Self-supporting positive electrode and preparation method therefor and use thereof
By using a conductive carrier to load a self-supporting cathode with nanometer sodium iron sulfate particles in a sodium-ion battery, the problem of poor electrochemical performance of the sodium-ion battery cathode material is solved, high energy density, power density and cycle stability are achieved, and the preparation is simplified process, suitable for industrial production.
Patent Information
- Application Number
- PCT/CN2023/137596
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-24
- Filing Date
- 2023-12-08
- Publication Date
- 2024-10-31
AI Technical Summary
Existing sodium-ion battery cathode materials have poor electrochemical properties, resulting in poor energy density, power density, and cycle stability. The preparation process is complex, making it difficult to meet the needs of industrial production.
A conductive carrier is used as a self-supporting cathode, loaded with nano-sodium iron sulfate particles, and prepared through solvothermal reaction and annealing treatment, which significantly improves the conductivity and particle uniformity and reduces dependence on conductive agents and binders.
It significantly improves the energy density, power density and rate performance of sodium-ion batteries, simplifies the preparation process, is suitable for large-scale industrial production, and improves cycle stability and electrochemical performance.
Smart Images

Figure CN2023137596_31102024_PF_FP_ABST
Abstract
Description
A self-supporting positive electrode and its preparation method and application Technical Field
[0001] The present invention relates to the technical field of secondary battery materials, and in particular to a self-supporting positive electrode and a preparation method and application thereof. Background Art
[0002] With the increasing scarcity of traditional fossil resources such as coal, oil, and natural gas, and the increasingly severe environmental pollution and greenhouse gas effects associated with fossil energy use, the development of renewable green energy sources such as solar, wind, tidal, and geothermal energy is imperative. However, renewable energy sources suffer from intermittent and unstable characteristics, making their effective utilization crucial for the development of efficient energy storage systems. Among various electrochemical energy storage devices, lithium-ion batteries (LIBs) have attracted significant attention due to their high energy density and long cycle life. Currently, LIBs are widely used in portable electronic devices, electric vehicles, and large-scale energy storage power stations. However, as energy demand soars, the price of lithium ore resources continues to rise, and the uneven distribution of lithium resources (85% of which is concentrated in the Americas) has limited the further development of LIBs. Therefore, the research and development of new energy storage devices is particularly urgent. Sodium, which also stores energy through the intercalation and deintercalation of ions between positive and negative electrode materials, has the advantages of abundant reserves, uniform distribution, and low cost. Furthermore, it shares similar physical and chemical properties with lithium, leading to widespread attention worldwide in the development of LIBs. The research on sodium-ion batteries can effectively avoid the problem of limited development of electrochemical energy storage technology caused by the shortage of lithium mineral resources.
[0003] In sodium ion batteries, the development of negative electrode materials and electrolytes is more mature than that of positive electrode materials, and the cost of positive electrode materials accounts for 1 / 3 of the total cost of the battery. Therefore, the development of low-cost positive electrode materials for sodium ion batteries is a key link in the practical application of sodium ion batteries. Common positive electrode materials for sodium ion batteries mainly include: layered metal oxides, Prussian blue system, polyanion system, etc. Layered metal oxides such as Na x VO2、Na x MnO2, etc., the average voltage is usually below 3V, and the lower voltage leads to lower energy density of the material. 1.72MnFe(CN)6, for example, is prone to forming [Fe(CN)6] vacancies in its structure, which are easily occupied by crystal water, resulting in poor battery cycling performance and low Coulombic efficiency. Fluorine-containing cathode materials in polyanion systems, due to the introduction of fluoride ions, enhance the inductive effect of the polyanion groups, increasing the material's operating voltage. However, the introduction of fluorine can easily pollute the environment and impose strict requirements on the production environment and equipment. Therefore, a sodium-ion battery cathode material that can meet the requirements of industrial production, environmental friendliness, low cost, and good electrochemical performance is urgently needed to meet practical application needs. Technical issues
[0004] Sodium ferric sulfate (also known as sodium ferrous sulfate, Na2Fe2(SO4)3 or its non-stoichiometric compounds) is an excellent, low-cost, iron-based polyanionic cathode material with a reversible voltage platform as high as 3.8V and a theoretical specific capacity of 120mAh / g, laying a solid foundation for high-energy-density sodium-ion batteries. This theoretical voltage of 3.8V is even higher than that of corresponding materials in lithium-ion batteries, offering significant advantages over other polyanionic sodium-ion cathode materials and effectively overcoming the low operating voltage and energy density issues faced by sodium-ion batteries.
[0005] However, due to the low intrinsic conductivity of the pure iron sulfate phase material, the sodium storage electrochemical performance of the positive electrode material is seriously affected, resulting in low sodium storage capacity, poor cycle stability and poor rate performance. Technical Solutions
[0006] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention provides a self-supporting positive electrode that, when used in a sodium ion battery, can effectively improve the energy density, power density, rate performance, and cycle performance of the resulting sodium ion battery.
[0007] The present invention also provides a method for preparing the self-supporting positive electrode.
[0008] The present invention also provides applications of the self-supporting positive electrode.
[0009] According to an embodiment of the first aspect of the present invention, a self-supporting positive electrode is provided, comprising a conductive support and nano-sodium iron sulfate particles supported on the conductive support.
[0010] The self-supporting positive electrode according to the embodiment of the present invention has at least the following beneficial effects:
[0011] (1) In traditional technology, in order to promote the practical application of sodium ferric sulfate in sodium ion batteries, sodium ferric sulfate has been modified in many ways, such as using carbon modification to improve the conductivity of sodium ferric sulfate positive electrode materials, in order to accelerate electron transfer and optimize the electrochemical performance of the electrode. The carbon modification methods include: compounding sodium ferric sulfate with graphene oxide (deposition / loading), or wrapping sodium ferric sulfate with graphene. In order to improve conductivity, the graphene used for carbon modification can also be doped. However, the modified sodium ferric sulfate still needs to be mixed with inactive substances such as conductive agents and binders to form a slurry, and then coated on the current collector to form a positive electrode; the inactive substances used will reduce the energy density, and the preparation process of the positive electrode is also very complicated. More importantly, the conductivity of the resulting positive electrode is poor, and the combination with the active ingredients is not tight. The electrical properties of the composite material are poor, and it is difficult to meet the needs of high-rate charge and discharge.
[0012] In the self-supporting positive electrode provided by the present invention, the conductive carrier can directly play the role of current collector and conductive agent, so it can be directly used as a positive electrode without the need for a conductive agent, a binder and a current collector, thereby significantly improving the energy density and power density of the self-supporting positive electrode battery. At the same time, the conductive carrier significantly enhances the conductivity of Na2Fe2(SO4)3, thereby improving the rate performance of the self-supporting positive electrode. The positive electrode has a developed pore structure (from the accumulation of nano-sodium iron sulfate particles and the pores of the conductive carrier itself, with a pore size at the nanometer level), which greatly shortens the diffusion distance of substances such as ions / electrons and electrolytes. Nano-sized sodium iron sulfate particles have a large specific surface area and can provide abundant active energy storage sites.
[0013] (2) According to conventional wisdom, the deposition mechanism and effect of sodium ferric sulfate on the same carrier are similar, regardless of the size of the carrier. However, the present invention found that when the size of the carrier is micrometer-scale or nanometer-scale (smaller), such as the carrier is carbon nanotubes, the deposition of sodium ferric sulfate is random, that is, some sodium ferric sulfate will directly agglomerate instead of being deposited on the carrier, and even if it is deposited on the carrier, the particle size of the sodium ferric sulfate is uneven and large (generally >1μm). On the other hand, a large-area carrier, such as carbon cloth, will provide sufficient deposition sites, prompting the sodium ferric sulfate to be uniformly and fully deposited on the carrier in small sizes.
[0014] The self-supporting positive electrode provided by the present invention has a conductive carrier that also functions as a current collector, resulting in a larger size. Specifically, the size and uniformity of the sodium ferric sulfate particles are adjusted through structural design. This further improves the cycling and rate performance of the self-supporting positive electrode and makes the preparation process more adjustable.
[0015] According to some embodiments of the present invention, the conductive support includes at least one of a carbon-based film, a metal mesh, and a conductive polymer film.
[0016] According to some embodiments of the present invention, the carbon-based film includes at least one of carbon cloth, carbon paper, porous carbon, graphene film and carbon nanotube film.
[0017] According to some embodiments of the present invention, the metal mesh includes at least one of foam nickel, foam copper, nickel mesh, copper mesh, titanium mesh, platinum mesh, stainless steel mesh, platinum-rhodium-palladium alloy mesh, platinum-rhodium alloy mesh, platinum-iridium alloy mesh, palladium-nickel alloy mesh and aluminum-magnesium mesh.
[0018] According to some embodiments of the present invention, the conductive polymer film includes at least one of a polyethylene-derived composite material, a polyvinyl alcohol-derived composite material, a polyester-derived composite material, a polyimide-derived composite material, a polyurethane-derived composite material, a polyethylene naphthalate-derived composite material, a polydimethylsiloxane-derived composite material, and a polyacrylonitrile-derived composite material.
[0019] According to some embodiments of the present invention, the conductive carrier includes at least one of a carbon-based film and a metal mesh.
[0020] According to some embodiments of the present invention, the conductive carrier includes at least one of carbon cloth, carbon paper, nickel foam, and copper mesh.
[0021] According to some embodiments of the present invention, the conductive carrier includes the carbon cloth.
[0022] According to some embodiments of the present invention, the loading amount of the nano-sodium iron sulfate particles on the conductive carrier is 2-15 mg / cm 2 .
[0023] According to some embodiments of the present invention, the loading amount of the nano sodium iron sulfate particles on the conductive carrier is 5-13 mg / cm 2 For example, it can be about 6 mg / cm 2 , 7mg / cm 2 , 8mg / cm 2 or 13 mg / cm 2 .
[0024] According to some embodiments of the present invention, the particle size of the nano sodium iron sulfate particles is between 500 and 1000 nm.
[0025] According to an embodiment of the second aspect of the present invention, a method for preparing the self-supporting positive electrode is provided, the method comprising the following steps:
[0026] S1. The conductive support is immersed in a dispersion comprising a sodium source, an iron source and a sulfur source to perform a solvothermal reaction;
[0027] S2. Annealing the solid product obtained in step S1. Beneficial effects
[0028] The preparation method according to the embodiment of the present invention has at least the following beneficial effects:
[0029] Traditional technologies include using freeze-drying + calcination to compound the carrier and sodium ferric sulfate. Although this method can compound the two and provides a preparation method for non-stoichiometric sodium ferric sulfate, the preparation process requires extremely low temperature and takes too long (about 48 hours), and the required conditions are relatively harsh. There are also technologies that use co-precipitation and hydrothermal methods to compound the carrier (usually a small-particle carbon-based carrier) and sodium ferric sulfate, but the preparation process may require higher temperatures, is difficult, and has a low safety factor. In addition, the cycle performance, energy density, and rate performance of the resulting sodium ferric sulfate-based composite material need to be further improved.
[0030] The preparation method provided by the present invention is simple and easy to operate, has low cost, low equipment requirements, and is suitable for large-scale industrial production. In the self-supporting positive electrode prepared, the load uniformity of sodium ferric sulfate is high, the particle size is small and uniform, and the electrochemical performance of the obtained self-supporting positive electrode is improved. Furthermore, the preparation method provided by the present invention can adjust the particle size, load amount, stoichiometric coefficient, etc. of the sodium ferric sulfate particles by fine-tuning the parameters in step S1, and can also improve the load strength and crystallization performance of the obtained sodium ferric sulfate by annealing in step S2. In other words, the preparation method provided by the present invention is easy to adjust, and the electrochemical performance of the obtained self-supporting positive electrode is good.
[0031] According to some embodiments of the present invention, step S1 further includes pre-treating the conductive carrier before immersing.
[0032] According to some embodiments of the present invention, the pretreatment comprises sequentially performing organic solvent washing, water washing, and drying; the organic solvent thereby removes oily impurities on the surface of the conductive carrier, and the subsequent water washing removes the organic solvent and water-soluble impurities. The water washing is performed ≥1 times and is stopped until the pH of the washing solution reaches ≈7. The solvent used in the organic solvent washing comprises at least one of acetone and ethanol. The organic solvent washing method includes ultrasonic cleaning.
[0033] According to some embodiments of the present invention, in step S1, the sodium source includes sodium sulfate, sodium bisulfate, sodium carbonate, sodium bicarbonate, sodium acetate (also known as sodium acetate), sodium nitrite, sodium oxalate, sodium persulfate, sodium hydroxide, sodium pyrosulfate, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium metabisulfite, sodium pyrophosphate, sodium hydrogen phthalate, sodium hydrogen oxalate, sodium sulfite, sodium sorbate, trisodium phosphate, sodium gluconate, sodium oleate, and at least one of hydrates of the above sodium sources.
[0034] According to some embodiments of the present invention, in step S1, the sodium source includes at least one of sodium bicarbonate, sodium sulfate, sodium acetate, sodium bisulfate and sodium hydroxide.
[0035] According to some embodiments of the present invention, in step S1, the sodium source includes at least one of sodium bicarbonate and sodium sulfate.
[0036] The type of sodium source has no significant effect on the performance of the self-supporting positive electrode, and its function is to provide sodium ions.
[0037] According to some embodiments of the present invention, in step S1, the iron source includes at least one of ferric sulfate, ferrous oxide, ferrous chloride, ferrous sulfate, ferrous hydroxide, ferrous oxide, ferric chloride, ferric hydroxide, and hydrates of the above iron sources.
[0038] According to some embodiments of the present invention, in step S1, the iron source includes at least one of ferrous sulfate, ferric sulfate, ferrous chloride and ferric oxide.
[0039] According to some embodiments of the present invention, in step S1, the iron source includes ferrous sulfate.
[0040] According to some embodiments of the present invention, in step S1, the sulfur source includes ferric sulfate, ferrous sulfite, ferrous sulfate, sodium bisulfate, potassium sulfate, ammonium sulfate, ferrous dithionite, ferrous thiosulfate, ferrous dithionate, ferrous tetrasulfide, sodium sulfate, sodium sulfite, sodium dithionite, sodium thiosulfate, sodium dithionate, sulfurous acid, sulfuric acid, ammonium persulfate, potassium persulfate, sodium persulfate, sodium dodecyl sulfate, sodium dodecylbenzenesulfonate, and at least one of hydrates of the above sulfur sources.
[0041] According to some embodiments of the present invention, in step S1, the sulfur source includes at least one of ferrous sulfate, sodium sulfate, ferric sulfate, sodium bisulfate, ammonium sulfate and potassium sulfate.
[0042] According to some embodiments of the present invention, in step S1, the sulfur source includes at least one of ferrous sulfate and sodium bisulfate.
[0043] Based on the sodium, sulfur, and iron sources listed above, it can be seen that the same substance may serve as both source substances. For example, ferric sulfate can serve as both a sulfur and iron source. Therefore, although the dispersion in step S1 contains a sodium, iron, and sulfur source, it may contain less than three solute compounds.
[0044] According to some embodiments of the present invention, in step S1, the solvent of the dispersion liquid includes at least one of water, methanol, anhydrous ethanol, acetone, ethylene glycol and pyridine.
[0045] According to some embodiments of the present invention, in step S1, the solvent of the dispersion includes water.
[0046] When other conditions are the same, the type of solvent in the dispersion will have a certain impact on the loading capacity of the nano-sodium iron sulfate particles because the solubility of the solute in different solvents and the speed of molecular movement are different, thus affecting the loading capacity and product purity.
[0047] According to some embodiments of the present invention, in step S1, the concentration of iron in the dispersion is 0.2-5 mol / L.
[0048] According to some embodiments of the present invention, in step S1, the concentration of iron in the dispersion is 0.3-2.3 mol / L.
[0049] According to some embodiments of the present invention, in step S1, the concentration of iron in the dispersion is approximately 0.33 mol / L, 0.44 mol / L, 1.33 mol / L, or 2.21 mol / L.
[0050] According to some embodiments of the present invention, in step S1, the molar ratio of sodium, iron and sulfur in the dispersion is 1-3:2:3.
[0051] According to some embodiments of the present invention, in step S1, the molar ratio of sodium to iron in the dispersion is 1-1.5:1.
[0052] According to some embodiments of the present invention, in step S1, the molar ratio of sodium to iron in the dispersion is 1.2 to 1.26:1, for example, 1.24 to 1.25:1.
[0053] According to some embodiments of the present invention, in step S1, the molar ratio of sodium, iron and sulfur in the dispersion is approximately 2:2:3.
[0054] Adjusting the sodium content in the dispersion will alter the molar ratio of the elements in the nano-sized sodium ferric sulfate particles to a certain extent, which in turn will affect the loading speed and loading capacity of the nano-sized sodium ferric sulfate particles on the conductive carrier to a certain extent. Specifically, when other conditions are the same, the loading capacity and the concentration of the sodium source show a certain degree of positive correlation.
[0055] According to some embodiments of the present invention, in step S1, the temperature of the solvothermal reaction is 60-200°C.
[0056] According to some embodiments of the present invention, in step S1, the temperature of the solvothermal reaction is 130-150°C, for example, about 140°C.
[0057] According to some embodiments of the present invention, in step S1, the temperature of the solvothermal reaction is 60-120°C.
[0058] According to some embodiments of the present invention, in step S1, the temperature of the solvothermal reaction is 80-100°C.
[0059] According to some embodiments of the present invention, in step S1, the duration of the solvothermal reaction is 2 to 24 hours.
[0060] According to some embodiments of the present invention, in step S1, the duration of the solvothermal reaction is 6 to 12 hours, for example, about 8 hours.
[0061] The product of the solvothermal reaction includes the conductive carrier and the sodium iron sulfate precursor (hereinafter referred to as the solid product) supported on the surface of the conductive carrier.
[0062] According to some embodiments of the present invention, step S1 further comprises cooling, washing, and drying the obtained solid product after the solvent thermal reaction.
[0063] The cooling includes cooling to room temperature. This temperature has no significant effect on the performance of the self-supporting positive electrode and is only considered from the perspective of experimental safety.
[0064] The cleaning comprises washing with ethanol and water in sequence;
[0065] The drying atmosphere for the solid product is air.
[0066] According to some embodiments of the present invention, in step S2, the temperature of the annealing treatment is 200-400°C.
[0067] According to some embodiments of the present invention, in step S2, the temperature of the annealing treatment is 300-400°C, for example, about 350°C.
[0068] According to some embodiments of the present invention, in step S2, the annealing treatment lasts for 8 to 48 hours.
[0069] According to some embodiments of the present invention, in step S2, the annealing treatment lasts for 35 to 40 hours, for example, about 36 hours.
[0070] According to some embodiments of the present invention, in step S2, the annealing treatment lasts for 12 to 24 hours, for example, about 18 hours.
[0071] According to some embodiments of the present invention, in step S2, the heating rate of the annealing treatment is 0.5-10°C / min.
[0072] According to some embodiments of the present invention, in step S2, the heating rate of the annealing treatment is 1-4°C / min, for example, 2-3°C / min.
[0073] According to some embodiments of the present invention, in step S2, the atmosphere of the annealing treatment is at least one of nitrogen, argon and hydrogen.
[0074] According to some embodiments of the present invention, when the atmosphere of the annealing process includes hydrogen, the volume percentage of the hydrogen is 5-10%.
[0075] According to an embodiment of the third aspect of the present invention, a sodium ion battery is provided, comprising the self-supporting positive electrode.
[0076] Since the sodium ion battery adopts all the technical solutions of the self-supporting positive electrode of the above embodiment, it has at least all the beneficial effects brought by the technical solutions of the above embodiment.
[0077] That is, the platform voltage, energy density, power density, rate performance and cycle performance of the sodium ion battery are significantly improved.
[0078] According to some embodiments of the present invention, the sodium ion battery further comprises a negative electrode, and a separator disposed between the self-supporting positive electrode and the negative electrode.
[0079] According to some embodiments of the present invention, the active material of the negative electrode includes at least one of sodium metal and graphite.
[0080] According to some embodiments of the present invention, the membrane comprises a glass fiber membrane.
[0081] According to some embodiments of the present invention, the sodium ion battery further comprises an electrolyte, wherein the electrolyte infiltrates the self-supporting positive electrode, the negative electrode and the separator.
[0082] According to some embodiments of the present invention, the electrolyte includes a sodium salt and an electrolyte solvent. The sodium salt includes sodium hexafluorophosphate. The electrolyte solvent includes an ester solvent. The concentration of the sodium salt in the electrolyte is approximately 1 mol / L.
[0083] According to some embodiments of the present invention, the operating voltage range of the sodium ion battery is 2~4.5V.
[0084] When the negative electrode of the sodium ion battery is sodium metal, the test voltage range is 2-4.5V, and the test current is 1C, the first efficiency is 75-91.6%, for example, 80%, 80%, or 90%.
[0085] When the negative electrode of the sodium ion battery is sodium metal, the test voltage range is 2-4.5V, and the test current is 1C, the first-cycle discharge capacity is 60-105mAh / g. For example, it can be about 80mAh / g, 90mAh / g, or 100mAh / g.
[0086] When the negative electrode of the sodium ion battery is sodium metal, the test voltage range is 2-4.5V, and the test current is 1C, the capacity retention rate after 500 cycles is ≥65%. It can be as high as 95%. For example, it can be approximately 90%, 85%, or 80%. This demonstrates that the sodium ion battery (self-supporting positive electrode) provided by the present invention has good cycle performance.
[0087] When the negative electrode of the sodium ion battery is sodium metal, the test voltage range is 2-4.5V, and the test current is 10C. The percentage of the capacity at 500 cycles to the capacity at 1C is ≥65%, reaching 97.3%. This demonstrates that the sodium ion battery (self-supporting positive electrode) provided by the present invention has excellent high-rate cycling performance.
[0088] According to an embodiment of the fourth aspect of the present invention, there is provided an application of the sodium ion battery in the fields of digital products, power batteries and energy storage batteries.
[0089] According to some embodiments of the present invention, the power battery field includes at least one of electric vehicles and electric bicycles.
[0090] According to some embodiments of the present invention, the field of digital products includes mobile electronic communication devices.
[0091] According to some embodiments of the present invention, the energy storage battery field includes energy storage power stations.
[0092] Unless otherwise specified, the term “about” in the present invention means that the error is allowed to be within the range of ±2%. For example, about 100 is actually 100±2%×100.
[0093] Unless otherwise specified, “between” in the present invention includes the number itself, for example, “between 2 and 3” includes the endpoint values 2 and 3.
[0094] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be obvious from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0095] The above and / or additional aspects and advantages of the present invention will become apparent and readily understood from the following description of the embodiments with reference to the accompanying drawings, in which:
[0096] FIG1 is a SEM image of the carbon cloth obtained in step D1 of Example 1 of the present invention;
[0097] FIG2 is a SEM image of the self-supporting positive electrode obtained in Example 1 of the present invention;
[0098] FIG3 is a SEM image of the material obtained in Comparative Example 1 of the present invention.
[0099] FIG4 shows the cycle performance of sodium ion batteries comprising the products obtained in Example 1 of the present invention and Comparative Example 1, respectively.
[0100] FIG5 is an impedance diagram of the self-supporting positive electrode obtained in the embodiment of the present invention and the positive electrode including the product obtained in Comparative Example 1. Best Mode for Carrying Out the Invention
[0101] The following will clearly and completely describe the concept and technical effects of the present invention in conjunction with the embodiments to fully understand the purpose, features and effects of the present invention. Obviously, the embodiments described are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.
[0102] In the description of the present invention, reference to terms such as "one embodiment," "some embodiments," "illustrative embodiments," "examples," "specific examples," or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the exemplary expressions of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in any one or more embodiments or examples.
[0103] Example 1
[0104] This embodiment prepares a self-supporting positive electrode, and the specific steps are as follows:
[0105] D1. First, cut the carbon cloth (conductive carrier) into 2 cm × 4 cm pieces. Ultrasonic cleaning was performed using acetone and ethanol, followed by washing with deionized water to a pH of 7. The carbon cloth was then dried at 60°C.
[0106] D2. Dissolve 1.4g of sodium bicarbonate, 10.1g of ferrous sulfate, and 4.7g of sodium sulfate in 50mL of deionized water. Immerse the treated carbon cloth obtained in step D1 in this mixed dispersion and place it in a hydrothermal kettle with a 100mL inner liner. React at 100°C for 8h. The solid product is a carbon cloth loaded with the Na2Fe2(SO4)3 precursor.
[0107] D3. The solid product obtained in step D2 was annealed at 350°C for 24 h in an argon atmosphere at a heating rate of 2°C / min to obtain a self-supporting positive electrode. The sodium iron sulfate loading was 7 mg / cm 2 .
[0108] In this example, the loading capacity is measured by weighing the weight difference between the self-supporting positive electrode and the conductive support obtained in step D1, and dividing the difference by the area of the conductive support. Unless otherwise specified, the loading capacity calculation method in other examples is the same as that in this example. Modes for Carrying Out the Invention
[0109] In order to verify the influence of the type of conductive carrier on the self-supporting positive electrode, the present invention provides Examples 2 to 4, specifically:
[0110] Example 2
[0111] This embodiment prepares a self-supporting positive electrode, which differs from Example 1 in that:
[0112] Replace the conductive support with carbon paper;
[0113] The loading of sodium iron sulfate in the obtained self-supporting positive electrode is 7 mg / cm 2 .
[0114] Example 3
[0115] This embodiment prepares a self-supporting positive electrode, which differs from Example 1 in that:
[0116] Replace the conductive carrier with nickel foam;
[0117] The loading of sodium iron sulfate in the obtained self-supporting cathode is about 7 mg / cm 2 .
[0118] Example 4
[0119] This embodiment prepares a self-supporting positive electrode, which differs from Example 1 in that:
[0120] Replace the conductive support with a copper mesh;
[0121] The loading of sodium iron sulfate in the obtained self-supporting positive electrode is 7 mg / cm 2 .
[0122] In order to verify the effects of the types and amounts of sodium source, iron source and sulfur source on the self-supporting positive electrode, the present invention provides Examples 5 to 12, specifically:
[0123] Example 5
[0124] This embodiment prepares a self-supporting positive electrode, which differs from Example 1 in that:
[0125] In step D2, the amount of sodium bicarbonate used is 0.6 g.
[0126] The loading of sodium iron sulfate in the obtained self-supporting positive electrode is 6 mg / cm 2 .
[0127] Example 6
[0128] This embodiment prepares a self-supporting positive electrode, which differs from Example 1 in that:
[0129] In step D2, 1.4 g of sodium bicarbonate in the example was replaced with 1.37 g of anhydrous sodium acetate;
[0130] The loading of sodium iron sulfate in the obtained self-supporting positive electrode is 7 mg / cm 2 .
[0131] Example 7
[0132] This embodiment prepares a self-supporting positive electrode, which differs from Example 1 in that:
[0133] In step D2, 1.4 g of sodium bicarbonate, 10.1 g of ferrous sulfate, and 4.7 g of sodium sulfate used in Example 1 were replaced with 7 g of sodium bicarbonate and 13.33 g of ferric sulfate;
[0134] The loading of sodium iron sulfate in the obtained self-supporting positive electrode is 7 mg / cm 2 .
[0135] Example 8
[0136] This embodiment prepares a self-supporting positive electrode, which differs from Example 1 in that:
[0137] In step D2, the 10.1 g ferrous sulfate and 4.7 g sodium sulfate used in Example 1 were replaced with 8.45 g ferrous chloride and 12 g sodium bisulfate, and sodium bicarbonate was not used;
[0138] The loading of sodium iron sulfate in the obtained self-supporting positive electrode is 8 mg / cm 2 .
[0139] Example 9
[0140] This embodiment prepares a self-supporting positive electrode, which differs from Example 1 in that:
[0141] In step D2, 1.4 g of sodium bicarbonate and 4.7 g of sodium sulfate used in Example 1 were replaced with 7 g of sodium bicarbonate and 4.4 g of ammonium sulfate;
[0142] The loading of sodium iron sulfate in the obtained self-supporting positive electrode is 7 mg / cm 2 .
[0143] Example 10
[0144] This embodiment prepares a self-supporting positive electrode, which differs from Example 1 in that:
[0145] In step D2, 1.4 g of sodium bicarbonate, 10.1 g of ferrous sulfate, and 4.7 g of sodium sulfate used in Example 1 were replaced with 3.33 g of sodium hydroxide, 5.33 g of ferric oxide, and 17.4 g of potassium sulfate;
[0146] The loading of sodium iron sulfate in the obtained self-supporting positive electrode is 7 mg / cm 2 .
[0147] Example 11
[0148] This embodiment prepares a self-supporting positive electrode, which differs from Example 1 in that:
[0149] In step D2, no sodium bicarbonate is added;
[0150] The loading of sodium iron sulfate in the obtained self-supporting positive electrode is 6 mg / cm 2 .
[0151] Example 12
[0152] This embodiment prepares a self-supporting positive electrode, which differs from Example 1 in that:
[0153] In step D2, 1.4 g of sodium bicarbonate, 10.1 g of ferrous sulfate, and 4.7 g of sodium sulfate used in Example 1 were replaced with 4.2 g of sodium bicarbonate, 10.1 g of ferrous sulfate, and 4.0 g of sodium bisulfate;
[0154] The loading of sodium iron sulfate in the obtained self-supporting positive electrode is 7 mg / cm 2 .
[0155] In order to verify the effects of the solute concentration and solvent type in the mixed dispersion obtained in step D2 on the self-supporting positive electrode, the present invention provides Examples 13 to 16, specifically:
[0156] Example 13
[0157] This embodiment prepares a self-supporting positive electrode, which differs from Example 1 in that:
[0158] In step D2, the volume of water used was 30 mL;
[0159] The loading of sodium iron sulfate in the obtained self-supporting positive electrode is 15 mg / cm 2 .
[0160] Example 14
[0161] This embodiment prepares a self-supporting positive electrode, which differs from Example 1 in that:
[0162] In step D2, the volume of water used is 150 mL, and the corresponding volume of the hydrothermal reactor lining is 300 mL;
[0163] The loading of sodium iron sulfate in the obtained self-supporting positive electrode is 6 mg / cm 2 .
[0164] Example 15
[0165] This embodiment prepares a self-supporting positive electrode, which differs from Example 1 in that:
[0166] In step D2, the volume of water used is 200 mL, and the corresponding hydrothermal kettle lining volume is 300 mL;
[0167] The loading of sodium iron sulfate in the obtained self-supporting positive electrode is 4 mg / cm 2 .
[0168] Example 16
[0169] This embodiment prepares a self-supporting positive electrode, which differs from Example 1 in that:
[0170] In step D2, the solvent used in the dispersion is ethanol;
[0171] The loading of sodium iron sulfate in the obtained self-supporting positive electrode is 2 mg / cm 2 .
[0172] In order to verify the effect of the solvothermal reaction conditions in step D2 on the self-supporting positive electrode, the present invention provides Examples 17 to 20, specifically:
[0173] Example 17
[0174] This embodiment prepares a self-supporting positive electrode, which differs from Example 1 in that:
[0175] In step D2, the temperature of the solvothermal reaction is 80°C;
[0176] The loading of sodium iron sulfate in the obtained self-supporting positive electrode is 7 mg / cm 2 .
[0177] Example 18
[0178] This embodiment prepares a self-supporting positive electrode, which differs from Example 1 in that:
[0179] In step D2, the temperature of the solvothermal reaction is 140°C;
[0180] The loading of sodium iron sulfate in the obtained self-supporting positive electrode is 8 mg / cm 2 .
[0181] Example 19
[0182] This embodiment prepares a self-supporting positive electrode, which differs from Example 1 in that:
[0183] In step D2, the solvent thermal reaction time is 6 h;
[0184] The loading of sodium iron sulfate in the obtained self-supporting positive electrode is 7 mg / cm 2 .
[0185] Example 20
[0186] This embodiment prepares a self-supporting positive electrode, which differs from Example 1 in that:
[0187] In step D2, the solvent thermal reaction time is 12 h;
[0188] The loading of sodium iron sulfate in the obtained self-supporting positive electrode is 7 mg / cm 2 .
[0189] In order to verify the effect of the annealing reaction conditions in step D3 on the self-supporting positive electrode, the present invention provides Examples 21 to 32, specifically:
[0190] Example 21
[0191] This embodiment prepares a self-supporting positive electrode, which differs from Example 1 in that:
[0192] In step D3, the annealing temperature is 200° C. The loading capacity is the same as that in Example 1. That is, the annealing process does not affect the loading capacity.
[0193] Example 22
[0194] This embodiment prepares a self-supporting positive electrode, which differs from Example 1 in that:
[0195] In step D3, the temperature of the annealing treatment is 300°C.
[0196] Example 23
[0197] This embodiment prepares a self-supporting positive electrode, which differs from Example 1 in that:
[0198] In step D3, the temperature of the annealing treatment is 400°C.
[0199] Example 24
[0200] This embodiment prepares a self-supporting positive electrode, which differs from Example 1 in that:
[0201] In step D3, the heating rate of the annealing treatment is 1°C / min.
[0202] Example 25
[0203] This embodiment prepares a self-supporting positive electrode, which differs from Example 1 in that:
[0204] In step D3, the heating rate of the annealing treatment is 3°C / min.
[0205] Example 26
[0206] This embodiment prepares a self-supporting positive electrode, which differs from Example 1 in that:
[0207] In step D3, the heating rate of the annealing treatment is 4°C / min.
[0208] Example 27
[0209] This embodiment prepares a self-supporting positive electrode, which differs from Example 1 in that:
[0210] In step D3, the annealing treatment lasts for 12 hours.
[0211] Example 28
[0212] This embodiment prepares a self-supporting positive electrode, which differs from Example 1 in that:
[0213] In step D3, the annealing treatment lasts for 18 hours.
[0214] Example 29
[0215] This embodiment prepares a self-supporting positive electrode, which differs from Example 1 in that:
[0216] In step D3, the annealing treatment lasts for 36 hours.
[0217] Example 30
[0218] This embodiment prepares a self-supporting positive electrode, which differs from Example 1 in that:
[0219] In step D3, the annealing treatment lasts for 48 hours.
[0220] Example 31
[0221] This embodiment prepares a self-supporting positive electrode, which differs from Example 1 in that:
[0222] In step D3, the annealing process is performed in a nitrogen atmosphere.
[0223] Example 32
[0224] This embodiment prepares a self-supporting positive electrode, which differs from Example 1 in that:
[0225] In step D3, the annealing treatment is performed in an atmosphere of a nitrogen / hydrogen mixed gas (volume ratio of 9.5:0.5). Industrial Applicability
[0226] Application Example 1
[0227] This application example provides a series of sodium-ion batteries (half-cells), specifically:
[0228] The steps of preparing sodium ion battery are as follows:
[0229] The self-supporting positive electrodes obtained in Examples 1 to 32 were punched out into electrode discs with a diameter of 8 mm as battery positive electrode sheets for standby use; the sodium ion batteries were numbered according to the examples from which their positive electrodes were derived.
[0230] Press the sodium metal into thin sheets and cut into 12mm diameter discs to be used as the negative electrode;
[0231] A glass fiber film was used as the separator, and 1M sodium hexafluorophosphate dissolved in a solvent of propylene carbonate and fluoroethylene carbonate (volume ratio 95:5) was used as the electrolyte. In an inert gas-protected glove box, the prepared positive electrode, separator, and battery negative electrode were tightly stacked in sequence, and the electrolyte was added dropwise to completely soak the separator. The stacked part was then encapsulated into a button battery casing to complete the battery assembly.
[0232] Comparative Example 1
[0233] This comparative example prepared a sodium ferric sulfate, and the specific steps were as follows:
[0234] A mixed solution consisting of 1.4 g of sodium bicarbonate, 10.1 g of ferrous sulfate, 4.7 g of sodium sulfate, and 50 mL of deionized water was directly placed into a hydrothermal autoclave with an inner lining volume of 100 mL and reacted at 100 °C for 8 h. The obtained solid product was then annealed at 350 °C for 24 h under an argon atmosphere with a heating rate of 2 °C / min.
[0235] Comparative Example 2
[0236] This comparative example prepared a sodium iron sulfate / carbon composite material, and the specific steps were as follows:
[0237] A mixed solution consisting of 1.4 g of sodium bicarbonate, 10.1 g of ferrous sulfate, 4.7 g of sodium sulfate, and 50 mL of deionized water was placed in a hydrothermal autoclave with an inner lining volume of 100 mL, and 1.8 g of glucose was added. The reaction was carried out at 100 ° C for 8 hours. The obtained solid material was then calcined under an argon atmosphere and annealed at 350 ° C for 24 hours with a heating rate of 2 ° C / min. During the annealing process, glucose underwent carbonylation to obtain a glucose-derived sodium ferrous sulfate / carbon composite material.
[0238] Comparative Example 3
[0239] This comparative example prepared a sodium iron sulfate / carbon nanotube composite material, and the specific steps were as follows:
[0240] A mixed solution consisting of 1.4 g of sodium bicarbonate, 10.1 g of ferrous sulfate, 4.7 g of sodium sulfate, and 50 mL of deionized water was directly placed in a hydrothermal autoclave with an inner lining volume of 100 mL, and 1.2 g of carbon nanotubes with a length of approximately 10 μm were added. The reaction was carried out at 100°C for 8 h. The obtained solid material was then calcined under an argon atmosphere and annealed at 350°C for 24 h with a heating rate of 2°C / min to obtain a sodium ferrous sulfate / carbon nanotube composite material.
[0241] Comparative Application Example 2
[0242] In this comparative example, the positive electrode was prepared using the materials obtained in Comparative Examples 1 to 3 as the positive electrode active material, and a sodium sheet was used as the negative electrode to prepare a sodium ion battery half-cell. The specific difference from Application Example 1 is:
[0243] Positive electrode preparation: Add the positive electrode active material, carbon black, and polyvinylidene fluoride to an appropriate amount of nitrogen-methyl pyrrolidone at a mass ratio of 8:1:1 and grind thoroughly to obtain a uniform slurry. Apply the slurry evenly to the surface of aluminum foil (positive electrode current collector) and vacuum dry. Cut the dried electrode sheet into 8mm diameter discs, compact them, and use them as the battery's positive electrode.
[0244] In this example, the obtained sodium ion battery is named according to the source of its positive electrode active material.
[0245] Test Example 1
[0246] This example uses visual inspection and scanning electron microscopy to test the appearance and structure of the conductive carrier used in the example, the self-supporting positive electrode obtained, and the positive electrode active material obtained in the comparative example. Specifically:
[0247] Due to the presence of the conductive carrier, the self-supporting positive electrode obtained in the examples of the present invention is flaky. Its structure is determined by the original shape of the conductive carrier and can be used directly to prepare electrodes without the addition of other substances. In contrast, the materials obtained in Comparative Examples 1-3 are powdered. For use in sodium-ion batteries, a conductive agent and a binder must be added for homogenous coating, which requires the introduction of additional inactive substances.
[0248] Furthermore, the carbon cloth used in Example 1 of the present invention (obtained in step D1) has a smooth surface and is almost free of visible impurities; its SEM image is shown in Figure 1. Compared with the carbon cloth used in Example 1 of the present invention, the self-supporting positive electrode obtained has a large number of particles with a particle size of 500-1000 nm accumulated on the surface, and the roughness is improved; and the distribution and particle size uniformity of the particles are high; this indicates that sodium ferric sulfate is uniformly deposited on the surface of the conductive support; the specific morphology is shown in Figure 2. In the remaining examples, the morphology of the conductive support used and the self-supporting positive electrode obtained is comparable to that of Example 1, the difference being the difference in the morphology of the conductive support itself, which will not be elaborated here. The morphology of the product obtained in Comparative Example 1 shows that the sodium ferric sulfate grows and agglomerates to form block materials of varying sizes, the specific morphology of which is shown in Figure 3. The morphology of the materials obtained in Comparative Examples 2-3 is comparable to that of Comparative Example 1. Even if a common carbon source such as carbon tubes is used as the growth site, there are still problems such as agglomeration and poor particle size consistency. This shows that the presence of a large-sized conductive carrier in the present invention can significantly improve the uniformity of the obtained sodium ferric sulfate particles and reduce their particle size, providing a basis for a high specific surface area and high activity positive electrode.
[0249] Test Example 2
[0250] This example tests the electrochemical performance of sodium-ion batteries obtained from the application examples and comparative application examples. Constant-current charge-discharge tests were conducted using a BTSDA test system from Shenzhen Xinwei Electronics Co., Ltd. in a constant temperature and humidity chamber (25°C, 35%), with a test voltage range of 2-4.5V. The sodium-ion batteries were cycled 500 times at current densities of 1C and 10C (1C = 120mA / g). The test results are shown in Table 1.
[0251] Table 1 Performance of sodium ion batteries obtained from application examples and comparative application examples
[0252] No. 1C first efficiency (%) 1C first discharge (mAh / g) 1C, 500 cycle capacity retention rate (%) 10C, 500 cycle Capacity retention rate relative to 1C, 500 cycle (%) Example 1 91.6103.494.497.3 Example 2 88.593.187.188.2 Example 3 87.287.390.591.3 Example 4 89.682.190.792.5 Example 5 88.795.791.193.5 Example 6 86.293.389.391.3 Example 7 87.387.18 9.689.2 Example 884.789.988.193.0 Example 986.392.989.394.6 Example 1087.191.786.087.0 Example 1185.173.783.984.0 Example 1284.991.985.588.1 Example 1386.784.883.485.2 Example 1489.687.984.591.7 Example 1583.876.078.480.3 Example 1681.963.865.367.4 Example 1783.175.680.878.0 Example 1887.687.283.687.4 Example 1982.484.585.286.9 Example 2087.985.783.688.6 Example 2175.772.071.973.3 Example 2281.886.577.682.1 Example 2386.192.578.684.3 Example 2485.394.185.793.2 Example 2588.196.587.291.8 Example 2687.79 0.890.192.5Example 2780.879.375.181.9Example 2881.881.078.183.0Example 2983.288.883.088.5Example 3082.393.485.790.8Example 3185.792.886.890.7Example 3287.591.688.292.1Comparative Example 183.272.273.882.3Comparative Example 282.877.572.281.3Comparative Example 380.075.470.280.1
[0253] The test results in Table 1 show that the self-supporting positive electrode provided by the present invention has a higher first-cycle coulombic efficiency and discharge specific capacity of the sodium ion battery assembled (between 70-110 mAh / g), and the capacity retention rate is higher after 500 stable cycles.
[0254] Examples 1-4 verify the effect of the type of conductive carrier on the performance of the self-supporting positive electrode. When carbon paper is used as a conductive carrier, its rate performance decreases. When nickel foam and copper mesh are used as conductive carriers, their discharge specific capacity and cycle capacity retention rate decrease. The results show that the product grown on carbon cloth has better conductivity than the product grown on the surface of carbon paper, and the electronic conductivity is improved, so the rate performance of the product is improved. When nickel foam and copper mesh are used as carriers, since the carrier itself has a large weight, it affects the overall performance of the electrode, resulting in a decrease in the overall specific capacity of the electrode.
[0255] Examples 5-12 verified the effects of sodium source, iron source, sulfur source, and Na:Fe:S molar ratio on the performance of the self-supporting positive electrode. The results showed that the types of sodium source, iron source, and sulfur source had little effect on the electrochemical performance of the sodium ion battery, because different types of sodium source, iron source, and sulfur source only provided sodium ions, iron ions, and sulfate ions, and the remaining ions did not participate in the reaction. However, the Na:Fe:S molar ratio had a certain effect on the electrochemical performance. When the proportion of sodium source was too low, the conversion rate and purity of the product decreased, resulting in a decrease in the cycle performance of the sodium ion battery.
[0256] Examples 13-15 examined the effect of the dispersion concentration used in the solvothermal reaction on the performance of the self-supporting cathode. The results showed that using too high or too low a dispersion concentration for the solvothermal reaction resulted in differences in the electrochemical performance of the self-supporting cathode. When the dispersion concentration was too high, the formed product tended to agglomerate on the support surface, resulting in performance degradation. When the dispersion concentration was too low, the product growth rate was affected, leading to decreased product loading and performance.
[0257] Example 16 and Example 1 verified the effect of the dispersion solvent type used in the solvothermal reaction on the performance of the self-supporting cathode. The results showed that differences in solvent type may have a certain impact on the electrochemical performance of the self-supporting cathode. Using ethanol as the solvent caused a sharp decline in the electrochemical performance of the product. This is because the solubility of the reactants in ethanol solvent is very low, resulting in low product purity and conversion rate, which affects product performance.
[0258] Examples 17-18 verified the effect of the solvothermal reaction temperature, and Examples 19-20 verified the effect of the solvothermal reaction duration. The results show that when the solvothermal reaction temperature is too low (<100°C), the cycle performance of the resulting self-supporting cathode decreases, but when the temperature is ≥100°C, the effect of temperature on performance is almost negligible. The reason is that after the temperature is ≥100°C, the growth environment provided has met the growth requirements of the product. In addition, the duration of the solvothermal reaction has little effect on the performance of the self-supporting cathode.
[0259] Examples 21-23 examined the effect of annealing temperature on the performance of self-supporting cathodes. The results showed that annealing temperature had a certain impact on the electrochemical performance of the self-supporting cathode. Specifically, lower annealing temperatures resulted in poorer electrochemical performance. This is because lower annealing temperatures lead to lower crystallinity and less stable material structures.
[0260] Examples 24-26 verified the effect of the heating rate during the annealing process on the performance of the self-supporting positive electrode. The results showed that the heating rate had little effect on its electrochemical performance.
[0261] Examples 27-30 examined the effect of annealing duration on the performance of self-supporting cathodes. The results showed that varying annealing durations had a certain impact on electrochemical performance. Specifically, shorter annealing durations resulted in decreased electrochemical performance of the resulting self-supporting cathodes. This is because shorter annealing durations lead to lower crystallinity and less stable structures.
[0262] Examples 31-32 verified the effect of annealing atmosphere on the performance of the self-supporting positive electrode. The results showed that different atmospheres had little effect on the electrochemical performance of the obtained self-supporting positive electrode.
[0263] Comparative Examples 1-3 used conventional coating methods to prepare sodium ion battery positive electrodes whose positive electrode active materials were Na2Fe2(SO4)3. The preparation process of sodium ion batteries is more complicated. In addition:
[0264] Comparative Example 1 is a Na2Fe2(SO4)3 sodium ion battery positive electrode material without a conductive carrier load. It can be seen that its discharge specific capacity is low, and the capacity retention rate after 500 cycles at different rates is low. The reason may be that the conductive properties deteriorate after the lack of a conductive carrier, and the added conductive agent is not enough to compensate for the decline in conductive performance. In addition, the uniformity of the particles decreases, so the isotropy of the internal stress of the sodium ion battery decreases during the charge and discharge process, and thus the cycle performance decreases. The overall performance is inferior to that of Example 1. The cycle process of the sodium ion battery represented by Example 1 and Comparative Example 1 is shown in Figure 4.
[0265] Comparative Examples 2-3 are carbon-composite Na2Fe2(SO4)3 sodium-ion battery positive electrode materials derived from different carbon sources without conductive carrier loading. It can be seen that their first-cycle coulombic efficiency is low, and their specific capacity and cycle stability are poor. The reason may be the formation of agglomeration between the material particles, poor carbon material composite effect, and low material utilization.
[0266] This example also conducted electrochemical impedance spectroscopy (EIS) testing using a Swiss Autolab electrochemical workstation. The test frequency range was 10 MHz to 100 kHz, measuring the charge transfer resistance and ion diffusion coefficient of the electrodes (from the application examples or comparative application examples) during different charge and discharge cycles.
[0267] The results show that in the high-frequency region, the self-supporting positive electrode provided by the present invention (e.g., Example 1) has a smaller semicircle radius than the electrode made of Na2Fe2(SO4)3 positive electrode material without a conductive carrier (e.g., Comparative Example 1), indicating that the self-supporting positive electrode provided by the present invention has lower charge transfer impedance and better conductivity. A comparison of the performance results of Example 1 and Comparative Example 1 is shown in Figure 5.
[0268] In summary, the self-supporting positive electrode provided by the present invention, through structural design, when used in sodium ion batteries, can significantly improve the cycle performance, rate performance, voltage, capacity and energy density of sodium ion batteries.
[0269] Since the sodium ion battery including the self-supporting positive electrode provided by the present invention has good performance, it is expected to be widely used in the fields of digital products, power batteries and energy storage batteries.
[0270] While the embodiments of the present invention have been described in detail above with reference to the accompanying drawings, the present invention is not limited to the embodiments described above. Various modifications may be made within the scope of knowledge possessed by a person skilled in the art without departing from the spirit of the present invention. Furthermore, the embodiments of the present invention and the features thereof may be combined with one another unless there is a conflict.
Claims
1. A self-supporting positive electrode, characterized in that: The self-supporting positive electrode comprises a conductive carrier and nano-sodium iron sulfate particles loaded on the conductive carrier.
2. The self-supporting positive electrode according to claim 1, characterized in that The conductive carrier includes at least one of a carbon-based film, a metal mesh and a conductive polymer film; preferably, the conductive carrier includes at least one of carbon cloth, carbon paper, porous carbon, graphene film, carbon nanotube film, nickel foam, copper foam, nickel mesh, copper mesh, titanium mesh, platinum mesh, stainless steel mesh, platinum-rhodium-palladium alloy mesh, platinum-rhodium alloy mesh, platinum-iridium alloy mesh, palladium-nickel alloy mesh, aluminum-magnesium mesh, polyethylene-derived composite materials, polyvinyl alcohol-derived composite materials, polyester-derived composite materials, polyimide-derived composite materials, polyurethane-derived composite materials, polyethylene glycol-derived composite materials, polydimethylsiloxane-derived composite materials and polyacrylonitrile-derived composite materials.
3. The self-supporting positive electrode according to claim 1 or 2, characterized in that: The loading amount of the nano sodium iron sulfate particles on the conductive carrier is 2-15 mg / cm 2 .
4. A method for preparing a self-supporting positive electrode according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: S1. Immersing the conductive support in a dispersion comprising a sodium source, an iron source and a sulfur source to perform a solvothermal reaction; S2. Annealing the solid product obtained in step S1.
5. The preparation method according to claim 4, characterized in that: In step S1, the molar ratio of sodium, iron and sulfur in the dispersion is 1-3:2:3; preferably, in step S1, the concentration of iron in the dispersion is 0.2-5 mol / L; preferably, the solvent of the dispersion includes at least one of water, methanol, anhydrous ethanol, acetone, ethylene glycol and pyridine.
6. The preparation method according to claim 4, characterized in that: In step S1, the sodium source includes sodium sulfate, sodium bisulfate, sodium carbonate, sodium bicarbonate, sodium acetate, sodium nitrite, sodium oxalate, sodium persulfate, sodium hydroxide, sodium pyrosulfate, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium pyrosulfite, sodium pyrophosphate, sodium hydrogen phthalate, sodium hydrogen oxalate, sodium sulfite, sodium sorbate, trisodium phosphate, sodium gluconate, sodium oleate, and at least one of the hydrates of the above sodium sources; preferably, the iron source includes ferrous sulfate, ferrous oxide, ferrous chloride, ferrous sulfate, ferrous hydroxide, trisodium phosphate, ferrous sulfate, trisodium phosphate ... Ferrous oxide, ferric chloride, ferric hydroxide, and at least one of the hydrates of the above iron sources; preferably, the sulfur source includes ferric sulfate, ferrous sulfite, sodium bisulfate, potassium sulfate, ammonium sulfate, ferrous dithionite, ferrous thiosulfate, ferrous dithionate, ferrous tetrasulfide, sodium sulfate, sodium sulfite, sodium dithionite, sodium thiosulfate, sodium dithionate, sulfurous acid, sulfuric acid, ammonium persulfate, potassium persulfate, sodium persulfate, sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, and at least one of the hydrates of the above sulfur sources.
7. The preparation method according to claim 4, characterized in that: In step S1, the temperature of the solvent thermal reaction is 60-200°C.
8. The preparation method according to claim 4, characterized in that: In step S2, the temperature of the annealing treatment is 200-400°C; preferably, the duration of the annealing treatment is 8-48 hours.
9. A sodium ion battery, characterized in that: The sodium ion battery comprises the self-supporting positive electrode as described in any one of claims 1 to 3 or the self-supporting positive electrode prepared by the preparation method as described in any one of claims 4 to 8.
10. Application of the sodium ion battery as claimed in claim 9 in the fields of digital products, power batteries and energy storage batteries.
Citation Information
Patent Citations
Sodium-ion battery positive pole Na2+2xFe2-x(SO4)3@ carbon composite material and preparing method thereof
CN105355886A
Sodium ferrous sulfate / graphene composite positive electrode material for sodium ion battery, and preparation method thereof
CN106848236A
Method of preparation of self-supporting anode for ammonium vanadate / nickel foam sodium-ion battery
CN106935807A
Flexible self-supporting Na3(VO)2(PO4)2F material, and preparation method and application thereof
CN111009661A
Sodium ferrous sulfate / carbon nanotube composite positive electrode material, preparation method and sodium ion battery
CN115172724A
Cited By
Cathode carbon nanosheet of fast-charging sodium-ion battery as well as preparation method and application of cathode carbon nanosheet