Silicon-based negative electrode material, preparation method therefor and use thereof
By using acrylic copolymers, functional small molecules and conductive agents on the surface of the silicon-based negative electrode material to form an artificial SEI film, the problem of powdering and expansion of silicon oxide materials during the cycle is solved, and the battery cycle performance and capacity are improved. Retention rate.
Patent Information
- Application Number
- PCT/CN2023/090922
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-24
- Filing Date
- 2023-04-26
- Publication Date
- 2024-10-31
AI Technical Summary
Silicon oxide anode materials are prone to powdering and volume changes during cycling, resulting in battery capacity loss. Existing improvement methods such as micronization and surface coating modification have limited effects and are difficult to effectively suppress expansion and improve cycle performance.
Using acrylic copolymers, small molecule compounds containing functional groups and conductive agents, an artificial SEI film is formed on the surface of the silicon-based core to form a conductive polymer network, which enhances ion conductivity and restrains the expansion of silicon.
It significantly reduces the full-charge expansion rate of the silicon-based anode material, improves the cycle performance and service life of the battery, increases the 50-cycle capacity retention rate, and significantly reduces the full-charge expansion rate and charge transfer resistance of the pole piece.
Smart Images

Figure CN2023090922_31102024_PF_FP_ABST
Abstract
Description
A silicon-based anode material, its preparation method and application Technical Field
[0001] This application belongs to the technical field of battery materials, for example, a silicon-based anode material, its preparation method and application. Background Art
[0002] Silicon monoxide (SiO X , 0 < x < 2) is an important type of silicon-based anode material. It has a low lithium potential, a high theoretical capacity (>1500 mAh / g), and rich reserves. It is generally regarded as the next-generation anode material, and its market demand has been increasing year by year. However, silicon monoxide anode materials currently still face many challenges. First, compared with graphite materials, silicon monoxide anode materials have a poor binding ability with binders, and silicon monoxide is prone to pulverization after multiple cycles, resulting in easy loss of electrical contact between the silicon monoxide anode material and the current collector, leading to capacity loss. Second, silicon monoxide materials will undergo huge volume changes during the process of lithium deintercalation and intercalation, which will damage the original SEI film and generate a new SEI film; this will continuously consume the electrolyte in the battery, causing the battery capacity to drop suddenly.
[0003] Currently, there are two means to improve the performance of silicon monoxide anode materials. One is to micronize the anode material, and the other is to perform surface coating modification on the silicon monoxide anode material. For example, CN111584831A discloses a polymer-coated silicon / sulfur-doped graphene anode material and its preparation method. By in-situ polymerization of dopamine monomers and pyrrole monomers, a conductive polymer coating layer can be formed on the surface of the silicon anode, and this coating layer can improve the cycling performance of the silicon anode material. However, in-situ polymerization requires reaction at 5 - 12°C for 8 - 12 hours, which is not conducive to large-scale industrial production.
[0004] CN114284481A discloses a high-rate silicon oxycarbide material, its preparation method and application. The high-rate silicon oxycarbide material has a multi-layer core-shell structure, which is, from the inside to the outside, a silicon monoxide core, a conductive three-dimensional network, a porous carbon layer or a porous carbon layer containing a conductive agent, and a dense carbon layer. The silicon oxycarbide material includes a polymerized carbon layer of a high-molecular polymer, which plays a role in inhibiting expansion, reducing specific surface area, improving conductivity, and reducing side reactions of the material. However, the effect of the material in inhibiting expansion and pulverization and the cycling performance of the battery need to be further improved.
[0005] Therefore, developing a silicon-based anode material that can effectively inhibit the expansion of silicon-based materials, weaken the pulverization of silicon-based anode materials after multiple cycles, reduce the full-charge expansion of silicon-based anode materials, and improve the cycling performance of the battery is an urgent technical problem to be solved in this field.
[0006] Summary of the Invention
[0007] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.
[0008] The present application provides a silicon-based anode material, its preparation method, and its application. The silicon-based anode material is coated with an artificial SEI film on its surface, and the material of the artificial SEI film adopts a specific formulation. This can effectively inhibit the volume expansion of the silicon-based core, reduce the pulverization of the silicon-based anode material after multiple cycles, reduce the expansion of the silicon-based anode material at full charge, and improve the cycle performance of the battery.
[0009] This application adopts the following technical solutions:
[0010] In a first aspect, an embodiment of the present application provides a silicon-based negative electrode material, which includes a silicon-based core and an artificial SEI film coated on the surface of the silicon-based core; the material of the artificial SEI film includes an acrylic copolymer, a small molecule compound containing a functional group and a conductive agent; the small molecule compound has a star structure; the functional group includes at least one of a hydroxyl group, a carbonyl group, an ester group or a carboxyl group.
[0011] In the embodiment of the present application, an acrylic copolymer, a small molecule compound containing a functional group and a conductive agent are compounded and coated on the surface of the silicon-based core to form a conductive polymer network, which can act as an artificial SEI film; the small molecule compound has a star structure and can undergo cross-linking or hydrogen bonding with the acrylic copolymer, so that the one-dimensional linear polymer forms a two-dimensional network structure, which increases the stability and density of the coating network, and the small molecule compound contains functional groups and can coordinate with lithium ions to promote the conduction of lithium ions in the polymer network, thereby enhancing the ion conduction performance; the three cooperate with each other and are indispensable, effectively restraining the expansion of silicon, reducing the pulverization of the silicon-based negative electrode material after multiple cycles, having lower full-charge expansion and better cycle performance, and greatly improving the service life of the lithium-ion battery.
[0012] In one embodiment, the material of the artificial SEI film includes, by weight percentage, 55-98% acrylic copolymer (for example, 55%, 56%, 58%, 60%, 62%, 64%, 66%, 68%, 70%, 72%, 74%, 76%, 78%, 80%, 82%, 84%, 86%, 88%, 90%, 92%, 94%, 96%, 98%, etc.), 1-25% small molecule compound containing functional groups (for example, 1% , 2%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%) and 1% to 20% conductive agent (for example, it can be 1%, 2%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%).
[0013] In one embodiment, the material of the artificial SEI film includes, by weight percentage, 65-95% of an acrylic copolymer, 4-20% of a small molecule compound containing a functional group, and 1-15% of a conductive agent.
[0014] In the examples of this application, the battery exhibits improved cycling performance when the acrylic copolymer, the small molecule compound containing functional groups, and the conductive agent are within the above-defined content ranges. The content of the acrylic copolymer in the artificial SEI film refers to the effective content, i.e., the mass percentage of the acrylic copolymer solids.
[0015] In one embodiment, the raw materials for preparing the acrylic copolymer include, by weight percentage, 50-95% acrylic monomer (for example, 50%, 52%, 54%, 56%, 58%, 60%, 62%, 64%, 66%, 68%, 70%, 72%, 74%, 76%, 78%, 80%, 82%, 84%, 86%, 88%, 90%, 92%, 94%, etc.), 1-40% first monomer (for example, 1%, 2%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 28%, 30%, 32%, %, 34%, 36%, 38%, 40%, etc.) and 1-40% of a second monomer (for example, 1%, 2%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 28%, 30%, 32%, 34%, 36%, 38%, 40%, etc.).
[0016] In the embodiment of the present application, the acrylic monomer includes acrylic acid and / or methacrylic acid.
[0017] In one embodiment, the first monomer and the second monomer are each independently selected from at least one of vinyl acetate, methyl methacrylate, acrylonitrile, hydroxyethyl methacrylate, acrylamide or N-vinyl pyrrolidone; and the first monomer is different from the second monomer.
[0018] In one embodiment, the mass ratio of the acrylic monomer, the first monomer and the second monomer is (5.5-9.5):(1-3):1, wherein the specific values of (5.5-9.5) can be, for example, 5.6, 5.8, 6, 6.1, 6.2, 6.3, 6.4, 6.5, 6.6, 6.7, 6.8, 6.9, 7, 7.1, 7.2, 7.4, 7.5, 7.6, 7. 7, 7.8, 8, 8.1, 8.2, 8.5, 8.6, 8.7, 8.8, 8.9, 9, 9.2, 9.4, etc.; the specific values in (1-3) can be, for example, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3, etc.
[0019] In the embodiments of the present application, when the ratio of the acrylic monomer, the first monomer, and the second monomer is within the above-defined range, the performance of the silicon-based negative electrode material is superior. The first monomer and the second monomer are selected from the same range of types. With the weight of the first monomer and the second monomer being 100%, the first monomer refers to the monomer with the larger weight, and the second monomer refers to the monomer with the smaller weight. The weight of the first monomer may also be equal to that of the second monomer.
[0020] In the embodiment of the present application, the acrylic copolymer exists in the form of its lithium salt.
[0021] In the embodiment of the present application, the preparation method of the acrylic copolymer includes:
[0022] In the presence of a protective atmosphere, the acrylic monomer, the first monomer, the second monomer and the solvent are mixed and stirred at room temperature for 20 to 40 minutes (for example, 20 minutes, 25 minutes, 30 minutes, 35 minutes, 40 minutes, etc.) at 300 to 500 rpm (for example, 300 rpm, 350 rpm, 400 rpm, 450 rpm, 500 rpm, etc.), the temperature is raised to 70 to 80° C. (for example, 70° C., 72° C., 74° C., 76° C., 78° C., 80° C., etc.), and the temperature is kept for 20 to 40 minutes (for example, 20 minutes, 25 minutes, 30 minutes, 35 minutes, 40 minutes, etc.). After the temperature of the system stabilizes, the initiator is added, and the mixture is stirred at 70 to 80° C. (for example, 70° C., 72° C., 74° C., 76° C., 78° C., 80° C., etc.) at a speed of 300 to 500 rpm (for example, 300 rpm, 350 rpm, 400 rpm, etc.). The mixture is stirred for 3 to 7 hours (for example, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, etc.) under conditions of 400 rpm, 450 rpm, 500 rpm, etc., and then the temperature is continuously raised to 80 to 90° C. (for example, 80° C., 82° C., 84° C., 86° C., 88° C., 90° C., etc.) and stirred for 1 to 3 hours (for example, 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, etc.). Subsequently, the system is evacuated for 20 to 40 minutes (for example, 20 minutes, 25 minutes, 30 minutes, 35 minutes, 40 minutes, etc.). After cooling to room temperature, an aqueous solution containing lithium hydroxide monohydrate is slowly added and stirred for 1 to 2 hours to obtain the acrylic copolymer.
[0023] In the embodiments of the present application, the solvent includes but is not limited to at least one of water, ethanol, methanol, N,N-dimethylformamide or N-methylpyrrolidone.
[0024] In the embodiments of the present application, the initiator includes but is not limited to ammonium persulfate. The amount of the initiator used is 0.05-5% of the total weight of the monomer, for example, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, etc.
[0025] In the embodiments of the present application, the molar content of the lithium hydroxide monohydrate in the system is 0.05 to 0.15 mol, for example, it can be 0.05 mol, 0.06 mol, 0.08 mol, 0.1 mol, 0.11 mol, 0.12 mol, 0.13 mol, 0.14 mol, 0.15 mol, etc.
[0026] In one embodiment, the small molecule compound containing a functional group includes tannic acid.
[0027] In one embodiment, the conductive agent includes at least one of graphene, acetylene black, carbon black, graphite black, single-walled carbon nanotubes, or multi-walled carbon nanotubes.
[0028] In one embodiment, the mass percentage of the artificial SEI film in the silicon-based negative electrode material is 0.1-10%, for example, it can be 0.1%, 0.5%, 0.8%, 1%, 1.2%, 1.5%, 1.8%, 2%, 2.2%, 2.5%, 2.8%, 3%, 3.2%, 3.5%, 3.8%, 4%, 4.2%, 4.5%, 4.8%, 5%, 5.2%, 5.5%, 5.8%, 6%, 6.2%, 6.5%, 6.8%, 7%, 7.2%, 7.5%, 7.8%, 8%, 8.2%, 8.5%, 8.8%, 9%, 9.2%, 9.5%, 10%, etc.
[0029] In one embodiment, the silicon-based core comprises a silicon oxide core.
[0030] In one embodiment, the particle size of the silicon oxide core is 500nm to 20μm, for example, 500nm, 600nm, 800nm, 1μm, 2μm, 4μm, 6μm, 8μm, 10μm, 12μm, 14μm, 16μm, 18μm, 20μm, etc.; the specific surface area of the silicon oxide core is 0.5 to 25m 2 / g, for example, 0.5m 2 / g、1m 2 / g, 2m 2 / g、4m 2 / g、6m 2 / g、8m 2 / g、10m 2 / g、12m 2 / g、14m2 / g、16m 2 / g、18m 2 / g, 20m 2 / g、22m 2 / g、24m 2 / g, 25m 2 / g, etc.
[0031] In one embodiment, the surface of the silicon monoxide core is coated with a carbon coating layer.
[0032] In the embodiment of the present application, the carbon coating layer can be directly purchased as a carbon-coated silicon-based material, or it can be prepared by conventional methods in related technologies; methods for obtaining the carbon coating layer include but are not limited to chemical vapor deposition, asphalt sintering, etc.
[0033] In one embodiment, the thickness of the carbon coating layer is 2 to 10 nm, for example, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, etc.
[0034] In one embodiment, the silicon-based negative electrode material includes a silicon monoxide core and a carbon coating layer and an artificial SEI film sequentially coated on the surface of the silicon monoxide core.
[0035] In a second aspect, an embodiment of the present application provides a method for preparing the silicon-based negative electrode material according to the first aspect, the preparation method comprising the following steps:
[0036] The acrylic copolymer, the small molecule compound containing a functional group and the conductive agent are mixed with the silicon-based core, and dried to obtain the silicon-based negative electrode material.
[0037] In one embodiment, the mixing is performed in a solvent; the solvent comprises at least one of water, ethanol, methanol, N,N-dimethylformamide or N-methylpyrrolidone, preferably water.
[0038] In one embodiment, the mixing speed is 100 to 5000 rpm, for example, it can be 100 rpm, 200 rpm, 500 rpm, 1000 rpm, 1200 rpm, 1500 rpm, 1800 rpm, 2000 rpm, 2500 rpm, 3000 rpm, 3500 rpm, 4000 rpm, 4500 rpm, 5000 rpm, etc.; the mixing time is 10 to 200 min, for example, it can be 10 min, 20 min, 50 min, 100 min, 150 min, 180 min, 200 min, etc.
[0039] In the embodiment of the present application, the stirring time and the rotation speed are within a specific range, and the dispersion is more uniform; if the stirring time is too short, the dispersion will be uneven, and if it is too long, it will cause unnecessary energy consumption.
[0040] In one embodiment, the drying temperature is 80-250°C, for example, 80°C, 85°C, 90°C, 95°C, 100°C, 120°C, 140°C, 160°C, 180°C, 200°C, 220°C, 250°C, etc.
[0041] In the embodiments of the present application, the drying method includes at least one of stirring drying, vacuum drying, oven drying or spray drying; the drying temperature is better within a specific range; too low a temperature will prolong the drying time, and too high a temperature will destroy the structure of the polymer layer. The preferred drying method is oven drying at a temperature of 90 to 120°C.
[0042] In the embodiments of the present application, the preparation process of the silicon-based negative electrode material is simple, the preferred solvent is water, the product production process is safe and environmentally friendly, has low energy consumption, low cost, and is easy to scale up industrially.
[0043] In a third aspect, an embodiment of the present application provides a battery, comprising the silicon-based negative electrode material as described in the first aspect.
[0044] In one embodiment, the battery comprises a lithium-ion battery.
[0045] In a fourth aspect, an embodiment of the present application provides an electrical device, which includes the silicon-based negative electrode material as described in the first aspect and / or the battery as described in the third aspect.
[0046] The numerical range described in the embodiments of the present application includes not only the point values listed above, but also any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the embodiments of the present application no longer exhaustively list the specific point values included in the range.
[0047] The beneficial effects of this application are:
[0048] (1) By using acrylic copolymers, small molecule compounds containing functional groups and conductive agents, a coating network is formed on the surface of the silicon-based core, which plays the role of an artificial SEI film, reduces the volume expansion of the silicon-based material, and reduces the full-charge expansion rate of the silicon-based negative electrode material.
[0049] (2) Acrylic copolymers and small molecule compounds containing functional groups form a unique network structure with excellent ion conductivity, which reduces the internal resistance of the battery.
[0050] (3) The artificial SEI film of small molecule compounds containing functional groups reduces the reaction between silicon-based negative electrode materials and electrolytes, improves the cycle performance of negative electrode materials, and significantly improves the battery's 50-week cycle capacity retention rate.
[0051] Still other aspects will become apparent upon reading and understanding the accompanying drawings and detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] The accompanying drawings are used to provide a further understanding of the technical solution of this article and constitute a part of the specification. Together with the embodiments of this application, they are used to explain the technical solution of this article and do not constitute a limitation on the technical solution of this article.
[0053] FIG1 is a curve showing a change in the 50-cycle capacity retention rate of a battery including the silicon-based negative electrode materials provided in Example 1 and Comparative Example 4 of the present application. DETAILED DESCRIPTION
[0054] The technical solution of the present application is further described below through specific implementation methods. Those skilled in the art should understand that the embodiments are only used to help understand the present application and should not be regarded as specific limitations of the present application.
[0055] Preparation Example 1
[0056] An acrylic copolymer, wherein the preparation method of the acrylic copolymer comprises the following steps:
[0057] 7.5 g of acrylic acid, 1.8 g of acrylonitrile (a first monomer), and 1.0 g of vinyl acetate (a second monomer) were dissolved in 230 g of deionized water. Nitrogen was slowly introduced and stirred at room temperature at 400 rpm for 0.5 hour. The mixture was then heated to 75°C and held for half an hour. After the system temperature stabilized, 0.07 g of ammonium persulfate was added. The mixture was stirred at 75°C and 400 rpm for 5 hours. The temperature was then raised to 85°C and stirred for 1 hour. The system was then evacuated for 0.5 hour. After cooling to room temperature, an aqueous solution containing 2.5 g of lithium hydroxide monohydrate was slowly added and stirred for 1 hour to obtain the acrylic copolymer.
[0058] Preparation Example 2
[0059] An acrylic copolymer differs from Preparation Example 1 only in that, in the preparation method, the content of the raw material acrylic acid is 7.2 g, the content of the first monomer acrylonitrile is 1.9 g, and the content of the second monomer vinyl acetate is 1.2 g; the other components, amounts, and process parameters are the same as those in Preparation Example 1.
[0060] Preparation Example 3
[0061] An acrylic copolymer differs from Preparation Example 1 only in that, in the preparation method, the content of the raw material acrylic acid is 8 g, the content of the first monomer acrylonitrile is 1.3 g, and the content of the second monomer vinyl acetate is 0.9 g; the other components, amounts, and process parameters are the same as those in Preparation Example 1.
[0062] Preparation Example 4
[0063] An acrylic copolymer differs from Preparation Example 1 only in that, in the preparation method, the raw materials include 6.2 g of methacrylic acid, 3 g of the first monomer N-vinyl pyrrolidone, and 1.1 g of the second monomer vinyl acetate; the other components, amounts, and process parameters are the same as those in Preparation Example 1.
[0064] Preparation Example 5
[0065] An acrylic copolymer differs from Preparation Example 1 only in that, in the preparation method, the raw materials include 8.5 g of acrylic acid, 0.9 g of acrylamide as a first monomer, and 0.9 g of methyl methacrylate as a second monomer, and the other components, amounts, and process parameters are the same as those in Preparation Example 1.
[0066] Preparation Example 6
[0067] An acrylic copolymer, which differs from Preparation Example 1 only in that the second monomer vinyl acetate is replaced by an equal amount of hydroxyethyl methacrylate, and the other components, amounts, and process parameters are the same as those in Preparation Example 1.
[0068] Preparation Example 7
[0069] An acrylic copolymer, which differs from Preparation Example 1 only in that the acrylonitrile and vinyl acetate are replaced by equal amounts of hydroxyethyl methacrylate, and the other components, amounts, and process parameters are the same as those in Preparation Example 1.
[0070] Preparation Example 8
[0071] An acrylic copolymer differs from Preparation Example 1 only in that the total amount of acrylic acid, the first monomer, and the second monomer remains unchanged, with a mass ratio of 5:0.5:1, and other components, amounts, and process parameters are the same as those in Preparation Example 1.
[0072] Preparation Example 9
[0073] An acrylic copolymer differs from Preparation Example 1 only in that the total amount of acrylic acid, the first monomer, and the second monomer remains unchanged, with a mass ratio of 10:3.5:1, and other components, amounts, and process parameters are the same as those in Preparation Example 1.
[0074] Example 1
[0075] This embodiment provides a silicon-based negative electrode material, which includes a silicon oxide core (mass of 100 g) and a carbon coating layer (thickness of 5 nm) and an artificial SEI film sequentially coated on the surface of the silicon oxide core; the material of the artificial SEI film includes an acrylic copolymer (Preparation Example 1) with an effective content of 1.37 g, 0.21 g of tannic acid and 0.02 g of graphene.
[0076] This embodiment provides a method for preparing the silicon-based negative electrode material, which specifically includes the following steps:
[0077] According to the formula, acrylic copolymer, tannic acid and graphene are dissolved in 160g of water, and mechanically stirred at a rotation speed of 1500rpm for 1h to obtain an artificial SEI membrane substrate slurry; subsequently, silicon oxide with a surface coated with a carbon coating layer is added thereto, and mechanical stirring is continued for 1h, and then dried at 100°C for 12 hours, and the product is crushed and dispersed to obtain the silicon-based negative electrode material; the preparation method of silicon oxide with a surface coated with a carbon coating layer comprises: adding silicon oxide to a CVD vapor deposition furnace for carbon coating treatment, introducing acetylene gas at a gas mass flow rate of 600sccm, depositing at 950°C for 3h, and placing the coated material under nitrogen protection, heating to 1200°C at a heating rate of 5°C / min, keeping warm for 3h, and naturally cooling to obtain carbon-coated silicon oxide.
[0078] Example 2
[0079] This embodiment provides a silicon-based negative electrode material, which includes a silicon oxide core (mass of 100 g) and a carbon coating layer (thickness of 5 nm) and an artificial SEI film sequentially coated on the surface of the silicon oxide core; the material of the artificial SEI film includes an acrylic copolymer (Preparation Example 2) with an effective content of 1.37 g, 0.25 g of tannic acid and 0.02 g of multi-walled carbon nanotubes.
[0080] This embodiment provides a method for preparing the silicon-based negative electrode material, and the specific steps are the same as those in Example 1.
[0081] Example 3
[0082] This embodiment provides a silicon-based negative electrode material, which includes a silicon oxide core (mass of 100 g) and a carbon coating layer (thickness of 5 nm) and an artificial SEI film sequentially coated on the surface of the silicon oxide core; the material of the artificial SEI film includes an acrylic copolymer (Preparation Example 3) with an effective content of 1.3 g, 0.26 g of tannic acid and 0.05 g of graphene.
[0083] This embodiment provides a method for preparing the silicon-based negative electrode material, and the specific steps are the same as those in Example 1.
[0084] Example 4
[0085] This embodiment provides a silicon-based negative electrode material, which includes a silicon oxide core (mass of 100 g) and a carbon coating layer (thickness of 5 nm) and an artificial SEI film sequentially coated on the surface of the silicon oxide core; the material of the artificial SEI film includes an acrylic copolymer (Preparation Example 1) with an effective content of 1.3 g, 0.28 g of tannic acid and 0.02 g of graphene.
[0086] This embodiment provides a method for preparing the silicon-based negative electrode material, and the specific steps are the same as those in Example 1.
[0087] Example 5
[0088] This embodiment provides a silicon-based negative electrode material, which includes a silicon oxide core (mass of 100 g) and a carbon coating layer (thickness of 5 nm) and an artificial SEI film sequentially coated on the surface of the silicon oxide core; the material of the artificial SEI film includes an acrylic copolymer (Preparation Example 1) with an effective content of 1.37 g, 0.07 g of tannic acid and 0.02 g of graphene.
[0089] This embodiment provides a method for preparing the silicon-based negative electrode material, and the specific steps are the same as those in Example 1.
[0090] Example 6
[0091] This embodiment provides a silicon-based negative electrode material, which includes a silicon oxide core (mass of 100 g) and a carbon coating layer (thickness of 5 nm) and an artificial SEI film sequentially coated on the surface of the silicon oxide core; the material of the artificial SEI film includes an acrylic copolymer (Preparation Example 1) with an effective content of 1.37 g, 0.14 g of tannic acid and 0.02 g of graphene.
[0092] This embodiment provides a method for preparing the silicon-based negative electrode material, and the specific steps are the same as those in Example 1.
[0093] Example 7
[0094] This embodiment provides a silicon-based negative electrode material, which includes a silicon oxide core (mass of 100 g) and a carbon coating layer (thickness of 5 nm) and an artificial SEI film sequentially coated on the surface of the silicon oxide core; the material of the artificial SEI film includes an acrylic copolymer (Preparation Example 4) with an effective content of 1.5 g, 0.3 g of tannic acid and 0.2 g of graphite black.
[0095] This embodiment provides a method for preparing the silicon-based negative electrode material, and the specific steps are the same as those in Example 1.
[0096] Example 8
[0097] This embodiment provides a silicon-based negative electrode material, which includes a silicon oxide core (mass of 100 g) and a carbon coating layer (thickness of 5 nm) and an artificial SEI film sequentially coated on the surface of the silicon oxide core; the material of the artificial SEI film includes an acrylic copolymer (Preparation Example 5) with an effective content of 1.04 g, 0.32 g of tannic acid and 0.24 g of graphite black.
[0098] This embodiment provides a method for preparing the silicon-based negative electrode material, and the specific steps are the same as those in Example 1.
[0099] Examples 9 to 12
[0100] A silicon-based negative electrode material, which differs from Example 1 only in that the acrylic copolymers are provided by Preparation Examples 6 to 9 respectively, and the other components, amounts and preparation methods are the same as those in Example 1.
[0101] Example 13
[0102] This embodiment provides a silicon-based negative electrode material, which differs from Example 1 only in that the total mass of the acrylic copolymer, tannic acid and graphene remains unchanged, and the mass percentages are 48%, 30% and 22% respectively. The other components, amounts and preparation methods are the same as those in Example 1.
[0103] Comparative Example 1
[0104] This comparative example provides a silicon-based negative electrode material, which differs from Example 1 only in that the material of the artificial SEI film does not contain tannic acid, and the other components, amounts and preparation methods are the same as those in Example 1.
[0105] Comparative Example 2
[0106] This comparative example provides a silicon-based negative electrode material, which differs from Example 6 only in that the material of the artificial SEI film does not contain graphene, and the other components, amounts and preparation methods are the same as those of Example 6.
[0107] Comparative Example 3
[0108] This comparative example provides a silicon-based negative electrode material, which differs from Example 1 only in that the surface of the silicon-based negative electrode material is not coated with an artificial SEI film. Other components, amounts and preparation methods are the same as those in Example 1.
[0109] Performance Testing
[0110] The silicon-based anode material was mixed with conductive carbon black, sodium carboxymethyl cellulose, and a polyacrylic acid binder in a ratio of 70:15:5:10 to form a slurry. The slurry was evenly coated onto copper foil and dried to form a negative electrode. The electrode was placed in an argon-filled glove box to form a button cell. A polypropylene microporous membrane served as the separator. The electrolyte used was 1 mol / L lithium hexafluorophosphate (the solvent was a mixture of ethylene carbonate, ethyl methyl carbonate, dimethyl carbonate, and fluoroethylene carbonate in a volume ratio of 30:30:30:10). The counter electrode used was a metallic lithium sheet. The resulting button cell was cycled for 50 cycles in a voltage range of 0.005V to 1.5V at a charge and discharge rate of 0.5C. After the cycling test, the capacity retention was calculated; where 50-cycle capacity retention = discharge capacity at the 50th cycle / discharge capacity at the first cycle × 100%.
[0111] After the button cell is assembled, an electrochemical impedance spectroscopy (EIS) test is performed on it using an electrochemical workstation, and the charge transfer resistance is used to characterize the internal resistance of the battery.
[0112] After the first cycle, disassemble the lithium-ion battery, measure the thickness of the negative electrode when fully charged, and calculate the expansion rate of the electrode when fully charged.
[0113] The expansion rate of the electrode when fully charged = (the thickness of the electrode after full charge - the thickness of the electrode before uncharged) / the thickness of the electrode before uncharged × 100%.
[0114] The specific test results are shown in Table 1:
[0115] Table 1
[0116] As can be seen from the table above, by using a combination of acrylic copolymers, small molecule compounds containing functional groups, and conductive agents, and coating them on the surface of the silicon-based core to form a conductive polymer network, it can act as an artificial SEI film, enhancing ion conductivity, effectively restraining silicon expansion, and reducing the pulverization of the silicon-based negative electrode material after multiple cycles. This results in good battery cycle performance, high capacity retention after 50 cycles, low electrode expansion rate at full charge, and low charge transfer resistance. As can be seen from Examples 1 to 8, the capacity retention rate of the battery can still reach 75.5-86.4% after 50 cycles, the electrode expansion rate at full charge is only 221-265%, and the charge transfer resistance is 3.5-3.8Ω. In terms of battery internal resistance, the charge transfer resistance of the button cell is significantly reduced after coating with the artificial SEI film, indicating that compared with the SEI film formed by electrolyte reduction, the artificial SEI film coated on the surface of the negative electrode material has better ion conductivity.
[0117] As can be seen from Examples 1 and 9 to 12, the raw materials for the preparation of the acrylic copolymers are not of a specific composition and ratio, resulting in poor effects of the synthesized acrylic copolymers, because the strength of the acrylic copolymers and the binding effect on the silicon-based materials are all different. The structural changes of the monomers bring about changes in the flexibility of the polymer material, which changes its binding effect on the silicon-oxygen core, thereby reducing the capacity retention rate of the battery and increasing the full-charge expansion rate of the electrode. As can be seen from Examples 1 and 13, the components in the artificial SEI film are not of a specific content, that is, the polymer content is low and the tannic acid content is high. The cross-linked network structure formed by the two is brittle and easily cracked during post-processing, resulting in partial failure; thereby reducing the capacity retention rate of the battery and increasing the full-charge expansion rate of the electrode. It can be seen from Example 1 and Comparative Example 1 that if the artificial SEI film lacks tannic acid, the cycle performance of the battery will deteriorate. The main reason is that the unique star-shaped structure of tannic acid interacts with the polymer, improves the structure of the coating network, and enhances the coating strength of the polymer network; it can be seen from Example 1 and Comparative Examples 2 and 3 that there is no conductive agent in the artificial SEI film, or the silicon-based negative electrode material is not coated with the artificial SEI film, and the cycle performance of the battery will deteriorate.
[0118] The experimental data above demonstrates that this type of artificial SEI membrane requires a uniquely structured polymer, tannic acid, and a conductive agent. Only through their coordinated application can the SEI membrane tightly coat the surface of the silicon anode material, providing excellent electrical and ion conductivity, thereby inhibiting silicon anode material expansion and enhancing cycling performance.
[0119] In summary, the silicon-based anode material provided herein, through surface coating with an artificial SEI film, and the specific formulation of the artificial SEI film material, can effectively inhibit the volume expansion of the silicon-based core, reduce the pulverization of the silicon-based anode material after multiple cycles, reduce the full-charge expansion of the silicon-based anode material, and improve the cycle performance of the battery. Furthermore, the preparation process of the silicon-based anode material is simple, low-cost, and suitable for industrial production.
[0120] The applicant declares that the above is only a specific implementation method of the present application, but the protection scope of the present application is not limited thereto. Technicians in the relevant technical field should understand that any technician in the relevant technical field can use the technology disclosed in this application.
Claims
1. A silicon-based negative electrode material, comprising a silicon-based core and an artificial SEI film coated on the surface of the silicon-based core; The material of the artificial SEI film includes an acrylic copolymer, a small molecule compound containing a functional group and a conductive agent; The small molecule compound has a star-shaped structure; The functional group includes at least one of a hydroxyl group, a carbonyl group, an ester group or a carboxyl group.
2. The silicon-based negative electrode material according to claim 1, wherein: The material of the artificial SEI film includes 55-98% of acrylic copolymer, 1-25% of small molecule compound containing functional groups and 1-20% of conductive agent in terms of mass percentage; Optionally, the material of the artificial SEI film includes, by weight percentage, 65-95% of an acrylic copolymer, 4-20% of a small molecule compound containing a functional group, and 1-15% of a conductive agent.
3. The silicon-based negative electrode material according to claim 1 or 2, wherein: The raw materials for preparing the acrylic copolymer include 50-95% acrylic monomer, 1-40% first monomer and 1-40% second monomer in terms of mass percentage; Optionally, the first monomer and the second monomer are each independently selected from at least one of vinyl acetate, methyl methacrylate, acrylonitrile, hydroxyethyl methacrylate, acrylamide or N-vinyl pyrrolidone; the first monomer is different from the second monomer; Optionally, the mass ratio of the acrylic monomer, the first monomer and the second monomer is (5.5-9.5):(1-3):
1.
4. The silicon-based negative electrode material according to any one of claims 1 to 3, wherein: The small molecule compound containing a functional group includes tannic acid; Optionally, the conductive agent includes at least one of graphene, acetylene black, carbon black, graphite black, single-walled carbon nanotubes or multi-walled carbon nanotubes.
5. The silicon-based negative electrode material according to any one of claims 1 to 4, wherein: The mass percentage of the artificial SEI film in the silicon-based negative electrode material is 0.1-10%; Optionally, the silicon-based core comprises a silicon oxide core; Optionally, the particle size of the silicon oxide core is 500nm to 20μm, and the specific surface area of the silicon oxide core is 0.5 to 25m 2 / g.
6. The silicon-based negative electrode material according to claim 5, wherein: The surface of the silicon oxide core is coated with a carbon coating layer; Optionally, the carbon coating layer has a thickness of 2 to 10 nm; Optionally, the silicon-based negative electrode material includes a silicon monoxide core and a carbon coating layer and an artificial SEI film sequentially coated on the surface of the silicon monoxide core.
7. A method for preparing the silicon-based negative electrode material according to any one of claims 1 to 6, the method comprising the following steps: The acrylic copolymer, the small molecule compound containing a functional group and the conductive agent are mixed with the silicon-based core and dried to obtain the silicon-based negative electrode material.
8. The preparation method according to claim 7, wherein: The mixing is carried out in a solvent; the solvent comprises at least one of water, ethanol, methanol, N,N-dimethylformamide or N-methylpyrrolidone; Optionally, the mixing speed is 100 to 5000 rpm, and the mixing time is 10 to 200 min; Optionally, the drying temperature is 80-250°C.
9. A battery, comprising the silicon-based negative electrode material according to any one of claims 1 to 6.
10. An electrical device, comprising the silicon-based negative electrode material according to any one of claims 1 to 6 and / or the battery according to claim 9.
Citation Information
Patent Citations
Anode active-material particle having synthetic SEI layer by using master link branching process
CN108155354A
Anode active-material particle having synthetic sei layer by using a living radical polymerization
CN108155355A
Silica composite material and preparation method thereof, and lithium ion battery
CN110364700A
Silicon-based negative electrode material, preparation method thereof and secondary battery
CN115513418A
Method for producing organic compound-coated bismuth oxide particle, method for manufacturing radiation shielding member, and radiation shielding member
JP2021135170A
Cited By
Self-healing modified binder for silicon negative electrode of lithium battery as well as preparation method and application of self-healing modified binder
CN119391332A