Carbon-coated nickel-palladium alloy nanoparticle composite material, preparation method therefor, and use thereof
By graphitized carbon coated with nickel-palladium alloy nanoparticle composite materials and sulfur-containing compounds, the problem of inactivation of palladium catalysts due to coalescence and poisoning in the hydrogenation reaction is solved, and high activity and stability are achieved, and high selection is achieved. The ability of hydrotonic and dechlorination avoids the inactivation of metal particles.
Patent Information
- Application Number
- PCT/CN2023/134959
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-25
- Filing Date
- 2023-11-29
- Publication Date
- 2024-11-28
AI Technical Summary
The prior art is difficult to effectively solve the problem of inactivation of palladium catalysts due to coalescence and poisoning in the hydrogenation reaction, especially in the presence of sulfur-containing compounds, and lacks a simple and effective method for producing graphitized carbon-coated palladium composite materials.
The composite material of graphitized carbon coated nickel-palladium alloy nanoparticles is used to promote carbon graphitization ability and the complexing of organic polycarboxylic acids to achieve effective coating of palladium, form a core-shell structure, and combine sulfur-containing compounds. Modified, used to catalyze hydrogenation reaction.
The high activity and stability of the palladium catalyst is achieved, the coalescence and poisoning of metal particles are avoided, the high selective hydrogenation capacity is achieved, and the catalyst is highly dechlorinated without using alkali. Poisoning and anti-active metal loss capacity.
Smart Images

Figure PCTCN2023134959-FTAPPB-I100001 
Figure PCTCN2023134959-FTAPPB-I100002 
Figure 00000027_0000
Abstract
Description
Composite material of carbon-coated nickel-palladium alloy nanoparticles, preparation method and application thereof Technical Field
[0001] The present invention relates to a composite material of carbon-coated nickel-palladium alloy nanoparticles, a preparation method thereof, and applications thereof. More specifically, it relates to a composite material of carbon-coated nickel-palladium alloy nanoparticles having a core-shell structure, a preparation method thereof, and applications of the composite material in catalytic reactions. Background Art
[0002] Metal particles have a long history and widespread application as active components in catalysts. In the field of catalytic hydrogenation, palladium is generally more active than nickel. For example, in hydrodechlorination reactions, palladium is generally recognized as having the highest catalytic activity.
[0003] Metal particle agglomeration is one of the main causes of catalyst deactivation. Smaller metal particle size improves catalytic activity, but also increases surface energy, making agglomeration more likely to cause deactivation. Reducing the particle size to a certain level can even pose a safety hazard. For example, nano-sized nickel and palladium can spontaneously combust in air. Metal poisoning is another major cause of catalyst deactivation. Hydrogenation feedstocks, such as hydrogen and reaction substrates, can contain sulfur, a common poison for nickel and palladium. Palladium is more susceptible to sulfur poisoning than nickel.
[0004] Many documents have reported composite materials with graphitized carbon-coated nickel nanoparticle core-shell structures. These core-shell structures are generally nickel nanoparticles coated with graphene layers with a thickness of less than 10 nm. When these composite materials are used for catalytic hydrogenation, they have both the stability of carbon nanomaterials and the high activity of nickel nanoparticles. CN114425341A has earlier disclosed the sulfur poisoning resistance of graphene-coated nickel nanoparticles. The strict coating of the graphitized carbon layer is one of the key factors for their sulfur poisoning resistance. Although the prior art discloses a large number of graphitized carbon-coated nickel nanomaterials, it is difficult to produce composite materials of graphitized carbon-coated palladium. Documents related to graphitized carbon-coated palladium are relatively rare, and the prior art still lacks a simple and effective method for manufacturing graphitized carbon-coated palladium. Therefore, how to utilize the advantages of high palladium catalytic activity while overcoming its shortcomings of easy aggregation and easy poisoning and inactivation is a technical problem that the prior art has not yet well solved.
[0005] Methods for improving reaction selectivity can be broadly divided into two categories: one is achieved by modifying the catalyst's properties during catalyst manufacturing; the other is achieved during the reaction itself by controlling reaction conditions or adding selectivity modifiers. While much of the literature on reaction selectivity focuses on reactions catalyzed by metals or metal oxides, there is little research on improving catalytic reaction selectivity by modifying carbon-coated metal materials.
[0006] Halogenated aromatic amines are important organic intermediates, and the catalytic hydrogenation of halogenated nitroaromatics is the most important method for their synthesis. Palladium and nickel are both commonly used metals in the catalytic hydrogenation of halogenated nitroaromatics. The main problem with the catalytic hydrogenation of halogenated nitroaromatics is the susceptibility to dehalogenation. Existing technologies focus on the atom economy of the reaction; however, even if only a small amount of dehalogenation occurs, the generated hydrogen halide can still lead to catalyst halogen poisoning and metal loss, resulting in a decrease in catalyst performance. Therefore, there is still a need for improvement.
[0007] The catalytic hydrogenation of halogenated nitroaromatics is a complex reaction process, and the reaction mechanism is different depending on the catalytic system. One of the main ways to solve the dehalogenation problem in the prior art is to add a dehalogenation inhibitor during the reaction process. Dehalogenation inhibitors are usually compounds containing nitrogen, sulfur, and phosphorus. These heteroatoms bind to the metal surface to block some highly active sites, thereby inhibiting the dehalogenation reaction. Its disadvantage is that these heteroatoms have a strong effect on the metal surface and are easy to form chemical adsorption bonds or directly react with the active center. Therefore, their type and dosage are very critical. Improper selection will cause the catalyst performance to decline seriously, or even lose its catalytic ability. The prior art can usually only add dechlorination inhibitors during the reaction. These toxic compounds are often present in the reaction product components, and it is difficult to completely remove them.
[0008] On the other hand, catalytic hydrodechlorination can be carried out in the gas phase or in the liquid phase. Generally, the chlorine on the aliphatic carbon is easy to remove, while the chlorine on the aromatic carbon is difficult to remove. At present, there are a large number of reports on the application of catalysts such as platinum, palladium, rhodium, ruthenium, and nickel in hydrodechlorination reactions. Among them, the catalytic activity of palladium is the highest, but the price of palladium is expensive, and the loss and recycling of palladium must be considered. Moreover, a large amount of HCl will be produced during the catalytic hydrodechlorination process, which is easy to cause catalyst poisoning. The prior art generally adds alkaline substances to protect the active sites of the catalyst. In the prior art, there are literature reports on composite materials of graphitized carbon layers coated with nickel nanoparticles. This composite material with a core-shell structure can efficiently catalyze the hydrogenation of unsaturated groups, but this type of composite material is usually not used for dechlorination.
[0009] Summary of the Invention
[0010] The first object of the present invention is to provide a composite material of carbon-coated nickel-palladium alloy nanoparticles with higher catalytic hydrogenation activity, more stable performance, and stronger resistance to sulfur poisoning. The second object of the present invention is to provide a modified composite material obtained by modifying the above-mentioned composite material with a sulfur-containing compound. The third object of the present invention is to provide a method and application of using the above-mentioned composite material or modified composite material as a catalyst for hydrogenation reaction in the presence of a sulfur-containing compound. The fourth object of the present invention is to provide a method and application of using the above-mentioned composite material or modified composite material as a catalyst for hydrogenation of nitro compounds. The fifth object of the present invention is to provide a method and application of using the above-mentioned composite material or modified composite material as a catalyst for selective hydrogenation of halogenated nitroaromatics. The sixth object of the present invention is to provide a method and application of using the above-mentioned composite material as a catalyst for catalytic hydrogenation removal of organic chlorine.
[0011] To achieve the above objectives, the present invention provides the following technical solutions.
[0012] 1. A composite material of carbon-coated nickel-palladium alloy nanoparticles, the composite material comprising a core-shell structure having a shell layer and a core, the shell layer being a graphitized carbon layer, and the core being nickel-palladium alloy nanoparticles; the composite material having a mass ratio of nickel to palladium of 3:1 to 100:1; and a total mass fraction of nickel and palladium of 1% to 80% based on the mass of the composite material.
[0013] 2. According to the aforementioned composite material; wherein the mass ratio of nickel to palladium is 4:1 to 100:1, preferably 4:1 to 9:1.
[0014] 3. A composite material according to any of the above; wherein, based on the composite material, the total mass fraction of nickel and palladium is 30% to 80%, preferably 50% to 78%.
[0015] 4. A composite material according to any of the preceding claims; wherein the composite material is a mesoporous and / or macroporous material, and the volume of the mesopores and / or macropores accounts for more than 50% of the total pore volume.
[0016] 5. A composite material according to any of the preceding claims; wherein the particle size of the nickel-palladium alloy nanoparticles is 1 nm to 50 nm, preferably 2 nm to 25 nm, and more preferably 3 nm to 15 nm.
[0017] 6. A composite material according to any of the preceding claims; wherein the thickness of the graphitized carbon layer is 0.5 nm to 10 nm, preferably 0.5 nm to 5 nm, and more preferably 1 nm to 5 nm.
[0018] 7. A composite material according to any of the preceding claims; wherein, in the XRD spectrum of the composite material, there is only one diffraction peak in the range of 2θ from 40.1° to 44.5°.
[0019] 8. A composite material according to any of the preceding claims; wherein, in the XRD spectrum of the composite material, a diffraction peak exists in the range of 2θ of 24° to 26°; and / or, in the XRD spectrum of the composite material, a diffraction peak exists in the range of 2θ of 43° to 45°, 50° to 54°, or 75° to 80°.
[0020] 9. A composite material according to any of the preceding claims, wherein the composite material has no diffraction peak within the range of 40.0°±0.1° in its XRD spectrum.
[0021] 10. A method for preparing a composite material of carbon-coated nickel-palladium alloy nanoparticles, comprising the following steps:
[0022] S1: in the presence of a first solvent, mixing a nickel source, a palladium source and an organic polycarboxylic acid to obtain a precursor solution, and then removing the first solvent to obtain a precursor;
[0023] S2 pyrolyzes the precursor in an inert gas.
[0024] 11. According to the aforementioned preparation method; wherein the first solvent is water and / or ethanol, preferably water.
[0025] 12. A preparation method according to any of the above; wherein the nickel source is one or more of nickel acetate, basic nickel carbonate and nickel carbonate.
[0026] 13. A preparation method according to any of the above; wherein the palladium source is palladium acetate, preferably a solution of palladium acetate in glacial acetic acid.
[0027] 14. A preparation method according to any of the above; wherein the organic polycarboxylic acid is one or more of citric acid, ethylenediaminetetraacetic acid, 2,5-pyridinedicarboxylic acid, malic acid, tartaric acid and terephthalic acid.
[0028] 15. A preparation method according to any of the above; wherein, calculated as metal elements, the mass ratio of the nickel source to the palladium source is 3:1 to 100:1, preferably 4:1 to 100:1, and more preferably 4:1 to 9:1.
[0029] 16. A preparation method according to any of the above; wherein the molar ratio of the total amount of the nickel source and the palladium source to the organic polycarboxylic acid is 0.1:1 to 3:1, preferably 0.3:1 to 1.5:1, wherein the total amount of the nickel source and the palladium source is calculated based on the total molar amount of the metal elements.
[0030] 17. A preparation method according to any of the above; wherein, in S2, the pyrolysis temperature is 500°C to 800°C, preferably 500°C to 700°C, and more preferably 550°C to 650°C.
[0031] 18. A preparation method according to any of the preceding claims, comprising an acid treatment step after S2.
[0032] 19. A composite material of modified carbon-coated nickel-palladium alloy nanoparticles; comprising the composite material described in 1 and a sulfur-containing compound supported thereon.
[0033] 20. The modified composite material according to 19, wherein the sulfur-containing compound is thiourea.
[0034] 21. The modified composite material according to 19 or 20, wherein the mass fraction of sulfur element determined by elemental analysis is 0.5% to 5%.
[0035] 22. A method for preparing a composite material of modified carbon-coated nickel-palladium alloy nanoparticles, comprising: a step of loading a sulfur-containing compound on the composite material described in 1.
[0036] 23. The preparation method according to 22; wherein the sulfur-containing compound is thiourea.
[0037] 24. The preparation method according to 22 or 23; wherein, relative to 1 mol of palladium element in the composite material according to 1, the amount of the sulfur-containing compound calculated as sulfur element is 0.01 mol to 20 mol.
[0038] 25. A composite material obtained by the preparation method described in any one of 10 to 18.
[0039] 26. The modified composite material obtained by the preparation method described in any one of 22 to 24.
[0040] 27. Use of any of the aforementioned composite materials or any of the aforementioned modified composite materials as a hydrogenation catalyst for catalytic hydrogenation in the presence of a sulfur-containing compound.
[0041] 28. The use according to 27, wherein the hydrogen and / or the hydrogenation substrate contains sulfur compounds.
[0042] 29. Use of any of the aforementioned composite materials or any of the aforementioned modified composite materials in the catalytic hydrogenation of nitro groups in organic compounds.
[0043] 30. A method for selectively hydrogenating a nitro group in a halonitroaromatic hydrocarbon, comprising the following steps: under liquid-phase catalytic hydrogenation conditions, in the presence of a sulfur-containing compound, contacting hydrogen with the halonitroaromatic hydrocarbon and a catalyst to carry out a liquid-phase catalytic hydrogenation reaction; the catalyst is a composite material described in any one of 1 to 9 and 25; the sulfur-containing compound is thiocyanate and / or thiourea, and the mass ratio of the sulfur-containing compound to the halonitroaromatic hydrocarbon is 1:100 to 1:10000.
[0044] 31. The method according to 30, wherein the mass ratio of the sulfur-containing compound to the halogenated nitroaromatic hydrocarbon is 1:100 to 1:150.
[0045] 32. A method for selectively hydrogenating a nitro group in a halonitroaromatic hydrocarbon, comprising the following steps: contacting hydrogen, the halonitroaromatic hydrocarbon and a catalyst under liquid-phase catalytic hydrogenation conditions to carry out a liquid-phase catalytic hydrogenation reaction; the catalyst being any one of the composite materials described in 19 to 21 and 26.
[0046] 33. The method for selective hydrogenation of nitro groups in halogenated nitroaromatics according to 30 to 32, further comprising the step of separating the composite material or modified composite material by magnetic separation.
[0047] 34. A method for removing organic chlorine by catalytic hydrogenation, comprising the following steps: contacting a chlorine-containing saturated or aromatic organic compound with hydrogen and a catalyst for reaction under liquid-phase catalytic hydrogenation dechlorination reaction conditions; the catalyst is a composite material described in any one of 1 to 9 and 25.
[0048] 35. The dechlorination method according to 33, characterized in that the reaction conditions of the liquid-phase catalytic hydrodechlorination are: temperature range 40-120°C, preferably 60-100°C, and hydrogen pressure range 0.1-3 MPa, preferably 1-2 MPa.
[0049] 36. The dechlorination method according to 33, characterized in that the chlorine-containing aromatic organic compound is one or more selected from monochlorophenol, dichlorophenol, trichlorophenol, chlorinated aromatic hydrocarbons, 2,4-dichlorophenoxyacetic acid and chloronitrobenzene.
[0050] 37. The dechlorination method according to 33, characterized in that the chlorine-containing saturated organic compound is one or more selected from chlorinated saturated aliphatic hydrocarbons.
[0051] 38. The dechlorination method according to 33, characterized in that a solvent is used in the method; the solvent is one or more selected from isopropyl alcohol, ethanol, acetone, tetrahydrofuran, cyclohexane and water.
[0052] 39. The dechlorination method according to 33, characterized in that the mass ratio of the catalyst to the chlorine-containing saturated or aromatic organic compound as the reaction substrate is 0.05-0.8:1, preferably 0.1-0.3:1.
[0053] 40. The dechlorination method according to 33, further comprising the step of separating the composite material by magnetic separation.
[0054] 41. The dechlorination method according to 33, characterized in that the mass ratio of nickel to palladium in the composite material is 3:1 to 10:1, preferably 3:1 to 6:1.
[0055] 42. The dechlorination method according to 33, characterized in that, based on the composite material, the total mass fraction of nickel and palladium is 20% to 80%, preferably 50% to 80%.
[0056] Compared with the prior art, the present invention has the following beneficial technical effects.
[0057] The present invention utilizes the ability of nickel to promote carbon graphitization, combined with the specific complexing effect and reducing ability of organic polycarboxylic acids, thereby, a nickel-palladium alloy can be coated in a carbon shell in the form of nanoparticles in a simple method, and the coating is relatively tight. Therefore, on the basis of a nickel source compound, when further combined with a palladium source compound, a composite material of carbon-coated nickel-palladium alloy nanoparticles can be obtained in a simple method, thereby achieving effective coating of palladium. The composite material has both the stability of nano-carbon materials and the catalytic characteristics of palladium metal nanoparticles. Specifically, the composite material has intrinsic safety, and theoretically there is no problem of metal particle agglomeration, deactivation and loss, nor is there a problem of poisoning of metal active components. In addition, in hydrogenation reactions, it exhibits a catalytic activity higher than that of carbon-coated nickel nanoparticle composite materials.
[0058] The present invention can also conveniently modify the composite material as needed, thereby adjusting the catalytic properties of the composite material and making it suitable for different uses, such as selective hydrogenation of nitro groups in organic compounds; and hydrogenation removal of chlorine atoms in organic compounds. Among them, when selectively hydrogenating nitro groups, whether adding sulfur-containing compounds during the reaction process or pre-loading sulfur-containing compounds on the surface of the composite material, highly selective hydrogenation of nitro groups in organic compounds can be achieved. When hydrodechlorinating organic compounds, the catalyst has inherent resistance to chlorine poisoning and resistance to active metal loss, and therefore can exhibit excellent catalytic effects. On the other hand, the catalytically active component is an alloy and has a low palladium content, but still has the catalytic hydrogenation dechlorination ability of palladium; no base is used in the reaction, and it still has high dechlorination activity; the dechlorination activity is high when the solvent contains water or does not contain water.
[0059] In addition, since nickel is present in the composite material and various modified composite materials of the present invention, the composite material and modified composite material have strong magnetism. After the reaction in which they act as catalysts is completed, magnetic separation can be used to conveniently recover the composite material and modified composite material used as catalysts.
[0060] Other features and advantages of the present invention will be described in detail in the detailed description section. BRIEF DESCRIPTION OF THE DRAWINGS
[0061] Figure 1 is a spherical aberration electron microscope image of the composite material prepared according to Preparation Example 3; Figure 1 (a) spherical aberration electron microscope image, Figure 1 (b) bright field image, Figure 1 (c) mixed distribution diagram of C, Pd, and Ni elements, Figure 1 (d) distribution diagram of C element, Figure 1 (e) distribution diagram of Pd element; Figure 1 (f) distribution diagram of Ni element.
[0062] FIG2 is an XRD pattern of the composite material prepared according to Preparation Example 3.
[0063] FIG3 is an XPS broad spectrum of the composite material prepared according to Preparation Example 4.
[0064] FIG4 is a morphological photograph of the composite material prepared according to Preparation Example 1 in the presence of a magnetic field. DETAILED DESCRIPTION
[0065] The present invention is described in detail below in conjunction with specific embodiments. However, it should be noted that the protection scope of the present invention is not limited by these specific embodiments and principle explanations, but is determined by the claims.
[0066] In the present invention, except for the contents explicitly described, any matters or issues not mentioned are directly applicable to the contents known in the art without any changes. Moreover, any embodiment described herein can be freely combined with one or more other embodiments described herein, and the technical solutions or technical ideas formed thereby are considered part of the original disclosure or description of the present invention and should not be regarded as new content not disclosed or anticipated herein, unless a person skilled in the art considers that the combination is obviously unreasonable.
[0067] All features disclosed in the present invention may be combined in any combination, and such combinations should be understood as disclosed or described in the present invention. Unless a person skilled in the art considers such combination to be obviously unreasonable, such combinations should be considered as specifically disclosed and described in the present invention. Unless otherwise specified, the numerical values disclosed in this specification include not only the numerical values specifically disclosed in the examples but also the endpoints of the numerical ranges in the specification. Any combination of these numerical values should be considered as the range disclosed or described in the present invention.
[0068] Technical and scientific terms in the present invention shall be understood according to their definitions if they are defined, and shall be understood according to their general meanings in the art if they are not defined.
[0069] The term "graphitized carbon layer" refers to a layered carbon structure, rather than an amorphous structure, that can be clearly observed under high-resolution transmission electron microscopy.
[0070] The term "mesopores" is defined as pores with a pore diameter in the range of 2 nm to 50 nm. Pores with a pore diameter less than 2 nm are defined as micropores, and pores with a pore diameter greater than 50 nm are defined as macropores.
[0071] The term "acid treatment" refers to the operation of acid washing the product generated after the high-temperature pyrolysis step at a temperature close to the boiling temperature of the acid solution when preparing the composite material of carbon-coated nickel-palladium alloy nanoparticles.
[0072] The term "inert gas" is defined as a gas that does not have a noticeable effect on the catalytic hydrogenation performance of the composite material, including but not limited to nitrogen, helium, argon, etc.
[0073] The term "soluble" means soluble in the solvent in which it is used.
[0074] The notation "PPMw" stands for parts per million by weight.
[0075] The term "optionally" means that it can be present or not, such as A and optionally B, which means "A is present and B is absent" or "both A and B are present".
[0076] The first aspect of the present invention provides a composite material of carbon-coated nickel-palladium alloy nanoparticles, which contains a core-shell structure having a shell layer and a core, wherein the shell layer is a graphitized carbon layer and the core is a nickel-palladium alloy nanoparticle; in the composite material, the mass ratio of nickel to palladium is 3:1 to 100:1; and based on the mass of the composite material, the total mass fraction of nickel and palladium is 1% to 80%.
[0077] According to the first aspect, the composite material is composed of nickel, palladium, carbon, and oxygen. It should be understood that the composite material of the present invention is primarily composed of zero-valent nickel, palladium, and carbon. Because the carbon source in the synthetic raw materials contains oxygen, a small amount of oxygen is inevitably incorporated into the surface carbon of the composite material. The composite material also absorbs oxygen on its surface when stored in air, and small or trace amounts of nickel and palladium may exist in an oxidized state. Impurities in the synthetic raw materials may also result in the presence of small or trace amounts of other elements. However, these factors do not significantly affect the performance of the composite material. The present invention does not consider it necessary to specify these factors.
[0078] According to the composite material of the first aspect, the mass ratio of nickel to palladium is 3:1 to 100:1, preferably 4:1 to 100:1; if a relatively higher catalytic hydrogenation activity is required, the mass ratio of nickel to palladium can be further controlled to be between 4:1 and 9:1, and can also be controlled to be between 3:1 and 10:1, or between 3:1 and 6:1. Within the above ratio range, the XRD spectrum of the composite material only has diffraction peaks of the fccNiPd alloy. If the palladium content is too high, characteristic peaks of elemental palladium will appear in the XRD spectrum, and these elemental palladium are not tightly coated by carbon and do not have the ability to resist agglomeration and poisoning deactivation.
[0079] According to the composite material of the first aspect, the total mass fraction of nickel and palladium, based on the composite material, is 1% to 80%, preferably 20% to 80%, more preferably 30% to 80%, further preferably 50% to 80%, and more preferably 50% to 78%. The present invention has found that even doping nickel with approximately 1% palladium significantly improves the catalytic hydrogenation ability of the composite material. In some embodiments of the present invention, even after acid treatment, the total mass fraction of nickel and palladium in the composite material can still reach approximately 75%.
[0080] According to the composite material of the first aspect, the shell structure is composed of a graphitized carbon layer. In other words, the shell structure of the present invention is not doped with other elements. However, it should be noted that the composite material of the present invention may contain trace amounts of amorphous carbon. This amorphous carbon exists only as an impurity and is not intended to be limiting in the present invention.
[0081] According to the composite material of the first aspect, it is a mesoporous and / or macroporous material, and the volume of mesopores and / or macropores accounts for more than 50% of the total pore volume. In some embodiments, the composite material has a mesoporous structure or a mesoporous and macroporous structure. It is well known in the art that pore structure is a macroscopic property of the catalyst.
[0082] The composite material according to the first aspect has a specific surface area of 50 m 2 / g~500m 2 / g, preferably 100m 2 / g~300m 2 / g.
[0083] According to the composite material of the first aspect, under transmission electron microscopy, the particle size of the nickel-palladium alloy nanoparticles is 1 nm to 50 nm, generally between 2 nm and 25 nm, and preferably between 3 nm and 15 nm. In some embodiments, the particle size distribution of the nickel-palladium alloy nanoparticles is relatively narrow, generally between 4 nm and 10 nm.
[0084] According to the composite material of the first aspect, under transmission electron microscopy observation, the thickness of the graphitized carbon layer is 0.5 nm to 10 nm, preferably 0.5 nm to 5 nm, and generally 1 nm to 5 nm.
[0085] According to the composite material of the first aspect, the core-shell structure is spherical or quasi-spherical.
[0086] According to the composite material of the first aspect, in some embodiments, the XRD spectrum of the composite material has only one diffraction peak within the range of 40.1° to 44.5° at 2θ.
[0087] According to the composite material of the first aspect, in the XRD spectrum of the composite material, there is a diffraction peak in the range of 2θ of 24° to 26°; and / or, in the XRD spectrum of the composite material, there is a diffraction peak in the range of 2θ of 43° to 45°, 50° to 54°, or 75° to 80°.
[0088] According to the composite material of the first aspect, in the XRD spectrum of the composite material, there is no diffraction peak within the range of 40.0°±0.1°.
[0089] The second aspect of the present invention provides a composite material of modified carbon-coated nickel-palladium alloy nanoparticles (hereinafter sometimes referred to as a modified composite material), which comprises the composite material of the first aspect and a sulfur-containing compound supported thereon.
[0090] The modified composite material according to the second aspect is composed of the composite material according to the first aspect and a sulfur-containing compound supported thereon.
[0091] According to the modified composite material of the second aspect, the molecular weight of the sulfur-containing compound is generally less than 200. The sulfur-containing compound can be either an organic sulfur compound or an inorganic sulfur compound; in the organic sulfur compound, the carbon-sulfur bond can be either a double bond or a single bond. The sulfur-containing compound is preferably thiourea.
[0092] Taking the modified composite material of the second aspect as a benchmark, the mass fraction of sulfur obtained by elemental analysis may be 0.1% to 10%, preferably 0.5% to 5%, and more preferably 0.8% to 1.8%.
[0093] The third aspect of the present invention provides a method for preparing the composite material of the first aspect, comprising the following steps:
[0094] S1: in the presence of a first solvent, mixing a nickel source, a palladium source and an organic polycarboxylic acid to obtain a precursor solution, and then removing the first solvent to obtain a precursor;
[0095] S2 pyrolyzes the precursor in an inert gas.
[0096] According to the preparation method of the third aspect, the first solvent is water and / or ethanol, preferably water.
[0097] According to the preparation method of the third aspect, the nickel source is a soluble nickel salt, which can be one or more of nickel acetate, basic nickel carbonate and nickel carbonate.
[0098] According to the preparation method of the third aspect, the palladium source is a palladium-containing solution, which can be a solution of palladium acetate, preferably a solution of palladium acetate in glacial acetic acid.
[0099] According to the preparation method of the third aspect, the organic polycarboxylic acid provides a carbon source for the composite material and acts as a complexing agent. Preferably, the organic polycarboxylic acid contains hydroxyl groups in the molecule. The organic polycarboxylic acid can be one or more of citric acid, ethylenediaminetetraacetic acid, 2,5-pyridinedicarboxylic acid, tartaric acid, or terephthalic acid, preferably citric acid.
[0100] According to the preparation method of the third aspect, the mass ratio of the nickel source to the palladium source, calculated as metal elements, is 3:1 to 100:1, preferably 4:1 to 100:1, and more preferably 4:1 to 9:1.
[0101] According to the preparation method of the third aspect, in S1, the molar ratio of the total amount of the nickel source and the palladium source to the organic polycarboxylic acid is 0.1:1 to 3:1, preferably 0.3:1 to 1.5:1, wherein the total amount of the nickel source and the palladium source is calculated based on the total molar amount of the metal elements.
[0102] According to the preparation method of the third aspect, in S1, the precursor solution can be prepared as follows: a nickel source, a palladium source and an organic polycarboxylic acid as a carbon source are added to water and / or ethanol and stirred at 40°C to 100°C for 8h to 16h, preferably at 50°C to 90°C for 10h to 12h; wherein the palladium source is provided in the form of a glacial acetic acid solution of 0.5g to 1.1g of palladium acetate per 100mL of glacial acetic acid, and the nickel source is provided in the form of nickel acetate (which may or may not contain crystal water). At this point, the amount of the nickel source is adjusted so that the mass ratio of the nickel source to the palladium source is 3: 1 to 100: 1, preferably 4: 1 to 100: 1, more preferably 4: 1 to 9: 1, based on the metal element; the amount of the polycarboxylic acid is adjusted so that the molar ratio of the total amount of the nickel source and the palladium source to the organic polycarboxylic acid is 0.1: 1 to 3: 1, preferably 0.3: 1 to 1.5: 1.
[0103] According to the preparation method of the third aspect, in S1, the first solvent in the precursor solution is preferably removed by direct evaporation. For example, the first solvent in the precursor solution can be evaporated to dryness on a rotary evaporator and / or dried in an oven.
[0104] According to the preparation method of the third aspect, S2 satisfies at least one of the following conditions: the pyrolysis temperature is 500°C to 800°C, preferably 500°C to 700°C, and more preferably 550°C to 650°C; and / or the pyrolysis time is 1h to 4h, preferably 1.5h to 3h; and / or the heating rate is 1°C / min to 10°C / min, preferably 2°C / min to 5°C / min.
[0105] According to the preparation method of the third aspect, in S2, the inert gas may be nitrogen, argon or helium.
[0106] The preparation method according to the third aspect also includes an optional acid treatment step after S2. The present invention has no restrictions on the type of acid used for acid treatment, the amount used and the treatment time, and those skilled in the art can select according to existing knowledge and / or simple experiments. Generally, a non-oxidizing strong acid is used for acid treatment, such as hydrochloric acid or sulfuric acid. In some embodiments of the present invention, hydrochloric acid is used, the concentration can be 0.5mol / L~2mol / L, the temperature can be 60℃~100℃, which can be close to the boiling temperature of the acid solution, and the time can be 3h~24h, or 3h~10h.
[0107] The preparation method according to the third aspect further comprises a post-processing step of acid washing the product, such as filtering, washing, drying, etc.
[0108] The fourth aspect of the present invention provides a method for preparing the modified composite material of the second aspect (hereinafter sometimes also referred to as "method for preparing the modified composite material"), which comprises the step of contacting the composite material of the first aspect with a sulfur-containing compound.
[0109] In the modified composite material obtained by the method for preparing the modified composite material of the present invention, the composite material of the first aspect is loaded with a sulfur-containing compound.
[0110] According to the fourth aspect of the method for preparing the modified composite material, there are no particular limitations on the contacting method for the sulfur-containing compound. Those skilled in the art may employ any known method to contact the composite material of the first aspect with the sulfur-containing compound to load the sulfur-containing compound onto the composite material of the first aspect. A preferred method is to first disperse the composite material of the first aspect in a second solvent, dissolve the sulfur-containing compound in a third solvent to form a solution, and then mix the two liquids. To ensure sufficient and uniform contact between the two liquids, mechanical stirring or ultrasonic mixing can be employed, or a combination of ultrasonic mixing followed by mechanical stirring can be employed. The contact time can range from 12 to 24 hours.
[0111] According to the fourth aspect of the method for preparing a modified composite material, the second solvent is water and / or an alcohol solvent, preferably water.
[0112] According to the fourth aspect of the method for preparing a modified composite material, the third solvent is water and / or an alcohol solvent, preferably water.
[0113] In some embodiments, the sulfur-containing compound is thiourea. In some embodiments, the first solvent and the second solvent are preferably water. In some embodiments, the ultrasonication time is 0.5 h to 3 h, the mechanical stirring time is 2 h to 24 h, and the load temperature is 25° C. to 90° C.
[0114] According to the fourth aspect of the method for preparing the modified composite material, the type and amount of the sulfur-containing compound can vary widely. The present inventors have discovered that treating the composite material of the first aspect with a sulfur-containing compound can significantly affect the selectivity during the catalytic hydrogenation reaction. Those skilled in the art can select the appropriate sulfur-containing compound and determine its amount through experiments based on actual needs. However, different small-molecule sulfur-containing compounds have different effects on the composite material. For example, when thiourea is used, the selectivity in the catalytic hydrogenation reaction of para-halonitrobenzene can reach 100%.
[0115] According to the fourth aspect of the method for preparing the modified composite material, the sulfur-containing compound can be loaded by impregnation. To achieve higher selectivity, the amount of the sulfur-containing compound, calculated as sulfur element, can be 0.01 mol to 20 mol, preferably 0.3 mol to 5 mol, relative to 1 mol of palladium element in the composite material of the first aspect.
[0116] The preparation method according to the fourth aspect further includes the steps of post-processing the loaded product, such as filtering, washing, drying, etc.
[0117] The fifth aspect of the present invention provides a composite material of carbon-coated nickel-palladium alloy nanoparticles prepared by the preparation method of any of the aforementioned aspects.
[0118] The sixth aspect of the present invention provides a composite material of modified carbon-coated nickel-palladium alloy nanoparticles prepared by the method for preparing the modified composite material according to any of the aforementioned aspects.
[0119] The seventh aspect of the present invention provides use of the composite material of any of the aforementioned aspects or the modified composite material of any of the aforementioned aspects as a hydrogenation catalyst when the catalytic hydrogenation system contains sulfur.
[0120] According to the application of the seventh aspect, hydrogen and / or hydrogenation substrates may contain sulfur. The production of hydrogen from fossil fuels is the main way to obtain industrial hydrogen in the petrochemical industry. Such raw materials will inevitably produce sulfur-containing compounds during the hydrogen production process. Although pressure swing adsorption (PSA) technology can make the hydrogen purity reach more than 99.9%, there are still sulfur-containing compounds in the hydrogen; some reaction substrates themselves contain sulfur, such as thionitroaromatics; sulfur-containing impurities may also exist in the reaction substrates, and the impact of these sulfur-containing compounds on the hydrogenation catalyst cannot be ignored. The present invention has found that even if the composite material of the present invention is treated with very high concentration and highly toxic thiourea, it still has a very high catalytic hydrogenation activity, so it has unique advantages when used as a hydrogenation catalyst in a catalytic hydrogenation system under the presence of these sulfur-containing compounds.
[0121] According to the seventh application, the hydrogenation substrate contains one or more functional groups selected from the group consisting of a nitro group, a carbon-carbon double bond, a carbon-carbon triple bond, a ketone group, an aldehyde group, and an aromatic ring. Prior art has already achieved hydrogenation of these functional groups using carbon-coated nickel nanoparticle composite materials or modified composite materials. The composite materials and modified composite materials of the present invention have higher catalytic hydrogenation activity than the carbon-coated nickel nanoparticle composite materials, and thus can also catalytically hydrogenate these functional groups contained in organic compounds.
[0122] An eighth aspect of the present invention provides a method for selectively hydrogenating the nitro group of a thionitroaromatic hydrocarbon, comprising the following steps: contacting hydrogen, the thionitroaromatic hydrocarbon, and a catalyst under liquid-phase catalytic hydrogenation conditions to carry out a liquid-phase catalytic hydrogenation reaction; the catalyst is the composite material of the first or fifth aspect or the modified composite material of the second or sixth aspect.
[0123] According to the eighth aspect of the application, the thionitroarene has a structure as shown in formula (I):
[0124] wherein X is selected from one or more of sulfur and sulfone groups, R1 is selected from one or more of hydrogen, C1-C6 hydrocarbon group, C1-C3 halogenated hydrocarbon group, C1-C3 hydroxyl hydrocarbon group, sulfhydryl group, C6-C10 aryl group and C6-C10 arylsulfenyl group, R2 is selected from one or more of hydrogen, C1-C6 hydrocarbon group, hydroxyl group, carboxyl group, halogen group, amino group, sulfhydryl group, C6-C10 aryl group, C6-C10 arylsulfenyl group and nitro group, and the aryl group is unsubstituted or substituted with one or more of the following groups: nitro group, C1-C6 hydrocarbon group, hydroxyl group, carboxyl group, halogen group, amino group or amino group.
[0125] In one embodiment of the present invention, the hydrocarbon group may be an alkyl, alkenyl or alkynyl, preferably an alkyl. In one embodiment of the present invention, the aryl group may be phenyl or naphthyl. In one embodiment of the present invention, the halogen and the halogen in the halogenated group may be fluorine, chlorine, bromine or iodine.
[0126] Common thionitroaromatics include 4-nitrothioanisole, 2-nitrodiphenyl sulfide, 4-nitrothiophenol, 3,3'-dinitrodiphenyl sulfone, and 4,4'-dinitrodiphenyl sulfone. Existing technologies have already achieved hydrogenation of these compounds using carbon-coated nickel nanoparticle composites. The composite materials and modified composite materials of the present invention exhibit higher catalytic hydrogenation activity than carbon-coated nickel nanoparticle composites, and therefore can also catalytically hydrogenate these organic compounds.
[0127] The ninth aspect of the present invention provides a method for selectively hydrogenating a nitro group in a halogenated nitroaromatic hydrocarbon, comprising the following steps: under liquid-phase catalytic hydrogenation conditions, in the presence of a sulfur-containing compound, hydrogen is contacted with a halogenated nitroaromatic hydrocarbon and a catalyst to carry out a liquid-phase catalytic hydrogenation reaction; the catalyst is the composite material of the first or fifth aspect of the present invention; the sulfur-containing compound is thiocyanate and / or thiourea, and the mass ratio of the sulfur-containing compound to the halogenated nitroaromatic hydrocarbon is 1:100 to 1:10000.
[0128] The present invention has discovered that the addition of a sulfur-containing compound can significantly affect the selectivity of the catalytic hydrogenation reaction. Those skilled in the art can select the appropriate sulfur-containing compound and determine its dosage based on actual needs through experiments. According to the method of the ninth aspect, the molecular weight of the sulfur-containing compound is generally below 200, which makes operation more convenient; the dosage range is generally wide, making control easier. However, different small-molecule sulfur-containing compounds have different effects on reaction selectivity. For example, in the selective hydrogenation of para-chloronitrobenzene to produce chloroaniline, the selectivity of sodium sulfide is only 70% to 80%, while the selectivity of thiocyanate is over 98%, and the selectivity of thiourea can reach 100%.
[0129] According to the method of the ninth aspect, the thiocyanate is usually potassium thiocyanate and / or sodium thiocyanate.
[0130] According to the method of the ninth aspect, the mass ratio of the sulfur-containing compound to the halogenated nitroaromatic hydrocarbon is preferably 1:100 to 1:150.
[0131] According to the method of the ninth aspect, the mass ratio of the catalyst to the halogenated nitroaromatic hydrocarbon is 1:1 to 1:15, preferably 1:1 to 1:7.
[0132] According to the method of the ninth aspect, the conditions for the liquid-phase catalytic hydrogenation are: temperature of 20°C to 100°C, preferably 40°C to 60°C; and / or hydrogen pressure of 0.5MPa to 4MPa, preferably 0.8MPa to 2MPa.
[0133] According to the method of the ninth aspect, the liquid-phase hydrogenation reaction uses a solvent, and the solvent is selected from one or more of isopropanol, ethanol, acetone and water, preferably isopropanol and / or water, and more preferably a mixed solvent with a volume ratio of isopropanol to water of 10:1 to 5:1.
[0134] According to the method of the ninth aspect, the halogenated nitroaromatic hydrocarbon is chloronitrobenzene, preferably m-chloronitrobenzene or p-chloronitrobenzene.
[0135] The tenth aspect of the present invention provides another method for selectively hydrogenating the nitro group in a halonitroaromatic hydrocarbon, comprising the following steps: under liquid-phase catalytic hydrogenation conditions, hydrogen, a halonitroaromatic hydrocarbon and a catalyst are contacted to carry out a liquid-phase catalytic hydrogenation reaction; the catalyst is the modified composite material of the second or sixth aspect of the present invention.
[0136] According to the method of the tenth aspect, the mass ratio of the catalyst to the halogenated nitroaromatic hydrocarbon is 1:1 to 1:15, preferably 1:1 to 1:7.
[0137] According to the method of the tenth aspect, the conditions for the liquid-phase catalytic hydrogenation are: temperature of 20°C to 100°C, preferably 40°C to 60°C; and / or hydrogen pressure of 0.5MPa to 4MPa, preferably 0.8MPa to 2MPa.
[0138] According to the method of the tenth aspect, the liquid-phase hydrogenation reaction uses a solvent, and the solvent is selected from one or more of isopropanol, ethanol, acetone and water, preferably isopropanol and / or water.
[0139] According to the method of the tenth aspect, the halogenated nitroaromatic hydrocarbon is chloronitrobenzene, preferably m-chloronitrobenzene or p-chloronitrobenzene.
[0140] The eleventh aspect of the present invention provides a method for catalytic hydrogenation removal of organic chlorine, comprising: under the reaction conditions of liquid-phase catalytic hydrogenation dechlorination, contacting a chlorine-containing saturated or aromatic organic compound with hydrogen and a catalyst for reaction; the catalyst is the composite material of the first or fifth aspect of the present invention.
[0141] According to the method of the eleventh aspect, in the composite material, the mass ratio of nickel to palladium is 3:1 to 10:1, preferably 3:1 to 8:1, and more preferably 3:1 to 6:1.
[0142] According to the method of the eleventh aspect, in the composite material, based on the composite material, the total mass fraction of nickel and palladium is 20% to 80%, preferably 30% to 80%, and more preferably 50% to 80%.
[0143] According to the method of the eleventh aspect, the reaction conditions of the liquid-phase catalytic hydrodechlorination are: temperature range 40-120° C., preferably 60-100° C., and hydrogen pressure range 0.1-3 MPa, preferably 1-2 MPa.
[0144] According to the method of the eleventh aspect, the chlorine-containing aromatic organic compound preferably has a chlorine atom directly connected to the aromatic ring, and is more preferably selected from one or more of monochlorophenol, dichlorophenol, trichlorophenol, chlorinated aromatic hydrocarbons, 2,4-dichlorophenoxyacetic acid and chloronitrobenzene.
[0145] According to the method of the eleventh aspect, the chlorine-containing saturated organic compound is one or more selected from chlorinated saturated aliphatic hydrocarbons.
[0146] According to the method of the eleventh aspect, a solvent may or may not be used in the method. Whether a solvent is used depends on whether the reaction substrate itself is in a suitable liquid state under hydrogenation conditions and the needs of those skilled in the art; the choice of solvent depends on ensuring that the reaction substrate can be dissolved, which are all known in the art. If used to treat organic chlorides dissolved in wastewater, water itself is the solvent. In addition, the solvents that can be used in the eleventh aspect of the present invention include, but are not limited to, one or more of isopropanol, ethanol, acetone, tetrahydrofuran, cyclohexane and water. If the organic chloride is soluble in alcohol but insoluble in water, a mixed solvent of alcohol and water is preferably used, and the volume ratio of alcohol to water is preferably 10:1 to 5:1.
[0147] According to the method of the eleventh aspect, the ratio of the catalyst to the chlorine-containing saturated or aromatic organic compound as the reaction substrate is 0.05 to 0.8:1 by mass, preferably 0.1 to 0.3:1.
[0148] According to the method of the eleventh aspect, in order to ensure the dechlorination efficiency, no sulfur-containing compounds are present in the reaction system.
[0149] According to the method of the eleventh aspect, the dechlorination method can be used in the fields of sewage dechlorination treatment, crude oil dechlorination pretreatment, organic by-product dechlorination recovery and organic synthesis.
[0150] Since the composite material and modified composite material of the present invention have strong magnetism, in the above methods of the present invention, after the reaction is completed, magnetic separation can be used to conveniently recover the composite material and modified composite material used as a catalyst.
[0151] Analysis and characterization
[0152] The surface morphology of the materials was characterized by high-resolution transmission electron microscopy (HRTEM, JEOL Ltd., JEM-2100) at an accelerating voltage of 200 kV.
[0153] The distribution of elements in the material was characterized by spherical aberration electron microscopy (STEM). The spherical aberration electron microscope used was JEM-ARM200F (JEOL Ltd.) and the test conditions were: acceleration voltage 200 kV.
[0154] XRD is used to obtain information such as the composition of the material and the structure or morphology of the atoms or molecules within the material. The XRD diffractometer used is an X'Pert Pro X-ray diffractometer purchased from PA Nalytical in the Netherlands. The test conditions are: Cu target, Kα radiation, tube voltage of 40 kV, tube current of 40 mA, and a 2θ scanning range of 5° to 80°.
[0155] X-ray photoelectron spectroscopy (XPS) was used to detect the elements on the material surface. The X-ray photoelectron spectrometer used was an ESCALab220i-XL from VG Scientific, equipped with Avantage V5.926 software. The X-ray photoelectron spectroscopy test conditions were: monochromatized A1Kα X-rays at 330 W of power, and a base vacuum of 3 × 10-9 mbar.
[0156] The specific surface area and pore size distribution of the materials were determined by the Brunauer-Emmett-Taller method (BET, Quantachrome AS-6B analyzer).
[0157] The carbon, hydrogen, oxygen, nitrogen, and sulfur content were measured on an Elementar Vario EL Cube elemental analyzer. The procedure was as follows: approximately 5 mg of sample was weighed into a tin cup, placed in an automatic sample feeder, and then fed through a ball valve into a combustion tube for combustion at 1000°C (a helium purge was used to eliminate atmospheric interference during injection). The carbon, hydrogen, nitrogen, and sulfur in the sample were converted to carbon dioxide, water, nitrogen, and sulfur dioxide, respectively. The mixed gases were separated by a chromatographic column and detected by a thermal conductivity cell. For oxygen determination, the sample was pyrolyzed in a high-temperature pyrolysis tube filled with carbon powder, converting oxygen to carbon monoxide. The pyrolysis products were then carried by a carrier gas to a series-connected scrubber to remove acid gases and water vapor before being detected by an infrared detector.
[0158] The content of nickel and palladium elements was determined by inductively coupled plasma optical emission spectrometry (ICP-OES). The specific method is as follows: (1) Nitrolysis: 10 mg of the catalyst sample was placed in a flask, 16 mL of freshly prepared aqua regia was added, and a magnetic stirrer was added. The flask was placed in an oil bath and refluxed at 120°C for 12 h. After cooling to room temperature, the solution was aspirated with a glass syringe and filtered with a disposable filter with a pore size of 0.22 μm. The filtrate was added to a 500 mL volumetric flask and made up to volume with ultrapure water. (2) Content test: 10 mL of the solution after nitrolysis was taken and the metal content was tested using an Agilent 5110 instrument.
[0159] Unless otherwise specified, all reagents used in the present invention are of analytical grade and commercially available.
[0160] Preparation Examples 1 to 5 are used to illustrate the composite material and its preparation method of the present invention.
[0161] Preparation Example 1
[0162] 1) Weigh 0.040 g of palladium acetate and 3 mL of glacial acetic acid. Add these to 170 mL of deionized water and stir at 50°C to dissolve. Using a nickel source to palladium source mass ratio of 100:1 (calculated as metal elements) and a total nickel-palladium to complexing agent molar ratio of 1:1, weigh citric acid monohydrate and nickel acetate tetrahydrate and add them to the solution. Stir at 70°C to obtain a homogeneous solution. Continue heating and evaporating to dryness. Grind the solid to obtain the precursor.
[0163] 2) The precursor obtained in step 1) was placed in a porcelain boat, and then the porcelain boat was placed in the constant temperature zone of a tube furnace, nitrogen was introduced at a flow rate of 150 mL / min, and the temperature was increased to 600°C at a rate of 2.5°C / min. After keeping the temperature constant for 2 hours, heating was stopped and the mixture was cooled to room temperature under a nitrogen atmosphere to obtain a pyrolysis product.
[0164] 3) The pyrolysis product obtained in step 2) was added to 200 mL of 1 mol / L HCl solution, stirred and refluxed at 90° C. for 4 h, the solution was filtered, washed with deionized water until neutral, and the powder was placed in an oven at 100° C. and dried for 2 h to obtain a carbon-coated nickel-palladium nanocomposite material.
[0165] Preparation Example 2
[0166] The method of Preparation Example 1 is followed, except that in step 1), 0.657 g of palladium acetate and 35 mL of glacial acetic acid are weighed. Add to 170 mL of deionized water and stir to dissolve at 50°C. According to the mass ratio of nickel source to palladium source of 17:3 (calculated as metal elements), the molar ratio of the total molar amount of nickel palladium to the complexing agent is 1:1, citric acid monohydrate and nickel acetate tetrahydrate are weighed and added to the above solution, stirred at 70°C to obtain a homogeneous solution, and continued to heat and evaporate to dryness. The solid is ground to obtain a precursor. The rest is the same as in Preparation Example 1 to obtain a carbon-coated nickel palladium nanocomposite material.
[0167] Preparation Example 3
[0168] The method of Preparation Example 1 is followed, except that in step 1), 0.943 g of palladium acetate and 60 mL of glacial acetic acid are weighed. Add to 170 mL of deionized water and stir to dissolve at 50 ° C. According to the mass ratio of nickel source to palladium source of 4: 1 (calculated as metal element), the molar ratio of the total molar amount of nickel palladium to the complexing agent is 1: 1, citric acid monohydrate and nickel acetate tetrahydrate are weighed and added to the above solution, stirred at 70 ° C to obtain a homogeneous solution, and continued to heat and evaporate to dryness, and the solid is ground to obtain a precursor. The rest is the same as in Preparation Example 1 to obtain a carbon-coated nickel palladium nanocomposite material.
[0169] Preparation Example 4
[0170] This preparation example is used to illustrate the sulfur-containing carbon-coated nickel-palladium nanocomposite material.
[0171] 0.5 g of the composite material obtained according to the method of Preparation Example 3 was weighed and added to 10 mL of deionized water, and ultrasonicated for 1 h to uniformly disperse the nanomaterial; 0.036 g of thiourea was weighed and added to 10 mL of deionized water, and ultrasonicated for 1 h to completely dissolve the thiourea; the above two liquids were mixed and ultrasonicated for 1 h, and then mechanically stirred for 12 h at a speed of 800 rpm, filtered, washed with deionized water 5 times, and freeze-dried to obtain a carbon-coated nickel-palladium nanocomposite material (modified composite material) loaded with a sulfur-containing compound (thiourea). The mass percentage of sulfur element measured by elemental analysis was 1.67%, and the specific surface area of the material measured by BET was 145.0 m 2 / g.
[0172] Preparation Example 5
[0173] 1) Weigh 0.411 g of palladium acetate and 30 mL of glacial acetic acid, add them to 170 mL of deionized water, and stir to dissolve at 50°C. Citric acid monohydrate and nickel acetate tetrahydrate are weighed and added to the solution, with a nickel source to palladium source mass ratio of 9:1 (calculated as metal elements) and a total nickel-palladium to complexing agent molar ratio of 1:1. Stir at 70°C to obtain a homogeneous solution, which is then evaporated to dryness. Grind the solid to obtain the precursor.
[0174] 2) The precursor obtained in step 1) was placed in a porcelain boat, and then the porcelain boat was placed in the constant temperature zone of a tube furnace, nitrogen was introduced at a flow rate of 150 mL / min, and the temperature was increased to 600°C at a rate of 2.5°C / min. After keeping the temperature constant for 2 hours, heating was stopped and the mixture was cooled to room temperature under a nitrogen atmosphere to obtain a pyrolysis product.
[0175] 3) The pyrolysis product obtained in step 2) was added to 200 mL of 1 mol / L HCl solution, stirred and refluxed at 90° C. for 4 h, the solution was filtered, washed with deionized water until neutral, and the powder was placed in an oven at 100° C. and dried for 2 h to obtain a carbon-coated nickel-palladium alloy nanocomposite material.
[0176] Examples 1 to 3 are used to illustrate the method of synthesizing p-chloroaniline by selective hydrogenation of p-chloronitrobenzene using the composite material of the present invention as a catalyst.
[0177] 100 mg of the carbon-coated nickel-palladium nanocomposite prepared according to the method of Preparation Examples 1 to 3, 315 mg of p-chloronitrobenzene, 2.4 mg of thiourea, 27 mL of isopropanol, and 3 mL of water were added to the reactor. After H2 was introduced into the reactor for replacement 4 times, the temperature was raised under low pressure with stirring to the predetermined reaction temperature of 60°C. H2 was introduced again to make the pressure in the reactor 1.0 MPa. The reaction was continued until the pressure did not change for 10 minutes. After cooling to room temperature, the pressure was released, and the reactor was opened to remove the product for chromatographic analysis. The conversion rate of the reactants and the selectivity of the target product were calculated by the following formula:
[0178] Conversion rate = mass of reactants reacted / amount of reactants added × 100%
[0179] Selectivity = target product mass / reaction product mass × 100%
[0180] The reaction time in Example 1 was 180 minutes until the pressure remained unchanged for 10 minutes. After analysis of the product, it was found that the conversion rate of p-chloronitrobenzene was 100% and the selectivity of p-chloroaniline was 100%.
[0181] The reaction time in Example 2 was 77 minutes until the pressure remained unchanged for 10 minutes. After analysis of the product, the conversion rate of p-chloronitrobenzene was 100%, and the selectivity of p-chloroaniline was 100%.
[0182] The reaction time in Example 3 was 50 minutes until the pressure remained unchanged for 10 minutes. After analysis of the product, the conversion rate of p-chloronitrobenzene was 100%, and the selectivity of p-chloroaniline was 100%.
[0183] Example 4
[0184] The method of Example 3 was followed, except that thiourea was replaced by potassium thiocyanate. The remaining conditions were the same as those of Example 3. Under the same conditions, the hydrogenation reaction of p-chloronitrobenzene was catalyzed. The conversion rate of p-chloronitrobenzene was 100%, and the selectivity of p-chloroaniline was 98.84%.
[0185] Example 5
[0186] The method of Example 1 was followed, except that thiourea was not added. The other conditions were the same as those of Example 1. Under the same conditions, the catalytic hydrogenation reaction of p-chloronitrobenzene was carried out. The conversion rate of p-chloronitrobenzene was 100%, the selectivity of p-chloroaniline was 65.5%, and the remainder was aniline.
[0187] Example 6
[0188] The method of Example 3 was followed, except that the modified composite material of Preparation Example 4 was used as the catalyst in an amount of 100 mg, thiourea was not added, and p-nitrochlorobenzene was used in an amount of 157.5 mg. All other conditions were the same as in Example 3. Under the same conditions, the p-chloronitrobenzene was catalyzed for hydrogenation, with a p-chloronitrobenzene conversion of 100% and a p-chloroaniline selectivity of 100%.
[0189] Comparative Example 1
[0190] The catalytic hydrogenation reaction was carried out under the same conditions as in Example 1, except that the catalyst was replaced with a commercial palladium-carbon catalyst (10 wt % Pd, 55% water content). The conversion of p-chloronitrobenzene was 0%. This indicates that the conventional supported Pd catalyst completely loses its catalytic activity in the presence of sulfur-containing poisons and lacks resistance to sulfur poisoning.
[0191] Comparative Example 2
[0192] The method of Example 1 was followed, except that the catalyst was replaced with a commercial palladium-carbon catalyst (10 wt% Pd, 55% water content) and thiourea was omitted. Under the same conditions as in Example 1, the p-chloronitrobenzene hydrogenation reaction was conducted. The p-chloronitrobenzene conversion was 100%, and the p-chloroaniline content in the product was approximately 0. This indicates that conventional supported Pd catalysts have poor selectivity for p-chloroaniline.
[0193] Table 1 Nickel and palladium mass fractions and nickel-palladium mass ratios in the composite materials of the present invention
[0194] As can be seen from Table 1, despite the acid wash and the large variation in the mass ratio of nickel to palladium, the metal content in the composite materials of the preparation examples is approximately 75%. That is, the composite materials of the present invention have a high metal content and are resistant to acid corrosion, which can avoid the loss of active metal when used in an acidic environment.
[0195] As can be seen from the spherical aberration electron microscopy images in Figure 1, in the composite material prepared according to Preparation Example 3, the metal nanoparticles are a mixture of nickel and palladium at the atomic scale. The other preparation examples of the present invention also have the same characteristics, that is, the metal nanoparticles in the composite material of the present invention are nickel-palladium alloys; the other preparation examples of the present invention also have the same characteristics. As can be seen from the image in the upper left corner of Figure 1, the particle size of the metal nanoparticles is between 2nm and 25nm, the thickness of the graphitized carbon layer is between 1nm and 5nm, and the core-shell structure of the carbon-coated nickel-palladium nanoparticles is spherical or quasi-spherical; the other preparation examples of the present invention also have the same characteristics.
[0196] As can be seen from the XRD pattern in Figure 2, the composite material prepared according to Preparation Example 3 has only diffraction peaks of fcc NiPd alloy, and no diffraction peaks of elemental nickel and elemental palladium. Other preparation examples of the present invention also have the same characteristics, that is, the metal nanoparticles in the composite material of the present invention are nickel-palladium alloy.
[0197] From the XPS spectrum of FIG3 , it can be seen that the surface layer of the modified composite material prepared according to Preparation Example 4 contains carbon, oxygen, nickel, palladium, sulfur and nitrogen elements.
[0198] As shown in Figure 4, the composite material prepared according to Preparation Example 1 is attracted to the tube wall on the side of the magnet under the influence of a magnetic field. When the magnet is removed, the composite material lies flat inside the tube under the influence of gravity. Other preparation examples of the present invention exhibit similar characteristics, namely, the composite materials of the present invention possess strong ferromagnetism and excellent fluidity.
[0199] As shown in Example 5, although a small amount of palladium is added to the metal nanoparticles, about 35% of the chlorine can be removed, indicating that the catalytic hydrogenation ability of the composite material is significantly improved, while the metal nanoparticles containing only elemental nickel have basically no hydrogenation and dechlorination ability.
[0200] Comparative Example 2 shows that the commercial palladium-on-carbon catalyst has high hydrogenation activity, removing almost all chlorine during the hydrogenation of p-chloronitrobenzene. Comparative Example 1 shows that the commercial palladium-on-carbon catalyst is not resistant to sulfur poisoning and loses all activity upon addition of approximately 80 ppmw of sulfide.
[0201] As can be seen from Examples 1 to 4, when a trace amount of sulfide is added to the reaction system, the composite material of the present invention exhibits good resistance to sulfur poisoning, maintains high catalytic activity when catalyzing the hydrogenation of p-chloronitrobenzene, and has a highly selective catalytic hydrogenation capability. In other words, the composite material of the present invention can be used to catalyze the hydrogenation of halonitroaromatics to produce halogenated aromatic amines with high activity and selectivity.
[0202] As can be seen from Example 6, even when treated with a high concentration of sulfide during the manufacture of the modified composite material, the modified composite material of the present invention has a highly active catalytic hydrogenation ability, indicating that the composite material of the present invention has extremely strong resistance to sulfur poisoning. Moreover, the treated composite material does not require the addition of sulfide to the reaction system to catalyze the selective hydrogenation of p-chloronitrobenzene to produce p-chloroaniline with high selectivity. In other words, the modified composite material of the present invention treated with a sulfur-containing compound can directly catalyze the hydrogenation of halonitroaromatics to produce halogenated aromatic amines with high activity and selectivity, avoiding the incorporation of toxic substances into the hydrogenation product.
[0203] Examples 7 to 8 illustrate the catalytic hydrodechlorination method using the composite material of the present invention as a catalyst.
[0204] 100 mg of carbon-coated nickel-palladium alloy nanocomposite prepared according to the methods of Preparation Example 5 and Preparation Example 3, 315 mg of p-chloronitrobenzene, 27 mL of isopropanol, and 3 mL of water were added to the reactor respectively. After H2 was introduced into the reactor for replacement 4 times, the reactor was stirred and heated under low pressure to a predetermined reaction temperature of 60°C. H2 was introduced again to make the pressure in the reactor 1.0 MPa. The reaction was continued until the pressure did not change for 10 minutes. After cooling to room temperature, the pressure was released, the reactor was opened, and the product was taken out for chromatographic analysis.
[0205] After analysis of the product of Example 7, the conversion rate of p-chloronitrobenzene was 100%, and the dechlorination rate (ie, aniline yield) was 93.0%.
[0206] After analysis of the product of Example 8, the conversion rate of p-chloronitrobenzene was 100%, and the dechlorination rate (ie, aniline yield) was 97.9%.
[0207] Example 9
[0208] 100 mg of the composite material from Preparation Example 3, 129 mg of 4-chlorophenol, and 30 ml of ethanol were added to a reactor. After H₂ was introduced into the reactor four times for displacement, the mixture was stirred and heated under low pressure to a predetermined reaction temperature of 80°C. H₂ was then introduced again to a pressure of 1.0 MPa in the reactor. The reaction was continued until the pressure remained stable for 10 minutes (approximately 60 minutes). After cooling to room temperature, the pressure was released, the reactor was opened, the product was removed, and chromatographic analysis was performed. The results showed that the conversion of 4-chlorophenol was 100%, and the dechlorination rate was 100%.
[0209] It can be seen from Examples 7 to 9 that although the composite material of the preparation example was acid-washed with hydrochloric acid at a relatively high temperature for a long time, it still had a high catalytic hydrogenation dechlorination ability, indicating that the composite material of the present invention has good resistance to chlorine poisoning.
[0210] It can be seen from Example 9 that, although only an organic solvent is used, the method of the present invention still has a very high catalytic hydrodechlorination ability.
Claims
1. A composite material of carbon-coated nickel-palladium alloy nanoparticles, the composite material comprising a core-shell structure having a shell layer and a core, the shell layer being a graphitized carbon layer, and the core being a nickel-palladium alloy nanoparticle; in the composite material, the mass ratio of nickel to palladium is 3:1 to 100:1, preferably 4:1 to 100:1, further preferably 4:1 to 9:1, more preferably; based on the mass of the composite material, the total mass fraction of nickel and palladium is 1% to 80%, preferably 30% to 80%, more preferably 50% to 78%.
2. The composite material according to claim 1, characterized in that in, The particle size of the nickel-palladium alloy nanoparticles is 1 nm to 50 nm, preferably 2 nm to 25 nm, more preferably 3 nm to 15 nm, and / or The thickness of the graphitized carbon layer is 0.5 nm to 10 nm, preferably 0.5 nm to 5 nm, more preferably 1 nm to 5 nm, and / or The composite material is a mesoporous and / or macroporous material, and the volume of the mesopores and / or macropores accounts for more than 50% of the total pore volume.
3. The composite material according to claim 1, characterized in that: In the XRD spectrum of the composite material: There is only one diffraction peak in the range of 2θ from 40.1° to 44.5°; and / or There is a diffraction peak in the range of 2θ from 24° to 26°; and / or, There are diffraction peaks in the range of 2θ of 43° to 45°, 50° to 54°, 75° to 80°; and / or There is no diffraction peak in the range of 40.0°±0.1°.
4. A method for preparing a composite material of carbon-coated nickel-palladium alloy nanoparticles, comprising the following steps: S1: in the presence of a first solvent, a nickel source, a palladium source and an organic polycarboxylic acid are mixed to obtain a precursor solution, and then the first solvent is removed to obtain a precursor; S2 pyrolyzes the precursor in an inert gas.
5. The preparation method according to claim 4, characterized in that: in, The first solvent is water and / or ethanol, preferably water; and / or The nickel source is one or more of nickel acetate, basic nickel carbonate and nickel carbonate; and / or The palladium source is palladium acetate, preferably a solution of palladium acetate in glacial acetic acid; and / or The organic polycarboxylic acid is citric acid, ethylenediaminetetraacetic acid, 2,5-pyridinedicarboxylic acid, One or more of fruit acid, tartaric acid and terephthalic acid, preferably citric acid; and / or Calculated as metal elements, the mass ratio of the nickel source to the palladium source is 3:1 to 100:1, preferably 4:1 to 100:1, more preferably 4:1 to 9:1; and / or The molar ratio of the total amount of the nickel source and the palladium source to the organic polycarboxylic acid is 0.1:1 to 3:1, preferably 0.3:1 to 1.5:1, wherein the total amount of the nickel source and the palladium source is based on the total molar amount of the metal elements; and / or In S2, the pyrolysis temperature is 500°C to 800°C, preferably 500°C to 700°C, and more preferably 550°C to 650°C.
6. The preparation method according to claim 4, characterized in that: An acid treatment step is included after S2.
7. A composite material of modified carbon-coated nickel-palladium alloy nanoparticles, characterized in that: The composite material comprises the composite material as claimed in claim 1 and a sulfur-containing compound supported thereon.
8. The composite material of modified carbon-coated nickel-palladium alloy nanoparticles according to claim 7, characterized in that: in, The mass fraction of sulfur is 0.1% to 10%, preferably 0.5% to 5%, more preferably 0.8% to 1.8%; and / or The sulfur-containing compound is thiourea.
9. A method for preparing a composite material of modified carbon-coated nickel-palladium alloy nanoparticles, comprising: The step of contacting the composite material of claim 1 with a sulfur-containing compound.
10. The preparation method according to claim 9, characterized in that: in, The amount of the sulfur-containing compound in terms of sulfur element is 0.01 mol to 20 mol, preferably 0.3 mol to 5 mol, relative to 1 mol of palladium element in the composite material according to claim 1; and / or The sulfur-containing compound is thiourea; and / or The contacting is performed by immersion.
11. A method for selectively hydrogenating a nitro group in a halogenated nitroaromatic hydrocarbon, comprising the following steps: under liquid phase catalytic hydrogenation conditions, in the presence of a sulfur-containing compound, contacting hydrogen with the halogenated nitroaromatic hydrocarbon and a catalyst to carry out a liquid phase catalytic hydrogenation reaction; the catalyst is the composite material according to claim 1; preferably, the sulfur-containing compound is thiocyanate and / or thiourea, and preferably, the mass ratio of the sulfur-containing compound to the halogenated nitroaromatic hydrocarbon is 1:100 to 1:10000, and more preferably, the mass ratio is 1:100 to 1:
150.
12. A method for selectively hydrogenating a nitro group in a halogenated nitroaromatic hydrocarbon, comprising the following steps: contacting hydrogen with the halogenated nitroaromatic hydrocarbon and a catalyst under liquid phase catalytic hydrogenation conditions to carry out a liquid phase catalytic hydrogenation reaction; the catalyst is the composite material of modified carbon-coated nickel-palladium alloy nanoparticles as described in claim 7.
13. A method for selectively hydrogenating nitro groups in thionitroaromatic hydrocarbons, comprising the following steps: contacting hydrogen with thionitroaromatic hydrocarbons and a catalyst under liquid phase catalytic hydrogenation conditions to carry out a liquid phase catalytic hydrogenation reaction; the catalyst is the composite material according to claim 1, and the thionitroaromatic hydrocarbon is preferably at least one selected from 4-nitroanisole, 2-nitrodiphenyl sulfide, 4-nitrothiophenol, 3,3'-dinitrodiphenyl sulfone and 4,4'-dinitrodiphenyl sulfone.
14. A method for removing organic chlorine by catalytic hydrogenation, comprising the following steps: contacting a chlorine-containing saturated or aromatic organic compound with hydrogen and a catalyst for reaction under liquid phase catalytic hydrogenation dechlorination reaction conditions; the catalyst is the composite material according to claim 1.
15. The method according to claim 14, wherein: The reaction conditions of the liquid phase catalytic hydrodechlorination are: temperature range 40-120° C., preferably 60-100° C., hydrogen pressure range 0.1-3 MPa, preferably 1-2 MPa; and / or The chlorine-containing aromatic organic compound is selected from one or more of monochlorophenol, dichlorophenol, trichlorophenol, chlorinated aromatic hydrocarbons, 2,4-dichlorophenoxyacetic acid and chloronitrobenzene; and / or The chlorine-containing saturated organic compound is one or more selected from chlorinated saturated aliphatic hydrocarbons; and / or A solvent is used in the method, and the solvent is one or more selected from isopropanol, ethanol, acetone, tetrahydrofuran, cyclohexane and water; and / or The mass ratio of the catalyst to the chlorine-containing saturated or aromatic organic compound as the reaction substrate is 0.05-0.8:1, preferably 0.1-0.3:1; and / or In the composite material, the mass ratio of nickel to palladium is 3:1 to 10:1, preferably 3:1 to 6:1; and / or Based on the composite material, the total mass fraction of nickel and palladium is 20% to 80%, preferably 50% to 80%.
16. The method according to any one of claims 11 to 14, further comprising the steps of: The step of separating the composite material of claim 1 and the composite material of modified carbon-coated nickel-palladium alloy nanoparticles of claim 7 from the reaction product by magnetic separation.
17. Use of the composite material of claim 1 or the composite material of modified carbon-coated nickel-palladium alloy nanoparticles of claim 7 as a hydrogenation catalyst for catalytic hydrogenation, preferably, the hydrogen and / or the hydrogenation substrate contain sulfur-containing compounds.
Citation Information
Patent Citations
Catalytic hydrogenation method of unsaturated compound containing sulfide impurities
CN114425341A
Method for preparing sulfo-arylamine through catalytic hydrogenation
CN114426506A
Cited By
Carbon-coated non-noble metal supported modified hydrodehalogenation catalyst
CN120733765A
Carbon-coated non-noble metal supported modified hydrodehalogenation catalyst
CN120733765B
Preparation process and product of anti-poisoning platinum catalyst
CN121423031A
Bimetal catalyst with core-shell structure as well as preparation method and application of bimetallic catalyst
CN121467091A
Non-magnetic printed circuit board and surface treatment EPAG process thereof