Silicon nanopowder manufacturing apparatus and silicon nanopowder manufacturing method
The silicon nanopowder manufacturing device and method address the challenges of impurities and inefficiencies in conventional silicon production by using a controlled reactor and acid washing to produce high-purity, uniform nanoparticles, enhancing the performance and economic viability of silicon-based anode materials for lithium-ion batteries.
Patent Information
- Application Number
- PCT/KR2024/095572
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-12
- Filing Date
- 2024-03-15
- Publication Date
- 2024-10-17
AI Technical Summary
Conventional silicon manufacturing methods face challenges in producing high-purity, uniform nano-silicon particles of 100 nm or less due to impurities, low productivity, and economic inefficiencies, which affect the cycle performance and capacity maintenance of silicon-based anode materials in lithium-ion batteries.
A silicon nanopowder manufacturing device and method involving a cylindrical reactor with rotating and tilting capabilities, using a reducing agent like magnesium in a controlled inert atmosphere, and acid washing to produce high-purity silicon nanoparticles, enabling continuous reduction and upcycling of process by-products.
The method achieves high-purity silicon nanoparticles with uniform sizes, improving the cycle performance and capacity maintenance of silicon-based anode materials, enhancing the economic feasibility and industrial applicability of silicon nanopowder in energy storage systems.
Smart Images

Figure KR2024095572_17102024_PF_FP_ABST
Abstract
Description
Silicon nanopowder manufacturing device and silicon nanopowder manufacturing method
[0001] The present invention relates to a silicon nanopowder manufacturing device and a silicon nanopowder manufacturing method.
[0002] In lithium-ion secondary batteries, lithium-containing metal composite oxides, such as lithium-cobalt composite oxide, are primarily used as positive electrode active materials, while multilayered carbon materials are primarily used as negative electrode active materials. Recently, silicon or silicon oxide, which have higher capacities than carbon, have been discussed as negative electrode active materials.
[0003] To improve the cycling performance of silicon anodes, nano-silicon, alloying silicon with metals, and combining silicon with carbon materials can generally be used to enhance the volume expansion effect of the silicon material. Here, the synthesis of nano-silicon and its uniform dispersion in a graphite matrix are key technologies.
[0004] Silicon can be obtained from silica, or silicon dioxide (SiO2), which is one of the most common components on Earth. Research is constantly being conducted to convert and purify low-value silica into high-value silicon.
[0005] The background technology described above is something that the inventor possessed or acquired in the process of deriving the disclosure of the present application, and cannot necessarily be said to be a publicly known technology disclosed to the general public prior to the present application.
[0006] Conventional silicon manufacturing methods mostly extract silica, the raw material for silicon, from minerals or sand. However, impurities such as boron and phosphorus contained in these minerals or sand are difficult to remove through acid treatment processes, making it difficult to directly reduce and produce high-purity silicon. In addition, batch-type reduction processes have low productivity and economic feasibility, and it is difficult to obtain nano-silicon particles smaller than 100 nm. They are often non-uniform in size and contain a large number of impurities (e.g., unreacted substances). Furthermore, it is difficult to obtain nano-silicon particles smaller than approximately 100 nm during pulverization. When non-uniform silicon particles and the content of impurities are high, cracks may occur due to volume expansion during charge and discharge when applied to anode materials, and the capacity retention rate may decrease.
[0007] A method for collecting slurry, a byproduct of silicon wafer and ingot processing, and surface treating it with plasma and laser to produce nano-silicon particles has been proposed. While this method offers the potential for upcycling process byproducts, it suffers from low productivity and efficiency. A method for producing and supplying high-purity silicon by reacting a reducing metal with silica at high temperatures may be economically effective, but it carries the risk of oxidation of the reactants and explosion of unreacted products.
[0008] Accordingly, in order to solve the above-mentioned problem, the present invention provides, according to one embodiment, a silicon nanopowder manufacturing device capable of providing uniform and high-purity silicon nanoparticles (e.g., silicon nanoparticles having a size of about 100 nm or less) or upcycling process byproducts generated during the manufacturing and / or processing of silicon-related materials, parts and / or products, and a silicon nanopowder manufacturing method using the same.
[0009] According to one embodiment, the present invention can provide a silicon nanopowder manufacturing device capable of improving process stability and providing a large amount of high-purity silicon nanoparticles, and a silicon nanopowder manufacturing method using the same.
[0010] According to one embodiment, high-purity and nano-level silicon nanopowders that can be utilized in various industrial fields (e.g., materials for electrical energy storage systems and / or electrical power generation systems) can be provided.
[0011] However, the problems to be solved by the present invention are not limited to those mentioned above, and other problems not mentioned will be clearly understood by those skilled in the art from the description below.
[0012] According to one embodiment, a device (100) for manufacturing silicon nanopowder may include a supply unit (110, 120) for supplying silicon-containing raw materials and a reducing agent; a cylindrical reactor (130) for reacting the silicon-containing raw materials and the reducing agent at a reduction temperature; and a powder recovery unit (140) for recovering reduced silicon powder from the cylindrical reactor (130).
[0013] According to one embodiment, it may further include a first seal (S1) formed at the boundary between the supply (110, 120) and the cylindrical reactor (130).
[0014] According to one embodiment, it may further include a second seal (S2) formed at the boundary between the supply (110, 120) and the powder recovery unit (140).
[0015] According to one embodiment, the first seal (S1) and the second seal (S2) may be a double lip seal, a lip seal or a metal lip seal, respectively.
[0016] According to one embodiment, the cylindrical reactor (130) may be supported such that it can rotate, tilt, or both.
[0017] According to one embodiment, the supply device (110, 120) may further include a gas vaporizer (122) that vaporizes a metal reducing agent to supply reducing gas inside or outside the supply device (110, 120).
[0018] According to one embodiment, the device for manufacturing silicon nanopowder (100) may further include a washing machine (200) for acid washing the reduced silicon powder.
[0019] According to one embodiment, a method for manufacturing silicon nanopowder may include: a step of supplying a silicon-containing raw material and a reducing agent; a step of reacting the silicon-containing raw material and the reducing agent to perform continuous reduction; and a step of acid-washing the silicon-containing raw material that has undergone the reducing step.
[0020] According to one embodiment, the continuous reducing step includes an oxygen removal step; and a step of forming a normal pressure in an inert atmosphere; and may be a continuous reduction in a metal reducing atmosphere.
[0021] In one embodiment, the oxygen removal step comprises: 1x10 -1 A low-oxygen state is formed by forming an atmosphere of less than 1 Torr or a low vacuum atmosphere, or by introducing an inert gas to replace the atmosphere with an inert atmosphere, and the low-oxygen state may have an oxygen concentration of 1% or less.
[0022] According to one embodiment, the step of forming a pressure in an inert atmosphere may be to maintain the inert atmosphere by introducing an inert gas.
[0023] According to one embodiment, the inert gas may be at least one inert gas selected from the group consisting of Ar, He, and N2.
[0024] According to one embodiment, the method for manufacturing the silicon nanopowder may be performed using a silicon nanopowder manufacturing device according to embodiments of the present invention (e.g., device (100) of FIG. 1).
[0025] According to one embodiment, the continuous reducing step may be performed by stirring and reacting the silicon-containing raw material and the reducing agent through rotation of a screw blade and a rotating screw shaft inside a cylindrical reactor.
[0026] According to one embodiment, the metal reducing atmosphere may be formed from at least one reducing agent selected from the group consisting of magnesium, sodium, potassium, calcium, and aluminum.
[0027] According to one embodiment, the continuous reducing step may be performed at a reduction temperature of 600° C. to 1100° C. and in a vacuum; or an atmosphere including an inert gas, a metallic gas including a metal reducing agent, or both.
[0028] According to one embodiment, the silicon-containing raw material may include at least one selected from the group consisting of silicon, a hydrate containing silicon, an oxide containing silicon, and a chloride containing silicon.
[0029] According to one embodiment, a device and method for manufacturing silicon nanopowder can provide high-purity silicon nanopowder and a method for manufacturing the same that can be utilized in various industrial fields.
[0030] In addition, various effects may be provided, either directly or indirectly, through this document.
[0031] FIG. 1 is a schematic diagram illustrating the configuration of a reduction device of the present invention according to one embodiment.
[0032] FIG. 2 is a schematic diagram illustrating a reactor of a reduction device of the present invention according to one embodiment.
[0033] FIG. 3a, FIG. 3b, and FIG. 3c are images of nano silicon powder according to a process in Example 1 of the present invention, according to one embodiment. FIG. 3a is a raw material powder, FIG. 3b is a powder after a reduction reaction has been completed, and FIG. 3c is a dried silicon powder.
[0034] FIG. 4 is a drawing schematically illustrating the configuration of a cleaning device according to one embodiment of the present invention.
[0035] Hereinafter, embodiments of the present invention will be described in detail with reference to the attached drawings. In describing the present invention, detailed descriptions of related known functions or configurations will be omitted if it is determined that such detailed descriptions may unnecessarily obscure the gist of the present invention. In addition, the terms used in this specification are terms used to appropriately express preferred embodiments of the present invention, and may vary depending on the intention of the user or operator, or the customs of the field to which the present invention belongs. Therefore, the definitions of these terms should be determined based on the contents throughout this specification. The same reference numerals presented in each drawing represent the same elements.
[0036] Throughout the specification, when we say that an element is "on" another element, this includes not only cases where the element is in contact with the other element, but also cases where another element exists between the two elements.
[0037] Throughout the specification, when a part is said to "include" a component, this does not mean that it excludes other components, but rather that it may include other components.
[0038] Hereinafter, the silicon nanopowder manufacturing device and silicon nanopowder manufacturing method of the present invention will be described in detail with reference to examples and drawings. However, the present invention is not limited to these examples and drawings.
[0039] According to one embodiment, FIG. 1 is a schematic diagram of an apparatus (100) for manufacturing silica nanoparticles using a rotary kiln according to one embodiment. Referring to FIG. 1, the apparatus (100) for manufacturing silica nanoparticles according to one embodiment may include a supply device for supplying silicon-containing raw materials and a reducing agent (e.g., a silica-containing raw material supply device (110) and a reducing agent supply device (120)), a cylindrical reactor (130), a powder recovery unit (140), and a heater (150).
[0040] According to one embodiment, a first seal (S1) formed at the boundary between the feeder (e.g., the silica-containing raw material feeder (110) and the reducing agent feeder (120)) and the cylindrical reactor (130) may be further included. For example, the first seal (S1) may be included at the boundary between the silica-containing raw material feeder (110) and the cylindrical reactor (130), and the first seal (S1) may be included at the boundary between the reducing agent feeder (120) and the cylindrical reactor (130).
[0041] According to one embodiment, a second seal (S2) may be further formed at the boundary between the supply (e.g., silica-containing raw material supply (110) and reducing agent supply (120)) and the powder recovery unit (140). For example, the second seal (S2) may be included at the boundary between the reducing agent supply (120) and the powder recovery unit (140).
[0042] According to one embodiment, the sealing member applied to the first seal (S1) and the second seal (S2) may each include a double lip seal, a lip seal, or a metal lip seal.
[0043] According to one embodiment, the silica-containing raw material supplier (110) supplies the silica-containing raw material, and the silica-containing raw material can be applied without limitation as long as it is a raw material used for producing silicon nanopowder, and for example, the silicon-containing raw material can include at least one selected from silicon; and a hydrate (e.g., SiOxHx), an oxide (e.g., SiOx) (wherein x is a free water), and a halide (e.g., chloride, SiCl4, SiHCl3, Si2Cl6, SiH2Cl2, SiH3Cl SiCl2) containing silicon.
[0044] According to one embodiment, the present invention may further include a screw feeder (112) that is connected to a silica-containing raw material supply device (110) and supplies the silica-containing raw material by stirring it through the rotation of a screw blade and a rotating screw shaft provided therein.
[0045] According to one embodiment, the reducing agent supply unit (120) supplies a reducing agent. For example, the reducing agent may include at least one selected from the group consisting of magnesium, sodium, potassium, calcium, and aluminum, or a combination thereof. Preferably, the reducing agent may be magnesium.
[0046] According to one embodiment, the reducing agent supply device (120) may further include a gas vaporizer (122) that vaporizes the reducing agent and supplies reducing gas inside or outside the reducing agent supply device (120).
[0047] In one embodiment, the reducing agent may be provided in the form of a metal powder; a lump metal; or a reducing gas in which the metal powder or lump metal is vaporized.
[0048] According to one embodiment, the reactor (130) may further include a carrier gas line (162) capable of carrying the reducing gas to the cylindrical reactor (130); and a carrier gas supply unit (160) for supplying the carrier gas. For example, the reducing gas may be supplied into the reactor (130) through the carrier gas line (162).
[0049] According to one embodiment, the carrier gas may include at least one selected from the group consisting of inert gases such as argon (Ar), nitrogen (N2), and helium (He).
[0050] According to one embodiment, the cylindrical reactor (130) can be supplied with the silica-containing raw material and the reducing agent to perform a reaction at a reduction temperature. For example, the reduction temperature may be 600°C or higher; about 700°C or higher; about 800°C or higher; about 900°C or higher; about 1,000°C or higher; about 600°C to about 1,100°C; about 800°C to about 1,100°C; or about 900°C to about 1,100°C.
[0051] In one embodiment, the cylindrical reactor (130) may be supported to be capable of rotation, tilting, and both. In one embodiment, the tilting angle of the cylindrical reactor (130) may be about -10° to 10°, about -10° to 5°, about -10° to 0°, about -10° to -5°, about -5° to 10°, about 0° to about 10°, or about 5° to about 10° when the cylindrical reactor (130) and the reducing agent supply (120) are horizontal.
[0052] According to one embodiment, the cylindrical reactor (130) can rotate at a speed of about 0.1 rpm to about 100 rpm, about 1 rpm to about 80 rpm, about 1 rpm to about 60 rpm, about 10 rpm to about 40 rpm, about 10 rpm to about 20 rpm, about 40 rpm to about 100 rpm, about 60 rpm to about 100 rpm, or about 80 rpm to about 100 rpm to stir the reduction reactant, and by such rotation, the reduction process can proceed uniformly and the time of the reduction process can be reduced, thereby improving the efficiency of the manufacturing process of silicon nanopowder.
[0053] According to one embodiment, the reactivity of the silica-containing raw material and the reducing agent can be increased by the rotation and / or tilting angle inclination of the cylindrical reactor (130), thereby controlling the capacity and unreacted materials. For example, the function of the silicon nanopowder manufactured by rotating the cylindrical reactor (130) can be improved, and for example, an electrode having a capacity of about 3,000 mAh / g to about 4,000 mAh / g can be provided using the manufactured silicon nanopowder. This can realize a capacity that is about 30% to about 50% higher than that of the silicon nanopowder manufactured without rotation.
[0054] According to one embodiment, the silica-containing raw material and the reducing agent may be stirred and reacted by rotating the screw blades and the rotating screw shaft inside the cylindrical reactor (130).
[0055] FIG. 2 is a schematic diagram of a screw and a screw shaft inside a cylindrical reactor (130) according to one embodiment. Referring to FIG. 2, the cylindrical reactor (130) may include a rotating screw shaft (134) connected from one end to the other end of the cylindrical reactor (130) and a plurality of screw blades (132) provided along the circumference of the rotating screw shaft (134). The plurality of screw blades (132) may be provided spaced apart from each other, and the screw blades (132) may be provided in a form wound around the stirring shaft. The silicon-containing raw material and the reducing agent may be stirred and reacted by the rotation of the screw blades (132) and the rotating screw shaft (134).
[0056] According to one embodiment, the reactivity can be increased without unreacted substances of the silica-containing raw material and the reducing agent through a screw inside the cylindrical reactor (130). In addition, a continuous reduction process can be implemented.
[0057] According to one embodiment, the powder recovery unit (140) recovers reduced silicon powder from the cylindrical reactor. For example, the powder recovery unit (140) may be a glove box with a vacuum or inert gas atmosphere to prevent explosion of unreacted materials. That is, the powder can be recovered by removing air through vacuum and replacing it with an inert gas atmosphere.
[0058] According to one embodiment, the heater (150) is a heating means capable of maintaining the temperature of the cylindrical reactor (130) within a certain range. The heater (150) may raise the temperature of the interior of the cylindrical reactor (130) to a high temperature of room temperature or higher; about 600°C or higher; about 700°C or higher; about 800°C or higher; about 600°C to about 1,100°C; about 800°C to about 1,100°C; or about 900°C to about 1,100°C so that the silica-containing raw material and the reducing agent can react.
[0059] According to one embodiment, at least one of the silica-containing raw material feeder (110), the reducing agent feeder (120), the cylindrical reactor (130), and the powder recovery unit (140) may be configured with a vacuum atmosphere or an inert gas atmosphere. For example, the powder may be recovered by removing air by vacuum and replacing it with an inert atmosphere. For example, the inert atmosphere may be formed by injecting at least one gas selected from the group consisting of argon (Ar), nitrogen (N2), and helium (He). For example, by implementing a vacuum in the cylindrical reactor (130), oxygen can be removed before the reduction process, which can prevent safety accidents and minimize unreacted products.
[0060] According to one embodiment, a pump (170) for maintaining a vacuum atmosphere may be further included. For example, the pump may be configured to maintain a vacuum of about 1Υ10 -3 It may be a vacuum pump that can be adjusted to less than Torr.
[0061] According to one embodiment, the pump (170) can control the vacuum in at least one, two, or all of the silica-containing raw material feeder (110), the reducing agent feeder (120), the cylindrical reactor (130), and the powder recovery unit (140). For example, from atmospheric pressure to a vacuum of about 1Υ10 -3Torr or less. For example, the pump (170) can be connected to lines (L3 and L4) to control the internal vacuum of the powder recovery unit (140), the cylindrical reactor (130), or the like. For example, the internal vacuum of the cylindrical reactor (130) filled with raw materials and a reducing agent (or refilled with raw materials during operation) can be controlled. For example, the pump (170) can be connected to line (L5) to control the internal vacuum of the silica-containing raw material feeder (110), the reducing agent feeder (120), or both. For example, after filling the silica-containing raw material feeder (110) with raw materials (or refilling the raw materials during operation) and filling the reducing agent feeder (120) with reducing agent (or refilling the reducing agent during operation), a vacuum can be created in the silica-containing raw material feeder (110) and the reducing agent feeder (120). For example, a vacuum can be further applied to the line (L2) through which the reducing agent moves, the line (L1) through which the raw material moves, or a section corresponding to both.
[0062] According to one embodiment, valves (e.g., V1, V2, V3, V4) are further added to each line, which may be appropriately arranged for controlling the flow of gases, raw materials, and products; and maintaining or controlling a vacuum; etc. For example, the valve (V1) may separate the silicon-containing raw material and the reducing agent from each feeder (e.g., the silicon-containing raw material feeder (110) and the reducing agent feeder (120)) and supply them to the reactor (130), and stirring may be performed in the reactor (130) after the supply. For example, the valve (V1) may separate the atmosphere of the external region and the reactor (130) region when the silicon-containing raw material and the reducing agent are supplied (or recharged) into the reactor (130). For example, the atmospheric pressure of the supply lines (L1 and L2) and the reducing (e.g., Mg) atmosphere section inside the reactor (130) may be separated.
[0063] According to one embodiment, at least one of the silica-containing raw material feeder (110), the reducing agent feeder (120), the cylindrical reactor (130) and the powder recovery unit (140) is 1x10 -1 A low-oxygen state can be formed by forming an atmosphere of less than 1 Torr or a low vacuum atmosphere, or by introducing an inert gas to replace the atmosphere with an inert gas. For example, the low-oxygen state can be one in which the oxygen concentration is about 1% or less; about 0.8% or less; about 0.5% or less; or about 0.1% or less.
[0064] According to one embodiment, at least one of the silica-containing raw material feeder (110), the reducing agent feeder (120), the cylindrical reactor (130), and the powder recovery unit (140) forms a low-oxygen state for removing oxygen, forms a normal pressure in an inert atmosphere, and performs a continuous reduction process in a metal reducing atmosphere. For example, 1x10 -1 A low-oxygen state can be formed by forming an atmosphere of less than 1 Torr or a low vacuum atmosphere, or by introducing an inert gas to replace the atmosphere with an inert gas. The low-oxygen state may have an oxygen concentration of about 1% or less; about 0.8% or less; about 0.5% or less; or about 0.1% or less.
[0065] According to one embodiment, the device for manufacturing silicon nanopowder (100) may further include a washing machine (200) for acid washing the reduced silicon powder.
[0066] According to one embodiment of the present invention, the cleaning device (200) can be controlled under a vacuum and inert atmosphere when synthesizing silicon nanopowder, thereby suppressing the risk of explosion and fire of unreacted metal reduction substances. Furthermore, powder transfer and recovery are possible to prevent contact with air, thereby enhancing the reactivity of reactants and reducing the risk of fire and explosion. Furthermore, the capacity of silicon powder and unreacted substances can be controlled, enabling continuous mass production of high-purity silicon powder.
[0067] Fig. 4 schematically illustrates the configuration of a cleaner (200) according to one embodiment of the present invention. Referring to Fig. 4, the cleaner (200) according to one embodiment of the present invention includes a first deionized water bath (210), a first nozzle (220), a first stirring tank (230), a first dehydration tank (240), a first conveyor (250), and an acid solution recovery tank (260).
[0068] According to one embodiment, the deionized water bath (210) may supply deionized water. The deionized water may be purified by passing it through an ion exchanger three times for desalination, for example.
[0069] According to one embodiment, the first nozzle (220) may spray the deionized water. By spraying the deionized water, the silica or silicon raw material and the silica or silicon solid formed by the acid solution can be neutralized.
[0070] According to one embodiment, the first stirring tank (230) may be configured to leach silica or silicon solids by stirring the silica or silicon raw material and the acid solution by a motor (232).
[0071] According to one embodiment, the acid solution may be selected from the group consisting of hydrochloric acid, hydrofluoric acid, nitric acid, phosphoric acid, sulfuric acid, and hydrofluoric acid. Preferably, it may be hydrochloric acid.
[0072] According to one embodiment, the acid solution may be an aqueous solution having a concentration of about 1 N or more; about 3 N or more; or about 2 N to about 6 N (Normality, N), and acid washing is performed by stirring in the acid solution at a temperature of room temperature to about 100° C.; about 20° C. to about 80° C.; or about 20° C. to about 50° C., and when this temperature range is applied, washing of impurities is well performed, so that high-purity silicon nanoparticles can be obtained.
[0073] According to one embodiment, the first dehydration tank (240) may dehydrate moisture in the silica or silicon solid. By rotating the first dehydration tank (240), the silica or silicon solid can be dehydrated and separated into a dehydrated liquid, i.e., an acid solution, and the silica or silicon cake.
[0074] According to one embodiment, the first conveyor (250) may transport the silica or silicon cake.
[0075] According to one embodiment, the first conveyor (250) may include a transport belt for moving the silica or silicon cake; and a roller that contacts the transport belt and drives the transport belt in one direction.
[0076] According to one embodiment, the acid solution recovery tank (260) may recover the dehydrated liquid produced by the above-described dehydration, i.e., the acid solution.
[0077] According to one embodiment, the cleaner (200) may further include a first compressor (not shown) capable of forming the silica or silicon cake (270). The moisture in the silica or silicon cake may be dehydrated to the maximum extent possible by the first compressor, and the silica or silicon cake may be compressed.
[0078] According to one embodiment, a method for manufacturing a silicon nanopowder is provided. According to one embodiment, the method for manufacturing a silicon nanopowder may include the steps of: preparing a silicon-containing raw material; supplying a silicon-containing raw material and a reducing agent; reducing the silicon-containing raw material; and acid-washing the powder after the reducing step. According to one embodiment, the method for manufacturing a silicon nanopowder may utilize a silicon nanopowder manufacturing device according to embodiments of the present invention (e.g., the device (100) of FIG. 1).
[0079] According to one embodiment, the silicon-containing raw material corresponds to a raw material used in the production of the silicon nanopowder of the present invention, and for example, the silicon-containing raw material may include at least one selected from silicon; and silicon-containing hydrates (e.g., SiOxHx), oxides (e.g., SiOx), and halides (e.g., chlorides, SiCl4, SiHCl3, Si2Cl6, SiH2Cl2, SiH3Cl SiCl2).
[0080] According to one embodiment, the silicon-containing raw material corresponds to a raw material used in the production of the silicon nanopowder of the present invention, and the silicon-containing raw material can be obtained from a process byproduct. For example, the process byproduct can be upcycled into silicon nanoparticles. For example, the silicon-containing raw material can be obtained from a process byproduct generated during a SiC CVD coating process on a substrate.
[0081] According to one embodiment, the step of preparing the silicon-containing raw material may prepare a silicon-containing raw material in the form of fine particles. For example, a silicon-containing raw material having a particle size of about 100 nm or less may be prepared at the nanoscale.
[0082] In one embodiment, the step of preparing the silicon-containing raw material may include a step of acid-cleaning the silicon-containing raw material, wherein the acid-cleaning process removes impurities and obtains a silicon-containing raw material at the nanoscale. For example, the silicon-containing raw material may be collected as a process byproduct.
[0083] According to one embodiment, the step of preparing the silicon-containing raw material may include the steps of: crushing the silicon-containing raw material; and acid-cleaning the crushed silicon-containing raw material. Through these processes, high-purity and / or high-yield nanopowder particles can be obtained through a reduction process, thereby improving the process efficiency of the manufacturing method. For example, the silicon-containing raw material may be collected from a process byproduct.
[0084] According to one embodiment, the step of grinding the silicon-containing raw material may utilize a grinding method known in the technical field of the present invention, for example, milling (e.g., ball milling, attrition milling, and air jet milling), ultrasonic grinding, etc., but is not limited thereto.
[0085] According to one embodiment, the acid-cleaning step is a step of removing impurities by acid-cleaning after collecting the silicon-containing raw material or the pulverized silicon-containing raw material, and for example, an acid solution containing at least one of hydrochloric acid, nitric acid, acetic acid, and hydrofluoric acid, an acid gas, or both may be used. For example, the acid-cleaning step may be performed by removing oxygen in a vacuum and acid-cleaning under normal pressure using an inert atmosphere gas.
[0086] In one embodiment, the acid solution may be an aqueous acid solution having a concentration (e.g., mass %) of about 0.8% to about 8%. For example, an acid solution having a concentration level of about 3% to about 8% hydrochloric acid, about 0.6% to about 1.5% hydrofluoric acid, about 3% to about 8% nitric acid, or about 0.6% to about 2% acetic acid may be used. In one embodiment, the acid washing step is performed at a temperature of about 100° C. or lower; about room temperature (e.g., 20° C.) to about 100° C.; about room temperature to about 80° C.; about room temperature to about 60° C.; or about room temperature to about 50° C., and when applied in this temperature range, impurities are well washed away, so that uniform and high-purity silicon nanoparticles can be obtained.
[0087] According to one embodiment, the method may further include a step of drying the acid-washed silicon-containing raw material. The drying step may include dehydrating the acid-washed powder and drying it at a temperature of about 60° C. to about 120° C.; a temperature of about 70° C. to about 120° C.; or a temperature of about 80° C. to about 120° C. and for about 10 hours or more; about 12 hours or more; or about 20 hours or more. In addition, an oven, freeze drying, spray drying, or the like may be used. The drying may be performed in an air atmosphere, an inert gas atmosphere, or a vacuum atmosphere.
[0088] According to one embodiment, the method may further include a step of adding a heat dispersant to the silicon-containing raw material and mixing the same to form a silicon-containing raw material mixture. The silicon-containing raw material may be mixed with the heat dispersant to undergo a reduction reaction process. For example, the above-mentioned acid-cleaned silicon-containing raw material (or the raw material dried after acid cleaning) may be mixed with the heat dispersant. For example, the above-mentioned silicon-containing raw material (e.g., the raw material not subjected to the acid cleaning process) may be mixed with the heat dispersant.
[0089] According to one embodiment, the thermal dispersant is present in an amount of about 50 wt% to about 1000 wt%; about 50 wt% to about 500 wt%; about 50 wt% to about 200 wt%; about 50 wt% to about 100 wt%; or about 50 wt% to about 80 wt% based on the total weight of the silicon-containing raw material mixture, and when included within the above range, heat dispersing between silicon-containing raw materials is well achieved in the thermal reduction process described below, so that a uniform reduction reaction can proceed and a silicon nanopowder having high purity and / or functionality can be provided.
[0090] According to one embodiment, the heat dispersant may be an alkaline substance, and may include at least one selected from the group consisting of NaOH, KOH, LiOH, RbOH, CsOH K2CO3, Ca(OH)2, and NaHCO3. For example, the heat dispersant may be added in the form of a solution, powder, or both of the alkaline substance.
[0091] According to one embodiment, the step of drying the silicon-containing raw material mixture mixed with the heat dispersing agent may further be included. The drying step may be performed at a temperature of about 60° C. to about 120° C.; a temperature of about 70° C. to about 120° C.; or a temperature of about 80° C. to about 120° C. and for about 10 hours or more; about 12 hours or more; or about 20 hours or more. In addition, an oven, freeze drying, spray drying, or the like may be used. The drying may be performed in an air atmosphere, an inert gas atmosphere, or a vacuum atmosphere.
[0092] According to one embodiment, the step of supplying the silicon-containing raw material and the reducing agent is to supply the silicon-containing raw material and the reducing agent obtained in the step of preparing the silicon-containing raw material to the reactor. According to one embodiment, the silicon-containing raw material and the reducing agent can be supplied to the cylindrical reactor (130) through a supply device (110, 120) of the device for manufacturing silicon nanopowder.
[0093] According to one embodiment, the step of reducing the silicon-containing raw material is to reduce the silicon-containing raw material by applying a metal reducing agent, for example, the silicon-containing raw material may be reduced using at least one selected from the group consisting of metal powder, lump metal, and metallic gas containing the metal reducing agent.
[0094] According to one embodiment, the metal reducing agent may include at least one selected from the group consisting of magnesium, sodium, potassium, calcium, and aluminum. The metallic gas containing the metal reducing agent may be formed by vaporizing a metal powder and / or lump metal containing the metal reducing agent.
[0095] In one embodiment, the metallic gas may be supplied alone or mixed with a carrier gas, an inert gas, or both, to form a metallic gas atmosphere of about 1% or more; about 30% or more; about 50% or more; or about 90% to about 100%.
[0096] According to one embodiment, the reducing step may be performed at a reduction temperature of about 600° C. to 1100° C., and in a vacuum; or in an atmosphere including an inert gas, a Mg gas containing a metal reducing agent, or both. For example, the reduction reaction rate may be increased in a vacuum atmosphere. For example, the reducing step may be performed at a temperature of about 600° C. or higher; about 700° C. or higher; about 800° C. or higher; about 600° C. to about 1200° C.; about 700° C. to about 1100° C.; about 800° C. to about 1100° C.; about 600° C. to about 1100° C.; or about 900° C. to about 1100° C. and for about 1 minute or longer; about 10 minutes or longer; about 30 minutes or longer; about 1 hour or longer; about 5 hours or longer. Alternatively, it may proceed by thermal reduction for about 3 to about 6 hours.
[0097] According to one embodiment, the reducing step may be performed by heating the silicon-containing raw material while mixing the metallic powder containing the metal reducing agent with the silicon-containing raw material, or by heating the silicon-containing raw material in an atmosphere containing a metallic gas containing the metal reducing agent. For example, continuous reduction may be performed in a metal reducing atmosphere.
[0098] According to one embodiment, the method for manufacturing the silicon nanopowder (e.g., the reducing step) may use a reducing device, for example, a rotary kiln (e.g., the device (100) of FIG. 1). According to one embodiment, the rotary kiln may include a feeder (110) for supplying a silica-containing raw material and a reducing agent; a cylindrical reactor (130) for supplying the silica-containing raw material and the reducing agent and reacting them at a reducing temperature; a powder recovery unit (140) for recovering the reduced silicon powder from the cylindrical reactor (130); a heater (150) for heating the cylindrical reactor; a carrier gas supply unit (160); and a pump (170), the respective components and functions of which may be found in the description of the device (100) of FIG. 1 mentioned above.
[0099] According to one embodiment, the method for manufacturing the silicon nanopowder may employ a step of continuously reducing the silicon-containing raw material and the reducing agent by reacting them using a rotary kiln (e.g., device (100) of FIG. 1). For example, the step of continuously reducing may include an oxygen removal step; and a step of forming a normal pressure in an inert atmosphere; and may be a step of continuously reducing in a metal reducing atmosphere.
[0100] For example, the above continuous reducing step may be performed at a reduction temperature of about 600°C to about 1100°C and in a vacuum; or in an atmosphere containing an inert gas, a metallic gas containing a metal reducing agent, or both.
[0101] For example, the metal reducing atmosphere may be formed from at least one reducing agent selected from the group consisting of magnesium, sodium, potassium, calcium, and aluminum.
[0102] For example, the silicon-containing raw material and the reducing agent may be stirred and reacted by rotating the screw blades and the rotating screw shaft (e.g., FIG. 2) inside the cylindrical reactor (130).
[0103] In one embodiment, the oxygen removal step comprises about 1x10 -1 A low-oxygen state is formed by forming an atmosphere of less than 1 Torr or a low vacuum atmosphere, or by introducing an inert gas to replace the atmosphere with an inert gas, and the low-oxygen state may have an oxygen concentration of about 1% or less; about 0.8% or less; about 0.5% or less; or about 0.1% or less.
[0104] According to one embodiment, the step of forming a normal pressure in the inert atmosphere may include maintaining the inert atmosphere by introducing an inert gas. For example, the inert gas may be at least one inert gas selected from the group consisting of argon (Ar), nitrogen (N2), and helium (He).
[0105] According to one embodiment, a rotary kiln (e.g., device (100) of FIG. 1) can transfer and recover powder to prevent contact with air, thereby increasing the reactivity of reactants (e.g., reduction reaction rate) and reducing the risk of fire and explosion. In addition, the capacity and unreacted matter of silicon powder can be controlled, and high-purity silicon powder can be continuously mass-produced. In addition, the particle size can be maintained uniformly and high-purity silica nanoparticles can be provided.
[0106] According to one embodiment of the present invention, the acid washing step is a step of removing impurities by acid washing after collecting the silicon-containing raw material that has gone through the reduction process, and for example, an acid solution containing at least one of hydrochloric acid, nitric acid, acetic acid, and hydrofluoric acid, an acid gas, or both may be used. For example, the acid washing step may implement a vacuum to increase the impurity washing ability. For example, the acid washing step may utilize the washing machine (200) of FIG. 4.
[0107] According to one embodiment, the method may include a step of grinding the silicon-containing raw material that has undergone the reduction process, before and / or after acid washing. This grinding may be performed using any grinding method known in the art, including, but not limited to, milling (e.g., ball milling, attrition milling, and air jet milling), ultrasonic grinding, and the like.
[0108] According to one embodiment, the acid washing step may be performed one or more times; or two or more times. When performed two or more times, the acid washing may be performed under the same or different conditions. For example, at least one of the acid type, acid solution, acid gas, and temperature may be different.
[0109] In one embodiment, the acid solution may be an aqueous acid solution having a concentration (e.g., mass %) of about 0.8% to about 8%. For example, an acid solution having a concentration level of about 3% to about 8% hydrochloric acid, about 0.6% to about 1.5% hydrofluoric acid, about 3% to about 8% nitric acid, or about 0.6% to about 2% acetic acid may be used. In one embodiment, the acid washing step is performed at a temperature of about 100° C. or lower; about room temperature (e.g., 20° C.) to about 100° C.; about room temperature to about 80° C.; about room temperature to about 60° C.; or about room temperature to about 50° C., and when this temperature range is applied, impurities are well washed away, so that uniform and high-purity silicon nanoparticles can be obtained.
[0110] According to one embodiment, the acid-washing step may further include a drying step, wherein the drying step may dehydrate the acid-washed powder and dry it at a temperature of about 60° C. to about 120° C.; a temperature of about 70° C. to about 120° C.; or a temperature of about 80° C. to about 120° C. and for about 10 hours or more; about 12 hours or more; or about 20 hours or more. In addition, an oven, freeze drying, spray drying, or the like may be used. The drying may be performed in an air atmosphere, an inert gas atmosphere, or a vacuum atmosphere.
[0111] According to one embodiment, the method comprises the steps of collecting the silicon-containing raw material that has undergone the reduction process; acid washing; dehydrating; and drying, and may further comprise a crushing step after at least one of the above-mentioned steps. For example, the method may further comprise a crushing step after at least one of the collecting step and the drying step.
[0112] According to one embodiment, the method comprises the steps of collecting a silicon-containing raw material that has undergone the reduction process; a first acid washing step; a dehydration step; a second acid washing step and a drying step, and may further comprise a second drying step after the dehydration step. The method may further comprise a pulverizing step after at least one of the above-mentioned steps. For example, the method may further comprise a pulverizing step after at least one of the collecting step and the drying step.
[0113] According to one embodiment, the present invention provides a method for producing silica nanopowder and a device for producing silica nanopowder (FIGS. 1 to 2) (e.g., a rotary kiln of FIG. 1) (e.g., a cylindrical reactor (130)), by performing a reduction process for reducing a silica-containing raw material and a reducing agent, thereby obtaining high-purity silicon powder (e.g., a purity of about 99.99% or more). In addition, high-purity silicon nanopowder having a uniform size of 100 nm or less can be provided. According to one embodiment, high-purity silicon nanopowder having a uniform size of 100 nm or less can be provided in the reducing step and the rotary kiln (e.g., the cylindrical reactor (130) of FIG. 1).
[0114] According to one embodiment, the rotary kiln (e.g., the cylindrical reactor (130) of FIG. 1) can implement a continuous reduction process in which the injection of the silicon-containing raw material and the reduction process of the silicon-containing raw material are continuously performed. In addition, powder transfer and recovery to prevent contact with air are possible, so that the reactivity of the reactants can be increased and the risk of fire and explosion can be reduced. By implementing such a continuous reduction process, the capacity and unreacted matter of the silicon nanopowder can be controlled, and high-purity silicon powder can be continuously mass-produced. In addition, the economic feasibility of the production of silicon nanopowder can be increased. In addition, the rotary kiln (e.g., the cylindrical reactor (130) of FIG. 1) can prevent safety accidents and minimize unreacted matter by removing oxygen before reduction by implementing a vacuum, and can improve the reductive property in the reduction reaction.
[0115] According to one embodiment, the silicon nanopowder may include a particle size of about 100 nm or less; about 90 nm or less; about 50 nm or less; about 20 nm or less; about 10 nm or less; or about 1 nm or more; about 10 nm or more; about 30 nm or more; from about 1 nm to about 80 nm; or from about 10 nm to about 60 nm. When the particle size is within the above range, the silicon nanopowder has a high possibility of being used as a material for a product requiring high-purity nanopowder characteristics, and can enhance the industrial value of the high-purity nanopowder. For example, a uniform silicon nanopowder having a particle size of about 100 nm or less can be used as a lithium secondary battery component or a material (e.g., a negative electrode material) of a lithium secondary battery that can suppress cracking during charge and discharge and achieve high capacity retention.
[0116] According to one embodiment, the particle size of the silicon nanopowder may be an average particle size that can be obtained by measuring with XRD, SEM, TEM, BET or dynamic light scattering, and for example, the particle size of the silicon nanopowder calculated using the half width in the XRD pattern may be an average crystal size of about 20 nm to about 60 nm, calculated from the XRD Scherre equation of Equation 1 below.
[0117]
[0118] According to one embodiment, the nano-silicon powder may be utilized as an electrode material of a lithium secondary battery (e.g., a lithium ion battery). For example, it may be applied as an anode material (e.g., an anode) of the lithium ion battery. More specifically, it may be an anode of a lithium ion battery manufactured with a composition for a secondary battery electrode (e.g., a lithium ion battery) including the silicon nanopowder, a binder, and a conductive material, and a lithium ion battery including the anode, a cathode, and a separator may be provided. The anode and the lithium ion battery may further include a configuration known in the art for driving and operating the present invention, which is not specifically mentioned in this document.
[0119] In one embodiment, the silicon nanopowder can be manufactured from various raw materials, and in one embodiment, the silicon nanopowder can be manufactured from a silicon-containing raw material including at least one selected from the group consisting of silicon; and silicon-containing hydrates (e.g., SiOxHx), oxides (e.g., SiOx), and halides (e.g., chlorides, SiCl4, SiHCl3, Si2Cl6, SiH2Cl2, SiH3Cl SiCl2).
[0120] According to one embodiment, the silicon nanopowder may be manufactured from a silicon-containing raw material, such as a process byproduct (e.g., an undeposited silicon-containing byproduct from a CVD deposition or coating process) generated during the manufacture of a material, component, or substrate containing silicon (e.g., ingot manufacturing, synthesis, crystal growth, deposition, coating).
[0121] Hereinafter, the present invention will be described in more detail through examples, but the following examples are for the purpose of explanation only and are not intended to limit the scope of the present invention.
[0122] Example 1
[0123] (1) Synthesis of silicon nanopowder
[0124] Byproducts or silicon-containing raw materials generated during CVD SiC were collected and pulverized. Next, the pulverized material was added to a 0.8% to 8% aqueous solution (hydrochloric acid or nitric acid: acid type) and stirred to remove impurities, thereby obtaining silicon-containing raw material powder. The powder was dried at a temperature of 60°C to 120°C for 12 hours to prepare silicon-containing raw material powder (Fig. 3a). The silicon-containing raw material powder was confirmed to have an average particle size of 40 nm to 60 nm by measuring SEM images.
[0125] These were placed in the silicon-containing raw material inlet of the reactor shown in Fig. 1, and the inside of the reactor was formed with an atmosphere of Mg vapor (atmosphere forming and inert gas at a weight ratio of 90% to 150%).
[0126] The above silicon-containing raw material was introduced into the reactor, heated to a temperature of 600°C to 1200°C, and a reduction reaction was performed for 1 to 6 hours while rotating the screw at a speed of 0.1 to 100 rpm. The powder (Fig. 3b) for which the reduction reaction was completed was collected and immersed in a 3% to 8% hydrochloric acid aqueous solution to perform a primary acid etching, and then a 0.6% to 1.5% hydrofluoric acid aqueous solution was poured to perform a secondary acid washing. The powder was washed several times with distilled water and dried at a temperature of 60°C to 120°C for 12 hours to obtain a silicon powder (Fig. 3c).
[0127] The X-ray diffraction (XRD) pattern, scanning electron microscope (SEM) image, and BET surface area of the dried silicon powder were measured. In addition, the content of impurities was confirmed using an elemental analyzer. The results are shown in Table 1.
[0128] The XRD pattern of the silicon particle crystal was confirmed, and using the SEM image, it was confirmed that the silicon particles had an average particle size of less than 100 nm. The crystal size of the silicon particles was calculated using the XRD Scherre equation from the XRD pattern, and the result was approximately 20 nm to 100 nm.
[0129] The BET specific surface area was calculated by obtaining the nitrogen gas adsorption amount at liquid nitrogen temperature (77 K), and the BET specific surface area was approximately 125 m 2 / g was confirmed. In addition, impurities were analyzed using ICP-MS (inductively coupled plasma mass spectrometry).
[0130]
[0131] In Table 1, high-purity nano-silica powder particles of about 99.5% or more can be confirmed. According to one embodiment, the manufacturing apparatus and manufacturing method of silicon nanopowder can manufacture small and uniform high-purity silicon nanoparticles of 100 nm or less by implementing a continuous reduction process. That is, the silicon nanoparticles can be utilized as an anode material that can solve the problem of cracking during charge and discharge caused by existing non-uniform or high-impurity silicon particle anode materials, and improve the capacity retention rate (e.g., implementing a capacity retention rate of 85% or more of initial efficiency in a secondary battery).
[0132] According to one embodiment, the device and method for manufacturing silicon nanopowder can increase economic efficiency (e.g., productivity) through a continuous reduction process and implement a vacuum for increasing reducibility (e.g., increasing reduction reaction rate).
[0133] According to one embodiment, a device and method for manufacturing silicon nanopowder can provide high-purity silicon nanopowder and a method for manufacturing the same that can be utilized in various industrial fields. For example, the silicon nanopowder can exhibit electrochemical properties or structural stability that can be utilized as a material for electrical energy storage systems and / or electrical power generation systems (e.g., secondary batteries, solar cells).
[0134] According to one embodiment, a device and method for manufacturing silicon nanopowder can upcycle process byproducts generated during the production and / or synthesis of silicon-related materials, parts and / or products, and realize efficiency and economy in the production process of silicon nanoparticles.
[0135] According to one embodiment, a manufacturing device and manufacturing method of silicon nanopowder can provide high-purity silicon nanopowder having a uniform particle size by upcycling process byproducts generated during the production and / or synthesis of silicon-related materials, parts and / or products, and can use the same to provide a lithium secondary battery or lithium secondary battery material (e.g., anode material) with improved performance and stability.
[0136] The present invention can manufacture high-purity silica nanopowder by upcycling process byproducts, which can achieve economic benefits through resource recycling and reuse in the supply and manufacture of silicon-containing raw materials and silicon nanopowder.
[0137] Although the embodiments have been described above with reference to limited examples and drawings, those skilled in the art will appreciate that various modifications and variations can be made based on the above teachings. For example, in this document, phrases such as "A or B," "at least one of A and B," "at least one of A or B," "A, B, or C," "at least one of A, B, and C," and "at least one of A, B, or C" can each include any one of the items listed together with the corresponding phrase, or all possible combinations thereof. For example, suitable results can be achieved even if the described techniques are performed in a different order than described, and / or the described components are combined or combined in a different form than described, or are replaced or substituted by other components or equivalents. Therefore, other implementations, other embodiments, and equivalents of the claims also fall within the scope of the claims described below.
Claims
1. A supply device that supplies silicon-containing raw materials and reducing agent; A cylindrical reactor for reacting the silicon-containing raw material and the reducing agent at a reducing temperature; and A powder recovery unit for recovering reduced silicon powder from the cylindrical reactor; including, A device for manufacturing silicon nanopowder.
2. In paragraph 1, Further comprising a first seal formed at the boundary of the above feeder and the above cylindrical reactor, A device for manufacturing silicon nanopowder.
3. In paragraph 1, It further includes a second seal formed at the boundary between the supply device and the powder recovery device. A device for manufacturing silicon nanopowder.
4. In paragraph 2 or 3, The first seal and the second seal are, respectively, a double lip seal, a lip seal or a metal lip seal. A device for manufacturing silicon nanopowder.
5. In paragraph 1, The above cylindrical reactor is supported to be capable of rotation, tilting and both. A device for manufacturing silicon nanopowder.
6. In paragraph 1, A gas vaporizer that supplies reducing gas by vaporizing a metal reducing agent inside or outside the above-mentioned supply device; which further includes, A device for manufacturing silicon nanopowder.
7. In paragraph 1, Further comprising a washing machine for acid washing the reduced silicon powder; A device for manufacturing silicon nanopowder.
8. Step of supplying silicon-containing raw materials and reducing agent; A step of continuously reducing by reacting the silicon-containing raw material and the reducing agent; and A step of acid-washing the silicon-containing raw material that has undergone the above-mentioned reducing step; including, Method for producing silicon nanopowder.
9. In paragraph 8, The above continuous reduction step is: Oxygen removal step; and comprising a step of forming a normal pressure in an inert atmosphere; It is a continuous reduction in a metal reducing atmosphere, Method for producing silicon nanopowder.
10. In paragraph 9, The above oxygen removal step is, 1x10 -1 By forming an atmosphere below 10 Torr or a low vacuum atmosphere, a low-oxygen state is formed, or It is to form a low-oxygen state by introducing an inert gas and replacing it with an inert atmosphere. The above hypoxic condition is one in which the oxygen concentration is less than 1%. Method for producing silicon nanopowder.
11. In paragraph 9, The step of forming atmospheric pressure in the above inert atmosphere is: Maintaining an inert atmosphere by introducing an inert gas, Method for producing silicon nanopowder.
12. In paragraph 10 or 11, The above inert gas is, At least one inert gas selected from the group consisting of Ar, He and N2, Method for producing silicon nanopowder.
13. In paragraph 8, The method for manufacturing the above silicon nanopowder is performed using a silicon nanopowder manufacturing device according to one of claims 1 to 7. Method for producing silicon nanopowder.
14. In paragraph 11, The silicon-containing raw material and the reducing agent are stirred and reacted by rotating the screw blade and the rotating screw shaft inside the cylindrical reactor. Method for producing silicon nanopowder.
15. In paragraph 9, The above metal reducing atmosphere is, Formed from at least one reducing agent selected from the group consisting of magnesium, sodium, potassium, calcium and aluminum, Method for producing silicon nanopowder.
16. In paragraph 8, The above continuous reduction step is, Reduction at a reduction temperature of 600°C to 1100°C and in a vacuum; or in an atmosphere containing an inert gas, a metallic gas containing a metal reducing agent, or both; Method for producing silicon nanopowder.
17. In paragraph 8, The above silicon-containing raw material comprises at least one selected from the group consisting of silicon, silicon-containing hydrate, silicon-containing oxide, and silicon-containing chloride. Method for producing silicon nanopowder.
Citation Information
Patent Citations
Anode material for lithium-ion secondary batteries containing nano-sized particles, anode for lithium-ion secondary batteries, lithium-ion secondary battery
JP5598836B2
Safety barrier for modular
KR1020240151449A
Process for the production of silicon-carbon composite materials
WO2022248347A1
Process for manufacturing silicon-containing materials in a cascade reactor system
WO2023006209A1