Battery, battery pack, electronic device, and energy storage system
By using a composite current collector, negative active material layer and porous film structure in the negative electrode sheet of the battery, the problems of poor battery cycle performance and safety hazards are solved, achieving higher cycle capacity retention rate and safety of use, and promoting the commercialization process of batteries.
Patent Information
- Application Number
- PCT/CN2023/141426
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-26
- Filing Date
- 2023-12-25
- Publication Date
- 2024-10-31
AI Technical Summary
Existing batteries have poor cycle performance and safety hazards, which affect battery life and hinder battery commercialization.
Design a battery, in which the negative electrode sheet includes a composite current collector, a negative active material layer and a porous film. The porous film is composed of a polymer and porous ceramic particles, and the carbon coating layer is covered between the metal foil and the negative active material layer. Reduce the contact between the negative active material and the electrolyte, reduce side reactions, and improve cycle capacity retention and use safety.
It effectively improves the cycle capacity retention rate and cycle life of the battery, and enhances the safety of the battery. The stability and low cost of the porous ceramic particles are conducive to the mass production and commercialization of the battery.
Smart Images

Figure CN2023141426_31102024_PF_FP_ABST
Abstract
Description
Batteries, battery packs, electronic devices and energy storage systems
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to a Chinese patent application filed with the Patent Office of China on April 26, 2023, with application number 202310471939.5, entitled “Batteries, battery packs, electronic devices and energy storage systems”, the entire contents of which are incorporated herein by reference. Technical Field
[0003] The present application relates to the field of battery technology, and in particular to a battery, a battery pack and electronic equipment using the battery, and an energy storage system using the battery pack. Background Art
[0004] With the development of economy and technology, most electronics industries (such as portable electronic devices, drones, and electric vehicles) urgently need energy storage devices with higher energy density, higher power density, longer cycle life, and greater safety. However, existing batteries have poor cycle performance and pose safety risks, which shorten battery life and hinder the commercialization of batteries.
[0005] Summary of the Invention
[0006] In view of this, in order to solve at least one of the above defects, an embodiment of the present application provides a battery, wherein the negative electrode can effectively improve the battery's cycle capacity retention rate and battery cycle life, and improve the battery's safety.
[0007] In addition, embodiments of the present application also provide a battery pack and electronic device using the above-mentioned battery, as well as an energy storage system using the above-mentioned battery pack.
[0008] In a first aspect, an embodiment of the present application provides a battery comprising a positive electrode sheet, a negative electrode sheet, and a separator, wherein the separator is disposed between the positive electrode sheet and the negative electrode sheet. The negative electrode sheet comprises a composite current collector, a negative electrode active material layer, and a porous film. The composite current collector comprises a metal foil and a carbon coating layer disposed on a surface of the metal foil, wherein the negative electrode active material layer is disposed on a side of the carbon coating layer facing away from the metal foil. The porous film is disposed on a side of the negative electrode active material layer facing away from the composite current collector, wherein the porous film comprises a polymer and porous ceramic particles, wherein the porous ceramic particles are dispersed in the polymer.
[0009] In the battery of the present application, the porous film in the negative electrode covers the negative electrode active material layer, which effectively reduces the direct contact between the negative electrode active material in the negative electrode active material layer and the electrolyte, thereby reducing the side reaction between the negative electrode active material and the electrolyte, slowing down the growth rate of the negative electrode electrolyte interface film (SEI film) during the charge and discharge cycle, and reducing the loss of active ions in the battery cycle, slowing down the continuous reduction of the battery capacity during the cycle, thereby improving the battery cycle capacity retention rate and its overall cycle life. The porous structure of the porous ceramic particles themselves and the porous structure formed after the porous film is formed enable the negative electrode plate to have a certain liquid absorption capacity, which is conducive to improving the battery's long-term charge and discharge cycle retention rate, and the porous structure of the porous ceramic particles themselves is conducive to the dispersed distribution of the pores in the porous film, which is conducive to avoiding the problem that the particles aggregate so that the local area of the porous film cannot form pores and the area cannot be ion deintercalated, thereby helping to ensure the energy density of the battery. Furthermore, the porous ceramic particles themselves offer stable performance, excellent erosion resistance, and a long service life, ensuring excellent stability of the porous film during battery use. Furthermore, the porous ceramic particles offer the advantage of low cost, facilitating mass production and commercialization of batteries. Furthermore, a carbon coating layer is provided between the metal foil and the negative electrode active material layer, which helps reduce the sheet resistance of the negative electrode and improves the interfacial adhesion between the negative electrode active material layer and the current collector, reducing the risk of the negative electrode active material layer shedding during battery cycling, thereby improving battery safety.
[0010] Based on the first aspect, in a possible implementation, the carbon coating layer includes one or both of graphene and carbon black.
[0011] In the above possible implementation methods, graphene has extremely high electronic conductivity, and its two-dimensional structure can more fully build a conductive network in the electrode, which is manifested as high atomic utilization. Carbon black has fine particles, dense network chains, large specific surface area, and many particles per unit mass, which is conducive to the formation of a chain conductive structure in the electrode and is a classic conductive agent. Therefore, the carbon coating layer of the above material is convenient for reducing the membrane resistance of the negative electrode. When carbon black and graphene are compounded, it can effectively reduce the agglomeration of graphene and improve the uniformity of the carbon coating layer. At the same time, it can also enhance the adhesion of the carbon coating layer to the aluminum foil current collector, which is conducive to avoiding the detachment of the carbon coating layer during battery cycling.
[0012] Based on the first aspect, in a possible implementation, the thickness of the carbon coating layer is 1 μm to 1.5 μm.
[0013] In the above possible implementations, the carbon coating layer of the above thickness is conducive to reducing the thickness of the negative electrode plate while ensuring the conductive performance. Among them, a carbon coating layer with a thickness of less than 1μm is more difficult to form on the one hand, and on the other hand, it is difficult to ensure the continuity and conductivity of the carbon coating layer. A carbon coating layer with a thickness greater than 1.5μm is not conducive to the carbon coating layer being embedded in the negative electrode active material layer during rolling, resulting in poor contact between the carbon coating layer and the negative electrode active material layer. On the other hand, it is also a waste of material and is not conducive to reducing the thickness of the plate and miniaturizing the overall battery structure.
[0014] Based on the first aspect, in a possible implementation, the porous ceramic particles include one or more of siliceous silicate materials, aluminosilicate materials, diatomaceous earth materials, coarse ceramic materials, pure siliceous materials, corundum, and corundum.
[0015] In the above possible implementations, the porous ceramic particles of the above material themselves have a porous structure, which facilitates the formation and dispersion of the porous structure in the porous film. At the same time, the porous ceramic particles of the above material are easy to obtain, which is conducive to cost reduction.
[0016] Based on the first aspect, in one possible implementation, the pore size of the porous ceramic particles is 2 nm to 50 nm.
[0017] In the above possible implementations, porous ceramic particles with the above pore size can better deintercalate active ions while reducing direct contact between the negative electrode active material and the electrolyte, thereby helping to ensure battery capacity. Specifically, if the pore size in the porous ceramic particles is too large, it is easy to increase the side reactions in the battery, affecting the battery cycle life. If the pore size in the porous ceramic particles is too small, it will affect the deintercalation of active ions such as sodium ions, affecting the battery cycle life and the battery's first coulombic efficiency.
[0018] Based on the first aspect, in a possible implementation, the particle size of the porous ceramic particles is 100 nm to 200 nm.
[0019] In the above possible implementations, porous ceramic particles of the aforementioned particle size facilitate uniform coating to form a porous film, while also facilitating uniform thickness across the porous film. Furthermore, if the particle size of the porous ceramic particles is too small, the contact surface for side reactions in the battery may increase, thereby reducing the battery's cycle life. If the particle size of the porous ceramic particles is too large, it may affect sodium ion intercalation and deintercalation, leading to a reduction in the initial Coulombic efficiency.
[0020] Based on the first aspect, in a possible implementation, the high molecular polymer includes one or more of polyvinylidene fluoride, acrylic esters, polyvinyl alcohol, polytetrafluoroethylene, and polyurethane.
[0021] In the above possible implementation, the porous film contains a high molecular polymer of the above material, so that the porous film has good flexibility, which is beneficial to avoid cracking of the porous film during use of the negative electrode plate.
[0022] Based on the first aspect, in a possible implementation, in the porous film, the mass percentage of the high molecular polymer is 50% to 80%, the mass percentage of the porous ceramic particles is 20% to 50%, and the porosity of the porous film is 40% to 80%.
[0023] In the above possible implementations, the porous film with a specific content of porous ceramic particles and high molecular polymers is conducive to ensuring the distribution of the porous structure while making the porous film have good flexibility, which is conducive to reducing the risk of cracking of the porous film while ensuring the battery capacity and improving the battery cycle life, thereby improving the overall service life of the battery. Too high a porosity will also lead to an increase in side reactions in the battery, affecting the cycle life of the battery, while too low a porosity will affect the deintercalation of active ions and reduce the battery's first coulombic efficiency and cycle life. In summary. A specific porosity is also conducive to further improving the flexibility of the porous film and helping to ensure battery performance.
[0024] Based on the first aspect, in a possible implementation manner, the thickness of the porous film is 1 μm to 10 μm.
[0025] In the above possible implementations, the porous film of the specified thickness facilitates film formation and reduces the risk of cracking during use of the negative electrode. However, excessively thick porous films can also affect battery pack margin design and increase battery internal resistance.
[0026] Based on the first aspect, in a possible implementation, the negative electrode active material layer includes hard carbon.
[0027] Among the possible implementation methods mentioned above, hard carbon has abundant carbon sources, low cost, non-toxicity and environmental protection, which facilitates the mass production and commercialization of negative electrode sheets. At the same time, hard carbon has low sodium storage potential and high sodium storage capacity, which facilitates the design of sodium ion batteries.
[0028] Based on the first aspect, in a possible implementation, the negative electrode active material layer further includes a conductive carbon material and polytetrafluoroethylene, and the mass ratio of hard carbon, conductive carbon material and polytetrafluoroethylene is 8:1:1.
[0029] In the above possible implementations, the negative electrode active material layer with the above specific composition is applied to the battery, which is beneficial for the battery to have better discharge capacity and cycle performance.
[0030] Based on the first aspect, in a possible implementation, the conductive carbon material includes carbon black and carbon nanotubes, and the mass ratio of the carbon black to the carbon nanotubes is 10:1.
[0031] In the above possible implementation, the carbon nanotubes in the above specific ratio dispersed among the carbon black particles can produce a synergistic conductive effect so that the negative electrode plate obtains higher electronic conductivity.
[0032] A second aspect of the present application provides a battery pack comprising a plurality of the above-described batteries, with any two batteries connected in series or in parallel. Because the negative electrodes in the above-described batteries are beneficial for improving the overall cycle life, long-term charge-discharge cycle retention, and safety of the batteries, they are also beneficial for improving the service life and safety of the battery packs incorporating the above-described batteries.
[0033] A third aspect of the present application provides an electronic device comprising a housing and a battery as described above, the battery being mounted within the housing. Because the negative electrode in the battery is beneficial for improving the overall cycle life, long-term charge-discharge cycle retention, and safety of the battery, it is beneficial for improving the service life and safety of electronic devices using the battery.
[0034] In a fourth aspect, an embodiment of the present application provides an energy storage system comprising a power converter and the aforementioned battery pack. The power converter is electrically connected to the battery pack, and is used to convert the voltage output by the battery pack into power and output it to a power grid or a load, and / or to convert the voltage output by an external power source into power and output it to the battery pack. Because the negative electrode in the aforementioned battery is beneficial for improving the overall cycle life of the battery, the retention rate of long-term charge and discharge cycles, and the safety of use, it is beneficial for improving the service life and safety of the energy storage system using the aforementioned battery pack. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] FIG1 is a schematic cross-sectional view of a negative electrode sheet according to an embodiment of the present application.
[0036] FIG2 is a schematic diagram of a battery according to an embodiment of the present application.
[0037] FIG3 is a schematic diagram of an electronic device according to an embodiment of the present application.
[0038] FIG4 is a graph showing the average value of the negative electrode sheet resistance measured in Comparative Example 1 and Examples 1-7 of the present application.
[0039] FIG5 is a cycle capacity retention curve of the batteries of Comparative Example 2, Example 6, and Examples 8-10 of the present application.
[0040] Description of main component symbols
[0041] Negative electrode 100
[0042] Composite current collector 11
[0043] Negative electrode active material layer 13
[0044] porous film 15
[0045] Metal Foil 111
[0046] Carbon coating 112
[0047] Battery cell 200a
[0048] Positive electrode 30
[0049] Isolation film 40
[0050] Battery 200
[0051] Electrolyte 50
[0052] Package 60
[0053] Electronic equipment 300
[0054] Housing 301 DETAILED DESCRIPTION
[0055] The following specific embodiments illustrate the implementation of the present application. Those skilled in the art can easily understand other advantages and effects of the present application from the contents disclosed in this specification. Although the description of the present application will be introduced in conjunction with the embodiments, this does not mean that the features of this application are limited to the implementation. On the contrary, the purpose of introducing the application in conjunction with the implementation is to cover other options or modifications that may be extended based on the claims of the present application. In order to provide an in-depth understanding of the present application, the following description will contain many specific details. The present application can also be implemented without using these details. In addition, in order to avoid confusion or blurring the focus of the present application, some specific details will be omitted in the description. It should be noted that the embodiments in the present application and the features in the embodiments can be combined with each other unless there is a conflict.
[0056] Hereinafter, if used, the terms "first," "second," etc., are used for descriptive purposes only and are not to be construed as indicating or implying relative importance or implicitly specifying the number of the technical features being referred to. Thus, a feature qualified as "first," "second," etc. may explicitly or implicitly include one or more of such features. In the description of this application, unless otherwise specified, "plurality" means two or more.
[0057] The following describes the embodiments of the present application in conjunction with the accompanying drawings. Unless otherwise specified, the data range values recorded in this application should include the end values.
[0058] Electrolyte interface film: During the first charge and discharge process of the battery, the electrode material and the electrolyte react at the solid-liquid interface to form a passivation layer covering the surface of the electrode material. The passivation layer formed on the negative electrode during the first charge and discharge of the battery is the solid electrolyte interface (SEI) film. The formation of the SEI film is a process that consumes active ions. Take sodium-ion batteries as an example: During the charge and discharge process of sodium-ion batteries, especially as the number of cycles increases, the SEI film will be continuously destroyed and rebuilt. During this series of processes, the thickness of the SEI film itself will continue to increase, which means that the active sodium ions in the battery will continue to be consumed, resulting in a decrease in the capacity of the sodium battery, resulting in poor cycle performance of the battery, affecting the service life of the battery, especially the cycle life of sodium-ion batteries with hard carbon as the negative electrode.
[0059] In view of this, an embodiment of the present application provides a negative electrode plate. As shown in FIG1 , the negative electrode plate 100 includes a composite current collector 11, a negative electrode active material layer 13, and a porous film 15. The negative electrode active material layer 13 is provided on the surface of the carbon-coated layer 112 facing away from the metal foil 111, and the porous film 15 is provided on the side of the negative electrode active material layer 13 facing away from the composite current collector 11. The porous film 15 includes a polymer and porous ceramic particles, and the porous ceramic particles are dispersed in the polymer.
[0060] A carbon coating layer 112 is provided between the negative electrode active material layer 13 and the metal foil 111, which helps to reduce the sheet resistance of the negative electrode plate and improve the interface bonding between the negative electrode active material layer and the current collector. When the negative electrode plate is used in a battery, the risk of the negative electrode active material layer falling off during the battery cycle is reduced, thereby helping to improve the safety of the negative electrode plate. The porous film 15 covers the negative electrode active material layer 13. When the negative electrode plate is used in a battery, it effectively reduces the direct contact between the negative electrode active material in the negative electrode active material layer and the electrolyte, thereby reducing the side reactions between the negative electrode active material and the electrolyte, slowing the growth rate of the negative electrode electrolyte interface film (SEI film) during the charge and discharge cycle, and reducing the loss of active ions during the battery cycle, slowing down the continuous reduction of battery capacity during the cycle, thereby improving the overall cycle life of the battery. The porous structure of the porous ceramic particles themselves and the porous structure formed after the porous film is formed give the negative electrode a certain ability to absorb liquid, which is beneficial to improving the battery's long-term charge and discharge cycle retention rate. The porous structure of the porous ceramic particles themselves is conducive to the dispersed distribution of pores in the porous film, which helps to avoid the problem of particle aggregation preventing the formation of pores in local areas of the porous film and causing the inability to perform ion deintercalation in that area, thereby helping to ensure the energy density of the battery. Furthermore, the porous ceramic particles themselves have stable performance, good erosion resistance, and long service life, which makes the porous film stable during the use of the negative electrode. The porous ceramic particles also have the advantage of low cost, which is conducive to the mass production and commercialization of negative electrode sheets.
[0061] The composite current collector 11 includes a metal foil 111 and a carbon coating layer 112 disposed on the surface of the metal foil 111. The metal foil 111 can be, but is not limited to, a metal plate or a metal mesh. Specifically, the material of the metal foil 111 can be, but is not limited to, copper foil, aluminum foil, stainless steel, etc.
[0062] The carbon coating layer 112 can be provided on one side of the metal foil 111 or on opposite sides of the metal foil 111. The thickness of the carbon coating layer 112 can be 1 μm to 1.5 μm, for example, but not limited to, 1.0 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm, and 1.5 μm. Carbon coating layers of such thickness are advantageous for reducing the thickness of the negative electrode sheet while ensuring conductivity. Carbon coating layers with a thickness of less than 1 μm are difficult to form and difficult to ensure continuity and conductivity. Carbon coating layers with a thickness greater than 1.5 μm are not conducive to embedding the carbon coating into the negative electrode active material layer during rolling, resulting in poor contact between the carbon coating layer and the negative electrode active material layer. Furthermore, they waste material and are not conducive to reducing the thickness of the electrode sheet and miniaturizing the overall battery structure. In some embodiments, the metal foil 111 can be 13 μm thick, and the carbon coating layer can be 1 μm thick.
[0063] In some embodiments, the carbon coating layer 112 may include conductive carbon particles and polymer materials. Conductive carbon particles include, but are not limited to, one or both of graphene and carbon black. Graphene has extremely high electronic conductivity, and its two-dimensional structure can more fully construct a conductive network in the electrode, which is manifested as high atomic utilization. Carbon black particles are fine, the network chains are tightly packed, the specific surface area is large, and there are many particles per unit mass, which is conducive to the formation of a chain conductive structure in the electrode and is a classic conductive agent. Therefore, the conductive carbon particles include one or both of graphene and carbon black to facilitate reducing the film resistance of the negative electrode. The polymer material may include, but is not limited to, one or more of polyvinylidene fluoride, acrylic esters, polyvinyl alcohol, polytetrafluoroethylene, and polyurethane, which facilitates film formation during subsequent coating to form the carbon coating layer, and is conducive to improving the flexibility of the carbon coating layer, thereby helping to avoid cracking of the carbon coating layer during the subsequent production or use of the negative electrode. In some embodiments, the conductive carbon particles may be composed of graphene and carbon black in a mass ratio of 1:3, and the mass percentage of the conductive carbon particles in the carbon coating layer 112 may be 10%, so as to facilitate the effective dispersion of the conductive carbon particles, avoid the agglomeration phenomenon caused by excessive content of the conductive carbon particles, improve the uniformity of the carbon coating layer, and at the same time enhance the adhesion of the carbon coating layer to the aluminum foil current collector, which helps to avoid the detachment of the carbon coating layer during the battery cycle. The increase in the carbon black content in the conductive carbon particles is conducive to reducing the diaphragm resistance of the negative electrode while also helping to reduce costs. However, when the ratio of graphene to carbon black is less than 1:3, it will lead to a significant increase in the diaphragm resistance of the negative electrode.
[0064] The material of the negative electrode active material layer 13 can be selected as needed. For example, in some embodiments, the negative electrode active material layer 13 can be made of hard carbon. Hard carbon has abundant carbon sources, is low-cost, and is non-toxic and environmentally friendly, facilitating mass production and commercialization of negative electrode sheets. Furthermore, hard carbon has a low sodium storage potential and a high sodium storage capacity, facilitating the design of sodium-ion batteries.
[0065] Specifically, the negative electrode active material layer 13 may include hard carbon, a conductive carbon material, and a binder. The hard carbon and the conductive carbon material are dispersed in the binder. The conductive carbon material may include, but is not limited to, one or more of carbon black, carbon nanotubes, and graphene. The binder may be, but is not limited to, one or more of styrene-butadiene rubber, polyvinylidene fluoride (PVDF), sodium alginate, polyvinyl alcohol, polymethyl methacrylate, hydrogenated nitrile rubber, polytetrafluoroethylene, and polyacrylic acid. In some embodiments, the binder may be polytetrafluoroethylene. In the negative electrode active material layer 13, the mass ratio of hard carbon, conductive carbon material, and polytetrafluoroethylene may be 8:1:1, which is conducive to the battery having better discharge capacity and cycle performance. The conductive carbon material may be composed of carbon black and carbon nanotubes in a mass ratio of 10:1. The carbon nanotubes dispersed between the carbon black particles can produce a synergistic conductive effect, so that the negative electrode plate obtains a higher electronic conductivity.
[0066] The porous ceramic particles in the porous film 15 may include but are not limited to one or more of siliceous silicate materials, aluminosilicate materials, diatomaceous earth materials, coarse ceramic materials, pure siliceous materials, corundum and corundum. The porous ceramic particles of the above materials themselves have a porous structure, which facilitates the formation and dispersion of the porous structure in the porous film 15, and is beneficial to reducing the phenomenon of particle aggregation leading to pore distribution or formation of unevenness when forming the porous film 15. At the same time, the porous ceramic particles of the above materials are easy to obtain, which is beneficial to cost reduction.
[0067] The pore size of the porous ceramic particles can be 2nm to 50nm, which is convenient for better deintercalation of active ions and can reduce the direct contact between the negative electrode active material and the electrolyte, which is beneficial to ensuring the battery capacity. Specifically, how high the pore size in the porous ceramic particles is likely to lead to an increase in side reactions in the battery, affecting the battery cycle life. If the pore size in the porous ceramic particles is too low, it will affect the deintercalation of active ions such as sodium ions, affecting the battery cycle life and the first coulomb efficiency of the battery. The particle size of the porous ceramic particles can be 100nm to 200nm, which is convenient for uniform coating to form a porous film, and is also beneficial to the uniformity of the thickness of each area of the porous film. Furthermore, if the particle size of the porous ceramic particles is too low, it will easily lead to an increase in the contact area of the side reactions in the battery and reduce the battery cycle life. If the particle size of the porous ceramic particles is too high, it will easily affect the deintercalation of sodium ions, resulting in a decrease in the first coulomb efficiency.
[0068] The polymer in the porous film 15 may include, but is not limited to, one or more of polyvinylidene fluoride, acrylic acid esters, polyvinyl alcohol, polytetrafluoroethylene, and polyurethane. This provides the porous film 15 with good flexibility, which helps prevent cracking of the porous film 15 during use of the negative electrode, thereby helping to ensure the electrochemical performance of the negative electrode. In some embodiments, the polymer may be polyvinylidene fluoride, optionally including, but not limited to, material model W#9300 (powder).
[0069] In some embodiments, the mass percentage of the high molecular weight polymer in the porous film 15 can be 50% to 80%, and the mass percentage of the porous ceramic particles can be 20% to 50%. This helps ensure the distribution of the porous structure while also giving the porous film good flexibility. This helps to reduce the risk of cracking of the porous film while maintaining battery capacity and improving battery cycle life, thereby increasing the overall service life of the battery. Furthermore, the mass percentage of the high molecular weight polymer can be 60%, and the mass percentage of the porous ceramic particles can be 40%.
[0070] The thickness of the porous film 15 can be 1 μm to 10 μm, for example, but not limited to 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm and 10 μm. This thickness is conducive to film formation and also helps to reduce the risk of cracking of the porous film during use of the negative electrode. However, if the thickness of the porous film is too large, it will easily affect the battery pack margin design and increase the internal resistance of the battery.
[0071] The porosity of the porous film 15 can be 40% to 80%. Furthermore, the porosity can be 60%, which is beneficial to improving the flexibility of the porous film 15, increasing the insertion and extraction rate of active ions such as sodium ions, and reducing the contact surface of related side reactions in the battery, which is beneficial to ensuring the initial efficiency and cycle life of the battery.
[0072] The negative electrode sheet 100 is used in a battery cell. Referring to FIG2 , the battery cell 200a also includes a positive electrode sheet 30 and a separator 40. The separator 40 is located between the positive electrode sheet 30 and the negative electrode sheet 100. The battery cell 200a can be a wound battery cell (as shown in FIG2 ) or a stacked battery cell.
[0073] The battery cell 200a is used in a battery. Referring to FIG. 2 , the battery 200 further includes an electrolyte 50 and a packaging case 60 . The battery cell 200a and the electrolyte 50 are encapsulated by the packaging case 60 , with the battery cell 200a in contact with the electrolyte 50 . The battery 200 employing the negative electrode sheet 100 can effectively improve the cycle capacity retention and cycle life of the battery 200 , and can also enhance the safety of the battery 200 .
[0074] Based on the same technical concept, an embodiment of the present application further provides an electronic device comprising a housing and the aforementioned battery installed within the housing. The electronic device may be, for example, a consumer electronic product such as a mobile phone, tablet computer, power bank, portable computer, notebook computer, and other wearable or portable electronic devices, or may be a vehicle, energy storage device, base station, or other device, but is not limited thereto.
[0075] Referring to FIG. 3 , an electronic device 300 according to an embodiment of the present application includes a housing 301 and the aforementioned battery 200 mounted within the housing 301 . In this embodiment, the electronic device 300 may be an electric vehicle. Using the aforementioned battery 300 can effectively extend the service life of electronic devices such as electric vehicles.
[0076] The present application will be described in more detail below using examples and comparative examples. However, the following examples are only provided to help understand the present application, and the content of the present application is not limited by the following examples.
[0077] Comparative Example 1
[0078] Preparation of the negative electrode sheet: Provide a hollow aluminum foil as a current collector. Hard carbon, conductive carbon particles and PTFE (polytetrafluoroethylene) are uniformly mixed in a mass ratio of 8:1:1, and then NMP (N-methylpyrrolidone) solvent is added to form a negative electrode active slurry. The negative electrode active slurry is evenly coated on the aluminum foil and dried and rolled to form a negative electrode active material layer. The siliceous silicate material is ball-milled to obtain porous ceramic particles, and the porous ceramic particles are dehydrated at a high temperature of 200 degrees Celsius to remove the moisture contained therein. The D50 of the porous ceramic particles is 150nm, the pore size distribution is 2nm-50nm (mesopores), and the porosity is 60%. The high-temperature-treated porous ceramic particles and PVDF (polyvinylidene difluoride) were added to NMP at a mass ratio of 2:3 and stirred evenly to obtain a white, milky coating slurry. The stirring speed was 25 r / min, the dispersion speed was 2000 r / min, and the stirring time was 3 hours. The coating slurry was applied to the surface of the negative electrode active material layer and dried to remove the NMP solvent, forming a porous film with a thickness of approximately 10 μm.
[0079] Preparation of positive electrode: NaFe 1 / 3 Ni 1 / 3 Mn 1 / 3O2, conductive carbon black and PVDF are evenly mixed in a mass ratio of 96:2:2, and stirred at high speed in a vacuum to form a positive electrode slurry; the slurry is evenly coated on a carbon-coated aluminum foil, and after drying, it is rolled and cut into sheets to obtain a positive electrode sheet.
[0080] The positive electrode sheet, the polyethylene film as an isolation membrane and the negative electrode sheet are assembled to form a battery cell, and the battery cell and the electrolyte (1 mol / L NaPF6 solution is selected, and ethylene carbonate is used as a solvent) are encapsulated in a packaging shell to obtain a soft-pack battery.
[0081] Comparative Example 2
[0082] The difference from Comparative Example 1 is that 1) an aluminum foil with a carbon coating is provided as a current collector. The current collector is prepared as follows: the aluminum foil is cleaned to remove impurities such as oil and oxide layer; PVDF and NMP are mixed to prepare a binder solution, and then graphene and carbon black are added in a mass ratio of 1:3 and mixed to obtain a conductive liquid, wherein the conductive liquid has a total mass percentage of 10% for graphene and carbon black, 5% for PVDF, and the remainder is NMP; the conductive liquid is applied to the surface of the cleaned aluminum foil and dried to obtain a current collector with a 1 μm thick carbon coating layer on the aluminum foil; 2) a porous film is not formed on the negative electrode active material layer, that is, the negative electrode plate does not contain a porous film.
[0083] Example 1
[0084] The difference from Comparative Example 1 is that a carbon-coated aluminum foil is provided as the current collector. The current collector is prepared as follows: the aluminum foil is cleaned to remove impurities such as oil and oxide layers; PVDF and NMP are mixed to prepare a binder solution, and carbon black is added and mixed to obtain a conductive liquid. The conductive liquid contains 10% by weight of carbon black, 5% by weight of PVDF, and the remainder is NMP; the conductive liquid is applied to the surface of the cleaned aluminum foil and dried to obtain a current collector with a 1 μm thick carbon-coated layer on the aluminum foil.
[0085] Example 2
[0086] The difference from Example 1 is that carbon black is replaced by graphene.
[0087] Example 3
[0088] The difference from Example 1 is that the carbon black is replaced by a mixture of graphene and carbon black in a mass ratio of 1:1.
[0089] Example 4
[0090] The difference from Example 3 is that the mass ratio of graphene to carbon black is replaced with 2:1.
[0091] Example 5
[0092] The difference from Example 3 is that the mass ratio of graphene to carbon black is replaced with 1:2.
[0093] Example 6
[0094] The difference from Example 3 is that the mass ratio of graphene to carbon black is replaced with 1:3.
[0095] Example 7
[0096] The difference from Example 3 is that the mass ratio of graphene to carbon black is replaced with 1:4.
[0097] Example 8
[0098] The differences from Example 3 are: 1) the mass ratio of graphene to carbon black is replaced with 1:3; 2) the mass ratio of porous ceramic particles to PVDF is replaced with 1:1.
[0099] Example 9
[0100] The differences from Example 3 are: 1) the mass ratio of graphene to carbon black is replaced to 1:3; 2) the mass ratio of porous ceramic particles to PVDF is replaced to 3:7.
[0101] Example 10
[0102] The differences from Example 3 are: 1) the mass ratio of graphene to carbon black is replaced to 1:3; 2) the mass ratio of porous ceramic particles to PVDF is replaced to 2:8.
[0103] Example 11
[0104] The difference from Example 6 is that the porous ceramic particle size D50 is 250 nm.
[0105] Example 12
[0106] The difference from Example 6 is that the porous ceramic particle size D50 is 100 nm.
[0107] Example 13
[0108] The difference from Example 6 is that the pore size of the porous ceramic is greater than 50 nm (macropore).
[0109] Example 14
[0110] The difference from Example 6 is that the pore size of the porous ceramic is less than 2 nm (micropores).
[0111] Example 15
[0112] The difference from Example 6 is that the porosity of the porous ceramic is 40%.
[0113] Example 16
[0114] The difference from Example 6 is that the porosity of the porous ceramic is 80%.
[0115] Six samples were taken from each of Comparative Example 1 and Examples 1-7, and the negative electrode sheet resistance of each sample was measured. The measurement results are recorded in Table 1 below. At the same time, Figure 4 intuitively reflects the average value of the negative electrode sheet resistance in Comparative Example 1 and Examples 1-7.
[0116] The battery samples corresponding to Comparative Example 2, Example 6, and Examples 8-16 were tested for their initial coulombic efficiency (hereinafter referred to as initial efficiency) and battery capacity cycle retention. The test results are reported in Table 2 and Figure 5 below. As shown in Figure 5, the battery corresponding to the negative electrode sheet with a porous film exhibits better battery capacity cycle retention. In particular, the battery corresponding to Example 6 achieved a battery capacity cycle retention of 97.69% after 50 charge-discharge cycles.
[0117] Table 1
[0118] It can be seen from the data recorded in the above table that compared with the negative electrode sheet in which the negative electrode active material layer is directly formed on the surface of the aluminum foil in Comparative Example 1, the carbon coating layer designed between the aluminum foil and the negative electrode active material layer in Examples 1 to 7 can reduce the membrane resistance of the negative electrode sheet.
[0119] Table 2
[0120] It should be noted that the above are only specific embodiments of the present application, but the scope of protection of the present application is not limited thereto. Any changes or substitutions that can be easily conceived by any person skilled in the art within the technical scope disclosed in the present application should be included in the scope of protection of the present application; the embodiments of the present application and the features of the embodiments can be combined with each other unless there is a conflict. Therefore, the scope of protection of the present application shall be based on the scope of protection of the claims.
Claims
1. A battery, characterized in that: It includes a positive electrode sheet, a negative electrode sheet and a separator, wherein the separator is arranged between the positive electrode sheet and the negative electrode sheet, and the negative electrode sheet includes: A composite current collector, the composite current collector comprising a metal foil and a carbon coating layer, wherein the carbon coating layer is disposed on a surface of the metal foil; A negative electrode active material layer is disposed on a side of the carbon coating layer away from the metal foil; The porous film is arranged on the side of the negative electrode active material layer away from the composite current collector. The porous film comprises a high molecular polymer and porous ceramic particles, and the porous ceramic particles are dispersed in the high molecular polymer.
2. The battery according to claim 1, characterized in that The carbon coating layer includes one or both of graphene and carbon black.
3. The battery according to any one of claims 1 to 2, characterized in that: The carbon coating layer has a thickness of 1 μm to 1.5 μm.
4. The battery according to any one of claims 1 to 3, characterized in that: The porous ceramic particles include one or more of siliceous silicate materials, aluminosilicate materials, diatomaceous earth materials, coarse ceramic materials, pure siliceous materials, corundum and corundum.
5. The battery according to claim 4, characterized in that The pore size of the porous ceramic particles is 2nm to 50nm.
6. The battery according to any one of claims 1 to 5, characterized in that: The particle size of the porous ceramic particles is 100 nm to 200 nm.
7. The battery according to any one of claims 1 to 6, characterized in that: The high molecular polymer includes one or more of polyvinylidene fluoride, acrylic esters, polyvinyl alcohol, polytetrafluoroethylene and polyurethane.
8. The battery according to any one of claims 1 to 7, characterized in that: In the porous film, the mass percentage of the high molecular polymer is 50% to 80%, the mass percentage of the porous ceramic particles is 20% to 50%, and the porosity of the porous film is 40% to 80%.
9. The battery according to any one of claims 1 to 8, characterized in that: The thickness of the porous film is 1 μm to 10 μm.
10. The battery according to any one of claims 1 to 9, characterized in that: The negative electrode active material layer includes hard carbon.
11. The battery according to claim 10, characterized in that The negative electrode active material layer also includes a conductive carbon material and polytetrafluoroethylene, and the mass ratio of the hard carbon, the conductive carbon material and the polytetrafluoroethylene is 8:1:
1.
12. The battery according to claim 11, characterized in that The conductive carbon material includes carbon black and carbon nanotubes, and the mass ratio of the carbon black to the carbon nanotubes is 10:
1.
13. A battery pack, characterized in that: The invention comprises a plurality of batteries according to any one of claims 1 to 12, wherein any two of the plurality of batteries are connected in series or in parallel.
14. An electronic device, characterized in that: The electronic device comprises a housing and a battery as claimed in any one of claims 1 to 12, wherein the battery is installed in the housing.
15. An energy storage system, characterized in that: The energy storage system comprises a power converter and at least one battery pack as claimed in claim 13; The power converter is electrically connected to the battery pack, and is used to convert the voltage output by the battery pack into power and output it to a power grid or a load, and / or to convert the voltage output by an external power source into power and output it to the battery pack.
Citation Information
Patent Citations
Battery cell and energy storage device
CN107516725A
Safe high-voltage high-energy-density lithium ion battery and preparation method thereof
CN109755557A
Sodium ion battery
CN110021755A
High-safety lithium ion battery and preparation method thereof
CN113381057A
Negative pole piece with coating, preparation method of negative pole piece and lithium ion battery
CN115513410A
Cited By
Composite foil as well as preparation method and application thereof