Lithium-sulfur battery

The lithium sulfur battery employs a sulfur-carbon composite and optimized electrolyte to maintain high output characteristics at elevated discharge rates, overcoming capacity and efficiency reductions, achieving 1,000 mAh/g specific capacity and 300 Wh/kg energy density at high C-rates.

WO2024242268A1PCT designated stage expired Publication Date: 2024-11-28LG ENERGY SOLUTION LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2023/020912
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-12-18
Filing Date
2023-12-18
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Lithium-sulfur batteries face a significant reduction in capacity and efficiency when discharge rates are increased, leading to inadequate energy release and reduced lifespan, particularly at high C-rates, which is a limitation for applications requiring high energy density and long cycle life.

Method used

The development of a lithium sulfur battery with a sulfur-carbon composite positive electrode active material, optimized electrolyte composition, and specific structural features that maintain high output characteristics by ensuring efficient conversion reactions even at high discharge rates, such as a sulfur/carbon weight ratio of 2.7 g/g or more and a non-aqueous solvent-based electrolyte, enhancing energy density and capacity retention.

Benefits of technology

The battery achieves a specific capacity of 1,000 mAh/g and energy density of 300 Wh/kg or more, even at 1.0C or higher discharge rates, maintaining performance comparable to lower rates, thus addressing the capacity retention issue and enhancing its suitability for high-energy applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2023020912_28112024_PF_FP_ABST
    Figure KR2023020912_28112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a lithium-sulfur battery and a method for evaluating the output characteristics of the lithium-sulfur battery, the lithium-sulfur battery comprising: a positive electrode; a negative electrode; a separator interposed between the positive electrode and the negative electrode; and an electrolyte, wherein the positive electrode includes a positive electrode active material containing a sulfur-carbon composite, and the lithium-sulfur battery has a ratio R(1.0C / 0.5C) of 80% or more according to relation 1. The lithium-sulfur battery has sufficient energy density and capacity even if discharged at a high rate. [Relation 1] R(1.0C / 0.5C) = [A(DOD 100)1.0C / A(DOD 100)0.5C] X 100 (%) In relation 1, A(DOD 100)1.0C is the amount of lithium sulfide (Li2S) that is discharged to 1.0C and is present in a DOD 100 state, and A(DOD 100)0.5C is the amount of lithium sulfide (Li2S) that is discharged to 0.5C and is present in a DOD 100 state.
Need to check novelty before this filing date? Find Prior Art

Description

lithium-sulfur battery

[0001] The present invention relates to a lithium-sulfur battery, and more particularly, to a lithium-sulfur battery exhibiting excellent capacity even at a high discharge rate.

[0002] This application claims priority to Korean Patent Application No. 2023-0066600, filed with the Korean Intellectual Property Office on May 23, 2023, the entire disclosure of which is incorporated herein by reference.

[0003] As the scope of application of lithium secondary batteries expands beyond portable electronic devices to include electric vehicles (EVs) and electric storage systems (ESS), the demand for lithium secondary batteries with high capacity, high energy density, and long lifespan is increasing.

[0004] Among various lithium secondary batteries, the lithium-sulfur battery is a battery system that uses a sulfur-based material containing a sulfur-sulfur bond as a positive electrode active material, and lithium metal, a carbon-based material in which lithium ions can be inserted / deinserted, or silicon or tin that forms an alloy with lithium as a negative electrode active material.

[0005] Sulfur, the main material of the cathode active material in lithium-sulfur batteries, has the advantages of being a low atomic weight, abundant in resources, easy to supply, inexpensive, non-toxic, and environmentally friendly material.

[0006] In addition, lithium-sulfur batteries have a conversion reaction between lithium ions and sulfur at the cathode (S8+16Li). + +16e --> The theoretical specific capacity from 8 Li2S) reaches 1,675 mAh / g, and when lithium metal is used as the negative electrode, it shows a theoretical energy density of 2,600 Wh / kg. This is a very high number compared to the theoretical energy density of other battery systems currently being studied (Ni-MH battery: 450 Wh / kg, Li-FeS battery: 480 Wh / kg, Li-MnO2 battery: 1,000 Wh / kg, Na-S battery: 800 Wh / kg) and lithium ion batteries (250 Wh / kg), and therefore, it is attracting attention as a high-capacity, eco-friendly, and low-cost lithium secondary battery among the secondary batteries being developed so far.

[0007] When a lithium-sulfur battery is discharged, sulfur (S8) at the positive electrode accepts electrons and goes through several stages of reduction reactions to form lithium polysulfide (LiPS, Li2S). x , x=2~8) and is finally converted to lithium sulfide (Li2S). At this time, it has a mechanism in which energy is released when converted to each substance.

[0008] Meanwhile, lithium-sulfur batteries are promising next-generation batteries for use in fields such as aviation where energy density is important. In order for lithium-sulfur batteries to exhibit high-output characteristics, the conversion of lithium polysulfide (LiPS) at all stages, specifically from Li2S8 to Li2S2, and the final stage, lithium sulfide (Li2S), must occur smoothly even at high discharge rates (C-rates). In particular, considering the properties required for a minimum usage time of approximately 30 minutes for a drone, the ability to release sufficient energy even during continuous discharge at a discharge rate of 2.0C may be required.

[0009] However, lithium-sulfur batteries currently under development are experiencing issues such as insufficient stepwise conversion reactions when the discharge rate is increased, resulting in significantly reduced capacity retention and reduced charge / discharge efficiency following repeated charge / discharge cycles. Consequently, lithium-sulfur batteries currently under development suffer from the problem of having lower capacities than their theoretical capacity when output is increased and discharge rates are increased.

[0010] Accordingly, there is a need to develop a lithium-sulfur battery that has sufficient capacity even at high discharge rates.

[0011] The present invention solves the above problems,

[0012] The aim is to provide a lithium-sulfur battery with excellent capacity retention even under high output conditions.

[0013] In particular, it is intended to provide a lithium-sulfur battery having excellent capacity retention even at a discharge rate (C-rate) of 1.0C or higher, for example, a discharge rate of 2.0C.

[0014] To solve the above problem,

[0015] According to one aspect of the present invention, a lithium sulfur battery of the following embodiments is provided.

[0016] A lithium sulfur battery according to the first embodiment,

[0017] A cathode; a positive electrode; and a separator interposed between the positive electrode and the negative electrode; and an electrolyte;

[0018] The above positive electrode has a positive electrode active material including a sulfur-carbon complex, and the lithium sulfur battery has a ratio R(1.0C / 0.5C) of 80% or more according to the following formula 1.

[0019] [Formula 1]

[0020] R(1.0C / 0.5C) = [A(DOD 100) 1.0 C / A(DOD 100) 0.5 C ] X 100 (%)

[0021] In the above equation 1,

[0022] Above A (DOD 100) 1.0 C is the amount of lithium sulfide (Li2S) present in the DOD 100 state when discharged at 1.0C.

[0023] Above A (DOD 100) 0.5 C is the amount of lithium sulfide (Li2S) present in a DOD 100 state when discharged at 0.5C.

[0024] According to the second embodiment, in the first embodiment,

[0025] The above R(1.0C / 0.5C) may be 85% or more.

[0026] According to the third embodiment, in the first embodiment or the second embodiment,

[0027] The above DOD 100 may be in a state having a potential of 1.7 V to 1.9 V.

[0028] According to the fourth embodiment, in any one of the first to third embodiments,

[0029] The above DOD 100 may be in a state having a potential of 1.8 V.

[0030] According to the fifth embodiment, in any one of the first to fourth embodiments,

[0031] The amount of the above lithium sulfide (Li2S) may be the weight, volume or mole number of the above lithium sulfide.

[0032] According to the sixth embodiment, in any one of the first to fifth embodiments,

[0033] The above ratio R(1.0C / 0.5C) is measured through the ratio of peak intensities of lithium sulfide (Li2S) on the X-ray diffraction spectrum for the lithium sulfur battery.

[0034] The above lithium sulfide (Li2S) has a scattering vector (q) = 1.85 to 1.92 Å on the X-ray diffraction spectrum. -1 It may have a characteristic peak in the area.

[0035] According to the seventh embodiment, in any one of the first to sixth embodiments,

[0036] The weight ratio of sulfur (S) in the electrolyte and the sulfur-carbon complex (El / S weight ratio) may be 2.7 g / g or more.

[0037] According to the eighth embodiment, in any one of the first to seventh embodiments,

[0038] The above electrolyte may include a non-aqueous solvent, a lithium salt, and an additive.

[0039] According to the ninth embodiment, in any one of the first to eighth embodiments,

[0040] The energy density of the above lithium sulfur battery may be 300 Wh / kg or more.

[0041] According to the tenth embodiment, in any one of the first to ninth embodiments,

[0042] The content of elemental sulfur (S) in the above sulfur-carbon complex may be 60 to 85 wt%.

[0043] According to the eleventh embodiment, in any one of the first to tenth embodiments,

[0044] The weight of the sulfur-carbon complex may be 90 wt% or more based on the total weight of the positive electrode.

[0045] According to the 12th embodiment, in any one of the 1st to 11th embodiments,

[0046] The above lithium sulfur battery may be a coin-type battery, a pouch-type battery, or a cylindrical battery.

[0047]

[0048] According to another aspect of the present invention, an evaluation method of the following embodiments is provided.

[0049] The evaluation method according to the 13th implementation example is:

[0050] A method for evaluating the output characteristics of a lithium sulfur battery comprising a cathode, a cathode, and a separator interposed between the cathode and the anode, and an electrolyte, wherein the cathode comprises a cathode active material including a sulfur-carbon complex,

[0051] A step of determining that a high-power lithium-sulfur battery is used when the ratio R(1.0C / 0.5C) according to the following formula 1 is 80% or more is included.

[0052] [Formula 1]

[0053] R(1.0C / 0.5C) = [A(DOD 100) 1.0 C / A(DOD 100) 0.5 C ] X 100 (%)

[0054] In the above equation 1,

[0055] Above A (DOD 100) 1.0 C is the amount of lithium sulfide (Li2S) present in the DOD 100 state when discharged at 1.0C.

[0056] Above A (DOD 100) 0.5 C is the amount of lithium sulfide (Li2S) present in a DOD 100 state when discharged at 0.5C.

[0057] According to the 14th embodiment, in the 13th embodiment,

[0058] The above high-power lithium-sulfur battery may be a battery that maintains an energy density of 300 Wh / kg or more under discharge conditions of 1.0 C-rate or more at room temperature.

[0059] According to the 15th embodiment, in the 13th embodiment or the 14th embodiment,

[0060] The above room temperature may be a temperature of 23°C to 25°C.

[0061] According to the 16th embodiment, in any one of the 13th to 15th embodiments,

[0062] Above A (DOD 100) x C (x=0.5 or 1.0) is obtained by discharging the lithium-sulfur battery at x C-rate and obtaining an X-ray diffraction spectrum at a DOD of 100, and the scattering vector (q)=1.85~1.92 Å on the obtained X-ray diffraction spectrum. -1 The peak intensity value in the region is measured, and the ratio R(1.0C / 0.5C) may be measured by calculating the ratio of each peak intensity obtained above.

[0063] A lithium-sulfur battery according to one aspect of the present invention has the advantage of having sufficient energy density and capacity even when discharged at a high C-rate.

[0064] Specifically, it can exhibit the effect of maintaining the energy density and capacity excellently when discharged at 0.5C even when discharged at a rate of 1.0C or higher.

[0065] In particular, the lithium-sulfur battery of the present invention can have a specific capacity of 1,000 mAh / g or more.

[0066] In particular, the lithium-sulfur battery of the present invention can have an energy density of 300 Wh / kg or more.

[0067] The following drawings attached to this specification illustrate preferred embodiments of the present invention and, together with the contents of the invention described above, serve to further understand the technical concept of the present invention. Therefore, the present invention should not be interpreted as being limited to the matters described in these drawings. Meanwhile, the shape, size, scale, or ratio of elements in the drawings included in this specification may be exaggerated to emphasize a clearer explanation.

[0068] Figure 1 is a discharge C-rate-energy density graph of the lithium-sulfur batteries of Example 1, Example 2, and Comparative Example 1.

[0069] Figure 2 is a specific capacity-voltage graph of the lithium sulfur batteries of Example 1, Example 2, and Comparative Example 1.

[0070] Figure 3 is a graph showing the nominal voltage at 0.5 C-rate discharge and 1.0 C-rate discharge of the lithium-sulfur batteries of Example 1, Example 2, and Comparative Example 1.

[0071] Figure 4 is a graph showing the amount of Li2S produced when the lithium-sulfur batteries of Example 1, Example 2, and Comparative Example 1 were discharged at a 0.5 C-rate.

[0072] Figure 5 is a graph showing the amount of Li2S produced when the lithium-sulfur batteries of Example 1, Example 2, and Comparative Example 1 were discharged at 1.0 C-rate.

[0073] Hereinafter, the present invention will be described in more detail.

[0074] Terms or words used in this specification and claims should not be interpreted as limited to their usual or dictionary meanings, but should be interpreted as meanings and concepts that conform to the technical idea of ​​the present invention, based on the principle that the inventor can appropriately define the concept of the term to explain his or her own invention in the best way.

[0075] The terminology used in the present invention is only used to describe specific embodiments and is not intended to limit the present invention. The singular expression includes the plural expression unless the context clearly indicates otherwise. It should be understood that the terms "comprise" or "have" in the present invention are intended to specify the presence of a feature, number, step, operation, component, part, or combination thereof described in the specification, but do not exclude in advance the possibility of the presence or addition of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.

[0076] Additionally, throughout the specification, whenever a part is said to "include," "comprise," "have," or "have" a component, this does not mean that it excludes other components, but rather that it may include other components, unless otherwise specifically stated.

[0077] Throughout this specification, references to 'A and / or B' mean 'A or B or both.'

[0078] Throughout this specification, "C-rate" refers to the current rate, which is a value indicating the speed at which a battery is charged or discharged. Throughout this specification, the "C-rate" may also be abbreviated as "C."

[0079] Throughout this specification, unless otherwise specified, temperature means Celsius temperature, and the unit is ℃.

[0080] The term "composite" used in this specification refers to a material in which two or more materials are combined to form physically and chemically different phases and exhibit more effective functions.

[0081] The term "(poly)sulfide" as used herein means "(poly)sulfide ion (S x 2- , 1≤ x ≤ 8)" and "lithium (poly)sulfide (Li2S x or Li2S x - It is a concept that includes all of 1≤ x ≤ 8).

[0082] The term "polysulfide" as used herein means "polysulfide ion (S x 2- , 1< x ≤ 8)" and "lithium (poly)sulfide (Li2S x or Li2S x - It is a concept that includes all of "1< x ≤ 8").

[0083] Lithium-sulfur batteries release energy when the starting material, sulfur (S8), is converted to lithium polysulfide (LiPS) and then lithium sulfide (Li2S) during discharge of the positive electrode.

[0084] According to one aspect of the present invention, a lithium-sulfur battery is provided in which the above conversion reaction is stably implemented even when discharged at a high discharge rate.

[0085]

[0086] According to one aspect of the present invention, a lithium-sulfur battery comprises a positive electrode; a negative electrode; and a separator interposed between the positive electrode and the negative electrode; and an electrolyte; wherein the positive electrode comprises a positive electrode active material including a sulfur-carbon complex.

[0087] At this time, the amount of Li2S generated when the lithium-sulfur battery is discharged to a depth of discharge (DOD) of 100 at a 1.0 C-rate is 80% or more than the amount of Li2S generated when the battery is discharged to a depth of discharge (DOD) of 100 at a 0.5 C-rate.

[0088] In one embodiment of the present invention, the lithium-sulfur battery may have an amount of Li2S generated when discharged to a depth of discharge (DOD) of 100 at a 1.0 C-rate that is 85% or more of the amount of Li2S generated when discharged to a depth of discharge (DOD) of 100 at a 0.5 C-rate.

[0089] In one embodiment of the present invention, the sulfur-carbon complex may include at least one of sulfur and sulfur-based compounds. Here, sulfur-based compounds collectively refer to substances containing elemental sulfur (S).

[0090] When the above sulfur-carbon complex contains sulfur (S8), lithium polysulfide is formed in the lithium-sulfur battery through a reduction reaction at the positive electrode during discharge. If the formed lithium polysulfide is dissolved by the electrolyte and eluted from the positive electrode into the electrolyte phase, the amount of lithium polysulfide oxidized at the positive electrode during charging of the lithium-sulfur battery decreases, which may result in a decrease in the capacity of the lithium-sulfur battery.

[0091] The above sulfur-containing compound may include, for example, all sulfur-containing compounds that can be formed through a reduction reaction of inorganic sulfur (S8) or an oxidation reaction of lithium sulfide (Li2S), and more specifically, lithium sulfide (Li2S), lithium polysulfide (Li2Sx, 1 < x ≤8), disulfide compounds, carbon-sulfur polymers ((C2S y ) n , y = 2.5 to 50, 2≤ n), or two or more of these.

[0092] However, when a lithium-sulfur battery contains inorganic sulfur (S8) as a positive electrode active material, lithium polysulfide (Li2Sx, 1 < x ≤ 8) is formed by a reduction reaction of sulfur at the positive electrode when the lithium-sulfur battery is discharged, and the lithium polysulfide is reduced again to lithium sulfide (Li2S). However, when the lithium-sulfur battery is discharged at a high C-rate, the reduction reaction does not proceed properly, so the amount of lithium polysulfide (Li2S) generated during discharge decreases, which causes a serious decrease in capacity.

[0093] In this way, when conventional lithium-sulfur batteries are discharged at a high C-rate, the efficiency of the reduction reaction of the positive electrode is low, which causes a decrease in the capacity of the battery.

[0094] However, a lithium-sulfur battery according to one aspect of the present invention has an advantage in that, when discharged to DOD 100 at 1.0 C-rate, the amount of Li2S produced is 80% or more, specifically 85% or more, compared to when discharged to DOD 100 at 0.5 C-rate, so that even when discharged at a high C-rate, the decrease in capacity is less than when discharged at a low C-rate.

[0095] In this specification, the DOD 100 indicates a state in which the depth of discharge is 100% based on a full charge state, i.e., a state of SOC (state of charge) 100%, i.e., a completely discharged state. In other words, it can indicate SOC 0%.

[0096] In one embodiment of the present invention, the DOD 100 may be in a state having a potential of, for example, 1.7 V to 1.9 V, and specifically, may be in a state having a potential of 1.8 V, but the present invention is not limited thereto.

[0097] Specifically, a lithium-sulfur battery having a ratio R (1.0C / 0.5C) of lithium sulfide (Li2S) of 80% or more according to Equation 1 below can exhibit the effect of having high output characteristics.

[0098] [Formula 1]

[0099] R(1.0C / 0.5C) = [A(DOD 100) 1.0 C / A(DOD 100) 0.5 C ] X 100 (%)

[0100] In the above equation 1,

[0101] Above A (DOD 100) 1.0 C is the amount of lithium sulfide present in a discharged state up to DOD 100 at 1.0C.

[0102] Above A (DOD 100) 0.5 C is the amount of lithium sulfide present when the battery is discharged to DOD 100 at 0.5C.

[0103] According to the above equation 1, the ratio of the amount of lithium sulfide generated in a lithium-sulfur battery at a fully discharged state at a rate of 1.0C, that is, at a state of discharge to DOD 100, and the amount of lithium sulfide generated in a lithium-sulfur battery at a fully discharged state at a rate of 0.5C can be derived. At this time, the higher the ratio, the higher the S8->Li2S of the positive electrode active material at a high output state. x (x=2~8)->It can be shown that the conversion efficiency of Li2S (lithium sulfide) is maintained excellently.

[0104] In one embodiment of the present invention, the ratio R(1.0C / 0.5C) of the lithium sulfide (Li2S) may be specifically 88% or more or 90% or more. For example, the ratio R(1.0C / 0.5C) of the lithium sulfide (Li2S) may be 80% to 100%, 85% to 100%, 88% to 99%, 90% to 95%, 85% to 93%, 88% to 93%, 90% to 93%, or 91% to 93%.

[0105] In the present specification, the amount of lithium sulfide (Li2S) may be expressed by weight, volume, or mole. In order to measure the ratio, the A(DOD 100) 1.0 C and A (DOD 100) 0.5 C As long as the measurement is based on the same standard, there is no particular limitation on whether the 'quantity' is weight, volume or mole.

[0106] In one embodiment of the present invention, the amount of Li2S in the lithium-sulfur battery in the discharged state may be measured by a method of analyzing the amount of Li2S in the battery by disassembling the battery, i.e., by a destructive method. However, it may be preferable to measure it by a non-destructive method in terms of preventing loss of Li2S in the battery and shortening the analysis time.

[0107] For example, the amount of Li2S in the lithium-sulfur battery in the discharged state can be measured through non-destructive X-ray diffraction (XRD) analysis. Specifically, the Li2S has a scattering vector (q) of 1.85 to 1.92 Å in the spectrum obtained through X-ray diffraction analysis. -1 It has a specific peak in the region of . Accordingly, the scattering vector (q) = 1.85~1.92 Å in the XRD patterns for the lithium-sulfur battery in the discharged state up to DOD 100 at different discharge rates. -1 The ratio of the amount of Li2S can be measured through the ratio of peak intensities (i.e., scattering intensities) in the human region.

[0108] Accordingly, in one embodiment of the present invention, the ratio R(1.0C / 0.5C) is measured through the ratio of peak intensities of lithium sulfide (Li2S) on the X-ray diffraction spectrum for the lithium sulfur battery, and the lithium sulfide (Li2S) has a scattering vector (q)=1.85~1.92 Å on the X-ray diffraction spectrum. -1 It may have a characteristic peak in the area.

[0109] In one embodiment of the present invention, the A (DOD 100) x C (x=0.5 or 1.0) is obtained by discharging the lithium-sulfur battery at x C-rate and obtaining an X-ray diffraction spectrum at a DOD of 100, and the scattering vector (q)=1.85~1.92 Å on the obtained X-ray diffraction spectrum. -1 It can be measured through the peak intensity value in the region. That is, the lithium-sulfur battery is discharged at 0.5 C-rate to obtain an X-ray diffraction spectrum in a DOD 100 state, and the scattering vector (q) = 1.85~1.92 Å on the obtained X-ray diffraction spectrum. -1 The peak intensity value in the region A (DOD 100) 0.5 C, and the lithium-sulfur battery was discharged at 1.0 C-rate to obtain an X-ray diffraction spectrum in a DOD 100 state, and the scattering vector (q) = 1.85 to 1.92 Å on the obtained X-ray diffraction spectrum. -1 The peak intensity value in the region A (DOD 100) 1.0 C By substituting in , the ratio of each peak intensity obtained above can be calculated to measure the ratio R(1.0C / 0.5C).

[0110] In one embodiment of the present invention, the X-ray diffraction spectrum can be obtained by irradiating the lithium sulfur battery with X-rays having a wavelength (λ) of 0.7 to 0.8 Å at room temperature.

[0111] In one embodiment of the present invention, the X-ray diffraction spectrum can be obtained by irradiating the lithium sulfur battery with X-rays having a wavelength (λ) of 0.709 Å at room temperature.

[0112] Specifically, the XRD analysis can be obtained through real-time X-ray diffraction (Operando X-ray diffraction, Operando XRD) analysis during operation. More specifically, the XRD pattern can be obtained by measuring the range of 2theta (2θ) 4 - 17° in transmission mode using Mo K-alpha X-ray (λ = 0.709 Å) of PANalyical Empyrean XRD at room temperature (23°C). At this time, one pattern can be obtained at 0.014° intervals for a total of 1 minute.

[0113] The ratio of the amount of Li2S in each discharge state measured according to the above method is measured, and a lithium-sulfur battery having the ratio of 80% or more, specifically 85% or more, can be defined as a lithium-sulfur battery having high output characteristics.

[0114]

[0115] Next, each component of the lithium sulfur battery will be described in detail.

[0116] anode

[0117] In one embodiment of the present invention, the positive electrode may include a positive electrode current collector and a positive electrode active material layer applied to one or both surfaces of the positive electrode current collector.

[0118] The above-mentioned positive electrode current collector supports the positive electrode active material and is not particularly limited as long as it has high conductivity without causing chemical changes in the battery. For example, copper, stainless steel, aluminum, nickel, titanium, palladium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, silver, etc., aluminum-cadmium alloy, etc. can be used.

[0119] The above positive electrode current collector can form fine irregularities on its surface to strengthen the bonding strength with the positive electrode active material, and can be used in various forms such as a film, sheet, foil, mesh, net, porous body, foam, and non-woven fabric.

[0120] The above positive electrode active material layer includes a positive electrode active material and may further include a conductive material, a binder, and additives.

[0121] In one embodiment of the present invention, the positive electrode active material comprises a sulfur-carbon complex.

[0122] In one embodiment of the present invention, the sulfur-carbon composite may include a porous carbon material; and a sulfur-based compound supported on at least one of the inside of the pores of the porous carbon material and the outer surface of the porous carbon material. In the case of sulfur acting as the positive electrode active material, since it does not have electrical conductivity alone, it is used in a composite with a conductive material such as a carbon material, and a porous carbon material may be used to support sulfur. In addition, the sulfur-based compound is added as the positive electrode active material, and for example, inorganic sulfur (S8), lithium sulfide (Li2S), lithium polysulfide (Li2Sx, 1 < x ≤ 8), a disulfide compound, a carbon-sulfur polymer ((C2S) y) n , y = 2.5 to 50, 2≤n), lithium sulfide (Li2S), or two or more thereof. Preferably, the sulfur-based compound may be inorganic sulfur (S8).

[0123] In one embodiment of the present invention, the porous carbon material is used to support a sulfur-based compound as a positive electrode active material, and to provide a framework in which the sulfur-based compound can be uniformly and stably fixed, while improving the conductivity of the positive electrode. Any porous carbon material can be used without particular limitation in its type.

[0124] The above porous carbon material can generally be manufactured by carbonizing precursors of various carbon materials. The porous carbon material includes pores that are not regular therein, and the average diameter of the pores ranges from 1 to 200 nm, and the porosity can range from 10 to 90 volume% of the total volume of the porous carbon material. If the average diameter of the pores is less than the above range, the pore size is only at the molecular level, making sulfur impregnation impossible. Conversely, if it exceeds the above range, the mechanical strength of the porous carbon material is weakened, making it undesirable for application to the electrode manufacturing process.

[0125] In one embodiment of the present invention, the 'average pore diameter' can be measured according to a method known in the art for measuring the pore diameter of a porous material, and the measuring method is not particularly limited. For example, the pore diameter can be measured according to a scanning electron microscope (SEM), a field emission electron microscope (laser diffraction method), a laser diffraction method, or the BET (Brunauer-Emmett-Teller) method. The measurement using the laser diffraction method can be, for example, using a commercially available laser diffraction particle size measuring device (for example, Microtrac MT 3000). In addition, the measurement according to the BET method can be, for example, using an analyzer of the BELSORP series of BEL Japan, but is not limited thereto.

[0126] In one embodiment of the present invention, the 'porosity' refers to the ratio of the volume occupied by pores to the total volume of a structure, and uses % as its unit, and can be used interchangeably with terms such as porosity and porosity. In the present invention, the measurement of the porosity is not particularly limited, and according to one embodiment of the present invention, for example, it can be measured according to the BET method using nitrogen gas or the mercury penetration method (Hg porosimeter) and ASTM D2873.

[0127] The shape of the above porous carbon material may be spherical, rod-shaped, needle-shaped, plate-shaped, tubular or bulk-shaped, and can be used without limitation as long as it is a shape commonly used in lithium-sulfur batteries.

[0128] The porous carbon material may be any material commonly used in the art that has a porous structure or a high specific surface area. For example, the porous carbon material may be at least one selected from the group consisting of graphite; graphene; carbon black such as Denka black, acetylene black, Ketjen black, channel black, furnace black, lamp black, and summer black; carbon nanotubes (CNTs) such as single-walled carbon nanotubes (SWCNTs) and multi-walled carbon nanotubes (MWCNTs); carbon fibers such as graphite nanofibers (GNFs), carbon nanofibers (CNFs), and activated carbon fibers (ACFs); and graphite and activated carbon such as natural graphite, artificial graphite, and expanded graphite, but is not limited thereto. Preferably, the porous carbon material may be a carbon nanotube.

[0129] In one embodiment of the present invention, the porous carbon material may include, for example, carbon nanotubes (CNTs).

[0130] In one embodiment of the present invention, the sulfur-carbon complex may have a sulfur / carbon weight ratio (S / C weight ratio) of, for example, 5 g / g or less, and more specifically, 2.5 g / g or less. For example, the sulfur-carbon complex may have a sulfur / carbon weight ratio of 2.4 g / g. When the S / C ratio of the sulfur-carbon complex is within the above-described range, it may be preferable in terms of securing the electron transfer ability (conductivity) and electrochemical specific surface area of ​​the sulfur-carbon complex, and for example, it may be preferable in suppressing the elution of sulfur from the anode by increasing the usable surface area of ​​the sulfur-carbon complex, but the present invention is not limited thereto.

[0131] The method for manufacturing the above sulfur-carbon composite is not particularly limited in the present invention, and any method commonly used in the art may be used. For example, a method may be used in which the sulfur and porous carbon material are simply mixed and then heat-treated to form a composite.

[0132] In addition to the composition described above, the positive electrode active material may further include one or more selected from among a transition metal element, a group ⅢA element, a group ⅥA element, a sulfur compound of these elements, and an alloy of these elements and sulfur.

[0133] The above transition metal elements include Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Os, Ir, Pt, Au or Hg, etc., the above group ⅢA elements include Al, Ga, In, Ti, etc., and the above group ⅥA elements may include Ge, Sn, Pb, etc.

[0134] In one embodiment of the present invention, the sulfur-carbon complex may be at least 50 wt% based on the total weight of the positive electrode. Specifically, the sulfur-carbon complex may be at least 80 wt%, at least 90 wt%, or at least 95 wt% based on the total weight of the positive electrode active material layer. Specifically, the sulfur-carbon complex may be included in an amount of 80 wt% to 100 wt%, more specifically 85 wt% to 99 wt%, 90 wt% to 99 wt%, 95 wt% to 98 wt%, or 95 wt% to 97 wt%, or 96 wt% based on the total weight of the positive electrode active material layer. If the content of the above sulfur-carbon complex is below the above range, the relative content of auxiliary materials such as conductive material and binder increases and the content of the sulfur-carbon complex decreases, making it difficult to implement a high-capacity, high-energy-density battery. Conversely, if it exceeds the above range, the content of the conductive material or binder described below is relatively insufficient, causing a problem in that the physical properties of the electrode deteriorate.

[0135] The above conductive material is a material that electrically connects the electrolyte and the positive electrode active material and serves as a path for electrons to move from the current collector to the positive electrode active material. Any conductive material that is physically distinct from the carbon contained in the sulfur-carbon complex and is a component of the electrode can be used without limitation.

[0136] In one embodiment of the present invention, the conductive material may be, for example, carbon black such as Super-P, Denka black, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, carbon black; carbon derivatives such as carbon nanotubes or fullerene; conductive fibers such as carbon fibers or metal fibers; metal powders such as fluorocarbon, aluminum, and nickel powder; or conductive polymers such as polyaniline, polythiophene, polyacetylene, and polypyrrole, which may be used alone or in combination.

[0137] In one embodiment of the present invention, the content of the conductive material may be 0 to 10 wt%, for example, 1 to 10 wt%, based on the total weight of the positive electrode active material. If the content of the conductive material is less than the above range, electron transfer between the positive electrode active material and the current collector may not be easy, which may result in a decrease in voltage and capacity. Conversely, if the content exceeds the above range, the proportion of the positive electrode active material may relatively decrease, which may result in a decrease in the total energy (charge) of the battery. Therefore, it is preferable to determine an appropriate content within the above-described range.

[0138] In one embodiment of the present invention, the positive electrode may include a positive electrode active material and a binder polymer, and may not include a conductive material. That is, the positive electrode may not include a conductive material other than the porous carbon material of the sulfur-carbon composite included in the positive electrode active material. Since the positive electrode may include more positive electrode active material as it does not include a conductive material, the energy density and / or capacity of the lithium-sulfur battery may be improved.

[0139] The above binder polymer maintains the positive electrode active material on the positive electrode current collector and organically connects the positive electrode active materials to further increase the bonding strength between them. Any binder polymer known in the industry can be used.

[0140] For example, the binder polymer may be a fluororesin binder including polyvinylidene fluoride (PVdF) or polytetrafluoroethylene (PTFE); a rubber binder including styrene butadiene rubber (SBR), acrylonitrile-butidiene rubber, styrene-isoprene rubber, etc.; a cellulose binder including carboxyl methyl cellulose (CMC), starch, hydroxy propyl cellulose, regenerated cellulose, etc.; a polyalcohol binder; a polyolefin binder including polyethylene, polypropylene, etc.; a polyimide binder; a polyester binder; a polyacrylic binder such as polyacrylic acid (PAA); a silane binder; a polyurethane binder; Or it may include a mixture of two or more of these, and further, the binder polymer may include a copolymer having repeating units derived from two or more of these binders.

[0141] The content of the above binder polymer may be 0.5 to 30 wt% based on 100 wt% of the total positive electrode active material layer. When the content of the above binder polymer satisfies this range, the physical properties of the positive electrode are improved, so that the phenomenon of the active material and conductive material within the positive electrode being detached can be prevented, and the ratio of the active material and conductive material in the positive electrode can be appropriately controlled, so that the battery capacity can be secured.

[0142] In the present invention, the method for manufacturing the positive electrode for the lithium secondary battery is not particularly limited, and various methods known to those skilled in the art or modified methods thereof can be used.

[0143] For example, the positive electrode for the lithium secondary battery may be manufactured by forming the positive electrode active material layer by preparing a positive electrode slurry composition including the composition described above and then applying the same to at least one surface of the positive electrode current collector.

[0144] The above positive electrode slurry composition includes the positive electrode active material described above, and may further include a binder, a conductive material, and a solvent.

[0145] The above solvent is one that can uniformly disperse the positive electrode active material. Water is most preferably an aqueous solvent, and the water may be distilled or deionized water. However, this is not necessarily limited to this, and if necessary, a lower alcohol that is easily mixed with water may be used. Examples of the lower alcohol include methanol, ethanol, propanol, isopropanol, and butanol, and preferably, these can be mixed with water and used.

[0146] The content of the above solvent may be contained at a level that has a concentration that can facilitate coating, and the specific content varies depending on the application method and device.

[0147] The above-mentioned positive electrode slurry composition may additionally contain, as necessary, substances commonly used in the relevant technical field for purposes such as improving its function. Examples thereof include viscosity modifiers, fluidizing agents, and fillers.

[0148] The method for applying the positive electrode slurry composition is not particularly limited in the present invention, and may include, for example, bar coating, doctor blade, die casting, comma coating, screen printing, dip, reverse roll, direct roll, gravure, or extrusion. In addition, the slurry may be applied onto a separate substrate to form a positive electrode active material layer, and then the positive electrode active material layer may be attached onto the positive electrode current collector by pressing or lamination.

[0149] The amount of the positive electrode slurry composition applied on the above-mentioned collector is not particularly limited, and can be controlled in consideration of the final desired thickness of the positive electrode active material layer.

[0150] After the above application, a drying process for solvent removal can be performed. The drying process is performed at a temperature and time that can sufficiently remove the solvent, and the conditions may vary depending on the type of solvent and are therefore not particularly limited to the present invention. Examples include drying using warm air, hot air, low-humidity air, vacuum drying, and drying using irradiation with (far) infrared rays and electron beams. The drying speed is usually adjusted to remove the solvent as quickly as possible within a speed range that does not cause cracks in the positive electrode active material layer due to stress concentration or cause the positive electrode active material layer to peel off from the positive electrode current collector.

[0151] Additionally, the density of the positive electrode active material within the positive electrode can be increased by pressing the entire body after drying. Pressing methods include mold pressing and roll pressing.

[0152] The porosity of the positive electrode, specifically the positive electrode active material layer, manufactured using the composition and manufacturing method described above may be 50 to 80% by volume, specifically 60 to 75% by volume.

[0153] When the porosity of the positive electrode satisfies 50 to 80 volume%, the filling degree of the positive electrode active material layer including the positive electrode active material, the conductive agent, and the binder is appropriately maintained, so that sufficient electrolyte capable of exhibiting ionic and / or electrical conduction can be maintained between the positive electrode active materials, the output characteristics or cycle characteristics of the battery can be improved, problems of overvoltage and discharge capacity reduction of the battery can be prevented, and physical and electrical connection with the current collector can be secured, so that the adhesive strength is improved, and the energy density of the battery can be improved.

[0154] In one embodiment of the present invention, the positive electrode has a capacity of 2 to 5 mAh / cm2 It may have a sulfur (S) loading amount. For example, the sulfur (S) loading amount of the positive electrode may be 2 to 4 mAh / cm 2 , 2.5 to 4 mAh / cm 2 , 2.5 to 3.5 mAh / cm 2 or 2.5 to 3.0 mAh / cm 2 However, the present invention is not limited thereto.

[0155]

[0156] cathode

[0157] In one embodiment of the present invention, the negative electrode may be a current collector-free type that does not include a current collector and is composed only of a negative electrode active material layer, or may be a type that includes a negative electrode current collector and a negative electrode active material layer formed on at least one surface of the negative electrode current collector.

[0158] In one embodiment of the present invention, the negative electrode may include a negative electrode current collector and a negative electrode active material layer applied to one or both surfaces of the negative electrode current collector. Alternatively, the negative electrode may be a lithium metal plate.

[0159] The above negative electrode current collector is for supporting the negative electrode active material layer, as described in the positive electrode current collector.

[0160] The above-mentioned negative electrode active material layer may include a conductive material, a binder, etc. in addition to the negative electrode active material. In this case, the conductive material and the binder follow the above-mentioned.

[0161] The above negative active material is lithium (Li + ) can be reversibly intercalated or deintercalated, a material that can react with lithium ions to form a reversibly lithium-containing compound, or a lithium metal or a lithium alloy.

[0162] The above lithium ion (Li +) can be reversibly inserted or de-inserted, for example, crystalline carbon, amorphous carbon, or a mixture thereof. The lithium ion (Li + ) can be, for example, tin oxide, titanium nitrate or silicon. The lithium alloy can be, for example, an alloy of lithium (Li) and a metal selected from the group consisting of sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), francium (Fr), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), radium (Ra), aluminum (Al) and tin (Sn).

[0163] According to one embodiment of the present invention, the negative electrode active material may be lithium metal, and specifically, may be in the form of a lithium metal thin film or lithium metal powder.

[0164] Preferably, the negative active material may be lithium metal, and specifically, may be in the form of a lithium metal thin film or lithium metal powder.

[0165] In one embodiment of the present invention, the negative electrode may have a thickness of 40 to 80 μm. For example, the thickness of the negative electrode may be 50 to 70 μm, or 60 μm. The thickness of the negative electrode may be measured using a known means for measuring the thickness of each component of the battery, and may be measured using, for example, a thickness measuring device from Mitutoyo, but is not limited thereto.

[0166]

[0167] membrane

[0168] The above separator separates or insulates the positive and negative electrodes from each other and enables lithium ion transport between the positive and negative electrodes. Any separator typically used in lithium-sulfur batteries may be used without any particular limitations. For example, it may be made of a porous non-conductive or insulating material. In particular, the separator may be an independent member such as a film, or may be a coating layer added to the positive and / or negative electrodes.

[0169] In one embodiment of the present invention, it may be preferable that the separator have low resistance to ion movement of the electrolyte and excellent moisture absorption capacity for the electrolyte.

[0170] In one embodiment of the present invention, the separator may include a porous substrate, and any porous substrate typically used in secondary batteries may be used as the porous substrate, and a porous polymer film may be used alone or in a laminated manner. For example, a nonwoven fabric or a polyolefin porous film made of high-melting-point glass fiber, polyethylene terephthalate fiber, etc. may be used, but is not limited thereto.

[0171] The material of the porous substrate is not particularly limited in the present invention, and any porous substrate commonly used in electrochemical devices can be used. For example, the porous substrate may be a polyolefin such as polyethylene, polypropylene, etc., a polyester such as polyethyleneterephthalate, polybutyleneterephthalate, polyamide, polyacetal, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenyleneoxide, polyphenylenesulfide, polyethylenenaphthalate, polytetrafluoroethylene, polyvinylidene fluoride, polyvinyl chloride, polyacrylonitrile, cellulose, nylon, It may include at least one material selected from the group consisting of poly(p-phenylene benzobisoxazole) and polyarylate.

[0172] In one embodiment of the present invention, the thickness of the porous substrate is not particularly limited, but may be 1 to 100 μm, preferably 5 to 50 μm. The thickness range of the porous substrate is not limited to the above-mentioned range, but if the thickness is excessively thinner than the above-mentioned lower limit, the mechanical properties may deteriorate, and the separator may be easily damaged during battery use.

[0173] In one embodiment of the present invention, the average diameter and porosity of the pores present in the porous substrate are not particularly limited, but may be 0.001 to 50 ㎛ and 10 to 95 volume%, respectively.

[0174] In one embodiment of the present invention, the separator may further include a porous coating layer formed on at least one surface of the porous substrate and including inorganic particles and a binder.

[0175] In one embodiment of the present invention, the inorganic particles and binder included in the porous coating layer may be used without particular limitation as long as they are commonly used in the porous coating layer of a separation membrane, and the manufacturing method thereof is also not particularly limited.

[0176]

[0177] electrolyte

[0178] The above electrolyte comprises a non-aqueous solvent as a medium through which ions involved in the electrochemical reaction of a lithium-sulfur battery can move and a lithium salt as an electrolyte.

[0179] The above electrolyte is not particularly limited as long as it has a composition that can be used in a lithium secondary battery, specifically a lithium-sulfur battery.

[0180] In one embodiment of the present invention, the electrolyte may include a non-aqueous solvent, a lithium salt, and an additive.

[0181] In one embodiment of the present invention, the non-aqueous solvent may be used without particular limitation as long as it is of a type that can be used in a lithium-sulfur battery, and for example, ether solvents, esters, amides, linear carbonates, and cyclic carbonates may be used.

[0182] In one embodiment of the present invention, the ester may be, for example, one selected from the group consisting of methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, γ-valerolactone, γ-caprolactone, σ-valerolactone, and ε-caprolactone, or a mixture of two or more thereof, but is not limited thereto.

[0183] In one embodiment of the present invention, the linear carbonate may be, for example, one selected from the group consisting of dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethylmethyl carbonate, methylpropyl carbonate, and ethylpropyl carbonate, or a mixture of two or more thereof, but is not limited thereto.

[0184] In one embodiment of the present invention, the cyclic carbonate is, for example, one selected from the group consisting of ethylene carbonate, propylene carbonate, 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate, vinylene carbonate, vinylethylene carbonate, and halogenides thereof, or a mixture of two or more thereof. Examples of the halogenides thereof include, but are not limited to, fluoroethylene carbonate.

[0185] In one embodiment of the present invention, the non-aqueous solvent may include an ether solvent.

[0186] In one embodiment of the present invention, the ether solvent may be included in an amount of 60% by volume or more, for example, 60% by volume to 100% by volume, 70% by volume to 100% by volume, 80% by volume to 100% by volume, 85% by volume to 100% by volume, 90% by volume to 100% by volume, 95% by volume to 100% by volume, 98% by volume to 100% by volume, 90% by volume to 98% by volume, or 90% by volume to 95% by volume, based on the total volume of the non-aqueous solvent. When the amount of the ether solvent is in the above-described range based on the total volume of the non-aqueous solvent, an advantageous effect may be exhibited in terms of the solubility of an electrolyte composition such as a lithium salt, but the present invention is not limited thereto.

[0187] In one embodiment of the present invention, the ether solvent may include an acyclic ether, a cyclic ether, or a mixture thereof.

[0188] In one embodiment of the present invention, the acyclic ether is selected from the group consisting of, for example, dimethyl ether, diethyl ether, dipropyl ether, dibutyl ether, diisobutyl ether, ethyl methyl ether, ethylpropyl ether, ethyl tertbutyl ether, dimethoxymethane, trimethoxymethane, dimethoxyethane, diethoxyethane, dimethoxypropane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, ethylene glycol divinyl ether, diethylene glycol divinyl ether, triethylene glycol divinyl ether, dipropylene glycol dimethylene ether, butylene glycol ether, diethylene glycol ethylmethyl ether, diethylene glycol isopropylmethyl ether, diethylene glycol butylmethyl ether, diethylene glycol tertbutylethyl ether, and ethylene glycol ethylmethyl ether. It may include one or more kinds. Preferably, it may include one or more kinds selected from the group consisting of dimethyl ether, dimethoxyethane, diethoxyethane, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, and tetraethylene glycol dimethyl ether, and more preferably, it may include dimethoxyethane.

[0189] In one embodiment of the present invention, the cyclic ether is, for example, 2-methylfuran, 1,3-dioxolane, 4,5-dimethyl-dioxolane, 4,5-diethyl-dioxolane, 4-methyl-1,3-dioxolane, 4-ethyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, 2,5-dimethyltetrahydrofuran, 2,5-dimethoxytetrahydrofuran, 2-ethoxytetrahydrofuran, 2-methyl-1,3-dioxolane, 2-vinyl-1,3-dioxolane, 2,2-dimethyl-1,3-dioxolane, 2-methoxy-1,3-dioxolane, 2-ethyl-2-methyl-1,3-dioxolane, tetrahydropyran, 1,4-dioxane, It may include at least one selected from the group consisting of 1,2-dimethoxybenzene, 1,3-dimethoxybenzene, 1,4-dimethoxybenzene, and isosorbide dimethyl ether. Preferably, it may include at least one selected from the group consisting of 2-methylfuran, 1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, and 2,5-dimethyltetrahydrofuran, and more preferably, it may include 2-methylfuran.

[0190] In one embodiment of the present invention, the non-aqueous solvent may include a mixture of an acyclic ether and a cyclic ether.

[0191] In one embodiment of the present invention, the non-aqueous solvent may include dimethoxyethane (DME) and 2-methylfuran (2-MeF).

[0192] In one embodiment of the present invention, the volume ratio of the acyclic ether and the cyclic ether may be 5:95 to 95:5 (v / v), specifically 95:5 to 50:50, more specifically 90:10 to 50:50, 90:10 to 70:30, 85:15 to 75:25, or 80:20. In the present invention, the volume ratio corresponds to the ratio of "volume % of acyclic ether": "volume % of cyclic ether" in the ether solvent.

[0193] In one embodiment of the present invention, the non-aqueous solvent may not contain a carbonate solvent in terms of the solubility of the electrolyte. Alternatively, the non-aqueous solvent may contain a very small amount of a carbonate solvent such that the carbonate solvent does not affect the solubility of the lithium salt. For example, when the non-aqueous solvent contains the carbonate solvent, the content of the carbonate solvent may be 3 wt% or less, 2 wt% or less, 1 wt% or less, 0.5 wt% or less, or 0 wt% (i.e., not contained at all) based on the total weight of the electrolyte for a lithium secondary battery.

[0194] In one embodiment of the present invention, the lithium salt may be used without particular limitation as long as it can be used as an electrolyte of a lithium secondary battery. The lithium salt may be, for example, LiCl, LiBr, LiI, LiClO4, LiBF4, LiB 10 Cl 10 , LiPF6, LiCF3SO3, LiCF3CO2, LiC4BO8, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, CF3SO3Li, (CF3SO2)2NLi, (C2F5SO2)2NLi, (SO2F)2NLi, (CF3SO2)3CLi, lithium chloroborane, lithium lower aliphatic carboxylate, lithium 4-phenylborate, lithium imide, or two or more thereof.

[0195] In one embodiment of the present invention, the concentration of the lithium salt may be appropriately determined in consideration of ionic conductivity, solubility, etc., and may be, for example, 0.1 to 4 M, preferably 0.2 to 2 M, 0.2 to 1 M, 0.5 to 2 M, 0.6 to 1 M, or 0.6 to 0.9 M. When the concentration of the lithium salt is in the above-described range, it is advantageous to secure ionic conductivity suitable for battery operation, or to exhibit an advantageous effect in terms of improving the mobility of lithium ions and suppressing the decomposition reaction of the lithium salt itself by exhibiting an appropriate viscosity of the electrolyte, but the present invention is not limited thereto.

[0196] In one embodiment of the present invention, the additive may include a nitrogen compound in addition to the lithium salt to improve the electrical conductivity of the electrolyte and to improve the lifespan of the lithium-sulfur battery.

[0197] Specifically, the nitrogen compound may, but its efficacy is not limited to, for example, inhibit the reduction reaction of polysulfide occurring during the charge / discharge process of a lithium-sulfur battery, thereby preventing irreversible consumption of polysulfide, thereby improving the performance of a lithium-sulfur battery.

[0198] In one embodiment of the present invention, the nitrogen compound may be used without particular limitation as long as it has the effect of stably forming a solid electrolyte membrane (SEI) of the negative electrode and improving charge / discharge efficiency, and may be, for example, a nitric acid compound, a nitrite compound, or a mixture thereof.

[0199] In one embodiment of the present invention, the nitrogen compound is, for example, an inorganic nitric or nitrous compound such as lithium nitrate (LiNO3), potassium nitrate (KNO3), cesium nitrate (CsNO3), barium nitrate (Ba(NO3)2), ammonium nitrate (NH4NO3), lithium nitrite (LiNO2), potassium nitrite (KNO2), cesium nitrite (CsNO2), ammonium nitrite (NH4NO2); an organic nitric or nitrous compound such as methyl nitrate, dialkyl imidazolium nitrate, guanidine nitrate, imidazolium nitrate, pyridinium nitrate, ethyl nitrite, propyl nitrite, butyl nitrite, pentyl nitrite, and octyl nitrite; It may be selected from the group consisting of organic nitro compounds such as nitromethane, nitropropane, nitrobutane, nitrobenzene, dinitrobenzene, nitropyridine, dinitropyridine, nitrotoluene, dinitrotoluene, and combinations thereof, and preferably may include lithium nitrate.

[0200] In one embodiment of the present invention, the nitrogen compound may be included in an amount of, for example, 1 wt% to 10 wt%, specifically 1 wt% to 7 wt%, or 1 wt% to 5 wt%, based on the total weight of the electrolyte, but is not limited thereto. When the nitrogen compound is included in the above-described amount, it may exhibit a more advantageous effect in terms of improving the electrical conductivity of the electrolyte by the nitrogen compound and suppressing the reduction of polysulfide when used in a lithium-sulfur battery, but the present invention is not limited thereto.

[0201]

[0202] In one embodiment of the present invention, the lithium-sulfur battery may have a weight ratio of sulfur (S) in the electrolyte and the sulfur-carbon composite (El / S weight ratio) of 2.7 g / g or more, 2.8 g / g or more, 2.9 g / g or more, or 3.0 g / g or more. For example, the El / S ratio may be 2.7 g / g to 4.0 g / g, 2.8 g / g to 3.7 g / g, 2.9 g / g to 3.5, 3.0 g / g to 3.5 g / g, 2.8 g / g to 3.4 g / g, 2.9 g / g to 3.4 g / g, or 3.0 g / g to 3.4 g / g. Here, El is the weight of the electrolyte, and S is the weight of sulfur (S) included in the positive electrode.

[0203] When the weight of electrolyte per weight of sulfur element included in the positive electrode of the lithium-sulfur battery (El / S) satisfies the above range, the reduction reaction of the positive electrode active material can occur smoothly even when the lithium-sulfur battery is discharged at a high C-rate, the capacity when discharged at a high C-rate can be greatly improved, and the decrease in capacity can be less than when discharged at a low C-rate.

[0204] In one embodiment of the present invention, the El / S ratio of the lithium-sulfur battery can be calculated by the ratio of the weight of sulfur in the sulfur-carbon composite of the positive electrode introduced in the manufacturing step immediately after manufacturing the lithium-sulfur battery to the weight of the introduced electrolyte.

[0205] In another embodiment of the present invention, the El / S ratio of the lithium-sulfur battery can be calculated by the ratio of the weight of sulfur in the sulfur-carbon complex of the positive electrode analyzed by disassembling the battery and the weight of the electrolyte introduced.

[0206] For example, when analyzing the El / S ratio of a lithium-sulfur battery by disassembling the battery, the total weight of the lithium-sulfur battery is measured in a charged state, and then the battery is disassembled, the positive electrode, the negative electrode, the separator, and the case are washed with a solvent and dried, and the sum of their respective weights is calculated, and the weight of the electrolyte is measured by deducting the weight of the positive electrode, the negative electrode, the separator, and the case from the measured total weight of the battery. At this time, it is preferable to use a solvent for the washing that can extract the electrolyte attached to the positive electrode, the negative electrode, the separator, and the case. Next, the positive electrode active material layer and the current collector are separated from the dried positive electrode, and then the weight of sulfur derived from the sulfur-carbon complex present in the positive electrode active material layer is measured, thereby measuring the weight of sulfur in the positive electrode. The El / S ratio of the lithium-sulfur battery can be calculated by the ratio of the weight of sulfur in the sulfur-carbon complex of the positive electrode obtained in this way to the weight of the introduced electrolyte.

[0207] In one embodiment of the present invention, a method for measuring the weight of sulfur derived from a sulfur-carbon complex present in the positive electrode active material layer may be, for example, measuring the content of sulfur (S) derived from the active material through thermal gravimetric analysis (TGA) on the result obtained by scraping off the obtained positive electrode active material layer, but the measuring method is not limited thereto.

[0208] In one embodiment of the present invention, the state of charge at which the lithium-sulfur battery is decomposed may be a full charge state, i.e., SOC 100%.

[0209] In another embodiment of the present invention, the state of charge at which the lithium-sulfur battery is decomposed may be SOC 95% to SOS 100%.

[0210] In one embodiment of the present invention, when disassembling a lithium-sulfur battery in a charged state, it must be performed under an inert atmosphere for safety reasons. For example, disassembly of a lithium-sulfur battery may be performed under an Ar atmosphere.

[0211]

[0212] In one embodiment of the present invention, the lithium-sulfur battery may have an energy density of 300 Wh / kg or more. For example, the energy density of the lithium-sulfur battery may be 300 Wh / kg to 500 Wh / kg, or 300 Wh / kg to 400 Wh / kg.

[0213] In one embodiment of the present invention, the lithium-sulfur battery can exhibit an excellent effect of maintaining the energy density exhibited when discharging at a high discharge rate at a level of the energy density exhibited when discharging at a low discharge rate.

[0214] For example, the lithium-sulfur battery may exhibit an energy density measured when discharging at a 1.0 C-rate that is 90% or more of the energy density measured when discharging at a 0.5 C-rate.

[0215] Furthermore, the lithium-sulfur battery may exhibit an energy density measured when discharging at a 2.0 C-rate that is 90% or more of the energy density measured when discharging at a 1.0 C-rate.

[0216] In one embodiment of the present invention, the energy density of the lithium-sulfur battery may be measured according to a known method, and the measurement method is not particularly limited. For example, the energy density of the lithium-sulfur battery may be measured according to the following equations by discharging once from 2.5 V to 1.8 V at 0.5 C-rate at room temperature, charging once to 2.5 V at 1.0 C-rate, and then driving the discharge at a constant rate selected from 0.5 C-rate to 2.0 C-rate.

[0217] [ceremony]

[0218] Energy density (Wh / kg) = {[(discharge capacity (mAh) X operating voltage (V)) / 1000] / (cell weight (kg))}

[0219] In one embodiment of the present invention, the room temperature may be, for example, a temperature of 23°C to 25°C, and specifically, may be measured at 23°C.

[0220] In one embodiment of the present invention, the specific capacity of the lithium-sulfur battery may be, for example, 1,000 mAh / g or more.

[0221] In one embodiment of the present invention, the specific capacity of the lithium-sulfur battery may be measured by, for example, driving the battery for charging and discharging at a 0.5 C-rate after one discharge in the range of 1.8 V to 2.5 V at a 0.5 C rate at room temperature.

[0222] In one embodiment of the present invention, the room temperature may be a temperature of 23°C to 25°C.

[0223] In one embodiment of the present invention, the lithium sulfur battery may be a coin-type battery, a pouch-type battery, or a cylindrical battery, but is not limited thereto.

[0224]

[0225] According to another aspect of the present invention, a method for evaluating high-power characteristics of a lithium-sulfur battery using the above formula 1 is provided.

[0226] The above evaluation method includes a step of determining a lithium sulfur battery having a lithium sulfide ratio R(1.0C / 0.5C) of 85% or more according to the above formula 1 as a high-output battery.

[0227] In one embodiment of the present invention, the high-power battery may be, for example, a battery that maintains an energy density of 300 Wh / kg or more under discharge conditions of 1.0 C-rate or more at room temperature. In this case, in one embodiment of the present invention, the room temperature may be a temperature of 23°C to 25°C.

[0228]

[0229] Hereinafter, the present invention will be described in more detail through examples, but the following examples are intended to illustrate the present invention, and the scope of the present invention is not limited to these examples.

[0230]

[0231] [Manufacturing of lithium-sulfur batteries]

[0232] Example 1

[0233] A sulfur-carbon composite (S / C weight ratio = 2.3 g / g) in which sulfur (S8) is loaded on carbon nanotubes (MWCNTs) was prepared as a cathode active material. The prepared sulfur-carbon composite and polyacrylic acid (PAA) as a binder were mixed in a weight ratio of 96:4 and added to water to prepare a cathode slurry composition. The cathode slurry composition was applied to an aluminum current collector and then dried to prepare a cathode. The loading of the prepared cathode was 2.7 mAh / cm 2 It was.

[0234] Lithium metal with a thickness of 60 μm was prepared as the cathode.

[0235] An electrode assembly was prepared by positioning the positive and negative electrodes so that they face each other and interposing a polyethylene separator having a thickness of 16 ㎛ and a porosity of 46 vol% between them.

[0236] The prepared electrode assembly was stored in a pouch-type case, and an electrolyte solution containing 0.75 M lithium salt (LiTFSI) and 3 wt% lithium nitrate (LiNO3) dissolved in a solvent mixed with dimethoxyethane:2-methylfuran (2-MeF) in a volume ratio of 8:2 was injected so that the El / S ratio became 3.0 g / g, thereby manufacturing a lithium-sulfur battery.

[0237]

[0238] Example 2

[0239] A lithium-sulfur battery was manufactured in the same manner as in Example 1, except that the electrolyte was injected so that the El / S ratio was 3.4 g / g.

[0240]

[0241] Comparative Example 1

[0242] A lithium-sulfur battery was manufactured in the same manner as in Example 1, except that the electrolyte was injected so that the El / S ratio was 2.6 g / g.

[0243]

[0244] [Analysis of Li2S production and battery performance evaluation]

[0245] The lithium-sulfur batteries of Example 1, Example 2 and Comparative Example 1 were charged to 2.4 V at 0.5 C rate at room temperature (23°C), then discharged to 1.8 V at 0.5 C-rate, 1.0 C-rate or 2.0 C-rate, and the battery capacity (mAh) and energy (Wh) at this time were measured, and then divided by each battery capacity to evaluate the specific capacity (mAh / g) and energy density (Wh / kg) of the battery. The results are shown in Figures 1 and 2 below.

[0246] Additionally, a graph comparing the average discharge voltage of the battery, i.e., the nominal voltage, at 0.5 C-rate discharge and 1.0 C-rate discharge, respectively, is shown in Fig. 3.

[0247] Referring to Fig. 1, when discharged at 2.0 C-rate, the lithium-sulfur batteries of Examples 1 and 2 showed a small decrease in energy density (both maintained at 300 Wh / kg or more), but the lithium-sulfur battery of Comparative Example 1 showed a large decrease in energy density.

[0248] Figure 2 is a graph when discharged to 1.8 V at a C-rate of 2.0. The lithium-sulfur batteries of Examples 1 and 2 showed specific capacities of 1,000 mAh / g or more, but it was confirmed that the lithium-sulfur battery of Comparative Example 1 had a significantly lower specific capacity.

[0249] The lithium-sulfur battery of Comparative Example 1 had an E / S of 2.6, and it was confirmed that the capacity and energy density were significantly reduced when discharged at 2.0C.

[0250] Referring to FIGS. 1 and 3, it was confirmed that Comparative Example 1 maintained an energy density of 300 Wh / kg or more at 1.0C discharge, but the nominal voltage was significantly inferior to Examples 1 and 2.

[0251] Figures 4 and 5 are graphs analyzing the amount of Li2S in the lithium-sulfur batteries of Example 1, Example 2, and Comparative Example 2 after discharging them to 1.8 V (DOD100) at 0.5 C or 1.0 C, respectively.

[0252] To measure the amount of Li2S in each discharge state, XRD patterns were obtained for the lithium-sulfur battery in the discharge state according to the following method.

[0253] First, XRD patterns were obtained for each battery while discharging at 0.5C rate or 1.0C rate in the range of 2.4 V to 1.8 V at room temperature (23°C). Specifically, the range of 2theta (2θ) 4-17° was measured in transmission mode using Mo K-alpha X-ray (λ=0.709 Å) of PANalyical Empyrean XRD, and one pattern was obtained at 0.014° intervals for a total of 1 minute. At this time, XRD measurements were performed using a pressurized jig equipped with a Be-window. The peak scattering intensity in Figs. 4 and 5 was measured in arbitrary units (au).

[0254] Li2S has a specific peak at a scattering vector (q) of 1.85–1.92 / Å in the XRD pattern. The amount of Li2S can be determined using the peak intensity (i.e., scattering intensity) at this time.

[0255] The characteristic peak of Li2S can also be expressed through the scattering vector (q) at 1.4-1.6 / Å. However, since it may overlap with the scattering vector of S8 in that region, a specific peak value at 1.85-1.92 / Å was used for the quantification of Li2S in this experiment.

[0256] Graphs showing the peak intensity of Li2S at 0.5C discharge (Fig. 4) and 1.0C discharge (Fig. 5) are shown in Figs. 4 and 5, respectively. Using the results of Figs. 4 and 5, the ratio R (1.0C / 0.5C) of lithium sulfide according to Equation 1 below was calculated and shown in Table 1 below.

[0257] [Formula 1]

[0258] R(1.0C / 0.5C) = [A(DOD 100) 1.0 C / A(DOD 100) 0.5 C ] X 100 (%)

[0259] In the above equation 1,

[0260] Above A (DOD 100) 1.0 C is the amount of lithium sulfide present in a discharged state up to DOD 100 at 1.0C.

[0261] Above A (DOD 100) 0.5C is the amount of lithium sulfide present when the battery is discharged to DOD 100 at 0.5C.

[0262] At this time, the above A (DOD 100) 1.0 C and the above A (DOD 100) 1.0 C was measured through the peak intensity values ​​of the XRD pattern.

[0263] Comparative Example 1 Example 1 Example 2A (DOD 100) 1.0 C 3.5 x 10 -1 4.2 x 10 -1 4.2 x 10 -1 A(DOD 100) 0.5 C 4.4 x 10 -1 4.5 x 10 -1 4.6 x 10 -1R(1.0C / 0.5C)79%93%91%

[0264] Referring to FIG. 4, FIG. 5 and Table 1, it was found that the lithium-sulfur battery of Comparative Example 1 produced significantly less Li2S when discharged at 1.0C.

[0265] Through the above results, it was confirmed that Examples 1 and 2, in which the ratio R (1.0C / 0.5C) of the lithium sulfide was 85% or more, had high output characteristics, whereas Comparative Example 1, in which the ratio was low, did not have high output characteristics.

[0266] As described above, although the present invention has been described by limited embodiments and drawings, the present invention is not limited thereto, and it is obvious that various modifications and variations are possible within the scope of the technical idea of ​​the present invention and the equivalent scope of the patent claims to be described below by a person having ordinary skill in the art to which the present invention pertains.

Claims

1. A lithium-sulfur battery comprising: a positive electrode; a negative electrode; and a separator interposed between the positive electrode and the negative electrode; and an electrolyte; The above positive electrode comprises a positive electrode active material including a sulfur-carbon complex, The lithium-sulfur battery is characterized in that the ratio R(1.0C / 0.5C) according to the following formula 1 is 80% or more: [Formula 1] R(1.0C / 0.5C) = [A(DOD 100) 1.0 C / A(DOD 100) 0.5 C ] X 100 (%) In the above equation 1, Above A (DOD 100) 1.0 C is the amount of lithium sulfide (Li2S) present in the DOD 100 state when discharged at 1.0C. Above A (DOD 100) 0.5 C is the amount of lithium sulfide (Li2S) present in a DOD 100 state when discharged at 0.5C.

2. In claim 1, A lithium-sulfur battery characterized in that the above R(1.0C / 0.5C) is 85% or more.

3. In claim 1, A lithium-sulfur battery characterized in that the above DOD 100 has a potential of 1.7 V to 1.9 V.

4. In claim 1, The above DOD 100 is a lithium-sulfur battery characterized in that it has a potential of 1.8 V.

5. In claim 1, A lithium-sulfur battery, characterized in that the amount of the lithium sulfide (Li2S) is the weight, volume or mole number of the lithium sulfide.

6. In claim 1, The above ratio R(1.0C / 0.5C) is measured through the ratio of peak intensities of lithium sulfide (Li2S) on the X-ray diffraction spectrum for the lithium sulfur battery. The above lithium sulfide (Li2S) has a scattering vector (q) = 1.85 to 1.92 Å on the X-ray diffraction spectrum. -1 A lithium-sulfur battery characterized by having a characteristic peak in the region.

7. In claim 1, A lithium-sulfur battery characterized in that the weight ratio of sulfur (S) in the electrolyte and the sulfur-carbon complex (El / S weight ratio) is 2.7 g / g or more.

8. In claim 1, A lithium-sulfur battery, characterized in that the electrolyte comprises a non-aqueous solvent, a lithium salt, and an additive.

9. In claim 1, A lithium-sulfur battery characterized in that the energy density of the lithium-sulfur battery is 300 Wh / kg or more.

10. In claim 1, A lithium sulfur battery characterized in that the content of elemental sulfur (S) in the sulfur-carbon complex is 60 to 85 wt%.

11. In claim 1, A lithium-sulfur battery characterized in that the weight of the sulfur-carbon complex is 90 wt% or more based on the total weight of the positive electrode.

12. In claim 1, A lithium-sulfur battery characterized in that the above lithium-sulfur battery is a coin-shaped battery, a pouch-shaped battery, or a cylindrical battery.

13. A method for evaluating the output characteristics of a lithium sulfur battery comprising a positive electrode; a negative electrode; and a separator interposed between the positive electrode and the negative electrode; and an electrolyte; wherein the positive electrode comprises a positive electrode active material including a sulfur-carbon complex. An evaluation method characterized by including a step of determining a high-power lithium-sulfur battery when the ratio R(1.0C / 0.5C) according to the following formula 1 is 80% or more: [Formula 1] R(1.0C / 0.5C) = [A(DOD 100) 1.0 C / A(DOD 100) 0.5 C ] X 100 (%) In the above equation 1, Above A (DOD 100) 1.0 C is the amount of lithium sulfide (Li2S) present in the DOD 100 state when discharged at 1.0C. Above A (DOD 100) 0.5 C is the amount of lithium sulfide (Li2S) present in a DOD 100 state when discharged at 0.5C.

14. In claim 13, An evaluation method characterized in that the above high-power lithium-sulfur battery is a battery that maintains an energy density of 300 Wh / kg or more under discharge conditions of 1.0 C-rate or more at room temperature.

15. In claim 14, An evaluation method characterized in that the above room temperature is a temperature of 23°C to 25°C.

16. In claim 15, Above A (DOD 100) x C (x=0.5 or 1.0) is, The above lithium-sulfur battery was discharged at x C-rate to obtain an X-ray diffraction spectrum at a DOD of 100, and the scattering vector (q) = 1.85 to 1.92 Å on the obtained X-ray diffraction spectrum. -1 Measured through peak intensity values ​​in the area, The above ratio R(1.0C / 0.5C) is An evaluation method characterized by calculating and measuring the ratio of each peak intensity obtained above.

Citation Information

Patent Citations

  • Apparatus and Method for replacing transformer without no interruption

    KR1020220116119A

  • Cake including juice and Manufacturing method thereof

    KR1020240030219A

  • Electrolyte for lithium secondary battery and lithium secondary battery comprising the same

    KR102115595B1

  • KR20210088025A