Low-temperature polymerized gel electrolyte and battery comprising same
By using low-temperature polymerized gel electrolytes in the battery and using specific polymer monomer combinations to achieve the stability of electrolyte additives and isolation of early thermal runaway reactions, the problems of thermal runaway and insufficient safety performance of the battery are solved, and the electrical performance of the battery is improved. and safety performance.
Patent Information
- Application Number
- PCT/CN2024/075713
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-18
- Filing Date
- 2024-02-04
- Publication Date
- 2024-10-24
AI Technical Summary
When existing battery technology increases the energy density of positive and negative electrode materials, it is easy to cause thermal runaway and explosion, and the stability of electrolyte additives is poor, resulting in insufficient battery safety performance.
Using low-temperature polymerized gel electrolyte, by selecting monofunctional acrylates, multifunctional acrylates and functional monomers, in-situ polymerization can be achieved at a temperature no higher than 40°C to avoid decomposition of electrolyte additives. And in the early stage of thermal runaway, a hard texture is formed to isolate gas diffusion and limit the thermal runaway reaction.
It improves the electrical performance and safety performance of the battery, avoids the decomposition of electrolyte additives, maintains the shape integrity of the separator, effectively isolates gas diffusion, and enhances the thermal stability and safety performance of the battery.
Smart Images

Figure PCTCN2024075713-FTAPPB-I100001 
Figure PCTCN2024075713-FTAPPB-I100002 
Figure PCTCN2024075713-FTAPPB-I100003
Abstract
Description
A low-temperature polymerized gel electrolyte and a battery containing the same Technical Field
[0001] The present invention belongs to the technical field of batteries, and in particular relates to a low-temperature polymerized gel electrolyte and a battery containing the same. Background Art
[0002] After decades of commercial application, batteries have changed the face of the world in many aspects. However, the development of power batteries, grid energy storage and other fields urgently requires further improvement of battery energy density. To achieve this goal, the most critical route is to increase the volumetric capacity and mass capacity of positive and negative electrode materials, such as developing high-nickel ternary materials for positive electrodes and silicon / graphite composite materials (silicon content >10%) for negative electrodes.
[0003] However, at the same time, it will also bring more serious safety problems, such as being more prone to thermal runaway, which can lead to fire and explosion. Thermal runaway is related to many factors, one of the key factors being that in the early stages of thermal runaway, the charged electrode materials will decompose and produce gases. For example, the high-nickel ternary positive electrode material will undergo a phase transition and release oxygen, and the silicon / graphite negative electrode material and SEI film will decompose and release reducing gases such as ethylene and acetylene. When these gases pass through the diaphragm and come into contact with the electrode material on the other side, they will further trigger the thermal runaway reaction to intensify and even cause an explosion. In addition, in order to improve the interfacial stability of the positive and negative electrode materials of the battery, the electrolyte formula is constantly updated, including the addition of high-efficiency film-forming additives such as fluoroethylene carbonate (FEC) and diethylene sulfate (DTD). However, these additives are not stable and will decompose and become inactivated when heated.
[0004] In order to limit leakage and improve safety performance, preparing semi-solid batteries is a feasible route. Among them, the scheme of forming a gel electrolyte in situ conforms to the actual production situation of the factory. There is no need to change the production line design. It only requires adding a polymer monomer and a small amount of initiator to a conventional electrolyte to form a gel electrolyte inside the battery cell under heating. CN113096969A discloses a polymer gel electrolyte / electrode and its preparation method, a supercapacitor and its preparation method. The invention provides a preparation method of a polymer gel electrolyte / electrode, comprising the following steps: mixing a polymer monomer, a conductive medium, water and an initiator to obtain a precursor solution; and in-situ polymerization is performed after the electrode is soaked in the precursor solution to obtain a polymer gel electrolyte / electrode. The invention improves the energy storage performance of the polymer gel electrolyte / electrode by infiltrating the precursor solution into the electrode material layer for an in-situ polymerization reaction, so that the surface of the electrode material is in full contact with the gel electrolyte, establishing an effective charge transfer interface. However, the in-situ polymerization temperature of the gel electrolyte provided by the invention is relatively high, and the electrolyte additive is sensitive to temperature and will decompose and lose its activity when heated. This poses a considerable challenge to the design of a new safe electrolyte system.
[0005] Current in-situ gelation technology requires temperatures above 60°C for thermal initiation, which consumes unreacted polymer monomers and achieves a high degree of polymerization. This decomposes electrolyte additives, causing discoloration (yellowing) and further degrading the battery's electrochemical performance. Furthermore, current in-situ gelation electrolytes only address leakage, but have no significant effect on thermal runaway caused by gas diffusion.
[0006] Therefore, it is expected to develop a gel electrolyte with a low in-situ polymerization temperature and the ability to effectively isolate gas shuttling.
[0007] Summary of the Invention
[0008] In response to the shortcomings of the prior art, the present invention aims to provide a low-temperature polymerizable gel electrolyte and a battery containing the same. The gel electrolyte, by selecting and combining three polymerizable monomers, enables in-situ polymerization at a relatively low temperature (no higher than 40°C), effectively avoiding decomposition of electrolyte additives and improving the electrical performance of the battery containing the same. In addition, the gel electrolyte can be further thermally cured and transformed into a hard texture when early thermal runaway occurs, thereby maintaining the integrity of the diaphragm shape and isolating gas diffusion, thereby limiting the further occurrence of thermal runaway reactions and effectively improving the safety performance of the battery.
[0009] To achieve this object, the present invention adopts the following technical solutions:
[0010] In a first aspect, the present invention provides a low-temperature polymerized gel electrolyte, wherein the raw material for preparing the low-temperature polymerized gel electrolyte is a gel precursor solution, wherein the gel precursor solution includes a combination of a polymerizable monomer, an electrolyte additive, a thermal initiator, a lithium salt, and a solvent;
[0011] The polymerizable monomers include monofunctional acrylic ester monomers, multifunctional acrylic ester monomers and functionalized monomers, and the functionalized monomers contain crosslinking groups and monovinyl groups.
[0012] The low-temperature polymerized gel electrolyte provided by the present invention is obtained by in-situ polymerization of a gel precursor solution, wherein the gel precursor solution contains polymerizable monomers, and the polymerizable monomers are limited to a combination of monofunctional acrylate monomers, multifunctional acrylate monomers, and functionalized monomers, and the functionalized monomers are further limited to contain cross-linking groups and monovinyl groups; on the one hand, by selecting the above three polymerizable monomers for combination, in-situ polymerization can be achieved at a relatively low temperature (not higher than 40°C), effectively avoiding the decomposition of electrolyte additives and improving the electrical performance of the battery; on the other hand, the monofunctional acrylate monomers are used to The in-situ polymerization process of the multifunctional acrylate monomers can form a three-dimensional network and a thermally stable polymer skeleton, and then the functional monomers are used to adjust the texture and fluidity of the formed gel electrolyte, so that the obtained gel electrolyte has a soft and sticky texture, which can fully infiltrate the battery cell without leakage. At the same time, when early thermal runaway (>100°C) occurs, the gel electrolyte can be further thermally cured to become hard, thereby maintaining the integrity of the diaphragm shape and isolating gas diffusion, thereby limiting the further occurrence of thermal runaway reactions and effectively improving the safety performance of the battery.
[0013] Preferably, the gel precursor solution comprises the following components in parts by weight:
[0014] The mass percentage of the polymerizable monomer in the gel precursor solution is 1-10%, for example, 2 parts by weight, 3 parts by weight, 4 parts by weight, 5 parts by weight, 6 parts by weight, 7 parts by weight, 8 parts by weight or 9 parts by weight, etc., preferably 1-5 parts by weight.
[0015] The mass percentage of the electrolyte additive in the gel precursor solution is 0 to 10 parts by weight and is not equal to 0, for example, 2 parts by weight, 3 parts by weight, 4 parts by weight, 5 parts by weight, 6 parts by weight, 7 parts by weight, 8 parts by weight or 9 parts by weight.
[0016] The mass percentage of the thermal initiator in the gel precursor solution is 0.02 to 0.05 parts by weight, such as 0.025 parts by weight, 0.03 parts by weight, 0.035 parts by weight, 0.04 parts by weight or 0.045 parts by weight.
[0017] The mass percentage of the lithium salt in the gel precursor solution is 8 to 20 parts by weight, for example, 10 parts by weight, 12 parts by weight, 14 parts by weight, 16 parts by weight or 18 parts by weight.
[0018] Preferably, the mass percentage of the solvent in the gel precursor solution is 50 to 80 parts by weight, for example, 53 parts by weight, 56 parts by weight, 59 parts by weight, 62 parts by weight, 65 parts by weight, 68 parts by weight, 71 parts by weight, 74 parts by weight or 77 parts by weight.
[0019] In some preferred embodiments, based on 100 parts by weight of the total mass of the gel precursor solution, the gel precursor solution comprises the following components in parts by weight:
[0020] In some preferred embodiments, the mass percentage of the polymerizable monomer in the gel precursor solution is 1% to 10%, for example, 2%, 3%, 4%, 5%, 6%, 7%, 8% or 9%, etc., preferably 1% to 5%.
[0021] In some preferred embodiments, the mass percentage of the electrolyte additive in the gel precursor solution is 0-10% and is not equal to 0, for example, 2%, 3%, 4%, 5%, 6%, 7%, 8% or 9%.
[0022] In some preferred embodiments, the mass percentage of the thermal initiator in the gel precursor solution is 0.02% to 0.05%, for example, 0.025%, 0.03%, 0.035%, 0.04% or 0.045%.
[0023] In some preferred embodiments, the mass percentage of lithium salt in the gel precursor solution is 8% to 20%, for example, 10%, 12%, 14%, 16% or 18%.
[0024] In some preferred embodiments, the mass percentage of the solvent in the gel precursor solution is 50% to 80%, for example, 53%, 56%, 59%, 62%, 65%, 68%, 71%, 74% or 77%.
[0025] Preferably, the mass ratio of the monofunctional acrylate monomer, the multifunctional acrylate monomer and the functionalized monomer is 1:(0.5-1.5):(0.1-0.5).
[0026] The mass ratio of the monofunctional acrylate monomer to the multifunctional acrylate monomer is 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1, 1:1.1, 1:1.2, 1:1.3 or 1:1.4.
[0027] The mass ratio of the monofunctional acrylate monomer to the functionalized monomer is 1:0.15, 1:0.2, 1:0.25, 1:0.3, 1:0.35, 1:0.4 or 1:0.45, etc.
[0028] As a preferred technical solution of the present invention, limiting the mass ratio of monofunctional acrylate monomers, multifunctional acrylate monomers, and functionalized monomers to 1:(0.5-1.5):(0.1-0.5) can optimize the overall performance of the resulting gel electrolyte. If the amount of monofunctional acrylate monomer added is relatively low, the gel electrolyte will be relatively hard and have relatively low ionic conductivity. If the amount of multifunctional acrylate monomer added is relatively low, the total amount of polymerized monomers required to form the gel electrolyte will increase, and the stability of the resulting gel electrolyte will be reduced. If the amount of functionalized monomer added is relatively low, a harder gel electrolyte cannot be formed during early thermal runaway, thereby failing to effectively improve the thermal stability of the battery.
[0029] In the present invention, the monofunctional acrylate monomer contains only one acrylate group or methacrylate group. Preferably, the monofunctional acrylate monomer includes any one of n-butyl acrylate, isobutyl acrylate, propyl acrylate, polyethylene glycol methacrylate, polyethylene glycol monomethyl ether methacrylate, 2-methoxyethyl acrylate, ethyl acrylate, hexyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, lauryl methacrylate, or n-octyl methacrylate, or a combination of at least two thereof.
[0030] In the present invention, the multifunctional acrylate monomer contains two or more groups selected from acrylate groups and methacrylate groups. Preferably, the multifunctional acrylate monomer includes any one or a combination of at least two of polyethylene glycol dimethacrylate, polyethylene glycol diacrylate, pentaerythritol tetraacrylate, ethoxylated trimethylolpropane triacrylate, ethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, or triethylene glycol diacrylate.
[0031] In the present invention, the monofunctional acrylate monomer and the multifunctional acrylate monomer do not contain the crosslinking group described herein.
[0032] In some embodiments, the cross-linking group refers to a functional group that does not polymerize at a relatively low temperature (eg, 20-40° C.) but begins to polymerize at a relatively high temperature (eg, >40° C.).
[0033] Preferably, the crosslinking group comprises a cyclic ether group and / or a silane group.
[0034] In the present invention, the functionalized monomer containing a monovinyl group means that the functionalized monomer contains one reactive carbon-carbon double bond.
[0035] Preferably, the functional monomer includes any one of glycidyl methacrylate, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltriisopropoxysilane or γ-methacryloxypropyltrimethoxysilane, or a combination of at least two thereof.
[0036] In some embodiments, the monofunctional acrylic ester monomer is n-butyl acrylate, the multifunctional acrylic ester monomer is polyethylene glycol dimethacrylate, and the functionalized monomer is glycidyl methacrylate.
[0037] Preferably, the electrolyte additive includes fluoroethylene carbonate (FEC) and / or diethylene sulfate (DTD). In some embodiments, the electrolyte additive includes FEC and DTD, and the mass ratio of FEC to DTD can be 1:1 to 3:1, such as 1.5:1, 2:1, or 2.5:1.
[0038] Preferably, the thermal initiator comprises a peroxide and / or an azo compound.
[0039] Preferably, the peroxide comprises benzoyl peroxide (BPO).
[0040] Preferably, the azo compound includes any one of azobisisobutyronitrile (AIBN), dimethyl azobisisobutyrate (AIBME) or azobisisoheptanenitrile (ABVN), or a combination of at least two thereof.
[0041] Preferably, the lithium salt comprises lithium hexafluorophosphate.
[0042] Preferably, the solvent comprises ethylene carbonate and / or diethyl carbonate. In some embodiments, the solvent comprises ethylene carbonate and diethyl carbonate, and the volume ratio of ethylene carbonate to diethyl carbonate can be 1:2 to 2:1, such as 1:1.5, 1:1, 1.5:1.
[0043] In a second aspect, the present invention provides a method for preparing the gel electrolyte as described in the first aspect, the method comprising: polymerizing a polymerization monomer, an electrolyte additive, a thermal initiator, a lithium salt and a solvent at 20 to 40° C. for 6 to 24 hours under a nitrogen atmosphere to obtain the gel electrolyte.
[0044] Preferably, the polymerization temperature is 20-40°C, for example, 22°C, 24°C, 26°C, 28°C, 30°C, 32°C, 34°C, 36°C or 38°C, more preferably 25-30°C.
[0045] Preferably, the polymerization time is 6 to 24 hours, such as 8 hours, 10 hours, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours or 22 hours, and more preferably 12 to 15 hours. As a preferred technical solution of the present invention, the preparation method of the gel electrolyte comprises the following steps:
[0046] (A) uniformly mixing a polymerizable monomer, an electrolyte additive, a thermal initiator, a lithium salt, and a solvent to obtain a gel electrolyte precursor solution (i.e., a gel precursor solution);
[0047] (B) The gel electrolyte precursor solution obtained in step (A) is transferred to a sealable glass container and subjected to three cycles of liquid nitrogen freezing, evacuation, restoration to room temperature, and filling with nitrogen to form a nitrogen atmosphere inside the system; finally, the glass container is placed at an ambient temperature of 20 to 40° C. and allowed to stand for 6 to 24 hours to obtain the gel electrolyte.
[0048] In step (A), the polymerization monomers, thermal initiator and other components of the gel precursor solution are preferably mixed in an open environment at a temperature of 20-25° C. and a humidity of 0-5% to avoid premature in-situ polymerization of the gel precursor solution.
[0049] It should be noted that in step (B) of the method for preparing the gel electrolyte provided by the present invention, air is discharged during the process of filling with nitrogen. After the air is discharged, the polymerization monomer begins to polymerize because the presence of oxygen in the air inhibits the occurrence of the polymerization reaction.
[0050] In a third aspect, the present invention provides a battery comprising a positive electrode, a negative electrode, a separator, and the low-temperature polymerized gel electrolyte as described in the first aspect.
[0051] Preferably, the battery is any one of a cylindrical battery, a soft-pack battery or a square battery.
[0052] Preferably, the battery comprises a wound battery or a stacked battery.
[0053] Preferably, the active material of the positive electrode includes nickel-cobalt-manganese ternary material.
[0054] Preferably, the nickel-cobalt-manganese ternary material is LiNi 1-x-y Co x Mn y O2, where 0.6≤1-xy<1;
[0055] Among them, 1-xy can be equal to 0.6, 0.7, 0.8 or 0.9, etc.
[0056] 0<x<0.4, for example, x can be equal to 0.05, 0.1, 0.2, 0.3, etc.
[0057] 0<y<0.4, for example, y can be equal to 0.05, 0.1, 0.2, 0.3, etc.
[0058] Preferably, the nickel-cobalt-manganese ternary material is LiNi 0.6 Co 0.2 Mn 0.2 O2、LiNi 0.8 Co 0.1 Mn 0.1 O2、LiNi 0.83 Co 0.08 Mn 0.09 O2 or LiNi 0.9 Co 0.05 Mn 0.05 Any one or a combination of at least two of O2.
[0059] Preferably, the active material of the negative electrode comprises a silicon / graphite composite material.
[0060] Preferably, the mass percentage of silicon in the silicon / graphite composite material is 5-30%, for example, 7%, 9%, 11%, 13%, 15%, 17%, 19%, 21%, 23%, 25%, 27% or 29%.
[0061] As a preferred technical solution of the present invention, the gel electrolyte provided by the present invention is more suitable for batteries in which the positive electrode active material is a nickel-cobalt-manganese ternary material with a high nickel content and the negative electrode active material is a silicon / graphite composite material with a high silicon content. This is because although the specific capacity of the positive and negative electrode active materials is improved, the interface stability is also reduced, and it is necessary to add indispensable electrolyte SEI film-forming electrolyte additives, such as fluoroethylene carbonate (FEC) and / or diethylene sulfate (DTD), etc. However, these electrolyte additives have poor thermal stability and are easily decomposed by heat. The method provided by the present invention can polymerize the gel at a temperature not higher than 40°C, which will not cause the decomposition and inactivation of the electrolyte additives.
[0062] Preferably, the diaphragm comprises a polyethylene diaphragm or a polypropylene diaphragm.
[0063] In a fourth aspect, the present invention provides a method for preparing the battery according to the third aspect, the method comprising the following steps:
[0064] (1) Assembling the positive electrode, the negative electrode and the separator to obtain a battery cell;
[0065] (2) Injecting the raw materials for preparing the gel electrolyte provided in the first aspect into the battery cell obtained in step (1), leaving it open and allowing it to stand, passing nitrogen, and then sealing it, and performing in-situ polymerization to obtain the battery.
[0066] Preferably, the assembling method in step (1) includes winding or lamination.
[0067] Preferably, the assembly in step (1) is carried out in an environment (e.g., air environment) with a temperature of 20-25°C (e.g., 21°C, 22°C, 23°C, or 24°C, etc.) and a humidity of 0-5% (e.g., 1%, 2%, 3%, or 4%, etc.).
[0068] As a preferred technical solution of the present invention, to prevent in-situ polymerization of the gel precursor solution before injection into the battery cell, the humidity of the environment should be controlled at 0-5% and the temperature at 20-25°C. Air inhibits in-situ polymerization of the monomer. Preferably, the open-air standing time is 20-26 hours, for example, 21 hours, 22 hours, 23 hours, 24 hours, or 25 hours.
[0069] As a preferred technical solution of the present invention, in order to allow the battery cell to be fully infiltrated, the battery cell needs to be left open for 20 to 26 hours after nitrogen is passed through the cell and before sealing.
[0070] Preferably, the open static state is carried out in an environment with a temperature of 20-25°C (for example, 21°C, 22°C, 23°C or 24°C, etc.) and a humidity of 0-5% (for example, 1%, 2%, 3% or 4%, etc.).
[0071] Preferably, the nitrogen passing time is 0 to 10 minutes and is not equal to 0, for example, 1 minute, 2 minutes, 3 minutes, 4 minutes, 5 minutes, 6 minutes, 7 minutes, 8 minutes or 9 minutes.
[0072] Preferably, the temperature of the in-situ polymerization is 20-40°C, such as 22°C, 24°C, 26°C, 28°C, 30°C, 32°C, 34°C, 36°C or 38°C, and more preferably 25-30°C.
[0073] Preferably, the in-situ polymerization time is 6 to 24 hours, for example, 8 hours, 10 hours, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours or 22 hours, and more preferably 12 to 15 hours.
[0074] Preferably, after the in-situ polymerization is completed, the steps of formation, exhaust and volume separation are further included.
[0075] As a preferred technical solution of the present invention, the method for preparing the battery comprises the following steps:
[0076] (1) mixing a polymerization monomer, an electrolyte additive, a thermal initiator, a lithium salt, and a solvent at a temperature of 20 to 25° C. and a humidity of 0 to 5% to obtain a gel precursor solution;
[0077] Assembling the positive electrode, the negative electrode and the separator to obtain a battery cell;
[0078] (2) injecting the gel precursor solution obtained in step (1) into the battery cell obtained in step (1), allowing it to stand for 20 to 26 hours in an environment with a temperature of 20 to 25° C. and a humidity of 0 to 5%, sealing it after passing nitrogen, and in-situ polymerizing it at 20 to 40° C. for 6 to 24 hours, forming, exhausting and volume separation to obtain the battery.
[0079] Compared with the prior art, the present invention has the following beneficial effects:
[0080] The raw material for preparing the low-temperature polymerized gel electrolyte provided by the present invention is a gel precursor solution, which includes a combination of polymerizable monomers, electrolyte additives, thermal initiators, lithium salts, and solvents. By limiting the polymerizable monomers to include monofunctional acrylate monomers, multifunctional acrylate monomers, and functionalized monomers, wherein the functionalized monomers contain cross-linking groups and monovinyl groups, the above three polymerizable monomers are combined to achieve in-situ polymerization at a relatively low temperature (no higher than 40°C), effectively avoiding the decomposition of the electrolyte additives and improving the electrical performance of the battery. In addition, the gel electrolyte can be further thermally cured to become hard when early thermal runaway occurs, thereby maintaining the integrity of the diaphragm shape and isolating gas diffusion, thereby limiting the further occurrence of thermal runaway reactions and effectively improving the safety performance of the battery. DETAILED DESCRIPTION
[0081] The technical solution of the present invention is further described below by way of specific embodiments. It should be understood by those skilled in the art that the embodiments are merely to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0082] Example 1
[0083] A low-temperature polymerized gel electrolyte, wherein the raw material for preparing the gel electrolyte is a gel precursor solution, wherein the gel precursor solution comprises 5% by weight of a polymerizable monomer, 7% by weight of an electrolyte additive, 0.05% by weight of a thermal initiator, 12.95% by weight of a lithium salt, and 75% by weight of a solvent;
[0084] The polymer monomers are composed of n-butyl acrylate, polyethylene glycol dimethacrylate and glycidyl methacrylate in a mass ratio of 1:0.8:0.2; the electrolyte additives are composed of fluoroethylene carbonate and vinyl sulfate in a mass ratio of 5:2; the thermal initiator is azobisisoheptanenitrile; the lithium salt is lithium hexafluorophosphate; and the solvent is ethylene carbonate and diethyl carbonate in a volume ratio of 1:1.
[0085] The preparation method of the gel electrolyte provided in this embodiment includes the following steps:
[0086] (1) dissolving a lithium salt in a solvent and adding an electrolyte additive to obtain an electrolyte;
[0087] (2) in an open environment at a temperature of 25° C. and a humidity of 2%, mixing the polymerizable monomer and the electrolyte obtained in step (1), adding a thermal initiator and mixing, to obtain a clear and transparent gel precursor solution;
[0088] (3) The gel precursor solution obtained in step (2) is transferred to a sealable glass container, and subjected to three cycles of liquid nitrogen freezing, evacuation, restoration to room temperature, and filling with nitrogen, so that the interior of the system is filled with nitrogen atmosphere. Finally, the glass container is placed at an ambient temperature of 25°C for polymerization for 12 hours to obtain the gel electrolyte.
[0089] Example 2
[0090] A low-temperature polymerized gel electrolyte, which differs from Example 1 only in that the polymerization temperature in step (3) is 40° C., and other substances, amounts and conditions are the same as those in Example 1.
[0091] Example 3
[0092] A low-temperature polymerized gel electrolyte, which differs from Example 1 only in that the polymerization temperature in step (3) is 20° C., and other substances, amounts and conditions are the same as those in Example 1.
[0093] Example 4
[0094] A low-temperature polymerized gel electrolyte, which differs from Example 1 only in that the polymerization temperature in step (3) is 60° C., and other substances, amounts and conditions are the same as those in Example 1.
[0095] Example 5
[0096] A low-temperature polymerized gel electrolyte is disclosed. The only difference from Example 1 is that the polymerizable monomers in the gel precursor solution are composed of n-butyl acrylate, polyethylene glycol dimethacrylate, and glycidyl methacrylate in a mass ratio of 1:0.4:0.2. Other substances, amounts, and parameters are the same as those in Example 1.
[0097] Example 6
[0098] A low-temperature polymerized gel electrolyte is disclosed. The only difference from Example 1 is that the polymerizable monomers in the gel precursor solution are composed of n-butyl acrylate, polyethylene glycol dimethacrylate, and glycidyl methacrylate in a mass ratio of 1:1.8:0.2. Other substances, amounts, and parameters are the same as those in Example 1.
[0099] Example 7
[0100] A low-temperature polymerized gel electrolyte is disclosed. The only difference from Example 1 is that the polymerizable monomers in the gel precursor solution are composed of n-butyl acrylate, polyethylene glycol dimethacrylate, and glycidyl methacrylate in a mass ratio of 1:0.8:0.05. Other substances, amounts, and parameters are the same as those in Example 1.
[0101] Example 8
[0102] A low-temperature polymerized gel electrolyte is disclosed. The only difference from Example 1 is that the polymerizable monomers in the gel precursor solution are composed of n-butyl acrylate, polyethylene glycol dimethacrylate, and glycidyl methacrylate in a mass ratio of 1:0.8:0.8. Other substances, amounts, and parameters are the same as those in Example 1.
[0103] Application Example 1
[0104] A battery with a capacity of 3.2Ah, comprising a positive electrode, a negative electrode, a gel electrolyte and a separator;
[0105] Among them, the active material of the positive electrode is 811NCM ternary material (LiNi 0.8 Co 0.1 Mn 0.1 O2), the conductive agent is carbon black, the binder is polyvinylidene fluoride (PVDF), and the preparation method of the positive electrode includes: dispersing 98wt% of the active material, 1wt% of the conductive agent and 1wt% of the binder in N-methylpyrrolidone (NMP) to prepare a positive electrode slurry, then coating the positive electrode slurry on a current collector aluminum foil and drying it, then rolling, slitting, punching the dried positive electrode sheet and then vacuum drying it at high temperature to obtain a positive electrode to be used;
[0106] The negative electrode active material is a silicon / graphite composite material (containing 12 wt% silicon), the conductive agent is carbon black, and the binder is sodium carboxymethyl cellulose (CMC). The negative electrode preparation method includes: dispersing 98 wt% of the active material, 0.8 wt% of the conductive agent, and 1.2 wt% of the binder in deionized water to form a negative electrode slurry, then coating the negative electrode slurry on a current collector and drying it, and then rolling, slitting, punching, and vacuum drying the dried negative electrode sheet at high temperature to obtain the negative electrode;
[0107] The diaphragm is a common commercial PE diaphragm;
[0108] The raw materials for preparing the gel electrolyte are a gel precursor solution, which includes 5% by weight of a polymerizable monomer, 7% of an electrolyte additive, 0.05% of a thermal initiator, 12.95% of a lithium salt, and 75% of a solvent. The polymerizable monomer is composed of n-butyl acrylate, polyethylene glycol dimethacrylate, and glycidyl methacrylate in a mass ratio of 1:0.8:0.2; the electrolyte additive is composed of fluoroethylene carbonate and vinyl sulfate in a mass ratio of 5:2; the thermal initiator is azobisisoheptonitrile; the lithium salt is lithium hexafluorophosphate; and the solvent is ethylene carbonate and diethyl carbonate in a volume ratio of 1:1.
[0109] The method for preparing the battery provided in this application example includes the following steps:
[0110] (1) dissolving a lithium salt in a solvent and adding an electrolyte additive to obtain an electrolyte;
[0111] (2) mixing the polymerizable monomer and the electrolyte obtained in step (1) at a temperature of 25° C. and a humidity of 2%, adding a thermal initiator and mixing to obtain a clear and transparent gel precursor solution;
[0112] (3) Assembling the positive electrode, negative electrode and separator into a battery cell in a winding manner;
[0113] (4) injecting the gel precursor solution obtained in step (2) into the battery cell obtained in step (3), and leaving it open for 24 hours in an environment with a temperature of 25°C and a humidity of 2% to allow the gel electrolyte precursor solution to fully penetrate the interior of the battery cell, then introducing nitrogen into the battery for 10 minutes, with the area of the nitrogen inlet port being 0.5 cm2 and the nitrogen flow rate being 5 cm / s. The battery cell is sealed and placed at 25°C for 12 hours. During this process, the gel electrolyte precursor solution is in situ polymerized inside the battery cell to form a gel electrolyte, which is then subjected to formation, exhaust, and volume separation to obtain the battery.
[0114] Application Example 2
[0115] A battery, which differs from Example 1 only in that the polymerizable monomers in the gel precursor solution are composed of n-butyl acrylate, polyethylene glycol dimethacrylate, and glycidyl methacrylate in a mass ratio of 1:0.5:0.5, and other substances, amounts, and parameters are the same as those in Example 1.
[0116] Application Example 3
[0117] A battery, which differs from Example 1 only in that the polymerizable monomers in the gel precursor solution are composed of n-butyl acrylate, polyethylene glycol dimethacrylate, and glycidyl methacrylate in a mass ratio of 1:1.5:0.1, and other substances, amounts, and parameters are the same as those in Example 1.
[0118] Application Example 4
[0119] A battery, which differs from Example 1 only in that the polymerizable monomers in the gel precursor solution are composed of n-butyl acrylate, polyethylene glycol dimethacrylate, and glycidyl methacrylate in a mass ratio of 1:0.4:0.2, and other substances, amounts, and parameters are the same as those in Example 1.
[0120] Application Example 5
[0121] A battery, which differs from Example 1 only in that the polymerizable monomers in the gel precursor solution are composed of n-butyl acrylate, polyethylene glycol dimethacrylate, and glycidyl methacrylate in a mass ratio of 1:1.8:0.2, and other substances, amounts, and parameters are the same as those in Example 1.
[0122] Application Example 6
[0123] A battery, which differs from Example 1 only in that the polymerizable monomers in the gel precursor solution are composed of n-butyl acrylate, polyethylene glycol dimethacrylate, and glycidyl methacrylate in a mass ratio of 1:0.8:0.05, and other substances, amounts, and parameters are the same as those in Example 1.
[0124] Application Example 7
[0125] A battery, which differs from Example 1 only in that the polymerizable monomers in the gel precursor solution are composed of n-butyl acrylate, polyethylene glycol dimethacrylate, and glycidyl methacrylate in a mass ratio of 1:0.8:0.8, and other substances, amounts, and parameters are the same as those in Example 1.
[0126] Comparative Application Example 1
[0127] A battery is provided, which differs from Example 1 only in that n-butyl acrylate is not added to the gel precursor solution, and other substances, amounts, and parameters are the same as those in Example 1.
[0128] Comparative Application Example 2
[0129] A battery is provided, which differs from Example 1 only in that polyethylene glycol dimethacrylate is not added to the gel precursor solution, and other substances, amounts and parameters are the same as those in Example 1.
[0130] Comparative Application Example 3
[0131] A battery is provided, which differs from Example 1 only in that glycidyl methacrylate is not added to the gel precursor solution, and other substances, amounts, and parameters are the same as those in Example 1.
[0132] Performance testing:
[0133] (1) Chroma: The test standard is based on the national standard GB / T 3143-1982 Liquid Chemical Product Color Determination Method (Hazen unit is platinum-cobalt color number). The color of the gel electrolyte sample and the standard platinum-cobalt solution of different concentrations are compared by naked eye. The chroma of the gel electrolyte is expressed in the Hazen (platinum-cobalt) color unit of the standard platinum-cobalt comparison solution closest to the sample.
[0134] (2) Free acid (in terms of HF): The test is carried out by acid-base titration. An appropriate amount of gel electrolyte is placed in an indicator methyl red-acetonitrile solution. After ultrasonic dispersion, the solution is titrated with 0.05 mol / L triethylamine-acetonitrile solution. The endpoint of the titration is when the indicator solution turns yellow.
[0135] (3) Ionic conductivity: The test uses the AC impedance method. The gel electrolyte precursor solution is placed in a lithium-lithium symmetrical button cell. After assembly, a polymerization reaction forms a gel electrolyte. The ionic conductivity value is calculated by measuring the total impedance contributed by the electrolyte in the cell and combining it with the size of the gel electrolyte being tested.
[0136] (4) Appearance: Observe the state of the gel electrolyte with the naked eye, including whether it is clear, transparent and fluid.
[0137] (5) Hot box test: First, charge the battery to be tested at a constant current of 0.5C to 4.2V, and then charge it at a constant voltage until the charging termination current drops to 0.05C, and then stop charging to make the battery fully charged; then perform the hot box test according to the following steps: stick the temperature wire to the center of the large surface of the soft-pack battery, one on each side, and place it in a hot box at 80℃ for 3h, then increase the temperature at a rate of 5℃ / min, and keep it for 30min every time the temperature rises by 5℃, until the battery experiences thermal runaway or the temperature reaches 200℃, and the test is terminated;
[0138] (6) Capacity test: At 25°C, charge the battery to 4.2V at a constant current of 0.5C, then charge at a constant voltage until the charge termination current drops to 0.05C, then stop charging and let it sit for 30 minutes; discharge at a current of 0.5C to 2.8V, and obtain the discharge capacity;
[0139] (7) Charge and discharge cycle performance: At 25°C, the battery to be tested is subjected to 100 charge and discharge cycles according to the capacity test procedure. The capacity retention rate is obtained by calculating the ratio of the discharge capacity before and after the cycle.
[0140] (8) Battery internal resistance: First charge the battery to be tested to 3.6V, and then use a voltage internal resistance meter to test the internal resistance of the battery.
[0141] The chromaticity, free acidity, ionic conductivity and appearance of the gel electrolytes provided in Examples 1 to 8 were tested according to the above test methods. The test results are shown in Table 1:
[0142] Table 1
[0143] According to the data in Table 1, we can see that:
[0144] Examples 1, 2, and 3 all formed gel electrolytes with ideal texture and strong fluidity. The color of the gel electrolytes was ≤40 Hazen and the free acid content was ≤30 ppm, meeting the actual requirements of the electrolyte. This indicates that 20-40°C is a suitable temperature range for the polymerization reaction. Furthermore, Example 1, which is within the further preferred range of 25-30°C, has relatively high ionic conductivity.
[0145] Compared with Example 1, Example 4 performed the polymerization reaction at an excessively high temperature (60°C), which increased the decomposition rate of the electrolyte additive, resulting in increased chromaticity and free acid content of the resulting gel electrolyte. Compared with Example 1, Example 5 had a lower proportion of multifunctional acrylate monomers, resulting in an inability to form a gel electrolyte. Compared with Example 1, Example 6 had a higher dosage of multifunctional acrylate monomers, resulting in a hard texture and significantly reduced ionic conductivity of the formed gel electrolyte. Compared with Example 1, Example 7 had a lower dosage of functionalized monomers, resulting in a good gel electrolyte state, but may cause a reduction in battery thermal safety. Compared with Example 1, Example 8 had a higher dosage of functionalized monomers, resulting in the precipitation of polymers from the electrolyte, and an inability to form a gel electrolyte.
[0146] According to the test methods provided above, the batteries provided in Examples 1 to 7 and Comparative Examples 1 to 3 were subjected to hot box, capacity, charge-discharge cycle performance, and internal resistance tests. The test results are shown in Table 2:
[0147] Table 2
[0148] According to the data in Table 2, Application Examples 1 to 3, due to the use of the preferred gel electrolyte formulation provided by the present invention, have the characteristics of low internal resistance, high discharge capacity, and excellent charge-discharge cycle performance. In addition, they passed the hot box test, indicating good thermal safety performance.
[0149] It can be seen from the data of Application Examples 4 to 7 that the gel electrolyte obtained when the mass ratio of the polymerized monomers is not within the preferred range defined by the present invention will result in a decrease in the electrochemical performance of the battery further prepared therefrom or lead to poor thermal safety.
[0150] From the comparison between comparative application example 1 and application example 1, it can be seen that the electrolyte does not contain monofunctional acrylate monomers, which causes the gel texture to be too hard, thereby leading to an increase in the internal resistance of the battery and a decrease in the charge and discharge cycle performance; from the comparison between comparative application example 2 and application example 1, it can be seen that the electrolyte does not contain multifunctional acrylate monomers, resulting in the inability to form a structurally stable gel electrolyte, which leads to poor thermal safety of the obtained battery; from the comparison between comparative application example 3 and application example 1, it can be seen that the electrolyte does not contain functionalized monomers, resulting in the battery being unable to further form a more structurally stable gel electrolyte at higher temperatures, resulting in slightly inferior thermal safety.
[0151] The applicant states that while the present invention illustrates a low-temperature polymerized gel electrolyte and a battery containing the same through the aforementioned embodiments, the present invention is not limited to these embodiments, nor does it necessarily rely on these embodiments for implementation. Persons skilled in the art should understand that any improvements to the present invention, equivalent substitutions for various raw materials in the present invention's products, additions of auxiliary components, and selection of specific methods, etc., fall within the scope of protection and disclosure of the present invention.
Claims
1. A low temperature polymerized gel electrolyte, characterized in that: The raw material for preparing the low-temperature polymerized gel electrolyte is a gel precursor solution, and the gel precursor solution includes a polymerizable monomer, an electrolyte additive, a thermal initiator, a lithium salt and a solvent; The polymerizable monomers include monofunctional acrylic ester monomers, multifunctional acrylic ester monomers and functional monomers, and the functional monomers contain crosslinking groups and monovinyl groups.
2. The low-temperature polymerized gel electrolyte according to claim 1, characterized in that: The gel precursor solution comprises the following components in parts by weight:
3. The low-temperature polymerized gel electrolyte according to claim 1, characterized in that: The mass ratio of the monofunctional acrylic ester monomer, the multifunctional acrylic ester monomer and the functionalized monomer is 1:(0.5-1.5):(0.1-0.5).
4. The low-temperature polymerized gel electrolyte according to claim 1, characterized in that: The monofunctional acrylic ester monomer includes any one of n-butyl acrylate, isobutyl acrylate, propyl acrylate, polyethylene glycol methacrylate, polyethylene glycol monomethyl ether methacrylate, 2-methoxyethyl acrylate, ethyl acrylate, hexyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, lauryl methacrylate or n-octyl methacrylate, or a combination of at least two thereof; The multifunctional acrylate monomer includes any one of polyethylene glycol dimethacrylate, polyethylene glycol diacrylate, pentaerythritol tetraacrylate, ethoxylated trimethylolpropane triacrylate, ethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate or triethylene glycol diacrylate, or a combination of at least two thereof.
5. The low-temperature polymerized gel electrolyte according to claim 1, characterized in that: The functional monomer includes any one of glycidyl methacrylate, vinyl trimethoxysilane, vinyl triethoxysilane, vinyl triisopropoxysilane or γ-methacryloxypropyl trimethoxysilane, or a combination of at least two thereof.
6. A method for preparing a low-temperature polymerized gel electrolyte as claimed in any one of claims 1 to 5, characterized in that: The method comprises: polymerizing a polymerization monomer, an electrolyte additive, a thermal initiator, a lithium salt and a solvent at 20 to 40° C. for 6 to 24 hours under a nitrogen atmosphere to obtain the gel electrolyte.
7. A battery, characterized in that: The battery comprises a positive electrode, a negative electrode, a separator and the low-temperature polymerized gel electrolyte according to any one of claims 1 to 5.
8. A method for preparing a battery as claimed in claim 7, characterized in that: The method comprises the following steps: (1) Assembling a positive electrode, a negative electrode and a separator to obtain a battery cell; (2) Injecting the raw material for preparing the low-temperature polymerized gel electrolyte as claimed in any one of claims 1 to 5 into the battery cell obtained in step (1), leaving it open and allowing it to stand, passing nitrogen gas, and then sealing it, and subjecting it to in-situ polymerization to obtain the battery.
9. The method according to claim 8, characterized in that The assembly in step (1) is carried out in an air environment with a temperature of 20-25° C. and a humidity of 0-5%.
10. The method according to claim 8, characterized in that The temperature of the in-situ polymerization in step (2) is 20 to 40° C. and the time is 6 to 24 hours.
Citation Information
Patent Citations
Polymer gel electrolyte-electrode, preparation method thereof, supercapacitor and preparation method of supercapacitor
CN113096969A
Gel electrolyte, preparation method thereof, battery using gel electrolyte and preparation method thereof
CN101807717A
Gel electrolyte and composition thereof, flexible lithium ion battery and preparation method of flexible lithium ion battery
CN114069036A
Low-temperature polymerized gel electrolyte and battery containing same
CN116169353A
Non-identical camera based image processing device
KR1020200095758A
Cited By
Composite electrode active material for inhibiting gas production of battery, preparation method of composite electrode active material and composite electrode
CN119812342A