Method for preparing polyether ester polyol and product thereof

The polyetherester polyol prepared through transesterification reaction is used to prepare easily dyeable spandex, which solves the problem of poor dyeing performance of polyester recycling and spandex, and achieves efficient recycling of polyester and excellent performance of spandex fiber.

WO2024217450A1PCT designated stage expired Publication Date: 2024-10-24ZHENGZHOU ZHONGYUAN SPANDEX ENG TECH CO LTD
View PDF 26 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/088284
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-04-16
Filing Date
2024-04-17
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

The existing polyester plastic recycling methods are complicated and the purity of the product is difficult to guarantee. The quality requirements for recycled plastic bottle flakes are high and difficult to be widely used. Moreover, the dyeing performance of spandex fiber is poor, which affects the appearance of textile products.

Method used

Polyester is used as raw material to prepare polyetherester polyol through transesterification reaction, which is used to prepare easily dyeable spandex. Its molecular structure is adjusted to improve the dye uptake rate and color fixing ability, and at the same time broaden the application methods of polyester recycled materials.

Benefits of technology

It simplifies the production process of polyetherester polyol, improves the dyeing performance and mechanical properties of spandex fiber, broadens the source of raw materials for polyurethane elastic fiber, and realizes the efficient use of recycled polyester.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2024088284-FTAPPB-I100001
    Figure PCTCN2024088284-FTAPPB-I100001
  • Figure PCTCN2024088284-FTAPPB-I100002
    Figure PCTCN2024088284-FTAPPB-I100002
  • Figure PCTCN2024088284-FTAPPB-I100003
    Figure PCTCN2024088284-FTAPPB-I100003
Patent Text Reader

Abstract

Provided in the present invention is a method for preparing polyether ester polyol and a product thereof. The method comprises: adding polyether glycol and a polyester as raw materials into a reaction kettle, heating the reaction kettle to a reaction temperature for an ester exchange reaction, and distilling, by means of a vacuum distillation method, micromolecular polyol produced during the ester exchange reaction, thereby preparing polyether ester polyol. The polyester contains an aromatic dibasic acid polyol ester structure; the polyether glycol has a polymerization degree of 2-20 and a molecular weight of 100-1000; the molar ratio of the polyether glycol to the aromatic group structure in the polyester is greater than 1.05:1; the reaction temperature is above the boiling point of the micromolecular polyol, but below the boiling point of the polyether glycol. By means of the method provided in the present invention, recovered polyester can be directly processed into polyether ester polyol suitable for the production of polyurethane elastic fibers, such that the production process of polyether ester polyol suitable for the production of spandex is simplified, and the raw material source of polyurethane elastic fibers is also expanded while recovered resources are utilized. Moreover, provided in the present invention are dyeable spandex prepared by utilizing polyether ester polyol, and a preparation method therefor. In the preparation process of the spandex, the polyether ester polyol provided in the present invention is added to a diol raw material, such that a molecular soft segment of the prepared spandex fiber contains a specific aromatic group–polyether block structure. Compared with conventional spandex, the dyeable spandex of the present invention can increase the dye uptake and color fixation capacity of the spandex so as to disperse dyes and acid dyes without compromising the mechanical properties of the spandex. By adjusting the mass ratio of the aromatic group–polyether block structure in the molecular soft segment of the spandex, the spandex has better alkali resistance when the spandex has adequate dye uptake and color fixation rate.
Need to check novelty before this filing date? Find Prior Art

Description

A method for preparing polyetherester polyol and its products

[0001] The present invention claims priority to the Chinese invention patent application with application number 202310424908.4, filed with the State Intellectual Property Office of China on April 18, 2023, entitled “A method for preparing polyether ester polyols and their products”; and claims priority to the Chinese invention patent application with application number 202410455754.X, filed with the State Intellectual Property Office of China on April 16, 2024, entitled “A kind of easy-to-dye spandex and its preparation method”. Technical Field

[0002] The present invention relates to the field of preparation methods of polymers and products thereof, and in particular to a method for preparing polyether ester polyols and products thereof. Background Art

[0003] Polyesters are a class of engineering materials with excellent performance and a wide range of applications. Polyesters with benzene rings in their structures, such as polyethylene terephthalate (PET), polypropylene terephthalate (PPT), and polybutylene terephthalate (PBT), are particularly common. These materials can be used as fibers, bottles, films, and other plastic products, making them indispensable in our daily lives. However, as the use of polyester plastic products grows, the environmental impact of non-degradable polyester plastics is gaining increasing attention. Plastic recycling is an effective means of addressing these environmental issues. Currently, the main method for recycling polyester plastics is to remelt and pelletize plastic bottle flakes as recycled material, which is then processed and remade into plastic products. However, this method places high demands on the quality of the recycled plastic bottle flakes, requiring minimal impurities, minimal color variation, and minimal molecular weight. Many plastic wastes that fail to meet these standards are difficult to recycle and reuse. In addition to recycling and granulation, there is also a method of removing impurities from the recycled polyester plastic and then decomposing it into terephthalic acid (PTA) or dimethyl terephthalate (DMT) through chemical methods, and then reusing it as a chemical raw material. However, this method is complex, the purity of the product is difficult to guarantee, and the use of the recycled product is limited.

[0004] Spandex, short for polyurethane elastic fiber, is currently the most widely used elastic fiber. It is a block copolymer of soft and hard segments. The soft segments are generally composed of flexible segments, typically derived from the reaction of polyols such as polyethers, polyesters, and hydroxyl-terminated polybutadiene, and polyisocyanates used to connect the polyols. The hard segments are composed of segments with excellent crystallinity, typically derived from the reaction of polyisocyanates with small-molecule polyols and small-molecule amine chain extenders. The mainstream spandex on the market is dry-process polyether spandex. The main raw materials for dry-process polyether spandex are polytetramethylene ether glycol, diphenylmethane diisocyanate, and chain-extending amines. A polyurethaneurea solution is prepared through a two-step polymerization reaction. Necessary additives are then added to prepare the polyurethaneurea spinning solution, which is then produced through tunnel spinning to produce spandex fiber. This method uses polytetramethylene glycol as the soft segment, resulting in well-balanced spandex fibers with generally high elastic elongation and a tensile modulus that generally meets the requirements of everyday clothing. However, this method is costly and cannot use recycled materials.

[0005] Spandex is rarely used as a standalone fabric and is often blended with other fibers. The mainstream spandex on the market is polyether spandex, produced by dry spinning using polytetramethylene ether glycol and diisocyanate. Conventional spandex is typically dyed with disperse or acid dyes. However, in practice, spandex exhibits poor dye uptake and color fastness. When blended with other fibers, it can result in color shift or whitening after dyeing, significantly impacting the appearance of textile products. The reason is that the molecular structure of spandex is mainly composed of a polyether part with lower polarity and a polyurethane or polyurethane urea part with higher polarity. The polyether part of mainstream spandex products is the residue of polytetramethylene ether diol, which belongs to the non-crystalline region in the microphase separation structure and has a loose structure. It provides elasticity for spandex fibers and is the main site for disperse dye dyeing, but has weak binding force with disperse dyes. The polyurethane or polyurethane urea part can theoretically dye acidic, neutral, acidic media and disperse dyes through hydrogen bonds and their coordination bonds, but because this part is a crystalline region, the molecular chain segments are tightly stacked, and it is difficult for dye molecules to diffuse into the interior of the crystalline region, which greatly reduces the dyeing rate.

[0006] The inventors discovered through long-term research that spandex with high elongation and high elastic recovery can be produced by using polyetherester polyols containing aromatic group-polyether blocks as the soft segments of spandex. Adding a small amount of small molecule diol structures to the block structure of the polyetherester polyols can adjust the elastic modulus and elastic recovery of the spandex. Furthermore, the structure of the polyetherester polyols is similar to that of common polyesters, making it possible to recycle polyester as a raw material for spandex. Generally speaking, the preparation method of such polyetherester polyols is to react dicarboxylic acids with aromatic groups with polyether diols. However, the process of recycling polyester to prepare terephthalic acid is complex, energy-intensive, and difficult to purify.

[0007] Therefore, the present invention attempts to provide a method for preparing polyetherester polyol suitable for producing spandex by recycling polyester, and preparing easy-to-dye spandex using polyetherester polyol, in order to optimize the production process of the polyetherester polyol and the performance of its products.

[0008] Summary of the Invention

[0009] To address the above-mentioned issues, the present invention provides a method for preparing a polyether-ester polyol suitable for producing spandex using polyester as a raw material, the polyether-ester polyol prepared by the method, and polyurethane elastic fibers, nonwoven fabrics, films, and elastomers prepared using the polyether-ester polyol, as well as methods thereof. The specific embodiments are as follows:

[0010] In one aspect, the present invention provides a method for preparing polyetherester polyol, comprising the steps of:

[0011] Step 1) adding a polyether diol and a polyester as raw materials into a reaction kettle, wherein the polyester contains an aromatic dibasic acid polyol ester structure, the degree of polymerization of the polyether diol is 2-20, the molecular weight is 100-1000, and the molar ratio of the aromatic groups in the polyether diol and the polyester is greater than 1.05:1;

[0012] Step 2) heating the reactor to the reaction temperature to carry out an ester exchange reaction, and using a vacuum distillation method to evaporate the small molecule polyol produced by the ester exchange reaction to prepare a polyether ester polyol, wherein the reaction temperature is above the boiling point of the small molecule polyol and below the boiling point of the polyether diol.

[0013] In the above method, the aromatic dibasic acid polyol ester structure refers to an ester structure formed by an aromatic dibasic acid and a polyol in a polyester. The aromatic ring includes an aromatic ring structure and an aromatic heterocyclic ring structure, wherein the aromatic ring can be at least one of a benzene ring, a naphthalene ring, an anthracene ring, a phenanthrene ring, etc.; the aromatic heterocyclic ring can be at least one of a pyridine ring, a furan ring, a thiazole ring, a pyrimidine ring, etc. Specifically, the aromatic dibasic acid can be one or more of terephthalic acid, phthalic acid, isophthalic acid, biphenyl dicarboxylic acid, 1,4-naphthalene dicarboxylic acid, 2,6-naphthalene dicarboxylic acid, 2,3-naphthalene dicarboxylic acid, 2,5-furan dicarboxylic acid, terephthalic acid, isophthalic acid, and phthalic acid. The polyol is one or more of a diol, a triol, or a tetraol, preferably a diol, more preferably one or more of ethylene glycol, 1,3-propylene glycol, 1,2-propylene glycol, 1,4-butanediol, 1,6-hexanediol, neopentyl glycol, 2-methyl-1,3-propanediol, and 3-methyl-1,5-pentanediol.

[0014] Alternatively, the polyester containing an aromatic dibasic acid polyol ester structure in the present invention may be one or more of polyethylene terephthalate (PET), polybutylene terephthalate (PBT), poly(t-butylene terephthalate) (PTT), butylene adipate-butylene terephthalate copolymer (PBAT), and polyethylene 2,5-furandicarboxylate (PEF). The polyester containing an aromatic dibasic acid polyol ester structure may also be any other common polyester containing a polyether ester structure or a triol or tetraol residue structure. As long as the polyester contains an aromatic dibasic acid polyol ester structure in its main chain, it can be used as a raw material in the method of the present invention.

[0015] Optionally, the polyether diol is a homopolymer or copolymer polyether diol prepared by condensation polymerization of a small molecule diol of C2-C5, or ring-opening polymerization of an epoxide of C2-C5, specifically, preferably one or more of polyethylene glycol (PEG), poly-1,3-propylene glycol (P3OG), poly-1,2-propylene glycol (PPG), polytetrahydrofuran (PTG), polyethylene glycol-1,2-propylene glycol copolymer, and polytetrahydrofuran-3-methyltetrahydrofuran copolymer.

[0016] Optionally, the molar ratio of the aromatic group structure in the polyether diol and the polyester is calculated by the following formula: R = (W + P-36) / (WA)

[0017] Where,

[0018] R is the molar ratio of the aromatic group structure in the polyether diol and the polyester,

[0019] W is the molecular weight of the target polyetherester polyol, and W is 1000-5000,

[0020] P is the molecular weight of the aromatic dibasic acid in the raw material of polyester,

[0021] A is the average molecular weight of the polyether diol.

[0022] The aromatic dibasic acid in the raw materials of the polyester is a dibasic acid raw material that forms the aromatic dibasic acid polyol ester structure, such as the terephthalic acid, phthalic acid, 2,5-furandicarboxylic acid, etc. mentioned above.

[0023] The polyether ester polyol prepared according to the method for preparing polyether ester polyol described above is characterized in that the polyether ester polyol comprises a structure represented by the following formula (1) and the following formula (2) and a blocked alcohol hydroxyl group:

[0024] wherein R1 is an aromatic group, and the mass content of R1 in the repeating unit of formula (1) is 4.5%-44%, R2 is at least one saturated alkane group having 2-5 carbon atoms, x is 2-20, and R3 is a residue of a polyol in the polyester raw material;

[0025] The mass ratio of formula (2) in the structure of the polyetherester polyol is less than 20%, preferably less than 10%;

[0026] The number average molecular weight of the polyetherester polyol is 1000-5000;

[0027] The average functionality of the capped alcoholic hydroxyl groups is 1.95-2.00.

[0028] Preferably, R2 is at least two of saturated alkane groups having 2 to 5 carbon atoms.

[0029] The polyetherester polyols described above can be used not only to produce spandex but also other polyurethane products. Therefore, the present invention also provides methods for preparing polyurethane elastic fibers, nonwoven fabrics, films, or elastomers using the polyetherester polyols described above as raw materials via solution processing or melt processing, as well as the polyurethane elastic fibers, nonwoven fabrics, films, or elastomers produced according to the methods.

[0030] On the other hand, the present invention provides an easy-to-dye spandex, characterized in that the soft segment of the molecular structure of the easy-to-dye spandex comprises a repeating unit described by the following formula (1):

[0031] wherein R1 is an aromatic group structure, and the mass content of R1 in the repeating unit is 4.5%-44%; R2 is at least one of a linear saturated alkane group having 2-3 carbon atoms; and x is 2-20;

[0032] The mass of the repeating unit represented by formula (1) accounts for more than 2%, preferably more than 5%, more preferably more than 10%, less than 70%, and preferably less than 65% of the mass of the spandex soft segment.

[0033] Optionally, the soft segment of the molecular structure of the spandex further includes a polytetramethylene ether segment.

[0034] The soft segment mass in this invention refers to the mass of the molecular structure of the spandex after the reaction of the diol raw material with diisocyanate, minus the terminal hydroxyl groups. The diol raw material refers to the diol compound used as the raw material for the polyurethane molecular weight soft segment, including the polyether ester polyols defined in this invention, as well as optional substances such as polytetramethylene ether glycol, and does not include small molecule diol compounds used as chain extenders.

[0035] The high resilience coarse denier spandex can be prepared by dry spinning or melt spinning. Specifically, the preparation method of dry spinning is as follows:

[0036] A method for preparing easy-to-dye spandex, characterized by comprising the following steps:

[0037] Step 1): using a diisocyanate raw material to cap a diol raw material to prepare a prepolymer;

[0038] Step 2): dissolving the prepolymer using a polar solvent to obtain a prepolymer solution;

[0039] Step 3): chain extending the prepolymer using a mixed solution of a linker and a terminator to obtain a polyurethane / polyurethane urea solution;

[0040] Step 4): adding an auxiliary agent to prepare a spinning solution;

[0041] Step 5): The obtained spinning solution is passed through a spinning device to obtain easy-to-dye spandex.

[0042] The preparation method of melt spinning is as follows:

[0043] A method for preparing easy-to-dye spandex comprises the following steps:

[0044] Step a) adding a diisocyanate raw material, a diol raw material, and a small molecule polyol chain extender into a reaction container respectively;

[0045] Step b) mixing the materials in the reaction container, and heating the materials during or after the mixing process to react and extruding and granulating the materials to produce polyurethane particles;

[0046] Step c) drying the polyurethane particles, adding an auxiliary agent and performing melt spinning to obtain easily dyeable spandex.

[0047] In one embodiment of the present invention, the diol raw material includes a polyether ester polyol having an aromatic group-polyether block structure, and the polyether ester polyol is composed of a repeating unit represented by formula (1) and a capped alcohol hydroxyl group:

[0048] Wherein R1 is an aromatic group structure, and the mass content of R1 in the repeating unit is 4.5%-44%; R2 is at least one of a linear saturated alkane group having 2-3 carbon atoms; x is 2-20, preferably 3-10; the average functionality of the end-capped alcohol hydroxyl group is 1.95-2.00; and the number average molecular weight of the polyetherester polyol is 800-5000, preferably 1000-3500, more preferably 1400-2500, and most preferably 1500-2300.

[0049] Optionally, the polyetherester polyol is heated at 90°C and a shear rate of 1s -1 The viscosity can be less than 500 poise, preferably less than 200 poise.

[0050] Optionally, the mass ratio of the polyetherester polyol in the diol raw material is greater than 2%, preferably greater than 5%, and more preferably greater than 10%.

[0051] Optionally, the mass ratio of the polyetherester polyol in the diol raw material is less than 70%, preferably less than 65%.

[0052] Optionally, the diol raw materials also include other diol compounds that can be used as spandex soft segments, as the second type of diol raw materials, such as polytetramethylene ether glycol, polyethylene glycol, polypropylene glycol and other polyether glycols, polybutylene adipate glycol ester glycol, adipic acid and mixed diols (such as ethylene glycol / 1,4-butanediol, ethylene glycol / 1,2-propylene glycol, 1,6-hexanediol / 2,2-dimethylpropylene glycol-1,3) copolyester diols, other polyether ester diols that can be used as spandex soft segments, or a mixture of at least two of the above diol compounds.

[0053] Preferably, the mass of the second type of diol raw material accounts for 30%-95% of the total diol raw materials. That is, the preferred solution is to blend the polyol and the second type of diol raw material as the diol raw material for spandex.

[0054] The preferred second type of diol starting material is furan ether diol.

[0055] In another embodiment of the present invention, the diol raw material includes a polyether ester polyol having an aromatic group-polyether block structure, and the polyether ester polyol comprises a repeating unit represented by formula (1) and a capped alcohol hydroxyl group:

[0056] Wherein R1 is an aromatic group structure, and the mass content of R1 in the repeating unit is 4.5%-44%; R2 is at least one of a linear saturated alkane group having 2-3 carbon atoms; x is 2-20, preferably 3-10; the mass percentage of the repeating unit represented by formula (1) in the polyether ester polyol is greater than 5%; the average functionality of the end-capped alcohol hydroxyl group is 1.95-2.00, and the number average molecular weight of the polyether ester polyol is 800-5000, preferably 1000-3500, more preferably 1400-2500, and most preferably 1500-2300.

[0057] The polyetherester polyol may contain some other polyester structures or polyether structures, or some aliphatic structures as a modified structure.

[0058] Likewise, the polyetherester polyols mentioned above can be blended with the second type of diol raw material mentioned above to serve as diol raw materials for spandex. Beneficial effects:

[0059] The method for preparing polyether ester polyol provided by the present invention uses polyester as raw material and can directly process recycled polyester into polyether ester polyol suitable for producing spandex, thereby simplifying the production process of polyether ester polyol suitable for producing spandex, utilizing recycled resources, and broadening the source of raw materials for polyurethane elastic fibers.

[0060] The easy-to-dye spandex provided by the present invention is made by adding a polyetherester polyol with a specific structure to a diol raw material, resulting in a spandex fiber with a specific aromatic group-polyether block structure in its soft segment. Compared to conventional spandex, the easy-to-dye spandex of the present invention improves the dye uptake and color fixation of disperse and acid dyes without sacrificing the spandex's mechanical properties.

[0061] By adjusting the mass ratio of the aromatic group-polyether block structure in the soft segment of the spandex molecule, the spandex has sufficient dye uptake and fixation rates while having better alkali resistance. DETAILED DESCRIPTION

[0062] Currently, the most common methods for recycling polyester materials are melt pelletization or chemical decomposition into terephthalic acid (PTA) or dimethyl terephthalate (DMT) for reuse as chemical raw materials. The present invention has discovered a method for preparing polyetherester polyols using polyester as a raw material. The resulting polyetherester polyols can be used as the soft segment raw material for spandex. This method allows polyester to be used as a direct raw material for polyurethane elastic fibers, broadening the uses of recycled polyester while also expanding the raw material sources for spandex.

[0063] Specifically, the present invention provides a method for preparing a polyether ester polyol, and a polyether ester polyol prepared by the method, wherein the polyether ester polyol comprises a structure represented by the following formula (1) and the following formula (2) and a blocked alcohol hydroxyl group:

[0064] wherein R1 is an aromatic group structure, and the mass content of R1 in the repeating unit of formula (1) is 4.5%-44%, R2 is at least one saturated alkane group having 2-5 carbon atoms, x is 2-20, and R3 is a residue of a polyol in a polyester raw material;

[0065] The mass ratio of formula (2) in the structure of the polyetherester polyol is less than 20%, preferably less than 10%, and more preferably 0;

[0066] The number average molecular weight of the polyetherester polyol is 1000-5000;

[0067] The average functionality of the blocked alcoholic hydroxyl groups is 1.95-2.00.

[0068] Hereinafter, unless otherwise specified, polyetherester polyol refers specifically to polyetherester polyol having the above characteristics.

[0069] The aromatic group structure described in the present invention includes an aromatic ring and an aromatic heterocycle, wherein the aromatic ring can be at least one of a benzene ring, a naphthalene ring, an anthracene ring, a phenanthrene ring, and the like; and the aromatic heterocycle can be at least one of a pyridine ring, a furan ring, a thiazole ring, a pyrimidine ring, and the like. When the content of the aromatic group R1 in the polyetherester polyol is too high, the resulting polyetherester polyol will be too rigid, resulting in excessive viscosity, which is not conducive to the production process of polyurethane elastic fibers. Therefore, the mass content of R1 in the repeating unit of formula (1) is 4.5% to 44%.

[0070] The structure of formula (2) is the residual structure of the polyester that has not been completely reacted in the method of the present invention. Since the reaction of the present invention is generally not 100% complete, a portion of the group structure of the polyester raw material will remain. Therefore, a portion of the structural units of the above formula (2) may exist in the polyether ester polyol finally obtained. However, by controlling the reaction conditions, the transesterification reaction can be made as complete as possible. The structure of formula (2) will significantly increase the melting point of the polyether ester polyol and also increase the intermolecular forces of the polyether ester diol. During prepolymerization, the viscosity of the prepolymer will be too high to complete the prepolymerization reaction. In addition, the aromatic dibasic acid polyol ester structure will also affect the elastic recovery of the final polyurethane, resulting in a lower elastic recovery rate and increased permanent deformation. Therefore, the mass ratio of formula (2) in the structure of the polyether ester polyol of the present invention is less than 20%, preferably less than 10%, and more preferably 0.

[0071] According to the present invention, the average functionality of the capped alcoholic hydroxyl groups of the polyetherester polyol can be 1.95-2.00, preferably 1.96-2.00, and more preferably 1.98-2.00. This ensures that the polyetherester polyol can be successfully capped with isocyanates and subsequently chain-extended with small amines or alcohols. If the average functionality is greater than 2.00, when the polyetherester polyol is used as a raw material for polyurethane production, the resulting polyurethane may exhibit crosslinked structures, preventing the formation of chain-like polyurethanes. Such polyurethanes may gel during continuous production, hindering the continuous production of spandex. If the average functionality is lower, the molecular weight of the resulting polyurethane will also be low, thus affecting the performance of polyurethane elastic fibers. In actual reactions, the polyether diol may undergo dehydration of terminal hydroxyl groups to form double bonds during the condensation polymerization / ring-opening polymerization process. In addition, due to the limitations of the actual reaction effect, the condensation reaction or ester exchange reaction of the polyether diol to form polyether ester polyol cannot be 100% completed. Therefore, the average functionality of the final polyether ester polyol generally cannot reach 2.00.

[0072] Here, the "average functionality" refers to the average number of moles of alcoholic hydroxyl groups that can participate in the reaction per mole of polyetherester polyol. In the present invention, taking into account the dehydration of the terminal hydroxyl groups of the polyether diol to form double bonds and the presence of unreacted carboxyl groups, the average functionality of the alcoholic hydroxyl groups can be calculated using the following formula:

[0073] Functionality = 2* number of moles of alcoholic hydroxyl groups / (number of moles of alcoholic hydroxyl groups + number of moles of carboxyl groups + number of moles of double bonds)

[0074] The polyetherester polyol of the present invention may have a melting point below 80°C and is preferably liquid at room temperature to prevent solidification during storage or transportation, thereby ensuring continuous industrial operation. Otherwise, it would need to be melted by heating, increasing energy consumption.

[0075] The inventors have discovered that polyetherester polyols with the aforementioned characteristics can replace polytetramethylene ether glycol as a raw material for the soft segment of spandex, resulting in spandex with a high elastic recovery rate. Based on this, the inventors have proposed a method for preparing the polyetherester polyols. Compared to the conventional method of reacting dicarboxylic acids with polyether glycols, the polyetherester polyols can be prepared using recycled polyester as a raw material. This broadens the utilization of recycled polyester and the source of spandex raw materials, while also being more environmentally friendly.

[0076] The specific preparation method of the polyether ester polyol proposed by the present invention comprises the following steps:

[0077] Step 1) adding a polyether diol and a polyester as raw materials into a reaction kettle, wherein the polyester contains an aromatic dibasic acid polyol ester structure, the degree of polymerization of the polyether diol is 2-20, preferably 3-10, and the molecular weight is 100-1000, and the molar ratio of the aromatic groups in the polyether diol and the polyester is greater than 1.05:1;

[0078] Step 2) heating the reactor to the reaction temperature to carry out an ester exchange reaction, and using a vacuum distillation method to evaporate the small molecule polyol produced by the ester exchange reaction to prepare a polyether ester polyol, wherein the reaction temperature is above the boiling point of the small molecule polyol and below the boiling point of the polyether diol.

[0079] In the method of the present invention, a polyester containing an aromatic group structure and a specific polyether diol are used as raw materials for an ester exchange reaction to produce a polyetherester polyol meeting the above characteristics. The molecular structure of the polyetherester polyol produced by the present invention is an aromatic group-polyether structure connected by ester bonds. Therefore, the above method selects a polyester containing an aromatic group structure as a raw material, thereby introducing the aromatic group structure in the polyester into the molecular structure of the polyetherester polyol. Specifically, the polyester containing an aromatic group structure can be any common polyester material copolymerized by an aromatic group and a small molecule polyol, such as polyethylene terephthalate (PET), polypropylene terephthalate (PTT), polybutylene terephthalate (PBT), butylene adipate and butylene terephthalate copolymer (PBAT), etc., which contain aromatic acid esters in the structure; or polyesters containing aromatic heteroacids in the structure such as polyethylene 2,5-furandicarboxylate (PEF), etc. The above polyesters can all be obtained through recycled polyester plastic bottles, polyester fibers, polyester films, etc. Compared with the rigid aromatic group structure, the polyether segment in the polyether ester polyol of the present invention provides elasticity to the molecule. In order to ensure that the final spandex has sufficient elastic recovery ability, the polyether segment should have a certain length. If the polyether segment length is too short, the viscosity of the polyether ester polyol will be too high, which is not conducive to the continuous implementation of the large-scale production process of spandex and will result in poor resilience of the spandex; and if the polyether segment length is too long, the elastic modulus of the spandex will be too poor. Therefore, in the present invention, the molecular weight of the polyether segment raw material is preferably a polyether diol with a polymerization degree of 2-20, more preferably 3-10, and a molecular weight of 100-1000, preferably 300-1000, and more preferably 600-900. Specifically, the polyether diol can be synthesized by ring-opening polymerization of epoxy monomers or by condensation polymerization of small molecule diols; it can be a homopolymer synthesized from a single monomer or a copolymer synthesized from two or more monomers. As an example, the polyether diol suitable for the present invention can be one or more of diethylene glycol (DEG), triethylene glycol (TEG), polyethylene glycol (PEG), poly 1,3-propylene glycol (P3OG), polypropylene glycol (PPG), polytetrahydrofuran (PTG), or a copolymer diol obtained by reacting tetrahydrofuran with a monomer such as ethylene oxide, propylene oxide, 2-methyltetrahydrofuran or 3-methyltetrahydrofuran.

[0080] The number average molecular weight of the polyetherester polyol of the present invention should be 1000-5000, preferably 1000-3500, more preferably 1400-2500, and most preferably 1500-2300. The larger the number average molecular weight of the polyetherester polyol, the greater its viscosity, making it difficult to perform continuous operations on an industrial scale. However, if the molecular weight of the polyetherester polyol is too small, when the molecular weight requirements of the polyurethane prepolymer are consistent, more diisocyanates are required to participate in the synthesis, resulting in a higher content of carbamate groups in the prepolymer, thereby enhancing the interaction between the prepolymer molecules and increasing the viscosity. Moreover, the soft segment length in the polyurethane formed at this time is shorter, which will affect the recovery properties of the final polyurethane elastic fiber. In a preferred embodiment, the polyetherester polyol of the present invention is heated at 90°C and a shear rate of 1S -1 The viscosity can be less than 500 poise, preferably less than 200 poise.

[0081] Since the method provided by the present invention uses a polyether diol to undergo an ester exchange reaction with a polyester containing aromatic groups to prepare a polyether ester polyol, the molecular weight of the polyether ester polyol can be adjusted by adjusting the molar ratio R of the aromatic groups in the polyether diol and the polyester. Hereinafter, the molar ratio R refers to the molar ratio of the aromatic groups in the polyether diol to the polyester. The higher the molar ratio R, that is, the greater the proportion of polyether diol in the raw material, the more terminal hydroxyl groups remain after the small molecule polyol residues in the polyester polymer are replaced by the polyether diol, and the smaller the number average molecular weight of the resulting polyether ester polyol. Conversely, the smaller the proportion of polyether diol in the raw material, the larger the number average molecular weight of the resulting polyether ester polyol. In order to regulate the molecular weight of the polyetherester polyol, the molar number of the polyether diol should be greater than the molar number of the aromatic group structure in the polyester. Theoretically, when the transesterification reaction is complete, the polyether diol replaces all the small molecular weight polyol residues in the polyester, and the excess polyether diol cuts the macromolecular polyester molecular chain to form a polyetherester polyol with a relatively small molecular weight. Therefore, the difference between the molar number of the polyether diol and the molar number of the aromatic group structure in the polyester is the molar number of the final polyetherester polyol obtained. Based on the above analysis, the calculation method for the theoretical expected molecular weight of the final polyetherester polyol is:

[0082] The specific molar ratio R of the aromatic groups in the polyether diol and the polyester can be obtained by reverse deduction using the above formula. The specific process is as follows:

[0083] The molecular weight of the final polyetherester polyol is set as W, the molecular weight of the polyether diol is set as A, and the number of moles of the feed is M, then the feed mass of the polyether diol is M·A; assuming that the polyester is obtained by reacting an aromatic dibasic acid with a molecular weight of P and a small molecule polyol with a molecular weight of Q, then the molecular weight of the polyester cycle unit is (P+Q-36), the number of moles of the aromatic group structure in the feed polyester is M / R, and the feed mass of the polyester is (P+Q-36)·M / R; Substituting the above letters into formula (1), the formula is as follows:

[0084] Simplifying the above formula (4) to obtain the relationship between the molecular weight W of the polyether ester polyol and the molar ratio R is as follows:

[0085] According to formula (5), when a polyetherester polyol with a specific molecular weight needs to be prepared, the molar ratio R of the feed can be calculated by the following formula:

[0086] As can be seen from formula (6), in order to prepare a polyetherester polyol having a molecular weight W of 1000-5000, in addition to the molar ratio R, the molecular weight P of the aromatic dibasic acid and the molecular weight A of the polyether diol are also relevant. However, it is certain that the molar number of the polyether diol in step (1) should be greater than the molar number of the aromatic groups in the polyester. Therefore, in the present invention, the molar ratio of the polyether diol to the aromatic groups in the polyester is greater than 1.05:1, preferably greater than 1.1:1.

[0087] In step (2), the temperature of the transesterification reaction should be controlled to be above the boiling point of the small molecule polyol and below the boiling point of the polyether diol, so that the exchanged small molecule polyol can be evaporated as much as possible, thereby promoting the complete transesterification.

[0088] During the transesterification reaction, a catalyst is preferably added to promote the reaction. In the present invention, the catalyst is selected from one or more of titanium, vanadium, tin, antimony, zirconium, bismuth and rare earth catalysts, preferably one or more of tetraisopropyl titanate, tetrabutyl titanate, dibutyltin dilaurate, stannous octoate and bismuth laurate.

[0089] The present invention also provides a method for preparing polyurethane products such as polyurethane elastic fibers, nonwoven fabrics, films, or elastomers using the aforementioned polyetherester polyol or the polyetherester polyol produced by the aforementioned method as a raw material. The polyurethane preparation method can employ a two-step prepolymer synthesis process or a one-pot process in which all the raw materials are added together.

[0090] The two-step method for preparing polyurethane comprises the following steps: (1) reacting a polyether ester polyol with a diisocyanate to form a prepolymer; and (2) polymerizing the prepolymer with a chain extender and a chain terminator. The one-pot method for preparing polyurethane comprises the following steps: (1) feeding the polyether ester polyol, diisocyanate and small molecule polyol chain extender separately, i.e., adding each material separately into a reaction vessel; (2) mixing the polyether ester polyol, diisocyanate and small molecule polyol chain extender in a reaction vessel, and heating the mixture to react, or heating the mixture to react during the mixing process. The diisocyanate can be selected from one or more of diphenylmethane diisocyanate, toluene diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, dicyclohexylmethane diisocyanate and isomers thereof. The chain extender can be an amine or alcohol chain extender. Amine chain extenders can be diamines having 2 to 30 carbon atoms, such as one or more of ethylenediamine, propylenediamine, propylenediamine, pentamethylenediamine, methylpentamethylenediamine, methylpropylenediamine, hexamethylenediamine, triethylenediamine, xylenediamine, phenylenediamine, diaminocyclohexane, hexamethylenediamine, and dopamine. Alcohol chain extenders can be one or more of common chain extenders, such as ethylene glycol, 1,4-butanediol, diethylene glycol, 1,6-hexanediol, 1,3-propylene glycol, and 1,4-dihydroxymethylcyclohexane. Chain terminators can be monoamines having 2 to 20 carbon atoms, such as one or more of ethylamine, isopropylamine, n-butylamine, tert-butylamine, hexylamine, dimethylamine, diethylamine, dipropylamine, di-n-butylamine, di-tert-butylamine, diisobutylamine, diisopropylamine, cyclohexylamine, and ethanolamine.

[0091] Unless otherwise specified in this specification, the corresponding operating conditions in existing methods for preparing polyurethane products such as polyurethane elastic fibers, non-woven fabrics, films and elastomers using polyether diols, such as solution processing or melt processing, can be applied to the present invention. For example, polyurethane elastic fibers can be produced by dry spinning of polyurethane solutions, such as the method and equipment described in patent document CN1147628C, or by melt spinning of polyurethane chips, such as the melt spinning method described in patent document CN1180137C; non-woven fabrics can be processed by melt blowing, solution electrospinning, and other methods, such as the melt blowing non-woven fabric manufacturing method described in patent document CN101400838A, and the non-woven fabric prepared by the solution electrospinning method described in patent document JP2009108422A; polyurethane membranes can be processed by solution blade coating, dip coating, melt extrusion, blown film, casting, and other methods, such as the melt spinning method described in patent document JP2009108422A. Polyurethane films can be prepared by the blade coating method described in WO2015064776A, the dip coating method described in WO2015064776A1, the extrusion method described in GB1137520A, the blown film method described in DE2239478A1, and the casting method described in JP2004203933A. Elastomers can be processed by extrusion, injection molding, casting, and other methods, specifically the extrusion method described in JP1996027376A, the injection molding method described in US3917792A, and the casting method described in CA1251294A. The polyurethane product production methods described in the above patent documents are all incorporated into the present invention. The above-mentioned methods for preparing polyurethane elastic fibers, nonwoven fabrics, films, and elastomers are merely examples. In addition to the aforementioned methods, the polyetherester polyols of the present invention can be used as diol raw materials to produce polyurethane products using any existing technology or means.

[0092] Furthermore, the present invention also provides an easy-dye spandex prepared using the above-mentioned polyetherester polyol and a preparation method, wherein the easy-dye spandex has good dye uptake and fixation ability for disperse dyes and acid dyes. The soft segment of the molecular structure of the easy-dye spandex comprises a repeating unit described by the following formula (1):

[0093] wherein R1 is an aromatic group structure, and the mass content of R1 in the repeating unit is 4.5%-44%; R2 is at least one of a linear saturated alkane group having 2-3 carbon atoms; and x is 2-20;

[0094] The mass of the repeating unit represented by formula (1) accounts for 5% or more, preferably 10% or more, of the mass of the soft segment.

[0095] Optionally, the soft segment of the molecular structure of the spandex further includes a polytetramethylene ether segment.

[0096] Since the dye molecules of disperse dyes and acid dyes are all dissolved in the aqueous solution of dye molecules, the dye molecules are completely dissolved in water. The glycol raw material used in ordinary spandex yarn is polytetrahydrofuran, and the prepared polyurethane urea polymer has hydrophobicity. The molecular structure of the easy-to-dye spandex provided by the present invention has the above formula (1), wherein (R2-O) x The hydrophilicity of the molecular chain is increased. This structure is introduced into the spandex molecular structure through polyetherester polyols prepared from PEG and P3OG (polyethylene glycol and poly-1,3-propylene glycol, especially polyethylene glycol) and aromatic dibasic acids. Compared with polytetrahydrofuran, this structure contains a higher density of ether oxygen bonds. The polyurethane urea polymer prepared using this polyetherester polyol has stronger hydrophilicity, making it easier for spandex to be swollen by the dye solution when dyeing with acid dyes and disperse dyes. The gaps between molecules become larger, making it easier for dye molecules to enter the spandex interior. In addition, because acid dye molecules and disperse dye molecules are mostly macromolecules containing aromatic rings, the aromatic ring structure introduced by the polyetherester polyol has stronger van der Waals interactions with the dye molecules. This makes the dye molecules that enter the spandex interior have stronger interaction with the polyetherester polyols and are more easily fixed to the spandex molecules, resulting in higher dye uptake and fixation rates for acid dyes and disperse dyes.

[0097] While meeting the requirements of dye uptake and fixation rate, the introduction of the structure of formula (1) should avoid affecting the mechanical properties of spandex as much as possible. Therefore, the present invention makes more specific requirements for the structure of formula (1) as described above.

[0098] Based on the consideration of the dye uptake and fixation rate of spandex, further, in the repeating unit of formula (1) contained in the soft segment of the easy-to-dye spandex molecular structure, R2 is preferably a straight-linked saturated alkane group with 2-3 carbon atoms. For easy-to-dye spandex, the fewer carbon atoms in R2, the greater the density of ether oxygen bonds, which can make the spandex more hygroscopic, more conducive to the entry of dye molecules into the interior of the spandex fiber, and help improve the dye uptake of spandex. Molecular structures containing side chains will have an adverse effect on the hygroscopicity of spandex. Therefore, in the present invention, R2 is preferably a straight-linked saturated alkane group, specifically, (R2-O) x It can be a polyether segment of PEG, a polyether segment of P3OG, or a polyether segment of ethylene glycol and 1,3-propylene glycol copolyether, among which a straight-chain saturated alkane group having 2 carbon atoms is most preferred.

[0099] In the easily dyeable spandex molecular structure of the present invention, the structure represented by formula (1) should account for a certain proportion in the soft segment to improve the dye uptake and fixation rate of the spandex. In the present invention, the weight proportion of the structure represented by formula (1) in the soft segment should be greater than 2%, preferably greater than 5%, preferably greater than 10%, more preferably greater than 30%, and most preferably greater than 50%.

[0100] The polyetherester structure represented by formula (1) has little effect on the mechanical properties of spandex, so its mass proportion in the soft segment can be appropriately increased. However, due to the presence of ester groups in this structure, the spandex containing this structure has a certain gap in alkali resistance compared to spandex made from polytetramethylene ether glycol, and may suffer a loss in mechanical properties during the dyeing and finishing process. Therefore, the mass proportion of the polyetherester structure represented by formula (1) in the spandex soft segment should not be too high, preferably less than 80%, more preferably less than 70%, and more preferably less than 65%. Specifically, spandex prepared from polyetherester polyol can be blended with spandex prepared from polyether polyol in the form of raw materials, prepolymers, and polymers to improve the alkali resistance of spandex prepared from polyetherester polyol.

[0101] The present invention also provides a method for preparing the easy-to-dye spandex. The easy-to-dye spandex can be prepared by dry spinning or melt spinning, wherein the dry spinning comprises the following steps:

[0102] Step 1): using a diisocyanate raw material to cap a diol raw material to prepare a prepolymer;

[0103] Step 2): dissolving the prepolymer using a polar solvent to obtain a prepolymer solution;

[0104] Step 3): chain extending the prepolymer using a mixed solution of a linker and a terminator to obtain a polyurethane / polyurethane urea solution;

[0105] Step 4): adding an auxiliary agent to prepare a spinning solution;

[0106] Step 5): The obtained spinning solution is passed through a spinning device to obtain easy-to-dye spandex.

[0107] Compared with conventional spandex dry spinning, the improvement of the solution of the present invention mainly lies in the change of diol raw materials.

[0108] In one embodiment of the present invention, the diol raw material includes a polyether ester polyol having an aromatic group-polyether block structure, and the polyether ester polyol is composed of a repeating unit represented by formula (1) and a capped alcohol hydroxyl group:

[0109] Wherein R1 is at least one of an aromatic ring and an aromatic heterocycle, and the mass content of R1 in the repeating unit is 4.5%-44%; R2 is at least one of a linear saturated alkane group having 2-3 carbon atoms; x is 2-20, preferably 3-10; the average functionality of the end-capped alcohol hydroxyl group is 1.95-2.00; and the number average molecular weight of the polyetherester polyol is 800-5000, preferably 1000-3500, more preferably 1400-2500, and most preferably 1500-2300.

[0110] Optionally, the polyetherester polyol is heated at 90°C and a shear rate of 1s -1 The viscosity can be less than 500 poise, preferably less than 200 poise.

[0111] In addition to being prepared by the method described above, the polyetherester polyol can also be prepared by a condensation reaction or transesterification reaction between an aromatic dibasic acid, its esterified product, or its anhydride and a polyether glycol. In one embodiment, the esterified product can be obtained by reacting an aromatic dibasic acid with a monohydric alcohol having a boiling point below 150°C, such as a small molecule alcohol such as methanol, ethanol, n-butanol, or n-hexanol. Thus, the esterified product can be easily removed by distillation in a subsequent esterification reaction or transesterification reaction; the small molecule alcohol is preferably methanol or ethanol. Moreover, compared to aromatic dibasic acids, the transesterification reaction between the esterified product and the polyether glycol can be carried out under milder reaction conditions, which facilitates production process design.

[0112] To ensure that dye molecules can more easily enter the interior of the spandex yarn, the polyether diol is preferably at least one of a series of directly connected saturated alkane groups with 2-3 carbon atoms. The high density of ether oxygen bonds can make the polyether segment more hydrophilic, making it easier for the spandex to be swollen by the dye solution during acid dyeing and disperse dyeing, increasing the gap between molecules and making it easier for the dye molecules to enter the interior of the spandex yarn. Specifically, the polyether diol can be polyethylene glycol (PEG), polypropylene glycol (P3OG), or a copolyether diol of ethylene glycol and propylene glycol. Preferably, the polyether diol is polyethylene glycol (PEG), which has a higher ether oxygen bond density and can make the spandex more hydrophilic, thereby making it easier for the dye molecules to enter the interior of the spandex yarn.

[0113] The aromatic dibasic acid can be selected from one or more of terephthalic acid, isophthalic acid, phthalic acid, biphenyl dicarboxylic acid, 1,4-naphthalene dicarboxylic acid, 2,6-naphthalene dicarboxylic acid, 2,3-naphthalene dicarboxylic acid, 2,5-furan dicarboxylic acid, terephthalic acid, isophthalic acid, and phthalic acid. Since most acidic dye molecules and disperse dye molecules are macromolecules containing aromatic rings, the aromatic ring structure introduced by the polyether ester polyol has stronger van der Waals interactions with the dye molecules, resulting in stronger interaction between the dye molecules and the polyether ester chain segments after entering the spandex, making them more easily fixed within the spandex molecules. Therefore, under the combined action of the polyether chain segments and the aromatic ring structure, the spandex with the polyether-aromatic ring structure has better dye uptake and fixation rates than conventional spandex.

[0114] By using the polyetherester polyol containing the aromatic group-polyether block structure as the soft segment raw material of spandex, the structure described in formula (1) can be introduced into the molecular structure of spandex.

[0115] Due to the presence of ester groups in the aforementioned polyetherester polyols, using them exclusively as diol raw materials for spandex results in a certain alkali resistance disadvantage compared to polyether-based spandex. Therefore, to limit the mass ratio of aromatic group-polyether block structures in the spandex soft segment, a specific method for controlling this mass ratio can be to blend spandex prepared from polyetherester polyols with spandex prepared from polyether-based polyols in the form of diol raw materials, prepolymers, or polymers to improve the alkali resistance of the spandex prepared from the polyetherester polyols.

[0116] Taking the blending of glycol raw materials for spandex as an example, in order to make spandex have better dye uptake and fixation rate, the mass ratio of the polyether ester polyol in the glycol raw material should be greater than 2%, preferably greater than 5%, preferably greater than 10%, more preferably greater than 20%, more preferably greater than 30%, more preferably greater than 40%, and most preferably greater than 50%.

[0117] In order to ensure the alkali resistance of the prepared spandex, the mass ratio of the polyether ester polyol in the diol raw material is less than 80%, preferably less than 70%, and more preferably less than 65%.

[0118] Optionally, in addition to the polyetherester polyols described above, the diol raw materials may also include other diol compounds that can serve as spandex soft segments, such as polytetramethylene ether glycol, polyethylene glycol, polypropylene glycol, and other polyether glycols; polybutylene adipate glycol; copolyester diols of adipic acid and mixed diols (such as ethylene glycol / 1,4-butanediol, ethylene glycol / 1,2-propylene glycol, 1,6-hexanediol / 2,2-dimethylpropylene glycol-1,3); other polyetherester diols that can serve as spandex soft segments; or mixtures of at least two of the above diol compounds. To ensure the alkali resistance of spandex, polyether glycols are preferred as the second diol raw material, with polytetramethylene ether glycol being most preferred. The mass of the second diol raw material preferably accounts for 30%-98%, preferably 35%-90%, of the total diol raw materials. That is, a preferred solution is to blend the polyetherester polyol with the second type of diol raw material as the diol raw material for spandex.

[0119] The method of blending with prepolymers or polymers is similar to the above and will not be described in detail here.

[0120] In order to ensure the alkali resistance of the prepared spandex, in another embodiment of the present invention, the diol raw material includes a polyether ester polyol having an aromatic group-polyether block structure, and the polyether ester polyol comprises a repeating unit represented by formula (1) and a capped alcohol hydroxyl group:

[0121] Wherein R1 is at least one of an aromatic ring and an aromatic heterocycle, and the mass content of R1 in the repeating unit is 4.5%-44%; R2 is at least one of a linear saturated alkane group having 2-3 carbon atoms; x is 2-20, preferably 3-10; the mass percentage of the repeating unit represented by formula (1) in the polyether ester polyol is greater than 2%, preferably greater than 5%, preferably greater than 10%; the average functionality of the end-capped alcohol hydroxyl group is 1.95-2.00, and the number average molecular weight of the polyether ester polyol is 800-5000, preferably 1000-3500, more preferably 1400-2500, and most preferably 1500-2300.

[0122] Unlike the previous embodiment, which employs a method of blending polyetherester polyol with the second type of diol raw material, this embodiment reduces the proportion of the cyclic structure in formula (1) in the polyetherester polyol. Similarly, to balance the dyeing performance and alkali resistance of spandex, in a preferred embodiment, the mass ratio of the cyclic structure in formula (1) in the polyetherester polyol should be greater than 5%, preferably greater than 10%, more preferably greater than 30%, and most preferably greater than 50%. It is also preferably less than 80%, more preferably less than 70%, and more preferably less than 65%. The remainder of the polyetherester polyol may contain some other polyester structures or polyether structures, or some aliphatic structures as modified structures. To ensure the mechanical properties of spandex, a polyether structure is preferred, and a polytetramethylene ether structure is most preferred.

[0123] Likewise, the polyetherester polyols mentioned above can be blended with the second type of diol raw material mentioned above to serve as diol raw materials for spandex.

[0124] In the method for preparing easy-dye spandex of the present invention, the diisocyanate raw material in step 1) can be one or more of diphenylmethane diisocyanate, toluene diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, dicyclohexylmethane diisocyanate and isomers thereof.

[0125] The polar solvent in step 2) is at least one of N,N-dimethylformamide and N,N-dimethylacetamide.

[0126] The chain extender in step 3) can be an amine or alcohol chain extender, wherein the amine chain extender can be a diamine with 2 to 30 carbon atoms, for example, it can be selected from one or more of ethylenediamine, propylenediamine, butylenediamine, pentamethylenediamine, methylpentamethylenediamine, methylpropylenediamine, hexamethylenediamine, triethylenediamine, phenylenediamine, phenylenediamine, diaminocyclohexane, hexamethylenediamine, and dopamine; the alcohol chain extender can be one or more of common chain extenders such as ethylene glycol, 1,4-butanediol, diethylene glycol, 1,6-hexanediol, 1,3-propylene glycol, and 1,4-dihydroxymethylcyclohexane. The chain terminator can be a monoamine having 2 to 20 carbon atoms, and can be selected from one or more of ethylamine, isopropylamine, n-butylamine, tert-butylamine, hexylamine, dimethylamine, diethylamine, dipropylamine, di-n-butylamine, di-tert-butylamine, diisobutylamine, diisopropylamine, cyclohexylamine or ethanolamine.

[0127] Melt spinning includes the following steps:

[0128] Step a) adding a diisocyanate raw material, a diol raw material, and a small molecule polyol chain extender into a reaction container respectively;

[0129] Step b) mixing the materials in the reaction container, and heating the materials during or after the mixing process to react and extruding and granulating the materials to produce polyurethane particles;

[0130] Step c) drying the polyurethane particles, adding an auxiliary agent and then performing melt spinning.

[0131] The raw materials for preparing the above-mentioned melt-spinning spandex, such as diisocyanate and diol raw materials, are similar to those for dry spinning, except that the chain extender in step a) is only an alcohol chain extender.

[0132] Example

[0133] The present invention is described in more detail below by way of examples, wherein the testing methods of the parameters involved are as follows:

[0134] 1. Average functionality:

[0135] Functionality = 2*moles of alcoholic hydroxyl groups / (moles of alcoholic hydroxyl groups + moles of carboxyl groups + moles of double bonds).

[0136] The acid value was measured using the method described in HG / T 2708-1995; the hydroxyl value was measured according to the method described in HG / T 2709 / 1995; and the degree of unsaturation was measured according to the method described in GB / T 12008.6-2010. The corresponding acid value, hydroxyl value, and degree of unsaturation were converted into the molar number of the corresponding end groups in the polyetherester diol.

[0137] 2. 300% tensile stress, breaking strength and elongation at break: all in accordance with the "Textile Industry Standard of the People's Republic of China" FZ / T 50006-2013, "Test method for tensile properties of spandex yarn".

[0138] 3. Plastic deformation test:

[0139] Clamp one end of the prepared specimen into the upper clamp, apply pre-tension to the other end, straighten the specimen axially and clamp it into the lower clamp, and start the instrument.

[0140] The specimen is stretched from 0% elongation L0 to 300% elongation L1 at a speed of 500 mm / min, and then returned to 0% elongation, and the stretching and recovery cycles are repeated four times; during the fifth stretching to 300% elongation, the force value F1 when stretched to 200% is recorded, and then it is delayed for 30 seconds and returned to 0% elongation. During this process, the force value F2 when it is recovered to 200% is recorded; after a delay of 30 seconds, the sixth stretching is performed, and the length L2 of the specimen stretched to the pre-tensioned position is recorded.

[0141] Plastic deformation rate calculation formula: (L2-L0) / L0*100%

[0142] Among them, "5LP200%" represents the stress value when it is stretched to 200% elongation for the 5th time, that is, F1; "5UP200%" represents the rebound stress value when it is stretched from 300% elongation to 200% elongation for the 5th time, that is, F2, which can be used to characterize the recovery modulus; "plastic deformation rate" represents the increase ratio of the spandex yarn length compared to the original length after 5 stretching; "5UP200% / 5LP 200%" represents the ratio of the 200% recovery stress to the 200% tensile stress in the 5th stretching cycle test.

[0143] 4. Dyeing rate of acid dyes and fixation rate after soaping:

[0144] In the present invention, acid red is used as the acid dye, and the dye concentration in the dye solution before dyeing is measured as A, the dye concentration after dyeing is measured as B, and the dye concentration in the washing solution after soaping is measured as C. The following are obtained: Acid dye uptake = (AB) / A Acid dye fixation rate after soaping = (ABC) / A

[0145] 5. Dyeing rate of disperse dyes and fixation rate after soaping:

[0146] In the present invention, disperse orange is used as the spinning dye, and the dye concentration in the dye liquor before dyeing is measured as P, the dye concentration after dyeing is measured as Q, and the dye concentration in the washing liquid after soaping is measured as M, and the following are obtained: Disperse dye uptake = (PQ) / P Disperse dye fixation rate after soaping = (PQM) / P

[0147] 6. Spandex alkali resistance test:

[0148] The spandex yarn was boiled in 10 g / L potassium hydroxide solution at 100°C for 1 hour, and the mechanical properties before and after boiling were tested.

[0149] In addition, the antioxidant mentioned in the following examples is antioxidant 245, the dyeing auxiliary is DH300R or 2462B, and the light stabilizer is Tinuvin 791, all of which are commercially available substances.

[0150] In the following examples, due to the presence of small molecule polyols distilled out as non-condensable gases during the reaction and the volatilization of small molecule components in the polyether diol, the actual alcohol-acid ratio participating in the reaction is less than the theoretical value. Therefore, the molecular weight of the final product is larger than the theoretical value, but the deviation is within an acceptable range.

[0151] Examples 1-6 below are about the preparation of polyetherester polyols using polyethylene terephthalate (PET) as a raw material.

[0152] Example 1 Preparation of polyetherester polyol with a molecular weight of 1200

[0153] First, polyethylene terephthalate was crushed, and 2081.9g of the crushed polyethylene terephthalate (PET) and 3000g of polyethylene glycol (PEG200) with a number average molecular weight of 200 were added to the reactor (i.e., the molar ratio was about 1.38). 3g of zinc acetate and 1.5g of Sb2O3 were added as catalysts, and the temperature was gradually raised to 235°C to start the transesterification reaction. The temperature was maintained at 235°C until the reaction system was homogeneous. The ethylene glycol in the reaction system was evaporated by vacuum distillation until the amount of ethylene glycol evaporated was close to the theoretical value. 650g of ethylene glycol was evaporated from the reaction system. A polyether ester polyol with a molecular weight of 1200 was obtained. The polyether ester polyol was heated at 40°C for 1S -1 The viscosity is 100 Poise, the acid value is 0.3, and it is a light yellow liquid at room temperature.

[0154] Example 2 Preparation of polyetherester polyol with a molecular weight of 2100

[0155] First, polyethylene terephthalate was crushed, and 2428.9 g of the crushed polyethylene terephthalate (PET) and 3000 g of polyethylene glycol (PEG200) with a number average molecular weight of 200 were added to the reactor (i.e., the molar ratio was about 1.19), 3 g of magnesium acetate and 1.5 g of Sb2O3 were added as catalysts, and the temperature was gradually raised to 235 ° C to start the ester exchange reaction. The temperature was maintained at 235 ° C until the reaction system was homogeneous, and the ethylene glycol in the reaction system was evaporated by vacuum distillation until the amount of ethylene glycol evaporated was close to the theoretical value. 781.9 g of ethylene glycol was evaporated from the reaction system. A polyether ester polyol with a molecular weight of 2100 was obtained. The polyether ester polyol was heated at 40 ° C for 1 s - 1 The viscosity is 210 Poise, the acid value is 0.3, and it is a light yellow liquid at room temperature.

[0156] Example 3 Preparation of polyetherester polyol with a molecular weight of 3400

[0157] First, polyethylene terephthalate was crushed, and 2602.4g of the crushed polyethylene terephthalate (PET) and 3000g of polyethylene glycol (PEG200) with a number average molecular weight of 200 were added to the reactor (i.e., the molar ratio was about 1.11), and 3g of zinc acetate and 1.5g of Sb2O3 were added as catalysts. The temperature was gradually raised to 235°C to start the transesterification reaction. The temperature was maintained at 235°C until the reaction system was homogeneous. The ethylene glycol in the reaction system was evaporated by vacuum distillation until the amount of ethylene glycol evaporated was close to the theoretical value. 842.3g of ethylene glycol was evaporated from the reaction system. A polyether ester polyol with a molecular weight of 3400 was obtained. The polyether ester polyol was heated at 40°C for 1S - 1 The viscosity is 650 Poise, the acid value is 0.3, and it is a light yellow liquid at room temperature.

[0158] Example 4 Preparation of polyetherester polyol with a molecular weight of 1500

[0159] First, polyethylene terephthalate was crushed, and 1296.5 g of the crushed polyethylene terephthalate (PET) and 4203 g of polyethylene glycol (PEG400) with a number average molecular weight of 400 were added to the reactor (i.e., the molar ratio was about 1.57). 3 g of zinc acetate and 1.5 g of Sb2O3 were added as catalysts, and the temperature was gradually raised to 245 ° C to start the ester exchange reaction. The temperature was maintained at 245 ° C until the reaction system was homogeneous. The ethylene glycol in the reaction system was evaporated by vacuum distillation until the amount of ethylene glycol evaporated was close to the theoretical value. 418.6 g of ethylene glycol was evaporated from the reaction system. A polyether ester polyol with a molecular weight of 1500 was obtained. The polyether ester polyol was heated at 40 ° C for 1 s - 1The viscosity is 73.5 Poise, the acid value is 0.3, and it is a light yellow liquid at room temperature.

[0160] Example 5 Preparation of polyetherester polyol with a molecular weight of 3450

[0161] First, polyethylene terephthalate was crushed, and 1019.2 g of the crushed polyethylene terephthalate (PET) and 4480 g of polyethylene glycol (PTG650) with a number average molecular weight of 650 were added to the reactor (i.e., the molar ratio was about 1.30), and 3 g of zinc acetate and 1.5 g of Sb2O3 were added as catalysts. The temperature was gradually raised to 245 ° C to start the ester exchange reaction. The temperature was maintained at 245 ° C until the reaction system was homogeneous. The ethylene glycol in the reaction system was evaporated by vacuum distillation until the amount of ethylene glycol evaporated was close to the theoretical value. 329 g of ethylene glycol was evaporated from the reaction system. A polyether ester polyol with a molecular weight of 3450 was obtained. The polyether ester polyol was heated at 40 ° C for 1 s -1 The viscosity is 35.2 Poise, the acid value is 0.3, and it is a light yellow liquid at room temperature.

[0162] Example 6 Preparation of polyetherester polyol with a molecular weight of 3500

[0163] First, polyethylene terephthalate was crushed, and 699g of the crushed polyethylene terephthalate (PET) and 4800.2g of poly 1,3-propylene glycol (P3OG1000) with a number average molecular weight of 1000 were added to the reactor (i.e., the molar ratio was about 1.32). 3g of zinc acetate and 1.5g of Sb2O3 were added as catalysts, and the temperature was gradually raised to 250°C to start the transesterification reaction. The temperature was maintained at 250°C until the reaction system was homogeneous. The ethylene glycol in the reaction system was evaporated by vacuum distillation until the amount of ethylene glycol evaporated was close to the theoretical value. 286g of ethylene glycol was evaporated from the reaction system. A polyether ester polyol with a molecular weight of 3500 was obtained. The polyether ester polyol was heated at 40°C for 1S -1 The viscosity is 28.5 Poise, the acid value is 0.3, and it is a light yellow liquid at room temperature.

[0164] Example 7 Preparation of polyetherester polyol with a molecular weight of 3480

[0165] First, polybutylene terephthalate was crushed, and 1137.14g of the crushed polybutylene terephthalate (PBT) and 4362.85g of polytetrahydrofuran (PTG650) with a number average molecular weight of 650 were added to the reactor (i.e., the molar ratio was about 1.30), 3g of zinc acetate and 1.5g of Sb2O3 were added as catalysts, and the temperature was gradually raised to 260°C to start the transesterification reaction. The temperature was maintained at 260°C until the reaction system was homogeneous, and the ethylene glycol in the reaction system was evaporated by vacuum distillation until the amount of ethylene glycol evaporated was close to the theoretical value. 465g of butanediol was evaporated from the reaction system. A polyether ester polyol with a molecular weight of 3480 was obtained. The polyether ester polyol was heated at 40°C for 1S -1 The viscosity is 35.8 Poise, the acid value is 0.3, and it is a light yellow liquid at room temperature.

[0166] Examples 8-10 below are examples of using polyetherester polyols to prepare polyurethane elastic fibers.

[0167] Example 8 The polyetherester polyol of Example 1 is used to prepare polyurethane elastic fiber

[0168] 100 kg of the polyetherester polyol prepared in Example 1 was added to a reactor that had been thermostatted to 45°C, stirring was started at a speed of 150 rpm, 31 kg of diphenylmethane diisocyanate was added, and after stirring for 5 minutes, the temperature was raised to 90°C; the mixture was reacted at 90°C for 2 hours to obtain a prepolymer.

[0169] The prepolymer was cooled to 50°C and dissolved in 166.72 kg of dimethylacetamide (DMAc). A 3.2% amine solution containing 2.40 kg of ethylenediamine and 0.29 kg of diethylamine was then added, with stirring increased to 300 rpm, to initiate a chain extension reaction. After the chain extension reaction was complete, the necessary antioxidants, dyeing aids, and other auxiliaries were added, and the mixture was aged for 30 hours to produce a spinning solution with a solids content of 35%. This solution was dry-spun to produce 40D polyurethane elastic fiber PUU-3.

[0170] Example 9 The polyetherester polyol of Example 6 is used to prepare polyurethane elastic fiber

[0171] 100 kg of the polyetherester polyol prepared in Example 1 was added to a reactor that had been thermostatted to 45°C, and stirring was started at a speed of 150 rpm. 16.15 kg of diphenylmethane diisocyanate was added, and the mixture was stirred for 5 minutes and then heated to 90°C; the mixture was reacted at 90°C for 2 hours to obtain a prepolymer.

[0172] The prepolymer was cooled to 50°C and dissolved in 147.82 kg of dimethylacetamide (DMAc). A 3.2% amine solution containing 2.13 kg of ethylenediamine and 0.26 kg of diethylamine was then added, with stirring increased to 300 rpm, to initiate a chain extension reaction. After the chain extension reaction was complete, the necessary antioxidants, dyeing aids, and other auxiliaries were added, and the mixture was aged for 30 hours to produce a spinning solution with a solids content of 35%. This solution was dry-spun to produce 40D polyurethane elastic fiber PUU-4.

[0173] Example 10 The polyetherester polyol of Example 7 is used to prepare polyurethane elastic fiber

[0174] 100 kg of the polyetherester polyol prepared in Example 1 was added to a reactor that had been thermostatted to 45°C, and stirring was started at a speed of 150 rpm. 16.20 kg of diphenylmethane diisocyanate was added, and the mixture was stirred for 5 minutes and then heated to 90°C; the mixture was reacted at 90°C for 2 hours to obtain a prepolymer.

[0175] The prepolymer was cooled to 50°C and dissolved in 147.89 kg of dimethylacetamide (DMAc). A 3.2% amine solution containing 2.14 kg of ethylenediamine and 0.27 kg of diethylamine was then added, with stirring increased to 300 rpm, to initiate a chain extension reaction. Following the chain extension reaction, the necessary antioxidants, dyeing aids, and other auxiliaries were added, followed by aging for 30 hours to produce a spinning solution with a solids content of 35%. This solution was dry-spun to produce 40D polyurethane elastic fiber PUU-5.

[0176] Comparative Example 1 Polytetramethylene glycol (PTMG) with a number average molecular weight of 2000 is used to prepare polyurethane elastic fibers

[0177] Add 100 kg of polytetrahydrofuran (PTMG2000) (number average molecular weight 2000) to a reactor maintained at 45°C and stir at 150 rpm. Add 22.2 kg of diphenylmethane diisocyanate, stir for 5 minutes, then heat to 90°C and react at 90°C for 2 hours to obtain a prepolymer.

[0178] The prepolymer was cooled to 50°C and dissolved in 155.5 kg of dimethylacetamide (DMAc). A 3.2% amine solution containing 2.26 kg of ethylenediamine and 0.28 kg of diethylamine was then added, with stirring increased to 300 rpm, to initiate a chain extension reaction. After the chain extension reaction was complete, the necessary antioxidants, dyeing aids, and other auxiliaries were added, and the mixture was aged for 30 hours to produce a spinning solution with a solids content of 35%. This solution was dry-spun to produce 40 denier polyurethane elastic fiber PUU-0.

[0179] Comparative Example 2 Polyethylene glycol with a number average molecular weight of 1500 is used to prepare polyurethane elastic fibers

[0180] Add 100 kg of polyethylene glycol (1500 number-average molecular weight) to a reactor maintained at 45°C and stir at 150 rpm. Add 26.5 kg of diphenylmethane diisocyanate, stir for 5 minutes, then heat to 90°C and react at 90°C for 2 hours to obtain a prepolymer.

[0181] The prepolymer was cooled to 50°C and dissolved in 161 kg of dimethylacetamide (DMAc). A 3.2% amine solution containing 2.32 kg of ethylenediamine and 0.28 kg of diethylamine was then added, with stirring increased to 300 rpm, to initiate a chain extension reaction. After the chain extension reaction was complete, the necessary antioxidants, dyeing aids, and other auxiliaries were added, and the mixture was aged for 30 hours to produce a spinning solution with a solids content of 35%. This solution was dry-spun to produce 40 denier polyurethane elastic fiber PUU-1.

[0182] Comparative Example 3: Polypropylene glycol with a number average molecular weight of 2000 is used to prepare polyurethane elastic fiber

[0183] Add 100 kg of polypropylene glycol (2000 number-average molecular weight) to a reactor maintained at 45°C and stir at 150 rpm. Add 21.98 kg of diphenylmethane diisocyanate, stir for 5 minutes, then heat to 90°C and react at 90°C for 2 hours to obtain a prepolymer.

[0184] The prepolymer was cooled to 50°C and dissolved in 155.24 kg of dimethylacetamide (DMAc). A 3.2% amine solution containing 2.24 kg of ethylenediamine and 0.28 kg of diethylamine was then added, with stirring increased to 300 rpm, to initiate a chain extension reaction. After the chain extension reaction was complete, the necessary antioxidants, dyeing aids, and other auxiliaries were added, and the mixture was aged for 30 hours to produce a spinning solution with a solids content of 35%. This solution was dry-spun to produce 40 denier polyurethane elastic fiber PUU-2.

[0185] Comparative Example 4 Preparation of polyetherester polyol with a molecular weight of 1200

[0186] First, polyethylene terephthalate is crushed, and 2602.4g of the crushed polyethylene terephthalate (PET) and 3000g of polyethylene glycol (PEG200) with a number average molecular weight of 200 are added to a reactor. 3g of zinc acetate and 1.5g of Sb2O3 are added as catalysts, and the temperature is gradually raised to 235°C to start the transesterification reaction. The temperature is maintained at 235°C until the reaction system becomes homogeneous. The ethylene glycol in the reaction system is distilled out by vacuum distillation, and 681g of ethylene glycol is distilled out of the reaction system. A polyether ester diol with a molecular weight of 1200 is obtained. The polyether ester diol is solid at 40°C, has a melting point of 60°C, an acid value of 0.3, and a molar proportion of the ethylene glycol ester structure is 20%.

[0187] Comparative Example 5 The polyether ester polyol of Comparative Example 4 is used to prepare polyurethane elastic fiber

[0188] 100 kg of the polyetherester polyol prepared in Comparative Example 4 was added to a reactor that had been thermostatted to 90° C., stirring was started at a speed of 150 rpm, and 31 kg of diphenylmethane diisocyanate was added to start a prepolymerization reaction. When the reaction was carried out for 57 minutes, the viscosity of the prepolymer was too high and the prepolymerization reaction could not be continued.

[0189] According to the above test method, the following parameters of the polyurethane elastic fibers (i.e., spandex yarns) obtained in Examples 8, 9, and 10 and Comparative Examples 1, 2, and 3 were tested, and the test results are summarized in the following table.

[0190] From the data in the above table, it can be seen that the polyurethane elastic fiber prepared using the polyether ester polyol of the present invention has a significantly improved tensile stress and breaking strength compared to the polyurethane elastic fiber prepared using polyethylene glycol as a raw material, and is close to or exceeds the polyurethane elastic fiber prepared using conventional polytetrahydrofuran ether diol, which can meet the performance requirements of spandex yarn for clothing; in addition, the plastic deformation rate of the polyurethane elastic fiber prepared using the polyether ester polyol of the present invention is significantly reduced; from the value of 5UP200%, the polyurethane elastic fiber using the polyether ester diol of the present invention has a greater 5UP200% recovery stress, that is, a greater recovery modulus, which indicates that the rebound force is greater and the fabric shape retention is better. In summary, the preparation method of the polyether ester polyol provided by the present invention can use post-consumer polyester as a raw material to prepare a polyether ester polyol raw material for spandex with performance comparable to that of existing polytetrahydrofuran, and the prepared spandex has similar performance to the spandex prepared from polytetrahydrofuran, has good mechanical properties, and effectively improves the wearing performance. Therefore, the polyether ester polyol prepared by the method for preparing polyether ester polyol from polyester provided by the present invention can be used as the soft segment raw material of spandex, which broadens the application path of polyester recycled materials and also broadens the raw material source of spandex.

[0191] The spinning solutions in Examples 8, 9, and 10 and Comparative Examples 1, 2, and 3 were diluted from a solid content of 35% to a solid content of 20%. Polyurethane film gloves were then prepared by dip coating. The corresponding film strips PUU-F3, PUU-F4, and PUU-F5 of the examples, and the corresponding film strips PUU-F0, PUU-F1, and PUU-F2 of the comparative examples, were cut and cut. The specific steps for preparing the film strips are as follows:

[0192] First, slowly immerse the hand mold in a tank filled with the diluted stock solution. Then, slowly lift the hand mold out of the tank and slowly rotate it to even out the stock solution on the surface. The hand mold is then dried in an oven. After drying, the glove is peeled off to obtain a polyurethane film glove with a wall thickness of approximately 150 microns. To test the mechanical properties of the glove film, the film is cut from the palm portion of the glove and cut into strips 6 mm wide and 10 cm long. The mechanical properties are then tested.

[0193] The mechanical properties are as follows:

[0194] As can be seen from the data in the table above, film gloves prepared using the polyetherester polyols of the present invention, when tested on film sheets cut from the palm of the hand, exhibit significantly improved tensile stress and breaking strength compared to thin-walled film sheets made from polyethylene glycol and polypropylene glycol. These performances approach or exceed the mechanical properties of film sheets made from polytetrahydrofuran, meeting the mechanical property requirements of elastic film gloves and consistent with findings for spandex yarn. Furthermore, polyurethane film gloves prepared using the polyetherester diols of the present invention exhibit low plastic deformation, resulting in a more stable film glove shape. The 5UP200% value indicates that polyurethane film sheets prepared using the polyetherester diols of the present invention exhibit greater 5UP200% resilience, resulting in better glove coverage. Furthermore, while maintaining sufficient coverage, the gloves can be made thinner, thereby reducing the raw material cost of the film gloves. The polyetherester polyol provided by the invention effectively improves the mechanical properties of polyurethane film membranes when the polyetherester polyol is used as the soft segment of the fiber. On this basis, it also enables thin-walled glove film products to have a lower plastic deformation rate and a higher recovery modulus, maintains the shape of the film glove products, improves the wrapping properties of the film glove products, and can reduce the raw material production cost.

[0195] Example 11 Melt-spun spandex prepared from the polyetherester polyol of Example 2

[0196] The polyetherester polyol of Example 2, 1,4-butanediol, and diphenylmethane diisocyanate were respectively metered into a twin-screw extruder at a molar ratio of 1.2:2:3.2, and continuously polymerized and extruded at 195°C. The extruder was granulated underwater and dried until the moisture content of the polyurethane pellets was less than 100 ppm. Then, necessary antioxidants, light stabilizers, and other additives were added and melt-spun to obtain spandex TPU-1 with a denier of 20D.

[0197] Comparative Example 6 Melt-spun spandex prepared from polytetrahydrofuran with a number average molecular weight of 2000

[0198] Polytetramethylene glycol (PTMG2000) (number average molecular weight of 2000), 1,4-butanediol, and diphenylmethane diisocyanate were respectively metered into a twin-screw extruder at a molar ratio of 1.2:2:3.2, and continuously polymerized and extruded at 190°C. The extrusion was performed underwater, and the polyurethane pellets were dried to a moisture content of less than 100 ppm. Then, necessary antioxidants, light stabilizers, and other additives were added and melt-spun together to obtain TPU-0 with a denier of 20D.

[0199] Comparative Example 7 Melt-spun spandex prepared from polyethylene glycol with a number average molecular weight of 1500

[0200] Polyethylene glycol with a number average molecular weight of 1500, 1,4-butanediol and diphenylmethane diisocyanate are respectively metered into a twin-screw extruder in a molar ratio of 1.2:2:3.2, and continuously polymerized and extruded at 190°C. The pellets are granulated underwater and dried until the moisture content of the polyurethane pellets is less than 100 ppm. Then, necessary antioxidants, light stabilizers and other additives are added and melt-spun together to obtain TPU-2 with a denier of 20D.

[0201] From the mechanical property comparison between the comparative example and the embodiment above, it can be seen that the tensile stress and recovery modulus of the melt-spun spandex yarn processed in melt form with polyether ester as the raw material are significantly higher than those of the melt-spun spandex processed in melt form with polytetrahydrofuran as the raw material, showing similar mechanical property characteristics and advantages to the dry-process spandex processed in solvent form.

[0202] Hereinafter, Examples 12-18 are used as dyeability tests for the easy-dye spandex provided by the present invention.

[0203] Example 12 Polyetherester polyol with a number average molecular weight of 1500 prepared from polyethylene glycol with a number average molecular weight of 600 and terephthalic acid

[0204] 17 parts by weight of polyethylene glycol PEG600 (number average molecular weight of 600) and 2.7 parts by weight of terephthalic acid were added into the reactor, and nitrogen was passed through to replace the air in the reactor. The stirring in the reactor was turned on and the stirring speed was 150 rpm. The system was programmed to heat up to 150°C and maintained for 5 hours; the temperature was continued to rise to 230°C and maintained at this temperature until the water output rate of the system reached more than 90% of the theoretical value and the solution became homogeneous. The catalyst tetraisopropyl titanate was added and the solution was gradually vacuumed to 2000 Pa; when the acid value was lower than 0.5 mgKOH / g, a polyether ester polyol with a number average molecular weight of 1500 was obtained. After testing, its average functionality was 1.98, 90°C 1S -1 The viscosity is 25 poise and it is liquid at room temperature.

[0205] For polyester recycling considerations, the polyetherester polyol with a number average molecular weight of 1500 in this embodiment can also be prepared using PEG600 and crushed PET as raw materials in a manner similar to that of Examples 1-6.

[0206] Example 13 The polyetherester polyol of Example 12 is used to prepare polyurethane elastic fiber

[0207] 100 kg of the polyetherester polyol prepared in Example 1 was added to a reactor that had been thermostatted to 45°C, stirring was started at a speed of 150 rpm, 31 kg of diphenylmethane diisocyanate was added, and after stirring for 5 minutes, the temperature was raised to 90°C; the mixture was reacted at 90°C for 2 hours to obtain a prepolymer.

[0208] The prepolymer was cooled to 50°C and dissolved in 166.72 kg of dimethylacetamide (DMAc). A 3.2% amine solution containing 2.40 kg of ethylenediamine and 0.29 kg of diethylamine was then added, with stirring increased to 300 rpm, to initiate a chain extension reaction. After the chain extension reaction was complete, the necessary antioxidants, dyeing aids, and other auxiliaries were added, and the mixture was aged for 30 hours to produce a spinning solution with a solids content of 35%. This solution was dry-spun to produce 40D polyurethane elastic fiber PUU-6.

[0209] Example 14 The polyetherester polyol of Example 12 and polytetramethylene glycol (PTMG) with a number average molecular weight of 2000 are used to prepare polyurethane fibers.

[0210] 50 kg of the polyetherester polyol prepared in Example 1 and 50 kg of polytetrahydrofuran with a number average molecular weight of 2000 were added to a reactor that had been thermostatted to 45°C. Stirring was started at a speed of 150 rpm. 21.88 kg of diphenylmethane diisocyanate was added. After stirring for 5 minutes, the mixture was heated to 90°C and reacted at 90°C for 2 hours to obtain a prepolymer.

[0211] The prepolymer was cooled to 50°C and dissolved in 161.3 kg of dimethylacetamide (DMAc). A 3.26% amine solution containing 2.38 kg of ethylenediamine and 0.29 kg of diethylamine was then added, with the stirring speed increased to 300 rpm to initiate a chain extension reaction. After the chain extension reaction was complete, the necessary antioxidants, dyeing auxiliaries, and other additives were added (the dyeing auxiliaries were added at a 1% concentration, 2462B). The mixture was aged for 30 hours to obtain a spinning solution with a solids content of 35%. This solution was dry-spun to produce 40D polyurethane elastic fiber PUU-7.

[0212] Example 15 The prepolymer prepared from the polyetherester polyol of Example 12 and polytetramethylene glycol (PTMG) with a number average molecular weight of 2000 is used to prepare polyurethane fibers.

[0213] 50 kg of the polyetherester polyol prepared in Example 1 was added to a reactor that had been thermostatted to 45° C., stirring was started at a speed of 150 rpm, 15.64 kg of diphenylmethane diisocyanate was added, and the mixture was stirred for 5 minutes and then heated to 90° C.; the mixture was reacted at 90° C. for 2 hours to obtain prepolymer 1.

[0214] 50 kg of polytetrahydrofuran with a number average molecular weight of 2000 was added to a reactor that had been thermostatted to 45°C. Stirring was started at a speed of 150 rpm. 11.1 kg of diphenylmethane diisocyanate was added. After stirring for 5 minutes, the mixture was heated to 90°C and allowed to react at 90°C for 2 hours to obtain prepolymer 2.

[0215] Prepolymers 1 and 2 were cooled to 50°C and transferred to the same reactor. 161.3 kg of dimethylacetamide (DMAc) was used to dissolve the prepolymers. A 3.26% amine solution containing 2.38 kg of ethylenediamine and 0.29 kg of diethylamine was then added. The stirring speed was increased to 300 rpm to initiate a chain extension reaction. After the chain extension reaction was complete, the necessary antioxidants, dyeing auxiliaries, and other additives were added (the dyeing auxiliaries were added at a 1% concentration, 2462B). The mixture was aged for 30 hours to obtain a spinning solution with a solids content of 35%. This solution was dry-spun to produce 40D polyurethane elastic fiber PUU-8.

[0216] Example 16 100 kg of the stock solution prepared in Example 13 and 100 kg of the stock solution prepared in Comparative Example 1 were blended to prepare a stock solution for preparing polyurethane fibers.

[0217] 100 kg of the stock solution prepared in Example 13 and 100 kg of the stock solution prepared in Comparative Example 1 were taken and mixed evenly using a stirring method combined with static mixing in a reactor. The above stock solutions were dry-spun to obtain a polyurethane elastic fiber PUU-9 with a denier of 40D.

[0218] Example 17 The polyetherester polyol of Example 12 and polytetramethylene glycol (PTMG) with a number average molecular weight of 2000 are used to prepare polyurethane fibers.

[0219] 10 kg of the polyetherester polyol prepared in Example 12 and 90 kg of polytetrahydrofuran with a number average molecular weight of 2000 were added to a reactor that had been thermostatted to 45°C. Stirring was started at a speed of 150 rpm. 21.88 kg of diphenylmethane diisocyanate was added, and the mixture was stirred for 5 minutes and then heated to 90°C. The mixture was reacted at 90°C for 2 hours to obtain a prepolymer.

[0220] The prepolymer was cooled to 50°C and dissolved in 161.3 kg of dimethylacetamide (DMAc). A 3.26% amine solution containing 2.38 kg of ethylenediamine and 0.29 kg of diethylamine was then added, with the stirring speed increased to 300 rpm to initiate a chain extension reaction. After the chain extension reaction was complete, the necessary antioxidants, dyeing auxiliaries, and other additives were added (the dyeing auxiliaries were added at a 1% concentration, 2462B). The mixture was aged for 30 hours to obtain a spinning solution with a solids content of 35%. This solution was dry-spun to produce 40D denier polyurethane elastic fiber PUU-10.

[0221] Example 18 The polyetherester polyol of Example 12 and polytetramethylene glycol (PTMG) with a number average molecular weight of 2000 are used to prepare polyurethane fibers.

[0222] 65 kg of the polyetherester polyol prepared in Example 12 and 35 kg of polytetrahydrofuran with a number average molecular weight of 2000 were added to a reactor that had been thermostatted to 45°C. Stirring was started at a speed of 150 rpm. 21.88 kg of diphenylmethane diisocyanate was added. After stirring for 5 minutes, the mixture was heated to 90°C and reacted at 90°C for 2 hours to obtain a prepolymer.

[0223] The prepolymer was cooled to 50°C and dissolved in 161.3 kg of dimethylacetamide (DMAc). A 3.26% amine solution containing 2.38 kg of ethylenediamine and 0.29 kg of diethylamine was then added, with the stirring speed increased to 300 rpm to initiate a chain extension reaction. After the chain extension reaction was complete, the necessary antioxidants, dyeing auxiliaries, and other additives were added (the dyeing auxiliaries were added at a 1% concentration, 2462B). The mixture was aged for 30 hours to obtain a spinning solution with a solids content of 35%. This solution was dry-spun to produce 40D polyurethane elastic fiber PUU-11.

[0224] According to the test method described above, the mechanical property test results of the polyurethane elastic fibers (i.e., spandex yarns) obtained in Examples 12-18 and Comparative Example 1 are summarized in the following table:

[0225] As can be seen from the above table, the easy-to-dye spandex yarn prepared by the method of the present invention has no obvious decrease in mechanical properties compared with conventional polyether spandex.

[0226] According to the test method described above, the dyeing properties of the polyurethane elastic fibers (i.e., spandex yarns) obtained in Examples 12-18 and Comparative Example 1 were tested. The dyeing results of acid dyes are summarized in the following table:

[0227] The dyeing results of disperse dyes are summarized in the following table:

[0228] As can be seen from the above table, the spandex yarn prepared by the method of the present invention has significantly improved dye uptake and fixation rates of acid dyes and disperse dyes compared with conventional polyether spandex.

[0229] According to the test method described above, the alkali resistance test results of the polyurethane elastic fibers (i.e., spandex yarns) obtained in Examples 12-18 and Comparative Example 1 are summarized in the following table:

[0230] As can be seen from the above table, after alkali boiling, the mechanical properties of PUU-6, which is made entirely of polyetherester polyol as the soft segment raw material, partially deteriorated, while the mechanical properties of PUU-7 to PUU-11, which are made of mixed soft segment raw materials, changed less than before alkali boiling.

[0231] The test results above demonstrate that the easy-dye spandex provided by the present invention significantly improves the dye uptake and fixation rates of acid and disperse dyes compared to conventional spandex, while maintaining mechanical properties. By adjusting the formula, the problem of deterioration in the spandex's alkali resistance is also avoided, meeting the requirements for mechanical properties, dyeability, and alkali resistance.

Claims

1. A method for preparing polyetherester polyol, It is characterized in that The steps include: Step 1) adding polyether diol and polyester as raw materials into a reaction kettle, wherein the polyester contains an aromatic dibasic acid polyol ester structure, the degree of polymerization of the polyether diol is 2-20, the molecular weight is 100-1000, and the molar ratio of the aromatic group structure in the polyether diol and the polyester is greater than 1.05:1; Step 2) heating the reactor to the reaction temperature to carry out an ester exchange reaction, and using a vacuum distillation method to evaporate the small molecule polyol produced by the ester exchange reaction to prepare a polyether ester polyol, wherein the reaction temperature is above the boiling point of the small molecule polyol and below the boiling point of the polyether diol.

2. The method for preparing polyetherester polyol according to claim 1, It is characterized in that The polyether diol is one or more of polyethylene glycol, poly-1,3-propylene glycol, poly-1,2-propylene glycol, polytetrahydrofuran, polyethylene glycol-1,2-propylene glycol copolymer, and polytetrahydrofuran-3-methyltetrahydrofuran copolymer.

3. The method for preparing polyether ester polyol according to claim 1, It is characterized in that The molar ratio of the aromatic group structure in the polyether diol and the polyester is calculated by the following formula: R = (W + P-36) / (WA) In the formula, R is the molar ratio of the aromatic group structure in the polyether diol and the polyester, W is the molecular weight of the target polyetherester polyol, and W is 1000-5000, P is the molecular weight of the aromatic dibasic acid in the polyester, A is the average molecular weight of the polyether diol.

4. The polyether ester polyol prepared by the method for preparing polyether ester polyol according to claim 1, It is characterized in that It comprises the structures shown in the following formula (1) and the following formula (2) and a blocked alcohol hydroxyl group: Where R 1 is an aromatic group structure, and R 1 The mass content of the repeating unit of formula (1) is 4.5%-44%, R 2 is at least one of saturated alkane groups having 2 to 5 carbon atoms, x is 2 to 20, R 3 It is the residue of polyol in polyester raw material; The mass ratio of formula (2) in the structure of the polyether ester polyol is less than 20%, preferably less than 10%; The number average molecular weight of the polyether ester polyol is 1000-5000; The average functionality of the capped alcohol hydroxyl groups is 1.95-2.

00.

5. The polyetherester polyol according to claim 4, It is characterized in that The R 2 At least two of the saturated alkane groups having 2 to 5 carbon atoms.

6. An easy-to-dye spandex, It is characterized in that The soft segment of the molecular structure of the easily dyeable spandex comprises a repeating unit represented by the following formula (1): Where R 1 is an aromatic group structure, and R 1 The mass content in the repeating unit is 4.5%-44%; R 2 is at least one of the straight-linked saturated alkane groups having 2 to 3 carbon atoms; x is 2 to 20; The mass of the repeating unit represented by formula (1) accounts for more than 2% and less than 70% of the mass of the spandex soft segment.

7. The easy-to-dye spandex according to claim 6, It is characterized in that The soft segment of the molecular structure of the spandex further comprises a polytetramethylene ether segment.

8. A method for preparing easily dyeable spandex, It is characterized in that The steps include: Step 1): using a diisocyanate raw material to cap a diol raw material to prepare a prepolymer; Step 2): dissolving the prepolymer using a polar solvent to obtain a prepolymer solution; Step 3): using a mixed solution of a linker and a terminator to chain extend the prepolymer to obtain a polyurethane / polyurethane urea solution; Step 4): adding an auxiliary agent to obtain a spinning solution; Step 5): the obtained spinning solution is passed through a spinning device to obtain easy-to-dye spandex; The diol raw materials include polyether ester polyols having an aromatic group-polyether block structure.

9. The method for preparing the easily dyeable spandex according to claim 8, It is characterized in that The polyetherester polyol is composed of a repeating unit and a capped alcohol hydroxyl group as shown in formula (1): Where R 1 is an aromatic group structure, and R 1 The mass content in the repeating unit is 4.5%-44%; R 2 It is at least one of the straight-linked saturated alkane groups having 2 to 3 carbon atoms; x is 2 to 20; preferably 3 to 10; the average functionality of the end-capped alcohol hydroxyl group is 1.95 to 2.00; the number average molecular weight of the polyether ester polyol is 800 to 5000, preferably 1000 to 3500, more preferably 1400 to 2500, and most preferably 1500 to 2300.

10. The method for preparing the easily dyeable spandex according to claim 9, It is characterized in that The mass ratio of the polyether ester polyol in the diol raw material is greater than 5% and less than 70%.

11. The method for preparing the easily dyeable spandex according to claim 9, It is characterized in that The diol raw materials also include one or more of polytetramethylene glycol, polyethylene glycol, polypropylene glycol, polybutylene adipate glycol, adipic acid and copolyester diol of mixed diols.

12. The method for preparing the easily dyeable spandex according to claim 8, It is characterized in that The diol raw material includes a polyether ester polyol having an aromatic group-polyether block structure, and the polyether ester polyol comprises a repeating unit represented by formula (1) and a capped alcohol hydroxyl group: Where R 1 is an aromatic group structure, and R 1 The mass content in the repeating unit is 4.5%-44%; R 2 is at least one of the straight-linked saturated alkane groups having 2 to 3 carbon atoms; x is 2 to 20; preferably 3 to 10; Formula (1) The mass percentage of the repeating units shown in the polyether ester polyol is greater than 5% and less than 70%; the average functionality of the end-capped alcohol hydroxyl group is 1.95-2.00, and the number average molecular weight of the polyether ester polyol is 800-5000, preferably 1000-3500, more preferably 1400-2500, and most preferably 1500-2300.

13. A method for preparing easily dyeable spandex, It is characterized in that The steps include: Step a) adding a diisocyanate raw material, a diol raw material, and a small molecule polyol chain extender into a reaction container respectively; Step b) mixing the materials in the reaction container, and heating the materials during or after the mixing process to react and extruding and granulating the materials to obtain polyurethane particles; Step c) drying the polyurethane particles, adding an auxiliary agent and performing melt spinning to obtain easily dyeable spandex; Wherein, the diol raw material includes polyether ester polyol with an aromatic group-polyether block structure.

14. The method for preparing the easily dyeable spandex according to claim 13, It is characterized in that The polyetherester polyol is composed of a repeating unit and a capped alcohol hydroxyl group as shown in formula (1): Where R 1 is an aromatic group structure, and R 1 The mass content in the repeating unit is 4.5%-44%; R 2 is at least one of the linear saturated alkane groups having 2 to 3 carbon atoms; x is 2 to 20; preferably 3 to 10; the average functionality of the end-capped alcohol hydroxyl group is 1.95 to 2.00; the number average molecular weight of the polyetherester polyol is 800 to 5000, preferably 1000 to 3500, more preferably 1400 to 2500, and most preferably 1500 to 2300; The mass ratio of the polyether ester polyol in the diol raw material is greater than 5% and less than 70%.

15. The method for preparing the easily dyeable spandex according to claim 13, It is characterized in that The polyetherester polyol comprises a repeating unit and a capped alcohol hydroxyl group as shown in formula (1): Where R 1 is an aromatic group structure, and R 1 The mass content in the repeating unit is 4.5%-44%; R 2 is at least one of the straight-linked saturated alkane groups having 2 to 3 carbon atoms; x is 2 to 20; preferably 3 to 10; the mass percentage of the repeating unit represented by formula (1) in the polyether ester polyol is greater than 5%; the average functionality of the end-capped alcohol hydroxyl group is 1.95 to 2.00, and the number average molecular weight of the polyether ester polyol is 800 to 5000, preferably 1000 to 3500, more preferably 1400 to 2500, and most preferably 1500 to 2300.

16. A method for preparing polyurethane elastic fiber, nonwoven fabric, film or elastomer by solution processing or melt processing, using the polyether ester polyol prepared by the method for preparing polyether ester polyol according to any one of claims 1 to 3 or the polyether ester polyol according to claim 4 as a raw material.

17. The polyurethane elastic fiber, nonwoven fabric, film or elastomer obtained by the method according to claim 16.

Citation Information

Patent Citations

  • Polyether polyurethane prepolymers and cast elastomers made therefrom

    CA1251294A

  • Nonwoven based on thermoplastic polyurethane

    CN101400838A

  • Prepn process and apparatus of polyurethane fiber

    CN1147628C

  • Modified melt spun spandex and its prepn. process

    CN1180137C

  • Method for preparing polyether ester polyol and product thereof

    CN118496489A