Exterior material for electricity storage device

The exterior material for power storage devices addresses moldability issues by using a heat-sealing layer with mixed particles and a lubricant to enhance slipperiness and formability, resulting in high-quality devices with improved reliability.

WO2024219399A1PCT designated stage expired Publication Date: 2024-10-24RESONAC PACKAGING CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015166
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-17
Filing Date
2024-04-16
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Conventional exterior materials for power storage devices face issues with unstable moldability due to variations in lubricant distribution and delamination at angled molding areas, and inconsistent slip properties across the surface, leading to poor formability and reliability.

Method used

The exterior material incorporates a heat-sealing layer with mixed particles of different sizes, including small, medium, and large particles with specific volume average diameters, and a lubricant, which are dispersed to create convex portions and unevenness, reducing contact area with molding jigs and improving slipperiness and moldability.

Benefits of technology

This solution enhances moldability by ensuring stable and consistent slip properties, preventing particle aggregation, and maintaining particle distribution, resulting in high-quality power storage devices with improved operational reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024015166_24102024_PF_FP_ABST
    Figure JP2024015166_24102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is an exterior material for an electricity storage device, said exterior material being excellent in moldability. The present invention targets an exterior material for an electricity storage device, said exterior material including: a metal foil layer 4; a base material layer 2 provided on the outer surface side of a metal foil layer 5; and a heat welding layer 3 provided on the inner surface side of the metal foil layer 4. A seal layer 31 of the heat welding layer 3 disposed on the innermost surface side includes at least two or more types of mixed particles having different volume average particle diameters as D50 that is the 50% particle diameter of a cumulative distribution in a particle size distribution measurement by the laser diffraction scattering method. When the particle diameters are counted from the smaller one in the cumulative distribution of the mixed particles, D10 that is the 10% particle diameter of the cumulative distribution is 2 μm or less, D90 that is the 90% particle diameter of the cumulative distribution is 6 μm or more, only one peak is included in the range of D10 to D90 in the particle size distribution of the mixed particles, and a peak value in the particle size distribution of the mixed particles is 1 μm to 10 μm.
Need to check novelty before this filing date? Find Prior Art

Description

Exterior materials for energy storage devices

[0001] The present invention relates to an exterior packaging material for electricity storage devices such as batteries and capacitors used in mobile devices such as smartphones and tablet terminals, and batteries and capacitors used for storing electricity in hybrid vehicles, electric vehicles, wind power generation, solar power generation, and nighttime electricity.

[0002] In recent years, as mobile devices such as smartphones and tablet terminals have become thinner and lighter, laminates consisting of a heat-resistant resin layer (substrate layer), an adhesive layer, a metal foil layer (barrier layer), an adhesive layer, and a thermoplastic resin layer (heat-sealing layer) have been used as the exterior materials for the lithium-ion secondary batteries, lithium polymer secondary batteries, lithium-ion capacitors, and electric double-layer capacitors used in these devices, instead of conventional metal cans. Furthermore, power sources for electric vehicles, large power sources for energy storage applications, capacitors, and the like are increasingly being packaged with laminates (exterior materials) having the above-described configuration. When forming exterior materials for energy storage devices, the laminates are cold-formed, such as by stretch molding or deep drawing, into a three-dimensional shape, such as a roughly rectangular parallelepiped shape. Forming the laminate into such a three-dimensional shape ensures that a storage space for the main body of the energy storage device can be secured. Therefore, improving formability is preferable to secure a highly accurate storage space.

[0003] For example, the packaging material for an electricity storage device disclosed in Patent Document 1 listed below ensures good moldability by adding a lubricant to the exposed surface of the inner layer (thermal adhesive layer) to improve slipperiness.

[0004] Furthermore, the exterior packaging material for an electricity storage device shown in Patent Document 2 listed below has an appropriate adjustment of the centerline average roughness (Ra) by phase-separating the exposed surface of the heat-sealing layer or by adding fine particles to the layer on the exposed surface, thereby ensuring good formability.

[0005] Patent No. 3774163 Patent No. 5380762

[0006] However, in the conventional exterior packaging material for an electricity storage device shown in Patent Document 1, the layer on the surface to which the lubricant is added is a surface layer that is easily transferred, so the amount of lubricant present changes during use, causing variations in slipperiness and making it impossible to obtain stable, good formability. Furthermore, delamination is likely to occur in areas where molding is performed at angles that are nearly right angles, such as the inside corners of the molding part, and this also makes it impossible to obtain good formability.

[0007] Furthermore, in the conventional exterior material for an electricity storage device shown in Patent Document 2, unevenness such as undulations is required over a wide range of the exposed surface. However, merely adjusting the center line average roughness (Ra) improves the slipperiness partially, but it is not possible to obtain uniform slipperiness over the entire area, and there is a problem in that stable and good formability cannot be obtained.

[0008] The preferred embodiments of the present invention have been made in light of the above and / or other deficiencies in the related art, and provide significant improvements over existing methods and / or apparatus.

[0009] The present invention has been made in view of the above-mentioned problems, and has an object to provide an exterior packaging material for an electricity storage device that can achieve stable and favorable formability.

[0010] Other objects and advantages of the present invention will be apparent from the following preferred embodiments.

[0011] In order to solve the above problems, the present invention comprises the following means.

[0012] [1] An exterior packaging material for an electricity storage device, comprising a metal foil layer, a resin base layer provided on the outer surface side of the metal foil layer, and a thermoplastic resin heat-sealing layer provided on the inner surface side of the metal foil layer, wherein the seal layer arranged on the innermost side of the heat-sealing layer contains at least two or more types of mixed particles having different volume average particle diameters as D50, which is the 50% particle diameter of a cumulative distribution, in particle size distribution measurement by a laser diffraction scattering method, wherein in the cumulative distribution of the mixed particles, counting from the smaller particle diameters, D10, which is the 10% particle diameter of the cumulative distribution, is 2 μm or less and D90, which is the 90% particle diameter of the cumulative distribution, is 6 μm or more, the particle size distribution of the mixed particles includes only one peak in the range of D10 to D90, and the peak value in the particle size distribution of the mixed particles is 1 μm to 10 μm.

[0013] [2] The exterior packaging material for an electricity storage device according to item 1, wherein the mixed particles include small particles, medium particles, and large particles that are incompatible particles with three distributions of different volume average particle diameters, the small particles having a volume average particle diameter of 0.05 μm to 5 μm, the medium particles having a volume average particle diameter of 3 μm to 8 μm, and the large particles having a volume average particle diameter of 7 to 15 μm.

[0014] [3] The packaging material for an electricity storage device according to item 1 or 2, wherein the sealing layer has a weight content of the mixed particles of 3,000 ppm to 20,000 ppm.

[0015] [4] The packaging material for an electricity storage device according to any one of items 1 to 3, wherein the sealing layer has a thickness of 5 μm or more.

[0016] [5] The exterior packaging material for an electricity storage device according to any one of items 1 to 4, wherein the mixed particles have an aspect ratio of 0.2 to 1.

[0017] [6] The packaging material for an electricity storage device according to any one of items 1 to 5, wherein the sealing layer contains a lubricant.

[0018] [7] The packaging material for an electricity storage device according to any one of items 1 to 6, wherein the packaging material satisfies the relational expression (D90-D10) / D50=0.5 to 5.

[0019] [8] A film used for a heat-sealing layer in the packaging material for an electricity storage device according to any one of items 1 to 7 above, wherein a portion corresponding to the sealing layer is formed of a resin layer containing the mixed particles.

[0020] [9] A method for producing a film used for a heat-sealing layer in the packaging material for an electricity storage device according to any one of items 1 to 7 above, wherein a portion corresponding to the sealing layer is formed by a resin layer containing the mixed particles.

[0021]

[10] An electricity storage device comprising: an electricity storage device main body; and the exterior material according to any one of items 1 to 7, wherein the electricity storage device main body is exterior-packaged with the exterior material.

[0022] According to the packaging material for an electricity storage device of invention [1], mixed particles with different particle sizes are added to the sealing layer on the inner surface side of the heat-sealing layer, so that large and small convex portions can be formed, and further, the mixed particles can be measured as particles having one peak within the conditions at a certain particle size distribution width in the particle size distribution measurement results, so that aggregation of the mixed particles is unlikely to occur, and each particle is dispersed one by one on the inner surface of the heat-sealing layer, so that convex portions can be formed without bias, and the contact area with the molding jig such as a mold can be reduced during molding, so that slipperiness can be improved, and stable and good moldability can be obtained.

[0023] According to the exterior packaging material for an electricity storage device of invention [2], the sealing layer contains small particles, medium particles, and large particles with specified particle sizes, which makes it easier to blend mixed particles with a desired particle size distribution, and enables the formation of targeted irregularities on the inner surface of the heat-sealing layer, making it possible to further reduce the contact area with the molding jig during molding, thereby further improving moldability.

[0024] According to the packaging material for an electricity storage device of invention [3], the content of the mixed particles in the sealing layer is specified, so that the mixed particles can be appropriately dispersed and arranged in a balanced manner within the sealing layer, and desired irregularities can be formed on the inner surface of the heat-sealing layer, thereby further improving moldability.

[0025] According to the packaging material for an electricity storage device of invention [4], the thickness of the sealing layer is specified, so that the mixed particles can be firmly fixed to the sealing layer in a stable state, and problems such as the mixed particles falling off can be prevented, thereby more reliably improving the moldability.

[0026] According to the exterior packaging material for an electricity storage device of invention [5], the aspect ratio of the mixed particles is specified, so that convex portions can be sufficiently formed regardless of the direction in which the mixed particles are tilted, and falling off is less likely to occur, thereby further improving formability.

[0027] According to the packaging material for an electricity storage device of invention [6], since the sealing layer contains a lubricant, the lubricant precipitates and appears on the inner surface of the heat-sealing layer when the temperature reaches a certain level or higher, thereby further improving the slipperiness and further improving the formability.

[0028] According to the packaging material for an electricity storage device of invention [7], the relational expression (D90-D10) / D50=0.5 to 5 is satisfied, and therefore the volume distribution of the mixed particles can be made broader more reliably, and the moldability during molding can be further improved.

[0029] According to the film for a heat-sealing layer of the packaging material for an electricity storage device of the invention [8], the packaging material of the invention can be reliably produced using the film.

[0030] According to the method for producing a film for a heat-sealing layer of an exterior packaging material for an electricity storage device of the invention [9], the exterior packaging material of the invention can be produced reliably.

[0031] According to the invention

[10] , since the exterior material having excellent sliding properties against the molding jig is provided, it is possible to provide a high-quality electricity storage device with high operational reliability.

[0032] FIG. 1 is a cross-sectional view showing an exterior material for an electricity storage device according to an embodiment of the present invention. FIG. 2 is a schematic cross-sectional view illustrating a heat-sealing layer of an exterior material for an electricity storage device according to an embodiment. FIG. 3 is a graph showing the particle size distribution of each particle and the entire mixed particles according to an embodiment. FIG. 4 is a graph showing the particle size distribution and cumulative distribution of mixed particles according to an embodiment. FIG. 5 is a graph illustrating a peak value in the particle size distribution of mixed particles according to an embodiment. FIG. 6 is a schematic cross-sectional view illustrating a sealing layer in which a lubricant is precipitated in a heat-sealing layer according to an embodiment. FIG. 7 is a cross-sectional view showing an electricity storage device manufactured using an exterior material according to an embodiment. FIG. 8 is an exploded perspective view showing an electricity storage device according to an embodiment.

[0033] Fig. 1 is a cross-sectional view showing an electrical storage device packaging material according to an embodiment of the present invention. As shown in the figure, this electrical storage device packaging material 1 includes a metal foil layer 4 made of metal foil, a base layer 2 made of heat-resistant resin and provided on the outer surface of the metal foil layer 4 as an outer layer, an adhesive layer 5 provided on the inner surface of the metal foil layer 4, and a heat-sealing layer (sealant layer) 3 made of heat-sealing resin and provided on the inner surface of the adhesive layer 5 as an inner layer.

[0034] In this specification, when describing the position of each layer constituting the battery packaging material in terms of direction (upward in Figure 1), the direction of the base material layer 2 is referred to as the outside, and the direction of the heat-sealing layer 3 (downward in Figure 1) is referred to as the inside.

[0035] The substrate layer 2 is preferably made of a polyamide resin, a polyester resin, a polyolefin resin, a polyimide resin, or the like, and can be formed as a coating or film. It is particularly preferable to use a biaxially oriented film of the above resin for the substrate layer 2, and particularly, a biaxially oriented polyamide film or a biaxially oriented polyester film is preferably used. Among these, the biaxially oriented polyamide film is not particularly limited, but suitable examples include biaxially oriented nylon 6 film, biaxially oriented nylon 6,6 film, and biaxially oriented MXD nylon film. Suitable polyester films include biaxially oriented polybutylene terephthalate (PBT) film, biaxially oriented polyethylene terephthalate (PET) film, and biaxially oriented polyethylene naphthalate (PEN) film.

[0036] Furthermore, as the heat-resistant resin constituting the base material layer 2, it is preferable to use a thermoplastic resin having a melting point of 10° C. or higher, more preferably 20° C. or higher, relative to the heat-sealable resin constituting the heat-sealable layer 3. The thickness of the base material layer 2 is preferably set to 9 μm to 50 μm.

[0037] The metal foil layer 4 can be made of a single metal foil such as aluminum (Al) foil, copper (Cu) foil, stainless steel (SUS) foil, titanium (Ti) foil, or nickel (Ni) foil, or a clad material made by bonding two or more metals together. The thickness of the metal foil layer 4 is preferably set to 20 μm to 150 μm. That is, if the thickness is too thin, there is a risk of reduced durability due to pinholes, etc., and conversely, if the thickness is too thick, there is a risk of reduced formability.

[0038] It is preferable to form a base layer on at least one of the inner and outer surfaces of the metal foil layer 4, particularly on the surface on the thermal adhesive layer 3 side (inner surface).

[0039] The underlayer can be formed by coating a silane coupling agent or by chemical conversion treatment such as chromate treatment, etc. The thickness of the underlayer is preferably set to 0.01 μm to 1 μm.

[0040] By forming the underlayer in this manner, the corrosion resistance of the metal foil layer 4 can be improved, and the adhesive strength with the adhesive layer 5 provided on the inner surface can be improved, thereby effectively preventing peeling of the adhesive layer 5.

[0041] When the base layer is formed using a coating obtained by chemical conversion treatment (chemical conversion treatment coating), the chemical conversion treatment coating may be selected depending on the combination with the adhesive layer 5. For example, a coating obtained by chromic acid treatment, a coating obtained by chromate phosphate treatment, a coating obtained by zinc phosphate treatment, a coating obtained by non-chromate treatment using zirconium or titanium as a metal component instead of Cr, or an oxide coating obtained by boehmite treatment can be suitably used.

[0042] The base material layer 2 is attached to the outer surface of this metal foil layer 4, if necessary via an adhesive, to form an integrated laminate.

[0043] An adhesive layer formed from a two-component curing adhesive can be suitably used as the adhesive for bonding the base layer 2 and the metal foil layer 4, and as the adhesive between films when the base layer 2 is formed from multiple films. For example, a two-component curing adhesive can be used, which is composed of a first component (base material) made of one or more polyols selected from the group consisting of polyurethane polyols, polyester polyols, polyether polyols, and polyester urethane polyols, and a second component (curing agent) made of an isocyanate. The thickness of this adhesive is preferably set to 2 μm to 5 μm.

[0044] The adhesive layer 5 provided on the inner surface of the metal foil layer 4 is preferably an adhesive containing one or more of polyurethane resin, acrylic resin, epoxy resin, polyolefin resin, elastomer resin, fluorine resin, or acid-modified polypropylene resin, and is particularly preferably an adhesive made of a polyurethane composite resin containing acid-modified polyolefin as the main component. The thickness of the adhesive layer 5 is preferably set to 2 μm to 5 μm.

[0045] The adhesive layer 5 may be formed by heat lamination using a modified polyolefin (for example, acid-modified polypropylene). In this case, the preferred thickness is 10 μm to 30 μm.

[0046] Examples of thermoplastic resins constituting the heat-sealable layer 3 include polyethylene-based resins such as LDPE (low-density polyethylene), LLDPE (linear low-density polyethylene), HDPE (high-density polyethylene), and polyethylene-based copolymers; polypropylene-based resins such as rPP (random polypropylene), bPP (block polypropylene), hPP (homopolypropylene), and polypropylene-based copolymers; polybutene-based copolymers; and ionomers. Among these, polypropylene-based resins are preferred because of their electrolyte resistance, water resistance, and oxygen barrier resistance. Furthermore, from the viewpoint of ease of handling, a film form is preferred, and unstretched polypropylene films such as CPP (cast polypropylene) and IPP (inflated polypropylene) are particularly preferred.

[0047] 2 is a cross-sectional view showing the heat-sealing layer 3 in the packaging material 1 of this embodiment. As shown in Fig. 1 and Fig. 2, in this embodiment, the heat-sealing layer 3 is composed of a three-layer laminate including a sealing layer 31 arranged on the innermost side, an outer layer 33 also called a metal foil side layer, a laminate layer, etc. arranged on the outermost side, and an intermediate layer 32 arranged between the sealing layer 31 and the outer layer 33.

[0048] In the present invention, the thermal adhesive layer 3 is not limited to three layers, and may be a single layer, two layers, or four or more layers. However, in the present invention, when the thermal adhesive layer 3 has a laminated structure, it is easier to form a desired laminated structure when it is a multi-layer structure.

[0049] Furthermore, in the present invention, it is not necessary to change the resin for each layer; for example, the resin of the innermost layer to which mixed particles are added and the resin of the adjacent layer to which mixed particles are not added may be the same type of resin, and the sealing layer 31, intermediate layer 32, and outer layer 33 may be constructed using this resin.

[0050] As mentioned above, the film for the heat-sealable layer 3 may be a single layer or a multilayer. However, considering heat-sealability, delamination resistance, and insulation properties, it is preferable to form it from a multilayer film such as a coextruded product. For example, in this embodiment, a three-layer coextruded CPP film in which an rPP layer is disposed on both sides of an hPP or bPP layer can be preferably used. In the heat-sealable layer 3 made of this three-layer coextruded CPP film, the middle hPP or bPP layer is configured as the intermediate layer 32, one of the rPP layers on both sides (inner and outer surfaces) is configured as the sealing layer 31, and the other rPP layer is configured as the outer layer 33.

[0051] In this embodiment, the thickness of the entire heat-sealing layer 3 is preferably set to 20 μm to 120 μm. The thickness of the sealing layer 31 is preferably set to 5 μm or more, more preferably 10 μm or more, and even more preferably 20 μm or more. In other words, when the thickness of the sealing layer 31 is specified within this range, the mixed particles contained in the sealing layer 31, which will be described later, can be reliably held in the sealing layer in a stable state, and problems such as the mixed particles falling off can be reliably prevented.

[0052] In this embodiment, the sealing layer 31 contains, as mixed particles, three types of particles M1 to M3 that are incompatible with each other, that is, incompatible particles that are immiscible with each other.

[0053] The mixed particles M1 to M3 can be made of metal oxides, resin beads, etc. Specific examples that can be used include silica, alumina, calcium carbonate, barium carbonate, titanium oxide, aluminum silicate, talc, kaolin, acrylic resin beads, polyethylene resin beads, and polyethylene elastomer. It is preferable that the mixed particles M1 to M3 be made by combining two or more of the above-mentioned particles. Using particles of two or more different compositions makes it less likely for the mixed particles to aggregate due to van der Waals forces, allowing the mixed particles to be dispersed within the sealing layer 31 and forming appropriate unevenness.

[0054] The content of the mixed particles M1 to M3 in the sealing layer 31 is preferably set to 3,000 ppm to 20,000 ppm by weight, and more preferably 7,000 ppm to 18,000 ppm by weight. In other words, when the content of the mixed particles M1 to M3 is set within this range, the mixed particles M1 to M3 can be appropriately dispersed and arranged in a well-balanced manner within the sealing layer 31, and the desired unevenness can be formed on the inner surface of the heat-sealing layer 3.

[0055] In this embodiment, the mixed particles (incompatible particles) contained in the sealing layer 31 are composed of three types of particles with different volume average particle diameters (median diameters), which are the 50% particle diameter D50 of the cumulative distribution, namely, small particles M1, medium particles M2, and large particles M3.

[0056] The sealing layer 31 contains small particles M1, medium particles M2, and large particles M3 of different sizes, and is arranged so that a portion of each particle M1 to M3 protrudes inward (toward the bottom of the figures) from the inner surface (the lower surface of Figures 1 and 2) of a resin component such as rPP, and the inner surface of the sealing layer 31 is uneven.

[0057] The small particles M1 preferably have a volume average particle size (D50) of 0.05 μm to 5 μm, more preferably 0.5 μm to 3 μm.

[0058] The medium particles M2 preferably have a volume average particle size (D50) of 3 μm to 8 μm, more preferably 4 μm to 7 μm.

[0059] The large particles M3 preferably have a volume average particle size (D50) of 7 μm to 15 μm, more preferably 8 μm to 13 μm.

[0060] In this embodiment, the sealing layer 31 contains three types of particles M1 to M3 with different particle diameters D50. The small particles M1 and large particles M3 broaden the particle size distribution, and the medium particles M2 combine them into a single distribution. This allows particles of each size to be dispersed throughout, contributing to the formation of unevenly distributed convex portions of various sizes. This reduces the contact area with a mold such as a molding jig when molding the exterior material 1, improves slipperiness, and ensures stable and favorable moldability.

[0061] Furthermore, if particles of the same size are mixed in place of particles of different sizes, the size of the convex portions will be uniform, which may result in a monotonous surface shape, which may result in a decrease in slipperiness and formability, or the convex portions may cause the exterior material 1 to be molded.

[0062] In addition, in this embodiment, the small particles M1 can form fine irregularities on the surface (inner surface) of the heat-sealing layer 3, which can suppress adhesion to a mold when molding the packaging material 1.

[0063] Furthermore, the large particles M3 can reliably form convex portions (protrusions) on the inner surface of the heat-sealing layer 3, thereby reducing the dynamic frictional force with the mold when molding the packaging material 1.

[0064] Furthermore, the medium particles M2 form small convex portions on the inner surface of the heat-sealing layer 3 and prevent the convex portions from being unevenly distributed, thereby further enhancing the effects of the small particles M1 and large particles M3.

[0065] Furthermore, in this embodiment, by specifying the particle diameter (D50) of each of the particles M1 to M3 within the above range, it becomes easier to blend mixed particles having a desired particle size distribution, and it is possible to form the desired unevenness on the inner surface of the heat-sealing layer 3, and it is possible to further reduce the contact area with the mold when molding the packaging material 1, etc., and it is possible to further improve moldability.

[0066] Furthermore, in this embodiment, when the content of the mixed particles is specified within the above range, or when the thickness of the sealing layer 31 is specified within the above range, it is possible to prevent each particle from falling off the sealing layer 31, and the effect of the convex portions can be fully exerted, thereby more reliably obtaining good moldability.

[0067] In this embodiment, the blending ratio (weight ratio) of large particles M3:medium particles M2:small particles M1 is preferably adjusted to 0.5-1.5:1-3:0.5-1.5, and more preferably 0.8-1.2:1.5-2.5:0.8-1.2. In other words, by adjusting the blending ratio within this range, the above-mentioned effects of blending particles M1 to M3 can be more reliably obtained.

[0068] 3 is a graph showing the particle size distribution of each of the small particles M1, medium particles M2, and large particles M3 in this embodiment, and the particle size distribution of a mixed particle obtained by mixing the small particles M1, medium particles M2, and large particles M3. As shown in the figure, the small particles M1 and medium particles M2 have smaller particle diameters than the large particles M3, and therefore when mixed in the same blending amount (weight or volume) as the large particles M3, the particle amount (number of particles), which is the amount present in the particle size distribution, becomes larger.

[0069] In the present invention, the particle size distribution and cumulative distribution are measured based on the laser diffraction method (laser diffraction scattering method).

[0070] In this embodiment, the mixed particles are described using three types of particles M1 to M3 with different volume average particle sizes (D50), but this is not limited thereto. As long as the mixed particles satisfy the particle size distribution conditions, the present invention may use at least two types of particles with different volume average particle sizes (D50). For example, the mixed particles may be made of two types of particles, small particles M1 and medium particles M2, or two types of particles, small particles M1 and large particles M3. Furthermore, the mixed particles may be made of four or more types of particles with different volume average particle sizes (D50).

[0071] 4 is a graph showing the particle size distribution and cumulative distribution of the mixed particles according to this embodiment. As shown in the figure, the particle size distribution of the mixed particles, counting from the smallest particle size, contains only one peak (mountain) within the range of 10% particle size (D10) to 90% particle size (D90) of the cumulative distribution, and there are no two or more peaks within that range.

[0072] Here, the present invention relates to a particle size distribution of mixed particles that contains only one peak within the range of D10 to D90, and even if there is a peak outside the range of D10 to D90, the peak outside that range is irrelevant to the present invention. For example, in the particle size distribution in Figure 5, a peak exists at a position below D10, but this peak is not counted in the present invention. In other words, the particle size distribution in the figure contains only one peak within the range of D10 to D90, and is therefore subject to the present invention.

[0073] In this embodiment, the cumulative distribution of the mixed particles has a D10 particle size of 2 μm or more and a D90 particle size of 6 μm or more. Furthermore, in this embodiment, the mode diameter as a peak value in the particle size distribution of the mixed particles is 1 μm to 10 μm.

[0074] In this embodiment, the D10 and D90 particle sizes and the mode diameter are specified to the above values, so that the mixed particles as a whole can have one broad distribution that is not sharp, and convex portions of the particles M1 to M3 can be formed by uniformly dispersing them without bias on the inner surface of the heat-sealing layer 3. Therefore, when molding the packaging material 1, stress concentration on the mold is less likely to occur, improving the slipperiness and further increasing the moldability.

[0075] In this embodiment, it is preferable to satisfy the relationship (D90 - D10) / D50 = 0.5 to 5, and more preferably the relationship (D90 - D10) / D50 = 1.5 to 3. In other words, when this relationship is satisfied, the volume distribution of the mixed particles as a whole can be more reliably made broad, and irregularities of various sizes can be provided, thereby further improving the moldability of the exterior packaging material 1 when it is molded.

[0076] Furthermore, in this embodiment, it is preferable to employ particles M1 to M3 constituting the mixed particles each having an aspect ratio (minor axis / major axis) of 0.2 to 1. In other words, in this case, the particles form a uniform mass, so that no matter in which direction the particles M1 to M3 are tilted, convex portions can be sufficiently formed, and falling off is unlikely to occur, thereby enabling more reliable improvement in formability when molding the exterior packaging material 1.

[0077] In this embodiment, it is preferable that the sealing layer 31 of the heat-sealing layer 3 contains a lubricant.

[0078] Examples of the lubricant include saturated fatty acid amides, unsaturated fatty acid amides, substituted amides, methylol amides, saturated fatty acid bisamides, unsaturated fatty acid bisamides, fatty acid ester amides, and aromatic bisamides.

[0079] More specifically, examples of saturated fatty acid amides include lauric acid amide, palmitic acid amide, stearic acid amide, behenic acid amide, and hydroxystearic acid amide.

[0080] Further, examples of unsaturated fatty acid amides include oleic acid amide and erucic acid amide.

[0081] Further, examples of substituted amides include N-oleyl palmitic acid amide, N-stearyl stearic acid amide, N-stearyl oleic acid amide, N-oleyl stearic acid amide, and N-stearyl erucic acid amide.

[0082] Further, examples of methylol amides include methylol stearic acid amide.

[0083] Further examples of saturated fatty acid bisamides include methylene bisstearic acid amide, ethylene biscapric acid amide, ethylene bislauric acid amide, ethylene bisstearic acid amide, ethylene bishydroxystearic acid amide, ethylene bisbehenic acid amide, hexamethylene bisstearic acid amide, hexamethylene bisbehenic acid amide, hexamethylene hydroxystearic acid amide, N,N'-distearyl adipic acid amide, and N,N'-distearyl sebacic acid amide.

[0084] Further, examples of unsaturated fatty acid bisamides include ethylene bisoleic acid amide, ethylene biserucic acid amide, hexamethylene bisoleic acid amide, N,N'-dioleyl adipamide, and N,N'-dioleyl sebacic acid amide.

[0085] Further, an example of the fatty acid ester amide is stearamidoethyl stearate.

[0086] Examples of aromatic bisamides include m-xylylene bisstearic acid amide, m-xylylene bishydroxystearic acid amide, and N,N'-cystearyl isophthalic acid amide.

[0087] The amount of lubricant deposited on the inner surface of the heat-sealing layer 3 is 0.1 μg / cm 2 ~1 μg / cm 2 (0.1 μg / cm 2 and 1 μg / cm 2 It is preferable to adjust the lubricant content to a value including the amount of lubricant precipitated. If the amount of lubricant precipitated is too small, it may not be possible to obtain good slip properties, which is not preferable. Conversely, if the amount of lubricant precipitated is too large, it may increase the frequency of occurrence of white powder and equipment contamination due to the lubricant, which is not preferable.

[0088] As shown in FIG. 6, the inner surface of the heat-sealing layer 3 is formed into an uneven structure by the particles M1 to M3, so that excessive precipitation of the lubricant on the inner surface of the heat-sealing layer 3 is suppressed, and at a predetermined temperature or higher, an appropriate amount of lubricant is precipitated, and the inner surface of the heat-sealing layer 3 is covered with a lubricant layer 6 of the lubricant, thereby further improving the slipperiness against the molding jig.

[0089] Furthermore, when the packaging material 1 of this embodiment is wound up, for example, into a roll, the heat-sealing layer 3 comes into contact with the outermost layer, such as the base material layer 2, and the positions of the convex portions of each of the particles M1 to M3 come into preferential contact with other parts (such as the base material layer 2), thereby making it possible to suppress the amount of lubricant transferred to other parts.

[0090] In the present invention, in order to further improve the slipperiness during molding, a substrate protective layer formed of a binder resin containing fine particles may be provided on the outer side of the substrate layer 2. The fine particles may be the incompatible particles used as the mixed particles in this embodiment, and the binder resin may be a urethane resin, an acrylic resin, an acrylic urethane resin, a fluorine-based resin, or the like.

[0091] The exterior material 1 for an electricity storage device of this embodiment configured as described above is used as an exterior case for an electricity storage device either in sheet form or, if necessary, formed into a predetermined shape by thermoforming such as deep drawing or stretch forming.

[0092] 7 and 8 are a cross-sectional view and an exploded perspective view showing an electricity storage device 30 manufactured using the exterior material 1 of this embodiment. As shown in both figures, this electricity storage device 30 is a lithium-ion secondary battery. In this embodiment, an exterior case 15 is configured by a tray member 14 obtained by molding the exterior material 1 and a lid member 10 made of a planar (sheet-like) exterior material 1. A substantially rectangular parallelepiped electricity storage device main body 35 (electrochemical element, etc.) is accommodated in an accommodation recess of the tray member 14 obtained by molding the exterior material 1 of the present invention. The lid member 10 (exterior material 1) of the present invention is placed on top of the electricity storage device main body 35 with its heat-sealing layer 3 facing inward (lower). The outer peripheral edge of the heat-sealing layer 3 of the lid member 10 and the heat-sealing layer 3 of the flange portion (sealing peripheral portion) 29 of the tray member 14 are heat-sealed and sealed to form the electricity storage device 30. The inner surface of the receiving recess of the tray member 14 is the heat-sealing layer 3, and the outer surface of the receiving recess faces the base layer 2.

[0093] 7, reference numeral "39" denotes a heat-sealed portion where the outer peripheral edge of the cover member 10 and the flange portion (sealing peripheral portion) 29 of the tray member 14 are joined (welded) together. In the electricity storage device 30, the tip end of the tab lead connected to the electricity storage device main body 35 is led out of the exterior case 15, but is not shown in the drawing.

[0094] The energy storage device 30 manufactured using the exterior material 1 of this embodiment has an exterior material 1 that has excellent slip resistance against the molding die and high adhesive strength between the heat-sealing layer 3 and the adhesive layer 5, and therefore has high operational reliability and can reliably provide a high-quality energy storage device product.

[0095] The power storage device main body 35 is not particularly limited, but examples thereof include a battery main body, a capacitor main body, and a condenser main body.

[0096] In the above embodiment, the outer case 15 is composed of a tray member 14 obtained by molding the outer case material 1 and a planar lid member 10, but the present invention is not particularly limited to such a combination. For example, the outer case 15 may be composed of a pair of planar (sheet-like) outer case materials 1, or may be composed of a pair of tray members 14 stacked opposite each other.

[0097]

[0098]

[0099] 1. Preparation of Film for Heat-Sealing Layer Example 1 As shown in Tables 1 and 2, a film for the heat-sealing layer 3 of Example 1 in the packaging material 1 for an electricity storage device was produced. That is, as the film for the heat-sealing layer 3, a CPP film was produced by laminating a 16 μm thick rPP for the sealing layer, a 48 μm thick bPP for the intermediate layer, and a 16 μm thick rPP for the outer layer by three-layer co-extrusion using a T-die.

[0100] In the film for the heat-sealing layer of Example 1, 3000 ppm of silica particles having an average particle size of 1.5 μm were added to the sealing layer 31 as small particles M1, 6000 ppm of silica particles having an average particle size of 6 μm as medium particles M2, and 3000 ppm of HDPE (high-density polyethylene) particles having an average particle size of 12 μm as large particles M3.

[0101] As shown in Table 2, for the mixed particles M1 to M3 added to the sealing layer 31, the 10% particle size (D10) was 0.8 μm, the 50% particle size (D50) was 3.8 μm, the 90% particle size was 8.2 μm, (D90-D10) / D50 was 1.9, the aspect ratio was 0.8, the number of peaks in the range of D10 to D90 in the volume distribution was one, and the peak position was 4.1 μm.

[0102] The particle size distribution of the mixed particles was measured using a laser diffraction method. Specifically, a Microtrac MT3000II was used as the device, and the measurement conditions were a measurement range of 0.02 μm to 2000 μm, a measurement time of 30 seconds, two measurements, methanol (refractive index 1.33) as the solvent, and non-spherical particles (refractive index 1.54).

[0103] The aspect ratio of each particle was measured using FPIA-3000 manufactured by Sysmex Corporation.

[0104] Examples 2 to 17 The resins for the seal layer, the resin for the intermediate layer and the resin for the outer layer shown in Tables 1 and 2 were laminated in the same manner as in Example 1 above to prepare films for the heat-sealable layer of Examples 2 to 17.

[0105] Examples 18 and 19 Using the resins for the seal layer shown in Tables 1 and 4, single-layer unstretched films were produced using a T-die to form heat-sealable films for Examples 18 and 19.

[0106] Comparative Examples 1 to 4 Films for heat-sealing layers were prepared by laminating the resins for the seal layer, the resin for the intermediate layer, and the resin for the outer layer shown in Tables 1 and 2 in the same manner as in Example 1. In the mixed particles of Comparative Example 1, the number of peaks within the range of D10 to D90 of the volume distribution was two, and the respective peak positions were 1.9 μm and 9.3 μm.

[0107] 2. Fabrication of an exterior material for an electricity storage device A chemical conversion treatment solution consisting of phosphoric acid, polyacrylic acid (acrylic resin), a chromium (III) salt compound, water, and alcohol was applied to both sides of a 40 μm thick aluminum foil (A8021-O) serving as the metal foil layer 4, and then dried at 180° C. to form a chemical conversion coating. The chromium deposition amount of this chemical conversion coating was 10 mg / m per side. 2 It was.

[0108] Next, a 15 μm-thick biaxially oriented 6 nylon (ONy) film was dry laminated (attached) to one surface (outer surface) of the chemically treated aluminum foil (metal foil layer 4) via a two-component curing urethane adhesive (3 μm) as the base material layer 2.

[0109] Next, the outer surface of the outer layer of the CPP film for the heat-sealing layer prepared in the above Examples and Comparative Examples was superimposed on the other surface (inner surface) of the dry-laminated aluminum foil (metal foil layer) via a two-component curing adhesive (2 μm) of maleic acid-modified polypropylene resin and isocyanate, and dry-laminated by being sandwiched and pressed between a rubber nip roll and a laminating roll heated to 100° C. Thereafter, the resultant was aged at 40° C. for 10 days to obtain exterior packaging materials (laminates) of the Examples and Comparative Examples as samples.

[0110] 3. Evaluation test for each exterior material

[0111]

[0112] <Moldability test> Each of the packaging materials of the Examples and Comparative Examples was cut into a predetermined size to prepare a packaging material test piece, which was then subjected to a deep drawing test using a deep drawing mold within an area of ​​55 mm length x 35 mm width, while increasing the forming height (drawing depth) in 0.5 mm increments. The gauge pressure of the wrinkle holding pressure during this forming was 0.475 MPa, and the actual pressure (calculated value) was 0.7 MPa.

[0113] It was visually confirmed using transmitted light whether pinholes were generated at the corners of the drawn recesses during this molding.

[0114] Then, samples in which pinholes were observed at a molding depth of 7 mm or more were evaluated as "◎", samples in which pinholes were observed at a molding depth of 6 mm or more but less than 7 mm were evaluated as "◯", samples in which pinholes were observed at a molding depth of 5 mm or more but less than 6 μm were evaluated as "△", and samples in which pinholes were observed at a molding depth of less than 5 mm were evaluated as "×". In this example, "◎", "◯", and "△" were considered to be acceptable. The results are shown in Table 3.

[0115] <Lamination Strength (Sealing Property) Test> Each packaging material of the Examples and Comparative Examples was cut into a 15 mm wide strip, and the peel strength between the metal foil layer and the heat-sealing layer was measured in accordance with JIS K6854-3 (1999). Peel strengths of 4.0 N / 15 mm or more were evaluated as "◎", 3.0 N / 15 mm or more but less than 4.0 N / 15 mm as "○", 2.0 N / 15 mm or more but less than 3.0 N / 15 mm as "△", and less than 2.0 N / 15 mm as "×". In this evaluation, "◎", "○", and "△" were considered to be acceptable in this example. The results are shown in Table 3.

[0116] <Slipperiness Test (Dynamic Friction Coefficient)> Each of the exterior materials of the Examples and Comparative Examples was cut into a size of 80 mm x 200 mm, and the dynamic friction coefficient was measured in accordance with JIS K 7125. The measurement conditions were a low cell weight of 100 N and a weight of 200 g (including the weight of the sliding piece). The results of the dynamic friction coefficient are shown in Table 3.

[0117] <General Comments> As shown in Table 3, although the results of the exterior packaging materials of the examples varied to some extent, all of the examples were evaluated as having no problems and met the pass standard.

[0118] In contrast, the packaging materials of Comparative Examples 1 to 4, which deviate from the gist of the present invention, were evaluated as being inferior in any one of moldability, sealing property, and slip property.

[0119] This application claims priority from Japanese Patent Application No. 2023-67332, filed on April 17, 2023, the disclosure of which is incorporated herein by reference in its entirety.

[0120] It should be understood that the terms and expressions used herein are used for the purpose of explanation and not for limiting interpretation, and do not exclude any equivalents of the features shown and described herein, but also allow various modifications within the claimed scope of the present invention.

[0121] The exterior packaging material for an electricity storage device of the present invention can be suitably used when producing electricity storage devices such as batteries and capacitors used in mobile devices such as smartphones and tablets, and batteries and capacitors used in hybrid vehicles, electric vehicles, wind power generation, solar power generation, and storing night-time electricity.

[0122] 1: Exterior material 2: Base material layer 3: Heat-sealing layer 30: Electricity storage device 31: Sealing layer 35: Device body 4: Metal foil layer 6: Lubricant layer M1: Small particles M2: Medium particles M3: Large particles

Claims

1. An exterior material for an electricity storage device comprising a metal foil layer, a resin base layer provided on the outer surface side of the metal foil layer, and a thermoplastic resin heat-sealing layer provided on the inner surface side of the metal foil layer, wherein the seal layer arranged on the innermost side of the heat-sealing layer contains at least two or more types of mixed particles having different volume average particle diameters as D50, which is the 50% particle diameter of a cumulative distribution, in particle size distribution measurement by a laser diffraction scattering method, wherein in the cumulative distribution of the mixed particles, counting from the smaller particle diameter, D10, which is the 10% particle diameter of the cumulative distribution, is 2 μm or less and D90, which is the 90% particle diameter of the cumulative distribution, is 6 μm or more, the particle size distribution of the mixed particles includes only one peak in the range of D10 to D90, and the peak value in the particle size distribution of the mixed particles is 1 μm to 10 μm.

2. The exterior material for an electricity storage device according to claim 1, wherein the mixed particles include small particles, medium particles and large particles which are incompatible particles having three different volume average particle diameters, the volume average particle diameter of the small particles being 0.05 μm to 5 μm, the volume average particle diameter of the medium particles being 3 μm to 8 μm, and the volume average particle diameter of the large particles being 7 to 15 μm.

3. The exterior packaging material for an electricity storage device according to claim 1 or 2, wherein the sealing layer has a weight content of the mixed particles of 3,000 ppm to 20,000 ppm.

4. The packaging material for an electricity storage device according to any one of claims 1 to 3, wherein the sealing layer has a thickness of 5 μm or more.

5. The exterior packaging material for an electricity storage device according to any one of claims 1 to 4, wherein the mixed particles have an aspect ratio of 0.2 to 1.

6. The packaging material for an electricity storage device according to any one of claims 1 to 5, wherein the sealing layer contains a lubricant.

7. The exterior packaging material for an electricity storage device according to any one of claims 1 to 6, which satisfies the relational expression (D90-D10) / D50=0.5 to 5.

8. A film for use in a heat-sealing layer in an exterior material for an electric storage device according to any one of claims 1 to 7, characterized in that the portion corresponding to the sealing layer is constituted by a resin layer containing the mixed particles.

9. A method for producing a film used for a heat-sealing layer in an exterior material for an electrical storage device according to any one of claims 1 to 7, characterized in that a portion corresponding to the sealing layer is formed by a resin layer containing the mixed particles.

10. An electricity storage device comprising: an electricity storage device main body; and an exterior material according to any one of claims 1 to 7, wherein the electricity storage device main body is exteriorly covered with the exterior material.

Citation Information

Patent Citations

  • Battery pack

    JP2014032966A

  • Sheath material for secondary battery

    JP2017004765A

  • Exterior material for power storage device, outer casing for power storage device and power storage device

    JP2019061938A

  • Sealant film for battery external material

    JP2021103679A

  • Exterior materials for energy storage devices

    JP2023017866A