LMFP / CNF carbon nanofiber composite material, preparation method and application
Preparation of LMFP/CNF carbon nanofiber composite materials by electrospinning method solves the problems of poor solubility and poor conductivity of LMFP, and forms an efficient cathode material, suitable for new energy batteries, achieving cost savings and energy consumption reduction .
Patent Information
- Application Number
- CN202411039972.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-07-31
AI Technical Summary
The poor solubility and poor conductivity of LMFP limit its application in new energy batteries.
Electrospinning method is used to mix lithium-source substances, manganese-source substances, iron-source substances, phosphate root substances and polymers, and preheating oxidation and carbonization treatment to prepare LMFP/CNF carbon nanofiber composite materials to form a continuous Carbon coating to improve electrochemical properties.
It improves the solubility and conductivity of LMFP, and forms an efficient cathode material, suitable for new energy batteries, with the advantages of cost saving, energy consumption reduction and easy amplification.
Smart Images

Figure CN119041054A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of new energy batteries, and in particular to a LMFP / CNF carbon nanofiber composite material, a preparation method and an application thereof. Background Art
[0002] New energy refers to a form of energy that is cleaner and more renewable than traditional fossil energy, with lower environmental impact. The development of new energy has become a focus of public attention worldwide. Lithium-ion battery products have been fully integrated into people's lives, powering mobile phones and laptops that have revolutionized modern society, and are now entering the transportation industry, such as plug-in hybrid vehicles and electric vehicles. Researchers are committed to discovering and developing 3D porous independent electrodes that can achieve a continuous conductive network for electron transport and interconnected hierarchical porosity for ion transport. Effectively improve the electrochemical properties of electrode materials, thereby promoting the development of electrochemical energy storage technology.
[0003] Lithium manganese iron phosphate (LMFP, LiMn x Fe 1-x PO4), which is formed by iron doping on the basis of LiMnPO4 modification. It has a stable structure and a high voltage platform, and is a very promising new cathode material. However, since the inorganic phosphorus sources (ammonium dihydrogen phosphate and phosphoric acid) commonly used in the synthesis of LMFP are difficult to dissolve in the PAN solution to form a uniform and stable electrospinning precursor solution, the reported electrospun LMFP are mostly based on hydrophilic polymer systems, such as polyvinyl alcohol (PVA) and polyvinyl pyrrolidone (PVP), and the mechanical properties of these systems are poor. Polymers with good mechanical stability, such as polyacrylonitrile, polyvinyl alcohol, polylactic acid, etc., have a high carbonization rate and structural stability, and are ideal polymers for forming self-supporting carbon nanonetworks by electrospinning. However, these high molecular polymers have strong selectivity for solvents, which limits their complete coverage of active substances, resulting in the inability to form a continuous carbon coating on the surface of the active material.
[0004] These problems have seriously affected the promotion and application of LMFP. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a LMFP / CNF carbon nanofiber composite material, a preparation method and an application thereof, so as to solve the problems of poor solubility and poor electrical conductivity of LMFP in the prior art.
[0006] The technical solution of the present invention to solve the above technical problems is as follows:
[0007] The present invention provides a method for preparing a LMFP / CNF carbon nanofiber composite material, comprising adding a lithium source material, a manganese source material, an iron source material, a phosphate source material and a high molecular polymer into an organic solvent to obtain a spinning solution, electrostatically spinning the spinning solution to obtain a precursor fiber; and sequentially preheating, oxidizing and carbonizing the precursor fiber to obtain the LMFP / CNF carbon nanofiber composite material.
[0008] The phosphate source includes one or more of 1-butyl-3-methylimidazole dihydrogen phosphate, phosphoric acid, potassium dihydrogen phosphate, and ammonium dihydrogen phosphate, and the high molecular polymer includes one or more of polyacrylonitrile, polyvinyl alcohol, and polylactic acid.
[0009] Based on the above technical solution, the present invention can also be improved as follows.
[0010] Furthermore, in the spinning solution, the mass percentage of the high molecular weight polymer is 10% to 12%.
[0011] Furthermore, in the spinning solution, the molar ratio of lithium, manganese, iron and phosphate is 1:(0.6-0.8):(0.4-0.2):1, and the mass ratio of the high molecular polymer to the lithium source is 4.56-15.27:1.
[0012] Furthermore, the lithium source material includes one or more of anhydrous lithium acetate, lithium bromide, and lithium fluoride, the manganese source material includes one or more of anhydrous manganese acetate, manganese nitrate, and manganese chloride, and the iron source material includes one or more of triacetylacetonate iron, ferric nitrate, and ferric chloride.
[0013] Furthermore, the organic solvent includes one or more of dimethylformamide, dimethylacetamide, and acetonitrile.
[0014] Furthermore, the preheating oxidation step includes preheating the precursor fiber in an air atmosphere, the preheating oxidation temperature is 230° C. to 250° C., and the preheating oxidation time is 2 h to 3 h.
[0015] Furthermore, the carbonization step includes carbonizing the precursor fiber that has been preheated and oxidized in a mixed atmosphere of an inert gas and hydrogen, the carbonization temperature is 700° C. to 750° C., and the carbonization time is 2 h to 6 h.
[0016] The present invention also provides a LMFP / CNF carbon nanofiber composite material, which is prepared by the above method.
[0017] Furthermore, the composite material includes LMFP grains, a carbon fiber structure and a thin carbon layer, the LMFP grains are embedded or coated in the carbon fiber structure, and the thin carbon layer uniformly covers the surface of the LMFP grains and / or the outer layer of the carbon fiber structure; the particle size of the LMFP grains is 50 to 150 nm.
[0018] The present invention also provides an application of the above-mentioned LMFP / CNF carbon nanofiber composite material in a new energy battery, characterized in that the composite material is used to prepare a positive electrode material.
[0019] The beneficial effects of the present invention are:
[0020] (1) The preparation method of the LMFP / CNF carbon nanofiber composite material of the present invention uses ionic liquid as a phosphate source, combined with preheating oxidation and carbonization treatment, so that the high molecular polymer (especially polyacrylonitrile) can be decomposed to cover the active material well, so that a continuous carbon coating can be formed on the surface of the active material;
[0021] (2) The preparation method of the LMFP / CNF carbon nanofiber composite material of the present invention has the advantages of saving costs, reducing energy consumption, optimizing the preparation process and being easy to scale up the preparation;
[0022] (3) The LMFP / CNF carbon nanofiber composite material of the present invention has the characteristics of good solubility, which improves the feasibility of preparing electrode materials by high molecular polymer-based electrospinning system;
[0023] (4) The LMFP / CNF carbon nanofiber composite material of the present invention can be used as a structure-directing agent to induce the formation of LMFP nanocubes, providing a convenient pathway for the transport of lithium ions;
[0024] (5) The LMFP / CNF carbon nanofiber composite material of the present invention can also form an N-doped dual-phase carbon coating during the heat treatment process, further improving the electronic conductivity of the entire electrode. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is the performance characterization test diagram of the LMFP / CNF carbon nanofiber composite material of the present invention, and each material obtained in Comparative Example 1, Figure 1 Figure a is the SEM image of LMFP / CNF-BP (6%). Figure 1 Figure b is the SEM image of LMFP / CNF-BP (8%). Figure 1 Figure c is the SEM image of LMFP / CNF-BP (10%). Figure 1 (d) is the SEM image of LMFP / CNF-BP (12%);
[0026] Figure 2 This is the performance characterization test diagram of the LMFP / CNF carbon nanofiber composite material of the present invention, and each material obtained in Comparative Example 2, Figure 2 Figure a is the SEM image of LMFP / CNF-BP (700℃). Figure 2 Figure b is the SEM image of LMFP / CNF-BP (750℃). Figure 2 (c) is the SEM image of LMFP / CNF-BP (800℃);
[0027] Figure 3 This is the performance characterization test diagram of the LMFP / CNF carbon nanofiber composite material of the present invention, and each material obtained in Comparative Example 3, Figure 3 Figure a is the FESEM image of LMFP / CNF-BP (2h). Figure 3 Figure b is the FESEM image of LMFP / CNF-BP (4h). Figure 3 Figure c is the FESEM image of LMFP / CNF-BP (6h). Figure 3 (d) is the FESEM image of LMFP / CNF-BP (8h);
[0028] Figure 4 This is the performance characterization test diagram of the LMFP / CNF carbon nanofiber composite material of the present invention, and each material obtained in Comparative Example 4, Figure 4 Figure a is the FESEM image of LMFP / CNF-BP. Figure 4 (b) is the FESEM image of LMFP / CNF-HP. Figure 4 (c) is the FESEM image of LMFP / C-BP;
[0029] Figure 5 This is the charge and discharge curve diagram of each material obtained in Comparative Example 1 of the LMFP / CNF carbon nanofiber composite material of the present invention. Figure 5 a is the first charge and discharge curve at 0.1C. Figure 5 b is the cycle stability performance diagram;
[0030] Figure 6 This is the charge and discharge curve diagram of each material obtained in Comparative Example 2 of the LMFP / CNF carbon nanofiber composite material of the present invention. Figure 6 a is the first charge and discharge curve at 0.1C. Figure 6 b is the cycle stability performance diagram;
[0031] Figure 7 The LMFP / CNF carbon nanofiber composite material of the present invention is a charge and discharge curve diagram of each material obtained in Comparative Example 3. Figure 7 a is the first charge and discharge curve at 0.1C. Figure 7 b is the cycle stability performance diagram;
[0032] Figure 8 The LMFP / CNF carbon nanofiber composite material of the present invention is a charge and discharge curve diagram of each material obtained in Comparative Example 4. Figure 8 a is the first charge and discharge curve at 0.1C. Figure 8 b is the cycle stability performance diagram DETAILED DESCRIPTION
[0033] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.
[0034] The preparation method of the LMFP / CNF carbon nanofiber composite material of the present invention comprises the following steps: adding a lithium source material, a manganese source material, an iron source material, a phosphate source material and a high molecular polymer into an organic solvent to obtain a spinning solution, electrostatically spinning the spinning solution to obtain a precursor fiber; and sequentially performing preheating oxidation and carbonization treatment on the precursor fiber to obtain the LMFP / CNF carbon nanofiber composite material. The phosphate source comprises one or more of 1-butyl-3-methylimidazole dihydrogen phosphate, phosphoric acid, potassium dihydrogen phosphate and ammonium dihydrogen phosphate, and the high molecular polymer comprises one or more of polyacrylonitrile, polyvinyl alcohol and polylactic acid.
[0035] The preparation method of the present invention uses ionic liquid (1-butyl-3-methylimidazole dihydrogen phosphate) as a phosphate source material, combined with preheating oxidation and carbonization treatment, so that the high molecular polymer (especially polyacrylonitrile) can cover the active material well after thermal decomposition, so that a continuous carbon coating can be formed on the surface of the active material. The composite material obtained in this way has good electrochemical performance when used as a positive electrode material.
[0036] In addition, in the preparation method of the present invention, due to the selection of a suitable organic solvent, when a non-ionic liquid phosphate source material (phosphoric acid, potassium dihydrogen phosphate, ammonium dihydrogen phosphate) is used, it can also be mixed and dissolved well with polyacrylonitrile, polyvinyl alcohol, and polylactic acid, thereby achieving good coverage of the high molecular polymer.
[0037] Preferably, in the spinning solution, the mass percentage of the high molecular weight polymer is 10% to 12%; the composite material prepared using the high molecular weight polymer within this mass percentage range has the best electrochemical performance.
[0038] More preferably, the high molecular polymer is polyacrylonitrile, and its mass percentage is 10%, 11%, 12%, etc.
[0039] Preferably, in the spinning solution, the molar ratio of lithium, manganese, iron and phosphate is 1:(0.6-0.8):(0.4-0.2):1, and the mass ratio of the high molecular polymer to the lithium source is 4.56-15.27:1.
[0040] Specifically, in the material prepared by the above ratio, the specific chemical formula of LMFP is LiMn 0.8 Fe 0.2 PO4 or LiMn 0.7 Fe 0.3 PO4 or others.
[0041] Preferably, the lithium source material includes one or more of anhydrous lithium acetate, lithium bromide, and lithium fluoride, the manganese source material includes one or more of anhydrous manganese acetate, manganese nitrate, and manganese chloride, and the iron source material includes one or more of ferric triacetylacetonate, ferric nitrate, and ferric chloride.
[0042] Preferably, the organic solvent includes one or more of dimethylformamide, dimethylacetamide, and acetonitrile.
[0043] In the preparation method of the present invention, the preheating oxidation step includes preheating the precursor fiber in an air atmosphere, the preheating oxidation temperature is 230° C. to 250° C., and the preheating oxidation time is 2 h to 3 h.
[0044] Further preferably, the temperature of preheating oxidation is 230°C, 235°C, 240°C, 245°C, 250°C, etc., and the time of preheating oxidation is 2h, 2.5h, 3h, etc.
[0045] Preferably, the preheating temperature rise rate is 1°C to 4°C / min; further preferably, the preheating temperature rise rate is 2°C / min.
[0046] In the preparation method of the present invention, the carbonization step includes carbonizing the preheated oxidized precursor fiber in a mixed atmosphere of inert gas and hydrogen, the carbonization temperature is 700°C to 750°C, and the carbonization time is 2h to 6h.
[0047] Preferably, the temperature of the carbonization treatment is 700°C, 710°C, 720°C, 730°C, 740°C, 750°C, etc., and the time of the carbonization treatment is 2h, 4h, 6h, etc.
[0048] Preferably, the heating rate of the carbonization treatment is 1°C to 7°C / min; further preferably, the heating rate of the carbonization treatment is 5°C / min.
[0049] Preferably, the mixed atmosphere of the inert gas and hydrogen is specifically an argon-hydrogen mixed gas, wherein the volume percentage of hydrogen is 2-6%; further preferably, the volume percentage of hydrogen is 5%.
[0050] The preparation method of the present invention comprises the following specific steps:
[0051] 1) Prepare lithium source material, manganese source material, iron source material, and phosphate source material according to the ratio, and then mix them with the polymer. After adding an appropriate amount of organic solvent, stir magnetically for a period of time in a water bath at 60°C to 80°C until the mixed solution forms a uniform spinning solution. Before electrospinning, the orange-red spinning solution is first ultrasonically treated.
[0052] Preferably, the ultrasonic treatment time is 10 min to 20 min.
[0053] 2) The spinning solution obtained in step 1) is placed in a 10 ml plastic syringe with a 20G (inner diameter 0.6 mm) stainless steel needle, and then the syringe is fixed on a micro-injection pump, one end of the needle is connected to the positive electrode of the high-voltage electrostatic generator, and the collecting device is connected to the negative electrode of the high-voltage electrostatic generator; the distance between the DC high-voltage electric needle with a voltage of 20 kV and the roller collecting device covered with aluminum foil is 12 cm, the spinning solution flow rate is 0.4 ml / h, the relative humidity of the environment is 25-30%, and the temperature is 24-28°C.
[0054] 3) The precursor fibers prepared by electrospinning were placed at room temperature overnight, and then the precursor fibers were transferred to a tubular furnace for preheating and oxidation, and then carbonization treatment to obtain LMFP / CNF materials.
[0055] The LMFP / CNF carbon nanofiber composite material of the present invention is prepared by the above method.
[0056] The composite material of the present invention comprises LMFP grains, a carbon fiber structure and a thin carbon layer, wherein the LMFP grains are embedded in or coated in the carbon fiber structure, and the thin carbon layer uniformly covers the surface of the LMFP grains and / or the outer layer of the carbon fiber structure; and the particle size of the LMFP grains is 50 to 150 nm.
[0057] The composite material of the invention has the characteristic of good solubility, and improves the feasibility of preparing electrode materials by a PAN-based electrospinning system.
[0058] The application of the LMFP / CNF carbon nanofiber composite material in new energy batteries is specifically used for preparing positive electrode materials.
[0059] Specifically, the composite material of the present invention can be used as a structure directing agent to induce the formation of LMFP nanocubes, providing a convenient pathway for the transmission of lithium ions.
[0060] The composite material of the present invention can also form an N-doped dual-phase carbon coating during the heat treatment process, thereby further improving the electronic conductivity of the entire electrode.
[0061] The present invention is described in detail below through specific examples.
[0062] Example 1
[0063] The method of the present invention is used to prepare the LMFP / CNF carbon nanofiber composite material. Specifically, the polymer used in this embodiment is polyacrylonitrile (PAN), and the phosphate source material is the ionic liquid 1-butyl-3-methylimidazole dihydrogen phosphate ([Bmim]H2PO4). Therefore, the composite material of this embodiment is a LMFP / CNF-BP composite positive electrode material. At the same time, according to the molar ratio of each element, the LMFP of the present invention is specifically LiMn 0.8 Fe 0.2 PO4.
[0064] The preparation method of this embodiment comprises the following steps:
[0065] 1) First, weigh 0.6 g of polyacrylonitrile powder, then weigh 1.2 mmol of anhydrous manganese acetate, 0.3 mmol of ferric triacetylacetonate, 1.5 mmol of anhydrous lithium acetate, and 1.5 mmol of 1-butyl-3-methylimidazole dihydrogen phosphate, add appropriate amount of DMF as solvent, stir magnetically for 6 h in a 70° C. water bath to form a uniform spinning solution, and ultrasonically treat the orange-red spinning solution for 15 min before electrospinning.
[0066] 2) Electrospinning the electrospinning precursor solution obtained in step 1). The precursor solution is placed in a 10 ml plastic syringe with a 20G (inner diameter 0.6 mm) stainless steel needle, and then the syringe is fixed on a micro-injection pump, one end of the needle is connected to the positive electrode of the high-voltage electrostatic generator, and the collecting device is connected to the negative electrode of the high-voltage electrostatic generator; the distance between the 20 kV DC high-voltage needle and the roller collecting device covered with aluminum foil is 12 cm, the spinning solution flow rate is 0.4 ml / h, the relative humidity of the environment is 25-30%, and the temperature is 24-28°C.
[0067] 3) The precursor fiber prepared by electrospinning was placed at room temperature overnight, and then the precursor fiber was transferred to a tube furnace, first pre-oxidized at 230°C in air for 2 hours, and then carbonized in an argon-hydrogen mixed gas atmosphere. The carbonization temperature was 750°C, the heating rate was 5°C / min, and the holding time was 4 hours. After the carbonization treatment, the LMFP / CNF-BP composite cathode material was obtained. Among them, the volume percentage of hydrogen in the argon-hydrogen mixed gas was 5%.
[0068] It should be noted that when potassium dihydrogen phosphate or ammonium dihydrogen phosphate is used as the phosphate source and polyvinyl alcohol or polylactic acid is used as the high molecular weight polymer, the properties of the prepared composite material are similar to those in Example 1. Although the present invention does not continue to list them in detail, these specific embodiments are still within the scope of protection of the present invention.
[0069] Comparative Example 1
[0070] In this comparative example, different mass percentages of polyacrylonitrile were used to prepare the corresponding LiMn 0.8 Fe 0.2 PO4 / CNF-BP composite cathode material. The specific preparation process is as follows:
[0071] 1) Prepare 4 parts of 1.2mmol anhydrous manganese acetate, 0.3mmol ferric triacetylacetonate, 1.5mmol anhydrous lithium acetate, and 1.5mmol 1-butyl-3-methylimidazole dihydrogen phosphate, and then mix them with 6%, 8%, 10%, and 12% polyacrylonitrile powder by mass, respectively. Add appropriate amount of DMF as solvent, stir magnetically for 6 hours in a 70℃ water bath to form a uniform spinning solution, and ultrasonically treat the orange-red spinning solution for 15 minutes before electrospinning.
[0072] 2) Electrospinning the electrospinning precursor solution obtained in step 1). The precursor solution is placed in a 10 ml plastic syringe with a 20G (inner diameter 0.6 mm) stainless steel needle, and then the syringe is fixed on a micro-injection pump, one end of the needle is connected to the positive electrode of the high-voltage electrostatic generator, and the collecting device is connected to the negative electrode of the high-voltage electrostatic generator; the distance between the 20 kV DC high-voltage needle and the roller collecting device covered with aluminum foil is 12 cm, the spinning solution flow rate is 0.4 ml / h, the relative humidity of the environment is 25-30%, and the temperature is 24-28°C.
[0073] 3) The precursor fiber prepared by electrospinning was placed at room temperature overnight, and then the precursor fiber was transferred to a tube furnace, first pre-oxidized at 230°C in air at a heating rate of 2°C / min for 2h, and then carbonized in an atmosphere of argon-hydrogen mixed gas, the carbonization temperature was 750°C, the heating rate was 5°C / min, and the holding time was 4h. Among them, the volume percentage of hydrogen in the argon-hydrogen mixed gas was 5%.
[0074] After the carbonization treatment was completed, composite positive electrode materials of LMFP / CNF-BP (6%), LMFP / CNF-BP (8%), LMFP / CNF-BP (10%), and LMFP / CNF-BP (12%) were obtained respectively.
[0075] The precursor nanomaterials of the above four composite cathode materials were analyzed and tested by SEM using a scanning electron microscope (TM3030). Figure 1 a to d correspond to the composite materials of LMFP / CNF-BP (6%), LMFP / CNF-BP (8%), LMFP / CNF-BP (10%), and LMFP / CNF-BP (12%), respectively.
[0076] according to Figure 1 It can be seen that when the mass percentage of PAN is 6% and 8%, no carbon fiber structure is found in the prepared composite cathode material; in addition, according to Figure 1 In c, when the mass fraction of PAN is 10%, the presence of carbon fiber structure can be seen, and the size of the material is significantly smaller than Figure 1 a and b; from Figure 1 It can be seen from figure d that when the mass fraction of PAN is 12%, the carbon fiber network structure of the material is obvious and the particle agglomeration phenomenon is greatly improved.
[0077] The four composite materials obtained above were subjected to the first charge and discharge test and the cycle stability performance test at 0.1C.
[0078] The results of the first charge and discharge test at 0.1C are as follows Figure 5 As shown in a. Figure 5 It can be seen that as the mass percentage of PAN increases, the first discharge capacity increases significantly. When the mass percentage of PAN reaches 12%, the first charge and discharge capacity of the composite material is 96.2 mAh g -1 When the mass percentage of PAN is 6%, the first discharge specific capacity of the composite material is the lowest, and the discharge platform of iron in the material is not obvious. Figure 5 b Analysis shows that with the increase of polymer mass fraction, the rate performance is also significantly improved.
[0079] It can be seen that when the mass percentage of PAN in the electrospinning solution is 12%, the electrochemical performance of the prepared LMFP / CNF-BP composite cathode material is optimal.
[0080] Comparative Example 2
[0081] This comparative example uses different carbonization temperatures to prepare corresponding LMFP / CNF-BP composite positive electrode materials. The specific preparation process is as follows:
[0082] 1) First, weigh polyacrylonitrile powder with a concentration of 12%, then weigh 1.2mmol anhydrous manganese acetate, 0.3mmol ferric triacetylacetonate, 1.5mmol anhydrous lithium acetate, and 1.5mmol 1-butyl-3-methylimidazole dihydrogen phosphate, add appropriate amount of DMF as solvent, stir magnetically for 6h in a 70°C water bath to form a uniform spinning solution, and ultrasonically treat the orange-red spinning solution for 15min before electrospinning.
[0083] 2) Electrospinning the electrospinning precursor solution obtained in step 1). The precursor solution is placed in a 10 ml plastic syringe with a 20G (inner diameter 0.6 mm) stainless steel needle, and then the syringe is fixed on a micro-injection pump, one end of the needle is connected to the positive electrode of the high-voltage electrostatic generator, and the collecting device is connected to the negative electrode of the high-voltage electrostatic generator; the distance between the 20 kV DC high-voltage needle and the roller collecting device covered with aluminum foil is 12 cm, the spinning solution flow rate is 0.4 ml / h, the relative humidity of the environment is 25-30%, and the temperature is 24-28 ° C.
[0084] 3) The precursor fibers prepared by electrospinning were placed at room temperature overnight, and then the precursor fibers were transferred to a tubular furnace and pre-oxidized in air at 230° C. for 2 h.
[0085] Then, the carbonization treatment was carried out in an atmosphere of argon-hydrogen mixed gas, and the carbonization treatment temperatures were 700°C, 750°C and 800°C, respectively, the heating rate was 5°C / min, and the holding time was 4h. Among them, the volume percentage of hydrogen in the argon-hydrogen mixed gas was 5%.
[0086] After carbonization treatment, LMFP / CNF-BP (700℃), LMFP / CNF-BP (750℃) and LMFP / CNF-BP (800℃) were obtained respectively.
[0087] The precursor nanomaterials of the above three composite materials were analyzed and tested by scanning electron microscope (TM3030). The SEM analysis results are as follows: Figure 2 shown.
[0088] according to Figure 2 As can be seen from a and b, when heat treated at lower temperatures (700°C, 750°C), the carbon fiber structure is obvious and more carbon fiber structures are retained. Figure 2 It can be seen from figure c that when the carbonization temperature is 800℃, a certain degree of aggregation occurs and the carbon fiber structure is not obvious.
[0089] The three composite materials obtained above were subjected to electrochemical tests respectively.
[0090] Figure 6 a is the first charge and discharge curve of the composite materials prepared at different carbonization temperatures at 0.1C. As the carbonization temperature increases, the discharge specific capacity of the LMFP / CNF-BP composite cathode material does not show a corresponding increase trend, but reaches the optimal value of 118.4 mAh g at 750 °C. -1 . Figure 6 b is the cycle stability performance diagram of the composite materials prepared at different carbonization temperatures. Figure 6It can be seen that when the carbonization temperature is 750°C, the discharge capacity reaches the optimal value and the rate performance of the material as a whole is well maintained. The discharge capacity is 80.3 mAh g at 5C. -1 .
[0091] Comparative Example 3
[0092] In this comparative example, different carbonization times were used to prepare the corresponding LiMn 0.8 Fe 0.2 PO4 / CNF-BP composite cathode material. The specific preparation process is as follows:
[0093] 1) First, weigh 0.6 g of polyacrylonitrile powder, then weigh 1.2 mmol of anhydrous manganese acetate, 0.3 mmol of ferric triacetylacetonate, 1.5 mmol of anhydrous lithium acetate, and 1.5 mmol of 1-butyl-3-methylimidazole dihydrogen phosphate, add an appropriate amount of DMF as a solvent, and stir magnetically for 6 h in a 70° C. water bath to form a uniform spinning solution. Before electrospinning, the orange-red spinning solution is ultrasonically treated for 15 min for use.
[0094] 2) Electrospinning the electrospinning precursor solution obtained in step 1). The precursor solution is placed in a 10 ml plastic syringe with a 20G (inner diameter 0.6 mm) stainless steel needle, and then the syringe is fixed on a micro-injection pump, one end of the needle is connected to the positive electrode of the high-voltage electrostatic generator, and the collecting device is connected to the negative electrode of the high-voltage electrostatic generator; the distance between the 20 kV DC high-voltage needle and the roller collecting device covered with aluminum foil is 12 cm, the spinning solution flow rate is 0.4 ml / h, the relative humidity of the environment is 25-30%, and the temperature is 24-28°C.
[0095] 3) The precursor fibers prepared by electrospinning were placed at room temperature overnight, and then the precursor fibers were transferred to a tubular furnace and pre-oxidized in air at 230° C. for 2 h.
[0096] Then, the carbonization treatment was carried out in an atmosphere of argon-hydrogen mixed gas, the temperature of the carbonization treatment was 750°C, the heating rate was 5°C / min, and the holding time was 2h, 4h, 6h and 8h respectively. Among them, the volume percentage of hydrogen in the argon-hydrogen mixed gas was 5%.
[0097] After carbonization treatment, LMFP / CNF-BP(2h), LMFP / CNF-BP(4h), LMFP / CNF-BP(6h) and LMFP / CNF-BP(8h) were obtained respectively.
[0098] The above four composite cathode materials were analyzed and tested by field emission scanning electron microscopy (Gemini SEM 300). The FESEM analysis results are as follows: Figure 3 shown.
[0099] Figure 3 a~d correspond to LMFP / CNF-BP(2h), LMFP / CNF-BP(4h), LMFP / CNF-BP(6h) and LMFP / CNF-BP(8h) respectively. Figure 3 It can be seen from a to c that in the shorter carbonization time (2h, 4h and 6h), the carbon fiber structure of the composite material is relatively intact. Figure 3 As can be seen in figure d, when the carbonization time increases to 8 h, most of the particles aggregate together, and only a few carbon fiber structures remain.
[0100] The four composite materials obtained above were subjected to electrochemical tests respectively.
[0101] Figure 7 a is the first charge-discharge curve of the composite material prepared with different carbonization times at 0.1C. Figure 7 It can be seen that when the carbonization time is 6 h, the discharge capacity of the composite material reaches the optimal value, which is 164.1 mAh g at 0.1 C. -1 . Figure 7 b is the cycle stability performance diagram of the composite materials prepared with different carbonization times. Figure 7 b It can be seen that when the carbonization time is 6 h, the rate performance of the material as a whole is significantly higher than that of other conditions, and the discharge specific capacities at 0.5C and 5C are 147.1 and 93.8 mAh g, respectively. -1 .
[0102] Comparative Example 4
[0103] In this comparative example, H3PO4 is used as the phosphate source to replace the ionic liquid ([Bmim]H2PO4), and the prepared composite material is LMFP / CNF-HP. In addition, this comparative example also uses the sol-gel method to prepare LMFP / C-BP material, wherein LMFP is specifically LiMn 0.8 Fe 0.2 PO4.
[0104] The phosphorus source for preparing LMFP / CNF-HP was phosphoric acid, the carbonization temperature was 750° C., and the other specific processes and conditions were the same as those in Example 1.
[0105] Preparation of LiMn by sol-gel method 0.8 Fe 0.2 The specific preparation process of PO4 / C-BP material is as follows:
[0106] 1) First, a certain amount of citric acid (C6H8O7·H2O) was weighed and used as a reducing agent and carbon source, dissolved in an appropriate amount of DMF, and a uniform solution was formed under magnetic stirring.
[0107] 2) Then, according to the stoichiometric ratio of lithium source: manganese source: iron source: phosphate source (Li:Mn:Fe:PO4) = 1:0.8:0.2:1, 4.8 mmol manganese acetate ((CH3COO)2Mn·4H2O), 1.2 mmol iron triacetylacetonate (Fe(acac)3), 6.0 mmol lithium acetate (CH3COOLi·2H2O), and 6.0 mmol 1-butyl-3-methylimidazole dihydrogen phosphate ([Bmim]H2PO4) were weighed respectively.
[0108] 3) The mixed solution was then heated in a 70° C. water bath in a fume hood under magnetic stirring to allow the solvent to evaporate slowly until a wet gel was formed, thereby obtaining a LMFP / C-BP material.
[0109] Field emission scanning electron microscopy (Gemini SEM 300) was used to perform FESEM analysis tests on the LMFP / CNF-BP (750° C.) prepared in Comparative Example 2, the LMFP / CNF-HP and the LMFP / C-BP prepared in this comparative example.
[0110] Figure 4 a~c correspond to LMFP / CNF-BP, LMFP / CNF-HP and LMFP / C-BP respectively. Figure 4 As can be seen from a and b in Figure 1, ionic liquids, as structure-directing agents, can induce the formation of LMFP nanoparticles to a large extent. Figure 4 As a comparison, it can be seen in middle c that under non-electrospinning conditions, the composite material prepared using ionic liquid alone exhibits a larger particle size.
[0111] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a LMFP / CNF carbon nanofiber composite material, characterized in that: Adding a lithium source material, a manganese source material, an iron source material, a phosphate source material and a high molecular polymer into an organic solvent to obtain a spinning solution, electrospinning the spinning solution to obtain a precursor fiber; sequentially preheating, oxidizing and carbonizing the precursor fiber to obtain the LMFP / CNF carbon nanofiber composite material; The phosphate source includes one or more of 1-butyl-3-methylimidazole dihydrogen phosphate, phosphoric acid, potassium dihydrogen phosphate, and ammonium dihydrogen phosphate, and the high molecular polymer includes one or more of polyacrylonitrile, polyvinyl alcohol, and polylactic acid.
2. The method for preparing a LMFP / CNF carbon nanofiber composite material according to claim 1, characterized in that: In the spinning solution, the mass percentage of the high molecular weight polymer is 10% to 12%.
3. The method for preparing a LMFP / CNF carbon nanofiber composite material according to claim 2, characterized in that: In the spinning solution, the molar ratio of lithium, manganese, iron and phosphate is 1:0.6-0.8:0.4-0.2:1, and the mass ratio of the high molecular polymer to the lithium source material is 4.56-15.27:
1.
4. The method for preparing a LMFP / CNF carbon nanofiber composite material according to claim 1, characterized in that: The lithium source material includes one or more of anhydrous lithium acetate, lithium bromide, and lithium fluoride; the manganese source material includes one or more of anhydrous manganese acetate, manganese nitrate, and manganese chloride; and the iron source material includes one or more of triacetylacetonate iron, ferric nitrate, and ferric chloride.
5. The method for preparing a LMFP / CNF carbon nanofiber composite material according to claim 1, characterized in that: The organic solvent includes one or more of dimethylformamide, dimethylacetamide and acetonitrile.
6. The method for preparing a LMFP / CNF carbon nanofiber composite material according to any one of claims 1 to 5, characterized in that: The preheating oxidation step includes preheating the precursor fiber in an air atmosphere, the preheating oxidation temperature is 230° C. to 250° C., and the preheating oxidation time is 2 hours to 3 hours.
7. The method for preparing a LMFP / CNF carbon nanofiber composite material according to any one of claims 1 to 5, characterized in that: The step of carbonization treatment includes carbonizing the precursor fiber that has been preheated and oxidized in a mixed atmosphere of inert gas and hydrogen, the temperature of the carbonization treatment is 700° C. to 750° C., and the time of the carbonization treatment is 2 hours to 6 hours.
8. A LMFP / CNF carbon nanofiber composite material, characterized in that: The composite material is prepared by the method according to any one of claims 1 to 7.
9. The LMFP / CNF carbon nanofiber composite material according to claim 8, characterized in that: The composite material comprises LMFP grains, a carbon fiber structure and a thin carbon layer, wherein the LMFP grains are embedded in or coated in the carbon fiber structure, and the thin carbon layer uniformly covers the surface of the LMFP grains and / or the outer layer of the carbon fiber structure; and the particle size of the LMFP grains is 50 to 150 nm.
10. An application of the LMFP / CNF carbon nanofiber composite material as claimed in claim 8 or 9 in a new energy battery, characterized in that: The composite material is used for preparing positive electrode material.
Citation Information
Patent Citations
Lithium iron phosphate nanofiber as lithium ion battery cathode material and preparation method thereof
CN102340002A
Preparation method of nano-composite membrane electrode material
CN104868100A
Lithium iron phosphate composite material, preparation method thereof, positive plate and battery
CN115986081A
Fabricating method of lithium-iron-metal-phosphate-carbon composite nanofiber cathode active material and cathode active material fabricated by the method
KR1020130117023A
Carbon nanofibers containing catalyst nanoparticles
US20110171565A1
Cited By
Conductive carbon fiber lithium iron manganese phosphate composite material and preparation method thereof
CN120575363A
A conductive carbon fiber lithium manganese iron phosphate composite material and its preparation method
CN120575363B
Lithium manganese iron phosphate / carbon fiber composite positive electrode material and preparation method thereof
CN121076114A
A lithium iron manganese phosphate / carbon fiber composite positive electrode material and a preparation method thereof
CN121076114B
Preparation method of Li5FeO4-loaded conductive carbon fiber
CN121675107A