Grain-oriented electrical steel sheet and method for forming insulating coating film
The grain-oriented electrical steel sheet with a crystalline metal phosphate intermediate layer and tension coating layer addresses the adhesion and space factor challenges, ensuring superior performance for transformer cores by providing excellent adhesion and magnetic properties without reducing the space factor.
Patent Information
- Application Number
- PCT/JP2024/014857
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-12
- Filing Date
- 2024-04-12
- Publication Date
- 2024-10-17
AI Technical Summary
The challenge is to develop a grain-oriented electrical steel sheet without a forsterite coating that maintains excellent adhesion and magnetic properties while preventing a decrease in the space factor, which is essential for transformer core performance, and to address the difficulties in ensuring sufficient adhesion between the tension coating and the steel sheet surface in the absence of a forsterite coating.
A grain-oriented electrical steel sheet is created with a surface layer containing a plate-shaped crystalline metal phosphate intermediate layer, formed by electrochemical conversion treatment, which provides excellent adhesion and magnetic properties without reducing the space factor, and a tension coating layer composed of metal phosphate and colloidal silica, ensuring improved adhesion and corrosion resistance.
The solution achieves excellent tension coating adhesion, magnetic properties, and maintains a high space factor, making it suitable for transformer cores with enhanced industrial applicability.
Smart Images

Figure JP2024014857_17102024_PF_FP_ABST
Abstract
Description
Grain-oriented electrical steel sheet and method for forming insulating coating
[0001] The present invention relates to a grain-oriented electrical steel sheet and a method for forming an insulating coating. This application claims priority to Japanese Patent Application No. 2023-064840, filed on April 12, 2023, the contents of which are incorporated herein by reference.
[0002] Grain-oriented electrical steel sheets are primarily used in transformers. Transformers are continuously excited over a long period of time, from installation to disposal, and continue to generate energy loss. Therefore, the energy loss during magnetization with AC, i.e., core loss, is a major indicator that determines the performance of a transformer.
[0003] To reduce the iron loss of grain-oriented electrical steel sheets, many technologies have been developed to date, including (a) increasing the concentration in the {110}<001> orientation (Goss orientation), (b) increasing the content of solid solution elements such as Si to increase the electrical resistance of the steel sheet, or (c) reducing the thickness of the electrical steel sheet.
[0004] Furthermore, applying tension to steel sheets is effective in reducing iron loss. Forming a coating made of a material with a smaller thermal expansion coefficient than the steel sheet at high temperatures on the steel sheet surface is an effective means for reducing iron loss. A forsterite-based coating (inorganic coating) with excellent coating adhesion is produced by the reaction of oxides on the steel sheet surface with an annealing separator during the finish annealing process of electrical steel sheets. This coating can apply tension to steel sheets.
[0005] Furthermore, for example, the method disclosed in Patent Document 1, in which a coating liquid mainly composed of colloidal silica and phosphate is baked onto the surface of a steel sheet to form an insulating coating, is an effective method for reducing iron loss because it is highly effective in applying tension to the steel sheet. Therefore, a common method for producing grain-oriented electrical steel sheets is to leave the forsterite-based coating formed in the final annealing step and then apply an insulating coating mainly composed of phosphate on top of it.
[0006] However, in recent years, there has been an increasing demand for smaller and higher-performance transformers. To achieve this, grain-oriented electrical steel sheets are required to have excellent high-field iron loss characteristics, i.e., good iron loss even at high magnetic flux densities. At the same time, it has become clear that forsterite-based coatings hinder domain wall movement, adversely affecting iron loss. In grain-oriented electrical steel sheets, magnetic domains change due to domain wall movement under an AC magnetic field. Smooth and rapid domain wall movement is effective in reducing iron loss. However, forsterite-based coatings are nonmagnetic and have an uneven structure at the steel sheet / coating interface. This uneven structure is thought to hinder domain wall movement and adversely affect iron loss.
[0007] Therefore, as means for improving high magnetic field iron loss, research has been conducted on a variety of techniques, including methods for removing the forsterite-based coating by mechanical means such as polishing or chemical means such as pickling, techniques for producing grain-oriented electrical steel sheets that do not have a forsterite-based coating by preventing the formation of a forsterite-based coating during high-temperature finish annealing, and techniques for making the steel sheet surface mirror-finished (in other words, techniques for magnetically smoothing the steel sheet surface).
[0008] As a technique for preventing the formation of a forsterite-based coating, for example, Patent Document 2 discloses a technique in which, after normal finish annealing, the steel sheet is pickled to remove surface deposits, and then chemically or electrolytically polished to a mirror finish. It has been found that forming a tensioned insulating coating on the surface of a grain-oriented electrical steel sheet that does not have a forsterite-based coating and that has been obtained by such a known method can provide an even more excellent iron loss improvement effect. Furthermore, the tensioned insulating coating can impart various properties, such as corrosion resistance, heat resistance, and slip resistance, in addition to improving iron loss.
[0009] However, in addition to exhibiting insulating properties, forsterite-based coatings also function as intermediate layers that ensure adhesion when forming tension coatings (tension-applying insulating coatings). That is, because forsterite-based coatings are formed in a state where they penetrate deeply into the steel sheet, they have excellent adhesion to the metal steel sheet. Therefore, when a tension-applying coating (tension coating) containing colloidal silica, phosphate, or the like as a main component is formed on the surface of a forsterite-based coating, the coating has excellent adhesion. However, because bonding between metals and oxides is generally difficult, it has been difficult to ensure sufficient adhesion between a tension coating and the steel sheet surface in the absence of a forsterite-based coating.
[0010] Therefore, when forming a tension coating on a grain-oriented electrical steel sheet that does not have a forsterite-based coating, it is being considered to provide a layer that takes the role of the intermediate layer of the forsterite-based coating.
[0011] For example, Patent Document 3 discloses that grain-oriented electrical steel sheets that do not have a forsterite-based coating (inorganic coating) are annealed in a weakly reducing atmosphere to selectively thermally oxidize silicon that is inevitably contained in the silicon steel sheets, thereby forming SiO on the steel sheet surface. 2 Patent Document 4 discloses a technique for forming a tension-applying insulating coating on a grain-oriented electrical steel sheet that does not have a forsterite-based coating (inorganic coating) by subjecting the steel sheet to an anodic electrolysis treatment in a silicate solution to form a SiO layer on the steel sheet surface. 2 After the layers are formed, a tensioned insulating coating is applied.
[0012] However, the technique disclosed in Patent Document 3 requires the preparation of annealing equipment capable of controlling the atmosphere in order to perform annealing in a weakly reducing atmosphere, which results in a problem of processing costs. Also, in the technique disclosed in Patent Document 4, anodic electrolysis is performed in a silicate aqueous solution, thereby forming SiO 2 which maintains sufficient adhesion with the tension-imparting insulating coating. 2 In order to obtain such a layer on the surface of the steel sheet, it is necessary to prepare new electrolytic treatment equipment, which increases the treatment cost.
[0013] In contrast, Patent Document 5 discloses a grain-oriented electrical steel sheet having a base steel sheet and an insulating coating formed on the surface of the base steel sheet, the insulating coating being formed on the base steel sheet side, an intermediate layer containing a crystalline metal phosphate, and a tensile coating layer formed on the surface side of the insulating coating. In this grain-oriented electrical steel sheet, the intermediate layer can be formed by chemical conversion treatment.
[0014] JP-A-48-039338 JP-A-49-96920 JP-A-6-184762 JP-A-11-209891 International Publication No. 2022 / 215709
[0015] The technology of Patent Document 5 improves coating adhesion, coating tension, and magnetic properties by providing an intermediate layer made of a crystalline metal phosphate between the base steel sheet and the tension coating. Furthermore, since the intermediate layer can be formed by chemical conversion treatment, no special equipment is required. Therefore, it is a useful technology. However, the technology of Patent Document 5 has a problem in that productivity deteriorates when attempting to further improve adhesion. This is because it takes time to precipitate the crystalline metal phosphate by chemical conversion treatment.
[0016] To address the above-mentioned issues, it is conceivable to precipitate crystalline metal phosphate by electrolytic chemical conversion treatment. However, when an attempt is made to form a crystalline metal phosphate layer on the surface of a grain-oriented electrical steel sheet without a forsterite-based coating by electrolytic chemical conversion treatment, the metal phosphate crystals may become coarse. If the metal phosphate crystals become large, the space factor will decrease when an actual transformer is manufactured.
[0017] Therefore, the present invention aims to provide a grain-oriented electrical steel sheet in which a layer containing metal phosphate is formed on the surface of a steel sheet having a forsterite-based coating by chemical conversion treatment, which has excellent adhesion and magnetic properties of a tension coating and does not reduce the space factor of a transformer (core), provided that the basic properties required of the coating, such as corrosion resistance and resistance to leaching of phosphoric acid, are not reduced.
[0018] The present inventors have investigated a method for obtaining grain-oriented electrical steel sheets that have excellent adhesion and magnetic properties of tension coatings and that do not reduce the space factor of transformer cores, based on the premise of forming a layer of crystalline metal phosphate on the surface of grain-oriented electrical steel sheets without a forsterite-based coating by electrolytic chemical conversion. As a result, they have found that coarsening of crystalline metal phosphates can be suppressed by performing electrolytic chemical conversion at a specific current density and by controlling the metal ion concentration, phosphate ion concentration, and nitrate ion concentration of the treatment solution within specific ranges. Furthermore, they have found that grain-oriented electrical steel sheets having such a layer of crystalline metal phosphate exhibit excellent adhesion and magnetic properties of tension coatings and a high space factor when used as transformers.
[0019] The present invention has been made in light of the above findings. The gist of the present invention is as follows. [1] A grain-oriented electrical steel sheet according to one aspect of the present invention comprises a base steel sheet and an insulating coating formed on a surface of the base steel sheet, the insulating coating being formed on the base steel sheet side and comprising an intermediate layer containing a crystalline metal phosphate and a tensile coating layer formed on the surface side of the insulating coating, the crystalline metal phosphate being plate-like and having an average particle size of 0.5 to 3.0 μm. [2] In the grain-oriented electrical steel sheet according to [1] above, the crystalline metal phosphate in the intermediate layer may comprise one or more of zinc phosphate, manganese phosphate, iron manganese phosphate, and zinc calcium phosphate. [3] In the grain-oriented electrical steel sheet according to [1] above, the intermediate layer may have a thickness of 0.1 to 9.0 μm. [4] A method of forming an insulating coating according to one aspect of the present invention is a method of forming the insulating coating provided in the grain-oriented electrical steel sheet according to [1] above, the method comprising the steps of: 2 O 3a finish annealing process in which an annealing separator containing 10 to 100 mass % of the above-mentioned compound is applied to the steel sheet after the finish annealing process, the steel sheet is dried, and then finish annealed; an annealing separator removing process in which excess annealing separator is removed from the steel sheet after the finish annealing process; a light pickling process in which the steel sheet after the annealing separator removing process is pickled with 0.1 to 10.0 mass % of one inorganic acid selected from sulfuric acid, chloric acid, nitric acid, and phosphoric acid at a solution temperature of 20 to 90°C for 1 to 20 seconds; and a mixed treatment solution having a solution temperature of 30 to 90°C and a metal ion concentration of 10 to 50 g / l, a phosphate ion concentration of 10 to 100 g / l, and a nitrate ion concentration of 20 to 80 g / l, at a current density of 1.0 to 50 A / dm 2 a drying step of removing the steel sheet after the intermediate layer forming step from the mixed treatment liquid, removing excess mixed treatment liquid, and then drying the steel sheet; and a tensile coating layer forming step of applying a coating liquid containing a metal phosphate and colloidal silica, the total concentration of the metal phosphate and the colloidal silica being 10 to 40 mass %, to the steel sheet after the drying step, drying the coating liquid, and then heating the steel sheet to a sheet temperature of 700 to 950°C for 10 to 60 seconds.
[0020] According to the present invention, it is possible to provide a grain-oriented electrical steel sheet that has excellent adhesion of a tension coating and magnetic properties, and that does not reduce the space factor of a transformer (core).
[0021] 1 is an example of a cross-sectional view of a grain-oriented electrical steel sheet according to an embodiment of the present invention.
[0022] A grain-oriented electrical steel sheet according to an embodiment of the present invention (the grain-oriented electrical steel sheet according to the present embodiment) and a method for manufacturing the grain-oriented electrical steel sheet according to the present embodiment, including a method for forming an insulating coating provided on the grain-oriented electrical steel sheet according to the present embodiment, will be described. First, the grain-oriented electrical steel sheet according to the present embodiment will be described.
[0023] As shown in Fig. 1, the grain-oriented electrical steel sheet 100 according to this embodiment has a base steel sheet 1 and an insulating coating 2 formed on the surface of the base steel sheet 1. In the grain-oriented electrical steel sheet 100 according to this embodiment, a forsterite-based coating is not intentionally formed on the surface of the base steel sheet 1, and in many cases a forsterite-based coating is not present, but the coating amount of the forsterite-based coating is 1.0 g / m 2 If it is below this value, its presence is permitted (in this case, it is present in a part between the base steel sheet 1 and the insulating coating 2).
[0024] The insulating coating 2 also has a tensile coating layer 22 formed on the surface side of the insulating coating 2 (i.e., the surface side of the grain-oriented electrical steel sheet 100), and an intermediate layer 21 formed on the base steel sheet 1 side and containing a crystalline metal phosphate.
[0025] The crystalline metal phosphate of the intermediate layer 21 is plate-shaped and has an average particle size of 0.5 to 3.0 μm. Each of these will be explained below.
[0026] <Base Steel Sheet> (Chemical Composition) The grain-oriented electrical steel sheet 100 according to this embodiment is significantly characterized by the structure of the insulating coating 2 formed on the surface of the base steel sheet 1, and the base steel sheet 1 included in the grain-oriented electrical steel sheet 100 is not limited in terms of its chemical composition. However, in order to obtain the properties generally required of a grain-oriented electrical steel sheet, it is preferable that the chemical components include the following: In this embodiment, % relating to the chemical components is % by mass unless otherwise specified.
[0027] C: 0.010% or less C (carbon) is an element effective for controlling the structure of steel sheets in the manufacturing process up to the completion of the decarburization annealing process. However, if the C content exceeds 0.010%, the magnetic properties of the finished grain-oriented electrical steel sheet deteriorate. Therefore, in the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment, the C content is preferably 0.010% or less. The C content is more preferably 0.005% or less. Although a lower C content is preferable, reducing the C content to less than 0.0001% saturates the effect of structural control and simply increases manufacturing costs. Therefore, the C content may be 0.0001% or more.
[0028] Si: 2.50 to 4.00% Si (silicon) is an element that increases the electrical resistance of grain-oriented electrical steel sheets and improves their iron loss characteristics. If the Si content is less than 2.50%, a sufficient eddy current loss reduction effect cannot be obtained. Therefore, the Si content is preferably 2.50% or more. The Si content is more preferably 2.70% or more, and even more preferably 3.00% or more. On the other hand, if the Si content exceeds 4.00%, the grain-oriented electrical steel sheets become embrittled and their threading properties deteriorate significantly. Furthermore, the workability of the grain-oriented electrical steel sheets decreases, and the steel sheets may break during rolling. Therefore, the Si content is preferably 4.00% or less. The Si content is more preferably 3.80% or less, and even more preferably 3.70% or less.
[0029] Mn: 0.01 to 0.50% Mn (manganese) is an element that combines with S to form MnS during the manufacturing process. This precipitate functions as an inhibitor (a suppressor of normal grain growth) and induces secondary recrystallization in the steel. Mn also enhances the hot workability of the steel. If the Mn content is less than 0.01%, the above-mentioned effects cannot be fully achieved. Therefore, the Mn content is preferably 0.01% or more. The Mn content is more preferably 0.02% or more. On the other hand, if the Mn content exceeds 0.50%, secondary recrystallization does not occur and the magnetic properties of the steel deteriorate. Therefore, in the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment, the Mn content is preferably 0.50% or less. The Mn content is more preferably 0.20% or less, and even more preferably 0.10% or less.
[0030] N: 0.010% or less N (nitrogen) is an element that bonds with Al during the manufacturing process to form AlN, which functions as an inhibitor. However, if the N content exceeds 0.010%, excessive inhibitors remain in the grain-oriented electrical steel sheet, resulting in reduced magnetic properties. Therefore, in the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment, the N content is preferably 0.010% or less. The N content is more preferably 0.008% or less. On the other hand, the lower limit of the N content is not particularly specified, but reducing the N content to less than 0.001% only increases manufacturing costs. Therefore, the N content may be 0.001% or more.
[0031] Sol. Al: 0.020% or less Sol. Al (acid-soluble aluminum) is an element that bonds with N to form AlN, which functions as an inhibitor, during the manufacturing process of grain-oriented electrical steel sheets. However, if the sol. Al content of the base steel sheet exceeds 0.020%, excessive inhibitors remain in the base steel sheet, resulting in reduced magnetic properties. Therefore, in the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment, the sol. Al content is preferably 0.020% or less. The sol. Al content is more preferably 0.010% or less, and even more preferably less than 0.001%. There is no particular restriction on the lower limit of the sol. Al content, but reducing it to less than 0.0001% only increases manufacturing costs. Therefore, the sol. Al content may be 0.0001% or more.
[0032] S: 0.010% or less S (sulfur) is an element that combines with Mn during the manufacturing process to form MnS, which functions as an inhibitor. However, if the S content exceeds 0.010%, the magnetic properties will be reduced due to the remaining inhibitor. Therefore, in the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment, the S content is preferably 0.010% or less. The S content in the grain-oriented electrical steel sheet is preferably as low as possible. For example, less than 0.001%. However, reducing the S content in the grain-oriented electrical steel sheet to less than 0.0001% will only increase the manufacturing cost. Therefore, the S content in the grain-oriented electrical steel sheet may be 0.0001% or more.
[0033] Balance: Fe and impurities The chemical composition of the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment may contain the above-mentioned elements, with the balance being Fe and impurities. However, for the purpose of improving magnetic properties, etc., Sn, Cu, Se, and Sb may also be contained in the ranges shown below. Furthermore, even if other elements, such as W, Nb, Ti, Ni, Co, V, Cr, and Mo, are contained in a total of 1.0% or less, the effects of the grain-oriented electrical steel sheet according to this embodiment are not impaired. Here, impurities refer to elements that are mixed in from raw materials such as ore, scrap, or the manufacturing environment during industrial production of the base steel sheet, and are allowed to be contained in amounts that do not adversely affect the function of the grain-oriented electrical steel sheet according to this embodiment.
[0034] Sn: 0 to 0.50% Sn (tin) is an element that contributes to improving magnetic properties through controlling the primary recrystallization structure. To obtain the effect of improving magnetic properties, the Sn content is preferably 0.01% or more. The Sn content is more preferably 0.02% or more, and even more preferably 0.03% or more. On the other hand, if the Sn content exceeds 0.50%, secondary recrystallization becomes unstable and magnetic properties deteriorate. Therefore, the Sn content is preferably 0.50% or less. The Sn content is more preferably 0.30% or less, and even more preferably 0.10% or less.
[0035] Cu: 0 to 0.50% Cu (copper) is an element that contributes to increasing the Goss orientation occupancy rate in the secondary recrystallized structure. To achieve the above effect, the Cu content is preferably 0.01% or more. The Cu content is more preferably 0.02% or more, and even more preferably 0.03% or more. On the other hand, if the Cu content exceeds 0.50%, the steel sheet becomes embrittled during hot rolling. Therefore, in the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment, the Cu content is preferably 0.50% or less. The Cu content is more preferably 0.30% or less, and even more preferably 0.10% or less.
[0036] Se: 0 to 0.020% Se (selenium) is an element that has the effect of improving magnetic properties. When Se is contained, the Se content is preferably 0.001% or more to effectively exhibit the effect of improving magnetic properties. The Se content is more preferably 0.003% or more, and even more preferably 0.006% or more. On the other hand, if the Se content exceeds 0.020%, the adhesion of the coating deteriorates. Therefore, the Se content is preferably 0.020% or less. The Se content is more preferably 0.015% or less, and even more preferably 0.010% or less.
[0037] Sb: 0 to 0.50% Sb (antimony) is an element that has the effect of improving magnetic properties. When Sb is contained, the Sb content is preferably 0.005% or more to effectively exhibit the effect of improving magnetic properties. The Sb content is more preferably 0.01% or more, and even more preferably 0.02% or more. On the other hand, if the Sb content exceeds 0.50%, the adhesion of the coating significantly deteriorates. Therefore, the Sb content is preferably 0.50% or less. The Sb content is more preferably 0.30% or less, and even more preferably 0.10% or less.
[0038] As described above, the chemical composition of the base steel sheet of the grain-oriented electrical steel sheet in this embodiment is, for example, one that contains the above-mentioned elements with the balance being Fe and impurities.
[0039] The chemical composition of the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment can be measured using a known ICP atomic emission spectroscopy. However, if an insulating coating is formed on the surface, it must be removed before measurement. The removal can be achieved by immersing the sample in a highly concentrated alkaline solution (e.g., a 30% sodium hydroxide solution heated to 85°C) for 20 minutes or more. Peeling can be determined visually. For small samples, removal can also be achieved by surface grinding.
[0040] <Insulating Coating> The grain-oriented electrical steel sheet 100 according to this embodiment has an insulating coating 2 formed on the surface of a base steel sheet 1. The insulating coating 2 is made up of, in order from the base steel sheet 1 side, an intermediate layer 21 and a tensile coating layer 22.
[0041] (Intermediate Layer) As described above, grain-oriented electrical steel sheets generally have a forsterite-based coating formed in the final annealing process and an insulating coating (tensile insulating coating) formed thereon. However, in recent years, it has become clear that this forsterite-based coating hinders the movement of domain walls and adversely affects iron loss. Therefore, grain-oriented electrical steel sheets without a forsterite-based coating have been studied to further improve magnetic properties. However, if a forsterite-based coating is not present, it is difficult to ensure sufficient adhesion between the tensile coating and the surface of the base steel sheet.
[0042] In the grain-oriented electrical steel sheet 100 of this embodiment, an intermediate layer 21 containing a crystalline metal phosphate is formed between the base steel sheet 1 and the tensile coating, thereby improving the adhesion between the base steel sheet 1 and the tensile coating layer 22 via the intermediate layer 21.
[0043] When the intermediate layer 21 contains crystalline metal phosphate, the tensile coating formed thereon (which becomes the tensile coating layer 22 after formation) also contains metal phosphate, resulting in high affinity and excellent adhesion between the intermediate layer and the tensile coating layer. Furthermore, when the intermediate layer is formed by immersion in a treatment solution containing metal phosphate, as described below, it can be formed on the surface of the base steel sheet 1 by utilizing a chemical reaction, and adhesion between the intermediate layer 21 and the base steel sheet 1 can also be ensured.
[0044] If the intermediate layer 21 does not contain a crystalline metal phosphate, the above-mentioned effect cannot be obtained. The proportion of the crystalline metal phosphate in the intermediate layer is preferably 80 mass % or more, and may be 100 mass %. In terms of adhesion, the metal phosphate is preferably one or more of zinc phosphate, manganese phosphate, iron phosphate, and zinc calcium phosphate.
[0045] The intermediate layer may contain oxides and elements such as Fe and Si diffused from the base steel sheet as the remainder of the metal phosphate.
[0046] However, if the crystals of the crystalline metal phosphate in the intermediate layer become coarse, when an actual transformer is manufactured, the space factor decreases, which reduces the magnetic flux density per unit volume and increases the transformer iron loss.
[0047] Therefore, in the grain-oriented electrical steel sheet according to this embodiment, the crystalline metal phosphate contained in the intermediate layer is plate-shaped and has an average particle size of 0.5 to 3.0 μm. Here, plate-shaped refers to a shape in which the length of one of the three sides of the crystal is less than 1 / 5 of the length of the other two sides. In contrast, a columnar shape is defined when the length of one of the three sides of the crystal is at least 5 times the length of the other two sides, and the lengths of the other two sides are 0.5 to less than 2.0 times each other. A granular shape is defined when the length of each of the three sides of the crystal is 0.5 to less than 2.0 times each other. An acicular shape is defined when the length of one of the three sides of the crystal is at least 20 times the length of the other two sides, and the lengths of the other two sides are 0.5 to less than 2.0 times each other.
[0048] If the crystalline metal phosphate is not in a plate shape, the space factor may decrease and the adhesion may become poor.
[0049] If the average particle size is less than 0.5 μm, the crystals will be sparse and the adhesion will be poor, whereas if the average particle size is more than 3.0 μm, the space factor will be poor.
[0050] The intermediate layer 21 is formed at a different time from the tensile coating formed thereon, but the intermediate layer 21 and the tensile coating layer 22 together function as the insulating coating 2 .
[0051] The thickness of the intermediate layer is preferably 0.1 to 9.0 μm in order to achieve both adhesion and magnetic properties. If the average thickness of the intermediate layer 21 is less than 0.1 μm, the effect of improving adhesion between the base steel sheet and the insulating coating via the intermediate layer may not be sufficiently obtained. On the other hand, if the average thickness of the intermediate layer exceeds 9.0 μm, the magnetic properties may deteriorate.
[0052] The mass fraction and type of the crystalline metal phosphate in the intermediate layer can be determined by measuring a cross section of the intermediate layer in the thickness direction using a scanning electron microscope and an energy dispersive elemental analyzer. Whether the metal phosphate in the intermediate layer 21 is a crystalline metal phosphate can be determined by X-ray crystal structure analysis.
[0053] The thickness of the intermediate layer can be measured as an average by observing the cross section of the sample with a scanning electron microscope and measuring the thickness at five or more points. The base steel sheet and the insulating coating can be distinguished based on the concentration of P (phosphorus) derived from metal phosphate (a P content of 1.0 mass% or more is considered to be an insulating coating, and a P content of less than 1.0 mass% is considered to be a base steel sheet). Furthermore, the intermediate layer 21 and the tensile coating layer 22 of the insulating coating 2 can be distinguished based on the presence or absence of silicon (Si) derived from silica (the tensile coating layer contains silica, as described below).
[0054] The average crystal grain size of crystalline metal phosphate can be determined by the following method. A steel sheet sample is cut into several millimeters square and subjected to ion milling (CP) to remove microscopic shape defects such as sagging and cracks. Then, a cross section of the steel sheet along the rolling direction and a cross section perpendicular to the rolling direction are observed using a scanning electron microscope. If two or more crystals with one side less than one-fifth the length of the other sides are observed from the observed crystalline morphology of the metal phosphate, it is determined that plate-like crystals have formed. The average crystal grain size is calculated by measuring the long sides of five or more crystals of each observed metal phosphate crystal. The electron microscope magnification during observation is 1000x, and five observation points are observed.
[0055] (Tension Coating Layer) In the grain-oriented electrical steel sheet 100 according to this embodiment, a tension coating is formed on the surface of the intermediate layer 21 , and thus a tension coating layer 22 is provided on the surface side of the insulating coating 2 .
[0056] The tensile coating layer 22 is not particularly limited as long as it is used as an insulating coating for grain-oriented electrical steel sheets, but from the viewpoint of adhesion to the intermediate layer 21 (adhesion to the base steel sheet 1 via the intermediate layer 21), it is preferable that the composition of the tensile coating layer 22 is mainly composed of a metal phosphate. It is more preferable that the composition of the tensile coating layer 22 essentially consists of a metal phosphate and silica.
[0057] The tensile coating layer 22 preferably contains metal phosphate and silica (derived from colloidal silica in the coating liquid) so that the silica content is 20% by mass or more. On the other hand, if the silica content of the tensile coating layer 22 exceeds 60% by mass, it may cause powdering, so it is preferably 60% by mass or less. Furthermore, it preferably contains a total of 70% by mass or more of metal phosphate and silica. The total of metal phosphate and silica may be 100% by mass. The remainder other than metal phosphate and silica may include ceramic particles such as alumina and silicon nitride. Aluminum phosphate is preferred as the metal phosphate in terms of heat resistance.
[0058] Although the thickness of the tensile coating layer 22 is not limited, the average thickness of the insulating coating 2 (intermediate layer 21 + tensile coating layer 22) is preferably 1.0 to 20.0 μm, assuming that the average thickness of the intermediate layer 21 is within the above range. If the average thickness of the insulating coating 2 is less than 1.0 μm, sufficient coating tension cannot be obtained. Furthermore, the amount of phosphate elution increases. This can cause stickiness and reduced corrosion resistance, and may even lead to coating peeling. Furthermore, if the thickness of the insulating coating 2 exceeds 20.0 μm, the space factor decreases, deteriorating magnetic properties, or cracks can occur, resulting in reduced adhesion and reduced corrosion resistance.
[0059] In the tensile coating layer 22, the mass proportion of the metal phosphate and the type of the metal phosphate can be determined in a cross section in the thickness direction in the same manner as in the intermediate layer.
[0060] As mentioned above, the tension coating layer and the intermediate layer can be distinguished by their different silica contents.
[0061] The thickness of the tensile coating layer 22 can be determined in the same manner as the intermediate layer 21. The sum of the thickness of the tensile coating layer 22 and the thickness of the intermediate layer 21 is the thickness of the insulating coating 2.
[0062] <Manufacturing Method> The grain-oriented electrical steel sheet according to this embodiment can be suitably manufactured by a manufacturing method that satisfies the manufacturing conditions described below. However, it goes without saying that the grain-oriented electrical steel sheet according to this embodiment is not particularly limited to a manufacturing method. In other words, a grain-oriented electrical steel sheet having the configuration described above is considered to be the grain-oriented electrical steel sheet according to this embodiment, regardless of its manufacturing conditions.
[0063] The grain-oriented electrical steel sheet according to this embodiment can be manufactured by a manufacturing method including the following steps: (I) a hot rolling step of hot-rolling a steel slab having a predetermined chemical composition to obtain a hot-rolled sheet, (II) a hot-rolled sheet annealing step of annealing the hot-rolled sheet, (III) a cold-rolling step of cold-rolling the hot-rolled sheet after the hot-rolled sheet annealing step to obtain a steel sheet (cold-rolled sheet), (IV) a decarburization annealing step of decarburizing the steel sheet after the cold-rolling step, and (V) a step of adding Al to the steel sheet. 2 O 3 (VII) an annealing separator removing step of removing excess annealing separator from the steel sheet after the final annealing step; (VIII) a light pickling step of pickling the steel sheet after the annealing separator removing step with 0.1 to 10.0 mass % of one inorganic acid selected from sulfuric acid, chloric acid, nitric acid, and phosphoric acid at a solution temperature of 20 to 90°C for 1 to 20 seconds; and (IX) a light pickling step of rinsing the steel sheet after the light pickling step with water, and then pickling the steel sheet after the light pickling step with a mixed treatment solution having a metal ion concentration of 10 to 50 g / l, a phosphate ion concentration of 10 to 100 g / l, and a nitrate ion concentration of 20 to 80 g / l at a solution temperature of 30 to 90°C, at a current density of 1.0 to 50 A / dm 2(X) a drying step of removing the steel sheet after the intermediate layer forming step from the mixed treatment solution, removing excess of the mixed treatment solution, and then drying, (XI) a tension coating layer forming step of applying a coating solution containing a metal phosphate and colloidal silica, the metal phosphate and the colloidal silica having a total concentration of 10 to 40 mass %, to the steel sheet after the drying step, drying, and then heating and holding the steel sheet at a sheet temperature of 700 to 950°C for 10 to 60 seconds. The method for producing a grain-oriented electrical steel sheet according to this embodiment may further include one or both of: (XII) a nitriding treatment step of nitriding the steel sheet between the decarburization annealing step and the finish annealing step; and (XIII) a magnetic domain refining step of controlling the magnetic domains of the steel sheet after the tension coating layer forming step. Of these, the manufacturing of the grain-oriented electrical steel sheet according to this embodiment is characterized by the steps (V) finish annealing step to (XI) tension coating layer forming step (these steps may be collectively referred to as the method for forming the insulating coating), which are mainly related to the formation of the insulating coating, and known conditions can be used for the other steps or conditions not described. These steps will be described below.
[0064] [Hot Rolling Process] In the hot rolling process, a steel billet such as a slab having a predetermined chemical composition is heated and then hot rolled to obtain a hot-rolled sheet. The heating temperature of the steel billet is preferably within the range of 1100 to 1450°C. The heating temperature is more preferably 1300 to 1400°C.
[0065] The chemical composition of the slab can be varied depending on the chemical composition of the grain-oriented electrical steel sheet to be finally obtained, but an example of such a chemical composition may include, in mass %, C: 0.01-0.20%, Si: 2.50-4.00%, sol. Al: 0.01-0.040%, Mn: 0.01-0.50%, N: 0.020% or less, S: 0.005-0.040%, Cu: 0-0.50%, Sn: 0-0.50%, Se: 0-0.020%, Sb: 0-0.50%, and the balance being Fe and impurities. The hot rolling conditions are not particularly limited and may be set appropriately based on the desired properties. The thickness of the hot-rolled sheet is preferably within the range of, for example, 2.0-3.0 mm.
[0066] [Hot-rolled sheet annealing process] The hot-rolled sheet annealing process is a process of annealing the hot-rolled sheet manufactured through the hot rolling process. By performing such annealing treatment, recrystallization occurs in the steel sheet structure, and good magnetic properties can be achieved, which is preferable.
[0067] When hot-rolled sheet annealing is performed, the hot-rolled sheet produced through a hot rolling process may be annealed according to a known method. The means for heating the hot-rolled sheet during annealing is not particularly limited, and known heating methods can be used. The annealing conditions are also not particularly limited. For example, the hot-rolled sheet may be annealed in a temperature range of 900 to 1200°C for 10 seconds to 5 minutes.
[0068] [Cold Rolling Step] In the cold rolling step, the hot rolled sheet after the hot rolled sheet annealing step is subjected to cold rolling to obtain a steel sheet (cold rolled sheet). The cold rolling may be a single cold rolling (a series of cold rolling steps without annealing in between), or may be multiple cold rolling steps with intermediate annealing between them, in which the cold rolling is interrupted and at least one or two or more intermediate annealing steps are performed before the final pass of the cold rolling step.
[0069] When intermediate annealing is performed, it is preferable to hold the steel sheet at a temperature of 1000 to 1200°C for 5 to 180 seconds. The annealing atmosphere is not particularly limited. In consideration of manufacturing costs, it is preferable to perform intermediate annealing three times or less.
[0070] Furthermore, before the cold rolling step, the surface of the hot-rolled sheet may be subjected to pickling.
[0071] In the cold rolling process according to this embodiment, the hot-rolled sheet after the hot-rolled sheet annealing process is cold-rolled according to a known method to obtain a steel sheet. For example, the final reduction can be in the range of 80 to 95%. A final reduction of 80% or more is preferable because it is possible to obtain Goss nuclei with a high concentration of {110}<001> orientation in the rolling direction. On the other hand, a final reduction of more than 95% is not preferable because it increases the possibility of unstable secondary recrystallization in the subsequent finish annealing process.
[0072] The final rolling reduction is the cumulative rolling reduction of cold rolling, and in the case where intermediate annealing is performed, it is the cumulative rolling reduction of cold rolling after final intermediate annealing.
[0073] [Decarburization Annealing Step] In the decarburization annealing step, the obtained steel sheet is subjected to decarburization annealing. In the decarburization annealing, the conditions for the decarburization annealing are not limited as long as the steel sheet undergoes primary recrystallization and C, which adversely affects magnetic properties, can be removed from the steel sheet. For example, the oxidation degree (PH) in the annealing atmosphere (furnace atmosphere) can be adjusted. 2 O / PH 2 ) is set to 0.3 to 0.6, and the annealing temperature is set to 800 to 900° C., and the holding is performed for 10 to 600 seconds.
[0074] [Nitriding Process] Nitriding may be performed between the decarburization annealing process and the finish annealing process described below. In the nitriding process, for example, the steel sheet after the decarburization annealing process is maintained at approximately 700 to 850°C in a nitriding atmosphere (an atmosphere containing hydrogen, nitrogen, and ammonia or other nitriding gases) to perform nitriding. When AlN is used as an inhibitor, it is preferable to set the N content of the steel sheet after the nitriding process to 40 ppm or more by the nitriding process. On the other hand, if the N content of the steel sheet after the nitriding process exceeds 1000 ppm, excess AlN remains in the steel sheet even after the completion of secondary recrystallization in the finish annealing. Such AlN can cause iron loss degradation. For this reason, it is preferable to set the N content of the steel sheet after the nitriding process to 1000 ppm or less.
[0075] [Finish annealing step] In the finish annealing step, Al is added to the steel sheet after the decarburization annealing step or after the nitriding treatment (after the nitriding treatment step). 2 O 3 After drying, finish annealing is performed.
[0076] In conventional methods for manufacturing grain-oriented electrical steel sheets, a forsterite-based coating is formed on the surface of a steel sheet (cold-rolled sheet) by applying an annealing separator mainly containing MgO and then performing finish annealing.
[0077] In contrast, in the method for producing a grain-oriented electrical steel sheet according to this embodiment, Al is added so that a forsterite-based coating is hardly formed. 2 O 3 On the other hand, an annealing separator containing Al is used. 2 O 3 The ratio of Al may be 100 mass %, but 2 O 3 From the viewpoint of preventing seizure of Al, in the method for producing a grain-oriented electrical steel sheet according to this embodiment, the annealing separator preferably contains MgO. Although the content of MgO may be 0%, in order to obtain the above effect, the content of MgO is preferably 5 mass% or more. When MgO is contained, the content of MgO is preferably 10 mass% or more. 2 O 3 The content of Al relative to the annealing separator is 90 mass % or less to ensure this. The content of MgO is preferably 50 mass % or less. 2 O 3 The total amount of MgO and MgO may be more than 50% by mass in terms of solid content.
[0078] Furthermore, in the method for producing a grain-oriented electrical steel sheet according to this embodiment, the annealing separator may further contain chloride. When the annealing separator contains chloride, the effect of making it more difficult for a forsterite-based coating to form is obtained. The chloride content is not particularly limited and may be 0%, but to obtain the above effect, a content of 0.5 to 10 mass% is preferable. Effective chlorides include, for example, bismuth chloride, calcium chloride, cobalt chloride, iron chloride, and nickel chloride.
[0079] The conditions for the finish annealing are not limited, but for example, conditions in which the steel is held at a temperature of 1150 to 1250° C. for 10 to 60 hours can be adopted.
[0080] [Annealing Separator Removal Step] In the annealing separator removal step, excess annealing separator is removed from the steel sheet after the finish annealing step. For example, the excess annealing separator can be removed by washing with water.
[0081] [Light Pickling Process] In the light pickling process, the steel sheet after the annealing separator removal process is pickled for 1 to 20 seconds with 0.1 to 10.0 mass % of one inorganic acid selected from sulfuric acid, chloric acid, nitric acid, and phosphoric acid at a solution temperature of 20 to 90°C. This has the effect of densifying the crystalline phosphate. If the light pickling conditions are not appropriate, the adhesion of the tension coating layer will be poor.
[0082] [Intermediate layer forming process] [Drying process] In the intermediate layer forming process, the steel sheet after the light pickling process is washed with water and then immersed in a treatment solution, and an electric current is passed through the treatment solution while immersed to form an intermediate layer. In the drying process, the steel sheet after the intermediate layer forming process is pulled out of the treatment solution, excess treatment solution is removed, and then the steel sheet is dried. This forms an intermediate layer on the surface of the base steel sheet.
[0083] The treatment liquid is a mixed treatment liquid having a metal ion concentration of 10 to 50 g / l, a phosphate ion concentration of 10 to 100 g / l, and a nitrate ion concentration of 20 to 80 g / l.
[0084] If the metal ion concentration in the mixed treatment solution is less than 10 g / L, the formation of crystalline metal phosphate is suppressed, resulting in granular crystals and poor adhesion. On the other hand, if the concentration exceeds 50 g / L, the formation of crystalline metal phosphate is likely to be uneven, resulting in the appearance of coarse crystals, a reduced space factor, and uneven formation of the intermediate layer. Furthermore, if the phosphate ion concentration in the mixed treatment solution is less than 10 g / L, the precipitation of crystalline metal phosphate takes a long time, resulting in the appearance of coarse crystals and poor space factor. On the other hand, if the concentration exceeds 100 g / L, the formation of crystalline metal phosphate is likely to be uneven, resulting in the formation of coarse crystals and the progression of etching of the steel sheet surface, resulting in a reduced space factor, corrosion resistance, and coating tension. Furthermore, if the nitrate ion concentration in the mixed treatment solution is less than 20 g / L, hydrogen gas generation cannot be suppressed, making it difficult for current to flow uniformly. This results in the intermediate layer being formed too thick in areas where current flows, resulting in poor adhesion, and in the intermediate layer being thin in areas where current does not flow, resulting in a low coating tension. On the other hand, if it exceeds 80 g / l, the concentration of phosphate ions will decrease, and it will take a long time for the crystalline metal phosphate to precipitate, resulting in coarse needle-like crystals and a poor space factor.
[0085] Furthermore, during immersion, the temperature of the mixed treatment solution is set to 30 to 90° C. If the temperature of the mixed treatment solution is below 30° C., it takes too long for the crystalline metal phosphate to precipitate, making it less economical. On the other hand, if the temperature exceeds 90° C., the mixed treatment solution becomes unstable, resulting in uneven formation of the intermediate layer.
[0086] When energizing, the current density is 1.0 to 50 A / dm 2 The current density is 1.0 A / dm 2 If the amount is less than this, it takes too long for the crystalline metal phosphate to precipitate, which is economically disadvantageous.
[0087] On the other hand, when the current density is 50 A / dm 2 If the current is too long, the current will not flow evenly through the sample, causing uneven formation of the intermediate layer known as 'skimming'. If the current application time is too short, it will take a long time to form the intermediate layer and the adhesion will be sparse. On the other hand, if the current application time is too long, the intermediate layer will be formed in some places excessively, causing uneven adhesion and a non-uniform state known as 'skimming'. Therefore, it is preferable to set the current application time to 3 to 30 seconds.
[0088] Furthermore, if the drying temperature is too high, voids may occur, resulting in poor adhesion, so the drying temperature is preferably 300° C. or lower, more preferably 200° C. or lower. The drying temperature is preferably 100° C. or higher.
[0089] [Tension coating layer forming process] In the tensile coating layer forming process, a coating liquid containing metal phosphate and colloidal silica, with a total concentration of the metal phosphate and colloidal silica of 10 to 40 mass %, is applied to the steel sheet after the drying process, dried, and then heated and held at a sheet temperature of 700 to 950°C for 10 to 60 seconds, thereby forming a tensile coating layer on the surface of the intermediate layer.
[0090] If the sheet temperature during holding is less than 700°C, the tension will be low and the magnetic properties will be inferior. Therefore, it is preferable that the sheet temperature be 700°C or higher. On the other hand, if the sheet temperature is higher than 950°C, the rigidity of the steel sheet will decrease and it will be more likely to deform. In this case, strain may be introduced into the steel sheet due to transportation, etc., resulting in inferior magnetic properties. Therefore, it is preferable that the sheet temperature be 950°C or lower.
[0091] Furthermore, if the holding time is less than 10 seconds, the elution resistance will be poor. Therefore, the holding time is set to 10 seconds or more. On the other hand, if the holding time is more than 60 seconds, the adhesion of the tensile coating layer will be poor. Therefore, the holding time is preferably 60 seconds or less.
[0092] The coating solution (insulating coating solution) should contain a total of 10 to 40% by mass of metal phosphate and colloidal silica. If the concentration is less than 10% by mass, the applied coating solution will tend to flow, causing uneven application. If the concentration is more than 40% by mass, the viscosity will be too high, causing uneven patterns and coating.
[0093] The metal phosphate may be one or a mixture of two or more selected from aluminum phosphate, zinc phosphate, magnesium phosphate, nickel phosphate, copper phosphate, lithium phosphate, cobalt phosphate, etc. Aluminum phosphate is preferred in terms of the stability of the coating liquid.
[0094] The coating liquid may contain additional elements such as vanadium, tungsten, molybdenum, zirconium, etc. When these elements are contained, they can be added to the coating liquid as, for example, an oxygen acid.
[0095] Colloidal silica can be of type S or type C. Type S colloidal silica refers to colloidal silica in which the silica solution is alkaline, while type C colloidal silica refers to silica particles whose surfaces are aluminum-treated, resulting in an alkaline to neutral silica solution. Type S colloidal silica is widely used and relatively inexpensive, but care must be taken as there is a risk of aggregation and precipitation when mixed with an acidic metal phosphate solution. Type C colloidal silica is stable even when mixed with a metal phosphate solution and there is no risk of precipitation, but it is relatively expensive due to the large number of processing steps required. It is preferable to use the appropriate type depending on the stability of the coating solution to be prepared.
[0096] [Magnetic Domain Refinement Step] The method for producing a grain-oriented electrical steel sheet according to this embodiment may further include a magnetic domain refinement step of refining magnetic domains on the steel sheet after the tension coating layer formation step. By performing the magnetic domain refinement treatment, it is possible to further reduce the iron loss of the grain-oriented electrical steel sheet.
[0097] Methods of magnetic domain subdivision include a method of narrowing the width of 180° magnetic domains (subdividing 180° magnetic domains) by forming linear or point-like grooves extending in a direction intersecting the rolling direction at predetermined intervals along the rolling direction, and a method of narrowing the width of 180° magnetic domains (subdividing 180° magnetic domains) by forming linear or point-like stress-strain portions or grooves extending in a direction intersecting the rolling direction at predetermined intervals along the rolling direction.
[0098] When forming stress-strained portions, laser beam irradiation, electron beam irradiation, etc. can be applied. When forming grooves, mechanical groove formation methods using gears, etc., chemical groove formation methods in which grooves are formed by electrolytic etching, and thermal groove formation methods using laser irradiation can be applied.
[0099] If the insulating coating is damaged by the formation of stress-strained portions or grooves, and the insulating properties and other characteristics are deteriorated, the insulating coating may be formed again to repair the damage.
[0100] A slab containing, in mass %, 0.08% C, 3.31% Si, 0.028% sol. Al, 0.008% N, 0.07% Mn, less than 0.0005% S, with the balance being Fe and impurities, was cast.
[0101] The slab was heated to 1350°C and then hot-rolled to form a hot-rolled sheet having a thickness of 2.2 mm, which was then annealed at 1100°C for 10 seconds.
[0102] Thereafter, the hot-rolled sheet was subjected to cold rolling to obtain a cold-rolled sheet having a thickness of 0.22 mm, which was then subjected to decarburization annealing by holding at 830°C for 90 seconds.
[0103] After decarburization annealing, MgO was added at 45 mass %, Al 2 O 3 50% by mass of bismuth chloride BiCl 3After drying, the steel sheet was subjected to finish annealing at 1200°C for 20 hours.
[0104] After the finish annealing, the steel sheet was rinsed with water to remove excess annealing separator, and no forsterite-based film was formed on the surface of the steel sheet. This steel sheet was then lightly pickled under the conditions shown in Tables 2A and 2B.
[0105] After light pickling, an intermediate layer was formed by electrolysis using a treatment solution (mixed treatment solution) containing a mixture of phosphate and additives under the conditions shown in Table 1. The drying temperature was 200°C. The obtained intermediate layer had the properties shown in Tables 2A and 2B. The proportion of crystalline metal phosphate in the intermediate layer was 80% by mass or more.
[0106] Thereafter, an insulating coating solution consisting of a metal phosphate and colloidal silica shown in Tables 2A and 2B was applied and dried at 850° C. for 30 seconds to form a tensile insulating coating on the surface of the steel sheet.
[0107] The thicknesses of the insulating coatings (intermediate layer and tensile coating layer) were as shown in Tables 2A and 2B. The tensile coating layer consisted essentially of metal phosphate and silica. The shape, average particle size, and thickness were measured as described above.
[0108]
[0109]
[0110]
[0111] The resulting steel sheet (grain-oriented electrical steel sheet) was subjected to magnetic domain refining treatment by irradiating it with a laser beam under conditions of UA (irradiation energy density) of 2.0 J and irradiation intervals of 5.0 mm pitch.
[0112] The iron loss W17 / 50 (iron loss at 50 Hz at 1.7 T) of the steel sheet after the magnetic domain refinement treatment was measured using a single sheet magnetic property measurement method (Single Sheet Tester: SST) in accordance with JIS C2556 (2015). If the iron loss W17 / 50 was 0.65 W / kg or less, it was determined that good magnetic properties were ensured. In addition, the space factor was measured as follows.
[0113] [Space Factor] The space factor was measured according to a method in accordance with JIS C 2550-5 (2020). Thirty test pieces, each 30 mm wide and 320 mm long, were used. After measuring the total mass of the sample, the distance between the upper and lower backing plates sandwiching the laminate was measured under a pressure of 1 MPa, and then calculated. If the space factor was 96.0% or higher, it was determined that a high space factor was ensured.
[0114] The steel sheets after the magnetic domain refining treatment were evaluated for coating adhesion, coating tension, corrosion resistance, elution resistance, and space factor by the following methods. The results are shown in Table 3.
[0115] [Coating Adhesion] Coating adhesion was evaluated by taking a sample 30 mm wide and 300 mm long from the steel sheet, subjecting this sample to stress relief annealing at 800°C for 2 hours in a nitrogen stream, and then winding it around a 10 mmφ cylinder and unwinding it to a bending adhesion test. The evaluation criteria were as follows, and a rating of ⊚ or ◯ was considered to indicate excellent coating adhesion.
[0116] ◎: Peeled area ratio 0-0.5% ○: Peeled area ratio over 0.5% and up to 5.0% △: Peeled area ratio over 5.0% and up to 20% ×: Peeled area ratio over 20% and up to 50% ××: Peeled area ratio over 50%
[0117] [Coating Tension] The coating tension was calculated by back-calculating from the state of curvature when one side of the insulating coating was peeled off. When the obtained coating tension was 4.0 MPa or more, it was determined that the coating tension was sufficient.
[0118] [Corrosion Resistance] Corrosion resistance was evaluated in accordance with the JIS salt spray test (JIS Z2371:2015), in which a 5% NaCl aqueous solution was allowed to fall naturally onto the sample for 7 hours in an atmosphere at 35°C. Thereafter, the rust area was evaluated on a 10-point scale. The evaluation criteria were as follows: A score of 5 or higher was considered to be excellent in corrosion resistance.
[0119] 10: No rust occurred 9: Very little rust occurred (area rate 0.10% or less) 8: Area rate where rust occurred = more than 0.10% but not more than 0.25% 7: Area rate where rust occurred = more than 0.25% but not more than 0.50% 6: Area rate where rust occurred = more than 0.50% but not more than 1.0% 5: Area rate where rust occurred = more than 1.0% but not more than 2.5% 4: Area rate where rust occurred = more than 2.5% but not more than 5.0% 3: Area rate where rust occurred = more than 5.0% but not more than 10% 2: Area rate where rust occurred = more than 10% but not more than 25% 1: Area rate where rust occurred = more than 25% but not more than 50%
[0120] [Elution Resistance] Elution resistance was evaluated based on whether or not the elution of phosphoric acid from the sample could be suppressed. The amount of elution was measured by boiling the sample in boiling pure water for 10 minutes, measuring the amount of phosphoric acid eluted in the pure water, and dividing the amount of phosphoric acid by the area of the insulating coating of the boiled grain-oriented electrical steel sheet. The amount of phosphoric acid eluted in the pure water was measured by cooling the pure water (solution) into which the phosphoric acid had eluted, and measuring the phosphoric acid concentration of the sample obtained by diluting the cooled solution with pure water using ICP-AES. When the elution amount was 40 mg / m 2 If the resistance is less than this, the resin is deemed to have excellent resistance to elution.
[0121]
[0122] As can be seen from Tables 1 to 3, the examples of the present invention were extremely excellent in the main properties of the coating, including adhesion, and had improved core loss and space factor. On the other hand, the comparative examples were inferior in one or more of the coating adhesion, coating tension, corrosion resistance, elution resistance, and space factor, because the insulating coating was formed using a method that did not meet the preferred conditions, and the intermediate layer did not contain the specified crystalline metal phosphate.
[0123] 100 Grain-oriented electrical steel sheet 1 Base steel sheet 2 Insulation coating 21 Intermediate layer 22 Tensile coating layer
[0124] According to the above aspect of the present invention, a grain-oriented electrical steel sheet can be obtained that has excellent adhesion of a tensile coating and magnetic properties, and that does not reduce the space factor of a transformer (core). Therefore, the grain-oriented electrical steel sheet obtained can be suitably used as an iron core material for transformers, and has high industrial applicability.
Claims
1. A grain-oriented electrical steel sheet comprising: a base steel sheet; and an insulating coating formed on the surface of the base steel sheet, wherein the insulating coating comprises: an intermediate layer formed on the base steel sheet side and containing a crystalline metal phosphate; and a tensile coating layer formed on the surface side of the insulating coating, wherein the crystalline metal phosphate is plate-shaped and has an average grain size of 0.5 to 3.0 μm.
2. The grain-oriented electrical steel sheet according to claim 1, wherein the crystalline metal phosphate in the intermediate layer comprises one or more of zinc phosphate, manganese phosphate, iron manganese phosphate, and zinc calcium phosphate.
3. The grain-oriented electrical steel sheet according to claim 1, characterized in that the thickness of the intermediate layer is 0.1 to 9.0 μm.
4. A method for forming the insulating coating of the grain-oriented electrical steel sheet according to claim 1, comprising the steps of: 2 O 3 a final annealing step of applying an annealing separator containing 10 to 100 mass % of the above-mentioned compound, drying the steel sheet, and then performing final annealing; an annealing separator removing step of removing excess annealing separator from the steel sheet after the final annealing step; a light pickling step of pickling the steel sheet after the annealing separator removing step with 0.1 to 10.0 mass % of one inorganic acid selected from sulfuric acid, chloric acid, nitric acid, and phosphoric acid at a liquid temperature of 20 to 90°C for 1 to 20 seconds; and a current density of 1.0 to 50 A / dm2 in a mixed treatment solution having a liquid temperature of 30 to 90°C, a metal ion concentration of 10 to 50 g / l, a phosphate ion concentration of 10 to 100 g / l, and a nitrate ion concentration of 20 to 80 g / l. 2 a drying step of pulling the steel sheet after the intermediate layer forming step out of the mixed treatment liquid, removing excess of the mixed treatment liquid, and then drying the steel sheet; and a tensile coating layer forming step of applying a coating liquid containing a metal phosphate and colloidal silica, the metal phosphate and the colloidal silica having a total concentration of 10 to 40 mass %, to the steel sheet after the drying step, drying the coating liquid, heating the steel sheet, and maintaining the sheet at a sheet temperature of 700 to 950° C. for 10 to 60 seconds.
Citation Information
Patent Citations
JP1973039338A
JP1974096920A
Formation of insulated film on grain-oriented silicon steel sheet
JP1994184762A
Formation of insulated film on silicon steel sheet
JP1999209891A
Application program, settlement system, and information processing method
JP2023064840A