Cleaning tape

The cleaning tape with a magnetic and underlayer configuration, using barium ferrite and alumina particles, addresses the challenge of removing small particles from magnetic heads, ensuring smooth surfaces and controlled abrasivity, thus preventing errors and head damage in next-generation recording systems.

WO2024241894A1PCT designated stage expired Publication Date: 2024-11-28SONY GROUP CORP

Patent Information

Application Number
PCT/JP2024/017205
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-24
Filing Date
2024-05-09
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Conventional cleaning tapes are unable to effectively remove small particles from the magnetic head in next-generation magnetic recording systems, leading to errors and head scratches, due to their inability to maintain a smooth surface and appropriate polishing force.

Method used

A cleaning tape with a magnetic layer and underlayer configuration, incorporating barium ferrite magnetic powder and alumina particles, optimized for surface smoothness and polishing power, to prevent particle shedding and head damage, while maintaining low abrasivity and electrical resistance.

Benefits of technology

The cleaning tape effectively suppresses particle shedding, maintains polishing power, and prevents head damage by ensuring a smooth surface and controlled abrasivity, enhancing data recording and reproduction accuracy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024017205_28112024_PF_FP_ABST
    Figure JP2024017205_28112024_PF_FP_ABST
Patent Text Reader

Abstract

The objective of the present technology is to provide a cleaning tape that has high cleaning power and can be used for next-generation media with small bit sizes. The present technology provides a cleaning tape including a magnetic layer and a base layer in this order, wherein the average thickness of the base layer is at least 1.60 µm, the surface roughness Rab of the magnetic layer surface is at most 2.9 nm, the abrasivity after being reciprocally rubbed 50 times on an AlFeSil prism is at most 65 µm, and the abrasivity after being reciprocally rubbed 100 times on an AlFeSil prism from the 50 times of reciprocal rubbing is at least 25 µm. The magnetic layer may contain magnetic powder. The magnetic powder may be barium ferrite magnetic powder.
Need to check novelty before this filing date? Find Prior Art

Description

cleaning tape

[0001] The present technology relates to cleaning tapes.

[0002] 2. Description of the Related Art With the development of IoT, big data, and artificial intelligence, the amount of data collected and stored is increasing dramatically. Magnetic recording media are often used as a medium for recording large amounts of data.

[0003] Data recording and reproduction in a magnetic recording / reproducing device using such a magnetic recording medium is performed while the magnetic head of the magnetic recording / reproducing device and the magnetic recording medium are in contact with each other. If abrasion dust from the magnetic recording medium adheres to the surface of the magnetic head (so-called "powder fall"), the reproduction output decreases, or even no reproduction output can be obtained. For this reason, various technologies have been proposed for cleaning tapes to remove abrasion dust adhered to the surface of the magnetic head. For example, Patent Document 1 below discloses a coating-type cleaning tape obtained by coating a non-magnetic support with a magnetic paint containing ferromagnetic powder and a binder. Patent Document 2 below also discloses a vapor-deposited cleaning tape configured with a non-magnetic support and a magnetic layer made of at least a thin magnetic metal film, the thin magnetic metal film being made of an alloy containing 60 to 100 atomic % Co, 0 to 40 atomic % Ni, and 5 atomic % or less of other elements.

[0004] JP 2000-57541 A JP 8-315327 A

[0005] The main purpose of this technology is to provide a cleaning tape with high cleaning power that can be used for next-generation media with small bit sizes.

[0006] The present technology provides a cleaning tape comprising a magnetic layer and an underlayer in this order, wherein the underlayer has an average thickness of 1.60 μm or more, the surface roughness Rab of the magnetic layer surface is 2.9 nm or less, the abrasivity after 50 round trips against an AlFeSil rectangular pillar is 65 μm or less, and the abrasivity after 50 to 100 round trips against an AlFeSil rectangular pillar is 25 μm or more. The magnetic layer may contain magnetic powder. The magnetic powder may contain barium ferrite. The average thickness (average total thickness) may be 9.2 μm or less. The average thickness of the underlayer may be 1.85 μm or less. After sliding a standard cleaning tape over the surface of a magnetic media abrasive tape while contacting it, an image of a portion of the surface of the magnetic media abrasive tape that has come into contact with the standard cleaning tape is captured, and the ratio of the pixels constituting the captured image that show powder that has fallen off from the standard cleaning tape to the pixels that show powder that has fallen off from the cleaning tape being inspected can be less than 1.0. 3 ~2000nm 3 The cleaning tape may further include abrasive particles in the magnetic layer. The abrasive particles may be alumina particles. The alumina particles may have an average particle size of 20 nm to 80 nm. The electrical resistance of the surface of the magnetic layer of the cleaning tape may be 1×10 3 Ω / sq ~ 5 x 10 10 Ω / sq. The average thickness of the underlayer may be 1.67 μm or more. A cleaning tape according to the present technology may include a magnetic layer, an underlayer, a base layer, and a back layer, in this order. The average thickness (average total thickness) may be 8.80 μm or more. The present technology also provides the cleaning tape, which is a cleaning tape for a magnetic recording system.

[0007] FIG. 1 is a cross-sectional view showing the configuration of a cleaning tape according to a first embodiment. FIG. 2 is a schematic diagram showing the configuration of a dedicated jig for abrassivity measurement. FIG. 3 is a schematic diagram showing an abrassivity bar. FIG. 4 is a schematic diagram showing the amount of wear (amount of scraping) of the abrassivity bar. FIG. 5 is an exploded perspective view showing an example of the configuration of a cleaning tape cartridge. FIG. 6 is a diagram showing an example of the shape of magnetic powder particles. FIG. 7 is an example of a TEM photograph of a cross section of a sample. FIG. 8 is another example of a TEM photograph of a cross section of a sample. FIG. 9 is a cross-sectional view showing the configuration of a rewinding machine.

[0008] Preferred embodiments for carrying out the present technology will be described below. Note that the embodiments described below are representative embodiments of the present technology, and the scope of the present technology is not limited to these embodiments.

[0009] The present technology will be described in the following order: 1. Description of the present technology 2. Embodiments of the present technology (1) Configuration of cleaning tape (2) Description of each layer (3) Physical properties and structure (4) Manufacturing method of cleaning tape (5) One embodiment of cleaning tape cartridge 3. Examples

[0010] In this specification, unless a measurement environment is specifically stated in connection with the explanation of the measurement method, the measurement is performed in an environment of 25°C ± 2°C and 50% RH ± 5% RH.

[0011] 1. Description of the technology

[0012] Next-generation media have smaller bit sizes to achieve higher density recording. As the bit size gets smaller, even small particles falling off the magnetic head can cause an error and stop the recording / playback device. Conventional cleaning tapes cannot remove small particles from the magnetic head, preventing errors.

[0013] The present inventors have found that by adjusting the abrasive force to a suitable level while maintaining a smooth surface of the cleaning tape, it is possible to suppress the shedding of small particles from the cleaning tape and remove deposits from the magnetic head without scratching the magnetic head. Furthermore, the present inventors have found that by smoothing the surface of the cleaning tape, it is possible to suppress the shedding of small particles, and by adjusting the abrasive force to a suitable level, it is possible to remove deposits while suppressing the occurrence of head scratches. Furthermore, the present inventors have found that, for example, by using a barium ferrite magnetic powder with a small particle size and alumina particles with a small particle size, it is possible to smooth the surface of the cleaning tape, and that the abrasive force can be maintained by optimizing the process conditions (such as lowering the calendering temperature).

[0014] That is, the cleaning tape according to the present technology includes a magnetic layer and an underlayer in this order. Furthermore, the cleaning tape according to the present technology may include a magnetic layer, an underlayer, a base layer, and a back layer in this order.

[0015] The cleaning tape according to the present technology may preferably be a long cleaning tape.

[0016] In a cleaning tape according to the present technology, the average thickness of the underlayer can be 1.60 μm or more, preferably 1.65 μm or more, more preferably 1.67 μm or more, and even more preferably 1.70 μm or more, from the viewpoint of preventing the magnetic layer from being crushed and the abrasiveness from being reduced, making it impossible to remove deposits from the magnetic head when the cleaning tape comes into contact with the magnetic head of a magnetic recording / reproducing device. Furthermore, from the viewpoint of preventing the abrasiveness from being increased and damaging the magnetic head, the average thickness of the underlayer can be 1.85 μm or less, preferably 1.80 μm or less, more preferably 1.78 μm or less, and even more preferably 1.75 μm or less. A method for measuring the average thickness of the underlayer will be described below in 2.(3).

[0017] From the viewpoint of adjusting the appropriate abrasiveness by the average thickness of the underlayer, the average thickness (average total thickness) t of the cleaning tape according to the present technology TThe average thickness (average total thickness) t of the cleaning tape is preferably 9.20 μm or less, more preferably 9.15 μm or less, even more preferably 9.10 μm or less, and even more preferably 9.00 μm or less. T The average thickness (average total thickness) t of the cleaning tape is, for example, preferably 8.60 μm or more, more preferably 8.70 μm or more, even more preferably 8.75 μm or more, and still more preferably 8.80 μm or more. T The measurement method will be explained in 2. (3) below.

[0018] In a cleaning tape according to the present technology, the average thickness of the magnetic layer can be preferably 0.060 μm or more, more preferably 0.063 μm or more, even more preferably 0.066 μm or more, and even more preferably 0.069 μm or more, from the viewpoint of preventing a decrease in abrasiveness when the magnetic head and the cleaning tape come into contact, making it impossible to remove deposits attached to the magnetic head. Furthermore, from the viewpoint of preventing an increase in abrasiveness and damage to the magnetic head, the average thickness of the magnetic layer can be preferably 0.080 μm or less, more preferably 0.077 μm or less, even more preferably 0.074 μm or less, and even more preferably 0.071 μm or less. A method for measuring the average thickness of the magnetic layer will be described below in 2.(3).

[0019] The average thickness of the base layer of the cleaning tape according to the present technology is preferably 6.3 μm or more, more preferably 6.4 μm or more, even more preferably 6.5 μm or more, and is preferably 6.8 μm or less, more preferably 6.7 μm or less, even more preferably 6.6 μm or less. The method for measuring the average thickness of the base layer will be described below in 2.(3).

[0020] The average thickness of the back layer of the cleaning tape according to the present technology is preferably 0.30 μm or more, more preferably 0.35 μm or more, even more preferably 0.40 μm or more, still more preferably 0.45 μm or more, and is preferably 0.65 μm or less, more preferably 0.60 μm or less, even more preferably 0.55 μm or less, still more preferably 0.50 μm or less. The method for measuring the average thickness of the back layer will be described below in 2.(3).

[0021] In order to obtain a good magnetic head cleaning performance, the cleaning tape according to the present technology may have a surface roughness Rab of the magnetic layer surface of 2.9 nm or less, preferably 2.8 nm or less, more preferably 2.7 nm or less, and even more preferably 2.6 nm or less. Furthermore, the surface roughness Rab of the magnetic layer surface may preferably be 2.0 nm or more. A method for measuring the surface roughness Rab of the magnetic layer surface will be described below in 2.(3).

[0022] In order to prevent excessive abrasive power from causing wear on the magnetic head and leading to damage to the magnetic head, the cleaning tape according to the present technology may have an abrasivity of 65 μm or less, preferably 60 μm or less, more preferably 55 μm or less, even more preferably 50 μm or less, and even more preferably 47 μm or less after 50 round trips on an AlFeSil rectangular pillar. Furthermore, in order to improve abrasive power and remove deposits from the magnetic head, the cleaning tape according to the present technology may have an abrasivity of 25 μm or more, preferably 26 μm or more, after 50 to 100 round trips on an AlFeSil rectangular pillar. The method for measuring the abrasivity on an AlFeSil rectangular pillar will be described below in 2.(3).

[0023] The magnetic layer of the cleaning tape according to the present technology may contain magnetic powder. The magnetic powder may preferably contain barium ferrite magnetic powder. The average particle volume of the barium ferrite magnetic powder is preferably 2000 nm 3 or less, more preferably 1800 nm 3 or less, and more preferably 1600 nm 3The average particle volume within the above range can provide a smooth surface for the cleaning tape. The average particle volume of the barium ferrite magnetic powder is preferably 500 nm or less. 3 More preferably, 800 nm or more 3 More preferably, 1000 nm or more 3 or more, and even more preferably 1200 nm 3 The method for measuring the average particle volume of the barium ferrite magnetic powder will be explained in 2.(3) below.

[0024] In order to prevent damage to the magnetic head due to the influence of an overcurrent or static electricity, the cleaning tape according to the present technology has an electrical resistance value on the magnetic layer surface that is preferably in the range of 1×10 3 Ω / sq ~ 5 x 10 10 It may be Ω / sq.

[0025] 2. Embodiments of the present technology

[0026] (1) Cleaning tape configuration

[0027] First, the configuration of a cleaning tape 10 according to an embodiment of the present technology will be described with reference to Fig. 1. As shown in Fig. 1, the cleaning tape 10 includes a long base layer (also referred to as a substrate) 11, an underlayer 12 provided on one main surface of the base layer 11, a magnetic layer 13 provided on the underlayer 12, and a back layer 14 provided on the other main surface of the base layer 11. Hereinafter, of the two main surfaces of the cleaning tape 10, the surface on which the magnetic layer 13 is provided will be referred to as the magnetic surface, and the surface opposite to the magnetic surface (the surface on which the back layer 14 is provided) will be referred to as the back surface.

[0028] The cleaning tape 10 has a long shape and runs in the longitudinal direction during recording and reproduction.

[0029] (2) Explanation of each layer

[0030] (base layer)

[0031] The base layer 11 can function as a support for the cleaning tape 10 and can be, for example, a flexible, long, non-magnetic substrate, particularly a non-magnetic film. The base layer 11 can contain, for example, at least one of polyester resins, polyolefin resins, cellulose derivatives, vinyl resins, aromatic polyether ketone resins, and other polymer resins. When the base layer 11 contains two or more of the above materials, the two or more materials may be mixed, copolymerized, or laminated.

[0032] The polyester-based resin may be, for example, one or a mixture of two or more of PET (polyethylene terephthalate), PEN (polyethylene naphthalate), PBT (polybutylene terephthalate), PBN (polybutylene naphthalate), PCT (polycyclohexylene dimethylene terephthalate), PEB (polyethylene-p-oxybenzoate), and polyethylene bisphenoxycarboxylate. According to a preferred embodiment of the present technology, the base layer 11 may be formed from PET or PEN.

[0033] The polyolefin resin may be, for example, one or a mixture of two or more of PE (polyethylene) and PP (polypropylene).

[0034] The cellulose derivative may be, for example, one or a mixture of two or more of cellulose diacetate, cellulose triacetate, CAB (cellulose acetate butyrate), and CAP (cellulose acetate propionate).

[0035] The vinyl resin may be, for example, one or a mixture of two or more of PVC (polyvinyl chloride) and PVDC (polyvinylidene chloride).

[0036] The aromatic polyetherketone resin may be, for example, one or a mixture of two or more of PEK (polyetherketone), PEEK (polyetheretherketone), PEKK (polyetherketoneketone), and PEEKK (polyetheretherketoneketone). According to a preferred embodiment of the present technology, the base layer 11 may be formed from PEEK.

[0037] The other polymer resin may be, for example, one or a mixture of two or more of PA (polyamide, nylon), aromatic PA (aromatic polyamide, aramid), PI (polyimide), aromatic PI (aromatic polyimide), PAI (polyamideimide), aromatic PAI (aromatic polyamideimide), PBO (polybenzoxazole, e.g., Zylon (registered trademark), polyether, polyetherester, PES (polyethersulfone), PEI (polyetherimide), PSF (polysulfone), PPS (polyphenylene sulfide), PC (polycarbonate), PAR (polyarylate), and PU (polyurethane).

[0038] (magnetic layer)

[0039] The magnetic layer 13 may contain magnetic powder. The magnetic powder may preferably contain barium ferrite magnetic powder. In addition to the barium ferrite magnetic powder, the magnetic layer 13 may also contain abrasive particles and conductive particles. In addition to the above components, the magnetic layer 13 may further contain a binder and additives.

[0040] (Magnetic powder)

[0041] Examples of magnetic particles constituting the magnetic powder contained in the magnetic layer 13 include, but are not limited to, hexagonal ferrite, barium ferrite (BaFe), Co ferrite, and strontium ferrite. The magnetic powder may be one of these, or a combination of two or more. Particularly preferably, the magnetic powder may include barium ferrite magnetic powder, cobalt ferrite magnetic powder, or strontium ferrite magnetic powder. These magnetic particles may be appropriately selected by those skilled in the art based on factors such as the manufacturing method of the magnetic layer 13.

[0042] The average particle size (average maximum particle size) D of the magnetic powder can be preferably 22 nm or less, more preferably 8 nm or more and 22 nm or less, and even more preferably 10 nm or more and 20 nm or less.

[0043] The average particle size D of the magnetic powder is determined as follows. First, the magnetic recording medium 10 to be measured is processed by a focused ion beam (FIB) method or the like to prepare a thin section, and the cross section of the thin section is observed by a TEM. Next, 500 ε-iron oxide particles are randomly selected from the TEM photograph, and the maximum particle size d of each particle is measured. max The maximum particle size d of the magnetic powder is measured. max The particle size distribution of the maximum particle size d max " means the so-called maximum Feret diameter, specifically the maximum distance between two parallel lines drawn from any angle so as to be tangent to the contour of the ε-iron oxide particle. Then, the calculated maximum particle size d max From the particle size distribution, the maximum particle size d max The median diameter (50% diameter, D50) is determined and used as the average particle size (average maximum particle size) D of the magnetic powder.

[0044] The shape of the magnetic powder is preferably at least one of plate-like and rectangular. The shape of the magnetic powder depends on the crystal structure of the magnetic particles. Examples of plate-like magnetic powder include BaFe and strontium ferrite, which have a hexagonal plate-like shape. Examples of rectangular-shaped magnetic powder include cobalt ferrite, which has a cubic shape.

[0045] According to another preferred embodiment of the present technology, the magnetic powder may include barium ferrite (BaFe) magnetic powder. The barium ferrite magnetic powder includes magnetic particles of iron oxide having barium ferrite as a main phase (hereinafter referred to as "barium ferrite particles"). The barium ferrite magnetic powder can achieve a smooth surface for the cleaning tape. From this perspective, the barium ferrite magnetic powder is preferred as the magnetic powder.

[0046] The average particle size of the barium ferrite magnetic powder can be preferably 50 nm or less, more preferably 10 nm or more and 40 nm or less, and even more preferably 12 nm or more and 25 nm or less.

[0047] According to yet another preferred embodiment of the present technology, the magnetic powder may be cobalt ferrite magnetic powder. The cobalt ferrite magnetic powder includes magnetic particles of iron oxide having cobalt ferrite as a main phase (hereinafter referred to as "cobalt ferrite magnetic particles"). The cobalt ferrite magnetic particles preferably have uniaxial anisotropy. The cobalt ferrite magnetic particles have, for example, a cubic or approximately cubic shape. The cobalt ferrite is cobalt ferrite containing Co. The cobalt ferrite may further include one or more elements selected from the group consisting of Ni, Mn, Al, Cu, and Zn in addition to Co.

[0048] Cobalt ferrite has, for example, an average composition represented by the following formula (1): Co x M y Fe 2 O z ... (1) (In formula (1), M is, for example, one or more metals selected from the group consisting of Ni, Mn, Al, Cu, and Zn. x is a value within the range of 0.4≦x≦1.0. y is a value within the range of 0≦y≦0.3. However, x and y satisfy the relationship (x+y)≦1.0. z is a value within the range of 3≦z≦4. A part of Fe may be substituted with another metal element.)

[0049] The average particle size of the cobalt ferrite magnetic powder may be preferably 25 nm or less, more preferably 23 nm or less.

[0050] According to yet another preferred embodiment of the present technology, the magnetic powder may include a powder of nanoparticles containing hexagonal ferrite (hereinafter referred to as "hexagonal ferrite particles"). The hexagonal ferrite particles have, for example, a hexagonal plate shape or an approximately hexagonal plate shape. The hexagonal ferrite may preferably contain at least one of Ba, Sr, Pb, and Ca, more preferably at least one of Ba and Sr. Specifically, the hexagonal ferrite may be, for example, barium ferrite or strontium ferrite. Barium ferrite may further contain at least one of Sr, Pb, and Ca in addition to Ba. Strontium ferrite may further contain at least one of Ba, Pb, and Ca in addition to Sr. More specifically, the hexagonal ferrite may be represented by the general formula MFe 12 O 19 The magnetic powder may have an average composition represented by the formula: where M is, for example, at least one metal selected from Ba, Sr, Pb, and Ca, preferably at least one metal selected from Ba and Sr. M may be a combination of Ba and one or more metals selected from the group consisting of Sr, Pb, and Ca. Alternatively, M may be a combination of Sr and one or more metals selected from the group consisting of Ba, Pb, and Ca. In the above general formula, part of Fe may be substituted with another metal element. When the magnetic powder contains a powder of hexagonal ferrite particles, the average particle size of the magnetic powder may be preferably 50 nm or less, more preferably 10 nm to 40 nm, and even more preferably 15 nm to 30 nm.

[0051] (abrasive particles)

[0052] The abrasive particles may preferably be inorganic particles. Examples of such abrasive particles include α-alumina with an α-conversion rate of 90% or more, β-alumina, γ-alumina, silicon carbide, chromium oxide, cerium oxide, α-iron oxide, corundum, silicon nitride, titanium carbide, titanium oxide, silicon dioxide, tin oxide, magnesium oxide, tungsten oxide, zirconium oxide, boron nitride, zinc oxide, calcium carbonate, calcium sulfate, barium sulfate, molybdenum disulfide, acicular α-iron oxide obtained by dehydrating and annealing magnetic iron oxide raw materials, optionally surface-treated with aluminum and / or silica, and diamond powder. Alumina particles such as α-alumina, β-alumina, and γ-alumina, and silicon carbide are preferably used as abrasive particles. These abrasive particles may be acicular, spherical, cubic, or other shapes, but those with angular shapes are preferred because they have high abrasiveness. The average particle size of the abrasive particles may be preferably 20 nm to 80 nm, more preferably 25 nm to 75 nm, even more preferably 30 nm to 70 nm, and even more preferably 35 nm to 65 nm. When the abrasive particles are alumina particles, the average particle size of the alumina particles may be preferably 20 nm to 80 nm, more preferably 25 nm to 75 nm, even more preferably 30 nm to 70 nm, and even more preferably 35 nm to 65 nm.

[0053] (Conductive particles)

[0054] The conductive particles may be fine particles primarily composed of carbon, preferably carbon particles, such as carbon black. Examples of carbon black include Asahi #15 and #15HS from Asahi Carbon Co., Ltd. Hybrid carbon, in which carbon is attached to the surface of silica particles, may also be used. The conductive particles may have an average particle size of preferably 30 to 90 nm, more preferably 40 to 80 nm, even more preferably 45 to 75 nm, and even more preferably 50 to 70 nm.

[0055] (Binder)

[0056] The binder is preferably a resin having a structure in which a crosslinking reaction is imparted to a polyurethane resin, a vinyl chloride resin, or the like. However, the binder is not limited to these, and other resins may be appropriately blended depending on the physical properties required for the cleaning tape 10. The resin to be blended is not particularly limited as long as it is a resin that is generally used in coating-type cleaning tapes 10.

[0057] Examples of the binder include polyvinyl chloride, polyvinyl acetate, vinyl chloride-vinyl acetate copolymer, vinyl chloride-vinylidene chloride copolymer, vinyl chloride-acrylonitrile copolymer, acrylic acid ester-acrylonitrile copolymer, acrylic acid ester-vinyl chloride-vinylidene chloride copolymer, acrylic acid ester-vinylidene chloride copolymer, methacrylic acid ester-vinylidene chloride copolymer, methacrylic acid ester-vinyl chloride copolymer, methacrylic acid ester-ethylene copolymer, polyvinyl fluoride, vinylidene chloride-acrylonitrile copolymer, acrylonitrile-butadiene copolymer, polyamide resin, polyvinyl butyral, cellulose derivatives (cellulose acetate butyrate, cellulose diacetate, cellulose triacetate, cellulose propionate, nitrocellulose), styrene-butadiene copolymer, polyester resin, amino resin, and synthetic rubber.

[0058] Furthermore, a thermosetting resin or a reactive resin may be used as the binder, and examples of such a resin include a phenolic resin, an epoxy resin, a urea resin, a melamine resin, an alkyd resin, a silicone resin, a polyamine resin, and a urea-formaldehyde resin.

[0059] In addition, in order to improve the dispersibility of the magnetic powder, each of the above-mentioned binders contains -SO 3 M, -OSO 3 M, -COOM, P=O(OM) 2 In the formula, M is a hydrogen atom or an alkali metal such as lithium, potassium, or sodium.

[0060] Furthermore, the polar functional group is -NR1R2, -NR1R2R3 + X - A side chain type having a terminal group of >NR1R2 + X - In the formula, R1, R2, and R3 are hydrogen atoms or hydrocarbon groups, and X - is a halogen ion such as fluorine, chlorine, bromine, or iodine, or an inorganic or organic ion. Examples of the polar functional group include —OH, —SH, —CN, and an epoxy group.

[0061] (Additives)

[0062] The magnetic layer 13 may further contain non-magnetic reinforcing particles such as aluminum oxide (α, β, or γ alumina), chromium oxide, silicon oxide, diamond, garnet, emery, boron nitride, titanium carbide, silicon carbide, titanium carbide, titanium oxide (rutile or anatase titanium oxide), etc.

[0063] (base layer)

[0064] The underlayer 12 is a non-magnetic layer containing non-magnetic powder and a binder as its main components. The above description of the binder contained in the magnetic layer 13 also applies to the binder contained in the underlayer 12. The underlayer 12 may further contain at least one additive selected from the group consisting of conductive particles, lubricants, hardeners, and rust inhibitors, as needed.

[0065] (Non-magnetic powder)

[0066] The non-magnetic powder contained in the underlayer 12 may include, for example, at least one type selected from inorganic particles and organic particles. One type of non-magnetic powder may be used alone, or two or more types of non-magnetic powder may be used in combination. The inorganic particles may include, for example, one or a combination of two or more types selected from metals, metal oxides, metal carbonates, metal sulfates, metal nitrides, metal carbides, and metal sulfides. More specifically, the inorganic particles may be, for example, one or more types selected from iron oxyhydroxide, hematite, titanium oxide, and carbon black. The shape of the non-magnetic powder may be, for example, acicular, spherical, cubic, plate-like, or other shapes, but is not particularly limited to these.

[0067] (Back layer)

[0068] The back layer 14 may contain a binder and a non-magnetic powder. The back layer 14 may also contain various additives such as a lubricant, a curing agent, and an antistatic agent, as necessary. The above description of the binder and non-magnetic powder contained in the underlayer 12 also applies to the binder and non-magnetic powder contained in the back layer 14.

[0069] The average particle size of the inorganic particles contained in the back layer 14 is preferably 10 nm or more and 150 nm or less, and more preferably 15 nm or more and 110 nm or less. The average particle size of the inorganic particles can be determined in the same manner as the average particle size D of the magnetic powder described above.

[0070] (3) Physical properties and structure

[0071] (Surface roughness Rab)

[0072] The surface roughness Rab is a value measured on the surface 13S of the magnetic layer 13 of the cleaning tape 10. The surface roughness Rab is determined as follows. First, the cleaning tape T housed in the cartridge 10A shown in FIG. 5 is unwound, and a length of approximately 10 cm is cut out from the cleaning tape T at a position 30 to 40 m longitudinally from the connection between the cleaning tape T and the leader tape LT, and attached to a glass slide (i.e., the back layer surface is attached to the glass slide) to obtain a sample piece. Next, the surface roughness of the magnetic layer surface 13S of the sample piece is measured using a non-contact roughness meter using optical interference described below.

[0073] <Surface roughness measurement conditions>

[0074] Equipment: Non-contact roughness meter using optical interference (non-contact surface and layer cross-sectional shape measurement system VertScan R5500GL-M100-AC manufactured by Ryoka Systems Co., Ltd.) Objective lens: 20x (approximately 236 μm x 177 μm field of view) Resolution: 640 points x 480 points Measurement mode: phase Wavelength filter: 520 nm Surface correction: Corrected using a fourth-order polynomial approximation surface

[0075] As described above, the surface roughness is measured at at least five positions in the longitudinal direction, and then the average value of the arithmetic mean roughnesses Sa (nm) automatically calculated from the surface profiles obtained at each position is defined as the surface roughness Rab (nm).

[0076] (Abrasivity)

[0077] Abrasivity is measured in accordance with ECMA-319 Annex C. Note that abrasivity is measured by changing the ceramic material of the abrasivity bar to AlFeSil. Abrasivity is an index that indicates the degree of wear on the magnetic head caused by the magnetic surface of the cleaning tape as the cleaning tape contacts and runs against the magnetic head. For example, a square-prism bar (abrasivity bar) A made of a ceramic material (AlFeSil) as shown in FIG. 3 is set in a dedicated jig (a jig described in ECMA-319 Annex C) as shown in FIG. 2 , and the jig is attached to the magnetic head of a tape drive or the like so that the corners of the square prism come into contact with the cleaning tape. The cleaning tape is run for a predetermined time or a predetermined number of passes, and after the run, the width B of the worn abrasive bar is measured as shown in FIG. 4 . For the measurement, a TOPCON universal tool microscope or a microscope with equivalent performance is used. The measured wear amount (amount of scraping) of the abrasive bar is used as an index of abrasivity. The larger the wear amount (amount of scraping), the better the abrasiveness and the greater the abrasive power. For example, abrasivity is measured as follows.

[0078] A square-prism bar (abrasive bar) A made of a ceramic material (AlFeSil) shown in FIG. 3 is set in the dedicated jig shown in FIG.

[0079] The square prism bar (abrasiveness bar) A was obtained by heat treating a ceramic material (Al: 5.4%, Si: 9.6%, Fe: 85%) at 1000°C and vacuum molding it, and has a Rockwell C hardness of 46. Next, this square prism bar was attached to the magnetic head of a tape drive or the like so that the corners of the bar came into contact with the cleaning tape. The cleaning tape was then run under the following conditions: Tape speed: 3.0 m / s, Tension: 1.0 N ± 0.1 N, Wrap angle: 12°, Running tape length: 580 m

[0080] The average wear pattern length of the abrassivity bar is preferably 12.5 μm to 20 μm after 50 reciprocating runs of a new cleaning tape. When the same measurement is repeated on the same part of the cleaning tape, the wear pattern length should be within 30%. The measurement is performed in an environment with a temperature of 23°C ± 2°C and a humidity of 45% ± 5%. The average wear pattern length of the abrassivity bar on the cleaning tape should be within a maximum of 20 μm after 50 reciprocating runs of the cleaning tape. After 50 reciprocating runs of the cleaning tape, the wear amount (abrasion amount) is measured at three positions, and these measurements are simply averaged (arithmetic mean) to determine the measured wear amount (abrasion amount). This measurement value is defined as the abrassivity of the 50 reciprocating runs. The three measurement positions are randomly selected from the sample so that they are different from each other in the width direction of the cleaning tape. The same applies hereinafter.

[0081] The abrasivity bar was then replaced with a new one, and the cleaning tape after 50 reciprocal runs was used to measure the amount of wear (abrasion) after 50 reciprocal runs, which was defined as the abrasivity between 50 and 100 reciprocal runs.

[0082] (Average thickness of cleaning tape (average total thickness) t T )

[0083] Average thickness t of cleaning tape T T is obtained as follows. First, the cleaning tape T housed in the cartridge 10A is unwound, and a sample of 250 mm is cut from the cleaning tape T at a position 30 m in the longitudinal direction from the connection between the cleaning tape T and the leader tape LT. Next, the thickness of the sample is measured at five positions using a Mitutoyo Laser Hologram (LGH-110C) as a measuring device, and the measured values ​​are simply averaged (arithmetic mean) to obtain the average thickness t T The five measurement positions are selected at random from the sample so that they are different positions in the longitudinal direction of the magnetic tape T.

[0084] (Average thickness of base layer)

[0085] The average thickness of the underlayer 12 is determined as follows. First, the cleaning tape T housed in the cartridge 10A is unwound, and three samples of 250 mm are cut from the cleaning tape T at three locations, 10 m, 30 m, and 50 m from the connection between the cleaning tape T and the leader tape LT, in the longitudinal direction. Each sample is then thinned using an FIB method or the like. When using the FIB method, a carbon layer and a tungsten layer are formed as protective films as a pretreatment for observing the cross-sectional TEM images described below. The carbon and tungsten layers are formed by vapor deposition on the surface of the cleaning tape T facing the magnetic layer 13 and the surface facing the back layer 14, and the tungsten layer is further formed by vapor deposition or sputtering on the surface facing the magnetic layer 13. The thinning is performed along the longitudinal direction of the cleaning tape T. That is, the thinning results in a cross section parallel to both the longitudinal direction and the thickness direction of the cleaning tape T.

[0086] The cross section of each of the obtained thinned samples is observed using a transmission electron microscope (TEM) under the following conditions: Apparatus: TEM (H9000NAR manufactured by Hitachi, Ltd.) Acceleration voltage: 300 kV Magnification: 100,000 times

[0087] Next, using the obtained TEM image, the thickness of the underlayer 12 is measured at at least 10 positions in the longitudinal direction of the cleaning tape T, and then the measured values ​​are simply averaged (arithmetic averaged) to obtain the average thickness (μm) of the underlayer 12.

[0088] (average thickness of base layer)

[0089] The average thickness of the base layer 11 is determined as follows. First, the cleaning tape T housed in the magnetic recording cartridge 10A is unwound, and a sample is prepared by cutting the magnetic tape T to a length of 250 mm at a position 30 m in the longitudinal direction from the joint between the cleaning tape T and the leader tape LT. In this specification, the "longitudinal direction" in the "longitudinal direction from the joint between the cleaning tape T and the leader tape LT" refers to the direction from one end on the leader tape LT side toward the other end on the opposite side.

[0090] Next, the layers other than the base layer 11 of the sample (i.e., the underlayer 12, magnetic layer 13, and back layer 14) are removed with a solvent such as MEK (methyl ethyl ketone) or dilute hydrochloric acid. Next, using a Mitutoyo Laser Hologram (LGH-110C) as a measuring device, the thickness of the sample (base layer 11) is measured at five positions, and the measured values ​​are simply averaged (arithmetic mean) to calculate the average thickness of the base layer 11. Note that the five measurement positions are randomly selected from the sample so that they are each different from the others in the longitudinal direction of the cleaning tape T.

[0091] (Average thickness of the back layer t b )

[0092] Average thickness t of the back layer 14 b is calculated as follows: First, the average thickness (average total thickness) t of the cleaning tape T T Measure the average thickness tT The method for measuring the average total thickness is as described above in "Average Thickness of Cleaning Tape." Next, the cleaning tape T housed in the cartridge 10A is unwound, and a sample is prepared by cutting the cleaning tape T into a length of 250 mm at a position 30 m longitudinally from the connection between the cleaning tape T and the leader tape LT. Next, the back layer 14 of the sample is removed with a solvent such as MEK (methyl ethyl ketone) or dilute hydrochloric acid. Next, the thickness of the sample is measured at five positions using a Mitutoyo Laser Hologram Gauge (LGH-110C), and the measured values ​​are simply averaged (arithmetic average) to obtain the average thickness t B Then, the average thickness t of the back layer 14 is calculated using the following formula: b The five measurement positions are selected at random from the sample so that they are different positions in the longitudinal direction of the cleaning tape T. b [μm] = t T [μm]-t B [μm]

[0093] (Average thickness of the magnetic layer t m )

[0094] Average thickness t of the magnetic layer 13 mis determined as follows. First, the cleaning tape T housed in the cartridge 10A is unwound, and three samples of 250 mm length are cut from the cleaning tape T at three positions, 10 m, 30 m, and 50 m from the connection between the cleaning tape T and the leader tape LT, in the longitudinal direction. Each sample is then thinned by FIB or other methods. When the FIB method is used, a carbon layer and a tungsten layer are formed as protective films as a pretreatment for observing the cross-sectional TEM images described below. The carbon layer is formed by vapor deposition on the surface of the cleaning tape T facing the magnetic layer 13 and the surface facing the back layer 14, and the tungsten layer is further formed by vapor deposition or sputtering on the surface facing the magnetic layer 13. The thinning is performed along the longitudinal direction of the cleaning tape T. That is, the thinning results in a cross section parallel to both the longitudinal direction and the thickness direction of the cleaning tape T.

[0095] The cross section of each obtained thinned sample is observed using a transmission electron microscope (TEM) under the following conditions to obtain a TEM image of each thinned sample. Note that the magnification and acceleration voltage may be adjusted appropriately depending on the type of device.

[0096] Apparatus: TEM (Hitachi H9000NAR) Acceleration voltage: 300 kV Magnification: 100,000 times

[0097] Next, using the TEM image of each obtained thinned sample, the thickness of the magnetic layer 13 is measured at 10 positions on each thinned sample. The 10 measurement positions on each thinned sample are randomly selected from the sample so that they are different positions in the longitudinal direction of the cleaning tape T. The measured values ​​of each obtained thinned sample (thickness of the magnetic layer 13 at 30 points in total) are simply averaged (arithmetic average) to obtain an average value, which is the average thickness t of the magnetic layer 13. m Let [nm].

[0098] (average particle size of magnetic powder)

[0099] When the magnetic powder contains hexagonal ferrite particles, the average particle size and average aspect ratio of the magnetic powder can be determined as follows. First, the cleaning tape T housed in the cartridge 10A is unwound, and the cleaning tape T is cut out at a position 30 m longitudinally from the connection between the cleaning tape T and the leader tape LT. Next, the cleaning tape T to be measured is processed into a thin section using an FIB method or the like. When using the FIB method, a carbon layer and a tungsten layer are formed as protective films as a pretreatment for observing the cross-sectional TEM image described below. The carbon layer is formed by vapor deposition on the surface of the cleaning tape T facing the magnetic layer 13 and the surface facing the back layer 14, and the tungsten layer is further formed by vapor deposition or sputtering on the surface facing the magnetic layer 13. The thinning is performed along the length (longitudinal direction) of the cleaning tape T. That is, the thinning results in a cross section parallel to both the longitudinal and thickness directions of the cleaning tape T.

[0100] The cross section of the obtained thin sample is observed using a transmission electron microscope (H-9500 manufactured by Hitachi High-Technologies Corporation) at an acceleration voltage of 200 kV and a total magnification of 500,000 times, so as to include the entire magnetic layer 13 in the thickness direction of the magnetic layer 13, and a TEM photograph is taken. The number of TEM photographs prepared is sufficient to extract 50 particles from which the plate diameter DB and plate thickness DA (see Figure 27) shown below can be measured.

[0101] In this specification, the size of a hexagonal ferrite particle (hereinafter referred to as "particle size") is defined as the plate diameter DB, which is the major axis of the plate surface or bottom surface, when the particle shape observed in the TEM photograph is plate-like or columnar (however, the thickness or height is smaller than the major axis of the plate surface or bottom surface) as shown in FIG. 6 . The thickness or height of the particle observed in the TEM photograph is defined as the plate thickness DA. When the plate surface or bottom surface of the particle observed in the TEM photograph is hexagonal, the major axis means the longest diagonal distance. When the thickness or height of a particle is not constant within a single particle, the thickness or height of the largest particle is defined as the plate thickness DA.

[0102] Next, 50 particles are selected from the TEM photograph based on the following criteria: Particles with parts outside the field of view of the TEM photograph are not measured, and only particles with a clear outline and that exist independently are measured. When particles overlap, particles with a clear boundary between them and whose overall shape can be determined are measured as individual particles, but particles with an unclear boundary and whose overall shape cannot be determined are not measured, as their shape cannot be determined.

[0103] Examples of TEM photographs are shown in Figures 7 and 8. In Figures 7 and 8, the particles indicated by arrows a and d are selected because their plate thickness (thickness or height) DA can be clearly confirmed. The plate thickness DA of each of the selected 50 particles is measured. The plate thicknesses DA thus obtained are simply averaged (arithmetic mean) to obtain the average plate thickness DA. ave Calculate the average plate thickness DA ave is the average particle plate thickness. Next, the plate diameter DB of each magnetic powder is measured. In order to measure the plate diameter DB of the particles, 50 particles whose plate diameter DB can be clearly confirmed are selected from the TEM photograph. For example, in Figures 7 and 8, the particles indicated by arrows b and c are selected because their plate diameter DB can be clearly confirmed. The plate diameter DB of each of the selected 50 particles is measured. The plate diameter DBs thus obtained are simply averaged (arithmetic averaged) to obtain the average plate diameter DB. ave Average plate diameter DB ave is the average grain size. And the average plate thickness DA ave and average plate diameter DB ave The average aspect ratio of the particles (DB ave / DA ave ) is required.

[0104] (Average particle volume of magnetic powder)

[0105] The average particle volume of the magnetic powder can be calculated as follows. First, as described above in relation to the method for calculating the average particle size of the magnetic powder, the average plate thickness DA ave and average plate diameter DB ave Next, the average particle volume V of the magnetic powder is calculated using the following formula:

[0106]

[0107] (Electrical Resistance)

[0108] Using electrodes with an interelectrode distance of 12.65 mm, a test piece (tape width 12.65 mm) is placed on this electrode with the magnetic layer surface facing down, a load of 1.62 N is applied to both ends, an applied voltage is applied, and after 1 minute of application, the electrical resistance is measured using an electrical resistance measuring device (ULTRA HIGH RESISTANCE METER R8340A, manufactured by ADVATEST). The applied voltage refers to the voltage actually applied to the test piece during measurement. The applied voltage during measurement is set as follows depending on the resistance value R.

[0109] Resistance value R>5×10 4 When Ω / sq: Applied voltage: 100±10V 5×10 4 Ω / sq > resistance value R > 5 x 10 3 When Ω / sq: Applied voltage: 10±1V Resistance value R<5×10 3 When Ω / sq: Applied voltage: Maximum voltage at which the cleaning tape does not deform

[0110] (4) Manufacturing method of cleaning tape

[0111] Next, a method for manufacturing the cleaning tape 10 having the above-described configuration will be described. First, a base layer-forming paint is prepared by kneading and / or dispersing non-magnetic powder, a binder, etc. in a solvent. Next, a magnetic layer-forming paint is prepared by kneading and / or dispersing magnetic powder, a binder, etc. in a solvent. The following solvents, dispersing devices, and kneading devices can be used to prepare the magnetic layer-forming paint and the base layer-forming paint.

[0112] Examples of solvents that can be used in preparing the coating material include ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; alcohol-based solvents such as methanol, ethanol, and propanol; ester-based solvents such as methyl acetate, ethyl acetate, butyl acetate, propyl acetate, ethyl lactate, and ethylene glycol acetate; ether-based solvents such as diethylene glycol dimethyl ether, 2-ethoxyethanol, tetrahydrofuran, and dioxane; aromatic hydrocarbon-based solvents such as benzene, toluene, and xylene; and halogenated hydrocarbon-based solvents such as methylene chloride, ethylene chloride, carbon tetrachloride, chloroform, and chlorobenzene. One of these may be used, or a mixture of two or more of them may be used.

[0113] Examples of the kneading device used in preparing the above-mentioned coating material include, but are not limited to, a continuous twin-screw kneader, a continuous twin-screw kneader capable of multi-stage dilution, a kneader, a pressure kneader, and a roll kneader. Examples of the dispersing device used in preparing the above-mentioned coating material include, but are not limited to, a roll mill, a ball mill, a horizontal sand mill, a vertical sand mill, a spike mill, a pin mill, a tower mill, a pearl mill (such as the "DCP Mill" manufactured by Eirich), a homogenizer, and an ultrasonic disperser.

[0114] Next, a paint for forming an underlayer is applied to one main surface of the base layer 11 and dried to form the underlayer 12. Subsequently, a paint for forming a magnetic layer is applied to the underlayer 12 and dried to form the magnetic layer 13 on the underlayer 12.

[0115] The resulting cleaning tape 10 is then rewound around a large diameter core and cured. Finally, the cleaning tape 10 is calendered and then cut to a predetermined width (e.g., 1 / 2 inch width). In order to maintain an appropriate abrasive force, the calendering temperature is preferably 95°C or less, more preferably 90°C or less, and even more preferably 85°C or less. In this manner, the desired elongated cleaning tape 10 is obtained.

[0116] (5) One embodiment of the cleaning tape cartridge

[0117] [Cartridge configuration]

[0118] A cleaning tape according to the present technology may be used housed in a cleaning tape cartridge, in which the cleaning tape may be wound around a reel, for example.

[0119] An example of the configuration of a cleaning tape cartridge 10A equipped with the cleaning tape T having the above-described configuration will be described with reference to FIG.

[0120] 5 is an exploded perspective view showing an example of the configuration of a cleaning tape cartridge 10A. The cleaning tape cartridge 10A is a cleaning tape cartridge that conforms to the LTO (Linear Tape-Open) standard, and includes a cartridge case 10B made up of a lower shell 212A and an upper shell 212B, a reel 10C around which a cleaning tape T is wound, a reel lock 214 and a reel spring 215 for locking the rotation of the reel 10C, a spider 216 for unlocking the locked state of the reel 10C, a sliding door 217 that straddles the lower shell 212A and the upper shell 212B and opens and closes a tape pull-out opening 212C provided in the cartridge case 10B, a door spring 218 that biases the sliding door 217 to a closed position of the tape pull-out opening 212C, a write protect 219 for preventing accidental erasure, and a cartridge memory 211. The reel 10C is generally disk-shaped with an opening in the center, and is composed of a reel hub 213A and a flange 213B made of a hard material such as plastic. A leader tape LT is connected to one end of the cleaning tape T. A leader pin 220 is provided at the tip of the leader tape LT.

[0121] The present technology can also employ the following configurations. [1] A cleaning tape including, in this order, a magnetic layer and an underlayer, wherein the underlayer has an average thickness of 1.60 μm or more, the surface roughness Rab of the magnetic layer surface is 2.9 nm or less, the abrasivity after 50 round trips against an AlFeSil rectangular pillar is 65 μm or less, and the abrasivity after 50 to 100 round trips against an AlFeSil rectangular pillar is 25 μm or more. [2] The cleaning tape according to [1], wherein the magnetic layer contains magnetic powder. [3] The cleaning tape according to [1] or [2], wherein the magnetic powder contains barium ferrite. [4] The cleaning tape according to any one of [1] to [3], wherein the average thickness (average total thickness) is 9.2 μm or less. [5] The cleaning tape according to any one of [1] to [4], wherein the average thickness of the underlayer is 1.85 μm or less. [6] The cleaning tape according to any one of [1] to [5], wherein a standard cleaning tape is brought into contact with and slid over the surface of a magnetic media abrasive tape, and then a partial area of ​​the surface of the magnetic media abrasive tape that has come into contact with the standard cleaning tape is photographed, and among the pixels constituting the photographed image, the ratio of the percentage of pixels that show powder that has fallen off from the standard cleaning tape and adhered to the magnetic media abrasive tape due to powder falling off from the cleaning tape to be inspected (powder fall rate) is greater than 1.0. [7] The cleaning tape according to any one of [1] to [5], wherein the average particle volume of the barium ferrite magnetic powder is 500 nm 3 ~2000nm 3 [8] The cleaning tape according to [1], further comprising abrasive particles in the magnetic layer. [9] The cleaning tape according to [8], wherein the abrasive particles are alumina particles.

[10] The cleaning tape according to [9], wherein the alumina particles have an average particle size of 20 nm to 80 nm.

[11] The cleaning tape according to

[10] , wherein the electrical resistance of the surface of the magnetic layer of the cleaning tape is 1×10 3 Ω / sq ~ 5 x 10 10

[10] The cleaning tape according to any one of [1] to

[10] , wherein the average thickness of the underlayer is 1.67 μm or more.

[12] The cleaning tape according to any one of [1] to

[11] , wherein the average thickness of the underlayer is 1.67 μm or more.

[13] The cleaning tape according to any one of [1] to

[12] , wherein the cleaning tape comprises a magnetic layer, an underlayer, a base layer, and a back layer in this order.

[14] The cleaning tape according to any one of [1] to

[13] , wherein the average thickness (average total thickness) is 8.80 μm or less.

[15] The cleaning tape according to any one of [1] to

[14] , wherein the cleaning tape is for use in a magnetic recording system.

[0122] 3. Working Example

[0123] Hereinafter, the present technology will be specifically explained using examples, but the present technology is not limited to these examples.

[0124] In this embodiment, the surface roughness of the magnetic layer surface, abrasivity, and the average thickness (average total thickness) of the cleaning tape t T , the average thickness of the magnetic layer t m The average thickness of the underlayer, the average thickness of the base layer, the average thickness of the back layer, and the electrical resistance were determined by the measurement method described in the above embodiment.

[0125] The powder shedding rate, cleaning power, and head damage were measured as follows.

[0126] (Powder shedding rate)

[0127] The powder shedding rate is determined by sliding a standard cleaning tape over the surface of a magnetic media abrasive tape while it is in contact with the surface, photographing a portion of the surface of the magnetic media abrasive tape that has come into contact with the standard cleaning tape, and calculating the ratio of the percentage of pixels that represent powder that has adhered to the magnetic media abrasive tape due to powder shedding from the cleaning tape being inspected to the percentage of pixels that represent powder that has adhered to the magnetic media abrasive tape due to powder shedding from the standard cleaning tape among the pixels that make up the photographed image.

[0128] <Sample preparation>

[0129] The sample for evaluating the powder shedding rate was prepared as follows. First, a rewinding machine as shown in FIG. 9 was prepared, and a cleaning tape 93 was set on the rewinding machine. Specifically, the long cleaning tape 93 was unwound from the unwinding reel 92 and set on the take-up reel 91 so that the back surface of the cleaning tape contacted six arc-shaped tape running guides 94 and two roughly cylindrical, rod-shaped rollers 97. The magnetic surface of the cleaning tape 93 was set so as to contact the surface of a magnetic media polishing tape (WA4000, manufactured by Mipox) 95 wound around the surface of a drive head 96. The magnetic media polishing tape 95 was a film coated with abrasive particles on the order of several μm in size.

[0130] The six tape running guides 94 (particularly their surfaces) and the two rollers 97 were all made of stainless steel SUS304.

[0131] The arrangement of the six arc-shaped tape travel guides 94 will be described with reference to FIG. 9 . As shown in FIG. 9 , the cleaning tape 93 was set in the six tape travel guides 94. Hereinafter, the six tape travel guides 94 will be referred to as the "first tape travel guide," the "second tape travel guide," the "third tape travel guide," the "fourth tape travel guide," the "fifth tape travel guide," and the "sixth tape travel guide" from the side closest to the supply reel 92. Between the first and second tape travel guides, the distance d1 by which the tape did not follow the tape travel guides was approximately 20 mm. Between the second and third tape travel guides, the distance d2 by which the tape did not follow the tape travel guides was approximately 20 mm. Two rollers 97 were set between the third and fourth tape travel guides. The diameter of these two rollers 97 was 7 mm. Hereinafter, the two rollers 97 will be referred to as the "first roller" and the "second roller" from the side closest to the supply reel 92. Between the first roller and the second roller, the cleaning tape 93 was set so as to contact the surface of the magnetic media polishing tape (WA4000, manufactured by Mipox) 95 wound on the surface of the drive head 96, forming an included angle of 10°. Between the fourth tape travel guide and the fifth tape travel guide, the distance d5 at which the tape did not follow the tape travel guides was approximately 20 mm. Between the fifth tape travel guide and the sixth tape travel guide, the distance d6 at which the tape did not follow the tape travel guides was approximately 20 mm. Furthermore, the six tape travel guides were fixed so as not to rotate, but the roller 97 was rotatable.

[0132] The cleaning tape 93 was held on the tape running guide 94, roller 97, and drive head 96 so as not to move in the width direction of the cleaning tape 93.

[0133] The sample for evaluating the powder shedding rate was prepared as follows. The cleaning tape 93 was unwound from the unwinding reel 92 and run under the following conditions while contacting a magnetic media abrasive tape 95 wound around the surface of a drive head 96. A magnetic media abrasive tape 95 with powder shed from the cleaning tape 93 attached thereto was obtained as a sample. The sample size was 13 mm in the longitudinal direction and 10 mm in the width direction. The number of samples was three. In addition to the evaluation samples of the examples and comparative examples to be tested, a reference sample was similarly prepared using a commercially available cleaning tape (a cleaning tape for LTO commercially available before 2022, manufactured by Sony Group Corporation) as a standard cleaning tape.

[0134] <Driving conditions>

[0135] Running mode: 400m x 5 round trips Tension: 1N Running speed: 3m / s Embracing angle: 10°

[0136] <Quantification>

[0137] The evaluation samples and the reference sample prepared as test subjects were evaluated by quantifying the powder adhering to the surface of the magnetic media abrasive tape as contaminants. The evaluation was carried out as follows: The evaluation samples and the reference sample were photographed in black and white using a stereomicroscope (SZX16, manufactured by Olympus Corporation) with a magnification of 25x and an exposure time of 1 / 20 seconds.

[0138] The image data captured by the stereo microscope is binarized by a computer and converted into image data in which each pixel is either white or black. More specifically, the binarization process is performed using image processing software (Image J) under the processing conditions described below.

[0139] <Binarization processing conditions for obtaining information about powder-shedding stains>

[0140] Software: Image J Ver. 1.44p Brightness: -100 Clarity: +100

[0141] The threshold value for the binarization process was set so that the area occupied by the portion where no powder had fallen from the cleaning tape and no powder had adhered to the magnetic media abrasive tape was judged as a white area, while the area where powder had fallen from the cleaning tape and where powder had adhered to the magnetic media abrasive tape was judged as a black area. Specifically, the image data of the reference sample was binarized, and the black / white judgment threshold value was adjusted so that the black area in the image data was 30 to 50%. The black area of ​​the image of the evaluation sample was also measured using the same black / white judgment threshold value.

[0142] The above process was carried out for both the evaluation sample and the reference sample, and based on the results, the ratio of the black area of ​​the evaluation sample to the black area of ​​the reference sample was calculated as powder falloff, as shown in the following formula (1).

[0143] Powder shedding rate = Black area of ​​evaluation sample / Black area of ​​reference sample (1) Here, the powder shedding rate refers to the ratio of the degree of powder shedding from the evaluation cleaning paper to the degree of powder shedding from a reference commercially available cleaning paper. The powder shedding rate may be preferably less than 1.0, preferably 0.8 or less, more preferably 0.6 or less, and even more preferably 0.5 or less. Note that a powder shedding rate exceeding 1.0 was evaluated as being inferior to the reference sample in terms of powder shedding properties.

[0144] (cleaning power)

[0145] In a drive with a reduced error rate, we checked whether the error rate would recover after using a cleaning tape. A drive with a reduced error rate due to magnetic head contamination was used. A cleaning process was performed under the following conditions. The error rate was measured using the drive that had undergone the cleaning process.

[0146] <Cleaning conditions>

[0147] Tension: 1N Number of reciprocations: 3

[0148] <Error rate measurement>

[0149] Using a tape running system from Mountain Engineering II, and a magnetic head from a commercially available LTO (Linear Tape Open)-9 drive, recording signals were recorded on a commercially available 1 / 2-inch magnetic tape (LTO-9 manufactured by Sony Group Corporation) at a recording density equivalent to that of the commercially available LTO-9. The error rate of the magnetic tape was then measured after 24 hours of running in an environment of 23°C and 50% relative humidity. The results are shown in Table 1. In Table 1, cleaning power was evaluated based on the measured error rate and using the following criteria: OK (good): Bit error rate was 5x10 -3 Less than NG (poor): Bit error rate is 5 x 10 -3 End

[0150] (head damage)

[0151] Using the magnetic head of an LTO-9 drive in three environments: room temperature, 35°C and 20% RH relative humidity, and 26°C and 80% RH relative humidity, the drive's flexible cable was first removed and the electrical resistance of the magnetic head was measured using an electrical resistance measuring device manufactured by Advantest. The magnetic head was then cleaned 56 times using a cartridge containing a cleaning tape. After cleaning, the electrical resistance of the magnetic head was measured using the electrical resistance measuring device manufactured by Advantest.

[0152] Damage to the magnetic head was evaluated based on the head resistance change rate described below.

[0153] Head resistance change rate=(electrical resistance value of magnetic head after cleaning process / electrical resistance value of magnetic head before cleaning process)

[0154] Damage to the magnetic head was evaluated according to the following criteria.

[0155] No head damage: Head resistance change rate over 20% Head damage: Head resistance change rate 20% or less

[0156] [Example 1]

[0157] (Preparation process of paint for forming magnetic layer)

[0158] The magnetic layer-forming paint was prepared as follows. First, a first composition having the following formulation was kneaded using an extruder. Next, the kneaded first composition and a second composition having the following formulation were added to a stirring tank equipped with a disperser and premixed. Subsequently, further sand mill mixing was performed and filtering was performed to prepare the magnetic layer-forming paint.

[0159] (First composition)

[0160] Magnetic powder (hexagonal ferrite with M-type structure, composition: Ba-Ferrite, shape: plate-like hexagonal particles, average particle volume: 1600 nm 3 Vinyl chloride resin (cyclohexanone solution 30% by mass): 46 parts by mass (degree of polymerization 300, Mn = 10,000, contains polar groups OSOK = 0.07 mmol / g and secondary OH = 0.3 mmol / g)

[0161] (Second composition)

[0162] Vinyl chloride resin: 1.6 parts by mass (as a 30% by mass resin in cyclohexanone solution) n-butyl stearate: 2 parts by mass Methyl ethyl ketone: 121.3 parts by mass Toluene: 121.3 parts by mass Cyclohexanone: 60.7 parts by mass Aluminum oxide powder: 7.5 parts by mass (α-Al2O3, average particle size 50 nm, manufactured by Sumitomo Chemical Co., Ltd., trade name: HIT100, Mohs hardness: 9) Carbon black: 2.0 parts by mass (average particle size 70 nm, manufactured by Tokai Carbon Co., Ltd., trade name: Seest TA)

[0163] Finally, 2 parts by weight of polyisocyanate (product name: Coronate L, manufactured by Nippon Polyurethane Co., Ltd.) and 2 parts by weight of myristic acid were added as curing agents to the magnetic layer-forming coating material prepared as described above.

[0164] (Preparation process of paint for forming base layer)

[0165] The paint for forming the primer layer was prepared as follows. First, the third composition having the following composition was kneaded using an extruder. Next, the kneaded third composition and the fourth composition having the following composition were added to a stirring tank equipped with a disperser and premixed. Subsequently, further mixing was performed using a sand mill and filtering was performed to prepare the paint for forming the primer layer.

[0166] (Third composition)

[0167] Acicular iron oxide powder: 100 parts by mass (α-Fe2O3, average major axis length 0.15 μm) Aluminum oxide powder: 5 parts by mass (α-Al 2 O 3 , average particle size 80 nm, manufactured by Sumitomo Chemical Co., Ltd., trade name: HIT82, Mohs hardness: 9) Vinyl chloride resin: 55.6 parts by mass (resin solution: resin content 30% by mass, cyclohexanone 70% by mass)

[0168] (Fourth composition)

[0169] Polyurethane resin UR8200 (manufactured by Toyobo Co., Ltd.): 18.5 parts by mass, n-butyl stearate: 2 parts by mass, methyl ethyl ketone: 108.2 parts by mass, toluene: 108.2 parts by mass, cyclohexanone: 18.5 parts by mass, carbon black: 10 parts by mass (average particle size 20 nm)

[0170] Finally, 2 parts by mass of polyisocyanate (trade name: Coronate L, manufactured by Tosoh Corporation) and 2 parts by mass of myristic acid were added as a curing agent to the base layer forming paint prepared as described above.

[0171] (Step of preparing paint for forming back layer)

[0172] A paint for forming a back layer was prepared as follows. The following raw materials were mixed in a stirring tank equipped with a disperser and filtered to prepare a paint for forming a back layer. Carbon black (manufactured by Asahi Carbon Co., Ltd., product name: #80): 100 parts by mass Polyester polyurethane: 150 parts by mass (resin solution: polyurethane resin blend amount 30% by mass, cyclohexanone blend amount 70% by mass) (manufactured by Nippon Polyurethane Co., Ltd., product name: N-2304) Methyl ethyl ketone: 500 parts by mass Toluene: 400 parts by mass Cyclohexanone: 100 parts by mass Polyisocyanate (product name: Coronate L, manufactured by Tosoh Corporation): 9 parts by mass

[0173] (Film forming process)

[0174] Using the coating material prepared as described above, a cleaning tape was prepared as follows.

[0175] First, a long PEN film (base film) with an average thickness of 6.57 μm was prepared as a support for the base layer of the cleaning tape. Next, a primer layer-forming paint was applied to one main surface of the PEN film and dried to form a primer layer on one main surface of the PEN film so that the average thickness of the final product would be 1.80 μm. Next, a magnetic layer-forming paint was applied to the primer layer and dried to form a magnetic layer on the primer layer so that the average thickness of the final product would be 0.07 μm.

[0176] Next, the PEN film on which the underlayer and magnetic layer were formed was subjected to a curing treatment, and then calendering was carried out at a calendering temperature of 80° C. to smooth the surface of the magnetic layer.

[0177] (Cutting process)

[0178] The cleaning tape obtained as described above was cut into a width of 1 / 2 inch (12.65 mm), thereby obtaining a long cleaning tape.

[0179] The cleaning tape having a width of 1 / 2 inch was wound around a reel provided in a cartridge case to obtain a cleaning tape cartridge.

[0180] The obtained cleaning tape had a surface roughness Rab of 2.6 nm on the magnetic side, an abrasivity of 46.8 μm after 50 reciprocations against the AlFeSil rectangular pillars, and an abrasivity of 29.0 μm after 50 reciprocations against the AlFeSil rectangular pillars. T The average thickness of the underlayer was 8.90 μm, and the average thickness of the underlayer was 1.80 μm.

[0181] [Example 2]

[0182] Example 1 refers to the cleaning tape with an average thickness (average total thickness) t TA cleaning tape was obtained in the same manner as in Example 1, except that the average thickness of the underlayer was 8.75 μm, the average thickness of the underlayer was 1.65 μm, the average thickness of the base layer was 6.56 μm, and the average thickness of the back layer was 0.47 μm. The obtained cleaning tape had a surface roughness Rab of 2.5 nm on the magnetic surface side, an abrasivity of 45.8 μm after 50 reciprocations against AlFeSil rectangular pillars, and an abrasivity of 26.3 μm after 50 reciprocations against AlFeSil rectangular pillars.

[0183] [Comparative Example 1]

[0184] Example 1 refers to the cleaning tape with an average thickness (average total thickness) t T A cleaning tape was obtained in the same manner as in Example 1, except that the average thickness of the underlayer was 8.75 μm, the average thickness of the underlayer was 1.65 μm, the average thickness of the base layer was 6.58 μm, the average thickness of the back layer was 0.45 μm, and the calendering temperature was 60° C. The obtained cleaning tape had a surface roughness Rab on the magnetic surface side of 2.7 nm, an abrasivity after 50 reciprocations against AlFeSil rectangular pillars of 68.1 μm, and an abrasivity after 50 to 100 reciprocations against AlFeSil rectangular pillars of 33.4 μm.

[0185] [Comparative Example 2]

[0186] Example 1 refers to the cleaning tape with an average thickness (average total thickness) t T A cleaning tape was obtained in the same manner as in Example 1, except that the average thickness of the underlayer was 8.55 μm, the average thickness of the underlayer was 1.45 μm, the average thickness of the base layer was 6.60 μm, the average thickness of the back layer was 0.43 μm, and the calendering temperature was 60° C. The obtained cleaning tape had a surface roughness Rab of 2.9 nm on the magnetic surface side, an abrasivity after 50 reciprocations against AlFeSil rectangular pillars of 44.8 μm, and an abrasivity after 50 to 100 reciprocations against AlFeSil rectangular pillars of 28.6 μm.

[0187] [Comparative Example 3]

[0188] Example 1 refers to the cleaning tape with an average thickness (average total thickness) t T A cleaning tape was obtained in the same manner as in Example 1, except that the average thickness of the underlayer was 8.55 μm, the average thickness of the underlayer was 1.45 μm, the average thickness of the base layer was 6.58 μm, and the average thickness of the back layer was 0.45 μm. The obtained cleaning tape had a surface roughness Rab of 2.7 nm on the magnetic surface side, an abrasivity of 41.0 μm after 50 reciprocations against an AlFeSil rectangular pillar, and an abrasivity of 22.5 μm after 50 reciprocations against an AlFeSil rectangular pillar.

[0189] [Comparative Example 4]

[0190] Example 1 refers to the cleaning tape with an average thickness (average total thickness) t T A cleaning tape was obtained in the same manner as in Example 1, except that the average thickness of the underlayer was 8.55 μm, the average thickness of the underlayer was 1.45 μm, the average thickness of the base layer was 6.59 μm, the average thickness of the back layer was 0.44 μm, and the calendering temperature was 100° C. The obtained cleaning tape had a surface roughness Rab on the magnetic surface side of 2.3 nm, an abrasivity after 50 reciprocations against AlFeSil rectangular pillars of 29.2 μm, and an abrasivity after 50 reciprocations to 100 reciprocations against AlFeSil rectangular pillars of 19.2 μm.

[0191] [Comparative Example 5]

[0192] A cleaning tape was obtained in the same manner as in Example 1, except that metal magnetic powder (Fe—Co acicular magnetic powder, average major axis length 0.1 μm) was used instead of barium ferrite magnetic powder, the average thickness of the underlayer of the cleaning tape was 1.45 μm, the average thickness of the base layer was 6.63 μm, the average thickness of the back layer was 0.62 μm, the average thickness of the magnetic layer was 0.20 μm, and the calendering temperature was 115° C. The obtained cleaning tape had a surface roughness Rab on the magnetic side of 3.1 nm, an abrasivity after 50 reciprocations against AlFeSil rectangular pillars of 45.4 μm, and an abrasivity after 50 reciprocations to 100 reciprocations against AlFeSil rectangular pillars of 33.1 μm.

[0193] Table 1 shows the constructions and evaluation results of the cleaning tapes of Examples 1 and 2 and Comparative Examples 1 to 5.

[0194]

[0195] The results shown in Table 1 reveal the following.

[0196] The cleaning tapes of Examples 1 and 2 all had underlayer thicknesses of 1.60 μm or more, magnetic layer surface roughnesses Rab of 2.9 nm or less, abrasivity after 50 reciprocating strokes against AlFeSil rectangular pillars of 65 μm or less, and abrasivity after 50 to 100 reciprocating strokes against AlFeSil rectangular pillars of 25 μm or more, exhibiting good cleaning power and causing no head damage to the magnetic head. On the other hand, the cleaning tapes of Comparative Examples 3 and 4 all had abrasivity after 50 to 100 reciprocating strokes against AlFeSil rectangular pillars of less than 25 μm, exhibiting insufficient cleaning power.

[0197] Comparing Example 1 and Comparative Example 5, the cleaning tape of Example 1 had an underlayer thickness of 1.60 μm or more, a surface roughness Rab of the magnetic layer surface of 2.9 nm or less, and had good cleaning power and did not cause head damage to the magnetic head. On the other hand, the cleaning tape of Comparative Example 5 had an underlayer thickness of less than 1.60 μm, a surface roughness Rab of the magnetic layer surface of more than 2.9 nm, and did not have sufficient cleaning power.

[0198] Comparing Example 2 and Comparative Example 2, the cleaning tape of Example 2 had a base layer thickness of 1.60 μm or more, a magnetic layer surface roughness Rab of 2.9 nm or less, and had good cleaning power and did not cause head damage to the magnetic head. On the other hand, the cleaning tape of Comparative Example 2 had a base layer thickness of less than 1.60 μm, a powder shedding rate of more than 1.0, and insufficient cleaning power.

[0199] Although the embodiments and examples of the present technology have been specifically described above, the present technology is not limited to the above-described embodiments and examples, and various modifications based on the technical ideas of the present technology are possible.

[0200] For example, the configurations, methods, steps, shapes, materials, and numerical values, etc., given in the above-described embodiments and examples are merely examples, and different configurations, methods, steps, shapes, materials, and numerical values, etc., may be used as necessary. Furthermore, the chemical formulas of compounds, etc., are representative, and are not limited to the valences, etc., given as long as they are general names of the same compounds.

[0201] Furthermore, the configurations, methods, processes, shapes, materials, numerical values, and the like of the above-described embodiments and examples can be combined with each other without departing from the spirit of the present technology.

[0202] Furthermore, in this specification, a numerical range indicated using "to" indicates a range that includes the numerical values ​​before and after "to" as the minimum and maximum values, respectively. In the numerical ranges described in stages in this specification, the upper limit or lower limit of a numerical range in a certain stage may be replaced with the upper limit or lower limit of a numerical range in another stage. Unless otherwise specified, the materials exemplified in this specification may be used alone or in combination of two or more types.

[0203] 10 cleaning tape 11 base layer 12 underlayer 13 magnetic layer 14 back layer

Claims

1. A cleaning tape comprising, in that order, a magnetic layer and an underlayer, wherein the average thickness of the underlayer is 1.60 μm or more, the surface roughness Rab of the magnetic layer surface is 2.9 nm or less, the abrasivity after 50 round trips against an AlFeSil rectangular pillar is 65 μm or less, and the abrasivity after 50 to 100 round trips against an AlFeSil rectangular pillar is 25 μm or more.

2. The cleaning tape of claim 1, wherein said magnetic layer comprises magnetic powder.

3. The cleaning tape of claim 1, wherein said magnetic powder comprises barium ferrite.

4. The cleaning tape according to claim 1, having an average thickness (average total thickness) of 9.2 μm or less.

5. The cleaning tape according to claim 1, wherein the average thickness of said undercoat layer is 1.85 μm or less.

6. A cleaning tape as described in claim 1, wherein a standard cleaning tape is brought into contact with and slid over a surface of a polishing tape for magnetic media, and then an image is taken of a portion of the surface of the polishing tape for magnetic media that has come into contact with the standard cleaning tape, and among the pixels constituting the photographed image, the ratio (powder fall rate) of the percentage of pixels that show powder that has fallen from the cleaning tape being inspected and has adhered to the polishing tape for magnetic media due to powder fall from the standard cleaning tape to the percentage of pixels that show powder that has fallen from the cleaning tape being inspected is less than 1.

0.

7. The average particle volume of the barium ferrite magnetic powder is 500 nm 3 ~2000nm 3 4. The cleaning tape of claim 3 .

8. The cleaning tape of claim 1 further comprising abrasive particles in said magnetic layer.

9. The cleaning tape of claim 8, wherein said abrasive particles are alumina particles.

10. The cleaning tape of claim 9, wherein the alumina particles have an average particle size of 20 nm to 80 nm.

11. The electrical resistance of the surface of the magnetic layer of the cleaning tape is 1×10 3 Ω / sq ~ 5 x 10 10 Ω / sq.

12. The cleaning tape of claim 1, wherein the average thickness of said undercoat layer is 1.67 μm or more.

13. The cleaning tape of claim 1, comprising, in that order, a magnetic layer, an undercoat layer, a base layer, and a backing layer.

14. The cleaning tape of claim 1, having an average thickness (average total thickness) of 8.80 μm or more.

15. The cleaning tape of claim 1 which is a cleaning tape for a magnetic recording system.

Citation Information

Patent Citations

  • Cleaning tape for magnetic head

    JP2004326995A

  • Cleaning tape

    JP2006107598A

  • Magnetic recording medium, magnetic tape cartridge and magnetic recording / reproducing device

    JP2023069536A

Cited By

  • Cleaning tape, cleaning tape cartridge, magnetic tape, and magnetic tape storage body

    WO2026172775A1