Composite pole piece and preparation method therefor, battery cell and preparation method therefor
By designing the composite electrode sheet and its preparation method, the problem of difficult to control the alignment of the battery cell during high-speed preparation is solved, the manufacturing speed and safety performance are improved, the battery cell structure is simplified, and the efficient electrochemical performance is achieved.
Patent Information
- Application Number
- PCT/CN2024/094948
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-26
- Filing Date
- 2024-05-23
- Publication Date
- 2024-12-05
AI Technical Summary
The alignment of the existing battery cells is difficult to control during high-speed preparation, and the positions of the positive and negative electrodes and the diaphragm move relatively during subsequent movement, resulting in the alignment not meeting the requirements and posing a safety hazard.
Using composite electrode sheets, including composite fluid collectors, positive electrode material layer and negative electrode material layer, through the design of insulating layer, positive electrode conductor layer and negative electrode conductor layer, combined with the use of hot press composite and adhesive layers, a high alignment is prepared. The composite electrode sheet is formed by a stacking or winding structure.
It improves the manufacturing speed and superiority of the battery cell, ensures the high safety performance and electrochemical performance of the battery cell, simplifies the internal structure of the battery cell, and reduces internal circuit consumption.
Smart Images

Figure CN2024094948_05122024_PF_FP_ABST
Abstract
Description
Composite pole piece and preparation method thereof, battery cell and preparation method thereof
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to Chinese patent application number 2023106115313 filed with the China Patent Office on May 26, 2023, entitled “Composite electrode and preparation method thereof, battery cell and preparation method thereof”, the entire contents of which are incorporated by reference into this application. Technical Field
[0003] The present disclosure relates to the field of battery technology, and in particular to a composite pole piece and a preparation method thereof, a battery cell and a preparation method thereof. Background Art
[0004] In the prior art, the preparation process of battery cells has the following defects:
[0005] In a wound-type battery cell, the four-layer structure of separator 1 / positive electrode sheet / separator 2 / negative electrode sheet is wound using a winding needle and then flattened and shaped. The negative electrode sheet must extend beyond the positive electrode sheet on both sides in the TD direction, and separators 1 and 2 must extend beyond the negative electrode sheet. The alignment accuracy of these components is ±0.5mm. During high-speed winding, alignment is difficult to control. In addition, the wound core needs to be moved in subsequent processes, which can easily cause the positive and negative electrodes and the separator to shift relative to each other, resulting in alignment that does not meet production requirements.
[0006] The manufacturing process for stacked cells is as follows: placement of the negative electrode sheet, separator, positive electrode sheet, separator, and negative separator. The negative electrode sheet must extend beyond the positive electrode sheet on all sides, and the separator must extend beyond the negative electrode sheet after placement. The alignment accuracy requirement for these components is also ±0.5mm, making alignment difficult to control during stacking. Furthermore, subsequent steps require the stacked cores to be moved, which can easily cause the positive and negative electrodes and separator to shift relative to each other, resulting in alignment that does not meet manufacturing requirements.
[0007] The winding process requires prefabrication of two types of units: positive electrode / diaphragm / negative electrode / diaphragm / positive electrode, and negative electrode / diaphragm / positive electrode / diaphragm / negative electrode. Both units require the positive and negative electrodes and the separator to be hot-pressed together, and each component must be precisely aligned.
[0008] Therefore, existing technologies have difficulty controlling alignment issues during high-speed cell production. Furthermore, subsequent cell movement can cause relative movement of the positive and negative electrodes and the separator, resulting in substandard alignment. Furthermore, conventional current extraction methods in cells can easily cause conduction between the positive and negative electrodes, posing a safety hazard.
[0009] Summary of the Invention
[0010] The present disclosure provides a composite electrode sheet, comprising a composite current collector, a positive electrode material layer and a negative electrode material layer, wherein the composite current collector comprises an insulating layer, a positive electrode conductor layer and a negative electrode conductor layer; the positive electrode conductor layer is arranged on the first surface of the insulating layer, and the negative electrode conductor layer is arranged on the second surface of the insulating layer; the positive electrode material layer is arranged on the surface of the positive electrode conductor layer away from the insulating layer; the negative electrode material layer is arranged on the surface of the negative electrode conductor layer away from the insulating layer; the width of the insulating layer is ≥ the width of the positive electrode conductor layer ≥ the width of the positive electrode material layer; the width of the insulating layer is ≥ the width of the negative electrode conductor layer ≥ the width of the negative electrode material layer.
[0011] In some embodiments, the projection of the positive electrode material layer is located within the area of the insulating layer; the first end of the positive electrode conductor layer along its width direction is aligned with the first end of the insulating layer, and the second end of the positive electrode conductor layer along its width direction is aligned with the second end of the insulating layer or with the positive electrode material layer; the surface of the positive electrode conductor layer has a first reserved area for connecting a first external conductor.
[0012] In some embodiments, the projection of the negative electrode material layer is located inside the area of the insulating layer; the first end of the negative electrode conductor layer along its width direction is aligned with the second end of the insulating layer, and the second end of the negative electrode conductor layer along its width direction is aligned with the first end of the insulating layer or with the negative electrode material layer; the surface of the negative electrode conductor layer has a second reserved area for connecting a second external conductor.
[0013] In some embodiments, the first reserved area is connected to a first external conductor, the second reserved area is connected to a second external conductor, and both the first external conductor and the second external conductor are parallel to the negative electrode material layer.
[0014] In some embodiments, the first reserved area is connected to a first external conductor, the second reserved area is connected to a second external conductor, the first external conductor and the second external conductor are both perpendicular to the negative electrode material layer, and the first external conductor and the second external conductor are arranged face to face.
[0015] In some embodiments, the material of the first external conductor includes at least one of aluminum and stainless steel.
[0016] In some embodiments, the second external conductor is made of at least one of copper and nickel.
[0017] In some embodiments, the insulating layer has a thickness of 1 to 10 μm.
[0018] In some embodiments, the positive electrode conductor layer includes at least one of a first metal conductive foil and a first conductive plating layer.
[0019] In some embodiments, the thickness of the positive electrode conductor layer is 0.5 to 10 μm.
[0020] In some embodiments, the positive electrode material layer includes a positive electrode active material, and the positive electrode active material includes lithium cobalt oxide, lithium iron phosphate, lithium manganese iron phosphate, lithium manganese oxide, ternary positive electrode material, Prussian blue, sodium iron phosphate, sodium vanadium fluorophosphate, sodium vanadium phosphate and Na x At least one of NaxMO2, wherein M in the NaxMO2 is a transition metal element.
[0021] In some embodiments, the surface of the positive electrode conductor layer has a concave structure.
[0022] In some embodiments, the negative electrode conductor layer includes at least one of a second metal conductive foil and a second conductive plating layer.
[0023] In some embodiments, the thickness of the negative electrode conductor layer is 0.5 to 8 μm.
[0024] In some embodiments, the negative electrode material layer includes a negative electrode active material, and the negative electrode active material includes at least one of graphite, hard carbon, and lithium titanate.
[0025] In some embodiments, a first bonding layer is further provided between the positive electrode conductor layer and the insulating layer.
[0026] In some embodiments, a second bonding layer is further provided between the negative electrode conductor layer and the insulating layer.
[0027] In some embodiments, the thickness of the first adhesive layer and the second adhesive layer are both 0.2 to 2 μm.
[0028] In some embodiments, a first carbon glue layer is further provided between the positive electrode conductor layer and the positive electrode material layer.
[0029] In some embodiments, a second carbon glue layer is further provided between the negative electrode conductor layer and the negative electrode material layer.
[0030] In some embodiments, the first carbon adhesive layer and the second carbon adhesive layer both include a conductive carbon material and a binder; the mass ratio of the conductive carbon material to the binder is (0.8-1):(0.8-1).
[0031] The present disclosure provides a method for preparing the composite electrode, comprising the following steps:
[0032] (a) preparing a composite current collector; the composite current collector comprises an insulating layer, a positive electrode conductor layer and a negative electrode conductor layer;
[0033] (b) preparing a positive electrode material layer on the surface of the positive electrode conductor layer, wherein the preparation of the positive electrode material layer comprises: performing a first hot pressing composite of the positive electrode conductor layer and a positive electrode material sheet, or coating the surface of the positive electrode conductor layer with a positive electrode slurry;
[0034] (c) preparing a negative electrode material layer on the surface of the negative electrode conductor layer, wherein the preparation of the negative electrode material layer comprises: performing a second hot pressing composite of the negative electrode conductor layer and a negative electrode material sheet, or coating the surface of the negative electrode conductor layer with a negative electrode slurry;
[0035] Wherein, step (b) and step (c) are carried out in a certain order.
[0036] In some embodiments, the method for preparing the positive electrode material sheet specifically includes: subjecting a mixture of a positive electrode conductor and a positive electrode binder to a first stirring treatment under heating conditions, and then subjecting the mixture to a first airflow grinding treatment to obtain a first material, subjecting the mixture of the first material and a positive electrode active substance to a second stirring treatment under heating conditions, and then subjecting the mixture to a first extrusion molding and a first tableting treatment.
[0037] In some embodiments, the method for preparing the negative electrode material sheet specifically includes: subjecting the mixture of the negative electrode conductive agent and the negative electrode binder to a third stirring treatment under heating conditions, and then subjecting the mixture of the negative electrode conductive agent and the negative electrode binder to a second air flow grinding treatment to obtain a second material, subjecting the mixture of the second material and the negative electrode active material to a fourth stirring treatment, and then subjecting the mixture to a second extrusion molding and a second tableting treatment.
[0038] In some embodiments, the rotation speed of the first stirring process and the third stirring process are both 700-850 r / min, the time is both 50-70 min, and the heating temperature is both 55-65°C.
[0039] In some embodiments, the air inlet pressure of the first airflow grinding process and the second airflow grinding process are both 0.8-1.2 MPa, and the feeding pressure is both 0.8-1.2 MPa.
[0040] In some embodiments, the rotation speed of the second stirring process and the fourth stirring process are both 180-220 r / min, the time is both 1.5-2.5 h, and the heating temperature is both 45-55° C.
[0041] In some embodiments, the temperatures of the first extrusion molding and the second extrusion molding are both 95-105° C.; after the first extrusion molding and the second extrusion molding, a film with a thickness of 280-320 μm is obtained.
[0042] In some embodiments, the temperature of the first tableting process and the second tableting process are both 115-125°C.
[0043] In some embodiments, the temperature of the first hot pressing composite and the second hot pressing composite are both 190-210°C.
[0044] In some embodiments, the method for preparing the positive electrode material sheet further includes: adding a solid electrolyte to the mixture of the first material and the positive electrode active material.
[0045] In some embodiments, the method for preparing the negative electrode material sheet further includes: adding a solid electrolyte to the mixture of the second material and the negative electrode active material.
[0046] In some embodiments, the method further includes: disposing a first external conductor on the first reserved area of the positive electrode conductor layer; and disposing a second external conductor on the second reserved area of the negative electrode conductor layer.
[0047] In some embodiments, the method further includes preparing a first adhesive on one surface of the insulating layer and preparing a second adhesive on the other surface of the insulating layer.
[0048] In some embodiments, the method further includes: preparing a first carbon glue layer on the surface of the positive electrode conductor layer, and preparing a second carbon glue layer on the surface of the negative electrode conductor layer.
[0049] The present disclosure also provides a battery cell comprising at least one composite electrode; the composite electrode is the composite electrode described above, or a composite electrode prepared by the preparation method described above; the composite electrode constitutes a battery cell in a stacked or wound structure; the stacked structure at least includes a wound structure; the wound structure includes at least one of a square, wound and cylindrical structure.
[0050] The present disclosure also provides a method for preparing a battery cell, comprising the following steps:
[0051] The composite pole piece and the diaphragm are matched and stacked or wound to obtain a battery cell; the battery cell includes at least one of a stacked structure, a wound structure, a cylindrical structure and a square structure.
[0052] In some embodiments, the preparation method of the battery cell with the stacked structure specifically includes: placing multiple composite electrodes on a diaphragm, the diaphragm including a first reserved diaphragm, a electrode accommodating area and a second reserved diaphragm in sequence along its length direction; multiple composite electrodes are located in the electrode accommodating area; the positive electrode material layers of any two adjacent composite electrodes are oriented in opposite directions, the length direction of the multiple composite electrodes is the same as the length of the diaphragm, and are arranged in a row along the length direction of the diaphragm; using a first reserved diaphragm to wrap the first composite electrode close to the first reserved diaphragm; stacking is performed along the direction from the first reserved diaphragm to the second reserved diaphragm, with the first composite electrode wrapped with the first reserved diaphragm as the starting end, to obtain a battery cell with a stacked structure; in the battery cell with the stacked structure, multiple composite electrodes are arranged in layers.
[0053] In some embodiments, the method for preparing the battery cell with the wound structure specifically includes: stacking a composite electrode on the upper part of the diaphragm, the length direction of the composite electrode is the same as the length direction of the diaphragm; and winding from one end of the diaphragm to form a battery cell with a wound structure.
[0054] In some embodiments, the cylindrical battery cell includes a battery cell body structure, a first external conductor, and a second external conductor.
[0055] The preparation method of the battery cell with the battery cell body structure specifically includes: placing multiple composite pole pieces on a diaphragm, the diaphragm including a first reserved diaphragm, a pole piece accommodating area and a second reserved diaphragm in sequence along its length direction; multiple composite pole pieces are located in the pole piece accommodating area; the positive electrode material layers of any two adjacent composite pole pieces are oriented in opposite directions, the length direction of the multiple composite pole pieces is the same as the length of the diaphragm, and they are arranged in a row along the length direction of the diaphragm; using a first reserved diaphragm to wrap the first composite pole piece close to the first reserved diaphragm; stacking along the direction from the first reserved diaphragm to the second reserved diaphragm with the first composite pole piece wrapped around the first reserved diaphragm as the starting end to obtain a battery cell body structure; in the battery cell body structure, multiple composite pole pieces are stacked.
[0056] The first external conductor and the second external conductor are separated on both sides of the battery core and are arranged face to face with each other; the length directions of the first external conductor and the second external conductor are the same as the stacking direction of the composite electrode; on one side of the battery core, the first reserved area in the positive electrode conductive layer forms a bending area and is connected to the first external conductor; on the other side of the battery core, the second reserved area in the negative electrode conductive layer forms a bending area and is connected to the second external conductor.
[0057] The present disclosure also provides a battery cell, which is prepared by the battery cell preparation method. BRIEF DESCRIPTION OF THE DRAWINGS
[0058] In order to more clearly illustrate the technical solutions of the embodiments of the present disclosure, the following will briefly introduce the drawings required for use in the embodiments. It should be understood that the following drawings only represent the embodiments of the present disclosure by way of example, and the dimensional ratios in the drawings do not directly correspond to the actual ratios of the embodiments. At the same time, the following drawings only show certain embodiments of the present disclosure and therefore should not be regarded as limiting the scope.
[0059] FIG1 is a schematic diagram of the main structure of the composite electrode in Example 1 of the present disclosure;
[0060] FIG2 is a schematic diagram of the main structure of the composite electrode in Example 4 of the present disclosure;
[0061] FIG3 is a schematic diagram of the main structure of the composite electrode in Example 5 of the present disclosure;
[0062] FIG4 is a schematic diagram of a top view of the composite electrode in Example 1 of the present disclosure;
[0063] FIG5 is a schematic structural diagram of a battery cell in Example 11 of the present disclosure;
[0064] FIG6 is a schematic diagram of a cell winding process in Example 11 of the present disclosure;
[0065] FIG7 is a schematic structural diagram of a battery cell in Example 12 of the present disclosure;
[0066] FIG8 is a schematic structural diagram of the battery cell in Example 13 of the present disclosure.
[0067] Figure numerals: 1-insulating layer, 2-first bonding layer, 3-second bonding layer, 4-positive electrode conductor layer, 5-negative electrode conductor layer, 6-positive electrode material layer, 7-negative electrode material layer, 8-first external conductor, 9-second external conductor, 10-first carbon glue layer, 11-second carbon glue layer, 12-diaphragm, 100-composite electrode piece.
[0068] Implementation Method
[0069] Advantages of the embodiments in the summary of the invention will be explained in the embodiment section of the following specification, and some of them are obvious from the specification, or can be obtained through some embodiments of the disclosed embodiments.
[0070] The technical solution of the present disclosure will be further described below with reference to the accompanying drawings and through some implementation methods.
[0071] In order to make the purpose, technical solutions and advantages of the present disclosure more clear, the present disclosure is further described in detail below with reference to the accompanying drawings and examples. It should be understood that the embodiments described herein are only used to explain the present disclosure and are not intended to limit the present disclosure. In addition, the technical features involved in the various embodiments of the present disclosure described below can be combined with each other as long as they do not conflict with each other. Without departing from the principles of the embodiments of the present disclosure, several improvements and modifications can be made, and these improvements and modifications are also considered to be within the scope of protection of the embodiments of the present disclosure.
[0072] Some embodiments provide a composite electrode sheet, including a composite current collector, a positive electrode material layer and a negative electrode material layer, the composite current collector including an insulating layer, a positive electrode conductor layer and a negative electrode conductor layer; the positive electrode conductor layer is provided on the first surface of the insulating layer, and the negative electrode conductor layer is provided on the second surface of the insulating layer; the positive electrode material layer is provided on the surface of the positive electrode conductor layer away from the insulating layer; the negative electrode material layer is provided on the surface of the negative electrode conductor layer away from the insulating layer; the width of the insulating layer ≥ the width of the positive electrode conductor layer ≥ the width of the positive electrode material layer; the width of the insulating layer ≥ the width of the negative electrode conductor layer ≥ the width of the negative electrode material layer.
[0073] The composite pole piece disclosed herein can solve the technical problem of poor alignment of battery cells during high-speed preparation; the composite pole piece disclosed herein can improve manufacturing speed and quality rate, and at the same time, can ensure that the battery cells have high safety performance.
[0074] In some embodiments, the projection of the positive electrode material layer is located inside the area of the insulating layer; the first end of the positive electrode conductor layer along its width direction is aligned with the first end of the insulating layer, and the second end of the positive electrode conductor layer along its width direction is aligned with the second end of the insulating layer or with the positive electrode material layer; the surface of the positive electrode conductor layer has a first reserved area for connecting a first external conductor.
[0075] In some embodiments, the projection of the negative electrode material layer is located inside the area of the insulating layer; the first end of the negative electrode conductor layer along its width direction is aligned with the second end of the insulating layer, and the second end of the negative electrode conductor layer along its width direction is aligned with the first end of the insulating layer or with the negative electrode material layer; the surface of the negative electrode conductor layer has a second reserved area for connecting a second external conductor.
[0076] In some embodiments, the first reserved area is connected to the first external conductor; and the second reserved area is connected to the second external conductor.
[0077] In some embodiments, the first external conductor and the second external conductor are both parallel to the negative electrode material layer.
[0078] In some embodiments, the first external conductor and the second external conductor are both perpendicular to the negative electrode material layer and are arranged face to face with each other; a portion of the first external conductor region is a bent region and is connected to the first external conductor; a portion of the second external conductor region is a bent region and is connected to the second external conductor.
[0079] In some embodiments, the material of the first external conductor includes at least one of aluminum and stainless steel, such as aluminum foil or stainless steel foil.
[0080] In some embodiments, the material of the second external conductor includes at least one of copper and nickel, such as copper foil or nickel foil.
[0081] In some embodiments, the insulating layer comprises at least one of a polymer film and a non-woven fabric. In some embodiments, the insulating layer has a thickness of 1 to 10 μm, such as, but not limited to, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 10 μm, or any range consisting of any two thereof.
[0082] In some embodiments, the positive electrode conductor layer includes at least one of a first metal conductive foil and a first conductive coating. Both the first metal conductive foil and the first conductive coating are made of aluminum. In some embodiments, the thickness of the positive electrode conductor layer is 0.5 to 10 μm, such as, but not limited to, 0.5 μm, 0.8 μm, 1 μm, 2 μm, 5 μm, 6 μm, 7 μm, 10 μm, or any range consisting of any two thereof.
[0083] In some embodiments, the positive electrode material layer includes a positive electrode active material, and the positive electrode active material includes lithium cobalt oxide, lithium iron phosphate, lithium manganese iron phosphate, lithium manganese oxide, a ternary positive electrode material, Prussian blue, sodium iron phosphate, sodium vanadium fluorophosphate, sodium vanadium phosphate, and Na x At least one of MO2, wherein M in NaxMO2 is a transition metal element; wherein the transition metal element includes at least one of Fe, Co, Ni, Mn, Cr and Ti.
[0084] In some embodiments, the surface of the positive electrode conductor layer has a concave structure.
[0085] In some embodiments, the negative electrode conductor layer includes at least one of a second metal conductive foil and a second conductive coating. The second metal conductive foil and the second conductive coating are made of copper or aluminum. In some embodiments, the thickness of the negative electrode conductor layer is 0.5 to 8 μm, for example, but not limited to, 0.5 μm, 1 μm, 2 μm, 5 μm, 7 μm, 8 μm, or a range of any two thereof. In some embodiments, the negative electrode material layer includes a negative electrode active material, which includes at least one of graphite, hard carbon, and lithium titanate.
[0086] In some embodiments, a first bonding layer is further disposed between the positive electrode conductor layer and the insulating layer. In some embodiments, a second bonding layer is further disposed between the negative electrode conductor layer and the insulating layer. In some embodiments, the material of both the first bonding layer and the second bonding layer includes at least one of maleic anhydride-modified PP, polyacrylic acid, and a cross-linked epoxy resin. In some embodiments, the thickness of both the first bonding layer and the second bonding layer is 0.2 to 2 μm, for example, but not limited to, 0.2 μm, 0.5 μm, 1 μm, 2 μm, or any range thereof.
[0087] In some embodiments, a first carbon glue layer is further provided between the positive electrode conductor layer and the positive electrode material layer. In some embodiments, a second carbon glue layer is further provided between the negative electrode conductor layer and the negative electrode material layer. In some embodiments, both the first carbon glue layer and the second carbon glue layer include a conductive carbon material and a binder; the mass ratio of the conductive carbon material to the binder is (0.8-1):(0.8-1), for example, 1:1, etc. The present disclosure provides a carbon glue layer for effective bonding and can improve the electrochemical performance of the composite electrode. In some embodiments, the conductive carbon material includes at least one of conductive carbon black, conductive graphite, carbon nanotubes, and graphene. In some embodiments, the binder includes at least one of polyacrylate, styrene-butadiene rubber, and PVDF.
[0088] The method for preparing a composite pole piece in some embodiments comprises the following steps:
[0089] (a) preparing a composite current collector; the composite current collector comprises an insulating layer, a positive electrode conductor layer and a negative electrode conductor layer;
[0090] (b) preparing a positive electrode material layer on the surface of the positive electrode conductor layer, wherein the preparation of the positive electrode material layer comprises: performing a first hot pressing composite of the positive electrode conductor layer and the positive electrode material sheet, or coating the surface of the positive electrode conductor layer with a positive electrode slurry;
[0091] (c) preparing a negative electrode material layer on the surface of the negative electrode conductor layer, wherein the preparation of the negative electrode material layer includes: performing a second hot pressing composite of the negative electrode conductor layer and the negative electrode material sheet, or coating the surface of the negative electrode conductor layer with a negative electrode slurry;
[0092] Wherein, step (b) and step (c) are carried out in a certain order.
[0093] In some embodiments, both the positive electrode conductor layer and the negative electrode conductor layer are composited with the insulating layer by bonding, or composited with the insulating layer by evaporation.
[0094] In some embodiments, the preparation method of the composite current collector disclosed herein includes: coating a binder on one side of the insulating layer, drying to form a first binder layer, then thermally compounding with a positive electrode conductor, and then performing a first aging treatment to obtain a positive electrode conductor layer; coating a binder on the other side of the insulating layer, drying to form a second binder layer, then thermally compounding with a negative electrode conductor, and then performing a second aging treatment to obtain a negative electrode conductor layer. In some embodiments, the binder is coated on both sides of the insulating layer at a coating density of 0.8 to 1.2 g / m 2 In some embodiments, the temperature for thermally combining the positive electrode conductor and the negative electrode conductor is 75-85° C. In some embodiments, the temperature for the first aging treatment and the second aging treatment is 70-80° C., and the aging time is 4-6 days.
[0095] In some embodiments, the preparation method of the composite current collector includes: depositing a positive electrode conductor layer on one side of the insulating layer and evaporating a negative electrode conductor layer on the other side of the insulating layer. In some embodiments, the initial vacuum degree of the evaporation vacuum chamber is 4×10 -2 ~6×10 -2 In some embodiments, the initial evaporation temperature is 1300-1400° C. In one embodiment, the initial vacuum degree of the evaporation negative electrode conductor layer is 10 -5 Pa, the evaporation temperature is 1790~1850℃.
[0096] In some embodiments, the preparation method of the positive electrode material sheet specifically includes: subjecting the mixture of the positive electrode conductor and the positive electrode binder to a first stirring treatment under heating conditions, and then subjecting the mixture to a first air flow grinding treatment to obtain a first material, subjecting the mixture of the first material and the positive electrode active material to a second stirring treatment under heating conditions, and then subjecting the mixture to a first extrusion molding and a first tableting treatment.
[0097] In some embodiments, the preparation method of the negative electrode material sheet specifically includes: subjecting the mixture of the negative electrode conductive agent and the negative electrode binder to a third stirring treatment under heating conditions, and then subjecting the mixture to a second air flow grinding treatment to obtain a second material, subjecting the mixture of the second material and the negative electrode active material to a fourth stirring treatment, and then subjecting the mixture to a second extrusion molding and a second tableting treatment.
[0098] In some embodiments, the rotation speeds of the first stirring treatment and the third stirring treatment are both 700-850 r / min, for example, but not limited to 700 r / min, 750 r / min, 780 r / min, 800 r / min, 820 r / min or 850 r / min, or a range consisting of any two thereof; the stirring treatment time is 50-70 min, for example, but not limited to 50 min, 55 min, 60 min, 70 min, or a range consisting of any two thereof; the heating temperature is 55-65°C, for example, but not limited to 55°C, 58°C, 60°C, 65°C, or a range consisting of any two thereof.
[0099] In some embodiments, the air inlet pressure of the first air flow grinding treatment and the second air flow grinding treatment are both 0.8 to 1.2 MPa, for example, but not limited to 0.9 MPa, 1 MPa, 1.1 MPa, etc., or a range of values consisting of any two thereof; the feeding pressure is both 0.8 to 1.2 MPa, for example, but not limited to 0.9 MPa, 1 MPa, 1.1 MPa, etc., or a range of values consisting of any two thereof.
[0100] In some embodiments, the rotation speed of the second stirring treatment and the fourth stirring treatment is 180-220 r / min, for example, it can be but not limited to 180 r / min, 190 r / min, 200 r / min, 210 r / min, 220 r / min, etc., or a range value composed of any two thereof; the stirring treatment time is 1.5-2.5 h, for example, it can be but not limited to 1.5 h, 2 h or 2.5 h, etc., or a range value composed of any two thereof; the heating temperature is 45-55 ° C, for example, it can be but not limited to 45 ° C, 50 ° C, 55 ° C, etc., or a range value composed of any two thereof.
[0101] In some embodiments, the temperatures of the first extrusion molding and the second extrusion molding are both 95-105°C, for example, but not limited to 95°C, 100°C, 105°C, etc., or a range of values consisting of any two thereof; after the first extrusion molding and the second extrusion molding, a film with a thickness of 280-320 μm is obtained, for example, but not limited to 290 μm, 300 μm, 310 μm, etc., or a range of values consisting of any two thereof.
[0102] In some embodiments, the temperature of the first tableting process and the second tableting process are both 115-125° C., for example, but not limited to, 115° C., 120° C., 125° C., or a range of any two thereof.
[0103] In some embodiments, the temperatures of the first hot pressing and the second hot pressing are both 190-210° C., which can be but not limited to 195° C., 200° C., 205° C., etc., or a range consisting of any two thereof.
[0104] In some embodiments, the method for preparing the positive electrode material sheet further includes: adding a solid electrolyte to the mixture of the first material and the positive electrode active material.
[0105] In some embodiments, the method for preparing the negative electrode material sheet further includes: adding a solid electrolyte to the mixture of the second material and the negative electrode active material.
[0106] In some embodiments, the method further includes: disposing a first external conductor on the first reserved area of the positive conductor layer; and disposing a second external conductor on the second reserved area of the negative conductor layer. In some embodiments, the first external conductor is connected to the first reserved area by welding (ultrasonic welding), conductive adhesive bonding, riveting, etc.; and the second external conductor is connected to the second reserved area by welding (ultrasonic welding), conductive adhesive bonding, riveting, etc.
[0107] The present disclosure also relates to a battery cell, which includes at least one composite electrode; the composite electrode is a composite electrode, or a composite electrode prepared by a preparation method; the composite electrode constitutes the battery cell in a stacked or wound structure; the stacked structure at least includes a wound structure; the wound structure includes at least one of a square (Pounch) winding and a cylindrical (winding) structure.
[0108] Compared with the existing technology, the characteristics of this structure are as follows: the circuit in the battery cell forms an integral series connection, and the unit structure between adjacent separators contains both the positive electrode (or positive electrode material layer) and the negative electrode (or negative electrode material layer), while the unit structure between adjacent separators in the existing technology is a single positive electrode or a single negative electrode;
[0109] The advantage of this structure is that the battery cells are connected in series, which reduces internal circuit consumption and simplifies the structure of internal and external circuits.
[0110] In some embodiments, a method for preparing a battery cell with a stacked structure specifically includes: placing multiple composite electrodes on a diaphragm, the diaphragm including a first reserved diaphragm, a electrode accommodating area and a second reserved diaphragm in sequence along its length direction; multiple composite electrodes are located in the electrode accommodating area; the positive electrode material layers of any two adjacent composite electrodes are oriented in opposite directions, the length direction of the multiple composite electrodes is the same as the length of the diaphragm, and are arranged in a row along the length direction of the diaphragm; using a first reserved diaphragm to wrap the first composite electrode close to the first reserved diaphragm; stacking is performed along the direction from the first reserved diaphragm to the second reserved diaphragm, with the first composite electrode wrapped around the first reserved diaphragm as the starting end, to obtain a battery cell with a stacked structure; in the battery cell with a stacked structure, multiple composite electrodes are arranged in layers.
[0111] Compared with the existing stacking process, each repeating unit of the battery cell with the stacking structure disclosed in the present invention is the same composite electrode. There is no need to composite the diaphragm and the electrode before the stacking process, and there is no need to consider the alignment of the positive and negative electrodes. The process is simple, the production speed is fast, and the quality rate is high.
[0112] In some embodiments, a method for preparing a wound structure battery cell specifically includes: stacking a composite electrode on top of a diaphragm, with the length direction of the composite electrode being the same as the length direction of the diaphragm; and winding from one end of the diaphragm to form a wound structure battery cell.
[0113] Compared with existing technologies, the battery cell produced by the winding process disclosed in this disclosure simplifies assembly by winding a composite electrode sheet and a layer of separator without the need for alignment; only the separator needs to be ensured to extend beyond the electrode sheet. The process is simple, the production speed is fast, and the yield rate is high.
[0114] In some embodiments, a cylindrical battery cell includes a battery cell body structure, a first external conductor, and a second external conductor;
[0115] The preparation method of the battery cell body structure specifically includes: placing multiple composite electrode sheets on a diaphragm, the diaphragm including a first reserved diaphragm, a electrode sheet accommodating area and a second reserved diaphragm in sequence along its length direction; the multiple composite electrode sheets are located in the electrode sheet accommodating area; the positive electrode material layers of any two adjacent composite electrode sheets are oriented in opposite directions, the length direction of the multiple composite electrode sheets is the same as the length of the diaphragm, and the multiple composite electrode sheets are arranged in a row along the length direction of the diaphragm; using the first reserved diaphragm to wrap the first composite electrode sheet close to the first reserved diaphragm; stacking along the direction from the first reserved diaphragm to the second reserved diaphragm, with the first composite electrode sheet wrapped by the first reserved diaphragm as the starting end, to obtain the battery cell body structure; in the battery cell body structure, the multiple composite electrode sheets are stacked;
[0116] The first external conductor and the second external conductor are separated on both sides of the battery cell and are arranged face to face with each other; the length directions of the first external conductor and the second external conductor are the same as the stacking direction of the composite electrode sheet; on one side of the battery cell, the first reserved area in the positive electrode conductive layer forms a bending area and is connected to the first external conductor; on the other side of the battery cell, the second reserved area in the negative electrode conductive layer forms a bending area and is connected to the second external conductor.
[0117] In the cylindrical battery cell disclosed herein, the first external conductor region and the first external conductor are welded by laser welding, and the second external conductor region and the second external conductor are welded by laser welding. Example
[0118] The following are typical but non-limiting embodiments of the present disclosure:
[0119] Example 1
[0120] A composite electrode sheet, comprising a composite current collector, a positive electrode material layer 6, and a negative electrode material layer 7. The composite current collector comprises a positive electrode conductor layer 4, a first bonding layer 2, an insulating layer 1, a second bonding layer 3, and a negative electrode conductor layer 5 stacked in sequence; the negative electrode material layer 7 is disposed on a surface of the negative electrode conductor layer 5 away from the insulating layer 1; and the positive electrode material layer 6 is disposed on a surface of the positive electrode conductor layer 4 away from the insulating layer 1.
[0121] The width of the insulating layer 1 = the width of the positive electrode conductor layer 4 > the width of the positive electrode material layer 6, and the projection of the positive electrode material layer 6 is located in the center of the insulating layer 1; the surface of the positive electrode conductor layer 4 has a first reserved area; the width of the insulating layer 1 = the width of the negative electrode conductor layer 5 > the width of the negative electrode material layer 7; the projection of the negative electrode material layer 7 is located in the center of the insulating layer 1; the surface of the negative electrode conductor layer 5 has a second reserved area; the first reserved area is connected to the first external conductor 8, and the second reserved area is connected to the second external conductor 9, and the first external conductor 8 and the second external conductor 9 are arranged opposite to each other (located on both sides of the composite electrode sheet).
[0122] The method for preparing the composite electrode in this embodiment includes the following steps:
[0123] (1) Preparation of composite current collector: Using 4.5 μm PET as the substrate, ZAR-1902B adhesive produced by Zhengzhou Zhuoertai New Material Technology Co., Ltd. was evenly coated on one side of the PET surface and dried. The coating surface density was 1.0 g / m 2 After drying, heat-compounding with 5μm aluminum foil at a roller temperature of 80°C, and then aging at 75°C for 5 days; applying the above-mentioned adhesive to the other side of the PET surface and drying, heat-compounding with 4.5μm copper foil at a roller temperature of 80°C, and then aging at 75°C for 5 days to prepare a composite current collector; wherein, the positive electrode conductor layer 4 is a 5μm aluminum foil, and the negative electrode metal layer is a 4.5μm copper foil;
[0124] (2) The negative electrode conductor layer 5 of the composite current collector is coated with a graphite negative electrode slurry and dried, and then rolled to form a negative electrode material layer 7. The negative electrode slurry comprises 97% graphite active material, 1.5% CMC, and 1.5% SBR by mass, and the negative electrode material layer density is 102 g / m 2 , the density after roller pressing is 1.72g / cm 3 The positive electrode slurry is coated on the positive electrode conductor layer 4 and dried, and then rolled to form the positive electrode material layer 6. The positive electrode slurry comprises 97% positive electrode active material (lithium manganese iron phosphate), 1.5% conductive carbon black, and 1.5% PVDF by mass percentage. The positive electrode material layer density is 206.5g / m 2 , density after rolling: 4.15g / cm 3; Use 10μm aluminum foil as the first external conductor 8, adhere the 10μm aluminum foil to the positive conductor layer 4 with conductive glue and dry it; use 5μm copper foil as the second external conductor 9, adhere the 5μm copper foil to the negative conductor layer 5 with conductive glue and dry it to form a composite electrode with an electrical connection portion.
[0125] The schematic diagram of the front view structure of the composite electrode in this embodiment is shown in FIG1 , and the schematic diagram of the top view structure of the composite electrode is shown in FIG4 .
[0126] Example 2
[0127] A method for preparing a composite electrode, which differs from Example 1 in that: the PET thickness is 2 μm, and after being composited with aluminum foil, it is corroded in a NaOH solution with a mass content of 10% until the aluminum layer thickness is 0.5 μm, and then rinsed; the thickness of the thermally composite copper foil is 0.5 μm.
[0128] Example 3
[0129] A method for preparing a composite electrode is different from Example 1 in that: the thickness of PET is 10 μm, the thickness of the composite aluminum foil is 10 μm, and the thickness of the composite copper foil is 8 μm.
[0130] Example 4
[0131] A method for preparing a composite electrode comprises the following steps:
[0132] (1) Place the 6 μm insulating layer 1 (PP film) into the vacuum chamber of the evaporation coating machine, and evacuate the vacuum chamber to a vacuum degree of 5×10 -2 Pa, the evaporation mechanism is heated to 1350 ° C, and then aluminum is sent to the evaporation mechanism for evaporation, and the aluminum layer is evaporated on the PP film with a thickness of 1 μm to form the positive electrode conductor layer 4; the evaporation chamber of the vacuum ion evaporation equipment is evacuated to a vacuum degree of 10 -5 After Pa, the PP film with an aluminum layer on one side is passed through a copper plating roller. Copper metal with a purity of 99.9% is evaporated in an evaporation boat at 1800°C. Copper is then deposited on the side of the PP film without an aluminum layer. The copper layer has a thickness of 1 μm to form the negative electrode conductor layer 5.
[0133] (2) A graphite negative electrode slurry is coated on the negative electrode conductor layer 5 of the above-mentioned composite current collector and dried, and then rolled to form a negative electrode material layer 7, and the composition of the negative electrode slurry is the same as that of Example 1; a positive electrode slurry is coated on the positive electrode conductor layer 4 and dried, and then rolled to form a positive electrode material layer 6, and the composition of the positive electrode slurry is the same as that of Example 1; a 10μm aluminum foil is used as the first external conductor 8, and the 10μm aluminum foil is bonded to the positive electrode conductor layer 4 using a conductive adhesive and dried; a 5μm copper foil is used as the second external conductor 9, and the 5μm copper foil is bonded to the negative electrode conductor layer 5 using a conductive adhesive and dried to form a composite electrode sheet with an electrical connection portion.
[0134] The main structural diagram of the composite electrode in this embodiment is shown in FIG2 .
[0135] Example 5
[0136] A composite electrode sheet, as shown in FIG3 , includes a composite current collector, a positive electrode material layer 6, and a negative electrode material layer 7. The composite current collector includes a first carbon glue layer 10, a positive electrode conductor layer 4, an insulating layer 1, a negative electrode conductor layer 5, and a second carbon glue layer 11 stacked in sequence; the positive electrode material layer 6 is disposed on the surface of the first carbon glue layer 10, and the negative electrode material layer 7 is disposed on the surface of the second carbon glue layer 11;
[0137] The width of the insulating layer 1 is greater than the width of the positive electrode conductor layer 4 and greater than the width of the positive electrode material layer 6. The projection of the positive electrode material layer 6 is located at the center of the insulating layer 1. The first end of the positive electrode conductor layer 4 along its width direction is aligned with the first end of the insulating layer 1, and the second end of the positive electrode conductor layer 4 along its width direction is aligned with the positive electrode material layer 6. The surface of the positive electrode conductor layer 4 has a first reserved area.
[0138] The width of the insulating layer 1 is greater than the width of the negative electrode conductor layer 5 and is greater than the width of the negative electrode material layer 7; the projection of the negative electrode material layer 7 is located at the center of the insulating layer 1; the first end of the negative electrode conductor layer 5 along its width direction is aligned with the second end of the insulating layer 1, and the second end of the negative electrode conductor layer 5 along its width direction is aligned with the negative electrode material layer 7; the surface of the negative electrode conductor layer 5 has a second reserved area;
[0139] The first reserved area is connected to the first external conductor 8 , and the second reserved area is connected to the second external conductor 9 . The first external conductor 8 and the second external conductor 9 are arranged opposite to each other (located on both sides of the composite pole piece).
[0140] The method for preparing the composite electrode in this embodiment includes the following steps:
[0141] (1) Place the 6 μm insulating layer 1 (PI film) into the vacuum chamber of the evaporation coating machine, and evacuate the vacuum chamber to a vacuum degree of 5×10 -2Pa, the evaporation mechanism is heated to 1350 ° C, and then aluminum is sent to the evaporation mechanism for evaporation, and the aluminum layer is evaporated on the PP film with a thickness of 1 μm to form the positive electrode conductor layer 4; the evaporation chamber of the vacuum ion evaporation equipment is evacuated to a vacuum degree of 10 -5 After Pa, the PP film with an aluminum layer on one side is passed through a copper plating roller. Copper metal with a purity of 99.9% is evaporated in an evaporation boat at 1800°C. Copper is then deposited on the side of the PP film without an aluminum layer. The copper layer has a thickness of 1 μm to form the negative electrode conductor layer 5.
[0142] (2) coating a first carbon paste slurry on the positive electrode conductor layer 4 and drying it to form a first carbon paste layer 10; then coating a second carbon paste slurry on the negative electrode conductor layer 5 and drying it to form a second carbon paste layer 11; the first carbon paste slurry and the second carbon paste slurry are the same, both comprising conductive carbon black, PVDF and NMP, the mass ratio of the conductive carbon black to the PVDF being 1:1, and the solid content of the slurry being 25%, to obtain a composite current collector;
[0143] (3) Using a mixer with strong shear force, the conductive agent and the binder are mixed and stirred for 1 hour, the speed is controlled at 800r / min, and the stirring temperature is 60℃; then a jet mill is used for mechanical mixing to obtain a first material, the air inlet pressure is 1MPa, and the feeding pressure is 1MPa; the positive electrode active material is added to the first material, and the mixer is used for mixing, the mixer speed is 200r / min, the mixing time is 2h, and the stirring temperature is controlled to be 50℃, and then the obtained material is extruded at 100℃ through a screw extruder to obtain a continuous 300μm thick sheet, and the sheet is rolled into a 90μm film at 120℃, i.e., the positive electrode material sheet is hot-pressed and composited with the aluminum layer of the composite current collector, and the composite temperature is controlled at 200℃ to form a positive electrode material layer 6; wherein the mass ratio of the positive electrode active material, the conductive agent, and the binder is 86:4:10, the positive electrode active material is lithium manganese iron phosphate, the conductive agent is conductive carbon black, and the binder is PVDF;
[0144] (4) Using a mixer with strong shear force, the conductive agent and the binder are mixed and stirred for 1 hour, the speed is controlled at 800 r / min, and the stirring temperature is 60°C to obtain a dry powder; the dry powder is then mixed with a jet mill, the air inlet pressure is 1 MPa, and the feeding pressure is 1.0 MPa to obtain a second material; the negative electrode active material is added to the second material, the mixer speed is 200 r / min, the mixing time is 2 hours, the stirring temperature is controlled at 50°C, and the obtained material is extruded at 100°C through a screw The negative electrode material layer 7 is formed by extrusion molding using a machine to obtain a continuous sheet with a thickness of 300 μm, and the obtained sheet is rolled into a 120 μm film and a negative electrode material sheet at 120° C. The negative electrode material sheet is hot-pressed and composited with the second carbon glue layer 11 of the composite current collector, and the composite temperature is controlled at 200° C. to form a negative electrode material layer 7, wherein the mass ratio of the negative electrode active material, the conductive agent, and the binder is 87:3:10, the negative electrode active material is graphite, the conductive agent is conductive carbon black, and the binder is CMC and SBR with a mass ratio of 1:1.
[0145] Example 6
[0146] A method for preparing a composite electrode sheet, except that the material of the negative electrode conductor layer 5 is aluminum, other conditions are the same as those of Example 4. The composite electrode sheet in this embodiment is used for sodium batteries.
[0147] Example 7
[0148] A method for preparing a composite electrode, wherein the conditions are the same as those in Example 1 except that the first external conductor 8 uses a 20 μm stainless steel sheet and the second external conductor 9 uses a 9 μm nickel sheet.
[0149] Example 8
[0150] The preparation method of the composite electrode of this embodiment is the same as that of Example 1, except that the first external conductor 8 is a 10 μm aluminum foil connected to the positive electrode conductive layer by riveting; the second external conductor 9 is a 6 μm copper foil connected to the negative electrode conductor layer 5 by riveting.
[0151] Example 9
[0152] A method for preparing a composite pole piece, which differs from Example 8 in that: the first external conductor 8 is connected to the first reserved area by ultrasonic welding; and the second external conductor 9 is connected to the second reserved area by ultrasonic welding.
[0153] Example 10
[0154] A method for preparing a composite electrode sheet, which differs from Example 5 in that: a method for preparing a positive electrode material sheet and a negative electrode material sheet:
[0155] The method for preparing the positive electrode material sheet in this embodiment includes using LiCoO2 as the positive electrode active material and mixing the positive electrode active material, solid electrolyte material Li7P3S11, and conductive agent carbon black in a weight ratio of 6:3:1 to obtain a positive electrode mixture; then using a press to form a positive electrode coating sheet with a thickness of 100 μm; and thermally bonding the positive electrode material sheet to the surface of the first carbon glue layer 10 of the composite current collector to obtain a positive electrode material layer 6.
[0156] The difference between the method for preparing the negative electrode material sheet in this embodiment and the method for preparing the positive electrode material sheet in this embodiment is that a negative electrode active material is used, and the negative electrode active material is graphite.
[0157] Example 11
[0158] A method for preparing a battery cell with a stacked structure is prepared using the composite electrode 100 in Example 5, specifically comprising: placing multiple composite electrodes on a diaphragm 12, the diaphragm 12 including a first reserved diaphragm 12, an electrode accommodating area and a second reserved diaphragm 12 in sequence along its length direction; multiple composite electrodes are located in the electrode accommodating area; the positive electrode material layers 6 of any two adjacent composite electrodes are oriented in opposite directions, the length direction of multiple composite electrodes is the same as the length of the diaphragm 12, and they are arranged in a row along the length direction of the diaphragm 12; using the first reserved diaphragm 12 to wrap the first composite electrode close to the first reserved diaphragm 12; stacking is performed along the direction from the first reserved diaphragm 12 to the second reserved diaphragm 12, with the first composite electrode wrapped in the first reserved diaphragm 12 as the starting end to obtain a battery cell with a stacked structure; in the battery cell with the stacked structure, multiple composite electrodes are arranged in layers.
[0159] The structural diagram of the battery cell in this embodiment is shown in FIG5 .
[0160] The schematic diagram of the cell stacking process in this embodiment is shown in FIG6 .
[0161] Example 12
[0162] A method for preparing a battery cell with a wound structure, using the composite electrode in Example 5, specifically comprising: stacking the composite electrode on the upper part of a diaphragm 12, wherein the length direction of the composite electrode is the same as the length direction of the diaphragm 12; winding from one end of the diaphragm 12 to form a battery cell with a wound structure; the length of the diaphragm 12 is greater than the length of the composite electrode, and the width of the diaphragm 12 is greater than the width of the composite electrode.
[0163] The structural diagram of the battery cell in this embodiment is shown in FIG7 .
[0164] Example 13
[0165] A cylindrical battery cell, as shown in FIG8 , includes a battery cell body structure, a first external conductor 8 and a second external conductor 9;
[0166] The preparation method of the battery cell body structure specifically includes: placing multiple composite pole pieces in Example 5 (excluding the first external conductor 8 and the second external conductor 9 in Example 5) on a diaphragm 12, and the diaphragm 12 includes a first reserved diaphragm 12, a pole piece accommodating area, and a second reserved diaphragm 12 in sequence along its length direction; multiple composite pole pieces are located in the pole piece accommodating area; the positive electrode material layers 6 of any two adjacent composite pole pieces are oriented in opposite directions, and the length direction of the multiple composite pole pieces is the same as the length of the diaphragm 12, and are arranged in a row along the length direction of the diaphragm 12; using the first reserved diaphragm 12 to wrap the first composite pole piece close to the first reserved diaphragm 12; stacking along the direction from the first reserved diaphragm 12 to the second reserved diaphragm 12, with the first composite pole piece wrapped with the first reserved diaphragm 12 as the starting end, to obtain a battery cell body structure; in the battery cell body structure, multiple composite pole pieces are stacked;
[0167] The first and second external conductors 8, 9 in this cell are located on opposite sides of the cell, facing each other. The lengths of the first and second external conductors 8, 9 align with the stacking direction of the composite electrode sheets. On one side of the cell, a first reserved area in the positive conductive layer forms a bend and connects to the first external conductor 8. On the other side of the cell, a second reserved area in the negative conductive layer 5 forms a bend and connects to the second external conductor 9. The first external conductor is laser welded; the second external conductor 9 is laser welded. Industrial Applicability
[0168] In summary, the present disclosure provides a composite electrode sheet and its preparation method, as well as a battery cell and its preparation method. The composite electrode sheet can improve manufacturing speed and quality, ensuring that the battery cell has high safety and electrochemical performance. The preparation method is highly efficient, can improve product quality, and ensure that the battery cell has high safety performance.
Claims
1. A composite pole piece, characterized in that: The invention comprises a composite current collector, a positive electrode material layer and a negative electrode material layer, wherein the composite current collector comprises an insulating layer, a positive electrode conductor layer and a negative electrode conductor layer; the positive electrode conductor layer is arranged on the first surface of the insulating layer, and the negative electrode conductor layer is arranged on the second surface of the insulating layer; the positive electrode material layer is arranged on the surface of the positive electrode conductor layer away from the insulating layer; and the negative electrode material layer is arranged on the surface of the negative electrode conductor layer away from the insulating layer; The width of the insulating layer ≥ the width of the positive electrode conductor layer ≥ the width of the positive electrode material layer; The width of the insulating layer is greater than or equal to the width of the negative electrode conductor layer and greater than or equal to the width of the negative electrode material layer.
2. The composite pole piece according to claim 1, characterized in that: The projection of the positive electrode material layer is located inside the region of the insulating layer; the first end of the positive electrode conductor layer along its width direction is aligned with the first end of the insulating layer, and the second end of the positive electrode conductor layer along its width direction is aligned with the second end of the insulating layer or aligned with the positive electrode material layer; the surface of the positive electrode conductor layer has a first reserved region for connecting a first external conductor; And / or, the projection of the negative electrode material layer is located inside the area of the insulating layer; the first end of the negative electrode conductor layer along its width direction is aligned with the second end of the insulating layer, and the second end of the negative electrode conductor layer along its width direction is aligned with the first end of the insulating layer or with the negative electrode material layer; the surface of the negative electrode conductor layer has a second reserved area for connecting a second external conductor.
3. The composite pole piece according to claim 2, characterized in that: Contains one of the following features (1) or (2): (1) The first reserved area is connected to a first external conductor, and the second reserved area is connected to a second external conductor, and both the first external conductor and the second external conductor are parallel to the negative electrode material layer; (2) The first reserved area is connected to a first external conductor, and the second reserved area is connected to a second external conductor. The first external conductor and the second external conductor are both perpendicular to the negative electrode material layer, and the first external conductor and the second external conductor are arranged face to face.
4. The composite pole piece according to claim 3, characterized in that: Contains at least one of the following features (1) to (3): (1) The material of the first external conductor includes at least one of aluminum and stainless steel; (2) the material of the second external conductor includes at least one of copper and nickel; (3) The thickness of the insulating layer is 1 to 10 μm.
5. The composite pole piece according to claim 3, characterized in that: Contains at least one of the following features (1) to (4): (1) The positive electrode conductor layer includes at least one of a first metal conductive foil and a first conductive coating; (2) The thickness of the positive electrode conductor layer is 0.5 to 10 μm; (3) The positive electrode material layer includes a positive electrode active material, and the positive electrode active material includes lithium cobalt oxide, lithium iron phosphate, lithium manganese iron phosphate, lithium manganese oxide, ternary positive electrode material, Prussian blue, sodium iron phosphate, sodium vanadium fluorophosphate, sodium vanadium phosphate and Na x At least one of MO2, wherein M in the NaxMO2 is a transition metal element; (4) The surface of the positive electrode conductor layer has a concave structure.
6. The composite pole piece according to claim 3, characterized in that: Contains at least one of the following features (1) to (3): (1) The negative electrode conductor layer includes at least one of a second metal conductive foil and a second conductive coating; (2) The thickness of the negative electrode conductor layer is 0.5 to 8 μm; (3) The negative electrode material layer includes a negative electrode active material, and the negative electrode active material includes at least one of graphite, hard carbon and lithium titanate.
7. The composite pole piece according to claim 3, characterized in that: Contains one of the following features (1) to (3): (1) A first bonding layer is further provided between the positive electrode conductor layer and the insulating layer; (2) a second bonding layer is further provided between the negative electrode conductor layer and the insulating layer; (3) The thickness of the first adhesive layer and the second adhesive layer are both 0.2 to 2 μm.
8. The composite pole piece according to claim 3, characterized in that: Contains one of the following features (1) to (3): (1) A first carbon glue layer is further provided between the positive electrode conductor layer and the positive electrode material layer; (2) A second carbon glue layer is further provided between the negative electrode conductor layer and the negative electrode material layer; (3) Both the first carbon glue layer and the second carbon glue layer include a conductive carbon material and a binder; the mass ratio of the conductive carbon material to the binder is (0.8-1):(0.8-1).
9. The method for preparing a composite pole piece according to any one of claims 1 to 8, characterized in that: The following steps are involved: (a) preparing a composite current collector; the composite current collector comprises an insulating layer, a positive electrode conductor layer and a negative electrode conductor layer; (b) preparing a positive electrode material layer on the surface of the positive electrode conductor layer, wherein the preparation of the positive electrode material layer comprises: performing a first hot pressing composite of the positive electrode conductor layer and a positive electrode material sheet, or coating the surface of the positive electrode conductor layer with a positive electrode slurry; (c) preparing a negative electrode material layer on the surface of the negative electrode conductor layer, wherein the preparation of the negative electrode material layer comprises: subjecting the negative electrode conductor layer to a second hot pressing composite with a negative electrode material sheet, or coating the surface of the negative electrode conductor layer with a negative electrode slurry; There is no order of precedence for step (b) and step (c).
10. The method for preparing a composite pole piece according to claim 9, characterized in that: Contains at least one of the following features (1) to (2): (1) The method for preparing the positive electrode material sheet specifically comprises: subjecting a mixture of a positive electrode conductive agent and a positive electrode binder to a first stirring treatment under heating conditions, and then subjecting the mixture to a first airflow grinding treatment to obtain a first material, subjecting the mixture of the first material and a positive electrode active material to a second stirring treatment under heating conditions, and then subjecting the mixture to a first extrusion molding and a first tableting treatment; (2) The method for preparing the negative electrode material sheet specifically comprises: subjecting the mixture of the negative electrode conductive agent and the negative electrode binder to a third stirring treatment under heating conditions, and then subjecting the mixture to a second air flow grinding treatment to obtain a second material, subjecting the mixture of the second material and the negative electrode active material to a fourth stirring treatment, and then subjecting the mixture to a second extrusion molding and a second tableting treatment.
11. The method for preparing a composite pole piece according to claim 10, characterized in that: The invention comprises at least one of the following features (1) to (6): (1) The speed of the first stirring process and the third stirring process are both 700-850 r / min, and the time is 50-70min, heating temperature is 55-65℃; (2) The air inlet pressure of the first airflow grinding process and the second airflow grinding process are both 0.8-1.2 MPa, and the feed pressure is both 0.8-1.2 MPa; (3) The rotation speed of the second stirring treatment and the fourth stirring treatment are both 180-220 r / min, the time is both 1.5-2.5 h, and the heating temperature is both 45-55° C.; (4) The temperatures of the first extrusion molding and the second extrusion molding are both 95 to 105° C.; after the first extrusion molding and the second extrusion molding, a film with a thickness of 280 to 320 μm is obtained; (5) The temperature of the first tableting process and the second tableting process is 115 to 125° C.; (6) The temperatures of the first hot pressing and the second hot pressing are both 190 to 210°C.
12. The method for preparing a composite pole piece according to claim 10, characterized in that: Contains at least one of the following features (1) to (2): (1) The method for preparing the positive electrode material sheet further comprises: adding a solid electrolyte to the mixture of the first material and the positive electrode active material; (2) The method for preparing the negative electrode material sheet further includes: adding a solid electrolyte to the mixture of the second material and the negative electrode active material.
13. The method for preparing a composite pole piece according to claim 10, characterized in that: Contains at least one of the following features (1) to (3): (1) further comprising: disposing a first external conductor on a first reserved area of the positive electrode conductor layer; disposing a second external conductor on a second reserved area of the negative electrode conductor layer; (2) further comprising: preparing a first adhesive on one surface of the insulating layer and preparing a second adhesive on the other surface of the insulating layer; (3) The method further includes: preparing a first carbon glue layer on the surface of the positive electrode conductor layer, and preparing a second carbon glue layer on the surface of the negative electrode conductor layer.
14. A battery cell, characterized in that: The battery cell comprises at least one composite electrode; the composite electrode is the composite electrode according to any one of claims 1 to 8, or the composite electrode prepared by the preparation method according to any one of claims 9 to 13; The composite pole pieces are stacked or wound to form a battery cell; The stacked structure at least comprises a rolled structure; The winding structure includes at least one of a square, a winding and a cylindrical structure.
15. The method for preparing a battery cell according to claim 14, characterized in that: The following steps are involved: The composite electrode sheet and the separator are matched and stacked or wound to obtain a battery cell; The battery cell includes at least one of a stacked structure, a wound structure, a cylindrical structure and a square structure.
16. The method for preparing a battery cell according to claim 15, characterized in that: The method for preparing the battery cell of the stacked structure specifically comprises: A plurality of composite pole pieces are placed on a diaphragm, and the diaphragm includes a first reserved diaphragm, a pole piece accommodating area and a second reserved diaphragm in sequence along its length direction; the plurality of composite pole pieces are located in the pole piece accommodating area; the positive electrode material layers of any two adjacent composite pole pieces are oriented in opposite directions, the length direction of the plurality of composite pole pieces is the same as the length of the diaphragm, and the plurality of composite pole pieces are arranged in a row along the length direction of the diaphragm; a first reserved diaphragm is used to wrap a first composite pole piece close to the first reserved diaphragm; along the direction from the first reserved diaphragm to the second reserved diaphragm, the first composite pole piece wrapping the first reserved diaphragm is used as the starting end for stacking to obtain a battery cell with a stacked structure; in the battery cell with the stacked structure, the plurality of composite pole pieces are stacked.
17. The method for preparing a battery cell according to claim 15, characterized in that: The method for preparing the battery cell of the winding structure specifically comprises: The composite pole piece is stacked on the upper part of the diaphragm, and the length direction of the composite pole piece is the same as the length direction of the diaphragm; and winding is started from one end of the diaphragm to form a battery cell with a winding structure.
18. The method for preparing a battery cell according to claim 15, characterized in that: The cylindrical battery cell comprises a battery cell body structure, a first external conductor and a second external conductor; The method for preparing the battery core body structure specifically comprises: A plurality of composite pole pieces are placed on a diaphragm, wherein the diaphragm includes a first reserved diaphragm, a pole piece accommodating area, and a second reserved diaphragm in sequence along its length direction; the plurality of composite pole pieces are located in the pole piece accommodating area; the positive electrode material layers of any two adjacent composite pole pieces are oriented in opposite directions, the length direction of the plurality of composite pole pieces is the same as the length of the diaphragm, and the plurality of composite pole pieces are arranged in a row along the length direction of the diaphragm; the first composite pole piece close to the first reserved diaphragm is wrapped with the first reserved diaphragm; along the direction from the first reserved diaphragm to the second reserved diaphragm, the first composite pole piece wrapped with the first reserved diaphragm is used as the starting end to stack to obtain a battery cell body structure; in the battery cell body structure, the plurality of composite pole pieces are stacked; The first external conductor and the second external conductor are separated on both sides of the battery cell and arranged face to face; the length directions of the first external conductor and the second external conductor are the same as the stacking direction of the composite electrode sheet; on one side of the battery cell, the first reserved area in the positive electrode conductive layer forms a bending area and is connected to the first external conductor; on the other side of the battery cell, the second reserved area in the negative electrode conductive layer forms a bending area and is connected to the second external conductor.
Citation Information
Patent Citations
Composite pole piece and battery cell with composite pole piece
CN112117418A
Bipolar current collector battery, manufacturing method and electric equipment thereof
CN114512679A
Bipolar current collector and preparation method thereof, lithium ion battery and vehicle
CN114784289A
Composite pole piece, preparation method of composite pole piece, battery cell and preparation method of battery cell
CN116504919A
Collector for bipolar battery
JP2010277862A
Cited By
Pole piece and diaphragm compounding device, compounding method and compounding unit
CN121790692A