Ion separator and compositon therefor

WO2024243815A1PCT designated stage expired Publication Date: 2024-12-05CELANESE INTERNATIONAL CORP +2
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/097217
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-30
Publication Date
2024-12-05

Smart Images

  • Figure CN2023097217_05122024_PF_FP_ABST
    Figure CN2023097217_05122024_PF_FP_ABST
Patent Text Reader

Abstract

An ion separator for electronic devices, such as batteries, is disclosed. The separator is formed from at least one polyethylene polymer. The polyethylene polymer is modified in a way that causes polymer chain interactions in an amount sufficient to increase the meltdown temperature of the membrane. Cross-linking or other chain interactions can occur using radiation or a chemical chain interactive agent, such as an acrylic acid. In one embodiment, the membrane is exposed to radiation and also is chemically cross-linked.
Need to check novelty before this filing date? Find Prior Art

Description

ION SEPARATOR AND COMPOSITON THEREFORBACKGROUND

[0001] Polyethylene polymers have numerous and diverse uses and applications. For example, high density polyethylenes are valuable engineering plastics, with a unique combination of abrasion resistance, surface lubricity, chemical resistance and impact strength. They find application in the production of high strength fibers for use in ropes and anti-ballistic shaped articles and in the production of other elongated articles, such as membranes for electronic devices. However, since the flowability of these materials in the molten state decreases as the molecular weight increases, processing by conventional techniques, such as melt extrusion, is not always possible.

[0002] One alternative method for producing fibers and other elongated components from polyethylene polymers is by gel-processing in which the polymer is combined with a solvent. The resultant gel is extruded into a fiber or membrane and may be stretched in one or two directions. Also, part or all of the solvent may be removed from the product.

[0003] Membranes made from polyethylene polymers through gel-processing can be formed to have many beneficial properties. For instance, the membranes can be formed with micro-pores. Microporous polyethylene membranes formed through gel-processing, for instance, are particularly well suited for use as a separator in a battery, such as a lithium ion battery. The microporous membrane, for instance, can separate an anode from a cathode and prevent a short circuit between the active battery components. At the same time, the microporous membrane permits ions to pass through due to the porous nature of the material. The ion permeability characteristics of the microporous polyethylene membrane makes the material particularly well suited for regulating electrochemical reactions within the battery.

[0004] In addition to the microporous nature of the polyethylene membrane and to possessing beneficial strength and other physical properties, the polyethylene membranes also offer what is referred to in the art as having an effective “shutdown effect” . The shutdown effect refers to the self-closing of micro-pores within the polyethylene separator when it surpasses a certain temperature. When  the pores in the polyethylene membrane are closed upon reaching a certain temperature, ions can no longer pass through the membrane and the electrochemical function of the battery stops. This effect becomes an important safety feature for the battery as it prevents thermal runaway reactions from continuing and prevents the battery from overheating and creating a potentially hazardous situation.

[0005] In addition to a shutdown temperature, polyethylene membranes also have a meltdown temperature, which refers to the temperature at which the membrane loses its mechanical stability and rupture occurs. Ideally, the polymer membrane has a relatively low shutdown temperature while possessing a relatively high meltdown temperature in order to provide electrical devices, such as batteries, with safety and stability.

[0006] In the past, in order to increase the meltdown temperature of polymer membranes, the membranes were either coated with a higher temperature material or formed with multiple polymer layers, such as through a coextrusion process. The above techniques, however, can adversely affect various physical properties of the membranes and / or have a detrimental effect on the shutdown temperature. In view of the above, a need currently exists for a polymer membrane that has an increased meltdown temperature. More particularly, a need exists for a polymer membrane having a desired shutdown temperature in combination with an increased meltdown temperature.SUMMARY

[0007] In general, the present disclosure is directed to polyolefin compositions well suited for gel-processing applications. More particularly, the present disclosure is directed to a polymer composition containing a high density polyethylene polymer well suited for producing microporous, ion permeable membranes that may be used as separators in batteries. In accordance with the present disclosure, the polymer composition is formulated so as to have a low shutdown temperature in combination with a higher meltdown temperature so that the membrane becomes substantially impermeable once the membrane is subjected to higher temperatures in a particular environment while remaining thermally stable. For instance, when used as a battery separator, the membrane can prevent the battery from a thermal runaway condition.

[0008] In one embodiment, the present disclosure is directed to an ion separator for dividing an anode from a cathode comprising a porous polymer film. The porous polymer film comprises a high density polyethylene polymer. In accordance with the present disclosure, the polymer chains within the film have undergone an interaction, such as a polar interaction or have been cross-linked in a manner that increases the meltdown temperature of the film without substantially impacting the shutdown temperature of the film. The polymer film, for example, can have a shutdown temperature of from about 120℃ to about 140℃ and can have a meltdown temperature of from about 140℃ to about 230℃. The difference between the meltdown temperature and the shutdown temperature can be greater than about 18℃, such as greater than about 20℃, such as greater than about 23℃, such as greater than about 28℃, such as greater than about 33℃, and generally less than about 110℃.

[0009] In various embodiments, the meltdown temperature of the polymer film can be greater than about 152℃, such as greater than about 155℃, such as greater than about 160℃, such as greater than about 165℃. The polymer film can have a thickness of from about 5 nm to about 25 nm, such as from about 7 nm to about 20 nm. The porosity of the film or membrane can be from about 20%to about 50%, such as from about 25%to about 45%.

[0010] The polyethylene polymer chains or molecules contained in the polymer film can be cross-linked or otherwise subjected to a chain interaction using various techniques that have shown to increase the meltdown temperature. In one embodiment, for instance, the polyethylene polymer is cross-linked by subjecting the film to radiation. The radiation, for instance, can be electron beam radiation, X-ray radiation, ultra-violet radiation, or gamma ray radiation.

[0011] Alternatively, the polyethylene polymer contained in the porous polymer film can be chemically cross-linked and / or subjected to a process that causes other chain interactions, such as polar interactions. For example, a chemical chain interactive agent can be combined with the polyethylene polymer that causes the polyethylene polymer chains to interact and cross-link or otherwise undergo a chain entanglement. In one embodiment, for instance, the chemical chain interactive agent can be any suitable group grafted onto the polyethylene polymer  chains that can form cross-links with similar chemical groups on opposing polymer chains and / or cause other chain interactions, such as polar interactions.

[0012] In one aspect, the chemical chain interactive agent can be a silane. The silane, for instance, can be grafted to the polyethylene polymer. Alternatively, the chemical chain interactive agent can be a polyethylene ionomer. The polyethylene ionomer, for instance, can be an ethylene-methacrylate copolymer or an ethylene-acrylate copolymer.

[0013] In another embodiment, the chemical chain interactive agent can comprise an acrylic acid that has been grafted to the polyethylene polymer. In one embodiment, the acrylic acid groups can be saponified and / or treated with an inorganic salt that enhances chain interactions or otherwise improves a property of the molded article. The inorganic salt, for instance, can be a metal salt, such as an alkaline earth metal halide salt. In one particular embodiment, the metal salt can be a calcium salt, such as calcium chloride. When a calcium salt is used, -O-Ca-O-cross-links may form between the polymer chains.

[0014] In another aspect, the acrylic acid groups can be saponified and / or treated with a base, such as a metal hydroxide. For instance, the base can be sodium hydroxide. The acrylic acid groups can be treated by exposing the polymer to a solution containing the base, such as an aqueous sodium hydroxide solution. In one embodiment, the acrylic acid groups can be treated with a solution containing a base, such as sodium hydroxide, followed by treatment with a metal salt, such as an alkaline earth metal salt solution or vice versus.

[0015] The acrylic acid can be incorporated into the polyethylene polymer generally in an amount of from about 0.01%to about 25%by weight, such as in an amount from about 0.1%to about 12%by weight. For instance, the acrylic acid can be incorporated into the polymer in an amount greater than about 2%by weight, such as in an amount greater than about 2.5%by weight, such as in an amount greater than about 3%by weight, such as in an amount greater than about 3.5%by weight, and generally in an amount less than about 20%by weight. The grafted high density polyethylene polymer can be used alone to produce molded articles, such as a membrane. Alternatively, the grafted high density polyethylene polymer can be combined with a non-grafted high density polyethylene polymer. The weight ratio between the grafted polyethylene polymer and the non-grafted  polyethylene polymer can be from about 10: 90 to about 90: 10, such as from about 40: 60 to about 80: 20. The resulting polymer blend can contain acrylic acid groups in an amount greater than about 0.4%by weight, such as in an amount greater than about 0.6%by weight, such as in an amount greater than about 0.8%by weight, such as in an amount greater than about 1.2%by weight, such as in an amount greater than about 1.6%by weight, such as in an amount greater than about 1.8%by weight, such as in an amount greater than about 2.2%by weight, such as in an amount greater than about 2.4%by weight, such as in an amount greater than about 2.8%by weight, such as in an amount greater than about 3.2%by weight, such as in an amount greater than about 3.4%by weight, such as in an amount greater than about 3.6%by weight, such as in an amount greater than about 3.8%by weight, such as in an amount greater than about 4%by weight, such as in an amount greater than about 4.2%by weight, such as in an amount greater than about 4.4%by weight, and in an amount less than about 20%by weight.

[0016] In one embodiment, the high density polyethylene used to produce the porous polymer film can have a relatively high molecular weight. The use of higher molecular weight polyethylene polymers may be beneficial, especially in applications where greater strength properties are needed or desired. For example, the polyethylene used to produce the film can have a molecular weight of greater than about 500,000 g / mol, such as greater than about 700,000 g / mol, such as greater than about 1,000,000 g / mol, such as greater than about 1,500,000 g / mol, and less than about 12,000,000 g / mol, such as less than about 8,000,000 g / mol. In one embodiment, the polyethylene used to produce the film comprises a Ziegler-Natta catalyzed high molecular weight polyethylene.

[0017] In one aspect, the porous film is primarily made from the polyethylene polymer. For instance, the high density polyethylene polymer can be present in the film or membrane in an amount from about 60%by weight to about 98%by weight.

[0018] The present disclosure is also directed to a battery, such as a lithium-ion battery. The battery includes an anode, a cathode and a separator membrane formed from the porous film as described above. The separator membrane can include a single layer polymer film that may optionally include a coating. For  example, the single layer polymer membrane can include an inorganic coating or a polymer coating.

[0019] The present disclosure is also directed to a process for producing polymer articles. The process includes the steps of forming a gel-like composition from the polymer composition described above containing a plasticizer. The gel-like composition is then extruded through a die to form a polymer article. The polymer article, for instance, may comprise a porous membrane. During formation of the polymer article, at least part of the plasticizer is separated and removed from the polyethylene article. For instance, in one embodiment, greater than 80%, such as greater than 90%, such as greater than 95%, such as greater than 98%of the plasticizer is removed during formation of the polymer article.

[0020] In one embodiment, an extraction solvent, such as dichloromethane is combined with the polymer composition before or during formation of the polymer article. The extraction solvent can be used to facilitate removal of the plasticizer.

[0021] In accordance with the present disclosure, the process further includes the step of cross-linking the polyethylene polymer contained within the porous membrane or otherwise causing polymer chain interactions within the polymer. The polyethylene polymer can be cross-linked by exposure to radiation and / or by incorporating a chemical chain interactive agent into the polymer composition that is used to form the membrane. In one aspect, acrylic acid is grafted onto the polyethylene polymer and saponified with an inorganic salt in order to form chain interactions. The acrylic acid groups can be saponified, for instance, by contacting the porous membrane with a solution containing an inorganic salt, such as a calcium salt.

[0022] In another aspect, the acrylic acid groups grafted to the polyethylene polymer can be treated with a base, such as a sodium hydroxide solution. Optionally, the acrylic acid groups can be treated with a base, such as a sodium hydroxide solution, and also treated with a solution containing an inorganic salt, such as a calcium chloride solution.

[0023] Other features and aspects of the present disclosure are discussed in greater detail below.BRIEF DESCRIPTION OF THE DRAWINGS

[0024] A full and enabling disclosure of the present disclosure is set forth more  particularly in the remainder of the specification, including reference to the accompanying figures, in which:

[0025] Fig. 1 is a plot or graph illustrating the shutdown temperature and the meltdown temperature of a microporous membrane using an Impedance Test; and

[0026] Fig. 2 is a cross-sectional view of an electronic device, such as a battery, incorporating a porous membrane made in accordance with the present disclosure.

[0027] Repeat use of reference characters in the present specification and drawings is intended to represent the same or analogous features or elements of the present invention.

[0028] DEFINITIONS

[0029] The shutdown temperature of a porous polymer membrane is the temperature at which the pores of the membrane close and no longer allow ions to pass through. For example, when tested according to the Impedance Test, it is the temperature at which the impedance initially increases to over 800 Ohms. It is also the temperature at which the polymer membrane starts to melt and pores close. The meltdown temperature of a porous membrane is the temperature at which the membrane loses its mechanical stability and rupture occurs. Under the thermomechanical analysis test (TMA test) , the dimension change of the membrane is measured while the sample is subjected to a temperature regime and a static force of 0.01N is applied. The test is performed over a temperature range from 40 ℃ to 200℃ with a heating rate of 5℃ / min. Data evaluation is done with a plot of dimension change versus temperature and the melt down temperature is indicated when dimension change increases and exceeds 1000 microns. The test can be conducted on a TA Instruments Thermo mechanical Analyzer (TMA) model Q400, Film / Fiber probe, MCA cooling system.

[0030] The shutdown temperature and meltdown temperature of a porous polymer membrane are illustrated, for instance, in FIG. 1.

[0031] The shutdown temperature or meltdown temperature of a polymer article, such as a microporous membrane, can vary depending upon the type of test and instrument used to measure the shutdown temperature. In fact, the shutdown temperature can vary widely depending upon the procedure, molecular weight of the base resin, and equipment used to make the determination. Thus,  any reported shutdown temperatures for various products can be much lower than if a different test or technique is used.

[0032] In the present disclosure, the shutdown temperature of a polymer article, such as a porous membrane or of a polymer composition can be determined according to the “Impedance Test, ” the “Thermomechanical Analysis Test, ” and the “Differential Scanning Calorimetry Test” . The Impedance Test, however, is the only test that directly measures shutdown temperature. The following tests are defined as follows.

[0033] Impedance Test

[0034] The impedance spectroscopy test setup consists of a glass measurement cell containing two steel electrodes. According to the impedance spectroscopy method, the sample is soaked in an electrolyte (1M LiPF6 in 1: 1 ethylene carbonate / dimethyl carbonate) and assembled into the cell between the electrodes. The measurement cell is then connected to an impedance spectrometer that records impedance spectrum every 50 seconds at a frequency between 100Hz and 100kHz. The measurement cell is then placed in an oven and heated over 2 hours from 110℃ to 150℃ while continuously recording impedance spectra. Data evaluation is done with a plot of impedance versus temperature and shutdown temperature is indicated by midway of a steep increase in impedance. An example plot is demonstrated in FIG. 1 in which the arrows indicate shutdown temperature. The test can be conducted using an HCP-803 potentiostat available from Biologic Science Instruments.

[0035] Thermo Mechanical Analysis (TMA Test)

[0036] Under the TMA method, the dynamic strain is measured while the sample is subjected to a temperature regime and a static force of 0.2N with a force multiplier of 0.5. The test is performed over a temperature range from room temperature (25-30℃) to 160℃ with a heating rate of 2℃ / min. The frequency is set at 0.1 Hz. Data evaluation is done with a plot of dynamic strain versus temperature and the softening point is indicated by the dynamic strain inflection point. The test can be conducted on a Perkin Elmer DMA 8000 dynamic mechanical analyzer.

[0037] Differential Scanning Calorimetry (DSC Test)

[0038] Using differential scanning calorimetry (DSC) , the melting point of the  sample can be determined by ISO Test No. 11357 under the following conditions: The sample is heated from 0℃ to 180℃ with a heating rate of 10℃ / min and held isothermally for 5 min at 180℃. After the isothermal hold, the sample is cooled to 0℃ with a heating rate of 10℃ / min. Finally, the sample is heated to 180℃ with a heating rate of 20℃. The sample is inerted with nitrogen during all steps of the DSC procedure. The test can be conducted using a DSC Q2000 calorimeter available from TA Instruments.

[0039] As used herein, puncture strength is measured according to ASTM Test D3763 and measures the ability of a membrane to withstand a foreign particle from causing a hole or defect. The test is conducted on a testing device, such as an Instron CEAST 9340 device. The drop height is 0.03 to 1.10 m. The impact velocity is 0.77 to 4.65 m / s. The maximum dropping mass is 37.5 kg and the maximum potential energy is 405 J. Puncture strength is measured in slow speed puncture mode at 1.67 mm / s.

[0040] The melt flow rate of a polymer or polymer composition is measured according to ISO Test 1133 at 190℃ and at a load of 2.16 kg (unless otherwise indicated) .

[0041] The density of a polymer is measured according to ISO Test 1183 in units of g / cm3.

[0042] Average particle size (d50) is measured using laser diffraction / light scattering, such as a suitable Horiba light scattering device.

[0043] The average molecular weight of a polymer is determined using the Margolies’ equation.

[0044] Tensile modulus, tensile stress at yield, tensile strain at yield, tensile stress at 50%break, tensile stress at break, and tensile nominal strain at break are all measured according to ISO Test 527-2 / 1B.

[0045] Gurley permeability can be measured according to the Gurley Test, using a Gurley permeability tester, such as Gurley Densometer, Model KRK 2060c commercially available from Kumagai Riki Kogyo Co., LTD. The test is conducted according to ISO Test 5636. The Gurley Test measures air permeability as a function of the time required for a specified amount of air to pass through a specified area under a specified pressure. The units are reported in sec / 100 ml.

[0046] Porosity (%) is measured according to the following procedure. During  the procedure, the following ASTM Standards are used as a reference: D622 Standard Test Method for Apparent Density of Rigid Cellular Plastics1; and D729 Standard Test Methods for Density and Specific Gravity (Relative Density) of Plastics by Displacement1. The following instruments are used: Calibrated Analytical Balance (0.0001 grams) ; Lorentzen&Wettre Micrometer, code 251 (0.1 um) ; and Deli 2056 art knife.

[0047] Procedure:

[0048] 1.1. Samples and sample preparation

[0049] Using the specimen art knife, cut each sample material into a minimum of three 60mm ±0.5 by 60mm±0.5 specimens

[0050] 1.2. Instrument and measurement

[0051] 3.2.1 Using the L&W micrometer, take five readings of the thickness at each 60mm by 60mm specimen (average of 5 readings) . Record this value as the thickness of this specimen.

[0052] 3.2.2 Weigh the specimen directly on the balance. Record this value as the weight of this specimen.

[0053] 3.2.3 The three specimens of the same sample are placed together and steps

[0054] 3.2.1 and 3.2.2 are repeated to obtain the [bulk] thickness and the [bulk] weight.

[0055] Calculate the density to three significant figures as follows

[0056] a. Dfilm =Density (film) = Wt. of Specimen

[0057] THK*Square

[0058] Dfilm = density of specimen, mg / mm3

[0059] Wt = weight of specimen, mg

[0060] THK= thickness of specimen, mm

[0061] Square= area of specimen, (mm2)

[0062] b. Dpolymer= Density (polymer) 0.95 (g / cm3)

[0063] Dpolymer: Density of raw materials, without the pores.

[0064] c. Porosity = (1-Dfilm / Dpolymer) *100%DETAILED DESCRIPTION

[0065] It is to be understood by one of ordinary skill in the art that the present discussion is a description of exemplary embodiments only and is not intended as limiting the broader aspects of the present disclosure.

[0066] In general, the present disclosure is directed to a polymer composition well suited for producing gel extruded articles, such as fibers and films, including porous membranes. The present disclosure is also directed to the articles made from the polymer composition. In one aspect, the present disclosure is particularly directed to producing porous membranes that are well suited for use as a separator in an electronic device that separates a cathode from an anode but allows ions to pass through for proper functioning of the device. For example, in one embodiment, the electronic device can be a lithium-ion battery.

[0067] In accordance with the present disclosure, the polymer article, such as the porous membrane, contains a polyethylene polymer that has been subjected to a treatment that causes polymer chain interactions, such as polar chain interactions or cross-linking. Cross-linking or other chain interactions within the polyethylene polymer in accordance with the present disclosure can provide numerous benefits and advantages. When producing an ion separator, for instance, the present disclosure is directed to modifying the polyethylene polymer contained in the membrane so as to increase the meltdown temperature of the membrane without compromising other properties, such as the shutdown temperature. Porous membranes made in accordance with the present disclosure, for instance, can have a relatively low shutdown temperature in combination with a relatively high meltdown temperature. Consequently, porous membranes made according to the present disclosure can prevent thermal runaway of a battery. For instance, when the battery overheats or subjected to higher temperatures, the membrane can prevent the battery from operating while still providing thermal stability in a manner that prevents rupturing. Of particular advantage, porous membranes made according to the present disclosure can be formed from a single polymer layer and, in one embodiment, can be made exclusively from high density polyethylene polymers, and can be free of other polymers, such as polypropylene polymers, and the like. In addition, membranes made according to the present disclosure can be deployed as an ion separator without any coatings designed to  increase the thermal stability or meltdown temperature of the separator. For instance, the ion separator of the present disclosure can be constructed so as not to include any ceramic coatings, organic coatings, including aramid coatings, or polymer coatings. Further, it was unexpectedly discovered that the above advantages can be achieved without having to increase the thickness of the ion separator.

[0068] As described above, the polyethylene polymer contained in the ion separator of the present disclosure is modified that causes polymer chain interactions, such as cross-linking. The polyethylene polymer can be modified or cross-linked using various methods and techniques. For example, in one embodiment, the polymer article can be extruded into a shape, such as the form of a porous membrane, and then subjected to radiation in an amount sufficient to cross-link the polyethylene polymer contained in the membrane. The cross-linking conditions are controlled in a manner that optimizes an increase in the meltdown temperature of the membrane without adversely affecting other properties.

[0069] In an alternative embodiment, the polyethylene polymer can be chemically modified to cause chain interactions, such as polar interactions and / or cross-linking. For example, a chemical chain interactive agent can be incorporated or combined with the polyethylene polymer that causes the polyethylene polymer chains to interact, such as cross-link. Cross-linking can occur during formation of the polymer article or can be activated after the polymer article is formed. Various different chemical chain interactive agents can be used. For instance, polymer chain interactions can be initiated using a silane chain interactive agent, using an ionomer, or using an acrylic acid chain interactive agent that may optionally be saponified and / or subjected to an alkaline treatment.

[0070] As described above, modifying or cross-linking the polyethylene polymer can increase the meltdown temperature of porous membranes made from the polymer without affecting many other properties, including the shutdown temperature. For instance, the meltdown temperature of the porous membrane can be increased by greater than about 5℃, such as greater than about 7℃, such as greater than about 10℃, such as greater than about 13℃, such as greater than about 15℃, such as greater than about 18℃, such as greater than about 20℃, and generally less than about 110℃, such as less than about 40℃ in  comparison to the same porous membrane that has not been modified or cross-linked. The meltdown temperature of the porous membrane, for instance, can be greater than about 150℃, such as greater than about 152℃, such as greater than about 155℃, such as greater than about 160℃, such as greater than about 165℃. The final meltdown temperature is generally less than about 230℃ , such as less than about 185℃, such as less than about 180℃, such as less than about 175℃.

[0071] The meltdown temperature can be increased as described above while maintaining the shutdown temperature of the porous membrane at less than about 145℃. For example, the shutdown temperature of the porous membrane can be less than about 140℃, such as less than about 138℃, such as less than about 136℃. The shutdown temperature is generally greater than about 120 ℃, such as greater than about 130℃, such as greater than about 132℃. In one aspect, the meltdown temperature and the shutdown temperature can be determined according to the impedance test.

[0072] In accordance with the present disclosure, the difference between the meltdown temperature and the shutdown temperature can be relatively great. For instance, the difference between the meltdown temperature and the shutdown temperature can be greater than about 18℃, such as greater than about 20℃, such as greater than about 23℃, such as greater than about 25℃, such as greater than about 28℃, such as greater than about 30℃, such as greater than about 33℃. The difference between the shutdown temperature and the meltdown temperature is generally less than about 110℃, such as less than about 55℃.

[0073] In general, any suitable high density polyethylene polymer may be used to form the primary polymer component and the matrix polymer of the polymer composition. The high density polyethylene has a density of about 0.93 g / cm3 or greater, such as about 0.94 g / cm3 or greater, such as about 0.95 g / cm3 or greater, and generally less than about 1 g / cm3.

[0074] The high density polyethylene polymer can be made from over 90%ethylene derived units, such as greater than 95%ethylene derived units, or from 100%ethylene derived units. The polyethylene can be a homopolymer or a copolymer, including a terpolymer, having other monomeric units.

[0075] The high density polyethylene can be a high molecular weight polyethylene, a very high molecular weight polyethylene, and / or an ultrahigh molecular weight polyethylene. "High molecular weight polyethylene" refers to polyethylene compositions with an average molecular weight of at least about 3x105 g / mol and, as used herein, is intended to include very-high molecular weight polyethylene and ultra-high molecular weight polyethylene. For purposes of the present specification, the molecular weights referenced herein are determined in accordance with the Margolies equation ( "Margolies molecular weight" ) .

[0076] "Very-high molecular weight polyethylene" refers to polyethylene compositions with a weight average molecular weight of less than about 3x106 g / mol and more than about 1x106 g / mol. In some embodiments, the molecular weight of the very-high molecular weight polyethylene composition is between about 2x106 g / mol and less than about 3x106 g / mol.

[0077] "Ultra-high molecular weight polyethylene" refers to polyethylene compositions with an average molecular weight of at least about 3x106 g / mol. In some embodiments, the molecular weight of the ultra-high molecular weight polyethylene composition is between about 3x106 g / mol and about 30x106 g / mol, or between about 3x106 g / mol and about 20x106 g / mol, or between about 3x106 g / mol and about 10x106 g / mol, or between about 3x106 g / mol and about 6x106 g / mol.

[0078] In one aspect, the high density polyethylene is a homopolymer of ethylene. In another embodiment, the high density polyethylene may be a copolymer. For instance, the high density polyethylene may be a copolymer of ethylene and another olefin containing from 3 to 16 carbon atoms, such as from 3 to 10 carbon atoms, such as from 3 to 8 carbon atoms. These other olefins include, but are not limited to, propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 4-methylpent-1-ene, 1-decene, 1-dodecene, 1-hexadecene and the like. Also utilizable herein are polyene comonomers such as 1, 3-hexadiene, 1, 4-hexadiene, cyclopentadiene, dicyclopentadiene, 4-vinylcyclohex-1-ene, 1, 5-cyclooctadiene, 5-vinylidene-2-norbornene and 5-vinyl-2-norbornene. However, when present, the amount of the non-ethylene monomer (s) in the copolymer may be less than about 10 mol. %, such as less than about 5 mol. %,  such as less than about 2.5 mol. %, such as less than about 1 mol. %, wherein the mol. %is based on the total moles of monomer in the polymer.

[0079] In one embodiment, the high density polyethylene may have a monomodal molecular weight distribution. Alternatively, the high density polyethylene may exhibit a bimodal molecular weight distribution. For instance, a bimodal distribution generally refers to a polymer having a distinct higher molecular weight and a distinct lower molecular weight (e.g. two distinct peaks) on a size exclusion chromatography or gel permeation chromatography curve. In another embodiment, the high density polyethylene may exhibit more than two molecular weight distribution peaks such that the polyethylene exhibits a multimodal (e.g., trimodal, tetramodal, etc. ) distribution. Alternatively, the high density polyethylene may exhibit a broad molecular weight distribution wherein the polyethylene is comprised of a blend of higher and lower molecular weight components such that the size exclusion chromatography or gel permeation chromatography curve does not exhibit at least two distinct peaks but instead exhibits one distinct peak broader than the individual component peaks.

[0080] Any method known in the art can be utilized to synthesize the polyethylene. The polyethylene powder is typically produced by the catalytic polymerization of ethylene monomer or optionally with one or more other 1-olefin co-monomers, the 1-olefin content in the final polymer being less or equal to 10%of the ethylene content, with a heterogeneous catalyst and an organo aluminum or magnesium compound as cocatalyst. The ethylene is usually polymerized in gaseous phase or slurry phase at relatively low temperatures and pressures. The polymerization reaction may be carried out at a temperature of between 50℃. and 100℃. and pressures in the range of 0.02 and 2 MPa.

[0081] The molecular weight of the polyethylene can be adjusted by adding hydrogen. Altering the temperature and / or the type and concentration of the co-catalyst may also be used to fine tune the molecular weight. Additionally, the reaction may occur in the presence of antistatic agents to avoid fouling and product contamination.

[0082] Suitable catalyst systems include but are not limited to Ziegler-Natta type catalysts. Typically Ziegler-Natta type catalysts are derived by a combination of transition metal compounds of Groups 4 to 8 of the Periodic Table and alkyl or  hydride derivatives of metals from Groups 1 to 3 of the Periodic Table. Transition metal derivatives used usually comprise the metal halides or esters or combinations thereof. Exemplary Ziegler-Natta catalysts include those based on the reaction products of organo aluminum or magnesium compounds, such as for example but not limited to aluminum or magnesium alkyls and titanium, vanadium or chromium halides or esters. The heterogeneous catalyst might be either unsupported or supported on porous fine grained materials, such as silica or magnesium chloride. Such support can be added during synthesis of the catalyst or may be obtained as a chemical reaction product of the catalyst synthesis itself.

[0083] In one embodiment, a suitable catalyst system can be obtained by the reaction of a titanium (IV) compound with a trialkyl aluminum compound in an inert organic solvent at temperatures in the range of -40℃. to 100℃., preferably -20℃. to 50℃. The concentrations of the starting materials are in the range of 0.1 to 9 mol / L, preferably 0.2 to 5 mol / L, for the titanium (IV) compound and in the range of 0.01 to 1 mol / L, preferably 0.02 to 0.2 mol / L for the trialkyl aluminum compound. The titanium component is added to the aluminum component over a period of 0.1 min to 60 min, preferably 1 min to 30 min, the molar ratio of titanium and aluminum in the final mixture being in the range of 1: 0.01 to 1: 4.

[0084] In another embodiment, a suitable catalyst system is obtained by a one or two-step reaction of a titanium (IV) compound with a trialkyl aluminum compound in an inert organic solvent at temperatures in the range of -40℃. to 200℃., preferably -20℃. to 150℃. In the first step the titanium (IV) compound is reacted with the trialkyl aluminum compound at temperatures in the range of -40℃. to 100℃., preferably -20℃. to 50℃. using a molar ratio of titanium to aluminum in the range of 1: 0.1 to 1: 0.8. The concentrations of the starting materials are in the range of 0.1 to 9.1 mol / L, preferably 5 to 9.1 mol / L, for the titanium (IV) compound and in the range of 0.05 and 1 mol / L, preferably 0.1 to 0.9 mol / L for the trialkyl aluminum compound. The titanium component is added to the aluminum compound over a period of 0.1 min to 800 min, preferably 30 min to 600 min. In a second step, if applied, the reaction product obtained in the first step is treated with a trialkyl aluminum compound at temperatures in the range of -10℃. to 150℃., preferably 10℃. to 130℃. using a molar ratio of titanium to aluminum in the range of 1: 0.01 to 1: 5.

[0085] In yet another embodiment, a suitable catalyst system is obtained by a procedure wherein, in a first reaction stage, a magnesium alcoholate is reacted with a titanium chloride in an inert hydrocarbon at a temperature of 50° to 100℃. In a second reaction stage the reaction mixture formed is subjected to heat treatment for a period of about 10 to 100 hours at a temperature of 110° to 200℃. accompanied by evolution of alkyl chloride until no further alkyl chloride is evolved, and the solid is then freed from soluble reaction products by washing several times with a hydrocarbon.

[0086] In a further embodiment, catalysts supported on silica, such as for example the commercially available catalyst system Sylopol 5917 can also be used.

[0087] Using such catalyst systems, the polymerization is normally carried out in suspension at low pressure and temperature in one or multiple steps, continuous or batch. The polymerization temperature is typically in the range of 30℃. to 130℃., preferably is the range of 50℃. and 90℃. and the ethylene partial pressure is typically less than 10 MPa, preferably 0.05 and 5 MPa. Trialkyl aluminums, like for example but not limited to isoprenyl aluminum and triisobutyl aluminum, are used as co-catalyst such that the ratio of Al: Ti (co-catalyst versus catalyst) is in the range of 0.01 to 100: 1, more preferably is the range of 0.03 to 50: 1. The solvent is an inert organic solvent as typically used for Ziegler type polymerizations. Examples are butane, pentane, hexane, cyclohexene, octane, nonane, decane, their isomers and mixtures thereof. The polymer molecular mass is controlled through feeding hydrogen. The ratio of hydrogen partial pressure to ethylene partial pressure is in the range of 0 to 50, preferably the range of 0 to 10. The polymer is isolated and dried in a fluidized bed drier under nitrogen. The solvent may be removed through steam distillation in case of using high boiling solvents. Salts of long chain fatty acids may be added as a stabilizer. Typical examples are calcium, magnesium and zinc stearate.

[0088] Optionally, other catalysts such as Phillips catalysts, metallocenes and post metallocenes may be employed. Generally a cocatalyst such as alumoxane or alkyl aluminum or alkyl magnesium compound is also employed. Other suitable catalyst systems include Group 4 metal complexes of phenolate ether ligands.

[0089] In accordance with the present disclosure, the high density polyethylene  polymer is formed into particles and combined with a plasticizer. Once combined with the plasticizer, a gel-like composition is produced that is then extruded to form various different articles, including porous membranes. In one embodiment, the polyethylene particles are made from a polyethylene polymer having a relatively low bulk density as measured according to DIN53466. For instance, in one embodiment, the bulk density is generally less than about 0.4 g / cm3, such as less than about 0.35 g / cm3, such as less than about 0.33 g / cm3, such as less than about 0.3 g / cm3, such as less than about 0.28 g / cm3, such as less than about 0.26 g / cm3. The bulk density is generally greater than about 0.1 g / cm3, such as greater than about 0.15 g / cm3. In one embodiment, the polymer has a bulk density of from about 0.2 g / cm3 to about 0.27 g / cm3.

[0090] In one embodiment, the polyethylene particles can be a free-flowing powder. The particles can have a median particle size (d50) by volume of less than 200 microns. For example, the median particle size (d50) of the polyethylene particles can be less than about 150 microns, such as less than about 125 microns. The median particle size (d50) is generally greater than about 20 microns. The powder particle size can be measured utilizing a laser diffraction method according to ISO 13320.

[0091] In one embodiment, 90%of the polyethylene particles can have a particle size of less than about 250 microns. In other embodiments, 90%of the polyethylene particles can have a particle size of less than about 200 microns, such as less than about 170 microns.

[0092] The molecular weight of the polyethylene polymer can vary depending upon the particular application. The polyethylene polymer, for instance, may have an average molecular weight, as determined according to the Margolies equation. The molecular weight can be determined by first measuring the viscosity number according to DIN EN ISO Test 1628. Dry powder flow is measured using a 25 mm nozzle. The molecular weight is then calculated using the Margolies equation from the viscosity numbers. The average molecular weight is generally greater than about 300,000 g / mol, such as greater than about 500,000 g / mol, such as greater than about 700,000 g / mol, such as greater than about 1,000,000 g / mol, such as greater than about 2,000,000 g / mol, such as greater than about 2,500,000 g / mol, such as greater than about 3,000,000 g / mol, such as greater than about 4,000,000  g / mol. The average molecular weight is generally less than about 12,000,000 g / mol, such as less than about 10,000,000 g / mol. In one aspect, the number average molecular weight of the high density polyethylene polymer can be less than about 4,000,000 g / mol, such as less than about 3,000,000 g / mol.

[0093] The polyethylene may have a viscosity number of from at least 100 mL / g, such as at least 500 mL / g, such as at least 1,500 mL / g, such as at least 2,000 mL / g, such as at least 4,000 mL / g to less than about 6,000 mL / g, such as less than about 5,000 mL / g, such as less than about 4000 mL / g, such as less than about 3,000 mL / g, such as less than about 1,000 mL / g, as determined according to ISO 1628 part 3 utilizing a concentration in decahydronapthalene of 0.0002 g / mL.

[0094] The high density polyethylene may have a crystallinity of from at least about 40%to 85%, such as from 45%to 80%.

[0095] Initially having the polyethylene polymer in the form of particles can facilitate blending with the plasticizer. In one embodiment, in forming polymer articles in accordance with the present disclosure, only polyethylene polymers having a molecular weight of greater than about 500,000 g / mol, such as greater than about 600,000 g / mol, such as greater than about 700,000 g / mol, such as greater than about 800,000 g / mol, such as greater than about 900,000 g / mol, such as greater than about 1,000,000 g / mol are used in producing the polymer articles. In one embodiment, only a single high molecular weight polyethylene polymer is used to produce the articles. Alternatively, the high molecular weight polyethylene polymer can be combined with other lower molecular weight polyethylene polymers.

[0096] When combined with a plasticizer, in general, the high density polyethylene particles are present in the polymer composition in an amount up to about 50%by weight. For instance, the high density polyethylene particles can be present in the polymer composition in an amount less than about 45%by weight, such as in an amount less than about 40%by weight, such as in an amount less than about 35%by weight, such as in an amount less than about 30%by weight, such as in an amount less than about 25%by weight, such as in an amount less than about 20%by weight, such as in an amount less than about 15%by weight. The polyethylene particles can be present in the composition in an amount greater  than about 5%by weight, such as in an amount greater than about 10%by weight, such as in an amount greater than about 15%by weight, such as in an amount greater than about 20%by weight, such as in an amount greater than about 25%by weight. During gel processing, a plasticizer is combined with the high density polyethylene particles which can be substantially or completely removed in forming polymer articles. For example, in one embodiment, the resulting polymer article can contain the high density polyethylene polymer in an amount greater than about 70%by weight, such as in an amount greater than about 80%by weight, such as in an amount greater than about 85%by weight, such as in an amount greater than about 90%by weight, such as in an amount greater than about 95%by weight.

[0097] In general, any suitable plasticizer can be combined with the polyethylene polymer as long as the plasticizer is capable of forming a gel-like material suitable for gel spinning or extruding.

[0098] The plasticizer, for instance, may comprise a hydrocarbon oil, an alcohol, an ether, an ester such as a diester, or mixtures thereof. For instance, suitable plasticizers include mineral oil, a paraffinic oil, decaline, and the like. Other plasticizers include xylene, dioctyl phthalate, dibutyl phthalate, stearyl alcohol, oleyl alcohol, decyl alcohol, nonyl alcohol, diphenyl ether, n-decane, n-dodecane, octane, nonane, kerosene, toluene, naphthalene, tetraline, and the like. In one embodiment, the plasticizer may comprise a halogenated hydrocarbon, such as monochlorobenzene. Cycloalkanes and cycloalkenes may also be used, such as camphene, methane, dipentene, methylcyclopentandiene, tricyclodecane, 1, 2, 4, 5-tetramethyl-1, 4-cyclohexadiene, and the like. The plasticizer may comprise mixtures and combinations of any of the above as well.

[0099] The plasticizer is generally present in the composition used to form the polymer articles in an amount greater than about 50%by weight, such as in an amount greater than about 55%by weight, such as in an amount greater than about 60%by weight, such as in an amount greater than about 65%by weight, such as in an amount greater than about 70%by weight, such as in an amount greater than about 75%by weight, such as in an amount greater than about 80%by weight, such as in an amount greater than about 85%by weight, such as in an amount greater than about 90%by weight, such as in an amount greater than  about 95%by weight, such as in an amount greater than about 98%by weight. In fact, the plasticizer can be present in an amount up to about 99.5%by weight.

[0100] The high density polyethylene particles blend with the plasticizer to form a homogeneous gel-like material.

[0101] In order to form polymer articles in accordance with the present disclosure, the high density polyethylene particles and the plasticizer are extruded through a die of a desired shape. In one embodiment, the composition can be heated within the extruder. For example, the plasticizer can be combined with the particle mixture and fed into an extruder. In accordance with the present disclosure, the plasticizer and particle mixture form a homogeneous gel-like material prior to leaving the extruder for forming polymer articles with little to no impurities.

[0102] In one embodiment, elongated articles are formed during the gel spinning or extruding process. The polymer article, for instance, may be in the form of a fiber or a film, such as a membrane.

[0103] During the process, at least a portion of the plasticizer is removed from the final product. The plasticizer removal process may occur due to evaporation when a relatively volatile plasticizer is used. Otherwise, an extraction liquid can be used to remove the plasticizer. The extraction liquid may comprise, for instance, a hydrocarbon solvent. One example of the extraction liquid, for instance, is dichloromethane. Other extraction liquids include acetone, chloroform, an alkane, hexene, heptene, an alcohol, or mixtures thereof.

[0104] If desired, the resulting polymer article can be stretched at an elevated temperature below the melting point of the polymer mixture to increase strength and modulus. Stretching of the polymer article can occur before the plasticizer is removed, after the plasticizer is removed, or while the plasticizer is being removed from the article. Suitable temperatures for stretching are in the range of from about ambient temperature to about 155℃. The draw ratios can generally be greater than about 4, such as greater than about 6, such as greater than about 8, such as greater than about 10, such as greater than about 15, such as greater than about 20, such as greater than about 25, such as greater than about 30. In certain embodiments, the draw ratio can be greater than about 50, such as greater than about 100, such as greater than about 110, such as greater than about 120,  such as greater than about 130, such as greater than about 140, such as greater than about 150. Draw ratios are generally less than about 1,000, such as less than about 800, such as less than about 600, such as less than about 400. In one embodiment, lower draw ratios are used such as from about 4 to about 10. The polymer article can be uniaxially stretched or biaxially stretched.

[0105] In accordance with the present disclosure, the polyethylene polymer contained within the polymer article is subjected to a treatment that causes polymer chain interactions, such as polar interactions or cross-linking. For instance, the polyethylene polymer can be cross-linked by exposure to radiation, can be chemically modified, or can undergo both radiation cross-linking and chemical modification. The manner and extent of polymer chain interactions or cross-linking can be carefully controlled in order to adjust one or more properties of the polymer article. In one embodiment, for instance, the treatment conditions are carefully controlled in order to increase the meltdown temperature of a porous membrane made from the polymer composition without deteriorating many of the other properties of the membrane. Cross-linking or other chain interactions can be initiated while the polymer article is being formed, such as during extrusion. Alternatively, cross-linking or other chain interactions can be initiated while the plasticizer is being removed from the polymer article and / or during stretching. In still another embodiment, cross-linking or other chain interactions can be initiated after the article has been formed and the plasticizer has been removed.

[0106] In one embodiment, the polyethylene polymer contained in the polymer article is cross-linked through exposure to radiation. The radiation can be, for instance, electron beam radiation, X-ray radiation, ultra-violet radiation, or gamma ray radiation.

[0107] In one aspect, the polymer article, such as the porous membrane, can undergo removal of the plasticizer and stretching and then dried prior to contact with ionizing radiation.

[0108] In one embodiment, the polyethylene polymer contained within the polymer article or porous membrane can be cross-linked using electron beam radiation. In fact, it was discovered that exposing the membrane to electron beam radiation improves the wettability of the membrane, while increasing the differential between the shutdown temperature and the meltdown temperature. Exposure to  electron beam radiation can occur while the polymer article is at room temperature. Alternatively, exposure to electron beam radiation can occur while the article is at a temperature of greater than about 28℃, such as greater than about 30℃, and generally less than about 120℃. In one embodiment, for instance, the polyethylene polymer can be exposed to electron beam radiation during stretching of the porous membrane, after stretching the membrane, or while removing the plasticizer.

[0109] During electron beam radiation, the accelerating voltage and the irradiation dose can be controlled. The accelerating voltage, for instance, can be, in one embodiment, less than 100 kV, such as less than about 90 kV, such as less than about 80 kV and generally greater than about 0.1 kV. Alternatively, the accelerating voltage can be about 20,000 kV or greater, such as greater than about 15,000 kV, such as greater than about 12,000 kV, such as greater than about 11,000 kV, such as greater than about 10,500 kV. The accelerating voltage is generally less than about 30,000 kV, such as less than about 25,000 kV, such as less than about 15,000 kV, such as less than about 12,000 kV.

[0110] The irradiation dose during electron beam exposure can generally be greater than about 25 kGy, such as greater than about 50 kGy, such as greater than about 75 kGy, such as greater than about 100 kGy, such as greater than about 125 kGy, such as greater than about 150 kGy, such as greater than about 175 kGy, such as greater than about 200 kGy, such as greater than about 225 kGy, such as greater than about 250 kGy, such as greater than about 275 kGy, such as greater than about 300 kGy, such as greater than about 305 kGy, such as greater than about 315 kGy, such as greater than about 325 kGy. The irradiation dose is generally less than about 500 kGy, such as less than about 450 kGy, such as less than about 400 kGy. In one aspect, higher irradiation doses may be preferred in order to more efficiently increase the meltdown temperature. In addition, electron beam radiation typically has a low irradiation depth. Thus, higher irradiation doses can ensure cross-linking throughout the thickness of the polymer article or membrane. Thus, in one embodiment, the irradiation dose is selected and occurs for a time sufficient such that cross-linking is uniform throughout the porous membrane.

[0111] In an alternative embodiment, the polyethylene polymer is cross-linked by exposure to gamma radiation. The use of gamma radiation has been found to increase the differential between shutdown temperature and meltdown temperature in porous membranes, while decreasing thermal shrinkage of the polymer article or membrane. Of particular advantage, gamma radiation can stabilize the permeability of porous membranes made in accordance with the present disclosure. In one aspect, the polymer article or porous membrane is exposed to gamma radiation at relatively low dose rates in order to achieve optimum results.

[0112] In still another embodiment, the polyethylene polymer can be cross-linked by exposure to X-ray radiation. The use of X-ray radiation can provide various advantages and benefits. For instance, X-ray radiation experiences a high irradiation depth. In addition, high dose rates can be used for minimizing time and exposure. Overall, an improved dose uniformity ratio can be experienced.

[0113] In still another embodiment, the polyethylene polymer can be cross-linked by exposure to ultra-violet radiation. When using ultra-violet radiation, a free radical initiator can be combined with the polyethylene polymer.

[0114] In an alternative embodiment, instead of or in addition to subjecting the polyethylene polymer to radiation, the polymer chains can be chemically cross-linked or otherwise modified to cause chain interactions. For instance, a chemical chain interactive agent can be incorporated into the polymer composition that is used to produce the polymer article. The chemical chain interactive agent can be activated at any time during the process in order to cross-link the polyethylene polymer or otherwise cause polymer chain interactions. For instance, polymer chain interactions, such as polar interactions or cross-linking, can occur during extrusion, during removal of the plasticizer, during stretching, and / or after the polymer article has been formed and dried. Chemical chain interactive agents that can be used include any suitable chemical group or species that promotes chain interactions.

[0115] In addition, any suitable technique can be used to modify the polyethylene polymer and cause chain interactions, such as cross-linking. For example, metal-ligand complexes can be formed between polymer chains by incorporating a chain interactive agent into the polymer and exposing the polymer  to a metal optionally in the presence of a pyridine. In another aspect, the chain interactive agent can be an ionomer that causes cross-linking to occur. In other aspects, the chain interactive agent on the polyethylene polymer can undergo multiple hydrogen bonding, such as triple hydrogen bonding or quadruple hydrogen bonding, to form chain interactions. Hydrogen bonding can occur in the presence of a nitrogen compound, such as ammonia, melamine, ureidopyrimidinone, or mixtures thereof.

[0116] In other embodiments, a diol can be used to cause ester cross-linking between the chain interactive agents incorporated into the polyethylene polymer chains. Alternatively, an amine, such as diamine, can be used to promote amide cross-linking with the chain interactive agents. In still another embodiment, the chain interactive agents can be used to form cross-links by undergoing a Diels-Alder reaction. A Diels-Alder reaction, for example, can occur in the presence of an amine, such as furfuryl amine, and an imide, such as bismaleimide.

[0117] As described above, any suitable chain interactive agent can be used to produce chain interactions within the polyethylene polymer. Once a chain interactive agent is selected, chain interactions can be formed using any suitable process or technique including any of the cross-linking techniques described above.

[0118] In one embodiment, for example, the chemical chain interactive agent can be a silane that is grafted to the polyethylene polymer. Cross-linking of the polymer or any other chain interaction can then occur using water or steam. If desired, a catalyst can also be added to the polymer composition that accelerates cross-linking. In one aspect, the silane grafted to the polyethylene polymer can be a vinylsilane. The polyethylene polymer can undergo solid state grafting with the vinylsilane followed by a condensation reaction that causes cross-linking.

[0119] In one embodiment, for instance, the silane incorporated into the polymer composition can be a vinylsilane having an alkoxy group. For instance, the silane can be trimethoxyvinylsilane, triethoxyvinylsilane, triacetoxyvinylsilane, or mixtures thereof. The vinylsilane can be combined with the polyethylene polymer in an amount generally greater than about 0.05%by weight, such as in an amount greater than about 0.1%by weight, such as in an amount greater than about 0.5%by weight, such as in an amount greater than about 0.75%by weight,  such as in an amount greater than about 1%by weight, such as in an amount greater than about 1.25%by weight, such as in an amount greater than about 1.5%by weight, such as in an amount greater than about 1.75%by weight, such as in an amount greater than about 2%by weight, such as in an amount greater than about 5%by weight, such as in an amount greater than about 8%by weight, such as in an amount greater than about 12%by weight, and generally less than about 30%by weight. The silane can be grafted onto the polyethylene polymer using any suitable method. In one aspect, the silane grafted polyethylene polymer is combined with a plasticizer to form a gel-like composition and extruded into a polymer article, such as a porous membrane. The porous membrane is then stretched and substantially all of the plasticizer is removed. After the porous membrane has been dried, the membrane can then be exposed to water in a way that causes cross-linking reactions to occur. For example, in one embodiment, the polymer article or porous membrane can be contacted with steam. The amount of silane incorporated into the polyethylene polymer in combination with the amount of steam that contacts the porous membrane can be used to control cross-linking in a manner that increases the meltdown temperature of the membrane to a desired level.

[0120] In addition to steam, the porous membrane can be contacted with water in other ways. For instance, the porous membrane can also be sprayed or dipped into a hot water bath. In still another embodiment, the porous membrane can be placed in a high humidity environment at an elevated temperature. For example, the humidity levels can be greater than about 70%and the temperature can be from about 30℃ to about 80℃, such as from about 40℃ to about 60℃.

[0121] In another embodiment, instead of using a silane, the chemical chain interactive agent can be an acrylic acid. The acrylic acid can be grafted to the polyethylene polymer contained in the polymer composition used to produce the polymer article. In one embodiment, the amount of acrylic acid incorporated into the polyethylene polymer can be greater than about 0.1%by weight, such as greater than about 1%by weight, such as greater than about 2%by weight, such as greater than about 3%by weight, such as greater than about 4%by weight, and generally less than about 25%by weight, such as less than about 15%by weight, such as less than about 10%by weight, such as less than about 8%by weight,  such as less than about 6%by weight, based on the total weight of the grafted polyethylene polymer.

[0122] In one aspect, the acrylic acid groups can be saponified by removing hydrogen atoms. The acrylic acid groups on the polymer resin can be saponified and / or the acrylic acid groups can be saponified after the polymer article is formed. The acrylic acid groups can be saponified using various different techniques and saponification agents. In one aspect, the acrylic acid groups can be exposed to a base, such as a sodium hydroxide solution. Alternatively, the acrylic acid groups can be exposed to a base in a solution optionally followed by contact with an inorganic salt, such as a metal salt, in an aqueous solution. The metal salt, for example, can be a calcium chloride. It is believed that treatment with a base, such as sodium hydroxide, causes deprotonation and removal of hydrogen atoms. The resulting carboxylate groups can be more polar which can lead to increasing polar interactions and higher melt down temperature. Further treatment with a metal salt may promote cross-linking. In an alternative aspect, the acrylic acid groups can be treated only with the metal salt.

[0123] The use of acrylic acid can provide various advantages and benefits. For example, it was unexpectedly discovered that the use of acrylic acid can more efficiently cross-link and / or cause polar interactions to occur within the polyethylene polymer and therefore more efficiently increase the meltdown temperature of polymer articles made from the polymer.

[0124] In one embodiment, an acrylic acid is grafted to a polyethylene polymer and formed into a polymer article, such as a porous membrane in accordance with the present disclosure. After the porous membrane is stretched and dried, acetic acid groups grafted to the polyethylene polymer can optionally be saponified, which causes the polyethylene chains to interact through cross-linking, through polar interactions, or through both.

[0125] For example, in one embodiment, a high density polyethylene polymer grafted with acrylic acid is combined with a plasticizer and formed into a porous membrane through gel extrusion. The porous membrane is then subjected to stretching and extraction. During extraction, greater than 90%, such as greater than about 95%, such as greater than about 98%of the plasticizer is removed. During stretching, the porous membrane can be stretched at a draw ratio of from  about 5 to about 10 in both the machine direction and the cross-machine direction. After or during stretching, the porous membrane can be annealed at a temperature of greater than about 100℃, such as greater than about 110℃, such as greater than about 115℃, and generally less than about 150℃, such as less than about 130℃ for a time of from about one minute to about 30 minutes, such as from about 5 minutes to about 15 minutes.

[0126] The resulting membrane can then optionally be contacted with a basic solution, such as a sodium hydroxide solution, can be contacted with a metal salt solution, or contacted with a basic solution followed by contact with a metal salt solution that causes the acrylic acid groups to saponify. For example, in one embodiment, the membrane can be contacted through spraying or by being submerged in an aqueous solution containing an inorganic salt. The inorganic salt, for instance, can be a metal salt, such as an alkaline earth metal halide salt. In one embodiment, for instance, the inorganic salt can be calcium chloride. The membrane, for instance, can be submerged in a calcium chloride solution at a temperature of about 23℃ or higher, such as from about 23℃ to about 60℃, such as from about 30℃ to about 50℃ for a time sufficient for saponification to occur. The calcium chloride solution can have any suitable concentration. For instance, the calcium chloride solution can be a 0.5 to about 3 molar calcium chloride solution. After saponification, the membrane can then be dried. During the process, the polyethylene polymer chains form interactions, such as cross-links or polar interactions. In particular, intrachain interactions and interchain interactions can occur. In one embodiment, the resulting cross-link structure can be formed:

[0127] In still another embodiment, the chemical chain interactive agent incorporated into the polymer composition can be an ionomer, such as a  polyethylene ionomer. The ionomer, for instance, can be an ethylene-methacrylate copolymer and / or an ethylene-acrylate copolymer.

[0128] In one embodiment, the ionomer is hygroscopic and can be compounded with the polyethylene polymer used to produce the polymer article. Once an ionomer is incorporated into the polymer composition, cross-linking can occur using any suitable method or technique. For instance, in one embodiment, the membrane can be exposed to a base, such as sodium hydroxide to remove hydrogen and afterwards exposed to a cross-linking catalyst, such as a metal salt, to induce cross-linking or other chain interactions. The ionomer can be incorporated into the polymer composition generally in an amount greater than about 3%by weight, such as in an amount greater than about 4%by weight, such as in an amount greater than about 5%by weight, and generally less than about 25%by weight, such as less than about 20%by weight, such as less than about 15%by weight, such as less than about 10%by weight, based upon the total weight of the polyethylene polymer and ionomer blend.

[0129] Any of the chemically modified polyethylene polymers described above can be combined with unmodified high density polyethylene polymers in formulating compositions for producing gel extruded articles. For example, based on the total amount of polyethylene polymers present, the modified polyethylene polymer can be present in an amount of from about 1%by weight to about 100%by weight, including all increments of 1%by weight therebetween. For instance, based on the total amount of polyethylene polymers present, the modified polyethylene polymer can be present in an amount greater than about 5%by weight, such as in an amount greater than about 10%by weight, such as in an amount greater than about 20%by weight, such as in an amount greater than about 30%by weight, such as in an amount greater than about 40%by weight, such as in an amount greater than about 50%by weight, such as in an amount greater than about 60%by weight, such as in an amount greater than about 70%by weight, such as in an amount greater than about 80%by weight.

[0130] When a high density polyethylene polymer grafted with acrylic acid groups is combined with a non-grafted high density polyethylene polymer, the resulting polymer blend can contain acrylic acid groups (or modified acrylic acid groups) in an amount greater than about 0.2%by weight, such as in an amount  greater than about 0.4%by weight, such as in an amount greater than about 0.8%by weight, such as in an amount greater than about 1%by weight, such as in an amount greater than about 1.5%by weight, such as in an amount greater than about 2%by weight, such as in an amount greater than about 2.5%by weight, such as in an amount greater than about 3%by weight, such as in an amount greater than about 3.5%by weight, such as in an amount greater than about 4%by weight, such as in an amount greater than about 4.5%by weight, and in an amount less than about 25%by weight, such as in an amount less than about 20%by weight, such as in an amount less than about 15%by weight, such as in an amount less than about 12%by weight, such as in an amount less than about 10%by weight, such as in an amount less than about 8%by weight.

[0131] Polymer articles made in accordance with the present disclosure have numerous uses and applications. For example, in one embodiment, the process is used to produce a membrane. The membrane can be used, for instance, as a battery separator. Alternatively, the membrane can be used as a microfilter. When producing fibers, the fibers can be used to produce nonwoven fabrics, ropes, nets, and the like. In one embodiment, the fibers can be used as a filler material in ballistic apparel.

[0132] Referring to Fig. 2, one embodiment of a lithium ion battery 10 made in accordance with the present disclosure is shown. The battery 10 includes an anode 12 and a cathode 14. The anode 12, for instance, can be made from a lithium metal. The cathode 14, on the other hand, can be made from sulfur or from an intercalated lithium metal oxide. In accordance with the present disclosure, the battery 10 further includes a porous membrane 16 or ion separator that is positioned between the anode 12 and the cathode 14. The porous membrane 16 minimizes electrical shorts between the two electrodes while allowing the passage of ions, such as lithium ions. As shown in Fig. 2, in one embodiment, the porous membrane 16 is a single layer polymer membrane and does not include a multilayer structure. In one aspect, the single layer polymer membrane may also include a coating. The coating can be an inorganic coating made from, for instance, aluminum oxide or a titanium oxide. Alternatively, the single layer polymer membrane may also include a polymeric coating. The coating can provide increased thermal resistance. In one embodiment, however, it should be  understood that the porous membrane or ion separator of the present disclosure can be coating free due to the increase in meltdown temperature.

[0133] Ion separators made according to the present disclosure can have various advantageous physical properties which can be a result of the cross-linking that occurs within the membrane. For instance, the membrane can have a relatively small thickness. The membrane, for instance, can have a thickness of less than about 25 nm, such as less than about 20 nm, such as less than about 18 nm, such as less than about 16 nm, such as less than about 14 nm, such as less than about 12 nm, such as less than about 8 nm, such as less than about 6 nm. The thickness of the membrane is generally greater than about 3 nm, such as greater than about 5 nm.

[0134] The porosity of the membrane can also be controlled based upon the final application. The porosity, for instance, can generally be greater than about 20%, such as greater than about 25%, such as greater than about 30%, such as greater than about 35%, such as greater than about 40%. The porosity is generally less than about 50%, such as less than about 45%, such as less than about 40%, such as less than about 38%.

[0135] The Gurley permeability can generally be greater than about 200 s, such as greater than about 210 s, such as greater than about 220 s, such as greater than about 230 s, such as greater than about 235 s. The Gurley permeability is generally less than about 270 s, such as less than about 250 s, such as less than about 245 s.

[0136] The polymer composition and polymer articles made in accordance with the present disclosure may contain various other additives, such as heat stabilizers, light stabilizers, UV absorbers, acid scavengers, flame retardants, lubricants, colorants, and the like.

[0137] In one embodiment, a heat stabilizer may be present in the composition. The heat stabilizer may include, but is not limited to, phosphites, aminic antioxidants, phenolic antioxidants, or any combination thereof.

[0138] In one embodiment, an antioxidant may be present in the composition. The antioxidant may include, but is not limited to, secondary aromatic amines, benzofuranones, sterically hindered phenols, or any combination thereof.

[0139] In one embodiment, a light stabilizer may be present in the composition.  The light stabilizer may include, but is not limited to, 2- (2′-hydroxyphenyl) -benzotriazoles, 2-hydroxy-4-alkoxybenzophenones, nickel containing light stabilizers, 3, 5-di-tert-butyl-4-hydroxbenzoates, sterically hindered amines (HALS) , or any combination thereof.

[0140] In one embodiment, a UV absorber may be present in the composition in lieu of or in addition to the light stabilizer. The UV absorber may include, but is not limited to, a benzotriazole, a benzoate, or a combination thereof, or any combination thereof.

[0141] In one embodiment, a halogenated flame retardant may be present in the composition. The halogenated flame retardant may include, but is not limited to, tetrabromobisphenol A (TBBA) , tetrabromophthalic acid anhydride, dedecachloropentacyclooctadecadiene (dechlorane) , hexabromocyclodedecane, chlorinated paraffins, or any combination thereof.

[0142] In one embodiment, a non-halogenated flame retardant may be present in the composition. The non-halogenated flame retardant may include, but is not limited to, resorcinol diphosphoric acid tetraphenyl ester (RDP) , ammonium polyphosphate (APP) , phosphine acid derivatives, triaryl phosphates, trichloropropylphosphate (TCPP) , magnesium hydroxide, aluminum trihydroxide, antimony trioxide.

[0143] In one embodiment, a lubricant may be present in the composition. The lubricant may include, but is not limited to, silicone oil, waxes, molybdenum disulfide, or any combination thereof.

[0144] In one embodiment, a colorant may be present in the composition. The colorant may include, but is not limited to, inorganic and organic based color pigments.

[0145] In one aspect, an acid scavenger may be present in the polymer composition. The acid scavenger, for instance, may comprise an alkali metal salt or an alkaline earth metal salt. The salt can comprise a salt of a fatty acid, such as a stearate. Other acid scavengers include carbonates, oxides, or hydroxides. Particular acid scavengers that may be incorporated into the polymer composition include a metal stearate, such as calcium stearate. Still other acid scavengers include zinc oxide, calcium carbonate, magnesium oxide, and mixtures thereof.

[0146] These additives may be used singly or in any combination thereof. In  general, each additive may be present in the polymer composition or in the resulting polymer article in an amount of at least about 0.05 wt. %, such as in an amount of at least about 0.1 wt. %, such as at least about 0.25 wt. %, such as at least about 0.5 wt. %, such as at least about 1 wt. %and generally less than about 20 wt. %, such as less than about 10 wt. %, such as less than about 5 wt. %, such as less than about 4 wt. %, such as less than about 2 wt. %. The sum of the wt. %of all of the components, including any additives if present, utilized in the polymer composition and articles will be 100 wt. %.

[0147] The present disclosure may be better understood with reference to the following examples. The following examples are given below by way of illustration and not by way of limitation. The following experiments were conducted in order to show some of the benefits and advantages of the present invention.

[0148] Example 1

[0149] The following example was conducted to demonstrate that resins made in accordance with the present disclosure yield membranes with higher meltdown temperatures compared to those of unmodified resins.

[0150] Various resin compositions were formulated containing a base resin of high density polyethylene. Specifically, the high density polyethylene polymer had an average molecular weight of 1.7 million g / mol. The resin compositions were prepared into membranes via gel extrusion, biaxial stretching, and solvent extraction as are conventional.

[0151] Specifically, porous polymer membranes were formed well suited for use as ion separators. Four different samples were produced. Sample Nos. 3 and 4 were subjected to electron beam radiation after drying. The irradiation dose was 150 kGy under vacuum.

[0152] The resulting samples were then tested for meltdown temperature and other physical properties. The following results were obtained.

[0153] The thickness, permeability and porosity of the membranes were also measured. Sample Nos. 1 and 2 had a thickness of 13 nm, a Gurley permeability of 178 s / 100 cc, and a porosity of 30%. Sample Nos. 3 and 4, on the other hand, had a thickness of 13.1 nm, a permeability of 178 sec / 100 cc, and a porosity of 30%. As shown, the meltdown temperature was significantly increased without changing the other above properties of the membrane.

[0154] Example No. 2

[0155] In this example, porous membranes were made according to the same process as described in Example No. 1 using a high density polyethylene polymer having an average molecular weight of 700,000 g / mol. The polyethylene polymer was grafted to acrylic acid in an amount of about 4.5%by weight. In some samples, the acrylic acid groups were saponified after extrusion, while in other samples, the groups were not saponified.

[0156] The grafted high density polyethylene polymer was combined with a non-grafted polyethylene polymer having the same molecular weight. The membranes were tested for melt down temperature and compared to the meltdown temperature of a membrane exclusively from the non-grafted high density polyethylene polymer. The ratio of grafted polyethylene polymer to non-grafted polyethylene polymer was varied in the different formulations. Some of the polymer compositions were made exclusively from the grafted polyethylene polymer.

[0157] The following polymer samples were formulated (remainder of composition was composed of non-grafted polyethylene polymer) :

[0158] The following results were obtained:

[0159] As shown by the examples above, high density polyethylene grafted with acrylic acid / acrylic acid salt (saponified) increases the melt down temperature of membranes when it is used alone or as a blend. This is believed to be due to chain interactions, such as polar interactions or ionic crosslinking. Treating the acrylic acid grafted polyethylene with sodium hydroxide and a calcium chloride aqueous solution increases the melt down temperature further.

[0160] These and other modifications and variations to the present invention may be practiced by those of ordinary skill in the art, without departing from the spirit and scope of the present invention, which is more particularly set forth in the appended claims. In addition, it should be understood that aspects of the various embodiments may be interchanged both in whole or in part. Furthermore, those of ordinary skill in the art will appreciate that the foregoing description is by way of example only and is not intended to limit the invention so further described in such appended claims.

Claims

1.An ion separator for dividing an anode from a cathode comprising: a porous polymer film, the porous polymer film comprising a high density polyethylene polymer, the polyethylene polymer having a number average molecular weight of greater than about 500,000 g / mol, and wherein the high density polyethylene polymer has been modified to form polymer chain interactions, and wherein the polymer film has a shutdown temperature of from about 120℃ to about 140℃ and has a meltdown temperature of from about 140℃ to about 230℃ and wherein the difference between the meltdown temperature and the shutdown temperature is greater than about 18℃.2.An ion separator as defined in claim 1, wherein the polymer chain interactions comprise cross-linking and wherein the polymer film has been cross-linked by exposure to radiation.3.An ion separator as defined in claim 2, wherein the radiation comprises electron beam radiation.4.An ion separator as defined in claim 2, wherein the radiation comprises X-ray radiation, ultra-violet radiation, or gamma ray radiation.5.An ion separator as defined in claim 1, wherein the polymer film has been chemically modified to form the polymer chain interactions.6.An ion separator as defined in claim 5, wherein the polyethylene polymer has been combined with a chemical chain interactive agent.7.An ion separator as defined in claim 6, wherein the chemical chain interactive agent comprises a silane, the silane being grafted to the polyethylene polymer.8.An ion separator as defined in claim 6, wherein the chemical chain interactive agent comprises a polyethylene ionomer, the polyethylene ionomer comprising an ethylene-methacrylate copolymer or an ethylene-acrylate copolymer.9.An ion separator as defined in claim 6, wherein the chemical chain interactive agent comprises an acrylic acid.10.An ion separator as defined in claim 9, wherein the acrylic acid has been grafted to the high density polyethylene polymer.11.An ion separator as defined in claim 10, wherein the acrylic acid groups grafted to the high density polyethylene polymer have been saponified to produce carboxylate groups.12.An ion separator as defined in claim 10 or 11, wherein the acrylic acid groups have been contacted with an inorganic salt.13.An ion separator as defined in claim 12, wherein the inorganic salt comprises a metal salt, such as an alkaline earth metal halide salt.14.An ion separator as defined in claim 12, wherein the inorganic salt comprises a calcium salt.15.An ion separator as defined in claim 14, wherein cross-links form that comprise -O-Ca-O-groups.16.An ion separator as defined in claim 10 or 11, wherein the acrylic acid groups have been contacted with a base, such as sodium hydroxide.17.An ion separator as defined in claim 10 or 11, wherein the acrylic acid groups have been contacted with a base, such as sodium chloride, and with an inorganic salt, such as an alkaline earth metal halide salt, such as a calcium salt.18.An ion separator as defined in any of claims 10-17, wherein the acrylic acid is present in the grafted polyethylene polymer in an amount from about 0.1%to about 25%by weight, such as in an amount from about 2%to about 12%by weight, such as in an amount from about 4%by weight to about 10%by weight.19.An ion separator as defined in any of the preceding claims, wherein the porous polymer film has a meltdown temperature of greater than about 145℃ , such as greater than about 152℃, such as greater than about 160℃, such as greater than about 165℃.20.An ion separator as defined in any of the preceding claims, wherein the difference between the meltdown temperature and the shutdown temperature is greater than about 20℃, such as greater than about 23℃, such as greater than about 28℃, such as greater than about 33℃, and less than about 110 ℃.21.An ion separator as defined in any of the preceding claims, wherein the porous polymer film has a thickness of from about 3 nm to about 25 nm, such as from about 4 nm to about 20 nm and has a porosity of from about 20%to about 50%, such as from about 25%to about 45%.22.An ion separator as defined in any of the preceding claims, wherein the high density polyethylene polymer is present in the membrane in an amount of from about 60%by weight to about 100%by weight.23.An ion separator as defined in claim 18, wherein the grafted polyethylene polymer is blended with a non-grafted polyethylene polymer to form a polymer blend and wherein the acrylic acid groups are present in the polymer blend in an amount greater than about 0.4%by weight, such as in an amount greater than about 0.8%by weight, such as in an amount greater than about 1.4%by weight, such as in an amount greater than about 1.8%by weight, such as in an amount greater than about 2%by weight, such as in an amount greater than about 2.2%by weight, such as in an amount greater than about 2.5%by weight, such as in an amount greater than about 2.7%by weight, such as in an amount greater than about 3%by weight, such as in an amount greater than about 3.4%by weight, such as in an amount greater than about 3.8%by weight, such as in an amount greater than about 4.2%by weight, such as in an amount greater than about 4.5%by weight, and in an amount less than about 20%by weight.24.A battery as defined in any of the preceding claims, wherein the ion separator is a single layer polymer membrane that may optionally include a coating.25.A battery as defined in claim 24, wherein the single layer polymer membrane includes a coating, the coating comprising an inorganic coating or a polymer coating.26.A process for producing a membrane comprising:combining a polymer composition with a plasticizer to form a gel-like composition, the polymer composition comprising a high density polyethylene polymer, the polyethylene polymer having a number average molecular weight of greater than about 500,000 g / mol;extruding the gel-like composition through a die to form a polymer membrane and removing at least a portion of the plasticizer; andcross-linking the polyethylene polymer contained in the polymer membrane an amount sufficient to increase a meltdown temperature of the membrane, and wherein the membrane has a shutdown temperature of from about 120℃ to about 140℃ and has a meltdown temperature of from about 140℃ to about 230℃ and wherein the difference between the meltdown temperature and the shutdown temperature is greater than about 18℃.27.A process as defined in claim 26, wherein the polyethylene polymer is cross-linked by exposing the polymer membrane to radiation, the radiation comprising electron beam radiation, X-ray radiation, ultra-violet radiation, or gamma ray radiation.28.A process as defined in claim 26, wherein the polymer composition contains a chemical chain interactive agent that causes the polyethylene polymer chains to form an interaction.29.A process as defined in claim 28, wherein the chain interactive agent comprises an acrylic acid and wherein after the polymer membrane is formed, the acrylic acid is saponified.30.A process as defined in claim 29, wherein the acrylic acid is saponified by being contacted with a sodium hydroxide solution, an alkaline earth metal halide salt solution, or a combination of both.

Citation Information

Patent Citations

  • Polyethylene composition for manufacturing lithium battery high-strength high-fusing temperature diaphragm

    CN105255201A

  • Improved microporous membranes, separators,lithium batteries, and related methods

    CN107636860A

  • Polymer composition for producing gel extruded articles and polymer articles made therefrom

    CN111094466A

  • Polymer compositions and films made therefrom with improved mechanical strength

    CN116096804A

  • Dry-process polyethylene membranes, coated membranes, separators, and related methods

    TW202231482A