Composite sodium-supplement agent, and positive electrode sheet and preparation method therefor, and electric device

By using a composite sodium replenishing agent on the positive electrode sheet of the sodium ion energy storage device, gradient sodium replenishment of the oxidation potential gradient is realized, which solves the problem of improving the electrochemical performance of the sodium ion energy storage device in the existing technology, simplifies the process flow, and reduces the cost. Cost and environmental impact.

WO2024222141A1PCT designated stage expired Publication Date: 2024-10-31XIAMEN HITHIUM ENERGY STORAGE TECHNOLOGY CO LTD

Patent Information

Application Number
PCT/CN2024/076093
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-02-05
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

It is difficult for the existing sodium supplementation technology to realize sodium supplementation in all stages from the initialization stage of the sodium ion energy storage device to the subsequent cycle charge and discharge stage. As a result, it is difficult to improve the electrochemical performance of the sodium ion energy storage device, and the industrial application is costly and environmentally friendly. , security and stability challenges.

Method used

Use a composite sodium supplementing agent, including a first sodium supplementing agent and a second sodium supplementing agent. The first sodium supplementing agent has an oxidation potential of less than 3.9V, and the second sodium supplementing agent has an oxidation potential of 3.9V to 4.4V. Through the positive electrode An oxidation potential gradient is formed on the chip, realizing gradient sodium supplementation, simplifying the process, and is suitable for industrial applications.

Benefits of technology

It realizes the full-stage sodium supplementation of the sodium ion energy storage device during the entire charge and discharge process, improves the electrochemical performance, simplifies the process, reduces the cost and environmental impact, and takes into account safety and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024076093_31102024_PF_FP_ABST
    Figure CN2024076093_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of energy storage apparatuses, in particular to a sodium-supplement agent, and a positive electrode sheet and preparation method therefor, and an electric device. The composite sodium-supplement agent is located on a positive electrode sheet of a sodium-ion energy storage apparatus, and the composite sodium-supplement agent comprises: a first sodium-supplement agent and a second sodium-supplement agent, wherein the first sodium-supplement agent has a first oxidation potential, and the second sodium-supplement agent has a second oxidation potential, the first oxidation potential being smaller than 3.9 V, and the second oxidation potential ranging from 3.9 V to 4.4 V. The composite sodium-supplement agent is provided on the positive electrode sheet, and therefore the advantages, such as realizing simple operation and processing, reducing treatment procedures and involving no harsh processing conditions, are achieved, and industrial application can be implement. In addition, the composite sodium-supplement agent has a relatively comprehensive sodium supplement function, and can form a certain gradient of oxidation potential, thereby achieving the effect of gradient sodium supplementation. Full-stage sodium supplementation can be performed on a sodium-ion energy storage apparatus from an initial formation stage to a subsequent cyclic charging / discharging stage, such that the electrochemical performance of the sodium-ion energy storage apparatus is improved throughout the whole process from formation to cyclic charging / discharging.
Need to check novelty before this filing date? Find Prior Art

Description

Composite sodium supplement, positive electrode sheet and preparation method thereof, and electrical equipment

[0001] Related cross-references

[0002] This disclosure claims priority to a Chinese patent application filed with the Patent Office of China on April 28, 2023, with application number 2023104829268 and public name “Compound sodium supplement, positive electrode sheet, preparation method thereof, and electrical equipment”, the entire contents of which are incorporated by reference into this disclosure. Technical Field

[0003] The present application relates to the technical field of energy storage devices, and in particular to a composite sodium supplement, a positive electrode sheet and a preparation method thereof, and electrical equipment. Background Art

[0004] Because sodium loss occurs in the cathode of sodium-ion energy storage devices, sodium replenishment technology can be used to replenish the lost sodium. However, current sodium replenishment technologies are either difficult to commercialize or have limited functionality. This makes it difficult to achieve sodium replenishment throughout the entire process from initial formation to subsequent charge and discharge cycles. Consequently, it is difficult to improve the electrochemical performance of sodium-ion energy storage devices from formation to charge and discharge cycles.

[0005] Summary of the Invention

[0006] The embodiments of the present application disclose a composite sodium supplement, a positive electrode sheet, a preparation method thereof, and an electrical device. The composite sodium supplement can be industrially applied and can achieve gradient sodium supplementation, achieving sodium supplementation in all stages from the initial formation stage to the subsequent cyclic charge and discharge stage, and can improve the electrochemical performance of the sodium ion energy storage device from the entire process of formation to cyclic charge and discharge.

[0007] In order to achieve the above objectives, in the first aspect, the present application discloses a composite sodium supplement, which is provided in the positive electrode of a sodium ion energy storage device, and the composite sodium supplement includes: a first sodium supplement and a second sodium supplement, the first sodium supplement having a first oxidation potential, the second sodium supplement having a second oxidation potential, the first oxidation potential being less than 3.9V, and the second oxidation potential being 3.9V to 4.4V.

[0008] In a second aspect, the present application discloses a positive electrode sheet of a sodium ion energy storage device, wherein the operating voltage of the sodium ion energy storage device is 1.5V to 4.1V, and the positive electrode sheet includes the composite sodium supplement agent as described in the first aspect.

[0009] In a third aspect, the present application discloses a method for preparing the positive electrode sheet according to the second aspect, the method comprising the following steps:

[0010] providing a positive electrode current collector;

[0011] coating the second sodium supplement, the positive electrode active material, the second conductive agent and the second solvent on the positive electrode current collector and drying the mixture to obtain a positive electrode active material layer;

[0012] The first sodium supplementing agent, the first conductive agent and the first solvent are mixed and processed onto the surface of the positive electrode active material layer to obtain a sodium supplementing layer.

[0013] As an optional embodiment, in an embodiment of the present application, in the step of mixing the first sodium supplement agent, the first conductive agent and the first solvent and processing them onto the positive electrode substrate and drying them to obtain the sodium supplement layer, electrostatic spraying or electrostatic spinning is used for processing.

[0014] In a fourth aspect, the present application also discloses an electrical device, which includes an electrical device body and a sodium ion energy storage device arranged in the electrical device body, the sodium ion energy storage device includes the positive electrode sheet as described in the second aspect, and the sodium ion energy storage device is used to supply power to the electrical device body.

[0015] Compared with the prior art, the present invention has the following advantages:

[0016] The composite sodium supplement provided in the embodiment of the present application forms a certain oxidation potential gradient by having a first sodium supplement and a second sodium supplement with different oxidation potentials, thereby achieving a gradient sodium supplement effect for the sodium ion energy storage device. Moreover, since the composite sodium supplement is provided on the positive electrode of the sodium ion energy storage device, it has the advantages of being easy to operate and process, reducing the processing steps, and having no harsh processing conditions, and is therefore suitable for industrial applications. Among them, the first oxidation potential of the first sodium supplement is less than or equal to 3.9V, and the second oxidation potential of the second sodium supplement is 3.9V to 4.4V.

[0017] The charging voltage of the sodium ion energy storage device during the initialization (Formation, which refers to the first charging of the sodium ion energy storage device after high temperature aging, used to activate the battery, during the initialization phase, a SEI film (solid electrolyte interface film) will be formed on the surface of the negative electrode. It is generally not higher than 3.9V, and the SOC (State of Charge, state of charge) is within 60%, and the first sodium supplement has a lower first oxidation potential of less than 3.9V, which can compensate for sodium before the second sodium supplement, thereby compensating for the sodium loss caused by the formation of the SEI film in the formation stage, and improving the initial charge and discharge efficiency of the sodium ion energy storage device. The oxidation potential of the sodium ion energy storage device in the subsequent multiple charge and discharge cycle stages is relatively high. The second sodium supplement with a second oxidation potential of 3.9V to 4.4V is set. Due to its higher oxidation potential, it can make up for the sodium loss in the charge and discharge cycle process, thereby improving the cycle performance of sodium ions. As a result, the sodium ion energy storage device can achieve full-stage sodium supplementation from the initial formation stage to the subsequent cyclic charge and discharge stage, so that the electrochemical performance of the sodium ion energy storage device can be improved throughout the entire process from the formation stage to the cyclic charge and discharge. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the following briefly introduces the drawings required for use in the embodiments. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0019] FIG1 is a schematic structural diagram of a positive electrode sheet disclosed in an embodiment of the present application;

[0020] FIG2 is a schematic structural diagram of another positive electrode sheet disclosed in an embodiment of the present application;

[0021] FIG3 is a flow chart of the method for preparing the positive electrode sheet disclosed in the embodiment of the present application.

[0022] Reference numerals: 100, positive electrode sheet; 1, positive electrode current collector; 2, positive electrode active material layer; 3, sodium supplement layer. DETAILED DESCRIPTION

[0023] The following will be combined with the drawings in the embodiments of this application to clearly and completely describe the technical solutions in the embodiments of this application. Obviously, the embodiments described are only part of the embodiments of this application, not all of the embodiments. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.

[0024] In this application, terms such as "upper," "lower," "left," "right," "front," "back," "top," "bottom," "inner," "outer," "center," "vertical," "horizontal," "transverse," and "longitudinal" indicate positions or locations based on the positions or locations shown in the accompanying drawings. These terms are primarily intended to better describe this application and its embodiments and are not intended to limit the devices, elements, or components indicated to having a specific orientation, or to being constructed or operated in a specific orientation.

[0025] Furthermore, some of the above terms may be used to express other meanings besides indicating a position or location. For example, the term "on" may also be used to indicate a dependency or connection in certain circumstances. Those skilled in the art will understand the specific meanings of these terms in this application based on the specific circumstances.

[0026] Furthermore, the terms "installed," "disposed," "provided with," "connected," and "connected" should be interpreted broadly. For example, they can refer to fixed connections, removable connections, or integral structures; mechanical connections or electrical connections; direct connections, indirect connections through an intermediary, or internal communication between two devices, elements, or components. Those skilled in the art will understand the specific meanings of these terms in this application based on the specific circumstances.

[0027] Furthermore, the terms "first," "second," etc., are primarily used to distinguish between different devices, elements, or components (which may or may not be of the same type and configuration), and are not intended to indicate or imply the relative importance or quantity of the devices, elements, or components indicated. Unless otherwise specified, "plurality" means two or more.

[0028] The technical solution of the present application will be further described below with reference to the embodiments and drawings.

[0029] Since sodium loss occurs in the positive electrode of sodium-ion energy storage devices, sodium replenishment technology can be used to replenish the lost sodium to a certain extent. Some sodium replenishment technologies cannot take into account cost, environmental protection, safety and stability factors, making it difficult to achieve industrial application. Specifically, physical pre-sodiumization is simple and convenient to operate, but it is difficult to ensure safety; electrochemical pre-sodiumization can obtain a stable SEI film, but the process flow is cumbersome; chemical reaction pre-sodiumization can also form a uniform and dense SEI film, but it has certain requirements for the atmosphere and the solvent is expensive; setting a sodium replenisher on the diaphragm increases the diaphragm treatment process and increases the difficulty of operation. Some sodium replenishment technologies have a single function, and it is difficult for sodium-ion energy storage devices to achieve full-stage sodium replenishment from the initial formation stage to the subsequent cyclic charge and discharge stage, and thus it is difficult to improve the electrochemical performance of sodium-ion energy storage devices from the formation stage to the cyclic charge and discharge stage.

[0030] This application addresses the problems existing in the above-mentioned existing sodium supplementation technology and proposes the following technical solutions.

[0031] In the first aspect, the present application provides a composite sodium supplement, which is located on the positive electrode of the sodium ion energy storage device. The composite sodium supplement includes: a first sodium supplement and a second sodium supplement, the first sodium supplement has a first oxidation potential, the second sodium supplement has a second oxidation potential, the first oxidation potential is less than 3.9V, and the second oxidation potential is 3.9V to 4.4V. Setting the composite sodium supplement directly on the positive electrode is simple to operate, does not require setting special reaction conditions and using expensive solvents, does not have harsh processing conditions, and can reduce the processing steps, and can achieve industrial application. The use of a composite sodium supplement can make up for the disadvantage of the single function of the existing sodium supplement technology. Specifically, the composite sodium supplement has a certain oxidation potential gradient, which can achieve gradient sodium supplementation when the sodium ion energy storage device is working, so that sodium supplementation can be achieved in all stages from the initial formation stage to the subsequent cycle charge and discharge stage, and the electrochemical performance of the sodium ion energy storage device can be improved throughout the entire charge and discharge process.

[0032] It can be understood that the first sodium supplement and the second sodium supplement (like the positive electrode active material) themselves have an oxidation potential range. When the operating voltage of the sodium ion energy storage device reaches the oxidation potential range of the first sodium supplement and the second sodium supplement, the first sodium supplement and the second sodium supplement will undergo an oxidation reaction to release sodium ions and electrons, and the released sodium ions will serve as sodium supplements.

[0033] In some embodiments, the operating voltage of the sodium ion energy storage device is 1.5V to 4.1V, and the charging voltage of the sodium ion energy storage device during the initial formation stage is relatively low, generally not higher than 3.9V. The first sodium supplement has a relatively low first oxidation potential of less than 3.9V, and can undergo an oxidation reaction during the initial formation stage. It can oxidize and release sodium ions before the second sodium supplement performs sodium compensation, thereby compensating for the sodium loss caused by the formation of the SEI film during the formation stage and improving the initial charge and discharge efficiency of the sodium ion energy storage device.

[0034] The working potential of the sodium ion energy storage device in the subsequent cycle stage is relatively high, generally higher than 3.9V. The second sodium supplementer with a second oxidation potential of 3.9V to 4.4V can undergo an oxidation reaction to release sodium ions during the cycle stage, which can replenish the sodium loss during the cycle, thereby improving the cycle performance of sodium ions. The second sodium supplementer can also achieve sodium compensation by increasing the cutoff voltage of the sodium ion energy storage device during the cycle stage, that is, increasing the cutoff voltage during the required time period to perform sodium compensation, which can achieve the effect of intermittent sodium supplementation. As a result, the sodium ion energy storage device can achieve sodium supplementation in all stages from the initial formation stage to the subsequent cyclic charge and discharge stage, thereby improving the electrochemical performance of the sodium ion energy storage device throughout the entire process from the formation stage to the cyclic charge and discharge.

[0035] If the first oxidation potential of the first sodium supplement exceeds 3.9V, it does not meet the operating potential range of the sodium ion energy storage device during the initial formation stage, and oxidative decomposition sodium supplementation cannot be achieved during the initial formation stage. In addition, a large amount of the first sodium supplement will remain on the surface of the positive electrode, resulting in an increase in the impedance of the positive electrode and affecting the electrochemical performance of the sodium ion energy storage device. If the second oxidation potential of the second sodium supplement exceeds 4.4V, it does not meet the operating voltage of the sodium ion energy storage device during the cycling stage and sodium supplementation cannot be achieved during the cycling stage. If the second oxidation potential is lower than 3.9V, the second sodium supplement will be consumed by the reaction during the initial formation stage and sodium supplementation cannot be achieved during the cycling stage, thus failing to achieve the effect of gradient sodium supplementation.

[0036] In some embodiments, the operating voltage of the sodium-ion energy storage device is 1.5V to 4.1V. If the operating voltage is lower than 1.5V, the positive electrode active material on the positive electrode sheet cannot undergo redox reactions, and the sodium-ion battery will not function properly. If the operating voltage is higher than 4.1V, the electrolyte in the sodium-ion energy storage device may decompose under high voltage, and the structure of the positive electrode sheet may also be damaged under high voltage, affecting the cycle life.

[0037] For example, the first oxidation potential may be any value within a range less than or equal to 3.9V, including but not limited to: 0.2V, 0.5V, 0.7V, 1V, 1.2V, 1.5V, 1.7V, 2V, 2.1V, 2.2V, 2.3V, 2.4V, 2.5V, 2.6V, 2.7V, 2.8V, 2.9V, 3V, 3.1V, 3.2V, 3.3V, 3.4V, 3.5V, 3.6V, 3.7V, 3.8V, 3.9V, etc., and the second oxidation potential may be any value within a range less than or equal to 3.9V, including but not limited to: 0.2V, 0.5V, 0.7V, 1V, 1.2V, 1.5V, 1.7V, 2V, 2.1V, 2.2V, 2.3V, 2.4V, 2.5V, 2.6V, 2.7V, 2.8V, 2.9V, 3V, 3.1V, 3.2V, 3.3V, 3.4V, 3.5V, 3.6V, 3.7V, 3.8V, 3.9V, etc. Any value within the range of 3.9V to 4.4V, including but not limited to 3.9V, 3.92V, 3.94V, 3.96V, 3.98V, 4.0V, 4.02V, 4.04V, 4.06V, 4.08V, 4.1V, 4.12V, 4.14V, 4.16V, 4.18V, 4.2V, 4.22V, 4.24V, 4.26V, 4.28V, 4.3V, 4.32V, 4.34V, 4.36V, 4.38V, 4.4V, etc. The operating voltage of the sodium ion energy storage device can be any value within the above range, for example, 1.5V, 2V, 2.5V, 3V, 3.5V, 4.0V, 4.1V, etc.

[0038] Preferably, in some embodiments, the first oxidation potential is less than or equal to 3.8V, and / or the second oxidation potential is between 3.9V and 4.1V, and / or the state of charge (SOC) of the sodium ion energy storage device is less than or equal to 60%, which better matches the operating voltage of the sodium ion energy storage device during the initial formation phase and subsequent cycling phases. During the formation phase, the voltage of the sodium ion energy storage device first rises rapidly to a peak value and then gradually decreases to an equilibrium state. During the cycling phase, the voltage of the sodium ion energy storage device also undergoes dynamic changes. Using the first and second oxidation potentials within the preferred ranges can better match the dynamically changing voltage windows of the sodium ion energy storage device during the formation and cycling phases. The first and second sodium supplements can more accurately undergo staged oxidation reactions, thereby releasing sodium ions and electrons, providing a gradient of sodium supplementation. The second sodium supplement can more accurately coordinate with the dynamically changing voltage to achieve intermittent sodium supplementation. It is understood that the SOC of a sodium ion energy storage device refers to the available charge in the energy storage device, that is, the ratio between the stored charge and the rated capacity of the energy storage device. The voltage of the sodium ion energy storage device at different stages is matched with the SOC, and the SOC of the sodium ion energy storage device is maintained at less than or equal to 60%, so that the first sodium supplement and the second sodium supplement can better play the role of gradient sodium supplement and even full-stage sodium supplement.

[0039] Regarding the materials for the first and second sodium supplements, the main types of sodium compounds include: organic sodium salts, organic sodium salt complexes, inorganic sodium salts, metallic sodium salts, and sodium oxides. Organic sodium salts have poor conductivity; inorganic sodium salts are highly toxic and explosive; metallic sodium salts have low capacity release efficiency; and sodium oxides are difficult to effectively combine with other sodium compounds.

[0040] In some embodiments, the first sodium supplement comprises NaNiO2, NaCrO2, Na2MnO2, NaFeO2, Na x Fe (1-y) Al y O2、Na x Fe (1-y) Ti y O2 (0.8≤x≤2, y≧0) and / or the second sodium supplement includes a mixture of one or more of Na2O2, Na2O, Na3P, Na2C2O2, and Na2C2O4. x Fe (1-y) Al y O2、Na x Fe (1-y) Ti yO2 (0.8≤x≤2, y≧0) is used as the first sodium supplement, which does not produce gas and can reduce the accumulation of impurity by-products, thereby not deteriorating the electrochemical performance. The above-mentioned first sodium supplement is selected to have a lower first oxidation potential, which can be used as a sodium supplement in the formation stage to supplement the sodium loss in the SEI film formation stage and improve the initial charge and discharge efficiency of the sodium ion energy storage device. The second sodium supplement has a high sodium content, high sodium supplement efficiency, and a higher oxidation potential. It can supplement the sodium loss in the cycle process and improve the cycle performance. The second sodium supplement does not produce gas during the sodium ion operation.

[0041] In some embodiments, the molar ratio of the first sodium supplementer to the second sodium supplementer is (2-5):1. The amount of the first sodium supplementer added is mainly determined according to the formation loss of the sodium ion energy storage device, and the amount of the second sodium supplementer added is mainly confirmed according to the cycle target. Below this molar ratio range, the amount of the second sodium supplementer added is too much, and the amount of the first sodium supplementer added is too little. Too much second sodium supplementer will reduce the content of other active substances in the positive electrode sheet, reduce the energy density, increase the polarization of the energy storage device, and accelerate the cycle attenuation; too little first sodium supplementer will not achieve the purpose of improving capacity and first charge and discharge efficiency. Exceeding this molar ratio range, the amount of the first sodium supplementer added is too much, and the second sodium supplementer is too little. Too much first sodium supplementer will increase the impedance of the sodium ion energy storage device, accumulate a large amount of by-products, and deteriorate the performance of the battery cell; too little second sodium supplementer will not provide enough sodium source, and the purpose of improving cycle performance cannot be achieved.

[0042] Illustratively, the molar ratio of the first sodium supplement and the second sodium supplement can be any ratio within the above range, including but not limited to: 2:1, 2.2:1, 2.4:1, 2.6:1, 2.8:1, 3:1, 3.2:1, 3.4:1, 3.6:1, 3.8:1, 4:1, 4.2:1, 4.4:1, 4.6:1, 4.8:1, 5:1, etc.

[0043] Preferably, the ratio of sodium supplement 1 to sodium supplement 2 is controlled within the range of (2-3):1, which can provide sufficient sodium source for the circulation stage, and the circulation capacity retention rate of the sodium ion energy storage device is better.

[0044] In the second aspect, the present application provides a positive electrode sheet of a sodium ion energy storage device, which includes the composite sodium supplement of the first aspect. The first sodium supplement and the second sodium supplement are arranged on the positive electrode sheet, which can directly supplement sodium for the positive electrode sheet, and is highly compatible with the manufacturing process of the positive electrode sheet produced by the sodium ion energy storage device. The process is simple and has low environmental requirements. The total cost depends on the cost of the first sodium supplement and the second sodium supplement materials themselves. The dosage can be determined according to the formation loss and cycle target of the sodium ion energy storage device to control the degree of sodium supplementation. The operation is simple and safe, and can take into account cost, environmental protection, safety and stability factors, thereby realizing industrial application. Sodium supplement agent one and sodium supplement agent two specifically have the following several settings, including but not limited to:

[0045] Referring to Figure 1 , in some embodiments, the positive electrode sheet includes a positive electrode current collector, and a positive electrode active material layer and a sodium supplement layer sequentially disposed on the positive electrode current collector. The positive electrode active material layer includes a second sodium supplement, and the sodium supplement layer includes a first sodium supplement. The first sodium supplement and the second sodium supplement of the present application have the following configurations to achieve gradient sodium supplementation:

[0046] The first type: the positive electrode active material layer 2 has the second sodium-supplementing agent but not the first sodium-supplementing agent, and the sodium-supplementing layer 3 has the first sodium-supplementing agent but not the second sodium-supplementing agent.

[0047] In some embodiments, referring to FIG. 1 , a positive electrode sheet 100 includes a positive electrode current collector 1, a positive electrode active material layer 2, and a sodium-supplementing layer 3 sequentially disposed on the positive electrode current collector 1. The sodium-supplementing layer 3 includes a first sodium-supplementing agent and a second sodium-supplementing agent. It should be noted that in this configuration, the positive electrode active material layer 2 does not include the first and second sodium-supplementing agents.

[0048] Furthermore, in some embodiments, referring to FIG. 2 , the positive electrode sheet 100 is composed of a positive electrode current collector 1 and a positive electrode active material layer 2 disposed on the positive electrode current collector 1 , and the positive electrode active material layer 2 includes a first sodium supplement and a second sodium supplement.

[0049] Preferably, the first setting is adopted, that is, the positive electrode sheet 100 includes a positive electrode current collector 1, and a positive electrode active material layer 2 and a sodium supplement layer 3 sequentially stacked on the positive electrode current collector 1, the positive electrode active material layer 2 only has the second sodium supplement, and the sodium supplement layer 3 only has the first sodium supplement. Thus, the sodium supplement layer 3 is formed directly on the positive electrode active material layer 2, and the first sodium supplement and the second sodium supplement are arranged in different layers. The sodium supplement layer 3 is close to the negative electrode side, and the sodium source generated by the first sodium supplement can move to the negative electrode side as quickly as possible to replenish the sodium consumed in the formation of the SEI film. The first sodium supplement is continuously consumed by redox reactions, so that the sodium supplement layer 3 is gradually consumed during the formation stage. During the cycle stage, the sodium supplement layer 3 can be completely consumed and will not cover the surface of the positive electrode active material layer 2 to increase polarization and affect the cycle stage.

[0050] In some embodiments, the sodium supplement layer further includes a first conductive agent and a first solvent, wherein the mass ratio of the first sodium supplement, the first conductive agent, and the first solvent is 80: (10-15): 150. Below this mass ratio, the first sodium supplement is less, and after the first sodium supplement is decomposed, the content of the first binder and the first conductive agent remaining on the surface is too high, which is not conducive to the improvement of the energy density of the sodium ion energy storage device. At the same time, it will cause the content of inactive substances remaining on the surface of the positive electrode active material layer to be too high, which will increase the polarization of the positive electrode surface. Above this mass ratio, there is too much first sodium supplement, and the proportion of the first binder is small, which easily causes the sodium supplement layer to fall off. The sodium supplement layer also includes a first binder, wherein the mass ratio of the first sodium supplement, the first conductive agent, the first binder, and the first solvent is 80: (10-15): (5-10): 150.

[0051] Illustratively, the mass ratio of the first sodium supplement, the first conductive agent, the first binder and the first solvent may be any ratio within the above range, including but not limited to: 80:10:10:150, 80:11:9:150, 80:12:8:150, 80:13:7:150, 80:14:6:150, 80:15:5:150, etc.

[0052] In some embodiments, the positive electrode active material layer further includes a positive electrode active material, a second conductive agent, and a second solvent, wherein the mass ratio of the second sodium supplement to the positive electrode active material is (1-5):100. Below this mass ratio, the second sodium supplement is too little, making it difficult to replenish sodium during the cycle. Above this mass ratio, the second sodium supplement is too much, increasing the resistance of the positive electrode sheet, reducing sodium ion kinetics, and increasing polarization, which is detrimental to the performance of the battery cell. The positive electrode active material layer also includes a second binder.

[0053] Illustratively, the mass ratio of the second sodium supplement and the positive electrode active material is any value within the above range, including but not limited to: 1:100, 2:100, 3:100, 4:100, 5:100, etc.

[0054] The positive electrode active material can be a transition metal oxide / layered oxide, for example: Na x MO2 (M=Co, Fe, Mn, Ni and their mixtures), such as NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2, can also be a Prussian compound, for example: Na x MA[MB(CN)6]·zH2O (MA and MB are transition metal ions), polyanionic materials, amorphous materials, etc.

[0055] The first binder may be a mixture of one or more of styrene-butadiene rubber, polyvinylidene fluoride, polytetrafluoroethylene, polyvinyl alcohol, polyacrylonitrile, polyacrylic acid, polyacrylate, carboxymethyl cellulose, and sodium alginate, and / or the first conductive agent may be a mixture of one or more of acetylene black, Super-P (conductive carbon black), CNTs (carbon nanotubes), carbon fibers, and graphene, and / or the second binder may be a mixture of one or more of styrene-butadiene rubber, PVDF (polyvinylidene fluoride), polytetrafluoroethylene, polyvinyl alcohol, polyacrylonitrile, polyacrylic acid, polyacrylate, carboxymethyl cellulose, and sodium alginate, and / or the second conductive agent may be a mixture of one or more of acetylene black, Super-P, carbon nanotubes, carbon fibers, and graphene, and / or the first and second solvents may be NMP (N-methylpyrrolidone).

[0056] In a third aspect, the present application provides a method for preparing the positive electrode sheet according to the second aspect, the method comprising the following steps:

[0057] providing a positive electrode current collector;

[0058] A film layer having a composite sodium supplement agent is formed on the positive electrode current collector to form a positive electrode sheet.

[0059] The positive electrode current collector can be aluminum foil made of metallic aluminum.

[0060] In some embodiments, a film layer having a composite sodium supplement agent is formed on the positive electrode current collector, and the steps of forming the positive electrode sheet are as follows:

[0061] coating a mixture of a second sodium supplement, a positive electrode active material, a second conductive agent, a second binder, and a second solvent on the positive electrode current collector and drying the mixture to obtain a positive electrode active material layer;

[0062] A first sodium supplementing agent, a first conductive agent, a second binder and a first solvent are mixed and processed onto the surface of the positive electrode active material layer to obtain a sodium supplementing layer.

[0063] In the step of preparing the sodium supplement layer, the sodium supplement layer is prepared by electrostatic spraying or electrostatic spinning. Preferably, the sodium supplement layer can be prepared by electrostatic spinning technology. The electrostatically spun nanofibers prepared by electrostatic spinning serve as the matrix of the sodium supplement layer, and have the characteristics of large specific surface area and high porosity. The micro / nanoparticles in the first sodium supplement agent, the first conductive agent, and the second binder can be distributed more evenly, preventing the micro / nanoparticles from agglomerating, which is conducive to the release of sodium in the first sodium supplement agent, and improving the sodium supplement efficiency of the first sodium supplement agent per unit volume or unit mass, so that the sodium supplement layer can supplement more sodium, thereby improving the capacity and initial charge and discharge efficiency of the sodium ion energy storage device.

[0064] In a fourth aspect, the present application further provides an electrical device, comprising an electrical device body and a sodium ion energy storage device such as the sodium ion energy storage device of the fourth aspect, disposed on the electrical device body, the sodium ion energy storage device being used to power the device body. The electrical device body comprises a positive electrode and a negative electrode, the positive electrode plate of the secondary energy storage device being electrically connected to the positive electrode of the device, and the negative electrode plate being electrically connected to the negative electrode of the device. The electrical device includes a large-scale grid-level energy storage system, a UPS uninterruptible power supply device, an energy storage base station, an electric vehicle, and the like.

[0065] The technical solution of this application will be further explained below with reference to specific embodiments and experimental data.

[0066] Example 1

[0067] This embodiment provides a sodium ion energy storage device, which is a sodium ion battery.

[0068] The sodium ion battery includes a positive electrode sheet, a negative electrode sheet, an electrolyte and a diaphragm, and the diaphragm is arranged between the positive electrode sheet and the negative electrode sheet.

[0069] The positive electrode sheet includes a current collector, a positive electrode active material layer sequentially stacked on the current collector, and a sodium supplement layer. The sodium supplement layer includes NaNiO2 as a first sodium supplement, PVDF as a first binder, Super P and CNTs as first conductive agents, and NMP as a first solvent. The mass ratio of the first sodium supplement, the first binder, the first conductive agent, and the first solvent is 80:10:10:150.

[0070] The positive electrode active material layer includes Na2O2 as the second sodium supplement, NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2 is used as the positive electrode active material, PVDF is used as the second binder, Super P and CNTs are used as the second conductive agents, and NMP is used as the second solvent. The mass ratio of the second sodium supplement, the positive electrode active material, the second binder, the second conductive agent, and the second solvent is 1:100:2.66:2.66:71.

[0071] The molar ratio of the first sodium supplement to the second sodium supplement is 3:1.

[0072] This embodiment also provides a method for preparing the positive electrode sheet, the method comprising:

[0073] Providing a positive electrode current collector, wherein the positive electrode current collector is an aluminum foil;

[0074] 1 part of the second sodium supplement Na2O2, 100 parts of the positive electrode active material NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3O2, 2.66 parts of the second conductive agent Super P and CNTs, 2.66 parts of the second binder PVDF and 71 parts of the second solvent NMP are mixed and coated on the positive electrode current collector aluminum foil and dried to obtain a positive electrode active material layer;

[0075] 3 parts of the first sodium supplementing agent NaNiO2, 0.375 parts of the first conductive agent Super P and CNTs, 0.375 parts of the second binder PVDF and 5.625 parts of the first solvent NMP were mixed and electrostatically sprayed onto the surface of the positive electrode active material layer to obtain a sodium supplementing layer.

[0076] This embodiment also provides a method for preparing a sodium ion battery, the method comprising:

[0077] preparing the above-mentioned positive electrode sheet with the sodium supplement layer;

[0078] Preparation of the negative electrode sheet of the sodium ion battery: 95 parts of hard carbon, 2.5 parts of Super P, 2.5 parts of CMC (carboxymethyl cellulose) and SBR (styrene-butadiene rubber) are mixed evenly in 80 parts of deionized water, coated on the negative electrode current collector copper foil, and then dried to obtain a dry negative electrode sheet.

[0079] Assembling sodium-ion batteries: The prepared positive electrode sheet with a sodium-supplemented layer was used as the positive electrode, the negative electrode sheet was used as the negative electrode, and porous glass fiber was used as the separator. 1 mol / L NaPF6 (sodium hexafluorophosphate) (ethylene carbonate EC:propylene carbonate PC:dimethyl carbonate DMC=1:1:1, and 5% fluoroethylene carbonate FEC) was used as the electrolyte. The button-type sodium-ion batteries were assembled in an argon glove box with a water oxygen value of less than 0.1 ppm.

[0080] Example 2

[0081] The only difference between Example 2 and Example 1 is that the molar ratio of the first sodium supplement to the second sodium supplement in Example 2 is 2:1.

[0082] Example 3

[0083] The only difference between Example 3 and Example 1 is that the molar ratio of the first sodium supplement to the second sodium supplement in Example 3 is 4:1.

[0084] Example 4

[0085] The only difference between Example 4 and Example 1 is that the molar ratio of the first sodium supplement to the second sodium supplement in Example 4 is 5:1.

[0086] Example 5

[0087] The only difference between Example 5 and Example 1 is that the mass ratio of the second sodium supplement to the positive electrode active material in Example 5 is 2:100.

[0088] Example 6

[0089] The only difference between Example 6 and Example 1 is that the mass ratio of the second sodium supplement to the positive electrode active material in Example 6 is 3:100.

[0090] Example 7

[0091] The only difference between Example 7 and Example 1 is that the mass ratio of the second sodium supplement to the positive electrode active material in Example 7 is 4:100.

[0092] Example 8

[0093] The only difference between Example 8 and Example 1 is that the mass ratio of the second sodium supplement to the positive electrode active material in Example 8 is 5:100.

[0094] Example 9

[0095] The only difference between Example 9 and Example 1 is that the sodium supplement layer is prepared by electrospinning in Example 9.

[0096] Example 10

[0097] The only difference between Example 10 and Example 1 is that the first sodium supplement in Example 10 is NaCrO 2 .

[0098] Example 11

[0099] The only difference between Example 11 and Example 1 is that the first sodium supplement in Example 11 is NaFeO 2 .

[0100] Example 12

[0101] The only difference between Example 1 and Example 1 is that the second sodium supplement in Example 12 is Na2C2O4.

[0102] Example 13

[0103] The only difference between Example 1 and Example 1 is that no sodium supplement layer is provided, and the first sodium supplement agent and the second sodium supplement agent are both mixed in the positive electrode active material layer.

[0104] Example 14

[0105] The only difference between Example 14 and Example 1 is that the first sodium supplement agent and the second sodium supplement agent are both mixed in the sodium supplement layer.

[0106] Comparative Example 1

[0107] The only difference between Comparative Example 1 and Example 1 is that the first sodium supplement and the second sodium supplement are not provided.

[0108] Comparative Example 2

[0109] The only difference between Comparative Example 2 and Example 1 is that the second sodium supplement is not provided.

[0110] Comparative Example 3

[0111] The only difference between Comparative Example 3 and Example 1 is that the first sodium supplement is not provided.

[0112] Comparative Example 4

[0113] The only difference between Comparative Example 1 and Example 1 is that the first sodium supplement in Comparative Example 1 is Na2O2, and the second sodium supplement is NaNiO2.

[0114] Table 1: Related data of Examples and Comparative Examples

[0115] Experimental testing

[0116] The sodium ion batteries in the above examples and comparative examples were subjected to electrochemical performance tests. The sodium ion batteries were subjected to constant current charge and discharge tests on an energy storage device measuring device, with a test voltage of 4.0V to 1.5V (vs Na / Na + The cyclic voltammetry test was carried out on a battery tester at a test voltage of 4.0 V to 1.5 V (vs Na / Na + ). The test results are as follows:

[0117] Table 2: Electrochemical performance test results of examples and comparative examples

[0118] From the records in Table 1 and Table 2, it can be seen that the first cycle discharge capacity, the first charge and discharge efficiency, and the capacity retention rate of Examples 1 to 14 are all higher than those of Comparative Example 1 in which the first sodium supplement and the second sodium supplement are not provided. It can be seen that the provision of the first sodium supplement and the second sodium supplement in the positive electrode sheet can significantly improve the electrochemical performance of the sodium ion battery.

[0119] Furthermore, when comparing Example 1 with Comparative Example 2, which did not include a second sodium supplement in the positive electrode active material layer, the capacity retention rate of Example 1 after 500 cycles was 95.4%, while that of Comparative Example 2 was 86%. This represents a nearly 10% decrease in capacity retention during the cycling phase compared to Example 1. This indicates that the second sodium supplement can effectively achieve gradient sodium supplementation during the cycling phase, thereby improving the cycling capacity retention rate of the sodium-ion battery.

[0120] Furthermore, compared with Example 1 and Comparative Example 3, Comparative Example 3 does not have a sodium supplement layer or a first sodium supplement agent. The first-cycle discharge capacity of Example 1 is 128.9mAh / g, the first charge and discharge efficiency is 98.2%, and the capacity retention rate after 500 cycles is 95.4%. The first-cycle discharge capacity of Comparative Example 3 dropped to 125.4mAh / g, a decrease of 3.5mAh / g, and the first charge and discharge efficiency also dropped to 88.8%, a decrease of 9.4%. The capacity retention rate after 500 cycles was 88.0%, a decrease of 7.4%. It can be seen from this that the first sodium supplement agent is not provided, which affects the sodium supplementation in the first charge and discharge formation stage, and further affects the electrochemical performance in the subsequent cycle stage.

[0121] Compared with Example 1 and Comparative Example 4, the first sodium supplement in Example 1 is the second sodium supplement in Comparative Example 4, and the second sodium supplement in Example 1 is the first sodium supplement in Comparative Example 4. That is, in Comparative Example 4, Na2O2 with a high oxidation potential is set in the sodium supplement layer, and NaNiO2 with a low oxidation potential is set in the positive electrode active material layer. The first cycle discharge capacity of Comparative Example 4 dropped to 124.6 mAh / g, a decrease of 4.3 mAh / g, the first charge and discharge efficiency was 88.2%, a decrease of 10%, and the capacity retention rate after 500 cycles was 85.7%, a decrease of 9.7%. Among the various comparative examples, the performance data of Comparative Example 4 dropped most significantly. It can be seen that the sodium supplement with a higher oxidation potential in the sodium supplement layer not only fails to supplement sodium, but also increases the impedance of the positive electrode sheet and reduces the conductivity of ions and electrons. A sodium supplement with a lower oxidation potential is set in the positive electrode active material layer and is consumed in the formation stage. Under the barrier of the sodium supplement layer, a large amount of by-products are easily accumulated in the positive electrode active material layer, which deteriorates the performance of the sodium ion battery.

[0122] In Examples 1 to 4, appropriately reducing the molar ratio of the first sodium supplement and the second sodium supplement, that is, appropriately increasing the amount of the second sodium supplement, is more conducive to compensating sodium in the cycle stage and is beneficial to improving the capacity retention rate of the sodium ion battery after 500 cycles.

[0123] In Examples 1 and 5 to 8, appropriately reducing the mass ratio of the second sodium supplement and the positive electrode active material is also beneficial to improving the capacity retention rate of the sodium ion battery after 500 cycles. Therefore, the amount of the second sodium supplement needs to take into account and balance the amount of the first sodium supplement and the positive electrode active material. Excessive or insufficient use will lead to a decrease in the capacity retention rate of the sodium ion battery after 500 cycles.

[0124] Among the various embodiments, Example 9 uses an electrostatic spinning process to make a sodium-filling layer, and its various electrochemical performance improvements are the most significant. The first-cycle discharge capacity of the sodium-ion battery of Example 9 is 129.5mAh / g, the first charge and discharge efficiency is 99.3%, and the capacity retention rate after 500 cycles is 96.4%. Compared with Comparative Example 1 (corresponding to 125.6mAh / g, 88.4%, and 82.5%), the discharge capacity is increased by 3.9mAh / g, the first charge and discharge efficiency is increased by nearly 10%, and the capacity retention rate is increased by 13.9%. It can be seen that the electrostatic spinning process for making a sodium-filling layer can significantly improve the various performances of sodium-ion batteries compared to the electrostatic spraying process.

[0125] In Examples 1, 10, and 11, the first sodium supplement in Example 1 is NaNiO2, in Example 10 it is NaCrO2, and in Example 11 it is NaFeO2. Based on the molecular weights of Ni, Cr, and Fe, the efficiency of sodium supplementation during the formation phase is ranked as NaCrO2 > NaFeO2 > NaNiO2. Therefore, the initial charge and discharge efficiencies of Examples 10 and 11 are slightly higher than those of Example 1. To balance the initial discharge capacity and capacity retention after 500 cycles, NaNiO2 is the preferred first sodium supplement.

[0126] Compared with Example 12 and Comparative Example 1, the second sodium supplement in Example 1 is Na2O2, while the second sodium supplement in Example 12 is Na2C2O4. Example 12 also improves the electrochemical performance of sodium ions, but the improvement is not as good as that in Example 1. Na2O2 has a high sodium content, has a better sodium supplement efficiency than Na2C2O4, and does not generate gas during the circulation stage.

[0127] Compared with Comparative Example 1, in Example 1 and Example 13, the first sodium supplement agent in Example 1 was located in the sodium supplement layer, while the second sodium supplement agent was located in the positive electrode active material layer. In Example 13, both the first and second sodium supplement agents were located in the positive electrode active material layer. The first and second sodium supplement agents in Example 13 also significantly improved the sodium supplement effect during the formation stage, resulting in higher initial charge and discharge efficiency and first-cycle discharge capacity, and slightly increased capacity retention, but the improvement was not as significant as in Example 1.

[0128] Compared with Comparative Example 1, Example 1 and Example 14, in Example 1, the first sodium supplement is set in the sodium supplement layer, and the second sodium supplement is set in the positive electrode active material layer. In Example 14, the first sodium supplement and the second sodium supplement are both in the sodium supplement layer. Example 14 can achieve effective sodium supplementation in the formation stage, and can significantly improve the first-cycle discharge capacity and the first charge and discharge efficiency, but its capacity retention rate after 500 cycles is slightly improved. It can be seen that arranging the first sodium supplement and the second sodium supplement respectively in the sodium supplement layer and the positive electrode active material layer can effectively take into account the sodium supplementation in the formation stage and the cycle stage, thereby being able to more comprehensively improve the electrochemical performance of the sodium ion battery.

[0129] The above is a detailed introduction to the composite sodium supplement, positive electrode sheet and preparation method thereof, and electrical equipment disclosed in the embodiments of the present application. Specific examples are used in this article to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the composite sodium supplement, positive electrode sheet and preparation method thereof, electrical equipment and its core ideas of the present application: At the same time, for general technical personnel in this field, based on the ideas of the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A composite sodium supplement, It is characterized in that The composite sodium supplement is used for the positive electrode of a sodium ion energy storage device. The composite sodium supplement includes: a first sodium supplement and a second sodium supplement. The first sodium supplement has a first oxidation potential, and the second sodium supplement has a second oxidation potential. The first oxidation potential is less than 3.9V, and the second oxidation potential is 3.9V to 4.4V.

2. The composite sodium supplement according to claim 1, It is characterized in that The first oxidation potential is less than or equal to 3.8V, and / or the second oxidation potential is 3.9V to 4.1V.

3. The composite sodium supplement according to claim 1, It is characterized in that The first sodium supplement comprises NaNiO 2 、NaCrO 2 、Na 2 MnO 2 、NaFeO 2 、Na x Fe (1-y) Al y O 2 、Na x Fe (1-y) Ti y O 2 (0.8≤x≤2, y≧0) or more, and the second sodium supplement comprises Na 2 O 2 、Na 2 O、Na 3 P, Na 2 C 2 O 2 、Na 2 C 2 O 4 A mixture of one or more.

4. The composite sodium supplement according to claims 1 to 3, It is characterized in that The molar ratio of the first sodium supplement to the second sodium supplement is (2-5):

1.

5. A positive electrode sheet for a sodium ion energy storage device, It is characterized in that The working voltage of the sodium ion energy storage device is 1.5V to 4.1V, and the positive electrode sheet includes the composite sodium supplement agent according to any one of claims 1 to 4.

6. The positive electrode sheet according to claim 5, It is characterized in that The positive electrode sheet includes a positive electrode current collector, and a positive electrode active material layer and a sodium supplement layer disposed on the positive electrode current collector. The positive electrode active material layer includes the second sodium supplement agent, and the sodium supplement layer includes the first sodium supplement agent.

7. The positive electrode sheet according to claim 6, It is characterized in that The sodium supplement layer further includes a first conductive agent and a first solvent, wherein the mass ratio of the first sodium supplement agent, the first conductive agent, and the first solvent is 80:(10-15):

150.

8. The positive electrode sheet according to claim 6, It is characterized in that The positive electrode active material layer further includes a positive electrode active material, a second conductive agent and a second solvent, wherein the mass ratio of the second sodium supplement to the positive electrode active material is (1-5):

100.

9. The positive electrode sheet according to claim 5, It is characterized in that The positive electrode sheet is composed of a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector, and the positive electrode active material layer includes the first sodium supplement and the second sodium supplement.

10. The positive electrode sheet according to claim 5, It is characterized in that The positive electrode sheet includes a positive electrode current collector, and a positive electrode active material layer and a sodium supplement layer sequentially arranged on the positive electrode current collector, and the sodium supplement layer includes the first sodium supplement agent and the second sodium supplement agent.

11. A method for preparing a positive electrode sheet according to any one of claims 5 to 10, It is characterized in that The preparation method comprises the following steps: providing a positive electrode current collector; Mixing the second sodium supplement, the positive electrode active material, the second conductive agent and the second solvent, coating the mixture on the positive electrode current collector and drying the mixture to obtain a positive electrode active material layer; The first sodium supplementing agent, the first conductive agent and the first solvent are mixed and processed onto the surface of the positive electrode active material layer to obtain a sodium supplementing layer.

12. The preparation method according to claim 11, It is characterized in that In the step of mixing the first sodium supplement agent, the first conductive agent and the first solvent and processing them onto the positive electrode substrate and drying them to obtain the sodium supplement layer, electrostatic spraying or electrostatic spinning is used for processing.

13. An electrical device, It is characterized in that The electrical equipment includes an electrical equipment body and a sodium ion energy storage device arranged in the electrical equipment body, the sodium ion energy storage device includes the positive electrode sheet according to any one of claims 5 to 10, and the sodium ion energy storage battery is used to supply power to the electrical equipment body.

Citation Information

Patent Citations

  • Sodium oxide composite sodium-supplementing positive electrode active material, positive electrode material, positive electrode, sodium-ion battery and sodium supplementing method for electric formation of sodium-ion battery

    CN111293289A

  • Sodium-rich transition metal oxide composite sodium-supplementing positive electrode active material, positive electrode material, positive electrode, preparation of positive electrode and application of positive electrode in sodium-ion battery

    CN111293290A

  • Sodium-ion battery positive plate, preparation method thereof and sodium-ion battery

    CN112768699A

  • Positive pole piece and sodium ion battery

    CN115084433A

  • Sodium supplementing composition and sodium ion battery

    CN115117558A

Cited By

  • Method for continuously supplementing sodium to improve cycle performance and application

    CN119230987A

  • Cathode for a sodium-ion battery cell, method for manufacturing such a cathode and method for manufacturing a sodium-ion battery cell

    DE102025116708A1