Composite material, preparation method therefor and lithium battery
By coating the surface of the halide solid electrolyte with a catecholamine autopolymer layer, the problem of poor environmental stability of the halide electrolyte is solved, and the electrochemical stability and interface contact of the battery are improved.
Patent Information
- Application Number
- PCT/CN2024/088072
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-25
- Filing Date
- 2024-04-16
- Publication Date
- 2024-10-31
AI Technical Summary
Halide solid electrolytes have poor environmental stability, which affects their further development and application.
The surface of the halide solid electrolyte is coated with a catecholamine autopolymer layer to form a composite material. This method improves the environmental stability of the material and enhances the interface contact stability with the metal electrode.
Effectively isolates air, improves the environmental stability of the material, improves the interface contact between the solid electrolyte and the metal electrode, and improves the electrochemical stability of the battery.
Smart Images

Figure CN2024088072_31102024_PF_FP_ABST
Abstract
Description
Composite material, preparation method thereof and lithium battery
[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on April 25, 2023, with application number 202310474299.3 and application name “Composite materials and preparation methods thereof, solid electrolyte film and lithium battery”, the entire contents of which are incorporated by reference into this application. Technical Field
[0002] The present application relates to the field of lithium batteries, and in particular to a composite material, a preparation method thereof, and a lithium battery. Background Art
[0003] Solid electrolytes, as a key component of solid-state batteries, together with electrode materials, determine the battery's energy density, cycle life, and safety performance. Inorganic solid electrolytes, with their inherent properties of single-ion conduction and high stability, exhibit advantages such as high thermal stability, low flammability and explosion resistance, high cycling stability, and strong impact resistance, making them the primary direction of future electrolyte development. Inorganic solid electrolytes are primarily classified into three categories: oxides, sulfides, and halides. Oxide-based inorganic solid electrolytes require high sintering temperatures during material synthesis and subsequent battery fabrication to improve poor interfacial contact, which not only easily induces interfacial reactions but also increases battery manufacturing costs. Sulfide-based solid electrolytes are limited by poor environmental stability, poor compatibility with oxide cathodes and electrode materials such as metallic lithium, poor interfacial contact at low voltages, and a narrow electrochemical window. Halide-based solid electrolytes, on the other hand, are considered promising next-generation solid electrolyte materials due to their high lithium ion mobility, good mechanical flexibility, high electrochemical oxidation voltage, good compatibility with high-voltage oxide cathode materials, and simple synthesis methods.
[0004] However, halide solid electrolytes have the problem of poor environmental stability, which affects the further development and application of halide solid electrolytes. Technical Solutions
[0005] Therefore, the present application provides a composite material, a preparation method thereof, and a lithium battery, aiming to solve the problem of poor environmental stability of existing halide solid electrolytes.
[0006] In a first aspect, the present application provides a composite material comprising a halide solid electrolyte and a coating layer coated outside the halide solid electrolyte, wherein the material of the coating layer comprises a catecholamine self-polymer.
[0007] Optionally, in some embodiments of the present application, the monomers of the catecholamine self-polymer include catecholamines and their derivatives, and the catecholamines include one or more of 3,4-dihydroxyphenylethylamine, (R)-4-(2-(methylamino)-1-hydroxyethyl]-1,2-benzenediol, and 1-(3,4-dihydroxyphenyl)-2-aminoethanol.
[0008] Optionally, in some embodiments of the present application, the thickness of the coating layer is 2 to 50 nm.
[0009] Optionally, in some embodiments of the present application, the chemical formula of the halide solid electrolyte is Li a MX b , wherein M is at least one of a Group IIIB metal element and a Group IIIA metal element, X is at least one of F, Cl, Br, and I, 10≥a≥0, and 13≥b≥1.
[0010] Optionally, in some embodiments of the present application, the halide solid electrolyte may be at least one of Li3ScCl3Br3, Li3InCl6, and Li3YBr6.
[0011] In a second aspect, the present application provides a method for preparing a composite material, comprising the following steps:
[0012] mixing a halide solid electrolyte, a coating monomer, and a solvent, wherein the coating monomer self-polymerizes on the surface of the halide solid electrolyte to form a coating layer, thereby obtaining a composite material;
[0013] Wherein, the coating monomer includes catecholamine and its derivatives.
[0014] Optionally, in some embodiments of the present application, the mass ratio of the halide solid electrolyte to the coating monomer is 70:(1-8).
[0015] Optionally, in some embodiments of the present application, the self-polymerization reaction is carried out at a pH of 8.5 to 8.8.
[0016] Optionally, in some embodiments of the present application, the catecholamines include one or more of 3,4-dihydroxyphenylethylamine, (R)-4-(2-(methylamino)-1-hydroxyethyl]-1,2-benzenediol, and 1-(3,4-dihydroxyphenyl)-2-aminoethanol; and / or,
[0017] The chemical formula of the halide solid electrolyte is Li a MX b , wherein M is at least one of a Group IIIB metal element and a Group IIIA metal element, X is at least one of F, Cl, Br, and I, 10≥a≥0, and 13≥b≥1.
[0018] Optionally, in some embodiments of the present application, a halide solid electrolyte, a coating monomer, and a solvent are mixed, and the coating monomer self-polymerizes on the surface of the halide solid electrolyte to form a coating layer, to obtain a composite material, comprising:
[0019] dispersing a halide solid electrolyte in a solvent to obtain an electrolyte dispersion;
[0020] Mixing the electrolyte dispersion and a buffer with a pH of 7.5 to 8.5 to form a mixed system, and then adding an alkaline substance to adjust the pH of the mixed system to 8.5 to 8.8;
[0021] The coating monomer is added into the mixed system, and the pH of the mixed system is controlled to be maintained at 8.5-8.8, and the reaction is carried out. Then, the reaction product is centrifuged and dried to obtain a composite material.
[0022] Optionally, in some embodiments of the present application, in the step of dispersing a halide solid electrolyte in a solvent to obtain an electrolyte dispersion, the concentration of the halide solid electrolyte in the electrolyte dispersion is 0.2 to 1 g / ml.
[0023] Optionally, in some embodiments of the present application, the solvent includes at least one of n-heptane, n-hexane, ethanol, methanol, isopropanol, ethylene glycol and ether.
[0024] Optionally, in some embodiments of the present application, the electrolyte dispersion and a buffer having a pH of 7.5 to 8.5 are mixed to form a mixed system, and then an alkaline substance is added to adjust the pH of the mixed system to 8.5 to 8.8.
[0025] The buffer comprises at least one of Tris-HCl buffer, 4-hydroxyethylpiperazineethanesulfonic acid, N-tris(hydroxymethyl)methylglycine, phosphoric acid, citric acid, carbonic acid, acetic acid, and barbituric acid.
[0026] Optionally, in some embodiments of the present application, the mass ratio of the halide solid electrolyte to the buffer is 70:(1-4).
[0027] Optionally, in some embodiments of the present application, the alkaline substance includes one or more of an inorganic base and an organic base, the inorganic base is selected from one or more of alkali metal oxides, alkali metal hydroxides, alkali metal bicarbonates, alkali metal carbonates, alkaline earth metal oxides, alkaline earth metal hydroxides, and alkaline earth metal bicarbonates; the organic base is selected from one or more of alkali metal salts of organic acids, alkali metal salts of alcohols, amine compounds, and alkylammonium hydroxides.
[0028] Optionally, in some embodiments of the present application, the inorganic base is selected from one or more of sodium hydroxide, potassium hydroxide, lithium hydroxide, calcium hydroxide, sodium oxide, potassium oxide, calcium oxide, sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, calcium bicarbonate, and barium hydroxide; the alkali metal salt of the organic acid includes one or more of sodium acetate and potassium acetate; the alkali metal salt of the alcohol includes one or more of sodium ethanol and potassium ethanol; the alkylamine compound includes one or more of ethylenediamine, octylamine, dioctylamine, trioctylamine, and oleylamine; the alkylammonium hydroxide includes one or more of tetramethylammonium hydroxide, tetraethylammonium hydroxide, and tetrapropylammonium hydroxide.
[0029] Optionally, in some embodiments of the present application, a coating monomer is added to the mixed system, and the pH of the mixed system is controlled to be maintained at 8.5 to 8.8, and the reaction is carried out, and then the reaction product is centrifuged and dried to obtain a composite material.
[0030] The reaction temperature is 20-80°C; and / or,
[0031] The reaction time is 0.5 to 24 hours.
[0032] Optionally, in some embodiments of the present application, the centrifugal speed is 2000-15000 r / min, and the time is 2-5 min.
[0033] Optionally, in some embodiments of the present application, a halide solid electrolyte, a coating monomer and a solvent are mixed, and the coating monomer self-polymerizes on the surface of the halide solid electrolyte to form a coating layer. The step of obtaining the composite material is carried out under an inert atmosphere, and the inert atmosphere includes one or more of nitrogen, helium and argon.
[0034] In a third aspect, the present application also proposes a lithium battery comprising a positive electrode, a solid electrolyte film and a negative electrode, wherein the material of the solid electrolyte film comprises a composite material, and the composite material comprises the composite material described above, or is prepared by the preparation method described above.
[0035] The technical solution provided in the present application, by coating a catecholamine self-polymer layer on the surface of the halide electrolyte, not only does not affect the structural characteristics of the halide solid electrolyte, but also can play a role in isolating the air, thereby effectively improving the environmental stability of the material; at the same time, the catecholamine self-polymer has good softness, and as a coating layer it improves the surface softness of the halide electrolyte. The solid electrolyte film made of the composite material has good contact with the active particles, thereby improving the interface contact stability between the solid electrolyte and the metal electrode, and enhancing the electrochemical stability of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.
[0037] FIG1 is a TEM image of the composite material proposed in an embodiment of the present application;
[0038] FIG2 is a schematic flow chart of a method for preparing a solid electrolyte film according to an embodiment of the present application;
[0039] FIG3 is an impedance spectrum of the electrical conductivity of the solid electrolyte film obtained in Example 1;
[0040] FIG4 is a second cycle charge and discharge curve diagram of the lithium battery prepared in Example 1;
[0041] FIG5 is a second cycle charge and discharge curve diagram of the lithium battery prepared in Comparative Example 1;
[0042] FIG6 is a schematic flow chart of a method for preparing a solid electrolyte film according to another embodiment of the present application;
[0043] FIG7 is a schematic structural diagram of a lithium battery proposed in an embodiment of the present application;
[0044] Reference numerals: 100 - lithium battery; 10 - positive electrode; 20 - solid electrolyte film; 30 - negative electrode.
[0045] Implementation Methods of the Application
[0046] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative work are within the scope of protection of this application. In addition, it should be understood that the specific embodiments described herein are only used to illustrate and explain the present application and are not used to limit the present application.
[0047] In this application, unless otherwise specified, directional words such as "upper" and "lower" refer specifically to the directions of the drawings in the accompanying drawings. In addition, in the description of this application specification, the term "including" means "including but not limited to".
[0048] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity and should not be understood as a hard limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numbers within the range. For example, the description of a range from 1 to 6 should be considered to have specifically disclosed sub-ranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which applies regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0049] In this application, "and / or" describes the association relationship between associated objects, indicating that three relationships can exist. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural.
[0050] In this application, "at least one" means one or more, and "plurality" means two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple.
[0051] The technical solution of this application is implemented as follows:
[0052] In a first aspect, the present application provides a composite material, as shown in FIG1 , wherein the composite material includes a halide solid electrolyte and a coating layer coated outside the halide solid electrolyte, wherein the material of the coating layer includes catecholamine self-polymer.
[0053] The technical solution provided in the present application plays a role in isolating air by coating a catecholamine self-polymer layer on the surface of the halide electrolyte, thereby effectively improving the environmental stability of the material; at the same time, the catecholamine self-polymer has good softness, and as a coating layer, it improves the surface softness of the halide electrolyte. The solid electrolyte film 20 made of the composite material has good contact with the active particles, thereby improving the interface contact stability between the solid electrolyte and the metal electrode, and enhancing the electrochemical stability of the battery.
[0054] The catecholamine self-polymer refers to a self-polymer product formed by the oxidation self-polymerization of catecholamine compounds. It has strong adhesion and can adhere well to the surface of the halide solid electrolyte to form a coating layer. The coating layer can partially coat the halide solid electrolyte or completely coat the halide solid electrolyte, which is not limited in this application. In some preferred embodiments, the coating layer completely encapsulates the halide solid electrolyte, further improving the environmental stability of the material and its compatibility with metallic lithium.
[0055] The catecholamine refers to an amine compound containing a catechol (i.e., catechol) structure, which has a dihydroxybenzene nucleus (two hydroxyl groups are located in the ortho position), and the benzene nucleus has an amino-containing side chain. The catecholamine and its derivatives can be oxidized and self-polymerized under mild weak alkaline wet conditions to form catecholamine self-polymers with extremely strong adhesion. In some embodiments, the monomers of the catecholamine self-polymer include one or more of 3,4-dihydroxyphenylethylamine (CAS: 51-61-6) and its derivatives, (R)-4-(2-(methylamino)-1-hydroxyethyl]-1,2-benzenediol (CAS: 51-43-4) and its derivatives, 1-(3,4-dihydroxyphenyl)-2-aminoethanol (CAS: 51-41-2) and its derivatives. The self-polymerization reaction of these materials is easy to control, with fewer by-products, the prepared coating has the best adhesion and insulation effect, and will not affect the properties of the halide solid electrolyte itself.
[0056] The chemical formula of the halide solid electrolyte is Li a MX b , wherein M is at least one of a Group IIIB metal element and a Group IIIA metal element, X is at least one of F, Cl, Br, and I, 10≥a≥0, 13≥b≥1; for example, the halide solid electrolyte can be Li3ScCl3Br3, Li3InCl6, Li3YBr6, etc.
[0057] In some embodiments, the coating layer has a thickness of 2 to 50 nm.
[0058] In a second aspect, the present application provides a method for preparing a composite material. Referring to FIG. 2 , the method comprises the following steps:
[0059] S100, mixing a halide solid electrolyte, a coating monomer, and a solvent, wherein the coating monomer self-polymerizes on the surface of the halide solid electrolyte to form a coating layer, thereby obtaining a composite material;
[0060] Wherein, the coating monomer includes catecholamine and its derivatives.
[0061] In some embodiments of the present application, the mass ratio of the halide solid electrolyte and the coating monomer is 70: (1 to 8). For example, the mass ratio of the two can be 70:1, 70:2, 70:3, 70:4, 70:5, 70:6, 70:7, 70:8 and values between any two values listed above. Within this range, it can be ensured that the coating layer formed by the polymerization of the coating monomer fully coats the halide solid electrolyte and has a certain thickness, which helps to improve the environmental stability of the material and its compatibility with metallic lithium, thereby ensuring the material optimization effect.
[0062] In some embodiments, the self-polymerization reaction is carried out at a pH of 8.5 to 8.8. This pH helps promote the reaction of the coating monomers to form a coating layer, thereby improving the insulation effect of the coating layer. The pH of the acid-base environment can be 8.5, 8.6, 8.7, 8.8, or any value between any two of the above values.
[0063] In some embodiments, the coating monomer includes one or more of 3,4-dihydroxyphenylethylamine (CAS: 51-61-6) and its derivatives, (R)-4-(2-(methylamino)-1-hydroxyethyl]-1,2-benzenediol (CAS: 51-43-4) and its derivatives, and 1-(3,4-dihydroxyphenyl)-2-aminoethanol (CAS: 51-41-2) and its derivatives.
[0064] In some embodiments, the chemical formula of the halide solid electrolyte is Li a MX b , wherein M is at least one of a Group IIIB metal element and a Group IIIA metal element, X is at least one of F, Cl, Br, and I, 10≥a≥0, 13≥b≥1; for example, the halide solid electrolyte can be Li3ScCl3Br3, Li3InCl6, Li3YBr6, etc.
[0065] Referring to FIG. 6 , in some embodiments, step S100 may be implemented as follows:
[0066] S10, dispersing a halide solid electrolyte in a solvent to obtain an electrolyte dispersion;
[0067] S20, mixing the electrolyte dispersion and a buffer having a pH of 7.5 to 8.5 to form a mixed system, and then adding an alkaline substance to adjust the pH of the mixed system to 8.5 to 8.8;
[0068] S30, adding a coating monomer to the mixed system, controlling the pH of the mixed system to be maintained at 8.5-8.8, and reacting, then centrifuging and drying the reaction product to obtain a composite material.
[0069] In some embodiments, in step S10, the solvent may be alcohols, alkanes, and ethers with good solubility, for example, including but not limited to at least one of n-heptane, n-hexane, ethanol, methanol, isopropanol, ethylene glycol, and dimethyl ether.
[0070] In some embodiments, the concentration of the halide solid electrolyte is 0.2 to 1 g / ml; for example, it can be 0.2 mg / ml, 0.3 mg / ml, 0.4 mg / ml, 0.5 mg / ml, 0.6 mg / ml, 0.7 mg / ml, 0.8 mg / ml, 0.9 mg / ml, 1 mg / ml, and any value between two of the above values. Selecting an electrolyte dispersion with a concentration within this range can, on the one hand, ensure the uniformity of the dispersion and avoid agglomeration; on the other hand, when it is mixed with the coating monomer, it can ensure sufficient concentration distribution, promote sufficient contact between the two, and allow the self-polymerization product of the coating monomer to be uniformly coated on the surface of the halide solid electrolyte.
[0071] In some embodiments, in order to promote the full dispersion of the halide solid electrolyte, after mixing it with the solvent, it is dispersed by ultrasound to obtain a uniform dispersion; wherein, the ultrasonic conditions can be a frequency of 30 to 50 kHz and a time of 0.05 to 2 hours. Within this condition range, the halide solid electrolyte can be uniformly dispersed in the solvent.
[0072] In step S20, a buffer is added to construct a stable acid-base environment close to pH 8.5-8.8. In some embodiments, the added buffer is a buffer with a pH of 7.5-8.5. Specifically, the buffer includes but is not limited to at least one of Tris-HCl buffer, 4-hydroxyethylpiperazineethanesulfonic acid, N-tris(hydroxymethyl)methylglycine, phosphoric acid, citric acid, carbonic acid, acetic acid, and barbituric acid buffer.
[0073] In order to make the reaction system reach the condition of pH 8.5-8.8, in some embodiments, it is necessary to add a pH adjuster to the mixed system to adjust its pH. In this embodiment, the pH adjuster is an alkaline substance; further, the alkaline substance includes one or more inorganic bases and organic bases, the inorganic base is selected from one or more of alkali metal oxides, alkali metal hydroxides, alkali metal bicarbonates, alkali metal carbonates, alkaline earth metal oxides, alkaline earth metal hydroxides, and alkaline earth metal bicarbonates; the organic base is selected from one or more of alkali metal salts of organic acids, alkali metal salts of alcohols, amine compounds, and alkylammonium hydroxides. The inorganic base is selected from one or more of sodium hydroxide, potassium hydroxide, lithium hydroxide, calcium hydroxide, sodium oxide, potassium oxide, calcium oxide, sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, calcium bicarbonate, and barium hydroxide; the alkali metal salt of the organic acid includes one or more of sodium acetate and potassium acetate; the alkali metal salt of the alcohol includes one or more of sodium ethoxide and potassium ethoxide; the alkylamine compound includes one or more of ethylenediamine, octylamine, dioctylamine, trioctylamine, and oleylamine; and the alkylammonium hydroxide includes one or more of tetramethylammonium hydroxide, tetraethylammonium hydroxide, and tetrapropylammonium hydroxide.
[0074] In specific implementation, the alkaline substance can be added in the form of a solution. For example, the alkaline substance is first dissolved in a solvent to prepare an alkaline solution. In this way, the alkaline solution can be quickly dispersed in the mixed system, avoiding the situation where the local pH changes too quickly and the pH adjustment of the mixed system deviates from the expected value. Specifically, the solvent can be an alcohol with good solubility, for example, it can include but is not limited to at least one of ethanol, methanol and ethylene glycol; the concentration of the alkaline substance in the alkaline solution can be 0.2 to 1 mol / L. In addition, in order to promote uniform dispersion of the alkaline substance, ultrasonic dispersion can be used, wherein the ultrasonic conditions can be a frequency of 30 to 50 kHz and a time of 5 to 20 minutes.
[0075] In some embodiments, the mass ratio of the halide solid electrolyte to the buffer is 70:(1-4); for example, the mass ratio of the two can be 70:1, 70:2, 70:3, 70:4, and a value between any two values listed above.
[0076] In step S30, the reaction temperature is 20-80°C, for example, 20°C, 30°C, 40°C, 50°C, 60°C, 65°C, 70°C, 80°C, and any two values between the above values. Within this range, the reaction can be accelerated. Preferably, the reaction temperature is 60°C.
[0077] In some embodiments of the present application, the reaction time is 0.5 to 24 h; for example, 0.5 h, 1 h, 2 h, 4 h, 6 h, 7 h, 8 h, 9 h, 10 h, 11 h, 12 h, 16 h, 18 h, 20 h, 22 h, 24 h and values between any two of the above values. Within this range, the uniformity of the coating and the degree of reaction can be well controlled.
[0078] In some embodiments, the coating monomer can be added in the form of a solution, for example, the coating monomer is first dissolved in a solvent to prepare a monomer solution. In this way, the monomer solution can be quickly dispersed in the mixed system to avoid the situation where the local coating monomer is excessive, thereby affecting the coating effect. Specifically, the solvent can be an alcohol with good solubility, for example, it can include but is not limited to at least one of ethanol, methanol and ethylene glycol; the concentration of the coating monomer in the monomer solution can be 0.04 to 0.16 mol / L, for example, 0.04 mol / L, 0.05 mol / L, 0.07 mol / L, 0.09 mol / L, 0.1 mol / L, 0.11 mol / L, 0.13 mol / L, 0.14 mol / L, 0.16 mol / L and values between any two values listed above. In addition, in order to promote uniform dispersion of the coating monomer, ultrasonic dispersion can be adopted, wherein the ultrasonic conditions can be a frequency of 30 to 50 kHz and a time of 5 to 20 min.
[0079] In some embodiments, the step of "adding a coating monomer to the mixed system, controlling the pH of the mixed system to maintain at 8.5 to 8.8, and reacting" is carried out under stirring conditions, and stirring is used to promote the coating monomer to be uniformly dispersed in the mixed system, so that it is uniformly coated on the outside of the electrolyte; the stirring speed can be 400 to 1200 r / min.
[0080] In some embodiments, the centrifugation is performed at a speed of 2000 to 15000 r / min and a time of 2 to 5 minutes, thereby effectively separating the composite material and improving the yield.
[0081] In some embodiments, the solid matter obtained by centrifugation is dried by vacuum drying at a temperature of 60 to 100° C., for example, 60° C., 70° C., 80° C., 90° C., 100° C., etc., so that the drying effect can be better controlled.
[0082] In addition, in some embodiments, each step (S100 or S10-S30) of the preparation method is carried out under an inert atmosphere, which includes nitrogen, helium, argon, etc.; during specific implementation, it can be carried out in a glove box to avoid the influence of water, oxygen, etc.
[0083] In a third aspect, the present application provides a solid electrolyte film 20 , wherein the material of the solid electrolyte film 20 includes a composite material, and the composite material includes the composite material as described above, or is prepared by the preparation method described above.
[0084] The preparation of the solid electrolyte film 20 includes placing a composite material on a substrate surface and cold pressing or hot pressing the composite material into a sheet to obtain the solid electrolyte film 20. The conditions for cold pressing or hot pressing the composite material to form the solid electrolyte film 20 include a pressure of 200 to 600 MPa and a time of 2 to 6 minutes.
[0085] The solid electrolyte film 20 provided in the present application has a firm and dense coating layer on its surface. The construction of the coating layer not only does not affect the structural characteristics of the halide solid electrolyte, but also can play a role in isolating the air, thereby effectively improving the environmental stability of the film; at the same time, the catecholamine self-polymer has good softness, and as a coating layer it improves the surface softness of the halide electrolyte, so that the solid electrolyte film 20 has better contact with the active particles, thereby improving the interface contact stability between the solid electrolyte and the metal electrode, and enhancing the electrochemical stability of the battery.
[0086] Fourthly, the present application further proposes a lithium battery 100 , as shown in FIG7 , the lithium battery 100 includes a positive electrode 10 , a solid electrolyte film 20 and a negative electrode 30 , wherein the solid electrolyte film 20 includes the solid electrolyte film 20 described above.
[0087] The solid electrolyte film 20 proposed in this application can replace the PP separator of the lithium battery 100 and be used in the lithium battery 100. By simply assembling it with the positive electrode 10 and the negative electrode 30, a lithium battery 100 with stable performance and long life can be formed.
[0088] The assembly steps of the all-solid-state lithium metal battery 100 include: using a mechanical fixture as a solid-state battery assembly test carrier, first placing the cut positive electrode 10 pole pieces at the bottom layer inside the fixture, then placing the composite material on the surface of the positive electrode 10 pole pieces and cold pressing them into sheets to obtain a positive electrode-solid electrolyte film sheet, then placing metallic lithium on the surface of the positive electrode-solid electrolyte film sheet, and cold pressing and packaging by pressure to obtain the all-solid-state lithium metal battery 100. The conditions for cold pressing the composite material to form the solid electrolyte film 20 include: a pressure of 200-600 MPa and a time of 2-6 minutes; the conditions for cold pressing and packaging include: a pressure of 30-200 MPa and a time of 0.5-2 hours.
[0089] It is understood that the above assembly steps are carried out under an inert atmosphere, which includes but is not limited to nitrogen, helium, argon, etc.; during specific implementation, it can be carried out in a glove box to avoid the influence of water, oxygen, etc.
[0090] The technical solutions and technical effects of the present application are described in detail below through specific examples and comparative examples. The following examples are only some examples of the present application and do not specifically limit the present application.
[0091] Example 1
[0092] (1) Preparation of composite materials:
[0093] (1) Lithium hydroxide is dispersed in ethanol and ultrasonically treated at a frequency of 50 kHz for 20 minutes to obtain a lithium hydroxide solution with a concentration of 0.5 mol / L; the coated monomer 3,4-dihydroxyphenylethylamine is dispersed in ethanol and ultrasonically treated at a frequency of 50 kHz for 20 minutes to obtain a monomer solution with a concentration of 0.08 mol / L of 3,4-dihydroxyphenylethylamine.
[0094] (2) Ultrasonic dispersion of the halide solid electrolyte Li3InCl6 in an ethanol solvent to obtain a uniform electrolyte dispersion with a concentration of 0.3 g / ml. The ultrasonic dispersion conditions include a frequency of 40 kHz and a time of 0.5 h.
[0095] (3) Mixing the Tris-HCl buffer solution with the electrolyte dispersion prepared in step (2), stirring them thoroughly, and adjusting the pH value of the mixed system to about 8.5 using the lithium hydroxide solution in step (1), stirring continuously at a speed of 1200 r / min during the process to obtain a mixed solution a; slowly adding the monomer solution in step (1) to the mixed solution a, stirring continuously at a speed of 1200 r / min during the process, and then continuing to stir for 0.5 h and 1 h respectively, and then performing two pH tests to ensure that the pH value of the mixed solution is about 8.5 (if the pH is not between 8.5 and 8.8, continue to add lithium hydroxide solution dropwise), to obtain a mixed solution b; wherein, the halide solid electrolyte, the coated monomer, and the Tris-HCl buffer solution are added according to a mass ratio of 70:4:2.
[0096] (4) The mixed solution b was heated to 60°C under stirring at a speed of 1200 r / min, and reacted at a constant temperature for 8 hours, then cooled to room temperature, and filtered to obtain a crude coated product. The crude coated product was washed with ethanol 2 to 3 times and centrifuged at a speed of 8000 r / min for 5 minutes. The precipitate was vacuum dried at 80°C for 24 hours to obtain a polydopamine-modified Li3InCl6 halide solid electrolyte (PDA@Li3InCl6), i.e., a composite material.
[0097] The above steps (1) to (4) are all carried out in a glove box with an argon environment.
[0098] The composite material was scanned using a transmission electron microscope. The results are shown in FIG1 . It can be seen that in the composite material, the surface of the halide solid electrolyte is coated with a coating layer with a thickness of about 3 nm.
[0099] (2) Preparation of positive electrode sheet:
[0100] Weigh 38.6g of the positive electrode active material lithium nickel cobalt manganese oxide LiNi 0.8 Co 0.1 Mn 0.1 The positive electrode slurry was prepared by ball milling O2 (NCM811), 0.48g of super PLL conductive carbon black, 0.24g of conductive graphite KS-6, 10.4g of 5% polyvinylidene fluoride glue, and n-methylpyrrolidone solvent. After coating, the slurry was initially dried and then transferred to a vacuum oven for drying. The positive electrode sheets were obtained by roller pressing and cutting. The mass ratio of the positive electrode active material NCM811, super PLL conductive carbon black, conductive graphite KS-6, and binder polyvinylidene fluoride (PVDF) was 96.9:1.2:0.6:1.3. The ball milling conditions included a speed of 300 r / min and a time of 3 hours. The vacuum drying conditions included a vacuum degree of ≤133 Pa, a temperature of 100°C, and a time of 24 hours.
[0101] (3) Assembly of all-solid-state lithium metal batteries:
[0102] A mechanical fixture is used as a solid-state battery assembly test carrier. First, the nickel cobalt manganese oxide (NCM811) positive electrode sheet cut in step (2) is placed at the bottom layer inside the fixture. Then, the composite material (PDA@Li3InCl6) obtained in step (1) is placed on the surface of the positive electrode sheet and cold-pressed into a sheet to obtain a positive electrode-solid electrolyte sheet (NCM811-PDA@Li3InCl6). Then, metallic lithium is placed on the surface of the positive electrode-solid electrolyte sheet (NCM811-PDA@Li3InCl6) and packaged by pressure cold pressing to obtain an all-solid-state metal lithium battery (NCM811|PDA@Li3InCl6|Li) based on a surface-coated halide solid electrolyte. The inner diameter of the mechanical fixture is Φ20mm, the diameter of the positive electrode sheet is Φ16mm, and the diameter of the metallic lithium is Φ18mm. The conditions for cold pressing the halide solid electrolyte into sheets include: a pressure of 300Mpa and a time of 4 minutes; the conditions for cold pressing packaging include: a pressure of 80Mpa and a time of 1 hour.
[0103] The battery assembly process in the above step (3) is carried out in a glove box with an argon environment.
[0104] Example 2
[0105] This embodiment is basically the same as embodiment 1, except that steps (1) to (4) are changed to:
[0106] (1) Lithium hydroxide is dispersed in ethanol and ultrasonically treated at a frequency of 50 kHz for 20 minutes to obtain a lithium hydroxide solution with a concentration of 0.5 mol / L; the coated monomer 3,4-dihydroxyphenylethylamine is dispersed in ethanol and ultrasonically treated at a frequency of 50 kHz for 20 minutes to obtain a monomer solution with a concentration of 0.08 mol / L of 3,4-dihydroxyphenylethylamine.
[0107] (2) Ultrasonic dispersion of the halide solid electrolyte Li3InCl6 in an ethanol solvent to obtain a uniform electrolyte dispersion with a concentration of 0.2 g / ml. The ultrasonic dispersion conditions include a frequency of 40 kHz and a time of 0.5 h.
[0108] (3) Mixing the Tris-HCl buffer solution with the electrolyte dispersion prepared in step (2), stirring them thoroughly, and adjusting the pH value of the mixed system to about 8.7 using the lithium hydroxide solution in step (1), stirring continuously at a speed of 600 r / min during the process to obtain a mixed solution a; slowly adding the monomer solution in step (1) to the mixed solution a, stirring continuously at a speed of 600 r / min during the process, and then continuing to stir for 0.5 h and 1 h respectively, and then performing two pH tests to ensure that the pH value of the mixed solution is about 8.7 (if the pH is not between 8.5 and 8.8, continue to add lithium hydroxide solution dropwise), to obtain a mixed solution b; wherein, the halide solid electrolyte, the coated monomer, and the Tris-HCl buffer solution are added according to a mass ratio of 70:4:2.
[0109] (4) The mixed solution b was heated to 60°C under stirring at a speed of 600 r / min, reacted at a constant temperature for 0.5 h, and then cooled to room temperature. The crude coated product was filtered to obtain the crude coated product. The crude coated product was washed with ethanol 2 to 3 times and centrifuged at a speed of 3000 r / min for 5 min. The precipitate was vacuum dried at 80°C for 24 h to obtain a polydopamine-modified Li3InCl6 halide solid electrolyte (PDA@Li3InCl6), i.e., a composite material.
[0110] The other steps and parameters remain unchanged.
[0111] Example 3
[0112] This embodiment is basically the same as embodiment 1, except that steps (1) to (4) are changed to:
[0113] (1) Lithium hydroxide is dispersed in isopropanol and ultrasonically treated at a frequency of 50 kHz for 20 minutes to obtain a lithium hydroxide solution with a concentration of 0.5 mol / L; the coated monomer 3,4-dihydroxyphenylethylamine is dispersed in isopropanol and ultrasonically treated at a frequency of 50 kHz for 20 minutes to obtain a monomer solution with a concentration of 0.08 mol / L of 3,4-dihydroxyphenylethylamine.
[0114] (2) Ultrasonic dispersion of the halide solid electrolyte Li3InCl6 in isopropyl alcohol to obtain a uniform electrolyte dispersion with a concentration of 1 g / ml. The ultrasonic dispersion conditions include a frequency of 40 kHz and a time of 0.5 h.
[0115] (3) Mixing the Tris-HCl buffer solution with the electrolyte dispersion prepared in step (2), stirring them thoroughly, and adjusting the pH value of the mixed system to about 8.5 using the lithium hydroxide solution in step (1), stirring continuously at a speed of 1200 r / min during the process to obtain a mixed solution a; slowly adding the monomer solution in step (1) to the mixed solution a, stirring continuously at a speed of 1200 r / min during the process, and then continuing to stir for 0.5 h and 1 h respectively, and then performing two pH tests to ensure that the pH value of the mixed solution is about 8.5 (if the pH is not between 8.5 and 8.8, continue to add lithium hydroxide solution dropwise), to obtain a mixed solution b; wherein, the halide solid electrolyte, the coated monomer, and the Tris-HCl buffer solution are added according to a mass ratio of 70:4:2.
[0116] (4) The mixed solution b was heated to 60°C under stirring at a speed of 1200 r / min, reacted at a constant temperature for 24 hours, and then cooled to room temperature. The crude coated product was filtered to obtain the crude coated product. The crude coated product was washed with ethanol 2 to 3 times and centrifuged at a speed of 2000 r / min for 3 minutes. The precipitate was vacuum dried at 80°C for 24 hours to obtain a polydopamine-modified Li3InCl6 halide solid electrolyte (PDA@Li3InCl6), i.e., a composite material.
[0117] Other parameters and steps remain unchanged.
[0118] Example 4
[0119] This embodiment is basically the same as embodiment 1, except that steps (1) to (4) are changed to:
[0120] (1) Lithium hydroxide is dispersed in ethanol and ultrasonically treated at a frequency of 50 kHz for 20 minutes to obtain a lithium hydroxide solution with a concentration of 0.5 mol / L; the coating monomer 1-(3,4-dihydroxyphenyl)-2-aminoethanol is dispersed in ethanol and ultrasonically treated at a frequency of 50 kHz for 20 minutes to obtain a 1-(3,4-dihydroxyphenyl)-2-aminoethanol monomer solution with a concentration of 0.08 mol / L.
[0121] (2) Ultrasonic dispersion of the halide solid electrolyte Li3InCl6 in an ethanol solvent to obtain a uniform electrolyte dispersion with a concentration of 0.3 g / ml. The ultrasonic dispersion conditions include a frequency of 40 kHz and a time of 0.5 h.
[0122] (3) Mixing the Tris-HCl buffer solution with the electrolyte dispersion prepared in step (2), stirring them thoroughly, and adjusting the pH value of the mixed system to about 8.8 using the lithium hydroxide solution in step (1), stirring continuously at a speed of 1200 r / min during the process to obtain a mixed solution a; slowly adding the monomer solution in step (1) to the mixed solution a, stirring continuously at a speed of 1200 r / min during the process, and then continuing to stir for 0.5 h and 1 h respectively, and then performing two pH tests to ensure that the pH value of the mixed solution is about 8.8 (if the pH is not between 8.5 and 8.8, continue to add lithium hydroxide solution dropwise), to obtain a mixed solution b; wherein, the halide solid electrolyte, the coated monomer, and the Tris-HCl buffer solution are added according to a mass ratio of 70:4:2.
[0123] (4) The mixed solution b was heated to 60°C under stirring at a speed of 1200 r / min, reacted at a constant temperature for 8 hours, and then cooled to room temperature. The crude coated product was filtered to obtain a crude coated product. The crude coated product was washed with ethanol 2 to 3 times and centrifuged at a speed of 15000 r / min for 2 minutes. The precipitate was vacuum dried at 80°C for 24 hours to obtain a poly 1-(3,4-dihydroxyphenyl)-2-aminoethanol modified Li3InCl6 halide solid electrolyte, i.e., a composite material.
[0124] Other parameters and steps remain unchanged.
[0125] Example 5
[0126] This embodiment is basically the same as Example 1, except that in step (1) of this embodiment, 3,4-dihydroxyphenylethylamine is replaced by (R)-4-(2-(methylamino)-1-hydroxyethyl]-1,2-benzenediol, and other parameters and steps remain unchanged.
[0127] Example 6
[0128] This embodiment is basically the same as embodiment 1, with the only difference being that in step (3) of this embodiment, the feed mass ratio is changed from 70:4:2 to 70:2:1, and other parameters and steps remain unchanged.
[0129] Example 7
[0130] This embodiment is basically the same as embodiment 1, with the only difference being that in step (3) of this embodiment, the feed mass ratio is changed from 70:4:2 to 70:8:4, and the other parameters and steps remain unchanged.
[0131] Example 8
[0132] This embodiment is basically the same as embodiment 1, with the only difference being that in step (3) of this embodiment, the feed mass ratio is changed from 70:4:2 to 70:10:5, and other parameters and steps remain unchanged.
[0133] Example 9
[0134] This embodiment is basically the same as embodiment 1, with the only difference being that in step (4) of this embodiment: the heating temperature is changed from 60° C. to 20° C., and the other parameters and steps remain unchanged.
[0135] Example 10
[0136] This embodiment is basically the same as embodiment 1, with the only difference being that in step (4) of this embodiment: the heating temperature is changed from 60° C. to 80° C., and the other parameters and steps remain unchanged.
[0137] Example 11
[0138] This embodiment is basically the same as embodiment 1, with the only difference being that in step (4) of this embodiment: the heating temperature is changed from 60° C. to 85° C., and the other parameters and steps remain unchanged.
[0139] Example 12
[0140] This embodiment is basically the same as embodiment 1, with the only difference being that, in step (2) of this embodiment, the halide solid electrolyte Li3InCl6 is changed to Li3YBr6, and the other parameters and steps remain unchanged.
[0141] Comparative Example 1
[0142] This comparative example is basically the same as Example 1, with the only difference being that, in this comparative example, in step (iii), the solid electrolyte membrane is prepared using a halide solid electrolyte that is not coated with catecholamine self-polymer, i.e., the composite material is changed to Li3InCl6, and accordingly, steps (1) to (4) are deleted.
[0143] Comparative Example 2
[0144] This comparative example is basically the same as Example 12, with the only difference being that, in this comparative example, in step (iii), the solid electrolyte membrane is prepared using a halide solid electrolyte that is not coated with catecholamine self-polymer, i.e., the composite material is changed to Li3YBr6, and accordingly, steps (1) to (4) are deleted.
[0145] The solid electrolyte films and lithium batteries prepared in Examples 1 to 12 and Comparative Examples 1 to 2 were subjected to performance testing using the following method:
[0146] (1) Using a charge-discharge cycle device and a constant current cut-off voltage charge-discharge method, the lithium battery is charged and discharged, and its charge-discharge curve is drawn;
[0147] (2) The cut Au sheet is placed at the bottom layer inside the fixture, and then the composite material prepared in the embodiment or the halide solid electrolyte in the comparative example that is not coated with catecholamine self-polymer is placed on the Au surface and cold-pressed into a sheet to obtain a gold-electrolyte sheet. Then, Au is placed on the surface of the gold-electrolyte sheet and cold-pressed to obtain a gold|solid electrolyte film|gold. The inner diameter of the mechanical fixture is Φ20 mm, the diameter of the positive electrode sheet is Φ16 mm, and the diameter of the metal lithium is Φ18 mm. The conditions for cold-pressing the halide solid electrolyte into a sheet include: a pressure of 300 MPa and a time of 4 minutes; the conditions for cold-pressing the packaging include: a pressure of 80 MPa and a time of 1 hour.
[0148] The two electrodes of gold|solid electrolyte film|gold were connected to the working electrode and auxiliary electrode of the electrochemical workstation respectively, and the electrochemical impedance spectroscopy (EIS) test was performed.
[0149] The results are shown in Figures 4 to 5 and Table 1. In Figures 4 and 5, the horizontal axis is the specific capacity (specific capacity), the unit is mAh / g; the vertical axis is the voltage (Voltage), the unit is V vs, Li + / Li.
[0150] Table 1
[0151] As can be seen from Figures 4 and 5, compared with the comparative example, the charge-discharge curves in Example 1 show a smaller charge-discharge polarization voltage and a higher charge-discharge capacity, indicating that the coated halide electrolyte has a positive effect on the ion transport of the porous electrode and the electrolyte-electrode interface contact; this indicates that the solid electrolyte film proposed in this application has greatly improved its environmental stability and its compatibility with metallic lithium by coating the catecholamine self-polymer coating layer, thereby improving the reversible capacity and charge-discharge cycle performance of the battery;
[0152] As can be seen from Table 1 and Figure 3, compared with the comparative example, each embodiment shows higher air stability, indicating that the solid electrolyte film proposed in the present application has greatly improved its environmental stability by coating the catecholamine self-polymer coating layer. In addition, by comparing the room temperature lithium|solid electrolyte|lithium initial AC impedance values of each embodiment and the comparative example in Table 1, it can be seen that the solid electrolyte film greatly reduces the interfacial impedance between the halide electrolyte and metallic lithium by coating the catecholamine self-polymer coating layer, which indicates that the coating layer improves its compatibility with metallic lithium, thereby improving the reversible capacity and charge and discharge cycle performance of the battery.
[0153] The above is a detailed introduction to the composite materials, preparation methods and lithium batteries provided in the embodiments of the present application. Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method and core ideas of the present application. At the same time, for technical personnel in this field, based on the ideas of the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.
Claims
1. A composite material, wherein: The invention comprises a halide solid electrolyte and a coating layer coated outside the halide solid electrolyte, wherein the material of the coating layer comprises catecholamine self-polymer.
2. The composite material according to claim 1, wherein The monomers of the catecholamine self-polymer include catecholamine and its derivatives, and the catecholamine includes one or more of 3,4-dihydroxyphenylethylamine, (R)-4-(2-(methylamino)-1-hydroxyethyl]-1,2-benzenediol, and 1-(3,4-dihydroxyphenyl)-2-aminoethanol.
3. The composite material according to claim 1 or 2, wherein: The coating layer has a thickness of 2 to 50 nm.
4. The composite material according to any one of claims 1 to 3, wherein: The chemical formula of the halide solid electrolyte is LiaMXb, wherein M is at least one of the metal elements of Group IIIB and Group IIIA, X is at least one of F, Cl, Br, and I, and 10≥a≥0, 13≥b≥1.
5. The composite material according to any one of claims 1 to 4, wherein: The halide solid electrolyte may be at least one of Li3ScCl3Br3, Li3InCl6, and Li3YBr6.
6. A method for preparing a composite material, wherein: The following steps are involved: A halide solid electrolyte, a coating monomer and a solvent are mixed, wherein the coating monomer self-polymerizes on the surface of the halide solid electrolyte to form a coating layer, thereby obtaining a composite material; Wherein, the coating monomer includes catecholamine and its derivatives.
7. The preparation method according to claim 6, wherein: The mass ratio of the halide solid electrolyte to the coating monomer is 70:(1-8).
8. The preparation method according to any one of claims 6 to 7, wherein: The catecholamines include one or more of 3,4-dihydroxyphenylethylamine, (R)-4-(2-(methylamino)-1-hydroxyethyl]-1,2-benzenediol, and 1-(3,4-dihydroxyphenyl)-2-aminoethanol.
9. The preparation method according to any one of claims 6 to 8, wherein: The steps of mixing a halide solid electrolyte, a coating monomer and a solvent, wherein the coating monomer self-polymerizes on the surface of the halide solid electrolyte to form a coating layer, and obtaining a composite material include: dispersing a halide solid electrolyte in a solvent to obtain an electrolyte dispersion; The electrolyte dispersion and a buffer with a pH of 7.5 to 8.5 are mixed to form a mixed system, and then Afterwards, an alkaline substance is added to adjust the pH of the mixed system to 8.5-8.8; The coating monomer is added into the mixed system, and the pH of the mixed system is controlled to be maintained at 8.5-8.8, and the reaction is carried out. Then, the reaction product is centrifuged and dried to obtain a composite material.
10. The preparation method according to claim 9, wherein: In the step of dispersing the halide solid electrolyte in a solvent to obtain an electrolyte dispersion, the concentration of the halide solid electrolyte in the electrolyte dispersion is 0.2 to 1 g / ml.
11. The preparation method according to claim 9 or 10, wherein: In the step of dispersing the halide solid electrolyte in a solvent to obtain an electrolyte dispersion, the solvent includes at least one of n-heptane, n-hexane, ethanol, methanol, isopropanol, ethylene glycol and ethers.
12. The preparation method according to any one of claims 9 to 11, wherein: In the step of mixing the electrolyte dispersion and a buffer having a pH value of 7.5 to 8.5 to form a mixed system, and then adding an alkaline substance to adjust the pH value of the mixed system to 8.5 to 8.8, The buffer comprises at least one of Tris-HCl buffer, 4-hydroxyethylpiperazineethanesulfonic acid, N-tricine, phosphoric acid, citric acid, carbonic acid, acetic acid, and barbituric acid.
13. The preparation method according to any one of claims 9 to 12, wherein: The mass ratio of the halide solid electrolyte to the buffer is 70:(1-4).
14. The preparation method according to any one of claims 9 to 13, wherein: The alkaline substance includes one or more of an inorganic base and an organic base. The inorganic base is selected from one or more of alkali metal oxides, alkali metal hydroxides, alkali metal bicarbonates, alkali metal carbonates, alkaline earth metal oxides, alkaline earth metal hydroxides, and alkaline earth metal bicarbonates; the organic base is selected from one or more of an alkali metal salt of an organic acid, an alkali metal salt of an alcohol, an alkylamine compound, and an alkylammonium hydroxide.
15. The preparation method according to any one of claims 9 to 14, wherein: In the step of adding a coating monomer to the mixed system, controlling the pH of the mixed system to be maintained at 8.5 to 8.8, reacting, and then centrifuging and drying the reaction product to obtain a composite material, The reaction temperature is 20 to 80°C; The reaction time is 0.5 to 24 hours.
16. The preparation method according to any one of claims 9 to 15, wherein: The coating monomer is added to the mixed system, and the pH of the mixed system is controlled to be maintained at 8.5-8.8 for reaction. Then, the reaction product is centrifuged and dried to obtain the composite material. The centrifugal speed is 2000-15000 r / min and the time is 2-5 min.
17. The preparation method according to any one of claims 9 to 16, wherein: A halide solid electrolyte, a coating monomer and a solvent are mixed, and the coating monomer self-polymerizes on the surface of the halide solid electrolyte to form a coating layer. The step of obtaining the composite material is carried out under an inert atmosphere, and the inert atmosphere includes one or more of nitrogen, helium and argon.
18. A lithium battery, wherein: It comprises a positive electrode, a solid electrolyte film and a negative electrode, wherein the material of the solid electrolyte film comprises a composite material, and the composite material comprises the composite material as described in any one of claims 1 to 5, or is prepared by the preparation method as described in any one of claims 6 to 17.
Citation Information
Patent Citations
Preparation method and application of high-performance solid electrolyte composite membrane
CN111952672A
Organic in-situ interface modified solid electrolyte and preparation method thereof
CN113363560A
Composite solid electrolyte membrane, preparation method thereof and all-solid-state lithium metal battery
CN114927753A
Preparation method of polymer-coated halide solid electrolyte and solid-state battery
CN115700941A
Solid electrolyte and preparation method thereof, positive electrode material, positive electrode plate and solid-state battery
CN116646590A
Cited By
Surface-modified Li3In x Ga 1-x Cl6 material, its preparation and application in lithium metal solid-state batteries