Composite material, preparation method therefor and light-emitting device
By using composite materials formed by connecting inorganic particles to ligands as electron transport layers in electroluminescent devices, the problem of traditional materials being susceptible to solvent erosion is solved, the electron injection efficiency and stability are improved, and the device life is extended.
Patent Information
- Application Number
- PCT/CN2023/122096
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-22
- Filing Date
- 2023-09-27
- Publication Date
- 2024-11-28
AI Technical Summary
In traditional electroluminescent devices, the electron transport layer material is susceptible to solvent erosion, resulting in uneven film formation and low electron injection efficiency, affecting the device life and stability.
A composite material is used as an electron transport layer, including inorganic particles connecting to the first ligand and the second ligand to form a network structure, improving the anti-solution erosion ability and electron injection efficiency.
It enhances the electron injection efficiency and stability of the light emitting device, reduces the risk of chemical reactions of electrode materials, and improves device life and performance.
Smart Images

Figure CN2023122096_28112024_PF_FP_ABST
Abstract
Description
Composite material, preparation method thereof and light-emitting device
[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on May 22, 2023, with application number 202310582502.9 and application name “Composite materials and preparation methods thereof, light-emitting devices and display devices”, the entire contents of which are incorporated by reference into this application. Technical Field
[0002] The present application relates to the field of display technology, and in particular to a composite material, a preparation method thereof, and a light-emitting device. Background Art
[0003] In traditional electroluminescent devices, inorganic materials are typically used as electron transport layers. For inverted light-emitting devices, these materials are susceptible to solvent erosion and have a work function mismatch with the electrode layer material, resulting in uneven film formation and poor electron injection efficiency, impacting device performance. Technical Solutions
[0004] The embodiments of the present application provide a composite material and a preparation method thereof, a light-emitting device and a display device. The composite material is used as an electron transport layer to be applicable to light-emitting devices of various structures, thereby improving the electron injection and electron transport capabilities of the device, thereby achieving the effect of increasing the device life and improving the stability.
[0005] An embodiment of the present application provides a composite material, which includes inorganic particles. The inorganic particles are connected to a first ligand and a second ligand, and the first ligand is connected to the second ligand.
[0006] Optionally, the first ligand and the second ligand are linked by a covalent bond; and / or
[0007] The composite material is formed into a network structure; and / or
[0008] The molar ratio of the first ligand to the second ligand is (5-12):1; and / or
[0009] The first ligand is at least one selected from the group consisting of unsubstituted or substituted amino, halogen, hydroxyl, carboxyl, nitro, sulfonic acid, aldehyde, mercapto, and cyano chain hydrocarbons with 1 to 30 carbon atoms, cyclic hydrocarbons with 3 to 30 ring atoms, aromatic hydrocarbons with 6 to 40 ring atoms, carboxylic acids with 1 to 30 carbon atoms, amines with 1 to 30 carbon atoms, and thiols with 1 to 30 carbon atoms; and / or
[0010] The second ligand is at least one selected from ketone and ketone derivatives, quinone and quinone derivatives.
[0011] Optionally, the first ligand is selected from at least one of R1-CH3, R2-COOH, R3-NH2, and R4-SH, wherein R1 to R4 are independently selected from any one of a chain hydrocarbon group with 1 to 20 carbon atoms and an aromatic hydrocarbon group with 6 to 18 ring atoms, which is unsubstituted or substituted with amino, halogen, hydroxyl, carboxyl, nitro, sulfonic acid, aldehyde, mercapto, or cyano; and / or
[0012] The second ligand is selected from one of R5-CO-R6, R7-CO-M-CO-R8, cyclohexadienedione or its derivatives; wherein R5 to R8 are independently selected from any one of a hydrocarbon group with 1 to 20 carbon atoms and an aromatic hydrocarbon group with 6 to 18 ring atoms, which is unsubstituted or substituted with amino, halogen, hydroxyl, carboxyl, nitro, sulfonic acid, aldehyde, mercapto or cyano, and M is selected from one of a single bond, -O-, -S-, -CO-, -CO-O-, -O-CO-, -O-CO-O-, -CH=N-, -N=CH-, -N=N-, a hydrocarbon group with 1 to 20 carbon atoms and an aromatic hydrocarbon group with 5 to 18 ring atoms.
[0013] Optionally, the first ligand is selected from at least one of R1-CH3, R2-COOH, R3-NH2, and R4-SH; wherein R1 to R4 are independently selected from any one of a chain hydrocarbon group having 4 to 18 carbon atoms and an aromatic hydrocarbon group having 6 to 18 ring atoms; and / or
[0014] The second ligand is selected from at least one of the following formulas (1) to (6):
[0015] Optionally, the inorganic particles are selected from at least one of metal oxides or doped metal oxides; wherein the doping substance in the doped metal oxide is selected from at least one of metals, halogens, inorganic substances, and organic polymers; and / or
[0016] The average particle size of the inorganic particles is 10 to 15 nm.
[0017] Optionally, the metal oxide is selected from at least one of ZnO, NiO, W2O3, Mo2O3, TiO2, SnO, ZrO2, Ta2O3, Ga2O3, Al2O3, CaO, and HfO2; and / or
[0018] The metal is selected from at least one of Mg, Ca, Li, Ga, Al, Co, Mn, and K; and / or
[0019] The halogen is selected from at least one of F, Cl, Br, and I; and / or
[0020] The inorganic substance is selected from at least one of graphene, octylene and molybdenum disulfide; and / or
[0021] The organic polymer is selected from at least one of PEDOT:PSS, polyaniline, polypyrrole, polythiophene and poly(p-phenylene vinylene).
[0022] Accordingly, the present invention also provides a method for preparing a composite material, comprising the following steps:
[0023] Providing a first solution containing a metal source, a first ligand, and a second solution containing a second ligand;
[0024] mixing the first solution with an alkaline solution to obtain a third solution, wherein the third solution includes inorganic particles connected to the first ligand;
[0025] The third solution is mixed with the second solution, reacted, centrifuged, and precipitated to obtain a composite material. The composite material includes inorganic particles. The inorganic particles are connected to a first ligand and a second ligand. The first ligand is connected to the second ligand.
[0026] Optionally, the first metal in the metal source is selected from at least one of Zn, Ni, W, Mo, Ti, Sn, Zr, Ta, Ga, Al, Ca, and Hf; and / or
[0027] The first solution further includes a doping source, and the doping substance in the doping source is selected from at least one of a second metal, a halogen, an inorganic substance, and an organic polymer.
[0028] Optionally, the molar ratio of the metal source, the doping source, the first ligand and the alkali in the alkali solution is (2-5): (0.1-0.2): 1: 1; and / or
[0029] The molar ratio of the inorganic particles connected with the first ligand to the second ligand is (5-12):1; and / or
[0030] The molar ratio of the first ligand to the second ligand is (5-12):1.
[0031] Optionally, the second metal is selected from at least one of Mg, Ca, Li, Ga, Al, Co, Mn, and K; and / or
[0032] The halogen is selected from at least one of F, Cl, Br, and I; and / or
[0033] The inorganic substance is selected from at least one of graphene, octylene and molybdenum disulfide; and / or
[0034] The organic polymer is selected from at least one of PEDOT:PSS, polyaniline, polypyrrole, polythiophene and poly(p-phenylene vinylene).
[0035] In addition, the present application also provides a light-emitting device, comprising a stacked first electrode, a light-emitting layer, and a second electrode, wherein at least one electron transport layer is further provided between the first electrode and the light-emitting layer;
[0036] The electron transport layer includes a composite material, the composite material includes inorganic particles, the inorganic particles are connected with a first ligand and a second ligand, and the first ligand is connected with the second ligand.
[0037] Optionally, the electron transport layer includes a first electron transport layer and a second electron transport layer stacked together; the first electrode is an anode, and the second electrode is a cathode; or, the first electrode is a cathode, and the second electrode is an anode;
[0038] The composite material of the first electron transport layer includes first inorganic particles, the first inorganic particles are selected from first doped metal oxides, and the doping material in the first doped metal oxide is selected from at least one of Ga, Li, Mg, Mn, and halogen;
[0039] The composite material of the second electron transport layer includes second inorganic particles, the second inorganic particles are selected from second doped metal oxides, and the doping material in the second doped metal oxide is selected from at least one of Al, K, graphene, footballene, molybdenum disulfide, PEDOT:PSS, polyaniline, polypyrrole, polythiophene and poly(p-phenylene vinylene).
[0040] Optionally, the material of the anode and / or cathode includes one or more of a metal, a carbon material and a metal oxide, the metal including one or more of Al, Ag, Cu, Mo, Au, Ba, Ca, Yb and Mg; the carbon material includes one or more of graphite, carbon nanotubes, graphene and carbon fiber; the metal oxide includes a doped or undoped metal oxide, including one or more of ITO, FTO, ATO, AZO, GZO, IZO, MZO and AMO, or includes a composite electrode in which a metal is sandwiched between doped or undoped transparent metal oxides, the composite electrode including one or more of AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, ZnS / Ag / ZnS, ZnS / Al / ZnS, TiO2 / Ag / TiO2 and TiO2 / Al / TiO2.
[0041] Optionally, the light-emitting layer includes a quantum dot material, and the light-emitting layer is a quantum dot light-emitting layer or an organic light-emitting layer; the material of the quantum dot light-emitting layer includes at least one of a single structure quantum dot and a core-shell structure quantum dot, and the material of the single structure quantum dot is selected from at least one of a II-VI group compound, a IV-VI group compound, a III-V group compound and a I-III-VI group compound, wherein the II-VI group compound is selected from CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, Cd At least one of HgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe and HgZnSTe, the IV-VI group compound is selected from at least one of SnS, SnSe, SnTe, PbS, PbSe, PbTe, SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe and SnPbSTe, the III-V group compound is selected from at least one of GaN, GaP, GaAs, At least one of GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs or InAlPSb, and the Group I-III-VI compound is at least one of CuInS2, CuInSe2 and AgInS2; and / or
[0042] The core of the core-shell structured quantum dots includes any one of the above-mentioned single-structure quantum dots, and the shell material of the core-shell structured quantum dots includes at least one of CdS, CdTe, CdSeTe, CdZnSe, CdZnS, CdSeS, ZnSe, ZnSeS, ZnS and the above-mentioned single-structure quantum dots; the material of the organic light-emitting layer includes at least one of 4,4'-bis(N-carbazole)-1,1'-biphenyl: tris[2-(p-tolyl)pyridine-C2,N)iridium(III), 4,4',4"-tris(carbazole-9-yl)triphenylamine: tris[2-(p-tolyl)pyridine-C2,N)iridium, diaromatic anthracene derivatives, distyrene aromatic derivatives, pyrene derivatives, fluorene derivatives, TBPe fluorescent materials, TTPX fluorescent materials, TBRb fluorescent materials and DBP fluorescent materials, polyacetylene and its derivatives, polyparaphenylene and its derivatives, polythiophene and its derivatives, and polyfluorene and its derivatives.
[0043] Optionally, it further includes an electron injection layer, a hole transport layer and a hole injection layer;
[0044] The electron injection layer is provided between the first electrode and the electron transport layer, and the material of the electron injection layer includes an inorganic material and / or an organic material; the inorganic material is selected from one or more of doped or undoped zinc oxide, barium oxide, aluminum oxide, nickel oxide, titanium oxide, tin oxide, tantalum oxide, zirconium oxide, nickel oxide, lithium titanium oxide, zinc aluminum oxide, zinc manganese oxide, zinc tin oxide, lithium zinc oxide, indium tin oxide, cadmium sulfide, zinc sulfide, molybdenum sulfide, tungsten sulfide, copper sulfide, zinc tin, indium phosphide, gallium phosphide, copper indium sulfide, copper gallium sulfide, and barium titanate, and the doped element includes one or more of aluminum, magnesium, lithium, manganese, yttrium, lanthanum, copper, nickel, zirconium, cerium, and gadolinium; the organic material is selected from one or more of quinoxaline compounds, imidazole compounds, triazine compounds, fluorene-containing compounds, and hydroxyquinoline compounds; and / or
[0045] The hole transport layer is arranged between the light-emitting layer and the second electrode, and the hole injection layer is arranged between the hole transport layer and the second electrode; the material of the hole transport layer and / or the hole injection layer includes at least one of TFB, CuPc, PVK, Poly-TPD, DNTPD, TCATA, TCCA, CBP, TPD, NPB, NPD, PEDOT:PSS, TAPC, MCC, F4-TCNQ, HATCN, 4,4',4'-tris(N-3-methylphenyl-Nphenylamino)triphenylamine, polyaniline, transition metal oxides, transition metal sulfides, transition metal tinides, doped graphene, undoped graphene and C60.
[0046] In addition, the present application also provides a method for preparing a light-emitting device, comprising the following steps:
[0047] Providing a substrate, the substrate comprising a first electrode;
[0048] forming at least one electron transport layer on the first electrode;
[0049] forming a light-emitting layer on the electron transport layer;
[0050] forming a second electrode on the light-emitting layer; or
[0051] providing a substrate, wherein the substrate includes a second electrode;
[0052] forming a light-emitting layer on the second electrode;
[0053] forming at least one electron transport layer on the light-emitting layer;
[0054] forming a first electrode on the electron transport layer;
[0055] Wherein, the electron transport layer comprises the composite material or the composite material prepared by the preparation method of the composite material.
[0056] Optionally, the step of forming at least one electron transport layer includes:
[0057] depositing a solution containing the composite material on the first electrode to react and form the electron transport layer; or,
[0058] A solution containing the composite material is deposited on a side of the light-emitting layer away from the second electrode, and reacted to form the electron transport layer.
[0059] In addition, the present application also provides a display device, which includes the light-emitting device; or, the display device includes the light-emitting device obtained by the preparation method. Beneficial effects
[0060] Compared with the prior art, the composite material of the present application includes inorganic particles, which are connected to a first ligand and a second ligand. Due to the bonding connection between the first ligand and the second ligand, the inorganic particles are connected to each other, and a composite material with a network structure is obtained; the composite material has a strong ability to resist solution erosion, the overall film formation is uniform, and the light-emitting device containing the composite material has a high electron injection efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0061] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.
[0062] FIG1 is a schematic flow chart of a method for preparing a composite material provided in an embodiment of the present application;
[0063] FIG2 is a schematic flow chart of another method for preparing a composite material provided in an embodiment of the present application;
[0064] FIG3 is a schematic diagram of the structure of inorganic particles provided in an embodiment of the present application;
[0065] FIG4 is a schematic diagram showing the connection between inorganic particles provided in an embodiment of the present application;
[0066] FIG5 is a schematic structural diagram of a light emitting device provided in an embodiment of the present application;
[0067] FIG6 is a schematic structural diagram of another light-emitting device provided in an embodiment of the present application;
[0068] FIG7 is a schematic flow chart of a method for preparing a light-emitting device provided in the present application;
[0069] FIG8 is a schematic flow chart of another method for preparing a light-emitting device provided in the present application;
[0070] FIG9 is a schematic flow chart of a method for preparing a light-emitting device according to Example 9 of the present application;
[0071] FIG10 is a schematic flow chart of a method for preparing a light-emitting device according to Example 10 of the present application;
[0072] FIG11 is a schematic flow chart of a method for preparing a light-emitting device according to Example 11 of the present application;
[0073] FIG12 is a schematic flow chart of a method for preparing a light-emitting device according to Example 12 of the present application;
[0074] FIG13 is a schematic flow chart of a method for preparing a light-emitting device according to Comparative Example 1 of the present application;
[0075] FIG14 is a schematic flow chart of a method for preparing a light-emitting device according to Comparative Example 2 of the present application;
[0076] FIG15 is a schematic flow chart of a method for preparing a light-emitting device according to Comparative Example 3 of the present application;
[0077] FIG16 is a schematic diagram of the surface morphology of the electron transport layer in the light-emitting device provided in Example 9 of the present application;
[0078] FIG17 is a schematic diagram of the surface morphology of the electron transport layer in the light-emitting device provided in Example 10 of the present application;
[0079] FIG18 is a schematic diagram of the surface morphology of the electron transport layer in the light-emitting device provided in Comparative Example 1 of the present application;
[0080] FIG19 is a schematic diagram of the surface morphology of the electron transport layer in the light-emitting device provided in Comparative Example 2 of the present application.
[0081] Reference numerals: 110 - first electrode, 120 - electron transport layer, 130 - light emitting layer, 140 - second electrode, 1211 - first electron transport layer, 1212 - second electron transport layer.
[0082] Implementation Methods of the Application
[0083] The following, in conjunction with the accompanying drawings, provides a clear and complete description of the technical solutions in the embodiments of the present application. It should be noted that the described embodiments are only a portion of the embodiments of the present application, and are not intended to be exhaustive. All other embodiments derived by persons skilled in the art based on the embodiments of the present application without inventive effort are intended to fall within the scope of protection of the present application. Furthermore, in the description of the present application, the term "including" means "including but not limited to." The terms "first," "second," and "third," etc., are used merely as designations and do not impose numerical requirements or establish a sequence. Various embodiments of the present application may be presented in the form of a range. It should be understood that describing in a range format is merely for convenience and brevity and should not be construed as a rigid limitation on the scope of the present application. Therefore, a range description should be considered to specifically disclose all possible subranges and individual numerical values within that range. For example, a range description of 1 to 6 should be considered to specifically disclose subranges, such as 1 to 3, 1 to 4, 1 to 5, 2 to 4, 2 to 6, 3 to 6, etc., as well as individual numerical values within the range, such as 1, 2, 3, 4, 5, and 6, regardless of the range. Additionally, whenever a numerical range is indicated herein, it is meant to include any cited numeral (fractional or integral) within the indicated range.
[0084] During the research and practice, the inventors of this application found that the traditional electroluminescent device structure is generally anode / hole injection layer / hole transport layer / luminescent layer / electron transport layer / cathode. In this structure, the electron transport layer is generally made of ZnO, TiO2, LiF, etc., and the cathode is made of low-work-function metal materials such as Mg, Ag, and Al. Since the above-mentioned cathode materials are sensitive to water and oxygen and are prone to chemical reactions, the life of the upright electroluminescent device is reduced and the stability is poor, which is not conducive to commercial application. In order to improve the stability of the device, the use of an inverted device structure is an effective method. However, in the inverted electroluminescent device structure, the material of the electron transport layer is easily washed away by the organic solvent prepared by the next functional layer, causing the function of the functional layer to be reduced or even fail, the roughness to increase, and affecting film formation. Secondly, the inverted electroluminescent device structure usually uses an upright anode as a cathode. Since the work function of this anode material is usually high, there will be a large electron injection barrier when it is used as a cathode, resulting in a work function mismatch problem, poor electron injection efficiency, and electron-hole imbalance, resulting in poor device performance.
[0085] Therefore, how to overcome the problems of uneven film formation of the electron transport layer, easy erosion, inability to prevent chemical reactions between water and oxygen, and electron injection efficiency is one of the keys to improving the performance of electroluminescent devices.
[0086] The present invention provides a composite material and preparation method, a light-emitting device and preparation method, and a display device. Each of these is described in detail below. It should be noted that the order in which the following embodiments are described does not limit the preferred order of the embodiments.
[0087] An embodiment of the present application provides a composite material, which includes inorganic particles. The inorganic particles are connected to a first ligand and a second ligand, and the first ligand is connected to the second ligand.
[0088] It can be understood that the composite material has a plurality of inorganic particles, and when the first ligand is connected to the second ligand, the plurality of inorganic particles can be connected to form a network structure.
[0089] Further, the inorganic particles of the present application are biligand inorganic particles having a first ligand and a second ligand connected at the same time. Due to the presence of multiple ligands, the solvent selectivity of the composite material is high; the first ligand and the second ligand have groups that can react with each other so that the first ligand and the second ligand can be bonded, and the principle of bonding is: under the action of external factors, free radicals are generated on the first ligand and the second ligand, and the free radicals react to form covalent bonds, thereby connecting adjacent inorganic particles. It is understandable that there is uncertainty in the above connection process, but due to steric hindrance, the first ligand or the second ligand on an inorganic particle will always give priority to bonding with the second ligand or the first ligand on another inorganic particle, and multiple inorganic particles can be not limited to bonding by only one group of the first ligand and the second ligand, and the connection between different inorganic particles allows the composite material as a whole to form a network structure.
[0090] The composite material of the present application has a network structure, which can not only prevent some water and oxygen from contacting the electrode material, reducing the probability of chemical reactions in the electrode material; it can also avoid being washed away by organic solvents. It has strong resistance to solution washing and high stability, which can solve the problems of low life and poor stability of upright light-emitting devices, and can also solve the problem of high work function of the electrode layer in inverted devices and difficulty in electron injection.
[0091] In some embodiments, the bonding method between the first ligand and the second ligand may include photo-induced polymerization, thermal-induced polymerization, etc.; the preferred method is photo-induced polymerization, because the photo-induced polymerization method is simple, and the ligand used for photopolymerization is a structurally engineered molecular scaffold, which is conducive to achieving an integrated cross-linked overall network structure.
[0092] In some embodiments, the molar ratio of the first ligand to the second ligand is (5-12): 1. It is understood that the molar ratio of the first ligand to the second ligand can be any one of 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, 11:1, 12:1, or a range between any two thereof.
[0093] In some embodiments, the first ligand is selected from at least one of a chain hydrocarbon with 1-30 carbon atoms, a cyclic hydrocarbon with 3-30 ring atoms, an aromatic hydrocarbon with 6-40 ring atoms, a carboxylic acid with 1-30 carbon atoms, an amine with 1-30 carbon atoms, and a thiol with 1-30 carbon atoms, which is unsubstituted or substituted with amino, halogen, hydroxyl, carboxyl, nitro, sulfonic, aldehyde, thiol, or cyano groups; and the second ligand is selected from at least one of a ketone and a ketone derivative, a quinone, and a quinone derivative. It is understood that the first ligand is a dispersing ligand, which has high selectivity and high degree of freedom, thus providing versatility and freedom in solvent selection; and the second ligand is a photocrosslinking ligand, preferably a photoinitiator, which activates free radicals of the photocrosslinking ligand under the action of ultraviolet light. The free radicals can form covalent bonds with the dispersing ligands of adjacent inorganic particles. The photocrosslinking ligand is a structurally engineered molecular scaffold, thereby achieving integrated crosslinking and an overall network structure.
[0094] Furthermore, the first ligand is selected from at least one of R1-CH3, R2-COOH, R3-NH2, and R4-SH, wherein R1 to R4 are independently selected from any one of a chain hydrocarbon group with 1 to 20 carbon atoms or an aromatic hydrocarbon group with 6 to 18 ring atoms, which is unsubstituted or substituted with amino, halogen, hydroxyl, carboxyl, nitro, sulfonic acid, aldehyde, mercapto, or cyano; the second ligand is selected from one of R5-CO-R6, R7-CO-M-CO-R8, cyclohexadienedione, or a derivative thereof; In the formula (I), R5 to R8 are independently selected from any one of a hydrocarbon group having 1 to 20 carbon atoms, which is unsubstituted or substituted with amino, halogen, hydroxyl, carboxyl, nitro, sulfonic acid, aldehyde, mercapto, or cyano, and an aromatic hydrocarbon group having 6 to 18 ring atoms; and M is selected from one of a single bond, -O-, -S-, -CO-, -CO-O-, -O-CO-, -O-CO-O-, -CH=N-, -N=CH-, -N=N-, an alkylene group having 1 to 20 carbon atoms, and an arylene group having 5 to 18 ring atoms. It is understood that an alkylene group refers to a divalent hydrocarbon group obtained by removing two hydrogen atoms from a hydrocarbon; and an arylene group refers to a divalent aromatic hydrocarbon obtained by removing two hydrogen atoms from an aromatic ring.
[0095] Furthermore, the first ligand is selected from at least one of R1-CH3, R2-COOH, R3-NH2, and R4-SH; wherein R1 to R4 are independently selected from any one of a chain hydrocarbon group having 4-18 carbon atoms and an aromatic hydrocarbon group having 6-18 ring atoms. A chain hydrocarbon group refers to a group containing only carbon and hydrogen atoms, generally referring to the free radical remaining after the corresponding hydrocarbon loses a hydrogen atom. Chain hydrocarbon groups are of various types, including monovalent saturated groups also known as alkyl groups and monovalent unsaturated groups also known as alkenyl or alkynyl groups. Aromatic hydrocarbon groups refer to organic compounds with aromatic rings, which must contain at least one conjugated double bond in their molecules and at least one carbon atom in their molecules. The carbon atoms in their molecules can be combined with atoms of other elements, such as hydrogen, oxygen, and nitrogen.
[0096] Furthermore, the second ligand is selected from at least one of the following formulas (1) to (6):
[0097] Wherein, the molecular formula of the compound of formula (1) is C 13 H 10 OS, CAS No. 1620-94-6; the molecular formula of the compound of formula (2) is C 13 H 10 OS2, CAS No. 37089-83-1; the molecular formula of formula (3) is C 20 H 114 O2S2, CAS No. 180286-04-8; the molecular formula of formula (4) is C 15 H 14 O, CAS No. 611-97-2; the molecular formula of formula (5) is C 14 H7IO2, CAS No. 10566-32-2; the molecular formula of formula (6) is C 14 H 10 O, CAS number is 90-44-8.
[0098] In some embodiments, the inorganic particles are selected from at least one of a metal oxide or a doped metal oxide; wherein the dopant in the doped metal oxide is selected from at least one of a metal, a halogen, an inorganic substance, and an organic polymer. It is understood that when the dopant is a metal, the metal used for doping is different from the metal in the metal oxide; and the organic polymer is a highly conductive polymer. It is understood that when the inorganic particles are selected from a metal oxide or a doped metal oxide, the composite material can function as an electron transport material.
[0099] In some embodiments, the metal oxide is selected from at least one of ZnO, NiO, W2O3, Mo2O3, TiO2, SnO, ZrO2, Ta2O3, Ga2O3, Al2O3, CaO, and HfO2.
[0100] In some embodiments, the metal is selected from at least one of Mg, Ca, Li, Ga, Al, Co, Mn, and K.
[0101] In some embodiments, the halogen is selected from at least one of F, Cl, Br, and I.
[0102] In some embodiments, the inorganic substance is selected from at least one of graphene, octylene, and molybdenum disulfide.
[0103] In some embodiments, the organic polymer is selected from at least one of PEDOT:PSS, polyaniline, polypyrrole, polythiophene, and poly(p-phenylene vinylene).
[0104] Furthermore, the functions of the resulting composite materials vary depending on the doped substances. For example, doping with metallic elements such as Ga, Li, Mg, and Mn, or halogen atoms, can adjust the composite material's work function; whereas doping with metallic elements such as Al and K, inorganic compounds, and organic polymers can improve the composite material's electron transport properties.
[0105] In some embodiments, the average particle size of the inorganic particles is 10-15 nm; for example, the average particle size of the inorganic particles is any one of 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, and 15 nm, or a range between any two values.
[0106] Referring to FIG1 , the present invention also provides a method for preparing a composite material, comprising the following steps:
[0107] Providing a first solution containing a metal source, a first ligand, and a second solution containing a second ligand;
[0108] mixing the first solution with an alkaline solution to obtain a third solution, the third solution comprising inorganic particles having first ligands attached thereto;
[0109] The third solution is mixed with the second solution, reacted, centrifuged, and precipitated to obtain a composite material. The composite material includes inorganic particles. The inorganic particles are connected to the first ligand and the second ligand. The first ligand is connected to the second ligand.
[0110] After the composite material of the present application is prepared by the above-mentioned method, the consistency of particle size can be guaranteed. The obtained composite material can be directly used in the commercial photolithography or inkjet printing process that allows commercial control of the structures of the two ligands, and will not affect the original optical properties of the inorganic particles or the photoelectric performance of subsequent devices. It can be suitable for any solution processing such as inkjet printing or spin coating.
[0111] In some embodiments, the first metal in the metal source is selected from at least one of Zn, Ni, W, Mo, Ti, Sn, Zr, Ta, Ga, Al, Ca, and Hf.
[0112] In some embodiments, the first solution further includes a doping source, and the doping substance in the doping source is selected from at least one of a second metal, a halogen, an inorganic substance, and an organic polymer.
[0113] Specifically, referring to FIG2 , a Zn source is used as a metal source and a potassium hydroxide solution is used as a reducing agent to prepare a composite material. The specific synthesis process includes the following steps:
[0114] S11: ZnO synthesis: Zn(CH3COO)2·2H2O and the first ligand are dissolved in 200 mL of N,N-dimethylformamide (DMF) solvent at the same time to obtain a first solution, and nitrogen is passed through and stirred for 1 hour; wherein, the molar mass ratio of the Zn source and the first ligand is (2-5):1; potassium hydroxide solution is taken in 100 mL of ethanol solution and stirred for 1 hour; after complete dissolution, it is injected into the above-mentioned first solution at an injection speed of 10 mL / min, and nitrogen is passed through and stirred for 1 hour, wherein, the molar ratio of the base and the first ligand is 1:1; after the reaction is completed, ethyl acetate is added and centrifuged to obtain a precipitate; the precipitate is dissolved in ethanol, and heptane is added to the ethanol, and then centrifuged to obtain a precipitate as an intermediate of ZnO-first ligand.
[0115] S21: The intermediate is dissolved in 100 mL of ethanol, heated to 50°C and stirred continuously. After half an hour, the second ligand is added to perform partial ligand exchange, and then stirred for half an hour; ethyl acetate is added and centrifuged to obtain a precipitate; the precipitate is dissolved in ethanol, and heptane is added to the ethanol, and then centrifuged to obtain an inorganic particle of ZnO-first ligand-second ligand; wherein the molar ratio of the first ligand to the second ligand is (5-12):1.
[0116] Please refer to Figure 3, which is a schematic diagram of the structure of the synthesized ZnO-first ligand-second ligand. Based on the central inorganic particle ZnO, a number of first ligands and second ligands are connected to the surface of the inorganic particle, wherein the long solid line represents the first ligand and the short dashed line represents the second ligand. Please refer to Figure 3 for a schematic diagram of the principle of the reaction between inorganic particles. Under the irradiation of ultraviolet light, free radicals are generated on the second ligand, and the free radicals react and bond with the first ligand, thereby connecting the inorganic particles. In Figure 3, the connection of inorganic particles can be between inorganic particles of the same type, as shown in Figure 3 (a), A1 and A2 represent inorganic particles of the same type; or as shown in Figure 3 (b), A and B represent different types of inorganic particles, respectively, and different types of inorganic particles are connected through the bonding of the first ligand and the second ligand.
[0117] It is understandable that in step S11, a doping source may be added to improve the function of the inorganic particles, wherein the molar ratio of the metal source, the doping source, the first ligand and the base is (2-5):(0.1-0.2):1:1.
[0118] Meanwhile, the molar ratio of the inorganic particles connected with the first ligand to the second ligand is (5-12):1.
[0119] An embodiment of the present application provides a light-emitting device, comprising a stacked first electrode, a light-emitting layer, and a second electrode, and at least one electron transport layer between the first electrode and the light-emitting layer; wherein the electron transport layer comprises a composite material, the composite material comprises inorganic particles, the inorganic particles are connected to a first ligand and a second ligand, and the first ligand is configured to be connected to the second ligand.
[0120] Furthermore, a first electron transport layer and a second electron transport layer are stacked between the first electrode and the light-emitting layer; the first electrode is an anode and the second electrode is a cathode; or the first electrode is a cathode and the second electrode is an anode;
[0121] The composite material of the first electron transport layer includes first inorganic particles, the first inorganic particles are selected from first doped metal oxides, and the doping material in the first doped metal oxide is selected from at least one of Ga, Li, Mg, Mn, and halogen;
[0122] The composite material of the second electron transport layer includes second inorganic particles, the second inorganic particles are selected from second doped metal oxides, and the doping material in the second doped metal oxide is selected from at least one of Al, K, graphene, footballene, molybdenum disulfide, PEDOT:PSS, polyaniline, polypyrrole, polythiophene and poly(p-phenylene vinylene).
[0123] It can be understood that the first electron transport layer can be used to adjust the work function of the electron transport layer, and the second electron transport layer can be used to adjust the transport capacity of the electron transport layer.
[0124] Furthermore, the light-emitting layer is a quantum dot light-emitting layer or an organic light-emitting layer; the material of the quantum dot light-emitting layer includes at least one of a single structure quantum dot and a core-shell structure quantum dot, and the material of the single structure quantum dot is selected from at least one of a II-VI group compound, a IV-VI group compound, a III-V group compound and a I-III-VI group compound, wherein the II-VI group compound is selected from CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnS At least one of CdTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe and HgZnSTe, and a Group IV-VI compound selected from SnS, SnSe, SnTe, PbS, PbSe, PbS At least one of SnPbTe, SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe and SnPbSTe, and the III-V compound is selected from GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, A At least one of lPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs or InAlPSb, and the I-III-VI group compound is selected from at least one of CuInS2, CuInSe2 and AgInS2.
[0125] The core of the core-shell structured quantum dots includes any one of the above-mentioned single-structure quantum dots, and the shell material of the core-shell structured quantum dots includes at least one of CdS, CdTe, CdSeTe, CdZnSe, CdZnS, CdSeS, ZnSe, ZnSeS, ZnS and the above-mentioned single-structure quantum dots; the material of the organic light-emitting layer includes 4,4'-bis(N-carbazole)-1,1'-biphenyl: tris[2-(p-tolyl)pyridine-C2,N)iridium(III), 4,4',4"-tris(carbazole-9-yl)triphenylamine: tris[2-(p-tolyl)pyridine-C2,N)iridium, diaromatic anthracene derivatives, distyrene aromatic derivatives, pyrene derivatives, fluorene derivatives, TBPe fluorescent materials, TTPX fluorescent materials, TBRb fluorescent materials and DBP fluorescent materials, polyacetylene and its derivatives, polyparaphenylene and its derivatives, polythiophene and its derivatives, polyfluorene and its derivatives.
[0126] In some embodiments, the cathode material can be one or more of a metal, a carbon-silicon material, and a metal oxide. The metal can be, for example, one or more of Al, Ag, Cu, Mo, Au, Ba, Ca, and Mg. The silicon-carbon material can be, for example, one or more of silicon, graphite, carbon nanotubes, graphene, and carbon fiber. The metal oxide can be a doped or undoped metal oxide, including one or more of ITO, FTO, ATO, AZO, GZO, IZO, MZO, and AMO. It also includes a composite electrode in which a metal is sandwiched between doped or undoped transparent metal oxides, including but not limited to one or more of AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, and ITO / Al / ITO. The thickness of the cathode layer is preferably 10 to 1000 nm.
[0127] In some embodiments, the anode material may be one or more of a metal, a carbon-silicon material, and a metal oxide. For example, the metal may be one or more of Al, Ag, Cu, Mo, Au, Ba, Ca, Yb, and Mg; the silicon-carbon material may be one or more of silicon, graphite, carbon nanotubes, graphene, and carbon fiber; the metal oxide may be a doped or undoped metal oxide, including one or more of ITO, FTO, ATO, AZO, GZO, IZO, MZO, and AMO, and also including a composite electrode in which a metal is sandwiched between doped or undoped transparent metal oxides. The composite electrode includes but is not limited to one or more of AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, TiO2 / Ag / TiO2, TiO2 / Al / TiO2, ZnS / Ag / ZnS, ZnS / Al / ZnS, TiO2 / Ag / TiO2, and TiO2 / Al / TiO2. The thickness of the anode layer is preferably 10 to 1000 nm.
[0128] In some embodiments, the light emitting device may be an inverted structure or an upright structure.
[0129] In some embodiments, a stacked hole transport layer and a hole injection layer are further included between the light-emitting layer and the second electrode layer, wherein the hole transport layer is connected to the light-emitting layer, and the hole injection layer is arranged between the hole transport layer and the second electrode, and is connected to the hole transport layer and the second electrode respectively.
[0130] Furthermore, the hole transport layer is selected from organic materials having hole transport capability, including but not limited to poly(9,9-dioctylfluorene-co-N-(4-butylphenyl)diphenylamine) (TFB), polyvinylcarbazole (PVK), poly(N,N'-bis(4-butylphenyl)-N,N'-bis(phenyl)benzidine) (poly-TPD), poly(9,9-dioctylfluorene-co-bis-N,N-phenyl-1,4-phenylenediamine) (PFB), 4,4',4"-tris(carbazol-9-yl)triphenylamine (TCATA), 4,4'-bis(9-carbazol)biphenyl (CBP), N,N'-diphenyl-N,N'-bis(3-methylphenyl)-1,1'- One or more of biphenyl-4,4'-diamine (TPD), N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine (NPB), poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonic acid) (PEDOT:PSS), Spiro-NPB, Spiro-TPD, doped graphene, undoped graphene, and C60; and inorganic materials having hole transport capabilities, including but not limited to one or more of doped or undoped NiO, MoO3, WO3, V2O5, p-type gallium nitride, CrO3, and CuO. The hole transport layer may have a thickness of 20 to 100 nm.
[0131] Furthermore, the hole injection layer is selected from hole injection materials, and the hole injection material can be one or more of TFB, CuPc, PVK, Poly-TPD, DNTPD, TCATA, TCCA, CBP, TPD, NPB, NPD, PEDOT:PSS, TAPC, MCC, F4-TCNQ, HATCN, 4,4',4'-tris(N-3-methylphenyl-Nphenylamino)triphenylamine, polyaniline, transition metal oxides, transition metal sulfides, transition metal tin compounds, doped graphene, undoped graphene, and C60, TiOPc (phthalocyanine titanium oxide), m-MTDATA (CAS 124729-98-2), 2-TNATA (4,4',4"-tris(2-naphthylphenylaminotriphenylamine)), transition metal oxides, and transition metal sulfide compounds. Among them, the transition metal oxide includes NiO x 、MoO x , WO x CrO x , CuO; metal sulfide compounds include MoS x 、MoSe x , WS x 、WSe x, CuS, or one or more thereof. The value of x in each compound can be determined based on the valence of the atoms in the compound. The thickness of the hole injection layer can be 20 to 50 nm.
[0132] In some embodiments, there is an electron injection layer between the first electrode and the electron transport layer, and the material of the electron injection layer includes inorganic materials and / or organic materials; the inorganic material is selected from one or more of doped or undoped zinc oxide, barium oxide, aluminum oxide, nickel oxide, titanium oxide, tin oxide, tantalum oxide, zirconium oxide, nickel oxide, lithium titanium oxide, zinc aluminum oxide, zinc manganese oxide, zinc tin oxide, lithium zinc oxide, indium tin oxide, cadmium sulfide, zinc sulfide, molybdenum sulfide, tungsten sulfide, copper sulfide, zinc tin, indium phosphide, gallium phosphide, copper indium sulfide, copper gallium sulfide, and barium titanate, and the doped elements include one or more of aluminum, magnesium, lithium, manganese, yttrium, lanthanum, copper, nickel, zirconium, cerium, and gadolinium; the organic material is selected from one or more of quinoxaline compounds, imidazole compounds, triazine compounds, fluorene compounds, and hydroxyquinoline compounds.
[0133] Referring to FIG5 , the light-emitting device 100 includes: a first electrode 110, a light-emitting layer 130, and a second electrode 140; an electron transport layer 120 is provided between the first electrode 110 and the light-emitting layer 130. The material of the electron transport layer 120 adopts the composite material provided in this embodiment. Since the composite material is an inorganic particle containing a first ligand and a second ligand, bonding occurs between the first ligand and the second ligand, so that adjacent inorganic particles are connected, and the composite material as a whole forms a network structure; when the light-emitting device 100 is an upright structure, the composite material with a network structure can prevent some water and oxygen from contacting the first electrode 110, thereby reducing the probability of chemical reaction between the first electrode 110 and water or oxygen; when the light-emitting device 100 is an inverted structure, the network structure improves the overall strength of the composite material, which can prevent the composite material itself from being washed away by organic solvents, so that the composite material has strong resistance to solution washing and high stability.
[0134] Referring to Figure 6 , a light-emitting device 200 includes a first electrode 110, a light-emitting layer 130, and a second electrode 140. A first electron transport layer 1211 and a second electron transport layer 1212 are stacked and supported on the first electrode 110 and the light-emitting layer 130. The first electron transport layer 1211 is connected to the first electrode 100, and the second electron transport layer 1212 is connected to the light-emitting layer. The composite material used to prepare the first electron transport layer 1211 includes first inorganic particles, selected from metal oxides doped with a first dielectric, wherein the first dielectric is selected from at least one of Ga, Li, Mg, Mn, and halogen atoms. By doping with the first dielectric, the first electron transport layer 1211 can adjust the work function when in contact with the first electrode 110. This adjustment of the work function allows more electrons to escape from the first electrode 110. The composite material used to prepare the second electron transport layer 1212 includes second inorganic particles, the second inorganic particles are selected from metal oxides doped with a second medium, and the second medium is selected from at least one of Al, K, graphene, octylene, molybdenum disulfide, PEDOT:PSS, polyaniline, polypyrrole, polythiophene and poly(p-phenylene vinylene); by doping the second medium, the electron transport ability of the second electron transport layer 1212 can be improved, so that when the second electron transport layer 1212 contacts the light-emitting layer 130, more electrons enter the light-emitting layer, thereby reducing the electron injection barrier, improving the electron injection efficiency, and reducing the problem of electron-hole imbalance.
[0135] Referring to FIG. 7 , an embodiment of the present application further provides a method for preparing a light-emitting device, comprising the following steps:
[0136] Providing a substrate, the substrate comprising a first electrode;
[0137] forming at least one electron transport layer on the first electrode;
[0138] forming a light-emitting layer on the electron transport layer;
[0139] forming a second electrode on the light-emitting layer;
[0140] Wherein, the electron transport layer includes the composite material or the composite material prepared by the preparation method of the composite material.
[0141] Alternatively, referring to FIG8 , another method for preparing a light-emitting device is provided, comprising the following steps:
[0142] providing a substrate, the substrate including a second electrode;
[0143] forming a light-emitting layer on the second electrode;
[0144] forming at least one electron transport layer on the light-emitting layer;
[0145] forming a first electrode on the electron transport layer;
[0146] Wherein, the electron transport layer includes the composite material or the composite material prepared by the preparation method of the composite material.
[0147] Furthermore, the step of forming at least one electron transport layer includes:
[0148] Depositing a solution containing the composite material on the first electrode, reacting to form an electron transport layer; or,
[0149] A solution containing the composite material is deposited on a side of the light-emitting layer away from the second electrode, and reacted to form an electron transport layer.
[0150] In some embodiments, the method of depositing the solution containing the composite material includes spin coating, dropping, or printing.
[0151] In some embodiments, in the step of forming at least one electron transport layer, the preferred reaction is to first irradiate with ultraviolet light and then anneal, wherein the wavelength of the ultraviolet light is 300-400 nm and the energy density is 3-6 mW / cm 2 The exposure time is 10 to 15 seconds; the annealing temperature is 80 to 120°C, and the annealing time is 10 to 15 minutes.
[0152] In some embodiments, the present application further provides a display device, comprising the light-emitting device provided in the embodiments of the present application. The light-emitting device included in the display device of the present application has excellent luminous efficiency and overall performance, and thus the display device also has excellent luminous efficiency and overall performance.
[0153] In order to enable those skilled in the art to clearly understand the above-mentioned implementation details and operations of the present application, as well as to significantly demonstrate the improved performance of the composite materials and preparation methods, light-emitting devices and preparation methods, and display devices in the embodiments of the present application, the above-mentioned technical solutions are illustrated by means of multiple embodiments below.
[0154] Example 1
[0155] This embodiment provides a composite material comprising inorganic particles, to which a first ligand and a second ligand are attached. The first ligand is configured to bond with the second ligand to link adjacent inorganic particles. The first ligand and the second ligand are covalently bonded; the bonding is achieved through photoinduced polymerization. The composite material forms a network structure through the connection of the inorganic particles.
[0156] The inorganic particles are ZnO doped with Mg, denoted as ZnMgO; the first ligand is oleylamine, with the molecular formula CH3(CH2)7CH=CH(CH2)7CH2NH2, denoted as OAm; the second ligand is:
[0157] The CAS number is 1620-94-6.
[0158] The method for preparing the composite material of this embodiment comprises the following steps:
[0159] 0.12 mol of Zn(Ac)2·2H2O, 0.006 mol of Mg(Ac)2·4H2O, and 0.05 mol of oleylamine (OA) were dissolved simultaneously in 200 ml of N,N-dimethylformamide (DMF) solvent, and stirred for 1 hour under nitrogen. 0.05 mol of potassium hydroxide was dissolved in 100 ml of ethanol solution and stirred for 1 hour. After complete dissolution, the solution was injected into the above solution at an injection rate of 10 ml / min, and stirred for 1 hour under nitrogen. After the reaction was completed, ethyl acetate was added and centrifuged to obtain a precipitate. The precipitate was dissolved in ethanol, and heptane was added to the ethanol, and the mixture was centrifuged again to obtain the intermediate ZnMgO-OAm.
[0160] Take 0.06 mol of ZnMgO-OAm and dissolve it in 100 ml of ethanol, heat it to 50°C and stir it continuously. After half an hour, add 0.005 mol of the second ligand for partial ligand exchange, and then stir for half an hour; add ethyl acetate and centrifuge to obtain a precipitate; the precipitate is dissolved in ethanol, and heptane is added to the ethanol, and then centrifuged to obtain a precipitate as a composite material of ZnMgO-OAm-second ligand.
[0161] Example 2
[0162] This embodiment provides a composite material comprising inorganic particles, to which a first ligand and a second ligand are attached. The first ligand is configured to bond with the second ligand to link adjacent inorganic particles. The first ligand and the second ligand are covalently bonded; the bonding is achieved through photoinduced polymerization. The composite material forms a network structure through the connection of the inorganic particles.
[0163] The inorganic particles are ZnO doped with Al, denoted as ZnAlO; the first ligand is oleylamine, with the molecular formula CH3(CH2)7CH=CH(CH2)7CH2NH2, denoted as OAm; the second ligand is:
[0164] The CAS number is 1620-94-6.
[0165] The method for preparing the composite material of this embodiment comprises the following steps:
[0166] 0.12 mol of Zn(Ac)2·2H2O, 0.006 mol of Al(Ac)2·4H2O, and 0.05 mol of oleylamine (OA) were dissolved simultaneously in 200 ml of N,N-dimethylformamide (DMF) solvent, and stirred for 1 hour under nitrogen. 0.05 mol of potassium hydroxide was dissolved in 100 ml of ethanol solution and stirred for 1 hour. After complete dissolution, the solution was injected into the above solution at an injection rate of 10 ml / min, and stirred for 1 hour under nitrogen. After the reaction was completed, ethyl acetate was added and centrifuged to obtain a precipitate. The precipitate was dissolved in ethanol, and heptane was added to the ethanol, and the mixture was centrifuged again to obtain the intermediate ZnAlO-OAm.
[0167] Take 0.06 mol of ZnAlO-OAm and dissolve it in 100 ml of ethanol, heat it to 50°C and stir it continuously. After half an hour, add 0.005 mol of the second ligand for partial ligand exchange, and then stir for half an hour; add ethyl acetate and centrifuge to obtain a precipitate; the precipitate is dissolved in ethanol, and heptane is added to the ethanol, and then centrifuged to obtain a precipitate as a composite material of ZnAlO-OAm-second ligand.
[0168] Example 3
[0169] The ZnMgO-OAm-second ligand of Example 1 and the ZnAlO-OA-second ligand of Example 2 were mixed in an ethanol solution at a mass ratio of 1:1 to obtain a mixed composite material.
[0170] Example 4
[0171] This embodiment provides a composite material comprising inorganic particles, to which a first ligand and a second ligand are attached. The first ligand is configured to bond with the second ligand to link adjacent inorganic particles. The first ligand and the second ligand are covalently bonded; the bonding is achieved through photoinduced polymerization. The composite material forms a network structure through the connection of the inorganic particles.
[0172] Among them, the inorganic particle is ZnO; the first ligand is oleic acid, with the molecular formula CH3(CH2)7CH=CH(CH2)7CH2COOH, denoted as OA; the second ligand is:
[0173] The CAS number is 10566-32-2.
[0174] The preparation method of the composite material of this embodiment is the same as that of the embodiment, except that the molar ratio of the metal source, the first ligand and the base is 3:1:1; and the molar ratio of the intermediate to the second ligand is 10:1.
[0175] Example 5
[0176] This embodiment provides a composite material comprising inorganic particles, to which a first ligand and a second ligand are attached. The first ligand is configured to bond with the second ligand to link adjacent inorganic particles. The first ligand and the second ligand are covalently bonded; the bonding is achieved through photoinduced polymerization. The composite material forms a network structure through the connection of the inorganic particles.
[0177] The inorganic particles are NiO doped with Cl; the first ligand is 9-octadecene; and the second ligand is:
[0178] The CAS number is 37089-83-1.
[0179] The preparation method of the composite material of this embodiment is the same as that of the embodiment, except that the molar ratio of the metal source, the doping source, the first ligand and the base is 5:0.12:1:1; and the molar ratio of the intermediate to the second ligand is 5:1.
[0180] Example 6
[0181] This embodiment provides a composite material comprising inorganic particles, to which a first ligand and a second ligand are attached. The first ligand is configured to bond with the second ligand to link adjacent inorganic particles. The first ligand and the second ligand are covalently bonded; the bonding is achieved through photoinduced polymerization. The composite material forms a network structure through the connection of the inorganic particles.
[0182] The inorganic particles are TiO2 doped with graphene; the first ligand is octadecanethiol; and the second ligand is:
[0183] The CAS number is 180286-04-8.
[0184] The preparation method of the composite material of this embodiment is the same as that of the embodiment, except that the molar ratio of the metal source, the doping source, the first ligand and the base is 2.5:0.2:1:1; and the molar ratio of the intermediate to the second ligand is 8:1.
[0185] Example 7
[0186] This embodiment provides a composite material comprising inorganic particles, to which a first ligand and a second ligand are attached. The first ligand is configured to bond with the second ligand to link adjacent inorganic particles. The first ligand and the second ligand are covalently bonded; the bonding is achieved through photoinduced polymerization. The composite material forms a network structure through the connection of the inorganic particles.
[0187] The inorganic particles are BaTiO3 doped with PEDOT:PSS; the first ligand is oleylamine; and the second ligand is:
[0188] The CAS number is 90-44-8.
[0189] The preparation method of the composite material of this embodiment is the same as that of the embodiment, except that the molar ratio of the metal source, the doping source, the first ligand and the base is 2:0.18:1:1; and the molar ratio of the intermediate to the second ligand is 5:1.
[0190] Example 8
[0191] This embodiment provides a composite material comprising inorganic particles, to which a first ligand and a second ligand are attached. The first ligand is configured to bond with the second ligand to link adjacent inorganic particles. The first ligand and the second ligand are covalently bonded; the bonding is achieved through photoinduced polymerization. The composite material forms a network structure through the connection of the inorganic particles.
[0192] Wherein, the inorganic particle is ZnO; the first ligand is oleylamine; the second ligand is:
[0193] The CAS number is 611-97-2.
[0194] The preparation method of the composite material of this embodiment is the same as that of the embodiment, except that the molar ratio of the metal source, the first ligand and the base is 4:1:1; and the molar ratio of the intermediate to the second ligand is 6:1.
[0195] Example 9
[0196] This embodiment provides a light-emitting device comprising a cathode, a first electron transport layer, a second electron transport layer, a light-emitting layer, a hole transport layer, a hole injection layer, and an anode, sequentially disposed on a substrate. The substrate is a glass sheet, the cathode material is an ITO substrate, the light-emitting layer material is CdSe quantum dots, the hole transport layer material is PVK, the hole injection layer material is PEDOT:PSS, the first electron transport layer material is the composite material prepared in Example 1, and the second electron transport layer material is the composite material prepared in Example 2.
[0197] Please refer to FIG9 , the method for preparing the light emitting device is as follows:
[0198] S101, depositing 100 nm of ITO on a glass substrate to obtain a cathode;
[0199] S102, spin coating an ethanol solution of ZnMgO-OAm-second ligand on the cathode to a thickness of 20 nm;
[0200] S103, select ultraviolet light with a wavelength of 355nm and an energy density of 4mW / cm 2 Under the same conditions, UV exposure was performed for 10 s;
[0201] S104, soaking the exposed substrate in an ethanol solution for 10 seconds; then annealing at 100° C. for 10 minutes to obtain a first electron transport layer;
[0202] S105, spin coating an ethanol solution of ZnAlO-OAm-second ligand on the first electron transport layer to a thickness of 20 nm;
[0203] S106, select ultraviolet light with a wavelength of 355nm and an energy density of 4mW / cm 2 Under the same conditions, UV exposure was performed for 10 s;
[0204] S107, soaking the exposed substrate in an ethanol solution for 10 seconds; then annealing at 100° C. for 10 minutes to obtain a second electron transport layer;
[0205] S108, depositing a CdSe quantum dot solution on the second electron transport layer to obtain a light-emitting layer, wherein the thickness of the light-emitting layer is 30 nm;
[0206] S109, depositing a layer of PVK on the light-emitting layer to obtain a hole transport layer with a thickness of 20 nm;
[0207] S110, depositing a layer of PEDOT:PSS on the hole transport layer to obtain a hole injection layer with a thickness of 50 nm;
[0208] S111. Deposit Ag on the hole injection layer to obtain an anode with a thickness of 100 nm.
[0209] Example 10
[0210] This embodiment provides a light-emitting device comprising a cathode, an electron transport layer, a light-emitting layer, a hole transport layer, a hole injection layer, and an anode, sequentially disposed on a substrate. The substrate is a glass sheet, the cathode material is an ITO substrate, the light-emitting layer material is CdZnS quantum dots, the hole transport layer material is PVK, the hole injection layer material is PEDOT:PSS, and the electron transport layer material is the composite material prepared in Example 3.
[0211] Please refer to FIG10 , the method for preparing the light emitting device is as follows:
[0212] S201, depositing 100 nm of ITO on a glass substrate to obtain a cathode;
[0213] S202, spin coating a mixed solution of ZnMgO-OAm-second ligand and ZnAlO-OA-second ligand on the cathode to a thickness of 40 nm;
[0214] S203, select ultraviolet light with a wavelength of 355nm and an energy density of 4mW / cm 2Under the same conditions, UV exposure was performed for 15s;
[0215] S204, soaking the exposed substrate in an ethanol solution for 15 seconds; then annealing at 100° C. for 10 minutes to obtain an electron transport layer;
[0216] S205, depositing a CdZnS quantum dot solution on the electron transport layer to obtain a light-emitting layer, wherein the thickness of the light-emitting layer is 30 nm;
[0217] S206, depositing a layer of PVK on the light-emitting layer to obtain a hole transport layer with a thickness of 20 nm;
[0218] S207, depositing a layer of PEDOT:PSS on the hole transport layer to obtain a hole injection layer with a thickness of 50 nm;
[0219] S208. Deposit Ag on the hole injection layer to obtain an anode with a thickness of 100 nm.
[0220] Example 11
[0221] This embodiment provides a light-emitting device, which has an upright stacked structure and includes an anode, a hole injection layer, a hole transport layer, a light-emitting layer, an electron transport layer, a hole injection layer, a hole transport layer, a light-emitting layer, an electron transport layer and a cathode, which are sequentially arranged on a substrate; wherein the substrate is a glass sheet, the anode material is ITO, the material of the light-emitting layer is CdSe quantum dots, the material of the hole transport layer is PVK, the material of the hole injection layer is PEDOT:PSS, and the material of the electron transport layer is the composite material prepared in Example 1.
[0222] Please refer to FIG11 , the method for preparing the light emitting device is as follows:
[0223] S301, depositing 100 nm of ITO on a glass substrate to obtain an anode;
[0224] S302, depositing a layer of PEDOT:PSS on the anode to obtain a hole injection layer with a thickness of 50 nm;
[0225] S303, depositing a layer of PVK on the hole injection layer to obtain a hole transport layer with a thickness of 20 nm;
[0226] S304, depositing a CdSe quantum dot solution on the hole transport layer to obtain a light-emitting layer, the thickness of the light-emitting layer being 30 nm;
[0227] S305, spin coating an ethanol solution of ZnMgO-OAm-second ligand on the light-emitting layer to a thickness of 20 nm;
[0228] S306, select ultraviolet light with a wavelength of 355nm and an energy density of 4mW / cm 2Under the same conditions, UV exposure was performed for 10 s;
[0229] S307, soaking the exposed substrate in an ethanol solution for 10 seconds; then annealing at 100° C. for 10 minutes to obtain an electron transport layer;
[0230] S308, depositing a layer of PEDOT:PSS on the electron transport layer to obtain a hole injection layer with a thickness of 50 nm;
[0231] S309, depositing a layer of PVK on the hole injection layer to obtain a hole transport layer with a thickness of 20 nm;
[0232] S310, depositing a CdSe quantum dot solution on the hole transport layer to obtain a light-emitting layer, wherein the thickness of the light-emitting layer is 30 nm;
[0233] S311, spin coating an ethanol solution of ZnMgO-OAm-second ligand on the light-emitting layer to a thickness of 20 nm;
[0234] S312, select ultraviolet light with a wavelength of 355nm and an energy density of 4mW / cm 2 Under the same conditions, UV exposure was performed for 10 s;
[0235] S313, soaking the exposed substrate in an ethanol solution for 10 seconds; then annealing at 100° C. for 10 minutes to obtain an electron transport layer;
[0236] S314. Deposit Ag on the electron transport layer to obtain a cathode with a thickness of 100 nm.
[0237] Example 12
[0238] This embodiment provides a light-emitting device, comprising an anode, a hole injection layer, a hole transport layer, a light-emitting layer, an electron transport layer and a cathode, which are sequentially arranged on a substrate; wherein the substrate is a glass sheet, the anode material is ITO, the material of the light-emitting layer is CdS quantum dots, the material of the hole transport layer is PVK, the material of the hole injection layer is PEDOT:PSS, and the material of the electron transport layer is the composite material prepared in Example 2.
[0239] Referring to FIG12 , the method for preparing the light emitting device is as follows:
[0240] S401, depositing 100 nm of ITO on a glass substrate to obtain an anode;
[0241] S402, depositing a layer of PEDOT:PSS on the anode to obtain a hole injection layer with a thickness of 50 nm;
[0242] S403, depositing a layer of PVK on the hole injection layer to obtain a hole transport layer with a thickness of 20 nm;
[0243] S404, depositing a CdS quantum dot solution on the hole transport layer to obtain a light-emitting layer, wherein the thickness of the light-emitting layer is 30 nm;
[0244] S405, spin coating an ethanol solution of ZnAlO-OA-second ligand on the light-emitting layer to a thickness of 20 nm;
[0245] S406, select ultraviolet light with a wavelength of 355nm and an energy density of 4mW / cm 2 Under the same conditions, UV exposure was performed for 10 s;
[0246] S407, soaking the exposed substrate in an ethanol solution for 10 seconds; then annealing at 100° C. for 10 minutes to obtain an electron transport layer;
[0247] S408 , depositing Ag on the electron transport layer to obtain a cathode with a thickness of 100 nm.
[0248] Example 13
[0249] This embodiment provides a light-emitting device comprising a cathode, a first electron transport layer, a second electron transport layer, a light-emitting layer, a hole transport layer, a hole injection layer, and an anode, sequentially disposed on a substrate. The substrate is a glass sheet, the cathode material is an ITO substrate, the light-emitting layer material is CdSe quantum dots, the hole transport layer material is PVK, the hole injection layer material is PEDOT:PSS, the first electron transport layer material is the composite material prepared in Example 4, and the second electron transport layer material is the composite material prepared in Example 5.
[0250] The specific preparation process is the same as that of Example 9.
[0251] Example 14
[0252] This embodiment provides a light-emitting device comprising a cathode, an electron transport layer, a light-emitting layer, a hole transport layer, a hole injection layer, and an anode, sequentially disposed on a substrate. The substrate is a glass sheet, the cathode material is an ITO substrate, the light-emitting layer material is CdZnS quantum dots, the hole transport layer material is PVK, the hole injection layer material is PEDOT:PSS, and the electron transport layer material is a mixture of the composite materials prepared in Example 6 and Example 7 in a 1:1 weight ratio.
[0253] The specific preparation process is the same as that of Example 10.
[0254] Example 15
[0255] This embodiment provides a light-emitting device, comprising an anode, a hole injection layer, a hole transport layer, a light-emitting layer, an electron transport layer and a cathode, which are sequentially arranged on a substrate; wherein the substrate is a glass sheet, the anode material is ITO, the material of the light-emitting layer is CdS quantum dots, the material of the hole transport layer is PVK, the material of the hole injection layer is PEDOT:PSS, and the material of the electron transport layer is the composite material prepared in Example 8.
[0256] The specific preparation process is the same as Example 12.
[0257] Comparative Example 1
[0258] This embodiment provides a light-emitting device comprising a cathode, a first electron transport layer, a second electron transport layer, a light-emitting layer, a hole transport layer, a hole injection layer, and an anode, sequentially disposed on a substrate. The substrate is a glass sheet, the cathode material is an ITO substrate, the light-emitting layer material is CdSe quantum dots, the hole transport layer material is PVK, the hole injection layer material is PEDOT:PSS, the first electron transport layer material is Mg-doped zinc oxide, denoted as ZnMgO, and the second electron transport layer material is Al-doped zinc oxide, denoted as ZnAlO.
[0259] Referring to FIG13 , the method for preparing the light emitting device is as follows:
[0260] S501, depositing 100 nm of ITO on a glass substrate to obtain a cathode;
[0261] S502, spin-coating a ZnMgO ethanol solution on the cathode to obtain a first electron transport layer with a thickness of 20 nm;
[0262] S503, spin coating an ethanol solution of ZnAlO on the first electron transport layer to obtain a second electron transport layer with a thickness of 20 nm;
[0263] S504, depositing a CdSe quantum dot solution on the second electron transport layer to obtain a light-emitting layer, the thickness of the light-emitting layer being 30 nm;
[0264] S505, depositing a layer of PVK on the light-emitting layer to obtain a hole transport layer with a thickness of 20 nm;
[0265] S506, depositing a layer of PEDOT:PSS on the hole transport layer to obtain a hole injection layer with a thickness of 50 nm;
[0266] S507 , depositing Ag on the hole injection layer to obtain an anode with a thickness of 100 nm.
[0267] Comparative Example 2
[0268] This embodiment provides a light-emitting device comprising a cathode, an electron transport layer, a light-emitting layer, a hole transport layer, a hole injection layer, and an anode, sequentially disposed on a substrate. The substrate is a glass sheet, the cathode material is an ITO substrate, the light-emitting layer material is CdZnS quantum dots, the hole transport layer material is PVK, the hole injection layer material is PEDOT:PSS, and the electron transport layer material is the intermediate prepared in Example 1, namely, ZnMgO-OAm.
[0269] Please refer to FIG14 , the method for preparing the light emitting device is as follows:
[0270] S601, depositing 100 nm of ITO on a glass substrate to obtain a cathode;
[0271] S602, spin-coating a mixed solution of ZnMgO-OAm on the cathode to obtain an electron transport layer with a thickness of 40 nm;
[0272] S603, depositing a CdZnS quantum dot solution on the electron transport layer to obtain a light-emitting layer, wherein the thickness of the light-emitting layer is 30 nm;
[0273] S604, depositing a layer of PVK on the light-emitting layer to obtain a hole transport layer with a thickness of 20 nm;
[0274] S605, depositing a layer of PEDOT:PSS on the hole transport layer to obtain a hole injection layer with a thickness of 50 nm;
[0275] S606 , depositing Ag on the hole injection layer to obtain an anode with a thickness of 100 nm.
[0276] Comparative Example 3
[0277] This embodiment provides a light-emitting device, including an anode, a hole injection layer, a hole transport layer, a light-emitting layer, an electron transport layer and a cathode, which are sequentially arranged on a substrate; wherein the substrate is a glass sheet, the anode material is ITO, the material of the light-emitting layer is CdS quantum dots, the material of the hole transport layer is PVK, the material of the hole injection layer is PEDOT:PSS, and the material of the electron transport layer is Mg-doped zinc oxide, denoted as ZnMgO.
[0278] Please refer to FIG15 , the method for preparing the light emitting device is as follows:
[0279] S701, depositing 100 nm of ITO on a glass substrate to obtain an anode;
[0280] S702, depositing a layer of PEDOT:PSS on the anode to obtain a hole injection layer with a thickness of 50 nm;
[0281] S703, depositing a layer of PVK on the hole injection layer to obtain a hole transport layer with a thickness of 20 nm;
[0282] S704, depositing a CdS quantum dot solution on the hole transport layer to obtain a light-emitting layer, wherein the thickness of the light-emitting layer is 30 nm;
[0283] S705, spin coating ZnMgO ethanol solution on the light-emitting layer to a thickness of 20 nm;
[0284] S706 , depositing Ag on the electron transport layer to obtain a cathode with a thickness of 100 nm.
[0285] The performance of the light emitting devices of Examples 9-15 and Comparative Examples 1-3 was characterized, and the test data are shown in Table 1. The performance test item is: external quantum efficiency (EQE, %), and the performance test results are shown in Table 1 below.
[0286] External quantum efficiency (EQE): measured using an EQE optical testing instrument.
[0287] Atomic force microscopy was performed on the electron transport layers of the light-emitting devices of Examples 9-10 and Comparative Examples 1-2, and the surface roughness was detailed in Table 2 below.
[0288] Table 1
[0289] Table 2
[0290] As can be seen from Table 1, compared with comparative examples 1-3, the light-emitting devices of Examples 9-15 of the present application have higher external quantum efficiencies after adopting the composite materials provided by this embodiment, indicating that regardless of whether it is a light-emitting device with an upright structure or an inverted structure, the performance of the light-emitting device can be greatly improved by adopting the composite materials of this embodiment.
[0291] Please refer to Figures 16, 17, 18 and 19, and combined with the data in Table 2, it can be seen that the surface roughness of Examples 9-10 is lower than the surface roughness of Comparative Examples 1-2, indicating that the electron transport layer prepared using the composite material of this embodiment has higher stability; at the same time, it can be seen in Figures 18 and 19 that there is an aperture in the middle part. The appearance of the aperture indicates that the difference in thickness inside and outside is large, which also indirectly explains that the electron transport layer of Comparative Examples 1 and 2 is easily eroded by organic solvents, but the electron transport layer of the present application has a strong resistance to solution erosion due to internal cross-linking to form a network structure.
[0292] The above is a detailed introduction to a composite material and its preparation method, light-emitting device and display device provided in the embodiments of the present application. Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea; at the same time, for technical personnel in this field, based on the ideas of the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.
Claims
1. A composite material, wherein: The invention comprises an inorganic particle, wherein a first ligand and a second ligand are connected to the inorganic particle, and the first ligand is connected to the second ligand.
2. The composite material according to claim 1, wherein The first ligand and the second ligand are connected by a covalent bond; the composite material is a network structure; the molar ratio of the first ligand to the second ligand is (5-12):
1.
3. The composite material according to claim 2, wherein: The first ligand is selected from one or more of chain hydrocarbons with 1 to 30 carbon atoms, cyclic hydrocarbons with 3 to 30 ring atoms, aromatic hydrocarbons with 6 to 40 ring atoms, carboxylic acids with 1 to 30 carbon atoms, amines with 1 to 30 carbon atoms, and thiols with 1 to 30 carbon atoms, which are unsubstituted or substituted with amino, halogen, hydroxyl, carboxyl, nitro, sulfonic acid, aldehyde, thiol, and cyano groups; the second ligand is selected from one or more of ketones and ketone derivatives, quinones and quinone derivatives.
4. The composite material according to claim 3, wherein The first ligand is selected from one or more of R1-CH3, R2-COOH, R3-NH2, and R4-SH, wherein R1 to R4 are independently selected from any one of a chain hydrocarbon group with 1 to 20 carbon atoms and an aromatic hydrocarbon group with 6 to 18 ring atoms, which is unsubstituted or substituted with amino, halogen, hydroxyl, carboxyl, nitro, sulfonic acid, aldehyde, thiol, or cyano.
5. The composite material according to claim 4, wherein: The second ligand is selected from one or more of R5-CO-R6, R7-CO-M-CO-R8, cyclohexadienedione or its derivatives; wherein R5 to R8 are independently selected from any one of a hydrocarbon group with 1 to 20 carbon atoms and an aromatic hydrocarbon group with 6 to 18 ring atoms which is unsubstituted or substituted with amino, halogen, hydroxyl, carboxyl, nitro, sulfonic acid, aldehyde, thiol or cyano, and M is selected from one of a single bond, -O-, -S-, -CO-, -CO-O-, -O-CO-, -O-CO-O-, -CH=N-, -N=CH-, -N=N-, a hydrocarbon group with 1 to 20 carbon atoms and an aromatic group with 5 to 18 ring atoms.
6. The composite material according to claim 5, wherein The first ligand is selected from one or more of R1-CH3, R2-COOH, R3-NH2, and R4-SH; wherein R1 to R4 are independently selected from any one of a chain hydrocarbon group having 4 to 18 carbon atoms and an aromatic hydrocarbon group having 6 to 18 ring atoms; The second ligand is selected from one or more of the following formulas (1) to (6):
7. The composite material according to any one of claims 1 to 6, wherein: The inorganic particles are selected from one or more of metal oxides or doped metal oxides; wherein the doping material in the doped metal oxide is selected from one or more of metals, halogens, inorganic substances, and organic polymers; and the average particle size of the inorganic particles is 10 to 15 nm.
8. The composite material according to claim 7, wherein The metal oxide is selected from one or more of ZnO, NiO, W2O3, Mo2O3, TiO2, SnO, ZrO2, Ta2O3, Ga2O3, Al2O3, CaO, and HfO2; the metal is selected from one or more of Mg, Ca, Li, Ga, Al, Co, Mn, and K.
9. The composite material according to claim 8, wherein The halogen is selected from one or more of F, Cl, Br, and I; the inorganic substance is selected from one or more of graphene, sphericalene, and molybdenum disulfide; and the organic polymer is selected from one or more of PEDOT:PSS, polyaniline, polypyrrole, polythiophene, and poly(p-phenylene vinylene).
10. A method for preparing a composite material, wherein: The following steps are involved: Providing a first solution containing a metal source, a first ligand, and a second solution containing a second ligand; mixing the first solution with an alkaline solution to obtain a third solution, wherein the third solution includes inorganic particles connected with the first ligand; The third solution is mixed with the second solution, reacted, centrifuged, and precipitated to obtain a composite material, wherein the composite material includes inorganic particles, the inorganic particles are connected with a first ligand and a second ligand, and the first ligand is connected with the second ligand.
11. The method for preparing a composite material according to claim 10, wherein: The first ligand is selected from one or more of R1-CH3, R2-COOH, R3-NH2, and R4-SH; wherein R1 to R4 are independently selected from any one of a chain hydrocarbon group having 4 to 18 carbon atoms and an aromatic hydrocarbon group having 6 to 18 ring atoms; The second ligand is selected from one or more of the following formulas (1) to (6):
12. The method for preparing a composite material according to claim 10, wherein: The metal in the metal source is a first metal, and the first metal is selected from one or more of Zn, Ni, W, Mo, Ti, Sn, Zr, Ta, Ga, All, Ca, and Hf.
13. The method for preparing a composite material according to claim 10, wherein: The first solution also includes a doping source, and the doping substance in the doping source is selected from one or more of a second metal, a halogen, an inorganic substance, and an organic polymer.
14. The method for preparing a composite material according to claim 13, wherein: The molar ratio of the metal source, the doping source, the first ligand and the alkali in the alkali solution is (2-5):(0.1-0.2):1:1; the molar ratio of the inorganic particles connected with the first ligand and the second ligand is (5-12):1; the molar ratio of the first ligand and the second ligand is (5-12):
1.
15. The method for preparing a composite material according to claim 13, wherein: The second metal is selected from one or more of Mg, Ca, Li, Ga, Al, Co, Mn, and K; the halogen is selected from one or more of F, Cl, Br, and I; The inorganic substance is selected from one or more of graphene, ethylenediamine, and molybdenum disulfide; the organic polymer is selected from one or more of PEDOT:PSS, polyaniline, polypyrrole, polythiophene, and poly(p-phenylene vinylene).
16. A light emitting device, wherein: It comprises a stacked first electrode, a light-emitting layer and a second electrode, wherein at least one electron transport layer is provided between the first electrode and the light-emitting layer; The electron transport layer includes a composite material, the composite material includes inorganic particles, the inorganic particles are connected with a first ligand and a second ligand, and the first ligand is connected with the second ligand.
17. The light emitting device according to claim 16, wherein: The first ligand is selected from one or more of R1-CH3, R2-COOH, R3-NH2, and R4-SH; wherein R1 to R4 are independently selected from any one of a chain hydrocarbon group having 4 to 18 carbon atoms and an aromatic hydrocarbon group having 6 to 18 ring atoms; The second ligand is selected from one or more of the following formulas (1) to (6): The inorganic particles are selected from one or more of metal oxides or doped metal oxides; wherein the doping material in the doped metal oxide is selected from one or more of metals, halogens, inorganic substances, and organic polymers.
18. The light emitting device according to claim 16, wherein: The electron transport layer comprises a first electron transport layer and a second electron transport layer stacked; the first electrode is an anode and the second electrode is a cathode; or, the first electrode is a cathode and the second electrode is an anode; wherein the composite material of the first electron transport layer comprises first inorganic particles, the first inorganic particles are selected from first doped metal oxides, and the doping material in the first doped metal oxide is selected from one or more of Ga, Li, Mg, Mn, and halogen; the composite material of the second electron transport layer comprises second inorganic particles, the second inorganic particles are selected from doped second doped metal oxides, and the doping material in the second doped metal oxide is selected from one or more of Al, K, graphene, soccer ene, molybdenum disulfide, PEDOT:PSS, polyaniline, polypyrrole, polythiophene, and poly(p-phenylene vinylene); The material of the anode and / or cathode includes one or more of metal, carbon material and metal oxide, the metal includes one or more of Al, Ag, Cu, Mo, Au, Ba, Ca, Yb and Mg; the carbon material includes one or more of graphite, carbon nanotubes, graphene and carbon fiber; the metal oxide includes doped or undoped metal oxide, including one or more of ITO, FTO, ATO, AZO, GZO, IZO, MZO and AMO, or includes a composite electrode with a metal sandwiched between doped or undoped transparent metal oxides, the composite electrode includes one or more of AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, ZnS / Ag / ZnS, ZnS / Al / ZnS, TiO2 / Ag / TiO2 and TiO2 / Al / TiO2; The light-emitting layer is a quantum dot light-emitting layer or an organic light-emitting layer; the material of the quantum dot light-emitting layer includes one or more of a single structure quantum dot and a core-shell structure quantum dot, and the material of the single structure quantum dot is selected from one or more of a II-VI group compound, a IV-VI group compound, a III-V group compound and a I-III-VI group compound, wherein the II-VI group compound is selected from CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, Zn One or more of SeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe and HgZnSTe, and the IV-VI group compound is selected from SnS, SnSe, SnTe, PbS, PbSe, P One or more of SnPbTe, SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe and SnPbSTe, wherein the III-V compound is selected from GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, A One or more of lPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs or InAlPSb, and the I-III-VI group compound is selected from one or more of CuInS2, CuInSe2 and AgInS2.
19. The light emitting device according to claim 18, wherein: The core of the core-shell structured quantum dots includes any one of the above-mentioned single-structure quantum dots, and the shell material of the core-shell structured quantum dots includes one or more of CdS, CdTe, CdSeTe, CdZnSe, CdZnS, CdSeS, ZnSe, ZnSeS, ZnS and the above-mentioned single-structured quantum dots; the material of the organic light-emitting layer includes one or more of 4,4'-bis(N-carbazole)-1,1'-biphenyl:tris[2-(p-tolyl)pyridine-C2,N)iridium(III), 4,4',4"-tris(carbazole-9-yl)triphenylamine:tris[2-(p-tolyl)pyridine-C2,N)iridium, diaromatic anthracene derivatives, distyrene aromatic derivatives, pyrene derivatives, fluorene derivatives, TBPe fluorescent materials, TTPX fluorescent materials, TBRb fluorescent materials and DBP fluorescent materials, polyacetylene and its derivatives, polyparaphenylene and its derivatives, polythiophene and its derivatives, polyfluorene and its derivatives; The light-emitting device further comprises an electron injection layer, a hole transport layer and a hole injection layer; the electron injection layer is arranged between the first electrode and the electron transport layer, and the material of the electron injection layer comprises an inorganic material and / or an organic material; the inorganic material is selected from one or more of doped or undoped zinc oxide, barium oxide, aluminum oxide, nickel oxide, titanium oxide, tin oxide, tantalum oxide, zirconium oxide, nickel oxide, lithium titanium oxide, zinc aluminum oxide, zinc manganese oxide, zinc tin oxide, lithium zinc oxide, indium tin oxide, cadmium sulfide, zinc sulfide, molybdenum sulfide, tungsten sulfide, copper sulfide, zinc tin, indium phosphide, gallium phosphide, copper indium sulfide, copper gallium sulfide, and barium titanate, and the doped elements comprise one or more of aluminum, magnesium, lithium, manganese, yttrium, lanthanum, copper, nickel, zirconium, cerium, and gadolinium; the organic material is selected from one or more of quinoxaline compounds, imidazole compounds, triazine compounds, fluorene compounds, and hydroxyquinoline compounds.
20. The light emitting device according to claim 18, wherein: The hole transport layer is arranged between the light-emitting layer and the second electrode, and the hole injection layer is arranged between the hole transport layer and the second electrode; the material of the hole transport layer and / or the hole injection layer includes one or more of TFB, CuPc, PVK, Poly-TPD, DNTPD, TCATA, TCCA, CBP, TPD, NPB, NPD, PEDOT:PSS, TAPC, MCC, F4-TCNQ, HATCN, 4,4',4'-tri(N-3-methylphenyl-Nphenylamino)triphenylamine, polyaniline, transition metal oxides, transition metal sulfides, transition metal tinides, doped graphene, undoped graphene and C60.
Citation Information
Patent Citations
Quantum dots, a composition or composite including the same, and an electronic device including the same
CN108102640A
Quantum dots with mixed amine and thiol ligands
CN109790452A
Particles, preparation method thereof, and quantum dot light-emitting diode
CN110746973A
Ligands for nano-sized materials
CN113574136A
Quantum dot structure, quantum dot light-emitting device, and manufacturing methods for quantum dot structure and quantum dot light-emitting device
CN114058373A