Low-temperature liquid-phase synthesis of lithium thiophosphate-borohydride solid electrolyte with high room-temperature ionic conductivity

The scalable low-temperature liquid-phase synthesis of lithium thiophosphate-borohydride solid electrolytes addresses the limitations of existing methods by producing electrolytes with high ionic conductivity and stability, enhancing the performance of lithium-sulfur all-solid-state batteries.

WO2024229218A1PCT designated stage expired Publication Date: 2024-11-07THE PENN STATE RES FOUND INC

Patent Information

Application Number
PCT/US2024/027407
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-03
Filing Date
2024-05-02
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

Current lithium thiophosphate solid electrolytes for all-solid-state batteries face challenges in scalability, electrochemical stability, cost, and density, with high-temperature synthesis methods resulting in low ionic conductivity and poor electrochemical stability.

Method used

A scalable low-temperature liquid-phase synthesis technique for lithium thiophosphate-borohydride solid electrolytes is developed, using a method involving precursors like Li2S and P2S5 in organic solvents, with stirring and annealing at controlled temperatures to produce electrolyte materials with high ionic conductivity and small particle size.

Benefits of technology

The technique yields electrolytes with high room-temperature ionic conductivity, good formability, and electrochemical stability, enabling high-performance lithium-sulfur all-solid-state batteries with improved cycle life and energy density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US2024027407_07112024_PF_FP_ABST
    Figure US2024027407_07112024_PF_FP_ABST
Patent Text Reader

Abstract

Embodiments relate to a scalable liquid-phase synthesis technique of lithium thiophosphate-borohydride solid electrolytes with high ionic conductivity at room temperature and its use in all-solid-state lithium batteries. A battery comprises an anode, a cathode, and a solid electrolyte layer positioned between the anode and the cathode. The liquid-phase synthesized solid electrolyte material can be used as the solid electrolyte layer or incorporated into anodes or cathodes.
Need to check novelty before this filing date? Find Prior Art

Description

LOW-TEMPERATURE LIQUID-PHASE SYNTHESIS OF LITHIUM THIOPHOSPHATE-BOROHYDRIDE SOLID ELECTROLYTE WITH HIGH ROOMTEMPERATURE IONIC CONDUCTIVITYCROSS-REFERENCE TO RELATED APPLICATIONS

[0001] This application claims priority to U.S. Provisional Patent Application No. 63 / 499,769, which was filed on May 3, 2023. The entirety of this application is incorporated by reference herein.STATEMENT REGARDING FEDERALLY SPONSORED RESEARCH DEVELOPMENT

[0002] This invention was made with government support under Grant No. DE-EE0008862 awarded by the Department of Energy. The Government has certain rights in the invention. FIELD OF THE INVENTION

[0003] Embodiments relate to a scalable liquid-phase synthesis technique of lithium thiophosphate-borohydride solid electrolytes and its use in all-solid-state lithium batteries. BACKGROUND OF THE INVENTION

[0004] Energy-dense, safe, and durable lithium all-solid-state battery (AS SB) utilizing inorganic solid electrolytes (SEs) is one of the most promising next-generation technologies for portable electronics, electric vehicles, and grid energy storage systems. The key to realizing such technology lies in developing and manufacturing SEs with desired properties, including high ionic conductivity, nonflammability, good electrochemical stability against both anode and cathode, good formability, scalability, low density, low cost, etc. Among various inorganic SEs, lithium thiophosphate SEs have garnered the most attention due to their highest ionic conductivity (10"4-l 0“2mS cm1) and good formability. However, they still fall short of meeting the desired criteria, particularly regarding scalability, electrochemical stability, cost, and density.Most are synthesized via high-temperature solid-phase or high-energy ball-milling methods in small quantities (< 2 grams), which is both energy- and time-consuming and can only produce the products in small quantities (< 2 grams). Only a few can be synthesized via scalable liquidphase methods, but they either require expensive high-temperature annealing (> 500 °C) or exhibit low ionic conductivity and poor electrochemical stability. Therefore, it is imperative to identify and develop new SEs with the desired properties for practical applications of ASSBs. SUMMARY OF THE INVENTION

[0005] We have developed a scalable low-temperature (< 200 °C) liquid-phase technique for synthesizing lithium thiophosphate-borohydride SEs with various compositions (see, e.g., FIGS. 93A-B). This method not only saves time and energy but also can produce SE powders in large quantities (over tens of grams depending on equipment settings), potentially suitable for mass production in industry. Meanwhile, the synthesized SEs possess (1) high room-temperature ionic conductivity (> 1 mS cm'1), (2) good formability, (3) small particle size, (4) low density, (5) good electrochemical stability against Li metal, and (6) superior electrochemical computability with sulfur cathode.

[0006] The unique properties of the obtained products have shown promising effects on improving the performance of Li ASSBs. Firstly, the high ionic conductivity of the developed SE can ensure fast ion transport through the electrode and SE separator. Secondly, the low density and small particle size of the developed SEs can help ensure high SE volume content and sufficient Li+pathways in the cathode. By using one of the developed SEs, high-performance lithium-sulfur (Li-S) ASSBs have been achieved with high sulfur content, long cycle life and improved discharge capacity and energy density.

[0007] Accordingly, embodiments relate to the scalable low-temperature liquid-phase synthesis technique of lithium thiophosphate-borohydride SEs and its use in Li ASSBs.

[0008] In an exemplary embodiment, a method of forming an electrolyte material comprises providing a first solution comprising first precursors and an organic solvent, wherein the first precursors comprise Li2S and P2Ss;stirring the first solution; adding second precursors to the first solution to form a second solution, wherein the second precursors comprise LiBEL alone or in combination with at least one compound selected from the group consisting of LiCl, LiBr, and Lil; stirring the second solution; evaporating the organic solvent from the second solution to provide electrolyte powders; and annealing the electrolyte powders to form the electrolyte material.

[0009] In some embodiments, providing the first solution comprises adding the first precursors (e.g., in particulate or liquid form) to the organic solvent.

[0010] In some embodiments, the organic solvent is a pure solvent or solvent mixture selected from the group consisting of tetrahydrofuran, cyclopentyl methyl ether, 2-methyltetrahydrofuran, dimethly formamide, dimethoxy ethane, pyridine, 1,3 -dioxolane, ethyl acetate, methyl acetate, acetonitrile, ethanol, methanol, propanol, butanol, and diethyl ether.

[0011] In some embodiments, the step of stirring the first solution is carried out at room temperature or at a temperature below the boiling temperature of the organic solvent.

[0012] In some embodiments, the step of stirring the second solution is carried out at room temperature or at a temperature below the boiling temperature of the organic solvent

[0013] In some embodiments, the step of evaporating the organic solvent from the second solution is carried out at a temperature less than or equal to 200 °C.

[0014] In some embodiments, the step of annealing the electrolyte powders is carried out at a temperature less than 300 °C, and wherein the step of annealing the electrolyte powders is carried out in an inert atmosphere or under vacuum.

[0015] In an exemplary embodiment, amethod of forming an electrolyte material comprises providing a first solution comprising first precursors and a first organic solvent, wherein the first precursors comprise U2S and P2S5; stirring the first solution; retrieving the precipitate from the first solution and washing the precipitate with a first organic solvent to provide intermediate powders; adding the intermediate powders to a second organic solvent to form a second solution; adding second precursors to the second solution to form a third solution, wherein the second precursors comprise LiBH4 alone or in combination with at least one compound selected from the group consisting of LiCl, LiBr, and Lil; stirring the third solution; evaporating the second organic solvent from the third solution to provide electrolyte powders; and annealing the electrolyte powders to form the electrolyte material.

[0016] In some embodiments, providing the first solution comprises adding the first precursors (e.g., in particulate or liquid form) to the first organic solvent.

[0017] In some embodiments, the first organic solvent is a pure solvent or solvent mixture selected from the group consisting of tetrahydrofuran, cyclopentyl methyl ether, 2- methyltetrahydrofuran, dimethly formamide, dimethoxyethane, pyridine, 1,3-dioxolane, ethyl acetate, methyl acetate, acetonitrile, ethanol, methanol, propanol, butanol, and diethyl ether.

[0018] In some embodiments, the step of stirring the first solution is carried out at room temperature or at a temperature below the boiling temperature of the organic solvent.

[0019] In some embodiments, the step of evaporating the first organic solvent from the first solution is carried out at a temperature less than or equal to 200 °C.

[0020] In some embodiments, the second organic solvent is a pure solvent or solvent mixture selected from the group consisting of tetrahydrofuran, cyclopentyl methyl ether, 2- methyltetrahydrofuran, dimethly formamide, dimethoxyethane, pyridine, 1,3-dioxolane, ethyl acetate, methyl acetate, acetonitrile, ethanol, methanol, propanol, butanol, and diethyl ether.

[0021] In some embodiments, the first organic solvent is the same as the second organic solvent.

[0022] In some embodiments, the first organic solvent is different from the second organic solvent.

[0023] In some embodiments, the step of stirring the third solution is carried out at room temperature or at a temperature below the boiling temperature of the organic solvent

[0024] In some embodiments, the step of evaporating the second organic solvent from the third solution is carried out at a temperature less than or equal to 200 °C.

[0025] In some embodiments, the step of annealing the electrolyte powders is carried out at a temperature less than 300 °C, and wherein the step of annealing the electrolyte powders is carried out in an inert atmosphere or under vacuum.

[0026] In an exemplary embodiment, an all-solid-state battery comprises an anode; a cathode; and an electrolyte comprising an electrolyte material and positioned between the anode and the cathode, wherein the electrolyte material comprises Li3PS4-xLiBH4-aLiCl-bLiBr-cLiI, wherein x is 1-3, a is 0-1, b is 0-1, and c is 0-1 , and wherein the cathode has a sulfur content of at least 40 wt% based on a total weight of the cathode.

[0027] In some embodiments, the electrolyte material has a primary particle size of less than 10pm, such as about 500 nm.

[0028] In some embodiments, the electrolyte material has a density of less than 2 g cm ’3, such as about 1.491 g cm "3.

[0029] In some embodiments, the electrolyte material has an ionic conductivity of greater than or equal to 1.0 mS cm at 25 °C, such as about 6.0 mS cm4at 25 °C.

[0030] In some embodiments, the cathode comprises a cathode active material, the electrolyte material, a polymer binder, and conductive carbon.

[0031] In some embodiments, the cathode active material is selected from the group consisting of sulfur, lithium cobalt oxide, and lithium nickel manganese cobalt oxide.

[0032] In some embodiments, the anode is a lithium or lithium alloy foil.

[0033] In some embodiments, the anode comprises an anode active material, the electrolyte material, a polymer binder, and conductive carbon.

[0034] In some embodiments, wherein the anode active material is selected from the group consisting of silicon, graphite, and tin.

[0035] In an exemplary embodiment, a method of making an all-solid-state battery comprises synthesizing an electrolyte material comprising Li3PS4-xLiBH4-aLiCl-bLiBr-cLiI, wherein x is 1-3, a is 0-1, b is 0-1, and c is 0-1; forming an electrolyte pellet comprising the electrolyte material; forming a cathode particulate material; forming a cathode on a first side of the electrolyte pellet, wherein the cathode has a sulfur content of at least 40 wt% based on a total weight of the cathode; and forming an anode on a second side of the electrolyte pellet such that the electrolyte pellet is positioned between the anode and the cathode.

[0036] In some embodiments, the electrolyte material has a primary particle size of less than 10pm, such as about 500 nm.

[0037] In some embodiments, the electrolyte material has a density of less than 2 g cm "3, such as about 1.491 g cm ’3.

[0038] In some embodiments, the electrolyte material has an ionic conductivity of greater than or equal to 1.0 mS cm at 25 °C, such as about 6.0 mS cm4at 25 °C.

[0039] In some embodiments, the step of synthesizing an electrolyte material is a liquid-phase synthesis step.

[0040] In some embodiments, the step of synthesizing an electrolyte material comprises adding Li2S, P2S5, and LiBt alone or in combination with at least one compound selected from the group consisting of LiCl, LiBr, and Lil to a solvent; and removing the electrolyte material from the solvent.

[0041] In some embodiments, the solvent is tetrahydrofuran.

[0042] In some embodiments, the cathode particulate material comprises sulfur, the electrolyte material, a polymer binder, and conductive carbon.

[0043] In some embodiments, the step of forming a cathode on a first side of the electrolyte pellet comprises depositing the cathode particulate material on the first side of the electrolyte pellet; and compressing the cathode particulate material to form the cathode.

[0044] In some embodiments, the step of forming an anode on a second side of the electrolyte pellet comprises compressing a lithium foil alone or in combination with a second foil to form the anode.

[0045] In some embodiments, the second foil is selected from the group consisting of indium, tin, aluminum, zinc, and magnesium.BRIEF DESCRIPTION OF THE DRAWINGS

[0046] The above and other objects, aspects, features, advantages, and possible applications of the present innovation will be more apparent from the following more particular descriptionthereof, presented in conjunction with the following drawings. Like reference numbers used in the drawings may identify like components.

[0047] FIG. 1 shows an exemplary embodiment of an all-solid-state battery.

[0048] FIG. 2 shows an exemplary method of making the all-solid-state battery of FIG. 1.

[0049] FIG. 3 is a schematic illustration showing that the sufficiency of Li+pathways increases upon increasing SE volume content (from left to right) in the sulfur cathode.

[0050] FIG. 4 is a graph showing the dependence of specific energy at the battery level and sulfur content at the cathode level on the density of SE. The estimation was performed by assuming fixed volume ratios of cathode (or battery) components. The weight of the sulfur cathode, SE membrane, Li anode, and current collectors was considered for calculating the specific energy of Li-S ASSBs.

[0051] FIG. 5 is a graph illustrating the influence of SE’s density on the cell-level specific energy of Li-S ASSBs (based on the weight of cathode, anode, SE membrane, and current collectors) using sulfur cathodes (50 vol% of sulfur) with areal sulfur loading of 3 mgsuifiir cm'2.

[0052] FIG. 6 is a graph illustrating the influence of SE’s density on the cell-level specific energy of Li-S ASSBs (based on the weight of cathode, anode, SE membrane, and current collectors) using sulfur cathodes (50 vol% of sulfur) with areal sulfur loading of 5 mgsuifiir cm'2.

[0053] FIG. 7 is a graph illustrating the influence of SE’s density on the cell-level specific energy of Li-S ASSBs (based on the weight of cathode, anode, SE membrane, and current collectors) using sulfur cathodes (50 vol% of sulfur) with areal sulfur loading of 6 mgsuifiir cm'2.

[0054] FIG. 8 is a schematic illustration of the liquid-phase synthesis of Li3PS4-2LiBH4 (LPB) SE.

[0055] FIG. 9 is a graph showing a comparison of density among LPB, non-aqueous liquid electrolyte solutions, polymer electrolytes, and inorganic SEs. LE: non-aqueous liquid electrolyte solutions; PEO: poly(ethylene oxide); LPB: LisPS4-2LiBH4; TTE: 1,1,2,2-tetrafluoroethyl- 2,2,3,3-tetrafluoropropyl ether; LPS: P-Li3PS4; LGPS: LiioGeP2Si2; LATP: Lii.3Alo.3Tii 7(P04)3; LLZO: Li7La3Zr20i2.

[0056] FIG. 10 is an Arrhenius plot for cold-pressed LPB SE pellet and the corresponding Nyquist impedance plot of the A1-C|LPB|ALC (Al-C stands for carbon-coated aluminum foil current collector) coin cell tested at different temperatures (i.e., 25, 40, 60, 80, 100 °C). The error bar represents the standard deviation of the measured ionic conductivity.

[0057] FIG. 11 is an Arrhenius plot for a hot-pressed LPB SE pellet and the corresponding Nyquist impedance plot of the A1-C|LPB|ALC coin cell tested from 25 to 100 °C. The error bar represents the standard deviation of the measured ionic conductivity.

[0058] FIG. 12 is a comparison of ionic conductivity (20-30 °C) and synthesis temperature of LPB SE and reported liquid-phase synthesized sulfide SEs.

[0059] FIG. 13 is a SEM image of LPB powders.

[0060] FIG. 14 is a SEM image of LPB powders. The scale bar is 20 pm.

[0061] FIGS. 15-17 are EDS mapping images of LPB powders. The scale bars are 20 pm.

[0062] FIG. 18 is a STEM image of LPB powders.

[0063] FIGS. 19-22 are STEM and EDS mapping of LPB powders. The scale bars are 500 nm.

[0064] FIG. 23 is a TEM image of LPB powders corresponding to the selected area diffraction pattern in FIG. 24. The porous structure observed in this image is caused by electron beam damage.

[0065] FIG. 24 is a SAED image of LPB powders.

[0066] FIG. 25 is a graph showing N2 adsorption / desorption isotherms of LPB powders at 77 K.

[0067] FIG. 26 is the XRD patterns of LPB, LPS, and LiBH4.

[0068] FIG. 27 is an XRD pattern of the Beryllium air-sensitive sample holder.

[0069] FIG. 28 is XRD patterns of LPB referenced to the PDF cards of LiePSslBHiJo.y, P-Li3PS4, and Li4P2S6.

[0070] FIG. 29 is a Raman spectra of LPB, LPS, and LiBH4.

[0071] FIG. 30 is a31P MAS NMR of LPB.

[0072] FIG. 31 is a7Li MAS NMR of LPB, LPS, and LiBH4.

[0073] FIG. 32 is a SEM image of p-Li3PS4(LPS).

[0074] FIG. 33 is a SEM image of LiioGeP2Si2 (LGPS).

[0075] FIG. 34 is a STEM image of LPS.

[0076] FIG. 35 is a STEM image of LGPS.

[0077] FIG. 36 is a schematic illustration of the Swagelok cell and the configuration of Li-S ASSBs.

[0078] FIG. 37 is a graph showing the cycling of a Li|LPB|Li symmetric cell at different current densities under 25 °C.

[0079] FIG. 38 is a graph showing the evolution of voltage polarization, total resistance, and interfacial resistance during cycling.

[0080] FIG. 39 shows X-ray photoelectron spectroscopy (XPS) spectra of (a-c) LPB SE, (d-i) solid electrolyte interphase (SEI) layer on the (d-f) Li metal surface, and (g-i) SE pellet surface at the Li / LPB interface.

[0081] FIG. 40 shows galvanostatic discharge-charge curves of S-C-LPB, S-C-LPS, and S-C-LGPS cathodes upon 167.5 mA g'1at 60 °C.

[0082] FIG. 41 shows differential capacity vs. voltage (dQ / dV) curves.

[0083] FIG. 42 shows a comparison of initial Coulombic efficiency (ICE, charge capacity / discharge capacity) and volume ratios of SE and carbon in different cathodes. The error bar represents the standard deviation of the average ICE.

[0084] FIG. 43 shows Arrhenius plots of LPS, LGPS, and LiePSsCl (LPSC) from 25 to 100 °C. The relative density of LPS pellet, LGPS pellet, and LPSC pellet is ~ 86% (1.57 g cm'3, bulk density), ~ 87% (1.78 g cm'3, bulk density), and ~ 92 % (1.64 g cm'3, bulk density), respectively.

[0085] FIG. 44 shows the rate performance of different sulfur cathodes.

[0086] FIG. 45 shows the corresponding voltage profiles of the cathodes of FIG. 44 at different rates.

[0087] FIG. 46 shows the cycling performance of a Li-In|LPB|C-LPB cell at 0.5 mA cm'2.

[0088] FIG. 47 shows corresponding voltage profiles at the 1st, 2nd, 10th’ and 100thcycles of the cell of FIG. 46.

[0089] FIG. 48 shows rate performance of Li-In|LPB|S-C-SE cells having positive electrodes with 50 wt% of sulfur (KB / S / SE=20 / 50 / 30, w / w / w) using different SEs under 167.5, 502.5, 837.5, and 1675 mA g'1.

[0090] FIG. 49 shows a comparison of initial Coulombic efficiency (ICE, charge capacity / discharge capacity) and volume ratios of SE and carbon for different cathodes. All cells were tested between 0.5 and 2.5 V vs. Li-In / Li+at 60 °C.

[0091] FIG. 50 shows galvanostatic discharge-charge curves of Li-In|LPB|S-C-SE cells having a positive electrode with 50 wt% sulfur and 40 wt% LPS or LGPS upon 167.5 mA g1at 60 °C.

[0092] FIG. 51 shows the corresponding differential capacity vs. voltage (dQ / dV) curves of the cells of FIG. 50.

[0093] FIG. 52 shows a comparison of initial Coulombic efficiency (ICE, charge capacity / discharge capacity) and volume ratios of SE and carbon for different cathodes.

[0094] FIG. 53 shows the rate performance of cells having positive electrodes with 50 wt% of sulfur (KB / S / LPB=20 / 50 / 30, w / w / w) using LPS or LGPS under 167.5, 502.5, 837.5, and 1675 mA g’1. All cells were tested between 0.5 and 2.5 V vs. Li-In / Li+at 60 °C.

[0095] FIG. 54 shows the cycling performance of the Li-In|LPB|S-C-LPB cell at 837.5 mA g'1under CCCV mode (cutoff current, 167.5 mA g’1; cutoff voltage, 2.5 V vs. Li-In / Li+) between 0.8 and 2.5 V at 60 °C.

[0096] FIG. 55 shows a comparison of specific energy and cycle life of a cell with S-C-LPB cathode and literature-reported results.

[0097] FIG. 56 shows the cycling performance of the Li-In|LPB| S-C-LPB cell with high areal sulfur loading of 5.9 mg cm'2under 167.5 mA g'1at 60 °C.

[0098] FIG. 57 shows galvanostatic discharge-charge curves of the Li-In|LPB| S-C-LPB cell cycled at the 1st, 10th, 100th, 400th, and 800thcycle. The cell was cycled at 837.5 mA g'1under CCCV mode (cutoff current, 167.5 mA g'1; cutoff voltage, 2.5 V vs. Li-In / Li+) between 0.8 and 2.5 V at 60 °C.

[0099] FIG. 58 shows electrochemical impedance spectroscopy (EIS) spectra of the Li-In|LPB|S- C-LPB cell before cycling.

[0100] FIG. 59 shows electrochemical impedance spectroscopy (EIS) spectra of the Li- InLPB | S-C-LPB cell after 1000 cycles.

[0101] FIG. 60 shows linear sweep voltammetry (LSV) curves of Li-In|LPB|C-LPB and Li-In|LPSC|C-LPSC from open-circuit voltage to 0 V vs. Li / Li+(-0.62 V vs. Li-In / Li+). Thetesting was performed at 60 °C. The areal loadings of C-LPB and C-LPSC cathodes are between 3-4 mg cm’2.

[0102] FIG. 61 shows linear sweep voltammetry (LSV) curves of Li-In|LPB|C-LPB and Li-In|LPSC|C-LPSC from open-circuit voltage to 5 V vs. Li / Li+(4.38 V vs. Li-In / Li+). The testing was performed at 60 °C. The areal loadings of C-LPB and C-LPSC cathodes are between 3-4 mg cm’2.

[0103] FIG. 62 shows XPS spectra of pristine S-C-LPB cathode.

[0104] FIG. 63 shows XPS depth profding spectra of the S-C-LPB cathode disassembled from a Li-ln|LPB|S-C-LPB cell after being cycled for 1000 cycles under 837.5 mA g’1(constantcurrent constant-voltage mode; cutoff current, 167.5 mA g’1; cutoff voltage, 2.5 V) between 0.8 and 2.5 V at the fully charged state. The sputtering duration is 0, 60, 120, and 150 mins for the curves from top to bottom. The sputtering rate is approximately 10 nm min’1for SiCL.

[0105] FIG. 64 shows XRD patterns of S-C-LPS and S-C-LPB cathode powders.

[0106] FIG. 65 shows the volumetric contents of cathode components in S-C-LPS, S-C-LPB, S-C-LGPS, and S-C-LPB-65. For estimation, we assumed the density of sulfur, carbon, LPB, LPS, and LGPS are 2.07, 1.491, 1.83, and 2.04 g cm’3.

[0107] FIG. 66 shows SEM images of S-C-LPS and S-C-LPB cathode powders.

[0108] FIG. 67 shows ex-situ SEM and EDS mapping images of pristine S-C-LPS cathode.

[0109] FIG. 68 shows ex-situ SEM and EDS mapping images of pristine S-C-LPB cathode.

[0110] FIG. 69 is a schematic illustration of bulky sulfur’s influence on cathode powder aggregate size. The primary cathode particles are composed of uniformly distributed sulfur, SE, and carbon.

[0111] FIG. 70 shows ex-situ SEM and EDS mapping images of the lithiated S-C-LPS cathode.

[0112] FIG. 71 shows ex-situ SEM and EDS mapping images of the lithiated S-C-LPB cathode.

[0113] FIG. 72 shows SEM images of S-C-LPB-65 powders and SEM and corresponding EDS mapping images of the pristine S-C-LPB-65 electrode.

[0114] FIG. 73 shows XRD patterns of S-C-LPB-65 cathode powders.

[0115] FIG. 74 shows galvanostatic discharge-charge curves of Li-In LPB| S-C-LPB-65 battery (S / KB / SE=50 / 10 / 17, w / w / w) at 167.5 mA g'1. Testing was performed at 60 °C.

[0116] FIG. 75 is a schematic illustration of the influence of SE’s volumetric content on interparticle Li+transport and the formation of inactive bulky sulfur particles.

[0117] FIG. 76 is a schematic illustration of the influence of SE’s volumetric content on Li+transport kinetics and cathode resistance.

[0118] FIG. 77 shows SEM and STEM images of Li6PS5Cl (LPSC) SE.

[0119] FIG. 78 is a graph showing initial galvanostatic discharge-charge curves at 167.5 mA g'1with 60 wt% of sulfur.

[0120] FIG. 79 is a graph showing the rate performance of cells using S-C-LPSC cathodes with 60 wt%.

[0121] FIG. 80 is a graph showing initial galvanostatic discharge-charge curves at 167.5 mA g'1with 40 wt% of sulfur.

[0122] FIG. 81 is a graph showing the rate performance of cells using S-C-LPSC cathodes with 40 wt% sulfur.

[0123] FIG. 82 is an SEM image of S-C-LPSC powders.

[0124] FIG. 83 is the XRD pattern of S-C-LPSC powders.

[0125] FIG. 84 shows SEM and EDS mapping images of pristine S-C-LPSC cathode.

[0126] FIG. 85 shows GITT and OCV curves of S-C-LPB and S-C-LPS cathodes at the third cycle. Current pulses of 50.25 mA g’1for 30 mins were employed, followed by 4-hour resting.

[0127] FIG. 86 is a schematic illustration of GITT curves at the selected steps during the discharging process.

[0128] FIG. 87 shows open-circuit voltage (OCV) profiles between selected voltage ranges of 1.57-1.28 V during the discharging process.

[0129] FIG. 88 shows open-circuit voltage (OCV) profiles between selected voltage ranges of 1.58 ~ 1.68 V during the charging process.

[0130] FIG. 89 shows a comparison of sulfur cathodes’ specific capacities at the selected voltage ranges during lithiation / delithiation processes.

[0131] FIG. 90 shows overpotential profiles of S-C-LPB and S-C-LPS cathodes from the GITT measurement.

[0132] FIG. 91 shows IR drop profiles of S-C-LPB and S-C-LPS cathodes during discharge.

[0133] FIG. 92 shows IR drop profiles of S-C-LPB and S-C-LPS cathodes during charge.

[0134] FIG. 93A shows an exemplary method of synthesizing an electrolyte material.

[0135] FIG. 93B shows an alternative method of synthesizing an electrolyte material.DETAILED DESCRIPTION OF THE INVENTION

[0136] The following description is of exemplary embodiments and methods of use that are presently contemplated for carrying out the present invention. This description is not to be taken in a limiting sense, but is made merely for the purpose of describing the general principles and features of various aspects of the present invention. The scope of the present invention is not limited by this description. Any order of steps described herein is merely illustrative and is not intended to limit the scope of the inventive concepts. For example, a step that is interpreted as being performed “first” may be performed first, second, third .. . etc. Similarly, any steps described as “following” other steps should not be interpreted to impart order, unless expressly indicated otherwise.

[0137] Referring to FIGS. 93A and 93B, embodiments generally relate to methods of synthesizing (e.g., liquid phase synthesis) an electrolyte material, such as an electrolyte material for lithium thiophosphate-borohydride solid electrolytes. As seen in FIG. 93A, in one embodiment, a liquid phase method 300 of synthesizing the electrolyte material may comprise step 302 of providing a first solution. The first solution may include first precursors provided in an organic solvent. The first precursors may include IJ2S and P2S5. The organic solvent may be a pure solvent or solvent mixture selected from the group consisting of tetrahydrofuran, cyclopentyl methyl ether, 2-methyltetrahydrofuran, dimethly formamide, dimethoxyethane, pyridine, 1,3 -di oxolane, ethyl acetate, methyl acetate, acetonitrile, ethanol, methanol, propanol, butanol, diethyl ether, and / or mixtures thereof. It is contemplated that the organic solvent is preferably a wet solvent. In some embodiments, the first precursors may be added to the organic solvent, preferrably in particulate (e.g., powder) form, to form the first solution. In alternative embodiments, the first solution may already include the first precursors. The method 300 mayfurther comprise step 304 of stirring the first solution. The first solution may be stirred at room temperature or at an elevated temperature (e.g., less than 80 °C) for a predetermined period of time.

[0138] The method 300 may further comprise step 306 of adding second precursors to the first solution to form a second solution. The second precursors may include any number of LiBLL, LiCl, LiBr, and Lil. The second precursors preferably include either LiBLL alone or in combination with at least one compound selected from the group consisting of LiCl, LiBr, and Lil. In preferred embodiments, the precursors may be added to the second solution in particulate (e.g., powder) form. It is contemplated that the composition of the electrolyte may be varied by tuning the ratio between the first and second precursors. The method 300 may further comprise step 308 of stirring the second solution. The second solution may be stirred at room temperature or at a temperature below the boiling temperature of the organic solvent (e.g., less than 80 °C) for a predetermined period of time.

[0139] The method 300 may further comprise step 310 of evaporating the organic solvent from the second solution to provide electrolyte powders. It is contemplated powders may be the electrolyte material (e.g. the electrolyte material for lithium thiophosphate-borohydride solid electrolytes) in particulate form. The evaporation step may be carried out at any particular temperature, for example at a temperature less than or equal to 200°C, such as less than equal to or 120 °C. The method 300 may further comprise step 312 of annealing the electrolyte powders. The annealing step 312 may be carried out in an inert atmosphere (e.g., Ar, N2, etc.) or under vacuum, and at a temperature less than 300°C, such as less than or equal to 200 °C. The annealing step 308 may be carried out for a predetermined period of time, which may be between ten minutes and two days.

[0140] As seen in FIG. 93B, in another embodiment, a liquid-phase method 400 of synthesizing the electrolyte material may comprise step 402 of providing a first solution. The first solution may include first precursors provided in a first organic solvent. The first precursors may include IJ2S and P2S5. The first organic solvent may be a pure solvent or solvent mixture selected from the group consisting of THF, cyclopentyl methyl ether, 2-methyltetrahydrofuran, dimethly formamide, dimethoxy ethane, pyridine, 1,3 -di oxolane, ethyl acetate, methyl acetate, acetonitrile, ethanol, methanol, propanol, butanol, diethyl ether, and / or mixtures thereof. It is contemplated that the organic solvent is preferably a wet solvent. In some embodiments, the first precursors may be added to the first organic solvent, preferably in particulate (e.g., powder) form or liquid form, to form the first solution. In alternative embodiments, the first solution may already include the first precursors. The method 400 may further comprise step 404 of stirring the first solution. It is contemplated that stirring the first solution provides a precipitate formed from the first solution. The first solution may be stirred at room temperature or at a temperature below the boiling temperature of the organic solvent (e.g., less than 80 °C) for a predetermined period of time. The method 400 may further comprise step 406 of retrieving precipitate powders from the solution via centrifugation and washing them with the first organic solvent.

[0141] The method 400 may further comprise step 408 of evaporating the first organic solvent from the first solution to provide intermediate powders. The evaporation step may be carried out at any particular temperature, for example, at a temperature less than or equal to 200°C, such as less than or equal to 80 °C. The method 400 may further comprise step 410 of adding the intermediate powders to a second organic solvent to form a second solution. The second organic solvent may include THF, cyclopentyl methyl ether, 2-methyltetrahydrofuran, dimethly formamide, dimethoxyethane, pyridine, 1,3-dioxolane, ethyl acetate, methyl acetate,acetonitrile, ethanol, methanol, propanol, butanol, diethyl ether, and / or mixtures thereof. It is contemplated that the organic solvent is preferably a wet solvent. The second organic solvent may be the same as or different than the first organic solvent.

[0142] The method 400 may further comprise step 412 of adding second precursors to the second solution to form a third solution. The second precursors may include LiBLL, LiCl, LiBr, and Lil, preferably LiBLL alone or in combination with at least one compound selected from the group consisting of LiCl, LiBr, and Lil. In preferred embodiments, the second precursors are added to the second solution in particulate (e.g., powder) form or liquid form. It is contemplated that the composition of the electrolyte may be varied by tuning the ratio between the first and second precursors. The method 400 may further comprise step 414 of stirring the third solution. The third solution may be stirred at room temperature or at a temperature below the boiling temperature of the organic solvent (e.g., less than 80 °C) for a predetermined period of time.

[0143] The method 400 may further comprise step 416 of evaporating the second organic solvent from the third solution to provide electrolyte powders. It is contemplated powders may be the electrolyte material (e.g. the electrolyte material for lithium thiophosphate-borohydride solid electrolytes) in particulate form. The evaporation step may be carried out at any particular temperature, for example, at a temperature less than or equal to 200°C, such as less than or equal to 120 °C. The method 400 may further comprise step 418 of annealing the electrolyte powders. The annealing step 418 may be carried out in an inert atmosphere (e.g., Ar, N2, etc.) or under vacuum and at a temperature less than 300°C, such as less than or equal to °C. The annealing step 418 may be carried out for a predetermined period of time, which may be between ten minutes and two days.

[0144] Embodiments further relate to an all-solid-state battery 100. The battery 100 comprises an anode 102, a cathode 104, and an electrolyte 106 positioned between the anode 102 and cathode 104. It is contemplated that the electrolyte 106 is configured to enable ionic transport between the anode 104 and the cathode 106. In preferred embodiments, the battery 100 is a lithium-sulfur all-solid-state battery.

[0145] The electrolyte 106 is a solid-state, inorganic electrolyte. The electrolyte 106 may be in the form of a layer positioned between the anode 102 and the cathode 104, wherein the thickness of the layer is between 1 and 1000 pm. The electrolyte 106 may have an electrolyte material. In a preferred embodiment, the electrolyte comprises a material of the formula LisPS4- xLiBH4-aLiCl-bLiBr-cLiI, wherein x is 1-3, a is 0-1, b is 0-1, and c is 0-1. In a more preferred embodiment, the electrolyte material comprises Li3PS4-2LiBH4 (LPB).

[0146] It is contemplated that an inorganic electrolyte may prevent dissolution in the battery 100, which may otherwise lead to loss of active material and affect battery performance (e g., capacity fade). It is further contemplated that a low-density, high ionically conductive electrolyte material with small particle size may advantageously enable efficient ionic transport and achieve a high-specific-capacity battery. Accordingly, the electrolyte material of the electrolyte 106 may be in the form of a particulate material (e.g., a powder), wherein the primary particle size is 10pm or less, preferably 500 nm or less, more preferably 1000 nm or less. The electrolyte material may further have a density of less than 2 g cm "3, such as approximately 1.491 g cm '3. It is contemplated that the electrolyte material may provide an ionic conductivity of greater than or equal to 1.0 mS cm1at 25 °C, such as 6.0 mS cm1at 25 °C.

[0147] The cathode 104 is a solid-state cathode. The cathode 104 may be in the form of a layer positioned adjacent to the electrolyte 106, wherein the thickness of the layer is between 1and 1000 m. For example, the cathode 104 may comprise one or more particulate-like materials(e.g., powders) that are compressed to form the layer. The cathode 104 may comprise a cathode active material and the electrolyte material of the electrolyte 106. The cathode active material may be selected from the group consisting of sulfur, lithium cobalt oxide, lithium nickel manganese cobalt oxide, and / or mixtures thereof. Preferably, the cathode active material is sulfur. In preferred embodiments, the cathode 104 comprises the cathode active material, the electrolyte material of the electrolyte 106, a polymer binder, and conductive carbon.

[0148] It is contemplated that a cathode comprising high sulfur content and utilization may achieve a high specific energy battery. However, developing a cathode with high sulfur content and utilization is challenging, as the electrolyte material present in the cathode is the component that regulates the transport of metal ions from the anode. Specifically, it is contemplated that the electrolyte material’s conductivity governs the ionic transport kinetics, while its volumetric content and particle size mainly determine the sufficiency of ionic pathways. However, if high sulfur content in the cathode is desired, the weight ratio of the electrolyte material necessarily drops and gives rise to deficient ionic pathways and, hence, mediocre sulfur utilization. Accordingly, the inventors found that a low-density electrolyte material, as described above, used together with a cathode 104 with high sulfur content may both (i) increase the electrolyte material volume ratio, preferably 25 vol% or more, in the cathode 104, (ii) reduce inactive sulfur and (iii) improves the content uniformity of the sulfur-based cathode 104, thus providing sufficient ionic pathways for improved performance of the battery 100.

[0149] In some embodiments, the cathode 104 may have a sulfur content of preferably 50 wt% or more. As stated above, in preferred embodiments, the cathode 104 comprises sulfur, the electrolyte material of the electrolyte 106, polymer binder, and conductive carbon. In suchembodiments, the sulfur comprises 40 wt% or more, preferably 50 wt% or more, more preferably60wt% or more based on the total weight of the cathode 104, the electrolyte material comprises preferably 40 wt% or less based on the total weight of the cathode 104, the polymer binder comprises preferably 10 wt% or less based on the total weight of the cathode 104, and the conductive carbon comprises preferably 20 wt% or less based on the total weight of the cathode 104.

[0150] The anode 102 is a solid-state anode. The anode 102 may be in the form of a layer positioned adjacent to the electrolyte 106, wherein the thickness of the layer is between 1 and 1000 pm. For example, the anode 102 may comprise one or more metal foils that may be compressed to form the layer. In some embodiments, the anode 102 may comprise a lithium or a lithium alloy foil. In alternative embodiments, the anode 102 may comprise an anode active material, the electrolyte material, a polymer binder, and conductive carbon, wherein the anode active material is selected from the group consisting of silicon, graphite, and tin.

[0151] The disclosed battery 100 has a high specific energy and a high specific capacity. For example, the battery 100 has a discharge capacity above 1000 mAh g-1at 167.5 mA g and 60 °C. The battery 100 further exhibits stable cycling properties and achieves an initial discharge capacity of 1004.6 mAh g-1at 837 mA g-1. The fading rate of the battery is preferably 0.03% per cycle or less for over 800 cycles at 77.5% capacity retention.

[0152] Embodiments further relate to methods of making the all-solid-state battery 100. The method 200 may comprise step 202 of synthesizing the electrolyte material. In some embodiments, step 202 encompasses the steps described above in method 300 or method 400. More generally, it is contemplated that step 202 comprises liquid-phase synthesis of the electrolyte material. The liquid phase synthesis may comprise adding starting components to anaqueous solvent to form an electrolyte precipitate in the solvent. The electrolyte precipitate may be removed from the solvent and dried to form the electrolyte material. In preferred embodiments, the solvent comprises THF, cyclopentyl methyl ether, 2-methyltetrahydrofuran, dimethly formamide, dimethoxyethane, pyridine, 1,3-dioxolane, ethyl acetate, methyl acetate, acetonitrile, ethanol, methanol, propanol, butanol, diethyl ether, and / or mixtures thereof. In preferred embodiments, using THF as a solvent may improve the ionic conductivity of electrolyte material. The method 200 may further comprise step 204 of forming an electrolyte pellet. The electrolyte pellet may be formed by compressing the electrolyte material produced from step 202.

[0153] The method 200 may further comprise step 206 of mixing cathode particulate material. The cathode particulate material comprises sulfur, the electrolyte material formed from step 202, and conductive carbon. For example, step 206 may comprise mixing (e.g., with a ball mill) the sulfur with the conductive carbon and then mixing the sulfur and conductive carbon with the electrolyte material. The method 200 may further comprise step 208 of forming the cathode. The cathode may be formed by depositing the cathode particulate material from step 206 onto one face of the electrolyte pellet formed in step 204, and compressing the cathode particulate material to form the cathode.

[0154] The method may further comprise step 210 of forming the anode. The anode may cop-rise one or more metal foils. If the anode comprises more than one metal foil, the foils may be compressed to form a single layer, wherein the layer is then compressed onto an opposite face of the electrolyte pellet formed in step 204.

[0155] The method may further comprise 212 of compressing the above-described components (i.e., the anode, the electrolyte pellet, and the cathode) to form the battery.

[0156] It is contemplated that the battery 100 as described here may be used in a number of different applications, including but not limited to, portable electronic devices, electric vehicles, drones, and grid energy storage systems.EXAMPLES

[0157] Exemplary all-solid-state batteries comprising anodes, cathodes, and electrolytes were constructed according to the disclosure provided herein. Experiments were conducted on the exemplary batteries, the methods and results of which are discussed below. Comparative all- solid-state batteries were also constructed and subject to experiments.Synthesis of the Solid Electrolytes

[0158] Li3PS4-2LiBH4(LPB), P-Li3PS4(LPS), and LiioGeP2Si2 (LGPS) solid electrolytes (SEs) were synthesized or collected for experimentation. Tetrahydrofuran (THF), a low-boiling- point solvent with low polarity, was selected as a reaction media to improve the ionic conductivity of the SE. THF (anhydrous, > 99.9%, Sigma-Aldrich), Li2S (99.98 %, Sigma- Aldrich), P2S5 (99 %, Sigma-Aldrich), LiBH4(95%, Sigma-Aldrich), and LiBH4solution (2.0 M in THF, Sigma-Aldrich) were purchased and used without any further treatment. Experiments were performed in an argon-filled glovebox (H2O < 1 ppm, O2 < 5 ppm).

[0159] As seen in FIG. 8, the LPB SE was synthesized via a liquid-phase method. To prepare the LPB SE, Li2S and P2S5 with a molar ratio of 3 to 1 were added to anhydrous THF and stirred for 24 hours at 25 °C. Next, the LiBH4solution with the desired amount (LiBH4:Li2S:P2S5=4:3: 1, molar ratios) was added to the above suspension using a single-channel high-precision pipette. After stirring for 48 hours, the obtained suspension was transferred to a Schlenk flask and dried under vacuum for 2 hours at 100 °C to remove the solvent. Finally,powders were collected and annealed at 160 °C for 3 hours in the argon atmosphere to obtain a LPB glass-ceramic argyrodite SE.

[0160] LPS (P-LisPS^ was also prepared via a liquid-phase method. Li2S and P2S5 with a stoichiometry of 3 to 1 were added to anhydrous THF and stirred for 24 hours at 25 °C. Next, the precipitation product was collected by centrifuge and washed with anhydrous THF for three times. Finally, the collected white precipitation was dried at 140 °C under vacuum for 3 hours, obtaining LPS powders.

[0161] LGPS (> 99.9%) was purchased from MSE Supplies LLC.Ionic Conductivity Measurement

[0162] A1-C|SE|A1-C symmetric cells were assembled to measure the ionic conductivity of SEs via analysis of the EIS measurements. In detail, - 150 mg LPB powders were sandwiched between two Al-C foils and pressed at - 500 MPa in a stainless-die sleeve at 25 °C for 10 mins. Next, it was heated to 160 °C and pressed again at - 500 MPa for another 20 mins, obtaining the hot-pressed LPB pellet. LPS and LGPS pellets were prepared similarly without being heated and pressed at high temperatures. Finally, the fabricated A1-C|SE|A1-C pellet was loaded into a CR2032 coin cell, and EIS measurement of the cell was performed from 0.1 Hz to 1 MHz with a bias of 10 mV under the potentiostat mode in the logarithmic manner (10 points per decade) on a Solartron Modulab at 25, 40, 60, 80, and 100 °C. The cell rested for around 30 mins at the testing temperature in the climatic chamber (Tenney) before each EIS measurement.Materials Characterization

[0163] Helium Pycnometry was used to measure the density of LPB. Specifically, - 0.4 g of LPB SE powders were loaded and sealed into the sample cup in an argon-filled glovebox (H2O < 1 ppm, O2 < 5 ppm) and then transferred to the Helium Pycnometry instrument with anair exposure time of less than 1 minute. The measurement was carried out at ~ 21 °C for ten times. SEM and EDS mapping images were collected on a Thermo Scientific Apreo SEM instrument and an ESEM Q250 instrument. The samples were exposed to air for less than 5 minutes during sample transfer. TEM and STEM images and SAED patterns of the LPB powders were collected on an FEZ Talos F200X TEM with an accelerating voltage of 200 kV. The TEM samples were prepared by loading dry LPB powders onto the Cu grids in an argon-filled glovebox (H2O < 1 ppm, O2 < 5 ppm). The grids were then transferred to a TEM holder and inserted into the microscope with < 1 min air-exposure time. The BET surface area of LPB was measured by a Micrometrics ASAP 2020 physisorption analyzer. A Rigaku Miniflex 11 spectrometer with Cu Kot radiation was used to collect the XRD patterns of the samples. An XRD air-sensitive sample holder with a Beryllium window (Rigaku Corp.) was used to load the sample powders in an argon-filled glovebox (H2O < 1 ppm, O2 < 5 ppm). Raman spectra of LPB powders were collected on a Horiba LabRam HR Evolution Vis-NIR optimized & AIST-NT Scanning Probe using the 532 nm laser. To prevent LPB from reacting with moisture in the air, we sealed the powdered sample between two transparent glass slides under argon. The XPS spectra and depth profiling characterization were carried out on a PHI VersaProbe II Scanning XPS Microprobe. We employed a vacuum transfer vessel to transfer the samples from the argon- filled glovebox (H2O < 1 ppm, O2 < 5 ppm) to the XPS instrument. Additionally,7Li and31P MAS NMR spectra were characterized on an Avance-III-HD ss500 instrument with a 4-mm Bruker CPMAS probe at a spinning speed of 10 kHz. CaHPCh 2H2O and LiCl were used as references for31P and7Li NMR spectra, respectively.Synthesis of the Cathodes

[0164] Carbon-sulfur composite was prepared by mixing sulfur99.0%, Sigma- Aldrich) and KB (Ketjenblack EC-600JD, AkzoNobel) with desired weight ratios (S:KB=50:10 or 50:20, w / w) and heated under 160 °C for 10 hours. The as-obtained carbon-sulfur composite powders (83.3 wt% or 71.4 wt% of sulfur) and SEs (LPB, LPS, or LGPS) with desired weight ratios were then mixed by mechanical ball milling under 350 rpm for 10 hours in 45 ml ZrCh jars (FRITSCH PULVERISETTE. 7 premium line), obtaining sulfur cathode powders. The C-SE cathode powders were prepared similarly by mixing 70 wt% of SE (i.e., LPB) and 30 wt% Super C using mechanical ball milling under 350 rpm for 10 hours in 45 ml ZrCh jars. All process was performed under an inert atmosphere filled with Argon (H2O < 1 ppm, O2 < 5 ppm).Fabrication of the All-Solid-State Cell and Electrochemical Testing

[0165] ASSBs were assembled in Swagelok cells with two stainless-steel rods as current collectors inside an Argon-filled glovebox (H2O < 1 ppm, O2 < 5 ppm). In detail, 80 mg of SE powders were firstly pressed at 100 Mpa for 1 min in the cell to form a pellet. Next, cathode powders with the desired amount were uniformly spread onto the pellet’s surface and pressed at 294 MPa for another 3 mins. The average thickness of the SE pellet is ~ 600 m. Lithium foil (3 ~ 4 mg; cut from Li chips, 99.9%, 0.6 mm thick, China Energy Lithium Co., Ltd) and indium foil (10 mm in diameter, 0.127 mm thick, 99.99%, Sigma-Aldrich) were then successively pressed together and attached to the other side of the pellet at 100 MPa for 1 min. Finally, the cells were compressed by three insulated bolts at 50 ~ 60 MPa, removed from the glovebox, and tested using a Landt cycler at 60 °C under ambient air in a forced air oven (Across International). The applied specific current and the measured specific capacity are based on the mass of sulfur in the positive electrode. Note that the Swagelok cell could not fully prevent the electrode from contacting ambient air. The EIS spectra were obtained on a Solartron Modulab from 0.1 Hz to 1MHz under the potentiostat mode in the logarithmic manner (10 points per decade) with a bias of5 mV at 60 °C. Before carrying out the EIS measurement, the cell rested at 60 °C for 1 hour. The linear sweep voltammetry of Li-In|SE|C-SE cells was carried out on a Solartron Modulab with a scan rate of 0.05 mV s'1from open-circuit voltage to 4.38 or -0.62 V vs. Li-In / Li+(5 or 0 V vs. Li / Li+) at 60 °C. For GITT measurements, the cells were firstly cycled at 167.5 mA g'1for two cycles between 0.5 ~ 2.5 V and then tested with a pulse current of 50.25 mA g'1for 30 mins and a resting time of 4 hours at 60 °C. All electrochemical tests were carried out at least two times and most of them were tested three times.Fabrication of Lithium Symmetric Cell and Testing

[0166] Li|LPB|Li symmetric cell was fabricated inside an argon-filled glovebox (H2O < 1 ppm, O2 < 5 ppm). Hot-pressed LPB pellets (~ 1.3 mm thick) were prepared following the procedure described in the ionic conductivity measurement section. Two pieces of 100-pm thick lithium chips (99.9%, China Energy Lithium Co., Ltd) with a diameter of 10 mm on Cu foils (fF 99.8%, 9 u m thick, MTI corporation) were attached to both sides of the SE pellet by pressing at 100 MPa for 2 mins. The symmetric cell was then loaded into a 10-mm diameter pressure- controlled split coin cell (MTI corporation) for electrochemical testing. A mechanical jig fixture was used to control the pressure of the cell to 6 ~ 8 MPa. Finally, the cell was tested using a Landt cycler under different current densities of 0.1, 0.25, 0.5, 0.75, and 1.0 mA cm'2at 25 °C with the duration of each discharge / charge process fixed at 1 hour. Three symmetric cells were assembled for testing.Experimental Results and Properties - Solid Electrolyte

[0167] The obtained LPB SE powder possessed a low density of 1.491 g cm'3at 21 °C, measured by the Helium Pycnometer. As seen in Table 1, the density of LPB was lower thanother inorganic SEs and comparable to conventional non-aqueous liquid electrolyte solutions (FIG. 9). The ionic conductivity of LPB was measured at different temperatures from 25 to 100 °C by electrochemical impedance spectroscopy (EIS) using an A1-C|LPB|A1-C symmetric cell (Al-C denotes the carbon-coated aluminum foil). The LPB pellet prepared by cold-pressing delivered a high ionic conductivity of 3.8 mS cm'1at 25 °C with a relative density of - 86.0% (FIG. 10). Further enhancing the relative density of the prepared LPB pellet to - 91.5% (1.364 g cm'3, bulk density) through the hot-pressing process led to a higher measured ionic conductivity of 6.0 mS cm'1at 25 °C with a low activation energy of 0.216 eV (FIG. 11). The result was among the highest ionic conductivities reported for liquid-phase synthesized sulfide SEs (FIG. 12). Notably, the synthesis temperature of LPB was 160 °C, lower than other liquid-phase- synthesized sulfide SEs with room-temperature ionic conductivity above 1 mS cm'1.Table 1: Summary of the density of different electrolytes for Li-S batteries.

[0168] The morphology of LPB was investigated using scanning electron microscopy(SEM) and transmission electron microscopy (TEM). The SEM and energy-dispersive X-ray spectroscopy (EDS) mapping images show that the as-synthesized LPB powders are aggregates of ~ 5 pm small particles with uniformly distributed sulfur and phosphorous elements on the surface (FIGS. 13-17). Furthermore, scanning transmission electron microscope (STEM) and TEM images reveal that the 5-pm LPB particles are constituted of smaller nanoparticles of ~ 500 nm with no apparent porous structure (FIGS. 18-22) and Brunauer-Emmett-Teller (BET) surface area of- 3.705 m2g'1(FIG. 23). The small particle size of as-synthesized LPB SE is favorable for attaining sufficient ionic percolation pathways in sulfur cathodes. Moreover, both diffraction spots and diffused diffraction rings were observed in the selected area electron diffraction (SAED) pattern image (FIG. 24, corresponding TEM image shown in FIG. 25), suggesting LPB is composed of both crystalline and amorphous phases.

[0169] The structure of the glass-ceramic LPB SE was investigated using the X-ray powder diffraction (XRD) technique and Raman spectroscopy. In FIG. 26, diffraction peaks associated with the crystalline Li6-xPS5.x(BH4)i+x(-l<x<l) cubic argyrodite phase were observed (FIG. 27 illustrated the XRD patterns of the sample holder). While both crystalline and amorphous phases in LPB possess high ionic conductivity, the formation of the crystalline phase was beneficial for further enhancing LPB’s ionic conductivity. The calculated lattice parameter from the crystalline peaks was around 10.05 A, and thus, the theoretical density of the Li6-xPSs-X(BH4)I+Xcrystal was - 1.59 g cm'3. Due to the amorphous phase’s presence, the LPB SE density shall be lower than the pure Li6-xPSs-x(BH4)i+xcrystal, explaining the measured lower density (1.491 g cm'3) of the as-obtained LPB powders. Meanwhile, low-intensity unknown peaks were also noticed in the XRD patterns, possibly originating from side reaction products orprecursors / intermediate product residuals (FIG. 28) during liquid-phase synthesis of the sulfide- based SEs. FIG. 29 presents the Raman spectra of the LPB SE. The high-intensity peak at ~ 418 cm'1was mainly attributed to PS ' units in the glass-ceramic LPB, while the low-intensity peak at ~ 386 cm'1stemmed from P2Se4' units in the impurity, Li4P2S6. Besides, the broad peak at ~ 2300 cm'1was ascribed to BH4' units, similar to that in the high-temperature hexagonal phase of LiBH4with weak electrostatic interaction between BFF and Li+ions3. This weak interaction was beneficial for improving Li+mobility and achieving SEs with high ionic conductivity.

[0170] Solid-state nuclear magnetic resonance (NMR) spectroscopic characterization of LPB was further carried out to attain more details of the LPB’s local chemical structure and discern the impurities. As shown in the31P NMR spectra (FIG. 30), three distinct peaks, I, II, and III, were observed. The asymmetric high-intensity Peak I is associated with the phosphorous in Li6-xPS5.x(BH4) i+x with a wide distribution of chemical shifts between 96 and 87 ppm. Peak I can be deconvoluted into two lines, implying the diverse chemical environment of PS ' tetrahedrons in the argyrodite Li6-xPS5-x(BH4)i+xinduced by the disorder in S27BH4' sublattices. This disorder is favorable for improving the ionic conductivity in argyrodite SE, which might explain the good Li+conductivity in LPB39. Peak II at ~ 86 ppm is attributed to the PS?' in P-Li3PS4(LPS), generated from the heat treatment of residual Li3PS4-3THF39. Peak III at ~ 109 ppm originates from the P2Se4' in Li4P2S639’41, consistent with the Raman result above. FIG. 31 presents the7Li NMR spectra of LPB (~ 1.93 ppm) in comparison with LiBH4(~ 0 ppm) and LPS (~ 2.07 ppm). In contrast to the broad peak at ~ 0 ppm in orthorhombic LiBH4, a sharp and narrow peak at ~ 1.93 ppm was observed in LPB, stemming from its significantly enhanced Li+mobility.Experimental Results and Properties - All-Solid-State Li-S Battery

[0171] Solid-state sulfur cathodes and Li-S ASSBs were fabricated and evaluated. The cathode powders constituted of sulfur, conductive carbon (Ketjenblack EC-600JD, KB), and SEs were prepared by ball milling with a high sulfur content of - 60 wt% (KB / S / SE= 10 / 50 / 24, w / w / w). LPB, LPS, and LiioGeP2Si2 (LGPS) SEs with particle sizes of < 5 pm (FIGS. 13, 18, and 32-35) were used to fabricate the sulfur cathodes for comparison (S-C-LPB, S-C-LPS, and S-C-LGPS). The assembled Li-S ASSBs (Li-In|LPB|S-C-SE, assembled at 294 MPa) were tested in a Swagelok cell at 60 °C and 50-60 MPa under ambient air, with its configuration illustrated in FIG. 36. While metastable interphase can be formed between LPB pellet and Li metal to inhibit the degradation of LPB (FIGS. 37-39), cell failure caused by lithium penetration may still occur under practical testing conditions. Therefore, Li-In alloy (~ 0.62 V vs. Li / Li+) was employed as the anode due to its compatibility with inorganic SEs under high-areal-capacity and high-current- density conditions.

[0172] Li-S ASSBs with an areal sulfur loading of 2.0 - 3.0 mg cm'2were tested between 0.5 and 2.5 V. As shown in FIG. 40, the S-C-LPB cathode delivered a higher discharge specific capacity (~ 1047.5 mAh g'1), higher initial Coulombic efficiency (ICE, charge capacity / discharge capacity, 100.2 %) than S-C-LPS (~ 802.1 mAh g'1, 74.3 %) and S-C-LGPS (~ 742.0 mAh g'1, 31.4 %) cathodes at 167.5 mA g'1. Differential capacity curves are shown in FIG. 41 to elucidate the differences in the electrochemical process among all the cathodes. For the S-C-LPB cathode, prominent peaks attributed to redox reactions of sulfur / Li2S were observed at - 1.51 V (peak I, 2.13 V vs. Li / Li+) and - 1.40 V (peak II, 2.02 V vs. Li / Li+) during the discharging process and at - 1.70 V (peak III, 2.32 V vs. Li / Li+) during the charging process. In stark contrast, for the S-C-LPS and S-C-LGPS cathodes, peaks I and II become indistinguishable and shift to lower potentials with smaller areas, and peak III shifts to higher potentials, suggesting greater voltagepolarization, lower sulfur utilization, and more sluggish reaction kinetics than S-C-LPB cathode. Such disparities in the cathode performance are attributed to the improved Li+transport in S-C- LPB cathode in terms of transport kinetics determined by SE’s ionic conductivity and Li+pathway sufficiency determined by SE’s volumetric content and particle size. Interestingly, we notice both ICE and initial discharge capacity, especially ICE, increase as the SE’s volumetric content ascends (FIG. 42), while there is no apparent correlation between cathode performance and SE’s ionic conductivity / particle size (FIGS. 11, 13, 18, 32-35, and 43). It might suggest that the low SE volume ratio induced Li+pathway deficiency rather than ionic conductivity governed transport kinetics is the limiting factor that jeopardizes the performance of high-sulfur-content cathodes (i.e., 60 wt%).Experimental Results and Properties - Cathode

[0173] The S-C-LPB cathode also shows better rate performance compared with S-C- LPS and S-C-LGPS cathodes (FIG. 44), presenting higher discharge capacities of 1144.6, 1024, 907.8, and 663 mAh g’1at 167.5, 502.5, 837.5 and 1675 mA g’1, respectively, with good reversibility under 60 °C (FIG. 45). The improved performance of the S-C-LPB cathode at 167.5 mA g’1is equivalent to a calculated Li-S cell specific energy of 1318.7 Wh kg’1and volumetric energy density of 2561.8 Wh L’1with an average discharge voltage of 1.935 V (vs. Li / Li+) (based on the weight / volume of sulfur cathodes, Supplementary Note 4). Since the redox reaction of LPB also contributed to capacity, we further investigated the solid electrolyte capacity contribution by cycling the Li-In|LPB|C-LPB cells (Super C / LPB=30 / 70, w / w, denoted as C- LPB) following previously reported methods (FIGS. 46 and 47). The result shows that the high discharge capacity is mainly contributed by the lithiation of sulfur to LizS (99.5% in the first cycle and > 82% in the following cycles). In addition, the S-C-LPB cathode with a lower sulfurcontent of 50 wt% (KB / S / SE=20 / 50 / 30, w / w / w) exhibited improved performance with > 1300 mAh g’1discharge capacity under 167.5 mAh g’1at 60 °C, better than the cathodes using LPS and LGPS SEs (FIGS. 48 and 49). Good electrochemical performances of sulfur cathodes using LPS and LGPS can only be achieved when a sufficient amount of SEs is added (S / KB / SE=50 / 10 / 40, w / w / w), giving rise to sufficient SE volume ratio and Li+pathways (FIGS. 50-53). Note that the cathode composite powders were prepared using the conventional mechanical dry powder ball-milling method, and further performance improvement might be achievable by fine-tuning local interfacial contact among carbon, sulfur, and SE.[00174J The cycling stability of the S-C-LPB cathode was investigated as well. A Li-S ASSB cell with an areal sulfur loading of - 2.57 mg cm’2was tested at 837.5 mA g’1under a constant current, constant voltage (CCCV) mode (cutoff current, 167.5 mA g’1; cutoff voltage, 2.5 V) between 0.8-2.5 V (FIG. 54). The S-C-LPB cathode cycled stably for over 800 cycles with a high initial discharge capacity of - 1004.6 mAh g’1and a low fading rate of - 0.028 % per cycle. The specific capacity gradually increased in the first 20 cycles to - 1068.1 mAh g’1, possibly attributed to the growth of capacity contribution from LPB’s redox reaction in the initial cycles (FIGS. 46 and 47). After 800 cycles, the discharge capacity remained at - 778.9 mAh g’1, corresponding to a discharge capacity retention of 77.5 %. The cell performance is among the best in literature in terms of sulfur content, specific energy (based on the weight of sulfur cathodes), and cycling stability (FIG. 55 and Table 2). Upon further increasing sulfur mass loading to around 6 mg cm’2, the S-C-LPB cathode delivered a high initial discharge capacity of 999.7 mAh g’1at 167.5 mAh g’1at 60 °C (FIG. 56).Table 2: Summary of the Li-S ASSBs performance.

[0175] In addition to the electrochemical performance, we also investigated the capacity fading mechanism of the S-C-LPB cathode. As shown in the voltage profdes (FIG. 57, corresponding to the cell in FIG. 54), the voltage polarization of the cell during the charge / discharge narrows within the first few cycles, possibly due to the activation processassociated with volume change-induced component redistribution. However, the polarization increases as cycling continues, leading to continuous capacity decay. Through EIS measurements and analysis, we found that the increment of the battery’s charge transfer resistance, which reached hundreds of ohms after over 1000 cycles (FIG. 58-59 and Table 3), is the culprit. Considering sulfide SE’s limited electrochemical stability voltage window and chemical reactivity against moisture, we speculate that the primary cause of the growing voltage polarization and the ensuing capacity decay is the continuous electrochemical and chemical degradation of LPB SE during cycling. Thereafter, we investigated the redox activity of LPB and found that LPB would undergo relatively reversible lithiation / delithiation for over 100 cycles in the designated voltage window (i.e., 0.5-2.5 V vs. Li-In / Li+), explaining the improved cycle life of the S-C-LPB cathode (FIGS. 46, 47, 60, and 61). Nevertheless, in the long-term cycling, the minor irreversible degradation may accumulate and lead to higher resistance, growth of voltage polarization, and capacity decay. Moreover, the X-ray photoelectron spectroscopy (XPS) spectra of the cycled S-C-LPB electrode were further collected (FIGS. 62 and 63). While the observation of P-Sx-P confirms the electrochemical oxidation of LPB, sulfate species in S 2p spectra suggest that the chemical degradation of LPB and active material might be another factor contributing to capacity decay.Table 3: Fitting parameters for the EIS spectra of the Li-S ASSB with the S-C-LPB cathode after1000 cycles.

[0176] To clarify the underlying reasons behind the improved electrochemical performance of the S-C-LPB cathode, we first performed XRD and SEM analyses of S-C-LPB and S-C-LPS at both material and electrode levels. The XRD patterns shown in FIG. 64 indicate the presence of crystalline sulfur particles in S-C-LPS cathode powders, in stark contrast to the amorphous sulfur particles in the S-C-LPB cathode. Moreover, it is found that the morphology and content uniformity of sulfur cathodes are correlated with the volumetric contents of SE and sulfur. The volumetric ratios of different cathode components, i.e., sulfur, carbon, and SE, are calculated and illustrated in FIG. 65. A higher SE volume ratio and lower sulfur volume ratio in S-C-LPB are obtained compared with S-C-LPS at the same weight contents, thanks to the lower density of LPB. As shown in the SEM images (FIG. 66), the S-C-LPB cathode aggregate powders are smaller than the S-C-LPS aggregate. Upon pressing the powders into electrodes, the formed S-C-LPB cathode made from small powders seems relatively denser than the S-C-LPS sulfur cathode with voids on the surface (FIGS. 67 and 68). In addition, distinct from the homogeneously distributed sulfur signals on the pristine S-C-LPB electrode surface, locally high-intensity sulfur signals are detected (marked in dashed circles) in the EDS mapping of the S-C-LPS electrode, indicating the presence of bulky sulfur particles. The absence of themicrometer bulky sulfur particles might help reduce the aggregate size of S-C-LPB powders(FIG. 69). After lithiation, massive aggregated IJ2S emerges and separates from carbon (FIG.70) in the S-C-LPS cathode. Given the poor electronic and ionic conductivity of sulfur / Li2S, the lithiation / delithiation of bulky sulfur / Li2S is kinetically less favorable than small sulfur / Li2S particles, thus leading to higher resistance and lower sulfur utilization of the S-C-LPS cathode. In stark contrast, the S-C-LPB cathode exhibits good content uniformity with homogenous distribution of all elements after lithiation (FIG. 71). Similarly, upon further decreasing LPB’s volume ratio to 27.9 vol% and increasing sulfur volume ratio to 59.2 vol% in S-C-LPB (65 wt% of sulfur, denoted as S-C-LPB-65), we also observed larger powder size, worsened content uniformity, and deteriorated battery performance with lower discharge capacity (678 mAh g'1) and poor ICE (62.3%) in the obtained S-C-LPB-65 cathode (FIGS. 72-74). It demonstrates that this phenomenon is independent of the type of SE but related to the SE volume ratio. Therefore, these results collectively reveal that an adequate volume ratio of SE is the prerequisite for avoiding inactive bulky sulfur particles, achieving good content uniformity, constructing sufficient ionic transport pathways, and thus attaining high-performance sulfur cathodes (FIGS. 75 and 76). Note that, in addition to the SE volume ratio, the large particle size of SE may likewise cause deficient Li+transport pathways and, thus, the mediocre performance of sulfur cathodes by inducing poor cathode content uniformity with inactive bulky sulfur particles and phase separation between carbon and large SE powders (FIGS. 77-84).

[0177] Furthermore, the galvanostatic intermittent titration technique (GITT) was performed using Li-S ASSBs with S-C-LPB and S-C-LPS cathodes to explicate sulfur cathodes’ electrochemical behaviors during charge / discharge and identify their correlations with the cathode features observed above. FIG. 85 depicts the obtained GITT and open-circuit voltage(OCV, defined as the voltage reached after each 4-hour resting) profiles (FIG. 86). Two voltage plateaus at ~ 1.59 and ~ 1.48 V (~ 2.21 and ~ 2.10 V vs. Li / Li ) during lithiation, which might involve the reduction of sulfur to lithium polysulfide (first plateau) and then to I 2S (second plateau), were noticed in both samples, agreeing with the differential capacity curves (FIG. 41). Note that the two reduction plateaus observed in the S-C-LPB cathode were also found in S-C- LPS and S-C-LGPS cathodes with a lower sulfur content of 50 wt% and higher SE content of 40 wt% (FIGS. 50-51). Next, assuming that the batteries reached thermodynamic equilibrium after each 4-hour resting and the electrochemical reactions in both cathodes are identical at the same OCV, we can compare the amount of electrochemically active sulfur in S-C-LPB and S-C-LPS cathodes. To do so, we calculated the discharge / charge specific capacity of cells with both cathodes within certain OCV ranges that are 1.57 ~ 1.28 V (2.19 ~ 1.9 V vs. Li / Li+) during lithiation and 1.58 ~ 1.68 V (2.20 ~ 2.30 V vs. Li / Li+) during delithiation (FIGS. 87 and 88). The higher lithiation / delithiation specific capacity of the S-C-LPB cathode (860 / 950 mAh g'1) than the S-C-LPS cathode (604 / 806 mAh g’1) implies more electrochemically active sulfur in the S-C-LPB cathode (FIG. 89). In addition, significantly lower overpotential and IR drop are observed in the cell with the S-C-LPB cathode during lithiation / delithiation (FIGS. 90-92), suggesting lower reaction resistance and improved Li+transport kinetics in the S-C-LPB cathode than in the S-C-LPS cathode. Together, the above analysis demonstrates that sufficient Li+transport pathways and fast Li+transport kinetics are achieved in the S-C-LPB cathode.

[0178] It should be understood that modifications to the embodiments disclosed herein can be made to meet a particular set of design criteria. For instance, the number of or configuration of components or parameters may be used to meet a particular objective.

[0179] It will be apparent to those skilled in the art that numerous modifications and variations of the described examples and embodiments are possible in light of the above teachings of the disclosure. The disclosed examples and embodiments are presented for illustration purposes only. Other alternative embodiments may include some or all of the features of the various embodiments disclosed herein. For instance, it is contemplated that a particular feature described, either individually or as part of an embodiment, can be combined with other individually described features or parts of other embodiments. The elements and acts of the various embodiments described herein can therefore be combined to provide further embodiments.

[0180] It is the intent to cover all such modifications and alternative embodiments as may come within the true scope of this invention, which is to be given the full breadth thereof. Additionally, the disclosure of a range of values is a disclosure of every numerical value within that range, including the end points. Thus, while certain exemplary embodiments of the device and methods of making and using the same have been discussed and illustrated herein, it is to be distinctly understood that the invention is not limited thereto but may be otherwise variously embodied and practiced within the scope of the following claims.

Claims

WHAT IS CLAIMED IS:

1. A method of forming an electrolyte material, comprising: providing a first solution comprising first precursors and an organic solvent, wherein the first precursors comprise U2S and P2S5; stirring the first solution; adding second precursors to the first solution to form a second solution, wherein the second precursors comprise LiBH4 alone or in combination with at least one compound selected from the group consisting of LiCl, LiBr, and Lil; stirring the second solution; evaporating the organic solvent from the second solution to provide electrolyte powders; and annealing the electrolyte powders to form the electrolyte material.

2. The method of claim 1, wherein providing the first solution comprises adding the first precursors to the organic solvent.

3. The method of claim 1, wherein the organic solvent is a pure solvent or solvent mixture selected from the group consisting of tetrahydrofuran, cyclopentyl methyl ether, 2- methyltetrahydrofuran, dimethly formamide, dimethoxyethane, pyridine, 1,3-dioxolane, ethyl acetate, methyl acetate, acetonitrile, ethanol, methanol, propanol, butanol, and diethyl ether.

4. The method of claim 1, wherein the step of stirring the first solution is carried out at room temperature or at a temperature below the boiling temperature of the organic solvent.

5. The method of claim 1, wherein the step of stirring the second solution is carried out at room temperature or at a temperature blow the boiling temperature of the solvent.

6. The method of claim 1, wherein the step of evaporating the organic solvent from the second solution is carried out at a temperature less than or equal to 200 °C.

7. The method of claim 1, wherein the step of annealing the electrolyte powders is carried out at a temperature less than 300 °C, and wherein the step of annealing the electrolyte powders is carried out in an inert atmosphere or under vacuum.

8. A method of forming an electrolyte material, comprising: providing a first solution comprising first precursors and a first organic solvent, wherein the first precursors comprise IJ2S and P2S5; stirring the first solution; retrieving a precipitate from the first solution and washing the precipitate with a first organic solvent to provide intermediate powders; adding the intermediate powders to a second organic solvent to form a second solution; adding second precursors to the second solution to form a third solution, wherein the second precursors comprise LiBT alone or in combination with at least one compound selected from the group consisting of LiCl, LiBr, and Lil;stirring the third solution; evaporating the second organic solvent from the third solution to provide electrolyte powders; and annealing the electrolyte powders to form the electrolyte material.

9. The method of claim 8, wherein providing the first solution comprises adding the first precursors to the first organic solvent.

10. The method of claim 8, wherein the first organic solvent is a pure solvent or solvent mixture selected from the group consisting of tetrahydrofuran, cyclopentyl methyl ether, 2- methyltetrahydrofuran, dimethly formamide, dimethoxyethane, pyridine, 1,3-dioxolane, ethyl acetate, methyl acetate, acetonitrile, ethanol, methanol, propanol, butanol, and diethyl ether.

11. The method of claim 8, wherein the step of stirring the first solution is carried out at room temperature or at a temperature below the boiling temperature of the organic solvent.

12. The method of claim 8, wherein the step of evaporating the first organic solvent from the first solution is carried out at a temperature less than or equal to 200 °C.

13. The method of claim 8, wherein the second organic solvent is a pure solvent or solvent mixture selected from the group consisting of tetrahydrofuran, cyclopentyl methyl ether, 2- methyltetrahydrofuran, dimethly formamide, dimethoxyethane, pyridine, 1,3-dioxolane, ethyl acetate, methyl acetate, acetonitrile, ethanol, methanol, propanol, butanol, and diethyl ether.

14. The method of claim 8, wherein the first organic solvent is the same as the second organic solvent.

15. The method of claim 8, wherein the first organic solvent is different from the second organic solvent.

16. The method of claim 8, wherein the step of stirring the third solution is carried out at room temperature or at a temperature below the boiling temperature of the solvent.

17. The method of claim 8, wherein the step of evaporating the second organic solvent from the third solution is carried out at a temperature less than or equal to 200 °C.

18. The method of claim 8, wherein the step of annealing the electrolyte powders is carried out at a temperature less than 300 °C, and wherein the step of annealing the electrolyte powders is carried out in an inert atmosphere or under vacuum.

19. An all-solid-state battery, comprising: an anode; a cathode; and an electrolyte comprising an electrolyte material and positioned between the anode and the cathode,wherein the electrolyte material is of the formula Li3PS4-xLiBH4-aLiCl-bLiBr-cLiI, wherein x is 1-3, a is 0-1, b is 0-1, and c is 0-1 , and wherein the cathode has a sulfur content of at least 40 wt% based on a total weight of the cathode.

20. The all-solid-state battery of claim 19, wherein the electrolyte material has a primary particle size of below 10 pm.

21. The all-solid-state battery of claim 19, wherein the electrolyte material has a density below 2.0 g cm'3.

22. The all-solid-state battery of claim 19, wherein the electrolyte material has an ionic conductivity of over 1.0 mS cm-1at 25°C.

23. The all-solid-state battery of claim 19, wherein the cathode comprises a cathode active material, the electrolyte material, a polymer binder, and conductive carbon.

24. The all-solid-state battery of claim 23, wherein the cathode active material is selected from the group consisting of sulfur, lithium cobalt oxide, and lithium nickel manganese cobalt oxide.

25. The all-solid-state battery of claim 19, wherein the anode is a lithium or lithium alloy foil.

26. The all-solid-state battery of claim 19, wherein the anode comprises an anode active material, the electrolyte material, a polymer binder, and conductive carbon.

27. The all-solid-state battery of claim 26, wherein the anode active material is selected from the group consisting of silicon, graphite, and tin.

28. A method of making an all-solid-state battery, comprising: synthesizing an electrolyte material of the formula Li3PS4-xLiBH4-aLiCl-bLiBr-cLil, wherein x is 1-3, a is 0-1, b is 0-1, and c is 0-1; forming an electrolyte pellet comprising the electrolyte material; forming a cathode particulate material; forming a cathode on a first side of the electrolyte pellet, wherein the cathode has a sulfur content of at least 40 wt% based on a total weight of the cathode; and forming an anode on a second side of the electrolyte pellet such that the electrolyte pellet is positioned between the anode and the cathode.

29. The method of claim 28, wherein the electrolyte material has a primary particle size of below 10 pm.

30. The method of claim 28, wherein the electrolyte material has a density below 2.0 g cm-3.

31. The method of claim 28, wherein the electrolyte material has an ionic conductivity of over 1.0 mS cm’1at 25°C.

32. The method of claim 28, wherein the step of synthesizing an electrolyte material is a liquid-phase synthesis step.

33. The method of claim 32, wherein the step of synthesizing an electrolyte material comprises: adding J2S, P2S5, and I BH4 alone or in combination with at least one compound selected from the group consisting of Li Cl, LiBr, and Lil to a solvent; and removing the electrolyte material from the solvent.

34. The method of claim 33, wherein the solvent is a pure solvent or solvent mixture selected from the group consisting of tetrahydrofuran, cyclopentyl methyl ether, 2-methyltetrahydrofuran, dimethly formamide, dimethoxy ethane, pyridine, 1,3 -dioxolane, ethyl acetate, methyl acetate, acetonitrile, ethanol, methanol, propanol, butanol, and diethyl ether.

35. The method of claim 28, wherein the cathode particulate material comprises sulfur, the electrolyte material, a polymer binder, and conductive carbon.

36. The method of claim 28, wherein the step of forming a cathode on a first side of the electrolyte pellet comprises: depositing the cathode particulate material on the first side of the electrolyte pellet; andcompressing the cathode particulate material to form the cathode.

37. The method of claim 28, wherein the step of forming an anode on a second side of the electrolyte pellet comprises: compressing a lithium foil alone or in combination with a second foil to form the anode.

38. The method of claim 37, wherein the second foil is selected from the group consisting of indium, tin, aluminum, zinc, and magnesium.

Citation Information

Patent Citations

  • Ionic conductor and method for producing the same

    US20170338512A1

  • Solid Electrolyte of Lithium Secondary Battery and Sulfide Compound for Said Solid Electrolyte

    US20200127325A1

  • Solid electrolyte material and solid-state battery made therewith

    US20210296690A1

  • Lithium, phosphorus, sulfur, and iodine including electrolyte and catholyte compositions, electrolyte membranes for electrochemical devices, and annealing methods of making these electrolytes and catholytes

    WO2017096088A1

Cited By

  • Double-layer solid electrolyte membrane, preparation method thereof and all-solid-state battery

    CN119627200A

  • A double-layer solid electrolyte membrane, a preparation method thereof, and a all-solid-state battery

    CN119627200B

  • Hydride ion conductor and preparation method thereof

    KR102901089B1