Flexible intelligent wood having response function, actuator, and manufacturing method
By combining the negative pressure method of impregnating azobenzene compounds with responsive function, flexible intelligent wood with responsive function is prepared, and the problem of insufficient flexibility of existing intelligent wood materials is solved, and the problem of inadequate flexibility of existing intelligent wood materials is achieved. The shape change response under light stimulation is suitable for a variety of flexible applications.
Patent Information
- Application Number
- PCT/CN2023/095221
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-15
- Filing Date
- 2023-05-19
- Publication Date
- 2024-11-21
AI Technical Summary
The limited range of changes in existing smart wood materials in terms of flexibility limits their applications in soft and flexible applications, such as electronic skin, flexible brakes and human tissue dressings.
Flexible smart wood with responsive function was prepared by dissolving sodium chlorite in acetic acid-sodium acetate buffer solution, removing hemicellulose, and impregnating azobenzene compounds in the negative pressure method.
The prepared flexible intelligent wood can respond through shape changes under light stimulation. It is suitable for intelligent flexible components and wireless drive robot fields such as batteries, cables, electronic components, etc., meeting the lightweight, miniaturization and controllability needs of micro robots. .
Smart Images

Figure CN2023095221_21112024_PF_FP_ABST
Abstract
Description
Flexible intelligent wood with responsive function, actuator and preparation method Technical Field
[0001] The present invention relates to the technical field of novel wood technology development, and in particular to a flexible intelligent wood with responsiveness, a brake and a preparation method thereof. Background Art
[0002] As a natural, renewable material, wood offers advantages over traditional metals, such as a naturally porous structure, a high strength-to-weight ratio, and environmental friendliness. The efficient and high-value utilization of wood has long been a hot topic in materials science research. In recent years, innovative research in wood has shifted from traditional basic research to advanced, multifunctional applied research. The development and utilization of its advanced functionalities has been a focus of international research, with projects such as transparent wood, super-strong wood, cooling wood, luminous wood, and self-healing wood attracting significant attention. The wood cell wall is primarily composed of cellulose, lignin, and hemicellulose. Cellulose, compared to lignin and hemicellulose, has a more regular shape and serves as a supporting skeleton within the wood. The natural honeycomb pores of wood not only facilitate the infiltration and reaction of chemicals with cell wall components, but also facilitate the filling of other modifiers. Based on these structural and compositional characteristics of wood, the natural porous structure of wood, along with the advantages of its multi-layered cell wall assembly and oriented fiber alignment, can be fully utilized. For example, transparent wood and super-strong wood can be constructed by filling wood with resin or densifying and compressing the porous structure. In addition, chemical modification can also be used to impart other functionalities to wood, such as magnetism, luminescence, radiative cooling, energy storage, and wave absorption. In summary, the research and application of wood are gradually developing towards high value-added and intelligent technologies, in order to meet people's diverse needs for functional wood materials.
[0003] To further enhance the added value of wood and expand its applications, research on wood is increasingly moving towards intelligent technologies. Natural wood possesses inherent environmental regulation capabilities. For example, houses decorated with solid wood retain their warmth in winter and coolness in summer. In environments that are too dry or too humid, wood can leverage the advantages of its composition to regulate humidity. Furthermore, after impact, wood can return to its original shape within its elastic deformation recovery range. Inspired by the adaptive regulatory properties of natural wood, chemical modifications can be used to impart intelligent behaviors such as environmental sensing and stimulus response. Intelligent functional wood materials developed from wood, such as self-healing wood, wood sponges, photochromic wood, and wood nanogenerators, are examples. However, currently developed intelligent wood materials primarily focus on the material's inherent electronic, photonic, or cellulose hydrogen bonding intelligent responses. These wood-based smart materials exhibit very limited flexibility, limiting their application in soft and flexible applications such as electronic skin, flexible actuators, and human tissue dressings. Therefore, there is an urgent need to develop intelligent flexible materials with advanced intelligent responsiveness and environmental friendliness.
[0004] Summary of the Invention
[0005] In view of this, the purpose of the present invention is to provide a flexible smart wood with responsive functions, a brake and a preparation method. The flexible smart wood provided by the present invention can respond to external stimuli by changing its shape when stimulated by light, and can be applied to the field of smart flexible components.
[0006] In order to achieve the above object, the present invention provides the following technical solution: a method for preparing flexible smart wood with responsive function, comprising the following steps:
[0007] (1) preparing an acetic acid-sodium acetate buffer solution, and dissolving sodium chlorite in the buffer solution to obtain solution A;
[0008] (2) Cutting the wood into wood chips and soaking them in solution A for delignification treatment;
[0009] (3) treating the wood chips obtained in step (2) with alkali to remove hemicellulose from the wood chips;
[0010] (4) impregnating the azobenzene compound into the alkali-treated wood chips by a negative pressure method;
[0011] (5) The wood chips obtained in step (4) are densified into a wood film to obtain a flexible smart wood with responsive functions.
[0012] Preferably, the pH of the buffer solution in step (1) is 4.6, and the content of sodium chlorite in the solution A is 1 to 1.5 wt%.
[0013] Preferably, the wood in step (2) includes balsa, poplar, pine, birch, beech, oak, basswood, elm, ironwood, ash, paulownia, camphor wood, rubber wood, oak, cypress and fir.
[0014] Preferably, the delignification treatment in step (2) is as follows: the cut wood chips are immersed in solution A, stirred at 500 r / min, and heated to 80° C. and steamed for 6 h.
[0015] Preferably, the alkali treatment in step (3) is to place the delignified wood chips in a 4% concentration NaOH solution and soak them for 3-6 hours.
[0016] Preferably, the azobenzene compound in step (4) includes azobenzene, azobenzene oxide, p-aminoazobenzene, 4-methoxyazobenzene, 3,3-dicarboxylic acid azobenzene, 4,4-dicarboxylic acid azobenzene, 4-aminoazobenzene-4-sodium sulfonate, 3,3-dimethylazobenzene, 4-sulfonyl chloride azobenzene, 4-(dimethylamino)-2-methylazobenzene, 4-nitrobenzene, 4-phenylazobenzoyl chloride, p-diaminoazobenzene, 4-chloro-4-dimethylaminoazobenzene, 4-carboxy-2-aminoazobenzene, 4'4 dimethyl dicarboxylate-azobenzene, 2,2-dihydroxyazobenzene, 4-aminoazobenzene hydrochloride, 4-(methylamino)azobenzene, 4-benzyloxyazobenzene, 2 4-Chloro-4-dimethylaminoazobenzene, azobenzene-4'4-dicarbonyl chloride, 4-hydroxyazobenzene-4-sulfonic acid sodium hydrate, 3-chloro-4-dimethylaminoazobenzene, 4,4-dipentyloxyazobenzene, 4-iodo-4-dimethylaminoazobenzene, 4-(dimethylamino)-2-methylazobenzene, 4-dimethylaminoazobenzene-4-carboxylic acid, 4,4-bis(maleamido)azobenzene, 4,4-dinonyloxyazobenzene, 4,4-bis(hexyloxy)-3-methylazobenzene, 4,4'-bis(decyloxy)-3-methylazobenzene, 4'-hydroxyazobenzene-4-carboxylic acid hydrate, diethyl azobenzene-4,4'-dicarboxylate, 4-acetamido-2 ',3-Dimethylazobenzene, ethyl 4-(4-hydroxyazobenzene) benzoate, 4-amino-1,1'-azobenzene-3,4'-disulfonic acid sodium salt, 4,4'-di-n-dodecyloxyazobenzene oxide, 4,4'-bis(dodecyloxy)-3-methylazobenzene, 4-dimethylaminophenylazobenzenesulfonyl chloride, 2,4-hexadiyn-1,6-diol bis(azobenzene-4-sulfonate), 4-(dimethylamino)azobenzene 4'-isothiocyanate, 4-[bis(9,9-dimethylfluoren-2-yl)amino]azobenzene, 4-dimethylaminoazobenzene-4'-sulfonyl-L-leucine, 5-sulfo-4'-diethylamino-2,2'-dihydroxyazobenzene , 4-(Diethylamino)azobenzene, 4-hydroxy-4'-dimethylaminoazobenzene, 4,4'-dioctyloxyazobenzene oxide, 2-aminoazotoluene hydrochloride, dimethyl yellow, o-aminoazotoluene, 4-(phenylazo)benzoic acid, 4,4'-azoxyanisole, 4-(4-bromophenylazo)phenol, 4-(4-nitrophenylazo)phenol, m-methyl red, dansyl-L-alanine, 4-(4-butylphenylazo)phenol, dimethyl yellow standard solution, methyl red hydrochloride, Sudan Orange G, diethyl 4,4'-azodibenzoate, methyl red sodium salt, 4-[4-(dimethylamino)phenylazo]benzoic acid N-succinimidyl ester, olsalazine sodium.
[0017] Preferably, the negative pressure method in step (4) is to immerse the wood chips in a container containing azobenzene compound solution and treat them at a negative pressure of -0.1 to -0.08 MPa for 1 hour.
[0018] The present invention also provides flexible intelligent wood with responsive function prepared by the preparation method described in the above technical solution.
[0019] The present invention also provides an intelligent response flexible wood actuator, which is obtained by editing the flexible intelligent wood.
[0020] Beneficial technical effects: The present invention provides a flexible intelligent wood, brake and preparation method with responsive functions. The preparation method provided by the present invention comprises treating the wood with sodium chlorite solution to remove lignin, removing hemicellulose by alkali treatment, compounding the wood chips with azobenzene compounds by negative pressure method, and then preparing the wood chips by densification treatment to form a film. The present invention uses wood as the main raw material, which is a natural green renewable material; the intelligent responsive flexible wood actuator can respond to external stimuli by changing its shape when stimulated by light; the intelligent responsive flexible wood actuator can not only enable wood to be applied to the field of intelligent flexible components, but also the intelligent responsive flexible wood actuator can be applied to the field of wireless drive robots without batteries, cables, electronic components, etc.; the characteristics of flexibility and intelligent response meet the requirements of lightweight, miniaturization and controllability of micro robots, etc., in the application scenarios of intelligent functional materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] FIG1 is a composition analysis diagram of the flexible smart wood prepared in Example 1;
[0022] FIG2 is a microscopic morphology of the original wood, the wood from which lignin has been removed, and the wood after alkali treatment in Example 1;
[0023] FIG3 is a surface microscopic morphology and a cross-sectional view of the original wood film and the azobenzene-loaded wood film in Example 1;
[0024] FIG4 is a diagram showing the transparency and haze of azobenzene-free wood film and azobenzene-loaded wood film in Example 1;
[0025] FIG5 is a test diagram of the effect of the flexible smart wood obtained in Example 1 in holding a toothpick in response to light;
[0026] FIG6 is a diagram showing the light response of a butterfly-shaped smart responsive flexible wood actuator;
[0027] Figure 7 is a diagram showing the effect of the intelligent responsive flexible wood actuator being used in a lifting device. DETAILED DESCRIPTION
[0028] The present invention provides a method for preparing flexible smart wood with responsive function, comprising the following steps:
[0029] (1) Sodium acetate and acetic acid were weighed and uniformly stirred in deionized water to prepare a buffer solution with a pH of 4.6. Sodium chlorite was weighed and dissolved in the buffer solution to obtain solution A, wherein the content of sodium chlorite in solution A was 1 to 1.5 wt%.
[0030] (2) Cut the wood into 20×50×0.8mm 3 The wood chips of different sizes were immersed in solution A and stirred at 500 r / min and 80 °C for 6 h to remove lignin.
[0031] (3) Wash the wood chips obtained in step (2) in deionized water, prepare a 4% NaOH solution, place the washed wood chips in the prepared 4% NaOH solution, and place the container in a vacuum drying oven under negative pressure for 30 minutes. Treat in the NaOH solution for 3-6 hours until the wood chips soften.
[0032] (4) The softened wood chips were washed with deionized water, and then the washed wood chips were placed in an acetone solution for cleaning. The above cleaning processes were completed in a vacuum drying oven at a pressure of -0.1 MPa, and each time was 20 minutes. Azobenzene compounds were dissolved in N'N-dimethylformamide (DMF, AR, 99.5%), and then the wood chips washed with acetone were placed in the DMF solution of azobenzene compounds. They were placed in a vacuum drying oven at a negative pressure of -0.1 to -0.08 MPa for 1 hour, in order to impregnate the azobenzene compounds into the pores of the wood chips.
[0033] (5) The wood chips impregnated with the azobenzene compound were removed and rinsed with deionized water to remove the azobenzene and residual DMF liquid on the surface of the wood chips. The wood chips were then placed between steel plates covered with a PES membrane. A 6-10 kg weight was applied to the steel plates to compress the wood chips into a membrane. The compressed wood chips were approximately 45-70 μm thick and translucent.
[0034] The present invention also provides a flexible smart wood with responsive function prepared by the preparation method described in the above technical solution
[0035] The present invention also provides a smart, responsive flexible wood actuator. This actuator is created by editing the flexible smart wood. Specifically, a wood piece is cut using the shape of an insect, such as a butterfly or dragonfly, to create a specially shaped piece. Alternatively, one end of the wood piece is fixed to serve as a lifting device. The designed wood piece, when exposed to ultraviolet light, ultimately creates a smart, responsive flexible wood actuator.
[0036] In order to better understand the present invention, the content of the present invention is further illustrated below in conjunction with the examples, but the content of the present invention is not limited to the following examples.
[0037] Example 1
[0038] (1) Weigh 4 g of sodium acetate and 18 g of acetic acid, stir them evenly in 3 L of deionized water to prepare a buffer solution with pH = 4.6. Weigh 6 g of sodium chlorite and dissolve it in 594 g of buffer solution to form solution A.
[0039] (2) Cut the balsa wood into 20×50×0.8mm 3 The wood chips of different sizes were immersed in solution A and stirred at 500 r / min and 80 °C for 6 h;
[0040] (3) Remove the wood chips, wash them in deionized water, prepare a 4% NaOH solution, place the cleaned wood chips in the prepared 4% NaOH solution, place the container in a vacuum drying oven at negative pressure for 30 minutes, and treat in the NaOH solution for 6 hours until the wood chips soften;
[0041] (4) The softened wood chips were washed twice again with deionized water, and then the washed wood chips were placed in 20 ml of acetone solution and washed twice. The above washing process was completed in a vacuum drying oven at a pressure of -0.1 MPa, and each time took 20 minutes; azobenzene was dissolved in N'N-dimethylformamide (DMF, AR, 99.5%), and then the wood chips washed with acetone were placed in the azobenzene DMF solution, and placed in a vacuum drying oven at a negative pressure of -0.1 MPa for 1 hour;
[0042] (5) The azobenzene-impregnated wood chips were removed and rinsed with deionized water to remove the azobenzene and residual DMF on the wood chip surface. The wood chip was then placed between a steel plate covered with a PES membrane. A 10 kg weight was applied to the steel plate to compress the wood chip into a film. The compressed wood chip was approximately 45 μm thick and translucent.
[0043] Compositional analysis of the original wood and the prepared flexible smart wood reveals, as shown in Figure 1, that the acid buffer and alkali treatments significantly reduced the lignin and hemicellulose content of the wood compared to the original wood, decreasing from 50% of the total to less than 20%. This explains the flexibility of the smart responsive flexible wood, as the hard components have been largely removed.
[0044] The micromorphology of the original wood, the wood after lignin removal, and the wood after alkali treatment was characterized, as shown in Figure 2. Figures a and d are the micromorphology of the original wood, b and e are the micromorphology of the wood after lignin removal, and e and f are the micromorphology of the wood after alkali treatment. Figure 2 shows that the wood cell walls are gradually becoming thinner, which is the result of the removal of lignin and hemicellulose in the cell walls. Further magnification of Figures d, e, and f shows that the intercellular angle changes from dense to loose and porous, which is consistent with the conclusion expressed by the composition analysis in Figure 1.
[0045] The surface micromorphology of the azobenzene-loaded wood film was characterized, as shown in Figure 3. The surface micromorphology of the original wood film is shown in (a-c), the surface micromorphology of the azobenzene-loaded wood film is shown in (d-f), the cross-section of the original wood film is shown in (g), and the cross-section of the azobenzene-loaded wood film is shown in (hi). Figure 3 shows that the surface of the original wood film is very smooth, while the surfaces of Figures d, e, and f contain granular azobenzene compounds. Figure g is a cross-section of the original wood film, and compared to Figures h and i, the azobenzene compounds are missing between the cellulose layers. This indicates that the azobenzene compounds are already loaded on the surface of the wood film.
[0046] The transparency and haze of the wood film and the azobenzene-loaded wood film were measured, as shown in Figure 4 (a), where the transparency graph and b the haze graph. Figure 4a shows that the addition of azobenzene compounds reduced the transparency of the original wood film by approximately 30%, which can affect the light response speed. Figure 4b shows that the haze of the original wood film did not change much compared to the wood film loaded with azobenzene compounds, indicating that the effect of azobenzene compounds on the haze of the wood film is negligible.
[0047] Example 2
[0048] (1) Weigh 4 g of sodium acetate and 18 g of acetic acid, stir them evenly in 3 L of deionized water to prepare a buffer solution with pH = 4.6. Weigh 6 g of sodium chlorite and dissolve it in 594 g of buffer solution to form solution A.
[0049] (2) Cut the poplar wood into 20×50×0.8mm 3 The wood chips of different sizes were immersed in solution A and stirred at 500 r / min and 80 °C for 6 h;
[0050] (3) Remove the wood chips, wash them in deionized water, prepare a 4% NaOH solution, place the cleaned wood chips in the prepared 4% NaOH solution, place the container in a vacuum drying oven at negative pressure for 30 minutes, and treat in the NaOH solution for 5 hours until the wood chips soften;
[0051] (4) The softened wood chips were washed twice again with deionized water, and then the washed wood chips were placed in 20 ml of acetone solution and washed twice. The above washing process was completed in a vacuum drying oven at a pressure of -0.1 MPa, and each time took 20 minutes; azobenzene was dissolved in N'N-dimethylformamide (DMF, AR, 99.5%), and then the wood chips washed with acetone were placed in the azobenzene DMF solution, and placed in a vacuum drying oven at a negative pressure of -0.1 MPa for 1 hour;
[0052] (5) The wood chips impregnated with azoxybenzene were removed and rinsed with deionized water to remove the azobenzene and residual DMF on the surface of the wood chips. The wood chips were then placed between steel plates covered with a PES membrane. A 10 kg weight was applied to the steel plates to compress the wood chips into a membrane. The compressed wood chips were approximately 50 μm thick and translucent.
[0053] Example 3
[0054] (1) Weigh 4 g of sodium acetate and 18 g of acetic acid, stir them evenly in 3 L of deionized water to prepare a buffer solution with pH = 4.6. Weigh 6 g of sodium chlorite and dissolve it in 594 g of buffer solution to form solution A.
[0055] (2) Cut the pine wood into 20×50×0.8mm 3 The wood chips of different sizes were immersed in solution A and stirred at 500 r / min and 80 °C for 6 h;
[0056] (3) Remove the wood chips, wash them in deionized water, prepare a 4% NaOH solution, place the cleaned wood chips in the prepared 4% NaOH solution, place the container in a vacuum drying oven at negative pressure for 30 minutes, and treat in the NaOH solution for 5 hours until the wood chips soften;
[0057] (4) The softened wood chips were washed twice again with deionized water, and then the washed wood chips were placed in 20 ml of acetone solution and washed twice. The above washing process was completed in a vacuum drying oven at a pressure of -0.1 MPa, and each time took 20 minutes; p-aminoazobenzene was dissolved in N'N-dimethylformamide (DMF, AR, 99.5%), and then the wood chips washed with acetone were placed in the p-aminoazobenzene DMF solution, and placed in a vacuum drying oven at a negative pressure of -0.1 MPa for 1 hour;
[0058] (5) The p-aminoazobenzene-impregnated wood chips were removed and rinsed with deionized water to remove the azobenzene and residual DMF on the wood chip surface. The wood chip was then placed between a steel plate covered with a PES membrane. A 10 kg weight was applied to the steel plate to compress the wood chip into a film. The compressed wood chip had a thickness of approximately 48 μm and was translucent.
[0059] Example 4
[0060] (1) Weigh 4 g of sodium acetate and 18 g of acetic acid, stir them evenly in 3 L of deionized water to prepare a buffer solution with pH = 4.6. Weigh 6 g of sodium chlorite and dissolve it in 594 g of buffer solution to form solution A.
[0061] (2) Cut birch into 20×50×0.8mm 3 The wood chips of different sizes were immersed in solution A and stirred at 500 r / min and 80 °C for 6 h;
[0062] (3) Take out the wood chips, wash them in deionized water, prepare a 4% NaOH solution, place the cleaned wood chips in the prepared 4% NaOH solution, place the container in a vacuum drying oven at negative pressure for 30 minutes, and treat in the NaOH solution for 4 hours until the wood chips soften;
[0063] (4) The softened wood chips were washed twice again with deionized water, and then the washed wood chips were placed in 20 ml of acetone solution and washed twice. The above washing process was completed in a vacuum drying oven at a pressure of -0.1 MPa, and each time took 20 minutes; p-aminoazobenzene was dissolved in N'N-dimethylformamide (DMF, AR, 99.5%), and then the wood chips washed with acetone were placed in the p-aminoazobenzene DMF solution, and placed in a vacuum drying oven at a negative pressure of -0.1 MPa for 1 hour;
[0064] (5) The p-aminoazobenzene-impregnated wood chips were removed and rinsed with deionized water to remove the azobenzene and residual DMF on the wood chip surface. The wood chip was then placed between a steel plate covered with a PES membrane. A 10 kg weight was applied to the steel plate to compress the wood chip into a membrane. The compressed wood chip had a thickness of approximately 55 μm and was translucent.
[0065] Example 5
[0066] The same as Example 4, except that p-aminoazobenzene was replaced with 4-methoxyazobenzene. The compressed wood chips had a thickness of about 52 μm and were translucent.
[0067] Example 6
[0068] The same as Example 4, except that p-aminoazobenzene was replaced with 3,3-dicarboxylic acid azobenzene. The compressed wood chips had a thickness of approximately 47 μm and were translucent.
[0069] Test example
[0070] The flexible smart wood obtained in Example 1 was tested for its light-responsiveness by lifting a toothpick. As shown in Figure 5, a weight (a toothpick) was placed at one end of the flexible smart wood at a distance d1 from the boundary. Upon exposure to UV light, the flexible wood responded by tilting the weighted end and pushing it to the right. The distance from the boundary at this point was measured to be d2. The figure shows that d2 > d1. Furthermore, the angle between the end of the flexible smart wood and the plane differed before and after exposure to light, indicating that β > α.
[0071] Example 7
[0072] The flexible smart wood obtained in Example 1 was cut into a butterfly shape as a template to obtain a wood brake with a special shape, and its effect was tested. The light response effect is shown in Figure 6. Under the irradiation of ultraviolet light, the wings flapped, and the change in the position of the wings can be seen from the figure.
[0073] Example 8
[0074] One end of the flexible smart wood obtained in Example 1 was fixed to serve as a lifting device, creating a wood brake, and its effectiveness was tested. As shown in Figure 7, upon exposure to UV light, the flexible smart wood responded, lifting a placed toothpick and acting as a lifting device without any wires or other connections.
[0075] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.
Claims
1. A method for preparing flexible smart wood with responsive function, characterized in that: The following steps are involved: (1) preparing an acetic acid-sodium acetate buffer solution, and dissolving sodium chlorite in the buffer solution to obtain a solution A; (2) cutting the wood into wood chips and immersing them in solution A for delignification treatment; (3) treating the wood chips obtained in step (2) with alkali to remove hemicellulose in the wood chips; (4) impregnating the azobenzene compound into the alkali-treated wood chips by a negative pressure method; (5) Densifying the wood chips obtained in step (4) into a wood film to obtain a flexible smart wood with responsive functions.
2. The preparation method according to claim 1, characterized in that: The pH of the buffer solution in step (1) is 4.6, and the content of sodium chlorite in the solution A is 1 to 1.5 wt%.
3. The preparation method according to claim 1, characterized in that: The wood material in step (2) includes balsa wood, poplar wood, pine wood, birch wood, beech wood, oak wood, basswood, elm wood, ironwood, ash wood, paulownia wood, camphor wood, rubber wood, oak wood, cypress wood and fir wood.
4. The preparation method according to claim 1, characterized in that: The delignification treatment in step (2) is as follows: the cut wood chips are immersed in solution A, stirred at 500 r / min and heated to 80° C. and cooked for 6 hours.
5. The preparation method according to claim 1, characterized in that: The alkali treatment in step (3) is to place the wood chips after the lignin is removed in a 4% concentration NaOH solution and soak them for 3-6 hours.
6. The preparation method according to claim 1, characterized in that: The azobenzene compound of step (4) includes azobenzene, azobenzene oxide, p-aminoazobenzene, 4-methoxyazobenzene, 3,3-dicarboxylic acid azobenzene, 4,4-dicarboxylic acid azobenzene, 4-aminoazobenzene-4-sodium sulfonate, 3,3-dimethylazobenzene, 4-sulfonyl chloride azobenzene, 4-(dimethylamino)-2-methylazobenzene, 4-nitrobenzene, 4-phenylazobenzoyl chloride, p-diaminoazobenzene, 4-chloro-4-dimethylaminoazobenzene, 4-carboxy-2-aminoazobenzene, 4'4 dimethyl dicarboxylate-azobenzene, 2,2-dihydroxyazobenzene, 4-aminoazobenzene hydrochloride, 4-(methylamino)azobenzene, 4-benzyloxyazobenzene, 2-chloro- 4-Dimethylaminoazobenzene, azobenzene-4'4-dicarbonyl chloride, 4-hydroxyazobenzene-4-sulfonate sodium hydrate, 3-chloro-4-dimethylaminoazobenzene, 4,4-dipentyloxyazobenzene, 4-iodo-4-dimethylaminoazobenzene, 4-(dimethylamino)-2-methylazobenzene, 4-dimethylaminoazobenzene-4-carboxylic acid, 4,4-bis(maleamido)azobenzene, 4,4-dinonyloxyazobenzene, 4,4-bis(hexyloxy)-3-methylazobenzene, 4,4'-bis(decyloxy)-3-methylazobenzene, 4'-hydroxyazobenzene-4-carboxylic acid hydrate, diethyl azobenzene-4,4'-dicarboxylate, 4-acetylamino-2', 3-Dimethylazobenzene, 4-(4-hydroxy-azobenzene) benzoic acid ethyl ester, 4-amino-1,1'-azobenzene-3,4'-disulfonic acid sodium salt, 4,4'-di-n-dodecyloxy azobenzene oxide, 4,4'-bis(dodecyloxy)-3-methylazobenzene, 4-dimethylaminophenylazobenzenesulfonyl chloride, 2,4-hexadiyne-1,6-diol bis(azobenzene-4-sulfonate), 4-(dimethylamino)azobenzene 4'-isothiocyanate, 4-[bis(9,9-dimethylfluoren-2-yl)amino]azobenzene, 4-dimethylaminoazobenzene-4'-sulfonyl-L-leucine, 5-sulfo-4'-diethylamino-2,2'-dihydroxyazobenzene, 4-(Diethylamino)azobenzene, 4-hydroxy-4'-dimethylaminoazobenzene, 4,4'-di-n-octyloxyazobenzene oxide, 2-aminoazotoluene hydrochloride, dimethyl yellow, o-aminoazotoluene, 4-(phenylazo)benzoic acid, 4,4'-azobenzene oxide, 4-(4-bromophenylazo)phenol, 4-(4-nitrophenylazo)phenol, m-methyl red, dansyl-L-alanine, 4-(4-butylphenylazo)phenol, dimethyl yellow standard solution, methyl red hydrochloride, Sudan Orange G, diethyl 4,4'-azodibenzoate, methyl red sodium salt, 4-[4-(dimethylamino)phenylazo]benzoic acid N-succinimidyl ester, olsalazine sodium.
7. The preparation method according to claim 1, characterized in that: The negative pressure method in step (4) is to immerse the wood chips in a container filled with azobenzene compound solution and treat them at a negative pressure of -0.1 to -0.08 MPa for 1 hour.
8. Flexible smart wood with responsive function prepared by the preparation method according to any one of claims 1 to 7.
9. An intelligent responsive flexible wood actuator, characterized in that: Obtained by editing the flexible smart wood as described in claim 8.
Citation Information
Patent Citations
Preparation method of photoresponse unbraced film and application thereof
CN109971009A
Preparation method of wood-based biomimetic artificial muscle
CN110253702A
Preparation method of high-strength flexible wood film
CN113858368A
Flame retardant woody material and its manufacturing method
JP2005161588A