Adjusting cathode temperature in electrodeposition
Patent Information
- Application Number
- PCT/US2024/025536
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-03
- Filing Date
- 2024-04-19
- Publication Date
- 2024-11-07
Smart Images

Figure US2024025536_07112024_PF_FP_ABST
Abstract
Description
ADJUSTING CATHODE TEMPERATURE IN ELECTRODEPOSITIONBACKGROUND
[0001] Electrodeposition can be used in integrated circuit manufacturing processes to deposit electrically conductive films onto substrates. Electrodeposition systems comprise a cathode chamber through which a catholyte solution circulates, and an anode chamber through which an anolyte solution circulates. Electrodeposition involves the electrochemical reduction of dissolved ions of a selected metal from the catholyte to an elemental state on a substrate to form a film of the selected metal. Process parameters such as ion concentrations, additives, applied voltage, and bath temperature are carefully controlled so that a resulting metal film covers substrate features of different shapes with a desired profile.SUMMARY
[0002] This Summary is provided to introduce a selection of concepts in a simplified form that are further described below in the Detailed Description. This Summary is not intended to identify key features or essential features of the claimed subject matter, nor is it intended to be used to limit the scope of the claimed subject matter. Furthermore, the claimed subject matter is not limited to implementations that solve any or all disadvantages noted in any part of this disclosure.
[0003] Examples are disclosed that relate to controllably heating or cooling a cathode surface of a substrate to allow electrodeposition processes to be performed at different cathode temperatures. In one example, an electrodeposition tool comprises an anode chamber configured to hold an anolyte, a cathode chamber configured to hold a catholyte, and a clamshell assembly. The clamshell assembly is configured to position a substrate in the cathode chamber during an electrodeposition process so that a cathode surface of the substrate is exposed to the catholyte. The clamshell assembly comprises at least a cup comprising a substrate interface and a cone configured to clamp the substrate within the cup. The cone comprises a thermal regulator operable to adjust a temperature of the cathode surface of the substrate.
[0004] In some such examples, the thermal regulator additionally or alternatively comprises one or more thermoelectric devices.
[0005] In some such examples, the thermal regulator additionally or alternatively comprises two or more concentric annular thermoelectric devices.
[0006] In some such examples, the thermoelectric devices are additionally or alternatively operable to reverse polarity and change a direction of heat transfer between the cone and the substrate.
[0007] In some such examples, the thermal regulator is additionally or alternatively embedded within the wall of the cone.
[0008] In some such examples, the thermal regulator is additionally or alternatively coupled to an outer surface of a wall of the cone.
[0009] In some such examples, the thermal regulator additionally or alternatively changes the temperature of the cathode surface of the substrate by indirect heat transfer.
[0010] In some such examples, the clamshell assembly additionally or alternatively comprises at least one temperature sensor configured to provide an indication of a temperature of the cathode surface of the substrate.
[0011] Another example provides a clamshell assembly for an electrodeposition tool. The clamshell assembly comprises a cup comprising a substrate interface, and a cone configured to clamp a substrate within the cup so that a cathode surface of the substrate is exposed to an exterior of the clamshell assembly, the cone comprising a thermal regulator coupled to a wall of the cone, the thermal regulator operable to adjust a temperature of a cathode surface of the substrate.
[0012] In some such examples, the thermal regulator additionally or alternatively comprises one or more thermoelectric devices.
[0013] In some such examples, the thermal regulator additionally or alternatively comprises two or more concentric annular thermoelectric devices.
[0014] In some such examples, the thermoelectric devices are additionally or alternatively operable to reverse polarity and change a direction of heat transfer between the cone and the substrate.
[0015] In some such examples, the thermal regulator is additionally or alternatively embedded within the wall of the cone.
[0016] In some such examples the thermal regulator is additionally or alternatively coupled to an outer surface of a wall of the cone.
[0017] In some such examples, the thermal regulator changes the temperature of the cathode surface of the substrate by indirect heat transfer.
[0018] In some such examples, the clamshell assembly additionally or alternatively comprises at least one temperature sensor configured to provide an indication of a temperature of the cathode surface of the substrate.
[0019] Another example provides a method for operating an electrodeposition tool. The method comprises performing a first electrodeposition process at a cathode surface of a substrate at a first cathode temperature. A thermal regulator coupled to a wall of a cone of a clamshell assembly is operated to adjust a temperature at the cathode surface of the substrate. A second electrodeposition process is then performed at a second cathode temperature.
[0020] In some such examples, the first electrodeposition process and the second electrodeposition process are additionally or alternatively performed on a same substrate.
[0021] In some such examples, the thermal regulator is additionally or alternatively operated based at least on a predetermined electrodeposition routine.
[0022] In some such examples, the thermal regulator is additionally or alternatively operated based at least on observations made during the first electrodeposition process.BRIEF DESCRIPTION OF THE DRAWINGS
[0023] FIG. 1 shows a block diagram of an example electroplating tool.
[0024] FIG. 2 illustrates defects in a plated metal film profile for a substrate.
[0025] FIGS. 3A-3C schematically illustrate diffusion of leveler molecules into substrate features of increasing size.
[0026] FIG. 4 schematically shows filling performance for a relatively larger recessed feature at different temperatures.
[0027] FIGS. 5A-5B schematically show filling performance for a relatively smaller recessed feature at different temperatures.
[0028] FIG. 6 shows an example plot of catholyte viscosity as a function of catholyte temperature.
[0029] FIG. 7 shows an example plot of showing changes in limiting current as a function of viscosity across a range of temperatures.
[0030] FIG. 8 shows a schematic sectional view of a clamshell assembly for an electrodeposition tool.
[0031] FIGS. 9A-9B show examples of a thermoelectric device integrated into a wall of a cone of a clamshell assembly.
[0032] FIGS. 10A-10B show an example cone configured with a reversible thermoelectric device.
[0033] FIG. 11 shows a flow diagram depicting an example method for operating an electrodeposition tool.
[0034] FIG. 12 schematically shows an example computing system.DETAILED DESCRIPTION
[0035] The term “accelerator” generally represents an organic additive to a catholyte that is configured to increase a rate of electrodeposition on substrate surfaces.
[0036] The term “anode chamber” generally represents a physical structure configured to hold at least an anode and anolyte in an electrodeposition system.
[0037] The term “anolyte” generally represents a solution used in an anode chamber during an electrodeposition process.
[0038] The term “cathode chamber” generally represents a physical structure configured to hold at least a cathode and catholyte in an electrodeposition system.
[0039] The term “catholyte” generally represents a solution used in a cathode chamber during an electrodeposition process.
[0040] The term “clamshell assembly” generally represents a physical structure configured to support a substrate in an electrodeposition tool during an electrodeposition process. A clamshell assembly comprises a cup and a cone.
[0041] The term “cone” generally represents a structure that presses a substrate against a seal of the cup.
[0042] The term “cup” generally represents a physical device comprising a substrate interface configured to support and provide electrical conduction to a substrate during an electrodeposition process.
[0043] The terms “electrodeposition,” “electroplating,” “plating,” “deposition” “electrodeposition process” and variants thereof generally represent a process in which dissolved ions of one or more metals are reduced on a substrate surface to form a film of the one or more metals. The term “predetermined electrodeposition routine” generally represents a sequence of preset steps performed in an electrodeposition process.
[0044] The term “electrodeposition tool” generally represents a machine configured to perform electrodeposition.
[0045] The term “indirect heat transfer” generally represents a process where heat energy is transferred between two physical objects through an intermediate medium.
[0046] The term “leveler” generally represents an organic additive to a catholyte that promotes a deposition of a metal film having a more level profile than features of an underlying substrate surface.
[0047] The term “plating surface” generally represents a side of a substrate that is positioned within the catholyte during an electrodeposition process to receive growth of a metal film.
[0048] The term “plating temperature” generally represents a temperature of catholyte at a cathode surface of a substrate.
[0049] The term “recessed feature” generally represents a topographic structure of a substrate that extends from a surface of the substrate toward an interior of the substrate.
[0050] The term “substrate” generally represents any object on which a film can be deposited.
[0051] The term “substrate interface” generally represents a portion of a cup that comes in direct contact with the substrate.
[0052] The term “suppressor” generally represents an organic additive to a catholyte that inhibits electrodeposition of a metal film when present on a substrate surface.
[0053] The term “temperature sensor” generally represents a device that outputs an electrical signal in response to thermal conditions.
[0054] The term “thermal regulator” generally represents a device that, when active, can adjust a temperature of adjacent media.
[0055] The term “thermoelectric device” generally represents a device that comprises a circuit of at least two conductors and at least two junctions, such that maintaining an electric circuit within the circuit causes cooling of one junction and heating of another junction.
[0056] In an electrodeposition process, it can be desirable to deposit a metal film having a smooth surface with a substantially level profile. However, a substrate surface to be covered with an electrodeposited metal film can have features withvarying depths and widths. Electrodepositing a metal film with a uniform thickness across such a substrate can yield a film with a varying surface profile influenced by the profile of the underlying substrate.
[0057] One common surface profile irregularity arises where metal deposits in a recessed feature are thicker toward the outer edges of the feature than in a middle region of the recessed feature. This can be referred to as “dishing” due to the dish-like indented shape of the irregularity.
[0058] To help achieve the electrodeposition of a metal film with a substantially level height profile, organic additives such as levelers can be used in a plating solution. A leveler enhances bottom-up electrodeposition of metals in recessed features. More specifically, the leveler is configured to suppress plating of metal ions. The leveler is a relatively large molecule that diffuses relatively slowly to lower regions of recessed features. As such, the leveler binds preferentially to surfaces in upper regions of recessed features. This suppresses plating in the upper regions of the recessed features. In contrast, relatively lower concentrations of leveler reach lower regions of recessed features. This can allow for relatively higher rates of plating to occur in the lower regions. This allows a growing metal film to fill the lower regions of the recessed features more quickly than the upper regions. As a result, a more level metal film is deposited.
[0059] However, as described below, the effectiveness of a leveler can decrease as a size of a recessed feature increases. This is because the relatively large leveler molecules can diffuse more easily into relatively larger recessed features than into relatively smaller recessed features. Thus, dishing can be observed for larger features even where a leveler is used.
[0060] Electrodeposition is influenced by other process parameters than organic additives. Examples include plating voltage, plating current, ion concentrations, and plating temperature. Plating temperature influences bath conductivity, reaction kinetics and surface adsorption of additives. These parameters, in turn, impact the final filling performance and uniformity. More specifically, relatively lower plating temperatures can lead to less dishing in larger features than relatively higher plating temperatures. On the other hand, relatively lower plating temperatures can lead to relatively slower film deposition rates than relatively higher plating temperatures.
[0061] In view of the effects of temperature on electrodeposition performance, one possible method to reduce dishing without unduly impacting deposition rate is toperform a multi-layer deposition process. In such a process, different conditions can be used to electrodeposit different layers of a metal film. For example, a relatively lower plating temperature can be used when filling the lower regions of larger features. Then, the temperature can be increased for the deposition of subsequent layers to increase a film growth rate when filling the upper regions of the larger features.
[0062] However, changing plating temperature in a relatively short time scale is a challenge. Currently, plating temperatures are adjusted by adjusting the temperature of the catholyte bath. A catholyte bath in a commercial electrodeposition system can have a volume of 100 L (liters) or more. Thus, adjusting the temperature of a catholyte bath can take a significant amount of time and impact system throughput. Due to the difficulties of adjusting the temperature of a catholyte bath, electrodeposition tools are often operated with a catholyte bath maintained at a temperature that is selected as a compromise to balance throughput and metal film uniformity.
[0063] Another approach is to use different electrodeposition tools having different catholyte bath temperatures to perform electrodeposition at different plating temperatures. Integrated circuits often have other film layers between different copper layers. As such, transfer of substrates between tools, and / or revisits of a substrate to a same tool, often occur during device fabrication. However, in such a processing environment, assigning tools having certain bath temperatures for different metal layers can bring challenges for processing tool time management. For example, an electrodeposition tool assigned to one copper layer to be deposited at one temperature can get quite busy at times, while other electrodeposition tools assigned to other copper layers at other temperatures can be underutilized at those times. Despite having multiple tools available, the electrodeposition tools configured for other metals can’t help share the copper workload. This can result in lower throughput compared to performing electrodeposition in a single tool using a single plating temperature.
[0064] Accordingly, examples are disclosed that relate to controlling a plating temperature without changing the bath temperature of an electrodeposition system. Briefly, the temperature of the cathode is adjusted and maintained through a thermal regulator integrated in the cone of a clamshell assembly that interfaces with the substrate during electrodeposition. The thermal regulator thus can control the temperature at the surface of the substrate where electrodeposition occurs. This allows for the varying of plating temperatures throughout an electrodeposition process. Controlling the plating temperature as disclosed can allow for different metal layers anddifferent substrate features to be plated under specifically-tailored process conditions, rather than using a single plating temperature as a compromise.
[0065] Prior to discussing these examples in more detail, FIG. 1 schematically shows a block diagram of an example electrodeposition tool 100. Electrodeposition tool 100 comprises an electrodeposition cell 102 comprising an anode chamber 104 and a cathode chamber 106. Electrodeposition tool 100 further comprises a cation exchange membrane 108 separating the anode chamber 104 and the cathode chamber 106. Electrodeposition tool 100 further comprises a high resistance virtual anode (HRVA)109 within cathode chamber 106.
[0066] Anode chamber 104 comprises an anode 110. Anode chamber 104 further comprises an anolyte. Cathode chamber 106 comprises a catholyte. The catholyte comprises an ionic species to be deposited on a cathode layer of a substrate111 as a metal by electrochemical reduction. Anode 110 can comprise a consumable anode formed from the metal being deposited, or can comprise an inert anode. Where anode 110 comprises the metal being deposited, electrochemical oxidation of anode110 at least partially replenishes the ionic species consumed by the electrodeposition process. Bulk anolyte and / or catholyte solutions can be added at times to replenish the ionic species.
[0067] Cation exchange membrane 108 prevents organic species and anionic species from crossing between cathode chamber 106 and anode chamber 104, while allowing metal ions to cross from anode chamber 104 to cathode chamber 106. As mentioned above, HRVA 109 comprises an ionically resistive element that approximates a suitably constant and uniform current source in proximity to a substrate cathode.
[0068] Substrate holder 112 is coupled to a substrate holder movement system 113 comprising a lift 114 that is configured to adjust a spacing between substrate holder112 and HRVA 109. For example, lift 114 can lower substrate holder 112 to position substrate 111 within the catholyte for electrodeposition. Lift 114 further can raise substrate holder 112 from the catholyte after electrodeposition. Substrate holder movement system 113 further can comprise components to control the opening and closing of substrate holder 112.
[0069] The catholyte can be circulated between cathode chamber 106 and a catholyte reservoir 120 by a combination of gravity and one or more pumps 122.Likewise, the anolyte can be circulated through anolyte reservoir 124 and anode chamber 104 by a combination of gravity and one or more pumps 126.
[0070] In some electrodeposition tools, plating operations can be performed in parallel on multiple substrates using multiple plating cells. In some such examples, central catholyte and / or anolyte reservoirs can supply multiple plating cells with catholyte and / or anolyte. In other such examples, separate catholyte and / or anolyte reservoirs can be used to supply multiple plating cells. In yet other examples, an electrodeposition tool can comprise a single plating cell. Where an electrodeposition tool comprises multiple plating cells, a single lift can be configured to lift two or more substrate holders for two or more different plating cells.
[0071] Substrate holder 112 is lowered by lift 114 toward HRVA 109 after substrate 111 is loaded into substrate holder 112. Substrate 111 faces a surface of the HRVA 109, and is spaced from HRVA 109 by a plating gap during electrodeposition. An electric field is established between anode 110 and substrate 111. This electric field drives dissolved metal cations from anode chamber 104 into cathode chamber 106. At substrate 111, the metal cations are electrochemically reduced to deposit on substrate 111. An anodic potential is applied to anode 110 using charge plate 115 and a cathodic potential is provided to the cathode of substrate 111 via a cathode electrical connection 116 to form a circuit. In some examples, substrate holder 112 can be rotated using a rotational motor 117 during electrodeposition.
[0072] Substrate holder 112 includes thermal regulator 127, which can be employed to adjust a temperature at a plating surface of substrate 111. More detailed aspects and further examples of substrate holder 112 and thermal regulator 127 are described in more detail herein and with regard to FIGS. 8-10B.
[0073] Electrodeposition tool 100 further comprises a computing system 130, aspects of which are described in more detail below with regard to FIG. 12. Computing system 130 can comprise instructions executable to control any suitable functions of electrodeposition tool 100. In some examples, computing system 130 can be configured to communicate with a remote computing system 140 by a suitable computer network. Remote computing system 140 can comprise any suitable computing system. Examples include a networked workstation computer, an enterprise computing system, and / or a cloud computing system. It will be understood that remote computing system 140 can be in communication with and control a plurality of electrodeposition tools in some examples.
[0074] In some examples, one or more sensors can be positioned in and around electrodeposition cell 102 to monitor conditions and to provide indications of nonuniformity that can be indicative of dishing, erosion, or other plating irregularities. For example, electrodeposition cell 102 can include a cathode electrical sensor array 142 and / or an optical sensor 144. Cathode electrical sensor array 142 can monitor electrical current and / or voltage at different locations at substrate 111. Optical sensor 144 can be positioned to observe a surface of substrate 111 to provide visual monitoring of metal ion electrodeposition. Optical sensor 144 can comprise a photodiode, a camera, and / or any other suitable optical sensing device. Additional optical sensors, and / or other sensors, other than those shown can be positioned in and around electrodeposition cell 102. Signals generated by cathode electrical sensor array 142 and / or optical sensor 144 can be transmitted to computing system 130 for analysis, and control signals can be generated or adjusted based on such signals.
[0075] FIG. 2 shows a plated substrate 200 including a metal film 202 plated onto a substrate 204 that includes a plurality of features. The plurality of features include a pad area 206. Pad area 206 is a recessed feature, and has a depth 208 from the bottom 210 of pad area 206 to the top of planar area 212. The overall desired thickness of metal film 202 is shown at 214. In this example, the profile of metal film 202 roughly follows the shape of pad area 206, yielding a pad plating thickness 216 and a field plating thickness 218. As pad plating thickness 216 and field plating thickness 218 are roughly equal in depth, plated substrate 200 becomes underplated (dished) over pad area 206, as shown at 220. Other regions, such as prominence 222, can be overplated, as shown at 224.
[0076] In this example, the dishing defect is a result of the relatively larger width of pad area 206 compared to other features on substrate 204. The term “size” also can be used herein to refer to a width of a recessed feature. As mentioned above, to help mitigate dishing, a leveler can be added to the catholyte as an organic additive. For example, polyvinylpyrrolidone (PVP) can be used as a leveler for copper electrodeposition. The leveler helps to suppress plating of metal ions. The leveler is a relatively large molecule that diffuses relatively slowly to the bottom of features compared to other organic additives (such as an accelerator, described below). As such, the leveler binds preferentially to the upper surfaces. This suppresses plating in upper regions of a recessed feature more strongly than in lower regions of the recessed feature. The leveler can also suppress plating at prominences more strongly than on surfaceslower than the prominences. The relatively lower concentrations of leveler at a lower region within a recessed feature can allow for relatively higher rates of plating to occur. This allows plating to fill the lower region of the recessed feature more quickly than the upper region. As a result, a more level film is deposited.
[0077] However, as mentioned above, the performance of the leveler is dependent on the size of the feature. For example, a leveler may help to mitigate dishing for smaller features size (e.g. recessed features having a width of 3-5 pm) more effectively than for larger features (e.g., recessed features having dimensions on the order of 40-60 pm).
[0078] FIGS. 3A-3C schematically show a series of features having differing widths but similar depths. FIG. 3A illustrates a smaller feature 300. FIG. 3B shows a medium feature 310 having an intermediate width. FIG. 3C shows larger feature 320. Leveler molecules are shown as triangles.
[0079] In FIG. 3 A, leveler molecules diffuse primarily into an upper region 330 region of the smaller feature 300. Thus, film electrodeposition is much more strongly suppressed at the upper region 330 of the smaller feature 300 than in a lower region 335 of the relatively narrower smaller feature 300. For medium feature 310, more leveler molecules 325 are able to diffuse into the lower region 345 of medium feature 310 than for smaller feature 300. This reduces the effect of leveler 325 for the medium feature 310 compared to the smaller feature 300. Thus, the medium feature 310 may experience some dishing during electrodeposition. For larger feature 320, leveler 325 can diffuse to all surfaces with the larger feature 320 at similar rates. The leveler molecules that diffuse into the trench restrain the plating rate at the lower region 350 of the feature at a similar or same rate as at the upper region 355 of the feature. This leads to more pronounced dishing than for the medium feature.
[0080] One approach to reducing or eliminating dishing is to reduce the plating temperature. This can reduce a rate of diffusion of the leveler molecules into the lower regions of the larger feature 320. For example, for a copper electrodeposition process, a plating temperature of 19° C or even 17° C can be used initially to slow leveler diffusion into larger / wider features. Then, for relatively smaller / narrower features, the plating temperature can be increased to a temperature within a range of 21° C to 25° C for higher film growth rates.
[0081] FIG. 4 schematically shows examples films formed in relatively wider feature 320 at different plating temperatures. At 410, a film 415 resulting from a 21° Cplating bath is shown. At 420, a film 425 resulting from a 19° C plating bath is shown. The higher plating temperature, at 410, yields a higher step height 430, and thus more dishing, than the step height 440 for the lower plating temperature at 420. Hence, a lower plating temperature can help to reduce dishing compared to a higher plating temperature.
[0082] However, adjusting the bath temperature by even a few degrees can take several hours. This cannot be performed quickly between segments of an electrodeposition routine, or between substrates without significant loss of throughput. It is possible to assign different tools within a facility for different plating conditions. However, such a strategy may not be an optimally efficient solution.
[0083] Further, lower deposition temperatures can cause problems for plating smaller features. This is because the lower deposition temperatures can affect other plating bath conditions than the leveler diffusion rates. For example, other organic molecules, such as accelerators and suppressors, are often used in plating baths in addition to levelers. For copper electrodeposition, bis[3-sulfopropyl]) disulfide (SPS) is a common accelerator, and polyethylene glycol] (PEG) and PVP are common suppressors.
[0084] A suppressor acts to locally suppress plating by polarizing feature sidewalls. An accelerator acts to locally accelerate plating. Suppressors, accelerators, and levelers have different molecular sizes. The accelerator molecule is the smallest. Thus, the accelerator molecules can diffuse to the bottom of features, encouraging rapid plating growth deep in the trenches of these features. The suppressor molecule is larger than the accelerator molecule. The leveler molecule is larger than the suppressor molecule. Utilizing these components in suitable proportions can promote the desired growth profile in many features.
[0085] However, lower temperatures used for reducing the rate of diffusion of the leveler can impact the plating of a metal film in smaller feature 300. This is illustrated in FIGS. 5A and 5B. First, FIG. 5A illustrates example diffusion behaviors of suppressor, accelerator, and level molecules at 21° C in smaller feature 300. Smaller feature 300 is shown at 512 at initiation of electrodeposition at 21° C. Smaller feature 300 comprises a seed metal layer 540. Seed metal layer 540 provides an electrically conductive surface for electrodeposition. Suppressor 532, accelerator 534, and leveler 536 molecules are depicted respectively as ovals, diamonds, and triangles. At 21° C, accelerator 534 diffuses easily into lower region 541 of substrate feature 510. Lesssuppressor 532 diffuses into lower region 541. Even less leveler 536 diffuses into lower region 541. As a result, referring to 515, substrate feature 510 fills evenly with metal layer 542A.
[0086] FIG. 5B illustrates example diffusion behaviors of suppressor, accelerator, and level molecules at 19° C in smaller feature 300, with otherwise equivalent reaction conditions to FIG. 5A. Smaller feature 300 is shown at 525 at initiation of electrodeposition at 21° C. At 19° C, accelerator 534 diffuses more slowly than at 21° C. Tus, accelerator does not reach surfaces in the lower region 541 at desired concentrations. Accordingly, metal layer 542B grows less evenly.
[0087] As shown in FIGS. 4, 5A and 5B, cooling the system down can positively impact plating performance for large pad areas (e.g., as shown in FIG. 4), but can negatively impact plating performance for smaller features (e.g., as shown in FIG. 5B). Conversely, heating the system can negatively impact plating performance for large pad areas (e.g., as shown in FIG. 4), but increase plating performance for smaller features (e.g., as shown in FIG. 5A).
[0088] The differing rates of diffusion of the organic additives are due at least in part to an increase in plating bath viscosity as the temperature decreases. FIG. 6 shows an idealized plot 600 indicating a decrease in viscosity of an aqueous solution corresponding to an increase in temperature of the solution. The decrease in temperature also causes the diffusion coefficient of metal ions to decrease.
[0089] The increase in viscosity and decrease in diffusion coefficient results in a lower limiting current during plating. A higher temperature can be needed to meet desired plating currents. The viscosity of an electrolyte solution including copper ions is represented by Eq. 1. In this example, ii,cis limiting current, where n is the number of electrons for the plating (red / ox) reaction (e.g., 2 for copper). F is the Faraday constant, A is area, Do is the diffusion coefficient of Cu2+ions, co is the rotation speed, v the viscosity, and [Cu]* is the concentration of Cu2+ions in the electrolyte.
[0090] As such, the limiting current (e.g., the highest attainable current for a device and set of conditions) also increases as the solution temperature goes up. FIG. 7 is a plot 700 showing current vs working electrode potential (voltage) for an Hg / HgSCh (saturated K2SO4) solution across a range of solution temperatures. As shown, as the solution temperature increases, the limiting current also increases.
[0091] Maximum growth rates of electrodeposition films are a function of limiting current. When the plating bath temperature is decreased to avoid dishing in relatively larger features, ion movement slows. This lowers the limiting current. In turn, this results is reduced maximum deposition rates. Further, as described above, this also can result in dishing in relatively smaller features.
[0092] The ability to closely control the plating environment temperature can allow for more precise electrodeposition routines that result in more uniform plating with less dishing or cratering effects. To avoid having to adjust a cathode bath temperature, the disclosed examples control the temperature of the catholyte in proximity to the cathode surface of the substrate. This can allow the plating temperature to be quickly changed during an electrodeposition process.
[0093] As mentioned above, to provide such control, the disclosed examples comprise a thermal regulator integrated into a cone of the clamshell assembly. For example, a thermoelectric device can be used as a thermal regulator. Through indirect heat transfer through the cone, the thermal regulator can rapidly change the temperature of the plating surface and thus the catholyte in proximity to the cathode surface of the substrate. The overall temperature of the bulk catholyte is not significantly altered, allowing the solubility and stability of the dissolved molecules in the catholyte to be maintained.
[0094] FIG. 8 shows a schematic sectional view of a clamshell assembly 800 for an electrodeposition tool. Clamshell assembly 800 is configured to hold a substrate during an electrodeposition process. Clamshell assembly 800 is an example of a substrate holder, such as substrate holder 112 of FIG. 1. Clamshell assembly 800 can be used to hold a substrate, such as substrate 111 of FIG. 1.
[0095] Clamshell assembly 800 comprises a cone 802 and a cup 804. Cup 804 comprises a substrate interface 806 that is configured to support a substrate 808. Substrate 808 is an example of a substrate 111 of FIG. 1. Substrate 808 comprises a cathode surface 809. Substrate interface 806 comprises a lip seal 810 and a plurality of electrical contacts 812. Lip seal 810 makes physical contact with substrate 808 to prevent plating solution from reaching electrical contacts 812 during electrodeposition. Each electrical contact of the plurality of electrical contacts 812 make electrical contact with substrate 808 at a location behind lip seal 810. Electrical contacts 812 are attached to a metal frame 813, which provides mechanical support and electrical conduction.
[0096] Cup 804 is supported by struts 814, which connect to other portions of clamshell assembly 800, such as a vertical lift. A position of cone 802 relative to cup 804 is controllable to selectively press substrate 808 against lip seal 810 with cone 802, and to allow substrate 808 to be removed from cup 804. In such a configuration, cone 802 can contact the entire backside of substrate 808.
[0097] Clamshell assembly 800 further comprises a top plate 816 and a spindle 818. Spindle 818 can be mechanically connected to a motor controllable to rotate clamshell assembly 800. Substrate 808 can be lowered towards a plating bath such that cathode surface 809 of substrate 808 is immersed in the plating bath during electroplating. Downward force applied by a substrate interface 819 of cone 802 helps form a fluid tight seal between substrate 808 and lip seal 810 during electroplating. This helps to isolate electrical contacts 812 from the plating bath.
[0098] Cone 802 further comprises a thermal regulator 820 coupled to a wall 822 of cone 802. Cone 802 is configured to clamp substrate 808 within cup 804 so that cathode surface 809 of substrate 808 is exposed to an exterior of clamshell assembly 800. Thermal regulator 820 is operable to adjust a temperature of a cathode surface 809 of substrate 808 during an electrodeposition process. Thermal regulator 820 can be attached to an outer surface of wall 822 or cone 802, and / or partially or fully embedded into wall 822 of cone 802. Thermal regulator 820 can operate by a conductive mechanism, a convective mechanism, and / or a radiative mechanism in various examples. For example, thermal regulator 820 can include a thermoelectric cooling device, a water cooling device, and / or any other suitable heat transfer mechanism.
[0099] In some examples, thermal regulator 820 can include a single device that can heat and cool substrate 808. For example, thermal regulator 820 can include a Peltier device, which operates as a solid-state active heat pump. In other examples, thermal regulator 820 can include separate heating and cooling devices. For example, separate thermoelectric devices can be used for heating and or cooling.
[0100] In some examples, thermal regulator 820 can be a continuous device that extends around the periphery of cone 802. Alternatively, thermal regulator 820 can include two or more pieces, or one discontinuous piece. FIG. 8 includes a dashed vertical line 821 that schematically illustrates thermal regulator 820 being separated into two or more separate pieces.
[0101] In some examples, thermal regulator 820 changes the temperature of cathode surface 809 of substrate 808 by indirect heat transfer. For example, as shownin FIG. 8, thermal regulator 820 may not directly contact substrate 808. Rather, heat is transferred between thermal regulator 820 and substrate 808 through wall 822 of cone 802. Substrate 808, as typically configured within cup 804, comprises sufficient thermal connectivity and coupling to cone 802 to support indirect heat transfer. In other examples, thermal regulator 820 can be in direct contact with substrate 808.
[0102] Referring to Equation 1 above, changing the temperature at cathode surface 809 will affect some of the constants related to the properties of the catholyte. For example, the diffusion constant will increase with increased temperature. Also, the viscosity will decrease with increased temperature. As such, increasing temperature at cathode surface 809 yields a higher limiting current in the proximity of substrate 808. While these effects will not be seen throughout the catholyte bath, the effects will be seen in proximity to cathode surface 809. The diffusion behavior of the organic additives to the catholyte can thus be actively adjusted to meet different requirements for plating different layers of metal to achieve a desired film profile.
[0103] Clamshell assembly 800 can also include a temperature sensor 826 configured to provide an indication of the temperature of cathode surface 809 of substrate 808. Temperature sensor 826 can also be integrated into wall 822 of cone 802, can be integrated into thermal regulator 820, or can be in direct connection with substrate 808 and / or cathode surface 809. When not directly coupled to substrate 808, temperature sensor 826 can be subject to calibration to predict the temperature of cathode surface 809. For example, this can allow the temperature at thermal regulator 820 to be monitored and adjusted in order to enact a specific change at cathode surface 809. In this manner, the cathode temperature becomes a parameter that can be adjusted by a controller to adjust the filling performance of the electrodeposition tool. This parameter can be adjusted between substrates or during electroplating of a single substrate.
[0104] FIG. 9A depicts another example cone assembly 900. Cone assembly 900 comprises a cone 902 having a wall 904, an outer assembly ring 906, a slip ring 908, and a top plate 910. Slip ring 908 and top plate 910 can be coupled to a spindle and motor controllable to rotate cone assembly 900. Cone assembly 900 further comprises a thermal regulator 912.
[0105] Thermal regulator 912 is depicted as a single piece, solid-state thermoelectric device located within an interior cone 902 as defined by a wall 904 of cone 902. Although described as a single thermoelectric device, thermal regulator 912can have multiple segments, as described for thermal regulator 820. In such examples, the segments of the thermoelectric device can be subject to a common control signal, so that thermal regulator 912, and thus cone 902, has a uniform thermal profile. Employing a single, flat surface can simplify routine maintenance activities when cleaning and wiping are required.
[0106] Thermal regulator 912 can be manufactured into different shapes with a hollow circle in the middle to circumvent slip ring 908 at the center of the cone. Thermal regulator 912 further can be embedded at least partially within wall 904 of cone 902.
[0107] FIG. 9B shows a second example cone assembly 920. Cone assembly 920 comprises a cone 922 having a wall 924, an outer assembly ring 926, a slip ring 928, and a top plate 930. Cone assembly 920 further comprises a thermal regulator 932. Thermal regulator 932 comprises concentric annular thermoelectric devices 934, 936, 938 having a range of radii. While three multiple concentric annular thermoelectric devices are shown, more or fewer can be included, such as two or more. Using multiple, smaller, concentric thermoelectric devices can require less overall energy transfer, and thus less voltage than for a single, large thermoelectric device. Further, additional levels of regulation can be provided by employing multiple thermoelectric devices. For example, the power output of each concentric thermoelectric device can be adjusted individually, allowing for additional fine-tuning of the plating profile during an electrodeposition process.
[0108] At present, the walls of clamshell assembly cones are most commonly manufactured from polyethylene terephthalate (PET) based materials. PET acts to seal the substrate into the clamshell assembly, and also to maintain a consistent pressure on the substrate. However, the thermal conductivity of PET is relatively low (0.3 W / (mK)). Thus, it can be challenging to move heat through the wall of the cone fast enough to rapidly change the temperature of the cathode. As such, it can take a relatively large power supply to change the temperature of the cathode by more than a few degrees.
[0109] To combat this, one example comprises integrating more thermally conductive materials in the substrate interface region of the wall of the cone. An example substrate interface region is shown in FIG. 8 at 819. Other materials such as silicon carbide (SiC) and aluminum nitride (AIN) have higher thermal conductivities than PET (270, 310 W / (mK) for SiC and AIN respectively), and thus can achieve a higher rate of heat transfer between the thermal regulator and the substrate than for PET. SiC and AIN are also electro-isolating materials. Such materials can help to shapethe electric field in the cell. Other materials can be employed at the interface, though metal and other high thermal conducting material can interfere with the electrical field at the substrate.
[0110] For at least the reasons described above, the electrodeposition process may be impinged upon by placing a highly conductive thermal regulator in direct contact with the substrate. As such, a PET buffer can be provided that interfaces with the substrate. In some examples, layers of SiC, AIN, and / or other materials that have higher thermal conductivities can be integrated into the wall of a PET cone, rather than manufacturing the entire cone wall from such materials. Such materials could be integrated on the substrate-interfacing side to promote heat transfer between the thermal regulator and the substrate. Such materials could also be integrated on the substrate- distal side of the cone to generate a larger thermal sink, thus improving heat transfer.
[0111] Compared to thermal regulators that use a heat transfer fluid such as water, a solid-state construction thermoelectric device does not need a heat transfer fluid. This can allow integration of a solid state thermal regulator into a cone without the giving rise to the potential for leaking or tangled piping issues. The flat construction and light weight of the solid-state cooler further can avoid negatively impacting rotation of the clamshell during electrodeposition. When combined with a temperature sensor and a controller, an automatic control system can be formed to adjust the substrate temperature in near real-time.
[0112] In some examples, the thermal regulator comprises separate heating and cooling devices. Each of the heating and cooling devices can comprise a separate thermoelectric device, for example. In other examples, the thermal regulator comprises thermoelectric devices that are operable to reverse polarity and change a direction of heat transfer between the cone and the substrate. Thus, heating and cooling devices are combined in one component. For example, thermoelectric cooling systems rely on current flowing through two different types of conductors. When direct current (DC) voltage is applied and direct current runs from one conductor to the other, a change in temperature is generated at the junction where the two conductors join. Reversing a direction of current reverses a direction of heat flow.
[0113] FIGS. 10A and 10B schematically show an example of a thermoelectric device 1000 in forward and reverse polarities, respectively. Thermoelectric device 1000 comprises an N-type semiconductor 1002 and a P-type semiconductor 1004. N-type semiconductor 1002 and a P-type semiconductor 1004 are electrically coupled byelectrical contact 1006. While one pair of semiconductors is shown, multiple pairs can be coupled between two ceramic plates to increase the heating / cooling effect. A DC voltage source 1008 drives a current between N-type semiconductor 1002 and a P-type semiconductor 1004. While shown as series circuit, in other examples, a parallel circuit could be employed.
[0114] Thermoelectric device 1000 is schematically shown as embedded within a wall 1010 of a cone 1012 of a clamshell assembly. A thermoelectric device also can be attached to a wall of a cone, rather than being embedded in the cone. Thermoelectric devices allow for the application of a voltage that drives heat transfer between faces of the thermoelectric device. Maintaining a voltage across the thermoelectric device allows for the device to pump heat in the selected direction.
[0115] In FIG. 10A, DC voltage source 1008 is driving a current in a first direction (through P-type semiconductor 1004 followed by N-type semiconductor1002). In this configuration, cold face 1020 is proximal to substrate 1022, while heat dissipation face 1024 is distal to substrate 1022. In this configuration, the cold side of thermoelectric device 1000 can be faced down (e.g., towards substrate 1022) to adsorb the heat from the bottom of cone 1012. The hot side of the thermoelectric device 1000 would thus be exposed to ambient temperatures. This cools the cathode surface of the substrate.
[0116] The thermoelectric device effectively acts as a dipole. If one side is cooling the system down, the other side will dissipate the heat. The polarity of the thermoelectric device can thus be reversed to drive heat transfer in either of two directions. In FIG. 10B, DC voltage source 1008 is driving a current in a second direction (through N-type semiconductor 1002 followed by P-type semiconductor 1004). In this configuration, heat dissipation face 1032 is proximal to substrate 1022, while cold face 1034 is distal to substrate 1022. This heats the cathode surface of the substrate. In this manner, the thermoelectric device can operate to heat or cool the cathode surface of the substrate and thereby influence plating behaviors without changing the temperature of the entire catholyte bath.
[0117] When operated to cool the cathode surface of the substrate, heat dissipation can be accomplished by the high-speed rotation of the clamshell itself during the electrodeposition process. When operated to heat the cathode surface of the substrate, the catholyte acts as the heat sink, and heat is removed as the catholyte is constantly circulated through the catholyte reservoir.
[0118] For different electrodeposition processes, different temperature profiles can be programmed. For example, temperatures can be changed when changing a bath component, changing the plating metal, and / or when fine-tuning electrodeposition for the features and topology of the substrate, allowing features to be approached sequentially. For examples, large pad areas and smaller features could be targeted separately. Changes in temperature can be preprogrammed, or can be reactive to sensed conditions, such as sensed temperature. For example, reactive changes in temperature can be performed by optical inspection of the plating surface of the substrate, or through analysis and monitoring of the plating voltage in constant current electrodeposition processes.
[0119] FIG. 11 shows a flow diagram illustrating an example method 1100 for operating an electrodeposition tool that has a thermal regulator coupled to the wall of a cone of a clamshell assembly. Method 1100 can be used to operate electrodeposition tool 100, for example. Method 1100 can be executed by a controller communicatively coupled to the electrodeposition tool, such as computing system 130.
[0120] At 1100, method 1100 comprises performing a first electrodeposition process at a cathode at a first cathode temperature. For example, a predetermined electrodeposition routine can have an initial temperature for depositing a first layer in a metal film at a first temperature.
[0121] At 1120, method 1100 comprises operating a thermal regulator of a cone of a clamshell assembly to adjust a temperature of the cathode. In some examples, the thermal regulator is operated based at least on observations made during the first electrodeposition process. One or more sensors can be positioned in and around the cathode to observe conditions. Signals from the one or more sensors can provide indications of conditions that can cause dishing, erosion, or other plating irregularities. For example, the observations can be optical observations of the plating surface of the substate, electrical observations (e.g., current, voltage) of the plating cell and / or substrate, and / or chemical observations of the catholyte.
[0122] Operating the thermal regulator to adjust cathode temperature further can allow for adjusting plating conditions based on changes in plating conditions. Conditions that can change over time include concentrations and / or composition of catholyte ions, bath additives, etc. In some examples, the thermal regulator can be operated to maintain a temperature of the catholyte (e.g., if bath / operating conditions drift or change). Further, each incoming substrate is somewhat unique, even comparedto substrates from the same batch. This may be manifested as varying substrate resistance and plating voltage. Such variances can be offset at least in part by adjusting the plating temperature as disclosed herein.
[0123] At 1130, method 1100 comprises performing a second electrodeposition process at the cathode at a second cathode temperature. The second cathode temperature may be higher or lower than the first cathode temperature. As described herein, raising and lowering the cathode temperature can be performed by a single thermal regulator device, or by two separate devices. In some examples, the first electrodeposition process and the second electrodeposition process are performed on a same substrate. However, the first electrodeposition process and the second electrodeposition process can additionally or alternatively be performed on different substrates. In some scenarios, method 1100 can be extended to include third, fourth, or more electrodeposition processes, with temperature changes between some or all of the electrodeposition processes.
[0124] FIG. 12 schematically shows an example of a computing system 1200 that can enact one or more of the methods and processes described above. Computing system 1200 is shown in simplified form. Computing system 1200 can take the form of one or more personal computers, workstations, computers integrated with substrate processing tools, and / or network accessible server computers.
[0125] Computing system 1200 includes a logic machine 1202 and a storage machine 1204. Computing system 1200 can optionally include a display subsystem 1206, input subsystem 1208, communication subsystem 1210, and / or other components not shown in FIG. 12. Computing system 130 is an example of computing system 1200.
[0126] Logic machine 1202 includes one or more physical devices configured to execute instructions. For example, the logic machine can be configured to execute instructions that are part of one or more applications, services, programs, routines, libraries, objects, components, data structures, or other logical constructs. Such instructions can be implemented to perform a task, implement a data type, transform the state of one or more components, achieve a technical effect, or otherwise arrive at a desired result.
[0127] The logic machine can include one or more processors configured to execute software instructions. Additionally or alternatively, the logic machine can include one or more hardware or firmware logic machines configured to execute hardware or firmware instructions. Processors of the logic machine can be single-coreor multi-core, and the instructions executed thereon can be configured for sequential, parallel, and / or distributed processing. Individual components of the logic machine optionally can be distributed among two or more separate devices, which can be remotely located and / or configured for coordinated processing. Aspects of the logic machine can be virtualized and executed by remotely accessible, networked computing devices configured in a cloud-computing configuration.
[0128] Storage machine 1204 includes one or more physical devices configured to hold instructions 1212 executable by the logic machine to implement the methods and processes described herein. When such methods and processes are implemented, the state of storage machine 1204 can be transformed — e.g., to hold different data.
[0129] Storage machine 1204 can include removable and / or built-in devices. Storage machine 1204 can include optical memory (e.g., CD, DVD, HD-DVD, Blu- Ray Disc, etc.), semiconductor memory (e.g., RAM, EPROM, EEPROM, etc.), and / or magnetic memory (e.g., hard-disk drive, floppy-disk drive, tape drive, MRAM, etc.), among others. Storage machine 1204 can include volatile, nonvolatile, dynamic, static, read / write, read-only, random-access, sequential-access, location-addressable, file- addressable, and / or content-addressable devices.
[0130] It will be appreciated that storage machine 1204 includes one or more physical devices. However, aspects of the instructions described herein alternatively can be propagated by a communication medium (e.g., an electromagnetic signal, an optical signal, etc.) that is not held by a physical device for a finite duration.
[0131] Aspects of logic machine 1202 and storage machine 1204 can be integrated together into one or more hardware-logic components. Such hardware-logic components can include field-programmable gate arrays (FPGAs), program- and application-specific integrated circuits (PASIC / ASICs), program- and applicationspecific standard products (PSSP / ASSPs), system-on-a-chip (SOC), and complex programmable logic devices (CPLDs), for example.
[0132] When included, display subsystem 1206 can be used to present a visual representation of data held by storage machine 1204. This visual representation can take the form of a graphical user interface (GUI). As the herein described methods and processes change the data held by the storage machine, and thus transform the state of the storage machine, the state of display subsystem 1206 can likewise be transformed to visually represent changes in the underlying data. Display subsystem 1206 can include one or more display devices utilizing virtually any type of technology. Suchdisplay devices can be combined with logic machine 1202 and / or storage machine 1204 in a shared enclosure, or such display devices can be peripheral display devices.
[0133] When included, input subsystem 1208 can comprise or interface with one or more user-input devices such as a keyboard, mouse, or touch screen. In some examples, the input subsystem can comprise or interface with selected natural user input (NUI) componentry. Such componentry can be integrated or peripheral, and the transduction and / or processing of input actions can be handled on- or off-board. Example NUI componentry can include a microphone for speech and / or voice recognition, and an infrared, color, stereoscopic, and / or depth camera for machine vision and / or gesture recognition.
[0134] When included, communication subsystem 1210 can be configured to communicatively couple computing system 1200 with one or more other computing devices. Communication subsystem 1210 can include wired and / or wireless communication devices compatible with one or more different communication protocols. As non-limiting examples, the communication subsystem can be configured for communication using a wireless telephone network, or a wired or wireless local- or wide-area network. In some examples, the communication subsystem can allow computing system 1200 to send and / or receive messages to and / or from other devices using a network such as the Internet.
[0135] It will be understood that the configurations and / or approaches described herein are exemplary in nature, and that these specific examples or examples are not to be considered in a limiting sense, because numerous variations are possible. The specific routines or methods described herein can represent one or more of any number of processing strategies. As such, various acts illustrated and / or described can be performed in the sequence illustrated and / or described, in other sequences, in parallel, or omitted. Likewise, the order of the above-described processes can be changed.
[0136] The subject matter of the present disclosure includes all novel and non- obvious combinations and sub-combinations of the various processes, systems and configurations, and other features, functions, acts, and / or properties disclosed herein, as well as any and all equivalents thereof.
Claims
CLAIMS:
1. An electrodeposition tool, comprising: an anode chamber configured to hold an anolyte; a cathode chamber configured to hold a catholyte; and a clamshell assembly configured to position a substrate in the cathode chamber during an electrodeposition process so that a cathode surface of the substrate is exposed to the catholyte, the clamshell assembly comprising at least: a cup comprising a substrate interface; and a cone configured to clamp the substrate within the cup, the cone comprising a thermal regulator operable to adjust a temperature of the cathode.
2. The electrodeposition tool of claim 1, wherein the thermal regulator comprises one or more thermoelectric devices.
3. The electrodeposition tool of claim 2, wherein the thermal regulator comprises two or more concentric annular thermoelectric devices.
4. The electrodeposition tool of claim 2, wherein the thermoelectric devices are operable to reverse polarity and change a direction of heat transfer between the cone and the substrate.
5. The electrodeposition tool of claim 1, wherein the thermal regulator is embedded within a wall of the cone.
6. The electrodeposition tool of claim 1, wherein the thermal regulator is coupled to an outer surface of a wall of the cone.
7. The electrodeposition tool of claim 1, wherein the thermal regulator is configured to change the temperature of the cathode by indirect heat transfer.
8. The electrodeposition tool of claim 1, wherein the clamshell assembly further comprises at least one temperature sensor configured to provide an indication of a temperature of the cathode.
9. A clamshell assembly for an electrodeposition tool, comprising:a cup comprising a substrate interface; and a cone configured to clamp a substrate within the cup so that a cathode surface of the substrate is exposed to an exterior of the clamshell assembly, the cone comprising a thermal regulator operable to adjust a temperature of the cathode surface of the substrate.
10. The clamshell assembly of claim 9, wherein the thermal regulator comprises one or more thermoelectric devices.
11. The clamshell assembly of claim 10, wherein the thermal regulator comprises two or more concentric annular thermoelectric devices.
12. The clamshell assembly of claim 10, wherein the thermoelectric devices are operable to reverse polarity and change a direction of heat transfer between the cone and the substrate.
13. The clamshell assembly of claim 10, wherein the thermal regulator is embedded within a wall of the cone.
14. The clamshell assembly of claim 10, wherein the thermal regulator is coupled to an outer surface of a wall of the cone.
15. The clamshell assembly of claim 10, wherein the thermal regulator changes the temperature of the cathode by indirect heat transfer.
16. The clamshell assembly of claim 10, further comprising: at least one temperature sensor configured to provide an indication of a temperature of the cathode.
17. A method for operating an electrodeposition tool, comprising: performing a first electrodeposition process at a cathode at a first cathode temperature; operating a thermal regulator coupled to a wall of a cone of a clamshell assembly to adjust a temperature of the cathode; andperforming a second electrodeposition process at a second cathode temperature.
18. The method of claim 17, wherein the first electrodeposition process and the second electrodeposition process are performed on a same substrate.
19. The method of claim 17, where the thermal regulator is operated based at least on a predetermined electrodeposition routine.
20. The method of claim 17, where the thermal regulator is operated based at least on observations made during the first electrodeposition process.
Citation Information
Patent Citations
Plating method and plating apparatus
JP2005146398A
Method of electro-chemical plating
US10954602B1
Temperature-controlled substrate holder for processing in fluids
US20040084143A1
Method and apparatus for electroplating
US20050224359A1
Heated workpiece holder for wet plating bath
US6221437B1