Display substrate and preparation method therefor, and display device
By adjusting the refractive index of the sub-pixel microcavity cushion layer in the OLED display substrate to match it with the corresponding color light wavelength, the problem of inconsistent structure thickness of the photon pixel microcavity of different colors is solved, and the display equality and light output effect are improved.
Patent Information
- Application Number
- PCT/CN2024/095854
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-30
- Filing Date
- 2024-05-28
- Publication Date
- 2024-12-05
AI Technical Summary
The thickness of the microcavity structure of photon pixels of different colors in the existing OLED display substrate is inconsistent, resulting in differences in light output and affecting the display equality.
By adjusting the refractive index of the sub-pixel microcavity cushion layer, it matches the corresponding color light wavelength, and meeting the constructive interference conditions, thereby reducing the thickness difference of the microcavity structure and improving display equality.
The difference in light output light effect between photon pixels of different colors is effectively reduced, and the display equality of multiple sub-pixels is improved.
Smart Images

Figure CN2024095854_05122024_PF_FP_ABST
Abstract
Description
Display substrate and manufacturing method thereof, and display device
[0001] This disclosure claims priority to Chinese patent application No. 202310627137.9, filed on May 30, 2023, entitled “A display substrate, a method for preparing the same, and a display device,” the entire contents of which are incorporated herein by reference. Technical Field
[0002] The present disclosure relates to the field of display technology, and more particularly to a display substrate and a preparation method thereof, and a display device. Background Art
[0003] OLED (Organic Light Emitting Diode) is an organic thin-film electroluminescent device with advantages such as simple preparation process, low cost, high luminous efficiency and easy formation of flexible structures. Therefore, display technology using OLED has become an important display technology.
[0004] To enhance the display quality of OLED products, current OLED products often utilize the microcavity effect to improve light output efficiency. For example, multiple sub-pixels within the display substrate of an OLED product have a microcavity structure, which enhances the light output efficiency of the sub-pixels.
[0005] Summary of the Invention
[0006] The present disclosure provides a display substrate, a method for manufacturing the same, and a display device that can improve the display balance of multiple sub-pixels. The technical solution is as follows:
[0007] In a first aspect, an embodiment of the present disclosure provides a display substrate, comprising:
[0008] A display substrate, comprising:
[0009] substrate;
[0010] A plurality of sub-pixels located on the substrate, wherein the sub-pixels have a microcavity structure, and the microcavity structure has a microcavity pad;
[0011] The refractive index of the microcavity pad layer in the sub-pixels corresponding to different color lights is different, and the refractive index of the microcavity pad layer in any sub-pixel matches the color light corresponding to the any sub-pixel. The refractive index of the microcavity pad layer matching any color light makes the microcavity structure where the microcavity pad layer is located meet the constructive interference condition of the any color light.
[0012] Optionally, the refractive index of the microcavity pad in any sub-pixel and the wavelength of the color light corresponding to any sub-pixel satisfy the following constraints:
[0013] Wherein, A is the optical path excluding the microcavity pad layer in the microcavity structure of any sub-pixel, and A is the same in the microcavity structures of the multiple sub-pixels, n is the refractive index of the microcavity pad layer in any sub-pixel, d is the thickness of the microcavity pad layer in any sub-pixel, k is a positive integer, and λ is the wavelength of the color light corresponding to any sub-pixel.
[0014] Optionally, the microcavity pads in the multiple sub-pixels have the same thickness.
[0015] Optionally, the materials of the microcavity pads in sub-pixels corresponding to light of different colors are the same or different.
[0016] Optionally, in response to the fact that the material of the microcavity pads in the sub-pixels corresponding to light of different colors is the same, the microcavity pads in the sub-pixels corresponding to light of different colors are doped with different particles.
[0017] Optionally, the sub-pixel further includes:
[0018] an undercut structure located on a side of the microcavity pad in the sub-pixel away from the substrate, the undercut structure having a recessed portion;
[0019] The undercut structure includes a first material layer and a second material layer, the first material layer is located on the side of the second material layer away from the substrate, and the orthographic projection of the surface of the first material layer surrounding the recessed portion on the substrate is located inside the orthographic projection of the surface of the second material layer surrounding the recessed portion on the substrate.
[0020] Optionally, the etching rate of the first material layer is lower than the etching rate of the second material layer.
[0021] Optionally, the first material layer and the second material layer satisfy any one of the following conditions:
[0022] The material of the first material layer is the same as the material with the slowest etching rate among the materials of the microcavity pad layers in the multiple sub-pixels, and the material of the second material layer is different from the material with the slowest etching rate among the materials of the microcavity pad layers in the multiple sub-pixels;
[0023] Furthermore, the material of the first material layer is different from the material with the fastest etching rate among the materials of the microcavity pads in the multiple sub-pixels, and the material of the second material layer is the same as the material with the fastest etching rate among the materials of the microcavity pads in the multiple sub-pixels.
[0024] Optionally, the plurality of sub-pixels include: a first sub-pixel and a second sub-pixel, the first sub-pixel is a blue sub-pixel, the second sub-pixel is a green sub-pixel, a material of a microcavity pad layer in the first sub-pixel includes silicon oxide, and a material of a microcavity pad layer in the second sub-pixel includes silicon nitride;
[0025] The first material layer is made of silicon oxide, and the second material layer is made of silicon nitride.
[0026] Optionally, the display substrate further includes a peripheral area surrounding the sub-pixel, the peripheral area including a first silicon oxide layer, a first silicon nitride layer, a second silicon nitride layer, and a second silicon oxide layer stacked in sequence;
[0027] The plurality of sub-pixels include: a first sub-pixel and a second sub-pixel, the sub-pixel further comprising: an undercut structure located on a side of the microcavity pad layer in the sub-pixel away from the substrate, the undercut structure having a recessed portion, the undercut structure comprising a first material layer and a second material layer, the first material layer being located on a side of the second material layer away from the substrate, an orthographic projection of a surface of the first material layer surrounding the recessed portion on the substrate being located inside an orthographic projection of a surface of the second material layer surrounding the recessed portion on the substrate;
[0028] Among them, the first silicon oxide layer is in the same layer as the microcavity pad layer in the first sub-pixel, the first silicon nitride layer is in the same layer as the microcavity pad layer in the second sub-pixel, the second silicon nitride layer is in the same layer as the second material layer, and the second silicon oxide layer is in the same layer as the first material layer.
[0029] Optionally, the sub-pixel further includes:
[0030] a reflective electrode layer located between the substrate and the microcavity pad layer;
[0031] a reflective electrode protection layer located between the reflective electrode layer and the microcavity pad layer;
[0032] a light-emitting layer and a semi-transparent electrode layer located on a side of the undercut structure away from the substrate and stacked in sequence;
[0033] A microcavity structure of the sub-pixel is formed between the reflective electrode layer and the semi-transparent electrode layer, and the multiple sub-pixels satisfy at least one of the following: the thickness and / or refractive index of the reflective electrode layer in the multiple sub-pixels are the same, the thickness and / or refractive index of the light-emitting layer in the multiple sub-pixels are the same, and the thickness and / or refractive index of the semi-transparent electrode layer in the multiple sub-pixels are the same.
[0034] Optionally, the microcavity pad layer of the sub-pixel has a via hole, and the via hole is filled with a conductive material, and the conductive material is used to electrically connect the structures on both sides of the microcavity pad layer.
[0035] Optionally, the via taper of the via hole is less than 45°.
[0036] In a second aspect, an embodiment of the present disclosure provides a display device, including a display substrate, wherein the display substrate includes:
[0037] substrate;
[0038] a plurality of sub-pixels having a microcavity structure, wherein the sub-pixels are located on the substrate, and the microcavity structure of the sub-pixels comprises a microcavity pad;
[0039] The refractive index of the microcavity pad layer in the sub-pixels corresponding to different color lights is different, and the refractive index of the microcavity pad layer in any sub-pixel matches the color light corresponding to the any sub-pixel. The refractive index of the microcavity pad layer matching any color light makes the microcavity structure where the microcavity pad layer is located meet the constructive interference condition of the any color light.
[0040] In a third aspect, an embodiment of the present disclosure provides a method for preparing a display substrate, the method comprising:
[0041] providing a substrate;
[0042] forming a plurality of sub-pixels on the substrate, wherein a microcavity structure is formed in the sub-pixels, and a microcavity pad is formed in the microcavity structure;
[0043] The refractive index of the microcavity pad layer in the sub-pixels corresponding to different color lights is different, and the refractive index of the microcavity pad layer in any sub-pixel matches the color light corresponding to the any sub-pixel. The refractive index of the microcavity pad layer matching any color light makes the microcavity structure where the microcavity pad layer is located meet the constructive interference condition of the any color light.
[0044] Optionally, forming a plurality of sub-pixels on the substrate includes:
[0045] forming a reflective electrode layer of the plurality of sub-pixels on the substrate;
[0046] On a side of the reflective electrode layer of the plurality of sub-pixels away from the substrate, sequentially forming the microcavity pad layers of the plurality of sub-pixels using the material of the microcavity pad layers in the plurality of sub-pixels;
[0047] On the side of the microcavity pad of the multiple sub-pixels away from the substrate, the light-emitting layers and the semi-transparent electrode layers of the multiple sub-pixels are formed in sequence to obtain the multiple sub-pixels, and the microcavity structure of any sub-pixel is formed between the reflective electrode layer and the semi-transparent electrode layer of any sub-pixel.
[0048] Optionally, the microcavity pad layers of the multiple sub-pixels are sequentially formed on a side of the reflective electrode layer of the multiple sub-pixels away from the substrate using the material of the microcavity pad layers in the multiple sub-pixels, including:
[0049] The microcavity pad layers of the multiple sub-pixels are formed in sequence using the materials of the microcavity pad layers in the multiple sub-pixels on the side of the reflective electrode layer of the multiple sub-pixels away from the substrate in an ascending order of etching rate of the materials of the microcavity pad layers in the multiple sub-pixels.
[0050] Optionally, the multiple sub-pixels include: a first sub-pixel and a second sub-pixel, the etching rate of the material of the microcavity pad layer in the first sub-pixel is lower than the etching rate of the material of the microcavity pad layer in the second sub-pixel, and the microcavity pad layers of the multiple sub-pixels are formed in sequence on a side of the reflective electrode layer of the multiple sub-pixels away from the substrate using the materials of the microcavity pad layers in the multiple sub-pixels in ascending order of etching rate, including:
[0051] forming a first material film on a side of the reflective electrode layer of the plurality of sub-pixels away from the substrate using the material of the microcavity pad layer in the first sub-pixel;
[0052] Etching the first material film to form a microcavity pad layer of the first sub-pixel;
[0053] After forming the microcavity pad layer of the first sub-pixel, forming a second material film on a side of the reflective electrode layer of the plurality of sub-pixels away from the substrate using the material of the microcavity pad layer in the second sub-pixel;
[0054] The second material film is etched to form a microcavity pad layer of the second sub-pixel.
[0055] Optionally, a ratio of an etching rate of a material of the microcavity pad layer in the first sub-pixel to an etching rate of a material of the microcavity pad layer in the second sub-pixel is less than or equal to a preset ratio threshold;
[0056] The material of the microcavity liner in the first sub-pixel includes silicon oxide, and the material of the microcavity liner in the second sub-pixel includes silicon nitride.
[0057] Optionally, after sequentially forming the microcavity pad layers of the multiple sub-pixels on the side where the reflective electrode layers of the multiple sub-pixels are away from the substrate using the material of the microcavity pad layers in the multiple sub-pixels, and before sequentially forming the light-emitting layers and the semi-transparent electrode layers of the multiple sub-pixels on the side where the microcavity pad layers of the multiple sub-pixels are away from the substrate, the method further includes:
[0058] Using a material with the fastest etching rate among the materials of the microcavity pad layers in the plurality of sub-pixels, a second material layer is formed on a side of the microcavity pad layers of the plurality of sub-pixels away from the substrate;
[0059] Using the material with the slowest etching rate among the materials of the microcavity pads in the plurality of sub-pixels, a first material layer is formed on a side of the second material layer of the plurality of sub-pixels away from the substrate;
[0060] The first material layer and the second material layer of the multiple sub-pixels are etched to form an undercut structure of the multiple sub-pixels, wherein the undercut structure has a recessed portion, and the orthographic projection of the surface of the first material layer surrounding the recessed portion on the substrate is located inside the orthographic projection of the surface of the second material layer surrounding the recessed portion on the substrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0061] FIG1 is a schematic diagram of a microcavity structure of a sub-pixel;
[0062] FIG2 is a schematic structural diagram of a display substrate in the related art;
[0063] FIG3 is a schematic structural diagram of a display substrate provided by an embodiment of the present disclosure;
[0064] FIG4 is a schematic diagram of the structure of a sub-pixel provided by an embodiment of the present disclosure;
[0065] FIG5 is a schematic diagram of the structure of another sub-pixel provided in an embodiment of the present disclosure;
[0066] FIG6 is a schematic diagram of the structure of another sub-pixel provided in an embodiment of the present disclosure;
[0067] FIG7 is a schematic flow chart of a method for preparing a display substrate according to an embodiment of the present disclosure;
[0068] FIG8 is a schematic flow chart of another method for preparing a display substrate provided by an embodiment of the present disclosure;
[0069] FIG9 is a schematic diagram of forming a display substrate provided by an embodiment of the present disclosure;
[0070] FIG10 is a schematic diagram showing the formation of another display substrate provided by an embodiment of the present disclosure;
[0071] FIG11 is a schematic diagram of forming another display substrate provided by an embodiment of the present disclosure;
[0072] FIG12 is a schematic diagram of forming another display substrate provided by an embodiment of the present disclosure;
[0073] FIG13 is a schematic diagram of forming another display substrate provided by an embodiment of the present disclosure;
[0074] FIG14 is a schematic diagram showing the formation of another display substrate provided by an embodiment of the present disclosure;
[0075] FIG15 is a schematic diagram showing the formation of another display substrate provided by an embodiment of the present disclosure;
[0076] FIG16 is a schematic diagram showing the formation of another display substrate provided by an embodiment of the present disclosure;
[0077] FIG17 is a schematic diagram of forming another display substrate provided by an embodiment of the present disclosure;
[0078] FIG18 is a schematic diagram showing the formation of another display substrate provided by an embodiment of the present disclosure;
[0079] FIG19 is a schematic diagram showing the formation of another display substrate provided by an embodiment of the present disclosure;
[0080] FIG20 is a schematic diagram showing the formation of another display substrate provided by an embodiment of the present disclosure;
[0081] FIG21 is a schematic diagram of forming another display substrate provided by an embodiment of the present disclosure;
[0082] FIG22 is a schematic diagram showing the formation of another display substrate provided by an embodiment of the present disclosure;
[0083] FIG23 is a schematic diagram showing the formation of another display substrate provided in an embodiment of the present disclosure. DETAILED DESCRIPTION
[0084] The following will be combined with the accompanying drawings in the embodiments of the present disclosure to clearly and completely describe the technical solutions in the embodiments of the present disclosure. Obviously, the embodiments described are only part of the embodiments of the present disclosure, rather than all the embodiments. Based on the embodiments of the present disclosure, all other embodiments obtained by ordinary technicians in this field based on the present disclosure are within the scope of protection of the present disclosure.
[0085] In order to improve the display effect of OLED products, current OLED products mostly use the microcavity effect to enhance the display light efficiency. For example, in the OLED product, multiple sub-pixels in the display substrate have a microcavity structure, and the sub-pixels use a microcavity structure to meet the constructive interference conditions of light waves, thereby enhancing the light-emitting light efficiency of the light waves. The microcavity structure meets the constructive interference conditions of light waves, which means that the optical path of light in the microcavity structure is an integer multiple of half the wavelength of the light wave. Figure 1 is a schematic diagram of a microcavity structure of a sub-pixel provided by the present disclosure. As shown in Figure 1, the microcavity structure includes a total reflection surface and a translucent surface (also called the light-emitting layer of the sub-pixel). After the light wave reaches the translucent surface of the sub-pixel in the microcavity structure, part of it is reflected and part is transmitted, so that there is a continuously oscillating light wave in the microcavity structure. When the optical path between the total reflection surface and the translucent surface is an integer multiple of half the wavelength of the light wave, the light-emitting light efficiency of the light wave in the microcavity structure is enhanced due to the constructive interference conditions.
[0086] At present, the thickness of the microcavity structure is mainly adjusted by adjusting the thickness of the microcavity pad layer in multiple sub-pixels, so that the microcavity structures of multiple sub-pixels meet the constructive interference conditions of light waves. As shown in Figure 2, the display substrate includes sub-pixel 1 and sub-pixel 2. The light wave emitted by sub-pixel 1 is smaller than the light wave emitted by sub-pixel 2. The microcavity structure of sub-pixel 1 includes microcavity pad layer 1. The microcavity structure of sub-pixel 2 includes microcavity pad layer 2. The thickness of microcavity pad layer 1 is smaller than the thickness of microcavity pad layer 2, so that the thickness D1 of the microcavity structure of sub-pixel 1 is smaller than the thickness D2 of the microcavity structure of sub-pixel 2.
[0087] However, because the wavelengths of light emitted by sub-pixels emitting different colors vary, adjusting the thickness of the microcavity structure to ensure constructive interference of light waves results in inconsistent thicknesses across sub-pixels emitting different colors. Furthermore, due to the light absorption effect, microcavity structures of varying thicknesses have varying light absorption capabilities, which in turn affects the light output efficiency. Consequently, sub-pixels emitting different colors experience varying light output efficiencies, leading to poor display uniformity across multiple sub-pixels.
[0088] In order to reduce the difference in light output efficiency between sub-pixels emitting light of different colors and improve the display balance of multiple sub-pixels, the embodiment of the present disclosure provides a display substrate. As shown in Figure 3, the display substrate provided by the embodiment of the present disclosure includes:
[0089] base 31;
[0090] A plurality of sub-pixels 32 are located on a substrate 31 , each of which has a microcavity structure, and a microcavity pad 321 is provided in the microcavity structure;
[0091] The refractive index of the microcavity pad 321 in the sub-pixels 32 corresponding to different colors of light is different, and the refractive index of the microcavity pad 321 in any sub-pixel 32 matches the color of light corresponding to that sub-pixel 32. The refractive index of the microcavity pad matching any color of light ensures that the microcavity structure in which the microcavity pad is located satisfies the constructive interference condition for that color of light. Any sub-pixel refers to any one of the multiple sub-pixels in the display substrate.
[0092] The above-mentioned display substrate 100 can be, for example, an organic light-emitting diode display substrate (OLED), a micro light-emitting diode (Micro LED) display substrate or a mini light-emitting diode (Mini Light Emitting) display substrate or a silicon-based OLED, etc., and the present disclosure does not make specific limitations on this. In one implementation, the above-mentioned base 31 can be a rigid substrate or a flexible substrate. The preparation material of the rigid substrate can include glass, quartz or plastic, etc. The preparation material of the flexible substrate can include PET (Polyethylene terephthalate), PEN (Polyethylenenaphthalate two formic acid glycol ester) or PI (Polyimide, polyimide), etc.
[0093] The multiple sub-pixels included in the display substrate may include multiple types of sub-pixels, and the color of the color light corresponding to the different types of sub-pixels is the color that the sub-pixel needs to display. For example, the display substrate includes red (R) sub-pixels, green (G) sub-pixels, and blue (B) sub-pixels. The color light required to be displayed by the red sub-pixel is red light, and the wavelength range is 622 to 760 nanometers (nm). The color light required to be displayed by the green sub-pixel is green light, and the wavelength range is 492 to 577nm. The color light required to be displayed by the blue sub-pixel is blue light, and the wavelength range is 435 to 450nm. The multiple sub-pixels 32 are located on the substrate 31, which means that the multiple sub-pixels 32 can be directly located on the substrate 31, or there can be an intermediate layer between the multiple sub-pixels 32 and the substrate 31.
[0094] In one implementation, the above-mentioned microcavity structure may include a total reflection surface and a semi-transparent surface. That is, the sub-pixel with a microcavity structure includes a total reflection surface and a semi-transparent surface, and the optical path between the total reflection surface and the semi-transparent surface meets the constructive interference condition of the color light emitted by the sub-pixel. Optionally, the total reflection surface can be the surface of the reflective electrode layer away from the substrate. The reflective electrode layer is, for example, an anode made of materials such as Al (aluminum), Ti (titanium) or Ag (silver). The semi-transparent surface can be the surface of the semi-transparent electrode layer close to the substrate. The semi-transparent electrode layer can include multiple material layers with different refractive indices, for example, composed of a metal and dielectric multilayer film, which is not specifically limited in the present disclosure.
[0095] Since the wavelengths of the color lights corresponding to different sub-pixels in the display substrate are inconsistent, in order to enable different sub-pixels to utilize the microcavity effect to enhance the luminous effect, it is necessary to make the optical path of the color lights emitted by different sub-pixels different. At present, the refractive index of each structural layer in the microcavity structure of different sub-pixels in the display substrate is the same. In order to enable different sub-pixels to utilize the microcavity effect to enhance the display light effect, when the refractive index of each structural layer is the same, the optical path of the different sub-pixel microcavity structures is adjusted by adjusting the thickness of the sub-pixel microcavity structure. For example, multiple sub-pixel microcavity structures include a microcavity pad layer, and the thickness of the sub-pixel microcavity structure is currently adjusted by adjusting the thickness of the microcavity pad layer. In this implementation method, since the thickness of the microcavity structure in different sub-pixels is inconsistent, and the thickness of the microcavity structure affects the light output efficiency, the light output efficiency of different sub-pixels is different, resulting in poor display balance of multiple sub-pixels.
[0096] In order to improve the display balance of multiple sub-pixels, in the embodiment of the present disclosure, the refractive index of the microcavity pad in the multiple sub-pixels 32 in the display substrate is different, and the refractive index of the microcavity pad 321 in any sub-pixel 32 matches the wavelength of the color light corresponding to the any sub-pixel 32. The refractive index of the microcavity pad that matches any color light makes the microcavity structure where the microcavity pad is located meet the constructive interference condition of the color light. Due to the different refractive indexes of the microcavity pads in different sub-pixels, the microcavity structures of the sub-pixels corresponding to different color lights all meet the constructive interference condition of the corresponding color light. Since the optical path is the product of the refractive index and thickness of the medium, compared to the case where the refractive index of the microcavity pad in the microcavity pad of multiple sub-pixels is the same, it is necessary to adjust the thickness of the microcavity pad. The present disclosure adjusts the refractive index of the microcavity pad, which is conducive to reducing the thickness of the microcavity pad. It can reduce the thickness difference of the microcavity pad in multiple sub-pixels corresponding to different color lights, reduce the difference in the microcavity structure in the sub-pixels, and thus reduce the difference in light output efficiency of the sub-pixels, thereby improving the display balance of multiple sub-pixels.
[0097] In one implementation, the refractive index of the microcavity pad in any of the above sub-pixels and the wavelength of the color light corresponding to the sub-pixel satisfy the following constraints:
[0098] Where A is the optical path length in the microcavity structure of the subpixel, excluding the microcavity pad layer. This optical path length is the same in the microcavity structures of multiple subpixels, meaning that the optical path lengths in the microcavity structures of subpixels corresponding to different colors of light are the same, excluding the microcavity pad layer. n is the refractive index of the microcavity pad layer in the subpixel. d is the thickness of the microcavity pad layer in the subpixel. k is a positive integer. λ is the wavelength of the color light corresponding to the subpixel.
[0099] For example, a display substrate includes sub-pixel 1 and sub-pixel 2, wherein:
[0100] The wavelength of the color light emitted by sub-pixel 1 is λ1, the refractive index of the microcavity cushion layer in its microcavity structure is n1, and the thickness of the microcavity cushion layer in the microcavity structure is d1, then:
[0101] The wavelength of the color light emitted by sub-pixel 2 is λ2, the refractive index of the microcavity cushion layer in its microcavity structure is n2, and the thickness of the microcavity cushion layer in the microcavity structure is d2, then:
[0102] For sub-pixel 1 and sub-pixel 2, the optical path lengths in their microcavity structures except for the microcavity cushion layer are the same, that is, they have the same A. Therefore, the refractive index and / or thickness of the microcavity cushion layer can be adjusted to make sub-pixel 1 and sub-pixel 2 meet the above constraints.
[0103] In one implementation, when the k values of multiple sub-pixels in a display substrate are the same, the refractive index of the microcavity pad in the multiple sub-pixels is positively correlated with the wavelengths of the color lights corresponding to the multiple sub-pixels. When the k values are the same, the longer the wavelength of the corresponding color light, the greater the refractive index of the microcavity pad. For example, when the k values are the same, the display substrate contains red sub-pixels, green sub-pixels, and blue sub-pixels. Since the wavelength of red light is greater than the wavelength of green light and the wavelength of blue light, the refractive index of the microcavity pad in the red sub-pixel is greater than the refractive index of the microcavity pad in the green sub-pixel and the refractive index of the microcavity pad in the blue sub-pixel. Since the optical path is the product of the refractive index and thickness of the medium, compared to the case where the refractive index in the microcavity pad of multiple sub-pixels corresponding to different color lights is the same, by adjusting the refractive index, the difference in the thickness of the microcavity pad in the multiple sub-pixels can be reduced.
[0104] In some current technologies, the refractive index of the microcavity backing layer in multiple sub-pixels is the same. Therefore, the optical path length is adjusted solely by thickness to match the optical path length of light in the sub-pixel's microcavity structure with the wavelength of the corresponding color light, resulting in different thicknesses for different sub-pixels. Based on this, the present disclosure uses a method of adjusting the refractive index to match the optical path length of light in the sub-pixel's microcavity structure with the wavelength of the corresponding color light, thereby reducing the thickness differences between multiple sub-pixels and improving the display balance of multiple sub-pixels corresponding to different colors of light.
[0105] In one approach, the present disclosure can achieve optical path and wavelength matching simply by adjusting the refractive index. In this case, the thickness of the microcavity pad in multiple sub-pixels is the same, which can minimize the difference in light output efficiency between different sub-pixels.
[0106] In another approach, the present disclosure can simultaneously adjust the thickness and refractive index of the microcavity pad layer, thereby enriching the means of optical path adjustment to better match different business needs. It should be noted that for the embodiments of the present disclosure, since the refractive index of the microcavity pad layer in any sub-pixel is positively correlated with the wavelength of the color light corresponding to the sub-pixel, even if there are differences in the thickness of the microcavity pad layer in the microcavity structure of multiple sub-pixels, the degree of difference is less than the degree of difference in thickness between the microcavity pad layers when the refractive index is the same in the related art.
[0107] In order to match the refractive index of the microcavity cushion layer in the sub-pixel with the wavelength of the color light corresponding to the sub-pixel, the material of the microcavity cushion layer in the embodiment of the present disclosure is a material with adjustable refractive index. Optionally, the material with adjustable refractive index includes at least one of SiO (silicon oxide), SiN (silicon nitride) and Al2O3 (aluminum oxide). The refractive index of each of the above materials can be adjusted by adjusting the film forming parameters. For example, in the process of preparing SiO, different particles can be doped in the process of preparing SiO to achieve adjustment of the refractive index of SiO. Alternatively, in the process of preparing the microcavity cushion layer, different particles are doped into the film layer formed by SiO to achieve adjustment of the refractive index of the microcavity cushion layer.
[0108] In one implementation, the material of the microcavity pad in multiple sub-pixels in the display substrate is the same. For example, the material of the microcavity pad in multiple sub-pixel microcavity structures can all be SiO, but the refractive index of the material SiO of the microcavity pad in different sub-pixel microcavity structures is different. For example, different refractive indices can be achieved by doping different particles into SiO. In another embodiment, the material of the microcavity pad in multiple sub-pixels in the display substrate is different. For example, the material of the microcavity pad in the green sub-pixel is SiN, and the material of the microcavity pad in the blue sub-pixel is SiO.
[0109] Optionally, due to the varying etching rates of different materials, when different sub-pixels use different materials for the microcavity liner, to reduce etching losses and prevent fluctuations in the cavity length of the microcavity structure due to etching losses, the order in which the microcavity liner is formed in sub-pixels corresponding to different colors can be inversely proportional to the etching rate of the material used to form the microcavity liner. Simply put, the slower the etching rate of the material, the earlier the material is used to form the microcavity liner.
[0110] In one implementation, the plurality of sub-pixels in the display substrate include: a first sub-pixel and a second sub-pixel, and the material of the microcavity pad layer in the first sub-pixel is silicon oxide, and the material of the microcavity pad layer in the second sub-pixel is silicon nitride. Because the etching rate of silicon oxide is lower than the etching rate of silicon nitride, the order of forming the microcavity pad layer in the first sub-pixel is earlier than the order of forming the microcavity pad layer in the second sub-pixel, that is, the microcavity pad layer of the first sub-pixel is first formed using silicon oxide, and then the microcavity pad layer of the second sub-pixel is formed using silicon nitride. Optionally, the first sub-pixel can be a blue sub-pixel, and the second sub-pixel can be a green sub-pixel.
[0111] In one implementation, in order to improve the stability of the sub-pixel structure, the sub-pixel 32 also includes: an undercut structure located on the side of the microcavity pad in the sub-pixel away from the substrate. Figure 4 is a structural schematic diagram of a sub-pixel provided by an embodiment of the present disclosure. As shown in Figure 4, the sub-pixel 32 includes a microcavity pad 321 and an undercut structure 322. The undercut structure 322 includes a first material layer 3221 and a second material layer 3222. The first material layer 3221 is located on the side of the second material layer 3222 away from the substrate. The undercut structure has a recessed portion, and the orthographic projection of the surface of the first material layer surrounding the recessed portion on the substrate is located inside the orthographic projection of the surface of the second material layer surrounding the recessed portion on the substrate. Due to the existence of the undercut structure 322, when other structural layers are formed on the undercut structure 322, the other structural layers can fill the recessed portion of the undercut structure 322, thereby improving the stability of the combination between the other structural layers and the undercut structure 322.
[0112] In order to form the undercut structure 322, the etching rate of the first material layer may be selected to be lower than the etching rate of the second material layer. In one implementation, the material of the first material layer 3221 in the undercut structure 322 of the multiple sub-pixels 32 is the same as the material with the slowest etching rate among the materials of the microcavity pads in the multiple sub-pixels 32; the material of the second material layer 3222 in the undercut structure 322 of the multiple sub-pixels 32 is different from the material with the slowest etching rate among the materials of the microcavity pads in the multiple sub-pixels 32. Exemplarily, when the multiple sub-pixels include the above-mentioned first sub-pixel and second sub-pixel, the material of the microcavity pad in the first sub-pixel is silicon oxide, and the material of the microcavity pad in the second sub-pixel is silicon nitride. Since the etching rate of silicon oxide is lower than the etching rate of silicon nitride, the material with the slowest etching rate among the materials of the microcavity pads in the multiple sub-pixels is silicon oxide. In this case, the material of the first material layer is silicon oxide, and the material of the second material layer is not silicon nitride.
[0113] In another implementation, the material of the first material layer 3221 in the undercut structure 322 of the multiple sub-pixels 32 is different from the material of the microcavity pad layer 321 having the fastest etching rate among the materials of the microcavity pad layers in the multiple sub-pixels 32; and the material of the second material layer 3222 in the undercut structure 322 of the multiple sub-pixels 32 is the same as the material of the microcavity pad layer 321 having the fastest etching rate among the materials of the microcavity pad layers in the multiple sub-pixels 32. Exemplarily, when the multiple sub-pixels include the first sub-pixel and the second sub-pixel, the material of the microcavity pad layer in the first sub-pixel is silicon oxide, and the material of the microcavity pad layer in the second sub-pixel is silicon nitride. Because the etching rate of silicon oxide is lower than the etching rate of silicon nitride, the material of the microcavity pad layer in the multiple sub-pixels having the fastest etching rate is silicon nitride. In this case, the material of the second material layer is silicon nitride, and the material of the first material layer is not silicon nitride.
[0114] Based on the above example, the material of the first material layer 3221 in the undercut structure 322 of the multiple sub-pixels 32 is the same as the material of the microcavity pad layer 321 with the slowest etching rate in the multiple sub-pixels 32; the material of the second material layer 3222 in the undercut structure 322 of the multiple sub-pixels 32 is the same as the material of the microcavity pad layer 321 with the fastest etching rate in the multiple sub-pixels 32. Exemplarily, when the multiple sub-pixels include the above-mentioned first sub-pixel and second sub-pixel, the material of the microcavity pad layer in the first sub-pixel is silicon oxide, and the material of the microcavity pad layer in the second sub-pixel is silicon nitride. Because the etching rate of silicon oxide is lower than the etching rate of silicon nitride, the material with the slowest etching rate among the materials of the microcavity pad layers in the multiple sub-pixels is silicon oxide, and the material with the fastest etching rate among the materials of the microcavity pad layers in the multiple sub-pixels is silicon nitride. In this case, the material of the first material layer is silicon oxide, and the material of the second material layer is silicon nitride.
[0115] Because the material of the first material layer in the undercut structure of the multiple sub-pixels is the same as the material with the slowest etching rate among the materials of the microcavity pad layer in the multiple sub-pixels, and the material of the second material layer in the undercut structure of the multiple sub-pixels is the same as the material with the fastest etching rate among the materials of the microcavity pad layer in the multiple sub-pixels, in order to form the recessed portion with a smaller top and a larger bottom in the undercut structure, the first material layer in the multiple sub-pixels is formed later than the second material layer, so that the first material layer is located on the side of the second material layer away from the backplane. At the same time, when etching the recessed portion, since the first material layer etches slower and the second material layer etches faster, a recessed portion with a smaller top and a larger bottom can be formed.
[0116] On this basis, in addition to the sub-pixels, the display panel also includes a peripheral area surrounding the sub-pixels. The peripheral area includes all or part of the material layers involved in the sub-pixel manufacturing process. In one implementation, the peripheral area includes a first silicon oxide layer, a first silicon nitride layer, a second silicon nitride layer, and a second silicon oxide layer stacked in sequence. Among them, the first silicon oxide layer is on the same layer as the microcavity pad layer in the first sub-pixel; the first silicon nitride layer is on the same layer as the microcavity pad layer in the second sub-pixel; the second silicon nitride layer is on the same layer as the second material layer, and the second silicon oxide layer is on the same layer as the first material layer. Among them, the two film layers being on the same layer means that the two film layers are formed by a single photolithography process.
[0117] Based on the above example, as shown in Figure 4, each sub-pixel 32 further includes a reflective electrode layer 323, a light-emitting layer 324, and a semi-transparent electrode layer 325. The reflective electrode layer 323 is located between the substrate 31 and the microcavity pad layer 321. The light-emitting layer 324 and the semi-transparent electrode layer 325 are located on the side of the undercut structure 322 away from the substrate 31 and are stacked in sequence. A microcavity structure is formed between the reflective electrode layer 323 and the semi-transparent electrode layer 325.
[0118] The multiple sub-pixels satisfy at least one of the following conditions: the thickness and / or refractive index of the reflective electrode layers in the multiple sub-pixels are the same, the thickness and / or refractive index of the light-emitting layers in the multiple sub-pixels are the same, and the thickness and / or refractive index of the semi-transparent electrode layers in the multiple sub-pixels are the same. When the thickness and refractive index of the reflective electrode layers in the multiple sub-pixels are the same, the thickness and refractive index of the light-emitting layers in the multiple sub-pixels are the same, and the thickness and refractive index of the semi-transparent electrode layers in the multiple sub-pixels are the same, the total optical path length of the light waves in the multiple sub-pixels through the reflective electrode layer, the light-emitting layer, and the semi-transparent electrode layer are the same. Thus, the total optical path length of the sub-pixels can be adjusted to match the optical path length of the color light emitted by the sub-pixels by adjusting the thickness and / or refractive index of the microcavity pad layer.
[0119] In one implementation, when the reflective electrode layer is made of a material that is easily corroded (such as Al), to protect the reflective electrode layer, as shown in FIG5 , each sub-pixel 32 further includes a reflective electrode protection layer 326 located between the reflective electrode layer 323 and the microcavity pad layer 321. The reflective electrode protection layer 326 can be made of a corrosion-resistant conductive material such as ITO (indium tin oxide).
[0120] Generally speaking, the microcavity pad layer is not conductive. In order to ensure that the structures on both sides of the microcavity pad layer can be electrically connected, as shown in Figure 6, the microcavity pad layer 321 may have a via (Via) 327, and the via hole is filled with a conductive material to electrically connect the structures on both sides of the microcavity pad layer through the conductive material. In one implementation, when the structures on both sides of the microcavity pad layer include a reflective electrode layer and a light-emitting layer, the conductive material in the via hole can electrically connect the reflective electrode layer and the light-emitting layer. For another example, when the structures on both sides of the microcavity pad layer include a reflective electrode protective layer and a light-emitting layer, the conductive material in the via hole can electrically connect the reflective electrode protective layer and the light-emitting layer. For another example, when the structures on both sides of the microcavity pad layer include a reflective electrode layer and an ITO layer, the conductive material in the via hole can electrically connect the reflective electrode layer and the ITO layer.
[0121] In one implementation, when vias are used to connect the structures on both sides of the microcavity pad, the via taper of the via in the microcavity pad of each sub-pixel is less than a specified angle threshold. The specified angle threshold can be controlled based on demand and experience. Optionally, to ensure that the structures on both sides of the microcavity pad are overlapped without abnormalities, the specified angle threshold can be 45°.
[0122] In one embodiment, the present disclosure further provides a display device. The display device includes the display substrate provided in the above-described embodiment of the present disclosure. Optionally, the display device includes, but is not limited to, mobile phones, computers, televisions, game consoles, automotive displays, electronic paper, tablet computers, laptop computers, digital photo frames, and navigation systems, and any other product or component with a display function.
[0123] In order to reduce the difference in light output effects between different sub-pixels and improve the display balance of multiple sub-pixels, corresponding to the display substrate provided in the embodiment of the present disclosure, as shown in Figure 7, the embodiment of the present disclosure also provides a method for preparing a display substrate, which includes steps S701-S702.
[0124] S701, providing a substrate.
[0125] Before forming the display substrate, a substrate is provided. The substrate may be a rigid substrate or a flexible substrate, which is not specifically limited in this disclosure. In one implementation, the substrate may include a CMOS (Complementary Metal-Oxide-Semiconductor) substrate.
[0126] S702, forming a plurality of sub-pixels on a substrate, wherein a microcavity structure is formed in the sub-pixels, and a microcavity cushion layer is formed in the microcavity structure; wherein the refractive index of the microcavity cushion layer in the sub-pixels corresponding to different colors of light is different, and the refractive index of the microcavity cushion layer in any sub-pixel matches the color of light corresponding to the sub-pixel, and the refractive index of the microcavity cushion layer matching any color of light makes the microcavity structure where the microcavity cushion layer is located meet the constructive interference condition of the color of light.
[0127] In this step, multiple sub-pixels can be formed on the substrate. The refractive index of the microcavity pad in the multiple sub-pixels is different, and the refractive index of the microcavity pad in any sub-pixel matches the wavelength of the color light corresponding to the sub-pixel. The refractive index of the microcavity pad matched with any color light makes the microcavity structure where the microcavity pad is located meet the constructive interference condition of any color light. In one implementation, the refractive index of the microcavity pad in any sub-pixel and the wavelength of the color light corresponding to any sub-pixel meet the following constraints:
[0128] Wherein, A is the optical path excluding the microcavity pad layer in the microcavity structure of any sub-pixel, and A is the same in the microcavity structures of multiple sub-pixels, n is the refractive index of the microcavity pad layer in any sub-pixel, d is the thickness of the microcavity pad layer in any sub-pixel, k is a positive integer, and λ is the wavelength of the color light corresponding to any sub-pixel.
[0129] In this way, since the refractive index of the microcavity pad layer matching any color of light makes the microcavity structure in which the microcavity pad layer is located meet the constructive interference condition for that color of light, the refractive index of the microcavity pad layer can be adjusted to make the microcavity structure of the sub-pixel meet the constructive interference condition for the corresponding color of light. Therefore, compared to the method of simply adjusting the thickness of the microcavity pad layer, the present disclosure can reduce the thickness difference of the microcavity pad layer in multiple sub-pixels of different wavelengths by adjusting the refractive index of the microcavity pad layer, thereby reducing the difference in light output efficiency of different sub-pixels and improving the display balance of multiple sub-pixels.
[0130] In one embodiment, as shown in FIG8 , step S702 includes steps S801 - S803 .
[0131] S801 , forming a reflective electrode layer of a plurality of sub-pixels on a substrate.
[0132] In one implementation, the thickness and / or refractive index of the reflective electrode layer in multiple sub-pixels may be the same. The reflective electrode layer may be the anode layer or cathode layer of the sub-pixel, which is not specifically limited in this disclosure. Optionally, as shown in FIG9 , a metal coating may be first performed on the substrate to obtain a metal film. For example, a metal such as Al (aluminum), Ti (titanium), or Ag (silver) may be used for coating to obtain a metal film layer that has a total reflection effect on light. After the metal film layer is formed, a photoresist is evenly applied to the metal film layer, which is then exposed, developed, and etched to obtain a reflective electrode layer.
[0133] Exposure involves covering a metal film layer coated with photoresist with a mask and then irradiating the metal film layer covered with the mask with light of a specific wavelength. When the photoresist not covered by the mask is exposed to light, the photosensitizer in the photoresist undergoes a photochemical reaction. If the photoresist is positive, the chemical composition of the photoresist not covered by the mask changes after exposure to light, becoming soluble in the developer, while the chemical composition of the photoresist not exposed remains unchanged and insoluble in the developer. If the photoresist is negative, the chemical composition of the photoresist not covered by the mask changes after exposure to light, becoming insoluble in the developer, while the chemical composition of the photoresist not exposed remains unchanged and soluble in the developer.
[0134] After the light exposure is completed, the photoresist on the metal film layer is cleaned with a developer, so that the photoresist on the metal film layer that is soluble in the developer is dissolved, while the photoresist that is insoluble in the developer is retained. As shown in Figure 10, after the developer is cleaned, part of the photoresist on the metal film layer is retained.
[0135] After being cleaned with a developer, the metal film layer can be further etched. Depending on different usage scenarios and requirements, different methods can be used for etching. In one implementation, the area on the metal film layer not covered by the photoresist can be dry-etched. Among them, there are many methods of dry etching, such as sputtering and ion beam milling, plasma etching (Plasma Etching), high-pressure plasma etching, high-density plasma etching and reactive ion etching. In another implementation, the area on the metal film layer not covered by the photoresist can be wet-etched. Among them, wet etching refers to the use of a chemical reaction between a solution and the material to be etched to remove the area not covered by the photoresist to achieve the etching purpose. As shown in Figure 11, after etching the metal film layer, reflective electrode layers of different sub-pixels are obtained, and there is a channel between adjacent reflective electrode layers.
[0136] In one implementation, if the reflective electrode layer is made of a material susceptible to corrosion, such as aluminum, a reflective electrode protective layer can be formed on the reflective electrode layer using a corrosion-resistant conductive material to protect the reflective electrode layer. Alternatively, as shown in FIG12 , the reflective electrode layer can be plated with a corrosion-resistant conductive material to form a secondary metal film. The plated film is then processed through processes such as coating, exposure, development, and etching to form a reflective electrode protective layer on the reflective electrode layer. As shown in FIG13 , a reflective electrode protective layer is formed on the reflective electrode layer. Optionally, the corrosion-resistant conductive material can be ITO.
[0137] S802 , sequentially forming microcavity pad layers of the plurality of sub-pixels on a side of the reflective electrode layer of the plurality of sub-pixels away from the substrate using the material of the microcavity pad layers in the plurality of sub-pixels.
[0138] After obtaining the reflective electrode layer of each pixel, the reflective electrode layer of multiple sub-pixels can be away from the substrate side, and the material of the microcavity pad in the multiple sub-pixels can be used to sequentially form the microcavity pad of multiple sub-pixels. Since the trenches shown in Figures 11 and 13 are formed during the etching process, the trenches can be filled before forming the microcavity pad. Optionally, SiO2 can be used to fill the trenches. For example, as shown in Figure 14, SiO2 can be first coated on the substrate with the reflective electrode layer, and then the trenches can be filled by coating, exposing, developing and dry etching to obtain a display substrate as shown in Figure 15, thereby reducing the transfer of the step difference of the reflective electrode layer to the semi-transparent electrode layer.
[0139] After the trench is filled, the microcavity pads of the multiple sub-pixels can be formed in sequence using the materials of the microcavity pads in the multiple sub-pixels on the side of the reflective electrode layer away from the substrate. In one implementation, the microcavity pads of the multiple sub-pixels can be formed in sequence using the materials of the microcavity pads in the multiple sub-pixels in the order of increasing etching rates relative to the materials of the microcavity pads in the multiple sub-pixels. In this way, when forming a certain film layer, etching losses to the previously formed film layer can be avoided.
[0140] For example, the multiple sub-pixels in the above-mentioned display substrate include: a first sub-pixel and a second sub-pixel. The etching rate of the material of the microcavity pad layer in the first sub-pixel is less than the etching rate of the material of the microcavity pad layer in the second sub-pixel. For example, the ratio of the etching rate of the material of the microcavity pad layer in the first sub-pixel to the etching rate of the material of the microcavity pad layer in the second sub-pixel is less than or equal to a preset ratio threshold. In one implementation, the preset ratio threshold may be 1:20. On this basis, the above-mentioned formation of the microcavity pad layers of the multiple sub-pixels on the side of the reflective electrode layer of the multiple sub-pixels away from the substrate in sequence using the materials of the microcavity pad layers in the multiple sub-pixels in accordance with the order of the etching rate from small to large. This may include steps A1-step A2.
[0141] In step A1, a first material film is formed on the side of the reflective electrode layer of the plurality of sub-pixels away from the substrate using the material of the microcavity pad layer in the first sub-pixel, and the first material film is etched to form the microcavity pad layer of the first sub-pixel.
[0142] Optionally, the material of the microcavity pad in the first sub-pixel can be used to form a first material film, and then the first material film is subjected to glue coating, exposure, development and etching to obtain the microcavity pad of the first sub-pixel. As shown in Figure 16, after forming a secondary SiO film using SiO on the side away from the substrate where the reflective electrode protective layer is formed, exposure, development and etching are performed using photoresist to obtain the microcavity pad of the first sub-pixel shown in Figure 17. In one implementation, in the process of forming the microcavity pad of the first sub-pixel, a via can be formed in the microcavity pad of the first sub-pixel at the same time. The via taper of the via can be optionally less than 45°.
[0143] In step A2, a second material film is formed on the side of the reflective electrode layer of the plurality of sub-pixels away from the substrate using the material of the microcavity pad layer in the second sub-pixel, and the second material film is etched to form the microcavity pad layer of the second sub-pixel.
[0144] Since the etching rate of the material of the microcavity pad layer in the first sub-pixel is lower than the etching rate of the material of the microcavity pad layer in the second sub-pixel, the microcavity pad layer of the second sub-pixel needs to be formed after the microcavity pad layer of the first sub-pixel is formed to reduce the etching loss of the first sub-pixel.
[0145] Optionally, the material of the microcavity pad in the second sub-pixel can be used to form a second material film, and then the second material film is coated, exposed, developed and etched to form the microcavity pad of the second sub-pixel. As shown in Figure 18, on the substrate with the microcavity pad of the first sub-pixel, after forming a SiN film using SiN, and then using photoresist for exposure, development and etching, the microcavity pad of the second sub-pixel shown in Figure 19 can be obtained. In one implementation, in the process of forming the microcavity pad of the second sub-pixel, a via hole can be formed in the microcavity pad of the second sub-pixel. The via taper of the via hole can be optionally less than 45°.
[0146] In one implementation, the material of the microcavity liner in the first sub-pixel can be silicon oxide, and the material of the microcavity liner in the second sub-pixel can be silicon nitride. In this case, a silicon oxide film can be formed first, and then the microcavity liner of the first sub-pixel can be etched out of the silicon oxide film. Then, a silicon nitride film can be formed, and then the microcavity liner of the second sub-pixel can be etched out of the silicon nitride film.
[0147] Optionally, the thickness of the microcavity pads in multiple sub-pixels is the same. Furthermore, the materials of the microcavity pads in sub-pixels corresponding to different colors of light are the same or different. For example, when the materials of the microcavity pads in sub-pixels corresponding to different colors of light are the same, different particles are doped into the microcavity pads in the sub-pixels corresponding to different colors of light to adjust the refractive index of the microcavity pads.
[0148] S803, sequentially forming light-emitting layers and semi-transparent electrode layers of the plurality of sub-pixels on the side of the microcavity pad layer away from the substrate to obtain the plurality of sub-pixels, wherein a microcavity structure of the sub-pixel is formed between the reflective electrode layer and the semi-transparent electrode layer of any sub-pixel.
[0149] Optionally, after obtaining the structure shown in Figure 19, a conductive material can be first used to form a film on a substrate formed with a microcavity pad layer, and then the sub-pixel space can be opened by coating, exposing, developing and dry etching. At the same time, since the conductive material is also deposited in the vias on the microcavity pad layer of multiple sub-pixels, the conductive material can be electrically connected to the structure under the microcavity pad layer. For example, the conductive material can be ITO. As shown in Figure 20, an ITO film is formed on the surface of the microcavity pad layer and in the via hole. After exposure, development and etching with photoresist, the ITO layer shown in Figure 21 can be obtained.
[0150] In order to improve the stability of the sub-pixel structure, after forming the microcavity pad layer of the multiple sub-pixels and before forming the light-emitting layer and the semi-transparent electrode layer of the multiple sub-pixels, an undercut structure of the multiple sub-pixels can be optionally formed first. Optionally, the undercut structure includes a first material layer and a second material layer, and the etching rate of the first material layer is less than the etching rate of the second material layer. For example, the first material layer and the second material layer meet any one of the following conditions: the material of the first material layer is the same as the material with the slowest etching rate among the materials of the microcavity pad layers in the multiple sub-pixels, and the material of the second material layer is different from the material with the slowest etching rate among the materials of the microcavity pad layers in the multiple sub-pixels; and the material of the first material layer is different from the material with the fastest etching rate among the materials of the microcavity pad layers in the multiple sub-pixels, and the material of the second material layer is the same as the material with the fastest etching rate among the materials of the microcavity pad layers in the multiple sub-pixels.
[0151] In one possible implementation, the material with the fastest etching rate among the materials of the microcavity pads in the multiple sub-pixels can be used to form a second material film layer on the side of the microcavity pads of the multiple sub-pixels away from the substrate. Then, the material with the slowest etching rate among the materials of the microcavity pads in the multiple sub-pixels can be used to form a first material film layer on the side of the second material film layer of the multiple sub-pixels away from the substrate. Then, the first material film layer and the second material film layer of the multiple sub-pixels are etched to form an undercut structure of the multiple sub-pixels. The undercut structure includes a stacked first material layer and a second material layer, and the undercut structure has a recessed portion. The orthographic projection of the surface of the first material layer surrounding the recessed portion on the substrate is located inside the orthographic projection of the surface of the second material layer surrounding the recessed portion on the substrate.
[0152] For example, if the material with the fastest etching rate among the materials of the microcavity pads in the multiple sub-pixels is SiNx, and the material with the slowest etching rate among the materials of the microcavity pads in the multiple sub-pixels is SiOx, then SiNx can be used to first form a SiNx material layer on the side of the microcavity pads in the multiple sub-pixels away from the substrate, and then SiOx can be used to form a SiOx material layer on the side of the SiNx material layer away from the substrate. Then, the SiNx material layer of each sub-pixel is opened using an etching solution, and the SiOx material layer is further laterally hollowed out using the etching solution, thereby forming an undercut structure with a smaller top and a larger bottom.
[0153] In one implementation, a composite film layer can be deposited sequentially using SiOx, SiNx, and SiOx on a substrate with a microcavity pad. The pixel definition layer (PDL) between the pixels is then opened through photoresist coating, exposure, development, and dry etching. Etching can be performed in four steps: the first step is to etch the PDL above the pixel using CF4 (carbon tetrafluoride). The second step is to enlarge the critical dimension (CD) etched between the sub-pixels using a lateral debonding method. The third step is to use CF4 to open the topmost SiOx layer in a timed pattern. The fourth step is to use SF6 (sulfur hexafluoride) for lateral indentation. Because SF6 can increase the SiOx / SiNx etching selectivity to at least greater than 7, the SF6 lateral indentation can create an undercut structure. This step forms the LLC (Lateral Leakage Cutoff) indentation structure to be footed, thus forming the pixel definition layer. Figure 22 shows a schematic diagram of the pixel definition layer after formation on the microcavity pad. The pixel definition layer has an undercut structure.
[0154] As can be seen from the previous description, the thickness of the microcavity pad layer of the sub-pixels corresponding to different colors of light in the present disclosure can be the same or different. Figure 22 is a schematic diagram of the microcavity pad layer of the sub-pixels corresponding to different colors of light having the same thickness. Figure 23 is a schematic diagram of the microcavity pad layer of the sub-pixels corresponding to different colors of light having different thicknesses.
[0155] After forming the pixel definition layer, a light-emitting layer and a semi-transparent electrode layer of multiple sub-pixels can be formed on the substrate on which the pixel definition layer is formed. A microcavity structure is formed between the reflective electrode layer of any sub-pixel and the semi-transparent electrode layer of the sub-pixel. For example, a light-emitting material can be used to form a film on a substrate on which a pixel definition layer is formed, and then the light-emitting layers of multiple sub-pixels are obtained by coating with glue, exposing, developing and dry etching. Then, a conductive material is used to form a film on the substrate on which the light-emitting layer is formed, and then the semi-transparent electrode layer is obtained by coating with glue, exposing, developing and dry etching. In one achievable embodiment, the thickness and / or refractive index of the light-emitting layer in the multiple sub-pixels can be the same, and the thickness and / or refractive index of the semi-transparent electrode layer in the multiple sub-pixels can be the same.
[0156] After the above process, a peripheral area surrounding the sub-pixel is also formed on the substrate. The peripheral area includes a first silicon oxide layer, a first silicon nitride layer, a second silicon nitride layer, and a second silicon oxide layer stacked in sequence. Among them, the first silicon oxide layer is in the same layer as the microcavity pad layer in the first sub-pixel, that is, the first silicon oxide layer is formed in the process of forming the microcavity pad layer in the first sub-pixel. The first silicon nitride layer is in the same layer as the microcavity pad layer in the second sub-pixel, that is, the first silicon nitride layer is formed in the process of forming the microcavity pad layer in the second sub-pixel. The second silicon nitride layer is in the same layer as the second material layer, that is, the second silicon nitride layer is formed in the process of forming the second material layer. The second silicon oxide layer is in the same layer as the first material layer, that is, the second silicon oxide layer is formed in the process of forming the first material layer.
[0157] In the embodiment of the present disclosure, since the refractive index of the microcavity pad layer that matches any color light makes the microcavity structure in which the microcavity pad layer is located meet the constructive interference condition of the color light, it means that the refractive index of the microcavity pad layer can be adjusted to make the microcavity structure of the sub-pixel meet the constructive interference condition of the corresponding color light. Therefore, compared with the method of simply adjusting the thickness of the microcavity pad layer, the method of adjusting the refractive index of the microcavity pad layer in the present disclosure is conducive to reducing the thickness of the microcavity pad layer, and can reduce the thickness difference of the microcavity pad layer in multiple sub-pixels corresponding to different colors of light, reduce the difference in light output efficiency of different sub-pixels, and improve the display balance of multiple sub-pixels.
[0158] It should be noted that, in this document, relational terms such as first and second, etc., are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship or order between these entities or operations. Moreover, the terms "comprises," "comprising," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or device comprising a series of elements includes not only those elements, but also other elements not explicitly listed, or elements inherent to such process, method, article, or device. In the absence of further limitations, an element defined by the phrase "comprising a ..." does not exclude the presence of other identical elements in the process, method, article, or device comprising the element.
[0159] Each embodiment in this specification is described in a related manner. Similar portions between the embodiments can be referenced to each other. Each embodiment focuses on the differences from other embodiments. In particular, the method embodiment is generally similar to the method embodiment, so the description is relatively simple. For related portions, refer to the description of the method embodiment.
[0160] The above are only preferred embodiments of the present disclosure and are not intended to limit the scope of protection of the present disclosure. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principles of the present disclosure are included in the scope of protection of the present disclosure.
Claims
1. A display substrate, comprising: substrate; A plurality of sub-pixels located on the substrate, wherein the sub-pixels have a microcavity structure, and the microcavity structure has a microcavity cushion layer; The refractive index of the microcavity pad layer in the sub-pixels corresponding to different color lights is different, and the refractive index of the microcavity pad layer in any sub-pixel matches the color light corresponding to the any sub-pixel. The refractive index of the microcavity pad layer matching any color light makes the microcavity structure where the microcavity pad layer is located meet the constructive interference condition of the any color light.
2. The display substrate according to claim 1, wherein the refractive index of the microcavity pad layer in any sub-pixel and the wavelength of the color light corresponding to the any sub-pixel satisfy the following constraints: in, A is the optical path of the microcavity structure of any sub-pixel excluding the microcavity pad layer, and A is the same in the microcavity structures of the multiple sub-pixels, n is the refractive index of the microcavity pad layer in any sub-pixel, d is the thickness of the microcavity pad layer in any sub-pixel, k is a positive integer, and λ is the wavelength of the color light corresponding to any sub-pixel. 3 . The display substrate according to claim 1 , wherein the thickness of the microcavity pads in the plurality of sub-pixels is the same. 4 . The display substrate according to claim 1 , wherein the materials of the microcavity pads in the sub-pixels corresponding to different colors of light are the same or different. 5 . The display substrate according to claim 4 , wherein the material of the microcavity pads in the sub-pixels corresponding to different color lights is the same, and different particles are doped in the microcavity pads in the sub-pixels corresponding to different color lights.
6. The display substrate according to any one of claims 1 to 5, wherein the sub-pixel further comprises: an undercut structure located on a side of the microcavity pad in the sub-pixel away from the substrate, the undercut structure having a concave portion; The undercut structure comprises a first material layer and a second material layer, wherein the first material layer is located on a side of the second material layer away from the substrate, and the orthographic projection of the surface of the first material layer surrounding the recessed portion on the substrate is located on the surface of the second material layer surrounding the recessed portion. The interior of the orthographic projection on the substrate. 7 . The display substrate according to claim 6 , wherein an etching rate of the first material layer is lower than an etching rate of the second material layer.
8. The display substrate according to claim 7, wherein the first material layer and the second material layer satisfy any one of the following conditions: The material of the first material layer is the same as the material with the slowest etching rate among the materials of the microcavity pad layers in the multiple sub-pixels, and the material of the second material layer is different from the material with the slowest etching rate among the materials of the microcavity pad layers in the multiple sub-pixels; Furthermore, the material of the first material layer is different from the material with the fastest etching rate among the materials of the microcavity pad layers in the multiple sub-pixels, and the material of the second material layer is the same as the material with the fastest etching rate among the materials of the microcavity pad layers in the multiple sub-pixels.
9. The display substrate according to any one of claims 6 to 8, wherein the plurality of sub-pixels comprises: A first sub-pixel and a second sub-pixel, the first sub-pixel is a blue sub-pixel, the second sub-pixel is a green sub-pixel, the material of the microcavity pad layer in the first sub-pixel includes silicon oxide, and the material of the microcavity pad layer in the second sub-pixel includes silicon nitride; The material of the first material layer includes silicon oxide, and the material of the second material layer includes silicon nitride.
10. The display substrate according to any one of claims 1 to 9, further comprising a peripheral region surrounding the sub-pixel, the peripheral region comprising a first silicon oxide layer, a first silicon nitride layer, a second silicon nitride layer, and a second silicon oxide layer stacked in sequence; The plurality of sub-pixels include: A first sub-pixel and a second sub-pixel, wherein the sub-pixel further comprises: an undercut structure located at a side of the microcavity pad layer in the sub-pixel away from the substrate, the undercut structure having a recessed portion, the undercut structure comprising a first material layer and a second material layer, the first material layer being located at a side of the second material layer away from the substrate, and an orthographic projection of a surface of the first material layer surrounding the recessed portion on the substrate being located inside an orthographic projection of a surface of the second material layer surrounding the recessed portion on the substrate; Among them, the first silicon oxide layer is in the same layer as the microcavity pad layer in the first sub-pixel, the first silicon nitride layer is in the same layer as the microcavity pad layer in the second sub-pixel, the second silicon nitride layer is in the same layer as the second material layer, and the second silicon oxide layer is in the same layer as the first material layer.
11. The display substrate according to any one of claims 6 to 9, wherein the sub-pixel further comprises: a reflective electrode layer located between the substrate and the microcavity pad layer; a reflective electrode protection layer located between the reflective electrode layer and the microcavity pad layer; A light-emitting layer and a semi-transparent electrode layer located on a side of the undercut structure away from the substrate and stacked in sequence; Among them, a microcavity structure of the sub-pixel is formed between the reflective electrode layer and the semi-transparent electrode layer, and the multiple sub-pixels satisfy at least one of the following: the thickness and / or refractive index of the reflective electrode layer in the multiple sub-pixels are the same, the thickness and / or refractive index of the light-emitting layer in the multiple sub-pixels are the same, and the thickness and / or refractive index of the semi-transparent electrode layer in the multiple sub-pixels are the same. 12 . The display substrate according to claim 1 , wherein the microcavity pad layer of the sub-pixel has a via hole, the via hole is filled with a conductive material, and the conductive material is used to electrically connect structures on both sides of the microcavity pad layer. The display substrate according to claim 12 , wherein a via taper of the via hole is less than 45°.
14. A display device, comprising a display substrate, the display substrate comprising: substrate; A plurality of sub-pixels having a microcavity structure, wherein the sub-pixels are located on the substrate, and the microcavity structure of the sub-pixels has a microcavity cushion layer; The refractive index of the microcavity pad layer in the sub-pixels corresponding to different color lights is different, and the refractive index of the microcavity pad layer in any sub-pixel matches the color light corresponding to the any sub-pixel. The refractive index of the microcavity pad layer matching any color light makes the microcavity structure where the microcavity pad layer is located meet the constructive interference condition of the any color light.
15. A method for preparing a display substrate, the method comprising: providing a substrate; forming a plurality of sub-pixels on the substrate, wherein a microcavity structure is formed in the sub-pixels, and a microcavity pad layer is formed in the microcavity structure; The refractive index of the microcavity pad layer in the sub-pixels corresponding to different color lights is different, and the refractive index of the microcavity pad layer in any sub-pixel matches the color light corresponding to the any sub-pixel. The refractive index of the microcavity pad layer matching any color light makes the microcavity structure where the microcavity pad layer is located meet the constructive interference condition of the any color light.
16. The method according to claim 15, wherein forming a plurality of sub-pixels on the substrate comprises: forming a reflective electrode layer of the plurality of sub-pixels on the substrate; On the side where the reflective electrode layers of the plurality of sub-pixels are away from the substrate, the plurality of sub-pixels are The material of the microcavity pad in the pixel sequentially forms the microcavity pads of the plurality of sub-pixels; On the side of the microcavity cushion layer of the multiple sub-pixels away from the substrate, the light-emitting layers and the semi-transparent electrode layers of the multiple sub-pixels are formed in sequence to obtain the multiple sub-pixels, and the microcavity structure of any sub-pixel is formed between the reflective electrode layer and the semi-transparent electrode layer of any sub-pixel.
17. The method according to claim 16, wherein the microcavity pad layers of the plurality of sub-pixels are sequentially formed by using the material of the microcavity pad layers in the plurality of sub-pixels on the side of the reflective electrode layer of the plurality of sub-pixels away from the substrate, comprising: In order of increasing etching rates of the materials of the microcavity pad layers in the multiple sub-pixels, the microcavity pad layers of the multiple sub-pixels are formed in sequence using the materials of the microcavity pad layers in the multiple sub-pixels on the side of the reflective electrode layers of the multiple sub-pixels away from the substrate.
18. The method according to claim 17, wherein the plurality of sub-pixels comprises: A first sub-pixel and a second sub-pixel, wherein the etching rate of the material of the microcavity pad layer in the first sub-pixel is lower than the etching rate of the material of the microcavity pad layer in the second sub-pixel, and the microcavity pad layers of the multiple sub-pixels are formed by sequentially using the materials of the microcavity pad layers in the multiple sub-pixels on the side of the reflective electrode layer of the multiple sub-pixels away from the substrate in the order of the etching rates of the materials of the microcavity pad layers in the multiple sub-pixels from small to large, comprising: On a side of the reflective electrode layer of the plurality of sub-pixels away from the substrate, forming a first material film using the material of the microcavity pad layer in the first sub-pixel; Etching the first material film to form a microcavity pad layer of the first sub-pixel; After forming the microcavity pad layer of the first sub-pixel, forming a second material film using the material of the microcavity pad layer in the second sub-pixel on a side of the reflective electrode layer of the plurality of sub-pixels away from the substrate; The second material film is etched to form a microcavity pad layer of the second sub-pixel.
19. The method according to claim 18, wherein the ratio of the etching rate of the material of the microcavity pad layer in the first sub-pixel to the etching rate of the material of the microcavity pad layer in the second sub-pixel is less than or equal to a preset ratio threshold; The material of the microcavity pad layer in the first sub-pixel includes silicon oxide, and the material of the microcavity pad layer in the second sub-pixel includes silicon nitride.
20. The method according to claim 16, after sequentially forming the microcavity pad layers of the plurality of sub-pixels on the side where the reflective electrode layers of the plurality of sub-pixels are away from the substrate using the material of the microcavity pad layers in the plurality of sub-pixels, and before sequentially forming the light-emitting layers and the semi-transparent electrode layers of the plurality of sub-pixels on the side where the microcavity pad layers of the plurality of sub-pixels are away from the substrate, the method further comprises: Using a material with the fastest etching rate among the materials of the microcavity pad layers in the plurality of sub-pixels, a second material layer is formed on a side of the microcavity pad layers of the plurality of sub-pixels away from the substrate; Using the material with the slowest etching rate among the materials of the microcavity pads in the plurality of sub-pixels, a first material layer is formed on a side of the second material layer of the plurality of sub-pixels away from the substrate; The first material layer and the second material layer of the multiple sub-pixels are etched to form an undercut structure of the multiple sub-pixels, wherein the undercut structure has a recessed portion, and the orthographic projection of the surface of the first material layer surrounding the recessed portion on the substrate is located inside the orthographic projection of the surface of the second material layer surrounding the recessed portion on the substrate.
Citation Information
Patent Citations
Light emitting device and display panel
CN110311048A
Display panel and display device thereof
CN110459564A
Display substrate and preparation method thereof and display device
CN110610975A
Display panel, display device and manufacturing method of display panel
CN116963546A