Phosphor and light emitting device

The development of a phosphor with specific composition and manufacturing optimizations addresses the limitations of conventional phosphors, enhancing external and internal quantum efficiency and light emission characteristics, making it suitable for advanced light-emitting devices.

WO2024247687A1PCT designated stage expired Publication Date: 2024-12-05DENKA CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/017603
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-26
Filing Date
2024-05-13
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conventional phosphors used in light-emitting devices have limitations in terms of external quantum efficiency and light emission characteristics, which can be improved.

Method used

A phosphor with the general formula Baα1Srα2CeβAlcSi dOeNf is developed, where specific composition ratios and manufacturing processes optimize the luminescent properties, including a peak wavelength of fluorescence between 412 to 420 nm, internal quantum efficiency of 50 to 90%, and appropriate particle size distribution, to enhance light emission characteristics.

Benefits of technology

The optimized phosphor achieves improved external quantum efficiency, internal quantum efficiency, and light emission characteristics, making it suitable for use in light-emitting devices such as LEDs, particularly in applications requiring broad spectrum emission like automotive lighting and industrial inspection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024017603_05122024_PF_FP_ABST
    Figure JP2024017603_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed is a phosphor which is represented by general formula Baa1Sra2CebAlcSidOeNf. In the general formula, when c + d = 5, the composition ratios a1, a2, b, c, d, e, and f satisfy a1 > a2, 0.70 ≤ a1 + a2 + b ≤ 1.20, 0.001 ≤ b ≤ 0.20, 1.50 ≤ c ≤ 2.50, 2.50 ≤ d ≤ 3.50, 3.05 ≤ e ≤ 6.50, and 2.75 ≤ f ≤ 4.40. In addition, the peak wavelength of fluorescence emitted when the phosphor is irradiated with light having a wavelength of 350 nm is 412-420 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Phosphor and light-emitting device

[0001] The present invention relates to a phosphor and a light-emitting device.

[0002] Phosphors are sometimes used industrially to form wavelength conversion components in light-emitting devices, i.e., components that convert short-wavelength light into long-wavelength light, and with the recent widespread use of LEDs (light-emitting diodes), phosphors have become increasingly important industrially.

[0003] Claim 1 of Patent Document 1 describes a compound represented by the general formula: Me a Re b Al c Si d O e N f (where Me is one or more elements selected from Sr and Ba, and Re is Eu), and a phosphor is disclosed in which the composition ratios a, b, c, d, e, and f have the following relationships: a+b=1 0.005<b<0.25 1.60<c<2.60 2.45<d<4.05 3.05<e<5.00 2.75<f<4.40

[0004] In addition, in Patent Document 2, in Example 11, a design composition is Ce 0.05 Sr 0.95 Al 2 Si 3 O 4 N 4 Patent Document 2 also describes that when this phosphor is irradiated with excitation light having a peak wavelength of 340 nm, light emission having a peak wavelength of 411 nm is observed.

[0005] Furthermore, Patent Document 3 can be cited as a document that describes a phosphor having a chemical structure or chemical composition similar to those of the phosphors described in Patent Documents 1 and 2.

[0006] International Publication No. 2014 / 091776 International Publication No. 2013 / 069696 International Publication No. 2015 / 093429

[0007] As a result of preliminary studies by the present inventors, it has been found that conventional phosphors such as those described in Patent Documents 1 to 3 have room for improvement in terms of luminescence properties such as external quantum efficiency.

[0008] The present invention has been made in view of the above circumstances, and one of the objects of the present invention is to provide a phosphor having good luminescence properties such as external quantum efficiency.

[0009] The present inventors have completed the invention provided below and solved the above problems.

[0010] 1. General formula Ba a1 Sr a2 Ce b Al c Si d O e N fwherein the composition ratios a1, a2, b, c, d, e, and f satisfy the following relationship when c+d=5, and the peak wavelength of fluorescence emitted when irradiated with light of a wavelength of 350 nm is 412 to 420 nm. a1>a2 0.70≦a1+a2+b≦1.20 0.001≦b≦0.20 1.50≦c≦2.50 2.50≦d≦3.50 3.05≦e≦6.50 2.75≦f≦4.40 2. A phosphor according to 1., wherein 0.50≦a1≦0.99. 3. A phosphor according to 1. or 2., wherein 0≦a2≦0.10. 4. A phosphor according to 1. to 3. 4. The phosphor according to any one of 1. to 4., wherein the half width of the spectrum of fluorescence emitted when irradiated with light having a wavelength of 350 nm is 75 to 130 nm. 5. The phosphor according to any one of 1. to 4., wherein the absorptance of light having a wavelength of 500 nm is 1 to 10%. 6. The phosphor according to any one of 1. to 5., wherein the internal quantum efficiency when irradiated with light having a wavelength of 350 nm is 50 to 90%. 7. The phosphor according to any one of 1. to 6., wherein in an X-ray diffraction spectrum obtained by X-ray diffraction measurement of the phosphor, the value of B / A is 0.3 or less, where A is the intensity of the peak in 2θ range of 25.0 to 26.0 degrees and B is the intensity of the peak in 2θ range of 29.0 to 30.0 degrees. 8. 1. to 7. 9. The phosphor according to any one of items 1. to 8., wherein the diffuse reflectance of light having a wavelength of 700 nm is 92 to 97%. 10. The phosphor according to any one of items 1. to 9., wherein the diffuse reflectance of light having a wavelength of 800 nm is 92 to 97%. 11. The phosphor according to any one of items 1. to 9., wherein the median diameter D 50a phosphor in the form of a powder having a particle size of 10 to 50 μm. 11. The phosphor according to any one of 1. to 10., which is substantially free of Eu. 12. A light emitting device comprising a light emitting element and the phosphor according to any one of 1. to 11.. 13. The light emitting device according to 12., wherein the light emitting element is a light emitting element emitting light at a wavelength of 300 to 400 nm. 14. The light emitting device according to 12. or 13., wherein the light emitting element is an LED element. 15. The light emitting device according to any one of 12. to 14., which is a lighting device or a signaling device.

[0011] According to the present invention, a phosphor having good luminescence properties such as external quantum efficiency is provided.

[0012] FIG. 2 is a diagram showing X-ray diffraction spectra of phosphors of Examples and Comparative Examples.

[0013] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. In this specification, the expression "X to Y" in the description of a numerical range means X or more and Y or less, unless otherwise specified. For example, "1 to 5 mass %" means "1 mass % or more and 5 mass % or less."

[0014] <Phosphor> The phosphor of this embodiment is a phosphor represented by the general formula Ba a1 Sr a2 Ce b Al c Si d O e N f In this general formula, when c + d = 5, the composition ratios a1, a2, b, c, d, e, and f have the following relationships: a1 > a2 0.70 ≦ a1 + a2 + b ≦ 1.20 0.001 ≦ b ≦ 0.20 1.50 ≦ c ≦ 2.50 2.50 ≦ d ≦ 3.50 3.05 ≦ e ≦ 6.50 2.75 ≦ f ≦ 4.40

[0015] Furthermore, when the phosphor of this embodiment is irradiated with light having a wavelength of 350 nm, the peak wavelength of the fluorescence emitted is 412 to 420 nm.

[0016] One of the characteristics of the phosphor of this embodiment is that it contains a relatively small amount of Ce from the viewpoint of composition. Based on past findings, it is believed that this relatively small amount of Ce functions as a luminescence center. Another characteristic of the composition is that a1 > a2, i.e., a relatively large amount of Ba is contained compared to Sr, and because a1 > a2, a1 > 0 automatically occurs, meaning that Ba is always contained in the composition (because a2 = 0 is possible). Although the details are unknown, the appropriate ratio of the luminescence center Ce to the surrounding elements such as Ba may lead to the good external quantum efficiency of the phosphor of this embodiment.

[0017] Furthermore, through further investigation, the inventors discovered that, for the above-mentioned composition and its neighboring compositions, the peak wavelength of fluorescence emitted when irradiated with light having a wavelength of 350 nm appears to correlate with the magnitude of external quantum efficiency. Based on this finding, the peak wavelength of fluorescence emitted when irradiated with light having a wavelength of 350 nm was adopted as one of the design indicators. Specifically, the external quantum efficiency was improved by designing a phosphor so that the peak wavelength of fluorescence emitted when irradiated with light having a wavelength of 350 nm is 412 to 420 nm. Although the details are unknown, it is presumed that if the phosphor contains a large amount of heterogeneous phases, impurities, fine particles, etc., which hinder the improvement of external quantum efficiency, the presence of these substances will cause the peak fluorescence wavelength to fall outside the range of 412 to 420 nm (often exceeding 420 nm). In contrast, if the phosphor contains few heterogeneous phases, impurities, fine particles, etc., the peak fluorescence wavelength is thought to fall within the range of 412 to 420 nm.

[0018] The phosphor of this embodiment can be manufactured by using appropriate raw materials in appropriate ratios and through an appropriate manufacturing process. In order to obtain a phosphor with good luminescence properties, it is effective to optimize the selection and blending of raw materials, as well as the manufacturing conditions. For example, with regard to the manufacturing process, the luminescence properties may be further improved by performing an acid treatment or classification treatment, which will be described later. On the other hand, if the manufacturing conditions are inappropriate, a phosphor with the desired properties may not be obtained even if appropriate raw materials are used in appropriate ratios.

[0019] The phosphor of this embodiment will be further described.

[0020] (General formula) General formula Ba a1 Sr a2 Ce b Al c Si d O e N f In the formula, when c+d=5, the values ​​of the composition ratios a1, a2, b, c, d, e, and f are as follows:

[0021] Regarding a1, a2, and b, it is sufficient that a1>a2, 0.70≦a1+a2+b≦1.20, and 0.001≦b≦0.20. From the viewpoint of particularly good light-emitting properties, a1 is preferably 0.50≦a1≦0.99, more preferably 0.70≦a1≦0.99, even more preferably 0.85≦a1≦0.97, and particularly preferably 0.90≦a1≦0.96. From the viewpoint of particularly good light-emitting properties, a2 is preferably 0≦a2≦0.10, more preferably 0≦a2≦0.05, and even more preferably 0≦a2≦0.02. a2 may be zero. From the viewpoint of particularly good light-emitting properties, b is preferably 0.001≦b≦0.15, and more preferably 0.003≦b≦0.10. With respect to a1+a2+b, 0.80≦a1+a2+b≦1.10 is preferable, and 0.90≦a1+a2+b≦1.00 is more preferable.

[0022] Although c may be in the range of 1.50≦c≦2.50, it is preferable that c is in the range of 1.70≦c≦2.30, more preferably 1.80≦c≦2.20, and even more preferably 1.90≦c≦2.10.

[0023] The value of d may be in the range of 2.50≦d≦3.50, preferably 2.70≦d≦3.30, more preferably 2.80≦d≦3.20, and even more preferably 2.90≦d≦3.10.

[0024] The value of e may be in the range of 3.05≦e≦6.50, preferably 4.00≦e≦6.50, more preferably 4.50≦e≦6.25, even more preferably 5.00≦e≦6.00, particularly preferably 5.00≦e≦5.80, and especially preferably 5.00≦e≦5.50.

[0025] The value of f may be in the range of 2.75≦f≦4.40, preferably 3.00≦f≦4.30, more preferably 3.00≦f≦4.00, and even more preferably 3.20≦f≦3.80.

[0026] From the viewpoint of stabilizing the crystal structure, the relative magnitudes between the respective values ​​are preferably as follows: c / d: preferably 0.50<c / d<0.80, more preferably 0.55<c / d<0.75, even more preferably 0.60<c / d<0.75, particularly preferably 0.62<c / d<0.73 e / f: preferably 0.90<e / f<2.00, more preferably 1.00<e / f<1.90, even more preferably 1.20<e / f<1.80

[0027] The phosphor of this embodiment usually does not substantially contain Eu. This is because, as described above, Ce is thought to function as the luminescence center in the phosphor of this embodiment. Specifically, "substantially does not contain" means that the ratio of Eu when c + d = 5 in the general formula described above is preferably 0.001 or less, more preferably 0.0001 or less. Preferably, the phosphor of this embodiment does not contain Eu.

[0028] (Regarding Fluorescence Emitted When Irradiated with Light Having a Wavelength of 350 nm) The phosphor of this embodiment may have a characteristic fluorescence spectrum due to its chemical composition, etc. As an example, the half-width (full width at half maximum) of the fluorescence spectrum emitted when irradiated with light having a wavelength of 350 nm to the phosphor of this embodiment is preferably 75 to 130 nm, more preferably 75 to 100 nm, even more preferably 80 to 95 nm, and particularly preferably 80 to 90 nm. From another perspective, the internal quantum efficiency when irradiated with light having a wavelength of 350 nm to the phosphor of this embodiment is preferably 50 to 95%, more preferably 60 to 95%, and even more preferably 70 to 90%. From another viewpoint, the chromaticity x of the fluorescence emitted when the phosphor of this embodiment is irradiated with light having a wavelength of 350 nm in the XYZ color system is preferably 0.168 to 0.182, more preferably 0.170 to 0.180, and the chromaticity y is preferably 0.095 to 0.135, more preferably 0.100 to 0.130.

[0029] (Absorptance of Light with a Wavelength of 500 nm) When the phosphor of this embodiment has an appropriate absorptance of light with a wavelength of 500 nm, it may be possible to further improve luminescence characteristics such as external quantum efficiency. Specifically, the absorptance of the phosphor of this embodiment with respect to light with a wavelength of 500 nm is preferably 1 to 10%, more preferably 3 to 9%, even more preferably 4 to 8%, and particularly preferably 4 to 7%.

[0030] (Crystal Structure and X-ray Diffraction Spectrum) According to the knowledge of the present inventors, the phosphor of this embodiment is generally a phosphor represented by the general formula BaAl 2 Si 3 O 4 N 4 Specifically, the phosphor of this embodiment has a crystal structure identical to or similar to that of a crystal of an inorganic compound represented by the general formula BaAl 2 Si 3 O 4 N 4 It can be considered that a part of Ba in the above crystal structure is substituted with Ce or Sr to form a solid solution. Due to the above crystal structure, the X-ray diffraction spectrum of the phosphor of this embodiment usually has a structure represented by the general formula BaAl 2 Si 3 O4 N 4 The peak is at approximately the same position (2θ) as the peak observed in the X-ray diffraction spectrum of a crystal of an inorganic compound represented by the general formula BaAl 2 Si 3 O 4 N 4 The positions of the peaks in the X-ray diffraction spectrum of the crystal of the inorganic compound represented by the formula (I) are shown at the bottom of FIG.

[0031] General formula BaAl 2 Si 3 O 4 N 4 The ratio of the heterophase in the phosphor of this embodiment can be estimated by comparing the X-ray diffraction spectrum of a crystal of an inorganic compound represented by the general formula BaAl with the X-ray diffraction spectrum of the phosphor of this embodiment and analyzing diffraction peaks that are not present in the former but are present in the latter. 2 Si 3 O 4 N 4 This phase has a crystal structure different from the crystal structure of the inorganic compound represented by the formula (I), and may not contribute to or may adversely affect the luminescence characteristics of the phosphor of this embodiment. Specifically, in the X-ray diffraction spectrum obtained by X-ray diffraction measurement of the phosphor of this embodiment, when the intensity of the peak in the 2θ range of 25.0 to 26.0° is defined as A and the intensity of the peak in the 2θ range of 29.0 to 30.0° is defined as B, the value of B / A is preferably 0.3 or less, more preferably 0.2 or less. Ideally, the value of B / A is zero, but considering production costs and the like, a practical value of 0.01 to 0.3 is preferable, and 0.03 to 0.2 is more preferable.

[0032] (Diffuse reflectance of light with a wavelength of 700 nm or 800 nm) The diffuse reflectance of the phosphor of this embodiment for light with a wavelength of 700 nm or 800 nm is preferably appropriate, which may further improve the luminescence characteristics of the phosphor of this embodiment. Although the details are unclear, the diffuse reflectance of light with a wavelength of 700 nm or 800 nm may also be related to the surface condition of the phosphor and the amount of heterogeneous phases in the phosphor that do not contribute to or may adversely affect the luminescence characteristics of the phosphor (diffuse reflectance may also vary depending on, for example, the conditions of acid treatment or elutriation treatment in phosphor production). Furthermore, according to past findings, there may be a correlation between the magnitude of diffuse reflectance in wavelength regions not directly related to luminescence and the degree of crystallinity of the host crystal. Since low crystallinity can inhibit luminescence (fluorescence), it is believed that a high diffuse reflectance and high crystallinity are preferable. For these presumed reasons, it is believed that by appropriately adjusting the diffuse reflectance of light with a wavelength of 700 nm or 800 nm, the performance of the phosphor, such as its luminescence characteristics, can be further improved.

[0033] Specifically, the diffuse reflectance of the phosphor of this embodiment for light with a wavelength of 700 nm is preferably 92 to 98%, more preferably 93 to 97%. The diffuse reflectance of the phosphor of this embodiment for light with a wavelength of 800 nm is preferably 92 to 98%, more preferably 93 to 97%.

[0034] (Particle size distribution: median diameter D 50 The phosphor of this embodiment is typically in a powder form. In other words, the phosphor of this embodiment is an aggregate of phosphor particles. By having an appropriate particle size distribution of the powdered phosphor of this embodiment, it may be possible to further improve various performances such as light-emitting characteristics. The particle size distribution can be adjusted, for example, by changing the pulverization conditions or the elutriation conditions in the phosphor manufacturing process described below.

[0035] Specifically, the median diameter D of the powdered phosphor of this embodiment is 50The volume-based cumulative 10% particle diameter D (measured by laser diffraction / scattering method) of the powdered phosphor of this embodiment is preferably 10 to 50 μm, more preferably 10 to 40 nm. 10 The volume-based cumulative 90% particle diameter D of the powdered phosphor of this embodiment, determined by a laser diffraction / scattering method, is preferably 3 to 25 μm, and more preferably 5 to 20 μm. 90 is preferably 20 to 80 μm, more preferably 25 to 70 μm.

[0036] From another perspective, (D 90 -D 10 ) / D 50 The value of is preferably 1.20 to 1.90, more preferably 1.30 to 1.80. This value indicates that the particle size distribution of the powdered phosphor is relatively sharp. A sharp particle size distribution means that the phosphor particles in the powdered phosphor are homogeneous at least in terms of particle size. This is expected to lead to stable light emission and to reduce variations in light emission characteristics between product lots. In addition, (D 90 -D 10 ) / D 50 The fact that the value of is not too large can also be said to mean that the powdered phosphor contains a relatively small proportion of coarse particles or phosphors with extremely small particle sizes (fine powder), which do not contribute to improving the light-emitting properties or have a negative effect on the light-emitting properties.

[0037] (Method for manufacturing phosphor) The phosphor of this embodiment can be manufactured by using appropriate raw materials in appropriate ratios and through an appropriate manufacturing process. If the raw materials used or their blending are inappropriate, or if the manufacturing conditions are inappropriate, it may not be possible to manufacture a phosphor with good luminescence characteristics. An example of a preferred manufacturing process will be described below.

[0038] Preparation of raw materials First, raw materials containing Ba, Eu, etc. are prepared. The raw materials are usually in powder form. Ba-containing raw materials include BaAl 2 O 4, BaCO 3 , BaO, Ba 2 N, Ba 3 N 2 Among these, from the viewpoint of further improving the performance of the phosphor that is finally produced, BaAl 2 O 4 When the phosphor of this embodiment contains Sr, the raw material containing Sr is preferably SrAl 2 O 4 , SrCO 3 , SrO, Sr 2 N, Sr 3 N 2 Examples of raw materials containing Ce include CeO, etc. Examples of raw materials containing Si include Si 3 N 4 Examples of raw materials containing Al include Al 2 O 3 Examples include:

[0039] Weighing and mixing the raw materials: Weigh the prepared raw materials and mix them thoroughly to form a mixture. The amount (molar ratio) of each raw material is determined by back-calculating the values ​​of a1, a2, b, c, d, e, and f in the general formula above. To ensure uniform mixing and remove coarse particles, it is preferable to pass the mixture through a sieve.

[0040] Firing: The mixture is filled into a heat-resistant container (preferably a boron nitride container) and heated to form a fired product. The firing temperature is preferably 1500 to 1800°C, more preferably 1500 to 1700°C. The firing time (the time the mixture is maintained at the temperature) is preferably 1 to 12 hours, more preferably 2 to 8 hours. Firing is preferably carried out in an inert gas atmosphere such as nitrogen gas. In this case, the gas pressure is preferably about 0.01 to 0.1 MPa·G.

[0041] Crushing / Pulverization The phosphor (calcined product) obtained by firing is usually in a lump form. Therefore, it is preferable to crush it appropriately. Furthermore, a pulverization treatment may be carried out to adjust the particle size. For example, a jet mill can be used for pulverization.

[0042] Annealing: Heating (annealing) the fired phosphor (fired product) at the same or lower temperature as the firing temperature can sometimes further improve the phosphor's luminescence and other performance characteristics. While the details are unclear, it is believed that annealing homogenizes and reconstructs the crystal structure within the phosphor. Annealing is preferably performed by placing the phosphor (fired product) in a heat-resistant container. A preferred heat-resistant container is a boron nitride container. The annealing temperature is preferably 1400 to 1550°C, more preferably 1450 to 1550°C. The annealing time (the time maintained at the temperature) is preferably 2 to 24 hours, more preferably 4 to 12 hours. Annealing is preferably performed in an inert gas atmosphere, such as nitrogen gas. The gas pressure is preferably about 0.01 to 0.1 MPa·G.

[0043] Acid Treatment The phosphor of this embodiment is preferably subjected to an acid treatment. The acid treatment can be performed, for example, by immersing the phosphor in an acid aqueous solution and stirring appropriately. The acid treatment may remove or reduce foreign matter on the phosphor surface or heterogeneous phases that do not contribute to fluorescence or that adversely affect the light-emitting characteristics. In other words, the acid treatment may further improve the properties of the phosphor. Incidentally, as a result of removing or reducing foreign matter or heterogeneous phases on the phosphor surface by the acid treatment, the light absorptance and diffuse reflectance of the phosphor may change.

[0044] The acid solution can be an aqueous solution containing one or more acids selected from hydrofluoric acid, sulfuric acid, phosphoric acid, hydrochloric acid, and nitric acid. Acid treatment can be performed by stirring the phosphor in the acid solution for several minutes to several hours (e.g., 10 minutes to 6 hours). A known stirrer or similar device can be used for stirring. In laboratories, a magnetic stirrer is preferably used. The temperature during stirring is, for example, 50 to 100°C, preferably 65 to 85°C (the liquid is maintained at this temperature). The stirring time is, for example, 1 minute to 2 hours, preferably 10 minutes to 1 hour. The stirring speed depends on the scale of the stirring device, but on a laboratory scale, it is, for example, 300 to 600 rpm, preferably 350 to 500 rpm. Stirring at a relatively high speed applies a strong shear force to the phosphor, thereby more effectively removing foreign matter and heterogeneous phases, which can ultimately lead to further improvements in the phosphor's performance. After the acid treatment, it is desirable to perform filtration, washing with water, drying, etc., as appropriate. Furthermore, when recovering the phosphor after the acid treatment, it is preferable to appropriately carry out decantation, suction filtration, or the like.

[0045] Classification (preferably elutriation) Classification is preferable to reduce the amount of extremely small particle size phosphor (fine powder) in the powdered phosphor, which does not contribute to improving or adversely affects the luminescence characteristics. While various specific classification methods are possible, in this embodiment, classification by elutriation is preferable. When performing classification, the classification point is preferably set to approximately 3 to 10 μm. Incidentally, when performing classification by elutriation, the classification point can be determined by calculation based on Stokes' equation or by several trial experiments. Elutriation is preferably performed by dispersing the powdered phosphor in an aqueous solution of sodium hexametaphosphate or water to create a dispersion, allowing the dispersion to stand, and then removing the supernatant. Other specific classification methods can be appropriately applied.

[0046] <Light-emitting device> A light-emitting device can be constructed by combining the above-mentioned phosphor with a light-emitting element. Specifically, a light-emitting device can be constructed by a light-emitting element that emits light capable of exciting the phosphor, and the above-mentioned phosphor that emits fluorescence upon receiving the light emitted from the light-emitting element. The phosphor is usually sealed with a sealing material and incorporated into the light-emitting device in the form of a wavelength conversion member.

[0047] In consideration of the characteristics of the phosphor described above, the light-emitting element is preferably a light-emitting element that emits light having a wavelength of 300 to 400 nm, and more preferably a light-emitting element that emits light having a wavelength of 345 to 385 nm. In consideration of manufacturing costs and applicability to various uses, the light-emitting element is preferably an LED element.

[0048] The application of the light-emitting device of this embodiment is not particularly limited. The light-emitting device of this embodiment can be applied to, for example, backlights for liquid crystal display devices, light source devices for projectors, lighting devices, traffic lights, etc. In addition, the light-emitting device of this embodiment is considered preferable as a lamp for indicating automatic driving (a lamp for indicating to the outside of the vehicle that the automobile is in automatic driving). This is because the light emitted from the light-emitting device of this embodiment can conform to the characteristics (chromaticity x, y, etc.) of lamps for indicating automatic driving proposed by SAE International (Society of Automotive Engineers).

[0049] In addition to the above applications, the light emitting device of this embodiment is considered to be suitable for use as a light source for inspection. Conventionally, halogen lamps with broad emission spectra have been used as light sources for industrial inspection. In order to reproduce this broad emission spectrum with an LED, it is preferable to use an LED that includes a phosphor as a wavelength conversion member that emits fluorescence with a broad spectrum when excited.

[0050] The spectrum of the fluorescence emitted when the phosphor of this embodiment is excited with light having a wavelength of 300 to 400 nm is relatively broad and flat in the wavelength region of 400 nm or slightly longer. Therefore, a light emitting device constructed by combining the phosphor of this embodiment with a light emitting element meets the above-mentioned objectives.

[0051] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various other configurations may be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of achieving the object of the present invention are included in the present invention.

[0052] The embodiments of the present invention will be described in detail based on Examples and Comparative Examples. However, it should be noted that the present invention is not limited to the Examples.

[0053] <Preparation of Raw Materials> The following raw materials were prepared: BaAl 2 O 4 : SrAl manufactured by Kojundo Kagaku Kenkyusho Co., Ltd. 2 O 4 : Si manufactured by High Purity Chemical Laboratory Co., Ltd. 3 N 4 : Manufactured by UBE Corporation (product number: E10) Al 2 O 3 : Manufactured by Sumitomo Chemical Co., Ltd. (product number: AA-03) CeO: Manufactured by Shin-Etsu Chemical Co., Ltd. (product number: C)

[0054] <Production of Phosphor> A phosphor was produced as follows. (1) Weighing and Mixing of Raw Materials Each raw material was weighed according to the mass ratio shown in Table 1 below. All of the weighed raw materials were placed in a polyethylene bag with a zipper, the zipper was closed, and the bag was shaken for 1 minute. In this way, a mixture of raw materials was obtained. The obtained mixture was passed through a #100 sieve, and the mixture that passed through the sieve was used in the next step.

[0055]

[0056] For reference, when it is assumed that the raw materials of the above composition are completely reacted, the general formula Ba a1 Sr a2 Ce b Al c Si d Oe N f The values ​​of a1, a2, b, c, d, e and f when c+d=5 are shown in Table 2.

[0057]

[0058] (2) Firing Approximately 100 g of the mixture obtained in (1) was filled into a 400 cc boron nitride container (manufactured by Denka, N1 grade). Then, it was fired under the following conditions. [Firing conditions] Firing furnace: Multipurpose firing furnace manufactured by Fuji Denpa Kogyo Co., Ltd. Firing temperature and holding time: Maximum temperature 1650°C for 4 hours in Examples 1 and 2, and maximum temperature 1550°C for 4 hours in Examples 3 to 5. Firing atmosphere: N 2 0.03MPa・G(N 2 )

[0059] (3) Crushing / Pulverization After the end of the calcination, the resulting calcined product was recovered from the container. In Examples 1 to 3, the calcined product was crushed using a mortar to the extent that it passed completely through a #200 sieve. In Examples 4 and 5, on the other hand, the calcined product was crushed using a mortar, and then jet mill pulverization was performed using a PJM-80SP device manufactured by Nippon New Match Co., Ltd., under the conditions of a sample supply rate of 20 g / min and a pulverization air pressure of 0.5 MPa.

[0060] (4) Annealing step The sample that had been crushed / pulverized in (3) was packed into a 400cc boron nitride container (manufactured by Denka, N1 grade). Then, an annealing treatment was carried out under the following firing conditions. After the annealing treatment, the sample was naturally cooled to room temperature, and the fired material was recovered from the container. The recovered material was crushed using a mortar so that it passed completely through a #200 sieve. [Annealing conditions] - Firing furnace: Multipurpose firing furnace manufactured by Fuji Denpa Kogyo Co., Ltd. - Firing temperature and holding time: 1500°C for 8 hours - Firing atmosphere: N 2 0.03MPa・G(N 2 )

[0061] (5) Acid Treatment and Decantation 10 mL of nitric acid (60% by mass, Fujifilm Wako Pure Chemical Industries, Ltd.) and 70 mL of ion-exchanged water were placed in a fluororesin beaker. The beaker was heated in a water bath until the liquid (acid aqueous solution) in the beaker reached 60°C. Approximately 20 g of the sample annealed and disintegrated in (4) was placed in the heated acid aqueous solution and stirred for 30 minutes. A magnetic stirrer was used for stirring. The rotation speed was set to 400 rpm. After stirring, the beaker was lifted from the water bath and moved, and allowed to stand for approximately 10 minutes. The supernatant was then removed by decantation, a total of three times. The slurry sample obtained after decantation was recovered by suction filtration. The recovered sample was then dried at 100°C for 12 hours. The dried sample was sieved through a #200 nylon sieve.

[0062] (6) Classification (elutriation) Based on Stokes' equation, the necessary and sufficient settling time of the phosphor powder to remove fine particles with a particle diameter of 7 μm or less when performing elutriation was calculated in advance. Based on this calculation, the sample (5) dispersed in the dispersion medium was placed in a 500 mL bottle and allowed to stand for a predetermined time, after which the supernatant liquid above a predetermined level was removed. A 0.05% by mass aqueous solution of sodium hexametaphosphate was used as the dispersion medium. This procedure was repeated several times. The powder finally obtained as a precipitate was recovered by filtration and dried. In this way, a dried powdered phosphor was obtained.

[0063] <Composition Analysis> A composition analysis was carried out on some of the phosphors of Examples 1 to 5. The Ba, Sr, Ce, Al, and Si contents in the phosphors were quantitatively analyzed using an ICP optical emission spectrometer (5110VDV manufactured by Agilent) after dissolving the phosphors by a pressure acid decomposition method. The O and N contents in the phosphors were quantitatively analyzed using an oxygen and nitrogen analyzer (EMGA-920 manufactured by Horiba, Ltd.)." Based on these analysis results, the general formula Ba a1 Sr a2 Ce b Al c Si d O e N fIn the above, the composition ratios a1, a2, b, c, d, e, and f were determined when c + d = 5. The results of the composition analysis are shown in Table 3. (Note: Although composition analysis of the phosphors of Examples 2 and 3 was not performed, given that the raw material compositions of Examples 2 and 3 are the same as those of Example 4 and that the manufacturing processes of Examples 2 and 3 are similar to that of Example 4, the compositions of the phosphors of Examples 2 and 3 are considered to be similar to that of Example 4.)

[0064]

[0065] <Particle size distribution measurement> Using Microtrac SYNC (manufactured by Microtrac Bell Co., Ltd.), measurement was performed by a laser diffraction scattering method in accordance with JIS R1629:1997. 0.2 g of phosphor powder was added to 80 mL of ion-exchanged water, and the mixture was dispersed for 90 seconds using a horn-type ultrasonic homogenizer (output: 300 W, horn diameter: 26 mm). Thereafter, the particle size distribution was measured using SYNC. From the obtained particle size distribution, the volume-based median diameter D 50 The obtained D 50 The values ​​are shown in Table 4.

[0066]

[0067] <X-ray diffraction measurement> The X-ray diffraction spectrum of the obtained sample was measured. For the measurement, an Ultima IV-N device manufactured by Rigaku Corporation was used. In the obtained X-ray diffraction spectrum, the peak intensity (maximum value) A in the 2θ range of 25.0 to 26.0° and the peak intensity (maximum value) B in the 2θ range of 29.0 to 30.0° were read. Then, the value of B / A was calculated.

[0068] The obtained X-ray diffraction spectrum is shown in Figure 1. For reference, the lower part of Figure 1 shows the general formula BaAl 2 Si 3 O 4 N 4 The values ​​of B / A are also shown in Table 5.

[0069]

[0070] <Diffuse reflectance of light with a wavelength of 700 nm or 800 nm, and absorbance of light with a wavelength of 500 nm> The diffuse reflectance of light with a wavelength of 700 nm or 800 nm was measured using an integrating sphere device (ISV-469) attached to a JASCO UV-Visible Spectrophotometer (V-550). Specifically, baseline correction was first performed using a standard reflector (Spectralon). Then, a solid sample holder filled with phosphor powder was attached to a predetermined position, and the diffuse reflectance for light with wavelengths of 700 nm and 800 nm was measured.

[0071] The absorptance (%) of light with a wavelength of 500 nm was determined in the same manner as in <Performance Evaluation> (absorptance, internal quantum efficiency, and external quantum efficiency when irradiated with light with a wavelength of 350 nm) described below, except that the wavelength of the irradiated light was 500 nm instead of 350 nm, and Qex and Qref were calculated from the spectrum in the wavelength range of 495 nm or more and 510 nm or less.

[0072] Table 6 shows the diffuse reflectance of light with a wavelength of 700 nm or 800 nm, and the absorptance of light with a wavelength of 500 nm.

[0073]

[0074] <Evaluation> (Absorptivity, Internal Quantum Efficiency, and External Quantum Efficiency When Irradiated with Light of 350 nm Wavelength) Using a spectrophotometer (MCPD-7000 manufactured by Otsuka Electronics Co., Ltd.), the absorptivity, internal quantum efficiency, and external quantum efficiency when the phosphor was irradiated with light of 350 nm wavelength were determined. The specific procedure was as follows: (1) The powdered phosphor was filled into a concave cell. At this time, the surface of the filled phosphor was made smooth. This cell was attached to a predetermined position on an integrating sphere. Monochromatic light separated into wavelengths of 350 nm from a light source (Xe lamp) was introduced into this integrating sphere using an optical fiber. This monochromatic light was irradiated onto the phosphor, and the fluorescence spectrum was measured. (2) A standard reflector with a reflectivity of 99% (Spectralon manufactured by Labsphere) was attached to a predetermined position on the integrating sphere, and the spectrum of excitation light of 350 nm wavelength was measured. The number of excitation light photons (Qex) was calculated from the spectrum in the wavelength range of 345 nm to 360 nm. (3) A cell filled with powdered phosphor was attached to a predetermined position on the integrating sphere, and the number of excitation light reflected photons (Qref) and the number of fluorescence photons (Qem) were calculated from the obtained spectral data. The number of excitation light reflected photons was calculated in the same wavelength range as the number of excitation light photons, and the number of fluorescence photons was calculated in the range of 360 nm to 700 nm. (4) The obtained Qex, Qref, and Qem were substituted into the following formulas to determine the absorptance, internal quantum efficiency, and external quantum efficiency: absorptance = (Qex - Qref) / Qex; internal quantum efficiency = Qem / (Qex - Qref); external quantum efficiency = Qem / Qex. Table 7 below lists the values ​​above multiplied by 100 and expressed as a percentage.

[0075] Furthermore, the peak wavelength, half-width, chromaticity x value, and chromaticity y value were determined from the fluorescence spectrum obtained by this measurement. Regarding the method for determining chromaticity, the chromaticity coordinates (x, y) were calculated using the calculation method for the XYZ color system specified in JIS Z 8701 in accordance with JIS Z 8724 (Method for measuring color - Light source color).

[0076] The evaluation results are summarized in Table 7.

[0077]

[0078] As shown in Table 7, the external quantum efficiency of the phosphors of Examples 1 to 4 was better than that of Example 5. a1 Sr a2 Ce b Al c Si d O e N f The phosphors that satisfy the following conditions, a1>a2, 0.70≦a1+a2+b≦1.20, 0.001≦b≦0.20, 1.50≦c≦2.50, 2.50≦d≦3.50, 3.05≦e≦6.50, and 2.75≦f≦4.40, and that emit fluorescence with a peak wavelength of 412 to 420 nm when irradiated with light of a wavelength of 350 nm, exhibited good luminescence characteristics. From the viewpoint of composition, it is thought that such good luminescence characteristics are due to the phosphor containing a relatively small amount of Ce and a relatively high content of Ba compared to Sr, etc.

[0079] <Reference: Changes in properties due to changes in manufacturing process conditions> For reference, the following two phosphors were manufactured. The properties of these phosphors were measured and evaluated, and compared with the phosphor of Example 5. (Example 5-1) A phosphor manufactured in the same manner as Example 4, except that in the above <Phosphor manufacturing>, (4) the annealing step, (5) acid treatment and decantation, and (6) elutriation were not performed. (Example 5-2) A phosphor manufactured in the same manner as Example 4, except that in the above <Phosphor manufacturing>, (5) acid treatment and decantation, and (6) elutriation were not performed.

[0080] The results are summarized in Table 8.

[0081]

[0082] As can be seen from Table 8, in Examples 4-1 and 4-2, which were not subjected to the annealing step or acid treatment, the various properties were different from those of Example 4. For example, in Examples 4-1 and 4-2, the peak wavelength of the fluorescence spectrum was greater than 520 nm. In addition, the B / A value determined by X-ray diffraction in Example 4-1 was large. From these results, it can be seen that the luminescence properties can be optimized by appropriately reducing heterogeneous phases, impurities, etc. through appropriate treatment after firing.

[0083] This application claims priority based on Japanese Patent Application No. 2023-086764, filed May 26, 2023, the disclosure of which is incorporated herein by reference in its entirety.

Claims

1. General formula Ba a1 Sr a2 C.E. b A c S d O e N f a1>a2 0.70≦a1+a2+b≦1.20 0.001≦b≦0.20 1.50≦c≦2.50 2.50≦d≦3.50 3.05≦e≦6.50 2.75≦f≦4.40 The composition ratios a1, a2, b, c, d, e, and f have the following relationship when c+d=5, and the peak wavelength of the fluorescence emitted when irradiated with light of a wavelength of 350 nm is 412 to 420 nm.

2. The phosphor according to claim 1, wherein 0.50≦a1≦0.

99.

3. The phosphor according to claim 1 or 2, wherein 0≦a2≦0.

10.

4. The phosphor according to claim 1 or 2, wherein the half-width of the fluorescence spectrum emitted when irradiated with light having a wavelength of 350 nm is 75 to 130 nm.

5. The phosphor according to claim 1 or 2, wherein the absorptance of light with a wavelength of 500 nm is 1 to 10%.

6. The phosphor according to claim 1 or 2, which has an internal quantum efficiency of 50 to 90% when irradiated with light having a wavelength of 350 nm.

7. A phosphor according to claim 1 or 2, wherein in an X-ray diffraction spectrum obtained by subjecting said phosphor to X-ray diffraction measurement, the peak intensity in the 2θ range of 25.0 to 26.0° is defined as A, and the peak intensity in the 2θ range of 29.0 to 30.0° is defined as B, and the value of B / A is 0.3 or less.

8. The phosphor according to claim 1 or 2, which has a diffuse reflectance of 92 to 97% for light with a wavelength of 700 nm.

9. The phosphor according to claim 1 or 2, which has a diffuse reflectance of 92 to 97% for light with a wavelength of 800 nm.

10. The phosphor according to claim 1 or 2, wherein the median diameter D 50 The phosphor is a powder having a particle size of 10 to 50 μm.

11. The phosphor according to claim 1 or 2, which is substantially free of Eu.

12. A light emitting device comprising a light emitting element and the phosphor according to claim 1 or 2.

13. A light emitting device according to claim 12, wherein the light emitting element emits light having a wavelength of 300 to 400 nm.

14. The light emitting device according to claim 12, wherein the light emitting element is an LED element.

15. A light emitting device according to claim 12, which is a lighting device or a signaling device.

Citation Information

Patent Citations

  • Silica nitride fluorescent powder and preparation method thereof

    CN102181285A

  • Phosphor, manufacturing method therefor, and light emitting device using the same

    JP2011037913A

  • Phosphor and production method therefor, and light emission device and image display device using phosphor

    WO2013069696A1

  • Phosphor, light-emitting device, and method for manufacturing same

    WO2015093429A1