Solid electrolyte membrane and all-solid-state battery comprising same
The use of a solid electrolyte membrane with first and second particles of varying Young's moduli and sizes in specific ratios addresses the resistance issues in all-solid-state batteries, enhancing their performance and longevity.
Patent Information
- Application Number
- PCT/KR2024/004927
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-16
- Filing Date
- 2024-04-12
- Publication Date
- 2024-11-21
AI Technical Summary
All-solid-state batteries face performance degradation due to high resistance at the interfaces between the anode, cathode, and solid electrolyte membrane, which affects their lifespan and rate characteristics.
A solid electrolyte membrane comprising first and second solid electrolyte particles with different Young's moduli, mixed in specific weight ratios and particle sizes, is used to minimize interfacial resistance and enhance bonding between the electrodes and the membrane.
The solution improves the lifespan and rate characteristics of all-solid-state batteries by reducing interfacial resistance and maintaining the membrane's structural integrity during charging and discharging.
Smart Images

Figure KR2024004927_21112024_PF_FP_ABST
Abstract
Description
Solid electrolyte membrane and all-solid-state battery containing the same
[0001] This application claims the benefit of priority to Korean Patent Application No. 10-2023-0063088, filed May 16, 2023, the entire disclosure of which is incorporated herein by reference.
[0002] The present invention relates to a solid electrolyte membrane and an all-solid-state battery including the same.
[0003]
[0004] Various batteries are being studied to overcome the limitations of current lithium secondary batteries in terms of battery capacity, safety, output, large-scale development, and miniaturization.
[0005] Representative examples include metal-air batteries with much larger theoretical capacity than lithium secondary batteries, all-solid-state batteries with no risk of explosion in terms of safety, supercapacitors for output, NaS batteries or RFBs (redox flow batteries) for large-scale applications, and thin film batteries for miniaturization, all of which are being continuously researched in academia and industry.
[0006] All-solid-state batteries replace the liquid electrolytes used in conventional lithium secondary batteries with solid electrolytes. Because they do not use flammable solvents, they eliminate the risk of fire or explosion caused by decomposition reactions of conventional electrolytes, significantly improving safety. Furthermore, because lithium metal or lithium alloys can be used as anode materials, they offer the advantage of dramatically improving the battery's energy density relative to its mass and volume.
[0007] All-solid-state batteries are manufactured by inserting a solid electrolyte membrane between the positive and negative electrodes and then performing high-pressure pressing. Lithium ions (Li) are formed at the interface between the positive electrode and the solid electrolyte membrane and the interface between the negative electrode and the solid electrolyte membrane. + ) can improve the performance of the all-solid-state battery. However, if the hardness of the solid electrolyte membrane is high, resistance to the movement of lithium ions occurs significantly at the interface between the positive electrode and the solid electrolyte membrane, and at the interface between the negative electrode and the solid electrolyte membrane, which can deteriorate the performance of the all-solid-state battery.
[0008] Therefore, there is a need for research to improve the performance of all-solid-state batteries by minimizing the resistance occurring at the interface between the positive electrode and the solid electrolyte membrane and the interface between the negative electrode and the solid electrolyte membrane.
[0009]
[0010] [Previous literature]
[0011] [Patent Document]
[0012] Republic of Korea Publication Patent No. 10-2021-0087919
[0013]
[0014] The present inventors have completed the present invention by confirming that a solid electrolyte membrane includes first solid electrolyte particles and second solid electrolyte particles, and that by controlling the Young's modulus, average particle size, and weight ratio of the first solid electrolyte particles and the second solid electrolyte particles, the interface bonding strength between the positive electrode and the solid electrolyte membrane and the interface bonding strength between the negative electrode and the solid electrolyte membrane can be improved, thereby minimizing the resistance occurring at the interface.
[0015] Accordingly, the present invention aims to provide a solid electrolyte membrane for an all-solid-state battery that can reduce resistance occurring at the interface between a positive electrode and a solid electrolyte membrane and at the interface between a negative electrode and a solid electrolyte membrane in an all-solid-state battery.
[0016] In addition, the present invention aims to provide an all-solid-state battery having excellent life characteristics and rate characteristics by including the solid electrolyte membrane.
[0017]
[0018] To achieve the above purpose,
[0019] The present invention relates to a solid electrolyte membrane for an all-solid-state battery comprising first solid electrolyte particles and second solid electrolyte particles,
[0020] The Young's modulus of the first solid electrolyte particle is higher than the Young's modulus of the second solid electrolyte particle,
[0021] The average particle size (D50) of the first solid electrolyte particles and the second solid electrolyte particles is 1 to 5 μm,
[0022] A solid electrolyte membrane for an all-solid-state battery is provided, wherein the first solid electrolyte particles and the second solid electrolyte particles are mixed in a weight ratio of 7:3 to less than 2:8.
[0023] In addition, the present invention provides an all-solid-state battery including a positive electrode, a negative electrode, and a solid electrolyte membrane interposed therebetween,
[0024] The above solid electrolyte membrane provides an all-solid-state battery, which is the solid electrolyte membrane of the present invention.
[0025]
[0026] The solid electrolyte membrane for an all-solid-state battery of the present invention comprises first solid electrolyte particles and second solid electrolyte particles, and by controlling the Young's modulus, average particle size and weight ratio of the first solid electrolyte particles and the second solid electrolyte particles, the interface bonding force between the positive electrode and the solid electrolyte membrane and the interface bonding force between the negative electrode and the solid electrolyte membrane can be improved, thereby minimizing the resistance occurring at the interface.
[0027] Therefore, an all-solid-state battery including the solid electrolyte membrane of the present invention can have excellent life characteristics and rate characteristics.
[0028]
[0029] Figure 1 is a life characteristic measurement graph of Example 1, Comparative Example 1, and Comparative Example 2.
[0030] Figure 2 is a life characteristic measurement graph of Comparative Example 4.
[0031] Figure 3 is a graph showing the rate characteristic measurements of Example 1, Comparative Example 2, and Comparative Example 3.
[0032]
[0033] Hereinafter, the present invention will be described in more detail.
[0034]
[0035] Terms or words used in this specification and claims should not be interpreted as limited to their usual or dictionary meanings, but should be interpreted as meanings and concepts that conform to the technical idea of the present invention, based on the principle that the inventor can appropriately define the concept of the term to explain his or her own invention in the best way.
[0036] The terminology used in the present invention is only used to describe specific embodiments and is not intended to limit the present invention. The singular expression includes the plural expression unless the context clearly indicates otherwise. In the present invention, it should be understood that the terms "comprise" or "have" are intended to specify the presence of a feature, number, step, operation, component, part, or combination thereof described in the specification, but do not exclude in advance the possibility of the presence or addition of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.
[0037]
[0038] Solid electrolyte membrane for all-solid-state batteries
[0039] The present invention relates to a solid electrolyte membrane for an all-solid-state battery,
[0040] The above solid electrolyte membrane includes first solid electrolyte particles and second solid electrolyte particles,
[0041] The Young's modulus of the first solid electrolyte particle is higher than the Young's modulus of the second solid electrolyte particle,
[0042] The average particle size (D50) of the first solid electrolyte particles and the second solid electrolyte particles is 1 to 5 μm,
[0043] The first solid electrolyte particles and the second solid electrolyte particles may be mixed in a weight ratio of 7:3 to less than 2:8.
[0044]
[0045] The solid electrolyte membrane for an all-solid-state battery of the present invention comprises first solid electrolyte particles and second solid electrolyte particles. The Young's modulus of the first solid electrolyte particles and the second solid electrolyte particles are different from each other, and the Young's modulus of the first solid electrolyte particles may be higher than the Young's modulus of the second solid electrolyte particles. By including heterogeneous solid electrolyte particles having different Young's moduli, the Young's modulus of the solid electrolyte membrane can be controlled. Therefore, the resistance occurring at the interface between the positive electrode and the solid electrolyte membrane of the all-solid-state battery and the interface between the negative electrode and the solid electrolyte membrane can be reduced, and accordingly, an all-solid-state battery with improved cycle life characteristics and rate characteristics can be provided.
[0046] The Young's modulus of the first solid electrolyte particles may be 40 to 80 GPa, preferably 40 to 60 GPa, and most preferably 40 to 50 GPa. Generally, the higher the Young's modulus of the particles, the harder the particles are and the less likely they are to break. Since the first solid electrolyte particles have a Young's modulus within the above range, the shape of the solid electrolyte membrane can be maintained even when volume changes occur during charging and discharging of the all-solid-state battery.
[0047] In addition, the Young's modulus of the second solid electrolyte particles may be 5 to 30 GPa, preferably 10 to 25 GPa, and most preferably 15 to 20 GPa. Since the second solid electrolyte particles have a Young's modulus within the above range, they can easily undergo shape deformation at high pressure, thereby enabling excellent bonding between the solid electrolyte membrane and the electrode. In addition, the second solid electrolyte particles may be positioned between the first solid electrolyte particles to minimize pores, thereby facilitating lithium ion movement and enhancing the interfacial bonding force between the solid electrolyte membrane and the electrode.
[0048] The difference in Young's modulus between the first solid electrolyte particles and the second solid electrolyte particles may be 15 to 50 GPa, and preferably 20 to 40 GPa. When the difference in Young's modulus is less than 15 GPa, the Young's modulus of the first solid electrolyte particles may be low, or the Young's modulus of the second solid electrolyte particles may be high. When the Young's modulus of the first solid electrolyte particles is low and the difference in Young's modulus is less than 15 GPa, the physical rigidity of the solid electrolyte membrane may decrease, and when the Young's modulus of the second solid electrolyte particles is high, the effect of improving the interfacial bonding between the solid electrolyte membrane and the electrode cannot be expected. In addition, when it exceeds 40 GPa, the Young's modulus of the first solid electrolyte particles increases, which may reduce the interfacial bonding force between the solid electrolyte membrane and the electrode, thereby reducing the interfacial resistance.
[0049] In addition, the average particle size (D50) of the first solid electrolyte particles and the second solid electrolyte particles may be the same, and may be 1 to 5 μm, preferably 2 to 3 μm. If the average particle size (D50) of the first solid electrolyte particles and the second solid electrolyte particles is less than 1 μm, the first solid electrolyte particles and the second solid electrolyte particles may not be easily dispersed during the manufacture of the solid electrolyte membrane, and thus an uneven surface may be manufactured as a solid electrolyte membrane. Accordingly, a problem of deterioration in the performance of an all-solid-state battery including the same may occur. In addition, since the first solid electrolyte particles and the second solid electrolyte particles have an average particle size within the above range, they are easily dispersed during a slurry process in the manufacture of the solid electrolyte membrane, and thus an electrolyte membrane having a uniform surface may be manufactured.
[0050] The first solid electrolyte particles and the second solid electrolyte particles may be mixed in a weight ratio of 7:3 to less than 2:8, preferably 6:4 to 4:6, and most preferably 5:5. If the content of the first solid electrolyte particles exceeds the above range, the Young's modulus of the solid electrolyte membrane may become excessively high, thereby lowering the interfacial bonding force between the solid electrolyte membrane and the electrode, thereby deteriorating the life characteristics of an all-solid-state battery including the same. On the other hand, if the content of the first solid electrolyte particles is less than the above range, the ionic conductivity of the solid electrolyte membrane may decrease, thereby increasing the resistance, and the life characteristics and rate characteristics of an all-solid-state battery including the same may deteriorate.
[0051] In the present invention, the Young's modulus of the solid electrolyte membrane may be 20 to 40 GPa, preferably 25 to 35 GPa. The solid electrolyte membrane of the present invention comprises the first solid electrolyte particles and the second solid electrolyte particles, wherein the Young's modulus of the first solid electrolyte particles is higher than that of the second solid electrolyte particles, and the average particle size (D50) of the first solid electrolyte particles and the second solid electrolyte particles is 1 to 5 μm, and the first solid electrolyte particles and the second solid electrolyte particles are mixed in a weight ratio of 7:3 to less than 2:8. The second solid electrolyte particles have a low Young's modulus and thus are soft, and the second solid electrolyte particles are positioned between the first solid electrolyte particles to minimize the space formed between the first solid electrolyte particles, i.e., pores, thereby improving the interfacial bonding force between the solid electrolyte membrane and the electrode, thereby reducing the resistance to lithium ion movement. That is, the interfacial resistance occurring at the interface between the solid electrolyte membrane and the electrode can be reduced. Accordingly, the life and rate characteristics of the all-solid-state battery including it can be improved.
[0052] Even if a solid electrolyte membrane containing one type of solid electrolyte has the same Young's modulus as that of the present invention, the space formed between solid electrolyte particles cannot be minimized, and thus the effect of reducing interfacial resistance cannot be obtained.
[0053]
[0054] The first solid electrolyte particles and the second solid electrolyte particles may be at least one selected from the group consisting of a sulfide-based solid electrolyte, a polymer-based solid electrolyte, and an oxide-based solid electrolyte, and preferably may be a sulfide-based solid electrolyte.
[0055] Additionally, the first solid electrolyte particles and the second solid electrolyte particles may be identical to each other, but may have different Young's moduli.
[0056] The above sulfide-based solid electrolyte contains sulfur (S) and has the ionic conductivity of a metal belonging to Group 1 or Group 2 of the periodic table, and may include Li-PS-based glass or Li-PS-based glass ceramic.
[0057] Specifically, the sulfide-based solid electrolyte may include at least one selected from the group consisting of Li6PS5Cl, Li6PS5Br, Li6PS5I, Li2S-P2S5, Li2S-LiI-P2S5, Li2S-LiI-Li2O-P2S5, Li2S-LiBr-P2S5, Li2S-Li2O-P2S5, Li2S-Li3PO4-P2S5, Li2S-P2S5-P2S5, Li2S-P2S5-SiS2, Li2S-P2S5-SnS, Li2S-P2S5-Al2S3, Li2S-GeS2, and Li2S-GeS2-ZnS, and preferably may include at least one selected from the group consisting of Li6PS5Cl, Li6PS5Br, and Li6PS5I. The above Li6PS5Cl, Li6PS5Br, and Li6PS5I may be argyrodite type solid electrolytes. In addition, the sulfide-based solid electrolyte may be in a form doped with trace elements, for example, Li6PS5Cl may be additionally doped with bromine (Br).
[0058] The above polymer-based solid electrolyte is a polymer electrolyte material formed by adding a polymer resin to a composite of a lithium salt and a polymer resin, that is, a solvated lithium salt, and is about 1x10 -7 S / cm or more, preferably about 1x10 -5 It can exhibit ionic conductivity of S / cm or more.
[0059] Non-limiting examples of the polymer resin include polyether polymers, polycarbonate polymers, acrylate polymers, polysiloxane polymers, phosphazene polymers, polyethylene derivatives, alkylene oxide derivatives such as polyethylene oxide, phosphate ester polymers, polyagitation lysine, polyester sulfide, polyvinyl alcohol, polyvinylidene fluoride, polymers containing ionic dissociation groups, etc., and may include one or more of these. In addition, the polymer electrolyte may include, as a polymer resin, a branched copolymer in which an amorphous polymer such as PMMA, polycarbonate, polysiloxane (PDMS) and / or phosphazene is copolymerized as a comonomer in a polyethylene oxide (PEO) main chain, a comb-like polymer, and a cross-linked polymer resin, and may include one or more of these.
[0060] In the above polymer solid electrolyte, the above-mentioned lithium salt is an ionizable lithium salt, Li + X - It can be expressed as . There is no particular limitation on the anion of these lithium salts, but F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , PF6 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH- , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - , (CF3CF2SO2)2N - Examples include:
[0061] The above oxide-based solid electrolyte may contain oxygen (O) and have the ionic conductivity of a metal belonging to Group 1 or Group 2 of the periodic table. For example, an LLTO-based compound, Li6La2CaTa2O 12 , Li6La2ANb2O 12 (A is Ca or Sr), Li2Nd3TeSbO 12 , Li3BO 2.5 N 0.5 , Li9SiAlO8, LAGP compounds, LATP compounds, Li1 +x Ti 2-x Al x Si y (PO4) 3-y (where, 0≤x≤1, 0≤y≤1), LiAl x Zr 2-x (PO4)3(where, 0≤x≤1, 0≤y≤1), LiTi x Zr 2-x (PO4)3 (wherein, 0≤x≤1, 0≤y≤1), may include at least one selected from among LISICON compounds, LIPON compounds, perovskite compounds, NASICON compounds, and LLZO compounds.
[0062]
[0063] The above solid electrolyte membrane may additionally include a binder. The type of the binder is not particularly limited as long as it is one used in the art.
[0064] For example, acrylonitrile butadiene rubber (NBR), styrene butadiene rubber (SBR), butadiene rubber (BR), styrene-butadiene-styrene copolymer (SBS), polybutadiene (PAN), styrene-ethylene / butylene-styrene block copolymer (SEBS), silicone rubber (SR), hydrogenated nitrile butadiene rubber (HNBR), poly(ethylene vinyl acetate) (PEVA), poly(methyl methacrylate) (PMMA), polyisobutene (PIB), polyacrylate, etc. can be used, but are not limited thereto.
[0065] The binder may be included in an amount of 0.5 to 5 wt% based on the total weight of the solid electrolyte membrane. In addition, the combined weight of the first solid electrolyte and the second solid electrolyte may be included in an amount of 95 to 99.5 wt% based on the total weight of the solid electrolyte membrane. By including the solid electrolyte and the binder as described above, a solid electrolyte membrane for an all-solid-state battery that can be maintained in a film form while minimizing the content of the binder that acts as a resistance to ionic conductivity can be manufactured.
[0066]
[0067] The solid electrolyte membrane for an all-solid-state battery of the present invention can be manufactured by a method of dispersing the first solid electrolyte particles and the second solid electrolyte particles in a solvent to prepare a slurry, applying the slurry to one surface of a release film, drying the slurry, and then removing the release film. The slurry may additionally include a binder.
[0068] The first solid electrolyte particles, the second solid electrolyte particles, and the binder follow the above-described contents.
[0069] The solvent is not particularly limited in type as long as it can disperse the first solid electrolyte particles, the second solid electrolyte particles, and the binder, and examples thereof include xylene, hexane, benzene, anisole, isobutyl isobutyrate, toluene, and butyl butyrate.
[0070]
[0071] The ionic conductivity of the solid electrolyte membrane for the above all-solid-state battery may be 1 to 1.6 mS / cm. The ionic conductivity may be measured at room temperature (25°C).
[0072]
[0073] All-solid-state batteries
[0074] The present invention relates to an all-solid-state battery comprising a positive electrode, a negative electrode, and a solid electrolyte membrane interposed therebetween, wherein the solid electrolyte membrane may be the solid electrolyte membrane of the present invention described above.
[0075] The above all-solid-state battery is a lithium secondary battery, and there is no limitation on the positive or negative electrode, and it may be a lithium-air battery, a lithium oxide battery, a lithium-sulfur battery, or a lithium metal battery.
[0076]
[0077] The above positive electrode may include a positive electrode current collector and a positive electrode active material applied to one or both sides of the positive electrode current collector.
[0078] The above positive electrode current collector is intended to support the positive electrode active material, and is not particularly limited as long as it has excellent conductivity and is electrochemically stable in the voltage range of the lithium secondary battery. For example, the positive electrode current collector may be any one metal selected from the group consisting of copper, aluminum, stainless steel, titanium, silver, palladium, nickel, alloys thereof, and combinations thereof. The stainless steel may be surface-treated with carbon, nickel, titanium, or silver. As the alloy, an aluminum-cadmium alloy may be preferably used. In addition, calcined carbon, a non-conductive polymer surface-treated with a conductive material, or a conductive polymer may be used.
[0079] The above positive electrode current collector can form fine irregularities on its surface to strengthen the bonding strength with the positive electrode active material, and can be used in various forms such as a film, sheet, foil, mesh, net, porous body, foam, and non-woven fabric.
[0080] The above positive electrode active material may optionally include a conductive material and a binder.
[0081] The above positive electrode active material may vary depending on the type of all-solid-state battery. For example, the positive electrode active material may be a layered compound such as lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; chemical formula Li 1+x Mn 2-x Lithium manganese oxides such as O4(0≤x≤0.33), LiMnO3, LiMn2O3, LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, V2O5, Cu2V2O7; chemical formula LiNi 1-x M x Ni-site lithium nickel oxide represented by O2 (M = Co, Mn, Al, Cu, Fe, Mg, B or Ga; 0.01≤x≤0.3); chemical formula LiMn 2-x M xLithium manganese composite oxides expressed as O2 (M = Co, Ni, Fe, Cr, Zn or Ta; 0.01≤x≤0.1) or Li2Mn3MO8 (M = Fe, Co, Ni, Cu or Zn); LiNi x Mn 2-x Lithium manganese composite oxide with spinel structure represented by O4; LiCoPO4; LiFePO4; Elemental sulfur (S8); Li2S n (n=1), organosulfur compounds or carbon-sulfur polymers (C2S x ) n : It may include sulfur series compounds such as x=2.5 ~ 50, n=2), but is not limited to these.
[0082] The above conductive material is a material that electrically connects the electrolyte and the positive electrode active material and serves as a path for electrons to move from the current collector to the positive electrode active material. Any material that does not cause chemical changes in a lithium secondary battery and has porosity and conductivity can be used without restriction.
[0083] For example, the conductive material may be a porous carbonaceous material, such as carbon black, graphite, graphene, activated carbon, carbon fiber, etc.; metallic fibers such as metal mesh; metallic powders such as copper, silver, nickel, aluminum, etc.; or organic conductive materials such as polyphenylene derivatives. The conductive materials may be used alone or in combination.
[0084] Current commercially available products include acetylene black series (such as those from Chevron Chemical Company or Gulf Oil Company), Ketjen Black EC series (from Armak Company), Vulcan XC-72 (from Cabot Company), and Super P (from MMM). Examples include acetylene black, carbon black, and graphite.
[0085] In addition, the positive electrode may additionally include a binder, and the binder increases the bonding strength between the components constituting the positive electrode and between them and the current collector, and any binder known in the art may be used.
[0086] For example, the binder may be a fluororesin binder including polyvinylidene fluoride (PVdF) or polytetrafluoroethylene (PTFE); a rubber binder including styrene butadiene rubber (SBR), acrylonitrile-butidiene rubber, and styrene-isoprene rubber; a cellulose binder including carboxyl methyl cellulose (CMC), starch, hydroxy propyl cellulose, and regenerated cellulose; a polyalcohol binder; a polyolefin binder including polyethylene and polypropylene; a polyimide binder; a polyester binder; and a silane binder. One, two or more mixtures or copolymers selected from the group consisting of may be used.
[0087]
[0088] The above-mentioned negative electrode may include a negative electrode current collector and a negative electrode active material positioned on the negative electrode current collector. In addition, the negative electrode, like the positive electrode, may include a conductive material and a binder as needed. In this case, the negative electrode current collector, conductive material, and binder are as described above.
[0089] The above negative active material is lithium ion (Li + ) can be reversibly intercalated or deintercalated, or any material that can react with lithium ions to form a reversibly lithium-containing compound.
[0090] For example, the negative active material may be at least one carbon-based material selected from the group consisting of crystalline artificial graphite, crystalline natural graphite, amorphous hard carbon, low-crystalline soft carbon, carbon black, acetylene black, Ketjen black, Super-P, graphene, and fibrous carbon, Si-based material, Li x Fe2O3(0≤x≤1), Li x WO2(0≤x≤1), Sn x Me 1-x Me´ y O z (Me: Mn, Fe, Pb, Ge; Me´: Al, B, P, Si, elements of group 1, 2, and 3 of the periodic table, halogens; 0 <x≤1; 1≤y≤3; 1≤z≤8) 등의 금속 복합 산화물; 리튬 금속; 리튬 합금; 규소계 합금; 주석계 합금; SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, Bi2O5등의 금속 산화물; 폴리아세틸렌 등의 도전성 고분자; Li-Co-Ni 계 재료; 티타늄 산화물; 리튬 티타늄 산화물 등을 포함할 수 있지만, 이들만으로 한정되는 것은 아니다.
[0091] Additionally, the negative electrode may include a negative electrode current collector and a coating layer including metal-carbon composite particles positioned on the negative electrode current collector. This may mean an anodeless electrode that does not include a negative electrode active material.
[0092] The above negative electrode may be such that when the all-solid-state battery is charged, lithium ions pass through the coating layer to reach the surface of the negative electrode current collector, and these are deposited to form a lithium metal layer.
[0093] The above metal-carbon composite particles may have a form in which carbon particles and metal particles are attached to each other or one surface is coated with the other, and may be physically or chemically bonded.
[0094] The above carbon particles may include natural graphite, artificial graphite, hard carbon, soft carbon, carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, carbon nanotubes, fullerene, carbon fiber, and fluorocarbon.
[0095] The above metal particles are lithium-philic metals, for example, Ni, Cu, Ag, Au, Pt, Al, Zn, Bi, etc., and may be one or a combination of two or more thereof. By introducing a metal having the above lithium-philic properties, it is advantageous to form a stable and uniform lithium layer on the surface of the current collector.
[0096] The above negative electrode may be manufactured by mixing a binder solution and the composite particles to prepare a slurry for forming a coating layer, and then applying and drying the slurry on a negative electrode current collector. In this case, the binder may be a conventional binder used in the art.
[0097]
[0098] The manufacture of the above all-solid-state battery is not particularly limited in the present invention, and a known method can be used.
[0099] For example, a solid electrolyte membrane is placed between the positive and negative electrodes, and then compressed to assemble the cell. The assembled cell is then installed within an outer packaging material and sealed by heating and compression, etc. The outer packaging material may be a laminate pack made of aluminum, stainless steel, or a metal container such as a cylindrical or square shape.
[0100] For example, the positive and negative electrodes are manufactured through a slurry coating process in which a slurry composition containing each electrode active material, solvent, and binder is manufactured, coated, and then dried.
[0101] Methods for coating the electrode slurry on the current collector include a method of distributing the electrode slurry on the current collector and then uniformly dispersing it using a doctor blade or the like, die casting, comma coating, screen printing, etc. In addition, the electrode slurry may be formed on a separate substrate and then bonded to the current collector by pressing or lamination. At this time, the final coating thickness can be controlled by adjusting the concentration of the slurry solution or the number of coatings.
[0102] The drying process is a process of removing the solvent and moisture within the slurry to dry the slurry coated on the metal collector. This process may vary depending on the solvent used. For example, it is performed in a vacuum oven at 50 to 200°C. Examples of drying methods include drying using warm air, hot air, or low-humidity air, vacuum drying, and drying using irradiation with (far) infrared rays or electron beams. The drying time is not particularly limited, but is typically performed within the range of 30 seconds to 24 hours.
[0103] After the above drying process, a cooling process may be further included, and the cooling process may be slow cooling to room temperature so that the recrystallized structure of the binder is well formed.
[0104] Additionally, if necessary, after the drying process, a rolling process may be performed to compress the electrode to a desired thickness by passing it between two high-temperature heated rolls to increase the capacity density of the electrode and enhance the adhesion between the current collector and the active materials. The rolling process is not particularly limited in the present invention, and any known pressing process is possible. For example, it may be performed by passing it between rotating rolls or using a flat plate press.
[0105] The shape of the above-mentioned all-solid-state battery is not particularly limited, and can be made into various shapes such as cylindrical, laminated, and coin-shaped.
[0106]
[0107] Hereinafter, preferred examples are presented to help understand the present invention, but the following examples are only illustrative of the present invention, and it is obvious to those skilled in the art that various changes and modifications are possible within the scope and technical idea of the present invention, and it is also natural that such changes and modifications fall within the scope of the appended patent claims.
[0108]
[0109] <All-solid-state battery manufacturing>
[0110] Example 1.
[0111] Agirodite (Li6PS5Cl) with a Young's modulus of 42 GPa and an average particle size (D50) of 2.5 μm was used as the first solid electrolyte particle. Agirodite (Li6PS5Cl) with a Young's modulus of 18 GPa and an average particle size (D50) of 2.5 μm was used as the second solid electrolyte particle. Butadiene rubber was used as the binder.
[0112] A slurry was prepared by adding the first solid electrolyte particles, the second solid electrolyte particles, and a binder to a butyl butyrate solvent, and the weight ratio of the first solid electrolyte particles and the second solid electrolyte particles was 5:5. In addition, the weight ratio of the first solid electrolyte particles, the second solid electrolyte particles, and the binder was 49:49:2.
[0113] Polyethylene terephthalate was used as a release film, and slurry was coated on the release film using a bar coater. Afterwards, the film was dried at room temperature for 5 hours, and the release film was removed to manufacture a solid electrolyte membrane for an all-solid-state battery. The Young's modulus of the solid electrolyte membrane for an all-solid-state battery was 30 GPa.
[0114] A positive electrode was manufactured by mixing a positive electrode active material (NCM 811), a conductive agent (carbon fiber), a solid electrolyte (Li6PS5Cl), and a binder (polytetrafluoroethylene) in a weight ratio of 84:0.2:14.8:1, applying the mixture to a positive electrode current collector, and then rolling it.
[0115] A negative electrode was manufactured by applying a mixture of a negative electrode active material (carbon black) and a binder (polyvinylidene fluoride) to a thickness of 150 μm on a 10 μm thick SUS, which is a negative electrode collector.
[0116] An all-solid-state battery was manufactured by interposing the solid electrolyte membrane between the positive and negative electrodes, and a driving pressure of 10 MPa was applied using a jig.
[0117]
[0118] Comparative Example 1.
[0119] An all-solid-state battery was manufactured in the same manner as in Example 1, except that agarodite (Li6PS5Cl) having a Young's modulus of 42 GPa and an average particle size (D50) of 2.5 μm was used as the first solid electrolyte particle, the second solid electrolyte was not used, and the first solid electrolyte particles were used in an amount twice that of Example 1. The Young's modulus of the solid electrolyte membrane for the all-solid-state battery was 42 GPa.
[0120]
[0121] Comparative Example 2.
[0122] An all-solid-state battery was manufactured in the same manner as in Example 1, except that agarodite (Li6PS5Cl) having a Young's modulus of 18 GPa and an average particle size (D50) of 2.5 μm was used as the second solid electrolyte particle, the first solid electrolyte particle was not used, and the second solid electrolyte particle was used in an amount twice that of Example 1. The Young's modulus of the solid electrolyte membrane for the all-solid-state battery was 18 GPa.
[0123]
[0124] Comparative Example 3.
[0125] An all-solid-state battery was manufactured in the same manner as in Example 1, except that the first solid electrolyte particles and the second solid electrolyte particles were mixed in a weight ratio of 2:8.
[0126]
[0127] Comparative Example 4.
[0128] An all-solid-state battery was manufactured in the same manner as in Example 1, except that agarodite (Li6PS5Cl) having an average particle size (D50) of 0.6 μm was used as the second solid electrolyte particle.
[0129]
[0130] Experimental Example 1. Measurement of the life characteristics of an all-solid-state battery.
[0131] The life characteristics of the all-solid-state batteries of Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 4 were measured.
[0132] The life characteristics were measured by measuring the capacity retention rate when the all-solid-state batteries of Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 4 were charged at 0.33C in CCCV mode at a temperature of 60°C until 4.25 V, and discharged to 3.0 V with a constant current, and then charged and discharged 100 times.
[0133] The results of Example 1, Comparative Example 1, and Comparative Example 2 are shown in Figure 1.
[0134] In the results of Fig. 1, the life characteristics of Example 1, which is an all-solid-state battery including the solid electrolyte membrane of the present invention, were measured to be the best.
[0135] Comparative Example 1 contained only agarodite (Li6PS5Cl) as solid electrolyte particles with a Young's modulus of 42 GPa and an average particle size (D50) of 2.5 μm, and did not contain second solid electrolyte particles. Comparative Example 1 showed very low interfacial adhesion between the solid electrolyte membrane and the positive electrode and between the solid electrolyte membrane and the negative electrode, resulting in deterioration of the life characteristics of the all-solid-state battery.
[0136] Comparative Example 2 contained only agarodite (Li6PS5Cl) as a solid electrolyte particle having a Young's modulus of 18 GPa and an average particle size (D50) of 2.5 μm, and did not contain the first solid electrolyte particle. Comparative Example 2 showed that the ionic conductivity of the solid electrolyte membrane was low, which increased the resistance of the all-solid-state battery, and as a result, the life characteristics of the all-solid-state battery deteriorated.
[0137] The results of Comparative Example 4 are shown in Fig. 2.
[0138] Comparative Example 4 used agarodite (Li6PS5Cl) with an average particle size (D50) of 0.6 μm as the second solid electrolyte particle. When manufacturing a solid electrolyte membrane, the second solid electrolyte particles were not easily dispersed, resulting in the manufacture of an uneven solid electrolyte membrane. Consequently, the life characteristics of the all-solid-state battery were very poor.
[0139]
[0140] Experimental Example 2. Measurement of the rate characteristics of an all-solid-state battery
[0141] The rate characteristics of the all-solid-state batteries of Example 1, Comparative Example 2, and Comparative Example 3 were measured.
[0142] The rate characteristics were measured by charging at 3.0 to 4.25 V, 0.1 C, and discharging at 0.1, 0.33, 0.5, and 1 C.
[0143] The results of Example 1, Comparative Example 2, and Comparative Example 3 are shown in Fig. 3.
[0144] In the results of FIG. 3, Example 1, an all-solid-state battery including the solid electrolyte membrane of the present invention, showed excellent rate characteristics.
[0145] Comparative Example 2 contained only agarodite (Li6PS5Cl) as a solid electrolyte with a Young's modulus of 18 GPa and an average particle size (D50) of 2.5 μm, and did not contain the first solid electrolyte particles. Comparative Example 2 showed that the ionic conductivity of the solid electrolyte membrane was low, which increased the resistance of the all-solid-state battery, resulting in poor rate characteristics of the all-solid-state battery.
[0146] Comparative Example 3 mixed the first solid electrolyte particles and the second solid electrolyte particles in a weight ratio of 2:8, and showed an effect of improving the rate characteristics compared to Comparative Example 2, but did not show the rate characteristics results of Example 1.
[0147]
[0148] From this, it includes first solid electrolyte particles and second solid electrolyte particles,
[0149] The Young's modulus of the first solid electrolyte particle is higher than the Young's modulus of the second solid electrolyte particle,
[0150] The average particle size (D50) of the first solid electrolyte particles and the second solid electrolyte particles is 1 to 5 μm,
[0151] It was confirmed that an all-solid-state battery including a solid electrolyte membrane for an all-solid-state battery in which the first solid electrolyte particles and the second solid electrolyte particles are mixed in a weight ratio of 7:3 to less than 2:8 has excellent life characteristics and rate characteristics.
[0152] It can be seen that this is an effect that appears as the solid electrolyte membrane minimizes the resistance that occurs at the interface between the positive electrode and the solid electrolyte membrane and the interface between the negative electrode and the solid electrolyte membrane.
Claims
1. A solid electrolyte membrane for an all-solid-state battery comprising first solid electrolyte particles and second solid electrolyte particles, The Young's modulus of the first solid electrolyte particle is higher than the Young's modulus of the second solid electrolyte particle, The average particle size (D50) of the first solid electrolyte particles and the second solid electrolyte particles is 1 to 5 μm, A solid electrolyte membrane for an all-solid-state battery, wherein the first solid electrolyte particles and the second solid electrolyte particles are mixed in a weight ratio of 7:3 to less than 2:
8.
2. In paragraph 1, A solid electrolyte membrane, wherein the Young's modulus of the first solid electrolyte particles is 40 to 80 GPa.
3. In paragraph 1, A solid electrolyte membrane, wherein the Young's modulus of the second solid electrolyte particles is 5 to 30 GPa.
4. In paragraph 1, A solid electrolyte membrane, wherein the difference in Young's modulus between the first solid electrolyte particles and the second solid electrolyte particles is 15 to 50 GPa.
5. In paragraph 1, A solid electrolyte membrane, wherein the first solid electrolyte particles and the second solid electrolyte particles have a particle size (D50) of 2 to 3 μm.
6. In paragraph 1, A solid electrolyte membrane, wherein the first solid electrolyte particles and the second solid electrolyte particles are mixed in a weight ratio of 6:4 to 4:
6.
7. In paragraph 1, A solid electrolyte membrane, wherein the first solid electrolyte particles and the second solid electrolyte particles include at least one selected from the group consisting of a sulfide-based solid electrolyte, a polymer-based solid electrolyte, and an oxide-based solid electrolyte.
8. In paragraph 7, A solid electrolyte membrane, wherein the first solid electrolyte particles and the second solid electrolyte particles are sulfide-based solid electrolytes.
9. In paragraph 1, A solid electrolyte membrane, wherein the solid electrolyte membrane further comprises a binder.
10. In paragraph 9, A solid electrolyte membrane, wherein the binder is included in an amount of 0.5 to 5 wt% based on the total weight of the solid electrolyte membrane.
11. An all-solid-state battery comprising a positive electrode, a negative electrode, and a solid electrolyte membrane interposed between them, An all-solid-state battery, wherein the above solid electrolyte membrane is the solid electrolyte membrane of claim 1.
12. In paragraph 11, The above negative electrode comprises a negative electrode current collector and a negative electrode active material positioned on the negative electrode current collector; or An all-solid-state battery comprising a negative electrode current collector and a coating layer comprising metal-carbon composite particles positioned on the negative electrode current collector.
Citation Information
Patent Citations
Mask and methode for making the same
KR1020230007099A
Solid electrolyte membrane and all-solid batteries comprising the same
KR1020240165663A
Lithium battery and method for manufacturing the same
JP2018190513A
Composite solid electrolyte and all-solid battery
JP2020027701A
All-solid-state battery
JP2022108202A