Negative electrode for nonaqueous electrolyte power storage elements, and nonaqueous electrolyte power storage element

The use of a negative electrode with low porosity graphite and specific X-ray diffraction characteristics addresses the output reduction in low-temperature environments by enhancing charge transport and maintaining performance in nonaqueous electrolyte storage devices.

WO2024241959A1PCT designated stage expired Publication Date: 2024-11-28GS YUASA INT LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/017761
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-22
Filing Date
2024-05-14
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Nonaqueous electrolyte storage devices, such as lithium-ion batteries, face a reduction in output performance in low-temperature environments due to increased resistance from high porosity graphite particles allowing electrolyte decomposition products to form films within the electrodes, and existing solutions do not effectively enhance charge transport at low temperatures.

Method used

A negative electrode with a graphite active material layer having internal porosity of 2% or less and a specific X-ray diffraction peak intensity ratio (I(110)/I(004)) of 0.055 or higher, which reduces internal film formation and facilitates easier charge transport by random orientation of graphene layers, enhancing low-temperature performance.

Benefits of technology

The solution significantly increases the output of nonaqueous electrolyte storage devices in low-temperature environments by minimizing internal resistance and improving charge transport efficiency, while maintaining capacity retention and input retention rates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024017761_28112024_PF_FP_ABST
    Figure JP2024017761_28112024_PF_FP_ABST
Patent Text Reader

Abstract

A negative electrode for nonaqueous electrolyte power storage elements according to one aspect of the present invention is provided with a negative electrode active material layer that contains graphite particles. The internal void fraction of the graphite particles is 2% or less, and the ratio (I(110) / I(004)) of the peak intensity I(110) attributed to the (110) plane of the graphite to the peak intensity I(004) attributed to the (004) plane of the graphite is 0.055 or more in an X-ray diffraction measurement of the negative electrode active material layer, the X-ray diffraction measurement using CuKα rays.
Need to check novelty before this filing date? Find Prior Art

Description

Negative electrode for non-aqueous electrolyte storage element and non-aqueous electrolyte storage element

[0001] The present invention relates to a negative electrode for a nonaqueous electrolyte storage element and a nonaqueous electrolyte storage element.

[0002] Due to their high energy density, non-aqueous electrolyte secondary batteries, typified by lithium ion secondary batteries, are widely used in electronic devices such as personal computers and communication terminals, automobiles, etc. In addition to non-aqueous electrolyte secondary batteries, capacitors such as lithium ion capacitors and electric double layer capacitors are also widely used as non-aqueous electrolyte energy storage elements.

[0003] A typical nonaqueous electrolyte storage element includes an electrode assembly in which a positive electrode containing a positive electrode active material and a negative electrode containing a negative electrode active material are stacked with a separator interposed therebetween. This electrode assembly is housed in a container together with a nonaqueous electrolyte to form a nonaqueous electrolyte storage element. Carbon materials such as graphite are widely used as the negative electrode active material (see Patent Documents 1 and 2).

[0004] Japanese Patent Application Publication No. 2005-222933 Japanese Patent Application Publication No. 2017-069039

[0005] Non-aqueous electrolyte energy storage elements are required to have various performance characteristics according to the environment in which they are used, etc. For example, a non-aqueous electrolyte energy storage element that is expected to be used in a low-temperature environment is desired to have a large output even in a low-temperature environment. The output here refers to the energy that can be extracted per unit time during discharge.

[0006] An object of the present invention is to provide a negative electrode for a nonaqueous electrolyte electricity storage element that can increase the output of the nonaqueous electrolyte electricity storage element in a low-temperature environment, and a nonaqueous electrolyte electricity storage element including such a negative electrode for a nonaqueous electrolyte electricity storage element.

[0007] A negative electrode for a nonaqueous electrolyte storage element according to one aspect of the present invention includes a negative electrode active material layer containing graphite particles, the graphite particles having an internal porosity of 2% or less, and in an X-ray diffraction measurement of the negative electrode active material layer using CuKα radiation, the ratio of a peak intensity I(110) attributable to a (110) plane of graphite to a peak intensity I(004) attributable to a (004) plane (I(110) / I(004)) is 0.055 or more.

[0008] A nonaqueous electrolyte storage element according to another aspect of the present invention includes the negative electrode for a nonaqueous electrolyte storage element according to the aspect of the present invention.

[0009] According to any one aspect of the present invention, it is possible to provide a negative electrode for a nonaqueous electrolyte electricity storage element that can increase the output of the nonaqueous electrolyte electricity storage element in a low-temperature environment, and a nonaqueous electrolyte electricity storage element including such a negative electrode for a nonaqueous electrolyte electricity storage element.

[0010] Fig. 1 is a see-through perspective view showing one embodiment of a nonaqueous electrolyte storage element. Fig. 2 is a schematic diagram showing one embodiment of an electricity storage device formed by assembling a plurality of nonaqueous electrolyte storage elements. Fig. 3 is a graph showing the results of measuring the output of a nonaqueous electrolyte storage element of an example in a low-temperature environment. Fig. 4 is a graph showing the results of measuring the capacity retention rate after storage of a nonaqueous electrolyte storage element of an example. Fig. 5 is a graph showing the results of measuring the input retention rate of a nonaqueous electrolyte storage element of an example in a low-temperature environment after storage.

[0011] First, an outline of the negative electrode for a nonaqueous electrolyte electricity storage element and the nonaqueous electrolyte electricity storage element disclosed in this specification will be described.

[0012] [1] A negative electrode for a nonaqueous electrolyte storage element (hereinafter also simply referred to as "negative electrode") according to one aspect of the present invention includes a negative electrode active material layer containing graphite particles, wherein the graphite particles have an internal porosity of 2% or less, and in X-ray diffraction measurement of the negative electrode active material layer using CuKα radiation, the ratio of a peak intensity I(110) assigned to a (110) plane of graphite to a peak intensity I(004) assigned to a (004) plane (I(110) / I(004)) is 0.055 or more.

[0013] The negative electrode described in [1] above can increase the output of a nonaqueous electrolyte storage element in a low-temperature environment. While the reason for this is unclear, the following reason is presumed. When graphite particles with a high internal porosity are used in the negative electrode of a nonaqueous electrolyte storage element, the nonaqueous electrolyte penetrates the voids inside the graphite particles, and a high-resistance coating derived from decomposition products of the nonaqueous electrolyte is likely to form inside the particles. In this case, the resistance of the nonaqueous electrolyte storage element tends to increase, resulting in a decrease in output in a low-temperature environment. In contrast, the negative electrode described in [1] above uses graphite particles with an internal porosity of 2% or less. When graphite particles with such a low internal porosity are used in the negative electrode of a nonaqueous electrolyte storage element, a high-resistance coating is unlikely to form inside the graphite particles, thereby suppressing the increase in resistance of the nonaqueous electrolyte storage element and increasing output in a low-temperature environment. The ratio (I(110) / I(004)) is an index representing the orientation of the crystal structure (graphene layer) of graphite. In the negative electrode active material layer of the negative electrode described in [1] above, the ratio (I(110) / I(004)) is 0.055 or more, the graphene layers are somewhat randomly oriented, and the edge planes of the graphene layers are relatively randomly oriented, making it relatively easy for charge transport ions (lithium ions, etc.) to be inserted and desorbed between the graphene layers. In graphite particles with an internal porosity of 2% or less, insertion and desorption of charge transport ions between the graphene layers occurs mainly at the edge planes exposed on the outer surface of the graphite particles. Therefore, when the edge planes of the graphene layers are randomly oriented, insertion and desorption of charge transport ions is facilitated at the edge planes exposed on the outer surface of the graphite particles. This, combined with the fact that a high-resistance coating is unlikely to form inside the graphite particles, is thought to result in increased output in low-temperature environments.

[0014] "Graphite particles" are particles of graphite. "Graphite" refers to particles of graphite that have an average lattice spacing (d 002) is 0.33 nm or more and less than 0.34 nm. Here, the "discharged state" of a carbon material refers to a state in which the carbon material, which is the negative electrode active material, is discharged so that charge-transporting ions capable of being absorbed and released during charging and discharging are sufficiently released. For example, in a half-cell using a negative electrode containing a carbon material as the negative electrode active material as the working electrode and metallic lithium as the counter electrode, the open-circuit voltage is 0.6 V or more. When preparing a carbon material to be subjected to X-ray diffraction measurement from an assembled nonaqueous electrolyte energy storage element, the carbon material is brought into the above-mentioned discharged state by the following method. First, the nonaqueous electrolyte energy storage element is discharged at a constant current of 0.1 C to the discharge end voltage during normal use. Then, the nonaqueous electrolyte energy storage element is disassembled, and the negative electrode is removed. A half-cell is assembled using the removed negative electrode as the working electrode and metallic lithium as the counter electrode. If the open circuit voltage of this half-cell is less than 0.6 V, the half-cell is discharged at a current of 0.1 C so that the open circuit voltage is 0.6 V or higher. Discharging the half-cell refers to an oxidation reaction in which charge-transporting ions are released from the carbon material (graphite) serving as the negative electrode active material. The half-cell is disassembled, the negative electrode is removed, and the negative electrode is thoroughly washed with dimethyl carbonate and then dried under reduced pressure at room temperature. The negative electrode active material layer containing the carbon material is then peeled from the negative electrode substrate, and the negative electrode active material layer is washed with a solvent that dissolves binders and other components to remove the binders and other components. The washed negative electrode active material layer is immersed in an acid or alkaline solution to remove metals derived from the negative electrode substrate and SEI (solid electrolyte interface) coating, followed by washing with water and drying under reduced pressure to obtain a carbon material. The process from disassembling the nonaqueous electrolyte storage element to preparing the carbon material to be measured is carried out in a dry air atmosphere with a dew point of −40°C or lower. Here, normal use refers to the use of the nonaqueous electrolyte electricity storage element under charge and discharge conditions recommended or specified for the nonaqueous electrolyte electricity storage element.

[0015] The "internal porosity" of graphite particles refers to the area ratio of voids within the particle to the total area of ​​the particle in the cross section of the particle observed in an SEM image obtained using a scanning electron microscope (SEM). The "internal porosity (area ratio of voids within the particle to the total area of ​​the particle)" of graphite particles is determined by the following procedure. (1) Preparation of Measurement Sample The negative electrode to be measured is fixed with a thermosetting resin. The cross section of the negative electrode fixed with the resin is exposed by ion milling to prepare a measurement sample. Note that, if a negative electrode before assembly of a nonaqueous electrolyte storage element can be prepared, it is used as is. When the negative electrode to be measured is prepared from an assembled nonaqueous electrolyte storage element, a negative electrode is used that has been subjected to the steps from disassembly of the nonaqueous electrolyte storage element to vacuum drying of the negative electrode in accordance with the procedure for preparing a carbon material to be subjected to X-ray diffraction from the assembled nonaqueous electrolyte storage element described above. (2) Obtaining SEM Images A JSM-7001F SEM (manufactured by JEOL Ltd.) was used to obtain SEM images. SEM images were obtained by observing secondary electron images. The acceleration voltage was 5 kV. The observation magnification was set so that 3 to 15 graphite particles appeared in one field of view. The obtained SEM images were saved as image files. Other conditions, such as spot diameter, working distance, irradiation current, brightness, and focus, were appropriately set so that the contours of the graphite particles were clearly visible. (3) Cutting Out the Contours of Graphite Particles The contours of the graphite particles were cut out from the obtained SEM images using the image cutout function of the image editing software Adobe Photoshop Elements 11. This contour cutout was performed by using the quick selection tool to select the area outside the contours of the graphite particles and editing everything except the graphite particles to a black background. At this time, if the number of graphite particles whose contours could be cut out is less than three, another SEM image is acquired, and this is repeated until the number of graphite particles whose contours could be cut out is three or more. (4) Binarization Processing The image of the first of the cut-out graphite particles is binarized using image analysis software PopImaging 6.00, with a threshold value set to a concentration 20% lower than the concentration at which the intensity is maximum. By the binarization processing, the area on the side with higher concentration is calculated, and this is determined as the "area S1 of voids within the particle."Next, the image of the first graphite particle, as before, is subjected to binarization processing using a concentration of 10% as a threshold. The outer edge of the graphite particle is determined by the binarization processing, and the area inside the outer edge is calculated to determine the "area S0 of the entire particle." The calculated S1 and S0 are used to calculate the ratio of S1 to S0 (S1 / S0), thereby calculating the "area ratio R1 of voids within the particle to the area of ​​the entire particle" for the first graphite particle. The images of the second and subsequent graphite particles among the cut-out graphite particles are also subjected to the binarization processing, to calculate the area S1 and area S0. The void area ratios R2, R3, ... of each graphite particle are calculated based on the calculated area S1 and area S0. (5) Determination of void area ratio The "internal porosity (area ratio of voids within the particle to the area of ​​the entire particle)" is determined by calculating the average value of all void area ratios R1, R2, R3, ... calculated by the binarization processing. It should be noted that instead of the scanning electron microscope used in the "obtaining an SEM image," the image editing software used in the "cutting out the contours of graphite particles," and the image analysis software used in the "binarization process," devices and software capable of performing measurements, image editing, and image analysis equivalent to these may be used.

[0016] When a negative electrode before assembling a nonaqueous electrolyte storage element can be prepared, X-ray diffraction measurement using CuKα radiation of the negative electrode active material layer is performed on the negative electrode active material layer of that negative electrode. When the negative electrode to be measured is prepared from an assembled nonaqueous electrolyte storage element, X-ray diffraction measurement is performed on the negative electrode active material layer of the negative electrode that has been subjected to the above-mentioned procedure of preparing a carbon material to be subjected to X-ray diffraction from an assembled nonaqueous electrolyte storage element, from disassembly of the nonaqueous electrolyte storage element to drying of the negative electrode under reduced pressure.

[0017] X-ray diffraction measurement of the negative electrode active material layer using CuKα radiation is performed according to the following procedure. The negative electrode active material layer to be measured is placed in an X-ray diffraction sample holder. Powder X-ray diffraction measurement is performed using an X-ray diffractometer (Rigaku's "MiniFlex II"). The radiation source is CuKα radiation, the tube voltage is 30 kV, and the tube current is 15 mA. Diffracted X-rays are passed through a 30 μm-thick Kβ filter and detected by a high-speed one-dimensional detector (model number: D / tex Ultra 2). The sampling width is 0.01°, the scan speed is 5° / min, the divergence slit width is 0.625°, the receiving slit width is 13 mm (OPEN), and the scattering slit width is 8 mm. Note that background removal is performed when analyzing the X-ray diffraction data. Peaks derived from Kα2 are not removed. The diffraction peak intensity refers to the integrated intensity of the diffraction peak. X-ray diffraction measurement using CuKα radiation on the above carbon material is also carried out according to this procedure.

[0018] [2] In the negative electrode according to the above [1], the ratio (I(110) / I(004)) may be 0.32 or less.

[0019] In addition to the effects of the negative electrode described in [1] above, the negative electrode described in [2] above can improve the capacity retention rate of a nonaqueous electrolyte energy storage element after storage when the negative electrode active material layer has a BET specific surface area of ​​the same order. Although the reason for this is unclear, it is presumed that when the edge planes of the graphene layers exposed on the outer surfaces of the graphite particles are appropriately oriented, localized film growth occurs on the outer surfaces of the graphite particles, which has an influence.

[0020] [3] The negative electrode according to [1] or [2] above, wherein the BET specific surface area of ​​the negative electrode active material layer is 3.8 m 2 / g or less.

[0021] The negative electrode described in [3] above can improve the input power retention rate and capacity retention rate of a non-aqueous electrolyte storage element in a low-temperature environment after storage, in addition to the effects of the negative electrode described in [1] or [2] above. Although the reason for this is unclear, it is presumed that the smaller the BET specific surface area of ​​the negative electrode active material layer, the lower its reactivity with the non-aqueous electrolyte. The input power refers to the energy that can be taken in per unit time during charging.

[0022] When a negative electrode can be prepared before assembling a nonaqueous electrolyte storage element, the "BET specific surface area" of the negative electrode active material layer is measured on the negative electrode active material layer of that negative electrode. When the negative electrode to be measured is prepared from an assembled nonaqueous electrolyte storage element, the measurement is performed on the negative electrode active material layer of the negative electrode, which has been subjected to the above-described procedure for preparing a carbon material to be subjected to X-ray diffraction from the assembled nonaqueous electrolyte storage element, from disassembly of the nonaqueous electrolyte storage element to vacuum drying of the negative electrode. The BET specific surface area of ​​the negative electrode active material layer is determined by pore size distribution measurement using a nitrogen adsorption method. This measurement is performed using an "autosorb iQ" manufactured by Quantachrome. Five points are extracted from the resulting adsorption isotherm in the P / P0 = 0.06 to 0.3 region, and a BET plot is performed. The BET specific surface area is calculated from the y-intercept and slope of the straight line.

[0023] [4] In the negative electrode according to the above [1] or [2], the ratio (I(110) / I(004)) may be 0.27 or less.

[0024] The negative electrode described in [4] above can further increase the input power retention rate and capacity retention rate after storage in a low-temperature environment after storage of a nonaqueous electrolyte storage element, in addition to the effects of the negative electrode described in [1] or [2] above.

[0025] [5] In the negative electrode according to the above [3], the ratio (I(110) / I(004)) may be 0.27 or less.

[0026] The negative electrode described in the above [5] can further enhance the effects of the negative electrode described in the above [3]. Specifically, the negative electrode described in the above [5] can significantly improve the input power retention rate and the capacity retention rate after storage in a low-temperature environment after storage of a nonaqueous electrolyte storage element.

[0027] [6] A nonaqueous electrolyte storage element according to another aspect of the present invention includes the negative electrode according to any one of [1] to [5] above.

[0028] The nonaqueous electrolyte storage element described in [6] above has a large output in a low-temperature environment because it includes the negative electrode described in any one of [1] to [5] above.

[0029] [7] A negative electrode for a nonaqueous electrolyte storage battery according to another aspect disclosed in the present specification includes a negative electrode active material layer containing graphite particles, wherein the graphite particles have an internal porosity of 2% or less, and in an X-ray diffraction measurement of the negative electrode active material layer using CuKα radiation, the ratio of a peak intensity I(110) attributable to a (110) plane of graphite to a peak intensity I(004) attributable to a (004) plane (I(110) / I(004)) is 0.32 or less.

[0030] The negative electrode described in the above [7] can increase the capacity retention rate after storage of a nonaqueous electrolyte storage element when the negative electrode active material layer has a similar BET specific surface area.

[0031] [8] A nonaqueous electrolyte storage element according to another aspect disclosed in the present specification includes the negative electrode according to the above [7].

[0032] The nonaqueous electrolyte storage element described in [8] above includes the negative electrode described in [7] above, and therefore has a high capacity retention rate after storage when the negative electrode active material layer has a similar BET specific surface area.

[0033] Hereinafter, a negative electrode, a method for manufacturing a negative electrode, a nonaqueous electrolyte electricity storage element, an electricity storage device, a method for manufacturing a nonaqueous electrolyte electricity storage element, and other embodiments according to one embodiment of the present invention will be described in detail. Note that the names of the components (elementary components) used in each embodiment may differ from the names of the components (elementary components) used in the background art.

[0034] A negative electrode (negative electrode for a non-aqueous electrolyte storage element) according to one embodiment of the present invention includes a negative electrode substrate and a negative electrode active material layer disposed on the negative electrode substrate directly or via an intermediate layer. The negative electrode is used in a non-aqueous electrolyte storage element such as a non-aqueous electrolyte secondary battery.

[0035] The negative electrode substrate has electrical conductivity. Whether or not it has electrical conductivity is determined by whether or not the volume resistivity measured in accordance with JIS-H-0505 (1975) is 10 -2 The resistance is determined using Ω cm as a threshold value. Metals such as copper, nickel, stainless steel, and nickel-plated steel, or alloys thereof, carbonaceous materials, etc., are used as the material for the negative electrode substrate. Among these, copper or copper alloys are preferred. Examples of the negative electrode substrate include foil, vapor-deposited film, mesh, and porous material, with foil being preferred from the viewpoint of cost. Therefore, copper foil or copper alloy foil is preferred as the negative electrode substrate. Examples of copper foil include rolled copper foil and electrolytic copper foil.

[0036] The average thickness of the negative electrode substrate is preferably 2 μm to 35 μm, more preferably 3 μm to 30 μm, even more preferably 4 μm to 25 μm, and particularly preferably 5 μm to 20 μm. By setting the average thickness of the negative electrode substrate within the above range, the strength of the negative electrode substrate can be increased while increasing the energy density per volume of the nonaqueous electrolyte storage element.

[0037] The intermediate layer is a layer disposed between the negative electrode substrate and the negative electrode active material layer. The intermediate layer contains a conductive agent such as carbon particles to reduce the contact resistance between the negative electrode substrate and the negative electrode active material layer. The configuration of the intermediate layer is not particularly limited, and may contain, for example, a binder and a conductive agent.

[0038] The negative electrode active material layer contains graphite particles, and optionally contains other negative electrode active materials besides the graphite particles, a conductive agent, a binder, a thickener, a filler, and the like.

[0039] The graphite particles are a component that functions as a negative electrode active material. The graphite particles may be particles consisting essentially of graphite. The graphite content of the graphite particles may be 90% by mass or more, 99% by mass or more, or even 100% by mass. The graphite constituting the graphite particles may be either artificial graphite or natural graphite, but natural graphite is preferred. Natural graphite is a general term for graphite extracted from natural resources. Examples of natural graphite include flake graphite, lump graphite (flake graphite), and earthy graphite. The graphite particles may be graphite particles obtained by spheroidizing flake graphite and consolidating it. The graphite particles may be coated on the surface with a carbon material other than graphite (e.g., non-graphitic carbon). The carbon material coating can be achieved, for example, by coating the surface of the graphite particles with pitch and firing the resulting particles.

[0040] Natural graphite may exhibit four peaks at a diffraction angle 2θ ranging from 40° to 50° in X-ray diffraction measurement using CuKα radiation measured before charge / discharge or in a discharged state. These four peaks are believed to be two peaks attributable to a hexagonal crystal structure and two peaks attributable to a rhombohedral crystal structure. In the case of artificial graphite, it is generally believed that only two peaks attributable to a hexagonal crystal structure appear. In X-ray diffraction measurement, the ratio of the peak intensity I(012) attributable to the (012) plane of graphite to the peak intensity I(100) attributable to the (100) plane (I(012) / I(100)) is preferably 0.3 or more, more preferably 0.4 or more. The ratio (I(012) / I(100)) is preferably 0.6 or less. The ratio (I(012) / I(100)) may be equal to or greater than any of the lower limits and equal to or less than the upper limit. Here, the (100) plane originates from a hexagonal crystal structure, and the (012) plane originates from a rhombohedral crystal structure.

[0041] The upper limit of the internal porosity of the graphite particles is 2%, preferably 1%, and more preferably 0.6%. When the internal porosity of the graphite particles is equal to or less than the above upper limit, the output of the nonaqueous electrolyte storage element in a low-temperature environment can be increased. The lower limit of the internal porosity may be 0% or 0.1%. The internal porosity may be equal to or greater than any of the above lower limits and equal to or less than any of the above upper limits. The internal porosity of the graphite particles can be set to a low value, such as 2% or less, by, for example, subjecting spheroidized graphite particles to a consolidation treatment.

[0042] The average particle size of the graphite particles is, for example, preferably 1 μm to 30 μm, more preferably 2 μm to 20 μm, and even more preferably 4 μm to 12 μm (e.g., 6 μm to 10 μm, 6 μm to 9 μm). Generally, the larger the particle size of graphite particles, the larger the internal voids tend to be. Therefore, when the present invention is applied to a negative electrode using graphite particles with an average particle size equal to or greater than the above lower limit, the effect of improving output performance by reducing the internal porosity to 2% or less is significantly achieved. On the other hand, when the average particle size of the graphite particles is equal to or less than the above upper limit, the contact area between particles increases, reducing the resistance of the negative electrode active material layer, and so on, thereby increasing the output of the nonaqueous electrolyte storage element in a low-temperature environment. Graphite particles having such an average particle size are also suitable from the viewpoint of achieving a value in the preferred range of the ratio (I(012) / I(100)).

[0043] The "average particle size" of the graphite particles and the positive electrode active material described later refers to the value at which the volume-based cumulative distribution calculated in accordance with JIS-Z-8819-2 (2001) is 50%, based on the particle size distribution measured in accordance with JIS-Z-8825 (2013) by a laser diffraction / scattering method for a diluted solution obtained by diluting particles with a solvent.

[0044] In order to obtain particles (powders) such as graphite particles with a predetermined particle size, a pulverizer, a classifier, or the like is used. Examples of pulverization methods include methods using a mortar, a ball mill, a sand mill, a vibration ball mill, a planetary ball mill, a jet mill, a counter jet mill, a swirling airflow jet mill, or a sieve. Wet pulverization in the presence of water or an organic solvent such as hexane can also be used during pulverization. As a classification method, a sieve, an air classifier, or the like is used as needed for both dry and wet methods.

[0045] The content of graphite particles in the negative electrode active material layer is preferably 60% by mass or more and 99.5% by mass or less, and more preferably 90% by mass or more and 99% by mass or less. By setting the content of graphite particles within this range, it is possible to achieve both high energy density and manufacturability of the negative electrode active material layer, and to further increase the output of the nonaqueous electrolyte storage element in a low-temperature environment.

[0046] The negative electrode active material layer may contain other negative electrode active materials in addition to graphite particles. Examples of other negative electrode active materials include non-graphitic carbon (easily graphitizable carbon or non-graphitizable carbon), metallic lithium, metals or semimetals such as Si and Sn, metal oxides or semimetal oxides such as Si oxide, Ti oxide, and Sn oxide, and Li 4 Ti 5 O 12 , LiTiO 2、 TiNb 2 O 7 Examples of the graphite particles include titanium-containing oxides such as titanium dioxide, polyphosphate compounds, and silicon carbide. However, the content of the graphite particles relative to the total negative electrode active material is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 99% by mass or more, even more preferably 99.9% by mass or more, and particularly preferably 100% by mass. In this way, when the negative electrode active material is essentially composed of graphite particles, the effect of increasing the output of the nonaqueous electrolyte storage element in a low-temperature environment is particularly remarkable.

[0047] The conductive agent is not particularly limited as long as it is a material that is conductive. Examples of such conductive agents include carbonaceous materials, metals, and conductive ceramics. Examples of carbonaceous materials include non-graphite carbon and graphene-based carbon. Examples of non-graphite carbon in the conductive agent include carbon nanofiber, pitch-based carbon fiber, and carbon black. Examples of carbon black include furnace black, acetylene black, and ketjen black. Examples of graphene-based carbon include graphene, carbon nanotubes (CNT), and fullerene. However, the graphite particles contained in the negative electrode active material layer and the non-graphite carbon in other conventionally known negative electrode active materials are not included in the conductive agent in the negative electrode active material layer. The conductive agent may be in the form of powder or fiber. As the conductive agent, one of these materials may be used alone, or two or more may be mixed and used. Furthermore, these materials may be used in combination. For example, a composite of carbon black and CNT may be used. Of these, carbon black is preferred from the viewpoint of electron conductivity and coatability, and acetylene black is particularly preferred.

[0048] The content of the conductive agent in the negative electrode active material layer can be, for example, 0.1% by mass to 5% by mass, and may be 3% by mass or less or 1% by mass or less, or the negative electrode active material layer may not contain a conductive agent.

[0049] Examples of binders include thermoplastic resins such as fluororesins (polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), etc.), polyethylene, polypropylene, polyacrylic, and polyimide; elastomers such as ethylene-propylene-diene rubber (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), and fluororubber; and polysaccharide polymers.

[0050] The content of the binder in the negative electrode active material layer is preferably 0.5% by mass to 5% by mass, more preferably 0.8% by mass to 3% by mass, whereby the graphite particles and the like can be stably held.

[0051] Examples of thickeners include polysaccharide polymers such as carboxymethyl cellulose (CMC), methyl cellulose, etc. When the thickener has a functional group that reacts with lithium or the like, this functional group may be deactivated in advance by methylation or the like.

[0052] The content of the thickener in the negative electrode active material layer is, for example, preferably 0.1% by mass or more and 6% by mass or less, and more preferably 0.5% by mass or more and 3% by mass or less.

[0053] The filler is not particularly limited, and examples of the filler include polyolefins such as polypropylene and polyethylene, inorganic oxides such as silicon dioxide, alumina, titanium dioxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, and aluminosilicates, hydroxides such as magnesium hydroxide, calcium hydroxide, and aluminum hydroxide, carbonates such as calcium carbonate, sparingly soluble ionic crystals such as calcium fluoride, barium fluoride, and barium sulfate, nitrides such as aluminum nitride and silicon nitride, substances derived from mineral resources such as talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, and mica, and artificial products thereof.

[0054] The content of the filler in the negative electrode active material layer may be, for example, 0.1% by mass to 8% by mass, or 0.5% by mass to 5% by mass, 3% by mass or less, or 1% by mass or less, or the negative electrode active material layer may not contain a filler.

[0055] The negative electrode active material layer may contain typical non-metallic elements such as B, N, P, F, Cl, Br, and I; typical metallic elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, and Ba; and transition metal elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Ta, Hf, Nb, and W as components other than the negative electrode active material, conductive agent, binder, thickener, and filler.

[0056] In the negative electrode according to one embodiment of the present invention, the ratio of the peak intensity I(110) attributable to the (110) plane to the peak intensity I(004) attributable to the (004) plane of graphite in X-ray diffraction measurement of the negative electrode active material layer using CuKα radiation (I(110) / I(004)) has a lower limit of 0.055, preferably 0.060, more preferably 0.065, or may be 0.080, 0.090, 0.100, 0.150, or 0.200. By having the ratio (I(110) / I(004)) be equal to or greater than the lower limit, the output of the nonaqueous electrolyte storage element in a low-temperature environment can be increased. The upper limit of the ratio (I(110) / I(004)) may be, for example, 0.400, but is preferably 0.320, more preferably 0.270, even more preferably 0.240, or may be 0.200. When the ratio (I(110) / I(004)) is equal to or less than the upper limit, it is possible to improve the capacity retention rate after storage of the nonaqueous electrolyte storage element, provided that the negative electrode active material layer has a comparable BET specific surface area. In particular, when the ratio (I(110) / I(004)) is 0.270 or less, it is possible to further improve the input power retention rate and the capacity retention rate after storage of the nonaqueous electrolyte storage element in a low-temperature environment after storage. The ratio (I(110) / I(004)) may be equal to or greater than any of the lower limits and equal to or less than any of the upper limits (however, the lower limit is less than the upper limit). The ratio (I(110) / I(004)) in the negative electrode active material layer can be adjusted by the type of graphite particles (e.g., the shape of the graphite particles), whether or not pressing is used during the production of the negative electrode, the pressure of the pressing, etc. For example, when the negative electrode active material layer is pressed under high pressure during the production of the negative electrode, the orientation of the graphite particles increases, and the ratio (I(110) / I(004)) tends to become smaller. The porosity of the negative electrode active material layer is not particularly limited, but may be approximately 40% or more (for example, more than 50% and not more than 65%, typically 52% or more and not more than 60%). The porosity of the negative electrode active material layer is determined by the apparent volume (volume including voids) V of the negative electrode active material layer. 1 and the sum V of the actual volumes of the materials constituting the negative electrode active material layer. 2 Therefore, porosity = [(V 1 -V 2 ) / V 1] × 100. The apparent volume of the negative electrode active material layer is calculated from the length, average thickness, and width of the negative electrode active material layer. The average thickness is the average of the values ​​measured at any five points. The sum of the actual volumes of the materials constituting the negative electrode active material layer, V 2 is calculated from the content of each material constituting the negative electrode active material layer and the true density of each material.

[0057] The BET specific surface area of ​​the negative electrode active material layer is not particularly limited, and its upper limit is, for example, 5.0 m 2 / g, but 3.8m 2 / g is preferred, and 3.0m 2 When the BET specific surface area of ​​the negative electrode active material layer is equal to or less than the upper limit, it is possible to improve the input power retention rate and capacity retention rate after storage in a low-temperature environment of the nonaqueous electrolyte storage element after storage. The lower limit of the BET specific surface area of ​​the negative electrode active material layer is 1.0 m 2 / g, and 1.5m 2 / g or 2.0m 2 / g. The BET specific surface area of ​​the negative electrode active material layer may be equal to or greater than any of the above-mentioned lower limits and equal to or less than any of the above-mentioned upper limits. The BET specific surface area of ​​the negative electrode active material layer can be adjusted by the particle size of the negative electrode active material particles, whether or not pressing is performed during production, the pressure of the pressing, etc.

[0058] <Method for manufacturing a negative electrode> A negative electrode according to one embodiment of the present invention can be produced by, for example, applying a negative electrode mixture paste to a negative electrode substrate directly or via an intermediate layer, and then drying. After drying, pressing or the like may be performed as necessary. The negative electrode mixture paste contains each component constituting the negative electrode active material layer, such as graphite particles and an optional binder. The negative electrode mixture paste usually further contains a dispersion medium. Water is preferred as the dispersion medium used in the negative electrode mixture paste.

[0059] <Non-aqueous electrolyte storage element> A non-aqueous electrolyte storage element (hereinafter also simply referred to as "storage element") according to one embodiment of the present invention comprises an electrode assembly having a positive electrode, a negative electrode, and a separator, a non-aqueous electrolyte, and a container that accommodates the electrode assembly and the non-aqueous electrolyte. The electrode assembly is typically a stacked type in which a plurality of positive electrodes and a plurality of negative electrodes are stacked with separators interposed therebetween, or a wound type in which a positive electrode and a negative electrode are stacked with a separator interposed therebetween and wound. At least a portion of the non-aqueous electrolyte exists in a state in which it is impregnated into the positive electrode, the negative electrode, and the separator. As an example of a non-aqueous electrolyte storage element, a non-aqueous electrolyte secondary battery (hereinafter also simply referred to as "secondary battery") will be described.

[0060] The positive electrode has a positive electrode substrate and a positive electrode active material layer disposed on the positive electrode substrate directly or via an intermediate layer. The configuration of the intermediate layer is not particularly limited and can be selected from the configurations exemplified for the negative electrode above, for example.

[0061] The positive electrode substrate is conductive. Examples of the material for the positive electrode substrate include metals such as aluminum, titanium, tantalum, and stainless steel, as well as alloys thereof. Among these, aluminum or aluminum alloys are preferred from the viewpoints of potential resistance, high conductivity, and cost. Examples of the positive electrode substrate include foil, vapor-deposited film, mesh, and porous material, with foil being preferred from the viewpoint of cost. Therefore, aluminum foil or aluminum alloy foil is preferred as the positive electrode substrate. Examples of aluminum or aluminum alloys include A1085, A3003, and A1N30, as specified in JIS-H-4000 (2014) or JIS-H-4160 (2006).

[0062] The average thickness of the positive electrode substrate is preferably 3 μm to 50 μm, more preferably 5 μm to 40 μm, even more preferably 8 μm to 30 μm, and particularly preferably 10 μm to 25 μm. By setting the average thickness of the positive electrode substrate within the above range, the strength of the positive electrode substrate can be increased while increasing the energy density per volume of the nonaqueous electrolyte storage element.

[0063] The positive electrode active material layer contains a positive electrode active material. The positive electrode active material layer contains optional components such as a conductive agent, a binder, a thickener, and a filler, as needed. The optional components such as the conductive agent, the binder, the thickener, and the filler can be selected from the materials exemplified for the negative electrode above.

[0064] The positive electrode active material can be appropriately selected from known positive electrode active materials. As the positive electrode active material for a lithium ion secondary battery, a material capable of absorbing and releasing lithium ions is usually used. Examples of the positive electrode active material include α-NaFeO 2 Examples of suitable lithium transition metal composite oxides include those having a α-type crystal structure, those having a spinel type crystal structure, polyanion compounds, chalcogen compounds, and sulfur. 2 As the lithium transition metal composite oxide having a crystalline structure, for example, Li[Li x Ni (1-x) ]O 2 (0≦x<0.5), Li[Li x Ni γ Co (1-x-γ) ]O 2 (0≦x<0.5, 0<γ<1, 0<1-x-γ), Li[Li x Co (1-x) ]O 2 (0≦x<0.5), Li[Li x Ni γ Mn (1-x-γ) ]O 2 (0≦x<0.5, 0<γ<1, 0<1-x-γ), Li[Li x Ni γ Mn β Co (1-x-γ-β) ]O 2 (0≦x<0.5, 0<γ, 0<β, 0.5<γ+β<1, 0<1−x−γ−β), Li[Li x Ni γ Co β Al (1-x-γ-β) ]O 2 (0≦x<0.5, 0<γ, 0<β, 0.5<γ+β<1, 0<1−x−γ−β), etc. Examples of lithium transition metal composite oxides having a spinel crystal structure include Li x Mn 2 O 4 , Li xNi γ Mn (2-γ) O 4 Examples of polyanion compounds include LiFePO 4 , LiMnPO 4 , LiNiPO 4 , LiCoPO 4 , Li 3 V 2 (P.O. 4 ) 3 , Li 2 MnSiO 4 , Li 2 CoPO 4 Examples of the chalcogen compound include titanium disulfide, molybdenum disulfide, and molybdenum dioxide. Atoms or polyanions in these materials may be partially substituted with atoms or anion species of other elements. The surfaces of these materials may be coated with other materials. In the positive electrode active material layer, one of these materials may be used alone, or two or more of them may be used in combination.

[0065] The positive electrode active material is usually in the form of particles (powder). The average particle size of the positive electrode active material is preferably, for example, 0.1 μm or more and 20 μm or less. By setting the average particle size of the positive electrode active material to the above lower limit or more, the positive electrode active material is easily manufactured or handled. By setting the average particle size of the positive electrode active material to the above upper limit or less, the electronic conductivity of the positive electrode active material layer is improved. When a composite of the positive electrode active material and another material is used, the average particle size of the composite is taken as the average particle size of the positive electrode active material. A pulverizer, a classifier, or the like is used to obtain powder with a predetermined particle size. The pulverization method and classification method can be selected, for example, from the methods exemplified for the negative electrode above.

[0066] The content of the positive electrode active material in the positive electrode active material layer is preferably 50% by mass to 99% by mass, more preferably 70% by mass to 98% by mass, and even more preferably 80% by mass to 95% by mass. By setting the content of the positive electrode active material within the above range, both high energy density and manufacturability of the positive electrode active material layer can be achieved.

[0067] The content of the conductive agent in the positive electrode active material layer is preferably 1% by mass or more and 10% by mass or less, and more preferably 3% by mass or more and 9% by mass or less. By setting the content of the conductive agent in this range, the energy density of the nonaqueous electrolyte storage element can be increased.

[0068] The content of the binder in the positive electrode active material layer is preferably 0.5% by mass to 10% by mass, more preferably 1% by mass to 9% by mass, inclusive. By setting the binder content within this range, the positive electrode active material can be stably maintained.

[0069] The content of the thickener in the positive electrode active material layer may be, for example, 0.1% by mass to 6% by mass, or 0.5% by mass to 3% by mass, or 1% by mass or less, or the positive electrode active material layer may not contain a thickener.

[0070] The content of the filler in the positive electrode active material layer may be, for example, 0.1% by mass to 8% by mass, or 0.5% by mass to 5% by mass, 3% by mass or less, or 1% by mass or less, or the positive electrode active material layer may not contain a filler.

[0071] The positive electrode active material layer may contain typical non-metallic elements such as B, N, P, F, Cl, Br, and I; typical metallic elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, and Ba; and transition metal elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, and Nb as components other than the positive electrode active material, conductive agent, binder, thickener, and filler.

[0072] (Negative Electrode) The negative electrode provided in the nonaqueous electrolyte electricity storage element according to one embodiment of the present invention is the negative electrode for the nonaqueous electrolyte electricity storage element according to one embodiment of the present invention described above.

[0073] (Separator) The separator can be appropriately selected from known separators. Examples of separators that can be used include separators consisting of only a substrate layer and separators in which a heat-resistant layer containing heat-resistant particles and a binder is formed on one or both surfaces of the substrate layer. Examples of the shape of the substrate layer of the separator include woven fabric, nonwoven fabric, and porous resin film. Among these shapes, porous resin films are preferred from the viewpoint of strength, and nonwoven fabrics are preferred from the viewpoint of non-aqueous electrolyte retention. Materials for the substrate layer of the separator are preferably polyolefins such as polyethylene and polypropylene from the viewpoint of shutdown function, and polyimide and aramid from the viewpoint of oxidative decomposition resistance. A composite material of these resins may also be used for the substrate layer of the separator.

[0074] The heat-resistant particles contained in the heat-resistant layer preferably exhibit a mass loss of 5% or less when heated from room temperature to 500°C under an air atmosphere at 1 atmosphere, and more preferably exhibit a mass loss of 5% or less when heated from room temperature to 800°C. Examples of materials exhibiting a mass loss of a predetermined value or less include inorganic compounds. Examples of inorganic compounds include oxides such as iron oxide, silicon oxide, aluminum oxide, titanium oxide, zirconium oxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, and aluminosilicate; nitrides such as aluminum nitride and silicon nitride; carbonates such as calcium carbonate; sulfates such as barium sulfate; sparingly soluble ionic crystals such as calcium fluoride, barium fluoride, and barium titanate; covalently bonded crystals such as silicon and diamond; mineral-derived substances such as talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, and mica, as well as artificial products thereof. As the inorganic compound, these substances may be used alone or in the form of a complex, or two or more of them may be used in combination. Among these inorganic compounds, silicon oxide, aluminum oxide, or aluminosilicate is preferred from the viewpoint of safety of the nonaqueous electrolyte storage element.

[0075] The porosity of the separator is preferably 80% by volume or less from the viewpoint of strength, and is preferably 20% by volume or more from the viewpoint of discharge performance. Here, "porosity" refers to a volume-based value measured with a mercury porosimeter.

[0076] The separator may be a polymer gel composed of a polymer and a non-aqueous electrolyte. Examples of polymers include polyacrylonitrile, polyethylene oxide, polypropylene oxide, polymethyl methacrylate, polyvinyl acetate, polyvinylpyrrolidone, and polyvinylidene fluoride. The use of a polymer gel has the effect of suppressing leakage. The separator may be a combination of the porous resin film or nonwoven fabric described above and a polymer gel.

[0077] (Non-aqueous electrolyte) The non-aqueous electrolyte can be appropriately selected from known non-aqueous electrolytes. The non-aqueous electrolyte may be a non-aqueous electrolyte solution. The non-aqueous electrolyte solution contains a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent.

[0078] The non-aqueous solvent can be appropriately selected from known non-aqueous solvents. Examples of non-aqueous solvents include cyclic carbonates, chain carbonates, carboxylic acid esters, phosphate esters, sulfonic acid esters, ethers, amides, and nitriles. Non-aqueous solvents in which some of the hydrogen atoms contained in these compounds have been substituted with halogens may also be used.

[0079] Examples of cyclic carbonates include ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinylene carbonate (VC), vinylethylene carbonate (VEC), chloroethylene carbonate, fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), styrene carbonate, 1-phenylvinylene carbonate, 1,2-diphenylvinylene carbonate, etc. Of these, EC is preferred.

[0080] Examples of the chain carbonate include diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diphenyl carbonate, trifluoroethyl methyl carbonate, bis(trifluoroethyl) carbonate, etc. Among these, EMC is preferred.

[0081] It is preferable to use a cyclic carbonate or a chain carbonate as the non-aqueous solvent, and it is more preferable to use a cyclic carbonate and a chain carbonate in combination. The use of a cyclic carbonate can promote dissociation of the electrolyte salt and improve the ionic conductivity of the non-aqueous electrolyte. The use of a chain carbonate can reduce the viscosity of the non-aqueous electrolyte. When a cyclic carbonate and a chain carbonate are used in combination, the volume ratio of the cyclic carbonate to the chain carbonate (cyclic carbonate:chain carbonate) is preferably in the range of, for example, 5:95 to 50:50.

[0082] The electrolyte salt can be appropriately selected from known electrolyte salts, such as lithium salts, sodium salts, potassium salts, magnesium salts, and onium salts. Of these, lithium salts are preferred.

[0083] The lithium salt is LiPF 6 , LiPO 2 F 2 , LiBF 4 , LiClO 4 , LiN(SO 2 F) 2 inorganic lithium salts such as lithium oxalate salts, lithium bis(oxalate)borate (LiBOB), lithium difluorooxalateborate (LiFOB), and lithium bis(oxalate)difluorophosphate (LiFOP); 3 CF 3 , LiN(SO 2 CF 3 ) 2 , LiN(SO 2 C 2 F 5 ) 2 , LiN(SO 2 CF 3 ) (SO2 C 4 F 9 ), LiC(SO 2 CF 3 ) 3 , LiC(SO 2 C 2 F 5 ) 3 Among these, inorganic lithium salts are preferred, and LiPF 6 is more preferred.

[0084] The content of the electrolyte salt in the non-aqueous electrolyte solution is 0.1 mol / dm at 20°C and 1 atmosphere. 3 2.5mol / dm or more 3 It is preferably 0.3 mol / dm or less. 3 2.0mol / dm or more 3 It is more preferable that it is 0.5 mol / dm or less. 3 More than 1.7mol / dm 3 It is more preferable that it is 0.7 mol / dm or less. 3 1.5mol / dm or more 3 By setting the content of the electrolyte salt within the above range, the ionic conductivity of the non-aqueous electrolyte can be increased.

[0085] The non-aqueous electrolyte may contain additives in addition to the non-aqueous solvent and the electrolyte salt. Examples of the additives include aromatic compounds such as biphenyl, alkylbiphenyl, terphenyl, partially hydrogenated terphenyl, cyclohexylbenzene, t-butylbenzene, t-amylbenzene, diphenyl ether, and dibenzofuran; partial halides of the aromatic compounds such as 2-fluorobiphenyl, o-cyclohexylfluorobenzene, and p-cyclohexylfluorobenzene; halogenated anisole compounds such as 2,4-difluoroanisole, 2,5-difluoroanisole, 2,6-difluoroanisole, and 3,5-difluoroanisole; vinylene carbonate, methylvinylene carbonate, ethylvinylene carbonate, succinic anhydride, glutaric anhydride, maleic anhydride, citraconic anhydride, glutaconic anhydride, itaconic anhydride, and cyclohexanedicarboxylic anhydride; and ethylene sulfite. Examples of the additives include propylene sulfite, dimethyl sulfite, methyl methanesulfonate, busulfan, methyl toluenesulfonate, dimethyl sulfate, ethylene sulfate, sulfolane, dimethyl sulfone, diethyl sulfone, dimethyl sulfoxide, diethyl sulfoxide, tetramethylene sulfoxide, diphenyl sulfide, 4,4'-bis(2,2-dioxo-1,3,2-dioxathiolane), 4-methylsulfonyloxymethyl-2,2-dioxo-1,3,2-dioxathiolane, thioanisole, diphenyl disulfide, dipyridinium disulfide, 1,3-propene sultone, 1,3-propane sultone, 1,4-butane sultone, 1,4-butene sultone, perfluorooctane, tristrimethylsilyl borate, tristrimethylsilyl phosphate, and tetrakistrimethylsilyl titanate. These additives may be used alone or in combination of two or more.

[0086] The content of the additive contained in the non-aqueous electrolyte is preferably 0.01% by mass to 10% by mass, more preferably 0.1% by mass to 7% by mass, even more preferably 0.2% by mass to 5% by mass, and particularly preferably 0.3% by mass to 3% by mass, based on the total mass of the non-aqueous electrolyte. By setting the content of the additive within the above range, it is possible to improve the capacity retention performance or cycle performance after high-temperature storage, and further improve safety.

[0087] The non-aqueous electrolyte may be a solid electrolyte, or a non-aqueous electrolytic solution and a solid electrolyte may be used in combination.

[0088] The solid electrolyte can be selected from any material that has ionic conductivity of lithium, sodium, calcium, etc. and is solid at room temperature (e.g., 15° C. to 25° C.) Examples of the solid electrolyte include sulfide solid electrolytes, oxide solid electrolytes, nitride solid electrolytes, and polymer solid electrolytes.

[0089] As the sulfide solid electrolyte, in the case of a lithium ion secondary battery, for example, Li 2 S-P 2 S 5 , LiI-Li 2 S-P 2 S 5 , Li 10 Ge-P 2 S 12 etc.

[0090] The shape of the nonaqueous electrolyte storage element of this embodiment is not particularly limited, and examples thereof include cylindrical batteries, prismatic batteries, flat batteries, coin batteries, and button batteries.

[0091] Figure 1 shows a nonaqueous electrolyte storage element 1 as an example of a prismatic battery. The figure is a see-through view of the inside of the container. An electrode assembly 2 having a positive electrode and a negative electrode wound with a separator sandwiched between them is housed in a prismatic container 3. The positive electrode is electrically connected to a positive electrode terminal 4 via a positive electrode lead 41. The negative electrode is electrically connected to a negative electrode terminal 5 via a negative electrode lead 51.

[0092] <Electricity Storage Device> The nonaqueous electrolyte energy storage element of the present embodiment can be mounted as an energy storage unit (battery module) comprising a plurality of nonaqueous electrolyte energy storage elements in an automobile power source such as an electric vehicle (EV), a hybrid electric vehicle (HEV), a plug-in hybrid electric vehicle (PHEV), etc., a power source for electronic devices such as a personal computer or a communication terminal, or a power source for power storage, etc. In this case, the technology of the present invention may be applied to at least one nonaqueous electrolyte energy storage element included in the energy storage unit.

[0093] 2 shows an example of an energy storage device 30 in which energy storage units 20, each of which is an assembly of two or more electrically connected nonaqueous electrolyte energy storage elements 1, are further assembled. The energy storage device 30 may include a bus bar (not shown) that electrically connects two or more nonaqueous electrolyte energy storage elements 1, a bus bar (not shown) that electrically connects two or more energy storage units 20, etc. The energy storage unit 20 or the energy storage device 30 may include a status monitoring device (not shown) that monitors the status of one or more nonaqueous electrolyte energy storage elements.

[0094] <Method for manufacturing nonaqueous electrolyte storage element> The method for manufacturing the nonaqueous electrolyte storage element of this embodiment can be appropriately selected from known methods. The manufacturing method includes, for example, preparing an electrode assembly, preparing a nonaqueous electrolyte, and housing the electrode assembly and the nonaqueous electrolyte in a container. Preparing the electrode assembly includes preparing a positive electrode and a negative electrode, and forming the electrode assembly by stacking or winding the positive electrode and the negative electrode with a separator interposed therebetween.

[0095] The positive electrode can be prepared, for example, by applying a positive electrode mixture paste to a positive electrode substrate directly or via an intermediate layer, and then drying. The positive electrode mixture paste contains components constituting the positive electrode active material layer, such as a positive electrode active material. The positive electrode mixture paste usually further contains a dispersion medium. After drying the applied positive electrode mixture paste, pressing or the like may be performed.

[0096] Preparing the negative electrode may be, for example, manufacturing the negative electrode by the method described above.

[0097] The method for placing the non-aqueous electrolyte in the container can be appropriately selected from known methods. For example, when a non-aqueous electrolyte solution is used as the non-aqueous electrolyte, the non-aqueous electrolyte solution may be poured into the container through an inlet formed in the container, and then the inlet may be sealed.

[0098] <Other Embodiments> The negative electrode for a nonaqueous electrolyte storage element and the nonaqueous electrolyte storage element of the present invention are not limited to the above-described embodiments, and various modifications may be made without departing from the spirit of the present invention. For example, the configuration of one embodiment can be added to the configuration of another embodiment, and part of the configuration of one embodiment can be replaced with the configuration of another embodiment or well-known technology. Furthermore, part of the configuration of one embodiment can be deleted. Also, well-known technology can be added to the configuration of one embodiment.

[0099] In the above embodiment, the nonaqueous electrolyte storage element is used as a chargeable and dischargeable nonaqueous electrolyte secondary battery (lithium ion secondary battery, etc.), but the nonaqueous electrolyte storage element may be of any type, shape, size, capacity, etc. The present invention can also be applied to various secondary batteries, electric double layer capacitors, lithium ion capacitors, and other capacitors.

[0100] In the above embodiment, the electrode assembly in which the positive electrode and the negative electrode are stacked with a separator interposed therebetween has been described, but the electrode assembly may not include a separator. For example, the positive electrode and the negative electrode may be in direct contact with each other in a state in which a non-conductive layer is formed on the active material layer of the positive electrode or the negative electrode.

[0101] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0102] [Example 1] (Preparation of Negative Electrode) Consolidated natural graphite particles (internal porosity 0.45%, average particle size 8 μm) were prepared as graphite particles. A negative electrode mixture paste was prepared using the graphite particles, styrene-butadiene rubber (SBR) as a binder, carboxymethyl cellulose (CMC) as a thickener, and water as a dispersion medium. The mass ratio of the graphite particles, SBR, and CMC was 98.5:1.0:0.5 (solid content equivalent). The negative electrode mixture paste was applied to both sides of copper foil as a negative electrode substrate and dried. Thereafter, roll pressing was performed to obtain a negative electrode in which negative electrode active material layers were laminated on both sides of the negative electrode substrate. The negative electrode active material layer of the obtained negative electrode was subjected to X-ray diffraction measurement using CuKα radiation by the above-mentioned method. As a result, the ratio of the peak intensity I(110) attributed to the (110) plane of graphite to the peak intensity I(004) attributed to the (004) plane (I(110) / I(004)) was 0.055.

[0103] (Preparation of Positive Electrode) LiNi as a positive electrode active material 1/3 Mn 1/3 Co 1/3 O 2 A positive electrode mixture paste was prepared using acetylene black (AB) as a conductive agent, polyvinylidene fluoride (PVDF) as a binder, and N-methylpyrrolidone (NMP) as a dispersion medium. The mass ratio of the positive electrode active material, AB, and PVDF was 93:5:2 (solid content equivalent). The positive electrode mixture paste was applied to both sides of aluminum foil as a positive electrode substrate and dried. Then, roll pressing was performed to obtain a positive electrode in which positive electrode active material layers were laminated on both sides of the positive electrode substrate.

[0104] (Preparation of non-aqueous electrolyte) LiPF 6 was added to a mixed solvent of ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) in a volume ratio of 30:35:35. 6 to 1.0 mol / dm 3 The non-aqueous electrolyte was obtained by dissolving the non-aqueous electrolyte at a concentration of 100 ppm.

[0105] (Preparation of Separator) A microporous polyolefin film was used as the separator.

[0106] (Assembly of non-aqueous electrolyte storage element) The negative electrode, positive electrode, and separator were used to obtain a wound electrode body. The electrode body was placed in a container, and a non-aqueous electrolyte was poured into the container and sealed to obtain the non-aqueous electrolyte storage element of Example 1.

[0107] [Examples 2 to 7, Comparative Examples 1 to 4] Non-aqueous electrolyte storage elements of Examples 2 to 7 and Comparative Examples 1 to 4 were obtained in the same manner as in Example 1, except that graphite particles having the internal porosity and average particle size shown in Table 1 were used as the graphite particles, and the ratio (I(110) / I(004)) of the negative electrode active material layer was set to the value shown in Table 1. Natural graphite particles were used as the graphite particles. Furthermore, natural graphite particles that had not been compacted were used in the non-aqueous electrolyte storage elements of Comparative Examples 2 to 4. The ratio (I(110) / I(004)) of the negative electrode active material layer using the same graphite particles was adjusted by changing the pressure during roll pressing.

[0108] (Initial Charge / Discharge) The obtained nonaqueous electrolyte storage elements of Examples 1 to 7 and Comparative Examples 1 to 4 were initially charged and discharged under the following conditions. In a thermostatic chamber at 25°C, constant current charging was performed with a charging current of 1.0 C and a charge cut-off voltage of 4.10 V, followed by constant voltage charging at 4.10 V. The charge was terminated until the total charge time reached 3 hours. A 10-minute rest period was then provided. Constant current discharge was then performed with a discharge current of 1.0 C and a discharge cut-off voltage of 3.0 V. These charge and discharge processes constitute one cycle, and two cycles were performed. The discharged electrical quantity in the second cycle was taken as the initial discharge capacity.

[0109] (Output in a Low-Temperature Environment) Next, for each of the nonaqueous electrolyte storage elements of Examples 1 to 7 and Comparative Examples 1 to 4, constant-current charging was performed at a charging current of 1.0 C in a temperature environment of 25°C, and the state of charge (SOC) was adjusted to 50%. Each nonaqueous electrolyte storage element was stored in a thermostatic chamber at -10°C for 4 hours and then discharged for 10 seconds at a constant current of 0.2 C, 0.5 C, or 1.0 C. After each discharge, constant-current charging was performed at a current of 0.05 C to adjust the SOC to 50%. The relationship between the current and the voltage 1 second after the start of discharge was plotted, and the DC resistance was calculated from the slope of the straight line obtained from the three plots. The output in a low-temperature environment was calculated based on the calculated DC resistance. Table 1 and FIG. 3 show the output (relative value) of each nonaqueous electrolyte storage element in a low-temperature environment, with the output of the nonaqueous electrolyte storage element of Comparative Example 1 in a low-temperature environment as the reference (100%).

[0110]

[0111] 3 , the nonaqueous electrolyte storage elements of Examples 1 to 7, which used graphite particles with an internal porosity of 2% or less and in which the ratio (I(110) / I(004)) in the negative electrode active material layer was 0.055 or more, had an output (relative value) of 109% or more in a low-temperature environment, indicating high output in a low-temperature environment. On the other hand, the nonaqueous electrolyte storage elements of Comparative Examples 2 to 4, which used graphite particles with an internal porosity of more than 2%, did not provide a sufficiently high output in a low-temperature environment, even when the ratio (I(110) / I(004)) in the negative electrode active material layer was 0.055 or more.

[0112] [Examples 8 to 15] Nonaqueous electrolyte storage elements of Examples 8 to 15 were obtained in the same manner as in Example 1, except that graphite particles having an internal porosity of 2% or less and an average particle size of 8 μm were used, and the ratio (I(110) / I(004)) and BET specific surface area of ​​the negative electrode active material layer were set to the values ​​shown in Table 2. Natural graphite particles that had been subjected to a compaction treatment were used as the graphite particles. The ratio (I(110) / I(004)) and BET specific surface area of ​​the negative electrode active material layer were adjusted by changing the pressure during roll pressing, for example.

[0113] (Initial Charge / Discharge) The obtained nonaqueous electrolyte storage elements of Examples 8 to 15 were initially charged and discharged in the same manner as the nonaqueous electrolyte storage element of Example 1, and the initial discharge capacity was determined.

[0114] (Storage Test) Next, each of the nonaqueous electrolyte storage elements of Examples 8 to 15 was subjected to constant current charging at a charging current of 1.0 C in a thermostatic bath at 25° C. to bring the SOC to 50%. Each of the nonaqueous electrolyte storage elements in this 50% SOC state was stored in a thermostatic bath at 65° C. for 90 days.

[0115] (Capacity Retention Rate After Storage) After the storage test, each nonaqueous electrolyte storage element was charged and discharged in the same manner as the initial charge and discharge, and the discharge capacity after the storage test was determined. The percentage of the discharge capacity after the storage test relative to the initial discharge capacity was determined as the capacity retention rate after storage. The determined capacity retention rates after storage are shown in Table 2 and FIG. 4.

[0116] (Power Input Retention Rate in a Low-Temperature Environment After Storage) Before and after the storage test, the power input of each nonaqueous electrolyte storage element in a low-temperature environment was measured using the following procedure. A constant-current charge was performed at a charging current of 1.0 C in a temperature environment of 25°C, and the SOC was adjusted to 50%. Each nonaqueous electrolyte storage element was stored in a thermostatic chamber at −30°C for 4 hours, and then charged for 10 seconds at a constant current of 5 C, 10 C, 15 C, 20 C, or 25 C. After each charge, a constant-current discharge was performed at a current of 1.0 C to adjust the SOC to 50%. The DC resistance was calculated from the slope of the current during each charge and the voltage 1 second after the start of charge. The power input in a low-temperature environment was calculated based on the calculated DC resistance. The percentage of the power input in a low-temperature environment after the storage test relative to the power input in a low-temperature environment before the storage test was calculated as the power input retention rate in a low-temperature environment after storage. The calculated power input retention rates in a low-temperature environment after storage are shown in Table 2 and FIG. 5.

[0117]

[0118] As shown in Table 2 and Figure 4, as the ratio (I(110) / I(004)) in the negative electrode active material layer decreased, the capacity retention rate after storage tended to increase. Furthermore, as shown in Table 2 and Figures 4 and 5, as the BET specific surface area of ​​the negative electrode active material layer decreased, the capacity retention rate after storage and the input power retention rate in a low-temperature environment after storage tended to increase. In particular, when the ratio (I(110) / I(004)) in the negative electrode active material layer was 0.27 or less and the BET specific surface area of ​​the negative electrode active material layer was 3.8 m 2 The nonaqueous electrolyte storage elements of Examples 14 and 15, in which the capacitance was 0.1 / g or less, had significantly higher capacity retention rates after storage and input power retention rates in a low-temperature environment after storage.

[0119] The present invention can be applied to electric storage elements used as power sources for electronic devices such as personal computers and communication terminals, and automobiles.

[0120] REFERENCE SIGNS LIST 1 nonaqueous electrolyte energy storage element 2 electrode body 3 container 4 positive electrode terminal 41 positive electrode lead 5 negative electrode terminal 51 negative electrode lead 20 energy storage unit 30 energy storage device

Claims

1. A negative electrode for a non-aqueous electrolyte storage element, comprising a negative electrode active material layer containing graphite particles, wherein the graphite particles have an internal porosity of 2% or less, and in an X-ray diffraction measurement of the negative electrode active material layer using CuKα radiation, the ratio of a peak intensity I(110) assigned to a (110) plane of graphite to a peak intensity I(004) assigned to a (004) plane of graphite (I(110) / I(004)) is 0.055 or more.

2. The negative electrode for a nonaqueous electrolyte storage element according to claim 1, wherein the ratio (I(110) / I(004)) is 0.32 or less.

3. The BET specific surface area of ​​the negative electrode active material layer is 3.8 m 2 The negative electrode for a nonaqueous electrolyte storage element according to claim 1 or 2, wherein the molecular weight of the negative electrode is 1 / g or less.

4. The negative electrode for a nonaqueous electrolyte storage element according to claim 1 or 2, wherein the ratio (I(110) / I(004)) is 0.27 or less.

5. The negative electrode for a nonaqueous electrolyte storage element according to claim 3, wherein the ratio (I(110) / I(004)) is 0.27 or less.

6. A non-aqueous electrolyte storage element comprising the negative electrode for a non-aqueous electrolyte storage element according to claim 1 or 2.

Citation Information

Patent Citations

  • Negative pole material for lithium battery, and lithium battery

    JP2005222933A

  • Negative electrode for power storage device, and power storage device

    JP2017069039A

  • Nonaqueous electrolyte secondary battery and negative electrode thereof

    JP1999154513A

  • Negative electrode material for lithium ion secondary battery and its manufacturing method, as well as negative electrode for lithium ion secondary battery and lithium ion secondary battery using negative electrode material

    JP2005050807A

  • Carbon material and negative electrode for nonaqueous secondary battery, and nonaqueous secondary battery

    JP2012216537A