage devices to have a variety of shapes as well as to be thinner and lighter in weight. However, the metallic exterior materials for electricity storage devices that have been widely used in the past have the drawbacks of being difficult to keep up with the diversification of shapes and also having limitations on how much they can be made lighter.
[0004] Therefore, a film-like laminate in which a base material layer, a metal foil layer, an adhesive layer, and a heat-sealable resin layer are laminated in this order has been proposed as an exterior material for an electricity storage device that can be easily processed into a variety of shapes and can be made thinner and lighter (see, for example, Patent Document 1).
[0005] In such an electrical storage device packaging material, a recess is generally formed by cold forming, and electrical storage device elements such as electrodes and electrolyte are placed in the space formed by the recess, and a heat-sealable resin layer is heat-sealed to obtain an electrical storage device in which the electrical storage device elements are housed inside the electrical storage device packaging material.
[0006] Japanese Patent Application Laid-Open No. 2008-287971
[0007] From the viewpoint of further increasing the energy density of the electricity storage device, it is required to form a deep recess in the film-like packaging material to accommodate the electricity storage device element. However, when the recess is formed by molding the film-like packaging material, there is a problem that cracks and pinholes are likely to occur.
[0008] A primary object of the present disclosure is to provide an exterior packaging material for an electricity storage device that is composed of a laminate having, from the outside in order, at least a base material layer, a metal foil layer, and a heat-sealable resin layer, and that has excellent formability.
[0009] The inventors of the present disclosure conducted extensive research to solve the above-mentioned problems. As a result, they found that, in an electrical storage device packaging material composed of a laminate including, from the outside, at least a substrate layer, a metal foil layer, and a heat-sealable resin layer, by setting the root-mean-square gradient Sdq at a laser wavelength of 408 nm, measured using a laser microscope, for at least one surface of the metal foil layer to a predetermined value or less, an electrical storage device packaging material with excellent formability can be obtained. They also found that by setting the kurtosis Sku at a laser wavelength of 408 nm, measured using a laser microscope, for at least one surface of the metal foil layer to a predetermined value or less, an electrical storage device packaging material with excellent formability can be obtained. Furthermore, they found that by setting the skewness Ssk at a laser wavelength of 408 nm, measured using a laser microscope, for at least one surface of the metal foil layer to a predetermined range, an electrical storage device packaging material with excellent formability can be obtained.
[0010] The present disclosure was completed based on these new findings and through further investigation.
[0011] That is, a first aspect of the present disclosure provides the following invention: An exterior packaging material for an electricity storage device, which is composed of a laminate including, in order from the outside, at least a base material layer, a metal foil layer, and a heat-sealable resin layer, wherein the root-mean-square gradient Sdq of at least one surface of the metal foil layer at a laser wavelength of 408 nm measured using a laser microscope is 0.28 or less.
[0012] In the first aspect of the present disclosure, the packaging material for an electricity storage device may not include a base material layer. That is, the first aspect of the present disclosure may be a packaging material for an electricity storage device that is composed of a laminate including, in order from the outside, at least a metal foil layer and a heat-sealable resin layer, and in which the root-mean-square gradient Sdq of at least one surface of the metal foil layer at a laser wavelength of 408 nm, measured using a laser microscope, is 0.28 or less.
[0013] A second aspect of the present disclosure provides the following invention: An exterior packaging material for an electricity storage device, which is composed of a laminate including, in order from the outside, at least a base material layer, a metal foil layer, and a heat-sealable resin layer, wherein the kurtosis Sku of at least one surface of the metal foil layer is 4.00 or less at a laser wavelength of 408 nm, as measured using a laser microscope.
[0014] In a second aspect of the present disclosure, the packaging material for an electricity storage device may not include a base material layer. That is, the second aspect of the present disclosure may be a packaging material for an electricity storage device that is composed of a laminate including, in order from the outside, at least a metal foil layer and a heat-sealable resin layer, and that has a kurtosis Sku of 4.00 or less at a laser wavelength of 408 nm measured using a laser microscope for at least one surface of the metal foil layer.
[0015] A third aspect of the present disclosure provides the following invention: An exterior packaging material for an electricity storage device, which is composed of a laminate including, in order from the outside, at least a base material layer, a metal foil layer, and a heat-sealable resin layer, wherein the skewness Ssk of at least one surface of the metal foil layer is −0.25 or more and 0.25 or less at a laser wavelength of 408 nm, as measured using a laser microscope.
[0016] In a third aspect of the present disclosure, the packaging material for an electricity storage device may not include a base material layer. That is, the third aspect of the present disclosure may be a packaging material for an electricity storage device that is composed of a laminate including, in order from the outside, at least a metal foil layer and a heat-sealable resin layer, and that has a skewness Ssk of −0.25 or more and 0.25 or less at a laser wavelength of 408 nm, measured with a laser microscope, for at least one surface of the metal foil layer.
[0017] According to the present disclosure, it is possible to provide an exterior packaging material for an electricity storage device that is composed of a laminate including, from the outside, at least a base material layer, a metal foil layer, and a heat-sealable resin layer, and that has excellent formability. Furthermore, according to the present disclosure, it is possible to provide an exterior packaging material for an electricity storage device that is composed of a laminate including, from the outside, at least a metal foil layer and a heat-sealable resin layer, and that has excellent formability. Furthermore, according to the present disclosure, it is also possible to provide a method for manufacturing these exterior packaging materials for an electricity storage device, and an electricity storage device that uses these exterior packaging materials for an electricity storage device.
[0018] Fig. 1 is a schematic diagram showing an example of the cross-sectional structure of an exterior material for an electricity storage device according to the present disclosure. Fig. 2 is a schematic diagram showing an example of the cross-sectional structure of an exterior material for an electricity storage device according to the present disclosure. Fig. 3 is a schematic diagram showing an example of the cross-sectional structure of an exterior material for an electricity storage device according to the present disclosure. Fig. 4 is a schematic diagram for explaining a method of housing an electricity storage device element in a package formed from an exterior material for an electricity storage device according to the present disclosure.
[0019] The packaging material for an electricity storage device according to a first aspect of the present disclosure is composed of a laminate including, in order from the outside, at least a base material layer, a metal foil layer, and a heat-sealable resin layer, and the root-mean-square gradient Sdq of at least one surface of the metal foil layer at a laser wavelength of 408 nm, as measured using a laser microscope, is 0.28 or less. As described above, in the first aspect of the present disclosure, the packaging material for an electricity storage device may not include a base material layer.
[0020] A packaging material for an electricity storage device according to a second aspect of the present disclosure is composed of a laminate including, in order from the outside, at least a base material layer, a metal foil layer, and a heat-sealable resin layer, and the surface of at least one side of the metal foil layer has a kurtosis Sku of 4.00 or less at a laser wavelength of 408 nm measured using a laser microscope. As described above, in the second aspect of the present disclosure, the packaging material for an electricity storage device may not include a base material layer.
[0021] A packaging material for an electricity storage device according to a third aspect of the present disclosure is composed of a laminate including, in order from the outside, at least a base material layer, a metal foil layer, and a heat-sealable resin layer, and the skewness Ssk of at least one surface of the metal foil layer at a laser wavelength of 408 nm, measured using a laser microscope, is not less than −0.25 and not more than 0.25. As described above, in the third aspect of the present disclosure, the packaging material for an electricity storage device may not include a base material layer.
[0022] The exterior packaging material for an electricity storage device of the present disclosure will be described in detail below. In the following description, matters specific to the first, second, or third aspect will be clearly indicated as to which aspect they relate to, and matters common to the first, second, and third aspects will be described without any specific indication, and will simply be described as relating to the present disclosure. In this specification, a numerical range indicated by "to" means "greater than or equal to" or "less than or equal to." For example, the expression "2 to 15 mm" means 2 mm or greater and 15 mm or less. In the numerical ranges described in stages in this disclosure, the upper or lower limit value described in a certain numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. Furthermore, separately described upper and lower limits, upper and lower limits, or lower and lower limits may each be combined to form a numerical range. Furthermore, in the numerical ranges described in this disclosure, the upper or lower limit value described in a certain numerical range may be replaced with a value shown in the examples.
[0023] In the case of the exterior packaging material for an electricity storage device, the MD (machine direction) and TD (transverse direction) of the metal foil layer 3 described below can usually be determined during the manufacturing process. For example, when the metal foil layer 3 is composed of a metal foil such as an aluminum alloy foil or a stainless steel foil, linear lines called rolling marks are formed on the surface of the metal foil in the rolling direction (RD) of the metal foil. Since the rolling marks extend along the rolling direction, the rolling direction of the metal foil can be determined by observing the surface of the metal foil. Furthermore, during the manufacturing process of a laminate, the MD of the laminate usually coincides with the RD of the metal foil, so the MD of the laminate can be determined by observing the surface of the metal foil of the laminate and identifying the rolling direction (RD) of the metal foil. Furthermore, since the TD of the laminate is perpendicular to the MD of the laminate, the TD of the laminate can also be identified.
[0024] Furthermore, when the MD of an electrical storage device packaging material cannot be determined due to rolling marks on a metal foil such as an aluminum alloy foil or a stainless steel foil, it can be determined by the following method. One method for determining the MD of an electrical storage device packaging material is to observe the cross section of the heat-sealable resin layer of the electrical storage device packaging material using an electron microscope to confirm the sea-island structure. In this method, the direction parallel to the cross section in which the average diameter of the island shapes in the direction perpendicular to the thickness direction of the heat-sealable resin layer is largest can be determined as the MD. Specifically, the sea-island structure is confirmed by observing, using an electron microscope, a cross section in the longitudinal direction of the heat-sealable resin layer and each cross section in a direction angled 10 degrees from the direction parallel to the longitudinal cross section (a total of 10 cross sections). Next, the shape of each individual island is observed in each cross section. For each island shape, the linear distance connecting the leftmost end in the direction perpendicular to the thickness direction of the heat-sealable resin layer to the rightmost end in the perpendicular direction is defined as the diameter y. For each cross section, the average of the 20 largest diameters y of the island shapes is calculated. The direction parallel to the cross section with the largest average diameter y of the island shapes is determined to be the MD.
[0025] 1. Laminated Structure of the Electricity Storage Device Exterior Material As shown in FIG. 1 , the electricity storage device exterior material 10 of the present disclosure is composed of a laminate including, from the outside in, a base material layer 1, a metal foil layer 3, and a heat-sealable resin layer 4. In the electricity storage device exterior material 10, the base material layer 1 is the outermost layer, and the heat-sealable resin layer 4 is the innermost layer. When assembling an electricity storage device using the electricity storage device exterior material 10 and an electricity storage device element, the heat-sealable resin layers 4 of the electricity storage device exterior material 10 are placed opposite each other, and the peripheries are heat-sealed to form a space, in which the electricity storage device element is housed. In the laminate constituting the electricity storage device exterior material 10 of the present disclosure, with the metal foil layer 3 as the reference, the heat-sealable resin layer 4 side relative to the metal foil layer 3 is the inner side, and the base material layer 1 side relative to the metal foil layer 3 is the outer side. The packaging material 10 for an electricity storage device according to the present disclosure may be composed of a laminate including, in this order, a metal foil layer 3 and a heat-sealable resin layer 4. In this case, the side of the metal foil layer 3 opposite to the heat-sealable resin layer 4 is the outermost layer, and the heat-sealable resin layer 4 is the innermost layer.
[0026] As shown in Figures 2 to 4, for example, the packaging material 10 for an electricity storage device may have an adhesive layer 2 between the base material layer 1 and the metal foil layer 3, if necessary, for the purpose of increasing the adhesion between these layers. Furthermore, as shown in Figures 3 and 4, for example, the packaging material 10 may have an adhesive layer 5 between the metal foil layer 3 and the heat-sealable resin layer 4, if necessary, for the purpose of increasing the adhesion between these layers. Furthermore, as shown in Figure 4, a surface coating layer 6 or the like may be provided on the outer side of the base material layer 1 (the side opposite to the heat-sealable resin layer 4 side), if necessary.
[0027] The thickness of the laminate constituting the electrical storage device exterior material 10 is not particularly limited, but from the viewpoint of cost reduction, improvement of energy density, etc., examples of the thickness include about 300 μm or less, preferably about 250 μm or less, about 210 μm or less, about 190 μm or less, about 180 μm or less, about 155 μm or less, and about 120 μm or less. Furthermore, from the viewpoint of maintaining the function of the electrical storage device exterior material to protect the electrical storage device elements, the thickness of the laminate constituting the electrical storage device exterior material 10 is preferably about 35 μm or more, about 45 μm or more, about 60 μm or more, about 155 μm or more, and about 190 μm or more. Furthermore, preferred ranges for the laminate constituting the exterior packaging material 10 for an electricity storage device are, for example, about 35 to 300 μm, about 35 to 250 μm, about 35 to 210 μm, about 35 to 190 μm, about 35 to 180 μm, about 35 to 155 μm, about 35 to 120 μm, about 45 to 300 μm, about 45 to 250 μm, about 45 to 210 μm, about 45 to 190 μm, about 45 to 180 μm, about 45 to 155 μm, about 45 to 120 μm, about 60 to 300 μm, about 60 to 250 μm, and about 60 to 300 μm. Examples of the thickness include about 210 μm, about 60 to 190 μm, about 60 to 180 μm, about 60 to 155 μm, about 60 to 120 μm, about 155 to 300 μm, about 155 to 250 μm, about 155 to 210 μm, about 155 to 190 μm, about 155 to 180 μm, about 190 to 300 μm, about 190 to 250 μm, and about 190 to 210 μm. In particular, when making the power storage device lightweight and thin, about 60 to 155 μm is preferred, and when improving formability, about 155 to 190 μm is preferred.
[0028] In the electrical storage device packaging material 10, the ratio of the total thickness of the base material layer 1, the adhesive layer 2 (if provided as needed), the metal foil layer 3, the adhesive layer 5 (if provided as needed), the heat-sealable resin layer 4, and the surface coating layer 6 (if provided as needed) to the thickness (total thickness) of the laminate constituting the electrical storage device packaging material 10 is preferably 90% or more, more preferably 95% or more, and even more preferably 98% or more. As a specific example, when the electrical storage device packaging material 10 of the present disclosure includes the base material layer 1, the adhesive layer 2, the metal foil layer 3, the adhesive layer 5, and the heat-sealable resin layer 4, the ratio of the total thickness of these layers to the thickness (total thickness) of the laminate constituting the electrical storage device packaging material 10 is preferably 90% or more, more preferably 95% or more, and even more preferably 98% or more. Furthermore, even when the electrical storage device packaging material 10 of the present disclosure is a laminate including a substrate layer 1, an adhesive layer 2, a metal foil layer 3, and a heat-sealable resin layer 4, the ratio of the total thickness of these layers to the thickness (total thickness) of the laminate constituting the electrical storage device packaging material 10 can be, for example, 80% or more, preferably 90% or more, more preferably 95% or more, and even more preferably 98% or more.
[0029] 2. Layers forming the packaging material for an electricity storage device [Substrate layer 1] In the present disclosure, the substrate layer 1 is a layer provided for the purpose of exhibiting the function as a substrate of the packaging material for an electricity storage device, etc. The substrate layer 1 is located on the outer layer side of the packaging material for an electricity storage device.
[0030] There are no particular limitations on the material forming the substrate layer 1, as long as it functions as a substrate, i.e., has at least insulating properties. The substrate layer 1 can be formed using, for example, a resin, which may contain an additive described below.
[0031] When the substrate layer 1 is formed of a resin, the substrate layer 1 can be formed of, for example, a resin film. When the substrate layer 1 is formed of a resin film, a pre-formed resin film may be used as the substrate layer 1 when the substrate layer 1 is laminated with a metal foil layer 3 or the like to produce the electrical storage device packaging material 10 of the present disclosure. Alternatively, the resin forming the substrate layer 1 may be formed into a film on the surface of the metal foil layer 3 or the like by extrusion molding, coating, or the like to form the substrate layer 1 formed of a resin film. The resin film may be an unstretched film or a stretched film. Examples of stretched films include uniaxially stretched films and biaxially stretched films, with biaxially stretched films being preferred. Examples of stretching methods for forming biaxially stretched films include sequential biaxial stretching, inflation, and simultaneous biaxial stretching. Examples of methods for applying the resin include roll coating, gravure coating, and extrusion coating.
[0032] Examples of resins that form the base layer 1 include polyester, polyamide, polyolefin, epoxy resin, acrylic resin, fluororesin, polyurethane, silicone resin, and phenolic resin, as well as modified versions of these resins. The resin that forms the base layer 1 may also be a copolymer of these resins, a modified version of the copolymer, or a mixture of these resins.
[0033] The base layer 1 preferably contains these resins as the main component, and more preferably contains polyester or polyamide as the main component. Here, "main component" means that the content of the resin component contained in the base layer 1 is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, and even more preferably 99% by mass or more. For example, "the base layer 1 contains polyester or polyamide as the main component" means that the content of polyester or polyamide among the resin components contained in the base layer 1 is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, and even more preferably 99% by mass or more.
[0034] Of these, polyester and polyamide are preferred as the resin for forming the base layer 1.
[0035] Specific examples of polyesters include polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, polyethylene isophthalate, and copolymer polyesters. Examples of copolymer polyesters include copolymer polyesters in which ethylene terephthalate is the main repeating unit. Specific examples include copolymer polyesters in which ethylene terephthalate is the main repeating unit and is polymerized with ethylene isophthalate (hereinafter abbreviated as polyethylene (terephthalate / isophthalate)), polyethylene (terephthalate / adipate), polyethylene (terephthalate / sodium sulfoisophthalate), polyethylene (terephthalate / sodium isophthalate), polyethylene (terephthalate / phenyl-dicarboxylate), and polyethylene (terephthalate / decanedicarboxylate). These polyesters may be used alone or in combination of two or more.
[0036] Specific examples of polyamides include aliphatic polyamides such as nylon 6, nylon 66, nylon 610, nylon 12, nylon 46, and copolymers of nylon 6 and nylon 66; hexamethylenediamine-isophthalic acid-terephthalic acid copolymer polyamides such as nylon 6I, nylon 6T, nylon 6IT, and nylon 6I6T (where I represents isophthalic acid and T represents terephthalic acid) containing structural units derived from terephthalic acid and / or isophthalic acid; and aromatic polyamides such as polyamide MXD6 (polymetaxylylene adipamide); alicyclic polyamides such as polyamide PACM6 (polybis(4-aminocyclohexyl)methane adipamide); polyamides copolymerized with a lactam component or an isocyanate component such as 4,4'-diphenylmethane-diisocyanate; polyesteramide copolymers and polyetheresteramide copolymers, which are copolymers of copolymerized polyamides with polyesters or polyalkylene ether glycols; and polyamides such as copolymers of these copolymers. These polyamides may be used alone or in combination of two or more.
[0037] The base layer 1 preferably includes at least one of a polyester film, a polyamide film, and a polyolefin film, and preferably includes at least one of a stretched polyester film, a stretched polyamide film, and a stretched polyolefin film, and more preferably includes at least one of a stretched polyethylene terephthalate film, a stretched polybutylene terephthalate film, a stretched nylon film, and a stretched polypropylene film, and even more preferably includes at least one of a biaxially oriented polyethylene terephthalate film, a biaxially oriented polybutylene terephthalate film, a biaxially oriented nylon film, and a biaxially oriented polypropylene film.
[0038] The base material layer 1 may be a single layer or may be composed of two or more layers. When the base material layer 1 is composed of two or more layers, the base material layer 1 may be a laminate in which resin films are laminated with an adhesive or the like, or a laminate of resin films formed by co-extrusion of resins into two or more layers. Furthermore, a laminate of resin films formed by co-extrusion of resins into two or more layers may be used as the base material layer 1 without being stretched, or may be uniaxially or biaxially stretched to form the base material layer 1.
[0039] Specific examples of the laminate of two or more resin films in the base layer 1 include a laminate of a polyester film and a nylon film, a laminate of two or more nylon films, and a laminate of two or more polyester films. A laminate of a stretched nylon film and a stretched polyester film, a laminate of two or more stretched nylon films, or a laminate of two or more stretched polyester films is preferred. For example, when the base layer 1 is a laminate of two resin films, a laminate of a polyester resin film and a polyester resin film, a laminate of a polyamide resin film and a polyamide resin film, or a laminate of a polyester resin film and a polyamide resin film is preferred. A laminate of a polyethylene terephthalate film and a polyethylene terephthalate film, a laminate of a nylon film and a nylon film, or a laminate of a polyethylene terephthalate film and a nylon film is more preferred. Furthermore, since polyester resins are less likely to discolor when an electrolytic solution adheres to their surface, it is preferred that the polyester resin film be located as the outermost layer of the base layer 1 when the base layer 1 is a laminate of two or more resin films. In the laminate of a polyester resin film and a polyamide resin film, preferred ranges of the thickness of the polyester resin film are about 2 to 33 μm, about 2 to 28 μm, about 2 to 23 μm, about 2 to 18 μm, about 2 to 11 μm, about 2 to 8 μm, about 10 to 33 μm, about 10 to 28 μm, about 10 to 23 μm, about 10 to 18 μm, about 18 to 33 μm, and about 18 to 28 μm. and about 18 to 23 μm. Preferred ranges of the thickness of the polyamide resin film include about 2 to 33 μm, about 2 to 28 μm, about 2 to 23 μm, about 2 to 18 μm, about 2 to 11 μm, about 2 to 8 μm, about 10 to 33 μm, about 10 to 28 μm, about 10 to 23 μm, about 10 to 18 μm, about 18 to 33 μm, about 18 to 28 μm, and about 18 to 23 μm.
[0040] When the base layer 1 is a laminate of two or more resin film layers, the two or more resin film layers may be laminated via an adhesive. Examples of preferred adhesives include those similar to those exemplified for adhesive layer 2 described below. The method for laminating two or more resin film layers is not particularly limited, and known methods can be used, such as dry lamination, sandwich lamination, extrusion lamination, and thermal lamination, with dry lamination being preferred. When laminating using the dry lamination method, it is preferable to use a polyurethane adhesive as the adhesive. In this case, the thickness of the adhesive may be, for example, about 2 to 5 μm. Alternatively, an anchor coat layer may be formed on the resin film before lamination. Examples of the anchor coat layer include those similar to those exemplified for adhesive layer 2 described below. In this case, the thickness of the anchor coat layer may be, for example, about 0.01 to 1.0 μm.
[0041] Furthermore, additives such as lubricants, flame retardants, antiblocking agents, antioxidants, light stabilizers, tackifiers, antistatic agents, and colorants may be present on at least one of the surface and the interior of the base material layer 1. Only one type of additive may be used, or two or more types may be mixed and used.
[0042] In the present disclosure, from the viewpoint of improving the formability of the exterior material for an electrical storage device, it is preferable that a lubricant be present on at least one of the surface and the interior of the base material layer 1. The lubricant is not particularly limited, but preferably an amide-based lubricant is used. Specific examples of amide-based lubricants include saturated fatty acid amides, unsaturated fatty acid amides, substituted amides, methylolamides, saturated fatty acid bisamides, unsaturated fatty acid bisamides, fatty acid ester amides, and aromatic bisamides. Specific examples of saturated fatty acid amides include lauric acid amide, palmitic acid amide, stearic acid amide, behenic acid amide, and hydroxystearic acid amide. Specific examples of unsaturated fatty acid amides include oleic acid amide and erucic acid amide. Specific examples of substituted amides include N-oleyl palmitic acid amide, N-stearyl stearic acid amide, N-stearyl oleic acid amide, N-oleyl stearic acid amide, and N-stearyl erucic acid amide. Specific examples of methylolamides include methylol stearic acid amide. Specific examples of saturated fatty acid bisamides include methylene bisstearic acid amide, ethylene biscapric acid amide, ethylene bislauric acid amide, ethylene bisstearic acid amide, ethylene bishydroxystearic acid amide, ethylene bisbehenic acid amide, hexamethylene bisstearic acid amide, hexamethylene bisbehenic acid amide, hexamethylene hydroxystearic acid amide, N,N'-distearyl adipamide, N,N'-distearyl sebacic acid amide, etc. Specific examples of unsaturated fatty acid bisamides include ethylene bisoleic acid amide, ethylene biserucic acid amide, hexamethylene bisoleic acid amide, N,N'-dioleyl adipamide, N,N'-dioleyl sebacic acid amide, etc. Specific examples of fatty acid ester amides include stearamidoethyl stearate, etc. Specific examples of aromatic bisamides include m-xylylene bisstearic acid amide, m-xylylene bishydroxystearic acid amide, and N,N'-distearylisophthalic acid amide.The lubricant may be used alone or in combination of two or more kinds, and it is preferable to use a combination of two or more kinds.
[0043] When a lubricant is present on the surface of the base layer 1, the amount of the lubricant is not particularly limited, but may be, for example, about 3 mg / m 2 or more, preferably about 4 mg / m 2 Above, about 5mg / m 2 The amount of lubricant present on the surface of the base layer 1 is, for example, about 15 mg / m 2 or less, preferably about 14 mg / m 2 Below, about 10mg / m 2 The preferred range of the amount of lubricant present on the surface of the base layer 1 is 3 to 15 mg / m 2 Degree, 3-14mg / m 2 Degree, 3-10mg / m 2 Degree, 4-15mg / m 2 Degree, 4-14mg / m 2 degree, 4-10mg / m 2 degree, 5-15mg / m 2 Degree, 5-14mg / m 2 degree, 5-10mg / m 2 The degree of
[0044] The lubricant present on the surface of the base layer 1 may be a lubricant exuded from the resin constituting the base layer 1, or a lubricant applied to the surface of the base layer 1.
[0045] The thickness of the substrate layer 1 is not particularly limited as long as it functions as a substrate, but may be, for example, about 3 μm or more, preferably about 10 μm or more, and may be, for example, about 100 μm or less, about 90 μm or less, about 70 μm or less, or about 50 μm or less, preferably about 35 μm or less, 11 μm or less, or 8 μm or less. In addition, preferred ranges of the thickness of the base layer 1 include about 3 to 100 μm, about 3 to 90 μm, about 3 to 70 μm, about 3 to 50 μm, about 3 to 35 μm, about 3 to 11 μm, about 3 to 8 μm, about 10 to 100 μm, about 10 to 90 μm, about 10 to 70 μm, about 10 to 50 μm, about 10 to 35 μm, and about 10 to 11 μm. In particular, when making the power storage device lighter and thinner, about 3 to 35 μm, about 3 to 11 μm, and about 3 to 8 μm are preferred, and when improving formability, about 35 to 50 μm is preferred. When the base layer 1 is a laminate of two or more resin films, the thickness of the resin films constituting each layer is not particularly limited, but can be, for example, about 2 μm or more, preferably about 10 μm or more, or about 18 μm or more. The thickness of the resin film constituting each layer is, for example, about 33 μm or less, preferably about 28 μm or less, about 23 μm or less, about 18 μm or less, 11 μm or less, or 8 μm or less. Preferred ranges for the thickness of the resin film constituting each layer include about 2 to 33 μm, about 2 to 28 μm, about 2 to 23 μm, about 2 to 18 μm, about 2 to 11 μm, about 2 to 8 μm, about 10 to 33 μm, about 10 to 28 μm, about 10 to 23 μm, about 10 to 18 μm, about 18 to 33 μm, about 18 to 28 μm, and about 18 to 23 μm.
[0046] The base material layer 1 contains a colorant, which allows the electrical storage device packaging material to be colored. Known colorants such as pigments and dyes can be used as the colorant. Only one type of colorant may be used, or two or more types may be mixed together.
[0047] The type of pigment is not particularly limited as long as it does not impair the function as a substrate of the substrate layer 1. Examples of organic pigments include azo-based, phthalocyanine-based, quinacridone-based, anthraquinone-based, dioxazine-based, indigothioindigo-based, perinone-perylene-based, isoindolenine-based, and benzimidazolone-based pigments, while examples of inorganic pigments include carbon black-based, titanium oxide-based, cadmium-based, lead-based, chromium oxide-based, and iron-based pigments, and other examples include finely powdered mica and fish scale foil.
[0048] Among colorants, carbon black is preferred for making the exterior material for an electricity storage device black, and mica is preferred from the viewpoint of dissipating heat generated from the electricity storage device.
[0049] The average particle size of the pigment is not particularly limited and may be, for example, about 0.03 to 5 μm, and preferably about 0.05 to 2 μm. The average particle size of the pigment is the median size measured with a laser diffraction / scattering particle size distribution analyzer.
[0050] The content of the colorant or pigment in the base layer 1 is not particularly limited as long as it colors the packaging material for an electricity storage device, and may be, for example, about 5 to 60 mass %, and preferably about 10 to 40 mass %.
[0051] [Adhesive Layer 2] In the packaging material for an electricity storage device according to the present disclosure, the adhesive layer 2 is a layer that is provided between the base material layer 1 and the metal foil layer 3 as needed for the purpose of increasing the adhesion between them.
[0052] The adhesive layer 2 is formed from an adhesive capable of bonding the base material layer 1 and the metal foil layer 3. There are no limitations on the adhesive used to form the adhesive layer 2, and it may be any of a chemical reaction type, a solvent volatilization type, a hot melt type, a hot pressure type, etc. It may also be a two-component curing adhesive (two-component adhesive), a one-component curing adhesive (one-component adhesive), or a resin that does not involve a curing reaction. The adhesive layer 2 may be a single layer or multiple layers.
[0053] Specific examples of adhesive components contained in the adhesive include polyesters such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, polyethylene isophthalate, and copolymer polyesters; polyethers; polyurethanes; epoxy resins; phenolic resins; polyamides such as nylon 6, nylon 66, nylon 12, and copolymer polyamides; polyolefin-based resins such as polyolefins, cyclic polyolefins, acid-modified polyolefins, and acid-modified cyclic polyolefins; polyvinyl acetate; cellulose; (meth)acrylic resins; polyimides; polycarbonates; amino resins such as urea resins and melamine resins; rubbers such as chloroprene rubber, nitrile rubber, and styrene-butadiene rubber; and silicone resins. These adhesive components may be used alone or in combination with two or more. Among these adhesive components, polyurethane adhesives are preferred. Furthermore, the adhesive strength of these adhesive component resins can be increased by using an appropriate curing agent in combination. The curing agent is selected appropriately from polyisocyanates, multifunctional epoxy resins, oxazoline group-containing polymers, polyamine resins, acid anhydrides, and the like, depending on the functional groups possessed by the adhesive components.
[0054] Examples of polyurethane adhesives include polyurethane adhesives containing a first part containing a polyol compound and a second part containing an isocyanate compound. Two-component curing polyurethane adhesives are preferred, with a polyol such as polyester polyol, polyether polyol, or acrylic polyol as the first part and an aromatic or aliphatic polyisocyanate as the second part. Examples of polyurethane adhesives include polyurethane adhesives containing a polyurethane compound obtained by reacting a polyol compound with an isocyanate compound in advance, and an isocyanate compound. Examples of polyurethane adhesives include polyurethane adhesives containing a polyurethane compound obtained by reacting a polyol compound with an isocyanate compound in advance, and a polyol compound. Examples of polyurethane adhesives include polyurethane adhesives obtained by reacting a polyurethane compound obtained by reacting a polyol compound with an isocyanate compound in advance with moisture, such as in the air, and then curing the polyurethane compound. Polyester polyols having hydroxyl groups on the side chains in addition to terminal hydroxyl groups in the repeating unit are preferably used as the polyol compound. Examples of the second part include aliphatic, alicyclic, aromatic, and araliphatic isocyanate compounds. Examples of isocyanate compounds include hexamethylene diisocyanate (HDI), xylylene diisocyanate (XDI), isophorone diisocyanate (IPDI), hydrogenated XDI (H6XDI), hydrogenated MDI (H12MDI), tolylene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), and naphthalene diisocyanate (NDI). Also included are polyfunctional isocyanate-modified compounds of one or more of these diisocyanates. Multimers (e.g., trimers) can also be used as polyisocyanate compounds. Examples of such multimers include adducts, biurets, and nurates. Forming the adhesive layer 2 using a polyurethane adhesive provides the electrical storage device exterior material with excellent electrolyte resistance, preventing peeling of the base layer 1 even when the electrolyte adheres to the side surface.
[0055] Furthermore, the adhesive layer 2 may contain other components as long as they do not impair adhesion, and may contain colorants, thermoplastic elastomers, tackifiers, fillers, etc. By including a colorant in the adhesive layer 2, the electrical storage device packaging material can be colored. Known colorants such as pigments and dyes can be used as colorants. Furthermore, only one type of colorant may be used, or two or more types may be mixed together.
[0056] The type of pigment is not particularly limited as long as it does not impair the adhesiveness of the adhesive layer 2. Examples of organic pigments include azo-based, phthalocyanine-based, quinacridone-based, anthraquinone-based, dioxazine-based, indigothioindigo-based, perinone-perylene-based, isoindolenine-based, and benzimidazolone-based pigments, while examples of inorganic pigments include carbon black-based, titanium oxide-based, cadmium-based, lead-based, chromium oxide-based, and iron-based pigments, and other examples include finely powdered mica and fish scale foil.
[0057] Among colorants, carbon black is preferred in order to give the exterior appearance of the electrical storage device packaging material a black color, for example.
[0058] The average particle size of the pigment is not particularly limited and may be, for example, about 0.03 to 5 μm, about 0.05 to 5 μm, or about 0.08 to 5 μm, and preferably about 0.03 to 2 μm, about 0.05 to 2 μm, or about 0.08 to 2 μm. The average particle size of the pigment is the median size measured with a laser diffraction / scattering particle size distribution analyzer.
[0059] The content of the colorant or the content of the pigment in the adhesive layer 2 is not particularly limited as long as the packaging material for an electricity storage device is colored, and may be, for example, about 5 to 60 mass %, and preferably 10 to 40 mass %.
[0060] The thickness of the adhesive layer 2 is not particularly limited as long as it can bond the base material layer 1 and the metal foil layer 3, but is, for example, about 1 μm or more, about 2 μm or more. The thickness of the adhesive layer 2 is, for example, about 10 μm or less, about 5 μm or less. Preferred ranges for the thickness of the adhesive layer 2 include about 1 to 10 μm, about 1 to 5 μm, about 2 to 10 μm, and about 2 to 5 μm.
[0061] [Colored Layer] The colored layer is a layer (not shown) that is provided between the base material layer 1 and the metal foil layer 3 as needed. When the adhesive layer 2 is provided, a colored layer may be provided between the base material layer 1 and the adhesive layer 2, or between the adhesive layer 2 and the metal foil layer 3. Alternatively, a colored layer may be provided on the outside of the base material layer 1. By providing a colored layer, the packaging material for an electricity storage device can be colored.
[0062] The colored layer can be formed, for example, by applying ink containing a colorant to the surface of the base layer 1 or the surface of the metal foil layer 3. Known colorants such as pigments and dyes can be used as the colorant. Only one type of colorant may be used, or two or more types may be mixed together.
[0063] Specific examples of the colorant contained in the colored layer include the same as those exemplified in the section [Adhesive layer 2].
[0064] [Metal Foil Layer 3] In the packaging material for an electricity storage device, the metal foil layer 3 is a layer (barrier layer) that prevents at least the penetration of moisture.
[0065] The metal foil layer 3 is a layer made of a metal material. Specific examples of the metal material constituting the metal foil layer 3 include aluminum alloys, stainless steel, titanium steel, and steel plates. The metal foil layer 3 preferably contains at least one of an aluminum alloy foil and a stainless steel foil. A plurality of metal foil layers 3 may be provided.
[0066] In the metal foil 3, the layer made of the aforementioned metal material may contain recycled metal material. Examples of recycled metal material include recycled aluminum alloy, stainless steel, titanium steel, or steel plate. These recycled materials can be obtained by known methods. Recycled aluminum alloy material can be obtained, for example, by the manufacturing method described in International Publication No. 2022 / 092231. The metal foil layer 3 may be made of recycled material alone, or may be made of a mixture of recycled and virgin material. Note that recycled metal material refers to metal material that has been made reusable by collecting, isolating, and refining various products used in the market or waste from manufacturing processes. Furthermore, virgin metal material refers to new metal material refined from natural metal resources (raw materials) and is not recycled material.
[0067] In a first aspect of the present disclosure, the root-mean-square gradient Sdq at a laser wavelength of 408 nm measured using a laser microscope on at least one surface of the metal foil layer is 0.28 or less. The larger the root-mean-square gradient Sdq value, the steeper the slope of the fine irregularities inevitably present in the metal foil layer. The steeper the slope of the irregularities on the surface of the metal foil layer, the more likely cracks will occur in the metal foil layer, originating from steeply sloped convex or concave portions, when the metal foil layer is stretched during the formation of an electrical storage device packaging material. In the present disclosure, by using a metal foil layer with a very gentle root-mean-square gradient Sdq of 0.28 or less on at least one surface of the metal foil layer, cracks in the metal foil layer during the formation of an electrical storage device packaging material can be suppressed, thereby demonstrating excellent formability. The method for measuring the root-mean-square gradient Sdq is described below. In the second and third embodiments, it is also preferable that the root-mean-square gradient Sdq of at least one surface of the metal foil layer at a laser wavelength of 408 nm, as measured using a laser microscope, is 0.28 or less.
[0068] In the present disclosure, for example, one side of the metal foil layer 3 is glossy and the other side is matte. In the packaging material for an electricity storage device of the present disclosure, the metal foil layer 3 may have a matte surface on the substrate layer 1 side or on the thermally adhesive resin layer 4 side, but from the viewpoint of making it easy to identify product information and the like printed on the substrate layer surface, it is preferable that the metal foil layer 3 has a matte surface on the substrate layer 1 side.
[0069] In the present disclosure, the surfaces of the metal foil layer 3 are compared, and the surface with a relatively lower gloss is the matte surface, while the surface with a relatively higher gloss is the glossy surface. More specifically, the maximum reflected light intensity of both sides of the metal foil layer is measured, and the surface with a higher gloss is the glossy surface of the metal foil layer, and the surface with a lower gloss is the matte surface of the metal foil layer. Furthermore, for example, during the production of aluminum alloy foil, the surface that contacts the rolling roll during rolling of the aluminum alloy foil is the glossy surface, and the surface where two sheets of aluminum alloy foil meet during two-sheet rolling is the matte surface. The physical properties of the glossy surface of the metal foil layer 3 are not particularly limited as long as they do not impair the effects of the present invention.
[0070] In addition, from the viewpoint of more suitably exerting the effects of the present disclosure, it is preferable that the matte surface of the metal foil layer 3 has the above-mentioned value of the root-mean-square gradient Sdq.
[0071] From the viewpoint of more suitably exerting the effects of the present disclosure, the root-mean-square gradient Sdq on at least one surface of the metal foil layer is preferably 0.28 or less, more preferably 0.25 or less, even more preferably 0.21 or less, and even more preferably 0.19 or less. The root-mean-square gradient Sdq is, for example, 0.10 or more, 0.15 or more, and preferred ranges for the root-mean-square gradient Sdq include about 0.10 to 0.28, about 0.10 to 0.25, about 0.10 to 0.21, about 0.10 to 0.19, about 0.15 to 0.28, about 0.15 to 0.25, about 0.15 to 0.21, and about 0.15 to 0.19. From the viewpoint of more suitably exerting the effects of the present disclosure, it is more preferable that the matte surface of the metal foil layer 3 has these root-mean-square gradient Sdq values.
[0072] In order to adjust the root-mean-square gradient Sdq to 0.28 or less, it is effective to adjust the amount of rolling oil or the conveying tension during rolling so as to make the surface as smooth as possible when producing the metal foil layer. It is preferable to confirm that the root-mean-square gradient Sdq of at least one surface of the obtained metal foil layer is 0.28 or less and use it as the metal foil layer of the exterior material for an electricity storage device of the present disclosure.
[0073] In a second aspect of the present disclosure, the kurtosis Sku of at least one surface of the metal foil layer measured using a laser microscope at a laser wavelength of 408 nm is 4.00 or less, and in order to adjust the kurtosis Sku to 4.00 or less, it is effective to adjust the amount of rolling oil or the conveying tension during rolling so that the convex or concave portions of the fine uneven shape that the metal foil layer inevitably has are not sharp as much as possible when manufacturing the metal foil layer. In the first and third aspects as well, the kurtosis Sku of at least one surface of the metal foil layer measured using a laser microscope at a laser wavelength of 408 nm is preferably 4.00 or less.
[0074] Furthermore, from the viewpoint of more suitably exhibiting the effects of the present disclosure, the kurtosis Sku at a laser wavelength of 408 nm measured using a laser microscope on at least one surface of the metal foil layer is preferably 4.00 or less, more preferably 3.50 or less, and even more preferably 3.00 or less. The kurtosis Sku is, for example, 2.00 or more, 2.50 or more, or 2.95 or more. Preferred ranges for the kurtosis Sku include about 2.00 to 4.00, about 2.00 to 3.50, about 2.00 to 3.00, about 2.50 to 4.00, about 2.50 to 3.50, about 2.50 to 3.00, about 2.95 to 4.00, about 2.95 to 3.50, and about 2.95 to 3.00. From the viewpoint of more suitably exhibiting the effects of the present disclosure, it is more preferable that the matte surface of the metal foil layer 3 has these kurtosis Sku values.
[0075] The larger the value of the kurtosis Sku, the sharper the convex or concave portion of the fine uneven shape that the metal foil layer inevitably has. The sharper the convex or concave portion of the uneven shape on the surface of the metal foil layer, the more likely it is that cracks will occur in the metal foil layer, starting from the sharp convex or concave portion, when the metal foil layer is stretched during the molding of the packaging material for an electric storage device. In the present disclosure, by controlling the kurtosis Sku on at least one surface of the metal foil layer to 4.00 or less, it can be considered that cracks in the metal foil layer during the molding of the packaging material for an electric storage device are more suitably suppressed, and particularly excellent formability is exhibited. The method for measuring the kurtosis Sku is as described below.
[0076] In a third aspect of the present disclosure, the skewness Ssk of at least one surface of the metal foil layer measured using a laser microscope at a laser wavelength of 408 nm is in the range of −0.25 to 0.25. In the first and second aspects as well, the skewness Ssk of at least one surface of the metal foil layer measured using a laser microscope at a laser wavelength of 408 nm is preferably in the range of −0.25 to 0.25.
[0077] Furthermore, from the viewpoint of more suitably exerting the effects of the present disclosure, the skewness Ssk of at least one surface of the metal foil layer at a laser wavelength of 408 nm, measured using a laser microscope, is preferably in the range of −0.25 to 0.25, more preferably −0.20 to 0.20, even more preferably −0.10 to 0.10, and still more preferably −0.07 to 0.07. From the viewpoint of more suitably exerting the effects of the present disclosure, it is more preferable that the matte surface of the metal foil layer 3 satisfy these skewness Ssk ranges.
[0078] The larger the absolute value of the skewness Ssk, the more sharp points there are in the fine irregularities that the metal foil layer inevitably has. The more sharp points there are in the irregularities on the surface of the metal foil layer, the more likely it is that cracks will occur in the metal foil layer, originating from sharp convex or concave portions, when the metal foil layer is stretched during the molding of the electrical storage device packaging material. In the present disclosure, by controlling the skewness Ssk on at least one surface of the metal foil layer to a range of -0.25 to 0.25, it can be considered that cracks in the metal foil layer during the molding of the electrical storage device packaging material are more suitably suppressed, resulting in particularly excellent formability. The method for measuring the skewness Ssk is as described below.
[0079] <Surface Properties of Metal Foil Layer (Laser Microscope)> The values of the root-mean-square gradient Sdq, kurtosis Sku, and skewness Ssk at a laser wavelength of 408 nm are measured using a laser microscope as follows for the surface of the metal foil layer of the packaging material for an electricity storage device.
[0080] The metal foil layer is removed from each electrical storage device packaging material using the following procedure and used as the measurement object. The base material layer of the electrical storage device packaging material is manually peeled off to obtain a laminate consisting of the metal foil layer, an adhesive layer (if required), a heat-sealable resin layer, etc. Furthermore, this laminate is immersed in orthodichlorobenzene under the following conditions to remove the adhesive layer, heat-sealable resin layer, etc. from the metal foil layer, and the surface of the metal foil layer is washed multiple times with ethanol and left to dry, resulting in a metal foil layer that is used as the measurement object.
[0081] Next, the values of the root-mean-square gradient Sdq, kurtosis Sku, and skewness Ssk at a laser wavelength of 408 nm are measured for the surface of the metal foil layer using a laser microscope under the following measurement conditions.
[0082] (Laser microscope measurement conditions) Measurements are made under the following conditions, with reference to ISO25178-2:2012. Device: laser microscope Laser wavelength: 408 nm Measurement optical system: confocal optical system Objective lens magnification: 150x Measurement mode: 9 screens connected (3 screens x 3 screens) Measurement size: standard (1024 data in the X direction, 768 data in the Y direction) The number of pixels per screen is 1024 points in the X direction, i.e., the MD direction of the laminate, and 768 points in the Y direction, i.e., the TD direction of the laminate, and the measurement area of the 9 screens is approximately 255 μm in the MD direction and approximately 185 μm in the TD direction. Measurement conditions: surface shape / high precision / with double scan The pitch of the Z axis is 0.08 μm. Data processing: Reference plane setting (tilt correction) all areas, wavy removal 1, leveling (simple average 3 x 3), height cut level medium In other words, to set the reference plane, tilt correction, wavy removal, smoothing (simple average 3 pixels x 3 pixels), and height cut are performed in that order in the entire area.
[0083] From the viewpoint of improving the formability of the electrical storage device packaging material, the aluminum alloy foil is preferably a soft aluminum alloy foil made of, for example, an annealed aluminum alloy, and from the viewpoint of further improving formability, an iron-containing aluminum alloy foil is preferred. In the iron-containing aluminum alloy foil (100% by mass), the iron content is preferably 0.1 to 9.0% by mass, more preferably 0.5 to 2.0% by mass. By having an iron content of 0.1% by mass or more, an electrical storage device packaging material with better formability can be obtained. By having an iron content of 9.0% by mass or less, an electrical storage device packaging material with better flexibility can be obtained. Furthermore, silicon, magnesium, copper, manganese, etc. may be added as necessary. Furthermore, softening can be performed by annealing or the like.
[0084] Examples of soft aluminum alloy foils include aluminum alloy foils having a composition defined by JIS H4160:1994 A8021H-O, JIS H4160:1994 A8079H-O, JIS H4000:2014 A8021P-O, or JIS H4000:2014 A8079P-O. The composition of JIS A8021 (composition of JIS H4160:1994 A8021H-O, JIS H4000:2014 A8021P-O) is specified as follows: Si is 0.15 mass% or less, Fe is 1.2 to 1.7 mass%, Cu is 0.05 mass% or less, other components (components other than Si, Fe, Cu, and Al) are each 0.05 mass% or less, the total of the other components is 0.15 mass% or less, and Al is the balance. The composition of JIS A8079 (JIS H4160:1994 A8079H-O, JIS H4000:2014 A8079P-O) is specified as follows: Si is 0.05 to 0.30 mass%, Fe is 0.7 to 1.3 mass%, Cu is 0.05 mass% or less, Zn is 0.10 mass% or less, other components (components other than Si, Fe, Cu, Zn, and Al) are each 0.05 mass% or less, the total of the other components is 0.15 mass% or less, and Al is the balance. The composition of the aluminum alloy foil can be measured by elemental analysis.
[0085] From the viewpoint of more suitably exhibiting the effects of the present disclosure, the Si content of the aluminum alloy foil is preferably 0.08% by mass or more, more preferably about 0.10% by mass or more, and even more preferably about 0.12% by mass or more. Also, preferably about 1.50% by mass or less, more preferably about 1.20% by mass or less, and even more preferably about 1.00% by mass or less. Preferred ranges include about 0.08 to 1.50% by mass, about 0.08 to 1.20% by mass, about 0.08 to 1.00% by mass, about 0.10 to 1.50% by mass, about 0.10 to 1.20% by mass, about 0.10 to 1.00% by mass, about 0.12 to 1.50% by mass, about 0.12 to 1.20% by mass, and about 0.12 to 1.00% by mass. Among aluminum alloy foils satisfying these Si contents, the Fe content is preferably 0.50% by mass or more, more preferably about 0.80% by mass or more, and even more preferably about 1.00% by mass or more, and is preferably about 1.50% by mass or less, more preferably about 1.40% by mass or less, and even more preferably about 1.30% by mass or less, and preferred ranges include about 0.50 to 1.50% by mass, about 0.50 to 1.40% by mass, about 0.50 to 1.30% by mass, about 0.80 to 1.50% by mass, and about 0.80 to 1.40% by mass. The Mg content is preferably 0% by mass or more, more preferably 0.80% by mass or more, and is also preferably 2.00% by mass or less, more preferably 1.50% by mass or less. Preferred ranges include about 0% by mass, about 0% by mass, about 0% by mass, about 0% by mass, about 0% by mass, about 0% by mass, about 0.80% by mass, about 0.80% by mass, about 0.80% by mass, about 0.80% by mass, about 0.50% by mass, and may be 0% by mass.The Al content is preferably 95.00% by mass or more, more preferably about 95.30% by mass or more, even more preferably about 95.50% by mass or more, and is preferably about 97.00% by mass or less, more preferably about 96.30% by mass or less, and even more preferably about 95.60% by mass or less. Preferred ranges include about 95.00 to 97.00% by mass, about 95.00 to 96.30% by mass, about 95.00 to 95.60% by mass, about 95.30 to 97.00% by mass, about 95.30 to 96.30% by mass, and about 95.30 to 95.60% by mass. It is preferable that other components (components other than Si, Fe, Mg, and Al) are each 0.05% by mass or less, the total of the other components is 0.15% by mass or less, and Al is the balance.
[0086] Examples of the stainless steel foil include austenitic, ferritic, austenitic-ferritic, martensitic, and precipitation hardened stainless steel foils. From the viewpoint of providing an exterior material for an electricity storage device that has excellent formability, the stainless steel foil is preferably made of austenitic stainless steel.
[0087] Specific examples of austenitic stainless steels that form the stainless steel foil include SUS304, SUS301, and SUS316L, with SUS304 being particularly preferred.
[0088] In the case of a metal foil, the thickness of the metal foil layer 3 should be sufficient to at least function as a metal foil layer to prevent moisture penetration, and may be, for example, approximately 9 to 200 μm. The thickness of the metal foil layer 3 is preferably approximately 85 μm or less, more preferably approximately 50 μm or less, even more preferably approximately 40 μm or less, and particularly preferably approximately 35 μm or less. The thickness of the metal foil layer 3 is preferably approximately 10 μm or more, even more preferably approximately 20 μm or more, and more preferably approximately 25 μm or more. Preferred thickness ranges for the metal foil layer 3 include approximately 10 to 85 μm, approximately 10 to 50 μm, approximately 10 to 40 μm, approximately 10 to 35 μm, approximately 20 to 85 μm, approximately 20 to 50 μm, approximately 20 to 40 μm, approximately 20 to 35 μm, approximately 25 to 85 μm, approximately 25 to 50 μm, approximately 25 to 40 μm, and approximately 25 to 35 μm. When the metal foil layer 3 is made of an aluminum alloy foil, the above-mentioned range is particularly preferred. From the viewpoint of imparting high formability and high rigidity to the electrical storage device packaging material 10, the thickness of the metal foil layer 3 is preferably about 35 μm or more, more preferably about 45 μm or more, even more preferably about 50 μm or more, and still more preferably about 55 μm or more, and is also preferably about 200 μm or less, more preferably about 85 μm or less, even more preferably about 75 μm or less, and still more preferably about 70 μm or less. Preferred ranges are approximately 35 to 200 μm, approximately 35 to 85 μm, approximately 35 to 75 μm, approximately 35 to 70 μm, approximately 45 to 200 μm, approximately 45 to 85 μm, approximately 45 to 75 μm, approximately 45 to 70 μm, approximately 50 to 200 μm, approximately 50 to 85 μm, approximately 50 to 75 μm, approximately 50 to 70 μm, approximately 55 to 200 μm, approximately 55 to 85 μm, approximately 55 to 75 μm, and approximately 55 to 70 μm. The high formability of the exterior packaging material 10 for an electricity storage device facilitates deep drawing, which can contribute to increasing the capacity of the electricity storage device. Furthermore, while increasing the capacity of an electricity storage device increases the weight of the electricity storage device, the increased rigidity of the exterior packaging material 10 for an electricity storage device can contribute to high sealing performance of the electricity storage device.In particular, when the metal foil layer 3 is composed of a stainless steel foil, the thickness of the stainless steel foil is preferably about 60 μm or less, more preferably about 50 μm or less, even more preferably about 40 μm or less, even more preferably about 30 μm or less, and particularly preferably about 25 μm or less. The thickness of the stainless steel foil is preferably about 10 μm or more, more preferably about 15 μm or more. Preferred ranges for the thickness of the stainless steel foil include about 10 to 60 μm, about 10 to 50 μm, about 10 to 40 μm, about 10 to 30 μm, about 10 to 25 μm, about 15 to 60 μm, about 15 to 50 μm, about 15 to 40 μm, about 15 to 30 μm, and about 15 to 25 μm.
[0089] Furthermore, the metal foil layer 3 preferably has a corrosion-resistant coating on at least the surface opposite the substrate layer to prevent dissolution and corrosion. The metal foil layer 3 may have a corrosion-resistant coating on both sides. Here, the corrosion-resistant coating refers to a thin film formed by, for example, hydrothermal conversion treatment such as boehmite treatment, chemical conversion treatment, anodizing treatment, plating treatment with nickel or chromium, or corrosion prevention treatment such as applying a coating agent, which provides the metal foil layer with corrosion resistance (e.g., acid resistance, alkali resistance, etc.). Specifically, the corrosion-resistant coating refers to a coating that improves the acid resistance of the metal foil layer (acid-resistant coating), a coating that improves the alkali resistance of the metal foil layer (alkali-resistant coating), or the like. The corrosion-resistant coating may be formed by one type of treatment or a combination of two or more types. Furthermore, not only one layer but also multiple layers can be formed. Furthermore, among these treatments, hydrothermal conversion treatment and anodizing treatment are treatments in which the metal foil surface is dissolved by a treatment agent to form a metal compound with excellent corrosion resistance. These treatments may be included in the definition of “chemical conversion treatment.” In addition, when the metal foil layer 3 is provided with a corrosion-resistant coating, the metal foil layer 3 includes the corrosion-resistant coating.
[0090] The corrosion-resistant coating prevents delamination between the metal foil layer (e.g., aluminum alloy foil) and the substrate layer during molding of the electrical storage device exterior material, prevents dissolution and corrosion of the metal foil layer surface due to hydrogen fluoride produced by the reaction between the electrolyte and water, and particularly prevents dissolution and corrosion of aluminum oxide present on the metal foil layer surface when the metal foil layer is an aluminum alloy foil, and also improves the adhesion (wettability) of the metal foil layer surface, thereby preventing delamination between the substrate layer and the metal foil layer during heat sealing and between the substrate layer and the metal foil layer during molding.
[0091] Various corrosion-resistant coatings formed by chemical conversion treatments are known, including mainly corrosion-resistant coatings containing at least one of phosphates, chromates, fluorides, triazine thiol compounds, and rare earth oxides. Examples of chemical conversion treatments using phosphates and chromates include chromate chromate treatment, phosphate chromate treatment, phosphate-chromate treatment, and chromate treatment. Examples of chromium compounds used in these treatments include chromium nitrate, chromium fluoride, chromium sulfate, chromium acetate, chromium oxalate, chromium biphosphate, chromate acetylacetate, chromium chloride, and potassium chromium sulfate. Examples of phosphorus compounds used in these treatments include sodium phosphate, potassium phosphate, ammonium phosphate, and polyphosphoric acid. Examples of chromate treatments include etching chromate treatment, electrolytic chromate treatment, and paint-on chromate treatment, with paint-on chromate treatment being preferred. This paint-type chromate treatment involves first degreasing at least the inner surface of a metal foil layer (e.g., aluminum alloy foil) using a well-known method such as alkali immersion, electrolytic cleaning, acid pickling, electrolytic pickling, or acid activation, and then coating the degreased surface with a treatment solution containing, as its main component, a metal phosphate such as chromium (Cr) phosphate, titanium (Ti) phosphate, zirconium (Zr) phosphate, or zinc (Zn) phosphate, or a mixture of these metal salts, or a treatment solution containing, as its main component, a nonmetallic phosphate and a mixture of these nonmetallic salts, or a mixture of these with a synthetic resin, by a well-known coating method such as roll coating, gravure printing, or immersion, and then drying. The treatment solution can be, for example, water, alcoholic solvents, hydrocarbon solvents, ketone solvents, ester solvents, or ether solvents, with water being preferred. Examples of the resin component used here include polymers such as phenolic resins and acrylic resins, and chromate treatment using an aminated phenol polymer having repeating units represented by the following general formulas (1) to (4). The aminated phenol polymer may contain one type of repeating unit represented by the following general formulas (1) to (4) alone, or two or more types of repeating units may be contained in any combination.The acrylic resin is preferably polyacrylic acid, an acrylic acid methacrylic acid ester copolymer, an acrylic acid maleic acid copolymer, an acrylic acid styrene copolymer, or a derivative thereof such as a sodium salt, an ammonium salt, or an amine salt. A derivative of polyacrylic acid, such as an ammonium salt, a sodium salt, or an amine salt of polyacrylic acid, is particularly preferred. In the present disclosure, polyacrylic acid refers to a polymer of acrylic acid. The acrylic resin is also preferably a copolymer of acrylic acid and a dicarboxylic acid or a dicarboxylic acid anhydride, or an ammonium salt, a sodium salt, or an amine salt of a copolymer of acrylic acid and a dicarboxylic acid or a dicarboxylic acid anhydride. Only one type of acrylic resin may be used, or two or more types may be mixed and used.
[0092]
[0093]
[0094]
[0095]
[0096] In the general formulas (1) to (4), X represents a hydrogen atom, a hydroxy group, an alkyl group, a hydroxyalkyl group, an allyl group, or a benzyl group. 1 and R 2 are the same or different and represent a hydroxy group, an alkyl group, or a hydroxyalkyl group. 1 and R 2 Examples of the alkyl group represented by X and R include linear or branched alkyl groups having 1 to 4 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, and tert-butyl. 1 and R 2Examples of the hydroxyalkyl group represented by the formula (1) include a linear or branched alkyl group having 1 to 4 carbon atoms substituted with one hydroxy group, such as a hydroxymethyl group, a 1-hydroxyethyl group, a 2-hydroxyethyl group, a 1-hydroxypropyl group, a 2-hydroxypropyl group, a 3-hydroxypropyl group, a 1-hydroxybutyl group, a 2-hydroxybutyl group, a 3-hydroxybutyl group, and a 4-hydroxybutyl group. 1 and R 2 The alkyl group and hydroxyalkyl group represented by the formula (1) may be the same or different. In the formulae (1) to (4), X is preferably a hydrogen atom, a hydroxy group, or a hydroxyalkyl group. The number average molecular weight of the aminated phenol polymer having repeating units represented by the formulae (1) to (4) is preferably about 500 to 1,000,000, for example, and more preferably about 1,000 to 20,000. The aminated phenol polymer can be prepared, for example, by polycondensing a phenol compound or a naphthol compound with formaldehyde to produce a polymer comprising repeating units represented by the formula (1) or (3), and then polycondensing the polymer with formaldehyde and an amine (R 1 R 2 NH) to form a functional group (-CHNR 1 R 2 The aminated phenol polymers may be used singly or in combination of two or more.
[0097] Another example of a corrosion-resistant coating is a thin film formed by a coating-type corrosion prevention treatment in which a coating agent containing at least one selected from the group consisting of a rare earth element oxide sol, an anionic polymer, and a cationic polymer is applied. The coating agent may further contain phosphoric acid or a phosphate salt, and a crosslinking agent for crosslinking the polymer. The rare earth element oxide sol contains rare earth element oxide fine particles (e.g., particles with an average particle size of 100 nm or less) dispersed in a liquid dispersion medium. Examples of rare earth element oxides include cerium oxide, yttrium oxide, neodymium oxide, and lanthanum oxide, with cerium oxide being preferred from the perspective of further improving adhesion. The rare earth element oxide contained in the corrosion-resistant coating can be used alone or in combination of two or more. Examples of liquid dispersion media for the rare earth element oxide sol include various solvents such as water, alcohol-based solvents, hydrocarbon-based solvents, ketone-based solvents, ester-based solvents, and ether-based solvents, with water being preferred. Preferred examples of cationic polymers include polyethyleneimine, ionic polymer complexes consisting of polyethyleneimine and a polymer having a carboxylic acid, primary amine-grafted acrylic resins in which a primary amine is graft-polymerized onto an acrylic backbone, polyallylamine or its derivatives, and aminated phenols. Preferred anionic polymers include poly(meth)acrylic acid or its salts, or copolymers primarily composed of (meth)acrylic acid or its salts. The crosslinking agent is preferably at least one selected from the group consisting of a compound having a functional group selected from an isocyanate group, a glycidyl group, a carboxyl group, or an oxazoline group, and a silane coupling agent. The phosphoric acid or phosphoric acid salt is preferably a condensed phosphoric acid or a condensed phosphate salt.
[0098] An example of a corrosion-resistant coating is one formed by applying a solution in which fine particles of a metal oxide such as aluminum oxide, titanium oxide, cerium oxide, or tin oxide, or barium sulfate are dispersed in phosphoric acid to the surface of a metal foil layer and then baking the solution at 150°C or higher.
[0099] The corrosion-resistant coating may have a laminated structure, if necessary, by further laminating at least one of a cationic polymer and an anionic polymer, such as those mentioned above.
[0100] The composition of the corrosion-resistant film can be analyzed by, for example, time-of-flight secondary ion mass spectrometry.
[0101] The amount of the corrosion-resistant film formed on the surface of the metal foil layer 3 in the chemical conversion treatment is not particularly limited. For example, in the case of a coating-type chromate treatment, the amount of the corrosion-resistant film formed on the surface of the metal foil layer 3 is 2 It is desirable that the chromate compound is contained in an amount, calculated as chromium, of about 0.5 to 50 mg, preferably about 1.0 to 40 mg, the phosphorus compound in an amount, calculated as phosphorus, of about 0.5 to 50 mg, preferably about 1.0 to 40 mg, and the aminated phenol polymer in an amount, calculated as phosphorus, of about 1.0 to 200 mg, preferably about 5.0 to 150 mg, per 1000 ml of the aqueous solution.
[0102] The thickness of the corrosion-resistant coating is not particularly limited, but is preferably about 1 nm to 20 μm, more preferably about 1 nm to 100 nm, and even more preferably about 1 nm to 50 nm, from the viewpoint of the cohesive strength of the coating and the adhesive strength with the metal foil layer and the heat-sealable resin layer. The thickness of the corrosion-resistant coating can be measured by observation with a transmission electron microscope, or by a combination of observation with a transmission electron microscope and energy dispersive X-ray spectroscopy or electron energy loss spectroscopy. Analysis of the composition of the corrosion-resistant coating using time-of-flight secondary ion mass spectrometry can reveal, for example, secondary ions consisting of Ce, P, and O (e.g., Ce2PO4 + , CePO4 - or at least one of ions of Cr, P, and O (e.g., CrPO2 + , CrPO4 - Peaks derived from at least one of the above are detected.
[0103] The chemical conversion treatment is carried out by applying a solution containing a compound used to form a corrosion-resistant coating to the surface of the metal foil layer by bar coating, roll coating, gravure coating, immersion, or the like, and then heating the metal foil layer to a temperature of approximately 70 to 200°C. Furthermore, before the chemical conversion treatment is carried out on the metal foil layer, the metal foil layer may be subjected to a degreasing treatment using an alkali immersion method, electrolytic cleaning, acid pickling, electrolytic acid pickling, or the like. By carrying out such a degreasing treatment, the chemical conversion treatment on the surface of the metal foil layer can be carried out more efficiently. Furthermore, by using an acid degreasing agent prepared by dissolving a fluorine-containing compound in an inorganic acid for the degreasing treatment, not only the metal foil can be degreased but also a fluoride of the metal, which is in a passive state, can be formed. In such cases, only the degreasing treatment may be carried out.
[0104] [Heat-fusible resin layer 4] In the exterior packaging material for an electricity storage device of the present disclosure, the heat-fusible resin layer 4 corresponds to the innermost layer and is a layer (sealant layer) that exhibits the function of sealing the electricity storage device elements by heat-fusible resin layers being heat-fused together when the electricity storage device is assembled.
[0105] The resin constituting the heat-sealable resin layer 4 is not particularly limited as long as it is heat-sealable, but resins containing a polyolefin skeleton, such as polyolefin and acid-modified polyolefin, are preferred. The presence of a polyolefin skeleton in the resin constituting the heat-sealable resin layer 4 can be determined by, for example, infrared spectroscopy, gas chromatography mass spectrometry, or the like. Furthermore, when the resin constituting the heat-sealable resin layer 4 is analyzed by infrared spectroscopy, a peak derived from maleic anhydride is preferably detected. For example, when maleic anhydride-modified polyolefin is measured by infrared spectroscopy, a peak derived from maleic anhydride is detected at a wavenumber of 1760 cm. -1 Nearby and wave number 1780 cm -1 A peak derived from maleic anhydride is detected around . When the thermally adhesive resin layer 4 is a layer made of maleic anhydride-modified polyolefin, a peak derived from maleic anhydride is detected by infrared spectroscopy. However, if the degree of acid modification is low, the peak becomes small and may not be detected. In such cases, analysis can be performed by nuclear magnetic resonance spectroscopy.
[0106] The heat-sealable resin layer 4 preferably contains a resin containing a polyolefin skeleton as a main component, more preferably a polyolefin as a main component, and even more preferably polypropylene as a main component. Here, "main component" refers to a resin component whose content of the resin components contained in the heat-sealable resin layer 4 is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, and even more preferably 99% by mass or more. For example, "the heat-sealable resin layer 4 contains polypropylene as a main component" means that the polypropylene content of the resin components contained in the heat-sealable resin layer 4 is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, and even more preferably 99% by mass or more.
[0107] Specific examples of polyolefins include polyethylenes such as low-density polyethylene, medium-density polyethylene, high-density polyethylene, and linear low-density polyethylene; ethylene-α-olefin copolymers; polypropylenes such as homopolypropylene, block copolymers of polypropylene (e.g., block copolymers of propylene and ethylene), and random copolymers of polypropylene (e.g., random copolymers of propylene and ethylene); propylene-α-olefin copolymers; and ethylene-butene-propylene terpolymers. Among these, polypropylene is preferred. When the polyolefin resin is a copolymer, it may be a block copolymer or a random copolymer. These polyolefin resins may be used alone or in combination of two or more.
[0108] The polyolefin may also be a cyclic polyolefin. Cyclic polyolefins are copolymers of olefins and cyclic monomers, and examples of olefins constituting the cyclic polyolefins include ethylene, propylene, 4-methyl-1-pentene, styrene, butadiene, and isoprene. Examples of cyclic monomers constituting the cyclic polyolefins include cyclic alkenes such as norbornene; and cyclic dienes such as cyclopentadiene, dicyclopentadiene, cyclohexadiene, and norbornadiene. Among these, cyclic alkenes are preferred, and norbornene is more preferred.
[0109] The polyolefin may also be an acid-modified polyolefin. An acid-modified polyolefin is a polymer modified by block polymerization or graft polymerization of a polyolefin with an acid component. Examples of the acid-modified polyolefin include the above-mentioned polyolefins, copolymers of the above-mentioned polyolefins with polar molecules such as acrylic acid or methacrylic acid, and polymers such as crosslinked polyolefins. Examples of the acid component used for acid modification include carboxylic acids or anhydrides thereof, such as maleic acid, acrylic acid, itaconic acid, crotonic acid, maleic anhydride, and itaconic anhydride.
[0110] The acid-modified polyolefin may be an acid-modified cyclic polyolefin. The acid-modified cyclic polyolefin is a polymer obtained by copolymerizing a part of the monomers constituting the cyclic polyolefin by replacing it with an acid component, or by block polymerizing or graft polymerizing an acid component onto the cyclic polyolefin. The acid-modified cyclic polyolefin is the same as described above. The acid component used for the acid modification is the same as the acid component used for the modification of the polyolefin.
[0111] Preferred acid-modified polyolefins include polyolefins modified with carboxylic acid or its anhydride, polypropylenes modified with carboxylic acid or its anhydride, maleic anhydride-modified polyolefins, and maleic anhydride-modified polypropylenes.
[0112] The thermally adhesive resin layer 4 may be formed of one type of resin alone or a blend polymer of two or more types of resins. Furthermore, the thermally adhesive resin layer 4 may be formed of only one layer, or may be formed of two or more layers of the same or different resins.
[0113] When the thermally adhesive resin layer 4 is laminated with the metal foil layer 3, the adhesive layer 5, or the like to produce the packaging material 10 for an electricity storage device of the present disclosure, a pre-formed resin film may be used as the thermally adhesive resin layer 4. Alternatively, the thermally adhesive resin that forms the thermally adhesive resin layer 4 may be formed into a film on the surface of the metal foil layer 3, the adhesive layer 5, or the like by extrusion molding, coating, or the like, to form the thermally adhesive resin layer 4 from a resin film.
[0114] Furthermore, the thermally adhesive resin layer 4 may contain a lubricant or the like as necessary. When the thermally adhesive resin layer 4 contains a lubricant, the formability of the electrical storage device packaging material can be improved. The lubricant is not particularly limited, and known lubricants can be used.
[0115] The lubricant is not particularly limited, but preferably an amide-based lubricant is used. Specific examples of the lubricant include those exemplified for the base layer 1. The lubricant may be used alone or in combination of two or more types, and a combination of two or more types is preferred.
[0116] In the present disclosure, from the viewpoint of improving the formability of the exterior material for an electrical storage device, it is preferable that a lubricant be present on at least one of the surface and the interior of the heat-sealable resin layer 4. The lubricant is not particularly limited, but preferably an amide-based lubricant is used. Specific examples of amide-based lubricants include saturated fatty acid amides, unsaturated fatty acid amides, substituted amides, methylolamides, saturated fatty acid bisamides, unsaturated fatty acid bisamides, fatty acid ester amides, and aromatic bisamides. Specific examples of saturated fatty acid amides include lauric acid amide, palmitic acid amide, stearic acid amide, behenic acid amide, and hydroxystearic acid amide. Specific examples of unsaturated fatty acid amides include oleic acid amide and erucic acid amide. Specific examples of substituted amides include N-oleyl palmitic acid amide, N-stearyl stearic acid amide, N-stearyl oleic acid amide, N-oleyl stearic acid amide, and N-stearyl erucic acid amide. Specific examples of methylolamides include methylol stearic acid amide. Specific examples of saturated fatty acid bisamides include methylene bisstearic acid amide, ethylene biscapric acid amide, ethylene bislauric acid amide, ethylene bisstearic acid amide, ethylene bishydroxystearic acid amide, ethylene bisbehenic acid amide, hexamethylene bisstearic acid amide, hexamethylene bisbehenic acid amide, hexamethylene hydroxystearic acid amide, N,N'-distearyl adipamide, N,N'-distearyl sebacic acid amide, etc. Specific examples of unsaturated fatty acid bisamides include ethylene bisoleic acid amide, ethylene biserucic acid amide, hexamethylene bisoleic acid amide, N,N'-dioleyl adipamide, N,N'-dioleyl sebacic acid amide, etc. Specific examples of fatty acid ester amides include stearamidoethyl stearate, etc. Specific examples of aromatic bisamides include m-xylylene bisstearic acid amide, m-xylylene bishydroxystearic acid amide, and N,N'-distearylisophthalic acid amide.The lubricant may be used alone or in combination of two or more kinds, and it is preferable to use a combination of two or more kinds.
[0117] When a lubricant is present on the surface of the heat-sealable resin layer 4, the amount of the lubricant is not particularly limited. However, from the viewpoint of improving the formability of the exterior material for an electrical storage device, the amount of the lubricant is preferably about 1 mg / m 2 or more, more preferably about 3 mg / m 2 or more, more preferably about 5 mg / m 2 or more, more preferably about 10 mg / m 2 or more, more preferably about 15 mg / m 2 or more, and preferably about 50 mg / m 2 or less, more preferably about 40 mg / m 2 The preferred range is 1 to 50 mg / m 2 Degree, 1-40mg / m 2 Degree, 3-50mg / m 2 Degree, 3-40mg / m 2 degree, 5-50mg / m 2 degree, 5-40mg / m 2 degree, 10-50mg / m 2 degree, 10-40mg / m 2 degree, 15-50mg / m 2 degree, 15-40mg / m 2 The degree of
[0118] When a lubricant is present inside the heat-sealable resin layer 4, the amount thereof is not particularly limited, but from the viewpoint of improving the formability of the packaging material for an electrical storage device, it is preferably about 100 ppm or more, more preferably about 300 ppm or more, and even more preferably about 500 ppm or more, and is preferably about 3000 ppm or less, more preferably about 2000 ppm or less, and preferred ranges include about 100 to 3000 ppm, about 100 to 2000 ppm, about 300 to 3000 ppm, about 300 to 2000 ppm, about 500 to 3000 ppm, and about 500 to 2000 ppm. When two or more types of lubricant are present inside the heat-sealable resin layer 4, the above amount of lubricant is the total amount of lubricant. Furthermore, when two or more types of lubricants are present inside the heat-sealable resin layer 4, the amount of the first type of lubricant present is not particularly limited, but from the viewpoint of improving the formability of the exterior material for an electrical storage device, it is preferably about 100 ppm or more, more preferably about 300 ppm or more, even more preferably about 500 ppm or more, and is preferably about 3000 ppm or less, more preferably about 2000 ppm or less, and preferred ranges include about 100 to 3000 ppm, about 100 to 2000 ppm, about 300 to 3000 ppm, about 300 to 2000 ppm, about 500 to 3000 ppm, and about 500 to 2000 ppm. The amount of the second type of lubricant present is not particularly limited, but from the viewpoint of improving the formability of the exterior material for an electricity storage device, it is preferably about 50 ppm or more, more preferably about 100 ppm or more, and even more preferably about 200 ppm or more, and is preferably about 1500 ppm or less, more preferably about 1000 ppm or less, and preferred ranges include about 50 to 1500 ppm, about 50 to 1000 ppm, about 100 to 1500 ppm, about 100 to 1000 ppm, about 200 to 1500 ppm, and about 200 to 1000 ppm.
[0119] The lubricant present on the surface of the heat-sealable resin layer 4 may be a lubricant exuded from the resin constituting the heat-sealable resin layer 4, or a lubricant applied to the surface of the heat-sealable resin layer 4.
[0120] The thickness of the heat-sealable resin layer 4 is not particularly limited as long as it functions to heat-seal the heat-sealable resin layers to each other and seal the electricity storage device element, but may be, for example, about 100 μm or less, preferably about 85 μm or less, and more preferably about 15 to 85 μm. Note that, for example, when the thickness of the adhesive layer 5 described below is 10 μm or more, the thickness of the heat-sealable resin layer 4 is preferably about 85 μm or less, more preferably about 15 to 45 μm. For example, when the thickness of the adhesive layer 5 described below is less than 10 μm or when the adhesive layer 5 is not provided, the thickness of the heat-sealable resin layer 4 is preferably about 20 μm or more, more preferably about 35 to 85 μm.
[0121] [Adhesive layer 5] In the packaging material for an electricity storage device according to the present disclosure, the adhesive layer 5 is a layer that is provided as needed between the metal foil layer 3 (or the corrosion-resistant coating) and the heat-sealable resin layer 4 in order to firmly bond them together.
[0122] The adhesive layer 5 is formed of a resin capable of bonding the metal foil layer 3 and the heat-fusible resin layer 4. As the resin used to form the adhesive layer 5, for example, the same adhesive as exemplified for the adhesive layer 2 can be used.
[0123] Furthermore, from the viewpoint of firmly adhering the adhesive layer 5 and the heat-sealable resin layer 4, the resin used to form the adhesive layer 5 preferably contains a polyolefin skeleton, and examples thereof include the polyolefins, acid-modified polyolefins, cyclic polyolefins, and acid-modified cyclic polyolefins exemplified for the heat-sealable resin layer 4 described above. On the other hand, from the viewpoint of firmly adhering the metal foil layer 3 and the adhesive layer 5, the adhesive layer 5 preferably contains an acid-modified polyolefin. Examples of acid-modified components include dicarboxylic acids such as maleic acid, itaconic acid, succinic acid, and adipic acid, as well as their anhydrides, acrylic acid, and methacrylic acid. However, maleic anhydride is most preferred in terms of ease of modification and versatility. Furthermore, from the viewpoint of the heat resistance of the electrical storage device exterior material, the olefin component is preferably a polypropylene-based resin, and the adhesive layer 5 most preferably contains maleic anhydride-modified polypropylene.
[0124] When the resin used to form the adhesive layer 5 contains a polyolefin skeleton, the adhesive layer 5 preferably contains a resin containing a polyolefin skeleton as a main component, more preferably an acid-modified polyolefin as a main component, and even more preferably an acid-modified polypropylene as a main component. Here, "main component" means that the content of the resin component contained in the adhesive layer 5 is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, and even more preferably 99% by mass or more. For example, when the adhesive layer 5 contains acid-modified polypropylene as a main component, it means that the content of acid-modified polypropylene among the resin components contained in the adhesive layer 5 is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, and even more preferably 99% by mass or more.
[0125] The presence of a polyolefin skeleton in the resin constituting the adhesive layer 5 can be determined by, for example, infrared spectroscopy, gas chromatography mass spectrometry, or the like, and the analysis method is not particularly limited. Furthermore, the presence of an acid-modified polyolefin in the resin constituting the adhesive layer 5 can be determined by, for example, measuring a maleic anhydride-modified polyolefin by infrared spectroscopy, and finding a wave number of 1760 cm -1 Nearby and wave number 1780 cm -1 A peak derived from maleic anhydride is detected around this point. However, if the degree of acid modification is low, the peak may be small and not be detected. In this case, analysis can be performed using nuclear magnetic resonance spectroscopy.
[0126] Furthermore, from the viewpoint of ensuring durability such as heat resistance and resistance to contents of the electrical storage device packaging material, and of ensuring moldability while reducing the thickness, the adhesive layer 5 is more preferably a cured product of a resin composition containing an acid-modified polyolefin and a curing agent. Preferred examples of the acid-modified polyolefin include those described above.
[0127] The adhesive layer 5 is preferably a cured product of a resin composition containing an acid-modified polyolefin and at least one selected from the group consisting of a compound having an isocyanate group, a compound having an oxazoline group, and a compound having an epoxy group. A cured product of a resin composition containing an acid-modified polyolefin and at least one selected from the group consisting of a compound having an isocyanate group and a compound having an epoxy group is particularly preferred. The adhesive layer 5 preferably contains at least one selected from the group consisting of polyurethane, polyester, and epoxy resin, and more preferably contains polyurethane and epoxy resin. Examples of polyesters include ester resins formed by the reaction of epoxy groups with maleic anhydride groups, and amide ester resins formed by the reaction of oxazoline groups with maleic anhydride groups. If unreacted curing agents such as compounds having an isocyanate group, compounds having an oxazoline group, or epoxy resins remain in the adhesive layer 5, the presence of the unreacted materials can be confirmed by a method selected from the group consisting of infrared spectroscopy, Raman spectroscopy, time-of-flight secondary ion mass spectrometry (TOF-SIMS), and the like.
[0128] Furthermore, from the viewpoint of further enhancing the adhesion between the metal foil layer 3 and the adhesive layer 5, the adhesive layer 5 is preferably a cured product of a resin composition containing a curing agent having at least one selected from the group consisting of an oxygen atom, a heterocycle, a C═N bond, and a C—O—C bond. Examples of curing agents having a heterocycle include curing agents having an oxazoline group and curing agents having an epoxy group. Examples of curing agents having a C═N bond include curing agents having an oxazoline group and curing agents having an isocyanate group. Examples of curing agents having a C—O—C bond include curing agents having an oxazoline group and curing agents having an epoxy group. Whether the adhesive layer 5 is a cured product of a resin composition containing such a curing agent can be confirmed by, for example, gas chromatography mass spectrometry (GCMS), infrared spectroscopy (IR), time-of-flight secondary ion mass spectrometry (TOF-SIMS), X-ray photoelectron spectroscopy (XPS), or other methods.
[0129] The compound having an isocyanate group is not particularly limited, but from the viewpoint of effectively improving the adhesion between the metal foil layer 3 and the adhesive layer 5, a polyfunctional isocyanate compound is preferably used. The polyfunctional isocyanate compound is not particularly limited as long as it has two or more isocyanate groups. Specific examples of polyfunctional isocyanate curing agents include pentane diisocyanate (PDI), isophorone diisocyanate (IPDI), hexamethylene diisocyanate (HDI), tolylene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), polymers or nurates thereof, mixtures of these, and copolymers with other polymers. Other examples include adducts, biurets, and isocyanurates.
[0130] The content of the compound having an isocyanate group in the adhesive layer 5 is preferably in the range of 0.1 to 50% by mass, and more preferably in the range of 0.5 to 40% by mass, of the resin composition constituting the adhesive layer 5. This can effectively improve the adhesion between the metal foil layer 3 and the adhesive layer 5.
[0131] The compound having an oxazoline group is not particularly limited as long as it is a compound having an oxazoline skeleton. Specific examples of the compound having an oxazoline group include those having a polystyrene main chain and those having an acrylic main chain. Examples of commercially available products include the Epocross series manufactured by Nippon Shokubai Co., Ltd.
[0132] The proportion of the compound having an oxazoline group in the adhesive layer 5 is preferably in the range of 0.1 to 50 mass %, and more preferably in the range of 0.5 to 40 mass %, of the resin composition constituting the adhesive layer 5. This makes it possible to effectively improve the adhesion between the metal foil layer 3 and the adhesive layer 5.
[0133] Examples of compounds having epoxy groups include epoxy resins. The epoxy resin is not particularly limited as long as it is a resin capable of forming a crosslinked structure by the epoxy groups present in the molecule, and known epoxy resins can be used. The weight-average molecular weight of the epoxy resin is preferably about 50 to 2,000, more preferably about 100 to 1,000, and even more preferably about 200 to 800. In the present disclosure, the weight-average molecular weight of the epoxy resin is a value measured by gel permeation chromatography (GPC) under conditions using polystyrene as a standard sample.
[0134] Specific examples of epoxy resins include glycidyl ether derivatives of trimethylolpropane, bisphenol A diglycidyl ether, modified bisphenol A diglycidyl ether, bisphenol F glycidyl ether, novolac glycidyl ether, glycerin polyglycidyl ether, polyglycerin polyglycidyl ether, etc. The epoxy resins may be used alone or in combination of two or more.
[0135] The proportion of the epoxy resin in the adhesive layer 5 is preferably in the range of 0.1 to 50 mass %, and more preferably in the range of 0.5 to 40 mass %, of the resin composition constituting the adhesive layer 5. This makes it possible to effectively improve the adhesion between the metal foil layer 3 and the adhesive layer 5.
[0136] The polyurethane is not particularly limited, and any known polyurethane can be used. The adhesive layer 5 may be, for example, a cured product of two-component curing polyurethane.
[0137] The proportion of polyurethane in the adhesive layer 5 is preferably in the range of 0.1 to 50 mass %, and more preferably in the range of 0.5 to 40 mass %, of the resin composition constituting the adhesive layer 5. This effectively improves the adhesion between the metal foil layer 3 and the adhesive layer 5 in an atmosphere containing a component that induces corrosion of the metal foil layer, such as an electrolyte solution.
[0138] In addition, when the adhesive layer 5 is a cured product of a resin composition containing at least one selected from the group consisting of a compound having an isocyanate group, a compound having an oxazoline group, and an epoxy resin, and the acid-modified polyolefin, the acid-modified polyolefin functions as the main agent, and the compound having an isocyanate group, the compound having an oxazoline group, and the compound having an epoxy group each function as a curing agent.
[0139] The adhesive layer 5 may contain a modifier having a carbodiimide group.
[0140] When the adhesive layer 5 is laminated with the metal foil layer 3, the heat-sealable resin layer 4, or the like to produce the packaging material for an electricity storage device 10 of the present disclosure, a pre-formed resin film may be used as the adhesive layer 5. Alternatively, the heat-sealable resin that forms the adhesive layer 5 may be formed into a film on the surface of the metal foil layer 3, the heat-sealable resin layer 4, or the like by extrusion molding, coating, or the like, to form the adhesive layer 5 from the resin film.
[0141] The thickness of the adhesive layer 5 is preferably about 50 μm or less, about 40 μm or less, about 30 μm or less, about 20 μm or less, or about 5 μm or less. The thickness of the adhesive layer 5 is preferably about 0.1 μm or more, or about 0.5 μm or more. The thickness of the adhesive layer 5 is preferably about 0.1 to 50 μm, about 0.1 to 40 μm, about 0.1 to 30 μm, about 0.1 to 20 μm, about 0.1 to 5 μm, about 0.5 to 50 μm, about 0.5 to 40 μm, about 0.5 to 30 μm, about 0.5 to 20 μm, or about 0.5 to 5 μm. More specifically, in the case of adhesives such as those exemplified for the adhesive layer 2 or a cured product of an acid-modified polyolefin and a curing agent, the thickness is preferably about 1 to 10 μm, more preferably about 1 to 5 μm. Furthermore, when a resin exemplified for the heat-fusible resin layer 4 is used, the thickness is preferably about 2 to 50 μm, more preferably about 10 to 40 μm. When the adhesive layer 5 is an adhesive exemplified for the adhesive layer 2 or a cured product of a resin composition containing an acid-modified polyolefin and a curing agent, the adhesive layer 5 can be formed, for example, by applying the resin composition and curing it by heating or the like. When a resin exemplified for the heat-fusible resin layer 4 is used, the heat-fusible resin layer 4 and the adhesive layer 5 can be formed, for example, by extrusion molding.
[0142] [Surface Coating Layer 6] The packaging material for an electricity storage device according to the present disclosure may, if necessary, have a surface coating layer 6 on the substrate layer 1 (the side of the substrate layer 1 opposite to the metal foil layer 3) for the purpose of improving at least one of design, electrolyte resistance, scratch resistance, formability, etc. The surface coating layer 6 is a layer located on the outermost layer side of the packaging material for an electricity storage device when an electricity storage device is assembled using the packaging material for an electricity storage device.
[0143] The surface coating layer 6 may be made of, for example, a resin such as polyvinylidene chloride, polyester, polyamide, epoxy resin, acrylic resin, fluororesin, polyurethane, silicone resin, or phenolic resin, or a modified version of these resins. It may also be a copolymer of these resins or a modified version of the copolymer. It may also be a mixture of these resins. The resin is preferably a curable resin. That is, the surface coating layer 6 is preferably made of a cured product of a resin composition containing a curable resin.
[0144] When the resin forming the surface coating layer 6 is a curable resin, the resin may be either a one-component curable resin or a two-component curable resin, but is preferably a two-component curable resin. Examples of two-component curable resins include two-component curable polyurethane, two-component curable polyester, and two-component curable epoxy resin. Among these, two-component curable polyurethane is preferred.
[0145] Examples of two-component curing polyurethanes include polyurethanes containing a first component containing a polyol compound and a second component containing an isocyanate compound. Preferred examples of two-component curing polyurethanes include those containing a polyol, such as polyester polyol, polyether polyol, or acrylic polyol, as the first component and an aromatic or aliphatic polyisocyanate as the second component. Examples of polyurethanes include polyurethanes containing an isocyanate compound and a polyurethane compound obtained by reacting a polyol compound with an isocyanate compound in advance. Examples of polyurethanes include polyurethanes containing a polyol compound and a polyurethane compound obtained by reacting a polyol compound with an isocyanate compound in advance. Examples of polyurethanes include polyurethanes obtained by reacting a polyol compound with an isocyanate compound in advance and then curing the polyurethane compound with moisture, such as in the air. Polyol compounds preferably include polyester polyols having hydroxyl groups on the side chains in addition to the terminal hydroxyl groups of the repeating units. Examples of second components include aliphatic, alicyclic, aromatic, and araliphatic isocyanate compounds. Examples of isocyanate compounds include hexamethylene diisocyanate (HDI), xylylene diisocyanate (XDI), isophorone diisocyanate (IPDI), hydrogenated XDI (H6XDI), hydrogenated MDI (H12MDI), tolylene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), and naphthalene diisocyanate (NDI). Also included are polyfunctional isocyanate-modified compounds of one or more of these diisocyanates. Furthermore, polymers (e.g., trimers) can also be used as polyisocyanate compounds. Examples of such polymers include adducts, biurets, and nurates. It should be noted that an aliphatic isocyanate compound refers to an isocyanate that has an aliphatic group but does not have an aromatic ring, an alicyclic isocyanate compound refers to an isocyanate that has an alicyclic hydrocarbon group, and an aromatic isocyanate compound refers to an isocyanate that has an aromatic ring.The surface coating layer 6 is formed from polyurethane, which provides the electrical storage device packaging material with excellent electrolyte resistance.
[0146] The surface coating layer 6 may contain additives such as lubricants, flame retardants, antiblocking agents, antioxidants, light stabilizers, tackifiers, antistatic agents, and pigments, as necessary, in at least one of the surface and interior of the surface coating layer 6, depending on the functionality to be provided to the surface of the surface coating layer 6. Examples of additives include fine particles with an average particle size of approximately 0.5 nm to 5 μm. The average particle size of the additive is the median size measured with a laser diffraction / scattering particle size distribution analyzer.
[0147] The additive may be either inorganic or organic. The shape of the additive is not particularly limited, and examples thereof include spherical, fibrous, plate-like, amorphous, and scaly shapes.
[0148] Specific examples of additives include talc, silica, graphite, kaolin, montmorillonite, mica, hydrotalcite, silica gel, zeolite, aluminum hydroxide, magnesium hydroxide, zinc oxide, magnesium oxide, aluminum oxide, neodymium oxide, antimony oxide, titanium oxide, cerium oxide, calcium sulfate, barium sulfate, calcium carbonate, calcium silicate, lithium carbonate, calcium benzoate, calcium oxalate, magnesium stearate, alumina, carbon black, carbon nanotubes, high-melting-point nylon, acrylate resin, crosslinked acrylic, crosslinked styrene, crosslinked polyethylene, benzoguanamine, gold, aluminum, copper, and nickel. The additives may be used alone or in combination of two or more. Among these additives, silica, barium sulfate, and titanium oxide are preferred from the viewpoints of dispersion stability and cost. The additives may also be subjected to various surface treatments, such as insulation treatment and high-dispersibility treatment.
[0149] The method for forming the surface coating layer 6 is not particularly limited, and examples thereof include a method of applying a resin to form the surface coating layer 6. When an additive is blended into the surface coating layer 6, a resin mixed with the additive may be applied.
[0150] In the present disclosure, from the viewpoint of improving the formability of the exterior material for an electrical storage device, it is preferable that a lubricant be present on at least one of the surface and the interior of the surface coating layer 6. The lubricant is not particularly limited, but preferably an amide-based lubricant is used. Specific examples of amide-based lubricants include saturated fatty acid amides, unsaturated fatty acid amides, substituted amides, methylolamides, saturated fatty acid bisamides, unsaturated fatty acid bisamides, fatty acid ester amides, and aromatic bisamides. Specific examples of saturated fatty acid amides include lauric acid amide, palmitic acid amide, stearic acid amide, behenic acid amide, and hydroxystearic acid amide. Specific examples of unsaturated fatty acid amides include oleic acid amide and erucic acid amide. Specific examples of substituted amides include N-oleyl palmitic acid amide, N-stearyl stearic acid amide, N-stearyl oleic acid amide, N-oleyl stearic acid amide, and N-stearyl erucic acid amide. Specific examples of methylolamides include methylol stearic acid amide. Specific examples of saturated fatty acid bisamides include methylene bisstearic acid amide, ethylene biscapric acid amide, ethylene bislauric acid amide, ethylene bisstearic acid amide, ethylene bishydroxystearic acid amide, ethylene bisbehenic acid amide, hexamethylene bisstearic acid amide, hexamethylene bisbehenic acid amide, hexamethylene hydroxystearic acid amide, N,N'-distearyl adipamide, N,N'-distearyl sebacic acid amide, etc. Specific examples of unsaturated fatty acid bisamides include ethylene bisoleic acid amide, ethylene biserucic acid amide, hexamethylene bisoleic acid amide, N,N'-dioleyl adipamide, N,N'-dioleyl sebacic acid amide, etc. Specific examples of fatty acid ester amides include stearamidoethyl stearate, etc. Specific examples of aromatic bisamides include m-xylylene bisstearic acid amide, m-xylylene bishydroxystearic acid amide, and N,N'-distearylisophthalic acid amide.The lubricant may be used alone or in combination of two or more kinds, and it is preferable to use a combination of two or more kinds.
[0151] When a lubricant is present on the surface of the surface coating layer 6, the amount of the lubricant is not particularly limited, but may be, for example, about 3 mg / m 2 or more, preferably about 4 mg / m 2 Above, about 5mg / m 2 The amount of lubricant present on the surface of the surface coating layer 6 is, for example, about 15 mg / m 2 or less, preferably about 14 mg / m 2 Below, about 10mg / m 2 The preferred range of the amount of lubricant present on the surface of the surface coating layer 6 is 3 to 15 mg / m 2 Degree, 3-14mg / m 2 Degree, 3-10mg / m 2 Degree, 4-15mg / m 2 Degree, 4-14mg / m 2 degree, 4-10mg / m 2 degree, 5-15mg / m 2 Degree, 5-14mg / m 2 degree, 5-10mg / m 2 The degree of
[0152] The lubricant present on the surface of the surface coating layer 6 may be a lubricant exuded from the resin that constitutes the surface coating layer 6, or a lubricant applied to the surface of the surface coating layer 6.
[0153] The surface coating layer 6 contains a colorant, which allows the electrical storage device exterior material to be colored. Known colorants such as pigments and dyes can be used as the colorant. Only one type of colorant may be used, or two or more types may be mixed together.
[0154] The type of pigment is not particularly limited, and examples of organic pigments include azo-based, phthalocyanine-based, quinacridone-based, anthraquinone-based, dioxazine-based, indigothioindigo-based, perinone-perylene-based, isoindolenine-based, and benzimidazolone-based pigments. Examples of inorganic pigments include carbon black-based, titanium oxide-based, cadmium-based, lead-based, chromium oxide-based, and iron-based pigments. Other examples include finely powdered mica and fish scale foil.
[0155] Among colorants, carbon black is preferred for making the exterior material for an electricity storage device black, and mica is preferred from the viewpoint of dissipating heat generated from the electricity storage device.
[0156] The average particle size of the pigment is not particularly limited and may be, for example, about 0.03 to 5 μm, and preferably about 0.05 to 2 μm. The average particle size of the pigment is the median size measured with a laser diffraction / scattering particle size distribution analyzer.
[0157] The content of the colorant or pigment in the surface coating layer 6 is not particularly limited as long as it colors the exterior material for an electricity storage device, and may be, for example, about 5 to 60 mass %, and preferably about 10 to 40 mass %.
[0158] The thickness of the surface coating layer 6 is not particularly limited as long as the surface coating layer 6 exhibits the above-mentioned functions, and may be, for example, about 0.5 to 10 μm, and preferably about 1 to 5 μm.
[0159] 3. Manufacturing Method of Electrical Storage Device Exterior Material The manufacturing method of the electrical storage device exterior material is not particularly limited, as long as it can produce a laminate in which the layers of the electrical storage device exterior material of the present invention are stacked. A manufacturing method of an electrical storage device exterior material according to a first aspect of the present disclosure includes a step of obtaining a laminate in which, from the outside, at least a substrate layer, a metal foil layer, and a heat-sealable resin layer are stacked, and the root-mean-square gradient Sdq of at least one surface of the metal foil layer, measured using a laser microscope at a laser wavelength of 408 nm, is 0.28 or less. Furthermore, a manufacturing method of an electrical storage device exterior material according to a second aspect of the present disclosure includes a step of obtaining a laminate in which, from the outside, at least a substrate layer, a metal foil layer, and a heat-sealable resin layer are stacked, and the kurtosis Sku of at least one surface of the metal foil layer, measured using a laser microscope at a laser wavelength of 408 nm, is 4.00 or less. In addition, a method for producing an electrical storage device packaging material according to a third aspect of the present disclosure is configured with a laminate including, in order from the outside, at least a metal foil layer and a heat-sealable resin layer, and the skewness Ssk at a laser wavelength of 408 nm, measured using a laser microscope, of at least one surface of the metal foil layer is -0.25 or more and 0.25 or less. As described above, when the laminate constituting the electrical storage device packaging material according to the present disclosure does not include a base material layer, the method for producing an electrical storage device packaging material according to the present disclosure includes a step of obtaining a laminate including, in order from the outside, at least a metal foil layer and a heat-sealable resin layer.
[0160] An example of a manufacturing method for an exterior material for an electricity storage device according to the present disclosure is as follows. First, a laminate (hereinafter, sometimes referred to as "laminate A") is formed in which a base material layer 1, an adhesive layer 2, and a metal foil layer 3 are laminated in this order. Specifically, the laminate A can be formed by a dry lamination method in which an adhesive used to form the adhesive layer 2 is applied to the base material layer 1 or to the metal foil layer 3, the surface of which has been chemically treated as necessary, by a coating method such as gravure coating or roll coating, and then dried, and the metal foil layer 3 or the base material layer 1 is laminated thereon, and the adhesive layer 2 is cured.
[0161] Next, a heat-sealable resin layer 4 is laminated on the metal foil layer 3 of the laminate A. When the heat-sealable resin layer 4 is laminated directly on the metal foil layer 3, the heat-sealable resin layer 4 may be laminated on the metal foil layer 3 of the laminate A by a method such as thermal lamination or extrusion lamination. When an adhesive layer 5 is provided between the metal foil layer 3 and the heat-sealable resin layer 4, the adhesive layer 5 and the heat-sealable resin layer 4 may be laminated by, for example, (1) extrusion lamination, (2) thermal lamination, (3) sandwich lamination, or (4) dry lamination. Examples of the (1) extrusion lamination method include a method of laminating the adhesive layer 5 and the heat-sealable resin layer 4 by extruding them onto the metal foil layer 3 of the laminate A (co-extrusion lamination, tandem lamination), etc. Examples of the (2) thermal lamination method include a method in which a laminate having an adhesive layer 5 and a heat-sealable resin layer 4 is separately formed, and then laminated on the metal foil layer 3 of the laminate A, or a method in which a laminate having an adhesive layer 5 laminated on the metal foil layer 3 of the laminate A is formed, and then laminated on the heat-sealable resin layer 4. Examples of the (3) sandwich lamination method include a method in which a molten adhesive layer 5 is poured between the metal foil layer 3 of the laminate A and a heat-sealable resin layer 4 previously formed into a sheet, and then the laminate A and the heat-sealable resin layer 4 are bonded together via the adhesive layer 5. Examples of the (4) dry lamination method include a method in which an adhesive for forming the adhesive layer 5 is solution-coated on the metal foil layer 3 of the laminate A, and then dried or baked, and then the heat-sealable resin layer 4 previously formed into a sheet is laminated on the adhesive layer 5.
[0162] When the surface coating layer 6 is provided, the surface coating layer 6 is laminated on the surface of the base layer 1 opposite to the metal foil layer 3. The surface coating layer 6 can be formed, for example, by applying the above-mentioned resin that forms the surface coating layer 6 to the surface of the base layer 1. The order of the step of laminating the metal foil layer 3 on the surface of the base layer 1 and the step of laminating the surface coating layer 6 on the surface of the base layer 1 is not particularly limited. For example, after the surface coating layer 6 is formed on the surface of the base layer 1, the metal foil layer 3 may be formed on the surface of the base layer 1 opposite to the surface coating layer 6.
[0163] As described above, a laminate is formed which includes the optional surface coating layer 6, the base material layer 1, the optional adhesive layer 2, the metal foil layer 3, the optional adhesive layer 5, and the heat-fusible resin layer 4 in this order. In order to strengthen the adhesion of the optional adhesive layer 2 and the optional adhesive layer 5, the laminate may be further subjected to a heat treatment.
[0164] In the packaging material for an electricity storage device, each layer constituting the laminate may be subjected to a surface activation treatment such as corona treatment, blast treatment, oxidation treatment, ozone treatment, etc. as necessary to improve processability. For example, by subjecting the surface of the base material layer 1 opposite to the metal foil layer 3 to corona treatment, the printability of ink on the surface of the base material layer 1 can be improved.
[0165] 4. Uses of the Electricity Storage Device Exterior Material The electricity storage device exterior material of the present disclosure is used in a package for hermetically housing electricity storage device elements such as a positive electrode, a negative electrode, and an electrolyte. That is, an electricity storage device can be formed by housing an electricity storage device element including at least a positive electrode, a negative electrode, and an electrolyte in a package formed from the electricity storage device exterior material of the present disclosure. In other words, an electricity storage device can be formed by wrapping an electricity storage device element in the electricity storage device exterior material of the present disclosure.
[0166] Specifically, an electricity storage device using the electricity storage device packaging material is provided by covering an electricity storage device element including at least a positive electrode, a negative electrode, and an electrolyte with the electricity storage device packaging material of the present disclosure in a state in which metal terminals connected to each of the positive electrode and the negative electrode protrude outward, so that a flange portion (a region where the heat-sealable resin layers contact each other) can be formed around the periphery of the electricity storage device element, and then heat-sealing the heat-sealable resin layers of the flange portion to form a hermetic seal. Note that when an electricity storage device element is housed in a package formed from the electricity storage device packaging material of the present disclosure, the package is formed so that the heat-sealable resin portion of the electricity storage device packaging material of the present disclosure faces inside (the surface that contacts the electricity storage device element). A package may be formed by overlapping two electrical storage device exterior materials with the heat-sealable resin layers facing each other and heat-sealing the peripheral edges of the overlapped electrical storage device exterior materials, or by folding one electrical storage device exterior material over and overlapping the materials and heat-sealing the peripheral edges, as in the example shown in Fig. 5. When the materials are folded over and overlapped, the package may be formed by heat-sealing the sides other than the folded side to form a three-sided seal, as in the example shown in Fig. 5, or by folding over the material so as to form a flange and seal all four sides. When the innermost and outermost layers of the electrical storage device exterior material are heat-sealable resin layers, the package may be formed by heat-sealing the innermost heat-sealable resin layer and the outermost heat-sealable resin layer.
[0167] The electricity storage device element may be sealed with a lid in addition to the electricity storage device exterior material. That is, the electricity storage device exterior material and the lid constitute an exterior (an exterior for an electricity storage device) that seals the electricity storage device element. For example, the electricity storage device element may be housed inside a cylindrically configured electricity storage device exterior material, and the opening may be closed with the lid. In another example, the electricity storage device element connected to the lid may be housed inside a cylindrically configured electricity storage device exterior material that has an opening, and the opening may be closed with the lid. The lid and the electricity storage device exterior material are preferably joined by any means. From the viewpoint of reducing dead space between the electricity storage device element and the electricity storage device exterior material to improve the volumetric energy density of the electricity storage device, the electricity storage device exterior material is preferably wrapped around the electricity storage device element and the lid.
[0168] The lid body can be formed, for example, from a resin molded product, a metal molded product, an exterior material for an electricity storage device, or a combination thereof. In this disclosure, when the lid body is referred to as a resin molded product, this does not include an embodiment in which the lid body is formed solely from a film defined by JIS K6900-1994 [Plastics - Terminology]. When the lid body is a metal molded product, the lid body also functions as a metal terminal, so the metal terminal can be omitted. The lid body may be formed from a resin material and a conductive material.
[0169] Furthermore, a recess for accommodating an electricity storage device element may be formed in the electricity storage device packaging material by deep drawing or bulging molding. As shown in the example in Fig. 5, a recess may be provided in one electricity storage device packaging material and no recess may be provided in the other electricity storage device packaging material, or a recess may also be provided in the other electricity storage device packaging material.
[0170] The exterior material for an electricity storage device of the present disclosure can be suitably used in an electricity storage device such as a battery (including a condenser, a capacitor, etc.). The exterior material for an electricity storage device of the present disclosure may be used in either a primary battery or a secondary battery, but is preferably used in a secondary battery. The type of secondary battery to which the exterior material for an electricity storage device of the present disclosure is applied is not particularly limited, and examples include lithium ion batteries, lithium ion polymer batteries, all-solid-state batteries, semi-solid batteries, quasi-solid batteries, polymer batteries, all-resin batteries, lead-acid batteries, nickel-metal hydride batteries, nickel-cadmium batteries, nickel-iron batteries, nickel-zinc batteries, silver oxide-zinc batteries, metal-air batteries, polyvalent cation batteries, condensers, and capacitors. Among these secondary batteries, lithium ion batteries and lithium ion polymer batteries are suitable applications for the exterior material for an electricity storage device of the present disclosure.
[0171] The present disclosure will be described in detail below with reference to examples and comparative examples, but the present disclosure is not limited to the examples.
[0172] <Manufacturing of Sheathing Materials for Electricity Storage Devices> Example 1 A stretched nylon film (thickness: 25 μm) was prepared as the substrate layer. Furthermore, aluminum alloy foils A (thickness: 40 μm) having the surface properties (physical properties of the matte surface) and composition listed in Table 1 were prepared as the metal foil layer. The matte surface of the aluminum alloy foil faced the substrate layer, and the glossy surface faced the thermally adhesive resin layer. Details of the aluminum alloy foils used in the Examples and Comparative Examples will be described later. Using a two-component urethane adhesive (a polyol compound and an aromatic isocyanate compound), the stretched nylon film side of the aluminum alloy foil and the substrate layer were dry-laminated so that the adhesive layer had a thickness of 3 μm after curing, followed by aging treatment to produce a substrate layer / adhesive layer / metal foil layer laminate. Both sides of the aluminum alloy foil were subjected to a chemical conversion treatment. The chemical conversion treatment of the aluminum alloy foil was performed using a treatment solution consisting of a phenolic resin, a chromium fluoride compound, and phosphoric acid, with a chromium coating amount of 10 mg / m. 2 (dry mass) was applied to both sides of an aluminum alloy foil by roll coating, and then baked.
[0173] Next, maleic anhydride-modified polypropylene as an adhesive layer (thickness 22.5 μm) and random polypropylene as a heat-sealable resin layer (thickness 22.5 μm) were co-extruded onto the metal foil layer of each of the laminates obtained above, thereby laminating the adhesive layer / heat-sealable resin layer on the metal foil layer, thereby obtaining an exterior packaging material for an electricity storage device in which the base material layer / adhesive layer / metal foil layer / adhesive layer / heat-sealable resin layer were laminated in this order.
[0174] Example 2 An outer casing material for an electricity storage device was obtained in the same manner as in Example 1, except that aluminum alloy foil B (thickness: 40 μm) described below was used instead of aluminum alloy foil A.
[0175] Example 3 An exterior material for an electricity storage device was obtained in the same manner as in Example 1, except that aluminum alloy foil C (thickness: 40 μm) described below was used instead of aluminum alloy foil A.
[0176] Comparative Example 1 An outer casing material for an electricity storage device was obtained in the same manner as in Example 1, except that aluminum alloy foil E (thickness: 40 μm) described below was used instead of aluminum alloy foil A.
[0177] <Aluminum alloy foil> Details of the aluminum alloy foils used as the metal foil layer in the examples and comparative examples are as follows. Aluminum alloy foil A (used in Example 1): an aluminum alloy foil having the composition of JIS A8021 and the composition shown in Table 1, which was adjusted to have the surface properties shown in Table 1 by setting the rolling speed and tensile tension during rolling under predetermined conditions. Aluminum alloy foil B (used in Example 2): an aluminum alloy foil having the composition of JIS A8021 and the composition shown in Table 1 (with an increased Si content compared to Aluminum Alloy Foil A) was adjusted to have the surface properties shown in Table 1 by setting the rolling speed and tensile tension during rolling under predetermined conditions. Aluminum alloy foil C (used in Example 3): an aluminum alloy foil having the composition of JIS A8021 and the composition shown in Table 1 (with an even higher Si content than Aluminum Alloy Foil B) was adjusted to have the surface properties shown in Table 1 by setting the rolling speed and tensile tension during rolling under predetermined conditions. Aluminum alloy foil E (used in Comparative Example 1): Aluminum alloy foil having the composition of JIS standard A8006 and the composition of Table 1 was adjusted to have the surface properties of Table 1 by setting the rolling speed and tensile tension during rolling under predetermined conditions.
[0178] <Surface Properties of Metal Foil Layer (Laser Microscope)> For the matte surface of each aluminum alloy foil of the packaging materials for an electricity storage device in the Examples and Comparative Examples, the values of the root-mean-square gradient Sdq, kurtosis Sku, and skewness Ssk at a laser wavelength of 408 nm were measured using a laser microscope.
[0179] Each aluminum alloy foil was removed from each packaging material for an electricity storage device by the following procedure and used as the measurement object. The base material layer of the packaging material for an electricity storage device was manually peeled off to obtain a laminate of the aluminum alloy foil, an adhesive layer, and a heat-sealable resin layer. This laminate was then immersed in orthodichlorobenzene under the following conditions to remove the adhesive layer and the heat-sealable resin layer from the aluminum alloy foil. The surface of the aluminum alloy foil was washed multiple times with ethanol and left to dry, and the resulting aluminum alloy foil was used as the measurement object.
[0180] Next, the values of the root-mean-square gradient Sdq, kurtosis Sku, and skewness Ssk at a laser wavelength of 408 nm were measured for the matte surface of each aluminum alloy foil using a laser microscope under the following measurement conditions. The results are shown in Table 1. (Measurement conditions for laser microscope) Measurements were made under the following conditions with reference to ISO25178-2:2012. Laser microscope: VK-X250 (controller) VK-X260 (measuring unit) manufactured by Keyence Laser wavelength: 408 nm Measurement optical system: confocal optical system Objective lens magnification: 150x (numerical aperture N.A. 0.95) Zoom: x1x Measurement mode: 9 screens connected together (3 screens x 3 screens) Measurement size: standard (1024 data in X direction, 768 data in Y direction) The number of pixels per screen is 1024 points in the X direction, i.e., the MD direction of the laminate, and 768 points in the Y direction, i.e., the TD direction of the laminate, and the measurement area of the 9 screens is approximately 255 μm in the MD direction and approximately 185 μm in the TD direction. Measurement conditions: surface shape / high precision / double scan included Z-axis pitch was 0.08 μm. Data processing: reference plane setting (tilt correction) full area, waviness removal 1, smoothing (simple average 3 pixels x 3 pixels), height cut level medium
[0181] <Evaluation of formability> Each electrical storage device exterior material was cut into a square with a length (MD direction) of 170 mm and a width (TD direction) of 170 mm to prepare a test sample. The MD of the electrical storage device exterior material corresponded to the rolling direction (RD) of the aluminum alloy foil, and the TD of the electrical storage device exterior material corresponded to the TD of the aluminum alloy foil. This sample was placed in a 25°C environment in a rectangular molding die (female die, the surface of which had a maximum height roughness (nominal value of Rz) of 3.2 μm as specified in Table 2 of the surface roughness standard for comparison in JIS B 0659-1:2002, Annex 1 (Reference), corner R2.0 mm, ridge R1.0 mm) with a diameter of 100 mm (MD) x 110 mm (TD) and a corresponding molding die (male die, the surface of the ridgeline had a maximum height roughness (nominal value of Rz) of 1.6 μm as specified in Table 2 of the surface roughness standard for comparison in JIS B 0659-1:2002, Annex 1 (Reference), corner R2.0 mm, ridgeline R1.0 mm). The maximum height roughness (nominal Rz value) of the comparative surface roughness standard specimen, as specified in Table 2, is 3.2 μm. Using a corner R of 2.0 mm and a ridge R of 1.0 mm, a pressing pressure (surface pressure) of 0.5 MPa was applied to ten samples, with the molding depth varied in 0.5 mm increments from a molding depth of 0.5 mm. The test samples were placed on a female mold with the heat-sealable resin layer facing the male mold. The clearance between the male and female molds was 0.3 mm. The cold-formed samples were illuminated with a penlight in a darkroom to confirm the presence of pinholes or cracks in the aluminum alloy foil. The deepest molding depth at which no pinholes or cracks occurred in the exterior packaging material for an electricity storage device in any of the ten cold-formed samples was determined as the limit molding depth for that sample. The evaluation criteria for the formability of the packaging material for an electricity storage device were as follows, and the results are shown in Table 1.
[0182] (Formability evaluation criteria) A+: The limit forming depth is 13.5 mm or more. A: The limit forming depth is 11.0 mm or more and 13.0 mm or less. B: The limit forming depth is 8.5 mm or more and 10.5 mm or less. C: The limit forming depth is 6.0 mm or more and 8.0 mm or less. D: The limit forming depth is 5.5 mm or less.
[0183]
[0184] Example 4 An exterior material for a power storage device was obtained in the same manner as in Example 2, except that a base material layer (stretched nylon film (thickness 20 μm)) was used instead of the base material layer (stretched nylon film (thickness 25 μm)), an adhesive layer (maleic anhydride-modified polypropylene (thickness 20 μm)) was used instead of the adhesive layer (maleic anhydride-modified polypropylene (thickness 22.5 μm)), and a heat-sealable resin layer (random polypropylene (thickness 15 μm)) was used instead of the heat-sealable resin layer (random polypropylene (thickness 22.5 μm)). In this example, a base material layer (stretched nylon film (thickness 20 μm)) / adhesive layer (thickness 3 μm) / metal foil layer (aluminum alloy foil B (thickness is 40 μm)) / adhesive layer (maleic anhydride-modified polypropylene (thickness is 20 μm)) / heat-sealable resin layer (random polypropylene (thickness 15 μm)) was used instead of the adhesive layer (stretched nylon film (thickness 25 μm)). In Example 4, two types of lubricants, saturated fatty acid amide (behenic acid amide) and unsaturated fatty acid amide (erucic acid amide), were used in combination as the lubricant contained in the heat-sealable resin layer. The exterior packaging material for an electricity storage device of Example 4 was evaluated as having moldability at the same level as that of Example 2.
[0185] Example 5 A laminated film in which a base material layer (a polyethylene terephthalate film (thickness 12 μm) and a stretched nylon film (thickness 15 μm) are laminated with an adhesive layer (thickness 3 μm)) was used instead of a base material layer (stretched nylon film (thickness 25 μm)), an adhesive layer (maleic anhydride modified polypropylene (thickness 22.5 μm)) was used instead of an adhesive layer (maleic anhydride modified polypropylene (thickness 40 μm)), and a heat-sealable resin layer (random polypropylene (thickness 22.5 μm)) was used instead of a heat-sealable resin layer (random polypropylene (thickness 22.5 μm)). In the same manner as in Example 2, except that a laminated film (a polyethylene terephthalate film (thickness 12 μm) and a stretched nylon film (thickness 15 μm) laminated with an adhesive layer (thickness 3 μm)) / adhesive layer (thickness 3 μm) / metal foil layer (aluminum alloy foil B (thickness 40 μm)) / adhesive layer (maleic anhydride-modified polypropylene (thickness 40 μm)) / thermal adhesive resin layer (random polypropylene (thickness 40 μm)) was obtained. In the production of the electrical storage device casing material, the stretched nylon film side of the base material layer was bonded to the metal foil layer via the adhesive layer. In Example 5, a saturated fatty acid amide (behenic acid amide) and an unsaturated fatty acid amide (erucic acid amide) were used in combination as lubricants contained in the thermal adhesive resin layer. The electrical storage device casing material of Example 5 had a moldability evaluation similar to that of Example 1.
[0186] As described above, the present disclosure provides the following aspects of the invention. Item 1. A packaging material for an electricity storage device, which is composed of a laminate including, in order from the outside, at least an optional base material layer, a metal foil layer, and a heat-sealable resin layer, and which has a root-mean-square gradient Sdq of 0.28 or less at a laser wavelength of 408 nm measured with a laser microscope on at least one surface of the metal foil layer. Item 2. A packaging material for an electricity storage device, which is composed of a laminate including, in order from the outside, at least an optional base material layer, a metal foil layer, and a heat-sealable resin layer, and which has a kurtosis Sku of 4.00 or less at a laser wavelength of 408 nm measured with a laser microscope on at least one surface of the metal foil layer. Item 3. Item 4. The packaging material for an electricity storage device according to Item 1 or 3, wherein the packaging material is composed of a laminate including, in order from the outside, at least any substrate layer, a metal foil layer, and a heat-sealable resin layer, and wherein the skewness Ssk of at least one surface of the metal foil layer, measured using a laser microscope at a laser wavelength of 408 nm, is -0.25 or more and 0.25 or less. Item 5. The packaging material for an electricity storage device according to Item 1 or 2, wherein the skewness Ssk of at least one surface of the metal foil layer, measured using a laser microscope at a laser wavelength of 408 nm, is -0.25 or more and 0.25 or less. Item 6. Item 2. The packaging material for an electricity storage device according to Item 2 or 3, wherein a root-mean-square gradient Sdq at a laser wavelength of 408 nm, measured using a laser microscope, for at least one surface of the metal foil layer is 0.28 or less. Item 7. The packaging material for an electricity storage device according to any one of Items 1 to 6, wherein the surface of the metal foil layer is a matte surface. Item 8. The packaging material for an electricity storage device according to any one of Items 1 to 7, wherein the metal foil layer includes at least one of an aluminum alloy foil and a stainless steel foil. Item 9. The packaging material for an electricity storage device according to any one of Items 1 to 8, further comprising an adhesive layer between the base layer and the metal foil layer.Item 10. The packaging material for an electricity storage device according to any one of Items 1 to 9, further comprising an adhesive layer between the metal foil layer and the heat-sealable resin layer. Item 11. The packaging material for an electricity storage device according to any one of Items 1 to 10, wherein the base layer includes a laminate of a polyester film and a polyamide film, a laminate of a polyester film and a polyester film, or a laminate of a polyamide film and a polyamide film. Item 12. The packaging material for an electricity storage device according to any one of Items 1 to 11, wherein the thickness of the laminate is 155 μm or less. Item 13. The packaging material for an electricity storage device according to any one of Items 1 to 12, wherein the thickness of the laminate is 155 μm or more and 190 μm or less. Item 14. Alternatively, the packaging material for an electricity storage device according to any one of Items 1 to 13, wherein the thickness of the laminate is 190 μm or more and 300 μm or less. Item 15. Item 16. The electrical storage device packaging material according to any one of Items 1 to 15, wherein at least one of the surface and interior of the base layer contains two or more types of lubricants. Item 17. The electrical storage device packaging material according to any one of Items 1 to 16, wherein at least one of the surface and interior of the base layer contains at least two types of lubricants selected from the group consisting of saturated fatty acid amides, unsaturated fatty acid amides, substituted amides, methylol amides, saturated fatty acid bisamides, unsaturated fatty acid bisamides, fatty acid ester amides, and aromatic bisamides. Item 18. The electrical storage device packaging material according to any one of Items 1 to 17, wherein the base layer has a thickness of 35 μm or less. Item 19. The electrical storage device packaging material according to any one of Items 1 to 18, wherein the metal foil layer has a thickness of 50 μm or less. Item 20. Item 21. The packaging material for an electricity storage device according to any one of items 1 to 20, wherein the metal foil layer has a thickness of 50 μm or more and 200 μm or less. Item 22. The packaging material for an electricity storage device according to any one of items 1 to 20, wherein the heat-sealable resin layer is made of a resin containing a polyolefin skeleton.Item 22. The packaging material for an electricity storage device according to any one of Items 1 to 21, wherein the heat-sealable resin layer contains at least one selected from the group consisting of polyolefins, cyclic polyolefins, acid-modified polyolefins, and acid-modified cyclic polyolefins. Item 23. The packaging material for an electricity storage device according to any one of Items 1 to 22, wherein the heat-sealable resin layer is formed from a blend polymer combining two or more types of resins. Item 24. The packaging material for an electricity storage device according to any one of Items 1 to 23, wherein the heat-sealable resin layer is formed from two or more layers of the same or different resins. Item 25. The packaging material for an electricity storage device according to any one of Items 1 to 24, wherein two or more types of lubricants are present on at least one of the surface and the interior of the heat-sealable resin layer. Item 26. Item 27. The packaging material for an electricity storage device according to any one of Items 1 to 26, wherein at least two selected from the group consisting of saturated fatty acid amides, unsaturated fatty acid amides, substituted amides, methylol amides, saturated fatty acid bisamides, unsaturated fatty acid bisamides, fatty acid ester amides, and aromatic bisamides are present on at least one of the surface and interior of the heat-sealable resin layer. Item 28. The packaging material for an electricity storage device according to any one of Items 1 to 27, further comprising an adhesive layer between the base material layer and the metal foil layer, the adhesive layer containing a colorant. Item 29. The packaging material for an electricity storage device according to any one of Items 1 to 28, further comprising a colored layer between the base material layer and the metal foil layer. Item 30. The packaging material for an electricity storage device according to any one of Items 1 to 29, further comprising a surface coating layer on the side of the base material layer opposite the metal foil layer. Item 31. Item 31. The electrical storage device packaging material according to Item 30, wherein the surface coating layer contains a colorant. Item 32. The electrical storage device packaging material according to Item 30, wherein the surface coating layer contains titanium oxide. Item 33. The electrical storage device packaging material according to Item 30, wherein the surface coating layer contains silica.Item 34. The packaging material for an electricity storage device according to Item 30, wherein the surface coating layer contains at least one selected from the group consisting of talc, silica, graphite, kaolin, montmorillonite, mica, hydrotalcite, silica gel, zeolite, aluminum hydroxide, magnesium hydroxide, zinc oxide, magnesium oxide, aluminum oxide, neodymium oxide, antimony oxide, titanium oxide, cerium oxide, calcium sulfate, barium sulfate, calcium carbonate, calcium silicate, lithium carbonate, calcium benzoate, calcium oxalate, magnesium stearate, alumina, carbon black, carbon nanotubes, high-melting-point nylon, acrylate resin, cross-linked acrylic, cross-linked styrene, cross-linked polyethylene, benzoguanamine, gold, aluminum, copper, and nickel. Item 36. A method for producing an electrical storage device packaging material, comprising a step of obtaining a laminate in which, from the outside, at least an arbitrary base material layer, a metal foil layer, and a heat-sealable resin layer are laminated, wherein the root-mean-square gradient Sdq at a laser wavelength of 408 nm, measured using a laser microscope, for at least one surface of the metal foil layer is 0.28 or less. Item 36. A method for producing an electrical storage device packaging material according to Item 35, further comprising an adhesive layer between the metal foil layer and the heat-sealable resin layer, wherein the adhesive layer and the heat-sealable resin layer are laminated by (1) extrusion lamination, (2) thermal lamination, (3) sandwich lamination, or (4) dry lamination. Item 37. A method for producing an electrical storage device packaging material according to Item 35 or 36, further comprising an adhesive layer between the metal foil layer and the heat-sealable resin layer, wherein the heat-sealable resin layer is formed of two or more layers of the same or different resins. Item 38. Item 35. An electricity storage device, wherein an electricity storage device element including at least a positive electrode, a negative electrode, and an electrolyte is housed in a package formed from the exterior packaging material for an electricity storage device according to any one of Items 1 to 34.
[0187] 1 Base material layer 2 Adhesive layer 3 Metal foil layer 4 Heat-fusible resin layer 5 Adhesive layer 6 Surface coating layer 10 Exterior material for power storage device
Claims
1. An exterior material for an electricity storage device, which is composed of a laminate having, in order from the outside, at least a base layer, a metal foil layer, and a heat-sealable resin layer, and the root-mean-square gradient Sdq of at least one surface of the metal foil layer at a laser wavelength of 408 nm, measured using a laser microscope, is 0.28 or less.
2. An exterior material for an electricity storage device, which is composed of a laminate having, in order from the outside, at least a base layer, a metal foil layer, and a heat-sealable resin layer, and the kurtosis (Sku) of at least one surface of the metal foil layer at a laser wavelength of 408 nm measured using a laser microscope is 4.00 or less.
3. An exterior material for an electricity storage device, which is composed of a laminate including, in order from the outside, at least a base layer, a metal foil layer, and a heat-sealable resin layer, and the skewness Ssk of at least one surface of the metal foil layer at a laser wavelength of 408 nm, measured using a laser microscope, is greater than or equal to -0.25 and less than or equal to 0.
25.
4. An exterior material for an electricity storage device according to claim 1 or 3, wherein the kurtosis Sku of at least one surface of the metal foil layer at a laser wavelength of 408 nm measured using a laser microscope is 4.00 or less.
5. The exterior packaging material for an electricity storage device according to claim 1 or 2, wherein the skewness Ssk of at least one surface of the metal foil layer at a laser wavelength of 408 nm, measured using a laser microscope, is -0.25 or more and 0.25 or less.
6. The exterior packaging material for an electricity storage device according to claim 2 or 3, wherein the root-mean-square gradient Sdq of at least one surface of the metal foil layer at a laser wavelength of 408 nm, measured using a laser microscope, is 0.28 or less.
7. The exterior packaging material for an electricity storage device according to any one of claims 1 to 3, wherein the surface of the metal foil layer is a matte surface.
8. The exterior packaging material for an electricity storage device according to any one of claims 1 to 3, wherein the metal foil layer includes at least one of an aluminum alloy foil and a stainless steel foil.
9. The packaging material for an electricity storage device according to any one of claims 1 to 3, further comprising an adhesive layer between the base layer and the metal foil layer.
10. The packaging material for an electricity storage device according to any one of claims 1 to 3, further comprising an adhesive layer between the metal foil layer and the heat-sealable resin layer.
11. The exterior material for an electricity storage device according to any one of claims 1 to 3, wherein the base layer comprises a laminate of a polyester film and a polyamide film, a laminate of a polyester film and a polyester film, or a laminate of a polyamide film and a polyamide film.
12. The exterior packaging material for an electricity storage device according to any one of claims 1 to 3, wherein the thickness of the laminate is 155 μm or less.
13. The exterior packaging material for an electricity storage device according to any one of claims 1 to 3, wherein the thickness of the laminate is 155 μm or more and 190 μm or less.
14. The exterior packaging material for an electricity storage device according to any one of claims 1 to 3, wherein the thickness of the laminate is 190 μm or more and 300 μm or less.
15. The exterior material for an electricity storage device according to any one of claims 1 to 3, wherein two or more types of lubricants are present on at least one of the surface and the interior of the base layer.
16. The exterior material for an electricity storage device according to any one of claims 1 to 3, wherein at least two types selected from the group consisting of saturated fatty acid amides, unsaturated fatty acid amides, substituted amides, methylol amides, saturated fatty acid bisamides, unsaturated fatty acid bisamides, fatty acid ester amides, and aromatic bisamides are present on at least one of the surface and interior of the base layer.
17. The exterior packaging material for an electricity storage device according to any one of claims 1 to 3, wherein the thickness of the base layer is 35 μm or less.
18. The exterior packaging material for an electricity storage device according to any one of claims 1 to 3, wherein the thickness of the base layer is 35 μm or more and 100 μm or less.
19. The exterior packaging material for an electricity storage device according to any one of claims 1 to 3, wherein the metal foil layer has a thickness of 50 μm or less.
20. The exterior packaging material for an electricity storage device according to any one of claims 1 to 3, wherein the metal foil layer has a thickness of 50 μm or more and 200 μm or less.
21. An exterior packaging material for an electricity storage device according to any one of claims 1 to 3, wherein the heat-sealable resin layer is composed of a resin containing a polyolefin skeleton.
22. An exterior material for an electricity storage device described in any one of claims 1 to 3, wherein the heat-sealable resin layer contains at least one selected from the group consisting of polyolefins, cyclic polyolefins, acid-modified polyolefins, and acid-modified cyclic polyolefins.
23. An exterior packaging material for an electricity storage device according to any one of claims 1 to 3, wherein the heat-sealable resin layer is formed from a blend polymer of two or more types of resin.
24. An exterior packaging material for an electricity storage device according to any one of claims 1 to 3, wherein the heat-sealable resin layer is formed of two or more layers of the same or different resins.
25. An exterior material for an electricity storage device according to any one of claims 1 to 3, wherein two or more types of lubricants are present on at least one of the surface and the interior of the heat-sealable resin layer.
26. An exterior material for an electricity storage device according to any one of claims 1 to 3, wherein at least two types selected from the group consisting of saturated fatty acid amides, unsaturated fatty acid amides, substituted amides, methylol amides, saturated fatty acid bisamides, unsaturated fatty acid bisamides, fatty acid ester amides, and aromatic bisamides are present on at least one of the surface and interior of the heat-sealable resin layer.
27. The exterior material for an electricity storage device according to any one of claims 1 to 3, which is colored.
28. The exterior packaging material for an electricity storage device according to any one of claims 1 to 3, further comprising an adhesive layer between the base material layer and the metal foil layer, the adhesive layer containing a colorant.
29. The exterior packaging material for an electricity storage device according to any one of claims 1 to 3, further comprising a colored layer between the base layer and the metal foil layer.
30. An exterior material for an electricity storage device according to any one of claims 1 to 3, further comprising a surface coating layer on the side of the base material layer opposite the metal foil layer.
31. The exterior packaging material for an electricity storage device according to claim 30, wherein the surface coating layer contains a colorant.
32. The exterior packaging material for an electricity storage device according to claim 30, wherein the surface coating layer contains titanium oxide.
33. The exterior packaging material for an electricity storage device according to claim 30, wherein the surface coating layer contains silica.
34. The exterior material for an electricity storage device according to claim 30, wherein the surface coating layer contains at least one selected from the group consisting of talc, silica, graphite, kaolin, montmorillonite, mica, hydrotalcite, silica gel, zeolite, aluminum hydroxide, magnesium hydroxide, zinc oxide, magnesium oxide, aluminum oxide, neodymium oxide, antimony oxide, titanium oxide, cerium oxide, calcium sulfate, barium sulfate, calcium carbonate, calcium silicate, lithium carbonate, calcium benzoate, calcium oxalate, magnesium stearate, alumina, carbon black, carbon nanotubes, high melting point nylon, acrylate resin, cross-linked acrylic, cross-linked styrene, cross-linked polyethylene, benzoguanamine, gold, aluminum, copper, and nickel.
35. A method for producing an exterior material for an electricity storage device, comprising the steps of obtaining a laminate in which, from the outside, at least a base layer, a metal foil layer, and a heat-sealable resin layer are laminated, and the root-mean-square gradient Sdq of at least one surface of the metal foil layer at a laser wavelength of 408 nm, as measured using a laser microscope, is 0.28 or less.
36. A method for producing an exterior material for an electricity storage device as described in claim 35, further comprising providing an adhesive layer between the metal foil layer and the heat-sealable resin layer, and the adhesive layer and the heat-sealable resin layer are laminated by (1) an extrusion lamination method, (2) a thermal lamination method, (3) a sandwich lamination method, or (4) a dry lamination method.
37. A method for producing an exterior material for an electrical storage device as described in claim 35 or 36, further comprising an adhesive layer between the metal foil layer and the heat-sealable resin layer, the heat-sealable resin layer being formed of two or more layers of the same or different resins.
38. An electricity storage device, comprising an electricity storage device element having at least a positive electrode, a negative electrode, and an electrolyte, housed in a packaging body formed from the exterior material for an electricity storage device according to any one of claims 1 to 3.
Citation Information
Patent Citations
Exterior material for power storage device and power storage device
JP2016081856A
Battery packaging materials and batteries
JP2022126645A
Cell pouch with excellent flexibility and secondary battery comprising the same
KR1020170014246A
Exterior material for power storage device, manufacturing method thereof, and power storage device
WO2020138060A1