A method for copper metallization for through-glass VIAS and a glass article manufacutured thereof

WO2024217394A1PCT designated stage expired Publication Date: 2024-10-24IND TECH RES INST

Patent Information

Application Number
PCT/CN2024/087935
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-17
Filing Date
2024-04-16
Publication Date
2024-10-24

Smart Images

  • Figure CN2024087935_24102024_PF_FP_ABST
    Figure CN2024087935_24102024_PF_FP_ABST
Patent Text Reader

Abstract

A method for metallizing through-glass vias in a glass substrate includes cleaning and modifying a surface of the glass substrate with a silane. The glass substrate has a thickness t and comprises a plurality of vias extending through the thickness t. The method further includes applying an electroless plating solution comprising a copper ion to deposit a copper seed layer on the surface of the glass and on the sidewall of the plurality of vias; disposing an electrolyte within the plurality of vias; positioning an electrode within the electrolyte and applying a first direct current under potential control mode for a first period of time between the electrode and the glass substrate so as to reduce the copper ions into copper to form a bridge attached on a sidewall and at the central part of each of the plurality of vias; applying a second direct current under current control mode for a second period of time between the electrode and the glass substrate to fill the vias such that each of the plurality of vias is filled with copper.
Need to check novelty before this filing date? Find Prior Art

Description

A METHOD FOR COPPER METALLIZATION FOR THROUGH-GLASS VIAS AND A GLASS ARTICLE MANUFACUTURED THEREOF

[0001] CROSS REFERENCE TO RELATED APPLICATION

[0002] This application claims the benefit of priority of Chinese Patent Application Serial No.202310408740.8 filed on April 17, 2023, the content of which is relied upon and incorporated herein by reference in its entirety.BACKGROUNDFIELD

[0003] The present specification generally relates to the manufacture of through-glass vias and, more specifically, to copper metallization of through-glass vias.

[0004] TECHNICAL BACKGROUND

[0005] Through-substrate vias provide electrical connections between layers in a physical electronic circuit or chip. For example, in a three-dimensional stacked integrated circuit, the through-substrate vias enable integration of electronic components both vertically and horizontally. Conventionally, through-substrate vias are used in organic and silicon substrates. However, because glass is less expensive than silicon, glass substrates are becoming more prevalent in electronic devices. Glass substrates may also provide improved electromagnetic loss properties, improved dielectric properties, tailorable coefficients of thermal expansion, and the ability to come in scalable form factors, including roll-to-roll forms. With all the advantages mentioned above, and the need for smaller via diameters which leads to high aspect ratio, the realization of Cu metallization in the vias is critical for such applications.

[0006] Conventional processes for metallizing vias include dry processes and wet processes. Dry processes, such as physical vapor deposition (PVD) and chemical vapor deposition (CVD) , are carried out in an environment under vacuum, which limits throughput and adds to manufacturing costs. Additionally, such dry processes may be limited in terms of their ability to produce a continuous metal layer within vias of glass substrates with aspect ratios greater  than 5, wherein the aspect ratio is the ratio of the thickness of the glass substrate to the average diameter of the vias, particularly where the via diameter is small (e.g., less than 50 μm) . Wet processes, such as electroless plating, are cost effective compared to dry processes, but have been conventionally limited to use on vias with large diameters (e.g., greater than 75 μm) .

[0007] Accordingly, a need exists for alternative methods for metallizing through-glass vias having small diameters and high aspect ratios.SUMMARY

[0008] According to various aspects disclosed herein, a method for metallizing through-glass vias in a glass substrate includes cleaning and applying a surface of the glass substrate and a sidewall of a plurality of vias with a silane. The glass substrate has a thickness t and comprises a plurality of vias extending through the thickness t. The method further includes applying an electroless plating solution comprising copper ions to deposit a copper seed layer on the surface of the glass and on the sidewall of the plurality of vias, disposing an electrolyte within the plurality of vias, wherein the electrolyte comprises copper ions to be deposited on the copper seed layer within the plurality of vias; positioning an electrode within the electrolyte; applying a first direct current under potential control mode for a first period of time between the electrode and the glass substrate, so as to reduce the copper ions into copper to form a bridge attached on a sidewall and at the central part of each of the plurality of vias; and applying a second direct current under current control mode for a second period of time between the electrode and the glass substrate to fill the vias such that each of the plurality of vias is filled with copper.

[0009] Another aspect includes the method of the previous aspect, wherein the thickness t of the glass substrate is greater than or equal to 50 μm and less than or equal to 1200 μm.

[0010] Another aspect includes the method of any of the previous aspects, wherein the thickness t of the glass substrate is greater than or equal to 200 μm and less than or equal to 400 μm.

[0011] Another aspect includes the method of any of the previous aspects, wherein the plurality of vias has an average diameter of greater than or equal to 8 μm and less than or equal to 30 μm;and an aspect ratio of the thickness t of the glass substrate to the average diameter of the plurality of vias is greater than 12: 1 and less than or equal to 150: 1.

[0012] Another aspect includes the method of any of the previous aspects, wherein the first electrolyte comprises a first additive. The first additive comprises a suppressor. In another aspect, the first additive further comprises a leveler.

[0013] Another aspect includes the method of any of the previous aspects, wherein the second electrolyte comprises a second additive consists of a suppressor, an accelerator, and a leveler. The suppressor is present in the first electrolyte in a concentration of greater than or equal to 100 ppm and less than or equal to 500 ppm.

[0014] Another aspect includes the method of the previous aspect, wherein the second additive consists of a suppressor, an accelerator and a leveler; wherein the accelerator is selected from at least one of bis- (sodium sulfopropyl) -disulfide (SPS) and 3-Mercapto-1-propanesulfonic acid (MPS) ; the suppressor is diamine comprises x is selected from at least one of co-polymer of polypropylene glycol and polyethylene glycol; y is selected from at least one of methylene, vinyl and propylene.

[0015] Another aspect includes the method of the previous aspect, wherein the suppressor is selected from polyethylene glycol and copolymer of polypropylene glycol and polyethylene glycol.

[0016] Another aspect includes the method of the previous aspect, wherein the suppressor is ethylenediamine tetrakis (ethoxylate-block-propoxylate) tetrol.

[0017] Another aspect includes the method of any of the previous aspects, wherein the electrolyte further comprises halide ions and an additive. The halide ions are present in the electrolyte in a concentration of greater than or equal to 1 ppm and less than or equal to 20 ppm.

[0018] Another aspect includes the method of any of the previous aspects, wherein the suppressor is present in the electrolyte in a concentration of greater than or equal to 100 ppm and less than or equal to 500 ppm.

[0019] Another aspect includes the method of any of the previous aspects, wherein applying the current under potential control mode comprises applying the current at a voltage of greater than or equal to 0.4 volt and less than or equal to 0.8 volt relative to a mercury- mercurous sulfate electrode potential for a period of greater than or equal to 10 min and less than or equal to 200 min.

[0020] Another aspect includes the method of any of the previous aspects, wherein applying the current under current control mode comprises applying the current at a current density of greater than or equal to 0.02 amps / dm2 and less than or equal to 2 amps / dm2 for a period of greater than or equal to 30 min and less than or equal to 500 min.

[0021] Another aspect includes the method of any of the previous aspects, wherein the vias filled with copper has a defect ratio of less than 4.8%.

[0022] Another aspect includes the method of any of the previous aspects, further comprising applying an adhesion layer on the surface of the glass substrate or / and in the plurality of vias before applying a silane on a surface of the glass substrate.

[0023] Another aspect includes the method of any of the previous aspects, wherein an adhesion layer comprises titanium / copper.

[0024] Another aspect includes the method of any of the previous aspects, wherein an adhesion layer comprises metal oxide or polyimide.

[0025] Another aspect includes the method of any of the previous aspects, wherein the copper in each of the plurality of vias is free of voids.

[0026] Another aspect includes the method of any of the previous aspects, further comprising cleaning the glass substrate prior to functionalizing the surface, wherein the glass substrate has a water contact angle of less than or equal to 5 degrees after the cleaning.

[0027] Another aspect includes the method of any of the previous aspects, further comprising annealing the glass substrate comprising the copper seed layer prior to disposing the electrolyte within the plurality of vias.

[0028] According to another aspect, a glass article includes a glass substrate having a first major surface and a second major surface opposite the first major surface and separated from the first major surface by a thickness of greater than or equal to 50 μm and less than or equal to 1200 μm; and a plurality of vias extending through the glass substrate from the first major surface to the second major surface, wherein the plurality of vias have an average diameter of greater than or equal to 8 μm and less than or equal to 30 μm; an aspect ratio of the thickness  of the glass substrate to the average diameter of the plurality of vias is greater than 12: 1 and less than or equal to 150: 1; the central part of each of the plurality of vias is filled with copper and form a bridge attached on a sidewall of the each of the plurality of vias; a thickness of a center of the bridge is greater than or equal to half of the average diameter of the plurality of vias; and a thickness of a sidewall of the bridge is less than or equal to three times of the thickness of the center of the bridge.

[0029] Another aspect includes the glass article of the previous aspect, wherein the thickness of a sidewall of the bridge is less than or equal to two times of the thickness of the center of the bridge;

[0030] Another aspect includes the glass article of the previous aspect, wherein the copper in each of the plurality of vias is free of voids.

[0031] Another aspect includes the glass article of the previous aspect, wherein the thickness of the glass substrate is greater than or equal to 50 μm and less than or equal to 1200 μm.

[0032] Another aspect includes the glass article of the previous aspect, wherein the surface of the glass substrate is deposited with a copper layer with a thickness t1 after the plurality of vias is filled with copper; wherein the thickness t1 is greater than or equal to 0.2 um and less than or equal to 10 um.

[0033] Additional features and advantages will be set forth in the detailed description which follows, and in part will be readily apparent to those skilled in the art from that description or recognized by practicing the embodiments described herein, including the detailed description which follows, the claims, as well as the appended drawings.

[0034] It is to be understood that both the foregoing general description and the following detailed description describe various embodiments and are intended to provide an overview or framework for understanding the nature and character of the claimed subject matter. The accompanying drawings are included to provide a further understanding of the various embodiments and are incorporated into and constitute a part of this specification. The drawings illustrate the various embodiments described herein, and together with the description serve to explain the principles and operations of the claimed subject matter.BRIEF DESCRIPTION OF THE DRAWINGS

[0035] FIG. 1 schematically depicts a cross-section of a glass substrate including a plurality of vias in accordance with one or more embodiments shown and described herein;

[0036] FIG. 2 Method for metallizing the plurality of vias in accordance with one or more embodiments shown and described herein;

[0037] FIG. 3 schematically depicts a cross-section of a glass substrate having a seed layer deposited thereon in accordance with one or more embodiments shown and described herein;

[0038] FIG. 4 schematically depicts a cross-section of a glass substrate in which the electroplated electrically conductive material forms a bridge attached on a sidewall and at the central part of each of the plurality of vias in accordance with one or more embodiments shown and described herein;

[0039] FIG. 5 schematically depicts a cross-section of a bridge attached on a sidewall and at the central part of each of the plurality of vias in accordance with one or more embodiments shown and described herein;

[0040] FIG. 6 schematically depicts a cross-section of a glass substrate in which the plurality of vias are filled with electrically conductive material in accordance with one or more embodiments shown and described herein;

[0041] FIG. 7A is an SEM image showing the formation of a bridge formed from the copper in the glass substrate having an aspect ratio of 12.5 in accordance with one or more embodiments shown and described herein;

[0042] FIG. 7B is a CT scan image further evidencing the formation of the plug formed from the copper within the vias in accordance with one or more embodiments shown and described herein;

[0043] FIG. 7C is a CT scan image showing the formation of a bridge formed from the copper in a glass substrate having an aspect ratio of 34 in accordance with one or more embodiments shown and described herein;

[0044] FIG. 8A is a XRM image showing the complete and void-free filling of the 10 μm vias with the copper in accordance with one or more embodiments shown and described herein;

[0045] FIG. 8B is another XRM image showing the complete and void-free filling of the 10 μm vias with the copper in accordance with one or more embodiments shown and described herein;

[0046] FIG. 9A is a SEM image showing the incomplete filling of the 10 μm vias with the copper;

[0047] FIG. 9B is additional SEM images further evidencing incomplete filling within the vias.DETAILED DESCRIPTION

[0048] Reference will now be made in detail to various embodiments, examples of which are illustrated in the accompanying drawings. Whenever possible, the same reference numerals will be used throughout the drawings to refer to the same or like parts.

[0049] Unless otherwise expressly stated, it is in no way intended that any method set forth herein be construed as requiring that its steps be performed in a specific order, nor that with any apparatus specific orientations be required. Accordingly, where a method claim does not actually recite an order to be followed by its steps, or that any apparatus claim does not actually recite an order or orientation to individual components, or it is not otherwise specifically stated in the claims or description that the steps are to be limited to a specific order, or that a specific order or orientation to components of an apparatus is not recited, it is in no way intended that an order or orientation be inferred, in any respect. This holds for any possible non-express basis for interpretation, including: matters of logic with respect to arrangement of steps, operational flow, order of components, or orientation of components; plain meaning derived from grammatical organization or punctuation, and the number or type of embodiments described in the specification.

[0050] As used herein, the singular forms “a, ” “an” and “the” include plural referents unless the context clearly dictates otherwise. Thus, for example, reference to “a” component includes aspects having two or more such components, unless the context clearly indicates otherwise. Also, the word “or” when used without a preceding “either” (or other similar language indicating that “or” is unequivocally meant to be exclusive –e.g., only one of x or y, etc. ) shall be interpreted to be inclusive (e.g., “x or y” means one or both x or y) .

[0051] The term “and / or” shall also be interpreted to be inclusive (e.g., “x and / or y” means one or both x or y) . In situations where “and / or” or “or” are used as a conjunction for a group of  three or more items, the group should be interpreted to include one item alone, all the items together, or any combination or number of the items. Moreover, terms used in the specification and claims such as have, having, include, and including should be construed to be synonymous with the terms comprise and comprising.

[0052] Unless otherwise indicated, all numbers or expressions, such as those expressing dimensions, physical characteristics, and the like, used in the specification (other than the claims) are understood to be modified in all instances by the term “approximately. ” At the very least, and not as an attempt to limit the application of the doctrine of equivalents to the claims, each numerical parameter recited in the specification or claims which is modified by the term “approximately” should be construed in light of the number of recited significant digits and by applying ordinary rounding techniques.

[0053] All disclosed ranges are to be understood to encompass and provide support for claims that recite any and all subranges or any and all individual values subsumed by each range. For example, a stated range of 1 to 10 should be considered to include and provide support for claims that recite any and all subranges or individual values that are between and / or inclusive of the minimum value of 1 and the maximum value of 10; that is, all subranges beginning with a minimum value of 1 or more and ending with a maximum value of 10 or less (e.g., 5.5 to 10, 2.34 to 3.56, and so forth) or any values from 1 to 10 (e.g., 3, 5.8, 9.9994, and so forth) .

[0054] All disclosed numerical values are to be understood as being variable from 0-100%in either direction and thus provide support for claims that recite such values or any and all ranges or subranges that can be formed by such values. For example, a stated numerical value of 8 should be understood to vary from 0 to 16 (100%in either direction) and provide support for claims that recite the range itself (e.g., 0 to 16) , any subrange within the range (e.g., 2 to 12.5) or any individual value within that range (e.g., 15.2) .

[0055] The drawings shall be interpreted as illustrating one or more embodiments that are drawn to scale and / or one or more embodiments that are not drawn to scale. This means the drawings can be interpreted, for example, as showing: (a) everything drawn to scale, (b) nothing drawn to scale, or (c) one or more features drawn to scale and one or more features not drawn to scale. Accordingly, the drawings can serve to provide support to recite the sizes, proportions, and / or other dimensions of any of the illustrated features either alone or relative to each other. Furthermore, all such sizes, proportions, and / or other dimensions are to be  understood as being variable from 0-100%in either direction and thus provide support for claims that recite such values or any and all ranges or subranges that can be formed by such values.

[0056] The terms recited in the claims should be given their ordinary and customary meaning as determined by reference to relevant entries in widely used general dictionaries and / or relevant technical dictionaries, commonly understood meanings by those in the art, etc., with the understanding that the broadest meaning imparted by any one or combination of these sources should be given to the claim terms (e.g., two or more relevant dictionary entries should be combined to provide the broadest meaning of the combination of entries, etc. ) subject only to the following exceptions: (a) if a term is used in a manner that is more expansive than its ordinary and customary meaning, the term should be given its ordinary and customary meaning plus the additional expansive meaning, or (b) if a term has been explicitly defined to have a different meaning by reciting the term followed by the phrase “as used in this document shall mean” or similar language (e.g., “this term means, ” “this term is defined as, ” “for the purposes of this disclosure this term shall mean, ” etc. ) . References to specific examples, use of “i.e., ” use of the word “invention, ” etc., are not meant to invoke exception (b) or otherwise restrict the scope of the recited claim terms. Other than situations where exception (b) applies, nothing contained in this document should be considered a disclaimer or disavowal of claim scope.

[0057] In the three-dimensional integrated circuit (3D-IC) industry, stacking devices is a technique being used to increase device performance in a limited space. The performance of the integrated circuit may be further enhanced through the use of smaller vias, which leads to higher aspect ratios (e.g., aspect ratios the thickness of the glass substrate to the average diameter of the via of greater than or equal to 4: 1) . However, the higher the aspect ratio, the more difficult it is to metallize the sidewalls of the vias, particularly when the vias have small (e.g., less than or equal to 50 μm) diameters, which may lead to voids within the electrically conductive material within the vias after filling.

[0058] The methods of the present disclosure enable through-glass vias to be filled with an electrically conductive material, such as copper or another metal, despite the challenges associated with the glass substrate having an aspect ratio of greater than 12: 1. As used herein, the term “aspect ratio” refers to the ratio of the thickness t of the glass substrate to the average diameter of the plurality of vias. For example, by utilizing a method that includes a wet  electroless plating step in conjunction with a wet electroplating step, the challenges associated with metallizing vias with a high aspect ratio in a glass substrate may be mitigated.

[0059] In the embodiment shown in FIG. 1, the glass article is in the form of a glass substrate 102 that includes a plurality of vias 104, or precision holes, defined by one or more sidewalls 105. For example, in the embodiments described herein, the vias 104 are circular in cross section and, as such, the vias 104 have a single sidewall 105. However, it should be understood that vias with other cross-sectional geometries are contemplated include, for example vias which have more than one sidewall. The glass substrate 102 may be used, for example, as an interposer to provide vertical electrical connections within a three-dimensional integrated circuit. The glass substrate 102 comprises a first face 110 and a second face 112 opposite the first face 110. The first face 110 of the glass substrate 102 is separated from the second face 112 of the glass substrate 102 by a thickness t of the glass substrate.

[0060] The composition of the glass substrate 102 is not particularly limited and may be selected based on the desired end use of the glass substrate 102. In some embodiments, the glass substrate 102 may be a flexible glass substrate. The glass substrate 102 may be formed from glasses suitable for electronics applications including, for example,  Eagle XGTM glass, manufactured by Corning, Inc. However, it should be understood that other glasses are contemplated and possible. For example, other types of ion-exchangeable glasses or fused silica may be used to form the glass substrate 102. Additionally, the glass substrate 102 may be in the shape of a wafer having a 10 cm, 15 cm, 20 cm, 30 cm, or 50cm diameter, for example. However, it should be understood that glass substrates 102 of other dimensions are contemplated and possible. The thickness of the glass substrate 102 may also vary depending on its end use, although in various embodiments, the thickness t of the glass substrate is greater than or equal to 50 μm and less than or equal to 1200 μm. For example, the glass substrate 102 may have a thickness of from greater than or equal to 200 μm and less than or equal to 400 μm. In various embodiments, the glass substrate 102 has a thickness of more than or equal to about 300 μm. However, it should be understood that glass substrates of any suitable thickness may be utilized. In some embodiments, the thickness of the glass substrate may be measured through interferometric methods at locations within the area of the substrate. Additionally, or alternatively, mechanical means (e.g., calipers) may be used to measure the thickness of the glass substrate. Unless otherwise specified, thickness of the glass substrate is measured by interferometric methods.

[0061] The plurality of vias 104 can be formed in the glass substrate 102 by any suitable method. For example, in some embodiments, the plurality of vias 104 may be drilled in the glass substrate 102 using a pulsed laser. The laser may be any laser having suitable optical properties for drilling through the glass substrate 102 as well as a sacrificial cover layer positioned on a surface of the glass substrate 102. Suitable lasers include, without limitation, ultra-violet (UV) lasers, such as frequency tripled neodymium doped yttrium orthovanadate (Nd: YVO4) lasers, which emit a beam of coherent light having a wavelength of about 355 nm. The beam of the laser may be directed onto a predetermined location on the surface of the glass substrate and pulsed to form each of the plurality of vias 104 in the glass substrate 102. Alternatively, the plurality of vias may be mechanically machined.

[0062] In some embodiments, a diameter of an opening of a via in face 110 of the glass substrate 102 and a diameter of an opening of the via in face 112 of the glass substrate 102 may be the same such that the via is cylindrical. Alternatively, a diameter of an opening of a via in face 110 of the glass substrate 102 and a diameter of an opening of the via in face 112 of the glass substrate 102 may differ by 2 μm or less, such that the via is substantially cylindrical. In other embodiments, a diameter of the vias may decrease from one face of the glass substrate 102 to the other face of the glass substrate 102 such that the vias have a cone shape. In various embodiments, each of the plurality of vias has an average diameter of greater than or equal to 8 μm and less than or equal to 30 μm, or greater than or equal to 8 μm and less than or equal to 15 μm. For example, each of the plurality of vias may have an average diameter of about 20 μm, about 15 μm, about 12 μm, or about 10 μm. As used herein, the term “average diameter” refers to the diameter of the via normal to the axis of the via through the thickness of the glass, averaged along the axis of the via. In some embodiments, the average diameter is measured using an SEM cross-section or visual metrology from the top / bottom side (e.g., averaging the top, waist (or some location within the via within the thickness of the glass) , and the bottom) . Unless otherwise specified, the average diameter is measured using an SEM cross-section.

[0063] According to various embodiments, the aspect ratio is greater than or equal to 12: 1, or greater than or equal to 20: 1. For example, the aspect ratio may be greater than 12: 1 and less than or equal to 150: 1, or greater than or equal to 20: 1 and less than or equal to 80: 1. or greater than or equal to 30: 1 and less than or equal to 50: 1.

[0064] In the embodiments described herein, the plurality of vias 104 is filled with an electrically conductive material 500 (shown in FIG. 6) . The electrically conductive material  may be, by way of example and not limitation, copper, silver, aluminum, nickel, alloys thereof, and combinations thereof. In some embodiments, the plurality of vias 104 is filled with a copper-containing material, such as a copper alloy. In some embodiments, the surface of the glass substrate is deposited with a copper layer with a thickness t1. The thickness t1 is greater than or equal to 0.2 um and less than or equal to 10 um. In some embodiments, the thickness t1 is greater than or equal to 0.5 um and less than or equal to 2 um. In various embodiments, the electrically conductive material in each of the plurality of filled vias has a defect ratio of less than 4.8%, less than or equal to 3%, less than or equal to 2%, or even less than or equal to 1%by volume. In some embodiments, the electrically conductive material in each of the plurality of filled vias is free of defections (i.e., voids, seams, discontinuous fillings) . In some embodiments herein, the defect ratio is measured based on analysis of a scanning electron microscope (SEM) cross-section image or an X-ray CT scan. Unless otherwise specified, the defect ratio is measured based on analysis of an SEM cross-section. Accordingly, “free of defections” and “substantially defection-free” mean that there are no voids or seams or discontinuous filings visible according to the resolution of the imaging equipment.

[0065] FIG. 2 depicts one embodiment of a method 200 for filling, or metallizing, the vias with the electrically conductive material. In particular, as shown in FIG. 2, the method generally includes cleaning a surface of the glass substrate (step 201) , modifying the surface of the glass substrate (step 203) , applying an electroless plating solution to deposit a seed layer on the functionalized surface (step 204) , wetting the glass substrate including the seed layer (step 206) , positioning an electrode and applying a first direct current under potential control mode in a first electrolyte for a first period of time between the electrode and the glass substrate, so as to reduce the copper ions into copper to form a bridge attached on a sidewall and at the central part of each of the plurality of vias (step 207) ; and applying a second direct current under current control mode in a second electrolyte for a second period of time between the electrode and the glass substrate to fill the vias such that each of the plurality of vias is filled with copper (step 208) .

[0066] In some embodiments, the method 200 is performed as a wet process that enables the electrically conductive material to be substantially void-free manner without the use of a temporary carrier, thereby enabling the method 200 to be employed in roll-to-roll manufacturing processes.

[0067] In some embodiments, cleaning may be performed according to any conventional cleaning process known and used in the art to remove organic residues and enrich hydroxyl groups on the surface of the glass substrate. For example, the glass substrate may be cleaned by a process such as O2 plasma, UV-ozone, or RCA cleaning to remove organics and other impurities (metals, for example) that would interfere with the silane reacting with the surface silanol groups. Washes based on other chemistries may also be used, for example, HF or H2SO4 wash chemistries. In some embodiments, the glass substrate may be cleaned with a detergent in an ultrasonic bath and rinsed with deionized water. In various embodiments, the glass substrate has a water contact angle of less than or equal to 7 degrees, less than or equal to 6 degrees, less than or equal to 5 degrees after cleaning, less than or equal to 4 degrees, or less than or equal to 2 degrees as measured using an goniometer, such as DSA100 available from Kruss GmbH (Germany) .

[0068] In some embodiments, prior to functionalizing the surface of the glass substrate, the glass substrate may be optionally applied with an adhesion layer (optional step 202) . At step 202. In some embodiments, the adhesion layer is sputtered titanium / copper. In some embodiments, the adhesion layer is applied on the surface of the glass substrate through solution processed metal oxide or polyimide. In some embodiments, the adhesion layer is applied on the surface of the glass substrate 102 and one or more of the sidewall (s) 105 of the plurality of vias 104, the first surface 110 of the glass substrate 102, and the second surface 112 of the glass substrate 102. In some embodiments, the adhesion layer is partial applied in the vias. The adhesion layer can increase the hermeticity and reliability of the samples.

[0069] At step 203, the surface of the glass substrate 102 is functionalized with a silane. In some embodiments, the surface of the glass substrate 102 that is functionalized includes at least a portion of one or more of the sidewall (s) 105 of the plurality of vias 104, the first surface 110 of the glass substrate 102, and the second surface 112 of the glass substrate 102. Silanes are chosen so as to produce a suitable surface energy on the functionalized surfaces, and so as to have sufficient thermal stability upon exposure to elevated temperatures experienced by the glass substrate 102 in downstream processing. Suitable silanes may include, by way of example and not limitation, cationic silanes or polymers, such as 3- (2-aminoethylamino) propyldimethoxy-methylsilane. Moreover, in various embodiments, silane modification of the surface of the glass substrate modifies the glass surface to have a positive  charge and enables binding of the palladium (Pd) used in the electroless plating to the surface of the glass substrate, as will be described in greater detail below.

[0070] In some embodiments, the surface modification is performed by diluting a silane in isopropanol to form a silane solution and submerging the glass substrate in the silane solution. Optionally, ultrasonic energy is applied to the silane solution with the submerged glass substrate and the glass substrate to enhance wetting and bubble removal. In some embodiments, the glass substrate is soaked in the silane solution for a predetermined period of time. For example, the glass substrate may be submerged in the silane solution for a period of time of greater than or equal to 15 minutes, greater than or equal to 20 minutes, or greater than or equal to 30 minutes. After soaking in the silane solution, the glass substrate may be dried, for example, in an oven. While one example of a modification process is described herein, it should be understood that other modification processes are contemplated, provided that such processes are effective to adsorb the silane to the surface of the glass substrate. In some embodiments, the glass substrate may be heated to control the surface hydroxyl concentration prior to modification, and / or may be heated after silane application to complete silane condensation with the hydroxyl groups on the surface of the glass substrate.

[0071] After modification, at step 204, electroless plating is used to deposit a seed layer 300 of a conductive material (e.g., a copper seed layer) on the surface of the glass substrate, as depicted in FIG. 3. In the embodiments described herein, the deposition of the seed layer renders the surfaces of the glass substrate electrically conductive, enabling an electroplating technique to be used to fill the vias with electrically conductive material. In particular, the seed layer 300 is deposited on the silane-modified surface 305 of the glass substrate 102. In some embodiments, commercially available kits and / or electroless plating solutions may be employed to deposit the seed layer 300. For example, in some embodiments, the glass substrate may be dipped into a catalyst mixture, such as a Pd / Sn colloid, and then rinsed. A coating of the catalyst mixture remains on the surfaces of the glass substrate after the rinsing. The catalyst on the surfaces of the glass substrate may then be activated, such as through removal of the Sn shell from the Pd. The activation may include, for example, dipping the glass substrate into an activation solution including fluoroboric acid and boric acid. Commercially available activation solutions include those available from Uyemura. After the catalyst is activated, the glass substrate may be dipped into an electroless plating bath to form the seed layer on the surface of the glass substrate. In some embodiments, the seed layer 300 is formed on at least  the sidewalls 105 of each of the plurality of vias 104, although it is contemplated that the seed layer 300 may additionally be formed on the first surface 110, the second surface 112 of the glass substrate 102, as shown in FIG. 3.

[0072] At optional step 205, the glass substrate may be optionally thermally annealed after the seed layer is deposited thereon to relieve stresses in the glass substrate and thereby reduce the impact of any downstream thermal processing steps which may otherwise affect the dimensional stability of the glass substrate materials, such as electrically conductive materials, deposited on the glass substrate. In some embodiments, the glass substrate may be heated to a temperature of greater than or equal to 400 ℃ for a period sufficient to relieve the stresses in the glass substrate.

[0073] Returning to FIG. 2, the glass substrate is wetted (step 206) following deposition of the seed layer and optional annealing. In some embodiments, the glass substrate is wetted by submerging the glass substrate including the seed layer in water to ensure that each of the vias is wetted. For example, the glass substrate may be dipped into deionized water for a period of greater than or equal to 2 minutes. In some embodiments, ultrasonic energy may be applied to the glass substrate while the glass substrate is submerged in the water to enhance wetting and bubble removal. Without being bound by theory, it is believed that wetting the glass substrate prior to electroplating ensures that the vias are pre-wetted thereby preventing bubbles from being trapped within the vias, which bubbles may create voids in the conductive material subsequently filled within the vias.

[0074] After the glass substrate is wetted at step 206, 2-step electroplating (step 207 and step 208) is carried out. In particular, an electrolyte is disposed within the plurality of vias. For example, the glass substrate may be submerged in an electrolyte solution such that the electrolyte enters the vias. The electrolyte includes ions of the electrically conductive material, for example, copper ions, to be deposited on the seed layer.

[0075] Electroplating is carried out by positioning one or more electrodes within the electrolyte. In various embodiments, two electrodes, three electrodes, or more can be positioned within the electrolyte. For example, in some embodiments, three electrodes are employed. In these embodiments, the glass substrate including the seed layer is the working electrode, or cathode, and the other two electrodes are anodes. In such embodiments, the anodes may be positioned on opposite sides of the glass substrate such that plating of the electrically conductive material  may be conducted symmetrically from both sides of the glass substrate. The anodes may be, by way of example and not limitation, copper plates. While a specific configuration of the electrodes is described herein, it should be understood that other configurations are contemplated and possible.

[0076] Thereafter, step 207 is carried out by applying a first direct current under potential control mode in a first electrolyte for a first period of time between the electrode and the glass substrate, so as to reduce the copper ions into copper to form a bridge attached on a sidewall and at the central part of each of the plurality of vias (step 207) . FIG. 5 and FIG. 7A-7C show the formation of the bridge, the thickness of a center of the bridge is greater than or equal to half of the average diameter of the plurality of vias; and the thickness of an end of the bridge is less than or equal to three times of the thickness of the center of the bridge. This short bridge shows better uniformity compared with a longer bridge resulting less chance to form defects in the glass articles.

[0077] Then by applying a second direct current under current control mode in a second electrolyte for a second period of time between the electrode and the glass substrate, the plurality of vias is filled with copper (step 208) . In some embodiments in which the electrolyte includes copper ions, the copper ions are reduced into copper within the plurality of vias such that each of the plurality of vias is filled with copper. In some particular embodiments, the electrolyte is an electrolyte bath consisting of CuSO4, H2SO4, chloride ions, and NTB. In such embodiments, the CuSO4 provides a source of copper ions, while the H2SO4 makes the bath conductive and acts as a charge carrier.

[0078] In some embodiments, the first direct current is applied at a voltage of greater than or equal to 0.5 volt and less than or equal to 0.8 volt relative to a mercury-mercurous sulfate electrode potential. The second direct current comprises a current at a current density of greater than or equal to 0.02 amps / dm2 and less than or equal to 2 amps / dm2. The current density is a measure of the total current passed over a time period divided by the total surface area over which the deposition took place. In various embodiments, the total surface is a summation of the first and second surfaces of the glass substrate and the interior surface areas of the vias. The current density, in various embodiments, is constant. However, the current density may be varied during the electroplating process.

[0079] In the first electroplating process (step 207) , as shown in FIG. 4, when vias are being filled with copper, the copper tends to begin to deposit on the walls at the center of the via where it plugs at the center forming a “bridge” or two vias. In the second electroplating process (step 208) , the two vias fill to complete the deposition of the through-glass vias. Without being bound by theory, at the step 207, the copper particles tend to deposit and build up along the center of the via sidewall as opposed to along the entrance to the via, which can seal up the via and result in voids within the copper material, particularly when coupled with the effects of the leveler in the electrolyte, which suppresses copper deposition near the entrance to the via, as described above.

[0080] After formation of the plug, or bridge 400, a second direct current may be applied under current control mode in a second electrolyte for a second period of time to continue filling the conductive material toward the open ends of the vias. In particular, the current density may be increased following the formation of the bridge 400 to fill the vias to improve throughput efficiency, since the diffusion limitation has decreased significantly.

[0081] In some embodiments, both the first electrolyte and the second electrolyte comprise ions of the electrically conductive material (e.g., copper ions) in addition to halide ions. The halide ions combine with the organic species in the solution to form a complex that slows down the plating rate. The halide ions may be present in a concentration of greater than or equal to 1 ppm and less than or equal to 20 ppm in the electrolyte or greater than or equal to 5 ppm and less than or equal to 15 ppm. In some embodiments, the halide ions are chloride ions. For example, the chloride ions may be present in a concentration of 20 ppm, 10 ppm, 8 ppm, 5 ppm, or even 1ppm.

[0082] In some embodiments, the first electrolyte further comprises a first additive. In some embodiments, the additive is a suppressor, such as is diamine with a structure of  x is selected from at least one of co-polymer of polypropylene glycol and polyethylene glycol; y is selected from at least one of methylene, vinyl and propylene. In some embodiments, the suppressor is selected from polyethylene glycol and copolymer of  polypropylene glycol and polyethylene glycol as shown in Table 2. In some embodiments, the suppressor is ethylenediamine tetrakis (ethoxylate-block-propoxylate) tetrol (Tetronic 701) or polyethylene glycol (PEG) . Inhibition of the Cu deposition requires co-adsorption of halide with the suppressor. Without being bound by theory, a complex film composed of PEG, Cu+, and Cl-and strongly adsorbed on the copper surface to provide an inhibition effect on surface. The leveler strong adsorbed and physically block the surface. It particularly prefers to adsorb on protrusion position with high electron density while plating. So, it inhibits Cu deposition at via entry as well. The absorption of leveler and suppressor are decreased along the depth of via due to concentration gradient. This results in a faster Cu deposition at the center position of through glass via. In some embodiments, the first electrolyte further comprises a leveler, such as azolium compound. In some embodiments, nitrotetrazolium blue chloride (NTB) is selected as leveler. The leveler may enhance current density in the center of the via and help control surface morphology of the deposited electrically conductive material. In addition, the leveler may possess several physiochemical characteristics, such as a potential-dependent electrochemical desorption or breakdown and a mass-transfer controlled electrochemical adsorption. The mass-transfer controlled electrochemical adsorption may create a concentration gradient of the leveler from the opening to the center of the via during plating. Without being bound by theory, it is believed that the physiochemical characteristics of the leveler, and in particular, the NTB, enable the copper particles to adsorb to the via sidewalls and suppress deposition of the electrically conductive material near the opening of the vias at a greater rate than near the center of the vias. In some embodiments, the suppressor is present in the first electrolyte in a concentration of greater than or equal to 100 ppm and less than or equal to 500 ppm. The leveler is present in the first electrolyte in a concentration of greater than or equal to 10 ppm and less than or equal to 200 ppm. )

[0083] In some embodiments, the second electrolyte further comprises a second additive consists of a suppressor, an accelerator and a leveler. In some embodiments, the accelerator is bis- (sodium sulfopropyl) -disulfide. In some embodiments, the accelerator is 3-Mercapto-1-propanesulfonic acid (MPS) . In some embodiments, the accelerator is added into the first electrolyte to form the second electrolyte. Without being bound by theory, researchers believe that the acceleration effect of MPS or SPS on Cu2+ reduction is caused by their interaction with chloride ion, namely, a chemically synergistic effect. Some researchers believe that accelerator adsorb to the Cu surface and compete for space with the suppressor and therefore it speeds up the Cu deposition. In addition, accelerator being a small molecule would have higher diffusion  coefficient. This leads to a gradient in surface coverage where the top of the via has high surface concentrations of suppressor and low surface concentrations of accelerant. Halide ions (e.g. Chloride ions) must be present in plating bath for suppressor to adsorb to electrode surface by the thiol end. Table 1 listed the molecular weight (MW) and structures of some additives in accordance with one or more embodiments.

[0084] Table 1. The molecular weight (MW) and structures of additives in accordance with one or more embodiments

[0085] Table 2. Different structures of copolymer of PEG and PPG in accordance with one or more embodiments

[0086] In some embodiments, the electroplated glass substrate may be thermally annealed (not shown in FIG. 2) after the electrically conductive material is deposited thereon to relieve the  stress in the glass substrate and reduce the impact of any downstream thermal processing steps. For example, the glass substrate may be heated to a temperature of greater than or equal to 400 ℃ for a time period sufficient to release the stresses. In various embodiments, after being filled with the electrically conductive material, the electrically conductive material in each of the plurality of vias has a defect ratio of less than or equal to 5%or less than or equal to 1%. In particular embodiments, the electrically conductive material in each of the plurality of vias is free of defections after being filled with the electrically conductive material.

[0087] Examples

[0088] The following examples illustrate one or more features of the embodiments described herein.

[0089] Glass substrates (HPFSTM glass available from Corning, Incorporated) having a thickness t of 340 μm and including 25 μm or 10 μm diameter vias were cleaned using a standard cleaning process. In particular, the substrates were cleaned with 2.5 vol%of PK-LCG225X-1 detergent at 70 ℃ for 8 minutes in an ultrasonic bath. The substrates were then rinsed with deionized water to remove organic residues and enrich hydroxyl groups on the substrate surfaces. After cleaning, the glass substrates showed good wettability with a water contact angle of less than 5 ° as measured using a DSA100 from Kruss GmbH (Germany) .

[0090] Next, adhesion layer is applied on the surface of the glass substrate. In some embodiments, a cleaned glass substrate is deposited Ti / Cu (100 nm / 200 nm) by physical vapor deposition in double sides to form an adhesion layer. Ti was deposited on glass in vacuum and followed by depositing Cu on top of Ti without breaking the vacuum. This process creates an oxide interface between Ti-glass and a metallic interface between Ti-Cu as an adhesion layer. This adhesion layer is deposited only covers a portion of the length in via sidewall (on both sides after double sides deposition) . In some embodiments, a polyimide coating may be applied on a substrate as a adhesion layer using any well-known coating method, including, for example, chemical vapor deposition, spray coating, spin coating, dip coating, slot coating, and / or printing including ink jet printing. In some embodiments, the polyimide solution layer is spray coated and thermally cured at a temperature range from 300℃ to 450℃.

[0091] Then, 1 vol%of 3- (2-aminoethylamino) propyldimethoxy-methylsilane (AEA-PDMMS) diluted in ispopropanol was used to functionalize the glass surfaces. In particular, the cleaned glass substrates were submerged into the AEA-PDMMS solution with applied ultra  sonic energy at 23 ℃ for 30 minutes. The glass substrates were then dried in an oven at 120 ℃for 1 hour.

[0092] The AEA-PDMMS-modified glass substrates were then processed using a copper electroless plating kit available from Uyemura, Taiwan. Specifically, the glass substrates were dipped into a Pd / Sn colloid at room temperature for 8 minutes, then gently rinsed with deionized water. Next, the glass substrates were dipped into an activation solution at room temperature for 3 minutes to remove the Sn shell from the Pd catalyst. Finally, the glass substrates were dipped into an electroless plating bath at 35 ℃ for 5 minutes to form a uniform copper layer having a thickness of greater than or equal to 130 nm and less than or equal to 600 nm on the surface of the glass substrates and on the via sidewalls.

[0093] Then, the glass substrates including the seed layer were annealed by rapid thermal process (RTA) at 400 ℃ for 8 minutes with a 10 ℃ / sramping rate to release the stress.

[0094] The glass substrates were then pre-wetted by dipping the glass substrate into DI water in an ultrasonic bath for 2 minutes.

[0095] Next, the wetted glass substrates were plated in a 2L electrolyte bath including 1 M CuSO4·5H2O and 0.56 M H2SO4. The electrolyte bath included 8 ppm of chloride ions, 40 ppm of nitrotetrazolium blue chloride, and 144 ppm Tetronic 701. The glass substrates were positioned between two copper plates (anodes) , and a constant potential of -0.8V was applied using an Auto-Lab PGSTAT 302N to plug the vias, forming the bridge shape within the vias, as shown in FIGS. 7A , 7B and 7C.

[0096] FIG. 7A is an SEM image showing the formation of a bridge formed from the copper in the glass substrate having an aspect ratio of 13.6. FIG. 7B is a CT scan image further evidencing the formation of the plug formed from the copper. FIG. 7C is a CT scan image showing the formation of a bridge formed from the copper in a glass substrate having an aspect ratio of 34. More specifically, the glass substrates having a thickness t of 340 μm and including 10 μm diameter (d) vias. The thickness of a center of the bridge (H1) in FIG. 9C is 7 μm (on average) , and the thickness on an end of the bridge (H2) is 14 μm (on average) .

[0097] Following formation of the plug within the through-glass vias, a 0.5ppm accelerator SPS is incorporated in the electrolyte to accelerate the Cu deposition. A constant current of 0.05 amps / dm2 was applied under current control mode between the electrode and the glass  substrate for 3 hrs, so that the plurality of vias is filled with copper. FIG. 8A is an SEM image showing the complete and void-free filling of the 10 μm vias with the copper. FIG. 8A is a XRM (X-ray microscopes) image showing the complete and void-free filling of the 10 μm vias with the copper. FIG. 8B is another XRM image showing the complete and void-free filling of the 10 μm vias with the copper. The XRM is measured through Zeiss 520 Versa which has an approximately 1.0 um voxel resolution.

[0098] As a comparative example, a glass substrate (HPFSTM glass available from Corning, Incorporated) having a thickness t of 340 μm and including 10 μm diameter vias was cleaned, processed using the copper electroless plating kit, and pre-wetted as described for the samples above. However, following pre-wetting, the wetted glass substrate was plated at -0.54 V 40min to form of the plug within the through-glass via. Then a current density of 0.025 amps / dm2 was applied for 1 hr, and then increased to 0.05 amps / dm2 to fill the vias with the copper. The electrolyte solution contains the same NBT and Tetronic 701, but without the accelerator SPS. FIG. 9A-9B show the results. In particular, FIG. 9A is an SEM image showing voids created within the vias as a result of the electroplating at the current density of 0.16 amps / dm2 through the entirety of the process. FIG. 9B and 9C are additional SEM images further evidencing the voids within the vias.

[0099] Accordingly, FIGS. 6-8B demonstrate that the methods described herein may be used to produce a thin (>200 μm thick) glass substrate including vias at an aspect ratio of greater than 12: 1 that are filled with copper such that the electrically conductive material in the filled vias have a defect ration of less than 5%.

[0100] It should now be understood that embodiments of the present disclosure enable through-glass vias to be formed in a thin glass substrate at an aspect ratio of greater than or equal to 5: 1 and metallized such that the electrically conductive material in the filled vias has a void volume fraction of less than or equal to 5%. In particular, various embodiments enable a glass substrate including through-glass vias to be metallized without the use of a carrier. Accordingly, such processes may be used in roll-to-roll processes to fill through holes in thin, flexible glass substrates without the creation of voids.

[0101] It will be apparent to those skilled in the art that various modifications and variations can be made to the embodiments described herein without departing from the spirit and scope of the claimed subject matter. Thus it is intended that the specification cover the modifications  and variations of the various embodiments described herein provided such modification and variations come within the scope of the appended claims and their equivalents.

Claims

1.A method for metallizing through-glass vias in a glass substrate, the method comprising:cleaning a glass substrate; wherein the glass substrate has a thickness t and comprises a plurality of vias extending through the thickness t; wherein an aspect ratio of the thickness t of the glass substrate to an average diameter of the plurality of vias is greater than or equal to 12: 1 and less than or equal to 150: 1;modifying a surface of the glass substrate with a silane;applying an electroless plating solution comprising a copper ion to deposit a copper seed layer on the surface of the glass substrate and the sidewall wall of the plurality of vias;wetting the glass substrate;disposing an electrolyte within the plurality of vias, wherein the electrolyte comprises copper ions to be deposited on the copper seed layer within the plurality of vias;positioning an electrode and applying a first direct current under potential control mode in a first electrolyte for a first period of time between the electrode and the glass substrate, so as to reduce the copper ions into copper to form a bridge attached on a sidewall and at the central part of each of the plurality of vias; andapplying a second direct current under current control mode in a second electrolyte for a second period of time between the electrode and the glass substrate to fill the vias such that each of the plurality of vias is filled with copper.2.The method of claim 1, further comprising applying an adhesion layer on the surface of the glass substrate.3.The method of claim 1, further comprising annealing the glass substrate prior to modifying the surface of the glass substrate.4.The method of claim 1, wherein the thickness t of the glass substrate is greater than or equal to 50 μm and less than or equal to 1200 μm.5.The method of claim 1, wherein the thickness t of the glass substrate is greater than or equal to 200 μm and less than or equal to 400 μm.6.The method of claim 1, wherein the plurality of vias has an average diameter of greater than or equal to 8 μm and less than or equal to 30 μm.7.The method of claim 1, wherein the first electrolyte comprises a first additive.8.The method of claim 7, wherein the first additive comprises a suppressor.9.The method of claim 8, wherein the first additive further comprises a leveler.10.The method of claim 1, wherein the second electrolyte comprises a second additive consists of a suppressor, an accelerator, and a leveler.11.The method of claim 8, wherein the suppressor is present in the first electrolyte in a concentration of greater than or equal to 100 ppm and less than or equal to 500 ppm.12.The method of claim 8, wherein the suppressor is diamine comprising wherein x is selected from at least one of co-polymer of polypropylene glycol and polyethylene glycol; wherein y is selected from at least one of methylene, vinyl and propylene.13.The method of claim 8, wherein the suppressor is selected from polyethylene glycol and copolymer of polypropylene glycol and polyethylene glycol.14.The method of claim 12, wherein the suppressor is ethylenediamine tetrakis (ethoxylate-block-propoxylate) tetrol.15.The method of claim 9, wherein the leveler is nitrotetrazolium blue chloride.16.The method of claim 10, wherein the accelerator is selected from at least one of bis- (sodium sulfopropyl) -disulfide and 3-Mercapto-1-propanesulfonic acid.17.The method of claim 1, wherein the first electrolyte and the second electrolyte further comprise halide ions.18.The method of claim 17, wherein the halide ions are present in a concentration of greater than or equal to 1 ppm and less than or equal to 20 ppm.19.The method of claim 1, wherein the first direct current comprises a current at a voltage of greater than or equal to 0.5 volt and less than or equal to 0.8 volt relative to a mercury-mercurous sulfate electrode potential.20.The method of claim 1, wherein the first period of time is in a range from 10 minutes to 200 minutes.21.The method of claim 1, wherein the second direct current comprises a current at a current density of greater than or equal to 0.02 amps / dm2 and less than or equal to 2 amps / dm2.22.The method of claim 1, wherein the second period of time is in a range from 30 minutes to 500 minutes.23.The method of claim 1, wherein the vias filled with copper has a defect ratio of less than 4.8%.24.The method of claim 1, wherein the copper in each of the plurality of vias is free of defections.25.The method of claim 2, wherein the adhesion layer comprises titanium / copper.26.The method of claim 2, wherein the adhesion layer comprises metal oxide or polyimide.27.The method of claim 1, wherein the surface of the glass substrate is deposited with a copper layer with a thickness t1 after the plurality of vias is filled with copper; wherein the thickness t1 is greater than or equal to 0.2 um and less than or equal to 10 um.28.A glass article comprising:a glass substrate having a first major surface and a second major surface opposite the first major surface and separated from the first major surface by a thickness of greater than or equal to 50 μm and less than or equal to 1200 μm;a plurality of vias extending through the glass substrate from the first major surface to the second major surface, wherein:the plurality of vias have an average diameter of greater than or equal to 8 μm and less than or equal to 30 μm;an aspect ratio of the thickness of the glass substrate to the average diameter of the plurality of vias is greater than 12: 1 and less than or equal to 150: 1;the central part of each of the plurality of vias is filled with copper and form a bridge attached on a sidewall of the each of the plurality of vias;a thickness of a center of the bridge is greater than or equal to half of the average diameter of the plurality of vias; anda thickness of an end of the bridge is less than or equal to three times of the thickness of the center of the bridge.29.The glass article of claim 28, wherein the thickness of the end of the bridge is less than or equal to two times of the thickness of the center of the bridge.30.The glass article of claim 28, wherein the copper in each of the plurality of vias is free of voids.31.The glass article of claim 28, wherein the thickness of the glass substrate is greater than or equal to 200 μm and less than or equal to 400 μm.32.The glass article of claim 28, wherein the surface of the glass substrate is deposited with a copper layer with a thickness t1 , wherein the thickness t1 is greater than or equal to 0.2 um and less than or equal to 10 um.33.The glass article of claim 32, wherein the thickness t1 is greater than or equal to 0.5 um and less than or equal to 2 um.

Citation Information

Patent Citations

  • Method for metallically filling glass adapter plate through holes

    CN111575684A

  • Glass blind hole machining method

    CN111816608A

  • Filling method into through-hole

    JP2005093934A

  • Wiring board with through electrode and manufacturing method of the same

    JP2014093406A

  • Through electrode substrate and method of manufacturing the same

    JP2017098402A

Cited By

  • Small via diameter TGV with adhesion layer

    WO2026164778A1