Magnetic ceramic substrate, substrate manufacturing method, and circulator

The magnetic ceramic substrate with a surface pattern conductor of Ag, amorphous glass, and voids addresses adhesion and thermal stress issues by optimizing density and glass content, resulting in enhanced adhesion and plating adhesion on the ferrite base material.

WO2024236669A1PCT designated stage expired Publication Date: 2024-11-21MITSUBISHI ELECTRIC CORP

Patent Information

Application Number
PCT/JP2023/018006
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

The existing methods for forming a surface pattern conductor on a magnetic ceramic substrate face challenges such as poor adhesion and thermal stress-induced peeling, particularly when using ferrite as the base material, due to differences in thermal expansion coefficients and mechanical strength, and excessive glass content affecting plating adhesion.

Method used

A magnetic ceramic substrate with a surface pattern conductor composed of Ag, amorphous glass, and voids, where the apparent density is adjusted to reduce thermal stress and elastic modulus, and the amorphous glass content is optimized between 3 vol% and 12 vol% to improve adhesion and plating adhesion, while minimizing glass floating.

Benefits of technology

The solution achieves excellent adhesion and plating adhesion of the surface pattern conductor on the ferrite base material, reducing thermal stress and maintaining electrical properties, with improved reliability and reduced risk of peeling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023018006_21112024_PF_FP_ABST
    Figure JP2023018006_21112024_PF_FP_ABST
Patent Text Reader

Abstract

A magnetic ceramic substrate (1) comprises a base material (2) formed from ferrite, and comprises, on the surface of the base material (2), a surface layer pattern conductor (6) which contains 3-12 vol% of an amorphous glass (4) and a metal conductor (3) composed of Ag, and the apparent density of which is 7.3-9.0 g / cm3.
Need to check novelty before this filing date? Find Prior Art

Description

Magnetic ceramic substrate, substrate manufacturing method, and circulator

[0001] The present disclosure relates to a magnetic ceramic substrate, a substrate manufacturing method, and a circulator.

[0002] Circulators are used in the transmission and reception circuits of electronic devices to control the flow of transmission and reception signals and share antennas. In the ceramic circuit board used in this circulator, a circuit pattern is formed by metallizing the surface of a magnetic ceramic substrate. A commonly used thick-film printing method for forming a circuit pattern is a simple method with excellent mass productivity. However, this circuit pattern formation method has the problem of difficulty in ensuring adhesion between the ceramic substrate and the conductor pattern and improving reliability during solder mounting. Furthermore, when a conductor paste containing a large amount of glass frit is used to improve the adhesion of the conductor pattern, there is the problem of poor plating adhesion during plating on the surface of the conductor.

[0003] Therefore, Patent Document 1 proposes a circuit board in which a first metallized layer with high adhesion is formed by applying a first paste to the surface of a ceramic substrate and firing the first paste, and a second metallized layer with high heat dissipation is formed by applying a second paste to the first metallized layer and firing the second paste, where the second paste has a lower ratio of glass component to metal particle component than the first paste.

[0004] Japanese Patent Application Laid-Open No. 2007-201346

[0005] According to the circuit board proposed in Patent Document 1, the first paste contains a glass component, which improves adhesion between the ceramic substrate and the conductor. However, this circuit board has a problem in that the conductor may peel off when thermal stress is applied to the interface during baking of the paste or thermal stress due to a heat cycle or the like.

[0006] The present disclosure aims to provide a magnetic ceramic substrate having a surface pattern conductor formed on a base material made of ferrite, which has excellent adhesion of the surface pattern conductor and excellent plating adhesion.

[0007] The magnetic ceramic substrate according to the present disclosure includes a base material made of ferrite, a metal conductor made of Ag, and 3 vol% to 12 vol% of amorphous glass, and has an apparent density of 7.3 g / cm. 3 9.0g / cm or more 3 The surface of the substrate is provided with a surface layer pattern conductor as follows.

[0008] According to the present disclosure, the apparent density of the surface pattern conductor is lower than the true density of Ag, and therefore the elastic modulus (apparent elastic modulus) of the surface pattern conductor is lower than the elastic modulus of Ag. Furthermore, because the surface pattern conductor contains amorphous glass, the thermal expansion coefficient of the entire surface pattern conductor is lower than the thermal expansion coefficient of Ag. Therefore, the difference in thermal expansion coefficient between the substrate and the surface pattern conductor is relatively small. Therefore, in the magnetic ceramic substrate according to the present disclosure, the thermal stress at the interface between the substrate and the surface pattern conductor is relatively small. Furthermore, in the magnetic ceramic substrate according to the present disclosure, the appropriate amount of amorphous glass reduces glass floating on the surface of the surface pattern conductor. Therefore, according to the present disclosure, a magnetic ceramic substrate having a surface pattern conductor formed on a substrate made of ferrite can be provided, which has excellent adhesion of the surface pattern conductor and excellent plating adhesion.

[0009] 1 is a cross-sectional view of a magnetic ceramic substrate 1 according to embodiment 1. FIG. 2 is a cross-sectional view of a magnetic ceramic substrate having a dense surface pattern conductor according to the prior art. FIG. 3 is an enlarged view of a surface pattern conductor 6 according to embodiment 1. FIG. 4 is an enlarged view of a surface pattern conductor not containing glass. FIG. 5 is an enlarged view of an interface between a substrate 2 having a smoothed surface and a surface pattern conductor 6 according to embodiment 1. FIG. 6 is an enlarged view of an interface between a substrate having a non-smoothed surface and a surface pattern conductor. FIG. 7 is a cross-sectional view of a magnetic ceramic substrate 1 according to embodiment 1. FIG. 8 is a cross-sectional view of a circulator 17 according to embodiment 2. FIG. 9 is a cross-sectional view of a circulator 17 according to embodiment 2. FIG. 10 is a table showing an overview of examples and comparative examples related to the magnetic ceramic substrate 1.

[0010] In the description of the embodiments and the drawings, the same elements and corresponding elements are denoted by the same reference numerals, and the description of the elements denoted by the same reference numerals will be omitted or simplified as appropriate.

[0011] Embodiment 1. This embodiment will be described in detail below with reference to the drawings. A known method for forming a surface pattern conductor on the surface of a sintered magnetic ceramic substrate involves printing a conductor paste containing glass as a binder on the surface of the magnetic ceramic substrate and then baking the printed conductor paste. However, due to differences in the thermal expansion coefficients between the substrate and the surface pattern conductor, thermal stress may occur at the interface between the substrate and the surface pattern conductor, potentially causing peeling of the surface pattern conductor. In particular, when ferrite, which has low mechanical strength, is used as the substrate, microcracks are likely to occur near the interface of the substrate, and these microcracks can serve as the starting point for peeling of the surface pattern conductor. Furthermore, when the amount of glass added is significantly increased to improve the adhesion of the surface pattern conductor, glass lift on the surface of the conductor pattern increases, resulting in poor plating adhesion on the surface of the conductor pattern. Therefore, the inventors of the present disclosure conducted extensive research to solve the above-mentioned problems and discovered the following regarding a magnetic ceramic substrate having a surface pattern conductor formed on a ferrite substrate. 1. 1. By reducing the apparent density of the surface pattern conductor, the elastic modulus of the surface pattern conductor can be reduced. 2. By incorporating amorphous glass, which has a thermal expansion coefficient lower than that of Ag, into the surface pattern conductor, the thermal expansion coefficient of the surface pattern conductor can be reduced, thereby reducing the difference in thermal expansion coefficient between the substrate and the surface pattern conductor, thereby reducing the thermal stress generated at the interface between the substrate and the surface pattern conductor and improving the adhesion between the substrate and the surface pattern conductor.

[0012] ***Description of Configuration*** FIG. 1 shows an example of a cross-sectional schematic diagram of a magnetic ceramic substrate 1 according to embodiment 1. As shown in FIG. 1, the magnetic ceramic substrate 1 is composed of a substrate 2 made of ferrite and a surface pattern conductor 6 formed on the surface of the substrate 2. The magnetic ceramic substrate 1 is used in circuit boards that utilize the magnetism of electronic devices. The surface of the substrate 2 is the surface of the substrate 2 that is in contact with the surface pattern conductor 6. Ferrite is also called magnetic ceramic. The surface pattern conductor 6 is composed of a metal conductor 3, amorphous glass 4, and voids 5, and is also called a conductor pattern. The metal conductor 3 is a conductor made of Ag, for example. The voids 5 are three-dimensional regions within the surface pattern conductor 6 that are not filled with the metal conductor 3. A plurality of voids 5 exist within the surface pattern conductor 6. At least a portion of the plurality of voids 5 is filled with amorphous glass 4.

[0013] Generally, in ceramic substrates, the thermal expansion coefficients differ between the substrate and the surface pattern conductor, resulting in thermal stress at the interface between the substrate and the surface pattern conductor when the surface pattern conductor is baked. If this thermal stress is excessively large, it can cause a decrease in adhesion of the surface pattern conductor. In particular, when a surface pattern conductor containing a glass binder is used, the strong adhesive strength of the glass at the interface between the substrate and the surface pattern conductor can cause microcracks in the substrate near the interface due to the thermal stress. The microcracks can then act as starting points for peeling of the surface pattern conductor, scraping it away from the substrate. Peeling of the surface pattern conductor originating from microcracks in the substrate rarely occurs when a ceramic substrate using a relatively high-strength substrate, such as a substrate made of aluminum oxide or silicon nitride, is used, but tends to occur more significantly when a relatively low-strength substrate, such as a substrate made of ferrite, is used. Therefore, when a substrate 2 made of ferrite is used, as in the magnetic ceramic substrate 1 according to embodiment 1, it is important to minimize the thermal stress generated at the interface in order to improve adhesion between the substrate 2 and the surface pattern conductor 6. Thermal stress occurring at the interface tends to increase as the difference in thermal expansion coefficients between the materials opposing each other at the interface increases and as the modulus of elasticity of each material increases. Therefore, in order to improve the adhesion between the substrate 2 and the surface pattern conductor 6, it is important to reduce the difference in thermal expansion coefficients between the substrate 2 and the surface pattern conductor 6 by lowering the modulus of elasticity and the thermal expansion coefficient of the surface pattern conductor 6. However, for the substrate 2, emphasis must be placed on its electrical and magnetic properties, which are the basic performance characteristics of a substrate. Therefore, it is difficult to improve the modulus of elasticity and the thermal expansion coefficient of the substrate 2. Therefore, in the magnetic ceramic substrate 1 according to embodiment 1, the occurrence of thermal stress at the interface is reduced by improving the surface pattern conductor 6.

[0014] The apparent density of the surface layer pattern conductor 6 is the true density of Ag, which is the main component of the surface layer pattern conductor 6 (10.49 g / cm 3) is smaller. By reducing the apparent density, the elastic modulus (apparent elastic modulus) of the surface pattern conductor 6 becomes lower than the elastic modulus of Ag (82.7 GPa). Therefore, the thermal stress generated at the interface can be reduced. On the other hand, as shown in Figure 2, when the surface pattern conductor has a dense structure, the elastic modulus of the surface pattern conductor becomes high (equivalent to the elastic modulus of Ag). Therefore, large thermal stress occurs at the interface, which may result in a decrease in adhesion. Figure 2 shows a cross-sectional view of a magnetic ceramic substrate according to the prior art, which has a dense surface pattern conductor.

[0015] The surface pattern conductor 6 also contains amorphous glass 4. As shown in FIG. 3 , in the surface pattern conductor 6, some of the spaces between the partially sintered Ag particles are filled with amorphous glass 4 that was once melted and solidified. The spaces between the Ag particles that are not filled with amorphous glass 4 are voids 5. Generally, the thermal expansion coefficient of glass tends to be smaller than that of Ag. Therefore, as shown in FIG. 3 , the presence of amorphous glass 4, which has a relatively small thermal expansion coefficient, between the partially sintered Ag particles makes the thermal expansion coefficient of the entire surface pattern conductor 6 smaller than that of Ag. Therefore, the difference in thermal expansion coefficient between the substrate 2 and the surface pattern conductor 6 can be kept relatively low, thereby reducing thermal stress generated at the interface.

[0016] On the other hand, as shown in Figure 4, when amorphous glass 4 is not present between the partially sintered Ag particles, the thermal expansion coefficient of the surface pattern conductor 6 does not decrease, i.e., the thermal expansion coefficient of the surface pattern conductor 6 is a relatively large value equivalent to the thermal expansion coefficient of Ag. Therefore, in this case, the effect of reducing thermal stress generated at the interface cannot be obtained. For this reason, the magnetic ceramic substrate 1 according to the first embodiment, having the above-mentioned configuration, has excellent adhesion of the surface pattern conductor 6 and excellent plating adhesion.

[0017] The material of the substrate 2 may be any material that satisfies the magnetic properties required for the application of the magnetic ceramic substrate 1. A specific example is garnet-type ferrite (Y3 Fe 5 O 12 etc.), M-type hexagonal ferrite (BaFe 12 O 19 , SrFe 12 O 19 ), W-type hexagonal ferrite (BaFe 18 O 27 , SrFe 18 O 27 ), Z-type hexagonal ferrite (Ba 3 Co 2 Fe 24 O 41 , Sr 3 Co 2 Fe 24 O 41 ), Y-type hexagonal ferrite (BaZnFe 12 O 22 ), or spinel-type ferrite (AFe 2 O 4 : A = Mn, Co, Ni, Cu, Zn). In particular, garnet-type ferrite is suitable as the material for the substrate 2 because it has low magnetic loss in the high frequency range and is in high demand as a magnetic circuit board for microwaves. Furthermore, it is preferable that the surface of the substrate 2 is smooth in order to suppress microcracks 8 in the substrate 2, which can cause a decrease in adhesion between the substrate 2 and the surface pattern conductor 6. The smooth surface makes it more difficult for microcracks 8 to occur in the substrate 2, as shown in FIG. 5, even if thermal stress occurs at the interface due to a difference in the thermal expansion coefficients between the substrate 2 and the surface pattern conductor 6.

[0018] On the other hand, as shown in FIG. 6 , when the surface of the substrate 2 is not smooth, stress due to the difference in thermal expansion coefficient between the substrate 2 and the surface pattern conductor 6 is concentrated on the protrusions 7 on the surface of the substrate 2, causing partial tensile stress to be applied to the protrusions 7. As a result, as shown in FIG. 6 , microcracks 8 are likely to occur mainly in the protrusions 7, and the microcracks 8 may serve as starting points for reducing the adhesion of the surface pattern conductor 6. Therefore, it is more preferable to smooth the surface of the substrate 2. A smooth surface refers to a surface that has been subjected to a mirror polishing process on the substrate 2 after cutting. Examples of mirror polishing methods include buffing, barrel polishing, and shot blast polishing. The surface smoothness is preferably 0.01 μm or more and 0.5 μm or less in terms of Ra, and more preferably 0.02 μm or more and 0.3 μm or less. When the surface smoothness exceeds 0.5 μm in Ra, the stress concentrated on the surface protrusions 7 becomes large, which may occasionally cause microcracks 8, and although this does not impair practicality, adhesion tends to decrease slightly. On the other hand, when the surface smoothness is less than 0.01 μm in Ra, excessive mirror finishing is required, which reduces productivity. Here, the arithmetic mean roughness (Ra) is a value calculated by [Equation 1] using data on the surface irregularities of the substrate 2 measured in the linear direction of a length of 10 mm and a width (l) using a contact roughness meter.

[0019]

[0020] The surface layer pattern conductor 6 is composed of a metal conductor 3, amorphous glass 4, and voids 5. The apparent density of the surface layer pattern conductor 6 is 7.3 g / cm 3 9.0g / cm or more 3 In this way, the apparent density of the surface layer pattern conductor 6 is adjusted to the true density of Ag (10.49 g / cm 3 ), the elastic modulus (apparent elastic modulus) of the surface layer pattern conductor 6 becomes lower than the elastic modulus of Ag (82.7 GPa). Therefore, it is possible to reduce the thermal stress generated at the interface. From the viewpoint of reducing the thermal stress generated at the interface, the lower the apparent density of the surface layer pattern conductor 6, the more the thermal stress can be reduced. However, when the apparent density is 7.3 g / cm3 If the apparent density is too low, such as less than 9.0 g / cm, the contact surface between the surface pattern conductor 6 and the substrate 2 becomes too sparse, resulting in poor adhesion. Furthermore, in this case, the volume resistivity deteriorates significantly, resulting in increased electrical loss and making it impossible for the surface pattern conductor 6 to function. 3 If the density exceeds this value, the effect of reducing the elastic modulus (apparent elastic modulus) becomes smaller, so the thermal stress generated at the interface increases, and microcracks 8 are more likely to occur in the substrate 2. Here, the apparent density is a value calculated by taking several photographs of the cross section of the surface pattern conductor 6 of the magnetic ceramic substrate 1 using a scanning electron microscope (SEM) at magnifications of several hundred to several thousand times, determining the areas occupied by the metal conductor 3, the amorphous glass 4, and the voids 5 by image analysis, and using the determined areas to calculate according to [Equation 2].

[0021]

[0022] Here, S Ag and S g and S p are the areas occupied by Ag, glass, and voids, respectively, determined by image analysis. Ag is the true density of Ag, 10.49 g / cm 3 ρ g is the true density of the glass, and ρ g A value according to the type of glass can be used as the true density of each glass. A known value can be used as the true density of each glass. As a specific example, for borosilicate glass, it is 2.51 g / cm 3 The type of glass can also be identified from the composition ratio obtained from the results of elemental analysis using an EPMA (Electron Probe Micro Analyzer) or the like.

[0023] On the other hand, as shown in FIG. 2 , when the surface pattern conductor 6 has a dense structure, the elastic modulus of the surface pattern conductor 6 is relatively high (equivalent to the elastic modulus of Ag). This can result in large thermal stress at the interface, which can reduce adhesion. Furthermore, when the surface pattern conductor 6 has a dense structure, the proportion of the amorphous glass 4 contained in the surface pattern conductor 6 that protrudes from the surface of the dense surface pattern conductor 6 increases. This can lead to a problem of poor plating deposition on the surface pattern conductor 6. Therefore, from the perspective of plating the surface pattern conductor 6, it is preferable to lower the apparent density. To avoid impairing plating deposition, the proportion of the exposed area of ​​the metal conductor 3 on the surface of the surface pattern conductor 6 opposite the substrate 2 is preferably 50% or more, more preferably 60% or more, and even more preferably 70% or more. Here, the ratio of the exposed area of ​​the metal conductor 3 is a value calculated by taking several photographs of the surface of the surface pattern conductor 6 of the magnetic ceramic substrate 1 enlarged several hundred to several thousand times using an SEM, determining the areas occupied by the metal conductor 3, the amorphous glass 4, and the voids 5 using image analysis, and using the determined areas to calculate using [Equation 3].

[0024]

[0025] The surface pattern conductor 6 according to this embodiment contains 3 vol% or more and 12 vol% or less of amorphous glass 4. The amorphous glass 4 contained in the surface pattern conductor 6 serves as a binder between the substrate 2 and the surface pattern conductor 6, thereby contributing to improved adhesion between the substrate 2 and the surface pattern conductor 6. Furthermore, since the thermal expansion coefficient of the amorphous glass 4 is smaller than that of the metal conductor 3, the inclusion of the amorphous glass 4 in the surface pattern conductor 6 reduces the thermal expansion coefficient of the surface pattern conductor 6. This also effectively suppresses thermal stress generated at the interface due to the difference in thermal expansion coefficient between the substrate 2 and the surface pattern conductor 6. However, if the content of the amorphous glass 4 is too high, the proportion of amorphous glass 4 protruding from the surface of the surface pattern conductor 6 will be higher than expected, resulting in poor plating deposition. From this perspective, the content of the amorphous glass 4 in the surface pattern conductor 6 is preferably 3 vol% or more and 12 vol% or less. If the content of amorphous glass 4 is less than 3 vol%, the effect as a binder is weakened, resulting in a decrease in the adhesive strength between the substrate 2 and the surface pattern conductor 6. If the content of amorphous glass 4 is more than 12 vol%, glass floating on the surface of the surface pattern conductor 6 increases, causing problems with plating deposition.

[0026] Considering the above-mentioned viewpoint, it is considered that the optimum content of the amorphous glass 4 in the surface pattern conductor 6 varies depending on the apparent density of the surface pattern conductor 6. Therefore, it is difficult to uniquely determine the optimum content. However, in the surface pattern conductor 6 according to this embodiment, the apparent density is set to 7.3 g / cm in order to reduce the elastic modulus as described above. 3 9.0g / cm or more 3The apparent density is adjusted as follows. Furthermore, it has been found that within this apparent density range, the preferred content of amorphous glass 4 is 3 vol% or more and 12 vol% or less. By setting the apparent density and the content of amorphous glass 4 within the above range, the thermal expansion coefficient and elastic modulus of the surface pattern conductor 6 can be effectively reduced. As a result, thermal stress generated at the interface can be suppressed, and a significant improvement in adhesion can be achieved. Furthermore, glass floating on the surface can be reduced, which is also effective in improving plating adhesion.

[0027] In the magnetic ceramic substrate 1 according to this embodiment, it is more preferable that the difference in thermal expansion coefficient between the substrate 2 and the surface pattern conductor 6 ((thermal expansion coefficient of the surface pattern conductor 6) - (thermal expansion coefficient of the substrate 2)) is 8.2 ppm / K or less. Here, the thermal expansion coefficient of the surface pattern conductor 6 varies depending on the content of the amorphous glass 4 (3 vol% or more and 12 vol% or less). On the other hand, the thermal expansion coefficient of the substrate 2 varies depending on the type of ferrite used. Therefore, the difference in thermal expansion coefficient between the two can be adjusted by combining the content of the amorphous glass 4 and the type of substrate 2. It is more preferable to adjust the difference in thermal expansion coefficient to 8.2 ppm / K or less. When the difference in thermal expansion coefficient exceeds 8.2 ppm / K, the thermal stress generated at the interface is relatively large, which may reduce adhesion, although not to the extent that it impairs practicality.

[0028] The surface pattern conductor 6 according to this embodiment is formed by printing Ag paste in a desired shape on the surface of the substrate 2 using a screen mask or metal mask by thick-film printing, and then baking the printed Ag paste at a desired temperature. Baking the Ag paste means firing the Ag paste. The Ag paste is an example of a conductor paste. The Ag paste contains coarse Ag particles with a particle size of 5 μm to 15 μm, fine Ag particles with a particle size of 1 μm to 3 μm, and amorphous glass powder made of amorphous glass 4. The firing shrinkage of the Ag paste is preferably 5% or less. By including the Ag paste containing coarse Ag particles and fine Ag particles and having a firing shrinkage of 5% or less, the apparent density of the surface pattern conductor 6 after firing the Ag paste can be easily adjusted to a desired value. The thickness of the surface pattern conductor 6 is 2 μm or more and 50 μm or less, preferably 5 μm or more and 30 μm or less, and more preferably 10 μm or more and 20 μm or less. When the thickness of the surface pattern conductor 6 is less than 2 μm, the pattern is likely to fade during thick-film printing, resulting in reduced productivity. On the other hand, when the thickness of the surface pattern conductor 6 exceeds 50 μm, the internal stress generated during baking increases, which may induce peeling of the surface pattern conductor 6. Here, the thickness of the surface pattern conductor 6 is, for example, the average thickness measured at 20 random locations on several SEM photographs of the cross section of the magnetic ceramic substrate 1, magnified several hundred to several thousand times. Furthermore, in order to reduce electrical loss, the volume resistivity of the surface pattern conductor 6 is preferably 6.5 μΩ·cm or less, and more preferably 5.5 μΩ·cm or less.

[0029] The metal conductor 3 may be any material as long as it can be fired at a temperature lower than the heat resistance temperature of the substrate 2 and satisfies the electrical conductivity required for the intended use of the magnetic ceramic substrate 1. Here, firing the metal conductor 3 at a temperature equal to or higher than the sintering temperature of the substrate 2 is not preferable because this may cause distortion in the substrate 2. Therefore, the firing temperature of the metal conductor 3 is preferably at least 300°C lower than the sintering temperature of the substrate 2, and more preferably at least 400°C lower than the sintering temperature of the substrate 2. Specific examples of such metal conductors 3 include Ag, Ag-Pd, and Cu. Among these, Ag, which has a relatively low volume resistivity, is preferred for the purpose of reducing loss as a conductor.

[0030] The glass contained in the surface pattern conductor 6 of the magnetic ceramic substrate 1 according to the first embodiment is preferably amorphous glass 4. After being melted once during firing of the surface pattern conductor 6, the amorphous glass 4 maintains its amorphous state and does not crystallize even when solidified again. Therefore, the amorphous glass 4 is likely to fully exert its effect as a binder that improves the adhesion between the surface pattern conductor 6 and the substrate 2. Specific examples of the amorphous glass 4 include zinc-based glass, silica-based glass, bismuth-based glass, and borosilicate glass, and these may be used alone or in combination of two or more. Regarding the melting temperature of the amorphous glass 4, when the softening point of the amorphous glass 4 is taken as the melting initiation temperature, it is preferable that the relationship between the softening point of the amorphous glass 4 and the sintering temperature of the metal conductor 3 satisfies the following: In other words, when the softening point of the amorphous glass 4 is set to T sof , the sintering temperature of the metal conductor 3 constituting the surface layer pattern conductor 6 is T sin When 100°C≦T sin -T sof It is preferable that T is ≦300°C. sin -T sofWhen the temperature is less than 100°C, the sintering temperature of the metal conductor 3 and the softening temperature of the amorphous glass 4 are too close, so the metal conductor 3 sinters, and after the metal conductor 3 is densely sintered, the amorphous glass 4 melts. Therefore, the dense metal conductor 3 acts as a lid, making it difficult for gas components such as water vapor contained in the amorphous glass 4 to escape. As a result, internal defects such as voids and bulges may occur in the surface pattern conductor 6. On the other hand, when the temperature is less than 100°C, the sintering temperature of the metal conductor 3 is too close to the softening temperature of the amorphous glass 4. Therefore, the dense metal conductor 3 acts as a lid, making it difficult for gas components such as water vapor contained in the amorphous glass 4 to escape. sin -T sof If the temperature exceeds 300°C, the amorphous glass 4 will be heated at a temperature excessively higher than the softening point of the amorphous glass 4. As a result, the viscosity of the molten amorphous glass 4 becomes excessively low, which may cause the amorphous glass 4 to float on the surface of the surface pattern conductor 6 and reduce plating adhesion on the surface of the surface pattern conductor 6. This makes it difficult to stably improve adhesion and plating adhesion. From the viewpoint of improving adhesion at the interface between the surface pattern conductor 6 and the substrate 2, the dispersion state of the amorphous glass 4 within the surface pattern conductor 6 should not be such that the amorphous glass 4 is unevenly dispersed near the surface other than the interface, thereby leaving only a very small amount of amorphous glass 4 contributing to adhesion at the interface. Therefore, the amorphous glass 4 may be uniformly dispersed throughout the surface pattern conductor 6 or unevenly dispersed near the interface between the substrate 2 and the surface pattern conductor 6.

[0031] As shown in FIG. 7 , the magnetic ceramic substrate 1 according to the first embodiment preferably includes a glass layer 9 having a thermal expansion coefficient of 5 ppm / K or more and 10 ppm / K or less on a portion of the surface of the substrate 2 and on the entire periphery of the end of the surface pattern conductor 6 in a plan view. The glass layer 9 is provided so as to press the end of the surface pattern conductor 6 against the surface of the substrate 2 in a plan view. The end of the surface pattern conductor 6 includes the side of the surface pattern conductor 6 and the area surrounding the side of the surface pattern conductor 6. The side of the surface pattern conductor 6 is the surface of the surface pattern conductor 6 excluding the surface in contact with the substrate 2 and the surface opposite to the surface in contact with the substrate 2. Specifically, the portion of the surface of the substrate 2 is the area of ​​the surface of the substrate 2 located outside the end of the surface pattern conductor 6 in a plan view. It is preferable that a portion of the glass layer 9 is impregnated into a void portion present at the end of the surface pattern conductor 6 in a plan view. The void portion present at the end corresponds to some of the multiple voids 5 present at the end. By providing the glass layer 9 having such a configuration, the glass layer 9 has the effect of physically pressing down the ends of the surface pattern conductor 6, thereby further improving the adhesion between the substrate 2 and the surface pattern conductor 6. In particular, the ends of the surface pattern conductor 6 tend to be thinner than the central portion of the surface pattern conductor 6, and tend to contain less amorphous glass 4. Therefore, by having the glass layer 9 physically press down the entire periphery of the ends of the surface pattern conductor 6, a more effective effect of improving adhesion can be obtained.

[0032] The surface pattern conductor 6 of the magnetic ceramic substrate 1 of the first embodiment may have a two-layer structure, as shown in Fig. 8, by further forming a second layer of surface pattern conductor 10 on the surface of a first layer of surface pattern conductor formed on the surface of the base material 2. The second layer of surface pattern conductor 10 does not contain glass. Since the second layer of surface pattern conductor 10 does not contain glass, plating adhesion on the surface of the surface pattern conductor 6 is further improved.

[0033] The magnetic ceramic substrate 1 in the first embodiment having the above-described configuration is a magnetic ceramic substrate that has excellent adhesion to the surface layer pattern conductors 6 .

[0034] ***Description of Manufacturing Method*** An example of the manufacturing process of the magnetic ceramic substrate 1 will be described. The manufacturing method of the magnetic ceramic substrate 1 corresponds to a substrate manufacturing method. First, a block of sintered ferrite is cut to a desired size and thickness to produce a base material 2 made of ferrite. The method for cutting the block is not particularly limited, and may be a method using a blade cutting machine, a wire processing machine, an electric discharge machine, a laser processing machine, or an NC (Numerical Control) processing machine.

[0035] Next, it is preferable to mirror-polish the surface of the cut substrate 2. The mirror-polishing is performed at least on the surface of the substrate 2 on which the conductive paste is thick-film printed, and specifically, it is performed on one or both sides of the substrate 2. When mirror-polishing both sides, one side may be processed at a time, or both sides may be processed simultaneously.

[0036] Next, a conductor paste is thick-film printed on the surface of the substrate 2. The conductor paste used for thick-film printing preferably contains coarse Ag particles having a particle size of 5 μm to 15 μm, fine Ag particles having a particle size of 1 μm to 3 μm, and amorphous glass powder. The firing shrinkage rate of the conductor paste is preferably 5% or less. The amount of amorphous glass powder in the conductor paste is preferably 3 vol% to 12 vol% relative to the amount of inorganic solids. The printing machine used for thick-film printing is not particularly limited and may be a manual printing machine or an automatic printing machine. Note that, from the viewpoint of maintaining constant printing and printing speed, it is preferable to use an automatic printing machine. A screen mask or a metal mask can be used as a mask for thick-film printing. When printing a conductor pattern with a more complex shape, it is preferable to use a screen mask. After thick-film printing, the conductor paste is dried using a thermostatic oven to remove the solvent components from the conductor paste. In this case, the drying temperature may be adjusted appropriately depending on the boiling point of the solvent component contained in the conductor paste, and is generally in the range of 80°C to 200°C.

[0037] Next, the dried conductor paste is baked onto the substrate 2 on which the conductor paste has been thick-film printed. The device used for baking is not particularly limited, and may be a box-type baking furnace, a tubular baking furnace, or a belt-conveying baking furnace. The baking temperature may be adjusted appropriately depending on the type of metal conductor used, and is generally about 600°C to 1000°C. By baking the conductor paste onto the substrate 2, the magnetic ceramic substrate 1 is completed.

[0038] The magnetic ceramic substrate 1 manufactured as described above is a magnetic ceramic substrate that has excellent adhesion of the surface layer pattern conductors 6 and excellent plating adhesion.

[0039] Next, a method for manufacturing the magnetic ceramic substrate 1 shown in FIG. 7 will be described. In this manufacturing method, the steps up to the step of drying the conductor paste are as described above. Therefore, the steps after the step of drying the conductor paste will be described. First, a glass paste containing glass powder having a thermal expansion coefficient of 5 ppm / K or more and 10 ppm / K or less is thick-film printed on a portion of the surface of the substrate 2 and on the entire periphery of the end, in a plan view, of the conductor paste that has been thick-film printed and dried on the surface of the substrate 2. Next, the thick-film printed glass paste is dried. Next, the dried glass paste and the dried conductor paste are baked onto the surface of the substrate 2 by co-firing.

[0040] ***Description of the effects of embodiment 1*** As described above, according to this embodiment, it is possible to provide a magnetic ceramic substrate 1 having excellent adhesion to the surface pattern conductor 6 and excellent plating adhesion, and a method for manufacturing the same.

[0041] Second Embodiment The following mainly describes the differences from the above-described embodiment with reference to the drawings.

[0042] ***Description of Configuration*** The following mainly describes the differences from the above-described embodiments with reference to the drawings. Embodiment 2 relates to a circulator 17 including the magnetic ceramic substrate 1 according to Embodiment 1.

[0043] Fig. 9 shows a specific example of a schematic cross-sectional view of a circulator 17 according to embodiment 2. As shown in Fig. 9, in the circulator 17, a permanent magnet 12 is mounted via a spacer 11 on the surface of the surface pattern conductor 6 of the magnetic ceramic substrate 1 according to embodiment 1. Furthermore, in the circulator 17, a through-hole conductor 13a and a through-hole conductor 13b are formed in the magnetic ceramic substrate 1. Furthermore, in the circulator 17, the surface pattern conductor 6 is electrically connected to an input / output terminal 14a by the through-hole conductor 13a, and the surface pattern conductor 6 is electrically connected to an input / output terminal 14b by the through-hole conductor 13b. Furthermore, the magnetic ceramic substrate 1 includes a ground conductor 15.

[0044] The type of permanent magnet 12 is not particularly limited and may be a metal magnet such as a neodymium-iron-boron, samarium-cobalt, alnico, or iron-chromium-cobalt magnet, or may be a ceramic magnet such as hexagonal ferrite. The surface pattern conductor 6 may be electrically connected to the input / output terminals 14a and 14b via side conductors 16a and 16b formed on the side surfaces of the magnetic ceramic substrate 1, as shown in FIG. 10 , in addition to a method of connecting via through-hole conductors. The "through-hole conductor" is a general term for the through-hole conductors 13a and 13b. The method of mounting the permanent magnet 12 and the method of forming the through-hole conductors are not particularly limited and may be any method known in the technical field.

[0045] ***Explanation of the Effects of Embodiment 2*** As described above, according to embodiment 2, it is possible to provide a circulator 17 that has excellent adhesion between the surface pattern conductor 6 and the substrate 2 and also has excellent mounting reliability.

[0046] The magnetic ceramic substrate 1 according to the present disclosure will be described below using examples and comparative examples. Fig. 11 is a table showing an overview of the examples and comparative examples. In Fig. 11, one table is divided into two.

[0047] [Example 1] Garnet-type ferrite (Y3 Fe 5 O 12 A magnetic ceramic substrate was produced by cutting a block of the magnetic ceramic substrate to a thickness of 1 mm using a grinding wheel cutter. Next, an Ag paste containing 60 vol% Ag powder with an average particle size of 13 μm, 34 vol% Ag powder with an average particle size of 2 μm, and 6 vol% borosilicate amorphous glass with a softening point 300°C lower than the sintering temperature of Ag was screen-printed onto the surface of the magnetic ceramic substrate using an automatic printing machine. The solvent was then removed by drying for 20 minutes in a thermostatic oven at 120°C. Next, a baking process was performed using a belt-type electric furnace with a top temperature of 800°C and a speed of 60 minutes from loading to unloading, thereby obtaining a magnetic ceramic substrate 1 for evaluation. Here, "from loading to unloading" refers to the period from loading into the furnace to unloading from the furnace.

[0048] Example 2 A magnetic ceramic substrate 1 for evaluation was obtained in the same manner as in Example 1, except that the baking process was carried out at a top temperature of 850° C. and in a time period of 60 minutes from loading to unloading.

[0049] Example 3 A magnetic ceramic substrate 1 for evaluation was obtained in the same manner as in Example 1, except that the top temperature was set to 890° C. and the baking process was carried out in 60 minutes from loading to unloading.

[0050] [Example 4] A magnetic ceramic substrate 1 for evaluation was obtained in the same manner as in Example 1, except that an Ag paste containing 61.9 vol% of Ag powder having an average particle size of 13 μm, 35.1 vol% of Ag powder having an average particle size of 2 μm, and 3 vol% of amorphous glass was used, the top temperature was set to 840°C, and the baking process was carried out at a rate of 60 minutes from loading to unloading.

[0051] [Example 5] A magnetic ceramic substrate 1 for evaluation was obtained in the same manner as in Example 1, except that an Ag paste containing 58.7 vol% of Ag powder having an average particle size of 13 μm, 33.3 vol% of Ag powder having an average particle size of 2 μm, and 8 vol% of amorphous glass was used, the top temperature was set to 840°C, and the baking process was carried out at a rate of 60 minutes from loading to unloading.

[0052] [Example 6] A magnetic ceramic substrate 1 for evaluation was obtained in the same manner as in Example 1, except that an Ag paste containing 56.2 vol% of Ag powder having an average particle size of 13 μm, 31.8 vol% of Ag powder having an average particle size of 2 μm, and 12 vol% of amorphous glass was used, the top temperature was set to 840°C, and the baking process was carried out at a rate of 60 minutes from loading to unloading.

[0053] [Example 7] A magnetic ceramic substrate 1 for evaluation was obtained in the same manner as in Example 1, except that spinel ferrite (Mn-Zn ferrite) with a thermal expansion coefficient of 11 ppm / K was used as the substrate 2, the top temperature was set to 840°C, and the baking process was carried out at a speed of 60 minutes from loading to unloading.

[0054] [Example 8] A magnetic ceramic substrate 1 for evaluation was obtained in the same manner as in Example 1, except that spinel ferrite (Mn-Zn ferrite) with a thermal expansion coefficient of 10.7 ppm / K was used as the substrate 2, the top temperature was set to 840°C, and the baking process was carried out at a speed of 60 minutes from loading to unloading.

[0055] [Example 9] A magnetic ceramic substrate 1 for evaluation was obtained in the same manner as in Example 1, except that spinel ferrite (Mn-Zn ferrite) with a thermal expansion coefficient of 10.6 ppm / K was used as the substrate 2, the top temperature was set to 840°C, and the baking process was carried out at a speed of 60 minutes from loading to unloading.

[0056] Example 10 A magnetic ceramic substrate 1 for evaluation was obtained in the same manner as in Example 1, except that the surface of the substrate 2 was mirror-polished for 30 minutes using a buffing machine.

[0057] Comparative Example 1 A magnetic ceramic substrate 1 for evaluation was obtained in the same manner as in Example 1, except that the baking process was carried out at a top temperature of 790° C. and in a time period of 60 minutes from loading to unloading.

[0058] Comparative Example 2 A magnetic ceramic substrate 1 for evaluation was obtained in the same manner as in Example 1, except that the baking process was carried out at a top temperature of 900° C. and in a time period of 60 minutes from loading to unloading.

[0059] [Comparative Example 3] A magnetic ceramic substrate 1 for evaluation was obtained in the same manner as in Example 1, except that an Ag paste containing 62.6 vol% of Ag powder having an average particle size of 13 μm, 35.4 vol% of Ag powder having an average particle size of 2 μm, and 2 vol% of amorphous glass was used, the top temperature was set to 840°C, and the baking process was carried out at a rate of 60 minutes from loading to unloading.

[0060] Comparative Example 4 A magnetic ceramic substrate 1 for evaluation was obtained in the same manner as in Example 1, except that an Ag paste containing 55.5 vol% of Ag powder having an average particle size of 13 μm, 31.5 vol% of Ag powder having an average particle size of 2 μm, and 13 vol% of amorphous glass was used, the top temperature was set to 840° C., and the baking process was carried out at a rate of 60 minutes from loading to unloading.

[0061] Comparative Example 5 A magnetic ceramic substrate 1 for evaluation was obtained in the same manner as in Example 1, except that an Ag paste containing 62.6 vol% of Ag powder having an average particle size of 13 μm, 35.4 vol% of Ag powder having an average particle size of 2 μm, and 2 vol% of amorphous glass was used, the top temperature was set to 900° C., and the baking process was carried out at a rate of 60 minutes from loading to unloading.

[0062] Comparative Example 6 A magnetic ceramic substrate 1 for evaluation was obtained in the same manner as in Example 1, except that an Ag paste containing 55.5 vol% of Ag powder having an average particle size of 13 μm, 31.5 vol% of Ag powder having an average particle size of 2 μm, and 13 vol% of amorphous glass was used, the top temperature was set to 900° C., and the baking process was carried out at a rate of 60 minutes from loading to unloading.

[0063] The adhesion of the surface pattern conductor 6 was evaluated for the magnetic ceramic substrates 1 obtained in the above examples and comparative examples. The adhesion evaluation was performed using the Cycas method, in which a diamond blade was inserted horizontally into the interface between the surface pattern conductor 6 and the substrate 2 and the resistance force when cutting into the interface was measured. In Figure 11, the adhesion evaluation results are shown as relative values, with the Cycas strength value in Example 1 set to 1. Furthermore, the plating adhesion was evaluated by visually observing the plating adhesion state when acidic electroless Ni plating was applied to the magnetic ceramic substrate 1. In the evaluation results shown in Figure 11, "◯" indicates that the plating was uniformly adhered to the entire surface of the surface pattern conductor 6, and "×" indicates that there were noticeable areas on the surface of the surface pattern conductor 6 where the plating was not adhered.

[0064] As shown in Table 1, the apparent density of the surface pattern conductor is 7.3 g / cm 3 9g / cm or more 3 The magnetic ceramic substrates 1 in each of Examples 1 to 10, in which the amorphous glass content was 3 vol% or more and 12 vol% or less, had a relatively large relative value of CYCUS strength and improved adhesion of the surface pattern conductors 6. Furthermore, plating adhesion was also good. In particular, Examples 7 and 8, in which the difference in thermal expansion coefficient between the substrate 2 and the surface pattern conductors 6 was 8.2 ppm / K or less, showed improved adhesion due to reduced thermal stress generated at the interface. Furthermore, when comparing samples with the same difference in thermal expansion coefficient, Example 10, in which the surface of the substrate 2 was mirror-polished, showed improved adhesion compared to Examples 1, 3, and 5, which were not mirror-polished. Meanwhile, the apparent density of the surface pattern conductors 6 was 7.2 g / cm3. 3 and 9.1 g / cm 3In Comparative Examples 1 and 2, where the amorphous glass content was 2 vol%, adhesion was significantly low. Furthermore, in Comparative Example 3, where the amorphous glass content was 2 vol%, adhesion was not improved because the content of glass as a binder was too low. Conversely, in Comparative Example 4, where the amorphous glass content was 13 vol%, adhesion was good, but glass lifting on the surface of the surface pattern conductor 6 increased, resulting in poor plating adhesion. Furthermore, in Comparative Example 5, where the amorphous glass content was 2 vol% and the apparent density of the surface pattern conductor 6 was 9.1 g / cm3, adhesion was significantly low. Furthermore, in Comparative Example 6, where the amorphous glass content was 13 vol% and the apparent density of the surface pattern conductor 6 was 9.1 g / cm3, adhesion was low and plating adhesion was also poor.

[0065] As can be seen from the above results, the present disclosure can provide a magnetic ceramic substrate 1 that has excellent adhesion of the surface layer pattern conductor 6 and excellent plating adhesion on the surface of the surface layer pattern conductor 6.

[0066] ***Other Embodiments*** The above-described embodiments can be freely combined, or any of the components of each embodiment can be modified, or any of the components can be omitted from each embodiment. Furthermore, the embodiments are not limited to those shown in Embodiments 1 and 2, and various modifications are possible as needed.

[0067] REFERENCE SIGNS LIST 1 magnetic ceramic substrate, 2 base material, 3 metal conductor, 4 amorphous glass, 5 voids, 6 surface pattern conductor, 7 protrusions, 8 microcracks, 9 glass layer, 10 second layer surface pattern conductor, 11 spacer, 12 permanent magnet, 13a, 13b through-hole conductors, 14a, 14b input / output terminals, 15 ground conductor, 16a, 16b side conductors, 17 circulator.

Claims

1. A ceramic substrate having a base material made of ferrite, containing a metal conductor made of Ag and 3 vol% to 12 vol% of amorphous glass, and having an apparent density of 7.3 g / cm 3 9.0g / cm or more 3 A magnetic ceramic substrate comprising a surface layer pattern conductor on the surface of the base material, the surface layer pattern conductor being as follows:

2. A magnetic ceramic substrate as described in claim 1, wherein the surface pattern conductor has a plurality of voids therein, each of which is a three-dimensional region not filled with the metal conductor, at least a portion of the plurality of voids is filled with the amorphous glass, and the difference in thermal expansion coefficient between the base material and the surface pattern conductor is 8.2 ppm / K or less.

3. A magnetic ceramic substrate according to claim 1 or 2, wherein the arithmetic mean roughness of the surface of the base material which is in contact with the surface pattern conductor is 0.01 μm or more and 0.5 μm or less.

4. A magnetic ceramic substrate according to any one of claims 1 to 3, wherein the surface pattern conductor is formed by firing a conductor paste containing coarse Ag particles having a particle size of 5 μm or more and 15 μm or less, fine Ag particles having a particle size of 1 μm or more and 3 μm or less, and amorphous glass powder made of the amorphous glass, and the firing shrinkage rate of the conductor paste is 5% or less.

5. The magnetic ceramic substrate further comprises a glass layer having a thermal expansion coefficient of 5 ppm / K or more and 10 ppm / K or less on a portion of the surface of the base material that is in contact with the surface pattern conductor and on the entire circumference of the end of the surface pattern conductor in a planar view, the glass layer being arranged so as to physically press the end of the surface pattern conductor in a planar view against the surface of the base material that is in contact with the surface pattern conductor, and a portion of the glass layer being impregnated into some of a plurality of voids present at the end. A magnetic ceramic substrate as described in any one of claims 1 to 4.

6. A magnetic ceramic substrate according to any one of claims 1 to 5, wherein the surface layer pattern conductor has a volume resistivity of 6.5 µΩ·cm or less.

7. A magnetic ceramic substrate according to any one of claims 1 to 6, wherein the ferrite is a garnet-type ferrite.

8. A circulator comprising a magnetic ceramic substrate according to any one of claims 1 to 7.

9. A method for manufacturing a magnetic ceramic substrate, comprising: mirror-polishing the surface of a base material made of ferrite; thick-film printing onto the surface of a conductor paste containing coarse Ag particles having a particle size of 5 μm or more and 15 μm or less, fine Ag particles having a particle size of 1 μm or more and 3 μm or less, and amorphous glass powder having a content of 3 vol% to 12 vol% based on the amount of inorganic solids; drying the thick-film printed conductor paste; and baking the dried conductor paste onto the surface, thereby manufacturing a magnetic ceramic substrate.

10. A method for manufacturing a substrate as described in claim 9, comprising thick-film printing a glass paste containing glass powder having a thermal expansion coefficient of 5 ppm / K or more and 10 ppm / K or less on a portion of the surface and on the entire circumference of the end, in a planar view, of a conductor paste that has been thick-film printed on the surface and dried, drying the thick-film printed glass paste, and baking the dried glass paste and the dried conductor paste onto the surface by simultaneously firing them.

Citation Information

Patent Citations

  • Production of multi-layer ceramic part and multi-layer ceramic part produced thereby

    JP1995082041A

  • Non-linear dielectric element

    JP1999214257A

  • Circuit board

    JP2002076639A

  • Circuit board, production method therefor and electronic device

    JP2003101181A

  • Conductive paste for forming conductive section for ferrite multilayer circuit board and ferrite multilayer circuit board using conductive paste

    JP2006108399A

Cited By

  • Magnetic ceramic substrate, circulator, and method for manufacturing magnetic ceramic substrate

    WO2026216121A1