Lithium-metal complex oxide, positive electrode active material for lithium secondary battery, positive electrode for lithium secondary battery, and lithium secondary battery

The development of a lithium metal composite oxide with a layered structure and specific elemental composition addresses the challenge of cycle characteristics in lithium secondary batteries by enhancing lithium ion diffusion and structural stability, resulting in improved battery performance and longevity.

WO2024219129A1PCT designated stage expired Publication Date: 2024-10-24SUMITOMO CHEM CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010408
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-17
Filing Date
2024-03-18
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Lithium secondary batteries face challenges in achieving excellent cycle characteristics, which are crucial for their performance and longevity, as existing materials do not effectively facilitate smooth lithium ion diffusion and stable structural integrity.

Method used

A lithium metal composite oxide with a layered structure, containing specific elements like Co, Si, Ca, Na, Fe, and Mg, is developed, optimizing the molar ratios and physical properties such as diffraction peak intensity ratios, BET specific surface area, and particle size distribution to enhance lithium ion diffusion and structural stability.

Benefits of technology

The optimized lithium metal composite oxide significantly improves the cycle characteristics of lithium secondary batteries by ensuring efficient lithium ion movement and maintaining structural integrity, leading to higher cycle retention rates and extended battery life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010408_24102024_PF_FP_ABST
    Figure JP2024010408_24102024_PF_FP_ABST
Patent Text Reader

Abstract

This lithium-metal complex oxide has a layered structure and satisfies (1) and (2). (1) Co, an element M1, and an element M2 are contained, and the molar ratio of the element M1 to Co is 0.05-6. The element M1 is at least one element selected from the group consisting of Si, Ca, and Na, and the element M2 is at least one element selected from the group consisting of Fe and Mg. (2) In X-ray diffraction measurement using CuKα rays, two diffraction peaks exist within a range of 2θ=38.0±0.5°, and, of the two diffraction peaks, when a diffraction peak on a low-angle side and a diffraction peak on a high-angle side are defined as peak A and peak B, respectively, the following formula is satisfied. 0.50≤IA / IB≤0.75 (where IA represents the peak area of the peak A, and IB represents the peak area of the peak B).
Need to check novelty before this filing date? Find Prior Art

Description

Lithium metal composite oxide, positive electrode active material for lithium secondary battery, positive electrode for lithium secondary battery, and lithium secondary battery

[0001] The present invention relates to a lithium metal composite oxide, a positive electrode active material for a lithium secondary battery, a positive electrode for a lithium secondary battery, and a lithium secondary battery. This application claims priority based on Japanese Patent Application No. 2023-067359, filed on April 17, 2023, the contents of which are incorporated herein by reference.

[0002] Lithium metal composite oxides are used as positive electrode active materials for lithium secondary batteries. The physical properties of lithium metal composite oxides affect the performance of lithium secondary batteries. For this reason, active development of lithium metal composite oxides is underway to improve the performance of lithium secondary batteries.

[0003] For example, Patent Document 1 discloses that a lithium metal composite oxide having a diffraction peak intensity ratio I(006) / I(102) of 0.44 or less between the (006) plane and the (102) plane in the Miller indices hkl of X-ray diffraction and satisfying other physical properties improves the charge / discharge capacity and rate characteristics of a lithium secondary battery.

[0004] JP-A-2013-112531

[0005] As the range of applications for lithium secondary batteries expands, further improvements in cycle characteristics are required.

[0006] An object of the present invention is to obtain a lithium metal composite oxide that can provide a lithium secondary battery with excellent cycle characteristics.

[0007] Another object of the present invention is to provide a positive electrode active material for a lithium secondary battery, a positive electrode for a lithium secondary battery, and a lithium secondary battery, each containing the lithium metal composite oxide.

[0008] The present invention encompasses the following [1] to

[11] . [1] A lithium metal composite oxide having a layered structure and satisfying the following (1) and (2): (1) It contains Co, an element M1, and an element M2, and the molar ratio of the element M1 to Co is 0.05 or more and 6 or less. The element M1 is one or more elements selected from the group consisting of Si, Ca, and Na, and the element M2 is one or more elements selected from the group consisting of Fe and Mg. (2) In powder X-ray diffraction measurement using CuKα radiation, there are two diffraction peaks within the range of 2θ = 38.0 ± 0.5°, and when the diffraction peak on the lower angle side of the two diffraction peaks is designated as Peak A and the diffraction peak on the higher angle side is designated as Peak B, the following formula is satisfied: 0.50≦I A / I B ≦0.75 ... Formula (I A is the peak area of ​​the peak A, and I B is the peak area of ​​the peak B.) [2] The lithium metal composite oxide according to [1], wherein the total mass of Co, the element M1, and the element M2 contained in the lithium metal composite oxide is 12,000 ppm or less. [3] The lithium metal composite oxide according to [1] or [2], wherein the element M1 contains Ca and Si, and the molar ratio of Si to Ca is 8 or more. [4] The lithium metal composite oxide according to any one of [1] to [3], wherein the element M1 contains Na and Si, and the molar ratio of Si to Na is 0.5 or more. [5] The lithium metal composite oxide according to any one of [1] to [3], wherein the element M1 contains Na and Si, and the molar ratio of Si to Na is 0.5 or more. [6] The lithium metal composite oxide according to [1], wherein the BET specific surface area is 1.0 m 2 / g or more 2.0m 2 [6] The lithium metal composite oxide according to any one of [1] to [4], wherein D 10 , D 50 and D 90 The lithium metal composite oxide according to any one of [1] to [5], wherein 0.5≦(D 90 -D 10 ) / D 50 ≦1.5...Formula (I) (D 10 is the 10% cumulative volume particle size of the lithium metal composite oxide, and D 50 is the 50% cumulative volume particle size of the lithium metal composite oxide, and D 90is the 90% cumulative volume particle size of the lithium metal composite oxide.) [7] The lithium metal composite oxide according to any one of [1] to [6], wherein the lithium metal composite oxide has an average particle strength of 20 MPa or more. [8] The lithium metal composite oxide according to any one of [1] to [7], wherein the standard deviation of the particle strength of the lithium metal composite oxide is 40% or less. [9] A positive electrode active material for a lithium secondary battery, containing the lithium metal composite oxide according to any one of [1] to [8].

[10] A positive electrode for a lithium secondary battery, containing the positive electrode active material for a lithium secondary battery according to [9].

[11] A lithium secondary battery having the positive electrode for a lithium secondary battery according to

[10] .

[0009] According to the present invention, a lithium metal composite oxide capable of providing a lithium secondary battery with excellent cycle characteristics can be obtained. Furthermore, a positive electrode active material for a lithium secondary battery, a positive electrode for a lithium secondary battery, and a lithium secondary battery containing such a lithium metal composite oxide can be provided.

[0010] 1A and 1B are schematic diagrams showing an example of a lithium secondary battery and an all-solid-state lithium secondary battery, respectively.

[0011] In this specification, a metal composite compound (Metal Composite Compound) will be referred to as "MCC", a lithium metal composite oxide (LiMO) will be referred to as "LiMO", and a cathode active material for lithium secondary batteries will be referred to as "CAM". A lithium secondary battery is a battery in which an electrolyte (such as a non-aqueous electrolyte or a solid electrolyte) is disposed between a positive electrode and a negative electrode, and charging and discharging are performed by lithium ions moving between the positive electrode and the negative electrode via the electrolyte.

[0012] "Ni" refers to nickel atoms, not nickel metal. Similarly, "Co" and "Li" refer to cobalt atoms, lithium atoms, etc., respectively.

[0013] When a numerical range is described as, for example, "1-10 μm" or "1 to 10 μm," it means a range from 1 μm to 10 μm, including the lower limit of 1 μm and the upper limit of 10 μm.

[0014] In the present specification, the upper and lower limits of the ranges of values ​​can be arbitrarily combined. The ranges of values ​​of the respective physical properties, compositions, and manufacturing conditions can be arbitrarily combined.

[0015] [Method for Measuring Cycle Retention Rate] In this specification, "excellent cycle characteristics" means that a lithium secondary battery prepared by the method described below has a cycle retention rate of 80% or more as measured as described below.

[0016] (Preparation of a Positive Electrode for a Lithium Secondary Battery) Using LiMO as CAM, the CAM, a conductive material (acetylene black), and a binder (PVdF) are mixed and kneaded in a ratio of CAM:conductive material:binder = 92:5:3 (mass ratio) to prepare a paste-like positive electrode mixture. N-methyl-2-pyrrolidone is used as an organic solvent when preparing the positive electrode mixture.

[0017] The resulting positive electrode mixture is applied to a 40 μm thick Al foil as a current collector and dried in vacuum at 150° C. for 8 hours to obtain a positive electrode for a lithium secondary battery. The electrode area of ​​this positive electrode for a lithium secondary battery is 1.65 cm 2 Let's say.

[0018] (Fabrication of Lithium Secondary Battery) The following operation is carried out in a glove box under an argon atmosphere. The above-mentioned lithium secondary battery positive electrode is placed on the bottom cover of a coin-type battery R2032 part (manufactured by Hosen Co., Ltd.) with the aluminum foil side facing down, and a separator (25 μm thick) made of porous polypropylene film is placed on top of it. 300 μl of electrolyte is poured into this. The electrolyte used is a liquid obtained by dissolving LiPF6 at a ratio of 1 mol / L in a mixture of ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate in a volume ratio of 30:35:35.

[0019] Next, a lithium metal negative electrode was placed on the separator, a lid was placed on the negative electrode via a gasket, and the negative electrode was crimped with a crimping machine to prepare a lithium secondary battery (coin-type half cell R2032). The assembled lithium secondary battery was left standing at room temperature for 12 hours to allow the separator and the positive electrode active material layer to be sufficiently impregnated with the electrolyte.

[0020] The test temperature was 25° C., and the current setting value for both charging and discharging was 0.2 CA. The maximum charging voltage was 4.3 V, and the minimum discharging voltage was 2.5 V.

[0021] Next, constant current / constant voltage charging and constant current discharging were repeated at a test temperature of 25°C under the following conditions: 50 charge / discharge cycles were performed: Charging: Current setting value 1 CA, maximum voltage 4.3 V, constant voltage / constant current charging; Discharging: Battery setting value 1 CA, minimum voltage 2.5 V, constant current discharging.

[0022] The cycle retention rate is calculated from the discharge capacity at the first cycle and the discharge capacity at the 50th cycle using the following formula. A higher cycle retention rate indicates better cycle characteristics because the decrease in battery capacity after repeated charging and discharging is suppressed. Cycle retention rate (%) = discharge capacity at the 50th cycle (mAh / g) / discharge capacity at the 1st cycle (mAh / g) × 100

[0023] <Lithium Metal Composite Oxide> The crystal structure of LiMO of this embodiment is a layered structure, and is more preferably a hexagonal crystal structure or a monoclinic crystal structure.

[0024] The hexagonal crystal structure is P3, P3 1 , P3 2 , R3, P-3, R-3, P312, P321, P3 1 12. P3 1 21, P3 2 12. P3 2 21, R32, P3m1, P31m, P3c1, P31c, R3m, R3c, P-31m, P-31c, P-3m1, P-3c1, R-3m, R-3c, P6, P6 1 , P6 5 , P6 2 , P6 4 , P63 , P-6, P6 / m, P6 3 / m, P622, P6 1 22, P6 5 22, P6 2 22, P6 4 22, P6 3 22, P6mm, P6cc, P6 3 cm, P6 3 mc, P-6m2, P-6c2, P-62m, P-62c, P6 / mmm, P6 / mcc, P6 3 / mcm, and P6 3 / mmc.

[0025] In addition, the monoclinic crystal structure is P2, P2 1 , C2, Pm, Pc, Cm, Cc, P2 / m, P2 1 / m, C2 / m, P2 / c, P2 1 It is assigned to any one space group selected from the group consisting of C1 / c, C2 / c, and C3 / c.

[0026] From the viewpoint of obtaining a lithium secondary battery having excellent cycle characteristics, the crystal structure of LiMO is more preferably a hexagonal crystal structure belonging to the space group R-3m or a monoclinic crystal structure belonging to the space group C2 / m.

[0027] [Method for Confirming Crystal Structure] The crystal structure of LiMO can be confirmed by observation using a powder X-ray diffraction measurement device (for example, Ultima IV manufactured by Rigaku Corporation).

[0028] Furthermore, the LiMO satisfies the following (1) and (2).

[0029] (1) LiMO contains Co, element M1, and element M2. Element M1 is at least one element selected from the group consisting of Si, Ca, and Na, and element M2 is at least one element selected from the group consisting of Fe and Mg. In LiMO, the molar ratio of element M1 to Co, i.e., M1 / Co, is 0.05-6.

[0030] M1 / Co is preferably 0.06 or more, and more preferably greater than 0.07. M1 / Co is preferably 5.5 or less, more preferably 5.0 or less, and even more preferably 4.5 or less. Examples of M1 / Co include 0.05-5.5, 0.06-5.0, 0.06-4.5, or greater than 0.07 and 4.5 or less.

[0031] During operation of a lithium secondary battery, lithium ions diffuse between the layers inside the LiMO crystal and move to the electrolyte interface. The more smoothly lithium ions can diffuse inside the LiMO crystal, the less the cycle characteristics will deteriorate, resulting in a lithium secondary battery with a longer life. In other words, if the crystal structure of LiMO can be controlled to one that allows lithium ions to diffuse more easily, the cycle characteristics of the lithium secondary battery can be easily improved.

[0032] One method for controlling the crystal structure of LiMO is to control the degree of sintering of the fired product obtained after the firing step. Specifically, by controlling the degree of sintering in the step of mixing and firing MCC containing Co and element M1 with a lithium compound, the degree of development of the layered structure of LiMO can be controlled.

[0033] The inventors have found that the use of LiMO that satisfies the above condition (1) improves the cycle characteristics of lithium secondary batteries. This is presumably because a layered structure that allows lithium ions to diffuse smoothly is easily formed.

[0034] The total mass of Co, element M1, and element M2 contained in LiMO is preferably 12,000 ppm or less, more preferably 10,000 ppm or less, even more preferably 8,000 ppm or less, and particularly preferably 6,100 ppm or less. The lower limit of the total mass of Co, element M1, and element M2 contained in LiMO is preferably 10 ppm or more, more preferably 50 ppm or more, even more preferably 100 ppm or more, and particularly preferably 580 ppm or more.

[0035] From the viewpoint of environmental regulations and stable mass production, it is preferable that the content of Co, a rare metal, be small. Here, element M1 is an element that acts on the site where Li is accommodated and contributes to the diffusion of lithium ions, and element M2 is an element that acts on the major metal elements (e.g., Ni and Mn) that constitute LiMO and contributes to the development of a layered structure. If element M1 is present in excess, it will hinder the diffusion of lithium ions, and if element M2 is present in excess, it will hinder the development of the layered structure. Therefore, from the viewpoint of cycle characteristics as well as the stable supply of lithium secondary batteries, it is preferable that the total amount of Co, element M1, and element M2 contained in LiMO be equal to or less than the above upper limit.

[0036] The total mass of Co, element M1, and element M2 contained in LiMO is, for example, 10-12,000 ppm, 50-10,000 ppm, 100-8,000 ppm, or 580-6,100 ppm, relative to 100 mass% of the total amount of metal elements other than Li contained in LiMO.

[0037] The element M1 may be at least one element selected from the group consisting of Si, Ca, and Na, and when two or more elements are included, the combination is not particularly limited. Furthermore, the element M1 may include all of Si, Ca, and Na.

[0038] When the element M1 contains Ca and Si, the molar ratio of Si to Ca (Si / Ca) is preferably 8 or more, more preferably 8.5 or more, and even more preferably 9 or more. Si / Ca is preferably 100 or less, more preferably 90 or less, still more preferably 85 or less, and particularly preferably 80 or less.

[0039] The Si / Ca ratio may be, for example, 8 to 100, 8.5 to 90, 9 to 85, or 8 to 80. When the Si / Ca ratio is within the above range, the cycle characteristics can be improved.

[0040] When the element M1 contains Na and Si, the molar ratio of Si to Na (Si / Na) is preferably 0.5 or more, more preferably 0.6 or more, and even more preferably 0.7 or more. The Si / Na ratio is preferably 10 or less, more preferably 9 or less, and even more preferably 8 or less.

[0041] The Si / Na ratio may be, for example, 0.5 to 10, 0.6 to 9, or 0.7 to 8. When the Si / Na ratio is within the above range, the cycle characteristics can be improved.

[0042] LiMO contains Li in addition to Co, element M1, and element M2. Preferably, LiMO further contains Ni and one or more elements M0 selected from the group consisting of Mn and Al.

[0043] (Composition Formula) In order to further improve cycle characteristics, the LiMO is preferably represented by the following composition formula (A): Li x Ni y Co z M0 s M1 t M2 u O 2   ... (A) (In formula (A), 0.80≦x≦1.20, 0.70≦y≦0.98, 0≦s<0.30, 0<z+t+u≦0.02, and y+z+s+t+u=1, M0 is the element M0, M1 is the element M1, and M2 is the element M2.)

[0044] x is preferably 0.81 or more, more preferably 0.82 or more. x is preferably 1.19 or less, more preferably 1.18 or less. Examples of x include 0.81 to 1.19, or 0.82 to 1.18.

[0045] y is preferably 0.71 or more, more preferably 0.72 or more, and even more preferably 0.80 or more. y is preferably 0.95 or less, more preferably 0.94 or less, and even more preferably 0.93 or less. Examples of y include 0.71-0.95, 0.72-0.94, and 0.80-0.93.

[0046] When LiMO contains the element MO, s is preferably 0.28 or less, more preferably 0.20 or less, even more preferably 0.10 or less, and particularly preferably 0.09 or less. For example, s is greater than 0 and 0.28 or less, greater than 0 and 0.20 or less, greater than 0 and 0.1 or less, or greater than 0 and 0.09 or less.

[0047] z+t+u is preferably 0.015 or less. z+t+u is preferably 0.0003 or more, more preferably 0.0005 or more. Examples of z+t+u include 0.0003-0.02, or 0.0005-0.015.

[0048] [Composition Analysis] The composition of LiMO is analyzed by dissolving LiMO powder in hydrochloric acid and then measuring the composition using an ICP optical emission spectrometer, such as Optima 7300 manufactured by PerkinElmer Co., Ltd.

[0049] (2) In powder X-ray diffraction measurement using CuKα radiation, the LiMO exhibits two diffraction peaks within the range of 2θ=38.0±0.5°. When the lower-angle diffraction peak is designated as Peak A and the higher-angle diffraction peak is designated as Peak B, the LiMO satisfies the following formula: 0.50≦I A / I B ≦0.75 ... Formula (I A is the peak area of ​​peak A, and I B is the peak area of ​​peak B.)

[0050] I A / I B is preferably 0.52 or more, and more preferably 0.53 or more. A / I B is more preferably 0.74 or less, and even more preferably 0.73 or less. A / I B More preferably, I satisfies the following formula (B) or (C): 0.52≦I A / I B ≦0.74 ...Formula (B) 0.53≦I A / I B ≦0.73...Formula (C)

[0051] Distortion in the crystal structure tends to hinder the smooth diffusion of lithium ions. Eliminating the distortion in the crystal structure further improves the cycle characteristics. In addition, if the crystal plane through which lithium ions can easily enter and exit is exposed to the electrolyte, the cycle characteristics are less likely to deteriorate. Through studies by the present inventors, it has been found that the cycle characteristics of a lithium secondary battery are improved when LiMO that satisfies both (1) and (2) above is used. This is presumably because the distortion in the crystal structure of LiMO is eliminated, exposing the crystal plane through which lithium ions can easily enter and exit to the electrolyte.

[0052] [I A / I B [Method for Obtaining the Powder X-ray Diffraction of LiMO] The powder X-ray diffraction measurement of LiMO is performed using a powder X-ray diffractometer. For example, a LINT2000 manufactured by Rigaku Corporation can be used as the powder X-ray diffractometer. Specifically, LiMO powder is loaded onto a dedicated substrate, and measurements are performed using a Cu-Kα source under conditions of a diffraction angle 2θ = 10° to 90°, a sampling width of 0.02°, and a scan speed of 4° / min to obtain a powder X-ray diffraction pattern. Using integrated powder X-ray analysis software, two diffraction peaks within the range of 2θ = 38.0 ± 0.5° are identified from the obtained powder X-ray diffraction pattern. The two peaks selected at this time are the peak with the maximum peak intensity and the peak with the second largest peak intensity. Of the two identified peaks, the diffraction peak on the lower angle side is designated Peak A, and the diffraction peak on the higher angle side is designated Peak B.

[0053] Next, the peak area of ​​peak A, I A and I, the peak area of ​​peak B. B Specifically, the peak area is calculated within the range enclosed by the peak curve from the peak start to the peak end of the peak and the baseline. In this specification, the peak start refers to the rising point of the peak after peak separation, and refers to the point of contact between the peak and the baseline. In this specification, the peak end refers to the end point of the peak after peak separation, and refers to the point of contact between the peak and the baseline.

[0054] The peak area can be calculated automatically using integrated powder X-ray analysis software, such as JADE manufactured by Materials Data.

[0055] The BET specific surface area of ​​LiMO is 1.0 m 2 / g or more is preferable, and 1.1m 2 / g or more is more preferable, and 1.2m 2 / g or more is more preferable. The BET specific surface area is 2.0 m 2 / g or less is preferable, and 1.8m 2 / g or less is more preferable, and 1.7m 2 The BET specific surface area is, for example, 1.0 to 2.0 m / g or less. 2 / g, 1.1-1.8m 2 / g, or 1.2-1.7m 2 / g.

[0056] When LiMO having a BET specific surface area equal to or greater than the lower limit is used, the reaction interface of LiMO increases, facilitating the ingress and egress of lithium ions, and the cycle characteristics are less likely to deteriorate. When LiMO having a BET specific surface area equal to or less than the upper limit is used, the contact area between LiMO and the electrolyte is less likely to increase, and a coating caused by decomposition of the electrolyte is less likely to form. If the amount of such a coating is small, lithium ion conductivity is less likely to be inhibited, and the cycle characteristics are less likely to deteriorate.

[0057] [Measurement of BET Specific Surface Area] The BET specific surface area of ​​LiMO can be measured using a BET specific surface area measuring device. As the BET specific surface area measuring device, for example, Macsorb (registered trademark) manufactured by Mountech Co., Ltd. can be used. When measuring powdered LiMO, it is preferable to dry it in a nitrogen atmosphere at 105°C for 30 minutes as a pretreatment.

[0058] LiMO's D 10 , D 50 and D 90 It is preferable that the following formula (I) is satisfied: 0.5≦(D 90 -D 10 ) / D 50 ≦1.5...Formula (I) (D 10is the 10% cumulative volume particle size of LiMO, and D 50 is the 50% cumulative volume particle size of LiMO, and D 90 is the 90% cumulative volume particle size of LiMO.

[0059] LiMO satisfying the above formula (I) is ideally packed as a powder into a crucible or a sheath, and sintering is facilitated, facilitating crystal growth, which in turn facilitates improvement in cycle characteristics.

[0060] (D 90 -D 10 ) / D 50 is preferably 0.6 or more, and more preferably 0.8 or more. 90 -D 10 ) / D 50 is more preferably 1.4 or less. 90 -D 10 ) / D 50 is, for example, 0.6-1.5, 0.6-1.4, or 0.8-1.4.

[0061] D 50 is preferably 8 μm or more, more preferably 10 μm or more. 50 is preferably 25 μm or less, more preferably 20 μm or less. 50 is, for example, 8-25 μm or 10-20 μm. 50 In the case of LiMO having a valence of 0.05 to 0.1, when LiMO is mixed with a conductive material and a binder in a layer, the particles of the LiMO are packed together in an ideal manner, and as a result, lithium ions can move efficiently within the electrode mixture layer during operation of the lithium secondary battery, which tends to improve the cycle characteristics.

[0062] [D 10 , D 90 and D 50 Measurement of the D of the above LiMO 10 (μm), D 50 (μm) and D 90 (μm) can be measured by the following dry method.

[0063] Specifically, first, dry particle size distribution is measured using 2 g of LiMO using a laser diffraction particle size distribution meter, and a volume-based cumulative particle size distribution curve is obtained. In the obtained cumulative particle size distribution curve, the particle diameter values ​​at 10%, 50%, and 90% accumulation from the fine particle side are respectively D 10 , D 50 , D 90 As the laser diffraction particle size distribution analyzer, for example, MS2000 manufactured by Malvern Instruments can be used.

[0064] The average particle strength of LiMO is preferably 20 MPa or more, more preferably 21 MPa or more, and even more preferably 25 MPa or more. The average particle strength of LiMO is preferably 60 MPa or less, more preferably 55 MPa or less, and even more preferably 50 MPa or less. The average particle strength of LiMO is, for example, 20 to 60 MPa, 21 to 55 MPa, or 25 to 50 MPa.

[0065] When LiMO having an average particle strength within the above range is used, the LiMO particles are less likely to crack during battery operation, which reduces the occurrence of cracks that could cause resistance and reduces the deterioration of cycle characteristics.

[0066] [Method for measuring average particle strength] The average particle strength of LiMO is measured by the following method. 50 At least three or more LiMO particles having a size of about ±2 μm are selected. 50 is the above [D 10 , D 90 and D 50 The particle size is measured by the method described in [Measurement of the particle size distribution in the measurement ...

[0067] Here, "major axis" means the longest diameter of the particle. "minor axis" means the shortest diameter of the particle. Next, a test pressure (load) is applied to one of the LiMO particles selected above, and the displacement of the LiMO particle is measured.

[0068] For the measurement, a "Micro Compression Tester MCT-510" manufactured by Shimadzu Corporation is used. Three or more particles selected above are placed in the device, and the test pressure is gradually increased. The pressure value at which the displacement amount is maximized while the test pressure remains almost constant is taken as the test force (P) (unit: MPa). From the obtained test force (P), the crushing strength (St) (unit: MPa) is calculated using the following formula (X) (see Journal of the Mining Industry of Japan, Vol. 81, (1965)). This operation is performed a total of seven times, and the average value of five measurements excluding the maximum and minimum values ​​of the crushing strength is calculated as the average particle strength. In the following formula (X), d is the secondary particle diameter (unit: μm) of the LiMO particles. St = 2.8 × P / (π × d × d) ... formula (X)

[0069] The standard deviation of the particle strength of LiMO is preferably 40% or less, more preferably 30% or less, and even more preferably 25% or less. The standard deviation is preferably 3% or more, more preferably 5% or more, and even more preferably 10% or more. The standard deviation is preferably 3-40%, more preferably 5-30%, and even more preferably 10-25%. When a positive electrode active material layer is produced using LiMO having the standard deviation in the above range, the particle strength within the positive electrode active material layer exhibits small variations, resulting in a homogeneous layer. As a result, the LiMO particles are less likely to crack during operation of the lithium secondary battery, and the cycle characteristics are less likely to deteriorate.

[0070] [Method for measuring standard deviation of particle strength] The standard deviation of particle strength is calculated using the values ​​of particle strength and average particle strength obtained by the above [Method for measuring average particle strength]. Specifically, the squares of the differences between the particle strength and the average particle strength of each data item are summed, and the positive square root of the sum obtained is divided by the total number of data items, and the standard deviation of particle strength is calculated.

[0071] <<Method for Producing LiMO>> The method for producing LiMO includes a step of obtaining MCC and a step of obtaining LiMO. Hereinafter, the step of obtaining MCC and the step of obtaining LiMO will be described in this order.

[0072] [Step of Obtaining MCC] MCC contains Co, element M1, and element M2. "MCC containing Co, element M1, and element M2" includes an embodiment in which Co, element M1, and element M2 are present in the crystal of MCC, and an embodiment in which Co, element M1, and element M2 are present in the periphery of MCC. Preferably, MCC further contains Ni and the above-mentioned element M0. Examples of MCC include metal composite hydroxides, metal composite oxides, and mixtures of metal composite hydroxides and metal composite oxides containing these elements.

[0073] MCC can be produced by a commonly known batch co-precipitation method or continuous co-precipitation method. The production method will be described in detail below using an MCC containing Ni, element M0, Co, element M1, and element M2 as an example.

[0074] First, a nickel salt solution, a metal salt solution of element M0, a cobalt salt solution, a metal salt solution of element M1, a metal salt solution of element M2, and an optional complexing agent are mixed by a coprecipitation method, particularly the continuous coprecipitation method described in JP-A-2002-201028, to produce a metal composite hydroxide.

[0075] The nickel salt that is the solute of the nickel salt solution is not particularly limited, but for example, one or more of nickel sulfate, nickel nitrate, nickel chloride, and nickel acetate can be used.

[0076] As the metal salt of element M0, which is the solute of the metal salt solution of element M0, for example, one or more of manganese sulfate, manganese nitrate, manganese chloride, manganese acetate, aluminum sulfate, and sodium aluminate can be used.

[0077] The nickel salt solution and the metal salt solution of element MO are used in a ratio corresponding to the desired composition ratio of LiMO (for example, composition formula (A)).

[0078] A nickel salt solution and a metal salt solution of element M0 are supplied to a reaction vessel and mixed to obtain a raw material liquid.

[0079] Next, the cobalt salt solution, the metal salt solution of element M1, and the metal salt solution of element M2 are added to the raw material liquid in the reaction vessel to obtain a mixed raw material liquid.

[0080] As the cobalt salt that is the solute of the cobalt salt solution, for example, one or more of cobalt sulfate, cobalt nitrate, cobalt chloride, and cobalt acetate can be used.

[0081] As the metal salt of element M1, which is the solute of the metal salt solution of element M1, when element M1 is Ca, one or more of calcium sulfate, calcium nitrate, calcium chloride, calcium acetate, calcium carbonate, calcium oxide, and calcium hydroxide can be used; when element M1 is Si, one or more of silicon dioxide, sodium silicate, and aluminum silicate can be used; and when element M1 is Na, one or more of sodium sulfate, sodium nitrate, sodium chloride, sodium acetate, sodium carbonate, sodium oxide, sodium hydroxide, and sodium silicate can be used.

[0082] As the metal salt of element M2, which is the solute of the metal salt solution of element M2, when element M2 is Fe, one or more of iron sulfate (II), iron sulfate (III), iron nitrate (II), iron nitrate (III), iron chloride (II), iron chloride (III), iron acetate (II), iron oxide (II), iron oxide (III), iron hydroxide (II), and iron hydroxide (III) can be used; when element M2 is Mg, one or more of magnesium sulfate, magnesium nitrate, magnesium chloride, magnesium acetate, magnesium carbonate, calcium oxide, and magnesium hydroxide can be used.

[0083] The cobalt salt solution, the metal salt solution of element M1, and the metal salt solution of element M2 are added so that M1 / Co is 0.05 to 6. This makes it possible to obtain LiMO that satisfies the above (1).

[0084] The amounts of the cobalt salt solution, the metal salt solution of element M1, and the metal salt solution of element M2 added are preferably such that the total mass of Co, element M1, and element M2 contained in the desired LiMO is 12,000 ppm or less.

[0085] The solvent for the nickel salt solution, the metal salt solution of element M0, the cobalt salt solution, the metal salt solution of element M1, and the metal salt solution of element M2 is, for example, water.

[0086] The complexing agent is a compound capable of forming a complex with Ni and ions of element M0 in an aqueous solution, such as ammonium ion donors, hydrazine, ethylenediaminetetraacetic acid, nitrilotriacetic acid, uracildiacetic acid, and glycine.

[0087] Examples of the ammonium ion donor include ammonium salts such as ammonium hydroxide, ammonium sulfate, ammonium chloride, ammonium carbonate, and ammonium fluoride.

[0088] When a complexing agent is contained, the amount of the complexing agent contained in the mixed liquid containing the mixed raw material liquid and the complexing agent is, for example, a molar ratio of more than 0 and not more than 2 to the total number of moles of the nickel salt, the metal salt of the element M0, the cobalt salt, the metal salt of the element M1, and the metal salt of the element M2 contained in the mixed liquid.

[0089] In the coprecipitation method, an alkaline aqueous solution such as a sodium hydroxide aqueous solution or a potassium hydroxide aqueous solution is added to the mixed solution before the pH of the mixed solution changes from alkaline to neutral in order to adjust the pH of the mixed solution.

[0090] In this specification, the pH value is defined as the value measured when the temperature of the mixed solution is 40° C. If the temperature of the mixed solution sampled from the reaction tank is not 40° C., the mixed solution is heated or cooled to 40° C. and then the pH is measured.

[0091] During the reaction, the temperature of the reaction vessel is controlled within the range of, for example, 20 to 80°C, preferably 30 to 70°C.

[0092] During the reaction, the pH value in the reaction vessel is controlled within the range of, for example, 9 to 13, preferably 11 to 13.

[0093] The materials in the reaction vessel are mixed by appropriate stirring. As the reaction vessel used in the continuous coprecipitation method, an overflow type reaction vessel can be used in order to separate the formed reaction precipitate.

[0094] Here, for example, an inert gas such as nitrogen, argon or carbon dioxide, an oxidizing gas such as air or oxygen, or a mixture of these gases may be supplied into the reaction vessel.

[0095] In order to control the atmosphere inside the reaction vessel to a desired level, a predetermined gas may be passed through the reaction vessel or the reaction solution may be directly bubbled through the reaction vessel.

[0096] After the above reaction, the resulting reaction precipitate is washed with water and, if necessary, dried to obtain a metal composite hydroxide. If necessary, the reaction precipitate may also be washed with weak acid water or an alkaline solution containing sodium hydroxide or potassium hydroxide.

[0097] When producing a metal composite oxide as MCC, the metal composite oxide is obtained by oxidizing a metal composite hydroxide.

[0098] In this case, the oxidation time, which is the total time from the start of temperature increase to the end of temperature maintenance after reaching the temperature, is preferably 2 to 10 hours. The oxidation temperature is preferably 500 to 800°C.

[0099] During oxidation, various gases may be supplied into the reaction vessel, for example, inert gases such as nitrogen, argon, and carbon dioxide, oxidizing gases such as air and oxygen, or mixtures thereof.

[0100] The MCC may be classified as appropriate.

[0101] [Step of Obtaining LiMO] The step of obtaining LiMO includes a mixing step of mixing MCC with a lithium compound, and a firing step of firing the resulting mixture.

[0102] Mixing step: MCC is mixed with a lithium compound. The lithium compound can be at least one of lithium carbonate, lithium nitrate, lithium acetate, lithium hydroxide, lithium hydroxide hydrate, lithium oxide, lithium chloride, and lithium fluoride. Among these, lithium hydroxide, lithium hydroxide hydrate, and lithium carbonate, or a mixture thereof, is preferred.

[0103] The lithium compound and MCC are mixed in consideration of the composition ratio of the final target product to obtain a mixture of the lithium compound and MCC. The amount (molar ratio) of Li relative to the total amount of Ni and optional element M0 contained in MCC is preferably 0.80 to 1.20, more preferably 0.90 to 1.10, even more preferably 0.91 to 1.10, and particularly preferably 0.92 to 1.10.

[0104] Calcination step: By calcining the mixture of MCC and a lithium compound, crystals grow and LiMO is obtained. For the calcination, dry air, an oxygen atmosphere, or the like is used depending on the desired composition. In this embodiment, calcination in an oxygen atmosphere is preferred.

[0105] The firing process may be a single firing or may have multiple firing stages. When multiple firing stages are used, the firing step at the highest temperature is referred to as the main firing. Prior to the main firing, preliminary firing may be performed at a temperature lower than that of the main firing. Furthermore, after the main firing, post-firing may be performed at a temperature lower than that of the main firing.

[0106] In this embodiment, it is preferable to first calcinate the mixture of MCC and the lithium compound, and then calcinate it. It is also preferable that both the calcination and the calcination are carried out in an oxygen atmosphere.

[0107] The calcination temperature during the calcination is preferably 600 to 900°C, more preferably 610 to 850°C, and even more preferably 620°C or higher and lower than 700°C. When the calcination temperature is equal to or higher than the lower limit, LiMO having a strong crystal structure can be obtained. On the other hand, when the calcination temperature is equal to or lower than the upper limit, volatilization of lithium ions on the surface of LiMO particles can be reduced.

[0108] The firing temperature during the main firing is preferably 600 to 900°C, more preferably 650 to 850°C, and even more preferably 700 to 820°C. When the firing temperature is equal to or higher than the lower limit, LiMO having a strong crystal structure can be obtained. On the other hand, when the firing temperature is equal to or lower than the upper limit, volatilization of lithium ions on the surface of LiMO particles can be reduced.

[0109] The firing temperature in this specification refers to the highest temperature maintained in the atmosphere inside the firing furnace during firing. When firing is performed multiple times, the firing temperature refers to the highest temperature at the stage of firing at the highest temperature. The firing furnace used for firing may be, for example, either a continuous static firing furnace or a fluidized bed firing furnace. Examples of continuous static firing furnaces include tunnel furnaces and roller hearth kilns. Examples of fluidized bed firing furnaces include rotary kilns.

[0110] The holding times during the pre-sintering and main sintering are preferably 1 to 50 hours, more preferably 2 to 20 hours. When the holding times are equal to or less than the upper limit, volatilization of lithium ions is suppressed, and deterioration of battery performance is suppressed. When the holding times are equal to or greater than the lower limit, crystal growth is promoted, and deterioration of battery performance is suppressed. By adjusting the conditions in the sintering step, the BET specific surface area, average particle strength, or standard deviation of particle strength of the resulting LiMO can be adjusted to fall within the above-mentioned ranges.

[0111] Crushing Step: The fired product obtained after the firing step is crushed using a stone mill grinder (for example, Masscolloider (registered trademark)). As the Masscolloider, for example, an MKCA6-5J manufactured by Masuko Sangyo Co., Ltd. can be used. In the crushing step, crushing is performed using the stone mill grinder under conditions of, for example, a rotation speed of 800 to 1500 rpm and a pitch of 10 to 1000 μm.

[0112] By crushing the fired product using a stone mill, LiMO that satisfies the above condition (2) can be obtained.

[0113] [Optional Steps] Washing Step: The crushed product obtained in the crushing step is preferably washed with a washing liquid such as pure water or an alkaline washing liquid. Examples of the alkaline washing liquid include an aqueous solution of one or more anhydrides selected from the group consisting of lithium hydroxide, sodium hydroxide, potassium hydroxide, lithium carbonate, sodium carbonate, potassium carbonate, and ammonium carbonate, an aqueous solution of a hydrate of the anhydrides, and ammonia.

[0114] The temperature of the cleaning solution is preferably not more than 20° C., more preferably not more than 15° C., and even more preferably not more than 10° C. By controlling the temperature of the cleaning solution to the upper limit value or less and at a temperature at which the cleaning solution does not freeze, excessive elution of lithium ions from the crystalline structure of the crushed material into the cleaning solution during cleaning can be suppressed.

[0115] It is preferable to wash with a washing solution in an amount of at least twice the mass of the crushed material. Furthermore, if washing is carried out batchwise, it is preferable to carry out washing two or more times. After washing with a solution other than water, it is preferable to further wash with water to prevent compounds derived from the solution from remaining in the crushed material.

[0116] Drying Step After the washing step, the washed crushed material may be dried. In this case, the drying temperature is preferably 80 to 250°C, more preferably 90 to 230°C. The drying time is preferably 0.5 to 24 hours, more preferably 1 to 10 hours. The drying pressure may be normal pressure or reduced pressure.

[0117] Through the above steps, the LiMO is obtained.

[0118] <CAM> The CAM of this embodiment contains LiMO produced by the method described above.

[0119] <Lithium secondary battery> A positive electrode for a lithium secondary battery suitable for use with the CAM containing LiMO of this embodiment will be described. Hereinafter, the positive electrode for a lithium secondary battery will be sometimes referred to as a positive electrode. Furthermore, a lithium secondary battery suitable for use as the positive electrode will be described.

[0120] An example of a suitable lithium secondary battery for use with the CAM of this embodiment has a positive electrode, a negative electrode, a separator sandwiched between the positive electrode and the negative electrode, and an electrolyte solution disposed between the positive electrode and the negative electrode.

[0121] 1 is a schematic diagram showing an example of a lithium secondary battery. For example, a cylindrical lithium secondary battery 10 is manufactured as follows.

[0122] First, as shown in the partially enlarged view of FIG. 1 , a pair of strip-shaped separators 1, a strip-shaped positive electrode 2 having a positive electrode lead 21 at one end, and a strip-shaped negative electrode 3 having a negative electrode lead 31 at one end are stacked in this order: separator 1, positive electrode 2, separator 1, negative electrode 3, and then wound to form an electrode group 4.

[0123] The positive electrode 2 includes, for example, a positive electrode active material layer 2 a containing CAM and a positive electrode current collector 2 b having the positive electrode active material layer 2 a formed on one surface thereof. The positive electrode 2 can be manufactured by first preparing a positive electrode mixture containing CAM, a conductive material, and a binder, and then supporting the positive electrode mixture on one surface of the positive electrode current collector 2 b to form the positive electrode active material layer 2 a.

[0124] Examples of the negative electrode 3 include an electrode in which a negative electrode mixture containing a negative electrode active material (not shown) is supported on a negative electrode current collector, and an electrode made of a negative electrode active material alone, and can be manufactured in the same manner as the positive electrode 2.

[0125] Next, the electrode group 4 and an insulator (not shown) are housed in the battery can 5, the bottom of the can is sealed, the electrode group 4 is impregnated with an electrolyte solution 6, and the electrolyte is disposed between the positive electrode 2 and the negative electrode 3. Furthermore, the top of the battery can 5 is sealed with a top insulator 7 and a sealing member 8, whereby a lithium secondary battery 10 can be manufactured.

[0126] The shape of the electrode group 4 can be, for example, a columnar shape such that the cross-sectional shape when the electrode group 4 is cut perpendicular to the winding axis is a circle, an ellipse, a rectangle, or a rectangle with rounded corners.

[0127] The shape of a lithium secondary battery having such an electrode group 4 can be any shape specified in IEC 60086, which is a standard for batteries established by the International Electrotechnical Commission (IEC), or JIS C 8500. Examples of shapes include a cylindrical shape and a rectangular shape.

[0128] Furthermore, the lithium secondary battery is not limited to the above-mentioned wound type configuration, and may be a stacked type configuration in which a stacked structure of a positive electrode, a separator, a negative electrode, and a separator is repeatedly stacked. Examples of stacked lithium secondary batteries include so-called coin type batteries, button type batteries, and paper type (or sheet type) batteries.

[0129] The positive electrode, separator, negative electrode, and electrolyte constituting the lithium secondary battery can be those described in, for example,

[0113] to

[0140] of WO2022 / 113904A1, and the materials and manufacturing methods therefor.

[0130] <All-Solid-State Lithium Secondary Battery> The CAM of this embodiment can be used as a CAM for an all-solid-state lithium secondary battery.

[0131] Fig. 2 is a schematic diagram showing an example of an all-solid-state lithium secondary battery. The all-solid-state lithium secondary battery 1000 shown in Fig. 2 includes a laminate 100 having a positive electrode 110, a negative electrode 120, and a solid electrolyte layer 130, and an exterior body 200 that houses the laminate 100. The all-solid-state lithium secondary battery 1000 may also have a bipolar structure in which a CAM and a negative electrode active material are disposed on both sides of a current collector. A specific example of a bipolar structure is the structure described in JP-A-2004-95400.

[0132] The positive electrode 110 includes a positive electrode active material layer 111 and a positive electrode current collector 112. The positive electrode active material layer 111 includes the above-described CAM and solid electrolyte. The positive electrode active material layer 111 may also include a conductive material and a binder.

[0133] The negative electrode 120 includes a negative electrode active material layer 121 and a negative electrode current collector 122. The negative electrode active material layer 121 contains a negative electrode active material. The negative electrode active material layer 121 may also contain a solid electrolyte and a conductive material.

[0134] The laminate 100 may have an external terminal 113 connected to the positive electrode current collector 112 and an external terminal 123 connected to the negative electrode current collector 122. In addition, the all-solid-state lithium secondary battery 1000 may have a separator between the positive electrode 110 and the negative electrode 120.

[0135] The all-solid-state lithium secondary battery 1000 further includes an insulator (not shown) that insulates the laminate 100 from the exterior body 200 , and a sealing body (not shown) that seals the opening 200 a of the exterior body 200 .

[0136] The exterior body 200 may be a container molded from a highly corrosion-resistant metal material such as aluminum, stainless steel, or nickel-plated steel. Alternatively, the exterior body 200 may be a bag-shaped container made of a laminate film having corrosion resistance on at least one surface.

[0137] The shape of the all-solid-state lithium secondary battery 1000 may be, for example, a coin type, a button type, a paper type (or a sheet type), a cylindrical type, a square type, or a laminate type (pouch type).

[0138] Although the all-solid-state lithium secondary battery 1000 is illustrated as having one laminate 100 as an example, the present embodiment is not limited to this. The all-solid-state lithium secondary battery 1000 may have a configuration in which the laminate 100 is used as a unit cell, and a plurality of unit cells (laminated bodies 100) are sealed inside an exterior body 200.

[0139] For the all-solid-state lithium secondary battery, for example, the configuration, materials and manufacturing method described in paragraphs

[0151] to

[0181] of WO2022 / 113904A1 can be used.

[0140] In the lithium secondary battery having the above-described configuration, the CAM is used, so that a lithium secondary battery having excellent cycle characteristics can be provided.

[0141] Furthermore, the positive electrode having the above-described structure has the CAM having the above-described structure, and therefore the cycle characteristics of the lithium secondary battery are excellent.

[0142] Furthermore, the lithium secondary battery having the above-described structure has excellent cycle characteristics because it has the above-described positive electrode.

[0143] While the preferred embodiments of the present invention have been described above with reference to the accompanying drawings, the present invention is not limited to these examples. The shapes and combinations of the components shown in the above examples are merely examples, and various modifications can be made based on design requirements, etc., without departing from the spirit of the present invention.

[0144] Next, the present invention will be described in more detail with reference to examples.

[0145] <Measurement of Various Parameters> The various parameters of LiMO produced by the method described below were measured using the above-mentioned [Method for Confirming Crystal Structure], [Composition Analysis], and [I A / I B [Method of obtaining], [Measurement of BET specific surface area], [D 10 , D 90 and D 50 Measurement was carried out using the measurement methods described in [Measurement of particle strength], [Method for measuring average particle strength], and [Method for measuring standard deviation of particle strength].

[0146] <Method for Measuring Cycle Retention Ratio> The cycle retention ratio of the lithium secondary battery prepared by the method described above was measured according to the method described in the above-mentioned [Method for Measuring Cycle Retention Ratio].

[0147] Example 1 Water was placed in a reaction tank equipped with a stirrer and an overflow pipe, and then an aqueous sodium hydroxide solution was added, and the liquid temperature (reaction temperature) was maintained at 50° C. A nickel sulfate aqueous solution, a manganese sulfate aqueous solution, and an aluminum sulfate aqueous solution were mixed in such a ratio that the atomic ratio of Ni to Mn to Al was 93:1:6, thereby preparing raw material solution 1.

[0148] Next, a 0.1 wt % aqueous calcium hydroxide solution, a 0.1 wt % aqueous magnesium sulfate solution, a 0.1 wt % aqueous sodium silicate solution, a 0.1 wt % aqueous iron chloride solution, and a 0.1 wt % aqueous cobalt sulfate solution were added to raw material liquid 1 in such proportions that (Si+Na+Ca) / Co=4.29, (Si+Fe+Mg+Na+Ca+Co) / (Ni+Mn+Al)=1680 ppm, Si / Na=6.61, and Si / Ca=69.18, thereby obtaining a mixed raw material liquid 1.

[0149] Next, in the reaction vessel, an aqueous ammonium sulfate solution was continuously added as a complexing agent to the mixed raw material liquid 1 under stirring. An aqueous sodium hydroxide solution was added dropwise at appropriate times under the condition that the pH of the mixed liquid in the reaction vessel became 12.1 (when the liquid temperature was 40° C.), thereby obtaining a reaction precipitate 1.

[0150] The obtained reaction precipitate 1 was washed and then dried at 105° C. for 20 hours to obtain MCC1, which is a metal composite hydroxide.

[0151] MCC1 and lithium hydroxide monohydrate powder were weighed and mixed in a ratio of Li / (Ni + Mn + Al) = 1.03 to obtain Mixture 1. Mixture 1 was then pre-fired at 650°C for 5 hours in an oxygen atmosphere. Next, it was fired at 750°C for 5 hours in an oxygen atmosphere to obtain Fired Product 1.

[0152] The obtained fired material 1 was crushed in a mass colloider to obtain crushed material 1. The operating conditions and equipment used for the mass colloider were as follows. (Operating conditions for the mass colloider) Equipment used: MKCA6-5J manufactured by Masuko Sangyo Co., Ltd. Rotation speed: 1200 rpm Gap: 100 μm

[0153] The crushed material 1 and pure water adjusted to a liquid temperature of 5°C were mixed in a ratio such that the mass ratio of the crushed material 1 to the total amount was 0.5, and the resulting slurry was stirred for 20 minutes. The mixture was then dehydrated and dried at 210°C for 10 hours under a nitrogen atmosphere to obtain LiMO-1 having a layered structure. In the composition formula (A), LiMO-1 had x = 0.99, y = 0.93, s = 0.064, z + t + u = 0.005, M0 was Mn and Al, M1 was Si, Ca, and Na, and M2 was Fe and Mg. The composition of LiMO-1, I A / I B , BET specific surface area, D 50 , (D 90 -D 10 ) / D 50 The average particle strength, the standard deviation of the particle strength, and the cycle retention rate are shown in Table 1. The same is true for the following Examples and Comparative Examples.

[0154] Example 2 Water was placed in a reaction vessel equipped with a stirrer and an overflow pipe, and then an aqueous sodium hydroxide solution was added, and the liquid temperature (reaction temperature) was maintained at 50° C. A nickel sulfate aqueous solution, a manganese sulfate aqueous solution, and an aluminum sulfate aqueous solution were mixed in an atomic ratio of Ni:Mn:Al of 93:3.5:3.5 to prepare raw material solution 2.

[0155] Next, a 0.1 wt % aqueous calcium hydroxide solution, a 0.1 wt % aqueous magnesium sulfate solution, a 0.1 wt % aqueous sodium silicate solution, a 0.1 wt % aqueous iron chloride solution, and a 0.1 wt % aqueous cobalt sulfate solution were added to raw material liquid 2 in proportions such that (Si+Na+Ca) / Co=0.65, (Si+Fe+Mg+Na+Ca+Co) / (Ni+Mn+Al)=758 ppm, Si / Na=1.80, and Si / Ca=15.69, thereby obtaining a mixed raw material liquid 2.

[0156] LiMO-2 having a layered structure was obtained in the same manner as in Example 1, except that mixed raw material solution 2 was used and the temperature during main firing was set to 770° C. In LiMO-2, in the composition formula (A), x = 0.95, y = 0.93, s = 0.066, z + t + u = 0.0017, M0 was Mn and Al, M1 was Si, Ca, and Na, and M2 was Fe and Mg.

[0157] Example 3 To the above-mentioned raw material liquid 2, a 0.1 wt % aqueous calcium hydroxide solution, a 0.1 wt % aqueous magnesium sulfate solution, a 0.1 wt % aqueous sodium silicate solution, a 0.1 wt % aqueous iron chloride solution, and a 0.1 wt % aqueous cobalt sulfate solution were added in such proportions that the ratios were (Si+Na+Ca) / Co=0.07, (Si+Fe+Mg+Na+Ca+Co) / (Ni+Mn+Al)=6197 ppm, Si / Na=0.92, and Si / Ca=12.84, thereby obtaining a mixed raw material liquid 3.

[0158] Next, in the reaction vessel, an aqueous ammonium sulfate solution was continuously added as a complexing agent to the mixed raw material liquid 3 under stirring. An aqueous sodium hydroxide solution was added dropwise at appropriate times under the condition that the pH of the mixed liquid in the reaction vessel became 12.1 (when the liquid temperature was 40° C.), thereby obtaining a reaction precipitate 3.

[0159] The obtained reaction precipitate 3 was washed and then dried at 105° C. for 20 hours to obtain MCC3, which is a metal composite hydroxide.

[0160] MCC3 and lithium hydroxide monohydrate powder were weighed and mixed in a ratio of Li / (Ni + Al + Mn) = 1.05 to obtain mixture 3. Except for using mixture 3, LiMO-3 having a layered structure was obtained in the same manner as in Example 1. In LiMO-3, in the composition formula (A), x = 0.98, y = 0.92, s = 0.073, z + t + u = 0.011, M0 was Mn and Al, M1 was Si, Ca, and Na, and M2 was Fe and Mg.

[0161] Example 4 To the above-mentioned raw material liquid 2, an aqueous calcium hydroxide solution having a concentration of 0.1 wt %, an aqueous magnesium sulfate solution having a concentration of 0.1 wt %, an aqueous sodium silicate solution having a concentration of 0.1 wt %, an aqueous iron chloride solution having a concentration of 0.1 wt %, and an aqueous cobalt sulfate solution having a concentration of 0.1 wt % were added in such proportions that the ratios were (Si+Na+Ca) / Co=0.73, (Si+Fe+Mg+Na+Ca+Co) / (Ni+Mn+Al)=588 ppm, Si / Na=0.95, and Si / Ca=9.98, thereby obtaining a mixed raw material liquid 4.

[0162] LiMO-4 having a layered structure was obtained in the same manner as in Example 1, except that mixed raw material liquid 4 was used. LiMO-4 had the following composition formula (A): x = 0.99, y = 0.94, s = 0.064, z + t + u = 0.0013, M0 was Mn and Al, M1 was Si, Ca, and Na, and M2 was Fe and Mg.

[0163] Example 5 To the above-mentioned raw material liquid 2, an aqueous calcium hydroxide solution having a concentration of 0.1 wt %, an aqueous magnesium sulfate solution having a concentration of 0.1 wt %, an aqueous sodium silicate solution having a concentration of 0.1 wt %, an aqueous iron chloride solution having a concentration of 0.1 wt %, and an aqueous cobalt sulfate solution having a concentration of 0.1 wt % were added in such proportions that the ratios were (Si+Na+Ca) / Co=0.67, (Si+Fe+Mg+Na+Ca+Co) / (Ni+Mn+Al)=570 ppm, Si / Na=1.64, and Si / Ca=11.41, thereby obtaining a mixed raw material liquid 5.

[0164] LiMO-5 having a layered structure was obtained in the same manner as in Example 1, except that mixed raw material solution 5 was used. LiMO-5 had the following composition formula (A): x = 1.00, y = 0.93, s = 0.066, z + t + u = 0.0013, M0 was Mn and Al, M1 was Si, Ca, and Na, and M2 was Fe and Mg.

[0165] Comparative Example 1 To the above-mentioned raw material liquid 2, an aqueous calcium hydroxide solution having a concentration of 0.1 wt %, an aqueous magnesium sulfate solution having a concentration of 0.1 wt %, an aqueous sodium silicate solution having a concentration of 0.1 wt %, an aqueous iron chloride solution having a concentration of 0.1 wt %, and an aqueous cobalt sulfate solution having a concentration of 0.1 wt % were added in such proportions that the values ​​were (Si+Na+Ca) / Co=8.34, (Si+Fe+Mg+Na+Ca+Co) / (Ni+Mn+Al)=3758 ppm, Si / Na=1.80, and Si / Ca=0.05, thereby obtaining a mixed raw material liquid 6.

[0166] Next, in the reaction vessel, an aqueous ammonium sulfate solution was continuously added as a complexing agent to the mixed raw material liquid 6 under stirring. An aqueous sodium hydroxide solution was added dropwise at appropriate times under the condition that the pH of the mixed liquid in the reaction vessel became 12.1 (when the liquid temperature was 40° C.), thereby obtaining a reaction precipitate 6.

[0167] The obtained reaction precipitate 6 was washed and then dried at 105°C for 20 hours to obtain MCC6, which is a metal composite hydroxide.

[0168] MCC6 and lithium hydroxide monohydrate powder were weighed and mixed in a ratio of Li / ((Ni + Mn + Al) = 1.15 to obtain Mixture 6. Mixture 6 was then pre-fired at 650°C for 5 hours in an oxygen atmosphere. Next, it was fired at 770°C for 5 hours in an oxygen atmosphere to obtain Fired Product 6.

[0169] LiMO-6 having a layered structure was obtained in the same manner as in Example 1, except for using the fired product 6. In LiMO-6, in the composition formula (A), x = 1.02, y = 0.93, s = 0.055, z + t + u = 0.0091, M0 was Mn and Al, M1 was Si, Ca, and Na, and M2 was Fe and Mg.

[0170] Comparative Example 2 To the above-mentioned raw material liquid 2, an aqueous calcium hydroxide solution having a concentration of 0.1 wt %, an aqueous magnesium sulfate solution having a concentration of 0.1 wt %, an aqueous sodium silicate solution having a concentration of 0.1 wt %, an aqueous iron chloride solution having a concentration of 0.1 wt %, and an aqueous cobalt sulfate solution having a concentration of 0.1 wt % were added in such proportions that the ratios were (Si+Na+Ca) / Co=0.03, (Si+Fe+Mg+Na+Ca+Co) / (Ni+Mn+Al)=13,196 ppm, Si / Na=13.09, and Si / Ca=22.82, thereby obtaining a mixed raw material liquid 7.

[0171] LiMO-7 having a layered structure was obtained in the same manner as in Example 3, except that mixed raw material solution 7 was used. LiMO-7 had the following composition formula (A): x = 1.02, y = 0.94, s = 0.034, z + t + u = 0.023, M0 was Mn and Al, M1 was Si, Ca, and Na, and M2 was Fe and Mg.

[0172] Comparative Example 3 To the above-mentioned raw material liquid 2, a 0.1 wt % aqueous calcium hydroxide solution, a 0.1 wt % aqueous magnesium sulfate solution, a 0.1 wt % aqueous sodium silicate solution, a 0.1 wt % aqueous iron chloride solution, and a 0.1 wt % aqueous cobalt sulfate solution were added in such proportions that the ratios were (Si+Na+Ca) / Co=117.92, (Si+Fe+Mg+Na+Ca+Co) / (Ni+Mn+Al)=130 ppm, Si / Na=1.39, and Si / Ca=3.47, thereby obtaining a mixed raw material liquid 8.

[0173] Next, in the reaction vessel, an aqueous ammonium sulfate solution was continuously added as a complexing agent to the mixed raw material liquid 8 under stirring. An aqueous sodium hydroxide solution was added dropwise at appropriate times under the condition that the pH of the mixed liquid in the reaction vessel became 12.1 (when the liquid temperature was 40° C.), thereby obtaining a reaction precipitate 8.

[0174] The obtained reaction precipitate 8 was washed and then dried at 105°C for 20 hours to obtain MCC8, which is a metal composite hydroxide.

[0175] MCC8 and lithium hydroxide monohydrate powder were weighed and mixed in a ratio of Li / (Ni + Mn + Al) = 1.03 to obtain mixture 8. Mixture 8 was then pre-fired at 650°C for 5 hours in an oxygen atmosphere. Next, it was fired at 750°C for 5 hours in an oxygen atmosphere to obtain fired product 8.

[0176] The obtained fired product 8 was crushed in a mortar to obtain crushed product 8.

[0177] LiMO-8 having a layered structure was obtained in the same manner as in Example 1, except that the crushed product 8 was used. LiMO-8 had the following composition formula (A): x = 1.00, y = 0.94, s = 0.061, z + t + u = 0.0004, M0 was Mn and Al, M1 was Si, Ca, and Na, and M2 was Fe and Mg.

[0178] Comparative Example 4: After water was placed in a reaction vessel equipped with a stirrer and an overflow pipe, an aqueous sodium hydroxide solution was added, and the liquid temperature (reaction temperature) was maintained at 50°C. A nickel sulfate aqueous solution, a manganese sulfate aqueous solution, and an aluminum sulfate aqueous solution were mixed in a ratio such that the atomic ratio of Ni to Mn to Al was 93:6:1 to prepare raw material solution 4. A 0.1 wt% aqueous calcium hydroxide solution, a 0.1 wt% aqueous magnesium sulfate solution, a 0.1 wt% aqueous sodium silicate solution, a 0.1 wt% aqueous iron chloride solution, and a 0.1 wt% aqueous cobalt sulfate solution were added to raw material solution 4 in ratios such that (Si + Na + Ca) / Co = 1.23, (Si + Fe + Mg + Na + Ca + Co) / (Ni + Mn + Al) = 925 ppm, Si / Na = 0.35, and Si / Ca = 12.84, thereby obtaining mixed raw material solution 9.

[0179] Next, in the reaction vessel, an aqueous ammonium sulfate solution was continuously added as a complexing agent to the mixed raw material liquid 9 under stirring. An aqueous sodium hydroxide solution was added dropwise at appropriate times under the condition that the pH of the mixed liquid in the reaction vessel became 12.1 (when the liquid temperature was 40° C.), thereby obtaining a metal composite hydroxide 9.

[0180] The obtained metal composite hydroxide 9 was washed and then dried at 105° C. for 20 hours to obtain MCC9, which is a metal composite hydroxide.

[0181] MCC9 and lithium hydroxide monohydrate powder were weighed and mixed in a ratio of Li / (Ni + Mn + Al) = 1.05 to obtain Mixture 9. LiMO-9 having a layered structure was obtained in the same manner as in Comparative Example 3, except that Mixture 9 was used and the temperature during main firing was set to 770°C. In LiMO-9, in the composition formula (A), x = 1.02, y = 0.93, s = 0.067, z + t + u = 0.0023, M0 was Mn and Al, M1 was Si, Ca, and Na, and M2 was Fe and Mg.

[0182] Comparative Example 5 To the above-mentioned raw material liquid 2, a 0.1 wt % aqueous calcium hydroxide solution, a 0.1 wt % aqueous magnesium sulfate solution, a 0.1 wt % aqueous sodium silicate solution, a 0.1 wt % aqueous iron chloride solution, and a 0.1 wt % aqueous cobalt sulfate solution were added in such proportions that the ratios were (Si+Na+Ca) / Co=0.64, (Si+Fe+Mg+Na+Ca+Co) / (Ni+Mn+Al)=752 ppm, Si / Na=1.80, and Si / Ca=39.22, thereby obtaining a mixed raw material liquid 10.

[0183] LiMO-10 having a layered structure was obtained in the same manner as in Comparative Example 3, except that mixed raw material liquid 10 was used. LiMO-10 had the following composition formula (A): x = 0.98, y = 0.93, s = 0.064, z + t + u = 0.0016, M0 was Mn and Al, M1 was Si, Ca, and Na, and M2 was Fe and Mg.

[0184]

[0185] As shown in Table 1 above, in Examples 1 to 5 which satisfied the above (1) and (2), the cycle retention rate was 80% or more, and the cycle characteristics were good.

[0186] On the other hand, in Comparative Examples 1 and 2 which did not satisfy the above (1), Comparative Examples 4 and 5 which did not satisfy the above (2), and Comparative Example 3 which did not satisfy the above (1) and (2), the cycle retention rate was less than 80%.

[0187] 1: separator, 2: positive electrode, 2a: positive electrode active material layer, 2b: positive electrode current collector layer, 3: negative electrode, 4: electrode group, 5: battery can, 6: electrolyte, 7: top insulator, 8: sealing body, 10: lithium secondary battery, 21: positive electrode lead, 31: negative electrode lead, 100: laminate, 110: positive electrode, 111: positive electrode active material layer, 112: positive electrode current collector, 113: external terminal, 120: negative electrode, 121: negative electrode active material layer, 122: negative electrode current collector, 123: external terminal, 130: solid electrolyte layer, 200: exterior body, 200a: opening, 1000: all-solid-state lithium secondary battery

Claims

1. A lithium metal composite oxide having a layered structure and satisfying the following (1) and (2): (1) It contains Co, element M1, and element M2, and the molar ratio of element M1 to Co is 0.05 or more and 6 or less. The element M1 is one or more elements selected from the group consisting of Si, Ca, and Na, and the element M2 is one or more elements selected from the group consisting of Fe and Mg. (2) In powder X-ray diffraction measurement using CuKα rays, there are two diffraction peaks within the range of 2θ=38.0±0.5°, and when the diffraction peak on the low angle side of the two diffraction peaks is designated as peak A and the diffraction peak on the high angle side is designated as peak B, the following formula is satisfied: 0.50≦I A / I B ≦0.75 ... Formula (I A is the peak area of ​​the peak A, and I B is the peak area of ​​the peak B.

2. The lithium metal composite oxide according to claim 1, wherein the total mass of Co, the element M1 and the element M2 contained in the lithium metal composite oxide is 12,000 ppm or less.

3. The lithium metal composite oxide according to claim 1 or 2, wherein the element M1 contains Ca and Si, and the molar ratio of Si to Ca is 8 or more.

4. The lithium metal composite oxide according to claim 1 or 2, wherein the element M1 contains Na and Si, and the molar ratio of Si to Na is 0.5 or more.

5. BET specific surface area is 1.0 m 2 / g or more 2.0m 2 The lithium metal composite oxide according to claim 1 or 2, wherein the Li-ion concentration is 0.1 to 0.5% by mass.

6. D 10 , D 50 and D. 90 The lithium metal composite oxide according to claim 1 or 2, wherein 0.5≦(D 90 -D 10 ) / D 50 ≦1.5...Formula (I) (D 10 is the 10% cumulative volume particle size of the lithium metal composite oxide, and D 50 is the 50% cumulative volume particle size of the lithium metal composite oxide, and D 90 is the 90% cumulative volume particle size of the lithium metal composite oxide.

7. The lithium metal composite oxide according to claim 1 or 2, wherein the average particle strength of said lithium metal composite oxide is 20 MPa or more.

8. The lithium metal composite oxide according to claim 1 or 2, wherein the standard deviation of particle strength of the lithium metal composite oxide is 40% or less.

9. A positive electrode active material for a lithium secondary battery, comprising the lithium metal composite oxide according to claim 1 or 2.

10. A positive electrode for a lithium secondary battery comprising the positive electrode active material for a lithium secondary battery according to claim 9.

11. A lithium secondary battery comprising the positive electrode for lithium secondary batteries according to claim 10.

Citation Information

Patent Citations

  • High density nickel hydroxide coprecipitated with cobalt and manganese, and method for producing the same

    JP2002201028A

  • Bipolar battery and its control method

    JP2004095400A

  • Lithium metal composite oxide and method for producing the same

    JP2013112531A

  • Communication device

    JP2023067359A

  • Method for producing lithium metal composite oxide

    WO2022113904A1