Compound, composite, and solid electrolyte and all-solid-state battery comprising same

The use of a lithium-friendly compound with specific repeating units and lithium salts in all-solid-state batteries addresses ionic conductivity and dendrite growth issues, enhancing battery stability and enabling rapid charging by improving lithium ion transport and transference numbers.

WO2024228578A1PCT designated stage expired Publication Date: 2024-11-07LG CHEM LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/005994
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-07-20
Filing Date
2024-05-03
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

Current solid electrolytes for all-solid-state batteries face challenges in ionic conductivity and stability, particularly with lithium dendrite growth on the surface of lithium metal anodes, limiting their performance and lifespan.

Method used

A compound with a lithium-friendly structure, represented by specific repeating units and lithium salts, is used to enhance ionic conductivity and suppress lithium dendrite formation by improving lithium ion transport and transference numbers, thereby improving battery stability and enabling rapid charging.

Benefits of technology

The compound significantly enhances ionic conductivity and electrochemical stability, reducing lithium dendrite formation, which extends battery lifespan and allows for rapid charging in all-solid-state batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTKR2024005994-APPB-IMG-000001
    Figure PCTKR2024005994-APPB-IMG-000001
  • Figure PCTKR2024005994-APPB-IMG-000002
    Figure PCTKR2024005994-APPB-IMG-000002
  • Figure PCTKR2024005994-APPB-IMG-000003
    Figure PCTKR2024005994-APPB-IMG-000003
Patent Text Reader

Abstract

The present invention aims to improve upon conventional low lithium ion conductivity and resolve the performance and safety issues of an all-solid-state battery, and relates to a compound comprising a repeating unit represented by chemical formula 1 described in the present specification or a compound which is a lithium salt thereof, a composite comprising the compound and a lithium compound, and a solid electrolyte and an all-solid-state battery comprising same.
Need to check novelty before this filing date? Find Prior Art

Description

Compounds, complexes, solid electrolytes containing the same, and all-solid-state batteries

[0001] Cross-citation with related applications

[0002] This application claims the benefit of priority to Korean Patent Application No. 10-2023-0057976, filed May 3, 2023, Korean Patent Application No. 10-2023-0057984, filed May 3, 2023, and Korean Patent Application No. 10-2023-0094880, filed July 20, 2023, the entire contents of which are incorporated herein by reference.

[0003]

[0004] Technology field

[0005] The present invention relates to a compound, a complex, a solid electrolyte and an all-solid-state battery comprising the same for improving the ionic conductivity of an all-solid-state battery and suppressing the growth of lithium dendrites occurring on the surface of a lithium metal negative electrode.

[0006]

[0007] High-energy-density lithium secondary batteries, currently primarily used in laptops and smartphones, consist of a lithium oxide anode, a carbon-based cathode, a separator, and a liquid or solid electrolyte. However, lithium secondary batteries composed of flammable liquid electrolytes have safety issues such as leakage, ignition, and explosion, and the design of these batteries becomes more complex to prevent these issues.

[0008] Therefore, to solve the problems of these liquid electrolytes, research on solid electrolytes having non-flammable or flame-retardant properties is in progress, and the solid electrolytes can be classified into sulfide-based electrolytes, oxide-based electrolytes, and polymer electrolytes.

[0009] The above sulfide-based electrolyte has the advantages of high ionic conductivity, low interfacial resistance, and stability over a wide voltage range, but there are cases where trace impurities such as moisture mixed inside the battery react with the sulfide-based electrolyte to generate hydrogen sulfide inside the battery, and there is a risk of hydrogen sulfide being generated even when charging and discharging the battery, so it has the problem of being poor in terms of stability.

[0010] In addition, although the oxide-based electrolyte has high chemical stability, it has the disadvantages of having low ionic conductivity compared to the sulfide-based electrolyte, requiring high-temperature sintering treatment, and making it difficult to manufacture large-area batteries.

[0011] Accordingly, since the polymer electrolyte has the advantages of being a solid electrolyte material due to its characteristics of low cost, flexibility, and process convenience, research on the polymer electrolyte is being actively conducted.

[0012] The polymer electrolytes described above are broadly categorized into gel and solid types. Gel polymer electrolytes exhibit conductivity by impregnating a high-boiling-point liquid electrolyte within a polymer film and fixing it together with a lithium salt. Because they contain a large amount of liquid electrolyte, they possess ionic conductivity similar to that of pure liquid electrolytes, but electrochemical stability issues still remain.

[0013] On the other hand, solid polymer electrolytes, which do not contain liquid electrolytes, not only improve stability issues related to leakage, but also offer the advantage of high chemical and electrochemical stability. However, their ionic conductivity at room temperature is lower than that of liquid electrolytes, and extensive research is being conducted to improve this.

[0014] Currently, the most widely used solid polymer electrolyte is polyethylene oxide (PEO), which possesses the ability to conduct lithium ions despite its solid state. However, linear PEO polymer electrolytes suffer from limitations in chain mobility due to their high crystallinity, a low dielectric constant (5.0), which prevents the dissociation of large amounts of lithium ions, and very low ionic conductivity at room temperature, making them difficult to apply to lithium secondary batteries.

[0015] (Patent Document 001) JP 1985-069140 A

[0016]

[0017] The problem to be solved by the present invention is to provide a compound for improving the ionic conductivity of a solid electrolyte and the performance and stability of an all-solid-state battery, a solid electrolyte including the compound, and an all-solid-state battery.

[0018] In addition, the problem to be solved by the present invention is to provide a compound for suppressing the growth of lithium dendritic crystals, i.e., dendrites, that occur on the surface of a lithium metal negative electrode, a solid electrolyte including the compound, and an all-solid-state battery.

[0019]

[0020] The present invention provides a compound, a complex, a solid electrolyte comprising the same, and an all-solid-state battery.

[0021] (1) The present invention provides a compound comprising a repeating unit represented by the following chemical formula 1 or a lithium salt thereof.

[0022] [Chemical Formula 1]

[0023]

[0024] In the above chemical formula 1,

[0025] The above X, Y and Z are each independently at least one selected from the group consisting of the following chemical formulas a-1, b and c-1,

[0026] The above n is an integer from 1 to 100,

[0027] The above q is an integer from 1 to 100,

[0028] The above o is an integer from 0 to 100,

[0029] The above * indicates a connecting portion or terminal portion between repeating units,

[0030] [Chemical formula a-1]

[0031]

[0032] [chemical formula b]

[0033]

[0034] [Chemical formula c-1]

[0035]

[0036] In the above chemical formulas a-1, b and c-1,

[0037] The above R1, R2 and R3 are each independently a hydrogen element; a halogen element; -CN; -NO2; substituted or unsubstituted C1-C 10 Alkyl group of; substituted or unsubstituted C1-C 10 Alkoxy group of; substituted or unsubstituted C2-C 10 Alkenyl group of; substituted or unsubstituted C2-C 10 an alkynyl group of; -C(=O)R5; -P(=O)(OR5)2; -P(OR5)(OR6); -OP(=O)(OR5)(OR6); -S(=O)R5; or -S(=O)2R5,

[0038] The above R4 is a hydrogen atom; or a substituted or unsubstituted C1-C 10 is an alkyl group,

[0039] The above R5 and R6 are each independently a hydrogen element; substituted or unsubstituted C1-C 10 an alkyl group of; or a substituted or unsubstituted C2-C 10 is an alkenyl group,

[0040] The above L1, L2 and L3 are each independently a direct bond; or a substituted or unsubstituted C1-C 10 is an alkylene group,

[0041] The above X1 and X2 are each independently a hydrogen element; a halogen element; -CN; -NO2; a substituted or unsubstituted C1-C 10 an alkyl group of; or a substituted or unsubstituted C6-C 12 is an aryl group,

[0042] The above m is an integer from 1 to 40,

[0043] The above p is an integer from 1 to 200.

[0044] (2) The present invention provides a compound in (1) above, wherein at least one of X, Y and Z comprises the chemical formula a-1.

[0045] (3) The present invention provides a compound in (1) or (2) above, wherein R2 and R4 are each independently a C1-C5 alkyl group.

[0046] (4) The present invention is one of the above (1) to (3), wherein the L 1, L2 and L3 each independently provide a compound which is an alkylene group of C1-C5.

[0047] (5) The present invention provides a compound in any one of the above (1) to (4), wherein X1 and X2 are each independently a hydrogen element; or a halogen element.

[0048] (6) The present invention provides a compound according to any one of the above (1) to (5), wherein n is an integer from 1 to 20, q is an integer from 1 to 20, o is an integer from 0 to 20, m is an integer from 1 to 10, and p is an integer from 1 to 50.

[0049] (7) The present invention provides a compound comprising a repeating unit represented by the chemical formula 1 in any one of the above (1) to (6), wherein the compound is represented by the following chemical formula 1-a or 1-b.

[0050] [Chemical Formula 1-a]

[0051]

[0052] [Chemical Formula 1-b]

[0053]

[0054] In the above chemical formulas 1-a and 1-b, n is an integer from 1 to 20, q is an integer from 1 to 20, and o is an integer from 1 to 20.

[0055] (8) The present invention provides a compound comprising at least one functional group selected from the group consisting of the following chemical formulae d to g at at least one terminal portion among the terminal portions in any one of the above (1) to (7).

[0056] [chemical formula d]

[0057]

[0058] [chemical formula e]

[0059]

[0060] [chemical formula f]

[0061]

[0062] [chemical formula g]

[0063]

[0064] In the above chemical formulas d to g,

[0065] The above R7 is a hydrogen atom; or a substituted or unsubstituted C1-C 10 is an alkyl group,

[0066] Above R8 to R 11are each independently, direct bond; substituted or unsubstituted C1-C 10 alkylene group of; or -R 12 -OR 13 -and,

[0067] The above R 12 and R 13 are each independently, directly bonded; or substituted or unsubstituted C1-C 10 is an alkylene group,

[0068] The above * indicates the binding position.

[0069] (9) In the present invention, in the above (8), R7 is a C1-C6 alkyl group, and R8 to R 11 are each independently a direct bond; a C1-C6 alkylene group substituted or unsubstituted with a fluorine atom; or -R 12 -OR 13 - and the above R 12 and R 13 Each independently provides a compound wherein the direct bond: or the fluorine atom is a substituted or unsubstituted C1-C6 alkylene group.

[0070] (10) The present invention provides a compound represented by the following chemical formula 1-c in the above (8) or (9).

[0071] [Chemical Formula 1-c]

[0072]

[0073] In the above chemical formula 1-c, n is an integer from 1 to 20, q is an integer from 1 to 20, and o is an integer from 1 to 20.

[0074] (11) The present invention provides a compound comprising a repeating unit represented by the following chemical formula 2, wherein the lithium salt is in any one of the above (1) to (10).

[0075] [Chemical Formula 2]

[0076]

[0077] In the above chemical formula 2,

[0078] The above X, Y and Z are each independently at least one selected from the group consisting of the following chemical formulas a-1, b and c-1,

[0079] The above n is an integer from 1 to 100,

[0080] The above q is an integer from 1 to 100,

[0081] The above o is an integer from 0 to 100,

[0082] The above * indicates a connecting portion or terminal portion between repeating units,

[0083] [Chemical formula a-1]

[0084]

[0085] [chemical formula b]

[0086]

[0087] [Chemical formula c-1]

[0088]

[0089] In the above chemical formulas a-1, b and c-1,

[0090] The above R1, R2 and R3 are each independently a hydrogen element; a halogen element; -CN; -NO2; substituted or unsubstituted C1-C 10 Alkyl group of; substituted or unsubstituted C1-C 10 Alkoxy group of; substituted or unsubstituted C2-C 10 Alkenyl group of; substituted or unsubstituted C2-C 10 an alkynyl group of; -C(=O)R5; -P(=O)(OR5)2; -P(OR5)(OR6); -OP(=O)(OR5)(OR6); -S(=O)R5; or -S(=O)2R5,

[0091] The above R4 is a hydrogen atom; or a substituted or unsubstituted C1-C 10is an alkyl group,

[0092] The above R5 and R6 are each independently a hydrogen element; substituted or unsubstituted C1-C 10 an alkyl group of; or a substituted or unsubstituted C2-C 10 is an alkenyl group,

[0093] The above L1, L2 and L3 are each independently a direct bond; or a substituted or unsubstituted C1-C 10 is an alkylene group,

[0094] The above X1 and X2 are each independently a hydrogen element; a halogen element; -CN; -NO2; a substituted or unsubstituted C1-C 10 an alkyl group of; or a substituted or unsubstituted C6-C 12 is an aryl group,

[0095] The above m is an integer from 1 to 40,

[0096] The above p is an integer from 1 to 200.

[0097] (12) The present invention provides a compound including a repeating unit represented by the chemical formula 2 in the above (11), wherein the compound is represented by the following chemical formula 2-a or 2-b.

[0098] [Chemical Formula 2-a]

[0099]

[0100] [Chemical Formula 2-b]

[0101]

[0102] In the above chemical formulas 2-a and 2-b, n is an integer from 1 to 20, q is an integer from 1 to 20, and o is an integer from 1 to 20.

[0103] (13) The present invention provides a compound comprising at least one functional group selected from the group consisting of the following chemical formulae d to g at at least one terminal portion among the terminal portions in (11) or (12).

[0104] [chemical formula d]

[0105]

[0106] [chemical formula e]

[0107]

[0108] [chemical formula f]

[0109]

[0110] [chemical formula g]

[0111]

[0112] In the above chemical formulas d to g,

[0113] The above R7 is a hydrogen atom; or a substituted or unsubstituted C1-C 10 is an alkyl group,

[0114] Above R8 to R 11 are each independently, direct bond; substituted or unsubstituted C1-C 10 alkylene group of; or -R 12 -OR 13 -and,

[0115] The above R 12 and R 13 are each independently, directly bonded; or substituted or unsubstituted C1-C 10 is an alkylene group,

[0116] The above * indicates the binding position.

[0117] (14) The present invention provides a compound including a repeating unit represented by the chemical formula 2 in the above (13), which is represented by the following chemical formula 2-c.

[0118] [Chemical Formula 2-c]

[0119]

[0120] In the above chemical formula 2-c, n is an integer from 1 to 20, q is an integer from 1 to 20, and o is an integer from 1 to 20.

[0121] (15) The present invention provides a complex comprising a compound according to at least one of (1) to (14) and a lithium compound.

[0122] (16) In the present invention, in the above (15), the lithium compound is LiCl, LiBr, LiI, LiBF4, LiClO4, LiB 10 Cl 10 , LiAlCl4, LiAlO4, LiPF6, LiCF3SO3, LiCH3CO2, LiCF3CO2, LiAsF6, LiSbF6, LiCH3SO3, LiFSI (lithium bis(fluorosulfonyl)imide, LiN(SO2F)2), LiBETI (lithium bisperfluoroethanesulfonimide, LiN(SO2CF2CF3)2) and LiTFSI (lithium (bis)trifluoromethanesulfonimide, LiN(SO2CF3)2).

[0123] (17) The present invention provides a complex in the above (15) or (16), wherein the complex is represented by at least one selected from the group consisting of the following chemical formulas 3-a, 4-a and 4-b.

[0124] [Chemical Formula 3-a]

[0125]

[0126] [Chemical Formula 4-a]

[0127]

[0128] [Chemical Formula 4-b]

[0129]

[0130] In the above chemical formulas 3-a, 4-a and 4-b, n is an integer from 1 to 20, q is an integer from 1 to 20, and o is an integer from 1 to 20.

[0131] (18) The present invention provides a solid electrolyte comprising at least one selected from the group consisting of compounds according to (1) to (14) and complexes according to (15) to (17).

[0132] (19) The present invention provides a solid electrolyte further comprising a crosslinking compound in the above (18).

[0133] (20) The present invention provides an all-solid-state battery including a solid electrolyte according to (19).

[0134] (21) The present invention provides a compound represented by the following chemical formula A.

[0135] [Chemical Formula A]

[0136]

[0137] In the above chemical formula A,

[0138] The above R 21 , R 22 and R 23 are each independently a hydrogen element; a halogen element; a substituted or unsubstituted C1-C 10 Alkyl group of; substituted or unsubstituted C1-C 10 Alkoxy group of; substituted or unsubstituted C2-C 10 an alkenyl group of; or a substituted or unsubstituted C2-C 10 is an alkynyl group,

[0139] The above R 24 is a hydrogen element; or substituted or unsubstituted C1-C 10 is an alkyl group,

[0140] Above L 21 and L 22are each independently substituted or unsubstituted C1-C 10 alkylene group of; -P(=O)(OR 25 )-; -(C=O)-; -(S=O)-; or -S(=O)2-,

[0141] Above X 21 and X 22 are each independently a halogen element; -NH2; phosphate (-OP(=O)(OR 25 )2); Nitrate(-ON(=O)(OR 25 )); tosylate (-OTs); sulfonate (-OS(=O)2R 25 ); or carboxylate (-OC(=O)CH3),

[0142] The above R 25 is substituted or unsubstituted C1-C 10 Alkyl group of; substituted or unsubstituted C2-C 10 an alkenyl group of; or a substituted or unsubstituted C2-C 10 is an alkynyl group.

[0143] (22) The present invention, in the above (21), the R 22 , R 24 and R 25 Each independently provides a compound having a C1-C5 alkyl group.

[0144] (23) The present invention, in the above (21) or (22), the L 21 and L 22 provides a compound of -S(=O)2-.

[0145] (24) The present invention is one of the above (21) to (23), wherein X 21 and X 22 Each independently provides a halogen element or a compound that is -NH2.

[0146] (25) The present invention provides a compound in which the compound represented by the chemical formula A in any one of the above (21) to (24) is at least one selected from the group consisting of the following chemical formulas Aa, Ab and Ac.

[0147] [Chemical formula Aa]

[0148]

[0149] [Chemical formula Ab]

[0150]

[0151] [Chemical formula Ac]

[0152] .

[0153] (26) The present invention provides a complex comprising a compound according to any one of (21) to (25) and a lithium compound.

[0154] (27) The present invention provides a complex represented by the following chemical formula B in the above (26).

[0155] [Chemical Formula B]

[0156]

[0157] In the above chemical formula B,

[0158] The above R 21 , R 22 and R 23 are each independently a hydrogen element; a halogen element; a substituted or unsubstituted C1-C 10 Alkyl group of; substituted or unsubstituted C1-C 10 Alkoxy group of; substituted or unsubstituted C2-C 10 an alkenyl group of; or a substituted or unsubstituted C2-C 10 is an alkynyl group,

[0159] The above R 24 is a hydrogen element; or substituted or unsubstituted C1-C 10 is an alkyl group,

[0160] Above L 21 and L 22 are each independently substituted or unsubstituted C1-C 10 alkylene group of; -P(=O)(OR 25 )-; -(C=O)-; -(S=O)-; or -S(=O)2-,

[0161] Above X 21 and X 22 are each independently a halogen element; -NH2; phosphate (-OP(=O)(OR 25 )2); Nitrate(-ON(=O)(OR 25 )); tosylate (-OTs); sulfonate (-OS(=O)2R 25 ); or carboxylate (-OC(=O)CH3),

[0162] The above R 25 is substituted or unsubstituted C1-C 10 Alkyl group of; substituted or unsubstituted C2-C 10 an alkenyl group of; or a substituted or unsubstituted C2-C 10 is an alkynyl group,

[0163] Above Y - is a halogen anion, BF4 - , ClO4 - , AlCl4 - , AlO4 - , PF6 - , CF3SO3 - , CH3CO2 - , CF3CO2 - , AsF6 - , SbF6 - , CH3SO3 - , FSI - (bis(fluorosulfonyl)imide, N(SO2F)2 - ), BETI (lithium bisperfluoroethanesulfonimide, N(SO2CF2CF3)2 - ) and TFSI ((bis)trifluoromethanesulfonimide, N(SO2CF3)2- ) is one or more selected from the group consisting of.

[0164] (28) The present invention provides a complex according to (26) or (27), wherein the complex is at least one selected from the group consisting of the following chemical formulas Ba, Bb and Bc.

[0165] [chemical formula Ba]

[0166]

[0167] [chemical formula Bb]

[0168]

[0169] [Chemical formula Bc]

[0170] .

[0171] (29) The present invention provides a polymer comprising a repeating unit derived from a compound according to any one of the above (21) to (25), a repeating unit derived from a complex according to any one of the above (26) to (28), or a combination thereof.

[0172] (30) The present invention provides a polymer in which the repeating unit derived from the compound according to any one of (21) to (25) in the above (29) is represented by the following chemical formula Wa or Wb.

[0173] [chemical formula Wa]

[0174]

[0175] [Chemical formula Wb]

[0176]

[0177] In the above chemical formulas Wa and Wb,

[0178] wherein n is an integer from 1 to 300,

[0179] The above * indicates a connection between repeating units.

[0180] (31) The present invention provides a polymer in which the repeating unit derived from the complex according to any one of (26) to (28) in the above (29) is represented by the following chemical formula Xa or Xb.

[0181] [chemical formula Xa]

[0182]

[0183] [chemical formula Xb]

[0184]

[0185] In the above chemical formulas Xa and Xb,

[0186] Above Y - is a halogen anion, BF4 - , ClO4 - , AlCl4 - , AlO4 - , PF6 - , CF3SO3 - , CH3CO2 - , CF3CO2 - , AsF6 - , SbF6 - , CH3SO3 - , FSI - (bis(fluorosulfonyl)imide, N(SO2F)2 - ), BETI (lithium bisperfluoroethanesulfonimide, N(SO2CF2CF3)2 - ) and TFSI ((bis)trifluoromethanesulfonimide, N(SO2CF3)2 - ) is one or more selected from the group consisting of,

[0187] The above n is an integer from 1 to 300,

[0188] The above * indicates a connection between repeating units.

[0189] (32) The present invention provides a polymer in which, in the above (29), a combination of a repeating unit derived from a compound according to any one of the above (21) to (25) and a repeating unit derived from a complex according to any one of the above (26) to (28) is represented by the following chemical formula Y or Z.

[0190] [Chemical formula Y]

[0191]

[0192] [Chemical formula Z]

[0193]

[0194] In the above chemical formulas Y and Z,

[0195] Above Y - is a halogen anion, BF4 - , ClO4 - , AlCl4 - , AlO4 - , PF6 - , CF3SO3 - , CH3CO2 - , CF3CO2 - , AsF6 - , SbF6 - , CH3SO3 - , FSI - (bis(fluorosulfonyl)imide, N(SO2F)2 - ), BETI (lithium bisperfluoroethanesulfonimide, N(SO2CF2CF3)2 - ) and TFSI ((bis)trifluoromethanesulfonimide, N(SO2CF3)2 - ) is one or more selected from the group consisting of,

[0196] The above n and m are each independently an integer from 1 to 300,

[0197] The above * indicates a connection between repeating units.

[0198] (33) The present invention provides a solid electrolyte comprising a polymer according to any one of (29) to (32).

[0199]

[0200] According to the present invention, when a compound having a lithium-friendly structure capable of chelating lithium ions and a lithium salt thereof are applied to an all-solid-state battery, the effect of improving ion conductivity and ion transport rate can be achieved.

[0201] According to the present invention, when a compound having a high lithium ion transport rate and a lithium salt thereof are applied to an electrolyte, the effect of suppressing the growth of lithium dendrite crystals occurring on the surface of a negative electrode can be achieved.

[0202]

[0203] Hereinafter, the present invention will be described in more detail to facilitate understanding. The terms and words used in this specification and claims should not be interpreted based on their conventional or dictionary meanings. Rather, they should be interpreted based on the principle that the inventor can appropriately define the concepts of terms to best explain his or her invention. Therefore, they should be interpreted based on meanings and concepts consistent with the technical spirit of the present invention.

[0204] The terminology used herein is for the purpose of describing exemplary embodiments only and is not intended to limit the present invention. Singular expressions include plural expressions unless the context clearly dictates otherwise.

[0205] In this specification, it should be understood that the terms “include,” “comprising,” or “having” are intended to specify the presence of a feature, number, step, component, or combination thereof, but do not preclude the possibility of the presence or addition of one or more other features, numbers, steps, components, or combinations thereof.

[0206] The term 'all solid state battery' used in this specification refers to a battery in which all components of the battery are solid, and is distinguished from a liquid electrolyte secondary battery that uses a liquid electrolyte such as an electrolyte, and a gel polymer secondary battery that uses a liquid electrolyte together with a polymer electrolyte instead of a separator.

[0207] The term "substituted or unsubstituted" in this specification means substituted with one or more substituents selected from among deuterium, halogen, hydroxy, amino, thiol, nitro, nitrile, silyl, and straight or branched C1-C6 alkoxy groups, or has no substituents.

[0208] The term “alkyl group” used herein may mean, unless otherwise specified, a straight or branched acyclic group having 1 to 20 carbon atoms, or 1 to 16 carbon atoms, or 1 to 12 carbon atoms, or 1 to 8 carbon atoms, or 1 to 6 carbon atoms; a cyclic group having 3 to 20 carbon atoms, or 3 to 16 carbon atoms, or 3 to 12 carbon atoms, or 3 to 8 carbon atoms, or 3 to 6 carbon atoms; or a saturated hydrocarbon group combined therewith.

[0209] The term “alkenyl group” used herein may mean, unless otherwise specified, a straight-chain branched acyclic group having 2 to 20 carbon atoms, or 2 to 16 carbon atoms, or 2 to 12 carbon atoms, or 2 to 8 carbon atoms, or 2 to 6 carbon atoms and having one or more double bonds; a cyclic group having 3 to 20 carbon atoms, or 3 to 16 carbon atoms, or 3 to 12 carbon atoms, or 3 to 8 carbon atoms, or 3 to 6 carbon atoms and having one or more double bonds; or an unsaturated hydrocarbon group combined therewith.

[0210] The term “alkynyl group” used herein may mean, unless otherwise specified, a straight or branched chain acyclic group having 2 to 20 carbon atoms, or 2 to 16 carbon atoms, or 2 to 12 carbon atoms, or 2 to 8 carbon atoms, or 2 to 6 carbon atoms and having one or more triple bonds; a cyclic group having 3 to 20 carbon atoms, or 3 to 16 carbon atoms, or 3 to 12 carbon atoms, or 3 to 8 carbon atoms, or 3 to 6 carbon atoms and having one or more triple bonds; or an unsaturated hydrocarbon group combined therewith.

[0211] In this specification, “*” is a bonding position, which is a position where a functional group is bonded to a connecting portion or terminal between repeating units, and in the case of a terminal, a hydrogen atom; -CN; -NH 2; Halogen elements; substituted or unsubstituted C1-C 10 Alkyl group of; substituted or unsubstituted C1-C 10 Alkoxy group of; substituted or unsubstituted C2-C 10 an alkenyl group of; or a substituted or unsubstituted C2-C 10 It may mean one or more selected from the group consisting of alkynyl groups.

[0212]

[0213] compound

[0214] The present invention provides a compound comprising a repeating unit represented by the following chemical formula 1 or a lithium salt thereof.

[0215] [Chemical Formula 1]

[0216]

[0217] In the above chemical formula 1,

[0218] The above X, Y and Z are each independently at least one selected from the group consisting of the following chemical formulas a-1, b and c-1,

[0219] The above n is an integer from 1 to 100,

[0220] The above q is an integer from 1 to 100,

[0221] The above o is an integer from 0 to 100,

[0222] The above * indicates a connecting portion or terminal portion between repeating units,

[0223] [Chemical formula a-1]

[0224]

[0225] [chemical formula b]

[0226]

[0227] [Chemical formula c-1]

[0228]

[0229] In the above chemical formulas a-1, b and c-1,

[0230] The above R1, R2 and R3 are each independently a hydrogen element; a halogen element; -CN; -NO2; substituted or unsubstituted C1-C 10 Alkyl group of; substituted or unsubstituted C1-C 10 Alkoxy group of; substituted or unsubstituted C2-C 10 Alkenyl group of; substituted or unsubstituted C2-C 10 an alkynyl group of; -C(=O)R5; -P(=O)(OR5)2; -P(OR5)(OR6); -OP(=O)(OR5)(OR6); -S(=O)R5; or -S(=O)2R5,

[0231] The above R4 is a hydrogen atom; or a substituted or unsubstituted C1-C 10 is an alkyl group,

[0232] The above R5 and R6 are each independently a hydrogen element; substituted or unsubstituted C1-C 10 an alkyl group of; or a substituted or unsubstituted C2-C 10 is an alkenyl group,

[0233] The above L1, L2 and L3 are each independently a direct bond; or a substituted or unsubstituted C1-C 10 is an alkylene group,

[0234] The above X1 and X2 are each independently a hydrogen element; a halogen element; -CN; -NO2; a substituted or unsubstituted C1-C 10 an alkyl group of; or a substituted or unsubstituted C6-C 12 is an aryl group,

[0235] The above m is an integer from 1 to 40,

[0236] The above p is an integer from 1 to 200.

[0237]

[0238] Conventional liquid electrolytes are flammable, which causes safety issues such as ignition. Solid electrolytes have excellent process stability because they do not cause liquid leakage problems, and they can be processed into thin films and films, which makes the process convenient. However, as described above, they have the disadvantage of significantly lower ionic conductivity compared to conventional liquid electrolytes. Therefore, the inventors of the present invention have developed a compound having a lithium ion-friendly structure and a solid electrolyte comprising the same.

[0239]

[0240] The compound including the repeating unit represented by the above chemical formula 1 and the lithium salt thereof are compounds having a lithium-friendly structure capable of chelating lithium ions. The compound including the repeating unit represented by the above chemical formula 1 and the lithium salt thereof contain sulfonimide or an anion of sulfonimide in which a proton bonded to a nitrogen atom in sulfonimide is detached, and therefore, when used as a material for a solid electrolyte, the affinity for lithium ions may be high. Meanwhile, in a process for manufacturing a solid electrolyte including a compound including the repeating unit represented by the above chemical formula 1, a proton bonded to a nitrogen atom in sulfonimide may be detached. In addition, the anion of the sulfonimide has a relatively small electron density compared to anions of other organic groups such as carboxylate, and thus the electrostatic attraction with lithium ions is weak, and therefore, the transport rate of lithium ions in the solid electrolyte can be increased. In particular, the lithium salt may have an effect of improving the lithium ion transference number compared to a material obtained by hydrogenating an existing ethylene oxide-based material or a material obtained by mixing lithium salts separately, for example, a PEO mixture mixed with lithium salts.

[0241] In addition, since the compound including the repeating unit represented by the above chemical formula 1 and the lithium salt thereof contain at least one selected from the group consisting of the above chemical formulas a-1, b, and c-1, the electrons of the sulfonimide anion can be delocalized, thereby further improving the ionic conductivity of the solid electrolyte. In addition, since the compound according to the present invention also performs the role of a conventional lithium salt in a solid electrolyte, it can replace a conventional lithium salt, thereby reducing the manufacturing cost of an all-solid-state battery.

[0242]

[0243] In addition, lithium metal anodes, which are anode materials that are in the spotlight in next-generation batteries including conventional all-solid-state batteries, have chronic problems such as shortened lifespan and side reactions due to the formation of lithium dendrites, i.e., lithium dendritic crystals. However, the solid electrolyte including the compound of the present invention has a high lithium ion transference number, and thus can improve the lifespan of the battery by suppressing the dendrite phenomenon. In addition, in a rapid charging environment, the formation of lithium dendrites is accelerated, making it difficult to introduce rapid charging in a conventional lithium metal battery composition. However, in the case of an all-solid-state battery including the compound of the present invention, the dendrite phenomenon is suppressed, and thus rapid charging may be possible. The compound of the present invention may be a compound including a repeating unit represented by Chemical Formula 1 and a lithium salt thereof, and the lithium salt may be a compound including a repeating unit represented by Chemical Formula 2, which will be described below. In particular, as a result of the experiments described below, the lithium salt has a significantly high lithium ion transference number, and thus can suppress dendrite formation more effectively.

[0244]

[0245] In addition, according to one embodiment of the present invention, X, Y and Z may each independently be one or two or more selected from the group consisting of the following chemical formulas a-1, b and c-1, and at least one of X, Y and Z may comprise chemical formula a-1. The compound including the repeating unit represented by the above chemical formula 1 and the lithium salt thereof are ion conductive polymers, and include a structure including an aromatic ring in which an alkoxy group is substituted at one carbon position of a benzene ring and an alkyl group substituted with a sulfonyl group is positioned on both sides of the ortho position, thereby having a lithium-friendly structure capable of chelating lithium ions. The present invention provides a compound having lithium ion conductivity capable of increasing the mobility of lithium ions through the lithium-friendly structure, and when the compound is used as a material of a solid electrolyte, it can have the effect of improving ion conductivity.

[0246]

[0247] Additionally, according to one embodiment of the present invention, R2 and R4 may be C1-C5 alkyl groups.

[0248] Additionally, according to one embodiment of the present invention, L1, L2 and L3 may be C1-C5 alkylene groups.

[0249] In addition, according to one embodiment of the present invention, X1 and X2 may each independently be a hydrogen element; or a halogen element, and the halogen element may be at least one selected from the group consisting of F, Cl, Br, and I. The compound including the repeating unit represented by the above chemical formula 1 and the lithium salt thereof may include an alkylene group substituted with a halogen element, and preferably, the halogen element may be fluorine. When the halogen element is fluorine, the anion of the neighboring sulfonimide may be delocalized by fluorine having high electronegativity, thereby reducing the electron density of the sulfonimide, and as a result, the electrostatic attraction between the lithium ion and the solid electrolyte may be alleviated. Accordingly, the dissociated lithium ion in the electrolyte can be moved with higher efficiency, and thus, compared to the existing alkylene oxide polymer, the polymer can have higher ionic conductivity, and when used in an all-solid-state battery, it can have electrochemical stability even at a high voltage.

[0250] In addition, according to one embodiment of the present invention, in the chemical formula 1, chemical formula a-1, b and c-1, n may be an integer from 1 to 20, q may be an integer from 1 to 20, o may be an integer from 1 to 20, m may be an integer from 1 to 10, and p may be an integer from 1 to 50.

[0251]

[0252] In addition, according to one embodiment of the present invention, the compound including the repeating unit represented by the chemical formula 1 may be represented by the following chemical formula 1-a or 1-b.

[0253] [Chemical Formula 1-a]

[0254]

[0255] [Chemical Formula 1-b]

[0256]

[0257] In the above chemical formulas 1-a and 1-b, n is an integer from 1 to 20, q is an integer from 1 to 20, and o is an integer from 1 to 20.

[0258] When the compound including the repeating unit represented by the above chemical formula 1 is represented by the above chemical formula 1-a or 1-b, it can have a higher lithium ion conductivity compared to the polymer material of the solid electrolyte used in the past.

[0259]

[0260] According to one embodiment of the present invention, at least one terminal portion among the terminal portions may include one or more functional groups selected from the group consisting of the following chemical formulae d to g.

[0261] [chemical formula d]

[0262]

[0263] [chemical formula e]

[0264]

[0265] [chemical formula f]

[0266]

[0267] [chemical formula g]

[0268]

[0269] In the above chemical formulas d to g,

[0270] The above R7 is a hydrogen atom; or a substituted or unsubstituted C1-C 10 is an alkyl group,

[0271] Above R8 to R 11 are each independently, direct bond; substituted or unsubstituted C1-C 10 alkylene group of; or -R 12 -OR 13 -and,

[0272] The above R 12 and R 13are each independently, directly bonded; or substituted or unsubstituted C1-C 10 is an alkylene group,

[0273] The above * indicates the binding position.

[0274] The compound can facilitate the formation of a network between repeating units in the compound by containing one or more functional groups selected from the group consisting of the chemical formulas d to g at least one of both terminals of the repeating unit, and the weight average molecular weight of the polymer can be greatly increased through the formation of the network, and thus, when the compound and its salt are applied to a solid electrolyte, the mechanical strength of the solid electrolyte can be improved.

[0275] In addition, according to one embodiment of the present invention, in the chemical formulas d to g, R7 is a C1-C6 alkyl group, and R8 to R 11 are each independently a direct bond; a C1-C6 alkylene group substituted or unsubstituted with a fluorine atom; or -R 12 -OR 13 - and the above R 12 and R 13 Each independently, may be a direct bond: or a C1-C6 alkylene group substituted or unsubstituted with a fluorine atom. Specifically, the functional groups of the above chemical formulas d to g may be at least one selected from the group consisting of acrylate, vinyl, isocyanate, and alcohol structures.

[0276] Meanwhile, in the process of polymerizing a compound included in the solid electrolyte of the present invention, in addition to the repeating unit represented by the above chemical formula 1 and the compound including at least one functional group selected from the group consisting of the following chemical formulas d to g at at least one of both terminals of the repeating unit and a lithium salt thereof, a crosslinking compound may be further included. The crosslinking compound may be at least one selected from the group consisting of a polyfunctional acrylate, a vinyl group, an isocyanate, and an alcohol structure.

[0277] For example, when a functional group of chemical formula d or chemical formula e having an acrylate or vinyl group structure is located at the end of the repeating unit, a network between the repeating units can be formed by adding a crosslinking compound containing pentaerythritol tetraacrylate (PETA). At this time, since the acrylate, vinyl group, and PETA contain a double bond structure, radical polymerization can be formed between the functional group of chemical formula d or chemical formula e and the double bond of the crosslinking compound.

[0278] In addition, for example, when the functional group of the chemical formula g having an alcohol structure (-OH) is located at the terminal of the repeating unit, a network between the repeating units can be formed by adding a crosslinking compound containing hexamethylene diisocyanate (1,6-diisocyanatohexane). In addition, when the functional group of the chemical formula f having an isocyanate structure (-NCO) is located at the terminal of the repeating unit, a network between the repeating units can be formed by adding a crosslinking compound containing glycerol or propane-1,2,3-tricarboxylic acid. At this time, the -OH group and the -NCO group can form a bond of the structure of -NHCOO- through an addition polymerization reaction.

[0279] Additionally, according to one embodiment of the present invention, the compound may be represented by the following chemical formula 1-c.

[0280] [Chemical Formula 1-c]

[0281]

[0282] In the above chemical formula 1-c, n is an integer from 1 to 20, q is an integer from 1 to 20, and o is an integer from 1 to 20.

[0283] Specifically, when the compound including the repeating unit represented by Chemical Formula 1 is represented by Chemical Formula 1-c, it can have higher lithium ion conductivity compared to the polymer material of the solid electrolyte used in the past.

[0284]

[0285] According to one embodiment of the present invention, the lithium salt of the compound including the repeating unit represented by the above chemical formula 1 may be a compound including the repeating unit represented by the following chemical formula 2.

[0286] [Chemical Formula 2]

[0287]

[0288] In the above chemical formula 2,

[0289] The above X, Y and Z are each independently at least one selected from the group consisting of the following chemical formulas a-1, b and c-1,

[0290] The above n is an integer from 1 to 100,

[0291] The above q is an integer from 1 to 100,

[0292] The above o is an integer from 0 to 100,

[0293] The above * is a connecting part between repeating units,

[0294] [Chemical formula a-1]

[0295]

[0296] [chemical formula b]

[0297]

[0298] [Chemical formula c-1]

[0299]

[0300] In the above chemical formulas a-1, b and c-1,

[0301] The above R1, R2 and R3 are each independently a hydrogen element; a halogen element; -CN; -NO2; substituted or unsubstituted C1-C 10 Alkyl group of; substituted or unsubstituted C1-C 10 Alkoxy group of; substituted or unsubstituted C2-C 10 Alkenyl group of; substituted or unsubstituted C2-C 10 an alkynyl group of; -C(=O)R5; -P(=O)(OR5)2; -P(OR5)(OR6); -OP(=O)(OR5)(OR6); -S(=O)R5; or -S(=O)2R5,

[0302] The above R4 is a hydrogen atom; or a substituted or unsubstituted C1-C 10 is an alkyl group,

[0303] The above R5 and R6 are each independently a hydrogen element; substituted or unsubstituted C1-C 10 an alkyl group of; or a substituted or unsubstituted C2-C 10 is an alkenyl group,

[0304] The above L1, L2 and L3 are each independently a direct bond; or a substituted or unsubstituted C1-C 10 is an alkylene group,

[0305] The above X1 and X2 are each independently a hydrogen element; a halogen element; -CN; -NO2; a substituted or unsubstituted C1-C 10 an alkyl group of; or a substituted or unsubstituted C6-C 12 is an aryl group,

[0306] The above m is an integer from 1 to 40,

[0307] The above p is an integer from 1 to 200.

[0308]

[0309] The compound including the repeating unit represented by the above chemical formula 2 is a lithiated compound including the repeating unit represented by the above chemical formula 1, and can have the effect of improving the lithium ion transference number.

[0310]

[0311] In addition, according to one embodiment of the present invention, the compound including the repeating unit represented by the chemical formula 2 may be a compound represented by the following chemical formula 2-a or 2-b.

[0312] [Chemical Formula 2-a]

[0313]

[0314] [Chemical Formula 2-b]

[0315]

[0316] In the above chemical formulas 2-a and 2-b, n is an integer from 1 to 20, q is an integer from 1 to 20, and o is an integer from 1 to 20.

[0317] When the compound including the repeating unit represented by the above chemical formula 2 is represented by the above chemical formula 2-a or 2-b, it can have a higher lithium ion conductivity compared to the polymer material of the solid electrolyte used in the past.

[0318]

[0319] According to one embodiment of the present invention, the lithium salt compound may include at least one functional group selected from the group consisting of the following chemical formulas d to g at at least one terminal portion among the terminal portions.

[0320] [chemical formula d]

[0321]

[0322] [chemical formula e]

[0323]

[0324] [chemical formula f]

[0325]

[0326] [chemical formula g]

[0327]

[0328] In the above chemical formulas d to g,

[0329] The above R7 is a hydrogen atom; or a substituted or unsubstituted C1-C 10 is an alkyl group,

[0330] Above R8 to R 11 are each independently, direct bond; substituted or unsubstituted C1-C 10 alkylene group of; or -R 12 -OR 13 -and,

[0331] The above R 12 and R 13 are each independently, directly bonded; or substituted or unsubstituted C1-C 10 is an alkylene group,

[0332] The above * indicates the binding position.

[0333]

[0334] In addition, according to one embodiment of the present invention, the compound including the repeating unit represented by the above chemical formula 2 may be represented by the following chemical formula 2-c.

[0335] [Chemical Formula 2-c]

[0336]

[0337] In the above chemical formula 2-c, n is an integer from 1 to 20, q is an integer from 1 to 20, and o is an integer from 1 to 20.

[0338] Specifically, when the compound including the repeating unit represented by Chemical Formula 2 is represented by Chemical Formula 2-c, it can have a higher lithium ion conductivity than the polymer material of the solid electrolyte used in the past.

[0339]

[0340] complex

[0341] The present invention provides a compound according to the present invention; and a complex comprising a lithium compound.

[0342] Specifically, the present invention provides a compound according to at least one selected from the group consisting of a compound of the above chemical formula 1 and a lithium salt thereof; and a complex comprising a lithium compound.

[0343] The above complex may be a complex including a repeating unit represented by the following chemical formula 3 or a repeating unit represented by the following chemical formula 4.

[0344] [Chemical Formula 3]

[0345]

[0346] [Chemical Formula 4]

[0347] In the above chemical formulas 3 and 4,

[0348] The above X, Y and Z are each independently at least one selected from the group consisting of the following chemical formulas a-2, b, c-1 and c-2, and at least one of the above X, Y and Z must include chemical formula a-2 or c-2.

[0349] The above n is an integer from 1 to 100,

[0350] The above q is an integer from 1 to 100,

[0351] The above o is an integer from 0 to 100,

[0352] The above * is a connecting part between repeating units,

[0353] [Chemical formula a-2]

[0354]

[0355] [chemical formula b]

[0356]

[0357] [Chemical formula c-1]

[0358]

[0359] [Chemical formula c-2]

[0360]

[0361] In the above chemical formulas a-2, b, c-1 and c-2,

[0362] The above R1, R2 and R3 are each independently a hydrogen element; a halogen element; -CN; -NO2; substituted or unsubstituted C1-C 10 Alkyl group of; substituted or unsubstituted C1-C 10 Alkoxy group of; substituted or unsubstituted C2-C 10 Alkenyl group of; substituted or unsubstituted C2-C 10 an alkynyl group of; -C(=O)R5; -P(=O)(OR5)2; -P(OR5)(OR6); -OP(=O)(OR5)(OR6); -S(=O)R5; or -S(=O)2R5,

[0363] The above R4 is a hydrogen atom; or a substituted or unsubstituted C1-C 10 is an alkyl group,

[0364] The above R5 and R6 are each independently a hydrogen element; substituted or unsubstituted C1-C 10 an alkyl group of; or a substituted or unsubstituted C2-C 10 is an alkenyl group,

[0365] The above L1, L2 and L3 are each independently a direct bond; or a substituted or unsubstituted C1-C 10 is an alkylene group,

[0366] The above X1 and X2 are each independently a hydrogen element; a halogen element; -CN; -NO2; a substituted or unsubstituted C1-C 10 an alkyl group of; or a substituted or unsubstituted C6-C 12 is an aryl group,

[0367] A above - is a halogen anion, BF4 - , ClO4 - , AlCl4 - , AlO4 - , PF6 - , CF3SO3 - , CH3CO2 - , CF3CO2 - , AsF6 - , SbF6 - , CH3SO3 - , FSI - (bis(fluorosulfonyl)imide, N(SO2F)2 - ), BETI (lithium bisperfluoroethanesulfonimide, N(SO2CF2CF3)2 - ) and TFSI ((bis)trifluoromethanesulfonimide, N(SO2CF3)2 - ) is one or more selected from the group consisting of,

[0368] The above m is an integer from 1 to 40,

[0369] The above p is an integer from 1 to 200.

[0370]

[0371] According to one embodiment of the present invention, the complex including the repeating unit represented by the chemical formula 3 or the repeating unit represented by the chemical formula 4 may include at least one of the compound including the repeating unit represented by the chemical formula 1 or a lithium salt thereof and a lithium compound, and at least one of the compound including the repeating unit represented by the chemical formula 1 or a lithium salt thereof and the lithium compound are bonded by electrostatic attraction. The complex of the present invention can increase the transport rate of lithium ions by further including the lithium compound, thereby improving ion conductivity and achieving the effect of reducing the diffusion resistance of lithium ions, thereby implementing the effect of improving the cycle capacity characteristics of a lithium secondary battery.

[0372]

[0373] According to one embodiment of the present invention, X, Y and Z are each independently one or more selected from the group consisting of the following chemical formulas a-2, b, c-1 and c-2, and at least one of X, Y and Z may necessarily include chemical formula a-2 or c-2. L1, L2 and L3 may be a C1-C5 alkylene group, X1 to X4 may each independently be a hydrogen element; or a halogen element, and the halogen element may be one or more selected from the group consisting of F, Cl, Br and I. In addition, n is an integer from 1 to 20, q is an integer from 1 to 20, o is an integer from 1 to 20, m is an integer from 1 to 10, and p may be an integer from 1 to 50. The effect according to the definition of the substituent is the same as the effect of the compound including the repeating unit represented by the chemical formula 1 described above and the lithium salt thereof.

[0374]

[0375] The above lithium compound is Li + Y - can be expressed as . The anion (Y) of the above lithium compound- ) is a halogen anion, BF4 - , ClO4 - , AlCl4 - , AlO4 - , PF6 - , CF3SO3 - , CH3CO2 - , CF3CO2 - , AsF6 - , SbF6 - , CH3SO3 - , FSI - (bis(fluorosulfonyl)imide, N(SO2F)2 - ), BETI (lithium bisperfluoroethanesulfonimide, N(SO2CF2CF3)2 - ) and TFSI ((bis)trifluoromethanesulfonimide, N(SO2CF3)2 - ) may be one or more selected from the group consisting of, and specifically, the anion (Y) of the lithium compound - ) may be a halogen anion.

[0376] According to one embodiment of the present invention, the R2 and R4 may be C1-C5 alkyl groups. When R4 in the structure of the chemical formula 3 or 4 is substituted with a C1-C5 alkyl group and the complex contains an alkoxy group, the lithium compound may be positioned close to the alkoxy group by electrostatic attraction, and specifically, the lithium compound may be Li + Y - can be located in the form of

[0377] Additionally, the lithium compound included in the complex may be included in an amount of 1 to 40 wt% within the complex. By including the lithium compound in the above range, the complex can increase the lithium ion transport rate and reduce battery resistance, thereby realizing an effect of improving cycle capacity characteristics.

[0378]

[0379] According to one embodiment of the present invention, the complex may include at least one functional group selected from the group consisting of the following chemical formulae d to g at at least one terminal portion among the terminal portions.

[0380] [chemical formula d]

[0381]

[0382] [chemical formula e]

[0383]

[0384] [chemical formula f]

[0385]

[0386] [chemical formula g]

[0387]

[0388] In the above chemical formulas d to g,

[0389] The above R7 is a hydrogen atom; or a substituted or unsubstituted C1-C 10 is an alkyl group,

[0390] Above R8 to R 11 are each independently, direct bond; substituted or unsubstituted C1-C 10 alkylene group of; or -R 12 -OR 13 -and,

[0391] The above R 12 and R 13 are each independently, directly bonded; or substituted or unsubstituted C1-C 10 is an alkylene group,

[0392] The above * indicates the binding position.

[0393]

[0394] According to one embodiment of the present invention, the complex may be a complex represented by at least one selected from the group consisting of the following chemical formulas 3-a, 4-a and 4-b.

[0395] [Chemical Formula 3-a]

[0396]

[0397] [Chemical Formula 4-a]

[0398]

[0399] [Chemical Formula 4-b]

[0400]

[0401]

[0402] In the above chemical formulas 3-a, 4-a and 4-b, n is an integer from 1 to 20, q is an integer from 1 to 20, and o is an integer from 1 to 20.

[0403] When the complex including the repeating unit represented by the above chemical formula 3 or the repeating unit represented by the above chemical formula 4 is a complex represented by at least one selected from the group consisting of the above chemical formulas 3-a, 4-a, and 4-b, it can have a higher lithium ion conductivity compared to the polymer material of the solid electrolyte previously used.

[0404]

[0405] compound (monomer)

[0406] The present invention provides a compound represented by the following chemical formula A.

[0407] [Chemical Formula A]

[0408]

[0409] In the above chemical formula A,

[0410] The above R 21 , R 22 and R 23 are each independently a hydrogen element; a halogen element; a substituted or unsubstituted C1-C 10 Alkyl group of; substituted or unsubstituted C1-C 10 Alkoxy group of; substituted or unsubstituted C2-C 10an alkenyl group of; or a substituted or unsubstituted C2-C 10 is an alkynyl group,

[0411] The above R 24 is a hydrogen element; or substituted or unsubstituted C1-C 10 is an alkyl group,

[0412] Above L 21 and L 22 are each independently substituted or unsubstituted C1-C 10 alkylene group of; -P(=O)(OR 25 )-; -(C=O)-; -(S=O)-; or -S(=O)2-,

[0413] Above X 21 and X 22 are each independently a halogen element; -NH2; phosphate (-OP(=O)(OR 25 )2); Nitrate(-ON(=O)(OR 25 )); tosylate (-OTs); sulfonate (-OS(=O)2R 25 ); or carboxylate (-OC(=O)CH3),

[0414] The above R 25 is substituted or unsubstituted C1-C 10 Alkyl group of; substituted or unsubstituted C2-C 10 an alkenyl group of; or a substituted or unsubstituted C2-C 10 is an alkynyl group.

[0415]

[0416] The compound represented by the above chemical formula A may be a monomer. The compound represented by the above chemical formula A may be an aromatic ring substance in which an alkoxy group is substituted at one carbon position in a benzene ring and an alkyl group substituted with a sulfonyl group is positioned at both sides of the ortho position. The compound is a target substance based on the structure-specific interaction between molecules based on the structural characteristics capable of chelating lithium ions, like a crown ether compound to which the molecular recognition concept of supramolecular chemistry is applied. + The present invention provides a compound having lithium ion conductivity that can increase the mobility of lithium ions (lithium ion transport rate) through the lithium-friendly structure, and when the compound is used as a material for a solid electrolyte, it can have the effect of improving ion conductivity.

[0417]

[0418] According to one embodiment of the present invention, in the chemical formula A, the R 22 , R 24 and R 25 may be an alkyl group of C1-C5.

[0419] According to one embodiment of the present invention, in the chemical formula A, the X 21 and X 22 Each independently may be a halogen element or -NH2. The compound represented by the above chemical formula A can form an ion-conducting polymer as a monomer, and when the compound represented by the above chemical formula A contains a halogen element, for example, at least one of F, Cl, I, and Br, or NH2, a condensation reaction may proceed between the halogen element and NH2 to form the ion-conducting polymer.

[0420] According to one embodiment of the present invention, in the chemical formula A, the L 21 and L 22 can be -S(=O)2-. Specifically, the compound represented by the above chemical formula A is the L 21 and L 22 Contains a sulfonyl group, and the above X 21 and X 22 When containing -NH2, the compound represented by the above chemical formula A contains an anion of sulfonimide or sulfonimide in which a proton bonded to a nitrogen atom in sulfonimide is detached, so when used as a material for a solid electrolyte, it may have high affinity for lithium ions. Meanwhile, in a process for manufacturing a solid electrolyte including a compound including a repeating unit represented by the above chemical formula A, a proton bonded to a nitrogen atom in sulfonimide may be detached. In addition, in this case, the anion of sulfonimide has a relatively low electron density compared to anions of other organic groups such as carboxylate, so that the electrostatic attraction with lithium ions becomes weak, and thus the transport efficiency of lithium ions, i.e., ion conductivity, may be improved. In addition, when the compound represented by the above chemical formula A contains an alkoxy group, the oxygen of the alkoxy group can chelate to lithium together with two sulfonyl groups adjacent to the ortho position, thereby improving lithium affinity, and as a result, it can have the effect of improving the lithium ion conductivity of a solid electrolyte using this material. In particular, the lithium salt can have the effect of improving the lithium ion transference number compared to a material obtained by hydrogenating an existing ethylene oxide-based material or a material obtained by mixing lithium salts separately, for example, a PEO mixture mixed with lithium salts.

[0421]

[0422] In addition, according to one embodiment of the present invention, the compound represented by the chemical formula A may be a compound selected from the group consisting of the following chemical formulas Aa, Ab, and Ac.

[0423] [Chemical formula Aa]

[0424]

[0425] [Chemical formula Ab]

[0426]

[0427] [Chemical formula Ac]

[0428]

[0429] When the compound represented by the above chemical formula A is at least one selected from the group consisting of the above chemical formulas Aa, Ab, and Ac, it can have a higher lithium ion conductivity compared to the polymer material of the solid electrolyte previously used.

[0430]

[0431] complex (monomer)

[0432] The present invention provides a composite comprising a compound represented by the above chemical formula A and a lithium compound. The composite of the present invention can increase the transport rate of lithium ions by further including the lithium compound, thereby improving ion conductivity and achieving the effect of reducing the diffusion resistance of lithium ions, thereby achieving the effect of improving the cycle capacity characteristics of a lithium secondary battery.

[0433] According to one embodiment of the present invention, the complex may be a complex represented by the following chemical formula B. In the complex represented by the chemical formula B, the compound represented by the chemical formula A and the lithium compound are bonded by electrostatic attraction.

[0434] [Chemical Formula B]

[0435]

[0436] In the above chemical formula B,

[0437] The above R 21 , R 22 and R 23 are each independently a hydrogen element; a halogen element; a substituted or unsubstituted C1-C 10 Alkyl group of; substituted or unsubstituted C1-C 10 Alkoxy group of; substituted or unsubstituted C2-C 10 an alkenyl group of; or a substituted or unsubstituted C2-C 10 is an alkynyl group,

[0438] The above R 24 is a hydrogen element; or substituted or unsubstituted C1-C 10 is an alkyl group,

[0439] Above L 21 and L 22 are each independently substituted or unsubstituted C1-C 10 alkylene group of; -P(=O)(OR 25 )-; -(C=O)-; -(S=O)-; or -S(=O)2-,

[0440] Above X 21 and X 22 are each independently a halogen element; -NH2; phosphate (-OP(=O)(OR 25 )2); Nitrate(-ON(=O)(OR 25 )); tosylate (-OTs); sulfonate (-OS(=O)2R 25 ); or carboxylate (-OC(=O)CH3),

[0441] The above R 25 is substituted or unsubstituted C1-C 10 Alkyl group of; substituted or unsubstituted C2-C 10 an alkenyl group of; or a substituted or unsubstituted C2-C 10 is an alkynyl group,

[0442] Above Y - is a halogen anion, BF4 - , ClO4 - , AlCl4- , AlO4 - , PF6 - , CF3SO3 - , CH3CO2 - , CF3CO2 - , AsF6 - , SbF6 - , CH3SO3 - , FSI - (bis(fluorosulfonyl)imide, N(SO2F)2 - ), BETI (lithium bisperfluoroethanesulfonimide, N(SO2CF2CF3)2 - ) and TFSI ((bis)trifluoromethanesulfonimide, N(SO2CF3)2 - ) is one or more selected from the group consisting of.

[0443] According to one embodiment of the present invention, in the chemical formula B, the R 22 , R 24 and R 25 may be a C1-C5 alkyl group. In addition, in the above chemical formula B, the L 21 and L 22 can be -S(=O)2-, and the above X 21 and X 22 Each independently may be a halogen element or -NH2. The halogen element may be any one of F, Cl, I, and Br. The effect according to the definition of the substituent is the same as the effect of the compound represented by the above chemical formula A.

[0444] The above lithium compound is Li + Y - can be expressed as . The anion (Y) of the above lithium compound - ) is a halogen anion, BF4 - , ClO4 - , AlCl4 - , AlO4 - , PF6 - , CF3SO3 -, CH3CO2 - , CF3CO2 - , AsF6 - , SbF6 - , CH3SO3 - , FSI - (bis(fluorosulfonyl)imide, N(SO2F)2 - ), BETI (lithium bisperfluoroethanesulfonimide, N(SO2CF2CF3)2 - ) and TFSI ((bis)trifluoromethanesulfonimide, N(SO2CF3)2 - ) may be one or more selected from the group consisting of, and specifically, the anion (Y) of the lithium compound - ) may be a halogen anion.

[0445] According to one embodiment of the present invention, in the structure of the chemical formula B, R 24 When the complex contains an alkoxy group by being substituted with an alkyl group, the lithium compound can be positioned close to the alkoxy group by electrostatic attraction, and specifically, the lithium compound is Li + Y - can be located in the form of

[0446] In addition, the lithium compound included in the complex may be included in an amount of 1 to 75 wt% within the complex. When the lithium compound is included in an amount within the above range, 1 to 4 mol of lithium cations may be present per mol of the complex, thereby increasing the lithium ion transport rate and reducing the diffusion resistance of lithium ions, thereby realizing an effect of improving cycle capacity characteristics.

[0447]

[0448] According to one embodiment of the present invention, the complex may be a complex selected from the group consisting of the following chemical formulas Ba, Bb and Bc.

[0449] [chemical formula Ba]

[0450]

[0451] [chemical formula Bb]

[0452]

[0453] [Chemical formula Bc]

[0454]

[0455] When the complex represented by the above chemical formula B is a complex selected from the group consisting of the above chemical formulas Ba, Bb and Bc, it can have a higher lithium ion conductivity compared to the polymer material of the solid electrolyte used in the past.

[0456]

[0457] polymer

[0458] The present invention provides a polymer comprising a repeating unit derived from a compound represented by the above chemical formula A, a repeating unit derived from a complex represented by the above chemical formula B, or a combination thereof.

[0459] According to one embodiment of the present invention, the compound and the complex may be monomers, and the monomers may be polymerized to form a polymer, which is a solid electrolyte material having ion conductivity. Specifically, the compound represented by the chemical formula A and the complex represented by the chemical formula B may be X 21 and X 22 The position may contain a halogen element or -NH2, and for example, the halogen element may be at least one of F, Cl, I, and Br. In this case, the compound represented by the chemical formula A and the complex represented by the chemical formula B may undergo polymerization by a condensation reaction between the contained halogen element and the -NH2, thereby forming a polymer including sulfonylimide.

[0460] Additionally, according to one embodiment of the present invention, the polymer may further include at least one repeating unit derived from a fluorine-based and alkylene oxide monomer in addition to the repeating unit derived from the compound and complex.

[0461] According to one embodiment of the present invention, the repeating unit derived from the compound may be represented by the following chemical formula Wa or Wb.

[0462] [chemical formula Wa]

[0463]

[0464] [Chemical formula Wb]

[0465]

[0466] In the above chemical formulas Wa and Wb,

[0467] wherein n is an integer from 1 to 300,

[0468] The above * indicates a connection between repeating units.

[0469] The above chemical formula Wb is a repeating unit derived from a lithium salt of a compound represented by the above chemical formula A, and a compound including the above repeating unit can have an effect of further improving the lithium ion transference number.

[0470]

[0471] Additionally, according to one embodiment of the present invention, the repeating unit derived from the complex may be represented by the following chemical formula Xa or Xb.

[0472] [chemical formula Xa]

[0473]

[0474] [chemical formula Xb]

[0475]

[0476] In the above chemical formulas Xa and Xb,

[0477] Above Y - is a halogen anion, BF4 - , ClO4 - , AlCl4 - , AlO4 - , PF6 - , CF3SO3 - , CH3CO2 - , CF3CO2 - , AsF6 - , SbF6 - , CH3SO3 - , FSI - (bis(fluorosulfonyl)imide, N(SO2F)2 - ), BETI (lithium bisperfluoroethanesulfonimide, N(SO2CF2CF3)2 - ) and TFSI ((bis)trifluoromethanesulfonimide, N(SO2CF3)2 - ) is one or more selected from the group consisting of,

[0478] The above n is an integer from 1 to 300,

[0479] The above * indicates a connection between repeating units.

[0480] The above chemical formula Xb may have the effect of further improving the lithium ion transference number of a solid electrolyte by including a lithiated compound.

[0481]

[0482] Additionally, according to one embodiment of the present invention, the combination of the repeating unit derived from the compound and the repeating unit derived from the complex may be represented by the following chemical formula Y or Z.

[0483] [Chemical formula Y]

[0484]

[0485] [Chemical formula Z]

[0486]

[0487] In the above chemical formulas Y and Z,

[0488] Above Y - is a halogen anion, BF4 - , ClO4 - , AlCl4 - , AlO4 - , PF6 - , CF3SO3 - , CH3CO2 - , CF3CO2 - , AsF6 - , SbF6 - , CH3SO3 - , FSI - (bis(fluorosulfonyl)imide, N(SO2F)2 - ), BETI (lithium bisperfluoroethanesulfonimide, N(SO2CF2CF3)2 - ) and TFSI ((bis)trifluoromethanesulfonimide, N(SO2CF3)2 - ) is one or more selected from the group consisting of,

[0489] The above n and m are each independently an integer from 1 to 300,

[0490] The above * indicates a connection between repeating units.

[0491] The above chemical formula Z may have the effect of further improving the lithium ion transference number of a solid electrolyte by including a lithiated compound.

[0492]

[0493] solid electrolyte

[0494] The present invention provides a solid electrolyte comprising at least one selected from the group consisting of the compound and the complex. Specifically, the compound may be a compound comprising a repeating unit represented by the chemical formula 1 or a repeating unit represented by the chemical formula 2, and the complex may be a complex comprising a repeating unit represented by the chemical formula 3 or 4. In addition, the present invention provides a solid electrolyte comprising the polymer. Here, the polymer may comprise a repeating unit derived from a compound represented by the chemical formula A, a repeating unit derived from the complex, or a combination thereof. Since the solid electrolyte comprises a polymer comprising a lithium ion-friendly structure, it may have the effect of improving lithium ion mobility and thus improving ion conductivity.

[0495]

[0496] According to one embodiment of the present invention, the solid electrolyte may further include a crosslinking compound, and the crosslinking compound may be at least one selected from the group consisting of polyfunctional acrylates, vinyl groups, isocyanates, and alcohol structures. At least one functional group selected from the group consisting of the following chemical formulas d to g at at least one terminal of the repeating unit and the crosslinking compound may form a network between repeating units through radical polymerization or addition polymerization. The content regarding the crosslinking compound is the same as that described under the table of contents of compounds.

[0497]

[0498] Meanwhile, the present invention can prepare a mixed solution by mixing at least one selected from the group consisting of a solvent and the compound and the complex, and form an ion conductive polymer electrolyte film through a film manufacturing process using the mixed solution. The solvent can be at least one selected from the group consisting of methanol, ethanol, 2-propanol, butanol, 2-ethoxyethanol, isopropyl alcohol, ethyl acetate, butyl acetate, acetone, dichloroethane, acetonitrile, tetrahydrofuran, N-methyl-2-pyrrolidone, N,N-dimethylformamide, N,N-diethylformamide, N,N-dimethylacetamide, dimethylsulfoxide, hexamethylphosphamide, 1,3-dimethyl-2-imidazolidinone, triethyl phosphate, and gamma-butyrolactone. The content of the above solvent can be determined by considering the viscosity of the mixed solution, etc.

[0499]

[0500] In addition, the film manufacturing process may be a solution casting method (solution casting method), a melt extrusion method, a calendar method, or a compression molding method, and more specifically, may be a solution casting method. The solution casting method may be performed by coating on a separate substrate, separating it, and then laminating it with the positive and negative electrodes. The substrate may be a glass substrate or a plastic substrate. Examples of the plastic substrate include various plastic films such as polyethylene terephthalate, polyethylene naphthalate, polypropylene, polyethylene, cellulose triacetate, cellulose diacetate, poly(meth)acrylic acid alkyl ester, poly(meth)acrylic acid ester copolymer, polyvinyl chloride, polyvinyl alcohol, polycarbonate, polystyrene, cellophane, polyvinylidene chloride copolymer, polyamide, polyimide, vinyl chloride / vinyl acetate copolymer, polytetrafluoroethylene, and polytrifluoroethylene. The thickness of the support is preferably 5 to 150 μm, more preferably 10 to 50 μm. In addition, the coating may be applied by any of the following methods: spin coating, dip coating, solvent casting, slot die coating, spray coating, roll coating, extrusion coating, curtain coating, die coating, wire bar coating, or knife coating.

[0501]

[0502] All-solid-state battery

[0503] The present invention provides an all-solid-state battery comprising the above solid electrolyte.

[0504] According to one embodiment of the present invention, the all-solid-state battery includes a positive electrode, a negative electrode (or anode-less), and a solid electrolyte layer including a solid electrolyte disposed between the positive electrode and the negative electrode. The all-solid-state battery according to the present invention has a small decrease in ionic conductivity, and the electronic conductivity of the included solid electrolyte is low, so that the initial efficiency, life characteristics, and output characteristics of the all-solid-state battery can be excellent. At this time, the all-solid-state battery of the present invention can be manufactured according to a conventional method known in the art. For example, it can be manufactured by laminating and pressing so that the solid electrolyte layer is present between the positive electrode and the negative electrode.

[0505]

[0506] (1) Bipolar

[0507] The above positive electrode can be manufactured by coating a positive electrode slurry containing a positive electrode active material, a binder, a conductive agent, a solvent, etc. on a positive electrode current collector.

[0508] The positive electrode current collector is not particularly limited as long as it is conductive and does not cause a chemical change in the battery. For example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the bonding strength of the positive electrode active material may be strengthened by forming fine irregularities on the surface, and may be used in various forms such as a film, sheet, foil, net, porous body, foam, or non-woven fabric.

[0509]

[0510] The above-mentioned positive electrode active material is a compound capable of reversible intercalation and deintercalation of lithium, and specifically may include a lithium metal oxide containing lithium and one or more metals such as cobalt, manganese, nickel or aluminum. More specifically, the lithium metal oxide may be a lithium-manganese oxide (e.g., LiMnO2, LiMn2O4, etc.), a lithium-cobalt oxide (e.g., LiCoO2, etc.), a lithium-nickel oxide (e.g., LiNiO2, etc.), a lithium-nickel-manganese oxide (e.g., LiNi 1-Y Mn Y O2 (here, 0 <Y<1), LiMn 2-z Ni z O4 (where 0<Z<2), etc.), lithium-nickel-cobalt oxides (e.g., LiNi 1-Y1 Co Y1 O2 (here, 0 <Y1<1) 등), 리튬-망간-코발트계 산화물(예를 들면, LiCo 1-Y2 Mn Y2 O2 (here, 0 <Y2<1), LiMn 2-z1 Co z1 O4 (wherein, 0<Z1<2) etc.), lithium-nickel-manganese-cobalt oxides (e.g., Li(Ni p Co q Mn r1 )O2(wherein, 0<p<1, 0<q<1, 0<r1<1, p+q+r1=1) or Li(Ni p1 Co q1 Mn r2 )O4 (wherein, 0<p1<2, 0<q1<2, 0<r2<2, p1+q1+r2=2) etc.), or lithium-nickel-cobalt-transition metal (M) oxide (e.g., Li(Ni p2 Co q2 Mn r3 M S2)O2 (wherein, M is selected from the group consisting of Al, Fe, V, Cr, Ti, Ta, Mg and Mo, and p2, q2, r3 and s2 are atomic fractions of independent elements, respectively, 0<p2<1, 0<q2<1, 0<r3<1, 0<s2<1, p2+q2+r3+s2=1), etc.), and one or more compounds of these may be included.

[0511] Among these, the lithium metal oxides are LiCoO2, LiMnO2, LiNiO2, lithium nickel manganese cobalt oxide (e.g., Li(Ni)) in that they can improve the capacity characteristics and stability of the battery. 1 / 3 Mn 1 / 3 Co 1 / 3 )O2, Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, Li(Ni) 0.5 Mn 0.3 Co 0.2 )O2, Li(Ni 0.7 Mn 0.15 Co 0.15 )O2 and Li(Ni 0.8 Mn 0.1 Co 0.1 )O2, etc.), or lithium nickel cobalt aluminum oxide (e.g., Li(Ni 0.8 Co 0.15 Al 0.05 )O2, etc.), and considering the remarkable improvement effect according to the control of the type and content ratio of the constituent elements forming the lithium composite metal oxide, the lithium composite metal oxide may be Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, Li(Ni) 0.5 Mn 0.3 Co 0.2 )O2, Li(Ni 0.7 Mn 0.15 Co 0.15 )O2 and Li(Ni 0.8 Mn 0.1 Co 0.1)O2, etc., and any one of these or a mixture of two or more of them may be used.

[0512] The above positive electrode active material may be included in an amount of 60 wt% or more, 70 wt% or more, 80 wt% or more, or 99 wt% or less, or 98 wt% or less, based on the total weight of the solid content excluding the solvent in the positive electrode slurry.

[0513] The above binder is a component that assists in bonding between the conductive material, the active material, and the current collector. Examples of such binders include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose, starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer, sulfonated ethylene-propylene-diene monomer, styrene-butadiene rubber, fluororubber, and various copolymers thereof.

[0514] Typically, the binder may be included in an amount of 1 wt% to 20 wt%, preferably 1 wt% to 15 wt%, and more preferably 1 wt% to 10 wt%, based on the total weight of solids excluding the solvent in the positive electrode slurry.

[0515] The above-mentioned conductive agent is a component for further improving the conductivity of the positive electrode active material.

[0516] The conductive material is not particularly limited as long as it is conductive and does not cause a chemical change in the battery, and for example, carbon-based materials such as graphite; carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers or metal fibers; metal powders such as fluorinated carbon, aluminum, and nickel powders; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives can be used.

[0517] Typically, the conductive material may be included in an amount of 1 wt% or more, 20 wt% or less, 15 wt% or less, or 10 wt% or less based on the total weight of solids excluding the solvent in the positive electrode slurry.

[0518] The solvent may include an organic solvent such as NMP (N-methyl-2-pyrrolidone), and may be used in an amount that provides a desirable viscosity when including the positive electrode active material, and optionally a binder and a conductive material. For example, the concentration of the solid content including the positive electrode active material, and optionally a binder and a conductive material may be 50 wt% or more, 60 wt% or more, 70 wt% or more, 95 wt% or less, 90 wt% or less, and 85 wt% or less.

[0519]

[0520] (2) Cathode

[0521] The above negative electrode can be manufactured, for example, by coating a negative electrode slurry containing a negative electrode active material, a binder, a conductive material, and a solvent on a negative electrode current collector, or a graphite electrode made of carbon (C) or lithium metal itself having a thickness of 50 μm or less can be used as the negative electrode, or the negative electrode can be excluded as an anode-less electrode.

[0522] For example, when manufacturing a negative electrode by coating a negative electrode slurry on the negative electrode current collector, the negative electrode current collector generally has a thickness of 3 to 500 ㎛. The negative electrode current collector is not particularly limited as long as it has high conductivity without causing a chemical change in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. can be used. In addition, like the positive electrode current collector, the bonding strength of the negative electrode active material can be strengthened by forming fine unevenness on the surface, and can be used in various forms such as a film, sheet, foil, net, porous body, foam, non-woven fabric, etc.

[0523] The above negative active materials include natural graphite, artificial graphite, carbonaceous materials; lithium-containing titanium composite oxide (LTO), Si, SiO x , Sn, Li, Zn, Mg, Cd, Ce, Ni or Fe; alloys composed of the above metals (Me); oxides (MeO) of the above metals (Me) x ); and one or more types of negative electrode active materials selected from the group consisting of complexes of the above metals (Me) and carbon. Specifically, the negative electrode active materials include silicon (Si), silicon oxide (SiO x ) or a silicon-based negative electrode active material or lithium metal including a silicon alloy, etc. can be used. In the case of a silicon-based negative electrode active material, a thin and stable SEI layer including a siloxane bond is formed, which can further improve the high-temperature stability and lifespan characteristics of the battery.

[0524] In addition, in the case of the lithium metal, it may be a conventional one including lithium metal or a lithium alloy (for example, an alloy of lithium with a metal such as aluminum, zinc, bismuth, cadmium, antimony, silicon, lead, tin, gallium, or indium). The lithium metal negative electrode active material may be in the form of a foil, and by depositing the lithium metal negative electrode active material on one surface of the negative electrode current collector, the lithium metal negative electrode active material may form a separate layer from the negative electrode current collector.

[0525] The above negative electrode active material may be included in an amount of 60 wt% or more, 70 wt% or more, 80 wt% or more, 99 wt% or less, or 98 wt% or less based on the total weight of solids excluding the solvent in the negative electrode slurry.

[0526] The above binder is a component that assists in bonding between the conductive material, the active material, and the current collector. Examples of such binders include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose, starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer, sulfonated ethylene-propylene-diene monomer, styrene-butadiene rubber, fluororubber, and various copolymers thereof.

[0527] Typically, the binder may be included in an amount of 1 wt% or more, 20 wt% or less, 15 wt% or less, or 10 wt% or less based on the total weight of solids excluding the solvent in the slurry for the negative electrode.

[0528] The above conductive agent is a component for further improving the conductivity of the negative electrode active material. The conductive agent is not particularly limited as long as it has conductivity without causing a chemical change in the battery, and examples thereof include graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, Ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fiber or metal fiber; metal powders such as fluorocarbon, aluminum, and nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.

[0529] The above-mentioned conductive agent may be included in an amount of 1 wt% or more, 20 wt% or less, 15 wt% or less, or 10 wt% or less based on the total weight of solids excluding the solvent in the negative electrode slurry.

[0530] The solvent may include water or an organic solvent such as NMP (N-methyl-2-pyrrolidone), and may be used in an amount that provides a desirable viscosity when including the negative electrode active material, and optionally a binder and a conductive material. For example, the concentration of the solid content including the negative electrode active material, and optionally a binder and a conductive material may be 50 wt% or more, 60 wt% or more, 70 wt% or more, 95 wt% or less, 90 wt% or less, or 85 wt% or less.

[0531] When using the metal itself as the above-mentioned cathode, it can be manufactured by physically bonding, rolling, or depositing the metal onto the metal thin film itself or the cathode current collector. The deposition method can use an electrical deposition method or a chemical vapor deposition method.

[0532] For example, the metal film itself or the metal bonded / rolled / deposited on the negative electrode current collector may include one or more metals selected from the group consisting of lithium (Li), nickel (Ni), tin (Sn), copper (Cu), and indium (In), or an alloy of two metals.

[0533]

[0534] (3) Solid electrolyte layer

[0535] The solid electrolyte layer may further include a binder in addition to the solid electrolyte comprising the compound according to the present invention.

[0536] The above binder is a component that assists in the bonding between solid electrolyte particles. Examples of such binders include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose, starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer, sulfonated ethylene-propylene-diene monomer, styrene-butadiene rubber, fluororubber, and various copolymers thereof.

[0537] The above binder may be included in an amount of 0.1 wt% or more, 5 wt% or less, 3 wt% or less, or 2 wt% or less based on the total weight of the solid electrolyte layer.

[0538]

[0539] The present invention provides a battery module including the above-described all-solid-state battery as a unit cell and a battery pack including the same. The battery module and battery pack include the above-described secondary battery having high capacity, high rate characteristics, and cycle characteristics, and thus can be used as a power source for medium- to large-sized devices selected from the group consisting of electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, and power storage systems.

[0540]

[0541] Hereinafter, embodiments of the present invention will be described in detail so that those skilled in the art can easily implement the invention. However, the present invention may be implemented in various different forms, and the following embodiments are merely illustrative examples to aid understanding of the present invention and do not limit the scope of the present invention. It will be apparent to those skilled in the art that various changes and modifications are possible within the scope and technical idea of ​​the present disclosure, and it is natural that such modifications and variations fall within the claims of this specification.

[0542]

[0543] Synthesis example 1.

[0544] Preparation of a compound represented by chemical formula a-1-1

[0545] A solution containing 1 equivalent of 4-methylanisole, 1.3 equivalents of p-formaldehyde, and 50 equivalents of HCl (6N aqueous solution) was stirred and heated at 80°C for 5 hours. After cooling to room temperature, the precipitate was separated and dried under reduced pressure to obtain a crude material. The crude material was purified by silica gel column chromatography to obtain the primary intermediate material 1,3-bis(chloromethyl)-2-methoxy-5-methylbenzene.

[0546] In a 3-Neck Round Bottom Flask (3-Neck RBF), an ACN (Acetonitrile) / H2O solution containing 2 equivalents of Na2S2O4 and 4 equivalents of NaHCO3 was added and stirred. The first intermediate material was added dropwise to the stirred material at a temperature of 45 °C, and the reaction was terminated after confirming that the conversion was complete through TLC (Thin Layer Chromatography). After the reaction was completed, stirring was stopped, and the aqueous layer was separated from the phase-separated mixture. The salt material was obtained by removing water under high temperature and reduced pressure using a rotary evaporator. After completely dissolving the salt material in a small amount of water, it was dropped into MeOH to obtain a precipitate. The precipitate was dispersed in a DCE (Dichloroethane) solution, and 3 equivalents of PCl5 were added. After stirring under reflux conditions for approximately 12 hours, the obtained crude solution was filtered to remove the remaining salts. The obtained filtered DCE solution was washed with H2O and dried over MgSO4 to remove the solvent, thereby obtaining (2-methoxy-5-methyl-1,3-phenylene)dimethanesulfonylchloride, a compound represented by the following chemical formula a-1-1.

[0547] [Chemical formula a-1-1]

[0548]

[0549] Whether the compound represented by chemical formula a-1-1 is synthesized 1 It was confirmed through H-NMR spectrum (Bruker, AVANCE NEO). The compound represented by the chemical formula a-1-1 1 H-NMR data are as follows.

[0550] 1H-NMR (400 MHZ. d6-Dimethyl sulfoxide): δ(ppm) = 6.99(s, 2H), 4.67(s, 4H), 3.78(s, 3H), 2.17(s, 3H)

[0551]

[0552] Synthesis Example 2

[0553] Preparation of a compound represented by chemical formula b-1

[0554] A 3-Neck Round Bottom Flask (RBF) was added with an ACN / H2O solution containing 2 equivalents of Na2S2O4 and 4 equivalents of NaHCO3 and stirred. 1,4-bromooctafluorobutane was added dropwise to the stirred material at 45°C. 19 After confirming that the conversion was complete through F NMR, the reaction was terminated. After the completion of the reaction, stirring was stopped, and the aqueous layer was separated from the phase-separated mixture. The water was removed using a rotary evaporator under high temperature and reduced pressure to obtain a salt substance. After completely dissolving the salt substance in a small amount of water, it was dropped into MeOH to obtain a precipitate. This precipitate was dispersed in a DCE (Dichloroethane) solution, and 3 equivalents of PCl5 were added. After stirring under reflux conditions for approximately 12 hours, the obtained crude solution was filtered to remove the residual salt. The obtained filtered DCE solution was washed with H2O and dried with MgSO4 to remove the solvent, thereby obtaining 1,1,2,2,3,3,4,4-octafluorobutane-1,4-disulfonyl dichloride, a compound represented by the chemical formula b-1 below.

[0555] [Chemical formula b-1]

[0556]

[0557] Whether the compound represented by chemical formula b-1 is synthesized 19 It was confirmed through F-NMR spectrum (Bruker, AVANCE NEO). The compound represented by the chemical formula b-1 above 19 The F-NMR data are as follows.

[0558] 19 F-NMR (400 MHZ. d6-Dimethyl sulfoxide): δ(ppm) = -104.2(t, 13Hz, 4F), -118.8(t, J = 12Hz, 4F)

[0559]

[0560] Synthesis Example 3

[0561] Preparation of a compound represented by chemical formula c-1-1

[0562] In a 3-Neck Round Bottom Flask (3-Neck RBF), 3 equivalents of NaH were dissolved in a THF (tetrahydrofuran) solution in which 1 equivalent of polyethylene glycol (number average molecular weight: 200) was dispersed, and the mixture was stirred. To the stirred material, a THF solution containing 1,3-propane sultone was added dropwise at 45°C. After stirring under reflux heating conditions, the conversion was confirmed to be complete through 1H NMR, and the solution was cooled to room temperature. After this, methanol (MeOH) was added to quench the remaining NaH. The solvent was removed under reduced pressure using a rotary evaporator to obtain a crude material, and the crude material was purified by washing with hexane and ether to obtain a primary intermediate material, (poly(ethylene glycol) bis(sodium propane-1-sulfonate).

[0563] The above first intermediate material was dispersed in a DCM (dichloromethane) solvent, and 3 equivalents of PCl5 were added. The mixture was stirred at 40°C for about 12 hours to obtain a crude solution, and the solvent was removed under reduced pressure using a rotary evaporator. The solution was then washed with hexane and ether and purified to obtain a second intermediate material, poly(ethylene glycol) bis(sodium propane-1-sulfonyl chloride).

[0564] Under a nitrogen atmosphere, 7 equivalents of NH4OH aqueous solution were added to a 3-Neck RBF and stirred at room temperature. The secondary intermediate material was dispersed in acetonitrile, and the dispersed solution was slowly added to the stirred material over 7 hours, and the solution was stirred at 40°C for about 12 hours. After that, water was added and the mixture was extracted several times with ethyl acetate. The organic layer was dried over Na2SO4, and the solvent was removed under reduced pressure using a rotary evaporator, washed and purified with ether, and dried to obtain poly(ethylene glycol) bis(propane-1-sulfonamide), a compound represented by the chemical formula c-1-1.

[0565] [Chemical formula c-1-1]

[0566]

[0567] Whether the compound represented by chemical formula c-1-1 is synthesized 1 It was confirmed through H-NMR spectrum (Bruker, AVANCE NEO). The compound represented by the chemical formula c-1-1 1 H-NMR data are as follows.

[0568] 1H-NMR (500 MHZ. d6-Dimethyl sulfoxide): δ(ppm) = 6.87(broad S, 4H), 3.43(m, 23H), 3.03(m, 4H), 1.89(m, 4H)

[0569]

[0570] Synthesis Example 4

[0571] Preparation of a compound represented by chemical formula d-1

[0572] In a 1-Neck Round Bottom Flask (1-Neck RBF), 1 equivalent of 3-sulfopropyl methacrylate potassium salt (TCI), 0.1 equivalent of DMF and THF (tetrahydrofuran) were added, and 5.5 equivalents of thionyl chloride were slowly added dropwise and stirred. After the reaction was completed after 3 hours, the mixture was quenched with water and extracted three times with DCM (dichloro methane) to obtain the organic layer. The solvent was removed under reduced pressure using a rotary evaporator to obtain 3-(chlorosulfonyl)propyl methacrylate.

[0573] [Chemical formula d-1]

[0574]

[0575] Whether the compound represented by chemical formula d-1 can be synthesized 1 It was confirmed through H-NMR spectrum (Bruker, AVANCE NEO). The compound represented by the chemical formula d-1 above 1 H-NMR data are as follows.

[0576] 1 H-NMR (500 MHZ. d6-Dimethyl sulfoxide): δ(ppm) = 6.13-5.63(s, 2H), 4.34(m, 2H), 3.79(m, 2H), 2.45(m, 2H), 1.96(s,3H)

[0577]

[0578] Synthesis Example 5

[0579] Preparation of a compound represented by the chemical formula Aa

[0580] A solution containing 1 equivalent of 4-methylanisole, 1.3 equivalents of p-formaldehyde, and 50 equivalents of HCl (6N aqueous solution) was stirred and heated at 80°C for 5 hours. After cooling to room temperature, the precipitate was separated and dried under reduced pressure to obtain a crude material. The crude material was purified by silica gel column chromatography to obtain the primary intermediate material 1,3-bis(chloromethyl)-2-methoxy-5-methylbenzene.

[0581] In a 3-Neck Round Bottom Flask (3-Neck RBF), an ACN (Acetonitrile) / H2O solution containing 2 equivalents of Na2S2O4 and 4 equivalents of NaHCO3 was added and stirred. The first intermediate material was added dropwise to the stirred material at a temperature of 45 °C, and the reaction was terminated after confirming that the conversion was complete through TLC (Thin Layer Chromatography). After the reaction was completed, stirring was stopped, and the aqueous layer was separated from the phase-separated mixture. The salt material was obtained by removing water under high temperature and reduced pressure using a rotary evaporator. After completely dissolving the salt material in a small amount of water, it was dropped into MeOH to obtain a precipitate. The precipitate was dispersed in a DCE (Dichloroethane) solution, and 3 equivalents of PCl5 were added. After stirring under reflux conditions for about 12 hours, the obtained crude solution was filtered to remove the remaining salts. The obtained filtered DCE solution was washed with H2O and dried over MgSO4 to remove the solvent, thereby obtaining (2-methoxy-5-methyl-1,3-phenylene)dimethanesulfonyl chloride, a compound represented by the following chemical formula Aa (same as the compound represented by the chemical formula a-1-1 prepared in Synthetic Example 1).

[0582] [Chemical formula Aa]

[0583]

[0584] Whether the compound represented by the chemical formula Aa can be synthesized 1 It was confirmed through H-NMR spectrum (Bruker, AVANCE NEO). The compound represented by the chemical formula Aa above 1 H-NMR data are as follows.

[0585] 1 H-NMR (500 MHZ. d6-Dimethyl sulfoxide): δ(ppm) = 6.99(s, 2H), 4.67(s, 4H), 3.78(s, 3H), 2.17(s, 3H)

[0586]

[0587] Synthesis Example 6

[0588] Preparation of a compound represented by the chemical formula Ab

[0589] Under a nitrogen atmosphere, 5 equivalents of NH3 (7 M in MeOH) were added to a 3-Neck RBF and stirred at room temperature. 1 equivalent of the compound represented by the chemical formula Aa prepared in Synthesis Example 1 was dispersed in acetonitrile, and the dispersed solution was slowly added to the stirred material over 7 hours, and the solution was stirred at 40°C for about 12 hours. After that, water was added and the mixture was extracted several times with ethyl acetate. The organic layer was dried over Na2SO4, and the solvent was removed under reduced pressure using a rotary evaporator, washed and purified with ether, and dried to obtain (2-methoxy-5-methyl-1,3-phenylene)dimethanesulfonamide, a compound represented by the following chemical formula Ab.

[0590] [Chemical formula Ab]

[0591]

[0592] Whether the compound represented by chemical formula Ab is synthesized 1 It was confirmed through H-NMR spectrum (Bruker, AVANCE NEO). The compound represented by the chemical formula Ab 1 H-NMR data are as follows.

[0593] 1H-NMR (500 MHZ. d6-Dimethyl sulfoxide): δ(ppm) = 7.12(broad s, 4H), 6.98(s, 2H), 4.35(s, 4H), 3.78(s, 3H), 2.17(s, 3H)

[0594]

[0595] Synthesis Example 7

[0596] Preparation of a compound represented by the chemical formula Ac

[0597] Under a nitrogen atmosphere, 1 equivalent of NH3 (7 M in MeOH) was added to a 3-Neck RBF and stirred at room temperature. 1 equivalent of the compound represented by the chemical formula Ab prepared in Synthesis Example 2 was dispersed in acetonitrile, and the dispersed solution was slowly added to the stirred material over 1 hour, and the solution was stirred at room temperature for about 24 hours. After that, water was added and the mixture was extracted several times with ethyl acetate. The organic layer was dried over Na2SO4, and the solvent was removed under reduced pressure using a rotary evaporator, washed and purified with ether, and dried to obtain (2-methoxy-5-methyl-3-(sulfamoylmethyl)phenyl)methanesulfonylchloride, a compound represented by the following chemical formula Ac.

[0598] [Chemical formula Ac]

[0599]

[0600] Whether the compound represented by the chemical formula Ac can be synthesized 1 It was confirmed through H-NMR spectrum (Bruker, AVANCE NEO). The compound represented by the chemical formula Ac 1 H-NMR data are as follows.

[0601] 1H-NMR (500 MHZ. d6-Dimethyl sulfoxide): δ(ppm) = 7.12(broad s, 2H), 6.97(s, 2H), 4.67(s, 2H), 4.35(s, 2H), 3.78(s, 3H), 2.16(s, 3H)

[0602]

[0603] Synthesis Example 8

[0604] Preparation of a compound represented by the chemical formula Ba

[0605] An acetonitrile solution containing 1 equivalent of the compound represented by the chemical formula Aa prepared in Synthetic Example 1 was stirred under a nitrogen atmosphere. An aqueous solution containing 5 equivalents of lithium bis(trifluoromethyl)sulfonylimide was slowly added to the mixture over 1 hour, and the solution was stirred at room temperature for about 24 hours. Thereafter, water was added and the mixture was extracted several times with ethyl acetate. After drying the organic layer with Na2SO4, the solvent was removed under reduced pressure using a rotary evaporator, washed and purified with ether, and dried to obtain (2-methoxy-5-methyl-1,3-phenylene)dimethanesulfonyl chloride, lithium bis(trifluoromethyl)sulfonylimide, a compound represented by the following chemical formula Ba.

[0606] [chemical formula Ba]

[0607]

[0608] Whether the compound represented by the chemical formula Ba can be synthesized 1 It was confirmed through H-NMR spectrum (Bruker, AVANCE NEO). The compound represented by the chemical formula Ba above 1H-NMR data are as follows.

[0609] 1 H-NMR (500 MHZ. d6-Dimethyl sulfoxide): δ(ppm) = 7.08(s, 2H), 4.67(s, 4H), 3.90(s, 3H), 2.17(s, 3H)

[0610]

[0611] Manufacturing Example 1

[0612] Preparation of a compound represented by chemical formula 1-a

[0613] 3 equivalents of triethylamine, 1 equivalent of the compound represented by the above chemical formula c-1-1, 0.2 equivalents of the compound represented by the above chemical formula a-1-1, and 0.8 equivalents of the compound represented by the above chemical formula b-1 were dispersed in a DMF (Dimethylformamide) solution, and then stirred at 120°C for 24 hours. Afterwards, the solution was cooled to room temperature, and water and dichloromethane were added, and the precipitate was separated by filtration from the obtained mixture. Thereafter, the obtained solid material was washed with methanol and then vacuum-dried. The vacuum-dried solid material and 3 equivalents of an ammonia solution (7 M in MEOH, Sigma-Aldrich) were dispersed in a DMF (Dimethylformamide) solution, and then stirred at 50°C for 24 hours. After this, the stirred solution was cooled to room temperature, and dichloromethane was added to the mixture, and the precipitate was filtered and separated to obtain a compound represented by the following chemical formula 1-a.

[0614] [Chemical Formula 1-a]

[0615]

[0616] In the above chemical formula 1-a, n is an integer from 1 to 20, q is an integer from 1 to 20, and o is an integer from 1 to 20.

[0617]

[0618] Whether the compound represented by the above chemical formula 1-a is synthesized 1 It was confirmed through H-NMR spectrum (Bruker, AVANCE NEO) and GPC (Waters, e2695 GPC). The number-average molecular weight (Mn) was analyzed as 11200 g / mol, PDI=1.8. The compound represented by the above chemical formula 1-a 1 H-NMR data are as follows.

[0619] 1 H-NMR (500 MHZ. d6-Dimethyl sulfoxide): δ(ppm) = 6.99(s, 0.4H), 4.29(s, 0.8H), 3.78(s. 0.6H), 3.43(m, 23H), 3.02(m, 4H), 2.17(s, 0.6H), 1.89(m, 4H)

[0620] 19 F-NMR (470 MHZ. d6-Dimethyl sulfoxide): δ(ppm) = -113.2(t, 4F), -119.1(t, 4F)

[0621]

[0622] Manufacturing Example 2

[0623] Preparation of a compound represented by chemical formula 1-b

[0624] 3 equivalents of triethylamine, 1 equivalent of the compound represented by the above chemical formula c-1-1, and 1 equivalent of the compound represented by the above chemical formula a-1-1 were dispersed in a DMF (Dimethylformamide) solution, and stirred at 120°C for 24 hours. Thereafter, the solution was cooled to room temperature, and water and dichloromethane were added, and the precipitate was separated by filtration from the obtained mixture. Thereafter, the obtained solid material was washed with methanol and then vacuum-dried. The vacuum-dried solid material and 3 equivalents of an ammonia solution (7 M in MEOH, Sigma-Aldrich) were dispersed in a DMF (Dimethylformamide) solution, and the mixture was stirred at 50°C for 24 hours. Thereafter, the stirred solution was cooled to room temperature, and dichloromethane was added, and the precipitate was separated by filtration from the obtained mixture, thereby obtaining a compound represented by the following chemical formula 1-b.

[0625] [Chemical Formula 1-b]

[0626]

[0627] In the above chemical formula 1-b, n is an integer from 1 to 20, and q is an integer from 1 to 20.

[0628]

[0629] Whether the compound represented by the above chemical formula 1-b is synthesized 1 It was confirmed through H-NMR spectrum (Bruker, AVANCE NEO) and GPC (Waters, e2695 GPC). The number-average molecular weight (Mn) was analyzed as 7100 g / mol, PDI=1.6. The compound represented by the above chemical formula 1-b 1 H-NMR data are as follows.

[0630] 1H-NMR (500 MHZ. d6-Dimethyl sulfoxide): δ(ppm) = 6.99(s, 2H), 4.29(s, 4H), 3.78(s, 3H), 3.43(m, 23H), 2.43(m, 4H), 2.17(s, 3H), 1.89(m, 4H)

[0631]

[0632] Manufacturing Example 3

[0633] Preparation of a compound represented by chemical formula 2-a

[0634] 3 equivalents of triethylamine, 1 equivalent of the compound represented by the above chemical formula c-1-1, 0.2 equivalents of the compound represented by the above chemical formula a-1-1, and 0.8 equivalents of the compound represented by the above chemical formula b-1 were dispersed in a DMF (Dimethylformamide) solution, and then stirred at 120°C for 24 hours. Afterwards, the solution was cooled to room temperature, and water and dichloromethane were added, and the precipitate was separated by filtration from the obtained mixture. Thereafter, the obtained solid material was washed with methanol and then vacuum-dried. The vacuum-dried solid material was dispersed in anhydrous DMF, and 5 equivalents of lithium hydride were slowly added, and the mixture was stirred at room temperature for 24 hours. Thereafter, unreacted lithium hydride was filtered, and the precipitate was separated by filtration using an excess of tetrahydrofuran (THF) in the obtained filtrate.

[0635] The precipitate obtained by filtration and 3 equivalents of ammonia solution (7 M in MEOH, Sigma-Aldrich) were dispersed in a DMF (Dimethylformamide) solution, and stirred at 50°C for 24 hours. Thereafter, the stirred solution was cooled to room temperature, and dichloromethane was added. The precipitate was separated by filtration from the resulting mixture, thereby obtaining a compound represented by the following chemical formula 2-a.

[0636] [Chemical Formula 2-a]

[0637]

[0638] In the above chemical formula 2-a, n is an integer from 1 to 20, q is an integer from 1 to 20, and o is an integer from 1 to 20.

[0639]

[0640] Whether the compound represented by the above chemical formula 2-a is synthesized 1 It was confirmed through H-NMR spectrum (Bruker, AVANCE NEO) and GPC (Waters, e2695 GPC). The number-average molecular weight (Mn) was analyzed as 12400 g / mol, PDI=1.9. The compound represented by the above chemical formula 2-a 1 H-NMR data are as follows.

[0641] 1 H-NMR (500 MHZ. d6-Dimethyl sulfoxide): δ(ppm) = 6.99(s, 0.4H), 4.64(s, 0.4H), 3.78(s. 0.6H), 3.43(m, 23H), 3.32(m, 4H), 2.17(s, 0.6H), 1.89(m, 4H)

[0642] 19 F-NMR (470 MHZ. d6-Dimethyl sulfoxide): δ(ppm) = -114.1(t, 4F), -119.1(t, 4F)

[0643]

[0644] Manufacturing Example 4

[0645] Preparation of a compound represented by chemical formula 2-b

[0646] 3 equivalents of triethylamine, 1 equivalent of the compound represented by the above chemical formula c-1-1, and 1 equivalent of the compound represented by the above chemical formula a-1-1 were dispersed in a DMF (Dimethylformamide) solution, and then stirred at 120°C for 24 hours. Thereafter, the solution was cooled to room temperature, and water and dichloromethane were added, and the precipitate was separated by filtration from the obtained mixture. Thereafter, the obtained solid material was washed with methanol and then vacuum-dried. The vacuum-dried solid material was dispersed in anhydrous DMF, and 5 equivalents of lithium hydride were slowly added, and the mixture was stirred at room temperature for 24 hours. Thereafter, unreacted lithium hydride was filtered, and the precipitate was separated by filtration using an excess of tetrahydrofuran (THF) in the obtained filtrate.

[0647] The precipitate obtained by filtration and 3 equivalents of ammonia solution (7 M in MEOH, Sigma-Aldrich) were dispersed in a DMF (Dimethylformamide) solution, and stirred at 50°C for 24 hours. Thereafter, the stirred solution was cooled to room temperature, and dichloromethane was added. The precipitate was separated by filtration from the resulting mixture, thereby obtaining a compound represented by the following chemical formula 2-b.

[0648] [Chemical Formula 2-b]

[0649]

[0650] In the above chemical formula 2-b, n is an integer from 1 to 20, and q is an integer from 1 to 20.

[0651]

[0652] Whether the compound represented by the above chemical formula 2-b is synthesized 1It was confirmed through H-NMR spectrum (Bruker, AVANCE NEO) and GPC (Waters, e2695 GPC). The number-average molecular weight (Mn) was analyzed to be 7300 g / mol, PDI=1.6. The compound represented by the above chemical formula 2-b 1 H-NMR data are as follows.

[0653] 1 H-NMR (500 MHZ. d6-Dimethyl sulfoxide): δ(ppm) = 6.99(s, 2H), 4.29(s, 4H), 3.78(s, 3H), 3.43(m, 23H), 3.33(m, 4H), 2.17(s, 3H), 1.89(m, 4H)

[0654]

[0655] Manufacturing Example 5

[0656] Preparation of a compound represented by chemical formula 1-c

[0657] After preparing the compound represented by Chemical Formula 1-a in the above Preparation Example 1, 3 equivalents of TEA, 1 equivalent of the compound represented by Chemical Formula 1-a, and 2.5 equivalents of the compound represented by Chemical Formula d-1 were dispersed in a DMF solution and stirred at room temperature for 24 hours. Thereafter, dichloromethane was added, and the precipitate was separated by filtration from the obtained mixture, thereby obtaining the compound represented by Chemical Formula X below.

[0658] [Chemical Formula 1-c]

[0659]

[0660] In the above chemical formula 1-c, n is an integer from 1 to 20, q is an integer from 1 to 20, and o is an integer from 1 to 20.

[0661] Whether the compound represented by the above chemical formula 1-c is synthesized 1It was confirmed through H-NMR spectrum (Bruker, AVANCE NEO) and GPC (Waters, e2695 GPC). The number-average molecular weight (Mn) was analyzed to be 15000 g / mol, PDI=1.9. The compound represented by the above chemical formula 1-c 1 H-NMR data are as follows.

[0662] 1 H-NMR (500 MHZ. d6-Dimethyl sulfoxide): δ(ppm) = 6.99(s, 0.4H), 6.0(s, 2H), 5.6(s, 2H), 4.29(s, 0.8H), 3.78(s. 0.6H), 3.43(m, 31H), 3.02(m, 8H), 2.1(s, 6.6H), 1.89(m, 4H)

[0663] 19 F-NMR (470 MHZ. d6-Dimethyl sulfoxide): δ(ppm) = -113.2(t, 4F), -119.1(t, 4F)

[0664]

[0665] Manufacturing Example 6

[0666] Preparation of a compound represented by chemical formula 2-c

[0667] After preparing the compound represented by Chemical Formula 2-a in the above Preparation Example 3, 3 equivalents of TEA, 1 equivalent of the compound represented by Chemical Formula 2-a, and 2.5 equivalents of the compound represented by Chemical Formula d-1 were dispersed in a DMF solution and stirred at room temperature for 24 hours. Thereafter, dichloromethane was added, and the precipitate was separated by filtration from the obtained mixture, thereby obtaining the compound represented by Chemical Formula 2-c below.

[0668] [Chemical Formula 2-c]

[0669]

[0670] Whether the compound represented by the above chemical formula 2-c is synthesized1 It was confirmed through H-NMR spectrum (Bruker, AVANCE NEO) and GPC (Waters, e2695 GPC). The number-average molecular weight (Mn) was analyzed as 15200 g / mol, PDI=1.9. The compound represented by the above chemical formula 2-c 1 H-NMR data are as follows.

[0671] 1 H-NMR (500 MHZ. d6-Dimethyl sulfoxide): δ(ppm) = 6.99(s, 0.4H), 6.0(s, 2H), 5.6(s, 2H), 4.64(s, 0.4H), 3.78(s. 0.6H), 3.43(m, 27H), 3.32(m, 8H), 2.4(m, 4H), 2.17(s, 6.6H), 1.89(m, 4H)

[0672] 19 F-NMR (470 MHZ. d6-Dimethyl sulfoxide): δ(ppm) = -114.1(t, 4F), -119.1(t, 4F)

[0673]

[0674] Manufacturing Example 7

[0675] Preparation of a compound represented by chemical formula W-1

[0676] 3 equivalents of triethylamine, 1 equivalent of the compound represented by the above chemical formula Aa, and 1 equivalent of the compound represented by the above chemical formula Ab were dispersed in a DMF (Dimethylformamide) solution, and stirred at 120°C for 24 hours. Thereafter, the solution was cooled to room temperature, and water and dichloromethane were added, and the precipitate was separated by filtration from the obtained mixture. Thereafter, the obtained solid material was washed with methanol and then vacuum-dried. The vacuum-dried solid material and 3 equivalents of an ammonia solution (7 M in MEOH, Sigma-Aldrich) were dispersed in a DMF (Dimethylformamide) solution, and the mixture was stirred at 50°C for 24 hours. Thereafter, the stirred solution was cooled to room temperature, and dichloromethane was added, and the precipitate was separated by filtration from the obtained mixture, thereby obtaining a compound represented by the following chemical formula W-1.

[0677] [Chemical Formula W-1]

[0678]

[0679] In the above chemical formula W-1, n is an integer from 1 to 300.

[0680] The synthesis of the compound represented by the above chemical formula W-1 was confirmed through GPC (Waters, e2695 GPC). The number-average molecular weight (Mn) was analyzed to be 9600 g / mol, PDI=1.9.

[0681]

[0682] Manufacturing Example 8

[0683] Preparation of a compound represented by chemical formula X-1

[0684] Under a nitrogen atmosphere, an acetonitrile solution containing 1 equivalent of the compound represented by the chemical formula W-1 prepared in Preparation Example 1 was dispersed and stirred. An aqueous solution containing 5 equivalents of lithium bis(trifluoromethyl)sulfonylimide was slowly added to the mixture over 1 hour, and the solution was stirred at room temperature for about 24 hours. After that, water was added and the mixture was extracted several times with ethyl acetate. The organic layer was dried over Na2SO4, and the solvent was removed under reduced pressure using a rotary evaporator, washed with ether, purified, and dried to obtain a compound represented by the following chemical formula X-1.

[0685] [Chemical Formula X-1]

[0686]

[0687] In the above chemical formula X-1, n is an integer from 1 to 300.

[0688] The synthesis of the compound represented by the above chemical formula X-1 was confirmed through GPC (Waters, e2695 GPC). The number-average molecular weight (Mn) was analyzed to be 9900 g / mol, PDI=1.9.

[0689]

[0690] Manufacturing Example 9

[0691] Preparation of a compound represented by the chemical formula Z-1

[0692] Under a nitrogen atmosphere, the material represented by the chemical formula X-1 prepared in the above Preparation Example 1 was dispersed in Anhydrous DMF, and then 5 equivalents of lithium hydride were slowly added, and the solution was stirred at room temperature for about 24 hours. Thereafter, unreacted lithium hydride was filtered, and the precipitate was separated by filtration using an excess amount of tetrahydrofuran (THF) in the obtained filtrate, thereby obtaining a compound represented by the following chemical formula Z-1.

[0693] [Chemical Formula Z-1]

[0694]

[0695] In the above chemical formula Z-1, n and m are each independently an integer from 1 to 300.

[0696] The synthesis of the compound represented by the above chemical formula Z-1 was confirmed through GPC (Waters, e2695 GPC). The number-average molecular weight (Mn) was analyzed to be 10200 g / mol, PDI=1.9.

[0697]

[0698] Manufacturing Example 10

[0699] Preparation of a compound represented by chemical formula Q

[0700] 3 equivalents of Trethylamine, 1 equivalent of (2,5-dimethyl-1,3-phenylene)dimethanesulfonamide, and 1 equivalent of (2,5-dimethyl-1,3-phenylene)dimethanesulfonyl chloride were dispersed in a DMF (Dimethylformamide) solution, and stirred at 120°C for 24 hours. Afterwards, the solution was cooled to room temperature, and water and dichloromethane were added, and the precipitate was separated by filtration from the obtained mixture. Thereafter, the obtained solid material was washed with methanol and dried under vacuum to obtain a compound represented by the following chemical formula Q.

[0701] [Chemical formula Q]

[0702]

[0703] In the above chemical formula Q, n is an integer from 1 to 300.

[0704] The synthesis of the compound represented by the above chemical formula Q was confirmed through GPC (Waters, e2695 GPC). The number-average molecular weight (Mn) was analyzed to be 6100 g / mol, PDI=1.7.

[0705]

[0706] Example 1

[0707] 3 g of the compound represented by Chemical Formula 1-a prepared from Manufacturing Example 1 was dispersed in 30 mL of N-Methyl-2-pyrrolidone solvent to obtain a transparent solution, which was then uniformly solution-cast onto a flat glass plate. The solution was then dried at 40°C for approximately 12 hours, and then dried in a vacuum oven at 70°C for 24 hours. Through this, an ion-conducting polymer electrolyte film having a thickness of 20-40 μm was prepared.

[0708]

[0709] Example 2

[0710] An ion-conducting polymer electrolyte film was manufactured in the same manner as in Example 1, except that 3 g of the compound represented by Chemical Formula 1-b manufactured from Manufacturing Example 2 was used.

[0711]

[0712] Example 3

[0713] An ion-conducting polymer electrolyte film was manufactured in the same manner as in Example 1, except that 3 g of the compound represented by Chemical Formula 2-a manufactured from Manufacturing Example 3 was used.

[0714]

[0715] Example 4

[0716] An ion-conducting polymer electrolyte film was manufactured in the same manner as in Example 1, except that 3 g of the compound represented by Chemical Formula 2-b manufactured from Manufacturing Example 4 was used.

[0717]

[0718] Example 5

[0719] Lithium bis(Trifluoromethyl)sulfonylimide (EO:Li +After dissolving (molar ratio = 20:1) in N-Methyl-2-pyrrolidone, 3 g (20 wt% vs N-Methyl-2-pyrrolidone) of the compound represented by the chemical formula 1-a prepared in Preparation Example 1 was added. The mixture was stirred at room temperature for 2 hours using an overhead stirrer. Thereafter, air bubbles were removed by sonication (exposure to sonication conditions) in a bath sonicator for 20 minutes, and a solution containing the compound represented by the chemical formula 3-a was obtained.

[0720] [Chemical Formula 3-a]

[0721]

[0722] In the above chemical formula 3-a, n is an integer from 1 to 20, q is an integer from 1 to 20, and o is an integer from 1 to 20.

[0723]

[0724] After this, the solution was uniformly solution-casted onto a flat glass plate. After this, it was dried at 40°C for approximately 12 hours, and then dried again at 70°C in a vacuum oven for 24 hours, thereby producing an ion-conducting polymer electrolyte film with a thickness of 20-40 μm.

[0725]

[0726] Example 6

[0727] An ion-conducting polymer electrolyte film containing a compound represented by the following chemical formula 4-a was manufactured in the same manner as in Example 5, except that 3 g of the compound represented by the chemical formula 2-a prepared from Preparation Example 3 was used instead of the compound represented by the chemical formula 1-a.

[0728] [Chemical Formula 4-a]

[0729]

[0730] In the above chemical formula 4-a, n is an integer from 1 to 20, q is an integer from 1 to 20, and o is an integer from 1 to 20.

[0731]

[0732] Example 7

[0733] 3 g of the compound represented by Chemical Formula 1-c prepared from Manufacturing Example 5 was dispersed in 30 mL of N-Methyl-2-pyrrolidone solvent to obtain a transparent solution, and 0.1 g of AINB was added. The solution was uniformly solution-casted onto a flat glass plate. Thereafter, the solution was dried at 40°C for approximately 12 hours, and then dried in a vacuum oven at 70°C for 24 hours. Through this, an ion-conducting polymer electrolyte film having a thickness of 20-40 μm was prepared.

[0734]

[0735] Example 8

[0736] An ion-conducting polymer electrolyte film was manufactured in the same manner as in Example 7, except that 0.1 g of AINB and 0.5 g of PETA were added instead of 0.1 g of AINB in ​​Example 7.

[0737]

[0738] Example 9

[0739] An ion-conducting polymer electrolyte film was manufactured in the same manner as in Example 7, except that 3 g of the compound represented by Chemical Formula 2-c manufactured from Manufacturing Example 6 was used.

[0740]

[0741] Example 10

[0742] An ion-conducting polymer electrolyte film was manufactured in the same manner as in Example 8, except that 3 g of the compound represented by Chemical Formula 2-c manufactured from Manufacturing Example 6 was used.

[0743]

[0744] Example 11

[0745] 3 g of the compound represented by the chemical formula W-1 prepared from Manufacturing Example 7 was dispersed in 30 mL of N-Methyl-2-pyrrolidone solvent to obtain a transparent solution, which was then uniformly solution-casted onto a flat glass plate. The solution was then dried at 40°C for approximately 12 hours, and then dried in a vacuum oven at 70°C for 24 hours. Through this, an ion-conducting polymer electrolyte film having a thickness of 20-40 μm was prepared.

[0746]

[0747] Example 12

[0748] An ion-conducting polymer electrolyte film was manufactured in the same manner as in Example 11, except that 3 g of the compound represented by the chemical formula X-1 manufactured from Manufacturing Example 8 was used.

[0749]

[0750] Example 13

[0751] An ion-conducting polymer electrolyte film was manufactured in the same manner as in Example 11, except that 3 g of the compound represented by the chemical formula Z-1 manufactured from Manufacturing Example 9 was used.

[0752]

[0753] Comparative Example 1

[0754] Lithium bis(Trifluoromethyl)sulfonylimide (EO:Li +After dissolving PEO (20 wt% vs. Acetonitrile) in acetonitrile, 3 g (20 wt% vs. Acetonitrile) was added. At this time, the PEO had a composition in which PEO (Sigma-Aldrich) with Mw=100,000 and PEO (Sigma-Aldrich) with Mw=600,000 were mixed in a weight ratio of 9:1. The mixture was stirred at room temperature for 2 hours using an overhead stirrer. After that, air bubbles were removed by sonication (exposure to sonication conditions) in a bath sonicator for 20 minutes, and a PEO-LiTFSI solution was obtained. After that, the PEO-LiTFSI solution was dropwise applied onto an MRF-38 release film using a film applicator and coated. First, it was dried for about 12 hours under room temperature conditions, and then vacuum-dried in a vacuum oven at 40°C for 8 hours. Through this, a PEO-LiTFSI polymer electrolyte film with a thickness of 10-50 μm was manufactured.

[0755]

[0756] Comparative Example 2

[0757] An ion-conducting polymer electrolyte film was manufactured in the same manner as in Example 11, except that 3 g of the compound represented by the chemical formula Q manufactured from Manufacturing Example 10 was used.

[0758]

[0759] Experimental Example 1 - Measurement of ionic conductivity

[0760] Inside a glove box, the polymer electrolyte film manufactured in the above examples and comparative examples was soaked in a solvent of EC / PC (1:1 volume ratio), and the polymer electrolyte film was sandwiched between two stainless steel electrodes (used as a negative electrode and a positive electrode) in a battery case to manufacture a coin cell including an electrode assembly.

[0761] The coin cell manufactured above was measured at room temperature (25℃) using a potentiostat (Biologics SP-200) with an amplitude of 10 mV over a frequency range of 0.1 Hz to 7 MHz. The impedance was measured, and the ionic conductivity was measured by substituting it into the equation L=I / RS (L= ionic conductivity, I= electrode thickness, R= measured impedance value, S= electrode area). The measured ionic conductivity is shown in Table 1 or 2 below.

[0762]

[0763] Experimental Example 2 - Measurement of lithium ion transport rate

[0764] In a glove box, the polymer electrolyte film manufactured in the above examples and comparative examples was soaked in a solvent of EC / PC (1:1 volume ratio), and the polymer electrolyte film was sandwiched between lithium foil electrodes (used as negative and positive electrodes) having a thickness of 200 ㎛ in a battery case, and a coin cell including an electrode assembly was manufactured by storing the polymer electrolyte film at a temperature of 60° C. for about 12 hours.

[0765] The resistance of the passivation layer of the coin cell manufactured above was measured before and after the chronoamperometry experiment using a potentiostat (Biologics SP-200). Li+ = I s (△V - I o R o ) / I o (△V - I S R S )(△V= voltage applied to the cell = 3 mV, I o = Initial current, I S = Steady-state current, R o = Initial resistance of the passivation layer on the lithium electrode surface, R S = steady-state resistance of the passivation layer on the lithium electrode surface) and substituted into the equation to obtain the lithium ion transport rate (t Li+) was measured. The measured lithium ion transport rate is shown in Table 1 or 2 below.

[0766]

[0767] Experimental Example 3 - Tensile strength and tensile strain

[0768] The tensile strength and tensile strain of the films manufactured according to Examples 7 to 10 and Comparative Example 1 were measured using static Materials Testing Machines (measuring equipment) from ZwickiLine, and the results are shown in Table 2 below. Specifically, a specimen cut to a width of 10 mm and a length of 30 mm was fixed to the measuring equipment, and the specimen was pulled at a speed of 5 mm per minute, and the force at the moment of breaking and the change in length of the specimen were measured. Tensile strength means the value obtained by dividing the force when deformation or fracture occurs by the cross-sectional area of ​​the specimen before deformation occurs, and tensile strain means the change in length of the specimen with respect to the applied force.

[0769]

[0770] Classification Solid electrolyte Ionic conductivity (mS / cm) Lithium ion transport rate Example 1 Solid electrolyte containing chemical formula 1-a 5.6 × 10 -4 0.33 Example 2 Solid electrolyte containing chemical formula 1-b 4.8 × 10 -4 0.29 Example 3 Solid electrolyte containing chemical formula 2-a 7.9 × 10 -3 0.94 Example 4 Solid electrolyte containing chemical formula 2-b 4.1 × 10 -3 0.91 Example 5 Solid electrolyte containing chemical formula 3-a 8.3 × 10 -4 0.83 Example 6 Solid electrolyte containing chemical formula 4-a 1.1 × 10 -2 0.74 Example 11 Solid electrolyte containing chemical formula W-1 4.2 × 10 -4 0.33 Example 12 Solid electrolyte containing chemical formula X-1 6.3 × 10 -4 0.31 Example 13 Solid electrolyte containing chemical formula Z-1 1.9 × 10 -30.92 Comparative example 1 Solid electrolyte containing PEO-LiTFSI 2.6 × 10 -4 0.28 Comparative Example 2 Solid electrolyte containing chemical formula Q 7.1 × 10 -5 0.30

[0771] Referring to Table 1, it can be confirmed that Examples 3 to 6 have higher lithium ion conductivity and ion transport rate than Comparative Example 1. In addition, it can be confirmed that Examples 1 and 2 also have lithium ion conductivity and ion transport rate at the same or higher level than Comparative Example 1. The above examples include ion-conducting polymers in which sulfonimide anions, which are friendly to lithium ions but have low electron density, are fixed to the main chain. Since such ion-conducting polymers can move dissociated lithium ions in the electrolyte with higher efficiency, the above examples can have higher ion conductivity and ion transport rate characteristics than the Comparative Examples including the existing alkylene oxide-based polymers.

[0772] In addition, it can be confirmed that Example 1 using the compound represented by Chemical Formula 1-a has higher ion conductivity and ion transport rate than Example 2 using the compound represented by Chemical Formula 1-b, and Example 3 using the compound represented by Chemical Formula 2-a has higher ion conductivity and ion transport rate than Example 4 using the compound represented by Chemical Formula 2-b. This can be seen as because fluorine having high electronegativity delocalizes the anion of the neighboring sulfonimide, thereby lowering the electron density of the sulfonimide, thereby alleviating the electrostatic attraction between the lithium ion and the solid electrolyte, and as a result, moving the dissociated lithium ion in the electrolyte with higher efficiency.

[0773] In addition, referring to Table 1, it can be confirmed that Examples 11 to 13 have superior ion conductivity and lithium ion transport rate compared to Comparative Examples 1 and 2. In particular, it can be confirmed that Example 13 is significantly superior to Comparative Examples 1 and 2. The compounds included in the solid electrolytes of Examples 11 to 13 have a lithium-affinity structure including an aromatic ring structure in which an alkoxy group is substituted at one carbon position of a benzene ring and an alkyl group substituted with a sulfonyl group is positioned on both sides of the ortho position, so that the ion conductivity and ion transport rate are excellent. In particular, the compound included in the solid electrolyte of Example 13 has an ion conductive structure in which a sulfonimide anion is fixed to the main chain, so that the dissociated lithium ion can be moved with higher efficiency. As a result, Examples 11 to 13 can have higher ion conductivity and ion transport rate compared to Comparative Example 2 which does not include the alkoxy group and Comparative Example 1 which includes a conventional alkylene oxide polymer.

[0774]

[0775] Classification Solid electrolyte Crosslinking compound Ion conductivity (mS / cm) Lithium ion transport rate Tensile strength (MPa) Tensile strain (%) Example 7 Solid electrolyte containing chemical formula 1-c X 6.0 × 10 -4 0.400.8231Example 8 Solid electrolyte containing chemical formula 1-c PETA7.2 × 10 -4 0.322.142Example 9 Solid electrolyte containing chemical formula 2-c X8.0 × 10 -3 0.9340.8929Example 10 Solid electrolyte containing chemical formula 2-cPETA9.1 × 10 -3 0.912.437Comparative example 1 Solid electrolyte containing PEO-LiTFSI-2.6 × 10 -4 0.280.110

[0776] Referring to Table 2, it can be confirmed that Examples 9 and 10 have higher lithium ion conductivity and ion transport rate than Comparative Example 1. In addition, it can be confirmed that Examples 7 and 8 also have higher lithium ion transport rates than Comparative Example 1. The above examples include ion-conducting polymers in which sulfonimide anions, which are friendly to lithium ions but have low electron density, are fixed to the main chain. Since such ion-conducting polymers can move dissociated lithium ions in the electrolyte with higher efficiency, the above examples can have higher ion conductivity and ion transport rate characteristics than the Comparative Examples including the existing alkylene oxide-based polymers.

[0777] In addition, it can be confirmed that Example 9 using the compound represented by Chemical Formula 2-c has higher ion conductivity and ion transport rate than Example 7 using the compound represented by Chemical Formula 1-c, and Example 10 with added PETA, a crosslinking compound, has slightly lower lithium ion transport rate than Example 9 without adding PETA. This is because a network was formed by a radical reaction between double bonds, and by forming a solid electrolyte structure firmly, the durability of physical strengths such as tensile strength and tensile strain is increased while maintaining structural uniformity, so that the ion conductivity and transport rate of lithium ions are not significantly reduced.

[0778]

[0779] Experimental Example 4 - Evaluation of Battery Life Characteristics

[0780] In a glove box, the polymer electrolyte film manufactured in the above examples and comparative examples was soaked in a solvent of EC / PC (1:1 volume ratio), and the polymer electrolyte film was sandwiched between lithium foil electrodes (used as negative and positive electrodes) having a thickness of 200 ㎛ in a battery case, and a coin cell including an electrode assembly was manufactured by storing the polymer electrolyte film for about 12 hours under conditions of 60°C.

[0781] The above coin cell was charged and discharged at 25°C with 0.2 mA / cm 2 The charge-discharge process was performed three times, with one cycle being a charge to the cut-off time of 1 hour at a current density of 1.0 mA / cm and a discharge time of 1 hour. Then, the coin cell was charged and discharged using a charger at 1.0 mA / cm 2 The charge-discharge process was performed 400 times, with one cycle being a charge to the cut-off time of 1 hour at a current density of 1.0 mA / cm and a discharge time of 1 hour. At this time, the current density was 1.0 mA / cm 2 The voltage generated in the first cycle is measured when the current density is 1.0 mA / cm 2 The cycle number at which a voltage 1.5 times higher than the voltage generated in the first cycle is shown in Table 3 below.

[0782] Cycles in which voltage is 1.5 times higher than the voltage generated in the first cycle Example 1236 Example 2227 Example 3389 Example 4342 Example 5>400 Example 6>400 Example 7260 Example 8300 Example 9380 Example 10>400 Example 11178 Example 12221 Example 13>400 Comparative Example 1118 Comparative Example 2144

[0783] Referring to Table 3, it can be confirmed that Examples 1 to 13 suppressed the voltage increase compared to Comparative Examples 1 and 2, i.e., the lifespan of the battery to which the lithium metal negative electrode was applied was improved. In particular, in the case of Examples 3 to 6, 9, 10, and 13 in which an ion-conducting polymer including a lithiated or lithium compound was applied, it can be confirmed that the lifespan improvement effect was significantly excellent. This can be seen as an effect caused by the compound including the ion-conducting polymer according to the present invention suppressing the increase in electrode surface resistance and preventing the formation of dendritic crystals on the surface of the lithium metal electrode in addition to improving ion conductivity and ion transport rate.

Claims

1. A compound containing a repeating unit represented by the following chemical formula 1 or a compound that is a lithium salt thereof: [Chemical Formula 1] In the above chemical formula 1, The above X, Y and Z are each independently at least one selected from the group consisting of the following chemical formulas a-1, b and c-1, The above n is an integer from 1 to 100, The above q is an integer from 1 to 100, The above o is an integer from 0 to 100, The above * indicates a connecting portion or terminal portion between repeating units, [Chemical formula a-1] [chemical formula b] [Chemical formula c-1] In the above chemical formulas a-1, b and c-1, The above R1, R2 and R3 are each independently a hydrogen element; a halogen element; -CN; -NO2; substituted or unsubstituted C1-C 10 Alkyl group of; substituted or unsubstituted C1-C 10 Alkoxy group; substituted or unsubstituted C2-C 10 Alkenyl group of; substituted or unsubstituted C2-C 10 an alkynyl group of; -C(=O)R5; -P(=O)(OR5)2; -P(OR5)(OR6); -OP(=O)(OR5)(OR6); -S(=O)R5; or -S(=O)2R5, The above R4 is a hydrogen atom; or a substituted or unsubstituted C1-C 10 is an alkyl group, The above R5 and R6 are each independently a hydrogen element; substituted or unsubstituted C1-C 10 an alkyl group of; or a substituted or unsubstituted C2-C 10 is an alkenyl group, The above L1, L2 and L3 are each independently a direct bond; or a substituted or unsubstituted C1-C 10 is an alkylene group, The above X1 and X2 are each independently a hydrogen element; a halogen element; -CN; -NO2; a substituted or unsubstituted C1-C 10 an alkyl group of; or a substituted or unsubstituted C6-C 12 is an aryl group, The above m is an integer from 1 to 40, The above p is an integer from 1 to 200.

2. In claim 1, A compound wherein at least one of the above X, Y and Z comprises the above chemical formula a-1.

3. In claim 1, A compound in which the above R2 and R4 are each independently a C1-C5 alkyl group.

4. In claim 1, A compound wherein the above L1, L2 and L3 are each independently a C1-C5 alkylene group.

5. In claim 1, A compound wherein X1 and X2 are each independently a hydrogen element; or a halogen element.

6. In claim 1, wherein n is an integer from 1 to 20, The above q is an integer from 1 to 20, The above o is an integer from 1 to 20, The above m is an integer from 1 to 10, A compound wherein the above p is an integer from 1 to 50.

7. In claim 1, A compound containing a repeating unit represented by the above chemical formula 1 is a compound represented by the following chemical formula 1-a or 1-b: [Chemical Formula 1-a] [Chemical Formula 1-b] In the above chemical formulas 1-a and 1-b, n is an integer from 1 to 20, q is an integer from 1 to 20, and o is an integer from 1 to 20.

8. In claim 1, A compound comprising at least one functional group selected from the group consisting of the following chemical formulae d to g at at least one terminal portion among the above terminal portions: [chemical formula d] [chemical formula e] [chemical formula f] [chemical formula g] In the above chemical formulas d to g, The above R7 is a hydrogen atom; or a substituted or unsubstituted C1-C 10 is an alkyl group, R8 to R above 11 are each independently, direct bond; substituted or unsubstituted C1-C 10 alkylene group of; or -R 12 -OR 13 -and, The above R 12 and R 13 are each independently, directly bonded; or substituted or unsubstituted C1-C 10 is an alkylene group, The above * indicates the binding position.

9. In claim 8, The above R7 is a C1-C6 alkyl group, R8 to R above 11 are each independently a direct bond; a C1-C6 alkylene group substituted or unsubstituted with a fluorine atom; or -R 12 -OR 13 -and, The above R 12 and R 13 Each independently, a direct bond: or a compound in which a fluorine atom is a substituted or unsubstituted C1-C6 alkylene group.

10. In claim 8, The compound is a compound represented by the following chemical formula 1-c: [Chemical Formula 1-c] In the above chemical formula 1-c, n is an integer from 1 to 20, q is an integer from 1 to 20, and o is an integer from 1 to 20.

11. In claim 1, The above lithium salt is a compound containing a repeating unit represented by the following chemical formula 2: [Chemical Formula 2] In the above chemical formula 2, The above X, Y and Z are each independently at least one selected from the group consisting of the following chemical formulas a-1, b and c-1, The above n is an integer from 1 to 100, The above q is an integer from 1 to 100, The above o is an integer from 0 to 100, The above * indicates a connecting portion or terminal portion between repeating units, [Chemical formula a-1] [chemical formula b] [Chemical formula c-1] In the above chemical formulas a-1, b and c-1, The above R1, R2 and R3 are each independently a hydrogen element; a halogen element; -CN; -NO2; substituted or unsubstituted C1-C 10 Alkyl group of; substituted or unsubstituted C1-C 10 Alkoxy group; substituted or unsubstituted C2-C 10 Alkenyl group of; substituted or unsubstituted C2-C 10 an alkynyl group of; -C(=O)R5; -P(=O)(OR5)2; -P(OR5)(OR6); -OP(=O)(OR5)(OR6); -S(=O)R5; or -S(=O)2R5, The above R4 is a hydrogen atom; or a substituted or unsubstituted C1-C 10 is an alkyl group, The above R5 and R6 are each independently a hydrogen element; substituted or unsubstituted C1-C 10 an alkyl group of; or a substituted or unsubstituted C2-C 10 is an alkenyl group, The above L1, L2 and L3 are each independently a direct bond; or a substituted or unsubstituted C1-C 10 is an alkylene group, The above X1 and X2 are each independently a hydrogen element; a halogen element; -CN; -NO2; a substituted or unsubstituted C1-C 10 an alkyl group of; or a substituted or unsubstituted C6-C 12 is an aryl group, The above m is an integer from 1 to 40, The above p is an integer from 1 to 200.

12. In claim 11, A compound containing a repeating unit represented by the above chemical formula 2 is a compound represented by the following chemical formula 2-a or 2-b: [Chemical Formula 2-a] [Chemical Formula 2-b] In the above chemical formulas 2-a and 2-b, n is an integer from 1 to 20, q is an integer from 1 to 20, and o is an integer from 1 to 20.

13. In claim 11, A compound comprising at least one functional group selected from the group consisting of the following chemical formulae d to g at at least one terminal portion among the above terminal portions: [chemical formula d] [chemical formula e] [chemical formula f] [chemical formula g] In the above chemical formulas d to g, The above R7 is a hydrogen atom; or a substituted or unsubstituted C1-C 10 is an alkyl group, R8 to R above 11 are each independently, direct bond; substituted or unsubstituted C1-C 10 alkylene group of; or -R 12 -OR 13 -and, The above R 12 and R 13 are each independently, directly bonded; or substituted or unsubstituted C1-C 10 is an alkylene group, The above * indicates the binding position.

14. In claim 13, A compound containing a repeating unit represented by the above chemical formula 2 is a compound represented by the following chemical formula 2-c: [Chemical Formula 2-c] In the above chemical formula 2-c, n is an integer from 1 to 20, q is an integer from 1 to 20, and o is an integer from 1 to 20.

15. A complex comprising a compound according to claim 1 and a lithium compound.

16. In claim 15, The above lithium compounds are LiCl, LiBr, LiI, LiBF4, LiClO4, LiB 10 Cl 10 A complex comprising at least one selected from the group consisting of LiAlCl4, LiAlO4, LiPF6, LiCF3SO3, LiCH3CO2, LiCF3CO2, LiAsF6, LiSbF6, LiCH3SO3, LiFSI (lithium bis(fluorosulfonyl)imide, LiN(SO2F)2), LiBETI (lithium bisperfluoroethanesulfonimide, LiN(SO2CF2CF3)2) and LiTFSI (lithium (bis)trifluoromethanesulfonimide, LiN(SO2CF3)2).

17. In claim 15, The above complex is a complex represented by at least one selected from the group consisting of the following chemical formulas 3-a, 4-a and 4-b: [Chemical Formula 3-a] [Chemical Formula 4-a] [Chemical Formula 4-b] In the above chemical formulas 3-a, 4-a and 4-b, n is an integer from 1 to 20, q is an integer from 1 to 20, and o is an integer from 1 to 20.

18. A solid electrolyte comprising at least one selected from the group consisting of the compound of claim 1 and the complex of claim 15.

19. In claim 18, A solid electrolyte further comprising a crosslinking compound.

20. An all-solid-state battery comprising a solid electrolyte according to claim 19.

21. A compound represented by the following chemical formula A: [Chemical Formula A] In the above chemical formula A, The above R 21 , R 22 and R 23 are each independently a hydrogen element; a halogen element; a substituted or unsubstituted C1-C 10 Alkyl group of; substituted or unsubstituted C1-C 10 Alkoxy group; substituted or unsubstituted C2-C 10 an alkenyl group of; or a substituted or unsubstituted C2-C 10 is an alkynyl group, The above R 24 is a hydrogen element; or substituted or unsubstituted C1-C 10 is an alkyl group, Above L 21 and L 22 are each independently substituted or unsubstituted C1-C 10 alkylene group of; -P(=O)(OR 25 )-; -(C=O)-; -(S=O)-; or -S(=O)2-, Above X 21 and X 22 are each independently a halogen element; -NH2; phosphate (-OP(=O)(OR 25 )2); Nitrate(-ON(=O)(OR 25 )); tosylate (-OTs); sulfonate (-OS(=O)2R 25 ); or carboxylate (-OC(=O)CH3), The above R 25 is substituted or unsubstituted C1-C 10 Alkyl group of; substituted or unsubstituted C2-C 10 an alkenyl group of; or a substituted or unsubstituted C2-C 10 is an alkynyl group.

22. In claim 21, The above R 22 , R 24 and R 25 are each independently a compound which is an alkyl group of C1-C5.

23. In claim 21, Above L 21 and L 22 is a compound of -S(=O)2-.

24. In claim 21, Above X 21 and X 22 are each independently a halogen element or a compound that is -NH2.

25. In claim 21, The compound represented by the above chemical formula A is a compound selected from the group consisting of the following chemical formulas Aa, Ab and Ac: [Chemical formula Aa] [Chemical formula Ab] [Chemical formula Ac] 26. A complex comprising a compound according to claim 21 and a lithium compound.

27. In claim 26, The above complex is a complex represented by the following chemical formula B: [Chemical Formula B] In the above chemical formula B, The above R 21 , R 22 and R 23 are each independently a hydrogen element; a halogen element; a substituted or unsubstituted C1-C 10 Alkyl group of; substituted or unsubstituted C1-C 10 Alkoxy group; substituted or unsubstituted C2-C 10 an alkenyl group of; or a substituted or unsubstituted C2-C 10 is an alkynyl group, The above R 24 is a hydrogen element; or substituted or unsubstituted C1-C 10 is an alkyl group, Above L 21 and L 22 are each independently substituted or unsubstituted C1-C 10 alkylene group of; -P(=O)(OR 25 )-; -(C=O)-; -(S=O)-; or -S(=O)2-, Above X 21 and X 22 are each independently a halogen element; -NH2; phosphate (-OP(=O)(OR 25 )2); Nitrate(-ON(=O)(OR 25 )); tosylate (-OTs); sulfonate (-OS(=O)2R 25 ); or carboxylate (-OC(=O)CH3), The above R 25 is substituted or unsubstituted C1-C 10 Alkyl group of; substituted or unsubstituted C2-C 10 an alkenyl group of; or a substituted or unsubstituted C2-C 10 is an alkynyl group, Above Y - is a halogen anion, BF4 - , ClO4 - , AlCl4 - , AlO4 - , PF6 - , CF3SO3 - , CH3CO2 - , CF3CO2 - , AsF6 - , SbF6 - , CH3SO3 - , FSI - (bis(fluorosulfonyl)imide, N(SO2F)2 - ), BETI (lithium bisperfluoroethanesulfonimide, N(SO2CF2CF3)2 - ) and TFSI ((bis)trifluoromethanesulfonimide, N(SO2CF3)2 - ) is one or more selected from the group consisting of.

28. In claim 26, The above complex is a complex comprising at least one selected from the group consisting of the following chemical formulas Ba, Bb and Bc: [chemical formula Ba] [chemical formula Bb] [Chemical formula Bc] .

29. A polymer comprising a repeating unit derived from a compound according to claim 21, a repeating unit derived from a complex according to claim 26, or a combination thereof.

30. In claim 29, A polymer in which the repeating unit derived from the compound according to claim 21 is represented by the following chemical formula Wa or Wb: [chemical formula Wa] [Chemical formula Wb] In the above chemical formulas Wa and Wb, wherein n is an integer from 1 to 300, The above * indicates a connection between repeating units.

31. In claim 29, A polymer in which the repeating unit derived from the complex according to claim 26 is represented by the following chemical formula Xa or Xb: [chemical formula Xa] [chemical formula Xb] In the above chemical formulas Xa and Xb, Above Y - is a halogen anion, BF4 - , ClO4 - , AlCl4 - , AlO4 - , PF6 - , CF3SO3 - , CH3CO2 - , CF3CO2 - , AsF6 - , SbF6 - , CH3SO3 - , FSI - (bis(fluorosulfonyl)imide, N(SO2F)2 - ), BETI (lithium bisperfluoroethanesulfonimide, N(SO2CF2CF3)2 - ) and TFSI ((bis)trifluoromethanesulfonimide, N(SO2CF3)2 - ) is one or more selected from the group consisting of, The above n is an integer from 1 to 300, The above * indicates a connection between repeating units.

32. In claim 29, A polymer comprising a combination of repeating units derived from the compound according to claim 21 and repeating units derived from the complex according to claim 26, wherein the combination is represented by the following chemical formula Y or Z: [Chemical formula Y] [Chemical formula Z] In the above chemical formulas Y and Z, Above Y - is a halogen anion, BF4 - , ClO4 - , AlCl4 - , AlO4 - , PF6 - , CF3SO3 - , CH3CO2 - , CF3CO2 - , AsF6 - , SbF6 - , CH3SO3 - , FSI - (bis(fluorosulfonyl)imide, N(SO2F)2 - ), BETI (lithium bisperfluoroethanesulfonimide, N(SO2CF2CF3)2 - ) and TFSI ((bis)trifluoromethanesulfonimide, N(SO2CF3)2 - ) is one or more selected from the group consisting of, The above n and m are each independently an integer from 1 to 300, The above * indicates a connection between repeating units.

33. A solid electrolyte comprising a polymer according to claim 29.

Citation Information

Patent Citations

  • Ionically conductive composite hydrophilic membrane

    JP1985069140A

  • Novel conjugated fluorine-containing sulfimide single ion conductor polymer and preparation and application methods thereof

    CN109456484A

  • Additive for nonaqueous electrolyte, nonaqueous electrolyte, and electrical storage device

    KR1020130033363A

  • Sulfonimide-containing poly(arylene ether)s and poly(arylene ether sulfone)s, methods for producing the same, and uses thereof

    US20040236062A1

  • Fluoropolymer comprising pendent groups with ionic BIS(sulfonyl)imide moiety and perfluoroether terminal group

    WO2021198808A1