Modified lithium cobaltate material, and preparation method therefor and use thereof
Through the parallel flow coating method and the control of pH value and Zeta potential, the problem of uneven coating and erosion of lithium cobalt oxide material is solved, efficient lithium cobalt oxide material coating is achieved, and its electrochemical performance and cycle performance are significantly improved. .
Patent Information
- Application Number
- PCT/CN2023/111985
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-23
- Filing Date
- 2023-08-09
- Publication Date
- 2024-10-31
AI Technical Summary
Existing lithium cobalt oxide materials have problems with uneven and loose coatings during the coating process, resulting in insufficient electrochemical performance of the material. In addition, traditional methods have greater corrosion and pH restrictions on lithium cobalt oxide, which limits the coating. variety and efficiency.
Using the parallel flow coating method, by controlling the pH value and Zeta potential of the lithium cobalt oxide material, combined with highly acidic salt solutions such as magnesium chloride and titanyl sulfate, uniform core-coated particles are formed to avoid acid solution erosion and utilize surface potential differences. Promote the bonding of coated particles.
Efficient coating of lithium cobalt oxide material has been achieved, improving its specific capacity and cycle performance. The retention rate can reach 92.5% after 50 cycles, and the 2C/0.5C rate performance can reach 91.9%, significantly improving the electrochemical performance.
Smart Images

Figure CN2023111985_31102024_PF_FP_ABST
Abstract
Description
A modified lithium cobalt oxide material and its preparation method and application Technical Field
[0001] The present application belongs to the technical field of battery materials and relates to a modified lithium cobalt oxide material and a preparation method and application thereof. Background Art
[0002] Lithium cobalt oxide (LCO) is widely used in products such as smartphones, tablets, and drones due to its high operating voltage, stable charge-discharge structure, high specific energy, good cycle stability, and environmental friendliness. With the development of electronic products, the demand for LCO's electrical performance is also increasing. To improve the cycle performance and specific capacity of LCO, common methods include ion doping and element coating.
[0003] Element coating is usually achieved by coating with oxides, phosphides, and fluorides to improve the stability of the material and the ion transport performance. The traditional coating method is usually to mix lithium cobalt oxide and the coating material in a solid state in a certain proportion and then calcine it at high temperature. This method is simple and easy to implement, but it also has the disadvantages of uneven coating and loose coating. Therefore, a large number of studies have proposed new process approaches for wet coating:
[0004] CN109994711A discloses a method for preparing a doped and coated lithium cobalt oxide positive electrode material. The method comprises dissolving anhydrous magnesium acetate, aluminum isopropoxide, and ethyl orthosilicate in an anhydrous ethanol solution and mixing the solution with the lithium cobalt oxide material in liquid form, thereby achieving the effect of uniformly coating the surface of the lithium cobalt oxide with oxides of Al, Mg, and Si, thereby improving the electrochemical performance of the lithium cobalt oxide material. However, the method does not propose how to control the effectiveness of the coating.
[0005] CN113346066A discloses a phosphate-coated lithium cobalt oxide cathode material and its preparation method. Using a sol-gel method, a milky white gel with a positive zeta potential is first formed. A negative zeta potential lithium cobalt oxide cathode material is then added. The material is then adsorbed onto the surface of the material by the attraction between the positive and negative charges of small particles in the liquid phase. The material is then stirred, heated, and evaporated to dryness, ultimately yielding a strontium aluminum tantalum zirconium phosphate fast ion conductor-coated lithium cobalt oxide battery cathode material. This method utilizes the principle that the potentials of the coating and lithium cobalt oxide are opposite to each other to improve the effectiveness of the coating. However, the requirement for a positive potential in the coating mixture limits the types of coatings that can be applied. Furthermore, the proposed method of adding a lithium cobalt oxide suspension to the coating solution further limits the pH value (cobalt begins to dissolve slightly in solutions with a pH below 3) and the types of coatings that can be applied.
[0006] Summary of the Invention
[0007] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.
[0008] The purpose of this application is to provide a modified lithium cobalt oxide material, its preparation method and application. This application provides a universal preparation method for coating different types of elements, which reduces the erosion of the coating solution on the material while improving the bonding between the material and the coating layer.
[0009] To achieve this goal, this application adopts the following technical solutions:
[0010] In a first aspect, an embodiment of the present application provides a method for preparing a modified lithium cobalt oxide material, the preparation method comprising the following steps:
[0011] (1) Mixing the lithium cobalt oxide material and the solvent to obtain a suspension, stirring and heating, and then testing the first pH and the first zeta potential.
[0012] (2) adding the alkali solution and the coating salt solution into the suspension in parallel, controlling the system to a second pH value to carry out the reaction;
[0013] (3) Determination of the second zeta potential after aging The modified lithium cobalt oxide material is obtained.
[0014] The embodiment of the present application adopts a parallel coating method to form uniform core-coated particles, especially for highly acidic salt solutions such as magnesium chloride, titanyl sulfate and the like, which can avoid the erosion of cobalt by the acid solution when added to the lithium cobalt oxide suspension and the destruction of the intrinsic structure of the lithium cobalt oxide material; at the same time, due to the presence of residual alkali in the lithium cobalt oxide material, the initial pH1 and the pH2 value range during stable coating feed are controlled, which can not only achieve the effect of completely precipitating the coating elements, but also promote the binding of the coated particles on the surface of the lithium cobalt oxide by utilizing the difference in surface potential.
[0015] In one embodiment, the solid-liquid ratio of the suspension in step (1) is 1:(8-80), for example: 1:8, 1:10, 1:20, 1:50 or 1:80.
[0016] In one embodiment, the temperature of the heating in step (1) is 50-80°C, for example, 50°C, 55°C, 60°C, 70°C or 80°C.
[0017] In one embodiment, the first pH is 10.5-12, for example, 10.5, 10.8, 11, 11.5 or 12.
[0018] In one embodiment, the first zeta potential The range is -200 to -20mV, for example: -200mV, -150mV, -100mV, -50mV or -20mV, etc.
[0019] In one embodiment, the concentration of the alkali solution in step (2) is 0.1 to 0.5 mol / L, for example, 0.1 mol / L, 0.2 mol / L, 0.3 mol / L, 0.4 mol / L or 0.5 mol / L.
[0020] In one embodiment, the solute of the coating salt solution includes any one of aluminum salt, magnesium salt, cobalt salt, manganese salt, zirconium salt, tantalum salt, strontium salt, silicate or titanium salt, or a combination of at least two thereof.
[0021] In one embodiment, the concentration of the coating salt solution is 0.001-0.1 mol / L, for example, 0.001 mol / L, 0.005 mol / L, 0.01 mol / L, 0.08 mol / L or 0.1 mol / L.
[0022] In one embodiment, the second pH in step (2) is 8 to 9.5, for example, 8, 8.2, 8.5, 9 or 9.5.
[0023] In one embodiment, the aging time in step (3) is 0.5 to 1 h, for example, 0.5 h, 0.6 h, 0.7 h, 0.8 h, 0.9 h or 1 h.
[0024] In one embodiment, the second zeta potential of step (3) It is -20~0mV, for example: -20mV, -15mV, -10mV, -5mV or 0mV, etc.
[0025] In one embodiment, the second zeta potential is determined The suspension is then washed until the conductivity is qualified and then dried to obtain the modified lithium cobalt oxide material.
[0026] In a second aspect, an embodiment of the present application provides a modified lithium cobalt oxide material, which is prepared by the method described in the first aspect.
[0027] In a third aspect, an embodiment of the present application provides a positive electrode plate, wherein the positive electrode plate comprises the modified lithium cobalt oxide material as described in the second aspect.
[0028] In a fourth aspect, an embodiment of the present application provides a lithium-ion battery, wherein the lithium-ion battery comprises the positive electrode sheet as described in the third aspect.
[0029] Compared with the prior art, this application has the following beneficial effects:
[0030] (1) The present application adopts a parallel coating method to form uniform core-coated particles, which can avoid the erosion of cobalt by the acid solution when it is added to the lithium cobalt oxide suspension, thereby destroying the intrinsic structure of the lithium cobalt oxide material. At the same time, due to the presence of residual alkali in the lithium cobalt oxide material, its initial pH1 is between 10.5 and 12. By stabilizing the pH2 value of the coating feed to be between 8 and 9.5, it can not only achieve the effect of completely precipitating the coating elements, but also promote the binding of the coating particles on the surface of the lithium cobalt oxide by utilizing the difference in surface potential.
[0031] (2) The modified lithium cobalt oxide material prepared by the method described in this application has a specific capacity of more than 189.6 mAh / g, a cycle retention rate of more than 92.5% after 50 cycles, and a 2C / 0.5C rate performance of more than 91.9%. Through the effective coating of the lithium cobalt oxide material, its electrical properties are significantly improved, the specific capacity is increased, and the cycle performance and rate performance are enhanced.
[0032] Still other aspects will become apparent upon reading and understanding the accompanying drawings and detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] The accompanying drawings are used to provide a further understanding of the technical solution of this article and constitute a part of the specification. Together with the embodiments of this application, they are used to explain the technical solution of this article and do not constitute a limitation on the technical solution of this article.
[0034] FIG1 is a SEM image of the modified lithium cobalt oxide material obtained in Example 1 of the present application. DETAILED DESCRIPTION
[0035] The technical solution of the present application is further described below through specific implementation methods. Those skilled in the art should understand that the embodiments are only used to help understand the present application and should not be regarded as specific limitations of the present application.
[0036] Example 1
[0037] This embodiment provides a modified lithium cobalt oxide material. The preparation method of the modified lithium cobalt oxide material is as follows:
[0038] (1) Add 200g of lithium cobalt oxide material to 4L of water to form a uniform suspension with a solid-liquid ratio of 1:20; ② Heat the lithium cobalt oxide suspension to 80℃ under stirring conditions, and detect its pH value as 10.6 using an industrial electrode. After reaching 80℃, take the suspension for zeta potential test -45.6mV;
[0039] (2) Prepare 500 mL of 0.006 mol / L titanyl sulfate solution and 0.2 mol / L sodium hydroxide solution, pump the titanyl sulfate solution into the lithium cobalt oxide suspension at a rate of 5 mL / min, while adjusting the flow rate of the sodium hydroxide solution and maintaining the pH at 9.5;
[0040] (3) After the addition of the titanyl sulfate solution, continue stirring and aging for 0.5 h, and take the coated lithium cobalt oxide suspension for zeta potential testing The suspension was washed until the conductivity reached a certain level and then dried to obtain the modified lithium cobalt oxide material. The SEM image of the modified lithium cobalt oxide material is shown in FIG1 .
[0041] Example 2
[0042] This embodiment provides a modified lithium cobalt oxide material. The preparation method of the modified lithium cobalt oxide material is as follows:
[0043] (1) Add 200g of lithium cobalt oxide material to 6L of water to form a uniform suspension with a solid-liquid ratio of 1:30; ② Heat the lithium cobalt oxide suspension to 73°C under stirring conditions, and use an industrial electrode to detect its pH value of 11. After reaching 73°C, take the suspension for zeta potential testing. -55.6mV;
[0044] (2) Prepare 500 mL of 0.05 mol / L magnesium sulfate solution and 0.3 mol / L sodium hydroxide solution, pump the magnesium sulfate solution into the lithium cobalt oxide suspension at a rate of 5 mL / min, while adjusting the flow rate of the sodium hydroxide solution and maintaining the pH at 9;
[0045] (3) After the addition of magnesium sulfate solution, continue stirring and aging for 0.8h, and take the coated lithium cobalt oxide suspension for zeta potential test The suspension was washed until the conductivity reached a qualified level and then dried to obtain the modified lithium cobalt oxide material.
[0046] Example 3
[0047] The only difference between this embodiment and embodiment 1 is that the first pH is 10, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0048] Example 4
[0049] The only difference between this embodiment and embodiment 1 is that the first pH is 12.5, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0050] Example 5
[0051] The only difference between this embodiment and embodiment 1 is that the second pH is 7.5, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0052] Example 6
[0053] The only difference between this embodiment and embodiment 1 is that the second pH is 10, and other conditions and parameters are exactly the same as those in embodiment 1.
[0054] Example 7
[0055] The only difference between this embodiment and embodiment 1 is that the first zeta potential The other conditions and parameters are exactly the same as those in Example 1.
[0056] Example 8
[0057] The only difference between this embodiment and embodiment 1 is that the first zeta potential The other conditions and parameters are exactly the same as those in Example 1.
[0058] Example 9
[0059] The only difference between this embodiment and embodiment 1 is that the second zeta potential The other conditions and parameters are exactly the same as those in Example 1.
[0060] Performance testing:
[0061] The modified lithium cobalt oxide material prepared in Examples 1-9, PVDF, and conductive carbon black were mixed in a mass ratio of 95.4:2.5:2.1, NMP was added, and stirred to form a slurry. The slurry was coated on aluminum foil and dried at 120°C to form a positive electrode sheet. This was then assembled with the negative electrode sheet, separator, and electrolyte to form a 063048 battery. The battery performance was tested, and the test results are shown in Table 1.
[0062] Table 1
[0063] As can be seen from Table 1, according to Examples 1-2, the modified lithium cobalt oxide material prepared by the method described in this application has a specific capacity of more than 189.6 mAh / g, a cycle retention rate of more than 92.5% after 50 cycles, and a 2C / 0.5C rate performance of more than 91.9%.
[0064] By comparing Example 1 with Examples 3-4, it can be seen that in the preparation process of the modified lithium cobalt oxide material described in the present application, the first pH will affect the performance of the modified lithium cobalt oxide material. When the first pH is controlled at 10.5-12, the performance of the lithium cobalt oxide material obtained is better. If the first pH is too low, the cycle performance of the lithium cobalt oxide is significantly reduced. If the first pH is too high, the specific capacity of the lithium cobalt oxide is significantly reduced and the rate performance deteriorates.
[0065] By comparing Example 1 with Examples 5-6, it can be seen that during the preparation process of the modified lithium cobalt oxide material described in the present application, the second pH will affect the performance of the modified lithium cobalt oxide material. When the second pH is controlled at 8 to 9.5, the performance of the lithium cobalt oxide material obtained is better. If the second pH is too low, the cycle performance of the lithium cobalt oxide is significantly reduced. If the second pH is too high, the specific capacity of the lithium cobalt oxide is significantly reduced and the rate performance deteriorates.
[0066] From the comparison between Example 1 and Examples 7-8, it can be seen that during the preparation of the modified lithium cobalt oxide material described in this application, the first zeta potential It will affect the performance of the modified lithium cobalt oxide material. Controlled at -200~-20mV, the lithium cobalt oxide material has better performance. If the first zeta potential If the first zeta potential is too low, the specific capacity of lithium cobalt oxide will be significantly reduced and the rate performance will be worse. If the concentration is too high, the cycle performance of lithium cobalt oxide will be significantly reduced.
[0067] From the comparison between Example 1 and Examples 9-10, it can be seen that during the preparation of the modified lithium cobalt oxide material described in this application, the second zeta potential It will affect the performance of the modified lithium cobalt oxide material. Controlled at -20~0mV, the lithium cobalt oxide material has better performance. If the second zeta potential If the concentration is too low, the cycle performance of lithium cobalt oxide will be significantly reduced.
[0068] The applicant declares that the above is only a specific implementation method of the present application, but the protection scope of the present application is not limited thereto. Technical personnel in the relevant technical field should understand that any changes or substitutions that can be easily thought of by technical personnel in the relevant technical field within the technical scope disclosed in this application fall within the protection scope and disclosure scope of this application.
Claims
1. A method for preparing a modified lithium cobalt oxide material, the preparation method comprising the following steps: (1) Mixing the lithium cobalt oxide material and the solvent to obtain a suspension, stirring and heating, and testing the first pH and the first zeta potential (2) adding the alkali solution and the coating salt solution into the suspension in parallel, and controlling the system to a second pH value to react; (3) Determination of the second zeta potential after aging The modified lithium cobalt oxide material is obtained.
2. The preparation method according to claim 1, wherein The solid-to-liquid ratio of the suspension in step (1) is 1:(8-80).
3. The preparation method according to claim 1 or 2, wherein: The temperature of the heating in step (1) is 50-80° C. Optionally, the first pH is 10.5 to 12; Optionally, the first zeta potential The range is -200~-20mV.
4. The preparation method according to any one of claims 1 to 3, wherein The concentration of the alkali solution in step (2) is 0.1-0.5 mol / L.
5. The preparation method according to any one of claims 1 to 4, wherein: The solute of the coating salt solution includes any one of aluminum salt, magnesium salt, cobalt salt, manganese salt, zirconium salt, tantalum salt, strontium salt, silicate or titanium salt, or a combination of at least two thereof; Optionally, the concentration of the coating salt solution is 0.001-0.1 mol / L.
6. The preparation method according to any one of claims 1 to 5, wherein: Step (2) The second pH is 8 to 9.
5.
7. The preparation method according to any one of claims 1 to 6, wherein: The aging time in step (3) is 0.5 to 1 h.
8. The preparation method according to any one of claims 1 to 7, wherein: Step (3) The second zeta potential -20~0mV; Optionally, the second zeta potential is determined The suspension is then washed until the conductivity is acceptable and then dried to obtain the modified lithium cobalt oxide material.
9. A modified lithium cobalt oxide material, wherein the modified lithium cobalt oxide material is prepared by the method according to any one of claims 1 to 8.
10. A positive electrode plate, comprising the modified lithium cobalt oxide material according to claim 9. 11 . A lithium ion battery, comprising the positive electrode sheet according to claim 10 .
Citation Information
Patent Citations
Method for preparing lithium cobaltate composite electrode material coated by iron phosphate
CN101276913A
Lithium cobaltate composite oxide coated by hydrolytic precipitation-roasting method and manufacturing method thereof
CN101872859A
Cobalt-aluminum composite metal oxide-coated LiCoO2 anode material and preparation method thereof
CN101894938A
Doped and surface coating co-modified anode material for lithium ion battery and preparation method thereof
CN103779556A
Method for preparing alumina coated lithium cobalt oxide lithium ion battery material by aluminum salt solution aftertreatment
CN105428625A