Light-emitting element, display device, method for manufacturing light-emitting element, and method for forming light-emitting layer
The use of a metal sulfide matrix with encapsulated quantum dots in QLEDs addresses the low durability and efficiency issues by optimizing quantum dot placement and composition, resulting in improved carrier balance and efficiency.
Patent Information
- Application Number
- PCT/JP2023/015421
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-18
- Publication Date
- 2024-10-24
AI Technical Summary
QLEDs suffer from low durability and luminous efficiency due to issues with the light-emitting layer, particularly in the formation and composition of the quantum dot-based light-emitting elements.
A light-emitting element with a matrix containing metal sulfide and encapsulated quantum dots, where the cross-sectional area of the quantum dots is optimized to improve carrier balance and efficiency, and a method involving a quantum dot solution with a specific weight ratio of quantum dots to metal sulfide precursor is used for forming the light-emitting layer.
The solution enhances the durability and luminous efficiency of QLEDs by ensuring better carrier balance and reducing brightness reduction due to charge-up, achieving improved external quantum efficiency and internal quantum yield.
Smart Images

Figure JP2023015421_24102024_PF_FP_ABST
Abstract
Description
Light-emitting element, display device, method for manufacturing light-emitting element, and method for forming light-emitting layer
[0001] The present disclosure relates to a light-emitting element, a display device, a method for manufacturing a light-emitting element, and a method for forming a light-emitting layer.
[0002] In recent years, quantum dot light-emitting diodes (QLEDs), which are light-emitting elements containing quantum dots, and display devices equipped with QLEDs have been attracting a great deal of attention because of their ability to achieve low power consumption, thinness, high image quality, and the like.
[0003] In the field of QLEDs, research into the light-emitting layer provided in QLEDs and methods for forming the light-emitting layer is being actively conducted.
[0004] For example, US Pat. No. 6,299,499 discloses quantum dots with fluoride-containing ligands or fluoride anions bound to their surfaces.
[0005] Patent Publication No. 2020-180278 (published November 5, 2020)
[0006] The invention described in Patent Document 1 has the problem that the durability and luminous efficiency of the light-emitting element are low.
[0007] An object of one embodiment of the present disclosure is to provide a light-emitting element, a display device, a method for manufacturing a light-emitting element, and a method for forming a light-emitting layer, which are capable of improving durability and luminous efficiency.
[0008] In order to solve the above-mentioned problems, the light-emitting element of the present disclosure comprises an anode, a cathode, and a light-emitting layer provided between the anode and the cathode, wherein the light-emitting layer includes a matrix containing a metal sulfide and a plurality of quantum dots encapsulated in the matrix, and in a cross-section of a portion of the light-emitting layer including cross-sections of a predetermined number of the plurality of quantum dots, an area C of the cross-section of the portion of the light-emitting layer is smaller than twice the area B obtained by combining the areas of the cross-sections of the predetermined number of quantum dots.
[0009] In order to solve the above-mentioned problems, the display device of the present disclosure includes the light-emitting element.
[0010] In order to solve the above-mentioned problems, the manufacturing method of the light-emitting element of the present disclosure is a manufacturing method of a light-emitting element including a step of forming the light-emitting layer, wherein the step of forming the light-emitting layer includes a step of preparing a quantum dot solution containing the plurality of quantum dots, a precursor of the metal sulfide, and a solvent, a step of applying the quantum dot solution, and a heat treatment step of thermally decomposing the precursor of the metal sulfide to form a matrix containing the metal sulfide, wherein in the step of preparing the quantum dot solution, the amount of the plurality of quantum dots and the amount of the precursor of the metal sulfide contained in the quantum dot solution are adjusted so that the value of ((weight of light-emitting layer - weight of quantum dots) / weight of light-emitting layer) x 100% in the light-emitting layer after the heat treatment step is greater than 3.3% but smaller than 35%.
[0011] In order to solve the above-mentioned problems, the method for forming a light-emitting layer of the present disclosure includes the steps of: preparing a quantum dot solution containing a plurality of quantum dots, a metal sulfide precursor, and a solvent; applying the quantum dot solution; and heat-treating the metal sulfide precursor by thermally decomposing the metal sulfide precursor to form a matrix containing the metal sulfide. In the step of preparing the quantum dot solution, the amounts of the plurality of quantum dots and the amount of the metal sulfide precursor contained in the quantum dot solution are adjusted so that the value of ((weight of light-emitting layer−weight of quantum dots) / weight of light-emitting layer)×100% in the light-emitting layer after the heat-treating step is greater than 3.3% and less than 35%.
[0012] In order to solve the above-mentioned problems, the manufacturing method of the light-emitting element of the present disclosure includes the steps of: forming one of an anode and a cathode; forming a light-emitting layer by the light-emitting layer formation method; and forming the other of the anode and the cathode.
[0013] According to one aspect of the present disclosure, it is possible to provide a light-emitting element, a display device, a method for manufacturing a light-emitting element, and a method for forming a light-emitting layer, which are capable of improving durability and luminous efficiency.
[0014] 1 is a plan view showing a schematic configuration of a display device of the present embodiment; FIG. 2 is a cross-sectional view showing a schematic configuration of a display region of the display device of the present embodiment; FIG. 3 is a cross-sectional view showing a schematic configuration of a red light-emitting element provided in the display device of the present embodiment; FIG. 4 is a cross-sectional view showing a schematic configuration of a red light-emitting layer of the red light-emitting element provided in the display device of the present embodiment; FIG. 5 is a diagram showing a red light-emitting layer of the red light-emitting element provided in the display device of the present embodiment, in which the material of the shell of the quantum dots and the continuous film containing metal sulfide contained in the red light-emitting layer are the same material; FIG. 6 is a diagram showing another red light-emitting layer that can be provided in the red light-emitting element provided in the display device of the present embodiment, in which the material of the shell of the quantum dots and the continuous film containing metal sulfide contained in the red light-emitting layer are different materials; FIG. 7 is a diagram showing an example of multiple types of quantum dot solutions containing multiple quantum dots, a metal sulfide precursor, and a solvent, which can be used in a process of forming the red light-emitting layer of the red light-emitting element provided in the display device of the present embodiment; FIG. 8 is a diagram showing the band levels of a hole transport layer, a red light-emitting layer, and an electron transport layer provided in the red light-emitting element of the display device of the present embodiment; and FIG. 9 is a diagram explaining why good external quantum efficiency (EQE) can be achieved in the red light-emitting element of the display device of the present embodiment. 8 is a diagram illustrating the band levels of a hole transport layer, a red light-emitting layer, and an electron transport layer provided in a red light-emitting device as a comparative example. It is a diagram illustrating the reason why a good external quantum efficiency (EQE) cannot be achieved in a red light-emitting device as a comparative example. It is a diagram illustrating the relationship between the voltage and the current density of an electron only device (EOD) including a red light-emitting layer formed using a quantum dot solution with a concentration of 0.02 M among the multiple types of quantum dot solutions shown in FIG. 7, and an electron only device (EOD) including a red light-emitting layer formed using a quantum dot solution with a concentration of 0.08 M. It is a diagram illustrating the relationship between the voltage and the current density of a hole only device (HOD) including a red light-emitting layer formed using a quantum dot solution with a concentration of 0.02 M among the multiple types of quantum dot solutions shown in FIG. 7, and an electron only device (EOD) including a red light-emitting layer formed using a quantum dot solution with a concentration of 0.08 M.10 is a diagram showing the degree of luminance reduction due to quantum dot charge-up when a red light-emitting device including a red light-emitting layer formed using a quantum dot solution with a concentration of 0.01 M among the multiple types of quantum dot solutions shown in FIG. 7 and a comparative red light-emitting device shown in FIG. 10 are intermittently driven.
[0033] FIG. 11 is a diagram showing PL intensity (photoluminescence intensity) at each wavelength for a red light-emitting layer formed using a quantum dot solution with a concentration of 0.01 M among the multiple types of quantum dot solutions shown in FIG. 7 and a red light-emitting layer formed using a quantum dot solution with a concentration of 0.16 M as a comparative example.
[0034] FIG. 12 is a diagram showing the relationship between the weight ratio of a continuous film containing a metal sulfide, which is a medium in multiple types of red light-emitting layers that are thin films formed using multiple types of quantum dot solutions shown in FIG. 7, and the internal quantum yield (PLQY).
[0035] FIG. 13 is a diagram showing the emission peak wavelength, internal quantum yield (PLQY), maximum external quantum efficiency (maximum EQE), and luminance reduction rate after 5 hours of operation for multiple types of red light-emitting devices including red light-emitting layers formed using multiple types of quantum dot solutions shown in FIG. 8 is a diagram showing the degree of change in luminance and voltage over the driving time of a red light-emitting element including a red light-emitting layer formed using a quantum dot solution with a concentration of 0.04 M out of the multiple types of quantum dot solutions shown in Fig. 7. It is a diagram showing the degree of change in luminance and voltage over the driving time of a red light-emitting element including a red light-emitting layer formed using a quantum dot solution with a concentration of 0.08 M out of the multiple types of quantum dot solutions shown in Fig. 7. It is a diagram for explaining the step of forming a red light-emitting layer included in the manufacturing method of the red light-emitting element provided in the display device of the present embodiment.
[0015] The following describes embodiments of the present disclosure with reference to Figures 1 to 20. For the sake of convenience, components having the same functions as those described in specific embodiments will be denoted by the same reference numerals, and descriptions thereof may be omitted.
[0016] FIG. 1 is a plan view showing a schematic configuration of a display device 1 according to the present embodiment.
[0017] As shown in Fig. 1, the display device 1 includes a frame area NDA and a display area DA. The display area DA of the display device 1 includes a plurality of pixels PIX, each of which includes a red subpixel RSP, a green subpixel GSP, and a blue subpixel BSP. In this embodiment, a case in which one pixel PIX is configured with a red subpixel RSP, a green subpixel GSP, and a blue subpixel BSP will be described as an example, but this is not limiting. For example, one pixel PIX may include subpixels of other colors in addition to the red subpixel RSP, the green subpixel GSP, and the blue subpixel BSP.
[0018] FIG. 2 is a cross-sectional view showing a schematic configuration of the display area DA of the display device 1 of this embodiment.
[0019] As shown in Figure 2, in the display area DA of the display device 1, a barrier layer 3, a thin film transistor layer 4 including a transistor TR, a red light-emitting element 5R, a green light-emitting element 5G, a blue light-emitting element 5B and a bank 23, a sealing layer 6, and a functional film 39 are provided on a substrate 12 in this order from the substrate 12 side.
[0020] The red sub-pixel RSP provided in the display area DA of the display device 1 includes a red light-emitting element 5R, the green sub-pixel GSP provided in the display area DA of the display device 1 includes a green light-emitting element 5G, and the blue sub-pixel BSP provided in the display area DA of the display device 1 includes a blue light-emitting element 5B.
[0021] The substrate 12 may be, for example, a resin substrate made of a resin material such as polyimide, or a glass substrate. In this embodiment, since the display device 1 is a flexible display device, a case where a resin substrate made of a resin material such as polyimide is used as the substrate 12 will be described as an example, but this is not limiting. If the display device 1 is a non-flexible display device, a glass substrate can be used as the substrate 12.
[0022] The barrier layer 3 is a layer that prevents foreign substances such as water and oxygen from penetrating into the transistor TR, the red light-emitting element 5R, the green light-emitting element 5G, and the blue light-emitting element 5B, and can be composed of, for example, a silicon oxide film, a silicon nitride film, a silicon oxynitride film, or a laminated film of these, formed by the CVD method.
[0023] The transistor TR portion of the thin film transistor layer 4 including the transistor TR includes the semiconductor film SEM and doped semiconductor films SEM′ and SEM″, an inorganic insulating film 16, a gate electrode G, an inorganic insulating film 18, an inorganic insulating film 20, a source electrode S and a drain electrode D, and a planarization film 21, and the portion of the thin film transistor layer 4 including the transistor TR other than the transistor TR portion includes the inorganic insulating film 16, the inorganic insulating film 18, the inorganic insulating film 20, and the planarization film 21.
[0024] The semiconductor films SEM, SEM', and SEM'' may be made of, for example, low-temperature polysilicon (LTPS) or an oxide semiconductor (for example, an In-Ga-Zn-O based semiconductor). In this embodiment, the case where the transistor TR has a top-gate structure will be described as an example, but the present invention is not limited to this, and the transistor TR may also have a bottom-gate structure.
[0025] The gate electrode G and the source electrode S and drain electrode D can be formed of a single layer or a multilayer film of a metal containing at least one of aluminum, tungsten, molybdenum, tantalum, chromium, titanium, and copper, for example.
[0026] The inorganic insulating films 16, 18 and 20 can be formed of, for example, a silicon oxide film, a silicon nitride film, a silicon oxynitride film, or a laminated film of these films, which are formed by the CVD method.
[0027] The planarizing film 21 can be made of a coatable organic material such as polyimide or acrylic, but may also be made of an inorganic film.
[0028] The red light-emitting element 5R included in the red subpixel RSP includes an anode 22 above the planarization film 21, a functional layer 24R including a red light-emitting layer, and a cathode 25. The green light-emitting element 5G included in the green subpixel GSP includes an anode 22 above the planarization film 21, a functional layer 24G including a green light-emitting layer, and a cathode 25. The blue light-emitting element 5B included in the blue subpixel BSP includes an anode 22 above the planarization film 21, a functional layer 24B including a blue light-emitting layer, and a cathode 25. The insulating bank 23 covering the edge of the anode 22 can be formed by applying an organic material such as polyimide or acrylic and then patterning it by photolithography, but it may also be formed from an inorganic film.
[0029] In this embodiment, the red light-emitting element 5R, the green light-emitting element 5G, and the blue light-emitting element 5B have a forward stack structure as an example, but this is not limited thereto, and the red light-emitting element 5R, the green light-emitting element 5G, and the blue light-emitting element 5B may have an inverted stack structure. The red light-emitting element 5R having a forward stack structure includes an anode 22 and a cathode 25 provided as an upper layer above the anode 22. The functional layer 24R including a red light-emitting layer provided between the anode 22 and the cathode 25 can be configured, for example, by stacking, in order from the anode 22 side, a hole injection layer, a hole transport layer, a red light-emitting layer, an electron transport layer, and an electron injection layer. Of the functional layer 24R including a red light-emitting layer, one or more of the hole injection layer, hole transport layer, electron transport layer, and electron injection layer other than the red light-emitting layer may be omitted as appropriate. In this embodiment, an example will be described in which the functional layer 24R including the red light-emitting layer 24REM is configured by stacking a hole transport layer 24HT, a red light-emitting layer 24REM, and an electron transport layer 24ET in this order from the anode 22 side, but the present invention is not limited to this.
[0030] A red light-emitting element having an inverted stack structure (not shown) includes a cathode and an anode above the cathode. The functional layer including the red light-emitting layer 24REM between the cathode and the anode can be configured by stacking, for example, an electron injection layer, an electron transport layer, the red light-emitting layer 24REM, a hole transport layer, and a hole injection layer, in this order from the cathode side. Among the functional layers including the red light-emitting layer 24REM, one or more of the electron injection layer, electron transport layer, hole transport layer, and hole injection layer other than the red light-emitting layer 24REM may be omitted as appropriate. While the above description has been about red light-emitting elements, green light-emitting elements, blue light-emitting elements, and the like can be similarly described and understood. That is, by replacing the "red" part of the description with "green" or "blue" and also replacing the "R" part of the symbol with "G" or "B," the description can be similarly described and understood.
[0031] The material used for the hole injection layer is not particularly limited as long as it is a hole injection material that can stabilize the injection of holes into the light emitting layer, and for example, a composite of poly(3,4-ethylenedioxythiophene) (PEDOT) and polystyrene sulfonic acid (PSS) (PEDOT:PSS) can be used.
[0032] Examples of materials used for the hole transport layer include organic materials such as poly[(9,9-dioctylfluorenyl-2,7-diyl)-co-(4,4'-(N-(4-sec-butylphenyl))diphenylamine)] (TFB), N,N'-bis(4-butylphenyl)-N,N'-bis(phenyl)-benzidine (poly-TPD), and polyvinylcarbazole (PVK), and nanoparticles having hole transport properties such as NiO particles. In this embodiment, the hole transport layer 24HT will be described using N,N'-bis(4-butylphenyl)-N,N'-bis(phenyl)-benzidine (poly-TPD) as an example, but the present invention is not limited thereto.
[0033] The material used for the electron transport layer may be, for example, an organic material such as 2,2′,2″-(1,3,5-benzinetriyl)-tris(1-phenyl-1-H-benzimidazole) (TPBi), or nanoparticles having electron transport properties such as ZnO particles. In this embodiment, the electron transport layer 24ET is made of particles of an oxide containing Zn and Mg, for example, Zn 0.9 Mg 0.1 Although the case where O particles are used will be described as an example, the present invention is not limited to this.
[0034] The material used for the electron injection layer is not particularly limited as long as it is an electron injection material that can stabilize the injection of electrons into the light-emitting layer. For example, alkali metals or alkaline earth metals such as aluminum, strontium, calcium, lithium, cesium, magnesium oxide, aluminum oxide, strontium oxide, lithium oxide, lithium fluoride, magnesium fluoride, strontium fluoride, calcium fluoride, barium fluoride, cesium fluoride, polymethyl methacrylate polystyrene sodium sulfonate, oxides of alkali metals or alkaline earth metals, fluorides of alkali metals or alkaline earth metals, organic complexes of alkali metals, etc. may be used.
[0035] In addition, in this embodiment, the functional layer 24R including the red light-emitting layer, the functional layer 24G including the green light-emitting layer, and the functional layer 24B including the blue light-emitting layer each include a hole transport layer formed in the same process using the same material and an electron transport layer formed in the same process using the same material, but this is not limited to this. For example, the hole injection layers included in each of the functional layers 24R, 24G, and 24B may be formed in the same process using the same material, or may be formed in different materials. Alternatively, the hole injection layers included in two of the functional layers 24R, 24G, and 24B may be formed in the same process using the same material, and only the hole injection layer included in the remaining functional layer may be formed in a separate process using a different material. Alternatively, the hole transport layers included in two of the functional layers 24R, 24G, and 24B may be formed using the same material in the same process, and the hole transport layer included in the remaining functional layer may be formed using a different material in a separate process. Similarly to the hole transport layers, the electron transport layers may be formed using the same material and the same process in any desired combination for the functional layers 24R, 24G, and 24B.
[0036] In this embodiment, an example will be described in which the red light-emitting element 5R, the green light-emitting element 5G, and the blue light-emitting element 5B are all QLEDs (quantum dot light-emitting diodes), but this is not limited to this, and it is sufficient that one or more of the red light-emitting element 5R, the green light-emitting element 5G, and the blue light-emitting element 5B are QLEDs, and the rest may be OLEDs.
[0037] In the present embodiment, when the red light-emitting element 5R, the green light-emitting element 5G, and the blue light-emitting element 5B are each a QLED, the light-emitting layer of each light-emitting element contains quantum dots. The quantum dots may have, for example, a core structure, a core / shell structure, a core / shell / shell structure, or a shell structure with a continuously varying core / shell ratio. The shell may partially cover the core, but it is more preferable for the shell to completely cover the core. Examples of the core material of the quantum dot include II-VI group semiconductor crystals such as MgS, MgSe, MgTe, CaS, CaSe, CaTe, BaS, BaSe, BaTe, ZnS, ZnSe, ZnTe, CdS, CdSe, CdTe, PbS, PbSe, HgS, HgSe, and HgTe; III-V group semiconductor crystals such as GaAs, GaP, InN, InAs, InP, and InSb; Ga 3 S 2 , Ga 2 Se 3 , In 2 S 3 , In 2 Se 3 Crystals of III-VI group semiconductors such as CuInGaS, AgInGaS, CuInGaS, AgInGaZnS, CuInGaSe, AgInGaSe, etc., crystals of I-III-VI group semiconductors such as C and Si, crystals of IV group semiconductors such as CsPbI 3 , CsPbBr 3 , CsPbCl 3 The shell material can be made of a semiconductor crystal with a perovskite structure such as the above. The shell material is selected from the same material group as the core material, and is preferably one that has a lattice constant close to that of the core material and a larger band gap than the core material.
[0038] When the quantum dots described above include organic or inorganic ligands (e.g., halogen ligands) disposed on or near the surface of the quantum dots, the quantum dots refer to those that include organic or inorganic ligands. Thus, when the quantum dots include a ligand such as an organic or inorganic ligand, each of the red, green, and blue light-emitting layers 24REM also includes a ligand.
[0039] The quantum dots have a maximum width excluding the ligand portion of 100 nm or less. The shape of the quantum dots excluding the ligand portion is not particularly limited as long as it satisfies the maximum width, and is not limited to a spherical three-dimensional shape (circular cross-sectional shape). For example, the quantum dots may have a polygonal cross-sectional shape, a rod-like three-dimensional shape, a branch-like three-dimensional shape, a three-dimensional shape with an uneven surface, or a combination thereof.
[0040] 2 may be of either a top-emission type or a bottom-emission type. The red light-emitting element 5R, green light-emitting element 5G, and blue light-emitting element 5B have a forward-laid structure in which the cathode 25 is disposed above the anode 22. To form the red light-emitting element 5R, green light-emitting element 5G, and blue light-emitting element 5B as a top-emission type, the anode 22 may be formed of an electrode material that reflects visible light, and the cathode 25 may be formed of an electrode material that transmits visible light. To form the bottom-emission type, the anode 22 may be formed of an electrode material that transmits visible light, and the cathode 25 may be formed of an electrode material that reflects visible light. On the other hand, when the red light-emitting element, the green light-emitting element, and the blue light-emitting element have an inverted stack structure in which the anode 22 is disposed as an upper layer than the cathode 25, in order to form a top emission type, the cathode 25 may be formed from an electrode material that reflects visible light, and the anode 22 may be formed from an electrode material that transmits visible light, and in order to form a bottom emission type, the cathode 25 may be formed from an electrode material that transmits visible light, and the anode 22 may be formed from an electrode material that reflects visible light.
[0041] The electrode material that reflects visible light is not particularly limited as long as it can reflect visible light and has electrical conductivity. Examples of the electrode material that reflects visible light include metal materials such as Al, Mg, Li, and Ag, alloys of the metal materials, laminates of the metal materials and transparent metal oxides (e.g., indium tin oxide, indium zinc oxide, indium gallium zinc oxide, etc.), and laminates of the alloys and the transparent metal oxides.
[0042] On the other hand, the electrode material that transmits visible light is not particularly limited as long as it can transmit visible light and has conductivity, and examples thereof include transparent metal oxides (e.g., indium tin oxide, indium zinc oxide, indium gallium zinc oxide, etc.), thin films made of metal materials such as Al and Ag, and nanowires made of metal materials such as Al and Ag.
[0043] The anode 22 and the cathode 25 can be formed by a general electrode formation method, for example, a physical vapor deposition (PVD) method such as vacuum deposition, sputtering, EB deposition, or ion plating, or a chemical vapor deposition (CVD) method. The method for patterning the anode 22 and the cathode 25 is not particularly limited as long as it can form the desired pattern with high precision, and specific examples include photolithography and inkjet printing.
[0044] The sealing layer 6 is a light-transmitting film, and can be composed of, for example, an inorganic sealing film 26 that covers the cathode 25, an organic film 27 that is above the inorganic sealing film 26, and an inorganic sealing film 28 that is above the organic film 27. The sealing layer 6 prevents foreign substances such as water and oxygen from penetrating into the red light-emitting element 5R, the green light-emitting element 5G, and the blue light-emitting element 5B.
[0045] The inorganic sealing films 26 and 28 are each an inorganic film, and may be formed, for example, by a CVD method using a silicon oxide film, a silicon nitride film, a silicon oxynitride film, or a laminated film thereof. The organic film 27 is a light-transmitting organic film with a planarizing effect, and may be formed, for example, using a coatable organic material such as acrylic. The organic film 27 may also be formed, for example, by an inkjet method. In this embodiment, the sealing layer 6 is formed of two inorganic films and one organic film disposed between the two inorganic films. However, the stacking order of the two inorganic films and one organic film is not limited to this. Furthermore, the sealing layer 6 may be formed solely of an inorganic film, solely of an organic film, one inorganic film and two organic films, or two or more inorganic films and two or more organic films.
[0046] The functional film 39 is a film having at least one of an optical compensation function, a touch sensor function, and a protection function, for example.
[0047] FIG. 3 is a cross-sectional view showing a schematic configuration of a red light emitting element 5R provided in the display device 1 of this embodiment.
[0048] As shown in FIG. 3, the red light emitting element 5R includes an anode 22, a cathode 25, and a red light emitting layer 24REM provided between the anode 22 and the cathode 25.
[0049] In this embodiment, the functional layer 24B including the red light-emitting layer 24REM provided in the red light-emitting element 5R is configured by stacking a hole transport layer 24HT, a red light-emitting layer 24REM, and an electron transport layer 24ET in this order from the anode 22 side.
[0050] 3, the red light-emitting layer 24REM includes a continuous film MR containing a metal sulfide and a plurality of quantum dots QDs encapsulated in the continuous film MR. In this embodiment, the case where all of the quantum dots QDs in the red light-emitting layer 24REM are encapsulated in the continuous film MR will be described as an example, but the present invention is not limited to this as long as the red light-emitting layer 24REM includes a plurality of quantum dots QDs encapsulated in the continuous film MR. The continuous film MR may be a matrix.
[0051] The continuous film MR is a continuous matrix. A matrix refers to a material that contains and holds other substances, and can be referred to as a substrate, a base material, or a filler. The continuous matrix may be a material that contains and holds multiple quantum dots QDs. The matrix may be filled in the light-emitting layer. The matrix may fill the region (space) between two adjacent quantum dots QDs. The matrix may also fill regions (spaces) in the light-emitting layer other than the multiple quantum dots QDs. "The matrix being filled between multiple quantum dots QDs" means that the region between two adjacent quantum dots QDs is filled with the matrix, and it is sufficient to know this. Since the desired effect is achieved as long as the matrix is filled in at least the region between two adjacent quantum dots QDs, it is not necessarily necessary to know that the matrix is filled between all (more than two) quantum dots QDs within a certain range. The outer edges (top and bottom) of the light-emitting layer may be covered with the matrix. Furthermore, the light-emitting layer may be configured such that a matrix portion extends from the outer edge thereof, and the quantum dot group is positioned away from the outer edge. The outer edge of the light-emitting layer may not be formed solely of the matrix, and a portion of the quantum dot group may be exposed from the matrix. The matrix may refer to the portion of the light-emitting layer excluding the quantum dot group. If the light-emitting layer includes a plurality of quantum dots QDs encapsulated in a matrix, the matrix may be formed so as to partially or completely fill the space formed between two adjacent quantum dots QDs. The light-emitting layer may have voids. If the light-emitting layer includes a plurality of quantum dots QDs encapsulated in a matrix, the light-emitting layer may have a plurality of quantum dots QDs, and the matrix may partially or completely fill the area other than the plurality of quantum dots QDs. Each of two adjacent quantum dots QDs included in the plurality of quantum dots QDs may be embedded in the matrix at an interval.
[0052] The continuous matrix, i.e., the continuous film MR, has an area of 1000 nm in the light-emitting layer. 2The matrix may be continuous within the above area range. A continuous film MR, i.e., a continuous matrix, refers to a film that is not separated in one plane by materials other than the material constituting the continuous film MR, i.e., the continuous matrix. In other words, it is sufficient that the film is partially connected, and this does not exclude cases where quantum dots or other materials are included in between. "Separated" refers to a film that is separated by a completely separate layer without any connected portions. The continuous film MR, i.e., the continuous matrix, may be an integrated film connected seamlessly by chemical bonds between the constituent materials. The continuous matrix may be made of the same material as the shells of the quantum dots (QDs). In this case, the average distance between adjacent cores of two adjacent quantum dots (QDs) may be 3 nm or more, or may be 5 nm or more. The core-to-core distance is the average distance between 20 adjacent cores in a space containing 20 cores. The core-to-core distance should be wider than the distance between shells when they are in contact with each other. Note that when observing the cross-section of a particle, the cross-sectional area varies depending on the cutting position of the particle. Therefore, the diameter of a circle having the same area as the average cross-sectional area of the top 10% of particles with the largest cross-sectional areas can be considered as the core diameter.
[0053] FIG. 4 is a cross-sectional view showing a schematic configuration of a red light-emitting layer 24REM of a red light-emitting element 5R provided in the display device 1 of this embodiment.
[0054] As shown in FIG. 4, in a cross section of a portion of the red light-emitting layer 24REM that includes cross sections of a predetermined number of quantum dots QDs among the multiple quantum dots QDs contained in the red light-emitting layer 24REM, the area C of the cross section of the portion of the red light-emitting layer 24REM is smaller than twice the area B, which is the sum of the areas of the cross sections of the predetermined number of quantum dots QDs.
[0055] In this embodiment, as shown in FIG. 4 , in a cross section of a portion of the red light-emitting layer 24REM including, for example, 52 quantum dots QDs among the multiple quantum dots QDs included in the red light-emitting layer 24REM, when comparing the area A (hatched area in FIG. 4 ) of the cross section of the continuous film MR containing metal sulfide with the area B obtained by combining the cross sections of the 52 quantum dots QDs, area A is smaller than area B. Furthermore, if the cross section of the portion of the red light-emitting layer 24REM including the cross sections of the 52 quantum dots QDs is area C, that is, if the cross section of the portion of the entire light-emitting layer including the cross sections of the quantum dots QDs and the matrix is area C, area C is smaller than twice the area B obtained by combining the cross sections of the 52 quantum dots QDs. Here, the cross section of a portion of the red light-emitting layer 24REM including 52 quantum dots QDs has been described as an example, but the present invention is not limited thereto. It is sufficient that the number of quantum dots QDs is 50 or more, and may be 50 or 100. 4, the cross-sectional size of the 52 quantum dots QD varies depending on the cutting position even if the quantum dots QD have the same particle diameter. Furthermore, for example, when the cross section of the red light-emitting layer 24REM is observed with a transmission electron microscopy (TEM), if voids of a discernible size are included, the cross-sectional area of the voids is not included in the area A of the cross section of the continuous film MR containing metal sulfide.
[0056] In this embodiment, the red light-emitting layer 24REM will be described as an example in which the cross-sectional area A of the continuous film MR containing metal sulfide is smaller than the area B obtained by combining the cross-sectional areas of a predetermined number, for example, 50 or more quantum dots QDs, at any cross-section obtained by cutting any part of the red light-emitting layer 24REM. However, the present invention is not limited to this, and the red light-emitting layer 24REM may include a cross-section including cross-sections of the predetermined number, for example, 50 or more quantum dots QDs, obtained by cutting a certain part of the red light-emitting layer 24REM, where the cross-sectional area A of the continuous film MR containing metal sulfide is smaller than the area B obtained by combining the cross-sectional areas of the predetermined number, for example, 50 or more quantum dots QDs. The fact that the red light-emitting layer 24REM has a cross section in part where "the cross-sectional area A of the continuous film MR containing metal sulfide is smaller than the combined area B of the cross-sectional areas of a predetermined number, for example, 50 or more quantum dots QDs" means that the red light-emitting layer 24REM includes a portion where "the cross-sectional area A of the continuous film MR containing metal sulfide is smaller than the combined area B of the cross-sectional areas of a predetermined number, for example, 50 or more quantum dots QDs." The inventors of the present disclosure have confirmed that if the red light-emitting layer 24REM includes a cross section including a predetermined number, for example, 50 or more quantum dots QDs, "where the cross-sectional area A of the continuous film MR containing metal sulfide is smaller than the combined area B of the cross-sectional areas of the predetermined number, for example, 50 or more quantum dots QDs," then the carrier balance and external quantum efficiency (EQE) can be improved and a decrease in brightness due to charge-up of the quantum dots can be suppressed. Therefore, the red light-emitting layer 24REM may include, for example, a cross-section including a predetermined number of quantum dots QDs, for example, 50 quantum dots QDs, where "the cross-sectional area A of the continuous film MR containing metal sulfide is smaller than the area B obtained by combining the cross-sectional areas of the predetermined number of quantum dots QDs, for example, 50 quantum dots QDs," or may include a cross-section including 100 quantum dots QDs, where "the cross-sectional area A of the continuous film MR containing metal sulfide is smaller than the area B obtained by combining the cross-sectional areas of the 100 quantum dots QDs."The area of the cross section of the portion of the red light-emitting layer 24REM including the cross sections of 52 quantum dots QDs may be determined by, for example, observing the cross section of the portion of the red light-emitting layer 24REM including the cross sections of 52 quantum dots QDs shown in FIG. 4 with a transmission electron microscope (TEM), and excluding voids that can be identified with the transmission electron microscope (TEM) from the value of the width in the horizontal direction of the cross section of the portion of the red light-emitting layer 24REM shown in FIG. 4 multiplied by the height in the vertical direction of the cross section of the portion of the red light-emitting layer 24REM shown in FIG. 4.
[0057] In a cross section of a portion of the red light-emitting layer 24REM including cross sections of 50 or more quantum dots QDs among the multiple quantum dots QDs included in the red light-emitting layer 24REM, the area A of the cross section of the continuous film MR including metal sulfide, i.e., the area A calculated by subtracting the area C from the area B, is preferably 3.4% or more and 27.0% or less of the area B obtained by adding up the areas of the cross sections of the predetermined number, for example, 50 or more quantum dots QDs.
[0058] A cross section of a portion of the red light-emitting layer 24REM including cross sections of a predetermined number of quantum dots QDs shown in FIG. 4 , for example, 50 or more quantum dots QDs, may be observed with a transmission electron microscope (TEM). In this case, the image of the transmission electron microscope (TEM) may include a first region having a higher electron density through which the irradiated electron beam has passed, and a second region having a lower electron density. The area of the first region may be defined as area A of the cross section of the continuous film MR including the metal sulfide, which is calculated by subtracting area B from area C. The area of the second region may be defined as area B, which is the sum of the areas of the cross sections of the 52 quantum dots QDs.
[0059] For example, by adjusting the display settings of a transmission electron microscope (TEM) image, it is possible to make it so that in areas containing heavier elements, the irradiated electron beam has less penetration, the electron density is lower, and the area is displayed in a lighter color, while in areas containing lighter elements, the irradiated electron beam has more penetration, the electron density is higher, and the area is displayed in a darker color.
[0060] The quantum dots QD, such as ZnSe, InP, and CdS, contain Se, In, and Cd, which are heavier elements than Zn, and are therefore displayed in a lighter color. The area B, which is the area of the second region with a lower electron density, may be determined from the area of the region displayed in a lighter color in a transmission electron microscope (TEM) image. On the other hand, the continuous film MR containing a metal sulfide (e.g., ZnS) contains Zn, which is a lighter element than Se, and is therefore displayed in a darker color. The area A, which is the area of the first region with a higher electron density, may be determined from the area of the region displayed in a darker color in a transmission electron microscope (TEM) image.
[0061] Furthermore, after determining the composition of the continuous film MR containing quantum dots QDs and metal sulfides contained in the red light-emitting layer 24REM by elemental analysis of the red light-emitting layer 24REM, X-ray diffraction may be performed on a cross section of a portion of the red light-emitting layer 24REM containing cross sections of a predetermined number of quantum dots QDs, for example, 50 or more, as shown in FIG. 4 . A cross section of a portion of the red light-emitting layer 24REM including cross sections of 50 or more quantum dots QDs includes a first region having a diffraction peak specific to the X-ray diffraction of the metal sulfide and a second region having a diffraction peak specific to the X-ray diffraction of the quantum dots QDs, and the area of the first region in the cross section of the portion of the red light-emitting layer 24REM obtained based on the diffraction peak specific to the X-ray diffraction of the metal sulfide may be taken as area A of the cross section of the continuous film MR including the metal sulfide obtained from area C minus area B, and the area of the second region in the cross section of the portion of the red light-emitting layer 24REM obtained based on the diffraction peak specific to the X-ray diffraction of the quantum dots QDs may be taken as area B, which is the sum of the areas of the cross sections of the 50 or more quantum dots QDs.
[0062] In addition, in a cross section of a portion of the red light-emitting layer 24REM including 50 or more quantum dots QDs as shown in Fig. 4, the number-average inter-quantum dot distance of the 50 or more quantum dots QDs is preferably 1 nm or more and 5 nm or less. Note that the number-average inter-quantum dot distance is a value that can be calculated by calculating N distances (N is a natural number of 2 or more) between quantum dots QDs that have the shortest inter-quantum dot distances among adjacent quantum dots QDs in a cross section of a portion of the red light-emitting layer 24REM including 50 or more quantum dots QDs as shown in Fig. 4, and calculating (the sum of the N shortest distances / N).
[0063] Figure 5 is a diagram showing the red light-emitting layer 24REM of the red light-emitting element 5R provided in the display device 1 of this embodiment, in which the material of the shell SH of the quantum dot QD contained in the red light-emitting layer 24REM and the continuous film MR containing metal sulfide are made of the same material.
[0064] As shown in FIG. 5 , in this embodiment, the quantum dots QDs included in the red light-emitting layer 24REM include a core CO and a shell SH, and the shell SH of the quantum dots QDs is composed of a metal sulfide. The metal sulfide included in the continuous film MR and the metal sulfide constituting the shell SH of the quantum dots QDs are both ZnS. This example is not limited to this example. The metal sulfide included in the continuous film MR and the metal sulfide constituting the shell SH of the quantum dots QDs may be different metal sulfides. The metal sulfide may contain one or more metal elements selected from Zn, Mg, and Ga, and may be any of zinc sulfide (e.g., ZnS), zinc magnesium sulfide (e.g., ZnMgS), gallium sulfide (e.g., GaS), zinc selenide sulfide (e.g., ZnSeS), zinc telluride sulfide (e.g., ZnTeS), magnesium sulfide (e.g., MgS), and zinc gallium sulfide (e.g., ZnGaS). The band gap of the continuous film MR containing metal sulfide as the matrix is larger than the band gap of the core CO of the quantum dot QD.
[0065] In the present embodiment shown in FIG. 5, when the shell SH of the quantum dot QD is composed of a metal sulfide, for example, when the metal sulfide contained in the continuous film MR and the metal sulfide constituting the shell SH of the quantum dot QD are both ZnS, the shell SH of the quantum dot QD composed of a metal sulfide is formed continuously with the continuous film MR, and can therefore be regarded as the continuous film MR.
[0066] Figure 6 is a diagram showing another red light-emitting layer 24REM' that can be provided in the red light-emitting element 5R provided in the display device 1 of this embodiment, in which the material of the shell SH' of the quantum dot QD' contained in the red light-emitting layer 24REM' and the continuous film MR containing metal sulfide are different materials.
[0067] As shown in Figure 6, the quantum dots QD' contained in the red light-emitting layer 24REM' include a core CO and a shell SH', and the shell SH' of the quantum dots QD' is composed of a material other than metal sulfide, and the band gap of the continuous film MR containing metal sulfide, which is the matrix, is larger than the band gap of the core CO of the quantum dots QD'.
[0068] As shown in FIG. 6, when the shell SH' of the quantum dot QD' is composed of a material other than metal sulfide, the shell SH' of the quantum dot QD' does not contain metal sulfide, and therefore the quantum dot QD is a quantum dot QD.
[0069] Figure 7 is a diagram showing an example of multiple types of quantum dot solutions containing multiple quantum dots QDs, a metal sulfide precursor, and a solvent, which can be used in the process of forming the red light-emitting layer 24REM of the red light-emitting element 5R provided in the display device 1 of this embodiment.
[0070] 7, in this embodiment, zinc ethylxanthogenate, which decomposes after heat treatment to form ZnS, is used as the metal sulfide precursor. However, the present invention is not limited to this example. As the metal sulfide precursor, a metal complex in which one or more selected from thiourea, N-methylthiourea, 1,3-dimethylthiourea, N,N'-dimethylthiourea, tetramethylthiourea, thioacetamide, and xanthogenic acid are coordinated to a metal atom may also be used. Furthermore, the metal sulfide precursor may comprise a metal source and a sulfur source, wherein the metal source is one or more selected from metal acetates, metal nitrates, and metal halides, and the sulfur source may be one or more selected from thiourea, N-methylthiourea, 1,3-dimethylthiourea, N,N'-dimethylthiourea, tetramethylthiourea, and thioacetamide.
[0071] In this embodiment, a case where a quantum dot QD having a core made of InP, a shell made of ZnS, and containing a halogen ligand as a ligand is used will be described as an example, but the present invention is not limited to this.
[0072] In this embodiment, the case where N,N-dimethylformamide is used as the solvent will be described as an example, but the solvent is not limited to this, and for example, dimethyl sulfoxide or the like may also be used.
[0073] 7 shows a quantum dot solution with a concentration [M] of 0.08, which is a mixture of quantum dots QDs, zinc ethylxanthate, and N,N-dimethylformamide, so that the quantum dots QDs have a concentration of 15 mg / ml and the zinc ethylxanthate (a precursor of metal sulfide) has a concentration of 24.64 mg / ml. The weight ratio of the quantum dots QDs in the red light-emitting layer 24REM formed using the quantum dot solution with a concentration [M] of 0.08 is 64.6%, and the weight ratio of the continuous film MR (medium) is 35.4%.
[0074] 7 shows a quantum dot solution with a concentration [M] of 0.04, which is a mixture of quantum dots QDs, zinc ethylxanthate, and N,N-dimethylformamide, so that the quantum dots QDs have a concentration of 15 mg / ml and the zinc ethylxanthate (a precursor of metal sulfide) has a concentration of 12.32 mg / ml. The weight ratio of the quantum dots QDs in the red light-emitting layer 24REM formed using the quantum dot solution with a concentration [M] of 0.04 is 78.5%, and the weight ratio of the continuous film MR (medium) is 21.5%.
[0075] 7 shows a quantum dot solution with a concentration [M] of 0.02, which is a mixture of quantum dots QDs, zinc ethylxanthate, and N,N-dimethylformamide, so that the quantum dots QDs have a concentration of 15 mg / ml and the zinc ethylxanthate (a precursor of metal sulfide) has a concentration of 6.16 mg / ml. The weight ratio of the quantum dots QDs in the red light-emitting layer 24REM formed using the quantum dot solution with a concentration [M] of 0.02 is 88.0%, and the weight ratio of the continuous film MR (medium) is 12.0%.
[0076] 7 shows a quantum dot solution with a concentration [M] of 0.01, which is a mixture of quantum dots QDs, zinc ethylxanthate, and N,N-dimethylformamide, so that the quantum dots QDs have a concentration of 15 mg / ml and the zinc ethylxanthate (a precursor of metal sulfide) has a concentration of 3.08 mg / ml. The weight ratio of the quantum dots QDs in the red light-emitting layer 24REM formed using the quantum dot solution with a concentration [M] of 0.01 is 93.6%, and the weight ratio of the continuous film MR (medium) is 6.4%.
[0077] 7 shows a quantum dot solution with a concentration [M] of 0.005, which is a mixture of quantum dots QDs, zinc ethylxanthate, and N,N-dimethylformamide, so that the quantum dots QDs have a concentration of 15 mg / ml and the zinc ethylxanthate (a precursor of metal sulfide) has a concentration of 1.54 mg / ml. The weight ratio of the quantum dots QDs in the red light-emitting layer 24REM formed using the quantum dot solution with a concentration [M] of 0.005 is 96.7%, and the weight ratio of the continuous film MR (medium) is 3.3%.
[0078] Regardless of whether the red light-emitting layer 24REM is formed using a quantum dot solution having a concentration [M] of 0.08, 0.04, 0.02, 0.01, or 0.005 as shown in FIG. 7 described above, in a cross section of a portion of the red light-emitting layer 24REM that includes cross sections of 50 or more quantum dots QDs among the multiple quantum dots QDs contained in the red light-emitting layer 24REM, the cross-sectional area A of the continuous film MR containing metal sulfide is smaller than the combined area B of the cross-sectional areas of the 50 or more quantum dots QDs.
[0079] FIG. 8 is a diagram schematically showing the band levels of the hole transport layer 24HT, the red light emitting layer 24REM, and the electron transport layer 24ET provided in the red light emitting element 5R of the display device 1 of this embodiment.
[0080] In a cross section of a portion of the red light-emitting layer 24REM including cross sections of 50 or more quantum dots QDs among the multiple quantum dots QDs contained in the red light-emitting layer 24REM provided in the red light-emitting element 5R, the cross-sectional area A of the continuous film MR including metal sulfide is smaller than the combined area B of the cross-sectional areas of the 50 or more quantum dots QDs.
[0081] With this configuration, as shown in FIG. 8 , holes H are injected from the level (−5.3 eV) at the upper end of the valence band of the hole transport layer 24HT to the level (−5.6 eV) at the upper end of the valence band of the core CO of the quantum dot QD and the level (−6.8 eV) at the upper end of the valence band of the shell SH of the quantum dot QD, and electrons E are injected from the level (−3.5 eV) at the lower end of the conduction band of the electron transport layer 24ET to the level (−3.6 eV) at the lower end of the conduction band of the core CO of the quantum dot QD and the level (−3.1 eV to −3.3 eV) at the lower end of the conduction band of the shell SH of the quantum dot QD, thereby ensuring a good carrier balance between holes H and electrons E.
[0082] FIG. 9 is a diagram illustrating the reason why the red light emitting element 5R of the display device 1 of this embodiment can achieve a good external quantum efficiency (EQE).
[0083] In the case of the red light-emitting element 5R, as described above, a good carrier balance between the holes H and the electrons E can be ensured, and therefore, as shown in Fig. 9, the holes H and the electrons E recombine at the center of the red light-emitting layer 24REM and emit light as excitons, thereby achieving a good external quantum efficiency (EQE). The red light-emitting element 5R can improve durability and luminous efficiency.
[0084] FIG. 10 is a diagram schematically showing the band levels of the hole transport layer 24HT, the red light-emitting layer 74REM, and the electron transport layer 24ET provided in the red light-emitting element 50R as a comparative example.
[0085] The red light-emitting layer 74REM provided in the comparative red light-emitting element 50R is, for example, a layer formed using a quantum dot solution having a concentration [M] of 0.3. The quantum dot solution having a concentration [M] of 0.3 is a solution obtained by mixing quantum dots QDs, zinc ethylxanthate, and N,N-dimethylformamide so that the quantum dot QD concentration is 15 mg / ml and the concentration of zinc ethylxanthate, a precursor of metal sulfide, is 92.4 mg / ml. In the red light-emitting layer 74REM formed using the quantum dot solution having a concentration [M] of 0.3, the weight ratio of the quantum dots QDs is 32.7%, and the weight ratio of the continuous film MR (medium) is 67.3%. Note that the concentration of zinc ethylxanthate, a precursor of metal sulfide, becomes 30.8 mg / ml due to decomposition after heat treatment.
[0086] In a cross section of a portion of the red light-emitting layer 74REM that includes cross sections of 50 or more quantum dots QDs out of the multiple quantum dots QDs contained in the red light-emitting layer 74REM, the cross-sectional area A of the continuous film MR containing metal sulfide is larger than the combined area B of the cross-sectional areas of the 50 or more quantum dots QDs.
[0087] In a cross section of a portion of the red light-emitting layer 74REM including cross sections of 50 or more quantum dots QDs among the multiple quantum dots QDs contained in the red light-emitting layer 74REM provided in the comparative example red light-emitting element 50R, the cross-sectional area A of the continuous film MR including metal sulfide is larger than the combined area B of the cross-sectional areas of the 50 or more quantum dots QDs.
[0088] With this configuration, as shown in FIG. 10 , holes H are mainly injected from the level (−5.3 eV) at the top of the valence band of the hole transport layer 24HT to the level (−6.8 eV) at the top of the valence band of the shell SH of the quantum dot QD, which has a relatively large level difference of 1.5 eV, and are less likely to be injected into the level (−5.6 eV) at the top of the valence band of the core CO of the quantum dot QD, which has a relatively small level difference of 0.3 eV, due to the influence of the continuous film MR containing metal sulfide, which occupies a large portion of the red light-emitting layer 74REM. On the other hand, the electrons E are injected from the level (−3.5 eV) of the lower end of the conduction band of the electron transport layer 24ET to the level (−3.6 eV) of the lower end of the conduction band of the core CO of the quantum dot QD and to the level (−3.1 eV to −3.3 eV) of the lower end of the conduction band of the shell SH of the quantum dot QD. As a result, the red light-emitting layer 74REM is in an excess state of electrons E, and the carrier balance between the holes H and the electrons E is disrupted.
[0089] FIG. 11 is a diagram illustrating the reason why the red light emitting element 50R, which is a comparative example, cannot achieve a good external quantum efficiency (EQE).
[0090] As shown in FIG. 11 , in the red light-emitting layer 74REM, which is in an excess state of electrons E, two electrons E and one hole H form a trion state, and after passing through this trion state, light is not emitted but is thermally deactivated, making it impossible to achieve a good external quantum efficiency (EQE).
[0091] FIG. 12 is a graph showing the relationship between voltage and current density for an electron only device (EOD) including a red light-emitting layer 24REM formed using a quantum dot solution with a concentration of 0.02 M out of the multiple types of quantum dot solutions shown in FIG. 7 , and an electron only device (EOD) including a red light-emitting layer 24REM formed using a quantum dot solution with a concentration of 0.08 M.
[0092] FIG. 13 is a graph showing the relationship between voltage and current density for a Hole Only Device (HOD) including a red light-emitting layer 24REM formed using a quantum dot solution with a concentration of 0.02 M out of the multiple types of quantum dot solutions shown in FIG. 7 , and a Hole Only Device (HOD) including a red light-emitting layer 24REM formed using a quantum dot solution with a concentration of 0.08 M.
[0093] FIG. 17 is a graph showing the emission peak wavelength, internal quantum yield (PLQY), maximum external quantum efficiency (maximum EQE), and luminance reduction rate after 5 hours of operation for multiple types of red light-emitting element 5R including red light-emitting layer 24REM formed using multiple types of quantum dot solutions shown in FIG.
[0094] As shown in FIG. 12 , when the voltage applied to the electron only device (EOD) is set to a certain value and the amount of injected electrons E in an electron only device (EOD) including a red light-emitting layer 24REM formed using a quantum dot solution with a concentration of 0.02 M is compared with that in an electron only device (EOD) including a red light-emitting layer 24REM formed using a quantum dot solution with a concentration of 0.08 M, it can be confirmed that when the concentration increases fourfold, the amount of injected electrons E decreases by 30%.
[0095] On the other hand, as shown in FIG. 13 , when the voltage applied to the Hole Only Device (HOD) is set to a certain value and the amount of injected holes H in a Hole Only Device (HOD) including a red light-emitting layer 24REM formed using a quantum dot solution with a concentration of 0.02 M is compared with that in a Hole Only Device (HOD) including a red light-emitting layer 24REM formed using a quantum dot solution with a concentration of 0.08 M, it can be confirmed that when the concentration increases fourfold, the amount of injected holes H decreases by 70%.
[0096] As described above, it can be confirmed that with an increase in concentration, the decrease in the amount of injected holes H is much greater than the decrease in the amount of injected electrons E. This can also be understood from the band levels shown in FIGS.
[0097] In order to ensure a better carrier balance between holes H and electrons E and to realize a better external quantum efficiency (EQE), it is preferable to form the red light-emitting layer 24REM using a quantum dot solution having a concentration [M] of 0.08, 0.04, 0.02, or 0.01, which shows a relatively high maximum EQE of 6.8% or more, as shown in FIG. 17 .
[0098] 14 is a diagram showing the degree of brightness reduction due to charge-up of quantum dots QD when a red light-emitting element 5R including a red light-emitting layer 24REM formed using a quantum dot solution with a concentration of 0.01 M from among the multiple types of quantum dot solutions shown in FIG. 7 and a comparative red light-emitting element 50R shown in FIG. 10 are intermittently driven.
[0099] 14 , when the red light-emitting element 5R and the comparative red light-emitting element 50R are driven intermittently by repeating a drive period, which is a constant continuous current-carrying period, and a non-drive period, which is a constant non-current-carrying period, the comparative red light-emitting element 50R experiences a large temporary drop in luminance during the drive period, which is a constant continuous current-carrying period, compared to the red light-emitting element 5R. This temporary drop in luminance during the drive period, which is a constant continuous current-carrying period, is due to charge-up of the quantum dots QDs, and is a reversible drop in luminance that can be resolved by applying a reverse voltage or leaving the element unpowered.
[0100] FIG. 18 is a graph showing the degree of change in luminance and voltage over the driving time of a red light-emitting element 5R including a red light-emitting layer 24REM formed using a quantum dot solution having a concentration of 0.04 M from among the multiple types of quantum dot solutions shown in FIG.
[0101] 19 is a graph showing the degree of change in luminance and voltage over the driving time of a red light-emitting element 5R including a red light-emitting layer 24REM formed using a quantum dot solution having a concentration of 0.08 M from among the multiple types of quantum dot solutions shown in FIG.
[0102] The initial luminance decrease rate (e.g., the luminance decrease rate within one hour) of the red light-emitting element 5R including the red light-emitting layer 24REM formed using the quantum dot solution having a concentration of 0.04 M shown in FIG. 18 is significantly reduced compared to the initial luminance decrease rate (e.g., the luminance decrease rate within one hour) of the red light-emitting element 5R including the red light-emitting layer 24REM formed using the quantum dot solution having a concentration of 0.08 M shown in FIG. 19 .
[0103] Furthermore, the initial increase in driving voltage (e.g., the increase in driving voltage within one hour) of the red light-emitting element 5R including the red light-emitting layer 24REM formed using the quantum dot solution having a concentration of 0.04 M shown in FIG. 18 is significantly reduced compared to the initial increase in driving voltage (e.g., the increase in driving voltage within one hour) of the red light-emitting element 5R including the red light-emitting layer 24REM formed using the quantum dot solution having a concentration of 0.08 M shown in FIG. 19.
[0104] From the above, when the initial luminance decrease rate (for example, the luminance decrease rate within one hour), the initial increase in driving voltage (for example, the increase in driving voltage within one hour), and the luminance decrease rate after 5 hours of driving shown in FIG. 17 are taken into consideration, it is preferable to form the red light-emitting layer 24REM using a quantum dot solution having a concentration [M] of any of 0.04, 0.02, 0.01, and 0.005 from among the multiple types of quantum dot solutions shown in FIG. 7 .
[0105] FIG. 15 is a graph showing the PL intensity (photoluminescence intensity) at each wavelength of the red light-emitting layer 24REM formed using a quantum dot solution with a concentration of 0.01 M from among the multiple types of quantum dot solutions shown in FIG. 7 , and a red light-emitting layer formed using a quantum dot solution with a concentration of 0.16 M as a comparative example.
[0106] As shown in FIG. 15 , the red light-emitting layer formed using a quantum dot solution with a concentration of 0.16 M, which is a comparative example, has an emission peak wavelength of 632 nm, while the red light-emitting layer 24REM formed using a quantum dot solution with a concentration of 0.01 M has an emission peak wavelength of 634 nm. Although a shift in the emission peak wavelength toward longer wavelengths due to the decrease in concentration is observed, the amount of shift is favorable at about 2 nm.
[0107] This shift in the emission peak wavelength to longer wavelengths is thought to be due to an increase in Förster resonance energy transfer (FRET). As shown in Figure 17, the emission peak wavelengths of the red light-emitting layers 24REM formed using quantum dot solutions with concentrations of 0.02M, 0.04M, and 0.08M were all 632 nm, and no shift in the emission peak wavelength to longer wavelengths was observed. This is thought to be because, in the case of the red light-emitting layers 24REM formed using quantum dot solutions with concentrations of 0.02M, 0.04M, and 0.08M, the distance between the cores of the quantum dots QDs could be maintained at a certain level or more, thereby suppressing Förster resonance energy transfer (FRET). On the other hand, in the case of the red light-emitting layer 24REM formed using a quantum dot solution with a concentration of 0.005M, the distance between the cores of the quantum dots QDs could not be maintained at a certain level or more, and an increase in Förster resonance energy transfer (FRET) is thought to have caused the emission peak wavelength to shift to longer wavelengths.
[0108] From the above, when the shift amount of the emission peak wavelength to the long wavelength side is taken into consideration, it is preferable to form the red light-emitting layer 24REM using a quantum dot solution having a concentration [M] of any of 0.08, 0.04, 0.02, and 0.01 among the multiple types of quantum dot solutions shown in FIG. 7 .
[0109] FIG. 16 is a graph showing the relationship between the weight ratio of the continuous film MR containing metal sulfide, which is a medium in the multiple red light-emitting layer 24REM, which is a thin film formed using the multiple quantum dot solutions shown in FIG. 7, and the internal quantum yield (PLQY).
[0110] 16 and 17, in the case of a red light-emitting device 5R including a red light-emitting layer 24REM formed using a quantum dot solution having a concentration [M] of 0.005 among the multiple types of quantum dot solutions shown in Fig. 7, the ZnS medium weight ratio in the red light-emitting layer 24REM is 3.3%, and the internal quantum yield (PLQY) is a favorable value of 60%. Also, in the red light-emitting devices 5R including red light-emitting layers 24REM formed using quantum dot solutions having concentrations [M] of 0.01, 0.02, 0.04, and 0.08, respectively, the ZnS medium weight ratio in the red light-emitting layer 24REM is 6.4% to 35.4%, and the internal quantum yield (PLQY) is a favorable value of 74% to 76%.
[0111] From the above, when the internal quantum yield (PLQY) is taken into consideration, it is preferable to form the red light-emitting layer 24REM using a quantum dot solution having a concentration [M] of any of 0.08, 0.04, 0.02, 0.01, and 0.005 among the multiple types of quantum dot solutions shown in FIG. 7 .
[0112] As shown in FIG. 17 , when the suppression of a shift in the emission peak wavelength, the internal quantum yield (PLQY), the maximum external quantum efficiency (maximum EQE), and the rate of decrease in luminance after 5 hours of operation are all taken into consideration, it is preferable that the weight ratio of the ZnS medium in the red light-emitting layer 24REM is greater than 3.3% and less than 35%. For example, it is preferable to form the red light-emitting layer 24REM using a quantum dot solution having a concentration [M] of 0.04, 0.02, or 0.01 from among the multiple types of quantum dot solutions shown in FIG. 7 . In the case of a red light-emitting element 5R including a red light-emitting layer 24REM formed using a quantum dot solution having a concentration [M] of any one of 0.04, 0.02, and 0.01, the amount of shift in the emission peak wavelength can be suppressed to 0 to 2 nm, the internal quantum yield (PLQY) can be achieved to 74% to 76%, the maximum external quantum efficiency (maximum EQE) can be achieved to 7.6% to 7.9%, and the rate of decrease in luminance after 5 hours of operation can be suppressed to 28% to 44%.
[0113] When the weight ratio of the ZnS medium in the red light-emitting layer 24REM is greater than 3.3% and less than 35%, in a cross section of a portion of the red light-emitting layer 24REM including cross sections of a predetermined number, for example, 50 or more quantum dots QDs, of the multiple quantum dots QDs included in the red light-emitting layer 24REM, the cross-sectional area A of the continuous film MR including metal sulfide as a matrix is 3.4% or more and 27.0% or less of the area B obtained by adding up the cross-sectional areas of the predetermined number, for example, 50 or more quantum dots QDs.
[0114] Furthermore, when the weight ratio of the ZnS medium in the red light-emitting layer 24REM is greater than 3.3% and less than 35%, the volume of the continuous film MR containing metal sulfide, which is the matrix in the red light-emitting layer 24REM, is 3.6% or more and 37.1% or less of the volume of the red light-emitting layer 24REM.
[0115] The preferable volume of the continuous film MR containing metal sulfide relative to the volume of the red light-emitting layer 24REM can be calculated, for example, as follows: For example, the core material of the quantum dots QD has a density of 4.81 g / cm 3 InP, which has a density of 4.09 g / cm, is used as the shell material for quantum dots (QDs). 3 Assuming that ZnS having a diameter of 3.2 nm and a shell thickness of 0.5 nm is used, the average density of the quantum dots is 4.41 g / cm 3 When 15 mg of quantum dots QDs are mixed with ZnS medium at a concentration of 0.005 M (the lower limit), the weight of the ZnS medium is 3.3% and the volume of the ZnS medium is 3.6%. On the other hand, when 15 mg of quantum dots QDs are mixed with ZnS medium at a concentration of 0.08 M (the upper limit), the weight of the ZnS medium is 35.4% and the volume of the ZnS medium is 37.1%.
[0116] Furthermore, the preferred area A of the cross section of the continuous film MR containing metal sulfide relative to the area B, which is the sum of the cross-sectional areas of the above-mentioned predetermined number, for example, 50 or more quantum dots QDs, can be calculated, for example, as follows. If the volume of the quantum dots QDs is V(QD) and the volume of the ZnS medium is V(MR), the volume V(24REM) of the red light-emitting layer 24REM is V(QD) + V(MR). If the thickness of the sample when observed with a transmission electron microscope (TEM) (thickness in the depth direction in FIG. 4) is the radius r of the quantum dots QDs, the cross-sectional area of the quantum dots QDs is ((V(QD) + V(MR)) / r). If the radius of the quantum dots QDs is r, the volume V(QD) of each of the n quantum dots QDs is 4 / 3 × π × r. 3 The maximum cross-sectional area of the quantum dot QD is πr 2 However, the total cross-sectional area of n quantum dots QDs cut at random positions is 0.66nπr 2 Therefore, when the volume of the ZnS medium is 3.6% of the red light-emitting layer 24REM, the cross-sectional area of the ZnS medium is 3.4% of the red light-emitting layer 24REM, and when the volume of the ZnS medium is 37.1% of the red light-emitting layer 24REM, the cross-sectional area of the ZnS medium is 27.0% of the entire red light-emitting layer 24REM.
[0117] Furthermore, a transmission electron microscope (TEM) image of a cross section of a portion of the red light-emitting layer 24REM including cross sections of 50 or more quantum dots QDs out of the plurality of quantum dots QDs may include a first region having a higher electron density, which corresponds to the area of the cross section of the continuous film MR containing a metal sulfide, and a second region having a lower electron density, which corresponds to the combined area of the cross sections of the 50 or more quantum dots QDs; the red light-emitting layer 24REM has a width L perpendicular to the cross section of the red light-emitting layer 24REM; a value F obtained by adding a product D of the area of the first region and the width L and a product E of the area of the second region and the width L represents the volume of the portion of the red light-emitting layer 24REM; and the product D may be the volume of the continuous film MR containing a metal sulfide, which is a matrix in the portion of the red light-emitting layer 24REM.
[0118] Furthermore, the red light-emitting layer 24REM includes a first region having a diffraction peak specific to the X-ray diffraction of a metal sulfide and a second region having a diffraction peak specific to the X-ray diffraction of quantum dots QD, the area of the first region in the cross section of the red light-emitting layer 24REM calculated based on the diffraction peak specific to the X-ray diffraction of the metal sulfide is area G, the area of the second region in the cross section of the red light-emitting layer 24REM calculated based on the diffraction peak specific to the X-ray diffraction of the quantum dots is area H, the red light-emitting layer 24REM has a width L perpendicular to the cross section of the red light-emitting layer 24REM, a value K obtained by adding a product I of the area G and the width L and a product J of the area H and the width L may be defined as a volume of a portion of the red light-emitting layer 24REM, and the product I may be defined as a volume of a continuous film MR containing metal sulfide that is a matrix in a portion of the red light-emitting layer 24REM.
[0119] FIG. 20 is a diagram for explaining a step of forming the red light-emitting layer 24REM included in the method of manufacturing the red light-emitting element 5R provided in the display device 1 of this embodiment.
[0120] As shown in FIG. 20 , the process for forming the red light-emitting layer 24REM included in the manufacturing method of the red light-emitting element 5R provided in the display device 1 includes a process (S1) of preparing a quantum dot solution containing a plurality of quantum dots QD, a metal sulfide precursor, and a solvent, a process (S2) of applying the quantum dot solution, and a heat treatment process (S3) of thermally decomposing the metal sulfide precursor to form a continuous film MR containing the metal sulfide as a matrix.
[0121] In the step (S1) of preparing the quantum dot solution shown in FIG. 20 , the amount of the plurality of quantum dots and the amount of the metal sulfide precursor contained in the quantum dot solution are adjusted so that the value of ((weight of red light-emitting layer 24REM−weight of quantum dots QD) / weight of red light-emitting layer 24REM)×100% in the red light-emitting layer 24REM after the heat treatment step (S3) is greater than 3.3% and smaller than 35%.
[0122] Although not shown, the manufacturing method of the red light emitting element 5R includes a step of forming one of the anode 22 and the cathode 25, a step of forming the above-mentioned red light emitting layer 24REM, and a step of forming the other of the anode 22 and the cathode 25.
[0123] In this embodiment, the configuration and manufacturing method of the red light-emitting element 5R have been described as an example, but the same configuration and manufacturing method can also be applied to the green light-emitting element 5G and the blue light-emitting element 5B.
[0124] [Additional Notes] The present disclosure is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present disclosure. Furthermore, new technical features can be formed by combining the technical means disclosed in each embodiment.
[0125] The present disclosure can be used in a light-emitting element, a display device, a method for manufacturing a light-emitting element, and a method for forming a light-emitting layer.
[0126] 1 Display device 3 Barrier layer 4 Thin film transistor layer 5R Red light emitting element (light emitting element) 5G Green light emitting element (light emitting element) 5B Blue light emitting element (light emitting element) 6 Sealing layer 12 Substrate 16, 18, 20 Inorganic insulating film 21 Planarization film 22 Anode 24R Functional layer including red light emitting layer 24G Functional layer including green light emitting layer 24B Functional layer including blue light emitting layer 24REM, 24REM' Red light emitting layer (light emitting layer) 24HT Hole transport layer 24ET Electron transport layer 25 Cathode 26, 28 Inorganic sealing film 27 Organic film 39 Functional film QD, QD' Quantum dot CO Quantum dot core SH, SH' Quantum dot shell MR Continuous film (matrix) PIX Pixel RSP Red subpixel GSP Green subpixel BSP Blue subpixel DA Display area NDA Frame area
Claims
1. A light-emitting device comprising: an anode; a cathode; and a light-emitting layer provided between the anode and the cathode, the light-emitting layer including a matrix containing a metal sulfide and a plurality of quantum dots encapsulated in the matrix, wherein in a cross-section of a portion of the light-emitting layer including cross-sections of a predetermined number of the plurality of quantum dots, an area C of the cross-section of the portion of the light-emitting layer is smaller than twice the combined area B of the cross-sections of the predetermined number of quantum dots.
2. The light-emitting element according to claim 1, wherein the area A calculated by subtracting the area B from the area C is 3.4% or more and 27.0% or less of the area B.
3. The light-emitting element described in claim 1 or 2, wherein a transmission electron microscope (TEM) image of the cross section of the light-emitting layer includes a first region having a higher electron density through which an irradiated electron beam has passed and a second region having a lower electron density, the area of the first region is area A calculated by subtracting area B from area C, and the area of the second region is area B.
4. The light-emitting element described in claim 1 or 2, wherein the cross-section of the light-emitting layer includes a first region having a specific diffraction peak due to X-ray diffraction of the metal sulfide and a second region having a specific diffraction peak due to X-ray diffraction of the quantum dots, an area of the first region in the cross-section of the light-emitting layer calculated based on the specific diffraction peak due to X-ray diffraction of the metal sulfide is area A calculated from area C - area B, and an area of the second region in the cross-section of the light-emitting layer calculated based on the specific diffraction peak due to X-ray diffraction of the quantum dots is area B.
5. A light-emitting element comprising: an anode; a cathode; and a light-emitting layer provided between the anode and the cathode, wherein the light-emitting layer contains a matrix containing a metal sulfide and a plurality of quantum dots encapsulated in the matrix, and a volume of the matrix in the light-emitting layer is 3.6% or more and 37.1% or less of the volume of the light-emitting layer.
6. The light-emitting element described in claim 5, wherein a transmission electron microscope (TEM) image of a cross-section of a portion of the light-emitting layer including cross-sections of a predetermined number of the plurality of quantum dots includes a first region corresponding to an area of the cross-section of the matrix and having a higher electron density through which the irradiated electron beam has passed, and a second region corresponding to an area equal to the combined area of the cross-sections of the predetermined number of quantum dots and having a lower electron density, the light-emitting layer has a width L perpendicular to the cross-section of the light-emitting layer, a value F obtained by adding up a product D of the area of the first region and the width L and a product E of the area of the second region and the width L is a volume of the portion of the light-emitting layer, and the product D is a volume of the matrix in the portion of the light-emitting layer.
7. The light-emitting element according to claim 5, wherein the light-emitting layer includes a first region having a specific diffraction peak due to X-ray diffraction of the metal sulfide and a second region having a specific diffraction peak due to X-ray diffraction of the quantum dots, an area of the first region on a certain surface of the light-emitting layer calculated based on the specific diffraction peak due to X-ray diffraction of the metal sulfide is area G, an area of the second region on the certain surface of the light-emitting layer calculated based on the specific diffraction peak due to X-ray diffraction of the quantum dots is area H, the light-emitting layer has a width L perpendicular to the certain surface of the light-emitting layer, a value K obtained by adding a product I of the area G and the width L and a product J of the area H and the width L is a volume of the light-emitting layer, and the product I is a volume of the matrix in the light-emitting layer.
8. A light-emitting element described in any one of claims 1 to 7, wherein in a cross-section of a portion of the light-emitting layer including cross-sections of a predetermined number of quantum dots among the plurality of quantum dots, the number-average inter-quantum dot distance of the predetermined number of quantum dots is 1 nm or more and 5 nm or less.
9. A light-emitting element according to any one of claims 1 to 8, wherein the quantum dot includes a core and a shell, the shell of the quantum dot is composed of a metal sulfide, and the band gap of the matrix is larger than the band gap of the core of the quantum dot.
10. A light-emitting element according to any one of claims 1 to 8, wherein the quantum dot includes a core and a shell, the shell of the quantum dot is composed of a material other than metal sulfide, and the band gap of the matrix is larger than the band gap of the core of the quantum dot.
11. The light-emitting element according to claim 1, wherein the metal sulfide contains one or more metal elements selected from the group consisting of Zn, Mg, and Ga.
12. The light-emitting element according to claim 11, wherein the metal sulfide is any one of zinc sulfide, zinc magnesium sulfide, gallium sulfide, zinc selenide sulfide, zinc telluride sulfide, magnesium sulfide, and zinc gallium sulfide.
13. The light-emitting device according to claim 12, wherein the metal sulfide is zinc sulfide.
14. A display device comprising a light-emitting element according to any one of claims 1 to 13.
15. A method for manufacturing a light-emitting element, comprising the step of forming the light-emitting layer, wherein the step of forming the light-emitting layer comprises: preparing a quantum dot solution containing the plurality of quantum dots, a precursor of the metal sulfide, and a solvent; applying the quantum dot solution; and a heat treatment step of thermally decomposing the precursor of the metal sulfide to form a matrix containing the metal sulfide, wherein in the step of preparing the quantum dot solution, the amount of the plurality of quantum dots and the amount of the precursor of the metal sulfide contained in the quantum dot solution are adjusted so that a value of ((weight of light-emitting layer-weight of quantum dots) / weight of light-emitting layer) x 100% in the light-emitting layer after the heat treatment step is greater than 3.3% and smaller than 35%.
16. A method for forming a light-emitting layer, the method comprising: preparing a quantum dot solution containing a plurality of quantum dots, a metal sulfide precursor, and a solvent; applying the quantum dot solution; and a heat treatment step of thermally decomposing the metal sulfide precursor to form a matrix containing the metal sulfide, wherein in the step of preparing the quantum dot solution, the amount of the plurality of quantum dots and the amount of the metal sulfide precursor contained in the quantum dot solution are adjusted so that the value of ((weight of light-emitting layer-weight of quantum dots) / weight of light-emitting layer) x 100% in the light-emitting layer after the heat treatment step is greater than 3.3% and smaller than 35%.
17. A method for manufacturing a light-emitting element, comprising: forming one of an anode and a cathode; forming a light-emitting layer by the method for forming a light-emitting layer according to claim 16; and forming the other of the anode and the cathode.
Citation Information
Patent Citations
Doped quantum dot, preparation method thereof and quantum dot photoelectric device
CN110003884A
Electroluminescent devices with improved power distribution
JP2010526420A
Quantum Dots with Inorganic Ligands in an Inorganic Matrix
JP2017505842A
Stabilized inks containing semiconductor particles and uses thereof - Patents.com
JP2022530420A
Light emitting device and method for preparing the same
KR1020170105156A
Cited By
Colored resin composition, colored film, black matrix, color filter, and organic el display device
WO2026163940A1