Layered oxide positive electrode material and preparation method therefor, positive electrode composition, and sodium-ion secondary battery and use thereof

By using Mg, Al and Ti as doping elements in the layered oxide positive electrode material, the CuO heterogeneous phase is eliminated, and the electrochemical performance problems caused by CuO heterogeneous phase under high Cu content is solved, and the retraction of sodium ion secondary batteries is improved. Electric first effect.

WO2024230150A1PCT designated stage expired Publication Date: 2024-11-14BEIJING HINA BATTERY TECH CO LTD

Patent Information

Application Number
PCT/CN2023/137095
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-05
Filing Date
2023-12-07
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

The prior art is difficult to reduce the CuO heterogeneous phase in the layered oxide positive electrode material under high Cu content, resulting in poor electrochemical performance of sodium ion secondary batteries, especially low first-term efficiency of the charge-delay.

Method used

Mg, Al and Ti as doping elements were used, and the CuO heterogeneous phase was eliminated by uniform mixing and sintering treatment of stoichiometric ratio to prepare a near-pure phase layered oxide positive electrode material with high Cu content.

Benefits of technology

The electrochemical performance of sodium ion secondary batteries is effectively improved, especially the first effect of charging, and without increasing the sintering temperature and time, the preparation of a high Cu content positive electrode material with a Cu mole ratio of less than 0.3 was achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023137095_14112024_PF_FP_ABST
    Figure CN2023137095_14112024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present invention are a layered oxide positive electrode material and a preparation method therefor, a positive electrode composition, and a sodium-ion secondary battery and the use thereof. The general formula of the layered oxide positive electrode material is NaxCuaNibFecMndMyO2+nδ, wherein each parameter in the general formula has a range as defined in the description, and a doping element M at least comprises Mg+Al+Ti. In the present invention, a CuO impurity phase in a product can be effectively eliminated under the condition of a relatively high Cu content, and the electrochemical performance of the corresponding sodium-ion secondary battery is improved, such as the initial efficiency of a button battery.
Need to check novelty before this filing date? Find Prior Art

Description

Layered oxide positive electrode material, preparation method thereof, positive electrode composition, sodium ion secondary battery and use thereof

[0001] This application claims priority to Chinese Patent Application No. 202310490958.2 filed on May 5, 2023, and the contents of the above-mentioned Chinese patent application disclosure are hereby incorporated by reference in their entirety as a part of this application. Technical Field

[0002] The present invention generally relates to the field of energy storage technology, in particular to the field of sodium ion secondary batteries. Specifically, the present invention relates to layered oxide positive electrode materials, methods for preparing the same, positive electrode compositions comprising the same, sodium ion secondary batteries comprising the positive electrode compositions, and uses of the sodium ion secondary batteries. Background Art

[0003] Lithium-ion secondary batteries (Li-ion batteries) are widely used in portable electronic devices and electric vehicles due to their high energy density and long cycle life. However, the limited and uneven distribution of lithium resources, particularly with the recent surge in the electric vehicle industry, has led to increasing scarcity of lithium resources and rising prices for upstream materials, posing significant challenges to the application of Li-ion secondary batteries. Compared to lithium, sodium, with its abundant reserves and low price, has attracted increasing attention.

[0004] Compared with lithium secondary batteries, sodium ion secondary batteries have a lower energy density. Although studies have found that layered oxide positive electrode materials have a higher theoretical capacity and therefore a higher energy density. However, the intrinsic air stability of layered oxide positive electrode materials is poor, resulting in poor consistency in the physical properties and electrochemical indicators of the finished materials. In this regard, people have found, after a lot of research, that the air stability can be improved by introducing Cu into the layered oxide positive electrode materials. However, the addition of Cu, especially when the Cu content is high, will cause the layered oxide positive electrode material to produce more CuO impurities, deteriorating the electrochemical performance of the sodium ion secondary battery, such as the first charge efficiency. In order to reduce the CuO impurity phase, the methods commonly used in the prior art include increasing the sintering temperature, extending the sintering time, optimizing the sintering atmosphere, and reducing the proportion of impurity raw materials. However, the above methods will have an adverse effect on the material properties, and the electrochemical performance of the positive electrode material obtained by reducing the proportion of impurity raw materials is not significantly improved or does not meet the modification requirements.

[0005] In view of the above problems, technicians urgently need to develop a new layered oxide positive electrode material, which contains a higher Cu content and less CuO impurities.

[0006] Summary of the Invention

[0007] In view of the problems existing in the prior art, the present invention provides a new layered oxide positive electrode material and a related sodium ion secondary battery, aiming to eliminate the CuO impurity phase in the layered oxide positive electrode material and effectively improve the electrochemical performance of the sodium ion secondary battery, such as the first charge efficiency.

[0008] In a first aspect, the present invention relates to a layered oxide cathode material having the general formula: Na x Cu a Ni b Fe c Mn d M y O 2+nδ ,

[0009] where 0.60≤x≤1.20, 0.05≤a≤0.40, 0.03≤b≤0.70, 0.10≤c≤0.45, 0.10≤d≤0.45, 0<y≤0.30, and x+2a+2b+3c+3d+2y<4<x+2a+3b+3c+4d+4y, 0.95≤a+b+c+d+y≤1.05, 0<n≤0.1, -1≤δ≤3; and

[0010] M includes Mg+Al+Ti, and optionally includes one or more of Ca, B, Li, K, W, Mo, Sr, Y, Sn, Sb, and Ce.

[0011] In a second aspect, the present invention relates to a method for preparing the layered oxide positive electrode material according to the first aspect of the present invention, comprising the following steps:

[0012] Step a: uniformly mixing a Na source, a Cu source, a Ni source, a Fe source, a Mn source, and a M source in a stoichiometric ratio to obtain a mixture precursor;

[0013] Step b: sintering the precursor obtained in step a; and

[0014] Step c: Cooling the product obtained in step b, and optionally crushing and screening it.

[0015] In a third aspect, the present invention relates to a positive electrode composition comprising the layered oxide positive electrode material according to the first aspect of the present invention.

[0016] In a fourth aspect, the present invention relates to a sodium ion secondary battery comprising the positive electrode composition according to the third aspect of the present invention.

[0017] In a fifth aspect, the present invention relates to the use of the sodium ion secondary battery of the fourth aspect of the present invention in an energy storage device for solar power generation, wind power generation, smart grid peak regulation, distributed power station, backup power supply or communication base station.

[0018] The present invention simultaneously utilizes Mg, Al and Ti as doping elements, effectively eliminating the CuO impurity phase in the layered oxide, and ultimately improving the electrochemical performance of the corresponding sodium ion secondary battery, such as the first charge efficiency. Compared with the prior art, the proportion of impurity raw materials in the present invention is relatively high, which effectively improves the performance of the layered oxide positive electrode material. In addition, the present invention also makes it possible to obtain a layered oxide positive electrode material with a high Cu content and a Cu molar ratio of less than 0.3 without increasing the sintering temperature and sintering time. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] To more clearly illustrate the technical solution of the present invention, the following briefly describes the drawings required for describing the embodiments. It should be understood that these drawings are only for the purpose of facilitating easier understanding of the present invention by technicians and are not intended to limit the scope of the present invention.

[0020] FIG1 shows XRD spectra of layered oxide positive electrode materials prepared in Comparative Examples C1-C5 and Examples E1-E10. DETAILED DESCRIPTION

[0021] In order to make the invention objectives, technical solutions and beneficial technical effects of this application clearer, this application will be described in detail below. It should be noted that the various aspects, features, implementation methods, and advantages described in this application may be compatible and / or combinable.

[0022] Unless otherwise specified, the meanings of the technical terms in this specification are the same as those generally understood by those skilled in the art.

[0023] The present invention relates to a layered oxide positive electrode material, a preparation method thereof, a positive electrode composition comprising the layered oxide positive electrode material, a sodium ion secondary battery comprising the positive electrode composition, and uses of the sodium ion secondary battery.

[0024] The present invention will be described in detail below.

[0025] Layered oxide cathode materials

[0026] The first aspect of the present invention provides a layered oxide positive electrode material having the following general formula: Na x Cu a Ni b Fe c Mn d M y O 2+nδ ,

[0027] where 0.60≤x≤1.20, 0.05≤a≤0.40, 0.03≤b≤0.70, 0.10≤c≤0.45, 0.10≤d≤0.45, 0<y≤0.30, and x+2a+2b+3c+3d+2y<4<x+2a+3b+3c+4d+4y, 0.95≤a+b+c+d+y≤1.05, 0<n≤0.1, -1≤δ≤3; and

[0028] M includes Mg+Al+Ti, and optionally includes one or more of Ca, B, Li, K, W, Mo, Sr, Y, Sn, Sb, and Ce.

[0029] In layered oxide positive electrode materials, the presence of CuO impurity phase will deteriorate the electrochemical performance of the corresponding sodium ion secondary battery, such as the first charge efficiency. Therefore, the presence of CuO impurity phase has hindered technicians from increasing the doping amount of Cu, because although adding a certain amount of Cu can improve air stability, it will seriously deteriorate performance such as the first charge efficiency. In order to eliminate the CuO impurity phase, the prior art usually adopts measures such as increasing the sintering temperature, extending the sintering time, and reducing the proportion of Cu, but these measures will either have an adverse effect on the performance of the resulting positive electrode material, or fail to achieve the expected doping effect due to the low content of the doping element. Compared with the prior art, the present invention uses Mg, Al and Ti as doping elements at the same time when the Cu content is high, which effectively eliminates the CuO impurity phase in the layered oxide and improves the electrochemical performance of the corresponding sodium ion secondary battery, such as the first charge efficiency.

[0030] In some embodiments, the layered oxide cathode material of the present invention is nearly pure phase. To evaluate the crystallinity of the layered oxide cathode material of the present invention, the present invention introduces two parameters, α and β, to characterize the corresponding ratio of the peak area and peak intensity of the CuO impurity phase in the XRD spectrum to the peak area and peak intensity of the specific peak of the layered oxide cathode material. The closer α and β are to 0, the less CuO impurity phase is in the product. The calculation method of α and β is as follows:

[0031] α=(AI (-111) %+AI (111) %) / (AI (003) %+AI (104) %)

[0032] β=(HI (-111) %+HI (111) %) / (HI (003) %+HI (104) %)

[0033] In the above formula, AI (003)% represents the ratio of the peak area of ​​the (003) peak in the XRD spectrum of the layered oxide positive electrode material to the peak area of ​​the highest peak in the XRD spectrum; AI (104) % represents the ratio of the peak area of ​​the (104) peak in the XRD spectrum of the layered oxide positive electrode material to the peak area of ​​the highest peak in the XRD spectrum; HI (003) % represents the ratio of the peak value (i.e., peak intensity, the same below) of the (003) peak in the XRD spectrum of the layered oxide positive electrode material to the peak value of the highest peak in the XRD spectrum; HI (104) % represents the ratio of the peak value of the (104) peak in the XRD spectrum of the layered oxide positive electrode material to the peak value of the highest peak in the XRD spectrum; AI (-111) % represents the ratio of the peak area of ​​the (-111) peak of the CuO impurity phase in the XRD spectrum of the layered oxide positive electrode material to the peak area of ​​the highest peak in the XRD spectrum; AI (111) % represents the ratio of the peak area of ​​the (111) peak of the CuO impurity phase in the XRD spectrum of the layered oxide positive electrode material to the peak area of ​​the highest peak in the XRD spectrum; HI (-111) % represents the ratio of the peak value of the (-111) peak of the CuO impurity phase in the XRD spectrum of the layered oxide positive electrode material to the peak value of the highest peak in the XRD spectrum; (111) % represents the ratio of the peak value of the (111) peak of the CuO impurity phase in the XRD spectrum of the layered oxide positive electrode material to the peak value of the highest peak in the XRD spectrum. When measuring the XRD spectrum (see the Examples for specific measurement methods), the same sample can be tested multiple times, and the average of the test results can be substituted into the above formula to calculate α and β.

[0034] In addition, α / β indirectly indicates the average half-width of the CuO impurity peak. A smaller α / β mainly indicates that α approaches 0 more quickly, indicating that the CuO impurity content is low and the relatively large grains are occasional precipitation, rather than widespread precipitation composed of many discrete small grains.

[0035] In some embodiments, in the layered oxide cathode material of the present invention, α<0.0500, β<0.0200, and α / β<2.5000.

[0036] The above-mentioned evaluation criteria of the present invention start from the basic indicators of the material, and use the two indicators of peak area ratio and peak intensity ratio for collaborative evaluation to assist in the verification of crystallinity. It can reduce detection misjudgments, improve the accuracy of the evaluation results, and have a higher credibility, making it possible to detect impurity phases in layered oxide positive electrode materials.

[0037] In the general formula of the layered oxide positive electrode material of the present invention, 0.60≤x≤1.20, preferably 0.70≤x≤1.20, more preferably 0.95≤x≤1.20, and even more preferably 0.95≤x≤1.02. As an example, x is 0.60, 0.61, 0.62, 0.63, 0.64, 0.65, 0.66, 0.67, 0.68, 0.69, 0.70, 0.71, 0.72, 0.73, 0.74, 0.75, 0.76, 0.77, 0.78, 0.79, 0.80, 0.81, 0.82, 0.83, 0.84, 0.85, 0.86, 0.87, 0.88, 0.89, 0.90, 0.91 , 0.92, 0.93, 0.94, 0.95, 0.96, 0.97, 0.98, 0.99, 1.00, 1.01, 1.02, 1.03, 1.04, 1.05, 1.06, 1.07, 1.08, 1.09, 1.10, 1.11, 1.12, 1.13, 1.14, 1.15, 1.16, 1.17, 1.18, 1.19, 1.20, or in the range consisting of any two of the above values.

[0038] In the general formula of the layered oxide positive electrode material of the present invention, 0.05≤a≤0.40, preferably 0.05≤a≤0.30. For example, a is 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.11, 0.12, 0.13, 0.14, 0.15, 0.16, 0.17, 0.18, 0.19, 0.20, 0.21, 0.22, 0.23, 0.24, 0.25, 0.26, 0.27, 0.28, 0.29, 0.30, 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37, 0.38, 0.39, 0.40, or a range consisting of any two of these values.

[0039] In the general formula of the layered oxide positive electrode material of the present invention, 0<y≤0.30, preferably 0.04≤y≤0.20. For example, y is 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.11, 0.12, 0.13, 0.14, 0.15, 0.16, 0.17, 0.18, 0.19, 0.20, 0.21, 0.22, 0.23, 0.24, 0.25, 0.26, 0.27, 0.28, 0.29, 0.30, or in a range consisting of any two of the foregoing values.

[0040] Similarly, those skilled in the art will appreciate that parameters b, c, and d may also be included in any specific value within the defined range or in a new range consisting of any specific value within the range. For example, in some embodiments, 0.03≤b≤0.70, preferably 0.03≤b≤0.60. For example, the parameter b is 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.11, 0.12, 0.13, 0.14, 0.15, 0.16, 0.17, 0.18, 0.19, 0.20, 0.21, 0.22, 0.23, 0.24, 0.25, 0.26, 0.27, 0.28, 0.29, 0.30, 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37, 0.38, 0.39, 0.40, 0.41, 0.42 0.42, 0.43, 0.44, 0.45, 0.46, 0.47, 0.48, 0.49, 0.50, 0.51, 0.52, 0.53, 0.54, 0.55, 0.56, 0.57, 0.58, 0.59, 0.60, 0.61, 0.62, 0.63, 0.64, 0.65, 0.66, 0.67, 0.68, 0.69, 0.70, or within the range consisting of any two of the above values, and / or 0.10≤c≤0.45, preferably 0.10≤c≤0.40, for example, parameter c is 0.10, d ≤ 0.15, 0.20, 0.21, 0.22, 0.23, 0.24, 0.25, 0.26, 0.27, 0.28, 0.29, 0.30, 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37, 0.38, 0.39, 0.40, 0.41, 0.42, 0.43, 0.44, 0.45, or in the range consisting of any two of the above values, and / or 0.10≤d≤0.45, preferably 0.1 0≤d≤0.40, for example, parameter d is 0.10, 0.11, 0.12, 0.13, 0.14, 0.15, 0.16, 0.17, 0.18, 0.19, 0.20, 0.21, 0.22, 0.23, 0.24, 0.25, 0.26, 0.27, 0.28, 0.29, 0.30, 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37, 0.38, 0.39, 0.40, 0.41, 0.42, 0.43, 0.44, 0.45, or in a range consisting of any two of the above values.

[0041] In the general formula of the layered oxide positive electrode material of the present invention, nδ = -0.05 to 0.15, for example, -0.05, -0.04, -0.03, -0.02, -0.01, 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.11, 0.12, 0.13, 0.14, 0.15, or in a range consisting of any two of the above values, for example, nδ = -0.02 to 0.02, for example, nδ = 0. In some embodiments, 0 < n ≤ 0.1, -1 ≤ δ ≤ 3, for example, n is 0.02, 0.05, 0.08, 0.10, and δ is -1, 0, 1, 2, or 3. Those skilled in the art understand that the parameters x, a, b, c, d, y, n and δ in the general formula of the layered oxide positive electrode material make the general formula satisfy chemical equilibrium.

[0042] After further research, the inventors also found that when the molar ratio of each element is within the range defined below, it is beneficial to further improve the electrochemical performance of the corresponding sodium ion secondary battery, such as the first charge efficiency.

[0043] In some embodiments, the molar ratio of Al / Mg is 1:3.50 to 1:0.25, and the molar ratio of Ti / Mg is 1:6.00 to 1:0.05. Preferably, the molar ratio of Al / Mg is 1:3.00 to 1:0.25. More preferably, the molar ratio of Ti / Mg is 1:5.00 to 1:0.05, more preferably 1:3.00 to 1:0.05. For example, the molar ratio of Al / Mg is 1:0.25, 1:0.50, 1:0.75, 1:1.00, 1:1.25, 1:1.50, 1:1.75, 1:2.00, 1:2.25, 1:2.50, 1:2.75, 1:3.00, 1:3.25, 1:3.50, or a range consisting of any two of the above values. As an example, the molar ratio of Ti / Mg is 1:0.05, 1:0.06, 1:0.15, 1:0.20, 1:0.33, 1:0.40, 1:0.50, 1:0.60, 1:0.70, 1:0.80, 1:0.90, 1:1.00, 1:1.20, 1:1.40, 1:1.60, 1:1.80, 1:2.00, 1:2.25, 1:2.50, 1:2.75, 1:3.00, 1:3.50, 1:4.00, 1:4.50, 1:5.00, 1:5.50, 1:6.00 or within the range formed by any two of the above values.

[0044] In a preferred embodiment, the ratio y / a of the subscript y of the doping element M to the subscript a of the element Cu is 1:9.00 to 1:0.10, preferably 1:7.50 to 1:0.25, more preferably 1:3.00 to 1:0.25. As an example, y / a is 1:0.10, 1:0.15, 1:0.25, 1:0.35, 1:0.50, 1:0.60, 1:0.75, 1:1.00, 1:1.25, 1:1.50, 1:1.75, 1:2.00, 1:2.25, 1:2.50, 1:2.86, 1:3.00, 1:3.75, 1:4.25, 1:5.00, 1:6.00, 1:7.50, 1:8.00, 1:8.50, 1:9.00, or within a range consisting of any two of the above values. When the molar ratio of the total content of the doping element to the Cu content is within the above range, it is beneficial to further eliminate the CuO impurity peak and improve the electrochemical performance of the corresponding sodium ion secondary battery, such as the first charge efficiency.

[0045] In some embodiments, the molar ratio of Mg / Cu is 1:40 to 1:1.00, preferably 1:30 to 1:2.00; and / or the molar ratio of Al / Cu is 1:30 to 1:1.50, preferably 1:20 to 1:3.50; and / or the molar ratio of Ti / Cu is 1:40 to 1:0.25, preferably 1:30 to 1:0.25, more preferably 1:20 to 1:0.25. As an example, the molar ratio of Mg / Cu is 1:1.00, 1:1.50, 1:2.00, 1:3.50, 1:5.00, 1:6.00, 1:7.50, 1:10.00, 1:15.00, 1:20.00, 1:30.00, 1:35.00, 1:40.00 or in the range consisting of any two of the above values, and / or the molar ratio of Al / Cu is 1:1.50, 1:2.00, 1:2.50, 1:3.50, 1:5.00, 1:7.50, 1:10.00, 1:15.00, 1:20.00, 1:30.00, 1:35.00, 1:40.00 or in the range consisting of any two of the above values. : 15.00, 1: 17.50, 1: 20.00, 1: 25.00, 1: 30.00 or within the range consisting of any two of the above values, and / or the molar ratio of Ti / Cu is 1: 0.25, 1: 0.28, 1: 0.47, 1: 1.00, 1: 3.00, 1: 5.00, 1: 7.50, 1: 10.00, 1: 12.00, 1: 15.00, 1: 20.00, 1: 25.00, 1: 30.00, 1: 35.00, 1: 40.00 or within the range consisting of any two of the above values.

[0046] In some embodiments, when the molar amount of the layered oxide positive electrode material is 1 mole, the content of the doping element Mg is 0.01 to 0.05 moles, preferably 0.01 to 0.03 moles. As an example, when the molar amount of the layered oxide positive electrode material is 1 mole, the content of the doping element Mg is 0.01 moles, 0.02 moles, 0.03 moles, 0.04 moles, 0.05 moles, or a range consisting of any two of the foregoing contents.

[0047] In some embodiments, the ratio d / a of the subscript d of the element Mn to the subscript a of the element Cu is 1:0.15 to 1:0.95, preferably 1:0.15 to 1:0.60. For example, d / a is 1:0.15, 1:0.20, 1:0.35, 1:0.40, 1:0.45, 1:0.50, 1:0.55, 1:0.60, 1:0.70, 1:0.80, 1:0.95, or a range consisting of any two of the above values.

[0048] In some embodiments, the ratio a / x of the subscript a of the element Cu to the subscript x of the element Na is 1:3.5 to 1:24, preferably 1:4.5 to 1:24. For example, a / x is 1:3.50, 1:4.50, 1:4.75, 1:6.80, 1:8.00, 1:10.00, 1:12.00, 1:15.00, 1:18.00, 1:20.00, 1:24.00, or a range consisting of any two of the above values.

[0049] In some embodiments, the doping element M is selected from any one of Mg+Al+Ti, Mg+Al+Ti+Li, Mg+Al+Ti+K, or Mg+Al+Ti+Sn.

[0050] In some embodiments, the layered oxide cathode material has an O3 type crystal structure.

[0051] In some embodiments, the pH of the layered oxide cathode material is from 11.00 to 13.00.

[0052] The particle size D50 of the layered oxide positive electrode material of the present invention is not particularly limited, and can be, for example, 1-500 μm, for example, 1, 5, 10, 15, 20, 25, 50, 100, 200, 300, 400, 500 μm, or within a range consisting of any two of the above values. The particle size can be measured by a laser scattering method commonly used in the art. It can be measured using a Malvern particle size analyzer commonly used in the art, such as a MASTERSIZER-3000.

[0053] Preparation method of layered oxide positive electrode material

[0054] Those skilled in the art will appreciate that the layered oxide cathode material of the present invention can be prepared by a variety of methods. As an example, the second aspect of the present invention provides a method for preparing the layered oxide cathode material according to the first aspect of the present invention, comprising the following steps:

[0055] Step a: uniformly mixing a Na source, a Cu source, a Ni source, a Fe source, a Mn source, and a M source in a stoichiometric ratio to obtain a mixture precursor;

[0056] Step b: sintering the precursor obtained in step a; and

[0057] Step c: Cooling the product obtained in step b, and optionally crushing and screening it.

[0058] Step a

[0059] In step a, a Na source, a Cu source, a Ni source, a Fe source, a Mn source, and an optional M source are uniformly mixed in a stoichiometric ratio to obtain a mixture precursor.

[0060] The sodium source can be any sodium-containing compound known to those skilled in the art for use in preparing positive electrode materials for sodium-ion secondary batteries. The sodium source can be one or more of a sodium-containing oxide, hydroxide, salt, and the like. In one or more embodiments, the Na source can be one or more selected from the following compounds: sodium carbonate, sodium bicarbonate, sodium nitrate, sodium acetate, sodium oxalate, sodium hydroxide, and sodium oxide.

[0061] The Cu source can be any copper-containing compound known to those skilled in the art for use in preparing positive electrode materials for sodium-ion secondary batteries. In one or more embodiments, the Cu source can be one or more selected from the following compounds: copper carbonate, copper nitrate, copper acetate, copper oxalate, copper hydroxide, and copper oxide.

[0062] The Ni source may be any nickel-containing compound known to those skilled in the art for use in preparing positive electrode materials for sodium ion secondary batteries. In one or more embodiments, the Ni source may be one or more selected from the following compounds: nickel carbonate, nickel nitrate, nickel acetate, nickel oxalate, nickel hydroxide, and nickel oxide.

[0063] The Fe source can be any nickel-containing compound known to those skilled in the art for use in preparing positive electrode materials for sodium ion secondary batteries. In one or more embodiments, the Fe source can be one or more compounds selected from the group consisting of iron carbonate, iron nitrate, iron acetate, iron oxalate, iron hydroxide, and iron oxide.

[0064] The element M in the M source includes Mg, Al and Ti, and one or more of the following elements: Ca, B, Li, K, W, Mo, Sr, Y, Sn, Sb, Ce. In some embodiments, the M source is one or more compounds selected from the following forms: carbonate, nitrate, acetate, oxalate, hydroxide and oxide.

[0065] The mixing can be performed in any suitable mixing manner known to those skilled in the art. In some embodiments, the mixing in step a is performed by dry mixing or wet mixing, preferably the wet mixing is performed by a sol-gel method or a coprecipitation method.

[0066] Step b

[0067] In step b, the precursor obtained in step a is sintered.

[0068] The sintering temperature is not particularly limited, and may be 700 to 1200°C, preferably 800 to 1100°C, and more preferably 900 to 1000°C. In one or more embodiments, the sintering temperature may be, for example, 700, 710, 720, 730, 740, 750, 760, 770, 780, 790, 800, 810, 820, 830, 840, 850, 860, 870, 880, 890, 900, 910, 920, 930, 940, 950, 960, 970, 980, 990, 1000, 1010, 1020, 1030, 1040, 1050, 1060, 1070, 1080, 1090, 1100, 1110, 1120, 1130, 1140, 1150, 1160, 1170, 1180, 1190, 1200°C, or a range defined by any two of the above values.

[0069] The sintering time is not particularly limited and can be 5 to 36 hours, preferably 8 to 36 hours, more preferably 12 to 20 hours. In some embodiments, the sintering time is 5, 10, 12, 14, 16, 18, 20, 25, 30, 36 hours, or a range defined by any two of the above values.

[0070] In some embodiments, the sintering in step b is performed in an oxidizing atmosphere, preferably compressed air or oxygen. As an example, the oxygen content in the oxidizing atmosphere is greater than 98.5% (volume fraction), and the absolute pressure of the compressed air is greater than 0.6 MPa, such as 0.8 MPa.

[0071] The heating rate during sintering is not particularly limited and can be 1 to 10°C / min, preferably 2 to 5°C / min, for example, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10°C / min, or a range defined by any two of the above values.

[0072] Step c

[0073] In step c, the product obtained in step b is cooled, optionally crushed and sieved.

[0074] The cooling, pulverizing and screening can be performed by any suitable means known to those skilled in the art.

[0075] Positive electrode composition

[0076] A third aspect of the present invention provides a positive electrode composition, which is a positive electrode composition for a sodium ion secondary battery, comprising the layered oxide positive electrode material according to the first aspect of the present invention.

[0077] In addition to the layered oxide cathode material of the present invention, the cathode composition for sodium ion secondary batteries may further include a conductive agent, a binder, and any other substances that can be used by those skilled in the art as needed, such as a dispersant and an additive for improving stability.

[0078] In some embodiments, based on the dry weight of the positive electrode composition for sodium ion secondary batteries, the content of the layered oxide positive electrode material may be a common amount in the art, for example, 70-95 wt %, such as 80-90 wt %.

[0079] The type of conductive agent is not particularly limited, as long as it has the function of enhancing the conductivity of the positive electrode and does not adversely affect the performance of the positive electrode material. Those skilled in the art can select the conductive agent commonly used in the art according to actual needs. As an example, the conductive agent for the positive electrode composition for sodium ion secondary battery can be selected from one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.

[0080] In some embodiments, based on the dry weight of the positive electrode composition for a sodium ion secondary battery, the content of the conductive agent may be a commonly used amount in the art, for example, 1-10 wt %, for example, 2-5 wt %.

[0081] The binder is not particularly limited, as long as it has the properties of enhancing the adhesion between the positive electrode active material particles and the adhesion to the current collector and does not adversely affect the performance of the positive electrode material. Those skilled in the art can select according to actual needs. As an example, the binder for the positive electrode composition for the sodium ion secondary battery can be selected from polyfluoroolefin binders such as polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), ethylene-vinyl acetate copolymer (EVA) or their modified (for example, carboxylic acid, acrylic acid, acrylonitrile, etc.) derivatives and one or more of styrene-butadiene rubber, acrylic resin, carboxymethyl cellulose, polyvinyl alcohol (PVA), etc.

[0082] In some embodiments, based on the dry weight of the positive electrode composition for a sodium ion secondary battery, the content of the binder is 1-10 wt %, for example, 2-5 wt %.

[0083] The positive electrode composition may be in the form of a slurry, ie, it may further include a solvent. The positive electrode composition may also be in a dry form, ie, it does not include a solvent, for example, it may be in the form of a positive electrode active material layer disposed on a positive electrode current collector.

[0084] Sodium ion secondary batteries

[0085] A fourth aspect of the present invention provides a sodium ion secondary battery. A sodium ion secondary battery generally includes a positive electrode, a negative electrode, a separator, and an electrolyte.

[0086] In some embodiments, the sodium ion secondary battery may further include an outer packaging for encapsulating the electrode assembly and the electrolyte. For example, the outer packaging may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc., or a soft package, such as a bag-type soft package, such as a soft package made of polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS).

[0087] The shape of the sodium ion secondary battery is not particularly limited, and it may be cylindrical, square, or any other shape.

[0088] Sodium ion secondary batteries can be prepared by methods commonly used in the art. For example, the positive electrode sheet, the negative electrode sheet and the separator can be made into a battery cell through a winding process or a lamination process, and then the electrolyte is injected.

[0089] positive electrode

[0090] The positive electrode (or positive electrode sheet) comprises a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector, the positive electrode active material layer comprising the positive electrode active material composition of the third aspect of the present invention, for example in dry form. The positive electrode also forms an aspect of the present invention.

[0091] The positive electrode current collector is not particularly limited, and the positive electrode current collector commonly used by those skilled in the art can be used. As an example, the positive electrode current collector can be made of a metal foil such as aluminum foil, nickel foil, or a composite current collector. The composite current collector can be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), 1,3-propane sultone (PS), polyethylene (PE), etc.), but the present invention is not limited to these materials.

[0092] The positive electrode sheet can be prepared according to the method commonly used in the art.

[0093] For example, the positive electrode can be formed by uniformly dispersing a positive electrode active material, a conductive agent, and a binder in a solvent (eg, N-methylpyrrolidone (NMP)) to obtain a positive electrode slurry; coating the slurry on a positive electrode current collector, drying, and pressing.

[0094] Alternatively, the positive electrode can also be formed by uniformly dispersing the positive electrode active material, the conductive agent, and the binder in a solvent (e.g., N-methylpyrrolidone (NMP)) to obtain a positive electrode slurry; casting the positive electrode slurry on a separate support, drying, separating the obtained positive electrode film from the support and laminating it on a positive electrode current collector.

[0095] negative electrode

[0096] The negative electrode (or negative electrode plate) may be a metal sodium plate, or may include a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode active material layer includes a negative electrode active material.

[0097] The negative electrode current collector is not particularly limited, and the negative electrode current collector commonly used by those skilled in the art can be used. As an example, the negative electrode current collector can be a metal foil such as copper foil, or a composite current collector. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector can be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.), but the present invention is not limited to these materials.

[0098] In some embodiments, the negative electrode active material may be an active material commonly used by those skilled in the art. For example, the negative electrode active material may be one or more of natural graphite, artificial graphite, mesophase microcarbon beads (MCMB), hard carbon, soft carbon, silicon-based materials, tin-based materials, lithium titanate, and metallic sodium. Silicon-based materials may be one or more of elemental silicon, silicon oxides, silicon-carbon composites, and silicon alloys, and tin-based materials may be one or more of elemental tin, tin oxides, and tin alloys.

[0099] In addition to the negative electrode active material, the negative electrode active material layer may further include a binder, a conductive agent, and any other optional auxiliary agents such as a thickener.

[0100] There is no particular requirement for the negative electrode conductive agent. As an example, the conductive agent can be selected from one or more of graphite, superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0101] In some embodiments, the conductive agent may be present in an amount of 1 to 10 wt %, for example, 2 to 5 wt %, based on the total weight (dry weight) of the negative electrode active material layer.

[0102] There is no particular requirement for the negative electrode binder. As an example, the binder is selected from one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl butyral (PVB), styrene-butadiene rubber (SBR), water-based acrylic resin and carboxymethyl cellulose (CMC).

[0103] In some embodiments, the binder may be present in an amount of 1 to 10 wt %, for example, 2 to 5 wt %, based on the total weight (dry weight) of the negative electrode active material layer.

[0104] The negative electrode can be prepared according to a method commonly used in the art.

[0105] For example, the negative electrode can be formed by uniformly dispersing the negative electrode active material and optional conductive agent, binder and thickener in a solvent (such as N-methylpyrrolidone (NMP) or deionized water) to form a negative electrode slurry; coating the negative electrode slurry on a negative electrode current collector, drying, and pressing.

[0106] Alternatively, the negative electrode can also be formed by uniformly dispersing the negative electrode active material and optional conductive agent, binder and thickener in a solvent (such as N-methylpyrrolidone (NMP) or deionized water) to form a negative electrode slurry; casting the negative electrode slurry on a separate support, drying, separating the obtained negative electrode film from the support and laminating it on a negative electrode current collector.

[0107] electrolytes

[0108] The electrolyte conducts ions between the positive and negative electrodes. The electrolyte is not particularly limited and can be selected based on needs. For example, the electrolyte can be selected from at least one of a solid electrolyte, a gel electrolyte, and a liquid electrolyte (i.e., an electrolyte solution).

[0109] In some embodiments, the electrolyte is an electrolyte solution comprising an organic aprotic solvent and an electrolyte sodium salt.

[0110] In some embodiments, the solvent can be selected from one or more of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS) and diethyl sulfone (ESE).

[0111] In some embodiments, the electrolyte sodium salt can be selected from one or more of sodium hexafluorophosphate (NaPF6), sodium tetrafluoroborate (NaBF4), sodium perchlorate (NaClO4), sodium hexafluoroborate (NaBF6), sodium bis(trifluoromethylsulfonyl)imide (NaFSI), sodium bis(trifluoromethylsulfonyl)imide (NaTFSI), sodium trifluoromethylsulfonate (NaTFS), sodium difluorooxalatoborate (NaDFOB), sodium dioxalatoborate (NaBOB), sodium difluorophosphate (NaPO2F2), sodium difluorobis(oxalatophosphate) (NaDFOP) and sodium tetrafluorooxalatophosphate (NaTFOP).

[0112] In some embodiments, the concentration of sodium ions in the electrolyte is 0.2 to 2 mol / L, for example, 0.5-1.0 mol / L.

[0113] In some embodiments, the electrolyte may optionally include additives. For example, the additives may include additives that facilitate negative electrode film formation or positive electrode film formation, or additives that improve battery performance, such as additives that improve high or low temperature performance of the battery.

[0114] diaphragm

[0115] The separator is not particularly limited, and a commonly used porous structure separator with electrochemical stability and chemical stability can be used. For example, it can be a single layer or multilayer film of one or more of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. When a solid electrolyte is used, the separator can also be omitted.

[0116] use

[0117] The fifth aspect of the present invention provides the use of the sodium ion secondary battery according to the fourth aspect of the present invention in an energy storage device for solar power generation, wind power generation, smart grid peak regulation, distributed power station, backup power supply or communication base station.

[0118] Those skilled in the art will appreciate that the sodium ion secondary battery of the fourth aspect of the present invention may also be used for other purposes. For example, the sodium ion secondary battery may be used as a power source or energy storage unit in mobile devices (e.g., mobile phones), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, electric bicycles, electric scooters, etc.), electric trains, etc.

[0119] Example

[0120] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0121] 1. Preparation Example

[0122] Comparative Example 1

[0123] Preparation of O3 type Na 1.02 Cu 0.05 Fe 0.34 Ni 0.28 Mn 0.33 O2: Na2CO3, CuO, Fe2O3, Ni(OH)2, and MnO2 were weighed in stoichiometric proportions, mixed thoroughly, and dried to obtain a precursor mixture. This mixture was sintered at 1050°C in an oxygen atmosphere (oxygen volume fraction > 98.5%) for 20 hours at a heating rate of 2°C / min. The mixture was cooled to room temperature, crushed, and sieved to obtain a product with a particle size D50 = 9.892 μm, designated C1.

[0124] The particle size D50 in each comparative example and embodiment was tested as follows: using a Malvern particle size analyzer (MASTERSIZER-3000), taking 1 g of the material to be tested, using pure water as the dispersion liquid, and performing a particle size volume distribution test under ultrasonic conditions. The test was repeated three times in parallel and the average value was taken.

[0125] Comparative Example 2

[0126] Preparation of O3 type Na 1.02 Cu 0.20 Fe 0.34 Ni 0.13 Mn 0.33 O2: Na2CO3, CuO, Fe2O3, Ni(OH)2, and MnO2 were weighed in stoichiometric proportions, mixed thoroughly, and dried to obtain a precursor mixture. This mixture was sintered at 950°C in a compressed air atmosphere (absolute pressure 0.8 MPa, the same below) for 15 hours at a heating rate of 3°C / min. After cooling to room temperature, the mixture was crushed and sieved to obtain a product with a particle size D50 = 10.013 μm, designated C2.

[0127] Comparative Example 3

[0128] Preparation of O3 type Na 0.95 Li 0.04 Cu 0.06 Fe 0.37 Ni 0.18 Mn 0.37 Al 0.02 Ti 0.02 Ca 0.02 O2: Na2CO3, Li2CO3, CuO, Fe2O3, Ni(OH)2, MnO2, Al2O3, TiO2, and CaO were weighed according to the stoichiometric ratios, mixed, and dried to obtain a precursor mixture. This mixture was sintered at 960°C in an oxygen atmosphere (oxygen volume fraction > 98.5%) for 24 hours at a heating rate of 3°C / min. The mixture was cooled to room temperature, crushed, and sieved to obtain a product with a particle size D50 = 10.124 μm, designated C3.

[0129] Comparative Example 4

[0130] Preparation of O3 type Na 1.10 Cu 0.30 Fe 0.33 Ni 0.03 Mn 0.30 Mg 0.01 Al 0.02 Ti 0.01 V 0.01O2: Na2CO3, CuO, Fe2O3, Ni(OH)2, MnO2, Mg(OH)2, Al2O3, TiO2, and V2O5 were weighed according to the stoichiometric ratios, mixed thoroughly, and dried to obtain a precursor mixture. This precursor mixture was sintered at 920°C in a compressed air atmosphere (absolute pressure 0.8 MPa) for 16 hours at a heating rate of 2°C / min. After cooling to room temperature, the mixture was crushed and sieved to obtain a product with a particle size D50 = 10.215 μm, designated C4.

[0131] Comparative Example 5

[0132] Preparation of O3 type Na 1.01 Cu 0.15 Fe 0.34 Ni 0.08 Mn 0.33 Al 0.01 Ti 0.02 O2: Na2CO3, CuO, Fe2O3, Ni(OH)2, MnO2, Al2O3, and TiO2 were weighed according to the stoichiometric ratios, mixed thoroughly, and dried to obtain a precursor mixture. This precursor mixture was sintered at 950°C in a compressed air atmosphere (absolute pressure 0.8 MPa) for 18 hours at a heating rate of 3°C / min. After cooling to room temperature, the mixture was crushed and sieved to obtain a product with a particle size D50 = 9.893 μm, designated C5.

[0133] Example 1

[0134] Preparation of O3 type Na 1.01 Cu 0.15 Fe 0.34 Ni 0.08 Mn 0.33 Mg 0.02 Al 0.01 Ti 0.02 O2: Na2CO3, CuO, Fe2O3, Ni(OH)2, MnO2, Mg(OH)2, Al2O3, and TiO2 were weighed according to the stoichiometric ratios, mixed thoroughly, and dried to obtain a precursor mixture. This precursor mixture was sintered at 970°C in a compressed air atmosphere (absolute pressure 0.8 MPa) for 14 hours at a heating rate of 3°C / min. After cooling to room temperature, the mixture was crushed and sieved to obtain a product with a particle size D50 = 9.976 μm, designated as E1.

[0135] Example 2

[0136] Preparation of O3 type Na 0.95 Li 0.04 Cu 0.2 Fe 0.37 Ni0.04 Mn 0.37 Mg 0.01 Al 0.01 Ti 0.01 O2: Na2CO3, Li2CO3, CuO, Fe2O3, Ni(OH)2, MnO2, Mg(OH)2, Al2O3, and TiO2 were weighed according to the stoichiometric ratios, mixed thoroughly, and dried to obtain a precursor mixture. This precursor mixture was sintered at 960°C in a compressed air atmosphere (absolute pressure 0.8 MPa) for 15 hours at a heating rate of 3°C / min. After cooling to room temperature, the mixture was crushed and sieved to obtain a product with a particle size D50 = 10.532 μm, designated as E2.

[0137] Example 3

[0138] Preparation of O3 type Na 1.10 Cu 0.30 Fe 0.34 Ni 0.03 Mn 0.33 Mg 0.01 Al 0.02 Ti 0.01 O2: Na2CO3, CuO, Fe2O3, Ni(OH)2, MnO2, Mg(OH)2, Al2O3, and TiO2 were weighed in stoichiometric proportions, mixed, and dried to obtain a precursor mixture. This mixture was sintered at 980°C in an oxygen atmosphere (oxygen volume fraction > 98.5%) for 18 hours at a heating rate of 3°C / min. The mixture was cooled to room temperature, crushed, and sieved to obtain a product with a particle size D50 = 10.723 μm, designated E3.

[0139] Example 4

[0140] Preparation of O3 type Na 0.70 Cu 0.07 Fe 0.18 Ni 0.15 Mn 0.40 Mg 0.03 Al 0.02 Ti 0.15 O2: Na2CO3, CuO, Fe2O3, Ni(OH)2, MnO2, Mg(OH)2, Al2O3, and TiO2 were weighed according to the stoichiometric ratios, mixed thoroughly, and dried to obtain a precursor mixture. This precursor mixture was sintered at 900°C in a compressed air atmosphere (absolute pressure 0.8 MPa) for 14 hours at a heating rate of 3°C / min. After cooling to room temperature, the mixture was crushed and sieved to obtain a product with a particle size D50 = 9.782 μm, designated E4.

[0141] Example 5

[0142] Preparation of O3 type Na 1.20 Cu 0.05 Fe 0.10 Ni 0.60 Mn 0.10 Mg 0.01 Al 0.01 Ti 0.18 O2: Na2CO3, CuO, Fe2O3, Ni(OH)2, MnO2, Mg(OH)2, Al2O3, and TiO2 were weighed in stoichiometric proportions, mixed, and dried to obtain a precursor mixture. This mixture was sintered at 1050°C in an oxygen atmosphere (oxygen volume fraction > 98.5%) for 20 h at a heating rate of 2°C / min. The mixture was cooled to room temperature, crushed, and sieved to obtain a product with a particle size D50 = 10.783 μm, designated E5.

[0143] Example 6

[0144] Preparation of O3 type Na 0.90 Cu 0.20 Fe 0.35 Ni 0.04 Mn 0.37 Mg 0.01 Al 0.01 Ti 0.01 Sn 0.01 O2: Na2CO3, CuO, Fe2O3, Ni(OH)2, MnO2, Mg(OH)2, Al2O3, TiO2, and SnO2 were weighed according to the stoichiometric ratios, mixed thoroughly, and dried to obtain a precursor mixture. This precursor mixture was sintered at 950°C in a compressed air atmosphere (absolute pressure 0.8 MPa) for 15 hours at a heating rate of 3°C / min. The mixture was cooled to room temperature, crushed, and sieved to obtain a product with a particle size D50 = 9.682 μm, designated E6.

[0145] Example 7

[0146] Preparation of O3 type Na 1.02 Cu 0.15 Fe 0.34 Ni 0.08 Mn 0.33 Mg 0.03 Al 0.01 Ti 0.01O2: Na2CO3, CuO, Fe2O3, Ni(OH)2, MnO2, Mg(OH)2, Al2O3, and TiO2 were weighed according to the stoichiometric ratios, mixed thoroughly, and dried to obtain a precursor mixture. This precursor mixture was sintered at 920°C in a compressed air atmosphere (absolute pressure 0.8 MPa) for 13 hours at a heating rate of 2°C / min. After cooling to room temperature, the mixture was crushed and sieved to obtain a product with a particle size D50 = 10.332 μm, designated E7.

[0147] Example 8

[0148] Preparation of O3 type Na 1.02 Cu 0.15 Fe 0.34 Ni 0.08 Mn 0.33 Mg 0.01 Al 0.01 Ti 0.03 O2: Na2CO3, CuO, Fe2O3, Ni(OH)2, MnO2, Mg(OH)2, Al2O3, and TiO2 were weighed according to the stoichiometric ratios, mixed thoroughly, and dried to obtain a precursor mixture. This precursor mixture was sintered at 930°C in a compressed air atmosphere (absolute pressure 0.8 MPa) for 14 hours at a heating rate of 3°C / min. After cooling to room temperature, the mixture was crushed and sieved to obtain a product with a particle size D50 = 9.972 μm, designated E8.

[0149] Example 9

[0150] Preparation of O3 type Na 1.10 Cu 0.30 Fe 0.34 Ni 0.03 Mn 0.33 Mg 0.03 Al 0.02 Ti 0.01 O2: Na2CO3, CuO, Fe2O3, Ni(OH)2, MnO2, Mg(OH)2, Al2O3, and TiO2 were weighed according to the stoichiometric ratios, mixed thoroughly, and dried to obtain a precursor mixture. This precursor mixture was sintered at 910°C in a compressed air atmosphere (absolute pressure 0.8 MPa) for 15 hours at a heating rate of 2°C / min. After cooling to room temperature, the mixture was crushed and sieved to obtain a product with a particle size D50 = 10.811 μm, designated E9.

[0151] Example 10

[0152] Preparation of O3 type Na 1.10 Cu 0.30 Fe 0.34Ni 0.03 Mn 0.33 Mg 0.05 Al 0.02 Ti 0.01 O2: Na2CO3, CuO, Fe2O3, Ni(OH)2, MnO2, Mg(OH)2, Al2O3, and TiO2 were weighed according to the stoichiometric ratios, mixed thoroughly, and dried to obtain a precursor mixture. This precursor mixture was sintered at 900°C in a compressed air atmosphere (absolute pressure 0.8 MPa) for 12 hours at a heating rate of 3°C / min. The mixture was cooled to room temperature, crushed, and sieved to obtain a product with a particle size D50 = 9.792 μm, designated E10.

[0153] 2. Manufacturing of button batteries

[0154] The products of Examples 1 to 10 and Comparative Examples 1 to 5 were each allowed to stand at a constant humidity of 50% for 30 minutes. They were then mixed as active materials in a mass ratio of 90:5:5 between active material SP (Swiss Special High Conductive Carbon Black SUPER P) and polyvinylidene fluoride (PVDF) (SOLVAY PVDF5130). N-methylpyrrolidone (NMP) was then added to form a viscous adhesive. The adhesive was applied to aluminum foil (16 μm thick) and then baked in a vacuum drying oven at 120°C for 12 hours to obtain a positive electrode sheet (active material layer thickness 34 ± 5 ​​μm). A sodium metal sheet (Aladdin) was used as the counter electrode (300 ± 50 μm thick). 2032 button cells were assembled in an Ar atmosphere protective glove box using glass fiber (Waterman) as the separator (thickness 675 μm) and NaPF6 solution with a sodium ion concentration of 1 mol / L (the solvent is a mixture of EC and DMC, with a volume ratio of EC / DMC = 1:1) (Alfa) as the electrolyte.

[0155] 3. Evaluation Example

[0156] Evaluation Example 1: X-ray diffraction analysis (XRD)

[0157] XRD analysis was performed on the materials prepared in Comparative Examples 1-5 and Examples 1-10 using an X-ray diffractometer (Bruker D8 ADVANCE) using a copper (Cu-Kα) target (accelerating voltage 40 kV, current 40 mA) (λ = 1.54056 nm), with a range of 10-80 degrees, a step size of 0.02 degrees, a time of 0.2, and a total duration of 712 seconds. The results are shown in Figure 1.

[0158] When calculating α and β, each sample is tested 5 times, and then the AI (003) %, HI (003)The average values ​​of the parameters such as % were calculated according to the formula described above. The calculation results are shown in Table 1.

[0159] Evaluation Example 2: pH test

[0160] The materials prepared in Comparative Examples 1-5 and Examples 1-10 were subjected to pH testing. An appropriate amount of layered oxide positive electrode material was added to a corresponding amount of distilled water at a mass ratio of 1:20. The mixture was then magnetically stirred at 600 ± 20 rpm for 10 minutes to ensure uniform mixing. The resulting mixture was then allowed to stand for 5 minutes. The pH of the mixture was then measured at 25°C using a pH meter (METTLER TOLEDO pH meter FE22-Standard). This represents the pH of the corresponding material. The test results are shown in Table 1.

[0161] Evaluation Example 3: Measurement of the First Effect of Power-On

[0162] After the 2032 button cell is assembled, the battery is tested at room temperature within the voltage range of 2.5-4.0V and cycled at 0.1C for 3 weeks. The first-week discharge capacity / first-week charge capacity × 100% is calculated as the first-week efficiency.

[0163] The experimental results of Comparative Examples C1-C5 and Examples E1-E10 are summarized in Table 1.

[0164] Table 1. Experimental results of Comparative Examples C1-C5 and Examples E1-E10

[0165] It can be seen from Table 1 and Figure 1 that, in the absence of doping, the product crystallinity of Comparative Examples C1 and C2 is low, and there are more CuO impurities. At the same time, it can be seen from C1 and C2 that, in the absence of Mg, Al and Ti, as the Cu content increases from 0.05 to 0.20, the CuO impurities in the XRD spectrum increase significantly, and the corresponding α and β also increase significantly, which ultimately leads to a significant decrease in the first charge efficiency of the corresponding sodium ion secondary battery (from 88.11% to 72.01%). It can be seen that in the absence of Mg, Al and Ti, if the Cu content is increased, the CuO impurities in the product will increase, thereby deteriorating the battery performance.

[0166] As can be seen from Comparative Examples C3-C5 and Figure 1, doping with Al, Ti, and Ca (or V) can reduce the CuO impurity phase in the XRD spectrum, thereby improving the initial charge efficiency of the sodium-ion secondary battery. However, the resulting product still contains a large amount of CuO impurity phase, and the initial charge efficiency of the corresponding sodium-ion secondary battery is still low.

[0167] Referring to Examples E1-E10 and Figure 1, it can be seen that when Mg, Al, and Ti are doped at the same time, the CuO impurity phase in the product XRD spectrum is further reduced, and the first buckle efficiency of the corresponding sodium ion secondary battery is further improved. In addition, it can be seen from Examples E1-E10 that when the ratio of the elements in the layered oxide positive electrode material to each other, especially the molar ratio of Ti / Mg, Al / Mg and the ratio y / a of the content y of the doping element M to the content a of Cu, the CuO impurity phase can be further eliminated, and the first buckle efficiency of the corresponding sodium ion secondary battery is further improved. In particular, when the molar ratio of Ti / Mg is 1:0.06 to 1:3.00, and / or y / a is 1:0.25 to 1:3.00, the CuO impurity phase is less (even completely eliminated, see Examples E1 and E2), and the first buckle efficiency of the corresponding sodium ion secondary battery is also higher.

[0168] The above description is merely an exemplary embodiment of the present invention. It should be noted that, for those skilled in the art, improvements can be made to the present invention without departing from the inventive concept of the present invention, and these improvements all fall within the scope of protection of the present invention.

Claims

1. A layered oxide positive electrode material having the following general formula: Na x Cu a Ni b Fe c Mn d M y O 2+nδ , where 0.60≤x≤1.20, 0.05≤a≤0.40, 0.03≤b≤0.70, 0.10≤c≤0.45, 0.10≤d≤0.45, 0<y≤0.30, and x+2a+2b+3c+3d+2y<4<x+2a+3b+3c+4d+4y, 0.95≤a+b+c+d+y≤1.05, 0<n≤0.1, -1≤δ≤3; and M includes Mg+Al+Ti.

2. The layered oxide positive electrode material according to claim 1, wherein M further comprises one or more of Ca, B, Li, K, W, Mo, Sr, Y, Sn, Sb, and Ce. 3 . The layered oxide positive electrode material according to claim 1 , wherein 0.70≤x≤1.

20. The layered oxide positive electrode material according to claim 1 , wherein 0.05≤a≤0.

30. 5 . The layered oxide positive electrode material according to claim 1 , wherein 0.03≤b≤0.

60. 6 . The layered oxide positive electrode material according to claim 1 , wherein 0.04≤y≤0.

20. 7 . The layered oxide cathode material according to claim 1 , wherein the molar ratio of Al / Mg is 1:3.50 to 1:0.25, and the molar ratio of Ti / Mg is 1:6.00 to 1:0.

05.

8. The layered oxide positive electrode material according to claim 1 or 2, wherein the molar ratio of Al / Mg is 1:3.00 to 1:0.

25.

9. The layered oxide positive electrode material according to claim 1 or 2, wherein the molar ratio of Ti / Mg is 1:5.00 to 1:0.

05.

10. The layered oxide positive electrode material according to claim 1 or 2, wherein y / a is in the range of 1:9.00 to 1:0.

10. 11 . The layered oxide cathode material according to claim 10 , wherein y / a is in the range of 1:7.50 to 1:0.

25.

12. The layered oxide cathode material according to claim 1 or 2, wherein the molar ratio of Mg / Cu is 1:40 to 1:1.00; and / or The molar ratio of Al / Cu is 1:30 to 1:1.50; and / or The molar ratio of Ti / Cu is 1:40 to 1:0.

25. 13 . The layered oxide cathode material according to claim 12 , wherein the molar ratio of Mg / Cu is 1:30 to 1:2.

00.

14. The layered oxide cathode material according to claim 12, wherein the molar ratio of Al / Cu is 1:20 to 1:3.

50. 15 . The layered oxide cathode material according to claim 12 , wherein the molar ratio of Ti / Cu is 1:30 to 1:0.

25. 16 . The layered oxide positive electrode material according to claim 1 , wherein M is any one of Mg+Al+Ti, Mg+Al+Ti+Li, Mg+Al+Ti+K, or Mg+Al+Ti+Sn.

17. The layered oxide positive electrode material according to claim 1 or 2, wherein nδ = -0.02 to 0.

02. The layered oxide positive electrode material according to claim 17 , wherein nδ=0.

19. The layered oxide positive electrode material according to claim 1 or 2, wherein the layered oxide positive electrode material has an O3 type crystal structure.

20. A method for preparing a layered oxide positive electrode material according to any one of claims 1 to 19, comprising the following steps: Step a: uniformly mixing a Na source, a Cu source, a Ni source, a Fe source, a Mn source, and a M source in a stoichiometric ratio to obtain a mixture precursor; Step b: sintering the precursor obtained in step a; and Step c: Cooling the product obtained in step b.

21. The method according to claim 20, wherein step c further comprises crushing and screening after cooling.

22. The method according to claim 20 or 21, wherein The Na source is one or more selected from the following compounds: sodium carbonate, sodium bicarbonate, sodium nitrate, sodium acetate, sodium oxalate, sodium hydroxide and sodium oxide; The Cu source is one or more selected from the following compounds: copper carbonate, copper nitrate, copper acetate, copper oxalate, copper hydroxide and copper oxide; The Ni source is one or more selected from the following compounds: nickel carbonate, nickel nitrate, nickel acetate, nickel oxalate, nickel hydroxide and nickel oxide; The Fe source is one or more selected from the following compounds: iron carbonate, iron nitrate, iron acetate, iron oxalate, iron hydroxide, and iron oxide; The Mn source is one or more selected from the following compounds: manganese carbonate, manganese nitrate, manganese acetate, manganese oxalate, manganese hydroxide, manganese oxide; and The M source is one or more compounds selected from the following forms: carbonate, nitrate, acetyl Salts, oxalates, hydroxides, oxides.

23. The method according to claim 20 or 21, wherein the mixing in step a is performed by dry mixing or wet mixing.

24. The method according to claim 23, wherein the wet mixing is mixing by a sol-gel method or a coprecipitation method.

25. The method according to claim 20 or 21, wherein the sintering in step b is performed in an oxidizing atmosphere.

26. The method of claim 25, wherein the oxidizing atmosphere is compressed air or oxygen.

27. The method according to claim 20 or 21, wherein the sintering temperature in step b is 700 to 1200°C, and the sintering time is 8 to 36 hours.

28. The method according to claim 27, wherein the sintering temperature in step b is 800 to 1100°C.

29. The method according to claim 27, wherein the sintering time in step b is 12 h to 20 h. 30 . A positive electrode composition, which is a positive electrode composition for a sodium ion secondary battery, comprising the layered oxide positive electrode material according to claim 1 .

31. A sodium ion secondary battery comprising the positive electrode composition according to claim 30.

32. Use of the sodium ion secondary battery as claimed in claim 31 in energy storage equipment for solar power generation, wind power generation, smart grid peak regulation, distributed power stations, backup power supplies or communication base stations.

Citation Information

Patent Citations

  • Sodium ion secondary battery composite positive electrode material, preparation method thereof and battery

    CN111082017A

  • Positive electrode material and preparation method and application thereof

    CN115312735A

  • Positive electrode active material and preparation method thereof, sodium ion battery and electric equipment

    CN115881917A

  • Layered oxide positive electrode material, preparation method thereof, positive electrode composition, sodium ion secondary battery and application

    CN116207250A

  • Method for manufacturing sodium-containing transition metal oxide, and method for manufacturing positive electrode for sodium ion secondary batteries

    JP2015222628A

Cited By

  • Positive electrode material for sodium ion battery, preparation method of positive electrode material, positive electrode composition, sodium ion secondary battery and application

    CN119581530A

  • Sodium-ion battery O3 type positive electrode material, preparation method thereof and sodium-ion battery

    CN120581588A