High-efficiency hemostatic material, and preparation method therefor and use thereof
The microgel modified with phthalaldehyde groups solves the problems of insufficient tissue adhesion and mechanical properties of existing hemostatic materials, achieving rapid and effective hemostasis, and is suitable for various hemostasis scenarios.
Patent Information
- Application Number
- PCT/CN2023/142857
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-17
- Filing Date
- 2023-12-28
- Publication Date
- 2024-10-24
AI Technical Summary
Existing hemostatic materials are inadequate in terms of tissue adhesion and mechanical properties after fluid absorption, and are particularly effective in dealing with active or pressure bleeding, making it difficult to achieve rapid and effective hemostasis.
Microgels modified with phthalaldehyde groups are covalently linked to water-soluble or hydrophilic polymers to form highly efficient hemostatic materials, including hemostatic sponges, hemostatic powders, and flowable hemostatic agents. The phthalaldehyde groups rapidly couple with free amine groups in the blood to form a second cross-linked network, enhancing mechanical properties and improving adhesion strength by chemically bonding with amine groups on the tissue surface.
It achieves rapid and effective hemostasis in various hemostasis scenarios, and is particularly suitable for irregular surfaces, active or pressure bleeding, and minimally invasive surgery. It has excellent tissue adhesion properties and mechanical strength, and hemostasis can be achieved without additional pressure.
Smart Images

Figure CN2023142857_24102024_PF_FP_ABST
Abstract
Description
High-efficiency hemostatic material and its preparation method and application Technical Field
[0001] The present invention belongs to the field of new medical materials technology, and in particular relates to a high-efficiency hemostatic material and its preparation method and application. Technical Background
[0002] Uncontrollable bleeding is one of the main causes of death after trauma, during surgery and in emergency situations. Timely and effective hemostasis can greatly reduce mortality and the risk of complications. Therefore, the development of hemostatic materials has attracted much attention.
[0003] Early hemostasis is mainly achieved by applying pressure with the aid of cotton gauze. However, cotton gauze has a long hemostatic time and is non-degradable, so its application is limited. In recent years, new hemostatic materials have been developed, mainly inorganic and hydrophilic polymer hemostatic materials. Inorganic hemostatic materials mainly include zeolite, clay, and kaolin. These materials have strong water absorption capacity and good hemostatic effect. However, because they are difficult to absorb into the body and may generate heat and cause damage to surrounding tissues while stopping bleeding, they are only used in emergency situations such as pre-hospital bleeding control in combat trauma settings. Hydrophilic polymer hemostatic materials refer to hydrophilic natural or synthetic polymers that are directly or cross-linked and processed into materials such as sponges, powders, hydrogels, films, or gauze. These materials have excellent biocompatibility, adjustable degradation, and strong water absorption properties. They can quickly absorb water from the blood to concentrate blood components such as blood cells and coagulation factors. They can also promote the adhesion, aggregation, and activation of platelets, thereby accelerating the formation of blood clots and achieving a hemostatic effect. However, current polymer hemostatic materials generally have defects such as inability to adhere to tissues and weak mechanical properties after fluid absorption, resulting in limited hemostatic effects, especially in the treatment scenarios of active or pressure bleeding.
[0004] In response to the above problems, researchers are committed to modifying and modifying hemostatic materials to improve the hemostatic effect. For example, the Celox hemostatic gauze developed by MedTrade has chitosan particles impregnated on the gauze surface. The positive charge on chitosan increases the adhesion and aggregation of blood cells and platelets through electrostatic action, further enhancing the hemostatic effect. Johnson & Johnson has developed Surgicel, an oxidized cellulose gauze. The carboxyl groups on the cellulose can acidify the blood to form a gel, which can also further enhance the hemostatic effect. The above strategies increase the interaction between the hemostatic material and the blood components and tissue surface by introducing cations or anions into the hemostatic material. However, this interaction comes from weak physical interactions and still cannot solve the problem of blocking active or pressure bleeding. When stopping bleeding, the gauze needs to be continuously pressed on the bleeding area, which is difficult to apply to bleeding wounds with irregular shapes and cannot be pressed. In order to further improve the tissue adhesion strength of hemostatic materials and the mechanical properties after absorbing blood, some researchers have modified chitosan hemostatic materials with catechol, using highly active catechol to quickly cross-link a large amount of plasma proteins to form a second cross-linked network with the hemostatic material. At the same time, catechol bonds to tissue surface groups to form a hemostatic barrier with a certain mechanical strength within a few seconds (K. Kim et al., Coagulopathy-independent, bioinspired hemostatic materials: A full research story from preclinical models to a human clinical trial. Sci. Adv. 2021); some researchers have also used carboxylic acid activated esters modified on polyacrylic acid to react with plasma proteins and amino groups on the tissue surface to form a hemostatic material and blood clot complex with a certain strength at the bleeding site, which covalently adheres to the tissue while quickly stopping bleeding, thereby achieving effective blocking of the bleeding point (H. Yuk et al., Rapid and coagulation-independent heemostatic sealing by a paste inspired by barnacle glue. Nat. Biomed. Eng. 2021). However, the oxidizability of the catechol group, the pH dependence of its tissue adhesion properties, and the nonspecific binding to proteins all pose challenges to its hemostatic application. Furthermore, defects such as the generation of byproducts during use and low cross-linking efficiency at low concentrations of activated carboxylic acid esters also limit their biomedical applications. Therefore, there is an urgent need to find an ideal (i.e., stable, efficient, rapid, and highly selective) bioactive reactive group to construct hemostatic materials with excellent tissue adhesion and mechanical properties to address various hemostatic scenarios and achieve rapid and safe hemostasis.
[0005] Summary of the Invention
[0006] In response to the defects of current hemostatic materials, namely weak tissue adhesion and poor mechanical properties after absorbing blood, the present invention proposes a series of high-efficiency hemostatic materials and their preparation methods and applications.
[0007] The purpose of the present invention can be achieved by the following technical solutions:
[0008] The first aspect of the present invention provides a type of microgel modified with o-phthalaldehyde groups.
[0009] The structure of the o-phthalaldehyde group-modified microgel is shown in Formula 1:
[0010] In Formula 1, MG represents microgel, which is a gel microparticle formed by cross-linking water-soluble or hydrophilic polymers, with a particle size of 5 mesh to 1000 mesh and a solid content of 0.01% to 50%;
[0011] In formula 1, n ≥ 2, which means that the average number of o-phthalaldehyde functional groups on a single microgel is greater than or equal to 2;
[0012] In Formula 1, the o-phthalaldehyde group and the microgel are connected via a covalent bond.
[0013] The water-soluble or hydrophilic polymer of the microgel is selected from natural polymers or synthetic polymers.
[0014] The water-soluble or hydrophilic natural polymer is selected from one or more of hyaluronic acid, alginic acid, dextran, chondroitin sulfate, heparin, polyglutamic acid, tragacanth gum, xanthan gum, agarose, gellan gum, guar gum, gum arabic, locust bean gum, starch, starch hydrolyzate or starch derivative, cellulose or cellulose derivative.
[0015] Wherein, the starch derivative can be selected from oxidized starch, esterified starch, etherified starch or alkylated starch;
[0016] The cellulose derivative may be selected from cellulose ethers, including but not limited to methyl cellulose, carboxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, hydroxypropyl methyl cellulose, and the like.
[0017] The water-soluble or hydrophilic synthetic polymer refers to an artificially synthesized polymer containing a large number of hydrophilic groups.
[0018] The hydrophilic groups include, but are not limited to, cationic groups (such as tertiary amines, quaternary amines, etc.), anionic groups (such as carboxylic acids, sulfonic acids, phosphoric acids and sulfuric acids, etc.) and polar nonionic groups (such as hydroxyl groups, ether groups, etc.).
[0019] In some embodiments of the present invention, the water-soluble or hydrophilic synthetic polymer can be selected from homopolymers or copolymers of (meth)acrylic acid and its esters containing the above-mentioned hydrophilic groups, homopolymers or copolymers of (meth)acrylamides, homopolymers or copolymers of polyvinyl alcohol, homopolymers or copolymers of polyethylene glycol, and homopolymers or copolymers of vinyl pyrrolidone.
[0020] Optionally, the homopolymer or copolymer of (meth)acrylic acid and its esters is selected from the group consisting of homopolymer or copolymer of (meth)acrylic acid, homopolymer or copolymer of hydroxyethyl (meth)acrylate, homopolymer or copolymer of hydroxypropyl (meth)acrylate, homopolymer or copolymer of glucose (meth)acrylate, homopolymer or copolymer of polyethylene glycol (meth)acrylate, and copolymer of polyethylene glycol methyl ether (meth)acrylate;
[0021] Optionally, the (meth)acrylamide homopolymer or copolymer is selected from copolymers of (meth)acrylamide, copolymers of N,N-dimethylacrylamide, homopolymers or copolymers of N-hydroxymethylacrylamide, homopolymers or copolymers of N-hydroxyethyl(meth)acrylamide, homopolymers or copolymers of N-hydroxypropyl(meth)acrylamide, copolymers of N-isopropylacrylamide and copolymers of 2-acrylamido-2-methylpropanesulfonic acid (AMPS), etc.
[0022] The above-mentioned (meth)acrylic acid refers to acrylic acid or methacrylic acid; the above-mentioned (meth)acrylamide refers to acrylamide or methacrylamide. Hereinafter, (meth)acrylic acid also refers to acrylic acid or methacrylic acid, and (meth)acrylamide also refers to acrylamide or methacrylamide.
[0023] In some embodiments of the present invention, more specifically, the water-soluble or hydrophilic polymer of the microgel is preferably one or more of hyaluronic acid, alginic acid, carboxymethyl starch, carboxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, polyglutamic acid, polyacrylic acid and carboxylated polyethylene glycol.
[0024] In some embodiments of the present invention, further, the structure of the o-phthalaldehyde group-modified microgel is selected from one of the following structures:
[0025] In Formulas 1-1 to 1-12, MG represents microgel,
[0026] Wherein, 1≤r≤20, 1≤s≤20, 1≤t≤50, and n≥2. Preferably, 1≤r≤6, 1≤s≤10, 1≤t≤30, and n≥2.
[0027] The second aspect of the present invention provides a method for preparing the o-phthalaldehyde group-modified microgel, the specific method is as follows:
[0028] (1) Preparation of microgels;
[0029] (2) covalently linking the aldehyde-preprotected o-phthalaldehyde precursor derivative to the active groups on the microgel to prepare the o-phthalaldehyde precursor derivative-modified microgel;
[0030] (3) Deprotecting the aldehyde group yields a microgel modified with o-phthalaldehyde groups.
[0031] In some embodiments of the present invention, the method for preparing the microgel in step (1) comprises: 1) preparing the microgel by directly crosslinking water-soluble or hydrophilic polymers; or, 2) preparing the microgel by polymerizing monomers and crosslinking.
[0032] Specifically, 1) refers to cross-linking a water-soluble or hydrophilic polymer into a gel through a specific cross-linking method, further physically breaking it by mechanical force and then sieving it through sieves of different sizes to obtain microgels with different particle size distributions; or preparing a water-soluble or hydrophilic polymer into an oil-water emulsion under the action of an emulsifier, and further cross-linking it through a specific cross-linking method to obtain microgels with a certain particle size.
[0033] Wherein, the specific cross-linking method includes chemical cross-linking and radiation cross-linking.
[0034] When the specific cross-linking method is chemical cross-linking, it includes the following three methods:
[0035] Polymers based on multifunctional acrylic or methacrylic acid modification are cross-linked via free radical chain polymerization;
[0036] Covalent crosslinking based on multifunctional crosslinkers (functionality ≥ 2) in the presence or absence of catalysts;
[0037] In the presence or absence of a catalyst, the polymer chain itself contains two or more reactive functional groups (such as hydroxyl, carboxyl, etc.) condensation cross-linking.
[0038] The chemical crosslinking is preferably covalent crosslinking based on a multifunctional crosslinking agent in the presence or absence of a catalyst.
[0039] Wherein, the multifunctional cross-linking agent can be selected from one or more of glutaraldehyde, polyamine, multifunctional epoxy, epichlorohydrin, divinyl sulfone (DVS), phosphorus oxychloride or sodium trimetaphosphate;
[0040] The multifunctional epoxy can be selected from one or more of 1,4-butanediol diglycidyl ether (BDDE), 1,6-hexanediol diglycidyl ether, ethylene glycol diglycidyl ether, neopentyl glycol diglycidyl ether, glycerol triglycidyl ether, trimethylolpropane triglycidyl ether, polyethylene glycol diglycidyl ether and polypropylene glycol diglycidyl ether; further, the multifunctional epoxy is preferably 1,4-butanediol diglycidyl ether;
[0041] The polyamine is a multifunctional crosslinking agent containing one or more functional groups selected from primary amine, hydrazine, hydrazide and hydroxylamine. Furthermore, the polyamine is selected from adipic acid dihydrazide (ADH) or hexamethylenediamine.
[0042] When the specific cross-linking method is radiation cross-linking, it includes electron beam radiation cross-linking or gamma ray radiation cross-linking.
[0043] Wherein, when the radiation crosslinking is selected from electron beam radiation crosslinking, the radiation dose rate is selected from 10 to 1000 Gy / s, and the radiation time is selected from 5 to 100 minutes;
[0044] When the radiation cross-linking is selected from gamma-ray radiation cross-linking, the radiation dose is selected from 10 to 100 kGy.
[0045] Specifically, 2) refers to copolymerizing and cross-linking monomers with multifunctional double bond cross-linking agents, or cross-linking monomers into gels through a specific cross-linking method after polymerization, and further physically breaking them by mechanical force and then screening them through sieves of different sizes to obtain microgels with different particle size distributions; or emulsion polymerization or precipitation polymerization of monomers with multifunctional double bond cross-linking agents to obtain microgels with a certain particle size, or first emulsion polymerization or precipitation polymerization of monomers and then cross-linking by a specific cross-linking method to obtain microgels with a certain particle size.
[0046] The monomer may be selected from one or more water-soluble monomers, or may be selected from one or more water-soluble monomers and other copolymerizable monomers.
[0047] The water-soluble monomer may be further selected from (meth)acrylic acid, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, glucose (meth)acrylate, polyethylene glycol methyl ether (meth)acrylate and polyethylene glycol (meth)acrylate, (meth)acrylamide, N,N-dimethylacrylamide, N-hydroxymethylacrylamide, N-hydroxyethyl (meth)acrylamide, N-hydroxypropyl (meth)acrylamide, N-isopropylacrylamide and 2-acrylamido-2-methylpropanesulfonic acid (AMPS), vinyl pyrrolidone, etc.;
[0048] The other copolymerizable monomers can be selected from (meth)acrylate monomers, (meth)acrylamide monomers, styrene monomers, vinyl acetate, acrylonitrile and the like.
[0049] The multifunctional double bond crosslinking agent refers to a crosslinking agent containing two or more polymerizable double bond functional groups, including but not limited to glucose acrylate, 2,9-decadiene, 2-hexadecenoic acid, N,N'-methylenebisacrylamide and glycerol acrylate.
[0050] The specific cross-linking method is selected from the following two methods:
[0051] Condensation crosslinking of polymer chains containing two or more reactive functional groups in the presence or absence of a catalyst;
[0052] Irradiation cross-linking.
[0053] In some embodiments of the present invention, the aldehyde-preprotected o-phthalaldehyde precursor derivative described in step (2) comprises an o-phthalaldehyde group with an aldehyde-preprotected o-phthalaldehyde group and a substituent R that can be connected to the active group on the microgel, and the structure is shown in Formula 2:
[0054] In Formula 2, R includes, but is not limited to, carboxyl substituents, vinyl sulfone substituents, epoxy substituents, halogenated alkane substituents, isocyanate substituents, and amino substituents.
[0055] In Formula 2, optionally, R may be directly connected to the benzene ring, or may be connected to the benzene ring through a single or multiple alkylene chains or alkoxy chains, wherein the multiple alkylene chains or alkoxy chains are connected through ether bonds, amide bonds, ester bonds, carbamate bonds or urea bonds.
[0056] In some embodiments of the present invention, the aldehyde group pre-protected o-phthalaldehyde precursor derivative is specifically selected from one or a combination of the following structures:
[0057] Wherein, 1≤r≤20, 1≤s≤20, 1≤t≤50. Preferably, 1≤r≤6, 1≤s≤10, 1≤t≤30.
[0058] In some embodiments of the present invention, the active groups on the microgel are selected from hydroxyl groups or carboxyl groups.
[0059] The covalent bond connection between the aldehyde group pre-protected o-phthalaldehyde precursor derivative and the active group on the microgel is selected from ether bond, amide bond, ester bond, carbamate bond or urea bond, preferably ether bond, amide bond and carbamate bond.
[0060] More specifically, when the active groups on the microgel are selected from hydroxyl groups, the covalent bond connection is based on an ether bond connection between the vinyl sulfone substituents, epoxy substituents and halogenated alkane substituents on the o-phthalaldehyde precursor derivative and the hydroxyl groups on the microgel, an ester bond connection between the carboxyl substituents on the o-phthalaldehyde precursor derivative and the hydroxyl groups on the microgel, and a carbamate bond connection between the isocyanate substituents on the o-phthalaldehyde precursor derivative and the hydroxyl groups on the microgel;
[0061] When the active groups on the microgel are selected from carboxyl groups, the covalent bond connection is based on an amide bond connection between the amino substituents on the o-phthalaldehyde precursor derivative and the carboxyl groups on the microgel.
[0062] In some embodiments of the present invention, the covalent bond is preferably selected from an ether bond between a vinyl sulfone substituent on an o-phthalaldehyde precursor derivative and a hydroxyl group on the microgel, an ether bond between an epoxy substituent on an o-phthalaldehyde precursor derivative and a hydroxyl group on the microgel, a carbamate bond between an isocyanate substituent on an o-phthalaldehyde precursor derivative and a hydroxyl group on the microgel, an ester bond between a carboxyl substituent on an o-phthalaldehyde precursor derivative and a hydroxyl group on the microgel, and an amide bond between an amino substituent on an o-phthalaldehyde precursor derivative and a carboxyl group on the microgel.
[0063] The present invention provides specific covalent bonding methods for preparing microgels modified with o-phthalaldehyde precursor derivatives. Specifically, the carboxyl groups on the microgels are used as active groups to undergo an amidation reaction with amine substituents on the o-phthalaldehyde precursor derivatives that have been pre-protected with aldehyde groups. The carboxyl groups on the microgels are activated with carbodiimide, 2-chloro-4,6-dimethyl-1,3,5-triazine (CDMT), 2-chloro-1-methylpyriiodide (CMPI), 1,1'-carbonyldiimidazole (CDI), and 4-(4,6-dimethoxytriazin-2-yl)-4-methylmorpholine hydrochloride (DMTMM), and then efficiently react with amine substituents on the o-phthalaldehyde precursor derivatives that have been pre-protected with aldehyde groups to form amide bonds.
[0064] In some embodiments of the present invention, the deprotection in step (3) refers to deprotecting the pre-protected o-phthalaldehyde functional group of the aldehyde group attached to the microgel under acidic conditions to obtain a microgel modified with an o-phthalaldehyde group.
[0065] The structures of the o-phthalaldehyde group-modified microgels provided in Formulas 1-1 to 1-12 of the first aspect of the present invention are merely exemplary of the o-phthalaldehyde group-modified microgels that can be obtained by using the aforementioned aldehyde group-preprotected o-phthalaldehyde precursor derivatives and microgels through certain preparation methods. Based on the disclosure of this application, those skilled in the art will appreciate that other aldehyde group-preprotected o-phthalaldehyde precursor derivative structures can be used to achieve the o-phthalaldehyde group-modified microgels described above.
[0066] The third aspect of the present invention provides a variety of highly effective hemostatic materials.
[0067] In some embodiments of the present invention, the highly effective hemostatic material is a highly effective hemostatic sponge having a porous structure obtained by drying the o-phthalaldehyde group-modified microgel provided by the first aspect of the present invention.
[0068] In some embodiments of the present invention, the microgel modified with o-phthalaldehyde groups can be placed in a mold and dried according to the required specifications and sizes.
[0069] In some embodiments of the present invention, the drying method is vacuum freeze drying.
[0070] Preferably, the vacuum freeze-drying conditions are freezing at -20°C for 6 hours, followed by freeze-drying at -60°C for 48 hours.
[0071] In some embodiments of the present invention, the highly effective hemostatic material is a highly effective hemostatic powder obtained by dehydrating and drying the o-phthalaldehyde group-modified microgel provided by the first aspect of the present invention.
[0072] In some embodiments of the present invention, the water removal is performed by replacing the water in the microgel modified with o-phthalaldehyde groups with an organic solvent, thereby reducing the water content of the microgel and precipitating it in the form of solid particles.
[0073] Wherein, the organic solvent is selected from methanol, ethanol, acetone, isopropanol, acetonitrile, etc. Preferably, the organic solvent is selected from ethanol.
[0074] In some embodiments of the present invention, the drying is direct drying and vacuum freeze drying followed by drying.
[0075] Preferably, the drying conditions are freezing at -20°C for 6 hours, freeze-drying at -60°C for 48 hours, and then drying at 30°C for 12 hours.
[0076] In some embodiments of the present invention, the particle size distribution of the high-efficiency hemostatic powder is 20 mesh to 500 mesh.
[0077] In some embodiments of the present invention, the high-efficiency hemostatic material is a high-efficiency flowable hemostatic agent directly obtained by uniformly dispersing the o-phthalaldehyde group-modified microgel provided by the first aspect of the present invention in a solvent; or, the high-efficiency hemostatic material is a high-efficiency flowable hemostatic agent obtained by uniformly dispersing a high-efficiency hemostatic sponge or a high-efficiency hemostatic powder in a solvent.
[0078] The solvent is selected from water, physiological saline, buffer solution, decellularized matrix or cell culture medium solution containing or not containing polyols, and the polyol is preferably one or more of propylene glycol, butanediol, 1,2-pentanediol, 1,2-hexanediol or glycerol;
[0079] The uniform dispersion process can utilize mechanical stirring or a mixer.
[0080] In some embodiments of the present invention, the solid content of the high-efficiency flowable hemostat is 1% to 20% (w / v). Preferably, the solid content of the high-efficiency flowable hemostat is selected from 5% to 12% (w / v).
[0081] A fourth aspect of the present invention provides a composite sponge.
[0082] The composite sponge is a composite sponge based on microgel modified with o-phthalaldehyde groups. The composite sponge is obtained by layering the microgel modified with o-phthalaldehyde groups and the microgel not modified with o-phthalaldehyde groups in a mold and drying them to obtain a composite sponge with a pore structure.
[0083] Wherein, the o-phthalaldehyde group-modified microgel is provided by the first aspect of the present invention;
[0084] The microgel without o-phthalaldehyde group modification refers to a microgel prepared from a water-soluble or hydrophilic polymer or a microgel prepared by polymerization and cross-linking of monomers. That is, the microgel without o-phthalaldehyde group modification is the microgel prepared in step (1) of the second aspect of the present invention;
[0085] The conditions such as the polymer skeleton, water content, particle size and pH value of the microgel modified with o-phthalaldehyde groups and the microgel not modified with o-phthalaldehyde groups can be the same or different.
[0086] The layering refers to spreading the microgel modified with o-phthalaldehyde groups and the microgel not modified with o-phthalaldehyde groups in layers in a mold to form a multilayer structure with different components distributed on different horizontal planes, and further drying to obtain a multilayer composite sponge.
[0087] In some embodiments of the present invention, preferably, the composite sponge has a double-layer structure, wherein one side is composed of microgels modified with o-phthalaldehyde groups, and the other side is composed of microgels not modified with o-phthalaldehyde groups.
[0088] In some embodiments of the present invention, a composite sponge with a double-layer structure can be applied to a variety of biomedical scenarios, wherein the side containing the microgel modified with o-phthalaldehyde groups can be used in various application scenarios such as hemostasis or tissue adhesion and sealing, and the side containing the microgel without o-phthalaldehyde group modification can achieve applications such as postoperative anti-adhesion due to the lubrication and low inflammatory stimulation properties of the corresponding polymer skeleton.
[0089] The fifth aspect of the present invention provides the use of the high-efficiency hemostatic material based on the third aspect of the present invention.
[0090] When the high-efficiency hemostatic material is a high-efficiency hemostatic sponge, the application of the high-efficiency hemostatic sponge is selected from one of the following applications:
[0091] Application of the high-efficiency hemostatic sponge in the preparation of non-compressive hemostatic products for penetrating wounds;
[0092] Application of the high-efficiency hemostatic sponge in the preparation of liver hemostatic products;
[0093] Application of the high-efficiency hemostatic sponge in the preparation of spleen hemostasis products;
[0094] Application of the high-efficiency hemostatic sponge in the preparation of surface arterial hemostasis products;
[0095] Application of the high-efficiency hemostatic sponge in the preparation of surface vein hemostasis products;
[0096] Application of the high-efficiency hemostatic sponge in the preparation of femoral artery hemostasis products;
[0097] Application of the high-efficiency hemostatic sponge in the preparation of abdominal aorta hemostasis products;
[0098] Application of the high-efficiency hemostatic sponge in the preparation of carotid artery hemostasis products;
[0099] Application of the high-efficiency hemostatic sponge in the preparation of cardiac hemostatic products;
[0100] Application of the high-efficiency hemostatic sponge in the preparation of coronary artery hemostasis products;
[0101] Application of the high-efficiency hemostatic sponge in the preparation of hemostatic products for tooth extraction wounds;
[0102] Application of the high-efficiency hemostatic sponge in the preparation of spinal hemostatic products;
[0103] The high-efficiency hemostatic sponge is used in preparing uterine wall hemostatic products.
[0104] When the high-efficiency hemostatic material is a high-efficiency hemostatic powder, the application of the high-efficiency hemostatic powder is selected from one of the following applications:
[0105] Application of the high-efficiency hemostatic powder in the preparation of liver hemostatic products;
[0106] Application of the high-efficiency hemostatic powder in the preparation of spleen hemostatic products;
[0107] Application of the high-efficiency hemostatic powder in the preparation of venous hemostasis products;
[0108] Application of the high-efficiency hemostatic powder in the preparation of surface arterial hemostatic products;
[0109] Application of the high-efficiency hemostatic powder in the preparation of surface vein hemostasis products;
[0110] Application of the high-efficiency hemostatic powder in the preparation of intestinal hemostatic products;
[0111] Application of the high-efficiency hemostatic powder in the preparation of skin hemostatic products;
[0112] Application of the high-efficiency hemostatic powder in the preparation of oral mucosal hemostatic products;
[0113] Application of the high-efficiency hemostatic powder in the preparation of hemostatic products for hysterectomy;
[0114] The application of the high-efficiency hemostatic powder in the preparation of spinal hemostatic products.
[0115] When the high-efficiency hemostatic material is a high-efficiency flowable hemostatic agent, the application of the high-efficiency flowable hemostatic agent is selected from one of the following applications:
[0116] Application of the high-efficiency mobile hemostatic agent in the preparation of non-compressive hemostatic products for penetrating wounds;
[0117] The high-efficiency mobile hemostatic agent is used in the preparation of digestive tract hemostatic products;
[0118] Application of the highly efficient mobile hemostatic agent in the preparation of hemostatic products during and after partial nephrectomy;
[0119] Application of the high-efficiency mobile hemostatic agent in the preparation of hemostatic products for narrow cavities of organisms;
[0120] Application of the high-efficiency mobile hemostatic agent in the preparation of spinal hemostatic products;
[0121] The high-efficiency mobile hemostatic agent is used in the preparation of hemostatic products for percutaneous puncture.
[0122] The applications provided above are merely exemplary of the application of the high-efficiency hemostatic material in various hemostasis scenarios. Based on the description of this application, those skilled in the art will be able to conceive that the high-efficiency hemostatic material can be applied to hemostasis in other scenarios.
[0123] A sixth aspect of the present invention provides an application of the composite sponge according to the fourth aspect of the present invention, selected from one of the following applications:
[0124] Application of the composite sponge in the preparation of postoperative anti-adhesion products;
[0125] Application of the composite sponge in the preparation of tissue leakage sealing products;
[0126] The composite sponge is used in preparing tissue fluid leakage blocking products.
[0127] Among them, the postoperative adhesion prevention includes but is not limited to abdominal wall adhesion prevention, pericardial adhesion prevention, tendon adhesion prevention and intrauterine adhesion prevention; the tissue leakage blocking includes but is not limited to lung parenchyma leakage blocking; the tissue fluid leakage blocking includes but is not limited to intestinal leakage blocking, pancreatic leakage blocking, cerebrospinal fluid leakage blocking, gastric leakage blocking, etc.
[0128] The reaction of o-phthalaldehyde with primary amines is characterized by high efficiency, rapidity and high selectivity. It has been proven to be used for quantitative detection of the content of amines and amino acids (MH Joseph, P. Davies, Electrochemical detection of amino acids, Curr. Sep. 1982), efficient coupling of biomacromolecules (CLTung, CT Wong, EY Fung, X. Li, Traceless and chemoselective amine bioconjugation via phthalimidine formation in native protein modification, Organic Letters 2016) and rapid cross-linking construction of hydrogel materials (Z. Zhang, C. He, Y. Rong, H. Ren, T. Wang, Z. Zou, et al., A fast and versatile cross-linking strategy via o-phthalaldehyde condensation for mechanically strengthened and functional hydrogels, National Science Review 2021), etc. Therefore, o-phthalaldehyde has the potential to serve as a modifying group in current polymer hemostatic materials, enabling efficient coupling between hemostatic materials and plasma proteins, forming a secondary cross-linked network to enhance mechanical properties, and simultaneously bonding with amino groups on the tissue surface to improve adhesion between the hemostatic material and tissue, thereby overcoming the shortcomings of current hemostatic materials, such as weak tissue adhesion and poor mechanical properties. However, there is no prior art for modifying microgels with o-phthalaldehyde groups and using them to prepare hemostatic materials.
[0129] The present invention provides a class of microgels modified with o-phthalaldehyde groups and a method for preparing the same, as well as various different forms of hemostatic materials prepared based on the microgels modified with o-phthalaldehyde groups, including hemostatic sponges, hemostatic powders, and mobile hemostatic agents. Compared with existing hemostatic materials, the hemostatic materials of the present invention have a highly efficient hemostatic function. On the one hand, the o-phthalaldehyde groups achieve efficient and rapid coupling with proteins containing free amino groups that are abundant in the blood, forming a second cross-linked network to enhance the mechanical properties of the material itself, achieving effective blocking of bleeding points and resisting their continued bleeding; on the other hand, the highly active o-phthalaldehyde groups simultaneously chemically bond with the amino groups on the tissue surface, providing long-lasting and stable adhesion to prevent the occurrence of rebleeding. Due to its excellent tissue adhesion and mechanical strength, the hemostatic material of the present invention does not require additional pressing when used, and can achieve rapid and effective hemostasis in a variety of hemostatic scenarios. It is particularly suitable for the treatment of hemostatic scenarios such as irregular surfaces, active or pressure bleeding, and minimally invasive surgery, and has important clinical application value and significance. BRIEF DESCRIPTION OF THE DRAWINGS
[0130] FIG1 is a hydrogen nuclear magnetic resonance spectrum of the degradation product of the hyaluronic acid microgel (ie, microgel HA-2) in Example 2.
[0131] FIG2 shows the results of in vitro hemostasis tests of hemostatic sponges with different o-phthalaldehyde derivative labeling rates, a control sponge, and a commercial absorbable gelatin sponge in Example 22.
[0132] FIG3 is a microscope image (left) and in vitro hemostasis test results (right) of the hemostatic powder modified with o-phthalaldehyde groups of different particle sizes in Example 23.
[0133] Figure 4 is a scanning electron microscopic morphology of the surface adhesion, aggregation, activation of platelets (left) and adsorption of red blood cells (right) of the hemostatic sponge of the present invention in Example 26.
[0134] Figure 5 is a photograph of the hemostatic sponge of the present invention (group a), the control sponge (group b) and the commercial absorbable gelatin sponge (group c) applied to non-compressive hemostasis of penetrating wounds in Example 27 and a visual photograph of the blood loss.
[0135] Figure 6 is a photograph of the hemostatic sponge of the present invention (group a), the control sponge (group b) and the commercial absorbable gelatin sponge (group c) applied to liver hemostasis in Example 28 and a visual photograph of the blood loss.
[0136] Figure 7 is a photograph of the hemostatic sponge of the present invention (group a), the control sponge (group b) and the commercial absorbable gelatin sponge group (group c) used for hemostasis in the rabbit ear artery in Example 30.
[0137] FIG8 is a photograph of the hemostatic powder of the present invention (group a), the control powder (group b) and the commercial chitosan hemostatic granules (group c) applied to liver hemostasis in Example 40.
[0138] Figure 9 is a comparison chart of the hemoglobin content measured in the blood clots collected from the hemostatic powder of the present invention (group a), the control powder (group b), the commercial chitosan hemostatic powder (group c) and the blank group (group d) in Example 45.
[0139] Figure 10 is a photograph of the mobile hemostatic agent of the present invention (group a), the control fluid (group b) and the commercial fluid gelatin (group c) applied to non-compressive hemostasis of penetrating wounds in Example 50.
[0140] Figure 11 is a photograph of the mobile hemostatic agent of the present invention (group a), the control fluid (group b) and the commercial fluid gelatin (group c) applied to percutaneous puncture hemostasis of the spleen in Example 55.
[0141] Figure 12 is the H&E staining results of the composite sponge (group a) and the control group (group b) used for postoperative abdominal adhesion prevention in Example 57 (I represents small intestine, L represents liver, and S represents composite sponge material). DETAILED DESCRIPTION
[0142] The present invention will be described in detail below with reference to the accompanying drawings and specific embodiments.
[0143] Example 1: Synthesis of aldehyde-preprotected o-phthalaldehyde precursor derivatives (i.e., compounds 1 to 12)
[0144] (I) Synthesis of Compounds 1-3 (s=2, t=7)
[0145] (1) Synthesis of compound 1: The synthesis process was based on the method disclosed in Zhen Zhang, Chaoliang He, Yan Rong, Hui Ren, Tianran Wang, Zheng Zou, Xuesi Chen, National Science Review, Volume 8, Issue 4, April 2021, nwaa128. 1 H NMR (400MHz, DMSO-d6): δ = 12.74 (brs, 1H), 8.29 (d, J = 7.6Hz, 1H), 8.12 (s, 1H), 7.65 (d, J = 7.6Hz, 1H), 6.30 (s, 1H), 6.11 (s, 1H), 3.40-3.30 (m, 6H).
[0146] (2) Synthesis of Compound 2: Compound 1 (10 g, 45 mmol) was dissolved in 10 mL of anhydrous dichloromethane (DCM), and 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide (EDC, 10.38 g, 67 mmol) and N-hydroxysuccinimide (NHS, 7.69 g, 67 mmol) were added, and stirred at room temperature for 30 minutes. Ethylenediamine (27.05 g, 0.45 mmol) was dissolved in anhydrous DCM and stirred, and the above reaction system was quickly added dropwise to the ethylenediamine solution, and the reaction was stirred at room temperature for 12 hours. After the reaction was completed, most of the solvent was removed, and the residual compound was extracted three times with ethyl acetate. The organic phases were combined, dried over anhydrous sodium sulfate, and the solvent was removed by rotary evaporation. The crude product was purified by silica gel chromatography to obtain Compound 2 (9.0 g, yield 75%). 1 H NMR (400MHz, DMSO-d6): δ=8.18(t,1H),8.07(d,1H),7.80(dd,1H),7.56(dd,1H),6.05(h,2 H),4.59(dt,1H),4.25(dt,1H),3.38(tt,J=5.1Hz,2H),3.34(s,3H),3.03(tt,J=6.3,2H).
[0147] (3) Synthesis of compound 3: α,ω-dicarboxyl polyethylene glycol (COOH-PEG-COOH, t=7, 8.26 g) was dissolved in 100 mL of anhydrous DCM, and EDC (3.52 g, 22.7 mmol) and NHS (2.61 g, 22.7 mmol) were added and stirred at room temperature for 30 minutes. Compound 2 (5 g, 18.8 mmol) was dissolved in anhydrous DCM (50 mL) and gradually added dropwise to the above system. The reaction was stirred at room temperature for 12 hours. After the reaction was completed, most of the solvent was removed, and the residual compound was extracted three times with ethyl acetate. The organic phases were combined, dried over anhydrous sodium sulfate, and the solvent was removed by rotary evaporation. The crude product was purified by silica gel column chromatography to obtain compound 3 (10.5 g, yield 79%). 1 H NMR (400MHz, DMSO-d6): δ = 8.86 (s, 1H), 8.21 (d, J = 7.6Hz, 1H), 7.93 (s, 1H), 7.61 ( d,J=7.6Hz,1H),6.38(s,1H),6.30(s,1H),3.80-3.48(m,28H),3.40-3.30(m,6H).
[0148] (II) Synthesis of Compounds 4-8 (r = 2, s = 6, t = 7)
[0149] (1) Synthesis of compound 4: The synthesis process was based on the method disclosed in Chun Ling Tung, Clarence TT Wong, Eva Yi Man Fung and Xuechen Li. Org. Lett. 2016, 18, 11, 2600-2603. 1 H NMR (400MHz, DMSO-d6): δ = 11.82 (s, 1H), 7.56 (dq, 1H), 7.43 (dd, 1H), 7.16 (ddt, 1H), 6.05 (m, 1H), 5.97 (q, 1H), 3.53 (dt, 2H), 3.40-3.30 (m, 6H).
[0150] (2) Synthesis of compound 5: The synthesis process was similar to that of compound 2. 1 H NMR (400MHz, DMSO-d6): δ = 7.56 (t, 1H), 7.48 (m, 2H), 7.14 (ddt, 1H), 6.06 (s, 1H), 5.97 (q, 1H), 3.40-3.30 (m, 6H), 3 .07(q,2H),2.90-2.72(m,4H),2.38(t,J=8.2Hz,2H),1.87(t,J=6.5Hz,2H),1.59-1.43(m,4H),1.46-1.30(m,4H).
[0151] (3) Synthesis of Compound 6: Compound 5 (5 g, 14.3 mmol) was dissolved in 100 mL of toluene, and succinic anhydride (1.5 g, 15 mmol) and triethylamine (TEA, 2.1 mL, 15 mmol) were added. The mixture was stirred at room temperature for 4 h. After completion of the reaction, the solvent was removed by rotary evaporation, and the crude product was purified by silica gel column chromatography to obtain Compound 6 (5.2 g, 80% yield). 1 H NMR (400MHz, DMSO-d6): δ = 11.87 (s, 1H), 7.62 (t, 1H), 7.56 (t, 1H), 7.44-7.36 (m, 2H), 7.14 (ddt, 1H), 6.08-6.02 (m, 1H), 5.97 (q, 1H), 3.40-3.30(m,6H),3.19-3.03(m,4H),2.77(tt,J=8.7Hz,2H),2.55(dd,2H),2.48-2.34(m,4H),1.56-1.43(m,4H),1.40-1.27(m,4H).
[0152] (4) Synthesis of compound 7: α,ω-diaminopolyethylene glycol (NH2-PEG-NH2, t=7, 8.8 g) was dissolved in 50 mL of anhydrous DCM. Compound 4 (5 g, 19.8 mmol) was dissolved in anhydrous DCM (50 mL), and EDC (4.65 g, 30 mmol) and NHS (3.45 g, 30 mmol) were added and stirred at room temperature for 30 minutes. The above reaction system was gradually added dropwise to the NH2-PEG-NH2 solution and stirred at room temperature for 12 hours. After the reaction was completed, most of the solvent was removed, and the residual compound was extracted three times with ethyl acetate. The organic phases were combined, dried over anhydrous sodium sulfate, and the solvent was removed by rotary evaporation. The crude product was purified by silica gel column chromatography to obtain compound 7 (10.4 g, yield 81%). 1 H NMR (400MHz, DMSO-d6): δ = 7.43-7.36 (m, 2H), 7.14 (ddt, 1H), 3.61-3.43 (m, 28H), 3.36-3.26 (m, 6H), 2.88-2.71 (m, 2H), 2.54-2.36 (m, 2H).
[0153] (5) Synthesis of Compound 8: Hexamethylene diisocyanate (HDI, 1.28 g, 7.6 mmol) was dissolved in anhydrous tetrahydrofuran (THF, 50 mL). Compound 7 (5 g, 7.6 mmol) was dissolved in anhydrous THF (50 mL) and slowly added dropwise to the rapidly stirred HDI solution. The mixture was stirred at room temperature for 2 h. The solvent was removed by rotary evaporation, and the mixture was redissolved in a small amount of DCM and poured into n-pentane to precipitate a solid. This reaction was repeated twice and then drained to obtain Compound 8 (5.5 g, 92% yield). 1 H NMR (400MHz, DMSO-d6): δ = 7.53 (t, 1H), 7.44-7.36 (m, 2H), 7.14 (ddt, 1H), 6.047 (s,1H),5.97(s,1H),5.87(t,1H),5.65(t,1H),3.63-3.51(m,32H),3.36-3.28(m ,4H),3.39-3.32(m,6H),3.31-3.18(m,4H),3.10(tdd,J=5.7,4.7,1.0Hz,2H),2. 90-2.71(m,4H),2.41(t,J=8.3Hz,2H),1.87(t,J=6.5Hz,2H),1.59-1.27(m,8H).
[0154] (III) Synthesis of Compounds 9-12
[0155] (1) Synthesis of Compound 9: Intermediate 1 (5 g, 25.5 mmol) was dissolved in anhydrous DCM (40 mL), and 0.2 M NaOH solution (85 mL) was added, followed by tetrabutylammonium bromide (TBAB, 0.82 g, 2.55 mmol), and the mixture was stirred at room temperature for 30 min. 1-Bromo-2-chloroethane (8.41 mL, 0.102 mol) was added dropwise, and the reaction was stirred at room temperature for 48 h. Subsequently, the phases were separated, and the organic phase was washed with brine, dried over anhydrous sodium sulfate, filtered, and concentrated under reduced pressure. The crude product was purified by silica gel chromatography to obtain Compound 9 (5.6 g, 85% yield). 1 H NMR (400MHz, DMSO-d6): δ = 7.45 (dd, 1H), 7.15 (dd, 1H), 6.88(dd,1H),6.07-5.97(m,2H),4.24(q,J=2.2Hz,2H),3.81(t,J=2.2Hz,2H),3.37-3.34(s,6H).
[0156] (2) Synthesis of Compound 10: HDI (6.43 g, 38.3 mmol) was dissolved in anhydrous DCM. Intermediate 1 (5 g, 25.5 mmol) was dissolved in anhydrous DCM, and TEA (3.53 mL, 25.5 mmol) was added. The mixture was slowly added dropwise to the rapidly stirred HDI solution, and the reaction was stirred at room temperature for 30 min. After removing the solvent by rotary evaporation, the mixture was redissolved in a small amount of DCM and poured into n-pentane to precipitate a solid. After repeating twice, Compound 10 (9.76 g, 70% yield) was obtained. 1 H NMR (400MHz, DMSO-d6): δ = 7.56 (dd, J = 8.4, 1H), 7.40 (s, 1H), 7.07 (dd, J = 8.3, 1H), 6.34 (t, J = 5.3Hz, 1 H),6.03–5.93(m,2H),3.38-3.31(s,6H),3.20-3.13(m,2H),3.06(q,J=5.5Hz,2H),1.67-1.27(m,8H).
[0157] (3) Synthesis of Compound 11: Under anhydrous and oxygen-free conditions, intermediate 1 (5 g, 25.5 mmol) was dissolved in anhydrous DCM. 2-Chloroethanesulfonyl chloride (5 g, 30.6 mmol) was slowly added dropwise to the solution in an ice bath at 0°C. After a 10-min reaction, anhydrous TEA (4.23 mL, 30.6 mmol) was slowly added dropwise and the reaction was continued at room temperature for 12 h. After completion of the reaction, the solvent was removed by rotary evaporation, and the crude product was purified by silica gel column chromatography to afford compound 11 (6.9 g, 95% yield). 1H NMR (400MHz, DMSO-d6): δ=7.48-7.41(m,1H),7.35(s,1H),7.08(dd,J=8.2,1H),6.26( dd,J=18.5,1H),6.15(dd,J=18.4,1H),6.03(dq,J=2.9,1.7Hz,2H),3.41-3.33(s,6H).
[0158] (4) Synthesis of Compound 12: Intermediate 1 (5 g, 25.5 mmol) was suspended in 30 mL of water and 1.5 M aqueous NaOH solution (10 mL) was added. The system gradually became clear. After stirring for 40 minutes, epichlorohydrin (7.1 g, 76.5 mmol) was added and stirred at room temperature for 24 hours. After the reaction was completed, most of the solvent was removed and the residual compound was extracted three times with ethyl acetate. The organic phases were combined, dried over anhydrous sodium sulfate, and the solvent was removed by rotary evaporation. The crude product was purified by silica gel column chromatography to obtain Compound 12 (5.8 g, 90% yield). 1 H NMR (400MHz, DMSO-d6): δ = 7.45 (s, 1H), 7.14 (s, 1H), 6.91 (dd, J = 8.3, 1H), 6.07-5.9 9(m,2H),4.11(d,J=3.3Hz,2H),3.42(s,1H),3.38-3.32(m,6H),2.91-2.78(m,2H).
[0159] Embodiment 2 to Embodiment 8:
[0160] Preparation of microgels
[0161] Example 2: Preparation of hyaluronic acid microgels (i.e., microgels HA-1 to HA-4)
[0162] (1) Preparation of HA-1 microgel: Hyaluronic acid (HA, 10 g, 890 kDa) was dissolved in 90 mL of 0.25 M NaOH solution and stirred until completely dissolved. Divinyl sulfone (DVS, 1.5 g, 13 mmol) was weighed and dissolved in 10 mL of 0.25 M NaOH solution and added to the reaction mixture. The mixture was stirred at 40°C for 2 h and then allowed to stand at room temperature overnight. The resulting hydrogel was dialyzed against physiological saline (pH = 7) for 2-3 days, then physically crushed and sieved to obtain microgels with a mesh size of 20 to 300. The microgel was resuspended in a 150 IU / mL hyaluronidase solution and incubated at 37°C for 24 hours. The degradation was observed. If incomplete degradation was observed, the enzyme solution was replaced and the incubation was continued. If complete degradation was observed, the solution was boiled, centrifuged, and the supernatant was freeze-dried. Based on the H-NMR spectrum, the cross-linking degree (molar ratio of cross-linker to polymer repeating unit) of the microgel HA-1 was calculated to be approximately 31.3%.
[0163] (2) Preparation of microgel HA-2: HA (10 g, 1.2 MDa) was dissolved in 90 mL of 0.25 M NaOH solution and stirred until completely dissolved. 1,4-Butanediol diglycidyl ether (BDDE, 2.2 g, 11 mmol) was weighed and dissolved in 10 mL of 0.25 M NaOH solution and added to the above reaction solution. The mixture was stirred at 40 °C for 2 h and then placed under constant temperature reaction conditions at 40 °C overnight. The hydrogel after the reaction was dialyzed with physiological saline (pH = 7) for 2-3 days, then physically broken and sieved to obtain microgels with mesh sizes of 20 to 300. The microgel was resuspended in 150 IU / mL hyaluronidase solution and incubated at 37 °C for 24 h. The degradation was observed. If it was not completely degraded, the enzyme solution was replaced and the incubation was continued. If it was completely degraded, the solution was boiled, centrifuged, and the supernatant was freeze-dried. In this embodiment, the H NMR spectrum of the hyaluronic acid microgel degradation product is shown in FIG1 . Based on the H NMR spectrum, the crosslinking degree (molar ratio of crosslinking agent to polymer repeating unit) of the microgel HA-2 can be calculated to be approximately 36.8%.
[0164] (3) Preparation of microgel HA-3: HA (1 g, 1.2 MDa) was dissolved in 10 mL of 0.25 M NaOH solution and stirred until completely dissolved. 40 mL of liquid paraffin was evenly mixed with 2% emulsifier Span80 as the oil phase. The stirring speed of the oil phase was adjusted to 1800 rpm, and 10 mL of HA solution was added dropwise to the oil phase. BDDE (0.4 g, 2 mmol) was weighed and added to the above emulsion, stirred at room temperature for 30 min, and reacted at 45°C for 12 h. After the cross-linking reaction was completed, the emulsion was washed with the same volume of ethyl acetate and anhydrous ethanol respectively. The above operation was repeated 2 to 3 times. The gel particles after standing and stratification were collected and dried to obtain microgel HA-3. The microgel was resuspended in 150 IU / mL hyaluronidase solution and incubated at 37°C for 24 h. The degradation was observed. If it was not completely degraded, the enzyme solution was replaced and the incubation was continued. If it was completely degraded, the solution was boiled, centrifuged, and the supernatant was freeze-dried. According to the H-NMR spectrum, the cross-linking degree (molar ratio of cross-linking agent to polymer repeating unit) of the microgel HA-3 was calculated to be approximately 35.0%.
[0165] (4) Preparation of microgel HA-4: HA (0.1 g, 1.2 MDa) was dissolved in 10 mL of deionized water and stirred until completely dissolved. 40 mL of liquid paraffin was evenly mixed with 5% of the emulsifier Span80 as the oil phase. Under the conditions of stirring the oil phase at 500 rpm and 30% ultrasound, 10 mL of HA solution was added dropwise to the oil phase, and the pH of the mixture was adjusted to 4.0-5.0. 1-Ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride (EDC-HCl, 50 mg, 0.26 mmol) and adipic acid dihydrazide (ADH, 0.1 g, 57.4 mmol) were quickly added. The rotation speed was increased to 800 rpm, and the pH of the system was maintained at 4.0-5.0. The reaction was carried out at room temperature for 6 h. After the reaction, the mixture was allowed to stand for 30 minutes. The same volume of isopropanol was added to the system, stirred, allowed to stand, and the supernatant removed. This process was repeated two to three times, followed by sonication for 20 minutes. The solids were then drained to obtain microgel HA-4. The microgel was resuspended in a 150 IU / mL hyaluronidase solution and incubated at 37°C for 24 hours. Degradation was observed. If degradation was incomplete, the enzyme solution was replaced and incubation continued. If degradation was complete, the solution was boiled, centrifuged, and the supernatant freeze-dried. Based on the H-NMR spectrum, the crosslinking degree (molar ratio of crosslinker to polymer repeating unit) of the microgel HA-4 was calculated to be approximately 25.0%.
[0166] Example 3: Preparation of carboxymethyl cellulose microgels (i.e., microgels CMC-1 and CMC-2)
[0167] (1) Preparation of CMC-1 microgel: Carboxymethyl cellulose (CMC, 10 g, viscosity 1200 mPa·s (25°C, 2%), DS: 0.7) was dissolved in 100 mL of 0.25 M NaOH solution and stirred until completely dissolved. BDDE (2.2 g, 11 mmol) was weighed and dissolved in 25 mL of 0.25 M NaOH solution and added to the reaction mixture. The mixture was stirred at 40°C for 2 h and then allowed to stand at room temperature overnight. The resulting hydrogel was dialyzed against physiological saline (pH = 7) for 2–3 days and then physically crushed and sieved to obtain microgels with mesh sizes ranging from 20 to 300. The microgels were resuspended in a 100 IU / mL lysozyme solution and incubated at 37°C for 24 hours. The degradation was observed. If incomplete degradation was observed, the enzyme solution was replaced and the incubation continued. If complete degradation was observed, the solution was boiled, centrifuged, and the supernatant was freeze-dried. Based on the H-NMR spectrum, the cross-linking degree (molar ratio of cross-linker to polymer repeating unit) of the microgel CMC-1 was calculated to be approximately 21.5%.
[0168] (2) Preparation of CMC-2 microgel: Carboxymethyl cellulose (CMC, 10 g, viscosity 2000 mPa·s (25°C, 2%), DS: 0.85) was dissolved in 100 mL of 0.5 M NaOH solution and stirred until completely dissolved. The system was heated to 50°C, and epichlorohydrin (ECH, 1.5 g, 16 mmol) was added dropwise to the reaction system. The mixture was stirred at 50°C for 2 h and then allowed to stand at room temperature overnight. The resulting hydrogel was dialyzed with physiological saline (pH = 7) for 2–3 days, then physically crushed and sieved to obtain microgels with mesh sizes ranging from 20 to 300. The microgel was resuspended in a 100 IU / mL lysozyme solution and incubated at 37°C for 24 hours. The degradation was observed. If incomplete degradation was observed, the enzyme solution was replaced and the incubation was continued. If complete degradation was observed, the solution was boiled, centrifuged, and the supernatant was freeze-dried. Based on the H-NMR spectrum, the cross-linking degree (molar ratio of cross-linker to polymer repeating unit) of the microgel CMC-2 was calculated to be approximately 18.5%.
[0169] Example 4: Preparation of Alginic Acid Microgel (i.e. Microgel Alg-1)
[0170] Alginic acid (10 g of sodium alginate, Alg, viscosity 1000 mPa·s (25°C, 2%)) was dissolved in 100 mL of 0.5 M NaOH solution and stirred until completely dissolved. The reaction mixture was heated to 50°C, and epichlorohydrin (ECH, 1.5 g, 16 mmol) was added dropwise to the reaction mixture. The mixture was stirred at 50°C for 2 hours and then allowed to stand at room temperature overnight. The resulting hydrogel was dialyzed against physiological saline (pH = 7) for 2-3 days, then physically crushed and sieved to obtain microgels with mesh sizes ranging from 20 to 300. The microgels were resuspended in a 20 IU / mL alginate lyase solution and incubated at 37°C for 24 hours. The degradation was observed. If incomplete degradation was observed, the enzyme solution was replaced and incubation continued. If complete degradation was observed, the solution was boiled, centrifuged, and the supernatant was freeze-dried. Based on the H-NMR spectrum, the cross-linking degree (molar ratio of cross-linker to polymer repeating unit) of the microgel Alg-1 was calculated to be approximately 15.8%.
[0171] Example 5: Preparation of cross-linked sodium starch glycolate microgels (i.e., microgels CMS-1 and CMS-2)
[0172] (1) Preparation of microgel CMS-1: 25 g of cassava starch and 48 mL of 95% ethanol were placed in a 500 mL three-necked flask, condensed and refluxed, and stirred thoroughly to form a uniform starch emulsion. Then, the pH was adjusted to 11 with 5% NaOH solution, heated to 55°C in a water bath, 0.09 g of ECH was added, and the reaction was carried out for 1 hour to obtain cross-linked starch. The cross-linked starch was cooled to 25°C, and 11 g of NaOH solid was added for pretreatment for 30 minutes. After the pretreatment, 11 g of chloroacetic acid was added, and the mixture was heated to 55°C and reacted for 4 hours. After the reaction was completed, the solution was neutralized with hydrochloric acid to pH = 7. The solution was filtered while hot, and the filter cake was washed with 95% ethanol until there was no white floc in the filtrate. Then, the solution was vacuum dried at 50°C, and the filter cake was crushed to obtain a white powder. A certain amount of sample was taken and constant weight was obtained at 105°C. The degree of carboxymethyl substitution was measured by copper salt precipitation method and was 0.8.
[0173] (2) Preparation of microgel CMS-2: 10 g of soluble starch was dissolved in NaOH solution (1%, w / w, 100 mL) to obtain a starch solution. Sodium trimetaphosphate (2 g) was added to the above starch solution and stirred until completely dissolved. Emulsifier Span80 (7.5 mL) and oil phase cyclohexane (150 mL) were added to a 250 mL three-necked flask, stirred at 50°C and condensed to reflux. When the emulsifier was completely dissolved and the system temperature was stable at 50°C, 15 mL of the prepared starch / sodium trimetaphosphate solution was taken and added dropwise to the three-necked flask at a speed of 800 rpm. Stirring was maintained at this speed for 5 h. After the reaction was completed, the lower layer of solid was collected by centrifugation and washed several times with acetone, petroleum ether, and deionized water respectively. Finally, it was dehydrated with anhydrous ethanol and vacuum dried at 40°C for 5 h to obtain a white powder, which was cross-linked starch. The preparation process of sodium carboxymethyl starch was referred to the preparation process of microgel CMS-1. A certain amount of the white powder was taken and heated to constant weight at 105° C., and the degree of carboxymethyl substitution was measured by a copper salt precipitation method to be 0.8.
[0174] Example 6: Preparation of polyglutamic acid microgel (i.e. microgel PGA-1)
[0175] Dissolve poly-γ-glutamic acid (PGA, 6g) in 100mL of deionized water and place them in a sealable 10mL radiation tube, filled with nitrogen for protection. 60 Co-γ ray irradiation (1.0 kGy / h, 10 kGy) was performed. The hydrogel after the reaction was dialyzed with physiological saline (pH=7) at 4°C for 2-3 days, and then physically crushed and sieved to obtain microgels with mesh sizes of 20 to 300, namely microgel PGA-1.
[0176] Example 7: Preparation of polyacrylic acid microgels (i.e., microgels PAA-1 and PAA-2)
[0177] (1) Preparation of microgel PAA-1: Acrylic acid (AA, 60 g) was weighed and added to a beaker with stirring. Approximately 40 mL of 30% sodium hydroxide solution was added dropwise to partially neutralize the AA. N,N'-methylenebisacrylamide (BIS, 0.5 g) and ammonium persulfate (APS, 0.4 g) were weighed and dissolved in a small amount of water before being added to the above system. After mixing, the mixture was allowed to polymerize and crosslink at 75°C for 3 h. The PAA hydrogel was collected and fully swollen in physiological saline for equilibrium. The microgel PAA-1 was then obtained by physical crushing and sieving.
[0178] (2) Preparation of microgel PAA-2: 5 g of acrylic acid was weighed and added to a beaker with stirring. Approximately 5 mL of 30% sodium hydroxide solution was added dropwise to partially neutralize the AA. A small amount of ammonium acrylate (0.1 g) and sodium acetate (0.05 g) were then added. 40 mL of kerosene and 9% of the emulsifier octoxynol (Op-10) were uniformly mixed to form the oil phase. With the oil phase stirred at 1000 rpm, 5 mL of the HA solution was added dropwise to the oil phase and stirred for 10-15 minutes to obtain a white emulsion. The emulsion was added to a four-necked flask equipped with a stirrer, thermometer, dropping funnel, and gas tube. After stirring and deoxygenating with nitrogen for 20 minutes, an aqueous solution of azobisisobutyronitrile (AIBN, 0.1g) and sodium bisulfite (0.05g) was added dropwise, followed by a solution of ethylene glycol dimethacrylate (EGDMA, 0.5g). The reaction was maintained at 40°C for 4 hours. After completion of the reaction, ethanol was added for precipitation, filtered under reduced pressure, washed two to three times with acetone, and dried to obtain the microgel PAA-2.
[0179] Example 8: Preparation of carboxylated polyethylene glycol microgel (i.e., microgel PEG-1)
[0180] 40 mL of liquid paraffin was uniformly mixed with 2% emulsifier Span80 to form the oil phase. A certain amount of carboxyl-terminated four-arm polyethylene glycol (20 kDa, n=113, 1 g) was weighed and dissolved in 5 mL of 0.01 mol / L MES buffer (pH 5.2), followed by the addition of EDC (38 mg) and NHS (20 mg). A 5% DMSO aqueous solution containing hexamethylenediamine (12 mg) was prepared and mixed. The two solutions were then quickly added to the rapidly stirred liquid paraffin. The oil phase stirring speed was adjusted to 1800 rpm and stirred at room temperature for 2 hours. A large amount of n-hexane was added to the emulsion. After the microspheres and the solvent separated naturally, the supernatant was decanted and washed with n-hexane 2-3 times. After standing and demixing, the gel particles were collected and dried to obtain the PEG-1 microgel.
[0181] Embodiment 9 to Embodiment 15:
[0182] Synthesis of Microgels Modified with O-Phthalaldehyde Groups
[0183] Example 9: Synthesis of o-phthalaldehyde group-modified hyaluronic acid microgels (i.e., microgels HA-2.1 to HA-2.4)
[0184] (1) Synthesis of microgel HA-2.1: The swollen microgel HA-2 (100 g) was resuspended in 100 mL of 0.01 mol / L 2-(N-morpholino)ethanesulfonic acid (MES) buffer solution (pH = 5.2) and stirred to disperse. Compound 2 (110 mg, 0.41 mmol, s = 2) was weighed and dissolved in 10 mL of dimethyl sulfoxide (DMSO) and then added to the above reaction solution. 4-(4,6-dimethoxytriazin-2-yl)-4-methylmorpholine hydrochloride (DMTMM, 4.1 g, 15 mmol) was weighed three times and dissolved in 3 mL of MES buffer solution respectively. The mixture was added to the above reaction solution and reacted at 37°C for 24 h. The reaction solution was adjusted to a pH of 8-9 and then dialyzed against saline for 2-3 days. The microgels were collected and 10% trifluoroacetic acid was added for 1 hour. The reaction system was then dialyzed against deionized water for 1 day to collect the HA microgels modified with o-phthalaldehyde groups, i.e., microgel HA-2.1. The supernatant of the reaction system was collected and the amount of residual compound 2 in the supernatant was determined by high-performance liquid chromatography. The labeling yield of compound 2 was calculated to be approximately 4.67% (w / w).
[0185] (2) Synthesis of microgels HA-2.2 with different labeling rates: The swelled microgels HA-2 (100 g) were resuspended in 100 mL of 0.01 mol / L MES buffer (pH = 5.2) and stirred for dispersion. Different weights (20, 50, 100, and 175 mg) of compound 5 (r = 2, s = 6) were weighed and dissolved in 10 mL of DMSO and added to the reaction solution. The remaining reaction process was similar to that of the synthesis of microgel HA-2.1. The supernatant of the reaction system was collected and the amount of residual compound 5 in the supernatant was determined by HPLC. The labeling rates of compound 5 were calculated to be 0.58%, 1.12%, 2.03%, and 4.21% (w / w), respectively, and were recorded as microgels HA-2.2 (0.58), HA-2.2 (1.12), HA-2.2 (2.03), and HA-2.2 (4.21), respectively.
[0186] (3) Synthesis of microgel HA-2.3: The swollen microgel HA-2 (100 g) was resuspended in 50 mL of 0.25 M NaOH solution and stirred to disperse. Compound 11 (68.6 mg, 0.24 mmol) was weighed and added to the above system. The reaction was carried out at 50°C for 8 h. After the reaction was completed, the pH of the reaction solution was neutralized to 7, and then dialyzed with normal saline for 2-3 days. The microgel was collected and added with 10% trifluoroacetic acid, and reacted for 1 h. The reaction system was then dialyzed with deionized water for 1 day, and the HA microgel modified with o-phthalaldehyde groups, i.e., microgel HA-2.3, was collected. The supernatant of the reaction system was collected, and the amount of residual compound 11 in the supernatant was determined by high-performance liquid chromatography. The labeling rate of compound 11 was calculated to be approximately 2.78% (w / w).
[0187] (4) Synthesis of microgel HA-2.4: The swollen microgel HA-2 (100 g) was resuspended in 50 mL of 0.25 M NaOH solution and stirred to disperse. Compound 12 (60 mg, 0.24 mmol) was weighed and added to the above system. The reaction was carried out at 40°C for 12 h. After the reaction, the reaction solution was neutralized to pH 7 and then dialyzed with normal saline for 2-3 days. The microgel was collected and added with 10% trifluoroacetic acid. The reaction was continued for 1 h. The reaction system was then dialyzed with deionized water for 1 day to collect the HA microgel modified with o-phthalaldehyde groups, i.e., microgel HA-2.4. The supernatant of the reaction system was collected and the amount of residual compound 12 in the supernatant was determined by high performance liquid chromatography. The labeling rate of compound 12 was calculated to be approximately 3.04% (w / w).
[0188] The above structural formula and examples provide exemplary structures and synthesis methods for o-phthalaldehyde group-modified hyaluronic acid microgels. Based on the disclosure of this application, one skilled in the art will appreciate that other hyaluronic acid microgels and other o-phthalaldehyde protected derivatives can be used to synthesize the o-phthalaldehyde group-modified hyaluronic acid microgels.
[0189] Example 10: Synthesis of o-phthalaldehyde group-modified carboxymethyl cellulose microgels (i.e., microgels CMC-1.1 to CMC-1.3)
[0190] (1) Synthesis of microgel CMC-1.1: The swollen microgel CMC-1 (100 g) was resuspended in 20 mL of deionized water and stirred to disperse. Compound 1 (54 mg, 0.24 mmol, s = 2), EDC (1.12 g, 7.2 mmol) and dimethylaminopyridine p-toluenesulfonate (DPTS, 1.8 g, 7.2 mmol) were added to the above system in sequence and reacted at room temperature for 24 h. After the reaction, the solution was dialyzed with sodium chloride aqueous solution (pH = 4) containing dilute hydrochloric acid for 2-3 days. The microgel was collected and added with 10% trifluoroacetic acid and reacted for 1 h. The reaction system was then dialyzed with deionized water for 1 day to collect the CMC microgel modified with o-phthalaldehyde groups, i.e., microgel CMC-1.1. The supernatant of the reaction system was collected and the amount of residual compound 1 in the supernatant was determined by high performance liquid chromatography. The labeling rate of compound 1 was calculated to be approximately 2.15% (w / w).
[0191] (2) Synthesis of Microgel CMC-1.2: The equilibrated microgel CMC-1 (100 g) was resuspended in 20 mL of 0.01 mol / L MES buffer (pH 5.2) and stirred for dispersion. Compound 5 (175 mg, 0.5 mmol, r = 2, s = 6) was weighed and dissolved in 10 mL of DMSO and added to the reaction solution. The remaining reaction procedures were similar to those for the synthesis of microgel HA-2.1. The supernatant of the reaction system was collected and the amount of residual compound 5 in the supernatant was determined by HPLC. The labeling yield of compound 5 was calculated to be approximately 3.14% (w / w).
[0192] (3) Synthesis of Microgel CMC-1.3: The equilibrated microgel CMC-1 (100 g) was resuspended in 20 mL of 0.01 mol / L MES buffer (pH = 5.2) and stirred for dispersion. Compound 7 (156 mg, 0.24 mmol, r = 2, t = 7) was weighed and dissolved in 10 mL of MES buffer and added directly to the reaction solution. The remaining reaction procedures were similar to those for the synthesis of microgel HA-2.1. The supernatant of the reaction system was collected and the amount of residual compound 7 in the supernatant was determined by HPLC. The labeling yield of compound 7 was calculated to be approximately 4.69% (w / w).
[0193] The above structural formula and examples provide exemplary structures and synthesis methods for o-phthalaldehyde-modified carboxymethyl cellulose microgels. Based on the disclosure of this application, one skilled in the art will appreciate that other carboxymethyl cellulose microgels and other o-phthalaldehyde-protected derivatives can be used to synthesize the o-phthalaldehyde-modified carboxymethyl cellulose microgels.
[0194] Example 11: Synthesis of alginate microgels modified with o-phthalaldehyde groups (i.e., microgels Alg-1.1 to Alg-1.3)
[0195] (1) Synthesis of Microgel Alg-1.1: The swollen microgel Alg-1 (100 g) was resuspended in 20 mL of deionized water and stirred to disperse. Compound 3 (160 mg, 0.24 mmol, s = 2, t = 7), EDC (1.12 g, 7.2 mmol), and DPTS (1.8 g, 7.2 mmol) were added sequentially to the above system. The remaining reaction process was similar to that of the synthesis of microgel CMC-1.1. The supernatant of the reaction system was collected and the amount of residual compound 3 in the supernatant was determined by HPLC. The labeling rate of compound 3 was calculated to be approximately 4.88% (w / w).
[0196] (2) Synthesis of Microgel Alg-1.2: 100 g of the equilibrated microgel Alg-1 was resuspended in 20 mL of 0.01 mol / L MES buffer (pH 5.2) and stirred. Compound 5 (175 mg, 0.5 mmol, r = 2, s = 6) was weighed and dissolved in 10 mL of DMSO and added to the reaction solution. The remaining reaction procedures were similar to those for the synthesis of microgel HA-2.1. The supernatant of the reaction system was collected and the amount of residual compound 5 in the supernatant was determined by HPLC. The labeling yield of compound 5 was calculated to be approximately 3.47% (w / w).
[0197] (3) Synthesis of Microgel Alg-1.3: The equilibrated microgel Alg-1 (100 g) was resuspended in 50 mL of 0.25 M NaOH solution and stirred for dispersion. Compound 11 (68.6 mg, 0.24 mmol) was weighed and added to the system. The remaining reaction procedures were similar to those for the synthesis of microgel HA-2.3. The supernatant of the reaction system was collected and the amount of residual compound 11 in the supernatant was determined by HPLC. The labeling yield of compound 11 was calculated to be approximately 2.44% (w / w).
[0198] The above structural formula and examples provide exemplary structures and synthesis methods for o-phthalaldehyde group-modified alginate microgels. Based on the disclosure of this application, one skilled in the art will appreciate that other alginate microgels and other o-phthalaldehyde protected derivatives can be used to synthesize the o-phthalaldehyde group-modified alginate microgels.
[0199] Example 12: Synthesis of o-phthalaldehyde group-modified sodium carboxymethyl starch microgels (i.e., microgels CMS-1.1 to CMS-1.3)
[0200] (1) Synthesis of Microgel CMS-1.1: Dried cross-linked sodium starch glycolate (i.e., microgel CMS-1, 10 g) was uniformly dispersed in 100 mL of deionized water and stirred. Compound 4 (0.6 g, 2.4 mmol, r = 2), EDC (1.12 g, 7.2 mmol), and DPTS (1.8 g, 7.2 mmol) were added sequentially to the above system. The remaining reaction process was similar to that of the synthesis of microgel CMC-1.1. The supernatant of the reaction system was collected and the amount of residual compound 4 in the supernatant was determined by high-performance liquid chromatography. The labeling rate of compound 4 was calculated to be approximately 2.17% (w / w).
[0201] (2) Synthesis of microgel CMS-1.2: The dried cross-linked sodium carboxymethyl starch (i.e., microgel CMS-1, 10 g) was uniformly dispersed in 50 mL of 0.25 M NaOH solution and stirred for dispersion. Compound 9 (0.65 g, 2.5 mmol) was weighed and added to the above reaction solution, and the mixture was reacted at 40°C for 12 h. After the reaction, the pH was adjusted to 7, and the mixture was reprecipitated with 10 volumes of anhydrous ethanol to precipitate a white powder. The white powder was resuspended in a 10% trifluoroacetic acid solution, stirred at room temperature for 1 h, and reprecipitated with 10 volumes of anhydrous ethanol to precipitate a white powder, i.e., cross-linked sodium carboxymethyl starch microgel modified with o-phthalaldehyde groups (i.e., microgel CMS-1.2). The supernatant of the reaction system was collected, and the amount of residual compound 9 in the supernatant was determined by high-performance liquid chromatography. The labeling rate of compound 9 was calculated to be approximately 2.43% (w / w).
[0202] (3) Synthesis of microgel CMS-1.3: The dried cross-linked sodium carboxymethyl starch (i.e., microgel CMS-1, 10 g) was uniformly dispersed in anhydrous DMSO and stirred. A solution of compound 10 (0.87 g, 2.4 mmol) in anhydrous DMSO was added dropwise to the above system, and dibutyltin dilaurate (13 μL, 20 μmol) was added as a catalyst, and nitrogen was added for protection. The reaction was stirred at 70°C for 24 h. After the reaction was completed, the reaction system was allowed to stand, the microgel was collected, and dialyzed in physiological saline (pH = 7) for 2-3 days. The microgel was collected and added with 10% trifluoroacetic acid solution, stirred at room temperature for 1 h. After the reaction was completed, it was reprecipitated with 10 times the volume of anhydrous ethanol to precipitate a white powder, i.e., cross-linked sodium carboxymethyl starch microgel modified with o-phthalaldehyde groups (i.e., microgel CMS-1.3). The supernatant of the reaction system was collected, and the amount of residual compound 10 in the supernatant was determined by high performance liquid chromatography. The labeling rate of compound 10 was calculated to be approximately 3.21% (w / w).
[0203] The above structural formula and examples provide exemplary structures and synthesis methods for o-phthalaldehyde group-modified carboxymethyl starch microgels. Based on the disclosure of this application, those skilled in the art will appreciate that other carboxymethyl starch microgels and other o-phthalaldehyde protected derivatives can be used to synthesize the o-phthalaldehyde group-modified carboxymethyl starch microgels.
[0204] Example 13: Synthesis of o-phthalaldehyde group-modified polyglutamic acid microgel (i.e., microgel PGA-1.1)
[0205] Microgel PGA-1 (100 g) was resuspended in 500 mL of 0.01 mol / L MES buffer (pH 5.2) and stirred. Compound 2 (1.6 g, 6 mmol, s = 2) and DMTMM (5 g, 18 mmol) were weighed and dissolved in 20 mL of DMSO before being added to the reaction mixture. The remaining reaction procedures were similar to those described for the synthesis of microgel HA-2.1. The supernatant was collected and the amount of residual compound 2 in the supernatant was determined by HPLC. The labeling yield of compound 2 was calculated to be approximately 0.88% (w / w).
[0206] The above structural formula and examples provide exemplary structures and synthesis methods for o-phthalaldehyde-modified polyglutamic acid microgels. Based on the disclosure of this application, one skilled in the art will appreciate that other polyglutamic acid microgels and other o-phthalaldehyde-protected derivatives can be used to synthesize the o-phthalaldehyde-modified polyglutamic acid microgels.
[0207] Example 14: Synthesis of polyacrylic acid microgel modified with o-phthalaldehyde groups (i.e., microgel PAA-2.1)
[0208] Microgel PAA-2 (100 g) was resuspended in 50 mL of 0.01 mol / L MES buffer (pH 5.2) and stirred to disperse. EDC (10.38 g, 67 mmol) and N-hydroxysuccinimide (NHS, 7.69 g, 67 mmol) were added to the reaction mixture and stirred at room temperature for 30 minutes. Compound 2 (53 mg, 0.2 mmol) was dissolved in 10 mL of DMSO and added to the reaction mixture. The reaction mixture was allowed to react at room temperature for 24 hours. The pH of the reaction mixture was adjusted to 8-9, and the mixture was dialyzed against saline for 2-3 days. The microgels were collected and added to 10% trifluoroacetic acid. The reaction mixture was then dialyzed against deionized water for 1 day. The PAA microgel modified with o-phthalaldehyde groups, i.e., microgel PAA-2.1, was collected. The supernatant of the reaction mixture was collected, and the amount of residual compound 2 in the supernatant was determined by high-performance liquid chromatography. The labeling yield of compound 2 was calculated to be approximately 2.68% (w / w).
[0209] The above structural formula and examples provide exemplary structures and synthesis methods for o-phthalaldehyde-modified polyacrylic acid microgels. Based on the disclosure of this application, those skilled in the art will appreciate that other polyacrylic acid microgels and other o-phthalaldehyde-protected derivatives can be used to synthesize the o-phthalaldehyde-modified polyacrylic acid microgels.
[0210] Example 15: Synthesis of carboxylated polyethylene glycol microgels modified with o-phthalaldehyde groups (i.e., microgels PEG-1.1 and PEG-1.2)
[0211] (1) Synthesis of Microgel PEG-1.1: 10 g of microgel PEG-1 was uniformly dispersed in 200 mL of deionized water and stirred. Compound 2 (1.6 g, 6 mmol, s = 2) and DMTMM (5 g, 18 mmol) were weighed and dissolved in 20 mL of DMSO and added to the reaction mixture. The remaining reaction procedures were similar to those for the synthesis of microgel HA-2.1. The supernatant of the reaction system was collected and the amount of residual compound 2 in the supernatant was determined by HPLC. The labeling yield of compound 2 was calculated to be approximately 6.05% (w / w).
[0212] (2) Synthesis of Microgel PEG-1.2: Microgel PEG-1 (10 g) was uniformly dispersed in 200 mL of deionized water and stirred. EDC (1.04 g, 6.7 mmol) and NHS (0.77 g, 6.7 mmol) were weighed and added to the above system, and stirred at room temperature for 30 minutes. Compound 5 (0.35 g, 1 mmol, r = 2, s = 6) was weighed and dissolved in 20 mL of DMSO and added to the above reaction solution. The remaining reaction process was similar to the synthesis of microgel HA-2.1. The supernatant of the reaction system was collected and the amount of residual compound 5 in the supernatant was determined by HPLC. The labeling rate of compound 5 was calculated to be approximately 1.10% (w / w).
[0213] The above structural formula and examples provide exemplary structures and synthesis methods for o-phthalaldehyde group-modified polyethylene glycol microgels. Based on the disclosure of this application, one skilled in the art will appreciate that other polyethylene glycol microgels and other o-phthalaldehyde protected derivatives can be used to synthesize the o-phthalaldehyde group-modified polyethylene glycol microgels.
[0214] Example 16 to Example 21:
[0215] Preparation of the hemostatic material of the present invention and its control material
[0216] Example 16: Preparation of hemostatic sponge
[0217] Taking the microgel HA-2.2 in Example 9 as an example, the microgel was fully dispersed in deionized water to obtain a suspension with a solid content of 0.5% to 1.5% (w / v). The suspension was poured into a mold, frozen at -20°C for 6 hours, and then freeze-dried at -60°C for 48 hours to obtain the hemostatic sponge of the present invention.
[0218] Other o-phthalaldehyde group-modified microgels can also be used to prepare hemostatic sponges.
[0219] Comparative Example 17: Synthesis of Control Sponge
[0220] Taking the microgel HA-2 in Example 2 as an example, the microgel was fully dispersed in deionized water to obtain a suspension with a solid content of 0.5% to 1.5% (w / v). The suspension was poured into a mold, frozen at -20°C for 6 hours, and then freeze-dried at -60°C for 48 hours to obtain a control sponge without o-phthalaldehyde group modification.
[0221] Example 18: Preparation of hemostatic powder
[0222] Taking the microgel CMC-1.2 synthesized in Example 10 as an example, the microgel was fully dispersed in deionized water and replaced with 75%, 90%, and anhydrous ethanol, respectively. The precipitated solid was collected and freeze-dried at -60°C for 48 hours, followed by vacuum drying at 30°C for 12 hours. The solid was then sieved through sieves of different mesh sizes to obtain powders of different mesh sizes, which are the hemostatic powders of the present invention.
[0223] Other o-phthalaldehyde group-modified microgels can also be used to prepare the hemostatic powder of the present invention.
[0224] Comparative Example 19: Synthesis of Control Powder
[0225] Taking the microgel CMC-1 synthesized in Example 3 as an example, the microgel was thoroughly dispersed in deionized water and replaced with 75%, 90%, and anhydrous ethanol, respectively. The precipitated solid was collected and freeze-dried at -60°C for 48 hours, followed by vacuum drying at 30°C for 12 hours. The solid was then sieved through sieves of varying mesh sizes to obtain powders of varying mesh sizes, which served as the control powders of the present invention.
[0226] Example 20: Preparation of fluid hemostatic agent
[0227] Taking the microgel HA-2.2 synthesized in Example 9 as an example, the microgel was frozen at -20°C for 6 hours, then freeze-dried at -60°C for 48 hours, redispersed in physiological saline containing 5% glycerol, and homogenized using a high-speed homogenizer to obtain a paste-like fluid with a solid content of 5% to 10% (w / v) and a certain fluidity, namely the mobile hemostatic agent of the present invention.
[0228] Other o-phthalaldehyde group-modified microgels can also be used to prepare the mobile hemostatic agent of the present invention.
[0229] Comparative Example 21: Synthesis of Control Fluid
[0230] Taking the microgel HA-2 synthesized in Example 2 as an example, the microgel was frozen at -20°C for 6 hours, then freeze-dried at -60°C for 48 hours, redispersed in physiological saline containing 5% glycerol, and homogenized using a high-speed homogenizer to obtain a paste-like fluid with a solid content of 5% to 10% (w / v) and a certain fluidity, i.e., the control fluid.
[0231] Example 22 to Example 26:
[0232] Verification experiment of hemostasis, tissue adhesion and mechanical property enhancement after blood absorption of the hemostatic material of the present invention
[0233] Example 22: In vitro thrombosis experiment of hemostatic sponges with different o-phthalaldehyde group labeling rates
[0234] In this example, the hemostatic ability of the hemostatic sponge of the present invention was characterized by a thrombosis experiment. The specific experimental method is as follows:
[0235] Microgels HA-2.2 (0.58), HA-2.2 (1.12), HA-2.2 (2.03), and HA-2.2 (4.21) with o-phthalaldehyde group labeling rates of 0.58%, 1.12%, 2.03%, and 4.21% (w / w), respectively, from Example 9 were selected for in vitro thrombosis experiments. A control sponge (i.e., with a labeling rate of 0) and a commercial absorbable gelatin sponge were used as control groups. The materials were placed in a clean container and preheated at 37°C. 100 μL of fresh 37°C EDTA-anticoagulated sheep blood was dripped onto the surface of the materials. For the blank control group, blood was dripped directly onto the wall of the container and allowed to stand at 37°C for 5 minutes. Then, pour 4 mL of deionized water into the container and shake it gently to rupture the red blood cells that have not been absorbed by the material. Aspirate the supernatant to detect the characteristic absorption of red blood cell hemoglobin at 540 nm, and calculate the thrombosis index according to the following formula. The lower the thrombosis index, the stronger the material's ability to form thrombi.
[0236] In this example, the in vitro hemostatic performance of a control group, hemostatic sponges with different o-phthalaldehyde group labeling rates, a control sponge, and a commercial absorbable gelatin sponge is shown in Figure 2. The experimental results show that labeling with o-phthalaldehyde groups significantly improves the thrombosis ability of the hemostatic sponges. Furthermore, a higher o-phthalaldehyde group labeling rate on the hemostatic sponge indicates a stronger thrombosis ability, indicating a better hemostatic effect of the sponge. This indicates that the o-phthalaldehyde groups modified on the hemostatic sponge of the present invention can effectively improve the hemostatic performance of the hemostatic material.
[0237] Other hemostatic sponges prepared based on o-phthalaldehyde group-modified microgels or other different forms of hemostatic materials also have excellent hemostatic properties.
[0238] Example 23: In vitro thrombosis experiment of hemostatic powders with different particle size distributions
[0239] In this embodiment, the hemostatic performance of the hemostatic powder is characterized by the thrombosis index. The specific experiment is as follows: the hemostatic powder with the same o-phthalaldehyde group labeling rate prepared in Example 18 is passed through sieves of different mesh sizes to collect hemostatic powder materials with different particle size distributions, and the materials are divided into five groups (Group 1: mesh size less than 20 mesh, Group 2: 20-32 mesh, Group 3: 32 mesh-80 mesh, Group 4: 80 mesh-200 mesh, Group 5: mesh size greater than 200 mesh). The materials are observed under a microscope, and an in vitro thrombosis experiment is performed: a certain mass (10 mg) of material is placed in a clean centrifuge tube and preheated at 37°C. 50 μL of fresh EDTA anticoagulated sheep blood at 37°C is dripped on the surface of the material. In the blank control group, blood is directly dripped on the wall of the container and allowed to stand at 37°C for 5 minutes. Subsequently, 2 mL of deionized water was poured into the container and slightly shaken. The supernatant was aspirated to detect the absorbance at 540 nm, and the thrombosis index was calculated according to the formula in Example 22.
[0240] In this embodiment, the microscopic images (left figure) and thrombosis test results (right figure) of hemostatic powder modified with o-phthalaldehyde groups of different particle sizes are shown in Figure 3. The results show that within a certain particle size range, the thrombosis ability of the hemostatic powder is closely related to its particle size. The smaller the particle size, the larger the specific surface area of the hemostatic powder, the larger the surface area in contact with blood, and the stronger the ability to form a thrombus, indicating that the hemostatic effect of the hemostatic powder is better.
[0241] Other hemostatic powders prepared based on microgels modified with o-phthalaldehyde groups also have excellent hemostatic properties.
[0242] Example 24: In vitro tissue adhesion test of hemostatic materials
[0243] The tissue adhesion of a hemostatic material is a necessary property for sealing bleeding points, effectively controlling bleeding, and reducing the risk of venous thrombosis over a long period of time. This example tested the tissue adhesion of the hemostatic sponge of the present invention using a standard lap shear test (ASTM F2255). The specific experimental method is as follows:
[0244] Standard lap shear tests were conducted using a tensile testing machine (INSTRON, Germany) to measure the adhesion strength of the different hemostatic materials on pigskin. A control hemostatic material from the present invention and commercially available Fibrin glue were used as control groups. Pigskin was cut into rectangular sections 20 mm wide and 40 mm long. During the mechanical testing, a transparent polymethyl methacrylate film served as a rigid tissue backing. For the sponge material, either the different hemostatic sponges or the control sponge were cut to the same thickness (3 mm) and area (20 mm × 20 mm) and attached to one end of a piece of pigskin (adhesion area 20 mm × 20 mm). Another piece of pigskin was immediately pressed onto the sponge material on the other piece of pigskin, applying a uniform force of 100 kPa for 2 minutes. A tensile test was then performed to evaluate the instantaneous tissue adhesion strength of the sponge materials. Subsequently, the pigskin was soaked in saline for 12 hours, and after wiping the surface liquid, a tensile test was performed again to evaluate the long-term tissue adhesion strength of the sponge materials. For powder materials, hemostatic powder or control powder was evenly spread on one end of pigskin (adhesion area 20mm×20mm) with a thickness of 1mm. Immediately, another piece of pigskin was pressed on top of the powder material on the other pigskin, and a uniform force of 100kPa was applied for 2 minutes. A tensile test was immediately performed to evaluate the transient tissue adhesion strength of the above powder materials. Subsequently, the pigskin was soaked in saline for 12 hours, and the surface liquid was wiped off before a tensile test was performed again to evaluate the long-term tissue adhesion strength of the above powder materials. For fluid materials, 0.2mL of flowing hemostatic agent or control fluid was evenly spread on one end of pigskin (adhesion area 20mm×20mm). Immediately, another piece of pigskin was pressed on top of the fluid, and a uniform force of 100kPa was applied for 2 minutes. A tensile test was immediately performed to evaluate the transient tissue adhesion strength of the fluid materials. Subsequently, the pigskin was soaked in saline for 12 hours, and the surface liquid was wiped off before a tensile test was performed again to evaluate the long-term tissue adhesion strength of the above fluid materials. For the Fibrin glue control group, the two-component solution was sprayed onto one end of a piece of pigskin (adhesion area 20 mm × 20 mm) using a dual-mixer. Immediately, another piece of pigskin was pressed onto the glue solution with a uniform pressure of 100 kPa for 2 minutes. Tensile testing was then performed to assess the transient tissue adhesion strength of the Fibrin glue. Subsequently, the pigskin was soaked in saline for 12 hours, the surface liquid wiped, and then tensile testing was performed to assess the long-term tissue adhesion strength of the Fibrin glue. Adhesion strength was calculated using the following formula, where Fmax is the maximum force. To ensure data reliability, three samples were measured for each condition.
[0245] In this embodiment, the instantaneous tissue adhesion strength and long-term tissue adhesion strength of different materials are shown in Table 1. The results show that the sponge material modified with o-phthalaldehyde groups in the present invention has excellent tissue adhesion performance compared to commercial Fibrin glue and a control sponge without o-phthalaldehyde group modification (i.e., a control sponge prepared based on microgel HA-2). Moreover, when the o-phthalaldehyde group labeling rate on the sponge material is higher, its instantaneous and long-term tissue adhesion is stronger. In a wet environment, the tissue adhesion of the sponge material without o-phthalaldehyde group modification is greatly attenuated, making it difficult to achieve long-term stable tissue adhesion, while the sponge material modified with o-phthalaldehyde groups has stable and long-term tissue adhesion. At the same time, other forms of hemostatic materials of the present invention also demonstrate stronger instantaneous tissue adhesion strength and long-term tissue adhesion strength than the control material and commercial Fibrin glue (fibrinogen glue).
[0246] Table 1
[0247] Example 25: Rheological testing of hemostatic materials
[0248] Physical barrier blocking bleeding points is a strategy for controlling bleeding using hemostatic materials. However, the mechanical properties of common hemostatic materials, such as gauze, sponges, hydrogels and powders, are often weakened in the presence of blood (wet environment), making it difficult to block bleeding points in a timely and long-term manner, especially to block active or pressure bleeding points. The hemostatic material prepared by the present invention is based on the chemical reaction of o-phthalaldehyde and amino groups, which can react with a large amount of plasma proteins in the blood to form a complex of material and thrombus, enhance the mechanical properties of the material, achieve compression blocking of bleeding points, and resist its continued bleeding. This example studies the changes in mechanical properties (storage modulus) before and after the reaction of the hemostatic material of the present invention with blood through rheological testing. The specific experimental method is as follows:
[0249] Rheological tests were conducted using a HAAKE MARS rheometer on a 37°C test platform (20 mm diameter). The sponge materials used were the hemostatic sponge described in Example 16 (component selected from microgel HA-2.2 (4.21)) and the control sponge described in Comparative Example 17 (component selected from microgel HA-2). The sponges were pre-cut into identical circular shapes (0.5 mm thick, 20 mm diameter) and placed on the test platform. 200 μL of either normal saline or fresh EDTA-anticoagulated sheep blood was dripped directly above the sponges and allowed to fully absorb at 37°C for 5 minutes. Rheological tests were then immediately performed, and the storage modulus (G') was recorded. For powder materials, the hemostatic powder in Example 18 (component selected from microgel HA-2.2 (4.21)) and the control powder in Comparative Example 19 (component selected from microgel HA-2) were used for testing: the same mass (50 mg) of powder was evenly spread on the test platform, and 200 uL of normal saline or fresh EDTA anticoagulated sheep blood was added directly above the material, fully absorbed at 37°C for 5 minutes, and then immediately subjected to rheological testing, and the storage modulus (G') was recorded. For fluid materials, the mobile hemostatic agent in Example 20 (component selected from microgel HA-2.2 (4.21)) and the control fluid in Comparative Example 21 (selected from microgel HA-2) were used for testing: the same volume (200 μL) of fluid was spread on the test platform, and 200 uL of normal saline or fresh EDTA anticoagulated sheep blood was added directly above the material, fully absorbed at 37°C for 5 minutes, and then immediately subjected to rheological testing, and the storage modulus (G') was recorded. To ensure the reliability of the data, three samples were measured under each condition.
[0250] Table 2
[0251] In this Example, the changes in mechanical properties of different hemostatic materials of the present invention before and after reaction with blood are shown in Table 2. The results show a significant difference in the storage modulus of the hemostatic materials of the present invention after absorbing blood and saline, with the storage modulus of the hemostatic materials significantly increasing after blood absorption. In contrast, for the unlabeled control material, there was no significant difference in the storage modulus after absorbing blood or saline. These results demonstrate that the hemostatic materials of the present invention can increase their storage modulus, i.e., enhance their mechanical properties, after contact and reaction with blood.
[0252] Other hemostatic materials prepared based on microgels modified with o-phthalaldehyde groups can also increase their storage modulus and enhance their mechanical properties after contact and reaction with blood.
[0253] Example 26: Scanning electron microscope image of the interaction between hemostatic sponge and blood cells
[0254] Platelet adhesion is the initial step in thrombus formation and plays an important role in the hemostasis process. In addition, the rapid adhesion and aggregation of red blood cells also contribute to thrombus formation. Platelet and red blood cell adhesion is one of the indicators for evaluating the quality of hemostatic performance. This example uses scanning electron microscopy (SEM) to characterize the adhesion of the hemostatic material of the present invention to platelets and red blood cells. The specific experimental method is as follows:
[0255] A NOVA NanoSEM 230 low vacuum ultra-high resolution field emission scanning electron microscope was used to observe the surface morphology in the fast electron backscatter diffraction EBSD mode. Fresh EDTA anticoagulated sheep blood was centrifuged at 1500 rpm for 12 minutes at room temperature. After centrifugation, the upper layer was platelet-rich plasma and the lower layer was packed white blood cells and red blood cells. The blood cells in the lower layer were collected. The platelet-rich plasma was transferred to a plastic test tube and centrifuged at 3500 rpm for 5 minutes to collect the platelets in the lower layer. The collected blood cells and platelets were resuspended in phosphate buffered saline (PBS) respectively, added dropwise to the sponge sample (the hemostatic sponge in Example 16, the component of which was selected from microgel HA-2.2 (4.21)), and reacted at 37°C for 5 minutes. The sample was washed 3 times with PBS and fixed with 5% glutaraldehyde solution for 4 hours. The fixed sample was then washed 3 times with PBS. The sample was then replaced with 30%, 50%, 70%, 90%, and 95% ethanol solutions and anhydrous ethanol for 10 minutes each. The ethanol was then replaced with tert-butyl alcohol at room temperature for three more times, each time for 15 minutes. The sample was frozen at 4°C for crystallization and freeze-dried. The sample was then plated with Pt metal.
[0256] In this example, scanning electron microscopic images of the hemostatic sponge of the present invention showing adherence, aggregation, and activation of platelets (left image) and adsorption of red blood cells (right image) are shown in Figure 4. The images clearly show that the platelets on the surface of the hemostatic sponge are tightly adhered to the material surface, and upon activation, the platelets transform from spheres into a multi-pseudopodal network. Numerous red blood cells are adsorbed and aggregated within the porous structure of the material. These experimental results demonstrate that the hemostatic sponge of the present invention can adhere to, aggregate, and activate platelets, adsorb red blood cells, and facilitate thrombus formation.
[0257] Embodiment 27 to Embodiment 39:
[0258] Hemostatic application of the hemostatic sponge of the present invention
[0259] Example 27: Application of hemostatic sponge in non-compression hemostasis of penetrating wounds
[0260] A SD rat liver perforation model was selected and divided into three groups for non-compressive hemostasis experiments on penetrating injuries, with 3 rats in each group: a hemostatic sponge group of the present invention (group a, the hemostatic sponge in Example 16, the component of which is selected from microgel HA-2.2 (4.21)); a sponge control group of the present invention (group b, the control sponge in comparative example 17, the component of which is selected from microgel HA-2); and a commercial absorbable gelatin sponge group (group c). After anesthetizing the SD rats, their abdominal cavity was opened, the liver was lifted and placed on a pre-weighed filter paper, and then a penetrating wound with a diameter of 5 mm was established on the liver to cause bleeding. Subsequently, the hemostatic materials of different groups were stuffed into the penetrating wound. The amount of blood loss was measured by the weight gain of the hemostatic material and the filter paper, and the hemostasis time was recorded by a timer. In this embodiment, photos of the hemostatic sponge of the present invention (group a), the control sponge (group b) and the commercial absorbable gelatin sponge (group c) applied to non-compressive hemostasis of penetrating injuries are shown in Figure 5. The experimental results showed that group a had the least blood loss (0.5±0.1g, 1.0±0.2g, and 1.2±0.2g, respectively) and the shortest hemostasis time (45±10s, 60±12s, and 80±15s, respectively). This suggests that the hemostatic sponge of the present invention can be used for non-compressive hemostasis of penetrating wounds.
[0261] Hemostatic sponges composed of other different materials can also be used for non-compression hemostasis of penetrating wounds.
[0262] Example 28: Application of hemostatic sponge to stop bleeding in the liver
[0263] A liver cross-sectional trauma model of SD rats was selected and divided into three groups for liver hemostasis experiments, with 3 rats in each group: a hemostatic sponge group of the present invention (group a, the hemostatic sponge in Example 16, the component of which was selected from microgel HA-2.4); a sponge control group of the present invention (group b, the control sponge in comparative example 17, the component of which was selected from microgel HA-2); and a commercial absorbable gelatin sponge group (group c). After anesthetizing the SD rats, their abdominal cavities were opened, the liver was lifted and placed on a pre-weighed filter paper, and then a cross-sectional section with a diameter of 10 mm was established on the liver to cause bleeding. Subsequently, the hemostatic materials of different groups were lightly pressed on the cross-sectional wound surface. The amount of blood loss was measured by the weight gain of the hemostatic material and the filter paper, and the hemostasis time was recorded by a timer. In this embodiment, photos of the hemostatic sponge of the present invention (group a), the control sponge (group b) and the commercial absorbable gelatin sponge (group c) applied to liver hemostasis are shown in Figure 6. The experimental results showed that group a had the least blood loss (0.3±0.1 g, 0.7±0.3 g, and 1.2±0.2 g), and the shortest hemostasis time (15±10 s, 60±20 s, and 150±13 s, respectively). This suggests that the hemostatic sponge of the present invention can be used to stop liver bleeding.
[0264] Hemostatic sponges made of other different materials can also be used to stop liver bleeding.
[0265] Example 29: Application of hemostatic sponge to spleen hemostasis
[0266] A spleen incision bleeding model of New Zealand white rabbits was selected, and the spleen hemostasis experiment was carried out in three groups, with 3 rabbits in each group: the hemostatic sponge group of the present invention (group a, the hemostatic sponge in Example 16, the component of which is selected from microgel HA-2.1); the sponge control group of the present invention (group b, the control sponge in comparative example 17, the component of which is selected from microgel HA-2); and the commercial absorbable hemostatic gauze (group c). After the New Zealand white rabbits were anesthetized and fixed, the abdominal hair was shaved, and an incision was made along the midline of the abdomen to open the abdominal cavity and expose the spleen. An incision (8 mm wide and 2 mm deep) was made in the spleen to cause spleen damage, and bleeding continued for 30 seconds. Subsequently, different groups of hemostatic materials were placed on the bleeding site and continuously compressed for 60 seconds and then observed. If the bleeding was not successfully stopped, the compression was continued. The experimental results showed that group a had the shortest hemostasis time (80 ± 20 s in group a, 3 rabbits in group b failed to stop bleeding after more than 5 minutes, and 240 ± 45 s in group c), and group a had the least blood loss (1.3 ± 0.3 g in group a, 5 ± 0.8 g in group b within 5 minutes, and 4 ± 0.65 g in group c). This shows that the hemostatic sponge of the present invention can be used to stop spleen bleeding.
[0267] Hemostatic sponges made of other different materials can also be used to stop spleen bleeding.
[0268] Example 30: Application of hemostatic sponge to hemostasis of superficial arteries
[0269] A New Zealand white rabbit ear artery bleeding model was selected and divided into three groups for a surface artery hemostasis experiment, with 3 rabbits in each group: a hemostatic sponge group of the present invention (group a, the hemostatic sponge in Example 16, the component of which was selected from microgel CMC-1.2); a control sponge group of the present invention (group b, the control sponge in comparative Example 17, the component of which was selected from microgel CMC-1); and a commercial absorbable gelatin sponge group (group c). After the rabbits were anesthetized, the rabbit ear artery was punctured with a needle, and then the hemostatic materials of different groups were lightly pressed on the wound site, and the hemostasis time was recorded by a timer. In this example, photos of the hemostatic sponge of the present invention (group a), the control sponge (group b) and the commercial absorbable gelatin sponge group (group c) applied to the rabbit ear artery for hemostasis are shown in Figure 7. The experimental results showed that group a had the shortest hemostasis time (13 ± 10 s, 65 ± 15 s, and 85 ± 13 s, respectively) and the least blood loss (0.2 ± 0.1 g, 1.2 ± 0.5 g, and 1.0 ± 0.4 g, respectively). This suggests that the hemostatic sponge of the present invention can be used for superficial arterial hemostasis.
[0270] Hemostatic sponges composed of other different materials can also be used to stop bleeding in superficial arteries.
[0271] Example 31: Application of hemostatic sponge to stop bleeding in superficial veins
[0272] A New Zealand white rabbit ear vein bleeding model was used to conduct a surface venous hemostasis experiment, with three rabbits in each group: a hemostatic sponge group (Group a, the hemostatic sponge in Example 16, whose components were selected from the microgel CMC-1.1); a sponge control group (Group b, the control sponge in Comparative Example 17, whose components were selected from the microgel CMC-1); and a commercial absorbable gelatin sponge group (Group c). After the rabbits were anesthetized, the ear vein was punctured with a needle. Subsequently, the hemostatic materials of the different groups were gently pressed against the wound, and the hemostasis time was recorded using a timer. The experimental results showed that Group a had the shortest hemostasis time (Group a 20±10s, Group b 50±12s, Group c 55±15s), and Group a had the least blood loss (Group a 0.5±0.1g, Group b 1.5±0.3g, Group c 1.5±0.2g). This shows that the hemostatic sponge of the present invention can be used for surface venous hemostasis.
[0273] Hemostatic sponges made of other different materials can also be used to stop bleeding in superficial veins.
[0274] Example 32: Application of hemostatic sponge to femoral artery hemostasis
[0275] A femoral artery bleeding model of SD rats was selected and divided into three groups for femoral artery hemostasis experiments, with 3 rats in each group: a hemostatic sponge group of the present invention (group a, the hemostatic sponge in Example 16, the component of which is selected from microgel Alg-1.2); a sponge control group of the present invention (group b, the control sponge in comparative example 17, the component of which is selected from microgel Alg-1); and a commercial absorbable gelatin sponge group (group c). After the SD rats were anesthetized and fixed, the hair on the left leg was shaved, and the covering muscles of the groin were opened to expose the femoral artery. Puncture was performed using a dissecting needle with a depth of 0.5 mm. Subsequently, the hemostatic materials of different groups were lightly pressed on the wound, and the hemostatic time was recorded by a timer. The hemostatic material was gently lifted every 5 seconds to observe the bleeding situation until the bleeding was completely stopped. The amount of blood loss was calculated by the weight gain of the pre-weighed hemostatic material. The experimental results showed that group a had the shortest hemostasis time (120 ± 25 s in group a, one rat in group b successfully stopped bleeding in 280 s, the other two rats failed to stop bleeding within 5 minutes, and all three rats in group c failed to stop bleeding within 5 minutes), and group a had the least blood loss (1.5 ± 0.4 g in group a, 3.5 ± 0.7 g in group b within 5 minutes, and 4.0 ± 1.0 g in group c within 5 minutes). It can be seen that the hemostatic sponge in the present invention can be used for femoral artery hemostasis.
[0276] Hemostatic sponges composed of other different materials can also be used for femoral artery hemostasis.
[0277] Example 33: Application of hemostatic sponge to hemostasis of abdominal aorta
[0278] The abdominal aorta bleeding model of SD rats was selected and the abdominal aorta hemostasis experiment was carried out in three groups, with 3 rats in each group: the hemostatic sponge group of the present invention (group a, the hemostatic sponge in Example 16, the component of which was selected from microgel HA-2.4); the sponge control group of the present invention (group b, the control sponge in comparative example 17, the component of which was selected from microgel HA-2); and the commercial absorbable gelatin sponge group (group c). After the SD rats were anesthetized and fixed, the abdominal hair was shaved, the abdominal cavity was opened, and the internal organs were exposed. A small piece of filter paper was used to gently push the intestine and fat to the left side of the abdomen of the rat, and the two larger blood vessels in front of the spine were separated. The slightly whiter one on the right was the abdominal aorta. Puncture was performed using a dissecting needle with a depth of 0.5 mm. Subsequently, the hemostatic materials of different groups were lightly pressed on the wound surface, and the hemostasis time was recorded by a timer. The hemostatic material was gently lifted every 5 seconds to observe the bleeding situation until the bleeding was completely stopped. The amount of blood loss was calculated by the weight gain of the pre-weighed hemostatic material. During the experiment, group a had the shortest hemostasis time (155 ± 45 s in group a, while none of the three rats in groups b and c achieved hemostasis within 5 minutes), and group a had the least blood loss (1.3 ± 0.5 g in group a, 2.4 ± 0.8 g and 2.8 ± 0.9 g in groups b and c, respectively). This indicates that the hemostatic sponge of the present invention can be used for hemostasis of the abdominal aorta.
[0279] Hemostatic sponges composed of other different materials can also be used to stop bleeding in the abdominal aorta.
[0280] Example 34: Application of hemostatic sponge to carotid artery hemostasis
[0281] A SD rat carotid artery bleeding model was selected and divided into three groups for carotid artery hemostasis experiments, with 3 rats in each group: a hemostatic sponge group of the present invention (group a, the hemostatic sponge in Example 16, the component of which was selected from microgel HA-2.3); a sponge control group of the present invention (group b, the control sponge in comparative example 17, the component of which was selected from microgel HA-2); and a commercial absorbable gelatin sponge group (group c). The SD rats were anesthetized, the neck hair was shaved and fixed, and the rats were wiped and disinfected with iodine tincture. A longitudinal incision of about 2 cm was made in the middle of the neck, and then a complete transect of the common carotid artery was performed. Subsequently, the hemostatic material was immediately applied to the bleeding site, and the same pressure was applied. The wound was observed approximately every 10 seconds, and the hemostasis time was recorded immediately after the bleeding completely stopped. The hemostatic material was weighed before and after use, and the difference was the total blood loss. The experimental results showed that the hemostatic sponge of the present invention (Group a) firmly adhered to the carotid artery transection site. Compared with the other groups, Group a had the shortest hemostasis time (250 ± 22 seconds for Group a, while Groups b and c failed to achieve successful hemostasis after more than 5 minutes), and Group a had the least blood loss (1.6 ± 0.5 g for Group a, 2.8 ± 0.9 g and 3.2 ± 1.1 g for Group b and Group c, respectively, within 5 minutes). It can be seen that the hemostatic sponge of the present invention can be used for carotid artery hemostasis.
[0282] Hemostatic sponges composed of other different materials can also be used to stop carotid artery bleeding.
[0283] Example 35: Application of hemostatic sponge to cardiac hemostasis
[0284] A cardiac bleeding model of SD rats was selected and divided into three groups for cardiac hemostasis experiments, with 3 rats in each group: a hemostatic sponge group of the present invention (group a, the hemostatic sponge in Example 16, the component of which was selected from microgel PAA-2.1); a sponge control group of the present invention (group b, the control sponge in comparative Example 17, the component of which was selected from microgel PAA-2); and a commercial absorbable hemostatic gauze group (group c). The SD rats were anesthetized and fixed, and the chest hair was shaved. The chest cavity was opened and the heart was exposed, and the pericardium was removed using fine tweezers. A biopsy punch was used to create a 2 mm diameter injury on the left or right ventricular wall of the heart. Subsequently, the hemostatic material was immediately applied to the bleeding site and a certain amount of pressure was applied. The wound was observed approximately every 10 seconds, and the hemostasis time was recorded immediately after the bleeding completely stopped. The hemostatic material was weighed before and after use, and the difference was the total blood loss. For rats that failed to successfully stop bleeding within 5 minutes, the rats were euthanized by bleeding. Experimental result shows that hemostatic sponge of the present invention (a group) firmly adheres to ventricular wound, and compared with other groups, the hemostatic time of a group is the shortest (a group 80 ± 12s, b group 200 ± 35s, c group 3 rats all failed to stop bleeding within 5 minutes), and a group blood loss is minimum (a group 1.6 ± 0.3g, b group 2.0 ± 0.5g, c group blood loss within 5 minutes is 3.7 ± 0.8g). After operation, a group SD rats all (3) successfully survived, and b group and c group rats all died within 30 minutes during the experiment or after the experiment ended. It can be seen that the hemostatic sponge in the present invention can be applied to cardiac hemostasis.
[0285] Hemostatic sponges made of other different materials can also be used to stop cardiac bleeding.
[0286] Example 36: Application of hemostatic sponge in coronary artery hemostasis
[0287] A Bama pig coronary artery injury model was selected and divided into three groups for coronary artery hemostasis experiments, with 3 pigs in each group: the hemostatic sponge group of the present invention (group a, the hemostatic sponge in Example 16, the component is selected from microgel HA-2.2 (4.21)); the sponge control group of the present invention (group b, the control sponge in comparative example 17, the component is selected from microgel HA-2); the commercial absorbable hemostatic gauze group (group c). The Bama pig was anesthetized, the chest cavity was opened and the heart was exposed, the coronary artery was isolated and clamped on both sides, and a dissecting needle was used to puncture the middle of the clamped ends on both sides with a depth of 1 mm. Subsequently, the hemostatic material was immediately applied to the bleeding site and a certain amount of pressure was applied. The wound was observed approximately every 20 seconds, and the hemostasis time was recorded immediately after the bleeding completely stopped. The hemostatic material was weighed before and after use, and the difference was the total blood loss. The experimental results showed that group a had the shortest hemostasis time (155 ± 25 seconds for group a, 380 ± 110 seconds for group b, and unsuccessful hemostasis for more than 10 minutes for group c), and group a had the least blood loss (10 ± 3.5 g for group a, 23 ± 8.2 g for group b, and 45 ± 9.0 g for group c within 10 minutes). This shows that the hemostatic sponge of the present invention can be used for coronary artery hemostasis.
[0288] Hemostatic sponges composed of other different materials can also be used for coronary artery hemostasis.
[0289] Example 37: Application of hemostatic sponge to hemostasis of tooth extraction wound
[0290] A beagle dog tooth extraction wound model was selected and divided into four groups for a tooth extraction wound hemostasis experiment: the hemostatic sponge group of the present invention (group a, the hemostatic sponge in Example 16, the component of which is selected from microgel PEG-1.1); the sponge control group of the present invention (group b, the control sponge in comparative example 17, the component of which is selected from microgel PEG-1); the commercial absorbable gelatin sponge group (group c); and the blank group (group d). The beagle dogs were anesthetized and fixed, the oral cavity was disinfected, and four premolars were symmetrically extracted on each side, leaving a tooth extraction wound. For group a, group b and group c, the tooth extraction wound was filled with the hemostatic sponge of the present invention, the sponge control group and the commercial absorbable gelatin sponge, respectively. Group d did not take any measures, and each group had 4 wounds. Observe the hemostasis. If the bleeding stops, it proves that the hemostasis is complete, and record the hemostasis time. If there is still fluid bleeding, continue to apply pressure until the bleeding stops. Observe for secondary bleeding 0.5, 1, 6, and 12 hours after complete hemostasis. The experimental results showed that compared with the other groups, group a had the shortest hemostasis time (55±10s in group a, 105±21s in group b, 200±20s in group c, and 266±35s in group d) and no obvious secondary bleeding occurred in the later period. One tooth extraction wound in group b and group c each had secondary bleeding one hour after complete hemostasis, and two tooth extraction wounds in group d both had secondary bleeding 0.5 hours after complete hemostasis. It can be seen that the hemostatic sponge of the present invention can be used to stop bleeding in tooth extraction wounds.
[0291] Hemostatic sponges made of other different materials can also be used to stop bleeding from tooth extraction wounds.
[0292] Example 38: Application of hemostatic sponge to hemostasis of spine
[0293] A spinal cord injury model was used in SD rats, and three groups were divided into three groups, each with three rats: a hemostatic sponge group (Group a, the hemostatic sponge described in Example 16, composed of microgel CMC-1.3); a sponge control group (Group b, the control sponge described in Example 17, composed of microgel CMC-1); and a commercial absorbable gelatin sponge group (Group c). The SD rats were anesthetized and immobilized. The hair on their backs was shaved, and the skin and fascia were incised sequentially, centered around T13 and L1, to expose the muscles in the surgical area. Using ophthalmic scissors, the muscles and tendons connected to the spinous process were cut closely to one side, creating an incision from T12 to L2 and deep enough to reach the articular process. Approximately 0.5 cm outside this incision, another parallel incision was made, with a length and depth similar to the previous one. The muscle between the two incisions was removed, exposing three pairs of articular processes (T12 to T13, T13 to L1, and L1 to L2). Expose the lateral wall of the spinal canal and the intervertebral foramen once, cut the two lateral walls of the spinal canal in parallel, expose the spinal cord, and create a bleeding wound. Subsequently, the hemostatic material is immediately applied to the bleeding site, and a certain pressure is applied. The wound is observed approximately every 10 seconds, and the hemostasis time is recorded immediately after the bleeding stops completely. The hemostatic material is weighed before and after use, and the difference is the total blood loss. The experimental result shows that the hemostasis time of group a is the shortest (60 ± 10s for group a, 200 ± 24s for group b, and 250 ± 28s for group c), and the amount of blood loss in group a is the least (0.5 ± 0.2g for group a, 1.2 ± 0.3g for group b, and 1.8 ± 0.8g for group c). As can be seen, the hemostatic sponge in the present invention can be applied to spinal hemostasis.
[0294] Hemostatic sponges composed of other different materials can also be used for spinal hemostasis.
[0295] Example 39: Hemostatic sponge applied to uterine wall to stop bleeding
[0296] A uterine incision model was established in female New Zealand white rabbits aged 12 to 18 weeks. Three groups, each containing three rabbits, were used for uterine wall hemostasis experiments: a hemostatic sponge group (Group a, the hemostatic sponge described in Example 16, composed of the microgel HA-2.2 (4.21)); a sponge control group (Group b, the control sponge described in Example 17, composed of the microgel HA-2); and a commercial absorbable gelatin sponge group (Group c). After anesthesia and immobilization, the New Zealand white rabbits were shaved from the lower abdomen and disinfected with iodine and 75% ethanol. The abdominal skin was incised, the tissue was dissected layer by layer, and the pelvic cavity was opened, slowly exposing the uterus. A 2 cm long incision was made on the right side of the uterus, 3.5 cm from the vagina, to form a bleeding wound, which constituted the model. The hemostatic material was immediately applied to the bleeding site and covered with pre-weighed gauze. The wound was observed approximately every 10 seconds, and the hemostasis time was recorded immediately after complete cessation of bleeding. The hemostatic material and gauze were weighed before and after use, and the difference was the total blood loss. The experimental results showed that group a had the shortest hemostasis time (30 ± 6 s, 60 ± 12 s, and 50 ± 8 s, respectively) and the least blood loss (1.8 ± 0.2 g, 3.4 ± 0.3 g, and 2.5 ± 0.5 g, respectively). This suggests that the hemostatic sponge of the present invention can be used to stop bleeding in the uterine wall.
[0297] Hemostatic sponges made of other different materials can also be used to stop bleeding in the uterine wall.
[0298] Embodiment 40 to Embodiment 49:
[0299] Hemostatic application of the hemostatic powder of the present invention
[0300] Example 40: Hemostatic powder is used to stop bleeding in the liver
[0301] A liver transverse section trauma model was used in SD rats, and three groups, each containing three rats, were used for a liver hemostasis experiment: a hemostatic freeze-dried powder group (Group a, the hemostatic powder described in Example 18, whose components were selected from the microgel HA-2.1); a control powder group (Group b, the control powder described in Example 19, whose components were selected from the microgel HA-2); and commercial chitosan hemostatic granules (Group c). After anesthesia and immobilization, the SD rats were anesthetized and immobilized, their upper abdominal hair shaved, their abdominal cavity opened, and the liver was lifted and placed on a pre-weighed filter paper. A 10 mm diameter transverse section was then created on the liver to induce bleeding. Subsequently, a certain amount of hemostatic material from each group was sprayed onto the transverse section. Blood loss was measured by weight gain of the filter paper and the material, and hemostasis time was recorded using a timer. In this example, photographs of the hemostatic powder of the present invention (Group a), the control powder (Group b), and the commercial chitosan hemostatic granules (Group c) applied to the liver for hemostasis are shown in Figure 8. The experimental results showed that group a had the least blood loss (group a 0.1 ± 0.05 g, group b 0.8 ± 0.1 g, group c 0.5 ± 0.2 g), and the shortest hemostasis time (group a 25 ± 5 s, group b 85 ± 12 s, group c 40 ± 10 s). This shows that the hemostatic powder of the present invention can be used to stop liver bleeding.
[0302] Hemostatic powders made of other different materials can also be used to stop liver bleeding.
[0303] Example 41: Hemostatic powder is used to stop bleeding in the spleen
[0304] A spleen incision bleeding model of SD rats was selected, and the spleen hemostasis experiment was carried out in three groups, with 3 rats in each group: the hemostatic powder group of the present invention (group a, the hemostatic powder in Example 18, the component of which is selected from microgel HA-2.2 (4.21)); the control powder group of the present invention (group b, the control powder in comparative example 19, the component of which is selected from microgel HA-2); and commercial chitosan hemostatic granules (group c). After the SD rats were anesthetized and fixed, an incision was made in the midline of the abdomen, the abdominal cavity was opened, and the spleen was exposed. An incision (8 mm wide and 2 mm deep) was made in the spleen to cause spleen injury, and bleeding continued for 20 seconds. Subsequently, different groups of hemostatic materials were sprinkled on the bleeding area and covered with gauze for continuous pressure for 60 seconds. The amount of blood loss was measured by the weight gain of the gauze and the material, and the hemostasis time was recorded by a timer. The experimental results showed that group a had the shortest hemostasis time (80 ± 12 seconds in group a, all three in group b failed to stop bleeding within 5 minutes, and 180 ± 20 seconds in group c), and group a had the least blood loss (0.9 ± 0.2 g in group a, 2.2 ± 0.8 g in group b within 5 minutes, and 1.3 ± 0.5 g in group c). This shows that the hemostatic powder of the present invention can be used to stop spleen bleeding.
[0305] Hemostatic powders made of other different materials can also be used to stop spleen bleeding.
[0306] Example 42: Application of hemostatic powder to stop bleeding in veins
[0307] A tail-mutilation model was used in SD rats, and three groups of rats were divided into three groups for tail vein hemostasis experiments, each with three rats: the hemostatic powder group of the present invention (Group a, the hemostatic powder described in Example 18, composed of microgel CMC-1.1); the control powder group of the present invention (Group b, the control powder described in Comparative Example 19, composed of microgel CMC-1); and commercial chitosan hemostatic granules (Group c). After anesthesia, weighed filter paper was placed under the tail of the rat, and the tail was cut with scissors to induce bleeding. Subsequently, the hemostatic materials from the different groups were sprinkled on the bleeding area and covered with gauze for continuous pressure. Blood loss was measured by weight gain on the filter paper, and hemostasis time was recorded using a timer. The experimental results showed that Group a had the least blood loss (Group a 0.4±0.05g, Group b 1.2±0.5g, Group c 0.9±0.2g) and the shortest hemostasis time (Group a 40±5s, Group b 90±15s, Group c 75±10s). It can be seen that the hemostatic powder of the present invention can be used for venous hemostasis.
[0308] Hemostatic powders made of other different materials can also be used to stop venous bleeding.
[0309] Example 43: Application of hemostatic powder to stop bleeding in superficial arteries
[0310] A New Zealand white rabbit ear artery bleeding model was used to conduct a surface artery hemostasis experiment in three groups, each consisting of three rabbits: the hemostatic powder of the present invention (Group a, the hemostatic powder of Example 18, composed of microgel CMC-1.2); the control powder of the present invention (Group b, the control powder of Comparative Example 19, composed of microgel CMC-1); and commercial chitosan hemostatic granules (Group c). After the rabbits were anesthetized, weighed filter paper was placed beneath their ears. The rabbit ear artery was punctured with a needle, and then the different groups of hemostatic materials were applied to the bleeding site. Blood loss was measured by weight gain of the filter paper, and hemostasis time was recorded using a timer. During the experiment, Group a had the shortest hemostasis time (Group a: 23±8 s, Group b: 65±15 s, Group c: 35±10 s) and the least blood loss (Group a: 0.8±0.2 g, Group b: 3.5±0.8 g, Group c: 1.2±0.4 g). This demonstrates that the hemostatic powder of the present invention can be used for surface artery hemostasis.
[0311] Hemostatic powders composed of other different materials can also be used to stop bleeding in superficial arteries.
[0312] Example 44: Hemostatic powder is used to stop bleeding in superficial veins
[0313] A New Zealand white rabbit ear vein bleeding model was used to conduct a surface venous hemostasis experiment in three groups, each consisting of three rabbits: the hemostatic powder of the present invention (Group a, the hemostatic powder of Example 18, composed of microgel CMC-1.3); the control powder of the present invention (Group b, the control powder of Comparative Example 19, composed of microgel CMC-1); and commercial chitosan hemostatic granules (Group c). After the rabbits were anesthetized, weighed filter paper was placed under their ears. The ear vein was punctured with a needle, and the different hemostatic materials were then applied to the bleeding site. The hemostatic time was recorded using a timer. The experimental results showed that Group a had the shortest hemostasis time (40±5s, 80±15s, and 45±8s) and the least blood loss (1.0±0.2g, 3.4±2.0g, and 1.2±0.4g). This indicates that the hemostatic powder of the present invention can be used for surface venous hemostasis.
[0314] Hemostatic powders made of other different materials can also be used to stop bleeding in surface veins.
[0315] Example 45: Application of hemostatic powder to intestinal hemostasis
[0316] A SD rat cecal bleeding model was used, and intestinal hemostasis experiments were conducted in four groups, each with three rats: the hemostatic powder group of the present invention (Group a, the hemostatic powder described in Example 18, whose components were selected from microgel CMC-1.2); the control powder group of the present invention (Group b, the control powder described in Comparative Example 19, whose components were selected from microgel CMC-1); commercial chitosan hemostatic granules (Group c); and a blank group (Group d). After anesthesia, the SD rats were opened, and the cecum was rubbed until a bleeding surface was obtained. Subsequently, the different groups of hemostatic materials were placed on the bleeding surface of the cecum. Blood loss was measured by the increment of the hemostatic material, and the hemostasis time was recorded using a counter. After the experiment, blood clots from the cecum and hemostatic materials were collected, and their absorbance at 400 nm was measured using a hemoglobin analysis kit to assess the hemostatic effect. In this example, the hemoglobin content of the blood clots collected from the hemostatic powder of the present invention (Group a), the control powder (Group b), the commercial chitosan hemostatic powder (Group c), and the blank group (Group d) is shown in Figure 9. The experimental results showed that group a had the least blood loss (group a 0.2±0.1g, group b 0.4±0.12g, group c 0.35±0.1g, group d 0.8±0.2g), and the shortest hemostasis time (group a 10±4s, group b 25±5s, group c 20±2s, group d 75±15s). This shows that the hemostatic powder of the present invention can be used for intestinal hemostasis.
[0317] Hemostatic powders made of other different materials can also be used to stop intestinal bleeding.
[0318] Example 46: Hemostatic powder is applied to the skin to stop bleeding
[0319] A Bama pig back skin tear and bleeding model was used to conduct a back skin hemostasis experiment in three groups, each with four wounds: the hemostatic powder group of the present invention (Group a, the hemostatic powder described in Example 18, whose component was selected from microgel Alg-1.2); the control powder group of the present invention (Group b, the control powder described in Example 19, whose component was selected from microgel Alg-1); and commercial chitosan hemostatic granules (Group c). Two-month-old male Bama miniature pigs (weighing 1.6-1.8 kg) were anesthetized and their back hair shaved. Four 2 cm long and 1 cm deep linear incisions were made on the pig's back with a scalpel to obtain bleeding wounds. Subsequently, the hemostatic material was immediately applied to the bleeding area and covered with gauze, applying a certain amount of pressure. The wound was observed approximately every 10 seconds, and the hemostasis time was recorded immediately after bleeding completely stopped. The hemostatic material and gauze were weighed before and after use, and the difference was the total blood loss. The experimental results showed that group a had the shortest hemostasis time (40 ± 10 seconds, 70 ± 14 seconds, and 55 ± 12 seconds, respectively) and the least blood loss (2.5 ± 0.8 grams, 4.0 ± 1.2 grams, and 3.7 ± 1.5 grams, respectively). Compared to the other groups, group a's hemostatic powder formed a gel layer with the blood at the bleeding wound surface. This suggests that the hemostatic powder of the present invention can be used to stop bleeding on the skin.
[0320] Hemostatic powders made of other different materials can also be used to stop bleeding on the skin.
[0321] Example 47: Application of hemostatic powder to oral mucosal bleeding
[0322] A SD rat hard palate mucosal injury model was used, and oral mucosal hemostasis experiments were conducted in three groups, each with three rats: a hemostatic powder group according to the present invention (Group a, the hemostatic powder described in Example 18, whose component was selected from microgel Alg-1.1); a control powder group according to the present invention (Group b, the control powder described in Example 19, whose component was selected from microgel Alg-1); and commercial chitosan hemostatic granules (Group c). After anesthetizing the SD rats, the rats' mouths were propped open with an eyelid device, and the palatal mucosa was disinfected with iodine and 75% ethanol. A disposable biopsy punch (3 mm diameter) was then used to create a circular, full-thickness hard palate mucosal defect in the middle of the rats' oral palate, creating a bleeding wound. Subsequently, a hemostatic material was immediately applied to the bleeding area, covered with gauze, and pressure was applied. The wound was observed approximately every 10 seconds, and the hemostasis time was recorded immediately after bleeding completely ceased. The hemostatic material and gauze were weighed before and after use, and the difference was the total blood loss. The experimental results showed that group a had the shortest hemostasis time (10±2s, 20±9s, and 20±5s), and the least blood loss (0.1±0.02g, 0.4±0.03g, and 0.3±0.02g, respectively). This indicates that the hemostatic powder of the present invention can be used to stop bleeding in the oral mucosa.
[0323] Hemostatic powders composed of other different materials can also be used to stop bleeding in the oral mucosa.
[0324] Example 48: Application of hemostatic powder to stop bleeding during hysterectomy
[0325] A hysterectomy model was established using female SD rats aged 6 to 8 weeks. Three groups, each containing three rats, were used for intraoperative hemostasis experiments: the hemostatic powder group of the present invention (Group a, the hemostatic powder described in Example 18, composed of the microgel CMS-1.1); the control powder group of the present invention (Group b, the control powder described in Example 19, composed of the microgel CMS-1); and the Arista absorbable hemostatic microspheres (Group c). After anesthesia and immobilization, the SD rats were shaved from the lower abdomen and disinfected with iodine and 75% ethanol. A longitudinal incision was made in the abdominal skin 2–3 cm above the pubic symphysis. The tissue was dissected layer by layer, and the abdominal cavity was opened. The rat's Y-shaped uterus was slowly removed, and incisions were made in each of the left and right uterine horns. Straight ophthalmic scissors were used to make a 2.5 cm longitudinal incision in the center of the midsection of the uterus, leaving the mesometrium intact. Curved ophthalmic scissors were then used perpendicular to the longitudinal incision to excise the endometrium, site by site, completely removing the entire endometrium. The depth was controlled to avoid breaching the uterine serosa, ensuring its integrity. Excision was performed until the uterine wall was thin and translucent. Following endometrial excision, hemostatic material was immediately applied to the bleeding area and covered with gauze, applying pressure. The wound surface was observed approximately every 10 seconds, and the time to hemostasis was recorded once bleeding had completely ceased. The hemostatic material and gauze were weighed before and after use, and the difference was used to determine the total blood loss. The experimental results showed that group a had the shortest hemostasis time (30±6s, 60±12s, and 50±8s) and the least blood loss (0.2±0.05g, 0.4±0.13g, and 0.35±0.08g, respectively). This suggests that the hemostatic powder of the present invention can be used to stop bleeding during hysterectomy.
[0326] Hemostatic powders made of other different materials can also be used to stop bleeding during hysterectomy.
[0327] Example 49: Application of hemostatic powder to stop bleeding in the spine
[0328] A spinal cord injury model was used in SD rats, and three groups of three rats were assigned to undergo spinal hemostasis experiments: the hemostatic powder of the present invention (Group a, the hemostatic powder described in Example 18, composed of microgel CMS-1.2); the control powder of the present invention (Group b, the control powder described in Example 19, composed of microgel CMS-1); and the Arista absorbable hemostatic microspheres (Group c). The SD rats were anesthetized and immobilized. The hair on the back was shaved, and the skin and fascia were incised sequentially, centered around T13 and L1, to expose the muscles in the surgical area. Using ophthalmic scissors, the muscles and tendons connected to the spinous process were cut closely to create an incision on one side. The incision was preferably from T12 to L2 and deep enough to reach the articular process. Approximately 0.5 cm lateral to this incision, another parallel incision was made, of approximately the same length and depth as the previous one. The muscle between the two incisions was removed, exposing three pairs of articular processes (T12 to T13, T13 to L1, and L1 to L2). Once the lateral wall of the spinal canal and the intervertebral foramen are exposed, the two lateral walls of the spinal canal are cut in parallel, the spinal cord is exposed, and a bleeding wound is created. Subsequently, each group of hemostatic materials is immediately sprinkled on the bleeding site and the wound is continuously observed. The hemostasis time is recorded immediately after the bleeding stops completely. The hemostatic material is weighed before and after use, and the difference is the total blood loss. The experimental result shows that the hemostasis time of group a is the shortest (60 ± 8s for group a, 120 ± 16s for group b, and 85 ± 15s for group c), and the blood loss of group a is the least (0.3 ± 0.1g for group a, 1.0 ± 0.4g for group b, and 0.7 ± 0.25g for group c). As can be seen, the hemostatic powder in the present invention can be applied to spinal hemostasis.
[0329] Hemostatic powders composed of other different materials can also be used to stop spinal bleeding.
[0330] Embodiment 50 to Embodiment 55:
[0331] Hemostatic application of the mobile hemostatic agent of the present invention
[0332] Example 50: Application of mobile hemostatic agent in non-compression hemostasis of penetrating wounds
[0333] A New Zealand white rabbit liver perforation model was selected and divided into three groups for non-compressive penetrating wound hemostasis experiments, with 3 rabbits in each group: the mobile hemostat group of the present invention (group a, the mobile hemostat in Example 20, the component of which was selected from microgel HA-2.2 (4.21)); the control fluid group (group b, the control fluid in comparative Example 21, the component of which was selected from microgel HA-2); and the commercial fluid gelatin group (group c). After anesthetizing the New Zealand white rabbits, their abdominal cavity was opened, the liver was lifted and placed on a pre-weighed gauze, and then a penetrating wound with a diameter of 6 mm was established on the liver to cause bleeding. Subsequently, the hemostatic materials of different groups were injected into the penetrating wound. The amount of blood loss was measured by the weight gain of the hemostatic material and the gauze, and the hemostasis time was recorded by a timer. In this example, photos of the mobile hemostat of the present invention (group a), the control fluid (group b) and the commercial fluid gelatin (group c) applied to non-compressive hemostasis of penetrating wounds are shown in Figure 10. The experimental results showed that group a had the least blood loss (2.6 ± 0.4 g, 9.0 ± 2.1 g, and 4.5 ± 0.8 g), and the shortest hemostasis time (25 ± 2 s, 135 ± 21 s, and 85 ± 14 s, respectively). This suggests that the flowable hemostatic agent of the present invention can be used for non-compressive hemostasis of penetrating wounds.
[0334] Other mobile hemostatic agents composed of different materials can also be used for non-compression hemostasis of penetrating wounds.
[0335] Example 51: Application of mobile hemostatic agent in digestive tract hemostasis under endoscopy
[0336] A Bama pig acute upper gastrointestinal arterial bleeding model was selected and the gastrointestinal hemostasis experiment was performed in three groups, with 2 pigs in each group: the mobile hemostatic agent group of the present invention (group a, the mobile hemostatic agent in Example 20, the component of which was selected from microgel CMC-1.2); the control fluid group (group b, the control fluid in comparative Example 21, the component of which was selected from microgel CMC-1); and the commercial fluid gelatin group (group c). Adult female Bama pigs (weighing 20-25 kg) were anesthetized and cannulated in the right femoral artery to monitor blood pressure. Subsequently, within 5 minutes, the baseline blood pressure (systolic pressure) of all animals was monitored and adjusted to 90-100 mm Hg, and then heparin (10 mg / kg) was administered intravenously to achieve systemic heparinization. Under endoscopy, the mucosa was peeled off and the submucosal pulsating artery in the stomach was identified. The artery was then cut with an endoscopic knife to induce acute upper gastrointestinal bleeding, and natural bleeding was maintained for 4 minutes. The mobile hemostatic agent of the present invention (group a), control fluid (group b) or commercial fluid gelatin (group c) is applied to the bleeding site through the endoscopic biopsy channel via a catheter. The bleeding site is continuously observed by endoscope within 30 minutes. Unless hemostasis is achieved, the hemostasis procedure is repeated, and the hemostasis time and the quality of the materials used are recorded. The experimental results show that compared with other groups, the hemostasis time of group a is the shortest (group a 3 ± 1.0 min, group c 13 ± 4.0 min, group b 12 ± 3.5 min), and the material used in group a is the least (group a 8 ± 2.5 g, group b 15 ± 4.5 g, group c 16 ± 5 g). It can be seen that the mobile hemostatic agent in the present invention can be applied to endoscopic digestive tract hemostasis.
[0337] Other mobile hemostatic agents composed of different materials can also be used for endoscopic gastrointestinal hemostasis.
[0338] Example 52: Application of mobile hemostatic agent for hemostasis during and after laparoscopic partial nephrectomy
[0339] A Bama pig partial nephrectomy model was selected and the subjects were divided into three groups for hemostasis experiments during and after partial nephrectomy, with 2 pigs in each group: the mobile hemostat group of the present invention (group a, the mobile hemostat in Example 20, the component of which was selected from microgel HA-); the control fluid group (group b, the control fluid in comparative Example 21, the component of which was selected from microgel HA-2); and the commercial fluid gelatin group (group c). Adult female Bama pigs (weighing 20-25 kg) were anesthetized and cannulated in the right femoral artery to monitor blood pressure. A pneumoperitoneum needle was inserted through a pararectal incision, and a one-third partial nephrectomy was performed under laparoscopy. The mobile hemostat of the present invention (group a), the fluid control group (group b), or the commercial fluid gelatin (group c) was applied to the bleeding site through the endoscopic biopsy channel via a catheter. The bleeding site was continuously observed using an endoscope within 30 minutes. Unless hemostasis was achieved, the hemostasis procedure was repeated, and the hemostasis time and material quality were recorded. The experimental results showed that Group A had the shortest hemostasis time (15 ± 3.5 minutes for Group A, while Groups B and C failed to achieve hemostasis within 60 minutes) and used the least amount of material (12 ± 3 g for Group A, while Groups B and C both used more than 30 g within 60 minutes). This indicates that the mobile hemostatic agent of the present invention can be used for hemostasis during and after laparoscopic partial nephrectomy.
[0340] Other mobile hemostatic agents composed of different materials can also be used for hemostasis during and after laparoscopic partial nephrectomy.
[0341] Example 53: Application of mobile hemostatic agent in hemostasis of narrow cavities
[0342] A New Zealand white rabbit cochlear bleeding model was selected, and the rabbits were divided into three groups for a narrow cavity hemostasis experiment, with 3 rabbits in each group: the flow hemostatic agent group of the present invention (Group a, the flow hemostatic agent in Example 20, the component of which was selected from microgel Alg-1.3); the control fluid group (Group b, the control fluid in comparative Example 21, the component of which was selected from microgel Alg-1); and the commercial fluid gelatin group (Group c). After the rabbits were anesthetized, they were scratched with a surgical blade at the cochlea to create a bleeding wound. Subsequently, the hemostatic materials of different groups were injected into the cochlea through a syringe. The hemostasis time was recorded by a timer. The experimental results showed that the hemostasis time of Group a was the shortest (Group a 20±5s, Group b 85±14s, Group c 45±9s). It can be seen that the flow hemostatic agent of the present invention can be used for hemostasis in narrow cavities.
[0343] Other mobile hemostatic agents composed of different materials can also be used to stop bleeding in narrow cavities.
[0344] Example 54: Application of mobile hemostatic agent to spinal hemostasis
[0345] A spinal cord injury model was used in SD rats, and three groups of three rats were used for spinal hemostasis experiments: the mobile hemostat of the present invention (Group a, the mobile hemostat described in Example 20, whose component was selected from microgel HA-2.1); the control fluid group (Group b, the control fluid described in Example 21, whose component was selected from microgel HA-2); and the commercial fluid gelatin group (Group c). The SD rats were anesthetized and immobilized. The hair on the back was shaved, and the skin and fascia were incised sequentially, centered around T13 and L1, to expose the muscles in the surgical area. Using ophthalmic scissors, the muscles and tendons connected to the spinous process were cut closely to one side, creating an incision from T12 to L2 and deep enough to reach the articular process. Approximately 0.5 cm outside this incision, another parallel incision was made, with a length and depth similar to the previous one. The muscle between the two incisions was removed, exposing three pairs of articular processes (T12 to T13, T13 to L1, and L1 to L2). The lateral walls of the spinal canal and the intervertebral foramen are exposed at one time, and the lateral walls of the spinal canal are cut in parallel to expose the spinal cord and create a bleeding wound. Subsequently, different groups of hemostatic materials are injected into the bleeding wound through a syringe. The wound is observed approximately every 10 seconds, and the hemostasis time is recorded immediately after the bleeding stops completely; if the bleeding does not stop, the hemostatic material is continued to be injected. The bleeding from the wound is collected with gauze and weighed to record the amount of blood loss. The experimental results show that the hemostasis time of group a is the shortest (30±6s for group a, 105±21s for group b, and 60±12s for group c), and the amount of blood loss in group a is the least (0.8±0.2g for group a, 1.2±0.3g for group b, and 1.0±0.3g for group c). It can be seen that the mobile hemostatic agent in the present invention can be applied to spinal hemostasis.
[0346] Other mobile hemostatic agents composed of different materials can also be used for spinal hemostasis.
[0347] Example 55: Application of mobile hemostatic agent in percutaneous hemostasis
[0348] A percutaneous puncture defect model was used in Bama pigs. Percutaneous hemostasis experiments were performed in three groups, each with three puncture defects: the flowable hemostat of the present invention (Group a, the flowable hemostat of Example 20, whose components were selected from the microgel CMS-1.2); the control fluid group (Group b, the control fluid of Example 21, whose components were selected from the microgel CMS-1); and the commercial fluid gelatin group (Group c). Adult female Bama pigs (weighing 20-25 kg) were anesthetized, and a midline abdominal incision was made. The abdominal cavity was gradually exposed and the spleen was continuously moistened with saline-soaked gauze. Starting at the distal end of the spleen, a 6 mm diameter surgical biopsy punch was used to create a similarly sized bleeding defect, and the right femoral artery was cannulated to monitor blood pressure. The flowable hemostat of the present invention (Group a), the control fluid group (Group b), or the commercial fluid gelatin (Group c) was applied to the bleeding site via syringe. Hemostasis was continuously observed. The hemostasis procedure was repeated unless hemostasis was achieved, and the time to hemostasis was recorded. In this example, photographs of the mobile hemostatic agent (Group a), control fluid (Group b), and commercial fluid gelatin (Group c) used for percutaneous hemostasis are shown in Figure 11. The experimental results showed that Group a quickly blocked the bleeding site, while blood in Groups b and c continued to seep out from the gap between the material and tissue. Compared to the other groups, Group a had the shortest hemostasis time (55 ± 10 seconds for Group a, 155 ± 25 seconds for Group b, and 90 ± 12 seconds for Group c). This demonstrates that the mobile hemostatic agent of the present invention can be used for percutaneous hemostasis.
[0349] Other mobile hemostatic agents composed of different materials can also be used for percutaneous hemostasis.
[0350] Embodiment 56 to Embodiment 59:
[0351] Preparation and application of composite sponge of the present invention
[0352] Example 56: Preparation of composite sponge
[0353] Taking the o-phthalaldehyde group-modified hyaluronic acid microgel prepared in Example 9 (i.e., HA-2.2 (4.21)) and the o-phthalaldehyde group-free hyaluronic acid microgel prepared in Example 2 (i.e., HA-2) as examples, the two microgels were fully dispersed in deionized water to obtain a suspension with a solid content of 0.5% to 1.5% (w / v). The suspensions were spread in molds (constituting the o-phthalaldehyde group-modified a side and the unmodified b side, respectively), frozen at -20°C for 6 hours, and then freeze-dried at -60°C for 48 hours to obtain a composite sponge.
[0354] Example 57: Composite sponge used to prevent adhesion after surgery
[0355] A postoperative intraperitoneal adhesion model involving scraping the liver surface of SD rats was used. Two groups, each containing three rats, were used for a postoperative intraperitoneal adhesion prevention experiment: the composite sponge described in Example 56 (Group a) and a blank control group (Group b). After anesthesia, the SD rats were opened and the liver surface rubbed until a bleeding wound surface was obtained. The sponge in Group a was placed against the liver surface with surface a pressed evenly for 1 minute to adhere to the surface, and surface b was moistened with saline. Group b received no treatment. Fourteen days after surgery, the SD rats' abdominal cavities were opened again, and the presence of intraperitoneal adhesions was recorded. The experimental results showed that of the three rats in Group a, two showed no adhesions, one had a mild adhesion that could be easily removed with forceps, and all three rats in Group b exhibited significant adhesions. Subsequently, tissue sections were sectioned and H&E stained for histological analysis. The H&E staining results for the composite sponge (Group a) and the blank control group (Group b) in this example are shown in Figure 12, where I represents the small intestine, L represents the liver, and S represents the composite sponge material. The staining results showed that the liver tissue in group a had a protective layer of composite sponge material and had no obvious adhesion to other organs or the abdominal wall, while the liver tissue in group b had obvious adhesion to the small intestine. This shows that the composite sponge of the present invention can be used to prevent postoperative adhesions.
[0356] Composite sponges made of other different materials can also be used to prevent adhesions after surgery.
[0357] Example 58: Application of composite sponge in blocking lung parenchymal air leakage
[0358] A lung parenchymal air leakage model was used in New Zealand white rabbits. Two groups were used for the lung parenchymal air leakage blocking experiment, with 3 rabbits in each group: the composite sponge described in Example 56 (group a) and a blank control group (group b). The New Zealand white rabbits were injected with 1% sodium pentobarbital at a dose of 3 mL / kg through the ear vein. The rabbits were intubated under general anesthesia and assisted with ventilation (VT 80 mL, R 30 bpm). Subsequently, a thoracotomy was performed, and the marginal tissue of the lung lobe was resected. The wound surface was approximately 1 cm 2 , at least one bronchial stump with a diameter of about 1 mm can be seen. The experimental group evenly pressed the a side of the composite sponge in Example 48 to the part of the lung defect, adhered it to the wound surface, closed the chest layer by layer, removed the residual air, and fully re-expanded the lung. The wound surface of the control group was not treated and the chest was directly closed. 14 days after the operation, the surgical side was observed for atelectasis and pleural effusion. The experimental results showed that the white rabbits in group b died of respiratory failure due to continuous air leakage within 4 hours after the operation, and the white rabbits in group a survived well. After 14 days, the chest was opened to observe the lung wound surface. The wound healing was good, no obvious air leakage was observed, and there was no atelectasis, ascites, etc. It can be seen that the composite sponge in the present invention can be used for sealing lung parenchymal air leakage.
[0359] Composite sponges composed of other different materials can also be used to seal lung parenchymal air leaks.
[0360] Example 59: Application of composite sponge in blocking intestinal leakage
[0361] A New Zealand rabbit intestinal leakage model was used to conduct a cecal leakage blocking experiment in two groups, with 3 rabbits in each group: the composite sponge in Example 56 (Group a) and a blank control group (Group b). After the New Zealand rabbits were anesthetized, their abdominal cavities were opened and a leakage model was created in their cecum. Group a placed the a side of the composite sponge close to the wound at the leakage site, pressed evenly for 1 minute, adhered it to the abdominal wall, and moistened the b side with normal saline; Group b did not perform any treatment after the wound was created. One rabbit in Group b died 2 days after surgery, and the other two rabbits died 3 days after surgery. The cecum was dissected and observed, and both had obvious leakage and severe inflammation. All rabbits in Group a survived for 4 weeks after surgery. After the New Zealand rabbits were euthanized in the fourth week, the cecum was extracted for observation, and no leakage or local inflammation was found. It can be seen that the composite sponge in the present invention can be used for intestinal leakage blocking.
[0362] Composite sponges composed of other different materials can also be used to block intestinal leakage.
[0363] The above Examples 27 to 39 provide the application of the hemostatic sponge of the present invention with a specific formula in a variety of hemostatic scenarios. These hemostatic applications mainly utilize the characteristics of the hemostatic sponge of the present invention that can react efficiently with blood and its tissue adhesion properties. According to the records of Example 22, Example 24 and Example 25, it can be seen that the hemostatic performance of the hemostatic sponge provided by the embodiment of the present invention is positively correlated with the modified o-phthalaldehyde group, and the hemostatic sponges of multiple formulas in the embodiments of the present invention all have good tissue adhesion and good mechanical properties after absorbing blood. Therefore, the hemostatic sponges prepared based on the microgels modified with multiple o-phthalaldehyde groups provided by the present invention can be used in a variety of hemostatic scenarios. The above Examples 40 to 49 and Examples 50 to 55 respectively provide the application of hemostatic powders and mobile hemostats with specific formulas in a variety of hemostatic scenarios. Similarly, it can be obtained that the hemostatic powders or mobile hemostats prepared based on the microgels modified with multiple o-phthalaldehyde groups provided by the present invention can be used in a variety of hemostatic scenarios.
[0364] The above Examples 56 to 59 provide the preparation of composite sponges with specific formulations and their corresponding biomedical applications. Based on the description of this application, those skilled in the art can prepare composite sponges from the o-phthalaldehyde group-modified or unmodified microgels provided by the present invention as needed. Similarly, based on the description of this application, those skilled in the art can prepare composite sponges from the o-phthalaldehyde group-modified or unmodified microgels provided by the present invention as needed for applications such as postoperative adhesion prevention, tissue air leakage blocking, and tissue fluid leakage blocking.
[0365] The above description of the embodiments is intended to facilitate understanding and use of the invention by those skilled in the art. It will be apparent that those skilled in the art can readily make various modifications to these embodiments and apply the general principles described herein to other embodiments without requiring inventive effort. Therefore, the present invention is not limited to the above-described embodiments. Improvements and modifications made by those skilled in the art based on the disclosure of the present invention, without departing from the scope of the present invention, should be within the scope of protection of the present invention.
Claims
1. A microgel modified with o-phthalaldehyde groups, characterized in that: The chemical structure of the microgel modified with o-phthalaldehyde groups is shown in Formula 1: In Formula 1, MG represents microgel, which is a gel microparticle formed by cross-linking water-soluble or hydrophilic polymers, with a particle size of 5 mesh to 1000 mesh and a solid content of 0.01% to 50%; In formula 1, n ≥ 2, that is, the average number of o-phthalaldehyde functional groups on a single microgel is greater than or equal to 2; In Formula 1, the o-phthalaldehyde group is connected to the microgel via a covalent bond.
2. The o-phthalaldehyde group-modified microgel according to claim 1, characterized in that: The water-soluble or hydrophilic polymer forming the microgel is selected from water-soluble or hydrophilic natural polymers or water-soluble or hydrophilic synthetic polymers; The water-soluble or hydrophilic natural polymer is selected from one or more of hyaluronic acid, alginic acid, dextran, chondroitin sulfate, heparin, polyglutamic acid, tragacanth gum, xanthan gum, agarose, gellan gum, guar gum, gum arabic, locust bean gum, starch, starch hydrolysate, starch derivative, cellulose or cellulose derivative; The water-soluble or hydrophilic synthetic polymer refers to an artificial synthetic polymer containing a hydrophilic group, selected from homopolymers or copolymers of (meth)acrylic acid and its esters, homopolymers or copolymers of (meth)acrylamides, homopolymers or copolymers of polyvinyl alcohol, homopolymers or copolymers of polyethylene glycol, and homopolymers or copolymers of vinyl pyrrolidone; Preferably, the homopolymer or copolymer of (meth)acrylic acid and its esters is selected from the group consisting of homopolymer or copolymer of (meth)acrylic acid, homopolymer or copolymer of hydroxyethyl (meth)acrylate, homopolymer or copolymer of hydroxypropyl (meth)acrylate, homopolymer or copolymer of glucose (meth)acrylate, homopolymer or copolymer of polyethylene glycol (meth)acrylate and copolymer of polyethylene glycol methyl ether (meth)acrylate; Preferably, the homopolymer or copolymer of (meth)acrylamide is selected from copolymers of (meth)acrylamide, copolymers of N,N-dimethylacrylamide, homopolymers or copolymers of N-hydroxymethylacrylamide, A homopolymer or copolymer of N-hydroxyethyl(meth)acrylamide, a homopolymer or copolymer of N-hydroxypropyl(meth)acrylamide, a copolymer of N-isopropylacrylamide, or a copolymer of 2-acrylamido-2-methylpropanesulfonic acid; Herein, (meth)acrylic acid refers to acrylic acid or methacrylic acid; and (meth)acrylamide refers to acrylamide or methacrylamide.
3. The o-phthalaldehyde group-modified microgel according to claim 2, characterized in that: The water-soluble or hydrophilic polymer forming the microgel is selected from one or more of hyaluronic acid, alginic acid, starch, carboxymethyl starch, carboxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, polyglutamic acid, polyacrylic acid or carboxylated polyethylene glycol.
4. The o-phthalaldehyde group-modified microgel according to claim 1, characterized in that: The chemical structure of the microgel modified with o-phthalaldehyde groups is selected from one of the following structures: In Formula 1-1 to Formula 1-12, MG represents microgel, Among them, 1≤r≤20, 1≤s≤20, 1≤t≤50, n≥2, preferably, 1≤r≤6, 1≤s≤10, 1≤t≤30, n≥2.
5. The method for preparing a microgel modified with o-phthalaldehyde groups according to any one of claims 1 to 4, characterized in that: The steps include: (1) preparing microgels; (2) covalently linking the aldehyde-preprotected o-phthalaldehyde precursor derivative to the active groups on the microgel to prepare the o-phthalaldehyde precursor derivative-modified microgel; (3) Deprotecting the aldehyde groups to obtain microgels modified with o-phthalaldehyde groups.
6. The method for preparing the microgel modified with o-phthalaldehyde groups according to claim 5, characterized in that: The method for preparing the microgel in step (1) comprises: 1) preparing the microgel by directly cross-linking a water-soluble or hydrophilic polymer; or, 2) preparing the microgel by polymerizing and cross-linking a monomer.
7. The method for preparing the microgel modified with o-phthalaldehyde groups according to claim 6, characterized in that: The preparation of microgels by direct cross-linking of water-soluble or hydrophilic polymers refers to: The water-soluble or hydrophilic polymer is cross-linked into a gel by a specific cross-linking method, and then physically broken by mechanical force and sieved through sieves of different sizes to obtain microgels with different particle size distributions; or, Water-soluble or hydrophilic polymers are prepared into an oil-water emulsion under the action of an emulsifier, and then cross-linked by a specific cross-linking method to obtain microgels with a certain particle size.
8. The method for preparing the microgel modified with o-phthalaldehyde groups according to claim 7, characterized in that: The specific cross-linking method is chemical cross-linking; The chemical crosslinking is selected from the following three methods: Based on multifunctional acrylic or methacrylic acid modified polymers cross-linked by free radical chain polymerization; or, Covalent crosslinking based on multifunctional crosslinking agents with a functionality ≥ 2 in the presence or absence of a catalyst; or In the presence or absence of a catalyst, the polymer chain itself contains two or more reactive functional groups that undergo condensation crosslinking.
9. The method for preparing the microgel modified with o-phthalaldehyde groups according to claim 8, characterized in that: The multifunctional crosslinking agent is selected from glutaraldehyde, polyamine, multifunctional epoxy, epichlorohydrin, divinyl sulfone, phosphorus oxychloride or sodium trimetaphosphate.
10. The method for preparing the microgel modified with o-phthalaldehyde groups according to claim 9, characterized in that: The multifunctional epoxy is selected from 1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, ethylene glycol diglycidyl ether, neopentyl glycol diglycidyl ether, glycerol triglycidyl ether, trimethylolpropane triglycidyl ether, polyethylene glycol diglycidyl ether or polypropylene glycol diglycidyl ether; The polyamine refers to a multifunctional crosslinking agent containing one or more functional groups of primary amine, hydrazine, hydrazide, and hydroxylamine, preferably adipic acid dihydrazide or hexamethylenediamine.
11. The method for preparing the microgel modified with o-phthalaldehyde groups according to claim 7, characterized in that: The specific cross-linking method is radiation cross-linking; The radiation crosslinking is selected from electron beam radiation crosslinking or gamma ray radiation crosslinking; Wherein, when the radiation crosslinking is selected from electron beam radiation crosslinking, the radiation dose rate is selected from 10 to 1000 Gy / s, and the radiation time is selected from 5 to 100 minutes; When the radiation cross-linking is selected from gamma-ray radiation cross-linking, the radiation dose is selected from 10 to 100 kGy.
12. The method for preparing the microgel modified with o-phthalaldehyde groups according to claim 6, characterized in that: The preparation of microgels by polymerization and cross-linking of monomers refers to: The monomers are copolymerized and cross-linked with multifunctional double-bond cross-linking agents or the monomers are polymerized and cross-linked into gels by a specific cross-linking method, and then physically broken by mechanical force and sieved through sieves of different sizes to obtain microgels with different particle size distributions; or, The monomer and the multifunctional double-bond crosslinking agent are subjected to emulsion polymerization or precipitation polymerization to obtain microgels with a certain particle size; or, The monomers are first emulsion polymerized or precipitated and then cross-linked by a specific cross-linking method to obtain microgels with a certain particle size; The monomer may be selected from one or more water-soluble monomers, or may be selected from one or more water-soluble monomers and other copolymerizable monomers.
13. The method for preparing the microgel modified with o-phthalaldehyde groups according to claim 12, characterized in that: The water-soluble monomer is selected from (meth)acrylic acid, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, glucose (meth)acrylate, polyethylene glycol methyl ether (meth)acrylate and polyethylene glycol (meth)acrylate, (meth)acrylamide, N,N-dimethylacrylamide, N-hydroxymethylacrylamide, N-hydroxyethyl (meth)acrylamide, N-hydroxypropyl (meth)acrylamide, N-isopropylacrylamide and 2-acrylamido-2-methylpropanesulfonic acid (AMPS), vinyl pyrrolidone; The other copolymerizable monomers may be selected from (meth)acrylate monomers, (meth)acrylamide monomers, styrene monomers, vinyl acetate and acrylonitrile; Herein, (meth)acrylic acid refers to acrylic acid or methacrylic acid; and (meth)acrylamide refers to acrylamide or methacrylamide.
14. The method for preparing the microgel modified with o-phthalaldehyde groups according to claim 12, characterized in that: The multifunctional double bond crosslinking agent refers to a crosslinking agent containing two or more polymerizable double bond functional groups, preferably glucose acrylate, 2,9-decadiene, 2-hexadecenoic acid, N,N'-methylenebisacrylamide or glycerol acrylate.
15. The method for preparing microgel modified with o-phthalaldehyde groups according to claim 12, characterized in that: The specific cross-linking method is selected from the following two methods: Condensation crosslinking of polymer chains containing two or more reactive functional groups in the presence or absence of a catalyst; Irradiation cross-linking.
16. The method for preparing the microgel modified with o-phthalaldehyde groups according to claim 5, characterized in that: The aldehyde-preprotected o-phthalaldehyde precursor derivative described in step (2) comprises an aldehyde-preprotected o-phthalaldehyde group and a substituent R that can be connected to an active group on the microgel, and the structure is shown in Formula 2: In Formula 2, R is selected from a carboxyl substituent, a vinyl sulfone substituent, an epoxy substituent, a haloalkane substituent, an isocyanate substituent or an amine substituent; In Formula 2, R is directly connected to the benzene ring, or connected to the benzene ring through a single or multiple alkylene chains or alkoxy chains, and the multiple alkylene chains or alkoxy chains are connected through ether bonds, amide bonds, ester bonds, carbamate bonds or urea bonds.
17. The method for preparing microgel modified with o-phthalaldehyde groups according to claim 16, characterized in that: The aldehyde group pre-protected o-phthalaldehyde precursor derivative is selected from one or more of the following structures: Among them, 1≤r≤20, 1≤s≤20, 1≤t≤50; preferably, 1≤r≤6, 1≤s≤10, 1≤t≤30.
18. The method for preparing microgel modified with o-phthalaldehyde groups according to claim 16, characterized in that: The active groups on the microgel are selected from hydroxyl groups or carboxyl groups; The covalent bond connection between the aldehyde group pre-protected o-phthalaldehyde precursor derivative and the active group on the microgel is selected from ether bond, amide bond, ester bond, carbamate bond or urea bond, preferably ether bond, amide bond and carbamate bond.
19. The method for preparing microgel modified with o-phthalaldehyde groups according to claim 18, characterized in that: When the active groups on the microgel are selected from hydroxyl groups, the covalent bond connection is based on an ether bond connection between vinyl sulfone substituents, epoxy substituents and halogenated alkane substituents on the o-phthalaldehyde precursor derivative and the hydroxyl groups on the microgel, based on an ester bond connection between carboxyl substituents on the o-phthalaldehyde precursor derivative and the hydroxyl groups on the microgel, and based on a carbamate bond connection between isocyanate substituents on the o-phthalaldehyde precursor derivative and the hydroxyl groups on the microgel; When the active groups on the microgel are selected from carboxyl groups, the covalent bond connection is based on an amide bond connection between the amino substituents on the o-phthalaldehyde precursor derivative and the carboxyl groups on the microgel.
20. The method for preparing microgel modified with o-phthalaldehyde groups according to claim 5, characterized in that: The deprotection described in step (3) refers to deprotecting the pre-protected o-phthalaldehyde functional group of the aldehyde group connected to the microgel under acidic conditions to obtain a microgel modified with o-phthalaldehyde groups.
21. Highly effective hemostatic material, characterized in that: Select one of the following materials: A highly efficient hemostatic sponge having a porous structure obtained by drying the microgel modified with the o-phthalaldehyde group according to any one of claims 1 to 4; The microgel modified with the o-phthalaldehyde group according to any one of claims 1 to 4 is used for dehydration and drying Afterwards, the obtained high-efficiency hemostatic powder; The invention is a highly efficient flowable hemostatic agent directly obtained by uniformly dispersing the microgel modified with the o-phthalaldehyde group described in any one of claims 1 to 4 in a solvent.
22. The high-efficiency hemostatic material according to claim 21, characterized in that: When the high-efficiency hemostatic material is a high-efficiency hemostatic sponge, the drying method is vacuum freeze drying; When the high-efficiency hemostatic material is a high-efficiency hemostatic powder, the dehydration is to replace the water in the microgel modified by the o-phthalaldehyde group with an organic solvent, so that the water content of the microgel is reduced and precipitated in the form of solid particles; the drying is direct drying or vacuum freeze drying followed by drying; the particle size distribution of the high-efficiency hemostatic powder is 20 mesh to 300 mesh; When the highly efficient hemostatic material is a highly efficient mobile hemostatic agent, the solvent is selected from water, physiological saline, buffer solution, decellularized matrix or cell culture medium solution containing or not containing polyols, and the polyol is preferably one or more of propylene glycol, butanediol, 1,2-pentanediol, 1,2-hexanediol or glycerol; The solid content of the high-efficiency flowable hemostat is 1% to 20% (w / v); preferably, the solid content of the high-efficiency flowable hemostat is selected from 5% to 12% (w / v).
23. A composite sponge, characterized in that: The composite sponge is a composite sponge having a porous structure obtained by layering the microgel modified with the o-phthalaldehyde group and the microgel not modified with the o-phthalaldehyde group according to any one of claims 1 to 4 in a mold, and then drying. The microgel without o-phthalaldehyde group modification refers to a microgel prepared from a water-soluble or hydrophilic polymer or a microgel prepared by polymerization and cross-linking of monomers.
24. The composite sponge according to claim 23, characterized in that The microgel modified with o-phthalaldehyde groups and the microgel not modified with o-phthalaldehyde groups have the same or different polymer skeleton, water content, particle size and pH value.
25. The composite sponge according to claim 23, characterized in that The composite sponge has a double-layer structure, one side of which is composed of microgels modified with o-phthalaldehyde groups, and the other side of which is composed of microgels not modified with o-phthalaldehyde groups.
26. Use of the high-efficiency hemostatic material according to claim 21 or 22, characterized in that: When the efficient hemostatic material is an efficient hemostatic sponge, the application of the efficient hemostatic sponge is selected from one of the following applications: Application of the highly efficient hemostatic sponge in the preparation of non-compressive hemostatic products for penetrating wounds; Application of the highly efficient hemostatic sponge in the preparation of liver hemostatic products; Application of the highly efficient hemostatic sponge in the preparation of spleen hemostatic products; Application of the high-efficiency hemostatic sponge in the preparation of surface arterial hemostatic products; Application of the highly efficient hemostatic sponge in the preparation of surface venous hemostasis products; Application of the high-efficiency hemostatic sponge in the preparation of femoral artery hemostatic products; Application of the high-efficiency hemostatic sponge in preparing abdominal aorta hemostasis products; Application of the high-efficiency hemostatic sponge in the preparation of carotid artery hemostasis products; Application of the highly efficient hemostatic sponge in the preparation of cardiac hemostatic products; Application of the highly efficient hemostatic sponge in the preparation of coronary artery hemostasis products; Application of the highly effective hemostatic sponge in the preparation of hemostatic products for tooth extraction wounds; Application of the highly efficient hemostatic sponge in the preparation of spinal hemostatic products; Application of the highly efficient hemostatic sponge in the preparation of uterine wall hemostatic products; When the efficient hemostatic material is efficient hemostatic powder, the application of the efficient hemostatic powder is selected from one of the following applications: Application of the highly effective hemostatic powder in the preparation of liver hemostatic products; Application of the highly effective hemostatic powder in the preparation of spleen hemostatic products; Application of the highly effective hemostatic powder in the preparation of venous hemostatic products; Application of the highly effective hemostatic powder in the preparation of surface arterial hemostatic products; Application of the highly effective hemostatic powder in the preparation of surface vein hemostatic products; Application of the highly effective hemostatic powder in the preparation of intestinal hemostatic products; Application of the highly effective hemostatic powder in the preparation of skin hemostatic products; Application of the highly effective hemostatic powder in the preparation of oral mucosal hemostatic products; Application of the highly effective hemostatic powder in the preparation of hemostatic products for hysterectomy; Application of the highly effective hemostatic powder in the preparation of spinal hemostatic products; When the highly efficient hemostatic material is a highly efficient flowing hemostatic agent, the application of the highly efficient flowing hemostatic agent is selected from one of the following applications: Application of the highly efficient mobile hemostatic agent in the preparation of non-compressive hemostatic products for penetrating wounds; The high-efficiency mobile hemostatic agent is used in the preparation of digestive tract hemostatic products; Application of the highly efficient mobile hemostatic agent in the preparation of hemostatic products during and after partial nephrectomy; Application of the highly efficient mobile hemostatic agent in the preparation of hemostatic products for narrow cavities of organisms; Application of the highly efficient mobile hemostatic agent in the preparation of spinal hemostatic products; The high-efficiency mobile hemostatic agent is used in the preparation of hemostatic products for percutaneous puncture.
27. Use of the composite sponge according to any one of claims 23 to 25, characterized in that: Select one of the following applications: Application of the composite sponge in preparing postoperative anti-adhesion products; Application of the composite sponge in the preparation of tissue leakage blocking products; Application of the composite sponge in the preparation of tissue fluid leakage blocking products; Wherein, the postoperative adhesion prevention includes abdominal wall adhesion prevention, pericardial adhesion prevention, tendon adhesion prevention and intrauterine adhesion prevention; The tissue air leakage blocking includes lung parenchyma air leakage blocking; The tissue fluid leakage blocking includes intestinal leakage blocking, pancreatic leakage blocking, cerebrospinal fluid leakage blocking, and gastric leakage blocking.
Citation Information
Patent Citations
Haemostatic and wound dressing containing same
CN102008742A
Injectable type self-healing hemostatic material as well as preparation method and application thereof
CN106983905A
Polyethylene glycol derivative and preparation method thereof, and polyethylene glycol hydrogel capable of rapidly generating cross-linking reaction
CN111440310A
Hydrogel powder for rapid hemostasis and preparation method and application thereof
CN114767919A
Low-swelling injectable hydrogel as well as preparation method and application thereof
CN114907558A
Cited By
Degradable composite hyaluronic acid polymer hemostatic material and application thereof
CN119424719A
Rapid asymmetric tissue sealing patch as well as preparation method and application thereof
CN120501917A
Degradable rapid hemostasis sealing adhesive and application
CN120939273A