Optical laminate and article provided with same

The optical laminate, with a layered structure of a transparent base material, hard coat layer, and refractive index layers, addresses the challenge of scratch and bending resistance in foldable displays by using surface-modified silica fillers, achieving superior durability and optical performance.

WO2024225472A1PCT designated stage expired Publication Date: 2024-10-31DEXERIALS CORP

Patent Information

Application Number
PCT/JP2024/016571
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-04-22
Filing Date
2024-04-26
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Optical laminates used in foldable displays face challenges in achieving both excellent scratch resistance and improved bending resistance, with existing antireflection films made of resin exhibiting poor scratch resistance and hard coat films lacking evaluation of scratch resistance.

Method used

A transparent base material with a hard coat layer, adhesion layer, high refractive index layer, and low refractive index layer are alternately laminated, with the hard coat layer containing silica filler and surface-modified with silane compounds, and the optical laminate satisfies specific conditions for Martens hardness and contact angle difference after friction testing.

Benefits of technology

The solution achieves excellent scratch resistance and further enhances bending resistance, ensuring the optical laminate remains durable and resistant to deformation when bent, while maintaining transparency and optical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016571_31102024_PF_FP_ABST
    Figure JP2024016571_31102024_PF_FP_ABST
Patent Text Reader

Abstract

An optical laminate 102 comprises in the following order: a transparent base material 11; a hard coat layer 12; an adhesion layer 13 comprising a sputtered film; an optical function layer 14 in which high refractive index layers each comprising a sputtered film and low refractive index layers each having a refractive index lower than that of the high refractive index layer are alternately laminated; and an antifouling layer 15. The hard coat layer 12 contains a silica filler, and the optical laminate satisfies condition 1 and condition 2. Condition 1: The ratio ((A) / (B)) of Martens hardness (A) on the optical laminate antifouling layer side to Martens hardness (B) on a hard coat layer side of a laminate having only the transparent base material and the hard coat layer is 3.6 or less. Condition 2: The difference in contact angle with respect to water between before and after friction is 20° or less in a case where a friction tester using steel wool conforming to JIS L0849 is used to horizontally reciprocate the steel wool 200 times.
Need to check novelty before this filing date? Find Prior Art

Description

Optical laminate and article including same

[0001] The present invention relates to an optical laminate and an article including the same, and in particular to an optical laminate used as an anti-reflection film suitable for displays that are used in a bent state, such as flexible displays, and an article including the same. This application claims priority based on Japanese Patent Application No. 2023-074698 filed in Japan on April 28, 2023, Japanese Patent Application No. 2024-063462 filed in Japan on April 10, 2024, and Japanese Patent Application No. 2024-069031 filed in Japan on April 22, 2024, the contents of which are incorporated herein by reference.

[0002] In recent years, mobile communication terminals such as smartphones and information devices such as notebook PCs equipped with foldable displays have been released on the market. Optical laminates such as anti-reflection films are sometimes used in these displays to reduce surface reflection. Optical laminates used in foldable displays are required to have higher durability against bending than non-foldable displays.

[0003] For example, Patent Document 1 proposes that in a hard coat film having a hard coat layer and an optical functional layer consisting of a sputtered film, the thickness ratio of the hard coat layer to the optical functional layer be set within a predetermined range to improve the flex resistance.

[0004] Furthermore, Patent Document 2 describes that the hard coat layer and the anti-reflection layer are made of resin to improve flex resistance.

[0005] JP 2022-185597 A JP 2020-74019 A

[0006] However, in Patent Document 1, although the abrasion resistance and flex resistance of the hard coat film can be improved, scratch resistance is not evaluated, and there is room for improvement. Also, in Patent Document 2, although the flex resistance of the antireflection film can be improved, scratch resistance is poor because the antireflection layer is made of resin.

[0007] The present invention has been made in consideration of the above problems, and aims to provide an optical laminate that can achieve excellent scratch resistance and further improves bending resistance, and an article including the same.

[0008] In order to solve the above problems, the present invention proposes the following means. [1] An optical laminate having, in this order, a transparent substrate, a hard coat layer, an adhesion layer made of a sputtered film, an optical functional layer formed by alternating high refractive index layers made of a sputtered film, and low refractive index layers having a refractive index lower than that of the high refractive index layer, and an antifouling layer, wherein the hard coat layer contains a silica filler, and the optical laminate satisfies the following conditions 1 and 2. Condition 1: The ratio ((A) / (B)) of the Martens hardness (A) measured from the antifouling layer side of the optical laminate to the Martens hardness (B) measured from the hard coat layer side of a laminate having only the transparent substrate and the hard coat layer is 3.6 or less. Condition 2: Using a friction tester using steel wool in accordance with JIS L0849, the difference in contact angle with water before and after friction in which the steel wool is horizontally reciprocated 200 times is 20° or less.

[0009] [2] The optical laminate according to the above [1], wherein the silica filler is surface-modified with a functional group derived from a silane compound.

[0010] [3] The optical laminate according to [2] above, wherein the silane compound is one or more selected from vinyl group-containing silane compounds, (meth)acryloyl group-containing silane compounds, amino group-containing silane compounds, isocyanate group-containing silane compounds, isocyanurate group-containing silane compounds, epoxy group-containing silane compounds, and mercapto group-containing silane compounds.

[0011] [4] The optical laminate according to the above [2], wherein the silane compound is a (meth)acryloyl group-containing silane compound.

[0012] [5] The optical laminate according to the above [2], wherein the hard coat layer contains a binder resin and a silica filler, and the functional group derived from the silane compound has the same functional group as the binder resin.

[0013] [6] The optical laminate according to the above [5], wherein the binder resin contains a (meth)acrylate compound, and the functional group derived from the silane compound is a (meth)acryloyl group.

[0014] [7] The optical laminate according to the above [1], wherein the average particle diameter of the silica filler is 800 nm or less.

[0015] [8] The optical laminate according to the above [1], wherein the thickness of the hard coat layer is 0.5 μm or more and 100 μm or less.

[0016] [9] The optical laminate according to the above [1], wherein when the optical laminate is bent 180° so that the surface on which the antifouling layer is formed faces outward, and a mandrel of the smallest diameter on which no cracks occur is used, the elongation S (%) of the optical functional layer calculated by the following formula (1) satisfies 1.3≦S: S (%)={(R2 / R1)−1}×100 (1) (where R2 is the distance from the axial center of the mandrel to the outer surface of the optical laminate, and R1 is the distance from the axial center of the mandrel to an imaginary line indicating a position corresponding to ½ of the total thickness of the optical laminate.)

[0017]

[10] The optical laminate according to claim 9, wherein when the optical laminate is bent 180 degrees so that the surface on which the antifouling layer is formed faces inward, and a mandrel of the smallest diameter on which no cracks occur is used, the compressibility C (%) of the optical functional layer calculated by the following formula (2) satisfies 4.5≦C: C (%)={1−(R3 / R1)}×100 (2) (where R3 is the distance from the axial center of the mandrel to the surface of the optical laminate on the antifouling layer side, and R1 is the distance from the axial center of the mandrel to an imaginary line indicating a position corresponding to ½ of the total thickness of the optical laminate.)

[0018]

[11] An article comprising the optical laminate according to any one of [1] to

[10] above.

[0019] According to the present invention, it is possible to provide an optical layered body that can achieve excellent scratch resistance and further improves flex resistance, and an article including the same.

[0020] 1 is a cross-sectional view showing another example of the optical laminate of the present embodiment. FIG. 2 is a cross-sectional view showing another example of the optical laminate of the present embodiment. FIG. 3 is a schematic view for explaining an example of a manufacturing apparatus that can be used in the manufacturing method of the optical laminate of the present embodiment.

[0021] The present embodiment will be described in detail below with reference to the drawings as appropriate. The drawings used in the following description may show characteristic portions enlarged for the sake of clarity, and the dimensional ratios of each component may differ from the actual ones. The materials, dimensions, etc. exemplified in the following description are merely examples, and the present invention is not limited thereto. Appropriate changes can be made within the scope of the present invention.

[0022] [Optical Laminate] FIG. 1 is a cross-sectional view showing another example of an optical laminate of this embodiment. The optical laminate 102 shown in FIG. 1 is formed by sequentially laminating a transparent substrate 11, a hard coat layer 12, an adhesion layer 13, an optical functional layer 14, and an antifouling layer 15. The adhesion layer 13 is a layer that provides adhesion between the hard coat layer 12 and the optical functional layer 14. The optical functional layer 14 is a layer that provides an optical function. The optical function is a function that controls the properties of light, such as reflection, transmission, and refraction, and examples thereof include an antireflection function, a selective reflection function, and a lens function. The optical functional layer 14 preferably includes one selected from an antireflection layer and a selective reflection layer. Known antireflection layers and selective reflection layers can be used. The antireflection layer and the selective reflection layer may each be a single layer or a laminate of multiple layers.

[0023] FIG. 2 is a cross-sectional view showing another example of the optical laminate of this embodiment. The optical laminate 101 shown in FIG. 2 is the same as the optical laminate 102 shown in FIG. 1 except that an antireflection layer is provided as the optical functional layer 14. As shown in FIG. 1, the optical functional layer 14 (antireflection layer) is composed of a laminate in which low-refractive-index layers 14b and high-refractive-index layers 14a are alternately stacked. The optical functional layer 14 shown in FIG. 1 is composed of a hard coat layer 12, an adhesive layer 13, a high-refractive-index layer 14a, a low-refractive-index layer 14b, a high-refractive-index layer 14a, a low-refractive-index layer 14b, and an antifouling layer 15 stacked in this order from the transparent substrate 11 side. Therefore, the antifouling layer 15 is in contact with the low-refractive-index layer 14b of the optical functional layer 14.

[0024] The transparent substrate 11 may be formed from a transparent material that can transmit light in the visible light range. For example, a plastic film is preferably used as the transparent substrate 11. Specific examples of materials that can be used for the plastic film include polyester-based resins, acetate-based resins, polyethersulfone-based resins, polycarbonate-based resins, polyamide-based resins, polyimide-based resins, polyolefin-based resins, (meth)acrylic-based resins, polyvinyl chloride-based resins, polyvinylidene chloride-based resins, polystyrene-based resins, polyvinyl alcohol-based resins, polyarylate-based resins, and polyphenylene sulfide-based resins.

[0025] In the present invention, the term "transparent material" refers to a material having a transmittance of 80% or more for light in the wavelength range used, provided that the effect of the present invention is not impaired. In addition, in this embodiment, "(meth)acrylic" means methacrylic and acrylic.

[0026] The transparent substrate 11 may contain a reinforcing material as long as the optical properties are not significantly impaired. Examples of the reinforcing material include cellulose nanofiber and nanosilica. In particular, polyester-based resins, acetate-based resins, polycarbonate-based resins, and polyolefin-based resins are preferably used as the reinforcing material. Specifically, a triacetyl cellulose (TAC) substrate is preferably used as the reinforcing material. Furthermore, a glass film, which is an inorganic substrate, can also be used as the transparent substrate 11.

[0027] When the plastic film is a TAC substrate, when the hard coat layer 12 is formed on one side thereof, a permeation layer is formed in which some of the components constituting the hard coat layer 12 penetrates into the transparent substrate 11. As a result, the adhesion between the transparent substrate 11 and the hard coat layer 12 is improved, and the occurrence of interference fringes due to the difference in refractive index between the layers can be suppressed.

[0028] The transparent substrate 11 may be a film having optical and / or physical functions, such as a polarizing plate, a retardation compensation film, a heat-shielding film, a transparent conductive film, a brightness-enhancing film, and a barrier-enhancing film.

[0029] The thickness of the transparent substrate 11 is not particularly limited, but is preferably, for example, 25 μm or more. The film thickness of the transparent substrate 11 is more preferably 40 μm or more. When the thickness of the transparent substrate 11 is 25 μm or more, the rigidity of the substrate itself is ensured, and wrinkles are less likely to occur even when stress is applied to the optical laminate 10. Furthermore, when the thickness of the transparent substrate 11 is 25 μm or more, wrinkles are less likely to occur even when the hard coat layer 12 is continuously formed on the transparent substrate 11, which is preferable as there are fewer concerns about production. When the thickness of the transparent substrate 11 is 40 μm or more, wrinkles are even less likely to occur, which is preferable.

[0030] When production is carried out using a roll, the thickness of the transparent substrate 11 is preferably 1000 μm or less, and more preferably 600 μm or less. When the thickness of the transparent substrate 11 is 1000 μm or less, the optical laminate 10 during production and the optical laminate 10 after production can be easily wound into a roll, and the optical laminate 10 can be produced efficiently. Furthermore, when the thickness of the transparent substrate 11 is 1000 μm or less, the optical laminate 10 can be made thinner and lighter. When the thickness of the transparent substrate 11 is 600 μm or less, the optical laminate 10 can be produced more efficiently and can be made even thinner and lighter, which is preferable.

[0031] The surface of the transparent substrate 11 may be previously subjected to an etching treatment such as sputtering, corona discharge, ultraviolet irradiation, electron beam irradiation, conversion treatment, oxidation, etc., and / or a primer treatment. By previously performing these treatments, it is possible to improve adhesion to the hard coat layer 12 to be formed on the transparent substrate 11. Furthermore, before forming the hard coat layer 12 on the transparent substrate 11, it is also preferable to remove dust and clean the surface of the transparent substrate 11 by subjecting the surface of the transparent substrate 11 to solvent washing, ultrasonic cleaning, etc., as necessary.

[0032] The hard coat layer 12 contains a binder resin and a filler as essential components, and may optionally contain other components such as a dispersant. Known binder resins can be used. The filler is contained in the binder resin to the extent that transparency is not impaired. The filler may be organic, inorganic, or a combination of organic and inorganic materials. From the viewpoints of hardness and flex resistance, inorganic fillers are preferred, and silica particles made of silica are even more preferred. Furthermore, surface-modified silica particles are particularly preferred.

[0033] The binder resin used in the hard coat layer 12 is preferably transparent, and examples thereof include ionizing radiation curable resins that are cured by ultraviolet light or electron beams, thermoplastic resins, and thermosetting resins.

[0034] Examples of the ionizing radiation curable resin used as the binder resin of the hard coat layer 12 include ethyl(meth)acrylate, ethylhexyl(meth)acrylate, styrene, methylstyrene, and N-vinylpyrrolidone. Examples of the ionizing radiation curable resin compound having two or more unsaturated bonds include trimethylolpropane tri(meth)acrylate, tripropylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, ditrimethylolpropane ... Examples of suitable polyfunctional compounds include erythritol penta(meth)acrylate, tripentaerythritol octa(meth)acrylate, tetrapentaerythritol deca(meth)acrylate, isocyanuric acid tri(meth)acrylate, isocyanuric acid di(meth)acrylate, polyester tri(meth)acrylate, polyester di(meth)acrylate, bisphenol di(meth)acrylate, diglycerin tetra(meth)acrylate, adamantyl di(meth)acrylate, isobornyl di(meth)acrylate, dicyclopentane di(meth)acrylate, tricyclodecane di(meth)acrylate, and ditrimethylolpropane tetra(meth)acrylate. Among these, pentaerythritol triacrylate (PETA), dipentaerythritol hexaacrylate (DPHA), and pentaerythritol tetraacrylate (PETTA) are preferably used. The term "(meth)acrylate" refers to methacrylate and acrylate. Furthermore, the ionizing radiation curable resin may be a resin obtained by modifying the above-mentioned compounds with PO (propylene oxide), EO (ethylene oxide), CL (caprolactone), or the like.Furthermore, urethane (meth)acrylate oligomers, epoxy (meth)acrylate oligomers, etc. can also be used from the viewpoint of film formation of the hard coat layer and adjustment of viscoelasticity.

[0035] Examples of thermoplastic resins used as the binder resin of the hard coat layer 12 include styrene-based resins, (meth)acrylic resins, vinyl acetate-based resins, vinyl ether-based resins, halogen-containing resins, alicyclic olefin-based resins, polycarbonate-based resins, polyester-based resins, polyamide-based resins, cellulose derivatives, silicone-based resins, and rubber or elastomers. The thermoplastic resins are preferably amorphous and soluble in organic solvents (particularly common solvents capable of dissolving multiple polymers and curable compounds). In particular, from the viewpoints of transparency and weather resistance, styrene-based resins, (meth)acrylic resins, alicyclic olefin-based resins, polyester-based resins, cellulose derivatives (cellulose esters, etc.), and the like are preferred.

[0036] The hard coat layer 12 includes, for example, a binder resin and silica particles as a filler. The silica particles preferably include silica particles that have been surface-modified in advance. Specific examples of silane compounds include vinyl group-containing silane compounds, (meth)acryloyl group-containing silane compounds, amino group-containing silane compounds, isocyanate group-containing silane compounds, isocyanurate group-containing silane compounds, epoxy group-containing silane compounds, and mercapto group-containing silane compounds. These compounds may be used alone or in combination. The silane compound is selected appropriately depending on the type of binder resin. However, when the binder resin contains a functional group, a silane compound having the same functional group as the binder resin is preferred. For example, when the binder resin contains a (meth)acrylate compound as an ionizing radiation-curable resin, the silane compound is preferably a (meth)acryloyl group-containing alkoxysilane compound. Note that "(meth)acrylate" refers to methacrylate and / or acrylate. Furthermore, in the present invention, methacrylate and acrylate are treated as the same substance in terms of reaction mechanism. The silane compound used for surface modification preferably has an alkoxysilyl group or a silanol group at its terminal, since this improves bonding with the hydroxyl groups present on the silica particle surface. Pre-surface modification of the silica particles improves dispersibility in the binder resin, and the reaction between the surface treatment agent used for surface modification and the binder resin results in stronger bonding with the binder resin, thereby improving the hardness of the optical laminate. These silica particles may be exposed on the surface of the hard coat layer 12 facing the optical functional layer 14. In this case, the hard coat layer 12 and the optical functional layer 14 are more strongly bonded via the adhesion layer 13. Examples of methods for exposing the silica particles include glow discharge treatment, which will be described later. In this case, the surface modification on the exposed silica surface is removed. Exposing the filler to the hard coat layer surface and removing the surface modification at this time generates an electrostatic attraction between the hydroxyl groups generated on the filler surface and the adhesion layer 13, which will be described later, thereby further improving adhesion. In addition, the exposed filler acts as an anchor and bites into the adhesive layer 13, which also contributes to improving the adhesiveness.The improvement in flex resistance is achieved by a combination of the bonding with the binder resin due to the surface modification of the silica surface and the interaction between the silica and the adhesive layer.

[0037] The average particle size of the filler in the hard coat layer 12 is, for example, 800 nm or less, preferably 780 nm or less, and more preferably 100 nm or less. When the particle size of the filler is within this range, the haze value of the entire optical laminate 10 is 2% or less. An optical laminate 10 with a haze of 2% or less has high transparency and serves as a so-called clear antireflection film.

[0038] The surface of the hard coat layer 12 is preferably subjected to, for example, glow discharge treatment, plasma treatment, ion etching, alkali treatment, etc. Among these, glow discharge treatment is preferred because it allows for large-area treatment. The intensity of the glow discharge treatment is, for example, 100 W / m as electrode power density. 2 ~11,000 W / m 2 and 1600 W / m 2 ~7000 W / m 2 It is preferable to perform the glow discharge treatment at a discharge intensity within the above range. By performing a glow discharge treatment on the surface of the hard coat layer 12, the surface of the hard coat layer 12 is roughened at the nanometer level, and substances with weak bonding strength present on the surface of the hard coat layer 12 are removed. As a result, the adhesion between the hard coat layer 12 and the adhesion layer 13 formed on the hard coat layer 12 is improved. This also has the effect of exposing silica particles from the hard coat layer 12. Furthermore, while increasing the strength during the discharge treatment tends to improve the flex resistance described below, this effect plateaus once the discharge intensity exceeds a certain level. Furthermore, excessive glow discharge intensity can lead to deterioration of the resin that constitutes the hard coat layer. Therefore, it is preferable to perform the glow discharge treatment at a discharge intensity within the above-mentioned range.

[0039] In addition, when an anti-glare optical laminate is desired, the average particle diameter of the filler in the hard coat layer 12 may be, for example, 0.5 μm or more. Organic fine particles such as acrylic resins are preferably used as fillers of this size. When the filler particle diameter is within this range, the haze value of the entire optical laminate 10 exceeds 2%. An optical laminate 10 with a haze of more than 2% has anti-glare properties and becomes a so-called anti-glare (AG) type anti-reflection film. Even in this case, the average particle diameter of the filler is preferably 10 μm or less, more preferably 5 μm or less, and particularly preferably 3 μm or less. Various reinforcing materials can be used as the filler contained in the hard coat layer 12 to impart toughness to the hard coat layer 12, as long as the optical properties are not impaired. Examples of reinforcing materials include cellulose nanofibers.

[0040] The thickness of the hard coat layer 12 is not particularly limited, but is preferably 0.5 μm or more, and more preferably 1 μm or more. The thickness of the hard coat layer 12 is preferably 100 μm or less. When the thickness of the hard coat layer 12 is 0.5 μm or more, sufficient hardness is obtained, making it less likely to suffer from scratches during production. Furthermore, when the thickness of the hard coat layer 12 is 100 μm or less, the optical laminate 10 can be made thinner and lighter. Furthermore, when the thickness of the hard coat layer 12 is 100 μm or less, microcracks in the hard coat layer 12 that occur when the optical laminate 10 is bent during production are less likely to occur, improving productivity.

[0041] The hard coat layer 12 may be a single layer or a laminate of multiple layers. The hard coat layer 12 may further be provided with known functions such as ultraviolet absorption, antistatic properties, refractive index adjustment, and hardness adjustment. The functions provided to the hard coat layer 12 may be provided in a single hard coat layer or may be provided separately in multiple layers.

[0042] The adhesion layer 13 is a layer formed to improve adhesion between the transparent substrate 11 or hard coat layer 12, which is an organic film, and the optical functional layer 14, which is an inorganic film. In the optical laminate 10 shown in FIG. 2 , the adhesion layer 13 is provided between the hard coat layer 12 and the optical functional layer 14. The adhesion layer 13 functions to adhere the hard coat layer 12 and the optical functional layer 14 to each other. The adhesion layer 13 is preferably made of an oxygen-deficient metal oxide or metal. An oxygen-deficient metal oxide refers to a metal oxide in which the number of oxygen atoms is deficient compared to the stoichiometric composition. Examples of oxygen-deficient metal oxides include SiOx, AlOx, TiOx, ZrOx, CeOx, MgOx, ZnOx, TaOx, SbOx, SnOx, and MnOx. Examples of metals include Si, Al, Ti, Zr, Ce, Mg, Zn, Ta, Sb, Sn, Mn, and In. The adhesion layer 13 may be, for example, SiOx, where x is greater than 0 and less than 2.0. The adhesion layer may also be formed from a mixture of multiple metals or metal oxides. From the viewpoint of maintaining transparency and adhesion with the optical functional layer and obtaining good optical properties, the thickness of the adhesion layer is preferably greater than 0 nm and not greater than 20 nm, and particularly preferably 1 nm or greater and not greater than 10 nm.

[0043] The optical function layer 14 is a laminate that exhibits an anti-reflection function. The optical function layer 14 shown in Fig. 2 is a laminate of four layers in total, in which high-refractive-index layers 14a and low-refractive-index layers 14b are alternately stacked in this order from the adhesive layer 13 side. The number of high-refractive-index layers 14a and low-refractive-index layers 14b is not particularly limited, and the number of high-refractive-index layers 14a and low-refractive-index layers 14b can be any number.

[0044] 2, the optical function layer 14 is made of a laminate in which low refractive index layers 14b and high refractive index layers 14a are alternately stacked, and therefore, light incident from the antifouling layer 15 side interferes with the optical function layer 14, thereby reducing the intensity of the reflected light and providing an antireflection function. Therefore, an antireflection function is obtained that prevents light incident from the antifouling layer 15 side from being reflected in one direction.

[0045] The low refractive index layer 14b contains, for example, a metal oxide. The low refractive index layer 14b may contain an oxide of Si, for example, SiO 2 It is preferable that the layer contains, as a main component, SiO (oxide of Si) or the like. 2 The single layer film is colorless and transparent. In this embodiment, the main component of the low refractive index layer 14b means a component contained in the low refractive index layer 14b at 50% by mass or more. When the low refractive index layer 14b is a layer whose main component is an oxide of Si, it may contain less than 50% by mass of another element. The content of elements other than the oxide of Si is preferably 10% or less. Examples of other elements that may be contained include Na for improving durability, Zr, Al, or N for improving hardness, and Zr and Al for improving alkali resistance.

[0046] The refractive index of the low refractive index layer 14b is preferably 1.20 to 1.60, and more preferably 1.30 to 1.50. The dielectric material used for the low refractive index layer 14b is magnesium fluoride (MgF 2 , refractive index 1.38).

[0047] The refractive index of the high refractive index layer 14a is preferably 2.00 to 2.60, and more preferably 2.10 to 2.45. The dielectric material used for the high refractive index layer 14a is niobium pentoxide (Nb 2 O 5 , refractive index 2.33), titanium oxide (TiO 2 , refractive index 2.33 to 2.55), tungsten oxide (WO 3 , refractive index 2.2), cerium oxide (CeO 2 , refractive index 2.2), tantalum pentoxide (Ta 2 O 5 , refractive index 2.16), zinc oxide (ZnO, refractive index 2.1), indium tin oxide (ITO, refractive index 2.06), zirconium oxide (ZrO 2 , refractive index 2.2). When it is desired to impart conductive properties to the high refractive index layer 14a, for example, ITO or indium zinc oxide (IZO) can be selected.

[0048] The optical function layer 14 uses, for example, niobium pentoxide (Nb2O5, refractive index 2.33) as the high refractive index layer 14a and SiO2 as the low refractive index layer 14b. 2 It is preferable to use one consisting of:

[0049] The thickness of the low-refractive index layer 14b may be in the range of 1 nm to 200 nm, and is appropriately selected depending on the wavelength range in which anti-reflection function is required. The thickness of the high-refractive index layer 14a may be, for example, in the range of 1 nm to 200 nm, and is appropriately selected depending on the wavelength range in which anti-reflection function is required. The thicknesses of the high-refractive index layer 14a and the low-refractive index layer 14b can be appropriately selected depending on the design of the optical function layer 14. For example, from the adhesive layer 13 side, the high-refractive index layer 14a can be 5 to 50 nm, the low-refractive index layer 14b can be 10 to 80 nm, the high-refractive index layer 14a can be 20 to 200 nm, and the low-refractive index layer 14b can be 50 to 200 nm.

[0050] Of the layers forming the optical function layer 14, a low refractive index layer 14b is disposed on the side of the antifouling layer 15. It is preferable that the low refractive index layer 14b of the optical function layer 14 is in contact with the antifouling layer 15, since this improves the antireflection performance of the optical function layer 14.

[0051] The antifouling layer 15 is formed on the outermost surface of the optical functional layer 14 and prevents the optical functional layer 14 from being soiled or damaged. Furthermore, when the antifouling layer 15 is applied to a touch panel or the like, its abrasion resistance suppresses wear of the optical functional layer 14. The antifouling layer 15 of this embodiment is made of a vapor-deposited film formed by vapor-depositing an antifouling material. In this embodiment, the antifouling layer 15 is formed by vacuum-depositing a fluorine-based organic compound as the antifouling material on one surface of the low refractive index layer 14b that constitutes the optical functional layer 14. In this embodiment, since the antifouling material contains a fluorine-based organic compound, the optical laminate 10 has even better abrasion resistance and alkali resistance.

[0052] A compound comprising a fluorine-modified organic group and a reactive silyl group (e.g., alkoxysilane) is preferably used as the fluorine-based organic compound constituting the antifouling layer 15. Examples of commercially available products include Optool DSX (manufactured by Daikin Corporation) and KY-100 series (manufactured by Shin-Etsu Chemical Co., Ltd.).

[0053] The fluorine-based organic compound constituting the antifouling layer 15 is a compound consisting of a fluorine-modified organic group and a reactive silyl group (for example, alkoxysilane), and the low refractive index layer 14b of the optical function layer 14 in contact with the antifouling layer 15 is made of SiO 2 When a compound consisting of fluorine-based organic compounds is used, the silanol groups in the skeleton of the fluorine-based organic compounds and SiO 2 This results in good adhesion between the optical function layer 14 and the antifouling layer 15, which is preferable.

[0054] The optical thickness of the antifouling layer 15 may be in the range of 1 nm or more and 20 nm or less, and is preferably in the range of 3 nm or more and 10 nm or less. If the thickness of the antifouling layer 15 is 1 nm or more, sufficient abrasion resistance can be ensured when the optical laminate 10 is used for touch panels, etc. Furthermore, if the thickness of the antifouling layer 15 is 3 nm or more, the liquid resistance, etc. of the optical laminate 10 is improved. Furthermore, if the thickness of the antifouling layer 15 is 20 nm or less, the time required for vapor deposition can be shortened, allowing for efficient production.

[0055] In the optical laminate 10, 102 configured as described above, the ratio ((A) / (B)) of the Martens hardness (A) measured from the antifouling layer 15 side of the optical laminate 10, 102 to the Martens hardness measured from the hard coat layer 12 side of a laminate having only the transparent substrate 11 and the hard coat layer 12 is 3.6 or less (Condition 1). Furthermore, the ratio ((A) / (B)) is preferably 3.5 or less, and more preferably 3.4 or less. When the ratio ((A) / (B)) is 3.6 or less, the difference in hardness between the hard coat layer surface and the antifouling layer surface is small, thereby suppressing deformation, and as a result, excellent scratch resistance can be achieved and bending resistance can be further improved.

[0056] Furthermore, in the optical laminate 10, 102 configured as described above, a difference in contact angle with water before and after 200 horizontal reciprocating movements of the steel wool is measured using a friction tester using steel wool in accordance with JIS L0849, and the difference is 20° or less (Condition 2). If the optical laminate 10, 102 has a high hardness, the difference in contact angle becomes 20° or less, and excellent scratch resistance can be achieved.

[0057] In the optical laminate 10, 102 configured as described above, when the optical laminate 10, 102 is bent 180 degrees so that the surface on which the antifouling layer 15 is formed faces outward, the elongation S (%) of the optical functional layer 14 calculated by the following formula (1) when a mandrel of the smallest diameter at which no cracks occur is used preferably satisfies 1.3≦S. This makes it possible to further improve the bending resistance of the optical laminate 10, 102. S={(R2 / R1)−1}×100 (1) (where R2 is the distance from the axial center of the mandrel to the outer surface of the optical laminate, and R1 is the distance from the axial center of the mandrel to an imaginary line indicating a position corresponding to ½ of the total thickness of the optical laminate.)

[0058] Furthermore, in the optical laminate 10, 102, when the optical laminate 10, 102 is bent 180 degrees so that the surface on which the antifouling layer 15 is formed faces inward, and a mandrel of the smallest diameter at which no cracks occur is used, the compression ratio C (%) of the optical functional layer 14 calculated by the following formula (2) preferably satisfies 4.5≦C, and more preferably satisfies 5≦C. This makes it possible to further improve the bending resistance of the optical laminate 10, 102. C (%)={1−(R3 / R1)}×100 (2) (where R3 is the distance from the axial center of the mandrel to the surface of the optical laminate on the antifouling layer side, and R1 is the distance from the axial center of the mandrel to an imaginary line indicating a position corresponding to ½ of the total thickness of the optical laminate.)

[0059] Furthermore, it is preferable that the optical functional layer 14 satisfy both the above-mentioned ranges for the elongation percentage S (%) and the above-mentioned ranges for the compression percentage C (%). That is, in the optical laminate 10, 102, when the optical laminate 10, 102 is bent 180° so that the surface on which the antifouling layer 15 is formed is on the outside, the elongation percentage S (%) of the optical functional layer 14 calculated by the following formula (1) satisfies 1.3≦S when a mandrel of the smallest diameter at which no cracks occur is used, and when the optical laminate 10, 102 is bent 180° so that the surface on which the antifouling layer 15 is formed is on the inside, the compression percentage C (%) of the optical functional layer 14 calculated by the above formula (2) satisfies 4.5≦C. This can further improve the bending resistance of the optical laminate 10, 102.

[0060] The above elongation percentages are values ​​when the substrate is made of PET and the thickness is 50 μm, and these values ​​may vary if the thickness is reduced.

[0061] In the optical laminate 10, 102 configured as described above, when the thickness of the hard coat layer of the optical laminate is 5 μm, if the optical laminate 10, 102 is bent 180° so that the surface on which the anti-fouling layer 15 is formed is facing outward, the diameter of the mandrel is gradually changed to one that is smaller, and the diameter of the mandrel that is 0.2 mm larger than the diameter of the mandrel at which the first crack was discovered is preferably 4.0φmm or less, more preferably 3.5φmm or less, and even more preferably 3.0φmm or less.

[0062] Furthermore, when the thickness of the hard coat layer of the optical laminate is 5 μm, if the optical laminate 10, 102 is bent 180° so that the surface on which the antifouling layer 15 is formed is on the inside, the diameter of the mandrel is gradually changed to one that is smaller, and the diameter of the mandrel that is 0.2 mm larger than the diameter of the mandrel at which the first crack was discovered is preferably 1.1φmm or less, and more preferably less than 1.0φmm.

[0063] Furthermore, when the thickness of the hard coat layer of the optical laminate is 5 μm, when the optical laminate 10, 102 is bent 180° so that the surface on which the anti-fouling layer 15 is formed is on the outside, it is more preferable that the diameter of the mandrel that is 0.2 mm larger than the diameter of the mandrel at which the first crack was discovered when the mandrel diameter is gradually reduced to 4.0 φmm or less, and that when the optical laminate 10, 102 is bent 180° so that the surface on which the anti-fouling layer 15 is formed is on the inside, the diameter of the mandrel that is 0.2 mm larger than the diameter of the mandrel at which the first crack was discovered when the mandrel diameter is gradually reduced to 1.1 φmm or less.

[0064] In the optical laminate 10, 102 configured as described above, when the thickness of the hard coat layer of the optical laminate is 10 μm, if the optical laminate 10, 102 is bent 180° so that the surface on which the anti-fouling layer 15 is formed is facing outward, the diameter of the mandrel is gradually changed to one that is smaller, and the diameter of the mandrel that is 0.2 mm larger than the diameter of the mandrel at which the first crack was discovered is preferably 4.0φmm or less, more preferably 3.5φmm or less, and even more preferably 3.0φmm or less.

[0065] Furthermore, when the thickness of the hard coat layer of the optical laminate is 10 μm, if the optical laminate 10, 102 is bent 180° so that the surface on which the antifouling layer 15 is formed is on the inside, the diameter of the mandrel is gradually changed to one that is smaller, and the diameter of the mandrel that is 0.2 mm larger than the diameter of the mandrel at which the first crack was discovered is preferably 1.4φmm or less, and more preferably 1.2φmm or less.

[0066] Furthermore, when the thickness of the hard coat layer of the optical laminate is 10 μm, when the optical laminate 10, 102 is bent 180° so that the surface on which the anti-fouling layer 15 is formed is on the outside, it is more preferable that the diameter of the mandrel is gradually reduced to 4.0φmm or less, and when the optical laminate 10, 102 is bent 180° so that the surface on which the anti-fouling layer 15 is formed is on the inside, it is more preferable that the diameter of the mandrel is gradually reduced to 0.2 mm larger than the diameter of the mandrel on which the first crack is found is 1.4φmm or less.

[0067] In the optical laminate 10, 102 configured as described above, when the thickness of the hard coat layer of the optical laminate is 2 μm, if the optical laminate 10, 102 is bent 180° so that the surface on which the anti-fouling layer 15 is formed is facing outward, the diameter of the mandrel is gradually changed to one that is smaller, and the diameter of the mandrel that is 0.2 mm larger than the diameter of the mandrel at which the first crack was discovered is preferably 4.0φmm or less, more preferably 3.5φmm or less, and even more preferably 3.0φmm or less.

[0068] Furthermore, when the thickness of the hard coat layer of the optical laminate is 2 μm, if the optical laminate 10, 102 is bent 180° so that the surface on which the antifouling layer 15 is formed is on the inside, the diameter of the mandrel is gradually changed to one that is smaller, and the diameter of the mandrel that is 0.2 mm larger than the diameter of the mandrel at which the first crack was discovered is preferably 1.1φmm or less, and more preferably less than 1.0φmm.

[0069] Furthermore, when the thickness of the hard coat layer of the optical laminate is 2 μm, when the optical laminate 10, 102 is bent 180° so that the surface on which the antifouling layer 15 is formed is on the outside, the diameter of the mandrel is gradually reduced, and the diameter of the mandrel that is 0.2 mm larger than the diameter of the mandrel at which a crack was first discovered is 4.0 φmm or less; and it is more preferable that when the optical laminate 10, 102 is bent 180° so that the surface on which the antifouling layer 15 is formed is on the inside, the diameter of the mandrel that is 0.2 mm larger than the diameter of the mandrel at which a crack was first discovered is 1.1 φmm or less.

[0070] The mandrel diameter is calculated by cutting out three pieces from the same sample, measuring them, and averaging the three measurements.

[0071] [Method for Manufacturing Optical Laminate] The optical laminate 10 of this embodiment shown in FIG. 2 can be manufactured, for example, by the method described below. In this embodiment, as an example of a method for manufacturing the optical laminate 10, a case in which the optical laminate 10 is manufactured using a transparent substrate 11 wound in a roll shape will be described. First, the transparent substrate 11 wound in a roll shape is unwound. Then, a slurry containing a material for forming the hard coat layer 12 is applied to the transparent substrate 11 by a known method, and cured by a known method corresponding to the material for forming the hard coat layer 12. Examples of the slurry used include a composition containing a binder resin and silica particles as a filler. This composition is applied to the transparent substrate 11 and then cured. This forms the hard coat layer 12 on the transparent substrate 11 (hard coat layer forming process). The composition may contain one or more additives, such as a polymerization initiator and a leveling agent, as necessary. As the polymerization initiator, for example, a photopolymerization initiator is used. Then, the transparent substrate 11 with the hard coat layer 12 formed on its surface is wound into a roll by a known method.

[0072] Next, an adhesion layer forming step is performed to form an adhesion layer 13 on the hard coat layer 12, and an optical function layer forming step is performed to form an optical function layer 14. Thereafter, an antifouling layer forming step is performed to form an antifouling layer 15 on the optical function layer 14. In this embodiment, it is preferable to perform a first surface treatment step to treat the surface of the hard coat layer 12 before the optical function layer forming step, and then perform the adhesion layer forming step and the optical function layer forming step. Also, in this embodiment, it is preferable to perform a second surface treatment step to treat the surface of the optical function layer 14 after the optical function layer forming step, and then perform the antifouling layer forming step.

[0073] In the method for producing the optical laminate 10 of this embodiment, the first surface treatment step, the adhesion layer formation step, the optical functional layer formation step, the second surface treatment step, and the antifouling layer formation step are preferably performed consecutively while the optical laminate in the middle of production is maintained under reduced pressure. When the first surface treatment step, the adhesion layer formation step, the optical functional layer formation step, the second surface treatment step, and the antifouling layer formation step are performed consecutively while the optical laminate in the middle of production is maintained under reduced pressure, for example, a sputtering device equipped with the thin film formation device described in Patent Document 4 can be used.

[0074] A specific example of a manufacturing apparatus that can be used in the method for manufacturing an optical laminate of this embodiment is a manufacturing apparatus 20 shown in Figure 3. The manufacturing apparatus 20 shown in Figure 3 includes a roll unwinding apparatus 4, a pretreatment apparatus 2A, a sputtering apparatus 1, a pretreatment apparatus 2B, a vapor deposition apparatus 3, and a roll winding apparatus 5. As shown in Figure 3, these apparatuses 4, 2A, 1, 2B, 3, and 5 are connected in this order. The manufacturing apparatus 20 shown in Figure 3 is a roll-to-roll type manufacturing apparatus that unwinds a substrate from a roll, passes the substrate through connected apparatuses (pretreatment apparatus 2A, sputtering apparatus 1, pretreatment apparatus 2B, and vapor deposition apparatus 3 in Figure 3) in succession, and then winds it up, thereby continuously forming multiple layers on the substrate.

[0075] When the optical laminate 10 is manufactured using a roll-to-roll manufacturing device, the conveying speed (line speed) of the optical laminate 10 during manufacturing can be appropriately set. The conveying speed is, for example, preferably 0.5 to 20 m / min, and more preferably 0.5 to 10 m / min.

[0076] <Roll Unwinding Device> The roll unwinding device 4 shown in Figure 3 has a chamber 34, the interior of which is maintained at a predetermined reduced pressure, one or more vacuum pumps 21 (one in Figure 3) that evacuate the gas inside the chamber 34 to create a reduced pressure atmosphere, and an unwinding roll 23 and a guide roll 22 installed in the chamber 34. As shown in Figure 3, the chamber 34 is connected to the chamber 31 of the sputtering apparatus 1 via a pretreatment device 2A. A transparent substrate 11 having a hard coat layer 12 formed on its surface is wound around the unwinding roll 23. The unwinding roll 23 supplies the transparent substrate 11 having the hard coat layer 12 formed on its surface to the pretreatment device 2A at a predetermined transport speed.

[0077] <Pretreatment Device 2A> Pretreatment device 2A shown in Fig. 3 has a chamber 32 with a predetermined reduced pressure atmosphere inside, a can roll 26, a plurality of guide rolls 22 (two in Fig. 3), and a plasma discharge device 42. As shown in Fig. 3, can roll 26, guide roll 22, and plasma discharge device 42 are installed in chamber 32. As shown in Fig. 3, chamber 32 is connected to chamber 31 of sputtering device 1.

[0078] The can roll 26 and guide roll 22 transport the transparent substrate 11 on which the hard coat layer 12 has been formed, sent from the roll unwinding device 4, at a predetermined transport speed, and send the transparent substrate 11 with the surface of the hard coat layer 12 treated thereon to the sputtering device 1. As shown in FIG. 3 , the plasma discharge device 42 is disposed opposite the outer circumferential surface of the can roll 26 at a predetermined distance. The plasma discharge device 42 ionizes the gas by glow discharge. The gas is preferably inexpensive, inert, and does not affect the optical properties. For example, argon gas, oxygen gas, nitrogen gas, helium gas, etc. can be used. In this embodiment, argon gas or oxygen gas is preferably used as the gas.

[0079] <Sputtering Apparatus> The sputtering apparatus 1 shown in Fig. 3 has a chamber 31 the interior of which is maintained at a predetermined reduced pressure, one or more vacuum pumps 21 (two in Fig. 3) that exhaust gas from the chamber 31 to create a reduced pressure atmosphere, a film-forming roll 25, a plurality of guide rolls 22 (two in Fig. 4), and a plurality of film-forming units 41 (four in the example shown in Fig. 3). As shown in Fig. 3, the film-forming roll 25, the guide roll 22, and the film-forming units 41 are installed in the chamber 31. As shown in Fig. 3, the chamber 31 is connected to a chamber 32 of a pretreatment device 2B.

[0080] The film-forming roll 25 and the guide roll 22 transport the transparent substrate 11 having the surface-treated hard coat layer 12 formed thereon, sent from the pretreatment device 2A, at a predetermined transport speed, and supply the transparent substrate 11 having the adhesion layer 13 and the optical functional layer 14 formed on the hard coat layer 12 to the pretreatment device 2B. In the sputtering device 1 shown in Fig. 3, the adhesion layer 13 is laminated by sputtering on the hard coat layer 12 of the transparent substrate 11 traveling on the film-forming roll 25, and high refractive index layers 14a and low refractive index layers 14b are alternately laminated thereon to form the optical functional layer 14.

[0081] As shown in FIG. 3 , multiple film forming units 41 are disposed facing the outer circumferential surface of the film forming roll 25 at a predetermined distance, surrounding the film forming roll 25. The number of film forming units 41 is determined based on the total number of layers including the adhesive layer 13 and the high-refractive index layers 14a and low-refractive index layers 14b that form the optical functional layer 14. When the total number of layers including the adhesive layer 13 and the high-refractive index layers 14a and low-refractive index layers 14b that form the optical functional layer 14 is large, making it difficult to ensure sufficient distance between adjacent film forming units 41, multiple film forming rolls 25 may be provided within the chamber 31, and film forming units 41 may be disposed around each film forming roll 25. When multiple film forming rolls 25 are provided, additional guide rolls 22 may be installed as necessary. Multiple chambers 31 each equipped with a film forming roll 25 and a film forming unit 41 may be connected together. Furthermore, the diameter of the film forming roll 25 may be appropriately changed to facilitate ensuring sufficient distance between adjacent film forming units 41.

[0082] A predetermined target (not shown) is installed in each film forming unit 41. A voltage is applied to the target using a known structure. In this embodiment, a gas supply unit (not shown) that supplies a predetermined reactive gas and carrier gas to the target at a predetermined flow rate, and a known magnetic field generating source (not shown) that forms a magnetic field on the surface of the target are installed near the target.

[0083] The target material and the type and flow rate of the reactive gas are appropriately determined depending on the compositions of the adhesive layer 13, the high refractive index layer 14a, and the low refractive index layer 14b formed on the transparent substrate 11 by passing between the film forming unit 41 and the film forming roll 25. For example, SiO 2 When forming a layer made of NbO, Si is used as the target and O is used as the reactive gas. Furthermore, when forming a layer made of NbO, for example, Nb is used as the target and O is used as the reactive gas. The low-refractive index layer 14b is preferably formed at a vacuum level of less than 0.5 Pa, and the high-refractive index layer 14a is preferably formed at a vacuum level of less than 1.0 Pa. When these layers are formed at the above vacuum levels, the optical function layer 14 becomes dense, the water vapor permeability decreases, and durability and other properties improve.

[0084] In this embodiment, it is preferable to use magnetron sputtering as the sputtering method from the viewpoint of increasing the film formation rate. However, the sputtering method is not limited to magnetron sputtering, and a two-pole sputtering method using plasma generated by direct current glow discharge or high frequency, a three-pole sputtering method with a hot cathode, or the like may also be used.

[0085] The sputtering apparatus 1 includes an optical monitor (not shown) as a measuring unit that measures optical properties after depositing each layer that will become the adhesion layer 13 and the optical functional layer 14. This makes it possible to confirm the quality of the formed adhesion layer 13 and the optical functional layer 14. When the sputtering apparatus 1 has, for example, two or more chambers, it is preferable to install an optical monitor in each chamber.

[0086] An example of an optical monitor (not shown) is one that uses an optical head capable of scanning in the width direction to measure the optical properties in the width direction of the adhesion layer 13 and the optical functional layer 14 formed on the hard coat layer 12. When such an optical monitor is provided, for example, the peak wavelength of reflectance is measured as the optical property, and the measured value is converted into an optical thickness, thereby measuring the optical thickness distribution in the width direction of the adhesion layer 13 and the optical functional layer 14. By measuring the optical properties using the optical monitor, it is possible to form an optical laminate 10 including an adhesion layer 13 and an optical functional layer 14 having optimal optical properties while adjusting the sputtering conditions in real time.

[0087] <Pretreatment device 2B> Pretreatment device 2B shown in Fig. 3 has a chamber 32, the interior of which is kept at a predetermined reduced pressure, a can roll 26, a plurality of guide rolls 22 (two in Fig. 3), and a plasma discharge device 42. As shown in Fig. 3, can roll 26, guide roll 22, and plasma discharge device 42 are installed in chamber 32. As shown in Fig. 3, chamber 32 is connected to chamber 33 of vapor deposition device 3.

[0088] The can roll 26 and the guide roll 22 transport the transparent substrate 11, on which each layer up to the optical functional layer 14 has been formed, sent from the sputtering device 1 at a predetermined transport speed, and send the transparent substrate 11, on which the surface of the optical functional layer 14 has been treated, to the vapor deposition device 3. As the plasma discharge device 42, for example, one similar to the pretreatment device 2A can be used.

[0089] 4 includes a chamber 33 the interior of which is maintained at a predetermined reduced pressure, one or more vacuum pumps 21 (one in FIG. 3 ) that exhaust gas from the chamber 33 to create a reduced pressure atmosphere, multiple guide rolls 22 (four in FIG. 3 ), a vapor deposition source 43, and a heating device 53. As shown in FIG. 3 , the guide rolls 22 and the vapor deposition source 43 are installed in the chamber 33. The chamber 33 is connected to a chamber 35 of the roll winding device 5.

[0090] The vapor deposition source 43 is disposed opposite the transparent substrate 11, the surface of which is treated and is being transported substantially horizontally between two adjacent guide rolls 22. The vapor deposition source 43 supplies evaporation gas composed of the material that will become the antifouling layer 15 onto the optical function layer 14. The orientation of the vapor deposition source 43 can be set as desired. The heating device 53 heats the material that will become the antifouling layer 15 to a vapor pressure temperature. The heating device 53 can be a resistance heating device, a heater heating device, an induction heating device, an electron beam heating device, or the like. In the resistance heating device, a container containing the antifouling material that will become the antifouling layer 15 is heated by passing electricity through it as a resistor. In the heater heating device, the container is heated by a heater disposed around the container. In the induction heating device, the container or the antifouling material is heated by electromagnetic induction from an externally installed induction coil.

[0091] The vapor deposition apparatus 3 shown in FIG. 3 includes a guide plate (not shown) for guiding the vapor deposition material evaporated by the vapor deposition source 43 to a predetermined position, a film thickness meter (not shown) for observing the thickness of the antifouling layer 15 formed by vapor deposition, a vacuum pressure gauge (not shown) for measuring the pressure inside the chamber 33, and a power supply (not shown). The guide plate may have any shape as long as it can guide the evaporated vapor deposition material to the desired position. If not necessary, the guide plate need not be provided. An ion gauge, for example, can be used as the vacuum pressure gauge. An example of the power supply is a high-frequency power supply.

[0092] <Roll Winding Device> The roll winding device 5 shown in Figure 3 has a chamber 35 the interior of which is maintained at a predetermined reduced pressure, one or more vacuum pumps 21 (one in Figure 3) that evacuate gas from the chamber 35 to create a reduced pressure atmosphere, and a winding roll 24 and a guide roll 22 installed in the chamber 35. A transparent substrate 11 (optical laminate 10) having each layer up to the antifouling layer 15 formed on its surface is wound around the winding roll 24. The winding roll 24 and the guide roll 22 wind up the optical laminate 10 at a predetermined winding speed. A carrier film may also be used as necessary.

[0093] 4 may be equipped with a dry pump, an oil rotary pump, a turbomolecular pump, an oil diffusion pump, a cryopump, a sputter ion pump, a getter pump, etc. The vacuum pumps 21 may be appropriately selected or combined to create a desired reduced pressure state in each of the chambers 31, 32, 33, 34, and 35.

[0094] The location and number of vacuum pumps 21 installed in manufacturing apparatus 20 are not particularly limited as long as they can maintain both chamber 31 of sputtering apparatus 1 and chamber 33 of vapor deposition apparatus 3 at the desired reduced pressure. In manufacturing apparatus 20 shown in FIG. 3 , roll unwinding device 4, pretreatment device 2A, sputtering apparatus 1, pretreatment device 2B, vapor deposition apparatus 3, and roll take-up device 5 are connected. Therefore, vacuum pumps 21 may be installed in each of chambers 31, 32, 33, 34, and 35, or may be installed in only some of chambers 31, 32, 33, 34, and 35, as long as they can maintain both chamber 31 of sputtering apparatus 1 and chamber 33 of vapor deposition apparatus 3 at the desired reduced pressure.

[0095] Next, a method for continuously performing the first surface treatment step, the adhesion layer forming step, the optical function layer forming step, the second surface treatment step, and the antifouling layer forming step while maintaining the optical laminate 10 under reduced pressure using the manufacturing apparatus 20 shown in Fig. 3 will be described. First, an unwinding roll 23 around which a transparent substrate 11 having a hard coat layer 12 formed on its surface is wound is placed in the chamber 34 of the roll unwinding device 4. Then, the unwinding roll 23 and the guide roll 22 are rotated, and the transparent substrate 11 having the hard coat layer 12 formed on its surface is sent to the pretreatment device 2A at a predetermined transport speed.

[0096] Next, in the chamber 32 of the pretreatment device 2A, a first surface treatment step is performed as a pretreatment for the surface on which the adhesion layer 13 and the optical functional layer 14 are to be formed. In this embodiment, the first surface treatment step is performed on the transparent substrate 11 on which the hard coat layer 12 has been formed. In the first surface treatment step, the can roll 26 and the guide roll 22 are rotated to transport the transparent substrate 11 on which the hard coat layer 12 has been formed at a predetermined transport speed, while treating the surface of the hard coat layer 12 running on the can roll 26.

[0097] For example, glow discharge treatment, plasma treatment, ion etching, alkali treatment, etc. can be used as a surface treatment method for the hard coat layer 12. As described above, among these, glow discharge treatment is preferred because it allows treatment over a large area.

[0098] Next, an adhesion layer forming step and an optical function layer forming step are performed in the chamber 31 of the sputtering apparatus 1. Specifically, the film forming roll 25 and the guide roll 22 are rotated to transport the transparent substrate 11 on which the hard coat layer 12 has been formed at a predetermined transport speed, and the adhesion layer 13 and the optical function layer 14 are formed on the hard coat layer 12 running on the film forming roll 25.

[0099] In this embodiment, the adhesion layer 13 is formed by sputtering while changing the target material installed in each film formation unit 41 or the type and flow rate of the reactive gas supplied from the gas supply unit, and high-refractive index layers 14a and low-refractive index layers 14b are alternately laminated on top of the adhesion layer 13. That is, the adhesion layer formation process and the optical function layer formation process are performed consecutively within the sputtering apparatus 1. In this manner, the adhesion layer 13 and the optical function layer 14, which is an anti-reflection layer, are formed. The high-refractive index layers 14a and low-refractive index layers 14b are each formed under conditions of a predetermined vacuum level or lower. Specifically, the high-refractive index layers 14a are formed at a vacuum level of less than 1.0 Pa, and the low-refractive index layers 14b are formed at a vacuum level of less than 0.5 Pa.

[0100] When a SiOx film is formed as the adhesion layer 13, it is preferably formed by reactive sputtering using a silicon target in a mixed gas atmosphere of oxygen gas and argon gas. When the adhesion layer 13, the high-refractive index layer 14a, and the low-refractive index layer 14b are successively laminated by sputtering, different target materials may be used for forming the adhesion layer 13, the high-refractive index layer 14a, and the low-refractive index layer 14b. Alternatively, for example, one type of material may be used as the target, and layers made of the target material and layers made of an oxide of the target material may be alternately formed by changing the oxygen (reactive gas) flow rate during sputtering, to form the adhesion layer 13, the high-refractive index layer 14a, and the low-refractive index layer 14b.

[0101] The pressure during sputtering to form the adhesion layer 13 and the optical function layer 14 varies depending on the metal to be sputtered, but may be 2 Pa or less, preferably 1 Pa or less, more preferably 0.6 Pa or less, and particularly preferably 0.2 Pa or less. When the pressure during sputtering is reduced to 1 Pa or less, the mean free path of the film-forming molecules becomes longer, and the film-forming molecules are deposited while maintaining high energy, resulting in a denser and better film quality. It is preferable that the pressure during sputtering of the high refractive index layer and the low refractive index layer be different. This is because the mean free path differs depending on the film-forming species. By changing the pressure for each film-forming species, a denser film can be formed.

[0102] Thereafter, the transparent substrate 11, on which the adhesion layer 13 and the optical functional layer 14 have been formed on the hard coat layer 12, is sent to the pretreatment device 2B by the rotation of the film-forming roll 25 and the guide roll 22. Next, a second surface treatment process is performed in the chamber 32 of the pretreatment device 2B as a pretreatment for the surface on which the antifouling layer 15 is to be formed. In this embodiment, the transparent substrate 11 on which the optical functional layer 14 has been formed, obtained in the optical functional layer forming process, is continuously subjected to the second surface treatment process while being maintained under reduced pressure without being exposed to the atmosphere. In the second surface treatment process, the can roll 26 and the guide roll 22 are rotated to transport the transparent substrate 11 on which each layer up to the optical functional layer 14 has been formed at a predetermined transport speed, while a discharge treatment is performed on the surface of the optical functional layer 14 running on the can roll 26.

[0103] Examples of methods that can be used to treat the surface of the optical functional layer 14 include glow discharge treatment, plasma treatment, ion etching, and alkali treatment. Among these, glow discharge treatment is preferred because it allows treatment over a large area.

[0104] When the surface of the optical functional layer 14 is subjected to a discharge treatment, the surface of the optical functional layer 14 is etched, and the surface condition of the optical functional layer 14 changes. The surface condition of the optical functional layer 14 is expressed by the surface roughness Ra or the average element length RSm. For example, in the case of a clear anti-reflection film in which the haze of the optical functional layer 14 is 2.0 or less, the surface condition of the optical functional layer 14 is easily defined by the surface roughness Ra. Furthermore, in the case of an AG anti-reflection film in which the haze of the optical functional layer 14 is greater than 2.0, the surface condition of the optical functional layer 14 is easily defined by the average element length RSm. The surface roughness Ra and the average element length RSm are measured in accordance with JIS B0601 (ISO 4287).

[0105] Thereafter, the transparent substrate 11 with the treated surface of the optical functional layer 14 is sent to the vapor deposition device 3 by rotation of the can roll 26 and the guide roll 22. Next, an antifouling layer forming step is performed in the chamber 33 of the vapor deposition device 3. In this embodiment, the transparent substrate 11 with the treated surface of the optical functional layer 14 obtained by the second surface treatment step is continuously subjected to the antifouling layer forming step while being maintained under reduced pressure without being exposed to the atmosphere. In the antifouling layer forming step, a vapor deposition source 43 is vapor-deposited on the surface of the optical functional layer 14 while the guide roll 22 is rotated and the transparent substrate 11 with the treated surface of the optical functional layer 14 is transported at a predetermined transport speed.

[0106] In this embodiment, for example, an antifouling material made of a fluorine-based organic compound that will become the antifouling layer 15 is heated to a vapor pressure temperature by a heating device 53, and the resulting evaporated gas is supplied from a vapor deposition source 43 in a reduced pressure environment and adhered to the surface-treated optical function layer 14, thereby forming the antifouling layer 15 by vacuum deposition. The pressure during vacuum deposition of the antifouling layer 15 is, for example, preferably 0.05 Pa or less, more preferably 0.01 Pa or less, and particularly preferably 0.001 Pa or less. When the pressure during vacuum deposition is a reduced pressure of 0.05 Pa or less, the mean free path of the film-forming molecules is long and the deposition energy is high, resulting in a denser and better antifouling layer 15.

[0107] By the above method, an optical laminate 10 is obtained in which the antifouling layer 15 is formed by vacuum deposition on the adhesion layer 13 and the optical function layer 14 formed by sputtering. The antifouling layer 15 after film formation preferably has an initial fluorine content of 0.03 or more as measured by X-ray fluorescence spectroscopy (XRF).

[0108] Thereafter, the transparent substrate 11 (optical laminate 10) on which each layer up to the antifouling layer 15 has been formed is sent to the roll winding device 5 by the rotation of the guide roll 22. Then, in the chamber 35 of the roll winding device 5, the optical laminate 10 is wound around the winding roll 24 by the rotation of the winding roll 24 and the guide roll 22.

[0109] In this embodiment, it is preferable to perform the optical functional layer forming process and the antifouling layer forming process continuously under reduced pressure. In particular, when the optical laminate 10 is continuously produced as a wound body using a roll-to-roll method, as in the manufacturing method of this embodiment using the manufacturing apparatus 20 shown in FIG. 3 , it is more preferable to perform the optical functional layer forming process and the antifouling layer forming process continuously in-line while maintaining a reduced pressure. "In-line" means that the antifouling layer forming process is performed without exposing the optical functional layer 14 formed in the optical functional layer forming process to the atmosphere. By performing the optical functional layer forming process and the antifouling layer forming process continuously under reduced pressure, the generation of a natural oxide film on the optical functional layer 14 formed in the optical functional layer forming process before the antifouling layer 15 is formed is suppressed. Furthermore, it is possible to prevent contamination such as foreign matter from adhering to the optical functional layer 14 during winding of the roll and inhibiting adhesion between the optical functional layer 14 and the antifouling layer 15. Therefore, compared to when, after the optical functional layer formation process, the transparent substrate 11 on which each layer up to the optical functional layer 14 has been formed is removed from the chamber under reduced pressure, and then placed back into the chamber to perform the anti-fouling layer formation process under reduced pressure, an optical laminate with good adhesion between the optical functional layer 14 and the anti-fouling layer 15 and excellent transparency can be obtained.

[0110] Furthermore, since the antifouling layer 15 of the optical laminate 10 of this embodiment is a vapor-deposited film, it has higher abrasion resistance than, for example, an antifouling film formed by a coating method. This is presumably due to the following reasons. In other words, an antifouling film formed by a coating method has voids caused by the solvent contained in the paint. In contrast, a vapor-deposited film does not have voids caused by the solvent. For this reason, it is presumed that a vapor-deposited film has a higher density and has higher abrasion resistance and alkali resistance than an antifouling film formed by a coating method.

[0111] The method for producing the optical laminate 10 of this embodiment includes an adhesion layer forming step of forming an adhesion layer 13, an optical function layer forming step of forming an optical function layer 14 by alternately laminating high refractive index layers 14a and low refractive index layers 14b, a second surface treatment step of treating the surface of the optical function layer 14, and an antifouling layer forming step of forming an antifouling layer 15 on the surface-treated optical function layer 14. Therefore, adhesion between the optical function layer 14 and the antifouling layer 15 formed on the optical function layer 14 is good, and the abrasion resistance and alkali resistance are further improved.

[0112] In this embodiment, when the first surface treatment process, the optical functional layer formation process, the second surface treatment process, and the antifouling layer formation process are performed successively while maintaining the optical laminate in the middle of production under reduced pressure, the reduced pressure conditions in the chambers of, for example, the sputtering apparatus and the vapor deposition apparatus may be different, as long as they do not interfere with each production process.

[0113] In this embodiment, it is preferable to measure the film formation results over time using a measuring device in one or more of the adhesion layer formation process, optical function layer formation process, and antifouling layer formation process, and feed the results back to the conditions of the subsequent manufacturing process. This makes it easier to optimize the properties of the entire optical laminate and make the in-plane properties of the optical laminate uniform. In addition, the measuring device can also be used to feedback the manufacturing conditions in the same process. In this case, the layer formed in that process will have uniform and stable properties.

[0114] In this embodiment, the second surface treatment step is performed between the optical functional layer forming step and the antifouling layer forming step, but the second surface treatment step may be performed as needed or may not be performed. Even when the second surface treatment step is not performed, it is preferable to perform the optical functional layer forming step and the antifouling layer forming step consecutively under reduced pressure.

[0115] In the manufacturing method of this embodiment, the optical function layer is formed under conditions of a predetermined vacuum level or less. This results in a dense optical function layer 14, a reduced water vapor permeability, and improved abrasion resistance and alkali resistance. Furthermore, by ensuring that the antifouling layer has a thickness equal to or greater than the predetermined thickness, sufficient abrasion resistance and alkali resistance can be ensured.

[0116] In the present embodiment, an example has been described in which optical laminate 10 is continuously produced by a roll-to-roll method using production apparatus 20 shown in Fig. 3 that includes pretreatment device 2A, sputtering device 1, pretreatment device 2B, vapor deposition device 3, roll unwinding device 4, and roll winding device 5, but the production apparatus for producing optical laminate 10 is not limited to production apparatus 20 shown in Fig. 3. For example, a production apparatus that does not include pretreatment device 2A and pretreatment device 2B, but instead includes roll unwinding device 4, sputtering device 1, vapor deposition device 3, and roll winding device 5 connected in this order, may be used.

[0117] 3 may be provided with a pretreatment chamber (not shown) between the chamber 33 of the vapor deposition device 3 and the chamber 32 of the pretreatment device 2B for cleaning the surface of the optical functional layer 14 on which the antifouling layer 15 is to be formed. The manufacturing device 20 shown in Fig. 3 may be provided with a posttreatment chamber (not shown) between the chamber 33 of the vapor deposition device 3 and the chamber 35 of the roll winding device 5 for cooling and / or inspecting the transparent substrate 11 on which each layer up to the antifouling layer 15 has been formed.

[0118] 3 may be provided with a hard coat layer forming device between the roll unwinding device 4 and the sputtering device 1 for forming a hard coat layer 12 on the surface of the transparent substrate 11. In this case, not only the optical functional layer 14 and the antifouling layer 15 but also the hard coat layer 12 can be continuously produced by the roll-to-roll method, which is preferable.

[0119] In this embodiment, an example has been described in which the optical functional layer formation process is performed using a sputtering device and the antifouling layer formation process is performed using a vapor deposition device, but if the second surface treatment process is not performed, the optical functional layer formation process and the antifouling layer formation process may be performed in the same device (within one chamber).

[0120] In the optical laminate 10 of this embodiment, various layers may be provided as needed on the surface of the transparent substrate opposite to the surface on which the optical functional layer or the like is formed. For example, a pressure-sensitive adhesive layer used for adhesion to other members may be provided. Furthermore, another optical film may be provided via this pressure-sensitive adhesive layer. Examples of other optical films include a polarizing film, a retardation compensation film, a half-wave plate, and a film that functions as a quarter-wave plate.

[0121] Furthermore, a layer having functions such as antireflection, selective reflection, antiglare, polarization, phase difference compensation, viewing angle compensation or expansion, light guiding, diffusion, brightness improvement, hue adjustment, and conductivity may be directly formed on the opposing surface of the transparent substrate. The optical laminate may have a smooth shape, or a shape having a nano-order uneven structure that exhibits moth-eye and antiglare functions. It may also have a geometric shape on the order of microns to millimeters, such as a lens or prism. The shape can be formed, for example, by a combination of photolithography and etching, shape transfer, heat pressing, or the like. In this embodiment, since the film is formed by vapor deposition or the like, even if the substrate has an uneven shape, the uneven shape can be maintained.

[0122] The article of this embodiment is, for example, a liquid crystal display panel, an organic EL display panel, etc., in which the above-described optical laminate 10 is provided on the display surface of an image display unit. This makes it possible to impart high abrasion resistance and alkali resistance to, for example, the touch panel display unit of a smartphone or an operating device, and to realize an image display device that is excellent in durability and suitable for practical use.

[0123] Furthermore, the article is not limited to an image display device, and may be any article to which the optical laminate 10 can be applied, such as window glass or goggles having the optical laminate of this embodiment provided on the surface, the light receiving surface of a solar cell, a smartphone screen or a display such as a notebook PC, an information input terminal, a tablet terminal, an AR (augmented reality) device, a VR (virtual reality) device, an electronic display board, the surface of a glass table, a gaming machine, an operation support device for an aircraft or a train, a navigation system, an instrument panel, or the surface of an optical sensor.

[0124] Although an embodiment of the present invention has been described above, this embodiment is presented as an example and is not intended to limit the scope of the invention. This embodiment can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are within the scope and spirit of the invention, as well as the invention described in the claims and their equivalents. For example, instead of the hard coat layer 12, an anti-glare layer can be formed, or any functional layer can be added as needed, such as a flexible soft coat layer. These may also be laminated.

[0125] Examples of the present invention will be described below. Note that the optical laminates produced in the following examples and comparative examples are examples that function as anti-reflection films, and the scope of the present invention is not limited to these.

[0126] <Preparation of Composition for Hard Coat Layer> First, a photocurable composition 1 was prepared, which contained 28 mass % of silica particles (filler) with an average particle size of 50 nm relative to the total solid content of the composition. Composition 1 was prepared by dissolving acrylate (binder resin), silica particles, and a photopolymerization initiator in a solvent, as shown in Table 1, and further adding a leveling agent.

[0127]

[0128] CN968: hexafunctional aliphatic urethane acrylate having a polyester skeleton SR610: polyethylene glycol diacrylate, average molecular weight of polyethylene glycol chain 600 PGM-AC-4130Y: silica sol surface-modified with a methacryloyl group-containing silane compound, dispersion medium propylene glycol monomethyl ether Ominirad 184: 1-hydroxy-cyclohexyl-phenyl-ketone

[0129] (Example 1) A 50 μm thick PET film was used as a transparent substrate, and the above-mentioned composition 1 was applied onto this PET film using a bar coater. Then, composition 1 was photopolymerized to form a 5 μm thick hard coat layer on the transparent substrate.

[0130] Next, the surface of the hard coat layer was subjected to an electrode power density of 5500 W / m 2 Subsequently, a surface treatment was carried out on the hard coat layer by glow discharge treatment using a Si target and a Nb target as sputtering targets, and Ar gas and O 2 The adhesive layer and the optical functional layer were successively formed by reactive sputtering using a mixed gas of Nb and Si. That is, a 3 nm thick adhesive layer made of silicon oxide (SiOx, 0<x<2) which may be oxygen deficient and a 10 nm thick Nb 2 O 5 a first high refractive index material layer made of SiO 2 a first low refractive index material layer made of Nb 2 O 5 and a second high refractive index material layer made of SiO 2 and a second low refractive index material layer made of the above material were deposited in this order.

[0131] Next, the pressure in the deposition chamber was 0.01 Pa, the deposition temperature was 230° C., and the retention time was 7.2 s. 2 An antifouling layer having a thickness of 3 nm and made of an alkoxysilane compound having a perfluoropolyether group (KY1903-1, manufactured by Shin-Etsu Chemical Co., Ltd.) was formed on the film by vapor deposition to prepare an optical laminate (anti-reflection film) of the example.

[0132] (Example 2) Electrode power density during glow discharge treatment was 5500 W / m 2 to 1100 W / m 2 An optical laminate was obtained in the same manner as in Example 1, except that the above-mentioned step was changed to the above-mentioned step.

[0133] (Example 3) The electrode power density of the glow discharge treatment was 5500 W / m 2 to 6600 W / m 2 An optical laminate was obtained in the same manner as in Example 1, except that the above-mentioned step was changed to the above-mentioned step.

[0134] Example 4 An optical layered body was obtained in the same manner as in Example 1, except that the thickness of the hard coat layer formed on the transparent substrate was 2 μm.

[0135] Example 5 An optical layered body was obtained in the same manner as in Example 1, except that the composition for the hard coat layer was changed to Composition 2.

[0136] Example 6 An optical layered body was obtained in the same manner as in Example 1, except that the composition for the hard coat layer was changed to Composition 3.

[0137] Example 7 An optical laminate was obtained in the same manner as in Example 1, except that a 23 μm thick PET film was used as the transparent substrate instead of the 50 μm thick PET film.

[0138] Example 8 An optical layered body was obtained in the same manner as in Example 1, except that the thickness of the hard coat layer formed on the transparent substrate was 10 μm.

[0139] (Example 9) Electrode power density during glow discharge treatment was 5500 W / m 2 to 3300 W / m 2 An optical laminate was obtained in the same manner as in Example 8, except that the above-mentioned step was changed to the above-mentioned step.

[0140] (Example 10) Electrode power density during glow discharge treatment was 5500 W / m 2 to 1100 W / m 2 An optical laminate was obtained in the same manner as in Example 8, except that the above-mentioned step was changed to the above-mentioned step.

[0141] (Example 11) Electrode power density during glow discharge treatment was 5500 W / m 2 to 550 W / m 2 An optical laminate was obtained in the same manner as in Example 8, except that the above-mentioned step was changed to the above-mentioned step.

[0142] (Comparative Example 1) Composition 1 for forming the hard coat layer was changed to composition 4 shown in Table 1, and the electrode power density during the glow discharge treatment was 5000 W / m 2 An optical laminate was obtained in the same manner as in Example 1, except that:

[0143] (Comparative Example 2) The thickness of the hard coat layer formed on the transparent substrate was 10 μm, and the electrode power density during the glow discharge treatment was 5000 W / m 2 to 1100 W / m 2 An optical laminate was obtained in the same manner as in Comparative Example 1, except that the above-mentioned step was changed to the above-mentioned step.

[0144] Next, the optical laminates obtained in Examples 1 to 11 and Comparative Examples 1 and 2 were measured and evaluated by the following methods.

[0145] <Bending Test> An optical laminate cut into a size of 1 cm x 15 cm was prepared as a sample. The cut surface of the optical laminate was confirmed to be free of cracks. A 5.0 mm mandrel was set in a bending tester capable of setting a mandrel. The optical laminate was set in this tester so that the surface on which the antifouling layer was formed faced outward. The tester was then bent over 2 seconds to bend the optical laminate 180° and held for 10 seconds. The presence or absence of cracks in the antifouling layer was then confirmed visually and with an optical microscope. The above procedure was repeated, with the mandrel diameter being replaced with a smaller one every 0.2 mm, until abnormalities such as cracks were observed visually and with an optical microscope on the surface of the antifouling layer side of the optical laminate. The diameter (φmm) of the mandrel 0.2 mm larger than the diameter of the mandrel at which the first crack was found was taken as the test result of the bending test. Similarly, measurements were also taken when the optical laminate was set in the above-mentioned testing machine so that the surface on which the antifouling layer was formed was bent inward, and the mandrel diameter (φmm) that was 0.2 mm larger than the mandrel diameter at which the first crack was discovered was taken as the test result of the bending test.

[0146] Furthermore, the theoretical elongation S (%) of the optical functional layer was calculated when a mandrel with the smallest diameter at which no cracks occurred was used. The elongation S was calculated as follows: S (%) = {(R2 / R1) - 1} x 100 (where R2 is the distance from the axial center of the mandrel to the outer surface of the optical laminate, and R1 is the distance from the axial center of the mandrel to a virtual line indicating a position corresponding to 1 / 2 of the total thickness of the optical laminate.)

[0147] Furthermore, when the optical functional layer was set so that the surface on which the antifouling layer was formed was bent inward, and a mandrel of the smallest diameter at which no cracks occurred was used, the theoretical compression ratio C (%) of the optical functional layer was calculated. The compression ratio C was calculated as follows: C (%) = {1 - (R3 / R1)} x 100 (where R3 is the distance from the axial center of the mandrel to the surface of the optical laminate on the antifouling layer side, and R1 is the distance from the axial center of the mandrel to an imaginary line indicating a position corresponding to 1 / 2 of the total thickness of the optical laminate.)

[0148] Three samples were prepared for each measurement, and each value was calculated as the average of the three measurements. The smallest mandrel diameter was 1.0 mm, and although 1.0 mm was used for measuring elongation, the result of the bending test was less than 1.0 mm because no cracks occurred.

[0149] <Martens Hardness> Using Compositions 1 to 4, laminates (samples) were prepared in which only a hard coat layer was formed on a transparent substrate. For the optical laminates obtained in Examples 1 to 11 and Comparative Examples 1 and 2, the Martens hardness of the antifouling layer side of the optical laminate was measured. For laminates in which only a hard coat layer was formed, the Martens hardness of the hard coat layer side of the laminate was measured. For the measurements, a microcompression tester (ENT-NEXUS, manufactured by Elionix, measuring indenter: Berkovich indenter) was used in accordance with ISO 14577-1. For the optical laminates, the hardness was measured at an indentation depth of 50 nm, and for laminates in which only a hard coat layer was formed, the hardness was measured when indented to a depth of 1 / 10 the thickness of the hard coat layer. The Martens hardness of the optical laminate measured above was designated (A), and the Martens hardness of a laminate in which only a hard coat layer was formed on a transparent substrate was designated (B), and the ratio (A) / (B) was calculated. The results are shown in Table 2.

[0150] The optical laminates obtained in Examples 1 to 11 and Comparative Examples 1 and 2 were measured and evaluated by the following methods.

[0151] <Contact angle measurement test for pure water> A fully automatic contact angle meter DM-700 (manufactured by Kyowa Interface Science Co., Ltd.) was used to measure by the ellipse fitting method under the following conditions. Pure water was placed in a glass syringe, and a stainless steel needle was attached to the tip, and the pure water was dripped onto the optical laminate (test piece). Amount of pure water dripped: 2.0 μL Measurement temperature: 25° C. The contact angles were measured at six arbitrary points on the surface of the test piece four seconds after the pure water was dripped onto the laminate (sample), and the average value was taken as the pure water contact angle.

[0152] <Steel wool sliding test> Using a friction tester type I conforming to JIS L0849, a friction body was horizontally reciprocated along the surface of the optical laminate (test piece) to obtain a test piece. Steel wool (#0000 manufactured by Bonstar Co., Ltd.) was used as the friction body. The test was set at a load of 1000 g / cm. 2 The sliding distance was 50 mm, the sliding speed was 60 rpm (1 reciprocation / second), and the number of reciprocations was 200 (100 reciprocations). After the sliding, the sample was subjected to the same test as the contact angle measurement test for pure water described above, and the difference in contact angle before and after the test was determined. The results are shown in Table 3.

[0153]

[0154]

[0155] The results in Table 2 indicate that in all of Examples 1 to 7, the ratio ((A) / (B)) of the Martens hardness (A) of the antifouling layer side of the optical laminate to the Martens hardness (B) of the hard coat layer side of a laminate having only a transparent substrate and a hard coat layer was 3.6 or less, thereby achieving excellent hardness while further improving flex resistance. In particular, it was found that the silica particles contained in the hard coat layer were surface-modified with methacryloyl groups derived from a methacryloyl group-containing silane compound, which is thought to more firmly bond the methacryloyl groups to the acrylate (binder resin), resulting in improved hardness of the optical laminate. Furthermore, it was found that the methacryloyl groups on the silica particle surfaces further improved adhesion between the hard coat layer and the adhesion layer, as well as between the hard coat layer and the optical functional layer via the adhesion layer, further improving flex resistance. Furthermore, in all of Examples 1 to 7, the difference in contact angle with water before and after rubbing, in which the steel wool was horizontally reciprocated 200 times, was 20° or less. This suggests that the silica particles contained in the hard coat layer are surface-modified with methacryloyl groups derived from the methacryloyl group-containing silane compound, and that the methacryloyl groups are more firmly bonded to the acrylate (binder resin). As a result, it was found that the hardness of the optical laminate was improved and excellent scratch resistance could be achieved.

[0156] ​Furthermore, from the results in Table 3, it was found that in all of Examples 8 to 11, the difference in contact angle with water before and after 200 horizontal reciprocating movements of steel wool was 20° or less, similar to Examples 1 to 7, and the hardness of the optical laminate was improved, enabling excellent scratch resistance to be realized. In addition, the ratio ((A) / (B)) of the Martens hardness (A) of the antifouling layer side of the optical laminate to the Martens hardness (B) of the hard coat layer side of a laminate having only a transparent substrate and a hard coat layer was 3.6 or less, and therefore it was found that excellent hardness could be realized while further improving flex resistance.

[0157] On the other hand, in Comparative Example 1, when a hard coat layer was formed using Composition 4 containing unsurface-modified silica particles, the ratio ((A) / (B)) was 3.71, resulting in a low hardness of the laminate. Furthermore, the elongation rate S (outward bending) was 1.22, and the compression rate C (inward bending) was 4.4, resulting in poor flex resistance.

[0158] In Comparative Example 2, when a hard coat layer was formed using Composition 2 containing unsurface-modified silica particles, the difference in contact angle was 23.6°, indicating a decrease in scratch resistance. Furthermore, the elongation rate S (outward bending) was 1.29, and the compression rate C (inward bending) was 3.63, indicating poor flex resistance.

[0159] DESCRIPTION OF SYMBOLS 10, 102...Optical laminate 11...Transparent substrate 12...Hard coat layer 13...Adhesion layer 14...Optical functional layer 14a...High refractive index layer 14b...Low refractive index layer 15...Anti-fouling layer 20...Manufacturing apparatus 1...Sputtering apparatus 2A, 2B...Pretreatment apparatus 3...Vapor deposition apparatus 4...Roll unwinding apparatus 5...Roll winding apparatus 20...Manufacturing apparatus 21...Vacuum pump 22...Guide roll 23...Unwinding roll 24...Winding roll 25...Film formation roll 26...Can roll 31, 32, 33, 34, 35...Chamber 41...Film formation section 42...Plasma discharge apparatus 43...Vapor deposition source 53...Heating apparatus

Claims

1. An optical laminate having a transparent substrate, a hard coat layer, an adhesion layer made of a sputtered film, an optical functional layer in which a high refractive index layer made of a sputtered film and a low refractive index layer having a refractive index lower than that of the high refractive index layer are alternately laminated, and an antifouling layer in this order, wherein the hard coat layer contains a silica filler, and the optical laminate satisfies the following conditions 1 and 2. Condition 1: The ratio ((A) / (B)) of the Martens hardness (A) measured from the antifouling layer side of the optical laminate to the Martens hardness (B) measured from the hard coat layer side of a laminate having only the entire transparent substrate and the hard coat layer is 3.6 or less. Condition 2: Using a friction tester using steel wool conforming to JIS L0849, the difference in contact angle with water before and after friction in which the steel wool is horizontally reciprocated 200 times is 20° or less.

2. The optical laminate according to claim 1, wherein the silica filler is surface-modified with a functional group derived from a silane compound.

3. The optical laminate according to claim 2, wherein the silane compound is one or more selected from a vinyl group-containing silane compound, a (meth)acryloyl group-containing silane compound, an amino group-containing silane compound, an isocyanate group-containing silane compound, an isocyanurate group-containing silane compound, an epoxy group-containing silane compound and a mercapto group-containing silane compound.

4. The optical laminate according to claim 2, wherein the silane compound is a (meth)acryloyl group-containing silane compound.

5. The optical laminate according to claim 2, wherein the hard coat layer contains a binder resin and a silica filler, and the functional group derived from the silane compound has the same functional group as that of the binder resin.

6. The optical laminate according to claim 5, wherein the binder resin contains a (meth)acrylate compound, and the functional group derived from the silane compound is a (meth)acryloyl group.

7. The optical laminate according to claim 1, wherein the average particle size of the silica filler is 800 nm or less.

8. The optical laminate according to claim 1, wherein the hard coat layer has a thickness of 0.5 μm or more and 100 μm or less.

9. The optical laminate according to claim 1, wherein when the optical laminate is folded 180° so that the surface on which the antifouling layer is formed is on the outside, and a mandrel of the smallest diameter on which no cracks occur is used, the elongation S (%) of the optical functional layer calculated by the following formula (1) satisfies 1.3≦S: S (%)={(R2 / R1)-1}×100 (1) (where R2 is the distance from the axial center of the mandrel to the outer surface of the optical laminate, and R1 is the distance from the axial center of the mandrel to a virtual line indicating a position equivalent to 1 / 2 of the total thickness of the optical laminate.) 10. The optical laminate according to claim 9, wherein, when the optical laminate is folded 180° so that the surface on which the antifouling layer is formed is on the inside, a compression ratio C (%) of the optical functional layer calculated by the following formula (2) using a mandrel of the smallest diameter at which no cracks occur satisfies 4.5≦C: C (%)={1-(R3 / R1)}×100...(2) (where R3 is the distance from the axial center of the mandrel to the surface of the optical laminate on the antifouling layer side, and R1 is the distance from the axial center of the mandrel to a virtual line indicating a position equivalent to 1 / 2 of the total thickness of the optical laminate.) 11. An article comprising the optical laminate according to any one of claims 1 to 10.

Citation Information

Patent Citations

  • Antireflection film

    JP2019164255A

  • Photocurable hard coat composition for plastic substrates and hard coat film

    JP2019214670A

  • Hard coat resin and hard coat film

    JP2021134303A

  • Optical laminate body, object, and method for manufacturing optical laminate body

    JP2022007992A

Cited By

  • Photosensitive composition, cured product, laminated film, and article

    WO2026163542A1