Thermosetting composition, prepreg including same, and high-frequency circuit board

The thermosetting composition of siloxane and aromatic polymers addresses the brittleness and production complexity issues of existing PPE resins by producing a material with superior dielectric and mechanical properties, suitable for high-frequency circuit boards and electronic devices.

WO2024241960A1PCT designated stage expired Publication Date: 2024-11-28DOW TORAY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/017762
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-19
Filing Date
2024-05-14
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Current thermosetting compositions for high-frequency circuit boards exhibit high brittleness, low hardness, and difficulty in adjusting mechanical properties, while also being costly to produce due to complex production processes of terminally modified polyphenylene ether (PPE) resins, which limits their suitability for next-generation electronic devices requiring high insulation and heat resistance.

Method used

A thermosetting composition comprising a siloxane compound with multiple alkenyl groups, an aromatic polymer with reactive functional groups, and a cycloolefin polymer, which can be cured to produce a material with low dielectric constant and loss tangent, excellent heat resistance, and adjustable physical properties, including toughness and transparency, by optimizing the mixing ratio and chemical structure of these components.

Benefits of technology

The resulting cured product demonstrates improved toughness, high elastic modulus at elevated temperatures, and excellent dielectric properties, making it suitable for high-frequency circuit boards and electronic devices with enhanced insulation and mechanical strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
Patent Text Reader

Abstract

[Problem] To provide: a thermosetting composition that is cured by heating, largely adjustable in terms of physical properties, and gives a cured product having excellent dielectric characteristics, transparency, molding processability, heat resistance, and toughness; and a use thereof. [Solution] A thermosetting composition and a use thereof, the thermosetting composition comprising: (A) a siloxane compound selected from (a1) a linear siloxane having two alkenyl groups and an aryl group, and (a2) a siloxane having two alkenyl groups and 8 or fewer silicon atoms; (B) an aromatic macromolecule / cycloolefin polymer having a reactive functional group; and (C) a thermal radical initiator.
Need to check novelty before this filing date? Find Prior Art

Description

Thermosetting composition, prepreg containing same, and high-frequency circuit board

[0001] The present invention relates to a heat-curable thermosetting composition comprising a specific siloxane compound having a reactive functional group and an aromatic polymer. The cured product obtained from the thermosetting composition of the present invention has excellent dielectric properties, particularly low relative permittivity and dielectric loss tangent, a high modulus of elasticity at high temperatures, and excellent heat resistance. These excellent properties make the composition suitable for use as a material for next-generation high-frequency circuit boards and as a coating material for electrical and electronic devices that require high insulation and heat resistance.

[0002] Due to their high heat resistance and excellent chemical stability, silicone resins have been used as coating agents, potting agents, insulating materials, etc. for electronic and electrical devices. Among silicone resins, many thermosetting silicone compositions containing reactive organopolysiloxanes have been reported.

[0003] In recent years, remarkable advances in information network technology have made it necessary to transmit large volumes of information at high speed while maintaining high quality, necessitating faster processing speeds for electronic devices. In addition to the already introduced 5G (fifth-generation mobile communication system) technology, in anticipation of future 6G technology, digital signals are becoming shorter in wavelength and higher in frequency to transmit large volumes of signals at high speed. Because signal degradation due to dielectric loss is significant in these high-frequency ranges, it is necessary to reduce the dielectric loss of insulating materials. Numerous resin materials with lower dielectric loss have been proposed as alternatives to epoxy resins, which are currently the primary choice. Among these, polyphenylene ether (hereinafter abbreviated as "PPE") resins have excellent dielectric properties, such as relative permittivity and dielectric loss tangent, and high heat resistance, making them widely considered as insulating materials for circuit boards of electrical and electronic devices that operate in high-frequency ranges (e.g., Patent Documents 1 to 3).

[0004] PPE resin compositions that utilize the reactivity of silicon-bonded alkenyl groups have also been studied. Patent Document 4 discloses a curable resin composition containing a terminal-modified PPE having a vinylsilyl group at the terminal and a silicon-free crosslinking aid. Patent Documents 5 and 6 disclose a polyphenylene ether resin composition containing a vinyl-modified polyphenylene ether resin and an organosilicone resin having an unsaturated double bond and a three-dimensional network structure, and a high-frequency circuit board using the same.

[0005] The cured products obtained from either composition have excellent dielectric properties such as dielectric loss tangent and heat resistance. However, these cured products are characterized by high brittleness or low hardness, making it difficult to adjust their mechanical properties. Furthermore, with regard to compositions containing terminally modified PPE, the production of the modified polymer is complicated, posing a cost issue.

[0006] That is, although a cured product made of a reactive PPE and an organic crosslinking agent and having excellent dielectric properties and heat resistance has been disclosed, it is difficult to say that a thermosetting composition and a cured product thereof that satisfy both the dielectric properties and moldability and that can adjust the physical properties over a wide range have been sufficiently disclosed.

[0007] Japanese Patent Application Laid-Open No. 2015-44934 WO2019-130735 Japanese Patent Application Laid-Open No. 2021-31612 Japanese Patent Application Laid-Open No. 2023-12895 Special Publication No. 2018-521210 Japanese Patent Application Laid-Open No. 2018-521211

[0008] The present invention has been made to solve the above-mentioned problems, and provides a thermosetting composition which, upon heating, gives a cured product having excellent dielectric properties, particularly low relative dielectric constant and dielectric loss tangent, and excellent transparency, moldability, heat resistance, and toughness, and further allows for a wide range of adjustment of physical properties, and uses thereof.

[0009] The present invention was made to solve the above-mentioned problems, and was completed based on the discovery that a thermosetting composition containing a siloxane compound having a predetermined structure and containing multiple alkenyl groups, and at least one compound selected from an aromatic polymer having a reactive functional group and a cycloolefin polymer having a reactive functional group, gives a cured product having low dielectric properties, particularly low relative dielectric constant and dielectric dissipation factor, and excellent heat resistance and toughness, and further that the physical properties of the cured product can be adjusted over a wide range.

[0010] The aromatic polymer having a reactive functional group and the cycloolefin polymer having a reactive functional group according to the present invention are preferably polymers that have a reactive functional group but have a low polar group concentration and a low relative dielectric constant and dielectric loss tangent, and from the viewpoint of technical effect, PPE having a reactive functional group is particularly preferred.

[0011] More specifically, the present invention relates to a thermosetting composition comprising: (A) 10 to 90 parts by mass of one or more siloxane compounds selected from the following (a1) and (a2): (a1) a linear siloxane having at least two alkenyl groups and at least one aryl group in the molecule; (a2) a siloxane having at least two alkenyl groups in the molecule and having 8 or less silicon atoms; (B) 10 to 90 parts by mass of at least one compound selected from aromatic polymers having reactive functional groups and cycloolefin polymers having reactive functional groups (wherein the sum of components (A) and (B) is 100 parts by mass); and (C) a thermal radical initiator in an amount of 0.1 to 5 parts by mass per 100 parts by mass of the combined total of components (A) and (B).

[0012] The component (B) may be a PPE having a reactive functional group at the molecular chain end.

[0013] The component (B) may be a PPE having at least one reactive functional group selected from an alkenyl group and a (meth)acrylate group at the molecular chain terminal.

[0014] The component (A) is preferably a compound that satisfies at least one of the following conditions (a3) ​​and (a4): (a1-1) A linear siloxane having at least two alkenyl groups in the molecule and having an aryl group molar fraction of 20% or more of all substituents on silicon atoms; (a2-1) A cyclic siloxane having at least two alkenyl groups in the molecule and having 8 or less silicon atoms.

[0015] The thermosetting composition of the present invention may further contain (D) an organic solvent. The content of component (D) may be in the range of 10 to 1000 parts by mass per 100 parts by mass of the total of components (A), (B), and (C).

[0016] The present invention further provides a cured product of the above-mentioned thermosetting composition. Also, the present invention provides a prepreg containing the above-mentioned cured product of the thermosetting composition and a fibrous reinforcing material.

[0017] The present invention further provides a high-frequency circuit board comprising a laminate of one or more sheets of the above prepreg.

[0018] The present invention further provides a method for curing and molding a thermosetting composition, comprising at least the following steps: step (i): removing component (D) from a thermosetting composition containing component (D) at a temperature in the range of about 80-100°C under atmospheric pressure or reduced pressure; and step (ii): subsequent to step (i), curing the thermosetting composition at a temperature of 150°C or higher and processing it into a desired shape.

[0019] The present invention further provides a method for producing a prepreg, which comprises impregnating a fibrous reinforcing material with a thermosetting composition containing the above-mentioned component (D), and then removing component (D) to cure the thermosetting composition.

[0020] The thermosetting composition of the present invention contains, as its main components, a siloxane compound having a predetermined structure and containing multiple alkenyl groups, and at least one compound selected from an aromatic polymer having a reactive functional group and a cycloolefin polymer having a reactive functional group. Because the compatibility between these two components is good, the transparency and moldability of the curable composition and the heat-cured cured product are particularly good after removal of the organic solvent. Furthermore, the cured product has excellent toughness and allows for a wide range of compositional design, allowing for good property adjustment of the cured product. Additionally, the cured product obtained by the present invention has good heat resistance and a very high modulus of elasticity even at high temperatures of 200°C or higher. Furthermore, the cured product obtained by the present invention has low relative permittivity and dielectric loss tangent, resulting in excellent dielectric properties. Therefore, the thermosetting composition of the present invention is useful as an insulating material for circuit boards in devices for transmitting digital signals at high speed and large capacity, particularly in electric and electronic devices that use high frequencies.

[0021] The thermosetting composition of the present invention comprises, as essential components, (A) one or more siloxane compounds selected from the following (a1) and (a2): (a1) a linear siloxane having at least two alkenyl groups and at least one aryl group in the molecule; (a2) a siloxane having at least two alkenyl groups in the molecule and having 8 or less silicon atoms; (B) at least one compound selected from an aromatic polymer having a reactive functional group and a cycloolefin polymer having a reactive functional group; and (C) a thermal radical initiator, and optionally (D) an organic solvent.

[0022] [Component (A)] Component (A) of the present invention is one or more siloxane compounds selected from the above (a1) and (a2), and two or more siloxane compounds may be used. This component has an alkenyl group, can chemically react with the reactive functional group of component (B), and acts as a crosslinker in the composition. (a1) A linear siloxane having at least two alkenyl groups and at least one aryl group in the molecule. (a2) A siloxane having at least two alkenyl groups in the molecule and having 8 or less silicon atoms.

[0023] To ensure good affinity with component (B), which will be described below, component (A) must satisfy either condition (a1) or (a2) above. Specifically, component (A) is either (a1) an alkenyl-containing siloxane compound having at least one aryl group in the molecule, or (a2) an alkenyl-containing siloxane compound having eight or fewer silicon atoms. Compounds that satisfy both of these conditions can also be used without any problems. More specifically, component (A) may be a siloxane compound that falls under either (a1) or (a2) (for example, a "linear siloxane having at least two alkenyl groups in the molecule, eight or fewer silicon atoms, and an aryl group" falls under both component (a1) and component (a2), and can therefore be used without any problems as component (A) of the present invention).

[0024] On the other hand, if the siloxane compound does not fall into either of the above (a1) or (a2), for example, if the number of silicon atoms in the siloxane compound exceeds 8 and it does not have a linear structure (for example, it has a resinous or branched structure), it may not be possible to ensure good affinity with component (B). Furthermore, in the case of a siloxane compound that does not have an alkenyl group in the molecule, it is not possible to ensure reactivity with component (B).

[0025] Specific examples of linear siloxane compounds that fall into the category of (a1) above include 1,1,3-trimethyl-3-phenyl-1,3-divinyldisiloxane, 1,3-dimethyl-1,3-diphenyl-1,3-divinyldisiloxane, 1,1,5,5-tetramethyl-3,3-diphenyl-1,5-divinyltrisiloxane, 1,1,7,7-tetramethyl-3,3,5,5-tetraphenyl-1,7-divinyltetrasiloxane, a copolymer of dimethylvinylsilyl at both ends and dimethyl / methylphenylsiloxane, a copolymer of dimethylvinylsilyl at both ends and dimethyl / diphenylsiloxane, a copolymer of dimethylvinylsilyl at both ends and polymethylphenylsiloxane, and a copolymer of trimethylsilyl at both ends and methylphenyl / methylvinylsiloxane.

[0026] Among the above-mentioned compounds, component (A) is preferably a linear siloxane (a1-1) having at least two alkenyl groups in the molecule and having an aryl group molar fraction of 20% or more of all substituents on the silicon atom. This characteristic further improves affinity with component (B) and contributes to improving the toughness of the cured product obtained from the composition. Specifically, 1,3-dimethyl-1,3-diphenyl-1,3-divinyldisiloxane, 1,1,5,5-tetramethyl-3,3-diphenyl-1,5-divinyltrisiloxane, 1,1,7,7-tetramethyl-3,3,5,5-tetraphenyl-1,7-divinyltetrasiloxane, a copolymer of dimethylvinylsilyl at both ends and dimethyl / methylphenylsiloxane having an aryl group molar fraction of 20% or more, a copolymer of dimethylvinylsilyl at both ends and dimethyl / diphenylsiloxane having an aryl group molar fraction of 20% or more, and a copolymer of dimethylvinylsilyl at both ends and polymethylphenylsiloxane are recommended as preferred component (A).

[0027] On the other hand, specific examples of siloxanes having 8 or less silicon atoms that fall into the category of (a2) above include 1,7-divinyl-1,1,3,3,5,5,7,7-octamethyltetrasiloxane, 1,3,5,7-tetramethyl-1,3,5,7-tetravinylcyclotetrasiloxane, methyltris(dimethylvinylsiloxy)silane, phenyltris(dimethylvinylsiloxy)silane, and tetrakis(dimethylvinylsiloxy)silane.

[0028] Of the compounds described above, component (A) is preferably a cyclic siloxane (a2-1) having at least two alkenyl groups in the molecule and containing eight or fewer silicon atoms. Another desirable condition is that the boiling point under atmospheric pressure is 220°C or higher. These properties not only improve the affinity with component (B) but also contribute to improving the modulus of elasticity of the cured product obtained from the composition. Specifically, 1,3,5,7-tetramethyl-1,3,5,7-tetravinylcyclotetrasiloxane is recommended as a preferred component (A).

[0029] Accordingly, the siloxane compounds classified into the above categories (a1-1) and (a2-1) can be preferably used as component (A) of the present invention. Specifically, the following compounds are recommended: 1,3-dimethyl-1,3-diphenyl-1,3-divinyldisiloxane, 1,1,5,5-tetramethyl-3,3-diphenyl-1,5-divinyltrisiloxane, 1,1,7,7-tetramethyl-3,3,5,5-tetraphenyl-1,7-divinyltetrasiloxane, a copolymer of dimethylvinylsilyl at both ends and dimethyl / methylphenylsiloxane having an aryl group molar fraction of 20% or more, a copolymer of dimethylvinylsilyl at both ends and dimethyl / diphenylsiloxane having an aryl group molar fraction of 20% or more, a copolymer of dimethylvinylsilyl at both ends and dimethylvinylsilyl-polymethylphenylsiloxane, and 1,3,5,7-tetramethyl-1,3,5,7-tetravinylcyclotetrasiloxane. These compounds can be used alone or in combination of two or more kinds.

[0030] [Component (B)] Component (B) is at least one compound selected from aromatic polymers having reactive functional groups and cycloolefin polymers having reactive functional groups. This component contributes to improving the heat resistance of the cured product obtained by heat curing of the curable composition, particularly increasing the elastic modulus at high temperatures, and also contributes to reducing the dielectric constant by taking advantage of the characteristics of its low polarity skeleton.

[0031] Component (B) may be an aromatic polymer, a cycloolefin polymer, or a mixture thereof, as long as it has a reactive functional group. That is, component (B) may be a single compound or a mixture of multiple compounds, and when used in combination with component (A), it can improve the physical properties of the cured product, reduce the dielectric constant, and impart low dielectric properties. Note that component (B) having an aromatic polymer skeleton and component (B) having a cycloolefin polymer skeleton can be appropriately selected depending on the application, physical properties, and desired dielectric constant of the cured product. In a preferred embodiment of the present invention, a mixture ratio of components (B) having different skeletons can be adjusted to achieve the desired properties.

[0032] [Aromatic Polymer Having Reactive Functional Group] While there are no limitations on the location of the reactive functional group in the aromatic polymer having a reactive functional group (component (B)), from the viewpoint of good reaction control, an aromatic polymer having a reactive functional group at the molecular chain end is preferred. Here, the term "aromatic polymer" refers to a polymer whose main chain is composed of aryl groups and heteroatom-containing groups connecting them, specifically linking groups such as ether groups, thioether groups, ester groups, thioester groups, amide groups, imide groups, urethane groups, thiourethane groups, urea groups, thiourea groups, and acid anhydride groups. Among these linking groups, the lower the polarity, the more preferable it is for reducing the dielectric constant. Therefore, ether bonds are the recommended linking group. That is, preferred component (B) includes polymers having aryl groups and ether bonds as main structural units, with polyphenylene ether (PPE) being the preferred polymer. In particular, PPE having a reactive functional group at the molecular chain end is a particularly preferred polymer.

[0033] Here, the PPE is formed from repeating units consisting of phenylene groups and ether bonds, but may contain copolymerization component units other than the phenylene ether unit structure, as long as the functions and effects of the present invention are not impaired. Specifically, PPE having a substituent, such as poly(2,6-dimethyl-1,4-phenylene ether), poly(2-methyl-6-ethyl-1,4-phenylene ether), poly(2-methyl-6-phenyl-1,4-phenylene ether), or poly(2,6-dichloro-1,4-phenylene ether), as well as PPE copolymers such as copolymers of 2,6-dimethylphenol and other phenols (e.g., 2,3,6-trimethylphenol, 2-methyl-6-butylphenol, etc.), and PPE copolymers obtained by coupling 2,6-dimethylphenol with biphenols or bisphenols, can also be used as component (B) of the present invention.

[0034] The reactive functional group of the aforementioned component (B) is preferably a functional group whose reaction is accelerated by heating, as with component (A), and specifically, is preferably one or more functional groups selected from an alkenyl group and a (meth)acrylate group. Preferred examples of the alkenyl group include alkenyl groups having 2 to 8 carbon atoms. Specific examples include vinyl groups, allyl groups, 1-butenyl groups, 1-pentenyl groups, 1-hexenyl groups, and styryl groups, with vinyl groups, allyl groups, and styryl groups being particularly preferred. Meanwhile, both acrylate groups and methacrylate groups are applicable as the (meth)acrylate group. Considering reactivity, acrylate groups are more preferred.

[0035] That is, in the present invention, recommended component (B) includes PPE having vinyl groups at both molecular chain terminals, PPE having a vinyl group at one molecular chain terminal, PPE having allyl groups at both molecular chain terminals, PPE having an allyl group at one molecular chain terminal, PPE having a styryl group at both molecular chain terminals, PPE having a styryl group at one molecular chain terminal, PPE having an acrylate group at both molecular chain terminals, PPE having an acrylate group at one molecular chain terminal, PPE having a methacrylate group at both molecular chain terminals, and PPE having a methacrylate group at one molecular chain terminal. Among these, PPE having reactive functional groups at both molecular chain terminals is preferred, and specifically, PPE having styryl groups at both molecular chain terminals, PPE having acrylate groups at both molecular chain terminals, and PPE having methacrylate groups at both molecular chain terminals are preferred component (B). As component (B), a widely used methacrylate-terminated PPE (product name: SA9000) manufactured by Sabic Innovative Plastics can also be used.

[0036] The molecular weight of the aromatic polymer having a reactive functional group, component (B), is not particularly limited, but it is recommended that the weight-average molecular weight, measured by gel permeation chromatography (GPC) in terms of standard polystyrene, be 1,000 to 5,000. A weight-average molecular weight of 1,000 to 3,000 is particularly desirable. This characteristic allows for the production of a cured product with low brittleness and good mechanical strength upon heat curing.

[0037] [Cycloolefin Polymer Having Reactive Functional Group] Component (B) may be a polymer having a cycloolefin ring structure as its basic skeleton, and a portion or all of the polymer may be a cycloolefin polymer having a reactive functional group. Specifically, the cycloolefin polymer of component (B) is a (co)polymer having, as an essential structural unit, a repeating unit derived from a cycloolefin having the reactive functional group in the molecule. The cycloolefin monomer (cyclic olefin compound) constituting the cycloolefin polymer (B) usable in the present invention is not particularly limited, and is a compound having a polymerizable carbon-carbon double bond capable of chain polymerization (metathesis ring-opening polymerization, addition polymerization, etc.) and having an alicyclic structure such as a monocyclic ring, a polycyclic ring, a fused polycyclic ring, a bridged ring, or a polycyclic ring formed by combining these. The cycloolefin monomer constituting component (B) of the present invention may be the cyclic olefin monomer described in paragraphs 0037 to 0063 of WO 2006 / 0118261. In addition, the cycloolefin polymers that can be used in the present invention include those disclosed in JP 2015-067671, JP 2014-162172, JP 2015-160326, JP 2015-123671, JP 2015-123670, JP 2014-205727, JP 2014-177568, JP 2018-034422, JP 2018-035257, JP 2017-125176, JP 2017-125175, JP 2017-125174, etc., and can be used without particular limitation. Cycloolefin polymers obtained by the structures, monomers, and synthesis examples disclosed in these documents can be used as part or all of component (B) of the present invention.

[0038] Component (B) may contain an aromatic polymer having a reactive functional group and a cycloolefin polymer having a reactive functional group in a mixing ratio of 100:0 to 0:100. For example, component (B) that is a cycloolefin polymer may be selected from the viewpoint of further improving the dielectric properties while maintaining good heat resistance and thermal stability of the resulting cured product, prepreg, or printed wiring board, or improving the impregnation of a sheet-like fiber substrate or the like with the curable resin composition when producing a prepreg. Alternatively, component (B) that is an aromatic polymer, such as polyphenylene ether (PPE) having a reactive functional group at the molecular chain end, may be selected from the viewpoint of the mechanical properties and low dielectric constant of the cured product.

[0039] The mixing ratio (parts by mass) of component (A) to component (B) in the thermosetting composition of the present invention is in the range of 10 to 90 parts by mass of (A) to 10 to 90 parts by mass of (B), assuming the sum of component (A) and component (B) is 100 parts by mass. This mixing ratio has a significant impact on the properties of the cured product, so it is preferable to design it within this range depending on the intended use of the cured product. Specifically, the mechanical properties, particularly the modulus of elasticity at high temperatures, depend on the type and content of reactive functional groups in component (A), but tend to increase with increasing the component (A) / component (B) ratio. Meanwhile, the toughness of the cured product depends on the concentration of alkenyl groups in component (A), and cured products obtained from compounds with a low concentration of alkenyl groups tend to exhibit high toughness. Therefore, by optimizing this mixing ratio and the chemical structure of component (A), the mechanical properties and dielectric properties of the resulting cured product can be tuned to the desired range.

[0040] [Use of Other Organic Resins in Combination] While the main components in the thermosetting composition of the present invention are components (A) and (B), reactive organic resins other than component (B) can be used in combination as long as the technical effects of the present invention are not impaired. For example, in the present invention, component (B) can be used in combination with one or more organic resins (B') selected from epoxy resins, polyimide resins, liquid crystal polymers, maleimide resins (including so-called BT resins), and polybutadiene resins. These organic resins are optional components, and their amounts are not particularly limited. However, one or more organic resins may be used in an amount of 0 to 500 parts by weight, 0 to 250 parts by weight, or 0 to 100 parts by weight per 100 parts by weight of component (AB), and this is preferred. Furthermore, in order to improve the compatibility of these organic resins with component (A) and component (B), a compatibilizer (B") selected from modified polyolefins, modified elastomers, compounds having a polar group and an unsaturated carbon bond capable of contributing to a polymerization reaction in the molecule, and the like may be contained.

[0041] The epoxy resin may be one or more selected from glycidyl ether epoxy resins such as phenol novolac epoxy resins, cresol novolac epoxy resins, bisphenol A epoxy resins, bisphenol F epoxy resins, bisphenol A novolac epoxy resins, bisphenol F novolac epoxy resins, brominated bisphenol A epoxy resins, brominated bisphenol F epoxy resins, and hydrogenated bisphenol A epoxy resins, alicyclic epoxy resins, glycidyl ester epoxy resins, glycidyl amine epoxy resins, isocyanurate epoxy resins, and epoxy resins having an alicyclic olefin structure or a fluorene structure. From the viewpoint of further improving the mechanical strength of the resulting cured product, at least one selected from bisphenol A epoxy resins and bisphenol A novolac epoxy resins may be selected.

[0042] Examples of polyimide resins include those described in paragraphs 0008 to 0011 of JP 2009-120696 A, and can be obtained by reacting a tetracarboxylic acid anhydride, diimide, or monoimide (hereinafter abbreviated as tetracarboxylic acid anhydride, etc.) with a diamine. The reaction of a tetracarboxylic acid anhydride, etc. with a diamine can be carried out using a generally known method, and commercially available products can also be used. The polyimide resin may be a linear polyimide.

[0043] The liquid crystal polymer is not particularly limited, but examples thereof include those described in paragraphs 0023 to 0029 of JP 2008-19400 A, which are melt-processable polymers capable of forming an optically anisotropic molten phase. The type of liquid crystal polymer is not particularly limited, but is preferably an aromatic polyester or an aromatic polyester amide, and may be a polyester partially containing an aromatic polyester or an aromatic polyester amide in the same molecular chain.

[0044] The maleimide resin is not particularly limited, but examples thereof include those described in paragraphs 0009 to 0013 of JP-A No. 2006-124494, which are maleimide resins obtained from a maleimide compound (X) having two or more maleimide groups in the molecule. The scope of maleimide resins also includes a mixture of the maleimide compound (X) and a triazine resin obtained by reacting a cyanate ester compound (Y) with the maleimide compound (X) (bismaleimide triazine resin (BT resin)).

[0045] Examples of the maleimide compound (X) include bis(4-maleimidophenyl)methane, 2,2-bis{4-(4-maleimidophenoxy)-phenyl}propane, bis(3,5-dimethyl-4-maleimidophenyl)methane, bis(3-ethyl-5-methyl-4-maleimidophenyl)methane, bis(3,5-diethyl-4-maleimidophenyl)methane, 2,2'-bis[4-(4-maleimidophenoxy)phenyl]propane, polyphenylmethane maleimide, m-phenylene bismaleimide, p-phenylene bismaleimide, 3,3'-dimethyl- Examples of suitable bismaleimides include 5,5'-diethyl-4,4'-diphenylmethane bismaleimide, 4-methyl-1,3-phenylene bismaleimide, 4,4'-diphenylether bismaleimide, 4,4'-diphenylsulfone bismaleimide, 1,3-bis(3-maleimidophenoxy)benzene, 1,3-bis(4-maleimidophenoxy)benzene, 1,6'-bismaleimido-(2,2,4-trimethyl)hexane, 1,2-bismaleimidoethane, 1,6-bismaleimidohexane, and polytetramethylene oxide-bis(4-maleimidobenzoate).

[0046] The cyanate ester compound (Y) is not particularly limited as long as it is a cyanate ester compound having two or more cyanate groups in one molecule, and examples thereof include 1,3- or 1,4-dicyanate benzene, 1,3,5-tricyanate benzene, 1,3-, 1,4-, 1,6-, 1,8-, 2,6- or 2,7-dicyanate naphthalene, 1,3,6-tricyanate naphthalene, 4,4-dicyanate biphenyl, bis(4-cyanate phenyl)methane, bis(3,5-dimethyl-4-cyanate phenyl)methane, 2,2-bis(4-cyanate phenyl)propane, 2,2-bis(3,5-dibromo-4-cyanate phenyl)propane, 2,2-bis(3, Examples of the cyanate ester compound include cyanate ester compounds obtained by reacting cyanogen halide with cyanogen halide and 5-dimethyl-4-cyanatephenyl)propane, bis(4-cyanatephenyl)ether, bis(4-cyanatephenyl)thioether, bis(4-cyanatephenyl)sulfone, tris(4-cyanatephenyl)phosphite, tris(4-cyanatephenyl)phosphate, oligomers (novolak, hydroxyl group-containing thermoplastic resins (hydroxypolyphenylene ether, hydroxypolystyrene, hydroxypolycarbonate, etc.)), and the like; and cyanate ester compounds obtained by reacting cyanogen halide with a polyfunctional phenol in which phenol is bonded via dicyclopentadiene.

[0047] The polybutadiene resin is not particularly limited, and examples thereof include 1,4-polybutadiene, 1,2-polybutadiene, terminal acrylate-modified polybutadiene, and terminal urethane methacrylate-modified polybutadiene.

[0048] [Component (C)] Component (C) is a thermal radical initiator that functions as a catalyst to accelerate the curing reaction by heating. Any compound that decomposes upon heating to generate free radical species can be used as component (C) of the present invention, regardless of its chemical structure. Typically, organic peroxides that decompose to generate oxygen radicals and azo compounds that decompose to generate carbon radicals are well known, and either group of compounds can be used alone or in combination of two or more. It is also possible to use an organic peroxide and an azo compound in combination.

[0049] Known organic peroxides are broadly classified according to their chemical structure into (I) diacyl peroxides, (II) peroxydicarbonates, (III) peroxyesters, (IV) peroxyketals, (V) dialkyl peroxides, (VI) hydroperoxides, and (VII) others. Specific examples of compounds classified as (I) include dibenzoyl peroxide and dilauroyl peroxide, compounds classified as (II) include di(2-ethylhexyl)peroxydicarbonate, compounds classified as (III) include tert-butyl peroxyacetate and tert-butyl peroxylaurate, compounds classified as (IV) include 1,1-di(tert-butylperoxy)cyclohexane and normal butyl-4,4-(tert-butylperoxy)valerate, compounds classified as (V) include dicumyl peroxide, di-tert-butyl peroxide and 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3, and compounds classified as (VI) include cumene hydroperoxide, diisopropylbenzene hydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide and di-tert-butyl hydroperoxide, but are not limited to these.

[0050] Known azo compounds are broadly classified into (I) azonitriles, (II) azoesters, (III) azoamides, and (IV) others, depending on their chemical structure. Specific examples of compounds classified into (I) include 2,2-azobis(2-methylbutyronitrile), 1,1-azobis(cyclohexane-1-carbonitrile), and 2,2-azobis(isobutyronitrile). Examples of compounds classified into (II) include dimethyl-2,2-azobis(isobutyrate). Examples of compounds classified into (III) include 2,2-azobis[N-(2-propenyl)-2-methylpropionamide] and 2,2-azobis(N-butyl-2-methylpropionamide]. Examples of compounds classified into (IV) include 2,2-azobis[2-(2-imidazolin-2-yl)propane], but are not limited to these.

[0051] The activity of the above-mentioned compounds is defined by the half-life temperature associated with decomposition in the temperature range used in the reaction, and is usually 10 hours half-life temperature (T 10h ) and 1-minute half-life temperature (T 1m In the present invention, taking into consideration the temperature range when the thermosetting composition described later is cured, T 10h is 110°C or higher and T 1m It is preferable to use as component (C) a compound that satisfies at least one of the conditions that the temperature is 170° C. or higher. When two or more compounds are used in combination, it is preferable that at least one of them satisfies this condition.

[0052] In view of the above conditions, it is desirable that component (C) of the present invention contains at least one compound selected from the group of compounds broadly classified as dialkyl peroxides and hydroperoxides. Specific examples of compounds that are preferably used include dicumyl peroxide, ditertiary butyl peroxide, 2,5-dimethyl-2,5-di(tertiary butylperoxy)hexyne-3, di(2-tertiary butylperoxyisopropyl)benzene, cumene hydroperoxide, diisopropylbenzene hydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide, ditertiary butyl hydroperoxide, and paramenthane hydroperoxide.

[0053] The content of component (C) in the present invention is an amount that is 0.1 to 5 parts by mass per 100 parts by mass of the total of the above components (A) and (B). A preferred content is 0.1 to 3 parts by mass, and more preferably 0.3 to 1 part by mass. If the content of this component is less than 0.1 part by mass, the time required for the curing reaction of the thermosetting composition described below will be longer, and there is a concern that the degree of cure in the cured product will be non-uniform. On the other hand, if the content exceeds 5 parts by mass, there is a high possibility that component (C) will remain even after the curing reaction is complete, which will have an adverse effect on the heat resistance, mechanical properties, etc. of the cured product.

[0054] [Component (D)] Component (D) is an organic solvent that serves as an auxiliary for mixing components (A), (B), and (C) to prepare a uniform curable composition. By removing component (D) from the system after mixing the raw materials constituting the curable composition, a uniform and highly transparent composition can be prepared. In addition to the above-mentioned purpose, component (D) also functions to adjust the film thickness of the coating film derived from the curable composition. While this component is an optional component, considering the above-mentioned function, it is practically desirable to use it at the stage of mixing the various components. As such an organic solvent, any organic solvent that has conventionally been blended in various organopolysiloxane-based curable compositions can be used without particular limitation.

[0055] Suitable examples of the organic solvent include (poly)alkylene glycol monoalkyl ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol mono-n-propyl ether, ethylene glycol mono-n-butyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol mono-n-propyl ether, diethylene glycol mono-n-butyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol mono-n-propyl ether, propylene glycol mono-n-butyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol mono-n-propyl ether, and dipropylene glycol mono-n-butyl ether; (Poly)alkylene glycol monoalkyl ether acetates such as methyl ether acetate, ethylene glycol monoethyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate (PGMEA), and propylene glycol monoethyl ether acetate; other ethers such as diethylene glycol dimethyl ether, diethylene glycol methyl ethyl ether, and diethylene glycol diethyl ether; ketones such as methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, 2-heptanone, 3-heptanone, 4-heptanone, 5-methyl-3-heptanone, 2,4-dimethyl-3-pentanone, and 2,6-dimethyl-4-heptanone; alkyl lactate esters such as methyl 2-hydroxypropionate and ethyl 2-hydroxypropionate;Ethyl 2-hydroxy-2-methylpropionate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, ethyl ethoxyacetate, ethyl hydroxyacetate, methyl 2-hydroxy-3-methylbutanoate, 3-methoxybutyl acetate, 3-methyl-3-methoxybutyl acetate, 3-methyl-3-methoxybutylpropionate, ethyl acetate, n-propyl acetate, i-propyl acetate, n-butyl acetate, i-butyl acetate, n-pentyl formate, i-pentyl acetate, n-butyl propionate, butyric acid Other esters such as ethyl butyrate, n-propyl butyrate, i-propyl butyrate, n-butyl butyrate, methyl pyruvate, ethyl pyruvate, n-propyl pyruvate, methyl acetoacetate, ethyl acetoacetate, and ethyl 2-oxobutanoate; aromatic hydrocarbons such as toluene, xylene, mesitylene, cumene, propylbenzene, diethylbenzene, and 1,3-diisopropylbenzene; and aromatic ethers such as anisole, phenetole, 2-methoxytoluene, 3-methoxytoluene, 4-methoxytoluene, 3,4-dimethoxytoluene, and 1,4-bis(methoxymethyl)benzene. Component (D) may be used alone, or multiple components (D) may be used in combination, taking into consideration the miscibility with components (A) to (C).

[0056] The content of component (D) is 0 to 1,000 parts by mass per 100 parts by mass of the total of components (A), (B), and (C) of the present invention. That is, component (D) does not have to be included in the present thermosetting composition, but it is preferable to include this component in order to efficiently prepare a uniform and transparent curable composition. The amount used may be 10 to 1,000 parts by mass, and is preferably 10 to 200 parts by mass, per 100 parts by mass of the total of components (A), (B), and (C).

[0057] [Other Additives] The thermosetting composition of the present invention may contain, if desired, other additives in addition to the above-described components (A) to (D). Examples of additives include, but are not limited to, those listed below.

[0058] [Crosslinking Agent] The thermosetting composition of the present invention may further contain a component capable of chemically reacting with component (B) as a crosslinking agent in order to control the crosslink density and adjust the physical properties, particularly the mechanical properties and dielectric properties, of the resulting cured product, or to adjust the efficiency of the curing reaction. Suitable examples of such components include silicon-free compounds. Considering the affinity with component (A), the refractive index (n D ) is 1.45 or more, with or without an aryl group is preferred.

[0059] The silicon-free compound preferably used as a crosslinking agent is preferably one having at least two polymerizable double bonds in the molecule, and specific examples thereof include trialkenyl isocyanurate compounds such as triallyl isocyanurate, trialkenyl cyanurate compounds such as triallyl cyanurate, polyfunctional (meth)acrylate compounds having two or more (meth)acrylate groups in the molecule, multivinylaryl compounds such as divinylbenzene, and polyfunctional maleimide compounds having two or more maleimide groups in the molecule, such as 4,4'-bismaleimide diphenylmethane.

[0060] There are no significant limitations on the amount of crosslinking agent added to the thermosetting composition of the present invention, but it is preferably in the range of 0.5 to 10 parts by mass, 1 to 10 parts by mass, or 1 to 5 parts by mass per 100 parts by mass of component (A).

[0061] [Adhesion Imparting Agent] An adhesion imparting agent can be added to the thermosetting composition of the present invention in order to improve the adhesion or adhesion to a substrate in contact with the composition. When the curable composition of the present invention is used for applications requiring adhesion or adhesion to a substrate, such as a coating agent or a sealant, it is preferable to add an adhesion imparting agent to the thermosetting composition of the present invention. Any known adhesion imparting agent can be used as this adhesion imparting agent, as long as it does not inhibit the curing reaction of the composition of the present invention.

[0062] Examples of adhesion promoters that can be used in the present invention include organosilanes having a trialkoxysiloxy group (e.g., trimethoxysiloxy group, triethoxysiloxy group) or a trialkoxysilylalkyl group (e.g., trimethoxysilylethyl group, triethoxysilylethyl group) and a hydrosilyl group or an alkenyl group (e.g., vinyl group, allyl group), or organosiloxane oligomers having a linear, branched or cyclic structure and about 4 to 20 silicon atoms; organosilanes having a trialkoxysiloxy group or a trialkoxysilylalkyl group and a methacryloxyalkyl group (e.g., 3-methacryloxypropyl group), Silanes or organosiloxane oligomers having a linear, branched, or cyclic structure and having about 4 to 20 silicon atoms; organosilanes or organosiloxane oligomers having a linear, branched, or cyclic structure and having about 4 to 20 silicon atoms, each having a trialkoxysiloxy group or trialkoxysilylalkyl group and an epoxy group-bonded alkyl group (e.g., 3-glycidoxypropyl group, 4-glycidoxybutyl group, 2-(3,4-epoxycyclohexyl)ethyl group, 3-(3,4-epoxycyclohexyl)propyl group); organic compounds having two or more trialkoxysilyl groups (e.g., trimethoxysilyl group, triethoxysilyl group);Examples thereof include reaction products of aminoalkyltrialkoxysilanes and epoxy group-bonded alkyltrialkoxysilanes, and epoxy group-containing ethyl polysilicates. Specific examples thereof include vinyltrimethoxysilane, allyltrimethoxysilane, allyltriethoxysilane, hydrogentriethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 1,6-bis(trimethoxysilane), silyl)hexane, 1,6-bis(triethoxysilyl)hexane, 1,3-bis[2-(trimethoxysilyl)ethyl]-1,1,3,3-tetramethyldisiloxane, a reaction product of 3-glycidoxypropyltriethoxysilane and 3-aminopropyltriethoxysilane, a condensation reaction product of a silanol group-blocked methylvinylsiloxane oligomer and 3-glycidoxypropyltrimethoxysilane, a condensation reaction product of a silanol group-blocked methylvinylsiloxane oligomer and 3-methacryloxypropyltriethoxysilane, and tris(3-trimethoxysilylpropyl)isocyanurate;

[0063] The amount of adhesion promoter added to the thermosetting composition of the present invention is not particularly limited, but is preferably in the range of 0.01 to 5 parts by mass, or 0.01 to 2 parts by mass, per 100 parts by mass of the total of components (A) to (C), in order not to promote the curing characteristics of the curable composition or discoloration of the cured product.

[0064] [Additional Optional Additives] Other additives may be added to the thermosetting composition of the present invention or its cured product, if desired, in addition to or instead of the crosslinking agent and adhesion promoter described above. Usable additives include flame retardants, heat stabilizers, weather stabilizers, antistatic agents, slip agents, antiblocking agents, antifogging agents, lubricants, dyes, pigments, natural oils, synthetic oils, waxes, organic or inorganic filler leveling agents, silane coupling agents not included in the adhesion promoters listed above, heat absorbers, antioxidants, polymerization inhibitors, fillers (functional fillers such as reinforcing fillers, insulating fillers, and thermally conductive fillers), and fibrous reinforcing materials such as glass cloth. Furthermore, a thixotropic agent may be added to the composition of the present invention, if necessary, especially when used as a sealing material. Furthermore, thermoplastic resins or thermosetting resins other than the above components (A), (B), (B'), and (B'') may be added to the composition to the extent that the object of the present invention is not impaired, and the amount added is appropriate.

[0065] [Method of Molding and Curing Thermosetting Composition] The thermosetting composition of the present invention typically contains component (D), an organic solvent. However, it is desirable that the cured product obtained from this composition does not contain component (D). Therefore, it is preferable to prepare a thermosetting composition containing components (A) to (C) by first preparing a thermosetting composition containing components (A) to (D) and then removing component (D). In other words, it is preferable to mix component (D) with components (A) to (C), and then remove it from the composition after a uniform and transparent composition containing components (A) to (C) is obtained.

[0066] Specifically, a method for molding and curing a thermosetting composition is recommended, which includes at least the following steps (i) and (ii): (i) removing component (D) from the thermosetting composition of the present invention (where the amount of component (D) is not 0 parts by mass) at a temperature in the range of about 80-100°C under normal pressure or reduced pressure; and (ii) curing the thermosetting composition at a temperature of 150°C or higher and processing it into a desired shape following step (i).

[0067] As described above, additives can be added to or impregnated into the thermosetting composition of the present invention as needed. If the prepared composition has sufficient fluidity, it can be molded by applying it to a desired substrate or by pouring it into a mold of a desired shape. On the other hand, if the composition does not have sufficient fluidity, it can be processed into the desired shape by a method such as press molding. The fluid or non-fluid thermosetting composition molded in this manner is in an uncured state and can be heat-cured in the subsequent step (ii) to obtain a cured product.

[0068] In step (i), the organic solvent (component (D)) is removed from the thermosetting composition molded by the above-described method by a commonly known method. Therefore, the thermosetting composition used in this production method is a composition containing the organic solvent (component (D)).

[0069] The method for removing component (D) in step (i) is not particularly limited. Specific examples of methods for removing component (D) at normal pressure include heating on a hot plate, heating in an oven, and heating in a press. Meanwhile, methods for removing component (D) under reduced pressure include heating in a vacuum oven and heating in a vacuum press. A temperature range of approximately 80-100°C is recommended for this step, and more specifically, a temperature range in which thermal curing of the composition hardly occurs is preferred. While it is desirable for the organic solvent to be completely removed in this step, it is practically acceptable for a small amount of organic solvent (D), for example, 0.1 to 10 parts by mass or less per 100 parts by mass of the total of components (A) to (C), to remain.

[0070] In step (ii), the thermosetting composition prepared above, containing almost no component (D), is thermally cured at a temperature of 150°C or higher while maintaining the desired shape. This step can be performed under normal pressure; however, if step (i) is performed under reduced pressure, the temperature can be raised and step (ii) can be performed under reduced pressure. Furthermore, even if component (D) remains at the end of step (i), step (ii) can be performed under reduced pressure, which is both possible and desirable. Taking into account the glass transition temperature of component (B), a temperature of 150°C or higher is strongly recommended for this step, but it can be adjusted appropriately taking into account the half-life temperature of component (C) described above. In practice, the temperature range may be 150 to 300°C, 150 to 270°C, or 150 to 250°C. Furthermore, the time required for step (ii) (curing time) is typically 1 to 5 hours. During curing, for example, two-stage curing, achieved by varying the temperature from low to high, is also possible and preferred.

[0071] The present invention also encompasses cured products obtained from the thermosetting composition containing the above components (A) to (C).

[0072] [Prepreg] Meanwhile, by impregnating the present thermosetting composition (provided the amount of component (D) is not 0 parts by mass) with a fibrous reinforcing material and then removing component (D), an uncured composition, commonly referred to as a prepreg, containing a reactive branched organopolysiloxane, at least one compound selected from an aromatic polymer having a reactive functional group and a cycloolefin polymer having a reactive functional group, and a fibrous reinforcing material as its main components is obtained. This prepreg is also encompassed by the present invention. The resulting prepreg can be converted into a fibrous reinforcing material-containing cured product by subjecting it to the heat curing process described above. The amount of fibrous reinforcing material is typically 30 to 200 parts by mass, preferably 40 to 150 parts by mass, per 100 parts by mass of the total of components (A) to (C).

[0073] Furthermore, the present invention also encompasses a high-frequency circuit board comprising a laminate in which one or more prepregs prepared by the above-described method are laminated.

[0074] More specifically, the prepreg may be formed by combining the thermosetting composition according to the present invention (provided that the amount of component (D) is not 0 parts by mass) with a sheet-like fiber substrate. The method for producing the prepreg is not particularly limited, and various known methods can be applied. For example, there is a method including a step of impregnating a sheet-like fiber substrate with the thermosetting composition containing component (D) to obtain an impregnated body, and a step of heating the obtained impregnated body to dry the solvent contained in the varnish.

[0075] The impregnation of the sheet-like fiber substrate with the thermosetting composition can be carried out, for example, by applying a thermosetting composition containing a predetermined amount of component (D) to the sheet-like fiber substrate by a known method such as spray coating, dip coating, roll coating, curtain coating, die coating, or slit coating, and then, if necessary, overlaying a protective film thereon and pressing from above with a roller or the like. Furthermore, the process of heating the impregnated body to dry the solvent contained in the thermosetting composition containing component (D) is not particularly limited, but examples include drying in air or nitrogen using a blower dryer in a batch process, or drying by passing through a heating furnace in a continuous process. For example, after impregnating the sheet-like fiber substrate with the thermosetting composition containing component (D), the resulting impregnated body is heated to a predetermined temperature, whereby the solvent contained in the composition (= component (D)) evaporates, and a prepreg is obtained.

[0076] The fibers constituting the sheet-like fiber substrate usable in the prepreg according to the present invention are not particularly limited, but examples thereof include organic fibers such as PET (polyethylene terephthalate) fibers, aramid fibers, polyamide (nylon) fibers, and liquid crystal polyester fibers; and inorganic fibers such as glass fibers, carbon fibers, alumina fibers, tungsten fibers, molybdenum fibers, titanium fibers, steel fibers, boron fibers, silicon carbide fibers, and silica fibers. Among these, organic fibers and glass fibers are preferred, and aramid fibers, liquid crystal polyester fibers, and glass fibers are particularly preferred. As glass fibers, fibers such as E-glass, NE-glass, S-glass, D-glass, H-glass, and T-glass can be suitably used.

[0077] The impregnation of the sheet-like fiber substrate with the thermosetting composition containing component (D) is carried out, for example, by immersion and coating. The impregnation process may be repeated multiple times as needed. These sheet-like fiber substrates can be used alone or in combination of two or more. The amount used is selected appropriately as desired, but is typically in the range of 30 to 200 mass%, preferably 40 to 150 mass%, and more preferably 40 to 120 mass% of the prepreg or laminate. This range is advantageous in that the dielectric properties and mechanical strength of the resulting laminate are well balanced.

[0078] The thickness of the prepreg according to the present invention is selected appropriately depending on the intended use, but is usually 0.001 to 10 mm, preferably 0.005 to 1 mm, and more preferably 0.01 to 0.5 mm. This range is suitable because it allows for sufficient shaping during lamination and the mechanical strength, toughness, and other properties of the laminate obtained by curing.

[0079] The prepreg according to the present invention may be formed into a metal-clad laminate by laminating a metal foil on at least one surface thereof and heat-curing the laminate using a lamination press, etc. Examples of the metal foil include copper foil, aluminum foil, nickel foil, gold foil, silver foil, and stainless steel foil.

[0080] [Uses] The thermosetting composition of the present invention is useful as a material for forming insulating layers constituting various articles, particularly electronic and electrical devices, taking advantage of the dielectric properties of the cured product obtained after curing, and is particularly useful as an insulating material for circuit boards of electrical and electronic devices that utilize high frequencies. Furthermore, the thermosetting composition of the present invention can also be used as a composition for insulating coating agents, taking advantage of its excellent coating properties.

[0081] The present invention will be further described below based on examples, but the present invention is not limited to the following examples.

[0082] The preparation and evaluation of the thermosetting composition of the present invention, and the preparation and evaluation of the cured product thereof will be described in detail with reference to examples.

[0083] [Preparation of Thermosetting Composition and Cured Product] A siloxane compound (a) having at least two alkenyl groups per molecule was mixed with a predetermined amount of an aromatic polymer (b) having reactive functional groups, a thermal radical initiator (c), and an equal mass of toluene (d) to the amount of the aromatic polymer having reactive functional groups to prepare a homogeneous toluene solution. Using a rotary evaporator, more than 90% of the toluene in the solution was removed to prepare a transparent, high-concentration varnish. The varnish was sandwiched between two polyimide films and the toluene was completely removed over three hours in a vacuum press set at 100°C. The press was heated to 200°C for two hours, then further heated to 220°C for two hours, yielding a light brown cured product approximately 0.5 mm thick.

[0084] [Appearance of Thermosetting Composition] The thermosetting composition (the high-concentration varnish) was visually observed, and the appearance including transparency was evaluated.

[0085] [Mechanical properties of cured product: moldability] The practical toughness of the cured product was evaluated using the following three-point scale based on the presence or absence of cracks in the cured product sheet prepared by the above method and its shape retention ability due to stress when peeled from the polyimide (PI) film. A: No cracks were observed, and the shape retention was good when peeled from the PI film. B: Some cracks were observed, and cracks occurred when peeled from the PI film. C: The sheet cracked when peeled from the PI film, making it difficult to prepare a homogeneous test piece.

[0086] [Mechanical Properties of Cured Product: Tensile Modulus and Glass Transition Temperature] A test piece approximately 50 mm long and approximately 5 mm wide was cut out from the cured product sheet prepared by the above method to prepare a test piece for measurement. Using a dynamic viscoelasticity analyzer RSA-G2 manufactured by TA Instrument, dynamic viscoelasticity was measured in tension mode under the following conditions to determine the storage modulus (E': MPa) and glass transition temperature (Tg: C). Measurement conditions: Frequency: 1 Hz, strain: 0.1%, heating rate: 3°C / min

[0087] [Mechanical properties of cured product: elongation at break, strength at break, and toughness] Test pieces similar to those used for dynamic viscoelasticity measurement were prepared from the cured product sheets prepared by the method described above. The test pieces were elongated at 25°C and a tensile speed of 5 mm / min using an Autograph AGS-X manufactured by Shimadzu Corporation, and the elongation at break and strength at break were recorded. Toughness (kJ / m 3 ) was calculated by integrating the area under the stress-strain curve for every 0.004% elongation.

[0088] [Dielectric Constant and Dielectric Loss Tangent] A test piece approximately 80 mm long and approximately 1.5 mm wide was cut from the cured product sheet prepared by the above method to prepare a measurement test piece. The measurement test piece was placed in an oven at 80°C and dried for 1 hour. The relative dielectric constant (Dk) and dielectric loss tangent (Df) at 10 GHz were measured by the cavity resonance method using a network analyzer N5222B manufactured by Keysight Technologies and a cavity resonator (CP531) manufactured by Kanto Electronics Application Development Co., Ltd., under an environment of 23°C ± 2°C and a relative humidity of 50 ± 5%.

[0089] [Examples and Comparative Examples] Using the following components, thermosetting compositions were prepared according to the compositions shown in Table 1 (parts by mass, excluding the solvent toluene). "Me", "Vi", and "Ph" in component A represent a methyl group, a vinyl group, and a phenyl group, respectively. (A-1): (ViMe 2 SiO) 2 SiPh 2 Siloxane (A-2) represented by the formula: (ViMe 2 SiO) 3 Siloxane represented by SiPh (A-3): ViMe 2 Si (OSiMePh) n OSiMe 2 Linear polysiloxane represented by Vi (average degree of polymerization n: 28) (A-4): (ViMeSiO) 4 Siloxane (A-5): (ViMe 2 SiO) 4 Siloxane represented by Si (A-6)*: HO(ViMeSiO) nH (average degree of polymerization n: 12) (A-7)*: triallyl isocyanurate (manufactured by Fuji Film Wako Co., Ltd.) (A-8)*: polybutadiene (manufactured by Nippon Soda Co., Ltd., B-1000) (B-1): polyphenylene ether resin modified with methacrylate at both ends (manufactured by SABIC Corporation, SA9000) (C-1): di(2-t-butylperoxyisopropyl)benzene (manufactured by NOF Corporation, Perbutyl P) * (A-6) to (A-8) are main agents for comparative experiments.

[0090]

[0091] As shown in Table 1, the thermosetting composition of the present invention exhibited high transparency and also had good moldability. It was confirmed that the cured product obtained from the composition had a high glass transition temperature of 190°C or higher, excellent heat resistance, and the physical properties could be adjusted over a wide range. On the other hand, the cured product obtained from the composition exhibited high toughness, and the toughness of the cured products obtained in Examples 1 and 3 was 73 and 91 kJ / m, respectively. 3 Furthermore, the dielectric properties were also good, and in particular, the cured material made from the linear organopolysiloxane containing aryl groups exhibited an extremely low dielectric tangent, suggesting its usefulness as an insulating material for circuit boards in electric and electronic devices that operate in the high-frequency range.

[0092] On the other hand, a composition containing the industrially widely used crosslinking agent triallyl isocyanurate (Comparative Example 2) was found to have insufficient molding processability, and the resulting cured product had very low toughness. Similarly, compositions containing well-known high-molecular-weight crosslinking agents (Comparative Examples 1 and 3) were found to be opaque and to have insufficient molding processability due to poor compatibility between the components. Furthermore, a cured product obtained from a composition that did not contain a specific organopolysiloxane as a crosslinking component (Comparative Example 4) did not have a sufficiently high modulus of elasticity at high temperatures, and the dielectric loss tangent was relatively high.

[0093] [Synthesis Example: Synthesis of Cycloolefin Polymer (B-2)] 225 ml of dicyclopentadiene (containing approximately 10% cyclopentadiene trimer), 0.54 g of diethylaluminum chloride, 0.99 g of a 70% solution of 1,3-dichloro-2-propanol in dicyclopentadiene, 1.9 ml of a 0.6 mol / L solution of tridodecylammonium molybdate in dicyclopentadiene, and 0.84 ml of a 8.2% solution of benzylidenebis(tricyclohexylphosphine)ruthenium dichloride in dichloromethane were charged in this order using a syringe into a thoroughly nitrogen-purged glass reaction vessel and vigorously stirred for 10 seconds. This reaction solution was preheated to 60°C and placed in a U-shaped resin spacer (5 mm thick) designed to have an internal volume of 20 × 20 × 0.5 cm3, and press-molded for 5 minutes to obtain poly(dicyclopentadiene).

[0094] Example VII A thermosetting composition is obtained in the same manner as in Example 1, except that the component (B-1) in Example 1 is replaced with the same mass of poly(dicyclopentadiene) (B-2) obtained by the above Synthesis Example. The cured product obtained by curing the thermosetting composition in the same manner as in Example 1 is expected to have good dielectric properties, as well as excellent physical strength such as elasticity and moldability.

Claims

1. A thermosetting composition comprising: (A) 10 to 90 parts by mass of one or more siloxane compounds selected from (a1) and (a2) below: (a1) a linear siloxane having at least two alkenyl groups and at least one aryl group in the molecule; (a2) a siloxane having at least two alkenyl groups in the molecule and having 8 or less silicon atoms; (B) 10 to 90 parts by mass of at least one compound selected from aromatic polymers having reactive functional groups and cycloolefin polymers having reactive functional groups (wherein the sum of components (A) and (B) is 100 parts by mass); and (C) a thermal radical initiator in an amount of 0.1 to 5 parts by mass per 100 parts by mass of the combined total of components (A) and (B).

2. The thermosetting composition according to claim 1, wherein component (B) is a polyphenylene ether having reactive functional groups at the molecular chain terminals.

3. The thermosetting composition according to claim 1, wherein component (B) is a polyphenylene ether having at least one reactive functional group selected from an alkenyl group and a (meth)acrylate group at the molecular chain terminal.

4. The thermosetting composition according to claim 1, wherein component (A) is one or more siloxane compounds selected from the following (a1-1) and (a2-1): (a1-1) a linear siloxane having at least two alkenyl groups in the molecule and having an aryl group molar fraction of 20% or more in all substituents on silicon atoms; (a2-1) a cyclic siloxane having at least two alkenyl groups in the molecule and having 8 or less silicon atoms; 5. The thermosetting composition of claim 1, further comprising (D) an organic solvent.

6. A cured product of the thermosetting composition according to any one of claims 1 to 5.

7. A prepreg comprising a cured product of the thermosetting composition according to any one of claims 1 to 5 and a fibrous reinforcing material.

8. A high-frequency circuit board comprising a laminate of one or more sheets of the prepreg according to claim 7.

9. A method for curing and molding the thermosetting composition according to claim 5, comprising at least the steps of: step (i): removing component (D) from the thermosetting composition according to claim 5 at normal pressure or reduced pressure in the temperature range of about 80-100°C; and step (ii): curing the thermosetting composition at a temperature of 150°C or higher following step (i), and processing the composition into a desired shape.

10. A method for producing a prepreg, comprising impregnating the thermosetting composition of claim 5 with a fibrous reinforcing material, then removing component (D) and curing the thermosetting composition.

Citation Information

Patent Citations

  • Cross-linking composite material and its laminate

    JP2003012820A

  • Resin composition and its application to high frequency circuit board

    JP2016531959A

  • Polyphenylene ether resin composition and high-frequency circuit board using the same

    JP2018521210A

  • Polyphenylene ether resin composition and high-frequency circuit board using the same

    JP2018521211A

  • Resin composition, prepreg, laminated plate, multilayer printed wiring board and semiconductor package

    JP2020169275A