Microlens coating and method of its production
A cost-effective two-step UV-curable resin process for producing microlenses on photovoltaic cells addresses the economic challenges of existing methods, achieving improved efficiency and resistance to external conditions, with the coated cells showing an 8% power increase over uncoated counterparts.
Patent Information
- Application Number
- PCT/IB2023/000290
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-06
- Publication Date
- 2024-11-14
AI Technical Summary
Current methods for producing microlenses for photovoltaic cells are labor-intensive and expensive, making them economically unprofitable, despite advancements in efficiency, as they require specialized preparation and equipment like inkjet printing, laser light, or precise molding, which increase production costs.
A two-step process involving a UV-curable resin base layer applied and cured on a substrate, followed by spraying and curing of resin droplets to form microlenses, allowing for adjustable size and distribution to optimize light concentration while maintaining cost-effectiveness.
The method produces microlenses with good functional properties, including high temperature resistance and efficient light concentration, while being economically viable for mass production, enhancing photovoltaic cell efficiency by up to 8% compared to uncoated cells.
Smart Images

Figure IB2023000290_14112024_PF_FP_ABST
Abstract
Description
[0001] Microlens coating and method of its production.
[0002] The subject of the invention is a microlens coating, especially for photovoltaic cells, and a method for its production.
[0003] For electricity supply, solar as a renewable (PV) energy source is being deployed at an accelerated pace due to its low generation costs, proven reliability and reduced associated carbon emissions. However, the performance of this technology has known limitations. The conversion efficiency of solar energy into electricity is about 18-22%. Research and development efforts are aimed at reducing the pnce of solar energy by reducing the cost of a photovoltaic module or increasing its efficiency.
[0004] A significant improvement in the efficiency of photovoltaic cells is achieved with concentrated photovoltaics (CPV) technology. CPV systems use optical equipment to concentrate solar radiation reaching the photovoltaic cells. The common goal of these systems is to channel more electromagnetic energy onto the PV surface and thus achieve more efficiency (electrical power) for the same size of PV panel. The highest efficiency of CPV cells known so far ranges from 38.9% to 46%. The disadvantage of the CPV system, however, is the high price and the need to use cooling systems to reducing the cell temperature.
[0005] To reduce the cost of CPV, photovoltaic panels with a micro-scale light concentrator (micro CPV - MCPV) where the diameter of the microlens is measured in micrometers have been proposed. The best produced solar cells in MCPV systems achieved an efficiency of about 44%, however, these systems are expensive and do not withstand competition with other rapidly developing photovoltaic systems, although they exceed them in efficiency.
[0006] The biggest problem of the MCPV technology, generating at the same time the highest production costs, is the method of producing microlenses. There are many methods for producing individual microlenses and arrays of microlenses, for example shown schematically in Figures 1 and 2, which can be directly applied to photovoltaic panels, but none of these methods guarantees the costeffectiveness of the production of photovoltaic panels.
[0007] Patent US 10121925B2 discloses amethod of forming microlenses by depositing microdroplets of photopolymerizable materials on a substrate in an inkjet printing process, and then photopolymerizing the material on the microlenses. This method is designed to place microlenses on LEDs or OLEDs. On-demand inkjet printing systems produce droplets that are approximately equal to the hole diameter of the drop generator. In this method, the surface on which the microlenses are to be formed is coated with a coating material that comprises at least one component for inducing a high contact angle with the resin and at least another component for copolymerization with the resin. The resin is deposited on the coating in the form of one or more microdroplets that are cured to form microlenses that are covalently bonded to the coating material by copolymerization between functional groups in the resin and copolymerizable components in the coating. The surface can be the substrate of an LED or an OLED. By repeating printing and curing cycles, microlens arrays can be created that can touch each other. Microlens arrays can have any but regular pattern, e.g. rows and columns, hexagonal, closely packed structures. Microlenses of various sizes can be printed using appropriate printers. This method, due to the need for special preparation of the substrate and the use of inkjet printers, is labour-intensive and expensive, and therefore unprofitable, e.g. for photovoltaic cells.
[0008] US10121925B2 also discloses a method for producing microlenses by depositing a layer of transparent resin on a surface and contacting the layer of resin with a mold that acts as a template for the microlenses. The mold may be a flat stamp or roll-to-roll printing mold where irradiation may occur before or after the mold is removed from the lenses. This method is laborious and requires the use of many molds to change the size of the created microlenses and is therefore unprofitable, e.g. for photovoltaic cells.
[0009] The patent US6970288 (B2) discloses a microlens system in which the unit lenses are arranged with a very fine division, so as to control the light diffusion characteristics in the direction of light emission not only in the horizontal direction, but also in the 360 degree range, using the lens function of one piece of lens sheet , the microlens sheet has a micro lens array section, wherein the unit lenses are arranged in an approximate array in a two-dimensional manner on at least one face of the base plate, and the microlens array section is formed on only one surface of the base plate, the microlens array section includes a unit lens having an aspherical shape , and the spacing of adjacent unit lenses is 200 pm or less. The microlenses are mechanically molded from a light-curing resin. This method is very complicated and requires high precision, and therefore it is unprofitable, e.g. for photovoltaic cells.
[0010] Patent US7706073 (B2) discloses a method of producing a microlens array on a suitable substrate using laser light. This is a method of producing microlenses, but economically unprofitable, e.g. for photovoltaic cells.
[0011] Patent US10505059 discloses a microlens array system that is made of silicone. This is a method of producing microlenses, but economically unprofitable, e.g. for photovoltaic cells. The patent KR20110023582A discloses a method of producing a photovoltaic cell together with an array of microlenses. The microlenses are molded by extrusion. Arrays of microlenses on a solar cell are being created - economically unprofitable
[0012] Patent CN 111863975A discloses a solar panel with micro lenses. Micro lenses are arranged on the solar panel in array mode. The width of each microlens ranges from 100 nanometres to 20 micrometers and the height of each microlens ranges from 10 micrometers to 50 micrometers. Microlens arrays are created where all microlenses produced have the same diameter. The surface of the solar panel is covered with a nanometer layer of silica gel, in which a model of the structure of the microlens matrix is imprinted. The whole thing is hardened with ultraviolet light. An economically unprofitable solution, e.g. for photovoltaic cells.
[0013] Patent JP2012181515 A discloses a method in which a matrix with microlenses is formed by fusing a resin pellet with a resin sheet. An economically unprofitable solution, e.g. for photovoltaic cells.
[0014] Patent application US20040263967A1 discloses a projection screen microlens array sheet having a predetermined area, the microlenses are arranged on one surface of the lens sheet in a horizontal and vertical direction (two dimensional array). The microlens matrix sheet of the projection screen is manufactured using the semiconductor device manufacturing process, reflow process and mold coating process, thereby improving the luminance. This solution is economically unprofitable for photovoltaic cells.
[0015] Patent application US2015020883A1 discloses a solar cell with a condensing microlens system, where the microlens system is placed in such away that there is a gap between the microlenses from the top of the photoactive layer and refracts the incident sunlight towards the photoactive layer.
[0016] However, this solution is economically unprofitable. Patent application CN101740653A discloses a method of forming an uneven layer of microlenses by pressing onto a resin -coated substrate using a mould. While the mold imprints the resin, ultraviolet (UV) light can be applied to the coated resin to cure the micro lenses. Then, after the mold is removed, the cured resin can be heated to further cure the microlenses. This solution is economically unprofitable for photovoltaic cells.
[0017] Patent application CN101510565 A discloses a synergistic solar cell film, which is a solar cell film having a microlens array structure, however, the patent application does not disclose a method of producing the film. This solution is economically unprofitable for photovoltaic cells.
[0018] Patent application CN 103885102 A discloses a microlens array device, a method for its manufacture and a solar cell module provided therewith which is manufactured in the shape of a microsphere, and thus the shape of the lens is limited by the shape of the microsphere. This solution is economically unprofitable for photovoltaic cells.
[0019] In presently known solutions, microlenses are fabricated in a plane as microlens arrays comprising a plurality of microlenses formed into a one -dimensional (Fig. la) or two-dimensional (Fig. lb and 1c) array on a support substrate. If the individual microlenses are circular and cannot overlap, they can be placed in a hexagonal pattern to maximize ground coverage. However, there will still be gaps between the lenses, which can only be reduced by making the non -circular microlenses.
[0020] The microlenses can be of the same or different diameter. The distances between the lenses result from the way the lenses are arranged.
[0021] The purpose of the invention was to develop a microlens coating with good functional properties and low cost of production and a method of its production. The present invention relates to a microlens coating comprising a base layer and microlenses characterized in that it comprises two layers of UV -curable resin, the first layer being a base layer having a thickness corresponding to: from minus 80% to plus 90% of the mean focal length of the microlenses and a second layer consisting of microlenses. The base layer and the microlenses are made of the same UV -curing resin, but in another embodiment of the invention they can be made of different UV-curing resins.
[0022] The schematic layout of the layers is shown in figure 3, where a microlens (2) is placed on the base layer (1).
[0023] The base layer preferably has a thickness ranging from minus 10% to plus 10% of the average focal length of the microlenses to be placed on the base layer, most preferably it has a constant thickness equal to the focal length of the microlenses that are planned for the layer microlens.
[0024] The base layer can have both flat and irregular surface, it is important that the average thickness corresponds to the assumed parameters.
[0025] The thickness of the base layer is determined as the average value of the focal lengths of the microlenses that are planned to be placed in the microlens layer.
[0026] The size of the focal length is determined based on the relation where:
[0027] F - means the focal length of the microlens
[0028] R - means the assumed radius of the produced microlenses. n - is the refractive index of the microlens material nail- indicates the refractive index of the air (or the material surrounding the microlens). The size and focal length of the microlenses can be adjusted to the purpose for which they are finally to be used.
[0029] Microlenses, shown schematically in the figure 4, present in a given coating, may have the same or different diameter D. Also, the height H of the microlenses may be equal or different. The size and shape, including height and diameter, of the microlenses is adapted to the purpose for which the microlens coating is to be used. If the microlenses have different diameters, it is preferable that these differences will not be greater than -99% to +400% of the assumed microlens diameter for a given coating.
[0030] In a variation of the invention, the microlenses have equal cross-sectional areas.
[0031] In a further variant of the invention, the microlenses have different cross-sectional areas.
[0032] The microlens layer should have micro lenses in such an amount that they occupy at least 30% of the surface of the base layer, and it is preferable that the entire surface is covered evenly.
[0033] The microlenses of the coating according to the invention are distributed over any surface and are formed into an irregular array, as shown for example in figure 5, the distribution of the microlenses (3) is irregular.
[0034] The microlenses can be adjacent to each other, but at the same time they can also be spaced apart. The microlens distribution is heterogeneous and irregular.
[0035] The microlens coating according to the invention can occur as an independent object applied, for example, to photovoltaic cells or be permanently formed directly on any substrate, in particular on glass, organic glass, e.g. plexiglass, photovoltaic cell, perovskite cell, optical systems, chemical reactors intended for photochemical reactions .
[0036] In a second aspect, the invention relates to a method for producing a microlens coating. The method of producing the microlens coating according to the invention is basically a two- step process, where in the first step, a base layer of UV light curable resin is applied to the substrate, and then, after curing the base layer, drops of liquid UV light curable resin are sprayed, which are then cured by UV light.
[0037] During the first step, an appropriate amount of UV light curable liquid resin is sprayed onto the substrate in the first step. By "adequate amount" of resin is meant the amount needed to obtain the desired thickness of the base layer, which thickness corresponds to the average focal length of the microlenses to be formed on this layer in the second step.
[0038] Depending on the planned shape of the microlenses and the average focal length of these microlenses, the thickness of the base layer (1) is adjusted.
[0039] The resin used to form the base layer should preferably belong to the group of acrylates and should contain the same basic component as the resin intended for making the microlenses.
[0040] The base layer is applied by spraying the resin onto the substrate. It is advantageous to use several movements of the head with the spray nozzle in different directions. An exemplary scheme of resin spraying onto the substrate is shown in figure 6, where a stream (6) of resin drops is sprayed onto the substrate (4) from the head (5), preferably the spray is carried out in different directions (7, 7') as shown, for example, in figure 7. It is preferable to spray the base layer at a pressure in the range of 0.3 - 2.0 [bar].
[0041] The material flowing out of the nozzle (5) under pressure is broken into drops (6), which, falling onto the substrate (4), form the base layer for the microlenses.
[0042] When applying the base layer to the substrate, it is preferable to maintain the following conditions:
[0043] • Ambient temperature 18-30°C
[0044] • Air humidity 25-65%
[0045] • Resin viscosity measured in Ford cup 4mm 12-25s
[0046] Resin flow at 0.3-2.0 bar pressure In the second step, the base layer is cured with UV light. The degree of curing of the base layer may be complete or partial. The curing time of the resin depends on the thickness of the base layer, the irradiance used and the individual properties of the resin used. It is advisable to determine the curves of curing rate versus time and irradiation intensity for each resin used, as well as the dependence of changes in surface tension on the degree of curing. The dependence curves obtained in this way will enable quick and effective determination of the curing parameters for a given specific case. As a result of curing the resin, the surface tension of the base layer changes.
[0047] It is advantageous to control the surface tension of the base layer during its curing in order to obtain the desired value of this tension, which is beneficial for the correct adjustment of the surface tension of the resin used in the second stage.
[0048] When curing the base layer, it is preferable to keep the following conditions:
[0049] • UV lamp travel speed Od O.lm / min to 8m / min
[0050] • UV exposure time from Is to 45s
[0051] In the second step, droplets of UV curable resin are sprayed onto the cured base layer in the first step, and after spraying resin microdroplets onto the base layer, the process of curing the microlenses with UV light is carried out in the second step. To spray the drops, a resin with a viscosity measured with a 4mm Ford cup in the range of 12 to 25s is used. The viscosity of the resin used for the microlenses should be similar to the viscosity of the resin used for the base layer, preferably within the range of plus / minus 25%.
[0052] When applying to the base layer of microlenses, it is preferable to maintain the following conditions:
[0053] • Resin drops may have different diameters, but the differences should not be greater than - 99% to +400% of the assumed microlens diameter for a given coating.
[0054] • Ambient temperature 18-30°C
[0055] • Air humidity 25-65%
[0056] • Resin viscosity measured in Ford cup 4mm 12-25s
[0057] Resin flow at 0.3-2.0 bar pressure When curing microlenses, it is beneficial to maintain the following conditions:
[0058] • The distance between the UV lamp and the irradiated surface is 1 cm to 30 cm, depending on the power of the used lamp.
[0059] • UV lamp travel speed from O.lm / min to 8m / min
[0060] • UV exposure time from Is to 45s.
[0061] Microlenses are formed as a result of the deformation of resin drops on the base layer, because due to the difference in surface tension between the base layer and the sprayed drop of resin, the resin drop takes the shape of a lens, which is fixed during the curing of the resin.
[0062] Resin droplets are formed in the atomization process at the outlet of the spray nozzle and have different diameters. The smaller the diameter of the drop, the smaller the diameter of the microlenses.
[0063] Drops of resin, after contact with the surface of the base layer, are deformed due to the difference in the density of the base layer and the density of the drops, as well as the difference in the surface tension of the resin drop and the base layer, and as a result, the falling drops merge with the base layer, but the falling drops do not completely dissolve on the base layer. Finally, the drops do not spread on the base layer, but form convex microlenses. This mechanism is shown schematically in figure 8 where the drop (8) falling on the base layer (1) has a spherical shape and gradually changes its shape over time, which is illustrated by the subsequent phases (8', 8"), finally taking the shape of a lens (8”’).
[0064] Reducing the pressure of the resin will reduce the size of the microlenses (and vice versa). This method, however, gives a large scatter in the cross-sectional areas of the microlenses, which is schematically shown in Figures 9 and 10 where the individual microlenses (9, 9', 9", 9"', ...) have different sizes.
[0065] The size of the resin droplets is regulated by:
[0066] • pressure change or,
[0067] • changing of the height of the injection nozzle relative to the substrate or base layer. The greater the distance from the base, the smaller the drops and the smaller the microlenses - this is due to the atomization process - the farther from the nozzle, the smaller the diameter of the drop.
[0068] • changing of the size of the nozzle opening,
[0069] • combinations of the above changes. This method produces microlenses of various sizes.
[0070] In a variant of the invention, in order to obtain micro lenses of similar size, additional devices are used to obtain drops of almost identical size, as schematically shown in Figures 11 and 12 where the individual microlenses (10, 10', 10", 10"',...) are of the same size. Such a device is, for example, an ultrasonic nozzle from Sonotek.
[0071] In a further variant of the invention, the spraying of drops on the microlenses is used several times, and the same or different spraying parameters can be used. As a result of such a procedure, a greater filling of the surface with micro lenses is obtained.
[0072] Figures 13-16 show pictures of exemplary coatings obtained by the method according to the invention.
[0073] The coating according to the invention is characterized by good performance properties, in particular:
[0074] • contains microlenses of different or similar diameter on the base layer
[0075] • thanks to a simple and cheap method of production, it has many applications (energy, chemical, space industry)
[0076] • is resistant to high temperature (250 Celsius degrees)
[0077] • can be directly produced on the target substrate or transferred from another substrate to the target substrate.
[0078] • mechanically strengthens the substrate on which it is applied
[0079] • can protect the substrate against the influence of external conditions (high temperature, humidity, etc.)
[0080] • its production method, by controlling the thickness of the base layer and controlling the size of the microlenses produced, allows you to control the place of maximum light concentration
[0081] • its method of manufacturing the base coat and microlenses allows it to be used in mass production
[0082] The subject of the invention has been presented in the embodiment examples.
[0083] Example 1
[0084] PEHALUX-H 1 C-UV PLASTIC PAINT resin, curable with UV light, was sprayed on the surface of the organic glass plate in an amount corresponding to the volume of the 1 mm thick base layer, which corresponded to the average focal length of the microlenses that would be applied in the next stage.
[0085] The following parameters were used when spraying the base layer:
[0086] Resin Viscosity (Ford Cup 4mm) 20s
[0087] Diluted PEHALUX-H 1C-UV PLASTIC PAINT resin was used (diluted in proportion to 1000 ml of resin, 300 ml of 1,6-Hexandioldiacrylate was added as a diluent)
[0088] Base spray pressure 1.3 bar
[0089] Base layer spray nozzle diameter 0.8 mm
[0090] Continuous spraying by moving the head in different directions.
[0091] Base layer spraying time 15 s
[0092] Then the base layer was cured with UV light for 30 s.
[0093] After the resin of the base layer was cured, resin drops were sprayed to form the microlenses. The same PEHALUX-H 1C-UV PLASTIC PAINT resin was sprayed on.
[0094] The following parameters were used during micro lens spraying:
[0095] Resin Viscosity (Ford Cup 4mm) 20s
[0096] Diluted PEHALUX-H 1C-UV PLASTIC PAINT resin was used (diluted in proportion to 1000 ml of resin, 300 ml of 1,6-Hexandioldiacrylate was added as a diluent)
[0097] Microlens spray pressure 1.3 bar
[0098] Microlens spray nozzle diameter 0.8 mm
[0099] Micro lens spray time 10s After the microlenses were sprayed, they were irradiated with UV light through 30s.
[0100] During the preparation of this exemplary microlens coating, the surface tension of both the cured base layer and the surface of the uncured resin was measured, respectively:
[0101] Surface tension of the hardened base layer 30 [mN / m]
[0102] Resin surface tension for microlenses 51 [mN / m]
[0103] The microlens coating shown in Figure 17 was obtained. The scale on the side of Figure 17 makes it possible to estimate differences in the size of the microlenses.
[0104] Example 2
[0105] Proceeding in the same way as in example 1, a microlens coating was made on the photovoltaic cell
[0106] In order to estimate the effect of the coating according to the invention on the efficiency of the photovoltaic cell, comparative measurements of the cell without the coating with the cell with the coating were carried out.
[0107] A standard measurement of the voltage and current (voltmeter and ammeter) of the current generated by the photovoltaic cell at various loads was performed. The measurements made it possible to build a graph of the dependence of the photovoltaic cell power on the voltage.
[0108] The results of the measurements are shown in figure 18 where the continuous graph shows the power dependence of the cell with microlenses on the voltage, and the dashed graph shows the dependence of the power of the cell without microlenses on the voltage.
[0109] The measured power of the photovoltaic cell with microlenses is 8% higher than the power of the cell without microlenses.
Claims
Claims1. A microlens coating characterized in that it comprises two layers of UV-curable resin where the first layer is a base layer (1) with a thickness corresponding to: from minus 80% to plus 90% of the mean focal length of the microlenses (2, 3, 8, 9,10), which are the second layer of the coating.
2. A coating according to claim 1, characterized in that the thickness of the base layer (1) is no more than 10% less than the mean focal length of the microlenses, which are the second layer of the coating.
3. A coating according to claim 1, characterized in that the thickness of the base layer (1) is no more than 10% greater than the mean focal length of the microlenses, which are the second layer of the coating.
4. A coating according to claim 1 or 2 or 3, characterized in that the base layer (1) has the same thickness at each point.
5. A coating according to claim 1 or 2 or 3 or 4 characterized in that the surface of the base layer (1) is flat.
6. A coating according to claim 1 or 2 or 3 or 4 or 5 characterized in that the microlenses (3, 8, 9, 10) cover at least 30% of the surface of the base layer (1).
7. A coating according to claim 1 or 2 or 3 or 4 or 5 or 6 characterized in that the microlenses (10, 10'...) have equal cross-sectional areas.
8. A coating according to claim 1 or 2 or 3 or 4 or 5 or 6 characterized in that the microlenses (9, 9') have different cross-sectional areas.
9. A coating according to claim 1 or 2 or 3 or 4 or 5 or 6 or 7 or 8 characterized in that the base layer (1) is of the same material as the microlenses (3, 8, 9, 10).
10. A coating according to claim 1 or 2 or 3 or 4 or 5 or 6 or 7 or 8 or 9 characterized in that the microlenses (9, 9', 9" . ) are arranged in a non-uniform manner.
11. A coating according to claim 1 or 2 or 3 or 4 or 5 or 6 or 7 or 8 or 9 or 10 characterized in that the microlenses (10, 10'...) have the same diameters.
12. A coating according to claim 1 or 2 or 3 or 4 or 5 or 6 or 7 or 8 or 9 or 10, characterized in that the microlenses have different diameters, the differences should not be greater than -99% to +400% of the assumed microlens diameter for a given coating.
13. A coating according to claim 1 or 2 or 3 or 4 or 5 or 6 or 7 or 8 or 9 or 10 or 11 or 12, characterized in that it is placed on a photovoltaic cell.
14. A coating according to claim 1 or 2 or 3 or 4 or 5 or 6 or 7 or 8 or 9 or 10 or 11 or 12, characterized in that it is placed on a plate of organic glass of any thickness.
15. A coating according to claim 1 or 2 or 3 or 4 or 5 or 6 or 7 or 8 or 9 or 10 or 11 or 12 characterized in that it is placed on a glass plate.
16. A coating according to claim 1 or 2 or 3 or 4 or 5 or 6 or 7 or 8 or 9 or 10 or 11 or 12 characterized in that it is placed on an organic photovoltaic cell.
17. A coating according to claim 1 or 2 or 3 or 4 or 5 or 6 or 7 or 8 or 9 or 10 or 11 or 12, characterized in that it is disposed on a perovskite material.
18. A method for producing a microlens coating comprising a base layer (1) and a microlens layer (3) characterized in that in the first step a UV light curable resin base layer is applied to the substrate, which is then cured by UV light, then onto the base layer using a spray nozzle, droplets of UV light curable resin are sprayed, which are then cured by UV light.
19. The method of claim 18, characterized in that the base layer is sprayed.
20. The method of claim A method according to claim 18 or 19, characterized in that the resin droplets fall onto the base layer by gravity.
21. The method of claim 18 or 19 or 20, characterized in that the sprayed resin drops have different diameters, the differences should not be greater than -99% to +400% of the assumed microlens diameter for a given coating.
22. The method of claim 18 or 19 or 20, characterized in that the sprayed resin droplets have the same diameter.
Citation Information
Patent Citations
Photosensitive composition, pattern film, low refractive index film, optical device, and solid state image sensor
JP2013152479A
Nanostructured moulded bodies and layers and method for producing same
WO1998051747A1
Cited By
Photovoltaic panel with microlens layer and method for its production
WO2026215179A1