Super-elastic fiber and preparation method therefor

By using specific components and tensile crosslinking processes, the problems of conductivity and porous fiber material accuracy of traditional fiber materials are solved, and high-conductivity and superelastic fibers are prepared to meet the needs of smart fabrics and wearable electronic products.

WO2024229756A2PCT designated stage expired Publication Date: 2024-11-14FUJIAN BILLION POLYMERIZATION FIBER TECHNOLOGY IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/093280
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Traditional fiber materials cannot meet the high conductivity and superelastic needs of smart fabrics and wearable electronic products, and the low preparation accuracy and uneven pore size distribution of porous fiber materials limit their application.

Method used

Using polyurethane TPU, polypropylene, refined terephthalic acid, ethylene glycol, polyglycerol, nano zinc oxide powder, acrylic elastomer and nano antimony trioxide particles, the fiber front is made through stretching and crosslinking process. The polymer molecules in the body are arranged in a directional manner and cross-linked to form superelastic fibers with high superstable conductivity and good tensile properties.

Benefits of technology

High-precision control and stable pore size distribution are achieved, and superelastic fibers with high, ultra-stable conductivity and good tensile properties are prepared, suitable for smart fabrics and wearable electronic products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 000011
    Figure 000011
  • Figure 00000010_0000
    Figure 00000010_0000
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

Superelastic fiber and preparation method thereof Technical Field

[0001] The present invention relates to the field of fiber technology, in particular to a superelastic fiber and a preparation method thereof. Background Art

[0002] With the rapid development of smart textiles and wearable electronics in recent years, highly conductive and superelastic fibers have become key components in these fields. Conventional fiber materials often fail to meet these requirements, necessitating the development of novel fiber materials to meet market demand. Currently, some studies have used coaxial wet spinning to produce highly conductive and superelastic fibers, but these methods present challenges such as a complex preparation process and unstable conductivity.

[0003] To address the application limitations of traditional fiber materials, porous fiber materials have been widely researched and applied in recent years. Their porous structure improves fiber softness and air permeability, offering broad application prospects in sound absorption, filtration, and thermal insulation. However, traditional porous fiber materials suffer from issues such as low preparation precision and uneven pore size distribution, which restrict their application in certain fields.

[0004] In view of this, the present invention is proposed. Summary of the Invention

[0005] The technical problem to be solved by the present invention is to overcome the shortcomings of the existing technology and provide a superelastic fiber and a preparation method thereof. The superelastic fiber should have high and ultra-stable electrical conductivity and good tensile properties, and its preparation method should be simple and easy to implement, and can achieve high-precision control and stable pore size distribution.

[0006] In order to solve the above technical problems, the basic concept of the technical solution adopted by the present invention is:

[0007] A superelastic fiber, composed of the following raw materials in parts by weight:

[0008] Polyurethane TPU 5-10 parts;

[0009] 6-20 parts of polypropylene;

[0010] 4-6 parts of purified terephthalic acid;

[0011] 5-8 parts of ethylene glycol;

[0012] Polyglycerol 0.5-1 part;

[0013] 0.05-0.2 parts of nano zinc oxide powder;

[0014] 20-30 parts of propylene-based elastomer;

[0015] 0.1 to 0.6 parts of nano antimony trioxide particles.

[0016] In a preferred embodiment of any of the above schemes, the polyglycerol is polyethylene glycol-10 alkyl ether.

[0017] In a preferred embodiment of any of the above schemes, the stretching rate of the superelastic fiber is ≥500%, and the rebound rate is ≥95%.

[0018] In a preferred embodiment of any of the above solutions, the diameter of the superelastic fiber is in the range of 10 nm to 100 μm.

[0019] In a second aspect, a method for preparing a superelastic fiber comprises the following steps:

[0020] dissolving a polymer material in a suitable solvent to form a fiber precursor;

[0021] Through stretching and cross-linking processes, the polymer molecules in the fiber precursor undergo directional arrangement, cross-linking and condensation reactions to form fibers with super elasticity.

[0022] In a preferred embodiment of any of the above schemes, the mixing ratio of the polymer materials is:

[0023] Polyurethane TPU 6-9 parts;

[0024] Polypropylene 7-19 parts;

[0025] 4.1-5 parts of purified terephthalic acid;

[0026] 6-7 parts of ethylene glycol;

[0027] Polyglycerol 0.5-1 part;

[0028] 0.06-0.2 parts of nano zinc oxide powder;

[0029] 21-29 parts of propylene-based elastomer;

[0030] 0.2 to 0.5 parts of nano antimony trioxide particles.

[0031] In a preferred embodiment of any of the above schemes, the method for preparing the superelastic fiber, the stretching process specifically comprises the following steps:

[0032] Adjust the mixing ratio and determine the mixing ratio and proportion of the fiber precursor according to different fiber precursor components;

[0033] Adding additives according to different fiber precursor components;

[0034] According to the type, morphology and chemical properties of the fiber precursor, the stretching speed and temperature are adjusted to control the arrangement state of the fiber precursor so that the polymer molecules are evenly arranged along the stretching direction and maintain a three-dimensional structure.

[0035] In a preferred embodiment of any of the above schemes, in the method for preparing the superelastic fiber, the cross-linking process specifically comprises the following steps:

[0036] Select the cross-linking agent and determine the type, content and addition method of the cross-linking agent based on the chemical properties and morphological requirements of the polymer;

[0037] Add the selected cross-linking agent to the polymer. Depending on the type of polymer and cross-linking agent, add the cross-linking agent in one go or in batches.

[0038] The cross-linking agent and the polymer are fully mixed and heated at a certain temperature to promote the reaction between the cross-linking agent and the polymer;

[0039] The crosslinker reaction product is fixed in the polymer by the curing process.

[0040] After adopting the above technical solution, the present invention has the following beneficial effects compared with the prior art.

[0041] Through stretching and cross-linking processes, the polymer molecules in the fiber precursor undergo directional arrangement, cross-linking and condensation reactions to form fibers with superelasticity. The superelastic fibers should have high and ultra-stable electrical conductivity and good tensile properties, and their preparation method should be simple and easy, capable of achieving high-precision control and stable pore size distribution.

[0042] The specific embodiments of the present invention will be described in further detail below with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation of the present application. Some specific embodiments of the present application will be described in detail in an illustrative and non-restrictive manner with reference to the drawings. The same reference numerals in the drawings indicate the same or similar components or parts. It should be understood by those skilled in the art that these drawings are not necessarily drawn to scale. In the drawings:

[0044] FIG1 is a schematic diagram of a method for preparing superelastic fibers according to the present invention.

[0045] It should be noted that these drawings and text descriptions are not intended to limit the scope of the present invention in any way, but rather to illustrate the concept of the present invention for those skilled in the art by referring to specific embodiments. The elements in the drawings are schematic and not drawn to scale. DETAILED DESCRIPTION

[0046] In order to enable those skilled in the art to better understand the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of this application.

[0047] The following embodiments of the present application take superelastic fibers and their preparation methods as examples to explain the solutions of the present application in detail, but this embodiment does not limit the scope of protection of the present application.

[0048] Example 1

[0049] The present invention provides a method for preparing a superelastic fiber, the method comprising the following steps:

[0050] Step 11, dissolving the polymer material in a suitable solvent to form a fiber precursor;

[0051] Step 12, through stretching and cross-linking process, the polymer molecules in the fiber precursor are oriented, cross-linked and condensed to form fibers with super elasticity. The mixing ratio of the polymer materials is: polyurethane TPU 6 parts; polypropylene 7 parts; purified terephthalic acid 4.1 parts; ethylene glycol 6 parts; polyglycerol 0.5 parts; nano zinc oxide powder 0.06 parts; propylene-based elastomer 21 parts; nano antimony trioxide particles 0.2 parts; the stretching process specifically includes the following steps: adjusting the mixing ratio, determining the mixing ratio and proportion of the fiber precursor according to different fiber precursor components; adding additives according to different fiber precursor components; adjusting the stretching speed and temperature according to the type, morphology and chemical properties of the fiber precursor, and controlling the arrangement state of the fiber precursor so that the polymer molecules are evenly arranged along the stretching direction and maintain a three-dimensional structure; the cross-linking process specifically includes the following steps: selecting a cross-linking agent, determining the type, content and addition method of the cross-linking agent according to the chemical properties and morphological requirements of the polymer; adding the selected cross-linking agent to the polymer, and selecting single or batch addition of the cross-linking agent according to different types of polymers and cross-linking agents; fully mixing the cross-linking agent and the polymer, and heating at a certain temperature to promote the reaction of the cross-linking agent and the polymer; fixing the cross-linking agent reaction product in the polymer through curing treatment. The present invention achieves superelastic fibers by uniformly aligning the polymer molecules in the fiber precursor along the stretching direction while maintaining a three-dimensional structure. This preparation method is simple and easy to implement, enabling high-precision control and stable pore size distribution, and has promising application prospects.

[0052] Example 2

[0053] The present invention provides a method for preparing a superelastic fiber, the method comprising the following steps:

[0054] Step 11, dissolving the polymer material in a suitable solvent to form a fiber precursor;

[0055] Step 12, through stretching and cross-linking process, the polymer molecules in the fiber precursor are oriented, cross-linked and condensed to form fibers with super elasticity. The mixing ratio of the polymer materials is: polyurethane TPU 7 parts; polypropylene 8 parts; purified terephthalic acid 4.2 parts; ethylene glycol 6.2 parts; polyglycerol 0.6 parts; nano zinc oxide powder 0.07 parts; propylene-based elastomer 22 parts; nano antimony trioxide particles 0.3 parts; the stretching process specifically includes the following steps: adjusting the mixing ratio, determining the mixing ratio and proportion of the fiber precursor according to different fiber precursor components; adding additives according to different fiber precursor components; adjusting the stretching speed and temperature according to the type, morphology and chemical properties of the fiber precursor, and controlling the arrangement state of the fiber precursor so that the polymer molecules are evenly arranged along the stretching direction and maintain a three-dimensional structure; the cross-linking process specifically includes the following steps: selecting a cross-linking agent, determining the type, content and addition method of the cross-linking agent according to the chemical properties and morphological requirements of the polymer; adding the selected cross-linking agent to the polymer, and selecting single or batch addition of the cross-linking agent according to different types of polymers and cross-linking agents; fully mixing the cross-linking agent and the polymer, and heating at a certain temperature to promote the reaction of the cross-linking agent and the polymer; fixing the cross-linking agent reaction product in the polymer through curing treatment.

[0056] In an embodiment of the present invention, the fiber has high elasticity, stretchability and wear resistance. The preparation method begins by dissolving a polymer material in a suitable solvent to form a fiber precursor. Then, through stretching and cross-linking processes, the polymer molecules are oriented, cross-linked and condensed to form a fiber with super elasticity. During the preparation process, multiple components such as polyurethane TPU, polypropylene, purified terephthalic acid, ethylene glycol, polyglycerol, nano zinc oxide powder, propylene-based elastomer and nano antimony trioxide particles are mixed. The mixing ratio is determined according to the characteristics of different fiber precursor components, and additives are added. The stretching speed and temperature are adjusted so that the polymer molecules are evenly arranged along the stretching direction. After cross-linking treatment, the cross-linking agent reaction product is fixed in the polymer. First, the super elastic fiber has high elasticity and wear resistance and is suitable for high-strength application scenarios. Secondly, through the stretching and cross-linking processes, the polymer molecules are arranged in an orderly manner to form a fiber system with a three-dimensional structure, which makes it have high elasticity and toughness. Finally, the excellent effect of this method comes from the reasonable mixing ratio and the addition of additives, which enable the fiber precursor to fully exert the effects of various components, thereby obtaining superior chemical and physical properties.

[0057] Example 3

[0058] The present invention provides a method for preparing a superelastic fiber, the method comprising the following steps:

[0059] Step 11, dissolving the polymer material in a suitable solvent to form a fiber precursor;

[0060] Step 12, through stretching and cross-linking process, the polymer molecules in the fiber precursor are oriented, cross-linked and condensed to form fibers with super elasticity. The mixing ratio of the polymer materials is: polyurethane TPU 7.1 parts; 9 parts of polypropylene; 4.3 parts of purified terephthalic acid; 6.3 parts of ethylene glycol; 0.7 parts of polyglycerol; 0.09 parts of nano zinc oxide powder; 25 parts of propylene-based elastomer; 0.4 parts of nano antimony trioxide particles; the stretching process specifically includes the following steps: adjusting the mixing ratio, determining the mixing ratio and proportion of the fiber precursor according to different fiber precursor components; adding additives according to different fiber precursor components; adjusting the stretching speed and temperature according to the type, morphology and chemical properties of the fiber precursor, and controlling the arrangement state of the fiber precursor so that the polymer molecules are evenly arranged along the stretching direction and maintain a three-dimensional structure; the cross-linking process specifically includes the following steps: selecting a cross-linking agent, determining the type, content and addition method of the cross-linking agent according to the chemical properties and morphological requirements of the polymer; adding the selected cross-linking agent to the polymer, and selecting single or batch addition of the cross-linking agent according to different types of polymers and cross-linking agents; fully mixing the cross-linking agent and the polymer, and heating them at a certain temperature to promote the reaction of the cross-linking agent and the polymer; and fixing the cross-linking agent reaction product in the polymer through curing treatment.

[0061] Example 4

[0062] The present invention provides a method for preparing a superelastic fiber, the method comprising the following steps:

[0063] Step 11, dissolving the polymer material in a suitable solvent to form a fiber precursor;

[0064] Step 12, through stretching and cross-linking process, the polymer molecules in the fiber precursor are oriented, cross-linked and condensed to form fibers with super elasticity. The mixing ratio of the polymer materials is: polyurethane TPU 8 parts; 11 parts of polypropylene; 4.5 parts of purified terephthalic acid; 6.7 parts of ethylene glycol; 0.8 parts of polyglycerol; 0.1 parts of nano zinc oxide powder; 25 parts of propylene-based elastomer; 0.4 parts of nano antimony trioxide particles; the stretching process specifically includes the following steps: adjusting the mixing ratio, determining the mixing ratio and proportion of the fiber precursor according to different fiber precursor components; adding additives according to different fiber precursor components; adjusting the stretching speed and temperature according to the type, morphology and chemical properties of the fiber precursor, and controlling the arrangement state of the fiber precursor so that the polymer molecules are evenly arranged along the stretching direction and maintain a three-dimensional structure; the cross-linking process specifically includes the following steps: selecting a cross-linking agent, determining the type, content and addition method of the cross-linking agent according to the chemical properties and morphological requirements of the polymer; adding the selected cross-linking agent to the polymer, and selecting single or batch addition of the cross-linking agent according to different types of polymers and cross-linking agents; fully mixing the cross-linking agent and the polymer, and heating them at a certain temperature to promote the reaction of the cross-linking agent and the polymer; and fixing the cross-linking agent reaction product in the polymer through curing treatment.

[0065] In an embodiment of the present invention, the preparation method comprises the following steps: dissolving a polymer material in a suitable solvent to form a fiber precursor. Through stretching and crosslinking processes, the polymer molecules in the fiber precursor are aligned, crosslinked, and condensed to form superelastic fibers. During the preparation process, the mixing ratio of various components, including polyurethane (TPU), polypropylene, purified terephthalic acid, ethylene glycol, polyglycerol, nano-zinc oxide powder, propylene-based elastomer, and nano-antimony trioxide particles, is designed. Furthermore, depending on the fiber precursor components, additives are added, and the stretching speed and temperature are adjusted to ensure uniform alignment of the polymer molecules along the stretching direction and maintain a three-dimensional structure. A suitable crosslinking agent is selected and added to the polymer. Depending on the polymer and crosslinking agent, the crosslinking agent can be added in a single addition or in batches. After adding the crosslinking agent, the mixture is thoroughly mixed and heated at a certain temperature to promote reaction between the crosslinking agent and the polymer. Finally, a curing process is performed to fix the position of the crosslinking agent reaction product within the polymer. The primary technical benefit of this preparation method is that the resulting superelastic fiber exhibits high elasticity, stretchability, and abrasion resistance, making it suitable for a variety of high-strength applications. Through stretching and cross-linking processes, the polymer molecules are oriented and maintain a three-dimensional structure, which gives the fiber excellent physical properties. Due to the reasonable mixing ratio and the use of additives, the various components can fully play their role, thus making the super elastic fiber have better chemical and physical properties.

[0066] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some or all of the technical features therein. These modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application.

Claims

1. A superelastic fiber, characterized in that: By weight, it is composed of the following raw materials: Polyurethane TPU 5-10 parts; Polypropylene 6-20 parts; 4-6 parts of purified terephthalic acid; 5-8 parts of ethylene glycol; Polyglycerol 0.5-1 part; 0.05-0.2 parts of nano zinc oxide powder; 20-30 parts of propylene-based elastomer; 0.1 to 0.6 parts of nano antimony trioxide particles.

2. The superelastic fiber according to claim 1, characterized in that The polyglycerol is polyethylene glycol-10 alkyl ether.

3. The superelastic fiber according to claim 2, characterized in that: The elongation rate of the superelastic fiber is ≥500%, and the resilience rate is ≥95%.

4. The superelastic fiber according to claim 3, characterized in that The diameter of the superelastic fiber ranges from 10 nm to 100 μm.

5. A method for preparing a superelastic fiber as claimed in any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps: dissolving a polymer material in a suitable solvent to form a fiber precursor; Through the stretching and cross-linking process, the polymer molecules in the fiber precursor are oriented, cross-linked and condensed to form fibers with super elasticity.

6. The method for preparing superelastic fiber according to claim 5, characterized in that: The mixing ratio of the polymer materials is: Polyurethane TPU 6-9 parts; Polypropylene 7-19 parts; 4.1-5 parts of purified terephthalic acid; 6-7 parts of ethylene glycol; Polyglycerol 0.5-1 part; 0.06-0.2 parts of nano zinc oxide powder; 21-29 parts of propylene-based elastomer; 0.2 to 0.5 parts of nano antimony trioxide particles.

7. The method for preparing superelastic fiber according to claim 6, characterized in that: The stretching process specifically comprises the following steps: Adjust the mixing ratio, and determine the mixing ratio and proportion of the fiber precursor according to different fiber precursor components; Adding additives according to different fiber precursor components; According to the type, morphology and chemical properties of the fiber precursor, the stretching speed and temperature are adjusted to control the arrangement state of the fiber precursor so that the polymer molecules are evenly arranged along the stretching direction and maintain a three-dimensional structure.

8. The method for preparing superelastic fiber according to claim 7, characterized in that: The cross-linking process specifically comprises the following steps: Select the cross-linking agent and determine the type, content and addition method of the cross-linking agent according to the chemical properties and morphological requirements of the polymer; Add the selected cross-linking agent to the polymer. Depending on the different types of polymers and cross-linking agents, add the cross-linking agent once or in batches; The cross-linking agent and the polymer are fully mixed and heated at a certain temperature to promote the reaction between the cross-linking agent and the polymer; The crosslinker reaction product is fixed in the polymer by the curing process.