Phosphor and light-emitting device
The phosphor with the formula Baα1Srα2EuβAlcSi dOeNf, optimized through specific composition and manufacturing methods, addresses the limitations of conventional phosphors by enhancing external quantum efficiency and temperature stability, making it suitable for advanced lighting and signaling applications.
Patent Information
- Application Number
- PCT/JP2024/017597
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-26
- Filing Date
- 2024-05-13
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional phosphors used in light-emitting devices have limitations in external quantum efficiency and stability, particularly under high temperatures, which affect their performance in applications such as lighting and signaling devices.
A phosphor with the general formula Baα1Srα2EuβAlcSi dOeNf is developed, where specific composition ratios and manufacturing processes enhance the incorporation of Eu, leading to improved luminescent properties and stability, including a high absorption rate and specific particle size distribution, resulting in enhanced external quantum efficiency and temperature resistance.
The phosphor achieves improved external quantum efficiency and maintains luminescent properties even at high temperatures, making it suitable for applications in lighting and signaling devices, including those in harsh environments like vehicle lighting.
Smart Images

Figure JP2024017597_05122024_PF_FP_ABST
Abstract
Description
Phosphor and light-emitting device
[0001] The present invention relates to a phosphor and a light-emitting device.
[0002] Phosphors are sometimes used industrially to form wavelength conversion components in light-emitting devices, i.e., components that convert short-wavelength light into long-wavelength light, and with the recent widespread use of LEDs (light-emitting diodes), phosphors have become increasingly important industrially.
[0003] Patent Document 1 describes a blue phosphor having an emission peak wavelength different from that of conventional blue phosphors. Specifically, claim 1 of Patent Document 1 describes a blue phosphor having a general formula: Me a Re b Al c Si d O e N f (where Me is one or more elements selected from Sr and Ba, and Re is Eu), and a phosphor is disclosed in which the composition ratios a, b, c, d, e, and f have the following relationships: a+b=1 0.005<b<0.25 1.60<c<2.60 2.45<d<4.05 3.05<e<5.00 2.75<f<4.40 According to the description in Patent Document 1, this phosphor is excited by light with a wavelength of 300 nm or more and 420 nm or less, and emits light having a peak wavelength of 450 nm or more and 485 nm or less.
[0004] Furthermore, Patent Documents 2 and 3 can be cited as documents that describe phosphors having chemical structures or chemical compositions similar to those of the phosphor described in Patent Document 1.
[0005] International Publication No. 2014 / 091776 International Publication No. 2013 / 069696 International Publication No. 2015 / 093429
[0006] As a result of preliminary studies by the present inventors, it has been found that conventional phosphors such as those described in Patent Documents 1 to 3 have room for improvement in terms of luminescence properties such as external quantum efficiency.
[0007] The present invention has been made in view of the above circumstances, and one of the objects of the present invention is to provide a phosphor having at least good external quantum efficiency.
[0008] The present inventors have completed the invention provided below and solved the above problems.
[0009] 1. General formula Ba a1 Sr a2 EU b Al c Si d O e N f wherein the composition ratios a1, a2, b, c, d, e, and f satisfy the following relationship when c + d = 5: a1 > a2 0.70 ≦ a1 + a2 + b ≦ 1.20 0.20 ≦ b ≦ 0.50 1.50 ≦ c ≦ 2.50 2.50 ≦ d ≦ 3.50 3.05 ≦ e ≦ 6.50 2.75 ≦ f ≦ 4.40 2. The phosphor according to 1., wherein 0 ≦ a2 ≦ 0.10. 3. The phosphor according to 1. or 2., wherein 0.40 ≦ a1 ≦ 0.80. 4. The phosphor according to any one of 1. to 3., wherein the absorptance of light at a wavelength of 405 nm is 89% or more. 5. 1. to 4. 6. The phosphor according to any one of 1. to 5., wherein the peak wavelength of the fluorescence emitted when irradiated with light having a wavelength of 405 nm is 475 to 495 nm. 50A phosphor that is a powder having a particle size of 10 to 30 μm. 7. The phosphor according to any one of 1. to 6., wherein in an X-ray diffraction spectrum obtained by X-ray diffraction measurement of the phosphor, the value of B / A is 0.15 or less, where A is the intensity of a peak in the 2θ range of 25.0 to 26.0 degrees and B is the intensity of a peak in the 2θ range of 29.0 to 30.0 degrees. 8. A light-emitting device comprising a light-emitting element and the phosphor according to any one of 1. to 7.. 9. The light-emitting device according to 8., wherein the light-emitting element is a light-emitting element that emits light at a wavelength of 340 to 450 nm. 10. The light-emitting device according to 8. or 9., wherein the light-emitting element is an LED element. 11. The light-emitting device according to any one of 8. to 10., wherein the light-emitting device is a lighting device or a signaling device.
[0010] According to the present invention, a phosphor having at least good external quantum efficiency is provided.
[0011] FIG. 2 is a diagram showing X-ray diffraction spectra of phosphors of Examples and Comparative Examples.
[0012] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. In this specification, the expression "X to Y" in the description of a numerical range means X or more and Y or less, unless otherwise specified. For example, "1 to 5 mass %" means "1 mass % or more and 5 mass % or less."
[0013] <Phosphor> The phosphor of this embodiment is a phosphor represented by the general formula: Ba a1 Sr a2 EU b Al c Si d O e N f In this general formula, when c + d = 5, the composition ratios a1, a2, b, c, d, e, and f have the following relationship: a1 > a2 0.70 ≤ a1 + a2 + b ≤ 1.20 0.20 ≤ b ≤ 0.50 1.50 ≤ c ≤ 2.50 2.50 ≤ d ≤ 3.50 3.05 ≤ e ≤ 6.50 2.75 ≤ f ≤ 4.40
[0014] The phosphor of this embodiment differs from conventional phosphors in that it has a relatively large b value and a relatively high Eu content. Based on past knowledge, Eu is thought to function as a luminescence center. Therefore, the phosphor of this embodiment, which has a relatively large b value and a relatively high Eu content, is thought to have good luminescence characteristics.
[0015] Incidentally, it is generally known that even if the Eu content in the raw materials is increased in order to increase the Eu content in the phosphor, a sufficient amount of Eu is often not incorporated into the phosphor. Furthermore, even if the Eu content in the phosphor is increased, this can lead to the formation of heterophases or changes in the crystal structure, which may limit the improvement in luminescence characteristics. However, in this embodiment, a phosphor in which a sufficient amount of Eu is incorporated into the crystal structure can be obtained at least through the manufacturing method described below. The luminescence characteristics of the obtained phosphor are good. One reason for this is that the crystal structure of the phosphor of this embodiment is a phosphor having a general formula BaAl 2 Si 3 O 4 N 4 This is thought to be because the phosphor of this embodiment is identical to or similar to the crystal of an inorganic compound represented by the general formula BaAl 2 Si 3 O 4 N 4 In this case, Ba can be regarded as being substituted into Eu or Sr to form a solid solution, and therefore, it is easy to include a relatively large amount of Eu in the crystal structure. Furthermore, even if a relatively large amount of Eu is included in the crystal structure, it is thought that unintended distortion of the crystal structure or a different phase is unlikely to occur.
[0016] Incidentally, the phosphor of this embodiment tends to suppress the deterioration of its luminescence characteristics even at high temperatures of about 200°C. Based on this tendency, the phosphor of this embodiment can be preferably applied to, for example, lighting devices used in vehicles or in harsh environments. Although it is speculated, the reason why the deterioration of its luminescence characteristics is suppressed even at high temperatures of about 200°C is that, as described above, the crystal structure of the phosphor of this embodiment has the general formula BaAl 2 Si 3 O 4 N4 This is thought to be because the crystals are identical to or similar to those of the inorganic compound represented by the general formula BaAl 2 Si 3 O 4 N 4 The crystal structure of the inorganic compound represented by the formula (I) is relatively stable against heat, and therefore, it is considered that the phosphor of this embodiment is also relatively stable against heat.
[0017] The phosphor of this embodiment will be further described.
[0018] (General formula) General formula Ba a1 Sr a2 EU b Al c Si d O e N f In the formula, when c+d=5, the values of the composition ratios a1, a2, b, c, d, e, and f can be as shown above.
[0019] Regarding a1 and a2, it is sufficient that a1>a2, but from the viewpoint of particularly good light-emitting properties, a1 is preferably 0.40≦a1≦0.80, more preferably 0.45≦a1≦0.75, and a2 is preferably 0≦a2≦0.10, more preferably 0≦a2≦0.05, and even more preferably 0≦a2≦0.02. a2 may be zero.
[0020] The value of b may be in the range of 0.20≦b≦0.50, and preferably in the range of 0.25≦b≦0.45. It is believed that when b is not too large, energy exchange between adjacent Eu atoms is less likely to occur, and the energy absorbed by Eu is more reliably converted into fluorescence.
[0021] Although c may be in the range of 1.50≦c≦2.50, it is preferable that c is in the range of 1.70≦c≦2.30, more preferably 1.80≦c≦2.20, and even more preferably 1.90≦c≦2.10.
[0022] The value of d may be in the range of 2.50≦d≦3.50, preferably 2.70≦d≦3.30, more preferably 2.80≦d≦3.20, and even more preferably 2.90≦d≦3.10.
[0023] The value of e may be in the range of 3.05≦e≦6.50, preferably 4.00≦e≦6.50, more preferably 4.50≦e≦6.25, even more preferably 5.00≦e≦6.00, and particularly preferably 5.00≦e≦5.80.
[0024] The value of f may be in the range of 2.75≦f≦4.40, preferably 3.00≦f≦4.30, and more preferably 3.50≦f≦4.20.
[0025] a1+a2+b may be in the range of 0.70≦a1+a2+b≦1.20, preferably 0.80≦a1+a2+b≦1.10, and more preferably 0.90≦a1+a2+b≦1.10.
[0026] From the viewpoint of further stabilizing the crystal structure, the relative magnitudes between the respective values are preferably as follows: c / d: preferably 0.50<c / d<0.75, more preferably 0.55c / d<0.75, and even more preferably 0.60<c / d<0.73 e / f: preferably 0.90<e / f<2.00, more preferably 1.00<e / f<1.90, and even more preferably 1.12<e / f<1.7
[0027] (Absorptance of Light with a Wavelength of 405 nm) The phosphor of this embodiment preferably has a high absorptance of light with a wavelength of 405 nm. High absorptance may further enhance luminescence characteristics such as external quantum efficiency. Specifically, the absorptance of the phosphor of this embodiment with respect to light with a wavelength of 405 nm is preferably 89% or more, more preferably 89 to 97%, and even more preferably 89 to 95%.
[0028] (Particle size distribution: median diameter D 50 The phosphor of this embodiment is typically in powder form. In other words, the phosphor of this embodiment is an aggregate of phosphor particles. By having an appropriate particle size distribution of the powdered phosphor of this embodiment, it may be possible to further improve various performances such as light-emitting characteristics. The particle size distribution can be adjusted, for example, by changing the pulverization conditions and classification conditions in the phosphor manufacturing process described below.
[0029] Specifically, the median diameter D of the powdered phosphor of this embodiment is 50 The volume-based cumulative 10% particle diameter D (measured by laser diffraction / scattering method) of the powdered phosphor of this embodiment is preferably 10 to 30 μm, more preferably 10 to 20 μm. 10 The volume-based cumulative 90% particle diameter D of the powdered phosphor of this embodiment, determined by a laser diffraction / scattering method, is preferably 5 to 15 μm, and more preferably 5 to 10 μm. 90 is preferably 20 to 40 μm, more preferably 23 to 35 μm.
[0030] From another perspective, (D 90 -D 10 ) / D 50 The value of is preferably 1.5 or less, more preferably 1.05 to 1.5. This value indicates that the particle size distribution of the powdered phosphor is relatively sharp. A sharp particle size distribution means that the phosphor particles in the powdered phosphor are homogeneous at least in terms of particle size. This is expected to lead to stable light emission and to reduce variations in light emission characteristics between product lots. In addition, (D 90 -D 10 ) / D 50 The fact that the value of is not too large can also be said to mean that the powdered phosphor contains a relatively small proportion of coarse particles and particles with extremely small particle diameters (fine powder), which do not contribute to improving the light-emitting properties or have a negative effect on the light-emitting properties.
[0031] (X-ray Diffraction Spectrum) As described above, the phosphor of this embodiment is typically a phosphor represented by the general formula BaAl 2 Si 3 O 4 N 4 Therefore, the X-ray diffraction spectrum of the phosphor of this embodiment usually has a crystal structure identical to or similar to that of the crystal of an inorganic compound represented by the general formula BaAl 2 Si 3 O 4 N 4The peak is at approximately the same position (2θ) as the peak observed in the X-ray diffraction spectrum of a crystal of an inorganic compound represented by the general formula BaAl 2 Si 3 O 4 N 4 The positions of the peaks in the X-ray diffraction spectrum of the crystal of the inorganic compound represented by the formula (I) are shown at the bottom of FIG.
[0032] General formula BaAl 2 Si 3 O 4 N 4 The ratio of the heterophase in the phosphor of this embodiment can be estimated by comparing the X-ray diffraction spectrum of a crystal of an inorganic compound represented by the general formula BaAl with the X-ray diffraction spectrum of the phosphor of this embodiment and analyzing diffraction peaks that are not present in the former but are present in the latter. 2 Si 3 O 4 N 4 and has a crystal structure different from that of the inorganic compound represented by the formula (I), and may not contribute to or may adversely affect the luminescence characteristics of the phosphor of this embodiment. Specifically, in the X-ray diffraction spectrum obtained by X-ray diffraction measurement of the phosphor of this embodiment, when the intensity of the peak in the 2θ range of 25.0 to 26.0° is defined as A and the intensity of the peak in the 2θ range of 29.0 to 30.0° is defined as B, the value of B / A is preferably 0 to 0.15. Ideally, the value of B / A is zero, but considering production costs and the like, a practical value of 0.03 to 0.15 is preferable, and 0.05 to 0.15 is more preferable.
[0033] (Absorption rate of light with a wavelength of 600 nm or 700 nm) By appropriately adjusting the absorption rate of light with a wavelength of 600 nm or 700 nm of the phosphor of this embodiment, the luminescence characteristics of the phosphor of this embodiment may be further improved. Although the details are unknown, the absorption rate of light with a wavelength of 600 nm or 700 nm may be related to the surface condition of the phosphor or the amount of heterogeneous phases in the phosphor that do not contribute to or may adversely affect the luminescence characteristics of the phosphor. This can be inferred from the inventor's findings, for example, from the fact that the absorption rate of light with a wavelength of 600 nm or 700 nm of the phosphor changes during the production of the phosphor by acid treatment or elutriation treatment, as described below. It is believed that by appropriately adjusting the absorption rate of light with a wavelength of 600 nm or 700 nm, the performance of the phosphor, such as its luminescence characteristics, can be further improved.
[0034] Specifically, the absorptance of the phosphor of this embodiment for light with a wavelength of 600 nm is preferably 2.6 to 5.0%, more preferably 3.0 to 4.5%, and the absorptance of the phosphor of this embodiment for light with a wavelength of 700 nm is preferably 2.5 to 4.5%, more preferably 2.5 to 4.0%.
[0035] (Diffuse reflectance of light with a wavelength of 700 nm or 800 nm) By appropriately setting the diffuse reflectance of light with a wavelength of 700 nm or 800 nm of the phosphor of this embodiment, the light-emitting characteristics of the phosphor of this embodiment may be further improved. Although the details are unclear, the diffuse reflectance of light with a wavelength of 700 nm or 800 nm may also be related to the surface condition of the phosphor and the amount of heterogeneous phases in the phosphor that do not contribute to or may adversely affect the light-emitting characteristics of the phosphor (diffuse reflectance may also change depending on, for example, the conditions of the acid treatment or elutriation treatment in the production of the phosphor). Therefore, it is believed that by appropriately adjusting these values, the performance of the phosphor, such as its light-emitting characteristics, can be further improved.
[0036] Specifically, the diffuse reflectance of the phosphor of this embodiment for light with a wavelength of 700 nm is preferably 93.0 to 98.5%, more preferably 94.0 to 98.0%, and the diffuse reflectance of the phosphor of this embodiment for light with a wavelength of 800 nm is preferably 93.0 to 98.5%, more preferably 94.0 to 98.0%.
[0037] (Peak Wavelength, Half-Width, Chromaticity, etc. of Emission Spectrum) The phosphor of this embodiment may exhibit characteristic emission due to, for example, having the composition of the general formula shown above. Specifically, the peak wavelength of the fluorescence emitted when the phosphor of this embodiment is irradiated with light having a wavelength of 405 nm is preferably 475 to 495 nm, more preferably 480 to 495 nm. Furthermore, the half-width (full width at half maximum) of the peak of the fluorescence emitted when the phosphor of this embodiment is irradiated with light having a wavelength of 405 nm is preferably 70 to 90 nm, more preferably 72 to 85 nm. Furthermore, in the XYZ color system, x of the fluorescence emitted when the phosphor of this embodiment is irradiated with light having a wavelength of 405 nm is preferably 0.170 to 0.225, and y is preferably 0.300 to 0.430.
[0038] Incidentally, the above-described characteristic light emission is different from the light emission of general-purpose phosphors (for example, the light emission of YAG phosphors that are often used as wavelength conversion materials for white LEDs). Therefore, it can be said that the phosphor of this embodiment can be preferably applied to applications other than ordinary lighting applications and display device applications. For example, the phosphor of this embodiment can be preferably applied as a wavelength conversion material for an autonomous driving indicator lamp (an indicator light for indicating to the outside of a vehicle that the vehicle is in autonomous driving) proposed by SAE International (Society of Automotive Engineers). Specifically, SAE International has proposed a light-emitting device for use as an automatic driving display lamp, which emits light within the region defined by connecting five points in the XYZ color system: (x, y) = (0.012, 0.495), (0.200, 0.400), (0.200, 0.320), (0.040, 0.320), and (0.012, 0.495). The phosphor of this embodiment is useful as a wavelength conversion member for constructing such a light-emitting device. Of course, the phosphor of this embodiment can be used in a variety of applications, not limited to the above applications.
[0039] (Method for manufacturing phosphor) The phosphor of this embodiment can be manufactured by using appropriate raw materials in appropriate ratios and through an appropriate manufacturing process. If the raw materials used or their blending are inappropriate, or if the manufacturing conditions are inappropriate, it may not be possible to manufacture a phosphor with good luminescence characteristics. An example of a preferred manufacturing process will be described below.
[0040] Preparation of raw materials First, raw materials containing Ba, Eu, etc. are prepared. The raw materials are usually in powder form. Ba-containing raw materials include BaAl 2 O 4 , BaCO 3 , BaO, Ba 2 N, Ba 3 N 2 Among these, from the viewpoint of further improving the performance of the phosphor that is finally produced, BaAl 2 O 4 When the phosphor of this embodiment finally contains Sr, the raw material containing Sr is preferably SrAl 2 O 4 , SrCO 3 , SrO, Sr 2 N, Sr 3 N 2 Examples of raw materials containing Eu include Eu 2 O 3 Examples of raw materials containing Si include Si 3 N 4 Examples of raw materials containing Al include Al 2 O 3 Examples include:
[0041] Weighing and mixing the raw materials: Weigh the prepared raw materials and mix them thoroughly to form a mixture. The amount (molar ratio) of each raw material is determined by back-calculating the values of a1, a2, b, c, d, e, and f in the general formula above. To ensure uniform mixing and remove coarse particles, it is preferable to pass the mixture through a sieve.
[0042] Firing: The mixture is filled into a heat-resistant container (preferably a boron nitride container) and heated to form a fired product. The firing temperature is preferably 1600 to 1800°C, more preferably 1600 to 1700°C. The firing time (the time the mixture is maintained at the temperature) is preferably 1 to 12 hours, more preferably 2 to 8 hours. Firing is preferably carried out in an inert gas atmosphere such as nitrogen gas. In this case, the gas pressure is preferably about 0.01 to 0.1 MPa·G.
[0043] Crushing / Pulverization The phosphor (calcined product) obtained by firing is usually in a lump form. Therefore, it is preferable to crush it appropriately. Furthermore, a pulverization treatment may be carried out to adjust the particle size. For example, a jet mill can be used for pulverization.
[0044] Annealing: Heating (annealing) the fired phosphor (fired product) at the same or lower temperature as the firing temperature can sometimes further improve the phosphor's luminescence and other performance characteristics. While the details are unclear, it is believed that annealing homogenizes and reconstructs the crystal structure within the phosphor. Annealing is preferably performed by placing the phosphor (fired product) in a heat-resistant container. A preferred heat-resistant container is a boron nitride container. The annealing temperature is preferably 1400 to 1550°C, more preferably 1450 to 1550°C. The annealing time (the time maintained at the temperature) is preferably 2 to 24 hours, more preferably 4 to 12 hours. Annealing is preferably performed in an inert gas atmosphere, such as nitrogen gas. The gas pressure is preferably about 0.01 to 0.1 MPa·G.
[0045] Acid Treatment The phosphor of this embodiment is preferably subjected to an acid treatment. The acid treatment can be performed, for example, by immersing the phosphor in an acid aqueous solution and stirring appropriately. The acid treatment may remove or reduce foreign matter on the phosphor surface or heterogeneous phases that do not contribute to fluorescence or that adversely affect the light-emitting characteristics. In other words, the acid treatment may further improve the properties of the phosphor. Incidentally, as a result of removing or reducing foreign matter or heterogeneous phases on the phosphor surface by the acid treatment, the light absorptance and diffuse reflectance of the phosphor may change.
[0046] The acid solution can be an aqueous solution containing one or more acids selected from hydrofluoric acid, sulfuric acid, phosphoric acid, hydrochloric acid, and nitric acid. Acid treatment can be performed by stirring the phosphor in the acid solution for several minutes to several hours (e.g., 10 minutes to 6 hours). A known stirrer or similar device can be used for stirring. In laboratories, a magnetic stirrer is preferably used. The temperature during stirring is, for example, 50 to 100°C, preferably 65 to 85°C (the liquid is maintained at this temperature). The stirring time is, for example, 1 minute to 2 hours, preferably 10 minutes to 1 hour. The stirring speed depends on the scale of the stirring device, but on a laboratory scale, it is, for example, 300 to 600 rpm, preferably 350 to 500 rpm. Stirring at a relatively high speed applies a strong shear force to the phosphor, thereby more effectively removing foreign matter and heterogeneous phases, which can ultimately lead to further improvements in the phosphor's performance. After the acid treatment, it is desirable to perform filtration, washing with water, drying, etc., as appropriate. Furthermore, when recovering the phosphor after the acid treatment, it is preferable to appropriately carry out decantation, suction filtration, or the like.
[0047] Classification (specifically, elutriation): Classification is preferably performed to reduce the amount of extremely small particle size phosphors (fine powder) in the powdered phosphor that do not contribute to improving the luminescence properties or adversely affect the luminescence properties. Specifically, elutriation is preferred for classification. The classification point is preferably set to approximately 3 to 10 μm. Incidentally, the classification point can be determined by calculation based on Stokes' equation or by several trial experiments. Elutriation is preferably performed by dispersing the powdered phosphor in an aqueous solution of sodium hexametaphosphate or water to create a dispersion, allowing the dispersion to stand, and then removing the supernatant. Other known methods can be used as the specific method of elutriation.
[0048] <Light-emitting device> A light-emitting device can be constructed by combining the above-mentioned phosphor with a light-emitting element. Specifically, a light-emitting device can be constructed by a light-emitting element that emits light capable of exciting the phosphor, and the above-mentioned phosphor that emits fluorescence upon receiving the light emitted from the light-emitting element. The phosphor is usually sealed with a sealing material and incorporated into the light-emitting device in the form of a wavelength conversion member.
[0049] In consideration of the characteristics of the phosphor described above, the light-emitting element is preferably a light-emitting element that emits light having a wavelength of 340 to 450 nm, and more preferably a light-emitting element that emits light having a wavelength of 375 to 410 nm. In consideration of manufacturing costs and applicability to various uses, the light-emitting element is preferably an LED element.
[0050] The application of the light emitting device of this embodiment is not particularly limited. The light emitting device of this embodiment can be applied to, for example, backlights for liquid crystal display devices, light source devices for projectors, lighting devices, traffic lights, etc. In addition, as described above, the light emitting device of this embodiment is considered to be useful as a lamp for indicating automatic driving.
[0051] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various other configurations may be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of achieving the object of the present invention are included in the present invention.
[0052] The embodiments of the present invention will be described in detail based on examples and comparative examples. It should be noted that the present invention is not limited to the examples. The steps, measurements, and evaluations described below were performed at 30°C unless otherwise specified.
[0053] <Preparation of Raw Materials> The following raw materials were prepared: BaAl 2 O 4 : SrAl manufactured by Kojundo Kagaku Kenkyusho Co., Ltd. 2 O 4 : Si manufactured by High Purity Chemical Laboratory Co., Ltd. 3 N 4 : Manufactured by UBE Corporation (product number: E10) Al 2 O 3 : Sumitomo Chemical Co., Ltd. (product number: AA-03) Eu 2 O 3 : Shin-Etsu Chemical Co., Ltd. (product number: RU)
[0054] <Production of Phosphor> A phosphor was produced as follows. (1) Weighing and Mixing of Raw Materials Each raw material was weighed in the amount shown in Table 1 below. All of the weighed raw materials were placed in a polyethylene bag with a zipper, the zipper was closed, and the bag was shaken for 1 minute. In this way, a mixture of raw materials was obtained. The resulting mixture was passed through a #100 sieve, and the mixture that passed through the sieve was used in the next step. In Table 1, the amount of each component is in grams.
[0055]
[0056] (2) Firing Approximately 100 g of the mixture obtained in (1) was filled into a 400 cc boron nitride container (manufactured by Denka, N1 grade). Then, it was fired under the following conditions. [Firing conditions] Firing furnace: Multipurpose firing furnace manufactured by Fuji Denpa Kogyo Co., Ltd. Firing temperature and holding time: 1650°C for 4 hours Firing atmosphere: N 2 0.03MPa・G(N 2 )
[0057] (3) Crushing / Pulverization The fired product was recovered from the container. The fired product was then crushed using a mortar. Thereafter, jet mill pulverization was carried out using a PJM-80SP device manufactured by Nippon New Match Industrial Co., Ltd., under the conditions of a sample supply rate of 20 g / min and a pulverization air pressure of 0.5 MPa.
[0058] (4) Annealing step The jet milled sample of (3) was filled into a 400 cc boron nitride container (manufactured by Denka, N1 grade). Then, annealing treatment was carried out under the following firing conditions. After annealing treatment, the sample was naturally cooled to room temperature, and the fired material was recovered from the container. The recovered material was crushed using a mortar so that it passed completely through a #200 sieve. [Annealing conditions] - Firing furnace: Multipurpose firing furnace manufactured by Fuji Denpa Kogyo Co., Ltd. - Firing temperature and holding time: 1500°C for 8 hours - Firing atmosphere: N 2 0.03MPa・G(N 2 )
[0059] (5) Acid Treatment and Decantation 10 mL of nitric acid (60% by mass, Fujifilm Wako Pure Chemical Industries, Ltd.) and 70 mL of ion-exchanged water were placed in a fluororesin beaker. The beaker was heated in a water bath until the liquid (acid aqueous solution) in the beaker reached 60°C. Approximately 20 g of the sample annealed and disintegrated in (4) was placed in the heated acid aqueous solution and stirred for 30 minutes. A magnetic stirrer was used for stirring. The rotation speed was set to 400 rpm. After stirring, the beaker was lifted from the water bath and moved, and allowed to stand for approximately 10 minutes. The supernatant was then removed by decantation, a total of three times. The slurry sample obtained after decantation was recovered by suction filtration. The recovered sample was then dried at 100°C for 12 hours. The dried sample was sieved through a #200 nylon sieve.
[0060] (6) Classification (elutriation) Based on Stokes' equation, the necessary and sufficient settling time of the phosphor powder to remove fine particles with a particle diameter of 7 μm or less when performing elutriation was calculated in advance. Based on this calculation, the sample (5) dispersed in the dispersion medium was placed in a 500 mL bottle and allowed to stand for a predetermined time, after which the supernatant liquid above a predetermined level was removed. A 0.05% by mass aqueous solution of sodium hexametaphosphate was used as the dispersion medium. This procedure was repeated several times. The powder finally obtained as a precipitate was recovered by filtration and dried. In this way, a dried powdered phosphor was obtained.
[0061] <Composition Analysis> The Ba, Sr, Eu, Al, and Si contents in the phosphor were quantitatively analyzed using an ICP optical emission spectrometer (5110VDV manufactured by Agilent) after dissolving the phosphor by pressure acid decomposition. The O and N contents in the phosphor were quantitatively analyzed using an oxygen and nitrogen analyzer (EMGA-920 manufactured by Horiba, Ltd.)." Based on these analysis results, the general formula Ba a1 Sr a2 EU b Al c Si d O e N f In this case, the composition ratios a1, a2, b, c, d, e, and f were determined when c+d=5. The results of the composition analysis are shown in Table 2.
[0062]
[0063] <Particle size distribution measurement> Using a Microtrac SYNC (manufactured by Microtrac Bell Co., Ltd.), measurement was performed by a laser diffraction scattering method in accordance with JIS R1629:1997. 0.2 g of phosphor powder was added to 80 cc of an aqueous solution containing 0.05 mass % sodium hexametaphosphate as a dispersant, and the mixture was dispersed for 90 seconds using a horn-type ultrasonic homogenizer (output 300 W, horn diameter 26 mm). The particle size distribution was then measured using the SYNC. From the obtained particle size distribution, the volume-based median diameter D 50 The obtained D 50 The values are shown in Table 3.
[0064]
[0065] <X-ray diffraction measurement> The X-ray diffraction spectrum of the obtained sample was measured. For the measurement, an Ultima IV-N device manufactured by Rigaku Corporation was used. In the obtained X-ray diffraction spectrum, the values of the peak intensity (maximum value) A in the 2θ range of 25.0 to 26.0° and the peak intensity (maximum value) B in the 2θ range of 29.0 to 30.0° were read. Then, the value of B / A was calculated.
[0066] The obtained X-ray diffraction spectrum is shown in Figure 1. For reference, the lower part of Figure 1 shows the general formula BaAl 2 Si 3 O 4 N 4 The table also shows the positions of peaks in the X-ray diffraction spectrum of the crystals of the inorganic compound represented by the formula (1). The values of B / A are also shown in Table 4. Just to be clear, the values of A and B shown in Table 4 are relative values.
[0067]
[0068] <Absorptance of Light with a Wavelength of 600 nm or 700 nm, and Diffuse Reflectance of Light with a Wavelength of 700 nm or 800 nm> The absorptance (%) of light with a wavelength of 600 nm was determined in the same manner as described below (Characteristics When Irradiated with Light of a Wavelength of 405 nm, Part 1), except that the wavelength of the irradiated light was 600 nm instead of 405 nm, and Qex and Qref were calculated from the spectrum in the wavelength range of 595 nm to 610 nm. The absorptance (%) of light with a wavelength of 700 nm was determined in the same manner as described below (Characteristics When Irradiated with Light of a Wavelength of 405 nm, Part 1), except that the wavelength of the irradiated light was 700 nm instead of 405 nm, and Qex and Qref were calculated from the spectrum in the wavelength range of 695 nm to 710 nm.
[0069] Diffuse reflectance was measured using an integrating sphere device (ISV-469) attached to a JASCO UV-visible spectrophotometer (V-550). Specifically, baseline correction was first performed using a standard reflector (Spectralon). Then, a solid sample holder filled with phosphor powder was attached to a predetermined position, and the diffuse reflectance for light with wavelengths of 700 nm and 800 nm was measured.
[0070] The above absorbance and diffuse reflectance values are shown in Table 5.
[0071]
[0072] <Performance Evaluation> (Various Characteristics When Irradiated with Light at a Wavelength of 405 nm) Using a spectrophotometer (MCPD-7000 manufactured by Otsuka Electronics Co., Ltd.), the absorptivity, internal quantum efficiency, and external quantum efficiency when the phosphor was irradiated with light at a wavelength of 405 nm were determined. The specific procedure was as follows: (1) The powdered phosphor was filled into a concave cell. The surface of the filled phosphor was made smooth. This cell was attached to a predetermined position on an integrating sphere. Monochromatic light, split into 405 nm wavelengths from a light source (Xe lamp), was introduced into the integrating sphere using an optical fiber. This monochromatic light was irradiated onto the phosphor, and the fluorescence spectrum was measured. (2) A standard reflector (Spectralon manufactured by Labsphere) with a reflectance of 99% was attached to a predetermined position on the integrating sphere, and the spectrum of excitation light at a wavelength of 405 nm was measured. The number of excitation light photons (Qex) was calculated from the spectrum in the wavelength range from 400 nm to 415 nm. (3) A cell filled with powdered phosphor was attached to a predetermined position on the integrating sphere, and the number of reflected excitation light photons (Qref) and the number of fluorescent photons (Qem) were calculated from the obtained spectral data. The number of reflected excitation light photons was calculated over the same wavelength range as the number of excitation light photons, and the number of fluorescent photons was calculated over the range of 415 nm to 800 nm. (4) The obtained Qex, Qref, and Qem were substituted into the following formulas to determine the absorptance, internal quantum efficiency, and external quantum efficiency: Absorptance = (Qex - Qref) / Qex Internal quantum efficiency = Qem / (Qex - Qref) External quantum efficiency = Qem / Qex Table 6 below lists the values above multiplied by 100 and expressed as a percentage.
[0073] Furthermore, the peak wavelength, half-width, chromaticity x value, and chromaticity y value were determined from the fluorescence spectrum obtained by this measurement. Regarding the method for determining chromaticity, the chromaticity coordinates (x, y) were calculated using the calculation method for the XYZ color system specified in JIS Z 8701 in accordance with JIS Z 8724 (Method for measuring color - Light source color).
[0074] (Characteristics at high temperatures) Integral intensity maintenance rate The integral intensity of the fluorescent spectrum when the phosphor is irradiated with light of 405 nm wavelength at 30°C is expressed as I 0 The integrated intensity of the fluorescence spectrum when the phosphor is irradiated with light of 405 nm wavelength at 200° C. is defined as I. Then, (I / I 0 ) × 100 (%) was calculated. The larger this value (the closer it is to 100%), the better the performance of the phosphor is maintained even in a high-temperature environment. Phosphors with a large integral intensity maintenance rate are preferably used for, for example, lighting devices used in vehicles or in harsh environments.
[0075] External quantum efficiency at 200° C. The external quantum efficiency was determined by the method described above (Various characteristics when irradiated with light having a wavelength of 405 nm, Part 1), except that the phosphor was heated to 200° C. In addition, the relative value of the external quantum efficiency of each phosphor was calculated, assuming that the external quantum efficiency of the phosphor of Example 1 was 100.
[0076] The results of the performance evaluation are summarized in Table 6.
[0077]
[0078] As shown in Table 6, the luminescence properties such as external quantum efficiency of the phosphors of Examples 2 to 4 were good. a1 Sr a2 EU b Al c Si d O e N fand the phosphors satisfying the following formulae a1>a2, 0.70≦a1+a2+b≦1.20, 0.20≦b≦0.50, 1.50≦c≦2.50, 2.50≦d≦3.50, 3.05≦e≦6.50, and 2.75≦f≦4.40 exhibited good luminescence characteristics. Such good luminescence characteristics are mainly due to the general formula Ba a1 Sr a2 EU b Al c Si d O e N f This is thought to be due to the relatively large value of b in the phosphors and the relatively large Eu content. Furthermore, the luminescence characteristics are thought to be further improved by acid treatment and elutriation treatment after firing the phosphors. Furthermore, the phosphors of Examples 2 to 4 exhibited good characteristics even at high temperatures of around 200°C.
[0079] This application claims priority based on Japanese Patent Application No. 2023-086760, filed May 26, 2023, the disclosure of which is incorporated herein by reference in its entirety.
Claims
1. General formula Ba a1 Sr a2 EU b A c S d O e N f and the composition ratios a1, a2, b, c, d, e, and f have the following relationship when c+d=5: a1>a2 0.70≦a1+a2+b≦1.20 0.20≦b≦0.50 1.50≦c≦2.50 2.50≦d≦3.50 3.05≦e≦6.50 2.75≦f≦4.40 2. The phosphor according to claim 1, wherein 0≦a2≦0.
10.
3. The phosphor according to claim 1 or 2, wherein 0.40≦a1≦0.
80.
4. The phosphor according to claim 1 or 2, which has an absorptivity of 89% or more for light with a wavelength of 405 nm.
5. The phosphor according to claim 1 or 2, which emits fluorescence having a peak wavelength of 475 to 495 nm when irradiated with light having a wavelength of 405 nm.
6. The phosphor according to claim 1 or 2, wherein the median diameter D 50 A phosphor that is a powder having a particle size of 10 to 30 μm.
7. The phosphor according to claim 1 or 2, wherein in an X-ray diffraction spectrum obtained by X-ray diffraction measurement of said phosphor, when the intensity of a peak in the 2θ range of 25.0 to 26.0° is defined as A and the intensity of a peak in the 2θ range of 29.0 to 30.0° is defined as B, the value of B / A is 0.15 or less.
8. A light emitting device comprising a light emitting element and the phosphor according to claim 1 or 2.
9. A light emitting device according to claim 8, wherein the light emitting element emits light having a wavelength of 340 to 450 nm.
10. The light emitting device according to claim 8, wherein the light emitting element is an LED element.
11. A light emitting device according to claim 8, which is a lighting device or a signaling device.
Citation Information
Patent Citations
Silica nitride fluorescent powder and preparation method thereof
CN102181285A
Phosphor and production method therefor, and light emission device and image display device using phosphor
WO2013069696A1
Phosphor, light-emitting device, and method for manufacturing same
WO2015093429A1