Lithium secondary battery having long lifespan
The lithium-sulfur battery design with a sulfur-carbon composite and nitrogen compound in the electrolyte solution addresses the shuttle phenomenon, achieving long lifespan and high energy density by limiting sulfur content, resulting in improved capacity retention and energy density.
Patent Information
- Application Number
- PCT/KR2023/015468
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-10-06
- Filing Date
- 2023-10-06
- Publication Date
- 2024-11-07
AI Technical Summary
Lithium-sulfur batteries face limitations in lifespan due to the shuttle phenomenon, where sulfur polysulfides are dissolved in the electrolyte, leading to passivation of the anode and irreversible capacity loss, which affects their long-term performance and energy density.
A lithium-sulfur battery design incorporating a sulfur-carbon composite positive electrode, a lithium metal layer with a solid electrolyte membrane, and an electrolyte solution containing a nitrogen compound like lithium nitrate, which limits the sulfur content in the cathode to 3% or less, enhancing the battery's lifespan and energy density.
The battery achieves a lifespan of 190 cycles or more with excellent capacity retention, maintaining over 80% of its initial capacity and achieving an energy density of 300 Wh/kg or more, effectively addressing the shuttle phenomenon and improving long-term performance.
Smart Images

Figure 000001 
Figure 000002 
Figure 000003
Abstract
Description
Long-life lithium secondary batteries
[0001] The present invention relates to a lithium secondary battery, and more particularly to a lithium-sulfur battery having a long lifespan.
[0002] This application claims priority to Korean Patent Application No. 10-2023-0058000, filed May 3, 2023, and Korean Patent Application No. 10-2023-0133560, filed October 6, 2023, both of which are incorporated herein by reference.
[0003] As the scope of application of lithium secondary batteries expands beyond portable electronic devices to include electric vehicles (EVs) and electric storage systems (ESS), the demand for lithium secondary batteries with high capacity, high energy density, and long lifespan is increasing.
[0004] Among various lithium secondary batteries, the lithium-sulfur battery is a battery system that uses a sulfur-based material containing a sulfur-sulfur bond as a positive electrode active material, and lithium metal, a carbon-based material in which lithium ions can be inserted / deinserted, or silicon or tin that forms an alloy with lithium as a negative electrode active material.
[0005] Sulfur, the main material of the cathode active material in lithium-sulfur batteries, has the advantages of being a low atomic weight, abundant in resources, easy to supply, inexpensive, non-toxic, and environmentally friendly material.
[0006] In addition, lithium-sulfur batteries have a conversion reaction between lithium ions and sulfur (S8+16Li) at the cathode. + +16e - -> The theoretical specific capacity from 8Li2S reaches 1,675 mAh / g, and when lithium metal is used as the negative electrode, it shows a theoretical energy density of 2,600 Wh / kg. This is a very high figure compared to the theoretical energy density of other battery systems currently being studied (Ni-MH battery: 450 Wh / kg, Li-FeS battery: 480 Wh / kg, Li-MnO2 battery: 1,000 Wh / kg, Na-S battery: 800 Wh / kg) and lithium ion batteries (250 Wh / kg), and therefore, it is attracting attention as a high-capacity, eco-friendly, and low-cost lithium secondary battery among the secondary batteries being developed so far.
[0007] When a lithium-sulfur battery is discharged, sulfur accepts electrons at the positive electrode and a reduction reaction occurs, and lithium polysulfide (Li2S) is formed at the positive electrode. x , x=1~8) are generated, some of which are easily dissolved in the electrolyte and completely reduced to precipitate in the form of a solid lithium sulfide (Li2S) on the negative electrode, or lithium polysulfide reacts with the lithium metal of the negative electrode to contaminate the negative electrode surface, causing sulfur (S) to be passivated on the negative electrode, resulting in irreversible loss of active material, which limits the implementation of long-life characteristics due to the shuttle phenomenon.
[0008] Therefore, there is a need to develop a lithium-sulfur battery that suppresses the passivation phenomenon of the negative electrode of a lithium-sulfur battery due to repeated charge and discharge and has long-life characteristics.
[0009] The present invention aims to solve the above-described problems and provide a lithium-sulfur battery having long-life characteristics.
[0010] In addition, the present invention seeks to provide a lithium-sulfur battery with high energy density.
[0011] To achieve the above purpose,
[0012] According to one aspect of the present invention, lithium-sulfur batteries of the following embodiments are provided.
[0013] A lithium-sulfur battery according to the first embodiment,
[0014] A lithium-sulfur battery comprising a positive electrode comprising a sulfur-carbon complex, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte,
[0015] The above negative electrode includes a lithium metal layer and a solid electrolyte membrane (SEI) formed on at least one surface of the lithium metal layer,
[0016] At SOC 100, the weight of elemental sulfur (S) present in the cathode is set to be 3 wt% or less based on the total weight of the cathode.
[0017] According to the second embodiment, in the first embodiment,
[0018] The above SOC 100 may have a potential of 2.4 V to 2.7 V.
[0019] According to the third embodiment, in the first embodiment or the second embodiment,
[0020] The weight of the sulfur element (S) in the cathode may be 3 wt% or less based on the combined weight of the sulfur element (S) and lithium element (Li) in the cathode.
[0021] According to the fourth embodiment, in any one of the first to third embodiments,
[0022] The weight of the sulfur element (S) in the cathode may be 2 wt% or less based on the combined weight of the sulfur element (S) and lithium element (Li) in the cathode.
[0023] According to the fifth embodiment, in any one of the first to fourth embodiments,
[0024] The weight of the sulfur element (S) in the cathode may be 1 wt% or less based on the total weight of the sulfur element (S) and lithium element (Li) in the cathode.
[0025] According to the sixth embodiment, in any one of the first to fifth embodiments,
[0026] The thickness of the above cathode may be 120 ㎛ or less.
[0027] According to the seventh embodiment, in any one of the first to sixth embodiments,
[0028] The thickness of the above cathode may be 70 ㎛ or less.
[0029] According to the eighth embodiment, in any one of the first to seventh embodiments,
[0030] The above sulfur-carbon complex may have a sulfur / carbon weight ratio (S / C weight ratio) of 2.5 g / g or less.
[0031] According to the ninth embodiment, in any one of the first to eighth embodiments,
[0032] The positive electrode comprises a current collector and a positive electrode active material layer including the sulfur-carbon complex,
[0033] The weight of the sulfur-carbon complex may be 90 wt% or more based on the total weight of the positive electrode active material layer.
[0034] According to the tenth embodiment, in any one of the first to ninth embodiments,
[0035] The weight ratio of sulfur in the electrolyte and the sulfur-carbon complex (El / S weight ratio) may be 3.5 g / g or less.
[0036] According to the eleventh embodiment, in any one of the first to tenth embodiments,
[0037] The above electrolyte may include a non-aqueous solvent, a lithium salt, and an additive.
[0038] According to the 12th embodiment, in any one of the 1st to 11th embodiments,
[0039] The above additive may include a nitrogen compound.
[0040] According to the 13th embodiment, in any one of the first to twelfth embodiments,
[0041] The above additive may include lithium nitrate (LiNO3).
[0042] According to the 14th embodiment, in any one of the first to 13th embodiments,
[0043] The above additive may include a nitrogen compound.
[0044] According to the 15th embodiment, in any one of the 1st to 14th embodiments,
[0045] The content of the above additive may be 1 wt% to 5 wt% based on the total weight of the electrolyte.
[0046] According to the 16th embodiment, in any one of the first to fifteenth embodiments,
[0047] The lithium-sulfur battery may have a lifespan of 190 cycles or more when repeating charge and discharge cycles at a rate of 0.3 to 0.5 C in a range of 1.8 V to 2.5 V at room temperature.
[0048] According to the 17th embodiment, in any one of the first to sixteenth embodiments,
[0049] The above room temperature may be a temperature of 23°C to 25°C.
[0050] According to the 18th embodiment, in any one of the first to seventeenth embodiments,
[0051] The energy density of the above lithium-sulfur battery may be 300 Wh / kg or more.
[0052]
[0053] According to another aspect of the present invention, a method for evaluating the life of a lithium-sulfur battery of the following embodiments is provided.
[0054] A method for evaluating the life of a lithium-sulfur battery according to the 19th embodiment,
[0055] Comprising a positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte comprising a sulfur-carbon complex,
[0056] The above negative electrode is a life evaluation method of a lithium-sulfur battery including a lithium metal layer and a solid electrolyte membrane (SEI) formed on at least one surface of the lithium metal layer,
[0057] A step of determining that the battery is a long-life lithium-sulfur battery is included when the weight of sulfur element (S) present in the negative electrode at SOC 100 is 3 wt% or less based on the total weight of the negative electrode.
[0058] According to the 20th embodiment, in the 19th embodiment,
[0059] The above long-life lithium-sulfur battery may have a lifespan of 190 cycles or more when repeating charge and discharge cycles at a rate of 0.3 to 0.5 C in the range of 1.8 V to 2.5 V at room temperature.
[0060] According to one aspect, the lithium-sulfur battery of the present invention can exhibit excellent capacity retention as charge and discharge characteristics are repeated.
[0061] For example, the lithium-sulfur battery of the present invention can exhibit an effect of maintaining 80% or more of the initial capacity even after 190 or more charge / discharge cycles.
[0062] According to one aspect, the lithium-sulfur battery of the present invention has the advantage of having a high energy density. In particular, the lithium-sulfur battery of the present invention can have an energy density of 300 Wh / kg or more.
[0063] According to one aspect, the lithium-sulfur battery of the present invention can have a high energy density and a long lifespan.
[0064] Hereinafter, the present invention will be described in more detail.
[0065] Throughout this specification, whenever a part is said to "include," "comprise," "have," or "have" a component, this does not mean that it excludes other components, but rather that it may include other components, unless otherwise stated.
[0066] In addition, the terms "about", "substantially", etc. used throughout this specification are used in the sense of numerical values or near numerical values when manufacturing and material tolerances inherent to the meanings stated are presented, and are used to prevent unscrupulous infringers from unfairly exploiting disclosures that mention exact or absolute values to aid understanding of this specification.
[0067] Throughout this specification, references to 'A and / or B' mean 'A or B or both.'
[0068] The term "composite" used in this specification refers to a material in which two or more materials are combined to form physically and chemically different phases and exhibit more effective functions.
[0069] The term "(poly)sulfide" as used herein means "(poly)sulfide ion (S x 2- , 1≤ x ≤8)" and "lithium (poly)sulfide (Li2S x or Li2S x- , 1≤ x ≤8)" is a concept that includes all of them.
[0070] In this specification, the term "polysulfide" means "polysulfide ion (S x 2- , 1< x ≤8)" and "lithium polysulfide (Li2S x or Li2S x - , 1< x ≤8)" is a concept that includes all of them.
[0071] The unit used in this specification is "mAh / g s " is intended to indicate capacity per weight of sulfur (S) unless otherwise specified, and may be used interchangeably with other expressions such as mAh / g(s), mAh / gs, etc.
[0072] The unit "mg" used in this specification s / cm 2 " is intended to represent the weight of sulfur (S) per unit area, unless otherwise stated, mg(s) / cm 2 or as loading capacity mAh / g s It can be used interchangeably with other expressions such as etc.
[0073] Lithium-sulfur batteries have a problem in that lithium (poly)sulfide, which is formed by the reduction reaction of sulfur (S8) at the positive electrode during charging and discharging, is eluted from the positive electrode into the electrolyte, and as a result, the capacity of the battery does not represent the theoretical capacity.
[0074] According to one aspect of the present invention, a lithium-sulfur battery having a long life, specifically, excellent capacity retention rate according to repeated charge and discharge cycles, is provided.
[0075]
[0076] A lithium-sulfur battery according to one aspect of the present invention comprises a positive electrode comprising a sulfur-carbon composite, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte.
[0077] In one embodiment of the present invention, the lithium-sulfur battery specifically includes an electrode assembly including the positive electrode, the negative electrode, and the separator, and a case that accommodates the electrode assembly and an electrolyte.
[0078] At this time, the negative electrode includes a lithium metal layer and a solid electrolyte membrane (SEI) formed on at least one surface of the lithium metal layer, and the weight of sulfur element (S) present in the negative electrode at SOC 100 is 3 wt% or less based on the total weight of the negative electrode.
[0079] As described above, lithium-sulfur batteries contain inorganic sulfur (S8) as a positive electrode active material. Within the lithium-sulfur battery, lithium (poly)sulfide is formed through a reduction reaction at the positive electrode during discharge. The formed lithium (poly)sulfide is dissolved by the electrolyte and eluted from the positive electrode into the electrolyte phase, and the eluted lithium (poly)sulfide reacts with the lithium metal of the negative electrode, so that elemental sulfur (S) immobilized by the precipitated lithium sulfide, etc., exists on the surface of the negative electrode. Consequently, this may result in damage to the negative electrode, which may lead to a reduction in the lifespan of the lithium-sulfur battery.
[0080] With reference to this mechanism, in the present specification, a substance containing elemental sulfur (S) derived from the positive electrode active material of the lithium-sulfur battery is collectively referred to as a "sulfur-based compound." The sulfur-based compound may include, for example, all sulfur-containing compounds that can be formed through a reduction reaction of inorganic sulfur (S8) or an oxidation reaction of lithium sulfide (Li2S), and more specifically, inorganic sulfur (S8), lithium sulfide (Li2S), lithium polysulfide (Li2Sx, 1 < x ≤ 8), disulfide compounds, and carbon-sulfur polymers ((C2S y ) n , y = 2.5 to 50, n≥2) or may include two or more of these.
[0081] Specifically, the sulfur compound may be inorganic sulfur (S8), lithium sulfide (Li2S), lithium polysulfide (Li2Sx, 1 < x ≤ 8), or a mixture of two or more thereof.
[0082] In this specification, lithium (poly)sulfide can also be expressed by the chemical formula Li2Sx (1 ≤ x ≤ 8), and in this case, the lithium (poly)sulfide is used as a term including lithium sulfide (Li2S).
[0083] The inventors of the present invention have discovered that when the lifespan of a lithium-sulfur battery is reduced by repeated charge and discharge cycles of the lithium-sulfur battery, when the content of sulfur (S) formed on the negative electrode is controlled to a certain level or lower, the battery can have a capacity of 80% or more of the initial capacity even after repeated charge and discharge cycles of 190 or more, or further, 195 or more, thereby completing the present invention.
[0084] According to one embodiment of the present invention, in order to prevent degradation of the lithium-sulfur battery, the lithium-sulfur battery may include a nitrogen compound, for example, lithium nitrate (LiNO3), as an additive in the electrolyte.
[0085] As described later, if the content of the additive in the electrolyte is too high, the additive may not dissolve in the non-aqueous solvent but rather precipitate, thereby accelerating the deterioration of the lithium-sulfur battery. Therefore, considering the solubility of the additive in the non-aqueous solvent, the additive may be included in an amount of 5 wt% or less, for example, 1 wt% to 5 wt%, based on the total weight of the non-aqueous solvent, but the present invention is not limited thereto. The composition of the additive in the electrolyte will be described later.
[0086] According to one aspect of the present invention, a new range of content of elemental sulfur (S) present in a cathode at a buffer state, i.e., a state of charge (SOC) of 100, is proposed.
[0087] Specifically, according to one aspect of the present invention, a lithium-sulfur battery is provided in which the weight of elemental sulfur (S) present in the negative electrode at an SOC of 100 is 3 wt% or less based on the total weight of the negative electrode.
[0088] The above negative electrode includes a lithium metal layer and a solid electrolyte membrane (SEI) formed on at least one surface of the lithium metal layer, and in order to implement long-life characteristics of the lithium-sulfur battery, the content of elemental sulfur (S) is limited to 3 wt% or less based on the combined weight of the lithium metal layer and the solid electrolyte membrane.
[0089] In one embodiment of the present invention, the weight of elemental sulfur (S) in the negative electrode may be, for example, 0 wt% to 3 wt%, 0.1 wt% to 3 wt%, 0.1 wt% to 3.0 wt%, 0.1 wt% to 2.5 wt%, 0.1 wt% to 2 wt%, 0.1 wt% to 1 wt%, or 0.1 wt% to 0.5 wt%, based on the combined weight of the lithium metal layer and the solid electrolyte membrane.
[0090] In one embodiment of the present invention, the lithium metal layer is a lithium foil made of lithium metal, which is an anode active material of a lithium-sulfur battery, or a lithium alloy foil made of a material capable of forming an alloy with lithium metal, and may have a thickness of, for example, 140 μm or less.
[0091] In one embodiment of the present invention, the thickness of the lithium metal layer may be 140 μm or less, specifically 120 μm or less, 100 μm or less, and more specifically 80 μm or less or 70 μm or less. For example, the thickness of the lithium metal layer may be 20 μm to 140 μm, 20 μm to 120 μm, 20 μm to 100 μm, specifically 30 μm to 80 μm, 40 μm to 70 μm, 50 μm to 70 μm, 50 μm to 65 μm, 55 μm to 65 μm, or 55 μm to 60 μm. In one embodiment of the present invention, when the thickness of the lithium metal layer is in the above-described range, there may be an advantage of exhibiting advantageous effects in terms of the weight and energy density of the battery.
[0092] In this specification, the thickness of the lithium metal layer may be measured using a known means for measuring the thickness of each component of the battery, and may be measured using a thickness measuring device from Mitutoyo, for example, but is not limited thereto. In one embodiment of the present invention, the thickness of the negative electrode may be measured according to ASTM D374.
[0093] In one embodiment of the present invention, the solid electrolyte interphase (SEI) is a thin passive film formed on the surface of the lithium metal layer during charging during the activation process of a lithium-sulfur battery, and can perform functions such as protecting the lithium metal and suppressing decomposition of the electrolyte, but the present invention is not limited thereto.
[0094] In one embodiment of the present invention, the total thickness of the negative electrode including the lithium metal layer and the solid electrolyte membrane may be 150 μm or less, specifically 120 μm or less, 100 μm or less, and more specifically 70 μm or less. For example, the total thickness of the negative electrode may be 40 μm to 120 μm, for example 40 μm to 70 μm or 55 μm to 65 μm.
[0095] In one embodiment of the present invention, the lithium-sulfur battery exhibits a beneficial effect in implementing long-life characteristics when the content of elemental sulfur (S) in the negative electrode is 3 wt% or less in a charged state, i.e., an SOC of 100. Specifically, the negative electrode may have a content of elemental sulfur (S) of 3 wt% or less based on the sum of the weights of elemental sulfur (S) and elemental lithium (Li) in the negative electrode. For example, the content of elemental sulfur (S) in the negative electrode may be 3 wt% or less, 2 wt% or less, 1 wt% or less, 0.5 wt% or less, or 0 wt% or less based on the sum of the weights of elemental sulfur (S) and elemental lithium (Li) in the negative electrode.
[0096] More specifically, the negative electrode may include elemental sulfur (S) in an amount of 0 wt% to 3 wt%, 0.1 wt% to 3 wt%, 0.1 wt% to 2.5 wt%, 0.1 wt% to 2 wt%, 0.1 wt% to 1 wt%, or 0.1 wt% to 0.5 wt%, based on the sum of the weight of sulfur (S) and lithium (Li) in the negative electrode in a SOC 100 state, i.e., a buffered state.
[0097] At this time, the above 0 wt% is intended to include not only cases where sulfur element (S) is not included at all, but also cases where it is measured as 0 wt% due to limitations in the measurement significant figures or measurement errors even when a trace amount is included. Accordingly, the above 0 wt% may also mean 0.1 wt% based on the total weight of the cathode.
[0098] In one embodiment of the present invention, the weight of lithium (Li) in the negative electrode may be, for example, 96 wt% or more, 99 wt% or more, 96 wt% to 100 wt%, 96 wt% to 99.9 wt%, or 99 wt% to 99.9 wt%, based on the sum of the weight of elemental sulfur (S) and lithium (Li) in the negative electrode. When the content of lithium is within the above-described range based on the sum of the weight of elemental sulfur (S) and lithium (Li) in the negative electrode in the buffered state, i.e., SOC 100, the lithium-sulfur battery may exhibit a beneficial effect on the long-life characteristics, but the present invention is not limited thereto.
[0099] In one embodiment of the present invention, the composition of the solid electrolyte membrane may vary depending on the composition of lithium salt and additives used in the electrolyte of a lithium-sulfur battery, and is not limited to a specific composition.
[0100] In one embodiment of the present invention, the solid electrolyte membrane may contain, for example, a Li-F functional group.
[0101] In one embodiment of the present invention, the elements contained in the negative electrode including the lithium metal layer and the solid electrolyte membrane in the lithium-sulfur battery at an SOC of 100 may include elemental sulfur (S), elemental lithium (Li), and elemental fluorine (F). Specifically, the elements contained in the negative electrode may include elemental sulfur (S), elemental lithium (Li), and elemental fluorine (F).
[0102] In one embodiment of the present invention, the lithium-sulfur battery may have a content of sulfur element (S) of 3 wt% or less, 2 wt% or less, 1 wt% or less, 0.5 wt% or less, 0.1 wt% or less, or 0 wt%, based on the sum of the weight of sulfur element (S), lithium element (Li), and fluorine element (F) in the negative electrode in a charged state, i.e., an SOC of 100. In this case, the 0 wt% is intended to include not only the case where sulfur element (S) is not included at all as described above, but also the case where it is measured as 0 wt% due to the limit of the measurement significant digit, a measurement error, etc. even if it is included in a trace amount.
[0103] In one embodiment of the present invention, the solid electrolyte membrane may include, for example, a complex formed by a chemical reaction between an electrolyte additive described below and lithium metal. In this case, the electrolyte additive may be, for example, a material containing nitrogen element (N), and thus the solid electrolyte membrane may include nitrogen element (N).
[0104] Accordingly, in one embodiment of the present invention, the lithium-sulfur battery may have a content of sulfur element (S) of 3 wt% or less, 2 wt% or less, 1 wt% or less, 0.5 wt% or less, 0.1 wt% or less, or 0 wt%, based on the sum of the weight of sulfur element (S), lithium element (Li), and nitrogen element (N) in the negative electrode in a charged state, i.e., an SOC of 100. In this case, the 0 wt% is intended to include not only the case where sulfur element (S) is not included at all as described above, but also the case where it is measured as 0 wt% due to the limit of the measurement significant digit, a measurement error, etc. even if it is included in a trace amount.
[0105] In another embodiment of the present invention, the lithium-sulfur battery may have a content of sulfur element (S) of 3 wt% or less, 2 wt% or less, 1 wt% or less, 0.5 wt% or less, 0.1 wt% or less, or 0 wt% based on the total weight of sulfur element (S), lithium element (Li), fluorine element (F), and nitrogen element (N) in the negative electrode in a charged state, i.e., an SOC of 100.
[0106] Next, a method for measuring the content of sulfur element (S) in the cathode will be described.
[0107] In one embodiment of the present invention, the SOC 100 refers to a fully charged state of the battery. For example, the SOC 100 state may indicate a state in which the battery is charged to a potential of 2.4 V to 2.7 V. Specifically, the SOC 100 may indicate a state in which the battery is charged to a potential of 2.5 V.
[0108] Specifically, the content of elemental sulfur (S) in the negative electrode at the SOC 100 can be measured by disassembling the lithium-sulfur battery in a fully charged state, for example, 2.4 V to 2.7 V, specifically, a state charged to 2.5 V, and then washing the electrolyte remaining on the negative electrode, and then analyzing the components.
[0109] In one embodiment of the present invention, the component analysis may be performed using, for example, IC (Ion chromatography) analysis, ICP-OES (Inductively Coupled Plasma Optical Emission Spectrometer) analysis, EA (Elemental Analyzer) analysis, ONH analysis, etc., but the component analysis method is not limited thereto. Accordingly, the content of elemental sulfur (S) in the negative electrode based on the total weight of the negative electrode at an SOC of 100 or the content of elemental sulfur (S) in the negative electrode based on the sum of the weights of elemental sulfur (S) and elemental lithium (Li) in the negative electrode at an SOC of 100 may be measured by the above-described component analysis, and may be measured, for example, by an ICP-OES measurement method.
[0110] In one embodiment of the present invention, before measuring the content of the elemental sulfur (S), the lithium-sulfur battery may be activated through at least one cycle, for example, 5 cycles or more, or 10 cycles or more, of charge and discharge at 0.5 C and 0.3 C in a range of 1.8 V to 2.5 V at room temperature, for example, 23° C. to 25° C., with 1 cycle being defined as discharge and charge.
[0111] As described above, in a conventional lithium-sulfur battery, sulfur element (S) is formed on the negative electrode by a sulfur compound derived from the positive electrode during discharge, which may cause deterioration of the battery as the battery is repeatedly charged and discharged. However, according to one aspect of the present invention, by limiting the upper limit of the content of sulfur element (S) in the negative electrode to 3 wt% or less, specifically 2 wt% or less, 1 wt% or less, or 0.5 wt% or less in a buffered state, i.e., SOC 100, it is possible to provide a lithium-sulfur battery having a long lifespan.
[0112]
[0113] Next, each component other than the negative electrode of the lithium-sulfur battery will be described in detail.
[0114] anode
[0115] In one embodiment of the present invention, the positive electrode may include a positive electrode current collector and a positive electrode active material layer applied to one or both surfaces of the positive electrode current collector.
[0116] The above-mentioned positive electrode current collector supports the positive electrode active material and is not particularly limited as long as it has high conductivity without causing chemical changes in the battery. For example, copper, stainless steel, aluminum, nickel, titanium, palladium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, silver, etc., aluminum-cadmium alloy, etc. can be used.
[0117] The above positive electrode current collector can form fine irregularities on its surface to strengthen the bonding strength with the positive electrode active material, and can be used in various forms such as a film, sheet, foil, mesh, net, porous body, foam, and non-woven fabric.
[0118] The above positive electrode active material layer includes a positive electrode active material and may further include a conductive material, a binder, and additives.
[0119] In one embodiment of the present invention, the positive electrode active material comprises a sulfur-carbon complex.
[0120] In one embodiment of the present invention, the sulfur-carbon composite may include a porous carbon material; and a sulfur-based compound supported on at least one of the inside of the pores of the porous carbon material and the outer surface of the porous carbon material. In the case of sulfur acting as the positive electrode active material, since it does not have electrical conductivity alone, it is used in a composite with a conductive material such as a carbon material, and a porous carbon material may be used to support sulfur. In addition, the sulfur-based compound is added as the positive electrode active material, and for example, inorganic sulfur (S8), lithium sulfide (Li2S), lithium polysulfide (Li2Sx, 1 < x ≤ 8), a disulfide compound, a carbon-sulfur polymer ((C2S)y ) n , y = 2.5 to 50, n≥2), or two or more of these. Preferably, the sulfur compound may be inorganic sulfur (S8).
[0121] In one embodiment of the present invention, the porous carbon material is used to support a sulfur-based compound as a positive electrode active material, and to provide a framework in which the sulfur-based compound can be uniformly and stably fixed, while improving the conductivity of the positive electrode. Any porous carbon material can be used without particular limitation in its type.
[0122] The above porous carbon material can generally be manufactured by carbonizing precursors of various carbon materials. The porous carbon material includes pores that are not regular therein, and the average diameter of the pores ranges from 1 to 200 nm, and the porosity can range from 10 to 90 volume% of the total volume of the porous carbon material. If the average diameter of the pores is less than the above range, the pore size is only at the molecular level, making sulfur impregnation impossible. Conversely, if it exceeds the above range, the mechanical strength of the porous carbon material is weakened, making it undesirable for application to the electrode manufacturing process.
[0123] In one embodiment of the present invention, the 'average pore diameter' can be measured according to a method known in the art for measuring the pore diameter of a porous material, and the measuring method is not particularly limited. For example, the pore diameter can be measured according to a scanning electron microscope (SEM), a field emission electron microscope (laser diffraction method), a laser diffraction method, or the BET (Brunauer-Emmett-Teller) method. The measurement using the laser diffraction method can be, for example, using a commercially available laser diffraction particle size measuring device (for example, Microtrac MT 3000). In addition, the measurement according to the BET method can be, for example, using an analyzer of the BELSORP series of BEL Japan, but is not limited thereto.
[0124] In one embodiment of the present invention, the 'porosity' refers to the ratio of the volume occupied by pores to the total volume of a structure, and uses % as its unit, and can be used interchangeably with terms such as porosity and porosity. In the present invention, the measurement of the porosity is not particularly limited, and according to one embodiment of the present invention, for example, it can be measured according to the BET method using nitrogen gas or the mercury penetration method (Hg porosimeter) and ASTM D2873.
[0125] The shape of the above porous carbon material may be spherical, rod-shaped, needle-shaped, plate-shaped, tubular or bulk-shaped, and can be used without limitation as long as it is a shape commonly used in lithium-sulfur batteries.
[0126] The porous carbon material may be any material commonly used in the art that has a porous structure or a high specific surface area. For example, the porous carbon material may be at least one selected from the group consisting of graphite; graphene; carbon black such as Denka black, acetylene black, Ketjen black, channel black, furnace black, lamp black, and summer black; carbon nanotubes (CNTs) such as single-walled carbon nanotubes (SWCNTs) and multi-walled carbon nanotubes (MWCNTs); carbon fibers such as graphite nanofibers (GNFs), carbon nanofibers (CNFs), and activated carbon fibers (ACFs); and graphite and activated carbon such as natural graphite, artificial graphite, and expanded graphite, but is not limited thereto. Preferably, the porous carbon material may be a carbon nanotube.
[0127] In one embodiment of the present invention, the porous carbon material may include, for example, carbon nanotubes (CNTs).
[0128] In one embodiment of the present invention, the sulfur-carbon complex may have a sulfur / carbon weight ratio (S / C weight ratio) of, for example, 5 g / g or less, for example, 4 g / g or less, and more specifically, 2.5 g / g or less, for example, 2.3 g / g or less. For example, the sulfur-carbon complex may have a sulfur / carbon weight ratio of 2.3 g / g. When the S / C ratio of the sulfur-carbon complex is within the above-described range, it may be preferable in terms of securing the electron transfer ability (conductivity) and electrochemical specific surface area of the sulfur-carbon complex, and for example, it may be preferable in suppressing the elution of sulfur from the anode because the available surface of the sulfur-carbon complex increases, but the present invention is not limited thereto.
[0129] In one embodiment of the present invention, the S / C ratio can be calculated from the weight (g) of sulfur and the weight (g) of carbon present in the sulfur-carbon complex. Alternatively, it can be calculated from the weight (wt%) of sulfur and the weight (wt%) of carbon based on the total weight of the sulfur-carbon complex. As such, the S / C ratio can be a unitless value.
[0130] In one embodiment of the present invention, the S / C weight ratio may have a value of, for example, 0.5 to 5.0, 0.5 to 4.0, 1.0 to 3.0, 1.5 to 2.5, 2.0 to 2.45, 2.25 to 2.35, or 2.3 to 3. For example, the S / C ratio may be calculated from the weight ratio of the inorganic sulfur (S8) to the weight ratio of the porous carbon material. For example, the S / C ratio may be calculated from the weight ratio of S8 / CNT.
[0131] The method for manufacturing the above sulfur-carbon composite is not particularly limited in the present invention, and any method commonly used in the art may be used. For example, a method may be used in which the sulfur and porous carbon material are simply mixed and then heat-treated to form a composite.
[0132] In addition to the composition described above, the positive electrode active material may further include one or more selected from among a transition metal element, a group ⅢA element, a group ⅣA element, a sulfur compound of these elements, and an alloy of these elements and sulfur.
[0133] The above transition metal elements include Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Os, Ir, Pt, Au or Hg, etc., the above group 13 elements include Al, Ga, In, Ti, etc., and the above group 14 elements may include Ge, Sn, Pb, etc.
[0134] In one embodiment of the present invention, the sulfur-carbon composite may be at least 50 wt% based on the total weight of the positive electrode. Specifically, the sulfur-carbon composite may be at least 80 wt%, at least 90 wt%, or at least 95 wt% based on the total weight of the positive electrode active material layer. Specifically, the sulfur-carbon composite may be included in an amount of 80 wt% to 100 wt%, more specifically 85 wt% to 99 wt%, 90 wt% to 99 wt%, 95 wt% to 98 wt%, or 95 wt% to 97 wt%, or 96 wt% based on the total weight of the positive electrode active material layer. In one embodiment of the present invention, the above-described content of the sulfur-carbon composite may refer to the content at a stage in which the lithium-sulfur battery is manufactured. In addition, in another embodiment of the present invention, the content of the sulfur-carbon complex may be measured by analyzing the components of the positive electrode after the lithium-sulfur battery is decomposed after being charged to an SOC of 100. If the content of the sulfur-carbon complex is less than the above range, the relative content of auxiliary materials such as conductive materials and binders increases and the content of the sulfur-carbon complex decreases, making it difficult to implement a high-capacity, high-energy-density battery. On the other hand, if it exceeds the above range, the content of the conductive material or binder described below is relatively insufficient, which causes a problem in that the physical properties of the electrode deteriorate.
[0135] The above conductive material is a material that electrically connects the electrolyte and the positive electrode active material and serves as a path for electrons to move from the current collector to the positive electrode active material. Any conductive material that is physically distinct from the carbon contained in the sulfur-carbon complex and is a component of the electrode can be used without limitation.
[0136] In one embodiment of the present invention, the conductive material may be, for example, carbon black such as Super-P, Denka black, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, carbon black; carbon derivatives such as carbon nanotubes or fullerene; conductive fibers such as carbon fibers or metal fibers; metal powders such as fluorocarbon, aluminum, and nickel powder; or conductive polymers such as polyaniline, polythiophene, polyacetylene, and polypyrrole, which may be used alone or in combination.
[0137] In one embodiment of the present invention, the content of the conductive material may be 0 to 40 wt%, 1 to 40 wt%, 15 to 40 wt%, 20 to 40 wt%, 25 to 35 wt%, 0 to 10 wt%, for example, 1 to 10 wt%, based on the total weight of the positive electrode active material. If the content of the conductive material is less than the above range, electron transfer between the positive electrode active material and the current collector is not easy, so the voltage and capacity decrease. On the contrary, if it exceeds the above range, the proportion of the positive electrode active material relatively decreases, so that the total energy (charge) of the battery may decrease. Therefore, it is preferable to determine an appropriate content within the above-mentioned range.
[0138] In one embodiment of the present invention, the binder maintains the positive electrode active material on the positive electrode current collector and organically connects the positive electrode active materials to further increase the bonding strength between them, and any binder known in the art can be used.
[0139] For example, the binder may be a fluororesin binder including polyvinylidene fluoride (PVdF), a polyvinylidene fluoride polymer including at least one vinylidene fluoride as a repeating unit, polytetrafluoroethylene (PTFE), or a mixture of two or more thereof; a rubber binder including styrene butadiene rubber (SBR), acrylonitrile-butidiene rubber, or styrene-isoprene rubber; an acrylic binder; a cellulose binder including carboxyl methyl cellulose (CMC), starch, hydroxy propyl cellulose, or regenerated cellulose; a polyalcohol binder; a polyolefin binder including polyethylene and polypropylene; a polyimide binder; a polyester binder; a silane binder; a polyacrylic acid binder; And a polyacrylonitrile-based binder; a mixture or copolymer of one or more selected from the group consisting of may be used. In one embodiment of the present invention, the binder may include polyacrylate (PAA).
[0140] In one embodiment of the present invention, the content of the binder may be 1 to 10 wt% based on the total weight of the positive electrode active material layer. If the content of the binder is less than the above range, the physical properties of the positive electrode may deteriorate, causing the positive electrode active material and conductive material to fall off. If the content of the binder is more than the above range, the ratio of the positive electrode active material and conductive material in the positive electrode may relatively decrease, resulting in a decrease in battery capacity. Therefore, it is preferable to determine an appropriate content within the above-described range.
[0141] In the present invention, the method for manufacturing the positive electrode for the lithium secondary battery is not particularly limited, and various methods known to those skilled in the art or modified methods thereof can be used.
[0142] For example, the positive electrode for the lithium secondary battery may be manufactured by forming the positive electrode active material layer by preparing a positive electrode slurry composition including the composition described above and then applying the same to at least one surface of the positive electrode current collector.
[0143] The above positive electrode slurry composition includes the positive electrode active material described above, and may further include a binder, a conductive material, and a solvent.
[0144] The above solvent is one that can uniformly disperse the positive electrode active material. Water is most preferably an aqueous solvent, and the water may be distilled or deionized water. However, this is not necessarily limited to this, and if necessary, a lower alcohol that is easily mixed with water may be used. Examples of the lower alcohol include methanol, ethanol, propanol, isopropanol, and butanol, and preferably, these can be mixed with water and used.
[0145] The content of the above solvent may be contained at a level that has a concentration that can facilitate coating, and the specific content varies depending on the application method and device.
[0146] The above-mentioned positive electrode slurry composition may additionally contain, as necessary, substances commonly used in the relevant technical field for purposes such as improving its function. Examples thereof include viscosity modifiers, fluidizing agents, and fillers.
[0147] The method for applying the positive electrode slurry composition is not particularly limited in the present invention, and examples thereof include methods such as doctor blade, die casting, comma coating, and screen printing. In addition, the positive electrode slurry may be applied onto the positive electrode current collector by molding it on a separate substrate and then pressing or lamination.
[0148] After the above application, a drying process for solvent removal can be performed. The drying process is performed at a temperature and time that can sufficiently remove the solvent, and the conditions may vary depending on the type of solvent and are therefore not particularly limited to the present invention. Examples include drying using warm air, hot air, low-humidity air, vacuum drying, and drying using irradiation with (far) infrared rays and electron beams. The drying speed is usually adjusted to remove the solvent as quickly as possible within a speed range that does not cause cracks in the positive electrode active material layer due to stress concentration or cause the positive electrode active material layer to peel off from the positive electrode current collector.
[0149] Additionally, the density of the positive electrode active material within the positive electrode can be increased by pressing the entire body after drying. Pressing methods include mold pressing and roll pressing.
[0150] The porosity of the positive electrode manufactured by the composition and manufacturing method described above, specifically, the positive electrode active material layer, may be 50 to 80% by volume, specifically, 60 to 75% by volume. If the porosity of the positive electrode is less than 50% by volume, the filling degree of the positive electrode slurry composition including the positive electrode active material, the conductive agent, and the binder becomes excessively high, so that sufficient electrolyte capable of exhibiting ionic and / or electrical conductivity cannot be maintained between the positive electrode active materials, which may result in a deterioration in the output characteristics or cycle characteristics of the battery, and a problem in that the overvoltage and discharge capacity of the battery become severe. On the other hand, if the porosity of the positive electrode exceeds 80% by volume and has excessively high porosity, there is a problem in that the physical and electrical connection with the current collector is lowered, which results in a deterioration in the adhesive strength and a difficulty in the reaction. In addition, the increased porosity may be filled with electrolyte, which may result in a problem in that the energy density of the battery may be lowered, and therefore, the porosity is appropriately controlled within the above range.
[0151] In one embodiment of the present invention, the loading amount of sulfur in the anode is, for example, 2.5 mg(s) / cm 2 Below, for example, 0 to 2.5 mg(s) / cm 2 , 0.1 to 2.4 mg(s) / cm 2 or 1.7 to 2.1 mg(s) / cm 2It can be. The loading amount of the sulfur may be a value calculated from the total weight of sulfur (S) included as a positive electrode active material in the positive electrode. At this time, the weight of sulfur in the positive electrode may be measured from the positive electrode active material introduced during the manufacturing step, and may be measured through thermogravimetric analysis (TGA) of the positive electrode after manufacturing. Meanwhile, when disassembling a manufactured lithium-sulfur battery, a charged lithium-sulfur battery is disassembled under an inert atmosphere to obtain a positive electrode, and then the positive electrode is washed and dried using an appropriate washing solvent, and the positive electrode active material layer is scraped off. The resultant product may be subjected to thermogravimetric analysis (TGA) to measure the content of sulfur (S) derived from the active material and calculate the calculation, but the measurement method is not limited thereto.
[0152] In another embodiment of the present invention, the loading amount of sulfur in the positive electrode is, for example, 3 mAh / cm 2 Below, specifically 0 mAh / cm 2 3 mAh / cm 2 It can be. For example, the loading amount of sulfur in the anode is 0.1 to 2.9 mAh / cm 2 , 0.5 to 2.8 mAh / cm 2 , 1 to 2.7 mAh / cm 2 , 1.5 to 2.6 mAh / cm 2 or 2.0 to 2.5 mAh / cm 2 It can be. The above sulfur loading amount can be a value calculated from the total weight of sulfur (S) included as a positive electrode active material in the positive electrode and the capacity value of the electrode calculated therefrom.
[0153]
[0154] cathode
[0155] The above negative electrode may include a negative electrode current collector and a negative electrode active material layer formed on at least one surface of the negative electrode current collector. Alternatively, the negative electrode may be a self-standing lithium metal plate or lithium metal foil without including a current collector.
[0156] In one embodiment of the present invention, the negative electrode current collector supports the negative electrode active material, and the same as that described above for the positive electrode current collector can be used.
[0157] The above negative active material is lithium (Li + ) can be reversibly intercalated or deintercalated, a material that can react with lithium ions to form a reversibly lithium-containing compound, or a lithium metal or a lithium alloy.
[0158] The above lithium ion (Li + ) can be reversibly inserted or de-inserted, for example, crystalline carbon, amorphous carbon, or a mixture thereof. The lithium ion (Li + ) can be, for example, tin oxide, titanium nitrate or silicon. The lithium alloy can be, for example, an alloy of lithium (Li) with one or more metals selected from the group consisting of sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), francium (Fr), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), radium (Ra), aluminum (Al) and tin (Sn).
[0159]
[0160] membrane
[0161] The separator separates or insulates the positive and negative electrodes from each other and enables lithium ion transport between the positive and negative electrodes. It may be made of a porous non-conductive or insulating material, and can be used without special restrictions as long as it is commonly used as a separator in a lithium secondary battery. The separator may be an independent member such as a film, or may be a coating layer added to the positive and / or negative electrodes.
[0162] It is preferable that the above separator have low resistance to ion movement of the electrolyte and excellent moisture absorption capacity for the electrolyte.
[0163] In one embodiment of the present invention, the separator may include a porous substrate, and any porous substrate typically used in secondary batteries may be used as the porous substrate, and a porous polymer film may be used alone or in a laminated manner. For example, a nonwoven fabric or a polyolefin porous film made of high-melting-point glass fiber, polyethylene terephthalate fiber, etc. may be used, but is not limited thereto.
[0164] The material of the porous substrate is not particularly limited in the present invention, and any porous substrate commonly used in electrochemical devices can be used. For example, the porous substrate may be a polyolefin such as polyethylene, polypropylene, etc., a polyester such as polyethyleneterephthalate, polybutyleneterephthalate, polyamide, polyacetal, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenyleneoxide, polyphenylenesulfide, polyethylenenaphthalate, polytetrafluoroethylene, polyvinylidene fluoride, polyvinyl chloride, polyacrylonitrile, cellulose, nylon, It may include at least one material selected from the group consisting of poly(p-phenylene benzobisoxazole) and polyarylate.
[0165] In one embodiment of the present invention, the thickness of the porous substrate is not particularly limited, but may be 1 to 100 μm, preferably 5 to 50 μm. The thickness range of the porous substrate is not limited to the above-mentioned range, but if the thickness is excessively thinner than the above-mentioned lower limit, the mechanical properties may deteriorate, and the separator may be easily damaged during battery use.
[0166] In one embodiment of the present invention, the average diameter and porosity of the pores present in the porous substrate are not particularly limited, but may be 0.001 to 50 ㎛ and 10 to 95 volume%, respectively.
[0167] In one embodiment of the present invention, the separator may further include a porous coating layer formed on at least one surface of the porous substrate and including inorganic particles and a binder.
[0168] In one embodiment of the present invention, the inorganic particles and binder included in the porous coating layer may be used without particular limitation as long as they are commonly used in the porous coating layer of a separation membrane, and the manufacturing method thereof is also not particularly limited.
[0169]
[0170] electrolyte
[0171] The above electrolyte comprises a non-aqueous solvent as a medium through which ions involved in the electrochemical reaction of a lithium-sulfur battery can move and a lithium salt as an electrolyte.
[0172] The above electrolyte is not particularly limited as long as it has a composition that can be used in a lithium secondary battery, specifically a lithium-sulfur battery.
[0173] In one embodiment of the present invention, the electrolyte may include a non-aqueous solvent, a lithium salt, and an additive.
[0174] In one embodiment of the present invention, the non-aqueous solvent may be used without particular limitation as long as it is of a type that can be used in a lithium-sulfur battery, and for example, ether solvents, esters, amides, linear carbonates, and cyclic carbonates may be used.
[0175] In one embodiment of the present invention, the ester may be, for example, one selected from the group consisting of methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, γ-valerolactone, γ-caprolactone, σ-valerolactone, and ε-caprolactone, or a mixture of two or more thereof, but is not limited thereto.
[0176] In one embodiment of the present invention, the linear carbonate may be, for example, one selected from the group consisting of dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethylmethyl carbonate, methylpropyl carbonate, and ethylpropyl carbonate, or a mixture of two or more thereof, but is not limited thereto.
[0177] In one embodiment of the present invention, the cyclic carbonate is, for example, one selected from the group consisting of ethylene carbonate, propylene carbonate, 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate, vinylene carbonate, vinylethylene carbonate, and halogenides thereof, or a mixture of two or more thereof. Examples of the halogenides thereof include, but are not limited to, fluoroethylene carbonate.
[0178] In one embodiment of the present invention, the non-aqueous solvent may include an ether solvent.
[0179] In one embodiment of the present invention, the ether solvent may be included in an amount of 60% by volume or more, for example, 60% by volume to 100% by volume, 70% by volume to 100% by volume, 80% by volume to 100% by volume, 85% by volume to 100% by volume, 90% by volume to 100% by volume, 95% by volume to 100% by volume, 98% by volume to 100% by volume, 90% by volume to 98% by volume, or 90% by volume to 95% by volume, based on the total volume of the non-aqueous solvent. When the amount of the ether solvent is in the above-described range based on the total volume of the non-aqueous solvent, an advantageous effect may be exhibited in terms of the solubility of an electrolyte composition such as a lithium salt, but the present invention is not limited thereto.
[0180] In one embodiment of the present invention, the ether solvent may include an acyclic ether, a cyclic ether, or a mixture thereof. The non-aqueous solvent may preferably be composed of an ether solvent in terms of the solubility of the lithium salt and / or additive described below.
[0181] In one embodiment of the present invention, the acyclic ether is selected from the group consisting of, for example, dimethyl ether, diethyl ether, dipropyl ether, dibutyl ether, diisobutyl ether, ethyl methyl ether, ethylpropyl ether, ethyl tertbutyl ether, dimethoxymethane, trimethoxymethane, dimethoxyethane, diethoxyethane, dimethoxypropane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, ethylene glycol divinyl ether, diethylene glycol divinyl ether, triethylene glycol divinyl ether, dipropylene glycol dimethylene ether, butylene glycol ether, diethylene glycol ethylmethyl ether, diethylene glycol isopropylmethyl ether, diethylene glycol butylmethyl ether, diethylene glycol tertbutylethyl ether, and ethylene glycol ethylmethyl ether. It may include one or more kinds. Preferably, it may include one or more kinds selected from the group consisting of dimethyl ether, dimethoxyethane, diethoxyethane, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, and tetraethylene glycol dimethyl ether, and more preferably, it may include dimethoxyethane.
[0182] In one embodiment of the present invention, the cyclic ether is, for example, 2-methylfuran, 1,3-dioxolane, 4,5-dimethyl-dioxolane, 4,5-diethyl-dioxolane, 4-methyl-1,3-dioxolane, 4-ethyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, 2,5-dimethyltetrahydrofuran, 2,5-dimethoxytetrahydrofuran, 2-ethoxytetrahydrofuran, 2-methyl-1,3-dioxolane, 2-vinyl-1,3-dioxolane, 2,2-dimethyl-1,3-dioxolane, 2-methoxy-1,3-dioxolane, 2-ethyl-2-methyl-1,3-dioxolane, tetrahydropyran, 1,4-dioxane, It may include at least one selected from the group consisting of 1,2-dimethoxybenzene, 1,3-dimethoxybenzene, 1,4-dimethoxybenzene, and isosorbide dimethyl ether. Preferably, it may include at least one selected from the group consisting of 2-methylfuran, 1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, and 2,5-dimethyltetrahydrofuran, and more preferably, it may include 2-methylfuran.
[0183] In one embodiment of the present invention, the non-aqueous solvent may include a mixture of an acyclic ether and a cyclic ether.
[0184] In one embodiment of the present invention, the non-aqueous solvent may include dimethoxyethane (DME) and 2-methylfuran (2-MeF).
[0185] In one embodiment of the present invention, the volume ratio of the acyclic ether and the cyclic ether may be 5:95 to 95:5 (v / v), specifically 95:5 to 50:50, more specifically 90:10 to 70:30, 85:15 to 75:25, or 80:20. In the present invention, the volume ratio corresponds to the ratio of "volume % of acyclic ether": "volume % of cyclic ether" in the ether solvent.
[0186] In one embodiment of the present invention, the non-aqueous solvent may not contain a carbonate solvent in terms of the solubility of the electrolyte. Alternatively, the non-aqueous solvent may contain a very small amount of a carbonate solvent such that the carbonate solvent does not affect the solubility of the lithium salt. For example, when the non-aqueous solvent contains the carbonate solvent, the content of the carbonate solvent may be 3 wt% or less, 2 wt% or less, 1 wt% or less, 0.5 wt% or less, or 0 wt% (i.e., not contained at all) based on the total weight of the electrolyte for a lithium secondary battery.
[0187] In one embodiment of the present invention, the lithium salt may be used without particular limitation as long as it can be used as an electrolyte of a lithium secondary battery. The lithium salt may be, for example, LiCl, LiBr, LiI, LiClO4, LiBF4, LiB 10 Cl 10 , LiPF6, LiCF3SO3, LiCF3CO2, LiC4BO8, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, CF3SO3Li, (CF3SO2)2NLi, (C2F5SO2)2NLi, (SO2F)2NLi, (CF3SO2)3CLi, lithium chloroborane, lithium lower aliphatic carboxylate, lithium 4-phenylborate, lithium imide, or two or more thereof.
[0188] In one embodiment of the present invention, the concentration of the lithium salt may be appropriately determined in consideration of ionic conductivity, solubility, etc., and may be, for example, 0.1 to 4 M, preferably 0.25 to 2. M, 0.5 to 2 M, or 0.5 to 1.5 M. When the concentration of the lithium salt is within the above-described range, it is advantageous to secure ionic conductivity suitable for battery operation, or to exhibit an advantageous effect in terms of improving the mobility of lithium ions and suppressing the decomposition reaction of the lithium salt itself by exhibiting an appropriate viscosity of the electrolyte, but the present invention is not limited thereto.
[0189] In one embodiment of the present invention, the additive may include a nitrogen compound in addition to the lithium salt to improve the electrical conductivity of the electrolyte and to improve the lifespan of the lithium-sulfur battery.
[0190] Specifically, the nitrogen compound may, but its efficacy is not limited to, for example, inhibit the reduction reaction of polysulfide occurring during the charge / discharge process of a lithium-sulfur battery, thereby preventing irreversible consumption of polysulfide, thereby improving the performance of a lithium-sulfur battery.
[0191] In one embodiment of the present invention, the additive, for example, a nitrogen compound, may be used without particular limitation as long as it has the effect of stably forming a solid electrolyte membrane (SEI) of the negative electrode and improving charge / discharge efficiency, and may be, for example, a nitric acid compound, a nitrite compound, or a mixture thereof.
[0192] In one embodiment of the present invention, the nitrogen compound is, for example, an inorganic nitric or nitrous compound such as lithium nitrate (LiNO3), potassium nitrate (KNO3), cesium nitrate (CsNO3), barium nitrate (Ba(NO3)2), ammonium nitrate (NH4NO3), lithium nitrite (LiNO2), potassium nitrite (KNO2), cesium nitrite (CsNO2), ammonium nitrite (NH4NO2); an organic nitric or nitrous compound such as methyl nitrate, dialkyl imidazolium nitrate, guanidine nitrate, imidazolium nitrate, pyridinium nitrate, ethyl nitrite, propyl nitrite, butyl nitrite, pentyl nitrite, and octyl nitrite; It may be selected from the group consisting of organic nitro compounds such as nitromethane, nitropropane, nitrobutane, nitrobenzene, dinitrobenzene, nitropyridine, dinitropyridine, nitrotoluene, dinitrotoluene, and combinations thereof, and preferably may include lithium nitrate.
[0193] In one embodiment of the present invention, the electrolyte may include a non-aqueous solvent and two types of lithium salts. In this case, the two types of lithium salts are different from each other, and one type of lithium salt may be a nitrogen-containing lithium salt, and the other type of lithium salt may be a nitrogen compound, such as lithium nitrate (LiNO3). For example, the two types of lithium salts may include LiTFSI as an electrolyte and LiNO3 as an additive.
[0194] In one embodiment of the present invention, the nitrogen compound may be included in an amount of, for example, 1 wt% to 10 wt%, 1 wt% to 8 wt%, 1 wt% to 6 wt%, 1 wt% to 5 wt%, 1.0 wt% to 5.0 wt%, 2.0 wt% to 5.0 wt%, 2.0 wt% to 4.9 wt%, 2.1 wt% to 3.5 wt%, or 3 wt% to 5 wt% based on the total weight of the electrolyte, but is not limited thereto. When the nitrogen compound is included in the above-described amount, it may exhibit a more advantageous effect in terms of improving the electrical conductivity of the electrolyte by the nitrogen compound and suppressing the reduction of polysulfide when used in a lithium-sulfur battery, but the present invention is not limited thereto.
[0195] In one embodiment of the present invention, the concentration of the nitrogen compound in the electrolyte may be, for example, 0.15 to 1.5 M (mol / L), specifically 0.20 to 1.0 M, 0.25 to 0.80 M, or 0.30 to 0.60 M. When the concentration of the nitrogen compound is in the above-described range, the nitrogen compound may exhibit a beneficial effect in improving electrical conductivity in the electrolyte and, when a lithium-sulfur battery is used, suppressing an increase in the amount of sulfur in the negative electrode due to a reduction reaction of (poly)sulfide, thereby improving battery deterioration.
[0196] In another embodiment of the present invention, the ratio of the molar concentration of the lithium salt to the molar concentration of the additive, for example, the nitrogen compound, may be, for example, 0.5 to 6.0 (molar concentration of lithium salt / molar concentration of additive), 0.5 to 5.5 (molar concentration of lithium salt / molar concentration of additive), 0.5 to 5.0, 0.90 to 5.0, 1.0 to 4.0, 1.0 to 3.0, or 1.5 to 2.5. When the ratio of the molar concentration of the lithium salt to the molar concentration of the additive is in the above-described range, the ionic conductivity and viscosity of the electrolyte may be appropriately exhibited, thereby exhibiting advantageous effects in terms of improving the mobility of lithium ions and suppressing the decomposition reaction of the lithium salt itself, but the present invention is not limited thereto.
[0197] In another embodiment of the present invention, the sum of the concentrations of the lithium salt and the additive in the electrolyte, i.e., the sum concentration, may be, for example, 0.5 M or more, specifically 0.9 M or more, for example, 0.9 M to 2 M, 0.9 M to 1.5 M, or 1.0 M to 1.5 M. When the sum concentration of the lithium salt and the additive in the electrolyte is in the above-described range, it is preferable in terms of the electrical conductivity and viscosity of the electrolyte, and thereby exhibits an advantageous effect in terms of improving the mobility of lithium ions and suppressing the decomposition reaction of the lithium salt itself, but the present invention is not limited thereto.
[0198] In one embodiment of the present invention, the lithium-sulfur battery may exhibit various energy densities depending on the ratio of the electrolyte and the positive electrode active material. However, in terms of the energy density of the lithium-sulfur battery, a smaller ratio of the electrolyte and the positive electrode active material may exhibit a more advantageous effect, and for example, the weight ratio of sulfur in the electrolyte and the sulfur-carbon complex (El / S weight ratio) may be 3.5 g / g or less.
[0199] In one embodiment of the present invention, the lithium-sulfur battery can be manufactured so that the El / S ratio is, for example, 3.0 g / g or less or 2.9 g or less.
[0200] According to one embodiment of the present invention, as described above, by limiting the content of elemental sulfur (S) in the cathode to 3 wt% or less, specifically 3.0 wt% or less, and especially 2.0 wt% or less at SOC 100, long-life characteristics can be exhibited.
[0201] In this specification, the lithium-sulfur battery having long life characteristics means that the capacity retention rate is excellent even when charge and discharge cycles are repeated.
[0202] In one embodiment of the present invention, the lithium-sulfur battery can exhibit an effect of maintaining 80% or more of the initial capacity even after 190 charge-discharge cycles, even when the charge-discharge cycle is repeated. Specifically, when the lithium-sulfur battery is subjected to repeated charge-discharge cycles at a rate of 0.3 to 0.5 C in a range of 1.8 V to 2.5 V at room temperature, the battery can exhibit 80% or more of the capacity measured at one charge-discharge cycle for at least 190 cycles.
[0203] In one embodiment of the present invention, the room temperature may be, for example, a temperature of 23°C to 25°C, and specifically, may be measured at 23°C.
[0204] In one embodiment of the present invention, the charge / discharge rate may be 0.3 C rate or 0.5 C rate, for example, charging at 0.3 C rate and discharging at 0.5 C rate, but is not particularly limited thereto as long as charging / discharging is performed within the above-described rate range.
[0205] In one embodiment of the present invention, the energy density of the lithium-sulfur battery may be, for example, 300 Wh / kg or more.
[0206] In one embodiment of the present invention, the energy density of the lithium-sulfur battery may be measured according to a known method for measuring the energy density, and the measurement method is not particularly limited. For example, the energy density of the lithium-sulfur battery may be measured by discharging at a 0.5 C rate and charging at a 0.3 C rate in a range of 1.8 V to 2.5 V at a room temperature of, for example, 23°C.
[0207] In one embodiment of the present invention, the lithium-sulfur battery may have various shapes, for example, a coin shape, a pouch shape, or a cylindrical shape, but is not limited thereto.
[0208]
[0209] According to another aspect of the present invention, a method for evaluating the life of a lithium-sulfur battery is provided.
[0210] In one embodiment of the present invention, the lithium-sulfur battery to be evaluated for life includes a positive electrode comprising a sulfur-carbon composite, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte.
[0211] Specifically, the lithium-sulfur battery may be a case in which an electrode assembly including the positive electrode, negative electrode, and separator is loaded together with an electrolyte.
[0212] At this time, the negative electrode includes a lithium metal layer and a solid electrolyte membrane (SEI) formed on at least one surface of the lithium metal layer.
[0213] The above evaluation method includes a step of determining a long-life lithium-sulfur battery when the weight of elemental sulfur (S) is 3 wt% or less based on the total weight of the cathode at SOC 100.
[0214] In one embodiment of the present invention, the long-life lithium-sulfur battery may be a battery having a lifespan of 190 cycles or more, particularly 200 cycles or more, when repeating charge and discharge cycles at a rate of 0.3 to 0.5 C in a range of 1.8 V to 2.5 V at room temperature, for example.
[0215] In one embodiment of the present invention, the lithium-sulfur battery to be evaluated is preferably a battery activated by, for example, an initial discharge and repeated charge and discharge cycles. For example, it may be preferable to be a battery activated by repeated charge and discharge cycles of 1 to 20 cycles, 5 to 15 cycles, or at least 10 cycles, for example, 10 cycles, but the present invention is not limited thereto.
[0216] In one embodiment of the present invention, the lithium-sulfur battery to be evaluated may be activated by 0.5C discharge and 0.3C discharge.
[0217] In one embodiment of the present invention, the lithium-sulfur battery to be evaluated may be charged and discharged in a range of 1.8 V to 2.5 V.
[0218] Additionally, the activation of the lithium-sulfur battery to be evaluated may be performed at room temperature, for example, at 23°C to 25°C, for example, at 23°C.
[0219] In one embodiment of the present invention, the lithium-sulfur battery may be discharged at 0.5C and charged at 0.3C in a range of 1.8V to 2.5V at room temperature, 23°C to 25°C.
[0220]
[0221] Hereinafter, preferred examples are presented to help understand the present invention, but the following examples are only illustrative of the present invention, and it is obvious to those skilled in the art that various changes and modifications are possible within the scope and technical idea of the present invention, and it is also natural that such changes and modifications fall within the scope of the appended patent claims.
[0222]
[0223] [Manufacturing of lithium-sulfur batteries]
[0224] Example 1
[0225] A sulfur-carbon composite (S / C weight ratio = 2.3) was prepared by mixing inorganic sulfur (S8) and carbon nanotubes (CNT) as positive electrode active materials, and a positive electrode slurry composition was prepared by mixing 96 wt% of the prepared sulfur-carbon composite and 4 wt% of polyacrylate (PAA) as a binder. The positive electrode slurry composition was applied to an aluminum current collector and then dried to prepare a positive electrode. The loading of the prepared positive electrode was 2.08 mg(s) / cm 2 (2.5 mAh / cm 2 ) was.
[0226] Lithium metal with a thickness of 60 μm was used as the cathode.
[0227] An electrode assembly was prepared by positioning the positive and negative electrodes so that they face each other and interposing a polyethylene separator having a thickness of 16 ㎛ and a porosity of 46 vol% between them.
[0228] The prepared electrode assembly was placed in a pouch-type case, and an electrolyte solution containing 0.75 M lithium salt (LiTFSI) and 2.1 wt% lithium nitrate (LiNO3) dissolved in a solvent mixed with dimethoxyethane (DME):2-methylfuran (2-MeF) in a volume ratio of 8:2 was injected to obtain an El / S ratio of 2.9 g / g, thereby manufacturing a lithium-sulfur battery. As a result, an electrolyte solution having a concentration of 0.33 M LiNO3 as a nitrogen compound was obtained.
[0229]
[0230] Example 2
[0231] A lithium-sulfur battery was manufactured in the same manner as in Example 1, except that 3.5 wt% of lithium nitrate (LiNO3) was dissolved in the electrolyte.
[0232]
[0233] Example 3
[0234] A lithium-sulfur battery was manufactured in the same manner as Example 1, except that 5.0 wt% of lithium nitrate (LiNO3) was dissolved in the electrolyte.
[0235]
[0236] Comparative Example 1
[0237] A lithium-sulfur battery was manufactured using the same method as Example 1, except that 0.8 wt% of lithium nitrate (LiNO3) was dissolved in the electrolyte.
[0238]
[0239] Comparative Example 2
[0240] A lithium-sulfur battery was manufactured in the same manner as in Example 1, except that 0.4 wt% of lithium nitrate (LiNO3) was dissolved in the electrolyte.
[0241]
[0242] LiNO3LiTFSILiTFSI / LiNO3 Molar Ratio Sum Concentration of LiTFSI and LiNO3Example 12.1 wt% (0.33 M) 0.75 M2.25 1.08 MExample 23.5 wt% (0.56 M) 0.75 M1.35 1.31 MExample 35.0 wt% (0.8 M) 0.75 M0.94 1.55 MComparative Example 10.8 wt% (0.13 M) 0.75 M5.90 0.88 MComparative Example 20.4 wt% (0.06 M) 0.75 M11.80 0.81 M
[0243] Energy Density Evaluation of Lithium-Sulfur Batteries
[0244] The lithium-sulfur battery manufactured above was discharged to 1.8 V at a 0.5 C rate at room temperature (23°C), charged once to 2.5 V at the same rate, and then discharged once to 1.8 V at a 0.5 C rate, and the energy density (Wh / kg) of the battery was measured.
[0245] It was confirmed that the energy density of the lithium-sulfur battery according to the examples and comparative examples satisfies 320 Wh / kg.
[0246]
[0247] [Evaluation of the content of elemental sulfur (S) in the cathode at SOC 100]
[0248] Each of the lithium-sulfur batteries manufactured in Examples 1 to 3 and Comparative Examples 1 and 2 above was activated by charging and discharging 10 times, with one cycle being a discharge at a 0.5 C rate and a charge at a 0.3 C rate in the range of 1.8 V to 2.5 V at room temperature (23°C), and then disassembling the battery at an SOC of 100 to obtain a negative electrode.
[0249] At this time, the obtained negative electrode includes a lithium metal layer used in the manufacture of a lithium-sulfur battery and a solid electrolyte membrane (SEI) formed by discharge and charge.
[0250] To obtain a cathode, the lithium-sulfur battery to be measured was disassembled to separate the cathode / separator / cathode, and the separated cathode was placed in a container containing a specified mass of solvent and washed for more than 5 minutes. The solvent used was the same non-aqueous solvent as the electrolyte.
[0251] The content of lithium (Li), sulfur (S), nitrogen (N), and fluorine (F) elements in the obtained cathode was analyzed, and the analysis results are shown in Table 2 below.
[0252] The method for analyzing the content of the above lithium (Li), sulfur (S), nitrogen (N), and fluorine (F) elements was performed as follows.
[0253] First, for the analysis of lithium, sulfur, and fluorine, a certain amount of sample weight was measured in a moisture-controlled dry room, and then a primary oxidation reaction was induced with water. After the primary oxidation reaction, nitric acid was added to dissolve the components in the sample in an ionic state. The treated solution was quantitatively analyzed using ICP-OES (or ICP-MS). The analysis of the fluorine element content was performed by immediately quantitatively analyzing the solution after the primary oxidation using IC.
[0254] The content of the above nitrogen element was determined by encapsulating a certain amount of the encapsulated sample with paraffin film in a dry room, thermally decomposing the encapsulated sample in an oxygen-filled atmosphere using an oxygen combustion chamber (bomb), and then saturating and dissolving the vaporized nitrogen in the internal solvent. The nitrogen absorption solution was quantitatively analyzed using IC.
[0255] The mass of each element analyzed according to the above method was calculated as a weight% based on the total weight of the cathode to be analyzed, and is shown in Table 2 below. At this time, the sum of the masses of each element analyzed was used as the total weight of the cathode.
[0256]
[0257] [Life Assessment]
[0258] Each of the lithium-sulfur batteries manufactured in Examples 1 to 3 and Comparative Examples 1 and 2 above was activated by discharging at a 0.5 C rate and charging at a 0.3 C rate in the range of 1.8 V to 2.5 V at room temperature (23°C), and then charging and discharging at a 0.5 C rate was repeated. The number of cycles until the capacity was maintained at 80% based on the battery capacity measured in the first cycle after activation was measured, and the results are shown in Table 2 below.
[0259]
[0260] Analysis of content in the cathode (wt%) at SOC 100 Lifetime evaluation LiSNFCycle Example 199.4 0.10.4 0.120 2 Example 299.20.5 0.20.1 198 Example 399.6 0.10.20.1 230 Comparative Example 195.3 3.5 0.7 0.5 178 Comparative Example 293.5 5.6 0.10.8 158
[0261] As confirmed in Table 2 above, it was confirmed that a lithium-sulfur battery having long-life characteristics can be implemented when the content of sulfur element (S) in the negative electrode is controlled to 3 wt% or less in the SOC100 state.
Claims
1. A lithium-sulfur battery comprising a positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte comprising a sulfur-carbon complex, The above negative electrode includes a lithium metal layer and a solid electrolyte membrane (SEI) formed on at least one surface of the lithium metal layer, A lithium-sulfur battery, wherein the weight of sulfur element (S) present in the negative electrode at SOC 100 is 3 wt% or less based on the total weight of the negative electrode.
2. In claim 1, The above SOC 100 is a lithium-sulfur battery having a potential of 2.4 V to 2.7 V.
3. In claim 1, A lithium-sulfur battery wherein the weight of sulfur element (S) in the negative electrode is 3 wt% or less based on the combined weight of sulfur element (S) and lithium element (Li) in the negative electrode.
4. In claim 3, A lithium-sulfur battery wherein the weight of sulfur element (S) in the negative electrode is 2 wt% or less based on the combined weight of sulfur element (S) and lithium element (Li) in the negative electrode.
5. In claim 3, A lithium-sulfur battery wherein the weight of sulfur element (S) in the negative electrode is 1 wt% or less based on the combined weight of sulfur element (S) and lithium element (Li) in the negative electrode.
6. In claim 1, A lithium-sulfur battery wherein the thickness of the above negative electrode is 120 ㎛ or less.
7. In claim 1, A lithium-sulfur battery wherein the thickness of the above negative electrode is 70 ㎛ or less.
8. In claim 1, The above sulfur-carbon complex is a lithium-sulfur battery having a sulfur / carbon weight ratio (S / C weight ratio) of 2.5 g / g or less.
9. In claim 1, The positive electrode comprises a current collector and a positive electrode active material layer including the sulfur-carbon complex, A lithium-sulfur battery in which the weight of the sulfur-carbon composite is 90 wt% or more based on the total weight of the positive electrode active material layer.
10. In claim 1, A lithium-sulfur battery having an El / S weight ratio of sulfur in the electrolyte and the sulfur-carbon complex of 3.5 g / g or less.
11. In claim 1, A lithium-sulfur battery wherein the electrolyte comprises a non-aqueous solvent, a lithium salt, and an additive.
12. In claim 11, The above additive is a lithium-sulfur battery containing a nitrogen compound.
13. In claim 11, The above additive is a lithium-sulfur battery containing lithium nitrate (LiNO3).
14. In claim 11, A lithium-sulfur battery, wherein the content of the additive is 1 wt% to 5 wt% based on the total weight of the electrolyte.
15. In claim 11, A lithium-sulfur battery, wherein the ratio of the molar concentration of the lithium salt to the molar concentration of the additive is 0.5 to 5 (molar concentration of lithium salt / molar concentration of additive).
16. In claim 1, The lithium-sulfur battery has a lifespan of 190 cycles or more when repeating charge and discharge cycles at a rate of 0.3 to 0.5 C in the range of 1.8 V to 2.5 V at room temperature.
17. In claim 16, The above room temperature is a lithium-sulfur battery having a temperature of 23°C to 25°C.
18. In claim 1, A lithium-sulfur battery having an energy density of 300 Wh / kg or more.
19. A cathode comprising a sulfur-carbon complex, a separator interposed between the cathode and the anode, and an electrolyte, The above negative electrode is a life evaluation method of a lithium-sulfur battery including a lithium metal layer and a solid electrolyte membrane (SEI) formed on at least one surface of the lithium metal layer, An evaluation method including a step of determining a long-life lithium-sulfur battery when the weight of sulfur element (S) present in the negative electrode at SOC 100 is 3 wt% or less based on the total weight of the negative electrode.
20. In claim 19, An evaluation method in which the above-mentioned long-life lithium-sulfur battery has a lifespan of 190 cycles or more when repeating charge and discharge cycles at a rate of 0.3 to 0.5 C in the range of 1.8 V to 2.5 V at room temperature.
Citation Information
Patent Citations
Electrolytes for lithium-sulfur electrochemical cells
KR1020070027512A
Lithium ion secondary battery
US20210083282A1
KR20200033186A